Substrate processing method, apparatus and system

The substrate processing method addresses residue issues from halogen-containing gases by using a halogen-containing gas followed by a reducing gas to reduce metal oxide films, ensuring low resistance and defect-free metal wiring on semiconductor wafers.

JP2024157409APending Publication Date: 2024-11-07TOKYO ELECTRON LTD

Patent Information

Application Number
JP2023071761
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing methods for removing metal oxide films on semiconductor wafers result in residue formation, which increases resistance and can cause failures in metal wiring due to the use of halogen-containing gases like titanium tetrachloride, leading to issues such as increased resistance and potential etching of the metal wiring.

Method used

A substrate processing method involving the use of a halogen-containing gas to reduce metal oxide films, followed by a reducing gas to remove residues, and then forming a ruthenium layer using CVD, all performed in a vacuum atmosphere to minimize damage and residue impact.

Benefits of technology

The method effectively reduces residue and oxygen content, maintaining low resistance in the metal wiring and preventing defects, thereby improving the precision and efficiency of metal wiring formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157409000001_ABST
    Figure 2024157409000001_ABST
Patent Text Reader

Abstract

To reduce residuals from halogen-containing gases that are not converted to plasma to reduce the metal oxide film, and to further reduce the metal oxide film, as well as to suppress the shape changes of wafer W.SOLUTION: A substrate processing method is a method for processing a substrate with a metal layer, and includes a step for supplying a halogen-containing gas to the substrate to reduce the metal oxide film formed on the surface of the metal layer, and a step for supplying a reducing gas to the substrate to reduce residuals in the metal layer left by the supply of the halogen-containing gas.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to substrate processing methods, apparatus, and systems. [Background technology]

[0002] The manufacturing process of a semiconductor device includes a process of forming metal wiring on a semiconductor wafer (hereinafter, referred to as "wafer"), which is a substrate. In the process of forming this wiring, a process of removing oxide formed by oxidation of the surface of the metal layer may be required. For example, Patent Document 1 describes a method of removing a tungsten oxide film formed by natural oxidation of the surface of a tungsten layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-059916 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides techniques for reducing residues from delivering halogen-containing gases to reduce metal oxide films. [Means for solving the problem]

[0005] The substrate processing method according to the present disclosure includes: 1. A method for treating a substrate having a metal layer, comprising the steps of: supplying a halogen-containing gas to the substrate to reduce a metal oxide film formed on a surface of the metal layer; Then, a reducing gas is supplied to the substrate, and a residue remaining on the metal layer is reduced by supplying the halogen-containing gas; Contains: Effect of the Invention

[0006] According to the present disclosure, residuals from supplying a halogen-containing gas to reduce a metal oxide film can be reduced. [Brief description of the drawings]

[0007] [Figure 1A] 3 is a vertical cross-sectional side view of a recess formed in a wafer according to a first embodiment of the present disclosure. FIG. [Figure 1B] FIG. 4 is a second vertical cross-sectional side view of the recess. [Figure 1C] FIG. 11 is a third vertical cross-sectional side view of the recess. [Figure 1D] FIG. 4 is a fourth vertical cross-sectional side view of the recess. [Diagram 2] 1 is a plan view of a substrate processing system according to a first embodiment. [Diagram 3] 4 is a vertical sectional side view of a first processing module provided in the substrate processing system. FIG. [Figure 4] FIG. 2 is a flowchart showing a processing procedure according to the first embodiment. [Figure 5A] FIG. 11 is a first graph showing experimental results of a preliminary test. [Figure 5B] FIG. 2 is a second graph showing experimental results of a preliminary test. [Figure 5C] FIG. 3 is a third graph showing experimental results of a preliminary test. [Figure 6A] FIG. 1 is a first graph showing the experimental results of Example 1. [Figure 6B] FIG. 2 is a second graph showing the experimental results of Example 1. [Figure 6C] FIG. 3 is a third graph showing the experimental results of Example 1. [Figure 7A] FIG. 13 is a first graph showing the experimental results of Example 2. [Figure 7B] FIG. 2 is a second graph showing the experimental results of Example 2. [Figure 7C] FIG. 3 is a third graph showing the experimental results of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] (First embodiment) Before describing a first embodiment of a substrate processing method according to the present disclosure, a configuration of a wafer W, which is a substrate to be processed, will be described. Fig. 1A is a vertical cross-sectional side view showing a portion of a surface layer of a wafer W before processing. The base layer of the wafer W is a silicon layer made of, for example, silicon (Si), but this silicon layer is not shown in the figure.

[0009] A silicon oxide (SiOx) layer 12 is formed on the upper side of this silicon layer. A plurality of vertically elongated recesses 11 are formed in this silicon oxide layer by etching from above so as to open upward. A silicon nitride (SiN) layer used in the etching is formed on the sidewall of the recess 11, but is not shown in FIGS. 1A to 1D. A tungsten (W) layer 13, which is a first metal layer, is exposed on the bottom surface of the recess 11. This tungsten layer 13 constitutes the metal wiring of a semiconductor device manufactured from the wafer W, and its lower end is laminated on the upper layer of the above-mentioned silicon layer via, for example, a titanium nitride (TiN) layer (not shown). A tungsten oxide film 14, which is a metal oxide film naturally oxidized when the wafer W is transported in the atmosphere, is formed on the surface of the tungsten layer 13 facing the inside of this recess 11.

[0010] For the above wafer W, a ruthenium (Ru) layer 17 is formed as a second metal layer in the recess 11 to form a metal wiring. On the other hand, if a tungsten oxide film 14 is formed between the tungsten layer 13 and the ruthenium layer 17, it not only increases the resistance of the metal wiring, but also causes poor filling of the ruthenium layer 17. For this reason, in the substrate processing method of the present disclosure, a process of reducing the tungsten oxide film 14 using a halogen-containing gas, for example, titanium tetrachloride (TiCl4) gas, is performed. While TiCl4 gas efficiently promotes the reduction of the tungsten oxide film 14, it also causes titanium (Ti) and chlorine (Cl) contained in the TiCl4 gas to remain in the tungsten film after reduction (the "reduced tungsten film 15" described later). Titanium also increases the resistance of the metal wiring, and when HCl is generated from chlorine, there is a risk that the metal wiring will be etched. In addition, chlorine may inhibit the formation of the ruthenium layer 17.

[0011] Therefore, in this embodiment, a step of reducing the residue in reduced tungsten film 15 is performed, and then a step of forming ruthenium layer 17 is performed. Hereinafter, the step of reducing tungsten oxide film 14 may be referred to as the reduction step, the step of reducing the residue as the removal step, and the step of forming ruthenium layer 17 as the film formation step.

[0012] A series of processes will be described below with reference to Fig. 1B to Fig. 4, which show changes in the surface of the wafer W. During the series of processes, the environment around the wafer W is a vacuum atmosphere. That is, the wafer W is not exposed to the atmosphere during the series of processes. For this reason, each step is performed with the wafer W stored in a processing vessel.

[0013] First, a reduction step is performed in which TiCl4 gas, which is a halogen-containing gas, is supplied to the wafer W. At this time, the TiCl4 gas is supplied to the wafer W without activation such as plasma generation. As a result, a reducing atmosphere is formed in the processing vessel in which the wafer W is accommodated. As a result, the tungsten oxide film 14 reacts with the TiCl4 gas to become a reduced tungsten film 15 as shown in FIG. 1B. The reduced tungsten film 15 is the tungsten oxide film 14 reduced, and has a lower oxygen content than the tungsten oxide film 14.

[0014] At this time, the reduced tungsten film 15 contains chlorine and titanium, which are the residues of titanium tetrachloride that reacted with the tungsten oxide film 14. "Containing titanium tetrachloride residues" does not only mean that the reduced tungsten film 15 contains the residues inside, but also includes the case where the residues are attached to the surface. Hereinafter, the titanium tetrachloride residues may be simply referred to as residues. In FIG. 1B, the reduced tungsten film 15 containing a large amount of residues after the reduction step is performed is shown with a sand-like pattern added to the diagonal hatching that slopes downward to the right.

[0015] Subsequently, a removal process is performed to remove the residue remaining on the reduced tungsten film 15 of the wafer W. In this embodiment, the removal of the residue is performed by supplying a reducing gas to the wafer W including the reduced tungsten film 15. The reducing gas is a gas for forming a reducing atmosphere in the space in which the wafer W is placed during processing, and can be exemplified by hydrogen gas plasma (hydrogen gas plasma). In addition, when hydrogen gas plasma is supplied, if accelerated high-energy hydrogen ions collide with the surface of the wafer W, the SiOx layer 12 constituting the recess 11 may be damaged. Specifically, a case can be exemplified in which the SiOx layer 12 constituting the opening portion or the middle region of the recess 11 is partially scraped off by the collision of ions, causing the recess 11 to partially expand.

[0016] Therefore, it is preferable that the hydrogen gas plasma supplied to the wafer W during the removal step is a low-energy hydrogen gas plasma containing ions and hydrogen radicals with reduced energy. A specific configuration of a substrate processing module (first processing module 51) that supplies low-energy hydrogen gas plasma will be described later with reference to FIG. 3. When the plasmatized hydrogen gas is supplied to the wafer W and enters the recess 11 to reach the reduced tungsten film 15, the residue reacts with the active species in the hydrogen gas plasma, and the residue is removed (FIG. 1C). In FIG. 1C, the reduced tungsten film 15 after the removal step is performed and the content of the residue is reduced is shown by hatching with diagonal lines slanting downward to the right without adding a sand-like pattern.

[0017] In addition, by using hydrogen gas plasma, which is a reducing gas, in the residue removal process, the content of oxygen remaining after the reduction process is reduced, which further suppresses the occurrence of poor embedding of ruthenium layer 17 into reduced tungsten film 15 and reduces wiring resistance.

[0018] Next, a film formation process is performed to form a ruthenium layer 17 on the wafer W by CVD. The film formation gas is, for example, Ru3(CO) 12 (Triruthenium dodecacarbonyl) gas. Hereafter, Ru3(CO) 12 The gas is sometimes called DCR gas. As a result, a ruthenium (Ru) layer 17 is formed so as to be embedded in the recesses 11 above the reduced tungsten film 15. Thereafter, the Ru layer 17 formed on the upper surface of the SiOx layer 12 is removed by CMP (Chemical Mechanical Polishing), so that ruthenium is embedded in the recesses 11 as shown in FIG. 1D. The ruthenium layer 17 and tungsten layer 13 (reduced tungsten film 15) thus formed constitute wiring with low oxygen and residue content on the wafer W and low resistance.

[0019] A substrate processing system 1, which is an embodiment of a substrate processing system capable of carrying out the above-mentioned series of processes, will be described with reference to the plan view of Fig. 2. The substrate processing system 1 includes a loader module 31, a load lock module 35, a vacuum transfer module 41 corresponding to a vacuum transfer device, a first processing module 51 for carrying out a reduction process and a removal process, and a second processing module 52 for carrying out a film formation process. The first processing module corresponds to the "substrate processing device" and the "first device" recited in the claims, and the second processing module 52 corresponds to the "second device."

[0020] The loader module 31, the load lock module 35, and the vacuum transfer module 41 are arranged linearly in this order in the front-rear direction. In the following description of the substrate processing system 1, the side where the loader module 31 is located is referred to as the front side, and the side where the vacuum transfer module 41 is located is referred to as the rear side.

[0021] The loader module 31 includes a housing whose interior is at atmospheric pressure, a transfer mechanism 32 for the wafer W provided in the housing, and a load port 33. In this example, four load ports 33 are provided in a row on the left and right side of the front side of the housing. A transfer container 34 for storing the wafer W, called a FOUP (Front Opening Unified Pod), is placed on each load port 33. The transfer mechanism 32 is, for example, configured by an articulated arm that can move left and right, and can transfer the wafer W between the transfer container 34 on each load port 33 and each load lock module 35.

[0022] In this embodiment, three load lock modules 35 are provided side by side when viewed from the front side. Each load lock module 35 has a housing, and the housing is connected to the loader module 31 and the vacuum transfer module 41 via gate valves G provided on the front and rear sides, respectively. When the gate valves G on the front and rear sides of the housing are closed, the pressure inside the housing can be freely changed between atmospheric pressure and vacuum pressure. A stage (not shown) on which the wafer W is placed is provided inside the housing, and the stage is configured to be able to deliver the wafer W to the transfer mechanism 32 and the vacuum transfer mechanism 44 (described later) that access the load lock module 35, respectively.

[0023] The vacuum transfer module 41 includes a housing 41A and a vacuum transfer mechanism 44 provided in the housing 41A. The housing 41A has exhaust ports 45, each of which is connected to one end of an exhaust pipe. The other end of the exhaust pipe is connected to an exhaust mechanism 46 formed of, for example, a turbo molecular pump, and the inside of the housing 41A is maintained in a vacuum atmosphere by exhausting air from the exhaust port 45 by the exhaust mechanism 46. The inside of the housing 41A, which is made into a vacuum atmosphere by the exhaust mechanism 46, corresponds to a vacuum atmosphere transfer path along which the wafer W is transferred.

[0024] A first processing module 51 and a second processing module 52 arranged side by side in the front and rear are connected via gate valves G1 to the left and right of the housing 41A of the vacuum transfer module 41 as viewed from the front side. The transfer of the wafer W between the first processing module 51, the second processing module 52, and the load lock module 35 is performed by a vacuum transfer mechanism 44 constituted by, for example, an articulated arm movable back and forth.

[0025] Correspondence between the processes performed in each of the process modules 51 and 52 and the series of processes described above is shown. In the first process module 51, a reduction process and a removal process are performed, and in the second process module 52, a film formation process is performed. Each of the process modules 51 and 52 includes a process vessel 61 that is evacuated to create a vacuum atmosphere inside, and each process is performed in the process vessel 61. Therefore, the reduction process and the removal process are performed on the wafer W in the same process vessel 61.

[0026] The substrate processing system 1 includes a control unit 30, which is a computer, and the control unit 30 includes a program. The program includes commands (each step) for processing the wafer W and transporting the wafer W as described above. The program is stored in a storage medium, such as a compact disc, a hard disk, or a DVD, and is installed in the control unit 30. The control unit 30 outputs control signals to each part of the substrate processing system 1 by the program, and controls the operation of each part. Specifically, the control unit 30 controls the operation of the processing modules 51 and 52, the opening and closing of the gate valves G and G1, the operation of the transport mechanism 32, the operation of the vacuum transport mechanism 44, the operation of the exhaust mechanism 46, the switching of the pressure in the load lock module 35, and the like. The control of the operation of the processing modules 51 and 52 includes, for example, the temperature control of the wafer W by supplying power to the heater 66, which will be described later, the control of the supply and cut-off of each gas into the processing vessel 61, and the control of plasma formation by turning on and off the high frequency power source 82, which will be described later.

[0027] Regarding the transfer path of the wafer W in the substrate processing system 1, the wafer W is first transferred in the order of the transfer container 34 → the loader module 31 → the load lock module 35 → the vacuum transfer module 41. The wafer W is then transferred in the order of the first processing module 51 → the vacuum transfer module 41 → the second processing module 52. Thereafter, the wafer W is transferred in the order of the vacuum transfer module 41 → the load lock module 35 → the loader module 31, and is returned to the transfer container 34.

[0028] Next, the first processing module 51, which performs the reduction step and the removal step as a representative of the processing modules 51 and 52, will be described with reference to the vertical side view of FIG. 3. As described above, a transfer port for the wafer W is formed on the side wall of the processing vessel 61 of the first processing module 51, and a gate valve G1 for opening and closing the transfer port is provided. The processing vessel 61 is also grounded. One end of an exhaust pipe 62 is connected to open to the wall of the processing vessel 61, and an exhaust mechanism 63 provided at the other end of the exhaust pipe 62 exhausts the inside of the processing vessel 61 to a vacuum atmosphere of a desired pressure. Specifically, the pressure in the processing vessel 61 is set to about 1330 Pa (10 torr) in the reduction step, and about 133 Pa (1 torr) in the removal step. The exhaust mechanism 63 exhausts the inside of the processing vessel 61 for, for example, about 10 seconds between the reduction step and the removal step, and replaces the gas in the processing vessel 61.

[0029] A substrate mounting table 64 for mounting a wafer W thereon is provided within the processing vessel 61, and the wafer W is transferred between the substrate mounting table 64 and the vacuum transfer mechanism 44 by means of lift pins 65 configured to be freely raised and lowered from the upper surface of the substrate mounting table 64. A heater (not shown) is embedded in the substrate mounting table 64, and heats the wafer W to a preset temperature during processing. Specifically, the heater temperature is controlled so that the wafer W is heated to about 400° C. in the reduction step and the removal step. A grounded electrode 67 for generating plasma is embedded in the substrate mounting table 64, forming a lower electrode.

[0030] An opening is formed in the upper part of the processing vessel 61, and a shower head 71 is fitted into the opening via an insulating member 68 so as to face the substrate mounting table 64. The shower head 71 is made of metal and has an overall cylindrical shape. The shower head 71 has an internal space 72 which serves as a gas diffusion space, and a shower plate 73 which forms the lower surface. The shower plate 73 is formed with a plurality of gas discharge holes 74 which each communicate with the internal space 72. The shower head 71 is formed with gas inlet holes for supplying various gases to the internal space 72. The gas inlet holes are connected to the downstream ends of gas supply units 75 for supplying various gases, and are provided to supply various gases to the internal space 72.

[0031] The gas supply unit 75 has gas supply sources 76 for a halogen-containing gas, a reducing gas, and argon (Ar) gas as a plasma generating gas, gas supply pipes 77 provided corresponding to each gas supply source 76, and flow rate controllers 78 provided for each gas supply pipe 77. The flow rate controller 78 is composed of a flow rate control mechanism such as a valve and a mass flow controller, and can individually adjust the flow rate of each gas and supply it into the processing vessel 61 by cutting off the supply of each gas to the downstream side according to a control signal from the control unit 30. The argon gas is not limited to being supplied as an auxiliary gas for plasma generation, but is also supplied as an inactivation gas together with the halogen-containing gas in the reduction process. The flow rate ratio of the halogen-containing gas to the argon gas in the reduction process is, for example, about 1:10, and the flow rate ratio of the reducing gas to the argon gas in the removal process is, for example, about 1:120.

[0032] A high-frequency power supply 82 is connected to the showerhead 71, which serves as an upper electrode, via a power supply line 81 to form the upper electrode. The high-frequency power supply 82 supplies high-frequency power of, for example, 10 kHz to 60 MHz and 300 W to the showerhead 71 to generate a capacitively coupled plasma of a reducing gas between the showerhead 71 and the substrate mounting table 64. A matching box 83 is connected to the power supply line 81 downstream of the high-frequency power supply 82. The matching box 83 matches the internal (or output) impedance of the high-frequency power supply 82 with the load impedance.

[0033] Between the high frequency power supply 82 and the upper electrode, more specifically, in the downstream portion of the matching box 83 of the power supply line 81, a voltage waveform shaping unit 84 is provided to shape the voltage waveform of the high frequency power supply so as to suppress the positive voltage (plus voltage) of the high frequency voltage applied to the upper electrode. In this embodiment, the voltage waveform shaping unit 84 uses, for example, that described in JP 2022-018062 A. That is, the voltage waveform shaping unit 84 has a capacitor 84a provided downstream of the matching box 83, and a ground circuit 84c that branches from the downstream side of the capacitor 84a and is grounded via a diode 84b. As the capacitor 84a, one having a sufficient capacity to lower the impedance as viewed from the high frequency power supply 82 is used.

[0034] If the voltage waveform shaping unit 84 were not provided in the first processing module 51, when the high frequency power output from the high frequency power supply 82 is a positive voltage, the sheath voltage (the difference between the plasma potential and the substrate potential) becomes large as a positive voltage. This sheath voltage accelerates the positively charged hydrogen ions contained in the plasma toward the wafer W, whose potential is zero, and collides with the wafer W with high kinetic energy.

[0035] In response to this, when the high frequency power supply 82 outputs a positive voltage, the voltage waveform shaping unit 84 prevents the application of a positive voltage to the upper electrode by causing the diode 84b to pass a current to the ground side, thereby reducing the sheath voltage and suppressing an increase in ion energy. At this time, the capacitor 84a stores power, and the stored power is input to the plasma region on the upper electrode side together with the high frequency power output when the high frequency power supply 82 outputs a negative voltage, thereby efficiently increasing the plasma density. The plasma supply mechanism 80, which is composed of the voltage waveform shaping unit 84, high frequency power supply 82, etc. as described above, can form a high-density plasma containing low-energy ions that can prevent damage to the wafer W by ions.

[0036] Next, the second processing module 52 will be described, focusing on the differences from the processing module 51. Since the second processing module 52 does not perform plasma processing, the plasma supply mechanism 80 and the electrode 67 of the substrate mounting table 64 may not be provided, and the processing chamber 61 may be configured so that plasma is not generated. In addition, the gas supply source 76 that supplies gas into the processing chamber 61 stores the gas used in the film formation process described above. Except for these differences, the processing module 52 has a configuration generally similar to that of the first processing module 51, but the temperature of the wafer W is set to a temperature lower than that during the reduction and removal processes in the first processing module 51, for example, 200° C. or lower.

[0037] 2 to 4, an operation of executing a series of processes on a wafer W using the substrate processing system 1 having the above-described configuration. First, when the vacuum transfer mechanism 44 in the vacuum transfer module 41 receives the wafer W to be processed from the load lock module 35, the gate valve G1 of the first processing module 51 is opened, and the wafer W is moved into the processing vessel 61 from the loading port by the vacuum transfer mechanism 44. Then, the wafer W is transferred from the vacuum transfer mechanism 44 to the substrate mounting table 64 using the lift pins 65, and the vacuum transfer mechanism 44 is moved out of the processing vessel 61 and the gate valve G1 is closed.

[0038] Then, a reduction step is performed first. The pressure inside the processing vessel 61 and the temperature of the wafer W are adjusted in accordance with the recipe settings for the reduction step. Next, TiCl4 gas is supplied into the processing vessel 61 together with argon gas. At this time, no high frequency power is supplied from the high frequency power supply 82 to the shower head 71. By reacting with the TiCl4 gas, the tungsten oxide film 14 on the wafer W is reduced (step S1 in FIG. 4) and becomes a reduced tungsten film 15 containing residues (FIG. 1B).

[0039] Next, the removal process is performed. The pressure and temperature in the processing vessel 61 are adjusted according to the recipe settings in the removal process. The set temperature of the wafer W in the removal process is in the same range as the set temperature of the wafer W in the reduction process, so that the throughput can be improved by performing both the reduction process and the removal process in the same processing vessel 61, that is, in the same first processing module 51. In the removal process, high-frequency power is applied to the shower head 71 from the high-frequency power source 82 while supplying hydrogen gas and argon gas. At this time, the voltage waveform shaping unit 84 described above supplies high-frequency power with a shaped voltage waveform, thereby forming low-energy, high-density hydrogen gas plasma containing hydrogen ions and hydrogen radicals with reduced energy. As described above, by supplying low-energy hydrogen gas plasma, damage to the SiOx layer 12 can be suppressed.

[0040] Then, by reaction with the plasmatized hydrogen gas, residues are removed from reduced tungsten film 15 exposed toward the inside of recess 11, and further reduction can be promoted (Step S2 in FIG. 4, FIG. 1C). At this time, the residues adhering to the inside of recess 11 are also removed by the plasmatized hydrogen gas, so that deterioration of the embedding property of ruthenium layer 17 can be suppressed.

[0041] According to the reduction step and removal step as described above, by utilizing reduction that does not physically remove the tungsten oxide film 14 as in etching, and low-energy hydrogen gas plasma, damage to the recess 11 is suppressed and the shape at the time of formation is easily maintained. By forming the ruthenium layer 17 in the recess 11 in which the shape at the time of formation is maintained in this manner, the formation accuracy of the metal wiring is improved. In addition, by preparing gas species capable of carrying out the reduction step and removal step in the gas supply source 76 connected to the first processing module 51 equipped with the plasma supply mechanism 80 including the voltage waveform shaping unit 84, these steps can be efficiently carried out in the same module.

[0042] After the removal step is completed, the wafer W is unloaded from the first processing module 51 in the reverse order to the loading step, and then the wafer W is loaded into the second processing module 52 in the same order as the loading step into the first processing module 51, where the film forming step is performed. When the wafer W is transferred from the first processing module 51 to the second processing module 52, the transfer is performed via the vacuum transfer module 41, which is a transfer path in a vacuum atmosphere, so that the wafer W is not exposed to the air atmosphere. Therefore, the reduced tungsten film 15 reduced in the reduction step and removal step can be prevented from being re-oxidized by the air atmosphere.

[0043] Next, a film forming process is performed. In the second process module 52, in which temperature and pressure have been adjusted according to the recipe settings for the film forming process, DCR gas that has not been turned into plasma is supplied into the process vessel 61. The DCR gas deposits a ruthenium layer 17 on the reduced tungsten film 15 of the wafer W (step S3), and a wiring layer is formed in the recess 11, in which the tungsten layer 13 and the ruthenium layer 17 are deposited. The interior of the recess 11 from which the residue has been removed in the removal process and the ruthenium layer 17 are well embedded in the recess 11, and the upper layer side of the tungsten layer 13 is the reduced tungsten film 15, so that a wiring layer with a low resistance value can be formed.

[0044] (Modification of the first embodiment) In the first embodiment, a removal step with high reducing power and suppressed damage to the recesses 11 is realized by performing low-energy plasma treatment by the voltage waveform shaping unit 84. On the other hand, if the film formation treatment is one in which the voltage waveform shaping unit 84 is used and the degree of deformation of the recesses 11 is acceptable, the removal step may be performed by a first treatment module 51A (not shown) that does not include the voltage waveform shaping unit 84. That is, in this case, the removal step may use plasma of a reducing gas that is not subjected to energy reduction treatment. In this case, an effect like that of Example 1-2 described later is expected.

[0045] Second embodiment The substrate processing system 1 according to the second embodiment uses the same substrate processing system 1 as the first embodiment, but performs the removal process using plasma containing ammonia (NH3) gas as a reducing gas in the removal process. In particular, the gas supply unit 75 of the first processing module 51 is configured to supply approximately the same amount of nitrogen (N2) gas as an auxiliary gas to a mixed gas of ammonia gas and hydrogen gas. In particular, the flow rate ratio of hydrogen gas to ammonia gas is 0.4 to 1.5, and preferably 1 to 1.2.

[0046] Using the gas supply unit 75 and plasma supply mechanism 80 configured as above, low-energy plasma of a mixed gas of ammonia gas and hydrogen is generated. This allows the process of removing residues from the reduced tungsten film 15 to be carried out while suppressing damage to the recess 11. According to the reducing gas of this embodiment, chlorine can be effectively reduced by ammonia gas, and nitridation after the removal process can be suppressed by hydrogen gas. The pressure inside the processing vessel 61 in the removal process is set to about 1 / 3 of that in the reduction process.

[0047] (Modification of the second embodiment) When the reducing gas used in the removal process contains ammonia gas, it is not essential to convert the gas into plasma. In other words, in the removal process, a mixed gas of ammonia gas and hydrogen may be supplied into the processing vessel 61 without being converted into plasma. In this modification, since plasma is not generated, the first processing module 51 does not need to include the plasma supply mechanism 80. When plasma is not used, the supply time of the reducing gas is about three times longer than that of the second embodiment using plasma.

[0048] (Modification) In the above-described first and second embodiments and their modified examples, the reduction step and the removal step are carried out in the same first treatment module 51 for the sake of efficiency, but they may be carried out in separate treatment modules.

[0049] Moreover, the halogen-containing gas is not limited to TiCl4 gas, and may be, for example, other halogen-containing gas. Specific examples include boron trichloride (BCl3) gas, tungsten hexafluoride (WF6) gas, tungsten pentachloride (WCl5) gas, tungsten hexachloride (WCl6) gas, and the like. Other halogen-containing gases may be used that are composed of molybdenum (Mo) or Ti other than TiCl4 gas. Although it has been described that argon gas is supplied as an inert gas together with the halogen-containing gas, the inert gas is not limited to argon gas, and may be, for example, nitrogen gas. The flow rate ratio of each gas described above is merely an example and may be changed as appropriate.

[0050] The ruthenium layer 17 in the recess 11 was formed using Ru3(CO) 12For example, gases including (2,4-dimethylpentadienyl)(ethylcyclopentadienyl)ruthenium[(Ru(DMPD)(EtCp)], bis(2,4-dimethylpentadienyl)Ruthenium[Ru(DMPD)2], (4-dimethylpentadienyl)(methylcyclopentadienyl) Ruthenium[(Ru(DMPD)(MeCp)], Bis(Cyclopentadienyl)Ruthenium[(Ru(C5H5)2], Cis-dicarbonyl bis(5-methylhexane-2,4-dionate)ruthenium(II), bis(ethylcyclopentadienyl)Ruthenium(II)[Ru(EtCp)2], Ru(chd)(ipmb), Ru(EtBz)(EtCHD) and the like may be used as Ru3(CO) 12 can be used instead of to deposit the ruthenium layer 17.

[0051] The second metal film formed in the recess 11 is preferably a ruthenium layer 17 in order to reduce the wiring resistance, but is not limited to the formation of the ruthenium layer 17. For example, it is preferable to form a molybdenum layer or a tungsten layer instead of the ruthenium layer 17 by supplying a film forming gas, since it is possible to obtain a relatively small wiring resistance. For the same reason, the first metal film constituting the bottom surface of the recess 11 is not limited to the tungsten layer 13, and may be a ruthenium layer, a molybdenum layer, a cobalt layer, or a titanium layer. The titanium layer may be the titanium nitride layer already described formed under the tungsten layer 13.

[0052] It should be noted that the embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, modified, or combined in various forms without departing from the scope and spirit of the appended claims. EXAMPLES

[0053] (Preliminary Examination) The tungsten oxide film 14 before the series of treatments and the reduced tungsten film 15 after the reduction process, in which only the reduction process of the present disclosure was performed, were examined by X-ray photoelectron spectroscopy (XPS) to confirm the change in the amount of oxygen and residues due to the reduction process. As for the residues, titanium and chlorine (Cl) derived from TiCl4 gas were measured.

[0054] A. Preliminary Examination Conditions Using the substrate processing system 1 of the first embodiment and a bare wafer having a TiN layer and a tungsten layer 13 laminated on the surface of a silicon wafer, the reduction process of the first embodiment is performed on a tungsten oxide film 14 formed by natural oxidation on the surface. XPS analysis was performed on the tungsten oxide film 14 before the reduction process and the reduced tungsten film 15 after the reduction process.

[0055] B. Preliminary Test Results Among the XPS analyses of the tungsten oxide film 14 before the reduction process and the reduced tungsten film 15 after the reduction process, the spectrum of the electrons emitted from the 1s orbital of the O atom, the spectrum of the electrons emitted from the 2p orbital of the Ti atom, and the spectrum of the electrons emitted from the 2p orbital of the Cl atom are shown in Figures 5A, 5B, and 5C. As shown in Figure 5A, the peak indicating oxygen is smaller after the reduction process than before the treatment, so it is understood that the tungsten oxide film 14 was effectively reduced and removed by the reduction process. Also, as shown in Figures 5B and 5C, the peaks indicating titanium and chlorine are larger after the reduction process than before the reduction process, so it is understood that a large amount of residue remains in the reduced tungsten film 15 due to the reduction process. For comparison with the following examples, the peak values ​​of the photoelectron spectrum of the O atom, Ti atom, and Cl atom after the reduction process are α, β, and γ, respectively.

[0056] (experiment) The reduction step similar to that of the preliminary test and the removal step in the first and second embodiments (including the modified examples of each embodiment) were performed, and the amounts of oxygen and residues were confirmed by XPS analysis for the reduced tungsten film 15 after the reduction step and the removal step. The oxygen and residues were analyzed for the same samples as those in the preliminary test.

[0057] A. Experimental conditions [Example 1] Using the same substrate processing system 1 and two wafers W as in the preliminary test, the reduction process and the removal process for the first embodiment and the modified example of the first embodiment were performed. Specifically, in Example 1-1, the reduction process and the removal process using hydrogen gas plasma of the first embodiment were performed on the wafer W, and the reduced tungsten film 15 after the removal process was analyzed by XPS. In Example 1-2, the reduction process and the removal process of the modified example of the first embodiment (when forming the hydrogen gas plasma, high-frequency power not subjected to voltage shaping using the voltage waveform shaping unit 84 was applied) were performed on the wafer W, and the reduced tungsten film 15 after the removal process was analyzed by XPS. In Examples 1-1 and 1-2, the TiCl4 gas and the reducing gas were each supplied once. The supply time of each reducing gas was set to, for example, 20 seconds, and the supply time of each TiCl4 gas was set to 10 times or more the supply time of each reducing gas. In order to confirm the difference in the reduced tungsten film 15 due to the difference in the technique of the embodiment, the operating conditions of each mechanism, such as the temperature of the substrate mounting table 64, were set to be the same for the same process in the embodiments 1-1 and 1-2 and the embodiments described later, unless otherwise specified.

[0058] [Example 2] Using the same substrate processing system 1 and two wafers W as in Example 1, the reduction process and the removal process in the second embodiment and the modified example of the second embodiment were performed. Specifically, in Example 2-1, the reduction process and the removal process in the second embodiment (a mixed gas of ammonia gas and hydrogen gas, and a plasma of nitrogen gas were supplied) were performed on the wafer W, and the reduced tungsten film 15 after the removal process was analyzed by XPS. In Example 2-2, the reduction process and the removal process in the modified example of the second embodiment (ammonia gas that was not plasmatized was supplied) were performed on the wafer W, and the reduced tungsten film 15 after the removal process was analyzed by XPS. In Examples 2-1 and 2-2, the pressure inside the processing vessel 61 during each removal process was set lower than the pressure inside the processing vessel 61 during the reduction process and higher than the pressure inside the processing vessel 61 during the removal process in Example 1. The supply time of the reducing gas in Example 2-2 was three times longer than that in Example 2-1.

[0059] [Example 3] In Example 3, based on Example 1-1, it was confirmed whether there was a change in the amount of oxygen or residue when the setting conditions of the removal process were changed. In Example 3-1, the supply time of the halogen-containing gas in Example 1-1 was the same, and the number of times that the halogen-containing gas and the reducing gas were supplied was divided into 4, 8, and 12 times, and XPS analysis was performed to confirm whether there was a change due to the number of times of supply. In Example 3-2, the high-frequency power was changed to 300W, 600W, and 900W, and the removal process was performed and XPS analysis was performed to confirm whether there was a change due to the magnitude of the high-frequency power.

[0060] B. Experimental Results [Example 1] The results of the XPS analysis for Example 1 are shown in Figures 6A to 6C. In these figures, the spectrum of the reduced tungsten film 15 of Example 1-1 is shown by a solid line, and the spectrum of the reduced tungsten film 15 of Example 1-2 is shown by a dashed line. In addition, the positions α, β, and γ of the peaks of O atoms, Ti atoms, and Cl atoms after the reduction process in the preliminary test are also shown. In Example 1-1, in which low-energy hydrogen plasma was used, the reduced tungsten film 15 after the reduction process was further reduced to reduce the oxygen content and the titanium-derived residues were also reduced. However, the chlorine-derived residues were hardly reduced. On the other hand, in Example 1-2, in which hydrogen plasma was formed by supplying high-frequency power without voltage shaping, the reduced tungsten film 15 after the reduction process was further reduced to reduce the oxygen content and also reduce the titanium-derived and chlorine-derived residues. According to Examples 1-1 and 1-2, it was found that both of them were able to remove the residues accompanying the implementation of the reduction process and to further promote reduction.

[0061] [Example 2] The results of the XPS analysis for Example 2 are shown in Figures 7A to 7C. In these figures, the spectrum of reduced tungsten film 15 of Example 2-1 is shown by a solid line, and the spectrum of reduced tungsten film 15 of Example 2-2 is shown by a dashed line. It was found that in both Example 2-1, in which plasma of an ammonia-containing gas with low energy ions was used, and Example 2-2, in which ammonia gas that was not plasmatized was used, reduced tungsten film 15 after the reduction step was further reduced, and titanium-derived and chlorine-derived residues were also reduced.

[0062] From the above results, it was found that the reduction of tungsten oxide film 14 and the reduction of residues due to the reduction process can be achieved by the reduction process using a halogen-containing gas and the removal process in which plasma of a reducing gas containing low-energy ions is supplied by plasma supply mechanism 80. It was also found that when the reducing gas is ammonia gas, the same effect can be achieved even when a gas that has not been made into plasma is used.

[0063] [Example 3] Although the analysis data of Examples 3-1 and 3-2 are omitted, the analysis results of Example 3-1 showed a tendency that the further reduction of the reduced tungsten film 15 proceeds with an increase in the number of times of supply. On the other hand, for the residue, the titanium-derived and chlorine-derived residues tended to exceed the peaks β and γ described above. For this reason, it was found that it may be preferable to supply the halogen-containing gas and the reducing gas once each, rather than repeatedly supplying them in multiple portions. According to the results of the XPS analysis of Example 3-2, a tendency was observed that further reduction was effectively performed when the high-frequency power supplied during the removal process was increased. On the other hand, no tendency was observed to further reduce the residue. [Explanation of symbols]

[0064] W wafer 13 Tungsten layer 14 Tungsten oxide film

Claims

1. 1. A method for treating a substrate having a metal layer, comprising: supplying a halogen-containing gas to the substrate to reduce a metal oxide film formed on the surface of the metal layer; Next, a step of supplying a reducing gas to the substrate to reduce residues remaining on the metal layer due to the supply of the halogen-containing gas; A substrate processing method comprising:

2. 2. The substrate processing method according to claim 1, wherein the halogen-containing gas is titanium tetrachloride gas.

3. the reducing gas includes at least one of hydrogen gas and ammonia gas; 2. The substrate processing method according to claim 1, wherein in the step of reducing the residue, the reducing gas is converted into plasma and supplied to the substrate.

4. The processing of the substrate is performed in a state where the substrate is placed on a substrate placement table provided in a processing chamber, 4. The substrate processing method according to claim 3, wherein the plasma of the reducing gas is formed by applying the high-frequency power, the positive voltage of which is suppressed by a voltage waveform shaping unit provided between the upper electrode and the high-frequency power supply, to the reducing gas supplied between a grounded lower electrode constituting the substrate mounting table and an upper electrode disposed in the processing vessel opposite the lower electrode and supplied with high-frequency power from a high-frequency power supply.

5. 2. The substrate processing method according to claim 1, wherein in the step of reducing the residue, ammonia gas that has not been converted into plasma is supplied to the substrate as the reducing gas.

6. 2. The substrate processing method of claim 1, wherein the metal layer forms a bottom surface of a recess formed in an insulating layer, and when the metal layer is referred to as a first metal layer, the method further comprises, after performing the step of reducing the residue, forming a second metal layer in the recess on the first metal layer.

7. the first metal layer comprises a metal selected from ruthenium, tungsten, cobalt, or titanium; 7. The substrate processing method of claim 6, wherein the second metal layer comprises a metal selected from ruthenium, tungsten, or molybdenum.

8. the step of reducing the metal oxide film and the step of reducing the residue are performed in a state where the substrate is accommodated in a first processing chamber the interior of which is maintained in a vacuum atmosphere; the step of forming the second metal layer is performed in a state in which the substrate is accommodated in a second processing vessel different from the first processing vessel, the inside of which is set to a vacuum atmosphere; 7. The substrate processing method according to claim 6, further comprising the step of transporting the substrate from the first processing vessel to the second processing vessel via a transport path in a vacuum atmosphere after the step of reducing the residue is performed.

9. 1. An apparatus for processing a substrate having a metal layer, comprising: a processing vessel in which the substrate is placed; a halogen-containing gas supply unit for supplying a halogen-containing gas into the processing vessel; a reducing gas supply unit for supplying a reducing gas into the processing vessel; a control unit, The control unit is configured to output a control signal to execute a step of supplying a halogen-containing gas to a substrate placed in the processing chamber to reduce a metal oxide film formed on the surface of the metal layer, and then a step of supplying a reducing gas to the substrate to reduce residues remaining on the metal layer due to the supply of the halogen-containing gas.

10. the reducing gas includes at least one of hydrogen gas and ammonia gas, a grounded lower electrode provided in the processing chamber and constituting a mounting table on which the substrate is placed; an upper electrode disposed opposite the lower electrode; a high frequency power source that applies high frequency power to the upper electrode to convert the reducing gas into plasma; 10. The apparatus according to claim 9, further comprising: a voltage waveform shaping unit provided between the high frequency power supply and the upper electrode, shaping a voltage waveform of the high frequency power supply so as to suppress a positive voltage of the high frequency power applied to the upper electrode.

11. 1. A substrate processing system, comprising: a first device, which is a device according to claim 9 or 10; When the metal layer is referred to as a first metal layer, a second device including a processing vessel for forming a second metal layer; a vacuum transfer device including a housing to which the processing vessel of the first device and the processing vessel of the second device are connected, and a substrate transfer mechanism disposed in the housing to transfer the substrate without exposing it to the atmosphere; The control unit, The control unit is configured to output a control signal to perform the steps of: after performing the step of reducing the residue, transporting the substrate from the processing chamber of the first apparatus to the processing chamber of the second apparatus using the vacuum transport device; and then, in the second apparatus, forming the second metal layer in the recess on top of the first metal layer from which the residue has been reduced.

12. the first metal layer comprises a metal selected from ruthenium, tungsten, or titanium; The system of claim 11 , wherein the second metal layer comprises a metal selected from ruthenium, tungsten, or molybdenum.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor device, and substrate processing system

    JP2021147691A

  • Plasma processing apparatus and plasma processing method

    JP2022018062A

  • Ruthenium film deposition method and processing equipment

    JP2022152438A

  • Low resistivity contacts and interconnects

    WO2021237032A1

  • Surface treatment method and treatment system

    JP2020059916A

Cited By

  • Gaming machine

    JP2026052290A

  • Gaming machine

    JP2026052291A

  • Gaming machine

    JP2026052292A

  • Gaming machine

    JP2026052293A

  • Gaming machine

    JP2026052295A