Electrolyte and battery

By using electrolytes of isocyanurate compounds and diisolate compounds in lithium-ion batteries, a stable solid electrolyte membrane is formed, which solves the problem of volume changes in silicon-based negative electrode materials and over-discharge safety, and improves lithium ions Energy density and safety of the battery.

CN119009129APending Publication Date: 2024-11-22ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
CN202411130173.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The huge volume changes caused by the deliquefaction of silicon-based negative electrode materials in lithium-ion batteries limit their energy density improvement, and silicon-based batteries are prone to gases due to unstable solid electrolyte membrane at high cutoff voltages, reducing safety.

Method used

Using an electrolyte containing isocyanurate compounds and diisocyanate compounds, these compounds form a stable solid electrolyte membrane on the surface of the negative electrode, inhibiting the production of hydrogen and improving the cycle life, while synergistically working with polynitrile compounds to enhance the synergy of the electrolyte. function to broaden the charge and discharge window.

Benefits of technology

The utilization rate of silicon-based negative electrode materials and the energy density of lithium-ion batteries are improved, over-discharge safety and high-temperature storage performance are improved, the battery impedance is increased, and the rapid charging and discharging capacity is maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009129A_ABST
    Figure CN119009129A_ABST
Patent Text Reader

Abstract

The invention relates to the field of batteries, and provides an electrolyte and a battery, the electrolyte comprises an isocyanurate compound as shown in a formula I and a diisocyanate compound as shown in a formula II; # imgabs0 # imgabs1 # R1 and R2 are each independently H, a halogen, a substituted or unsubstituted C1-C6 linear alkyl group, a substituted or unsubstituted C2-C6 alkenyl group, a substituted or unsubstituted C2-C6 alkynyl group or a substituted or unsubstituted C2-C6 epoxy group, and the substituent is a halogen; r3 is a substituted or unsubstituted C3-C10 linear alkyl group, a substituted or unsubstituted C3-C10 cycloalkyl group, and a substituted or unsubstituted C6-C10 aryl group, and a substituent group is halogen and / or a cyano group. According to the electrolyte, the SEI stability of a silicon-based negative electrode of the lithium ion battery can be improved, the charging and discharging window of the lithium ion battery is widened, and the over-discharging safety of the lithium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an electrolyte and a battery. Background Art

[0002] In order to improve the energy density of lithium-ion batteries, high-capacity silicon-based materials have been widely studied as a new generation of lithium-ion battery negative electrode materials. However, the huge volume change caused by the insertion and extraction of lithium in the silicon negative electrode limits the increase in its usage. In addition, the lithium insertion and extraction platform of silicon-based materials is higher than that of traditional graphite materials. In the application of full batteries, if the discharge cut-off voltage is high, the lithium storage capacity of silicon-based materials will not be fully utilized. However, in current applications, if the cut-off voltage of the battery containing silicon system is lower than 3V, in the late cycle, lithium-ion batteries often produce gas due to the instability of the solid electrolyte membrane (SEI) on the surface of the silicon negative electrode, resulting in battery failure. Similarly, lithium-ion batteries that use silicon as anode materials are prone to gas production under over-discharge conditions, and the gas produced under non-extreme over-discharge conditions (≥1.5V) is mainly hydrogen, which reduces the safety of lithium-ion batteries.

[0003] In order to improve the utilization rate of silicon-based negative electrode materials and improve the safety of over-discharge of silicon-based lithium-ion batteries, it is necessary to further improve the electrolyte technology, optimize the ratio and synergistic effect of each component in the electrolyte, and improve the stability of SEI on the surface of silicon-based negative electrode materials. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and provide an electrolyte and a battery, wherein the electrolyte can improve the SEI stability of the silicon-based negative electrode of the lithium-ion battery, broaden the charge and discharge window of the lithium-ion battery, and improve the over-discharge safety of the lithium-ion battery.

[0005] In order to achieve the above object, the first aspect of the present invention provides an electrolyte, wherein the electrolyte comprises a functional additive, wherein the functional additive comprises a first additive, and the first additive comprises an isocyanurate compound having a chemical formula shown in Formula I and a diisocyanate compound having a chemical formula shown in Formula II;

[0006]

[0007] wherein R1 and R2 are each independently H, halogen, substituted or unsubstituted C1-C6 straight-chain alkyl, substituted or unsubstituted C2-C6 alkenyl, substituted or unsubstituted C2-C6 alkynyl or substituted or unsubstituted C2-C6 epoxy, and if substituted, the substituent is halogen;

[0008] R3 is a substituted or unsubstituted C3-C10 straight-chain alkyl group, a substituted or unsubstituted C3-C10 cycloalkyl group, or a substituted or unsubstituted C6-C10 aromatic group. If substituted, the substituent is halogen and / or cyano.

[0009] A second aspect of the present invention provides a battery, wherein the battery comprises the electrolyte described in the first aspect.

[0010] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0011] The present invention uses a novel electrolyte additive combination to optimize the synergistic effect of electrolyte components, improve the SEI stability of the silicon-based negative electrode of the lithium-ion battery, broaden the charge and discharge window of the lithium-ion battery, increase the utilization rate of the silicon-based negative electrode material and the energy density of the lithium-ion battery, and improve the over-discharge safety of the lithium-ion battery.

[0012] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. DETAILED DESCRIPTION

[0013] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0014] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0015] A first aspect of the present invention provides an electrolyte, the electrolyte comprising a functional additive, the functional additive comprising a first additive, the first additive comprising an isocyanurate compound having a chemical formula shown in Formula I and a diisocyanate compound having a chemical formula shown in Formula II;

[0016]

[0017] wherein R1 and R2 are each independently H, halogen, substituted or unsubstituted C1-C6 straight-chain alkyl, substituted or unsubstituted C2-C6 alkenyl, substituted or unsubstituted C2-C6 alkynyl or substituted or unsubstituted C2-C6 epoxy, and if substituted, the substituent is halogen;

[0018] R3 is a substituted or unsubstituted C3-C10 straight-chain alkyl group, a substituted or unsubstituted C3-C10 cycloalkyl group, or a substituted or unsubstituted C6-C10 aromatic group. If substituted, the substituent is halogen and / or cyano.

[0019] The allyl group on the isocyanurate compound can cause it to be reduced and polymerized at the negative electrode to form a relatively stable SEI, which is beneficial to inhibit the excessive volume expansion of the silicon-based negative electrode material and improve the cycle life of the silicon-based negative electrode material. In addition, the isocyanurate group can capture active hydrogen. In addition to inhibiting the damage of the acid to the SEI during the cycle, it can also inhibit the generation of hydrogen during the over-discharge process. Therefore, adding the isocyanurate compound can improve the stability of the SEI on the surface of the silicon-based negative electrode material, improve the cycle life of the silicon-based negative electrode material and inhibit the over-discharge gas generation of the lithium-ion battery. The isocyanate group in the diisocyanate compound can react with active hydrogen. On the one hand, it can react with the silanol group on the surface of the silicon-based material to form SEI on the surface of the silicon-based material. The residual isocyanate group can also capture active hydrogen, so it can also improve the stability of the SEI and inhibit the destruction of the SEI to produce hydrogen in the case of over-discharge; on the other hand, the isocyanate group can react with the acid and water in the electrolyte, inhibiting the autocatalytic reaction after the decomposition of LiPF6, which is beneficial to improve the storage capacity of the lithium-ion battery at high temperature. During the experiment, it was unexpectedly discovered that when the two are used at the same time, it is possible to achieve the goal of broadening the charge and discharge range of lithium-ion batteries and inhibiting over-discharge and gas production of lithium-ion batteries with a smaller addition amount, while not excessively increasing the impedance of the lithium-ion battery and deteriorating the battery's kinetic performance.

[0020] In some embodiments, R1 and R2 are each independently H, halogen, substituted or unsubstituted C1-C4 straight chain alkyl (C1-C4 straight chain alkyl is for example methyl, ethyl, n-propyl, n-butyl), substituted or unsubstituted C2-C4 alkenyl (C2-C4 alkenyl is for example ethenyl, propenyl, butenyl), substituted or unsubstituted C2-C4 alkynyl (C2-C4 alkynyl is for example ethynyl, propynyl, butynyl) or substituted or unsubstituted C2-C4 epoxy (C2-C4 epoxy is for example epoxy, methyl epoxy, ethyl epoxy).

[0021] The halogen may be at least one of F, Cl, Br, and I. In some embodiments, the halogen is F.

[0022] Isocyanurate is a polyisocyanate containing isocyanurate in the molecular structure, and has a carbon-nitrogen six-membered ring structure generated by the trimerization reaction of isocyanate. In some embodiments, the isocyanurate compound includes at least one of triallyl isocyanurate (TAIC, Formula I-1), diallyl isocyanurate (Formula I-2), 1-oxiranylmethyl-3,5-di-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (Formula I-3), diallyl n-propyl isocyanurate (Formula I-4), diallyl methyl isocyanurate (Formula I-5), and allyl dimethyl isocyanurate (Formula I-6).

[0023]

[0024] In some embodiments, the amount of the isocyanurate compound added is 0.1-2wt% of the total mass of the electrolyte, such as 0.1wt%, 0.2wt%, 0.4wt%, 0.6wt%, 0.8wt%, 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%. A small amount of addition will improve the battery to a small extent, while excessive addition will increase the impedance of the battery and easily lead to lithium precipitation.

[0025] In some embodiments, R3 is a substituted or unsubstituted C3-C8 straight chain alkyl group (for example, a C3-C8 straight chain alkyl group is n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl), a substituted or unsubstituted C3-C8 cycloalkyl group (for example, a C3-C8 cycloalkyl group is cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane), or a substituted or unsubstituted C6-C8 aromatic group (for example, a C6-C8 aromatic group is phenyl, tolyl, ethylphenyl, xylyl).

[0026] The diisocyanate compound refers to a compound containing two isocyanate groups. In some embodiments, the diisocyanate compound comprises at least one of the compounds shown in Formula II-1 to Formula II-6;

[0027]

[0028] In some embodiments, the amount of the diisocyanate compound added is 0.1-2wt% of the total mass of the electrolyte, such as 0.1wt%, 0.2wt%, 0.4wt%, 0.6wt%, 0.8wt%, 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%. The diisocyanate compound can improve the cycle stability of the silicon negative electrode, inhibit the over-discharge gas production of the lithium-ion battery, and improve the high-temperature storage performance of the lithium-ion battery. The improvement effect of a small amount of addition is not obvious, and too much addition will significantly increase the impedance of the battery, which is easy to deteriorate the rate charge and discharge capacity of the lithium-ion battery, resulting in lithium deposition in the battery.

[0029] In some embodiments, the amount of the isocyanurate compound added is 0.1-2wt% of the total mass of the electrolyte, and the amount of the diisocyanate compound added is 0.1-2wt% of the total mass of the electrolyte. Since the volume change of silicon-based materials during the charge and discharge process is large, the SEI formed on its surface is usually thicker, and the risk of over-discharge gas production is greater. In addition, the conductivity of silicon-based materials is poor. Controlling the content of the two substances in the first additive in the electrolyte can make the formed SEI more stable and have a better ability to bind hydrogen, while not excessively increasing the electrochemical polarization, thereby stabilizing the silicon negative electrode and improving the over-discharge gas production.

[0030] In some embodiments, the functional additive further comprises a second additive, the second additive being a polynitrile compound, the number of cyano groups in the polynitrile compound being 3 or more, for example, 3, 4, 5, 6 or more. The polynitrile compound can be complexed with the high-valent metal ions (such as Co ions) in the positive electrode, inhibit the dissolution of cobalt ions, and improve the stability of the positive electrode material. In addition, the cobalt ions are dissolved and deposited on the negative electrode, which easily catalyzes the decomposition of SEI and reduces the stability of SEI. Therefore, when the electrolyte further comprises a polynitrile compound, the first additive improves the over-discharge stability of SEI from the chemical composition, and the second additive inhibits the catalytic decomposition of metal ions on SEI on the negative electrode. The synergistic effect of the two can not only improve the stability of the positive electrode material, but also reduce the catalytic effect of metal ions on the negative electrode SEI, so that the lithium ion battery has a wider charge and discharge window and better over-discharge resistance. On the other hand, compared with dinitrile compounds, polynitrile compounds have a higher nitrile content per unit molecule and a relatively large molecular weight, are not easy to react with the negative electrode and can better inhibit the gas production of the electrolyte, which is beneficial to improve the high temperature storage performance of the battery.

[0031] In some embodiments, the polynitrile compound comprises at least one of 1,3,6-hexanetrinitrile, glyceroltrinitrile, 2,4,6-tricyano-1,3,5-triazine, tetrafluorotetracyanoquinodimethane, 1,2,3-trinitrilepropane, pentatricarbonitrile, 1,3,5-cyclohexanetricarbonitrile, 1,2,4,5-benzenetetracarbonitrile, 1,1,3,3-propanetetracarbonitrile, 7,7,8,8-tetracyanoquinolinemethane, tetrafluorotetracyanoquinodimethane, and 1,2,3-tris(2-cyanoethoxy)propane.

[0032] In some embodiments, the amount of the second additive added is 0.5wt%-4wt% of the total mass of the electrolyte, such as 0.5wt%, 0.8wt%, 1.2wt%, 1.6wt%, 2wt%, 2.4wt%, 2.8wt%, 3.2wt%, 3.6wt%, 4wt%. The second additive can improve the stability of the positive electrode material and improve the battery cycle performance; inhibit the dissolution of metal ions and improve the battery's ability to withstand over-discharge. Too low an amount of addition will result in insufficient protection of the positive electrode and will not significantly inhibit over-discharge gas production; excessive addition will increase the viscosity and impedance of the electrolyte, which is not conducive to the rapid charge and discharge capabilities of the lithium-ion battery.

[0033] In some embodiments, the electrolyte further comprises a non-aqueous solvent, a lithium salt and other functional additives.

[0034] In some embodiments, the non-aqueous solvent comprises carbonate and / or carboxylate.

[0035] In some embodiments, the solvent includes but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propionate (MP), methyl butyrate (MB), ethyl butyrate (EB), ethyl acetate (EA), propyl acetate (PA), etc.

[0036] In some embodiments, the lithium salt comprises at least one of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium hexafluoroantimonate (LiSbF6), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethylsulfonyl imide (LiTFSI), lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium, or lithium bis(trifluoromethylsulfonyl)imide, lithium difluorooxalatoborate (LiDFOB), lithium difluorobisoxalatophosphate, lithium tetrafluoroborate (LiBF4), lithium bis(difluorophosphoryloxy)difluoroborate, and lithium tetrakis(difluorophosphoryloxy)borate.

[0037] The other functional additives may be selected from one or more commonly used additives to further improve the cycle performance or high and low temperature performance of the battery, such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), propene sultone (PST), methylene disulfonate (MMDS), 1,3-propane sultone (PS), vinyl sulfate (DTD), divinyl sulfate (BiDTD), tetravinylsilane (TVS), tris(trimethylsilyl)borate (TMSB), hexamethyldisilazane (HMDS), fluorobenzene (FB), triphenyl phosphite (TPPi), pentafluoroethoxycyclotriphosphazene (PFPN), etc. At least one of the above.

[0038] In some embodiments, the non-aqueous solvent accounts for 50wt%-80wt% of the total mass of the electrolyte, for example, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, or 80wt%.

[0039] In some embodiments, the lithium salt accounts for 12wt%-25wt% of the total mass of the electrolyte, for example, it can be 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, or 25wt%.

[0040] In some embodiments, the added amount of the functional additive is 8wt%-25wt% of the total mass of the electrolyte, for example, it can be 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%.

[0041] A second aspect of the present invention provides a battery, wherein the battery comprises the electrolyte described in the first aspect.

[0042] When silicon-based materials are used as negative electrode active materials, volume expansion will occur during the cycle process, which can easily lead to continuous rupture and regeneration of the SEI film. Therefore, silicon-based batteries often add functional additives (such as fluoroethylene carbonate FEC) that can form an organic-inorganic composite SEI film rich in LiF on the surface of the silicon negative electrode to improve the cycle life of the silicon negative electrode. However, it is easy to decompose and produce HF during use, which leads to the thickening of the SEI and the accumulation of active hydrogen during the battery cycle. During the research process, it was found that isocyanurate compounds can capture the active hydrogen obtained by the decomposition of functional additives, inhibit the SEI film from being destroyed by acid, and improve the over-discharge resistance of the SEI. However, due to the unstable double bonds on the isocyanurate compounds, it will cause almost all of the isocyanurate compounds to react to form SEI, and it is impossible to remove the active hydrogen in the electrolyte and the newly formed SEI after multiple cycles. When used with diisocyanate compounds, it can remove the active hydrogen generated during the cycle. The amount of isocyanurate compounds and diisocyanate compounds and silicon additives must be controlled within an appropriate range to achieve a better improvement effect. When the relative content of isocyanurate compounds and diisocyanate compounds is too high, the impedance of the battery will increase significantly and the rapid charge and discharge capability of the battery will be reduced; when the amount of silicon added is large and the amount of the first and diisocyanate compounds added is small, due to insufficient protection of the silicon material and the SEI on the surface of the silicon material, the battery's cycle and over-discharge resistance will deteriorate.

[0043] In some embodiments, the battery further includes a negative electrode sheet, a positive electrode sheet and a separator, the negative electrode sheet includes a negative electrode collector and a negative electrode active material layer located on one side or both sides of the negative electrode collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-based material; the battery satisfies the relationship: 2≤S / (A+B+C)≤20, for example, it can be 2, 4, 6, 8, 10, 12, 14, 16, 18, 20; wherein the amount of the isocyanurate compound added to the electrolyte is Awt%, the amount of the diisocyanate compound added to the electrolyte is Bwt%, the amount of the second additive added to the electrolyte is Cwt%, and the amount of the silicon-based material added to the negative electrode active material is Swt%.

[0044] In some embodiments, 4≤S≤30, such as 4, 6, 8, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30. Silicon-based negative electrode materials have a high lithium storage capacity. Adding an appropriate amount of silicon-based materials can effectively improve the energy density of lithium-ion batteries. However, due to the large volume expansion caused by the insertion and extraction of lithium in silicon-based materials, SEI is easily broken and regenerated continuously. Therefore, excessive addition of silicon-based materials will cause the electrolyte film-forming agent to be consumed too quickly and the volume expansion of the battery is too large. When the content of silicon-based materials is within this range, a higher battery energy density can be obtained and the volume expansion can be alleviated.

[0045] In some embodiments, the silicon-based material comprises silicon (such as nano-silicon, amorphous silicon, porous silicon, silicon nanowires, etc.), silicon-oxygen materials (SiO x , 0<x<2) and at least one of silicon-carbon materials (such as carbon-coated silicon-carbon materials, materials in which silicon is deposited on a carbon skeleton, etc.).

[0046] In some embodiments, the negative electrode active material further comprises a carbon-based material.

[0047] In some embodiments, the carbon material comprises at least one of natural graphite, artificial graphite, soft carbon, hard carbon, and graphene.

[0048] In some embodiments, the content of impurity metal in the negative electrode sheet is less than 1500ppm by weight, such as 1ppm, 10ppm, 50ppm, 100ppm, 300ppm, 500ppm, 700ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1300ppm, 1400ppm, 1500ppm or less, and the impurity metal is a metal element other than Li, Na, and Cu. Generally speaking, in addition to the Li element, the negative electrode sheet may also contain Na elements introduced by sodium-containing raw materials (such as sodium carboxymethyl cellulose) and copper introduced due to corrosion of the negative electrode current collector copper foil, that is, the negative electrode sheet will also contain a certain amount of Na elements and Cu elements. However, due to the preparation or purification process of battery materials and the battery manufacturing process, other metal element impurities such as K, Mg, Fe, Ni, etc. may remain or be mixed. In addition, the metal elements in the positive electrode material may also be freed to the negative electrode for reduction due to structural instability during the charge and discharge process. When there are too many impurities, the negative effects on the battery outweigh the positive effects. For example, during over-discharge and high-temperature storage of the battery, metal impurities may catalyze the decomposition of SEI, resulting in increased gas production; excessive K will cause graphite exfoliation and deteriorate the cycle performance. When the content of metal impurities is controlled at the above level, some metal impurities may even improve certain battery properties. For example, when the negative electrode contains a trace amount of K element, since the monovalent potassium ions can be co-embedded in the interlayer of the graphite negative electrode like lithium ions, the local interlayer spacing of the graphite is increased, which is conducive to the rapid insertion and extraction of lithium ions; if the negative electrode contains a trace amount of divalent or multivalent metal impurities, these metal impurities cannot interact with the negative electrode material, but can partially replace the lithium ions in the SEI to produce divalent or multivalent metal alkoxy metal compounds and alkyl carbonate metal compounds; since these divalent or multivalent metals can connect two or more alkoxy or carbonate groups, the interaction between the SEI components is increased, and the stress-strain stability of the SEI is increased, so the cycle performance of the lithium-ion battery can be improved to a certain extent.

[0049] The surface density mainly reflects the loading amount of the negative electrode paste. The greater the loading amount, the higher the capacity of the negative electrode, but too much loading amount is prone to foil peeling on the one hand, and on the other hand it is easy to cause excessive polarization, thus causing lithium precipitation. In the case where silicon-based materials are included in the negative electrode sheet, the specific capacity of the material is increased, so the surface density of the negative electrode can be reduced. When the surface density is too low, a large amount of silicon needs to be incorporated, and the coating thickness is too low. Due to the high silicon content, the side reactions of the battery increase, the polarization increases, and the SEI by-products also increase, thereby increasing the risk of over-discharge and gas production. In addition, due to the small coating thickness, the carbon content around the silicon particles is insufficient, and the buffer space for the silicon particles to embed and extract lithium is insufficient, so the cycle performance of the battery will also deteriorate. In some embodiments, the surface density of the negative electrode sheet is 4-7mg / cm 2 , for example 4 mg / cm 2 , 4.5mg / cm 2 , 5mg / cm 2 , 5.5mg / cm 2 , 6mg / cm 2 、6.5mg / cm 2 , 7mg / cm 2 When the negative electrode surface density is controlled within this range, the cycle performance of the battery can be further improved and the volume expansion of the battery can be alleviated.

[0050] In some embodiments, the negative electrode active material layer further includes a negative electrode conductor and a negative electrode binder.

[0051] In some embodiments, the negative electrode active material layer comprises 80-99.8 wt % of a negative electrode active material, 0.1-10 wt % of a negative electrode conductor, and 0.1-10 wt % of a negative electrode binder.

[0052] In some embodiments, the negative electrode active material layer comprises 90-99 wt % of a negative electrode active material, 0.5-5 wt % of a negative electrode conductor, and 0.5-5 wt % of a negative electrode binder.

[0053] In one embodiment, the negative electrode conductive agent includes at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder, and carbon fiber.

[0054] In one embodiment, the negative electrode binder includes at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, polyethylene oxide, polyacrylic acid, sodium polyacrylate, lithium polyacrylate, sodium alginate, and polyvinylidene fluoride.

[0055] The negative electrode current collector may be a negative electrode current collector commonly used in the art, such as copper foil or a composite current collector.

[0056] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material.

[0057] In some embodiments, the chemical formula of the positive electrode active material includes LiCo 1-d-e M d N e O2, wherein 0≤d≤0.5, 0≤e≤0.5, M includes at least one of Mn and Al, and N includes at least one of Mg, Zr, Ni, Y, Sr, W, Sc, B, W, Si, Ti, Zr, Sr, Sn, Tb, Nb, Sb, Se, Ce and Te.

[0058] In some embodiments, the positive electrode active material layer further includes a positive electrode conductor and a positive electrode binder.

[0059] In some embodiments, the mass percentage of each component in the positive electrode active material layer is: 80-99.8wt% of positive electrode active material, 0.1-10wt% of positive electrode conductive agent, and 0.1-10wt% of positive electrode binder.

[0060] In some embodiments, the mass percentage of each component in the positive electrode active material layer is: 90-99wt% of positive electrode active material, 0.5-5wt% of positive electrode conductive agent, and 0.5-5wt% of positive electrode binder.

[0061] In some embodiments, the positive electrode conductive agent includes at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, and metal powder.

[0062] In some embodiments, the positive electrode binder includes at least one of polyvinylidene fluoride, polyethylene-tetrafluoroethylene copolymer, sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, and polyethylene oxide.

[0063] In some embodiments, the positive electrode current collector may be a positive electrode current collector conventionally used in the art, such as aluminum foil or a composite current collector.

[0064] The separator can be any conventional type in the art. In some embodiments, the base film is made of polyolefin, more preferably polypropylene and / or polyethylene. The separator can be commercially available.

[0065] If not otherwise specified, other options for the lithium-ion battery are conventional options in the art. The battery can be assembled in a conventional manner in the art.

[0066] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0067] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0068] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0069] Example 1

[0070] (1) Preparation of negative electrode sheet:

[0071] The negative electrode active material, styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), conductive carbon black (SP) and carbon nanotubes (CNTs) are mixed uniformly in a mass ratio of 96:1.5:0.5:1:1, and then appropriate amount of deionized water is added step by step to obtain negative electrode slurry under the action of a vacuum mixer; the negative electrode active slurry is evenly coated on the two surfaces of the copper foil by a coating machine; after drying, rolling, slitting and die cutting, the negative electrode sheet is obtained. The negative electrode active material is composed of 90wt% artificial graphite + 10wt% silicon oxide, that is, the content S wt% of silicon-based materials in the negative electrode active material is 10wt%, S=10. The surface density of the negative electrode sheet is 5.5mg / cm 2 .

[0072] (2) Preparation of positive electrode sheet:

[0073] Commercial lithium cobalt oxide (LiCoO2) material, polyvinylidene fluoride (PVDF), SP and carbon nanotubes (CNTs) were dry mixed in a mass ratio of 96:2:1.5:0.5. Then, under the action of a vacuum mixer, an appropriate amount of N-methylpyrrolidone (NMP) was gradually added to mix into a uniform slurry; then, a coating machine was used to evenly coat the positive electrode active slurry and ceramic glue slurry on both surfaces of the aluminum foil; then, the required positive electrode sheet was obtained after drying, rolling, slitting and die cutting.

[0074] (3) Preparation of electrolyte

[0075] In a glove box filled with argon (H2O<0.1ppm, O2<0.1ppm), ethylene carbonate (EC), propylene carbonate (PC), propyl propionate (PP), and ethyl butyrate (EB) are mixed in a mass ratio of 15:15:50:20. Then, 12wt% of LiPF6 and 5wt% of LiTFSI based on the total mass of the electrolyte are quickly added thereto, and after dissolution, 10wt% of FEC, Cwt% of polynitrile compounds, Bwt% of diisocyanate compounds, and Awt% of isocyanurate compounds based on the total mass of the electrolyte are added. After stirring evenly, the desired electrolyte is obtained after passing the tests of moisture, free acid, color, etc. The isocyanurate compound is TAIC shown in formula I-1, the diisocyanate compound is hexamethylene diisocyanate HDI shown in formula II-1, the polynitrile compound is HTCN, and the contents of the isocyanurate compound, the diisocyanate compound and the polynitrile compound in the electrolyte are A wt%, B wt% and Cwt%, respectively, as shown in Table 1.

[0076] (4) Preparation of lithium-ion batteries

[0077] The negative electrode sheet prepared in the above steps, the commercial separator, and the positive electrode sheet prepared in the above steps are stacked in a certain way so that the separator completely separates the positive and negative electrodes, and the negative electrode paste completely covers the positive electrode paste, and then a winding core with a certain thickness and width is made by winding. Subsequently, an aluminum-plastic film is used for packaging and the electrolyte prepared in the above steps is injected. After vacuum packaging, aging, formation, shaping, sorting and other processes, a soft-pack lithium-ion battery is obtained. It has been determined that the content of impurity metals in the negative electrode sheet is 150ppm.

[0078] Comparative Example 1

[0079] The operation was carried out according to the method described in Example 1, except that no isocyanurate compound and / or diisocyanate compound was added to the electrolyte, as shown in Table 1.

[0080] Example 2 Group

[0081] The method described in Example 1 was followed, except that the type and amount of the isocyanurate compound added were different, as shown in Table 1.

[0082] Example 3 Group

[0083] The method described in Example 1 was followed, except that the type and amount of diisocyanate compound added were different, as shown in Table 1.

[0084] Example 4 Group

[0085] The method described in Example 1 was followed, except that the type and amount of the second additive were different, as shown in Table 1.

[0086] Example 5 Group

[0087] The operation was carried out according to the method described in Example 1, except that the content of the silicon-based material in the negative electrode active material was different, that is, S was different, as shown in Table 1.

[0088] Example 6 Group

[0089] The operation is carried out according to the method described in Example 1, except that the contents of the isocyanurate compound, the diisocyanate compound and the second additive in the electrolyte and the content of the silicon-based material in the negative electrode active material are different, that is, A, B, C and S are different, as shown in Table 1.

[0090] Table 1

[0091]

[0092] Note: "*" in Table 1 indicates the same as Example 1.

[0093] Example 7 Group

[0094] The method described in Example 1 is followed, except that impurity metal elements are added to the negative electrode slurry, wherein:

[0095] Example 7-1: KCl was added to the negative electrode slurry, and the content of K element in the negative electrode sheet was about 500 ppm by weight.

[0096] Example 7-2: KCl was added to the negative electrode slurry, and the content of K element in the negative electrode sheet was about 1700 ppm by weight.

[0097] Test Case

[0098] The performance of the batteries prepared in the examples and comparative examples was tested according to the following method. The test results are shown in Table 2.

[0099] (1) Lithium-ion battery cycle performance test: The voltage window of the lithium-ion test is set to 2.8-4.5V. The battery is placed in a constant temperature box, charged to the upper limit voltage at a rate of 1C, then charged to full power at a constant voltage, and then discharged to 2.8V at a rate of 0.7C. This is one cycle. After 500T of cycling, the capacity retention rate of the battery is calculated and the surface state of the battery is observed.

[0100] Among them, if the appearance is flat but the thickness is different from the initial state, it is marked as normal appearance; the battery side is thicker than the middle and is marked as ridged; the top and bottom of the battery are convex and thicker, which is marked as bulging; the aluminum-plastic film can be seen bulging on the appearance of the battery, which can be pressed down and rebound, but the surrounding aluminum-plastic film is still close to the battery cell and the thickness expansion is less than or equal to 10%, which is marked as slight bulging; the aluminum-plastic film of the battery is bulging and most of it has been separated from the battery body and the thickness expansion is greater than 10% and less than or equal to 20%, which is marked as bulging; the aluminum-plastic film is separated from the battery body and the thickness expansion is greater than or equal to 20%, which is marked as severe bulging.

[0101] (2) Lithium-ion battery overdischarge test: A lithium-ion battery with a cycle of 100T was discharged at a rate of 0.7C to 3V, and then gradually discharged at a rate of 0.002C to 1.5V. The surface state of the battery was observed and the surface state of the battery when it was overdischarged to 1.5V after a cycle of 100T was recorded.

[0102] (3) High temperature storage test for lithium-ion batteries: Charge the lithium-ion batteries to full capacity and place them in a constant temperature box at 60°C. Measure the thickness of the batteries every 7 days until the thickness of the batteries expands by more than 20% of the initial thickness. Record the number of days required for the thickness of the batteries to expand by more than 20% of the initial thickness.

[0103] Table 2

[0104]

[0105]

[0106] It should be noted that, in this article, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the method and device in the embodiment of the present invention is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An electrolyte, characterized in that: The electrolyte comprises a functional additive, wherein the functional additive comprises a first additive, and the first additive comprises an isocyanurate compound having a chemical formula shown in Formula I and a diisocyanate compound having a chemical formula shown in Formula II; wherein R1 and R2 are each independently H, halogen, substituted or unsubstituted C1-C6 straight-chain alkyl, substituted or unsubstituted C2-C6 alkenyl, substituted or unsubstituted C2-C6 alkynyl or substituted or unsubstituted C2-C6 epoxy, and if substituted, the substituent is halogen; R3 is a substituted or unsubstituted C3-C10 straight-chain alkyl group, a substituted or unsubstituted C3-C10 cycloalkyl group, or a substituted or unsubstituted C6-C10 aromatic group. If substituted, the substituent is halogen and / or cyano.

2. The electrolyte according to claim 1, characterized in that R1 and R2 are each independently H, halogen, substituted or unsubstituted C1-C4 straight-chain alkyl, substituted or unsubstituted C2-C4 alkenyl, substituted or unsubstituted C2-C4 alkynyl or substituted or unsubstituted C2-C4 epoxy; and / or R3 is a substituted or unsubstituted C3-C8 straight chain alkyl group, a substituted or unsubstituted C3-C8 cycloalkyl group, or a substituted or unsubstituted C6-C8 aromatic group; and / or Halogen is F; Preferably, the isocyanurate compound comprises at least one of triallyl isocyanurate, diallyl isocyanurate, 1-oxiranylmethyl-3,5-di-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, diallyl-n-propyl isocyanurate, diallyl methyl isocyanurate, and allyl dimethyl isocyanurate; Preferably, the diisocyanate compound comprises at least one of the compounds represented by Formula II-1 to Formula II-6; 3. The electrolyte according to claim 1 or 2, characterized in that The amount of the isocyanurate compound added is 0.1-2% of the total mass of the electrolyte; and / or The added amount of the diisocyanate compound is 0.1-2% of the total mass of the electrolyte.

4. The electrolyte according to any one of claims 1 to 3, characterized in that The functional additive further comprises a second additive, and the second additive is a polynitrile compound; Preferably, the polynitrile compound comprises at least one of 1,3,6-hexanetrinitrile (HTCN), glyceroltrinitrile, 2,4,6-tricyano-1,3,5-triazine, tetrafluorotetracyanoquinodimethane, 1,2,3-trinitrile propane, pentatricarbonitrile, 1,3,5-cyclohexanetricarbonitrile, 1,2,4,5-benzenetetracarbonitrile, 1,1,3,3-propanetetracarbonitrile, 7,7,8,8-tetracyanoquinolinemethane, tetrafluorotetracyanoquinodimethane, and 1,2,3-tris(2-cyanoethoxy)propane; Preferably, the amount of the second additive added is 0.5wt%-4wt% of the total mass of the electrolyte.

5. The electrolyte according to any one of claims 1 to 4, characterized in that The electrolyte also contains a non-aqueous solvent, a lithium salt and other functional additives; Preferably, the non-aqueous solvent comprises carbonate and / or carboxylate; Preferably, the lithium salt comprises at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium or lithium bis(trifluoromethylsulfonyl)imide, lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(difluorophosphoryloxy)difluoroborate, and lithium tetrakis(difluorophosphoryloxy)borate; Preferably, the other functional additives include at least one of vinylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, trifluoromethylethylene carbonate, propylene sultone, methylene disulfonate, 1,3-propane sultone, vinyl sulfate, vinyl disulfate, tetravinylsilane, tris(trimethylsilyl)borate, hexamethyldisilazane, fluorobenzene, triphenyl phosphite, and pentafluoroethoxycyclotriphosphazene; Preferably, the non-aqueous solvent accounts for 50wt%-80wt% of the total mass of the electrolyte, the lithium salt accounts for 12wt%-25wt% of the total mass of the electrolyte, and the functional additive accounts for 8wt%-25wt% of the total mass of the electrolyte.

6. A battery, characterized in that: The battery comprises the electrolyte according to any one of claims 1 to 5; Preferably, the battery further comprises a negative electrode sheet, a positive electrode sheet and a separator, the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer located on one side or both sides of the negative electrode current collector, the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises a silicon-based material; the battery satisfies the relationship: 2≤S / (A+B+C)≤20; Among them, the amount of the isocyanurate compound added to the electrolyte is A wt%, the amount of the diisocyanate compound added to the electrolyte is B wt%, the amount of the second additive added to the electrolyte is Cwt%, and the amount of the silicon-based material added to the negative electrode active material is S wt%.

7. The battery according to claim 6, characterized in that 4≤S≤30。 8. The battery according to claim 6 or 7, characterized in that: The silicon-based material comprises at least one of silicon, silicon-oxygen material and silicon-carbon material; and / or The negative electrode active material further comprises a carbon-based material; preferably, the carbon material comprises at least one of natural graphite, artificial graphite, soft carbon, hard carbon and graphene.

9. The battery according to any one of claims 6 to 8, characterized in that: The content of impurity metal in the negative electrode sheet is less than 1500 ppm by weight, and the impurity metal is a metal element other than Li, Na, and Cu; and / or The surface density of the negative electrode is 4-7 mg / cm 2 .

10. The battery according to any one of claims 6 to 9, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material; Preferably, the chemical formula of the positive electrode active material includes LiCo 1-d-e M d N e O2, wherein 0≤d≤0.5, 0≤e≤0.5, M includes at least one of Mn and Al, and N includes at least one of Mg, Zr, Ni, Y, Sr, W, Sc, B, W, Si, Ti, Zr, Sr, Sn, Tb, Nb, Sb, Se, Ce and Te.

Citation Information

Patent Citations

  • Nonaqueous electrolyte solution and nonaqueous electrolyte battery using same

    CN104995784A

  • Lithium ion battery electrolyte and lithium ion battery

    CN116632345A

  • Non-aqueous electrolyte and non-aqueous electrolyte secondary battery

    CN117059895A

  • Lithium ion battery

    CN118315674A

  • Nonaqueous type electrolyte and nonaqueous electrolyte secondary battery using the same

    JP2016143536A

Cited By

  • Lithium ion battery electrolyte and application thereof

    CN119581667A

  • Electrolyte solution, electrochemical device, and electronic apparatus

    CN119674225A

  • Secondary battery

    CN119674235A