Lithium-rich lithium ferrite material as well as preparation method and application thereof

By introducing specific doping elements into lithium-rich lithium ferrate materials, the binding force between the core and the cladding layer and binding oxygen molecules is solved, and the battery capacity and high rate performance are improved .

CN118970048AActive Publication Date: 2024-11-15HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202411043344.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing lithium-rich lithium ferrate positive electrode lithium supplement agents have poor stability during the first charging process, difficult to exert lithium supplement capacity, and large gas production, resulting in reduced battery capacity and swelling.

Method used

The core has oxygen vacancy and the cladding has nucleation sites by introducing a first doping element (such as Ti, W, Ni, Ce) and a second doping element (such as B, N, S, O, P). Enhance the bond strength of the core to the cladding and bind oxygen molecules or oxygen radicals to the inside of the material through oxygen vacancies and nucleation sites, reducing gas production.

Benefits of technology

The stability and battery capacity of lithium-rich lithium ferrate materials are improved, and the gas production is reduced, ensuring that high lithium supplement capacity can still be exerted during high-rate charging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972944240000111
    Figure BDA0004972944240000111
Patent Text Reader

Abstract

The invention provides a lithium-rich lithium ferrite material as well as a preparation method and application thereof, and belongs to the technical field of lithium ion batteries. The lithium-rich lithium ferrite material comprises an inner core and a coating layer coating the surface of the inner core, the material of the inner core is lithium-rich lithium ferrite doped with a first doping element, and the material of the coating layer is a carbon material doped with a second doping element; wherein the first doping element comprises at least one of Ti, W, Ni, Ce and Co, and the second doping element comprises at least one of B, N, S, O and P. When the lithium-rich lithium ferrite material is applied to a battery as a lithium supplement agent, the capacity of the battery can be further improved, and the gas production rate can be further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a lithium-rich lithium ferrite material and a preparation method and application thereof. Background Art

[0002] In recent years, the increasing demand for longer-range portable devices and electric vehicles has placed higher demands on the capacity of lithium-ion batteries. During the initial charging process of a lithium-ion battery, a solid electrolyte membrane (SEI) forms on the negative electrode surface, permanently consuming lithium from the positive electrode, resulting in irreversible capacity loss. This results in a low coulombic efficiency during the first cycle and reduces the battery's capacity. Therefore, how to replenish the lithium ions consumed during SEI formation to increase battery capacity is a current research hotspot.

[0003] Currently, pre-lithiation technologies exist that add lithium to batteries to replenish lithium ions, primarily through negative and positive electrode replenishment. Lithium-rich ferrite cathode replenishers have garnered widespread attention due to their high potential and good compatibility with existing battery materials. However, their poor lithium ion and electronic conductivity, as well as their poor stability, hinder their ability to achieve full capacity and affect the processing performance of the slurry.

[0004] At present, most of the methods are to coat the surface of the positive electrode lithium supplement agent with a carbon layer to improve its lithium ion and electronic conductivity and stability. On the one hand, the carbon layer is used to isolate the external environment, and on the other hand, the carbon layer is used to form a conductive network to improve the conductivity of the material itself. However, the carbon layer has poor compatibility with lithium-rich ferrite, and the coating is often uneven and not firm, which will affect its stability in the slurry and the capacity of the battery. In addition, the lithium-rich ferrite positive electrode lithium supplement agent will produce oxygen molecules or oxygen free radicals during the first charging process. The oxygen molecules or oxygen free radicals diffuse into the electrolyte and react with some components in the electrolyte to produce a large amount of carbon dioxide and hydrogen and other gases. The gas production increases, causing the battery to swell and other phenomena, which still hinder the application of lithium-rich ferrite as a positive electrode lithium supplement agent. Therefore, how to reduce the gas production while ensuring its stability and lithium supplement capacity is a technical problem that needs to be solved urgently in this field. Summary of the Invention

[0005] The main purpose of the present invention is to provide a lithium-rich lithium ferrite material and its preparation method and application, so as to solve the problems in the prior art of poor stability, difficulty in exerting lithium replenishment capacity and large gas production when lithium-rich lithium ferrite is used as a positive electrode lithium replenisher.

[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a lithium-rich lithium ferrite material, comprising a core and a coating layer coated on the surface of the core, the material of the core is lithium-rich lithium ferrite doped with a first doping element, and the material of the coating layer is a carbon material doped with a second doping element; wherein the first doping element includes at least one of Ti, W, Ni, Ce, and Co, and the second doping element includes at least one of B, N, S, O, and P.

[0007] By introducing the first doping element and the second doping element, the core has oxygen vacancies and the coating layer has nucleation sites. On the one hand, an adsorption effect is formed between the oxygen vacancies in the core and the nucleation sites of the coating layer, thereby enhancing the bonding strength between the core and the coating layer, making the coating layer more uniform and firm, thereby improving the coating effect. In this way, the poor stability of the lithium-rich lithium ferrite material and the difficulty in maximizing the lithium replenishment capacity caused by the unevenness and looseness of the coating layer are avoided, thereby helping to further improve the stability of the lithium-rich lithium ferrite material and the capacity of the battery; on the other hand, due to the presence of oxygen vacancies in the core and the nucleation sites in the coating layer, the oxygen molecules or oxygen free radicals generated by the battery during the first charging process can be bound inside the material through typing or adsorption, reducing escape and avoiding the problem of further reaction of oxygen molecules or oxygen free radicals with the electrolyte to produce a large amount of gas, thereby reducing the gas production of the battery and reducing the polarization problem of the lithium-rich lithium ferrite material, so that it can still exert a high lithium replenishment capacity at a high rate, thereby making the battery have a high capacity when charged at a high rate.

[0008] Further, the first doping element includes at least one of Ti, W, Ni, and Ce; and / or the second doping element includes at least one of N, S, and O.

[0009] By optimizing the coordination between the elements, the stability, capacity and gas production can be further improved.

[0010] Furthermore, the D50 particle size of the lithium-rich lithium ferrite material is 3 to 8 μm.

[0011] By limiting the D50 particle size of the lithium-rich lithium ferrite to the above range, it is evenly dispersed in the slurry, ensuring efficient and stable lithium replenishment effect.

[0012] Furthermore, the coating layer has a thickness of 1 to 20 nm.

[0013] By limiting the thickness of the coating layer to the above range, the physical isolation function and the conductivity enhancement function of the coating layer can be maximized while avoiding the loss of lithium replenishment capacity.

[0014] Furthermore, in the material of the core, the molar ratio of iron to the first doping element is 1:(0.001-0.0021); and / or, in the material of the coating layer, the molar ratio of carbon to the second doping element is (4-9):(0.2-0.5).

[0015] By limiting the molar ratio of the above elements, it is ensured that there are sufficient doping elements in the lithium-rich lithium ferrite material, and at the same time, it is ensured that the lithium-rich lithium ferrite has sufficient active lithium for lithium replenishment. In addition to helping to further reduce the gas production of the battery and improve stability, it also helps to further improve the capacity of the battery.

[0016] Furthermore, the chemical formula of the core is Li5Fe (1-x) M x O4, wherein M is the first doping element, 0.001≤x≤0.002.

[0017] A second aspect of the present invention provides a method for preparing the lithium-rich lithium ferrite material provided in the first aspect, comprising the following steps:

[0018] Step S1, performing a first mixed grinding of a lithium source, an iron source and a first doping material, and performing a first sintering treatment to obtain a core material;

[0019] Step S2, mixing and dispersing the carbon source and the second doping material in a solvent, and heating and stirring until the solvent evaporates to obtain a coating layer precursor;

[0020] Step S3, performing a second mixing and grinding of the core material and the coating layer precursor, and performing a second sintering treatment to obtain a lithium-rich lithium ferrite material;

[0021] The first doping material contains a first doping element, and the second doping material contains a second doping element. The first doping element includes at least one element of Ti, W, Ni, Ce, and Co, and the second doping element includes at least one element of B, N, S, O, and P.

[0022] By implementing the above steps, the present invention can prepare a lithium ferrite-rich material with a specific structure and specific doping elements, and the preparation method is simple and easy to operate, and can achieve large-scale production.

[0023] Furthermore, in step S1, the first doping material includes at least one of TiO2, WO3, NiO, CeO2, and Co2O3; and / or, in step S3, the second doping material includes at least one of cyanamide, glutathione, sodium borohydride, and phytic acid.

[0024] By limiting the specific types of the first doping material and the second doping material, it is helpful to prepare a lithium ferrite-rich material having the above-mentioned doping elements.

[0025] Furthermore, in step S1, the lithium source includes at least one of Li2O, LiOH, Li2C2O4, and Li2CO3; and / or, the iron source includes at least one of Fe2O3, Fe2(C2O4)3, and Fe(NO3)3; and / or, in step S2, the carbon source includes at least one of conductive carbon black, acetylene black, graphite, and graphene.

[0026] Furthermore, in step S1, the molar ratio of lithium element in the lithium source, iron element in the iron source and the first doping element in the first doping material is (5.5~6):1:(0.001~0.0021); and / or, in step S2, the mass ratio of the carbon source to the second doping material is (5~10):1; and / or, in step S3, the mass ratio of the core material to the coating layer precursor is (20~50):1.

[0027] By limiting the ratio of each raw material component, it is not only helpful to prepare the element-doped lithium ferrite material rich in the above structure, but also can make the reaction more complete and avoid raw material loss.

[0028] Furthermore, in step S1, the first sintering treatment is carried out by microwave-assisted heating at a temperature of 600-800°C, a time of 5-10 hours, a microwave power of 1-3kW, and a heating rate of 5-10°C / min; and / or, in step S2, the solvent includes at least one of water, ethanol, and acetone, and the heating temperature is 60-100°C.

[0029] By limiting microwave-assisted heating, coating and element doping are more uniform, further improving capacity and stability. In addition, carbon thermal reactions that reduce purity can be avoided.

[0030] Furthermore, in step S3, the second sintering treatment is carried out under an inert atmosphere, which includes a first sintering stage and a second sintering stage; wherein the temperature of the first sintering stage is 400-600°C and the time is 4-6 hours; the temperature of the second sintering stage is 700-850°C and the time is 3-5 hours; the inert atmosphere is at least one of Ar and He.

[0031] By limiting the segmented sintering, the coating and element doping are made more uniform, thereby further improving the capacity and stability.

[0032] The third aspect of the present invention provides a positive electrode sheet, which comprises a positive electrode active material and a lithium supplement, wherein the lithium supplement comprises the lithium-rich lithium ferrite material provided by the first aspect or the lithium-rich lithium ferrite material prepared by the preparation method provided by the second aspect.

[0033] Since the above-mentioned lithium-rich lithium ferrite material is used as a positive electrode lithium supplement in the positive electrode sheet, the capacity of the battery can be further improved and the gas production can be reduced.

[0034] A fourth aspect of the present invention provides a lithium-ion battery comprising a positive electrode sheet, an electrolyte, a separator and a negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet provided in the third aspect.

[0035] Due to the inclusion of the above-mentioned positive electrode sheet, the lithium-ion battery provided by the present invention has the advantages of high capacity, high stability, low gas production, etc.

[0036] The implementation of the present invention has at least the following beneficial effects:

[0037] The lithium-rich lithium ferrite material provided by the present invention introduces a first doping element and a second doping element so that the core has oxygen vacancies and the coating has nucleation sites. On the one hand, adsorption occurs between the oxygen vacancies in the core and the nucleation sites in the coating, thereby enhancing the bonding strength between the core and the coating and making the coating more uniform and firm, thereby improving the coating effect. In this way, the poor stability of the lithium-rich lithium ferrite material and the difficulty in maximizing the lithium replenishment capacity due to the unevenness and infirmity of the coating are avoided, thereby helping to further improve the stability of the lithium-rich lithium ferrite material and the capacity of the battery. On the other hand, due to the presence of oxygen vacancies in the core and nucleation sites in the coating, the oxygen molecules or oxygen free radicals generated by the battery during the first charging process can be bound inside the material through typing or adsorption, reducing escape and avoiding the problem of further reaction of the oxygen molecules or oxygen free radicals with the electrolyte to generate a large amount of gas, thereby reducing the gas production of the battery and reducing the polarization problem of the lithium-rich lithium ferrite material, so that the high lithium replenishment capacity can still be exerted at a high rate, thereby making the battery have a high capacity when charged at a high rate. DETAILED DESCRIPTION

[0038] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the embodiments.

[0039] As described in the background art, the existing technology has the problems of poor stability, difficulty in exerting the lithium replenishment capacity, and large gas production when lithium-rich lithium ferrite is used as a positive electrode lithium replenisher. In order to solve the above technical problems, the first aspect of the present invention provides a lithium-rich lithium ferrite material, including a core and a coating layer coated on the surface of the core, the core material is lithium-rich lithium ferrite doped with a first doping element, and the coating layer material is a carbon material doped with a second doping element; wherein the first doping element includes at least one of Ti, W, Ni, Ce, and Co, and the second doping element includes at least one of B, N, S, O, and P.

[0040] The lithium-rich lithium ferrite material of the present invention can be directly used as a positive electrode lithium replenisher in pre-lithiation technology. For example, the lithium-rich lithium ferrite material can be mixed with the positive electrode slurry, or the slurry formed by the lithium-rich lithium ferrite material can be coated on the surface of the positive electrode current collector or the positive electrode active layer to form a lithium replenishing layer.

[0041] The lithium-rich lithium ferrite material of the present invention has a core-shell structure, with a shell layer disposed on the outer surface of the core, which serves as a coating. The core and coating each independently comprise a matrix material and a doping element. Research has shown that doping the matrix material with a specific doping element can help improve the electrochemical performance of the lithium-rich lithium ferrite material when used as a positive electrode lithium supplement.

[0042] Specifically, the matrix material of the core is lithium-rich lithium ferrite, the matrix material of the coating layer is carbon material, and the first doping element and the second doping element are independently doped into the lithium-rich lithium ferrite and carbon material in the form of a simple substance or a compound.

[0043] According to the research of the present invention, the above-mentioned lithium-rich lithium ferrite material is used as a positive electrode lithium supplement in a battery, which can further increase the capacity of the battery and reduce the gas production. This is because, by introducing the first doping element and the second doping element, the present invention allows the core to have oxygen vacancies and the coating to have nucleation sites. On the one hand, adsorption occurs between the oxygen vacancies in the core and the nucleation sites in the coating, enhancing the bonding strength between the core and the coating, making the coating more uniform and firm, thereby improving the coating effect. In this way, the poor stability of the lithium-rich lithium ferrite material and the difficulty in maximizing the lithium replenishment capacity caused by the uneven and loose coating are avoided, thereby helping to further improve the stability of the lithium-rich lithium ferrite material and the capacity of the battery. On the other hand, due to the presence of oxygen vacancies in the core and nucleation sites in the coating, the oxygen molecules or oxygen free radicals generated by the battery during the first charging process can be bound inside the material through typing or adsorption, reducing escape and avoiding the problem of further reaction of oxygen molecules or oxygen free radicals with the electrolyte to produce a large amount of gas, thereby reducing the gas production of the battery and reducing the polarization problem of the lithium-rich lithium ferrite material, so that it can still exert a high lithium replenishment capacity at a high rate, thereby making the battery have a high capacity when charged at a high rate.

[0044] Preferably, the first doping element includes at least one of Ti, W, Ni, and Ce; and / or the second doping element includes at least one of N, S, and O.

[0045] The present invention does not limit the specific size of the lithium-rich ferrite material, as long as it contains the above-mentioned materials and specific doping elements. The specific size can be adjusted according to actual needs. In some embodiments, the D50 particle size of the lithium-rich ferrite material is 3 to 8 μm. Thus, by limiting the D50 particle size of the lithium-rich ferrite to the above range, it is evenly dispersed in the slurry, ensuring efficient and stable lithium replenishment.

[0046] The present invention does not limit the thickness of the coating layer, and the thickness can be adjusted according to actual needs. In some embodiments, the thickness of the coating layer is 1 to 20 nm, for example, 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, or any two thereof. By limiting the thickness of the coating layer to the above range, the physical isolation and conductivity enhancement effects of the coating layer can be maximized while avoiding loss of lithium replenishment capacity.

[0047] The present invention does not limit the doping amount of the doping elements, and can be adjusted according to actual needs. For example, in some embodiments, in the material of the inner core, the molar ratio of the iron element to the first doping element is 1: (0.001~0.0021), such as 1:0.001, 1:0.002, 1:0.0021 or a range composed of any two of them; and / or, in the material of the coating layer, the molar ratio of the carbon element to the second doping element is (4~10): (0.2~0.5). By limiting the molar ratio of the above elements, it is ensured that there are sufficient doping elements in the lithium-rich lithium ferrite material, and at the same time, it is ensured that the lithium-rich lithium ferrite has sufficient active lithium for lithium supplementation. In addition to helping to further reduce the gas production of the battery and improve stability, it also helps to further improve the capacity of the battery. Preferably, in some embodiments, the chemical formula of the inner core is Li5Fe (1-x) M x O4, wherein M is the first doping element, 0.001≤x≤0.002.

[0048] A second aspect of the present invention provides a method for preparing the above-mentioned lithium-rich lithium ferrite material, comprising the following steps:

[0049] Step S1, performing a first mixed grinding of a lithium source, an iron source and a first doping material, and performing a first sintering treatment to obtain a core material;

[0050] Step S2, mixing and dispersing the carbon source and the second doping material in a solvent, and heating and stirring until the solvent evaporates to obtain a coating layer precursor;

[0051] Step S3, performing a second mixing and grinding of the core material and the coating layer precursor, and performing a second sintering treatment to obtain a lithium-rich lithium ferrite material;

[0052] The first doping material contains a first doping element, and the second doping material contains a second doping element. The first doping element includes at least one element of Ti, W, Ni, Ce, and Co, and the second doping element includes at least one element of B, N, S, O, and P.

[0053] By implementing the above steps, the present invention can prepare a lithium ferrite-rich material with a specific structure and specific doping elements, and the preparation method is simple and easy to operate, and can achieve large-scale production.

[0054] The first mixed grinding and the second mixed grinding can be carried out in a ball mill. For example, the ball-to-material ratio of the first mixed grinding is (1-10):1, for example, 1:1, 2:1, 4:1, 5:1, 8:1, 10:1 or a range consisting of any two thereof, the rotation speed is 200-500 rpm, for example, 200 rpm, 300 rpm, 400 rpm, 500 rpm or a range consisting of any two thereof, and the time is 1-6 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h or a range consisting of any two thereof.

[0055] The first sintering treatment can be carried out under a vacuum state. In some embodiments, the first sintering treatment is carried out by microwave-assisted heating, and the temperature is 600-800°C, for example, 600°C, 700°C, 800°C or a range consisting of any two thereof, the time is 5-10h, for example, 5h, 6h, 7h, 8h, 9h, 10h or a range consisting of any two thereof, the microwave power is 1-3kW, for example, 1kW, 2kW, 3kW or a range consisting of any two thereof, and the heating rate is 5-10°C / min, for example, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min or a range consisting of any two thereof.

[0056] In step S2, the carbon material and the second doping material are mixed and dispersed in a solvent, and then heated and stirred until the solvent evaporates. This is actually to ensure that the second doping material is evenly attached to the surface of the carbon material. The mixing and dispersion can be assisted by ultrasound, for example, ultrasonic dispersion for 1 to 10 minutes. In some embodiments, the solvent includes at least one of water, ethanol, and acetone, and the heating temperature is 60 to 100°C, for example, 60°C, 70°C, 80°C, 90°C, 100°C, or a range consisting of any two thereof. The heating can be oil bath heating.

[0057] In step S3, the second mixed grinding can be carried out under the condition of dew point ≤-40°C, and the mixed grinding time is 20 to 60 minutes. The second sintering treatment can be a staged sintering to make the coating and element doping more uniform. In some embodiments, the second sintering treatment is carried out under an inert atmosphere, which includes a first stage sintering and a second stage sintering. The temperature of the first stage sintering is 400 to 600°C and the time is 4 to 6 hours. The temperature of the second stage sintering is 700 to 850°C and the time is 3 to 5 hours. The inert atmosphere is at least one of Ar and He. The heating rate of the two stages of sintering in the second sintering treatment can be 5 to 10°C / min.

[0058] The present invention is not limited to the specific selection of raw materials for preparation. For example, in some embodiments, in step S1, the lithium source includes at least one of Li2O, LiOH, Li2C2O4, and Li2CO3; and / or the iron source includes at least one of Fe2O3, Fe2(C2O4)3, and Fe(NO3)3. In some embodiments, in step S2, the carbon source includes at least one of conductive carbon black, acetylene black, graphite, and graphene.

[0059] The first doping material of the present invention includes a first doping element. Correspondingly, in some embodiments, in step S1, the first doping material includes at least one of TiO2, WO3, NiO, CeO2, and Co2O3.

[0060] The second doping material of the present invention includes a second doping element. Correspondingly, in some embodiments, in step S3, the second doping material includes at least one of cyanamide, glutathione, sodium borohydride, and phytic acid.

[0061] The present invention does not limit the ratio of the raw materials used in the preparation, and can be adjusted according to actual needs. For example, in some embodiments, in step S1, the molar ratio of the lithium element in the lithium source, the iron element in the iron source, and the first doping element in the first doping material is (5.5-6):1:(0.001-0.0021); and / or, in step S2, the mass ratio of the carbon source to the second doping material is (5-10):1; and / or, in step S3, the mass ratio of the core material to the coating layer precursor is (20-50):1.

[0062] The molar ratio of the iron element in the iron source to the first doping element in the first doping material is 1:(0.001-0.0021), such as 1:0.001, 1:0.002, 1:0.0021, or any combination thereof. In step S1, the excess lithium can effectively reduce side reactions and avoid affecting the purity of the final product.

[0063] The third aspect of the present invention provides a positive electrode sheet, which comprises a positive electrode active material and a lithium supplement, wherein the lithium supplement comprises the lithium-rich lithium ferrite material provided by the first aspect or the lithium-rich lithium ferrite material prepared by the preparation method provided by the second aspect.

[0064] Since the above-mentioned lithium-rich lithium ferrite material is used as a positive electrode lithium supplement in the positive electrode sheet, the capacity of the battery can be further improved and the gas production can be reduced.

[0065] Specifically, in one embodiment, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer, wherein the positive electrode active material layer includes a positive electrode active material and a lithium replenisher. Thus, in the specific implementation process of the present invention, the lithium replenisher, the positive electrode active material, the conductive agent, and the binder are mixed to form a slurry, which is then coated on the positive electrode current collector. After drying and slicing, the positive electrode sheet is obtained. In another embodiment, the positive electrode sheet includes a positive electrode current collector, the positive electrode active material layer, and the lithium replenisher layer. The positive electrode active material layer includes the positive electrode active material, and the lithium replenisher layer includes the lithium replenisher. Thus, in the specific implementation process of the present invention, the lithium replenisher and the positive electrode active material are each independently mixed with a conductive agent and a binder to form a slurry, which is then separately coated on the positive electrode current collector. After drying and slicing, the positive electrode sheet is obtained.

[0066] A fourth aspect of the present invention provides a lithium-ion battery comprising a positive electrode sheet, an electrolyte, a separator and a negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet provided in the third aspect.

[0067] Due to the inclusion of the above-mentioned positive electrode sheet, the lithium-ion battery provided by the present invention has the advantages of high capacity, high stability, low gas production, etc.

[0068] The beneficial effects of the present application will be further illustrated below with reference to examples.

[0069] Example 1

[0070] Step S1: According to the molar ratio of Li, Fe and the first doping element Ti being 5.5:1:0.001, lithium oxide Li2O, iron oxide Fe2O3 and titanium dioxide TiO2 are weighed respectively, placed in a ball mill, and mixed at a ball-to-material ratio of 5:1 at a speed of 300 rpm for 3 hours. Microwave sintering is performed under vacuum to obtain a core material, wherein the microwave sintering power is 1 kW, the sintering temperature is 600°C, the sintering time is 5 hours, and the heating rate is 5°C / min.

[0071] Step S2: Conductive carbon black and cyanamide were weighed in a mass ratio of 5:1, ultrasonically dispersed in ethanol for 5 minutes, and stirred in an oil bath at 60° C. until evaporated to dryness to obtain a coating layer precursor.

[0072] Step S3: Weigh the core material and the coating layer precursor in a mass ratio of 20:1, grind and mix them for 30 minutes in an environment with a dew point of ≤-40°C, and then heat them in an Ar (ventilation rate of 10m 3 / h) protection, the mixture was kept at 400° C. in a sintering furnace for 4 h, then heated to 700° C. at a rate of 10° C. / min and kept for 3 h to obtain the lithium-rich lithium ferrite material of this embodiment.

[0073] Example 2

[0074] The difference from Example 1 is that in step S1, the first doping element Ti is replaced by W, and correspondingly, titanium dioxide TiO2 is replaced by WO3.

[0075] Example 3

[0076] The difference from Example 1 is that in step S1, the first doping element Ti is replaced by Ni, and correspondingly, titanium dioxide TiO2 is replaced by NiO.

[0077] Example 4

[0078] The difference from Example 1 is that in step S1, the first doping element Ti is replaced by Ce, and correspondingly, titanium dioxide TiO2 is replaced by CeO2.

[0079] Example 5

[0080] The difference from Example 1 is that in step S1, the first doping element Ti is replaced by Co, and correspondingly, titanium dioxide TiO2 is replaced by Co2O3.

[0081] Example 6

[0082] The difference from Example 1 is that in step S2, cyanamide is replaced by glutathione.

[0083] Example 7

[0084] The difference from Example 1 is that in step S2, cyanamide is replaced by sodium borohydride.

[0085] Example 8

[0086] The difference from Example 1 is that, in step S2, cyanamide is replaced by phytic acid.

[0087] Example 9

[0088] The difference from Example 1 is that in step S1, the microwave sintering temperature is 800°C and the time is 10 hours; in step S3, the temperature is kept at 600°C for 6 hours, then the temperature is increased to 850°C at a rate of 10°C / min and kept for 5 hours.

[0089] Example 10

[0090] The difference from Example 1 is that in step S1, the molar ratio of Li, Fe, and the first doping element Ti is 6:1:0.002.

[0091] Example 11

[0092] The difference from Example 1 is that in step S2, the mass ratio of conductive carbon black to cyanamide is 10:1.

[0093] Example 12

[0094] The difference from Example 1 is that in step S3, the mass ratio of the core material to the coating layer precursor is 50:1.

[0095] Example 13

[0096] The difference from Example 1 is that in step S1, the microwave sintering temperature is 850°C and the time is 15 hours; in step S3, the temperature is kept at 600°C for 8 hours, then the temperature is increased to 850°C at a rate of 10°C / min and kept at this temperature for 8 hours.

[0097] Example 14

[0098] The difference from Example 1 is that in step S1, the molar ratio of Li, Fe, and the first doping element Ti is 5.5:1:0.003.

[0099] Example 15

[0100] The difference from Example 1 is that in step S2, the mass ratio of conductive carbon black to cyanamide is 15:1.

[0101] Example 16

[0102] The difference from Example 1 is that in step S3, the mass ratio of the core material to the coating layer precursor is 80:1.

[0103] Comparative Example 1

[0104] Step S1: lithium oxide and iron oxide Fe2O3 are weighed respectively according to a molar ratio of Li to Fe of 5.5:1, placed in a ball mill, and mixed at a speed of 300 rpm for 3 hours at a ball-to-material ratio of 5:1, and microwave sintered under vacuum to obtain a core material, wherein the microwave sintering power is 1 kW, the sintering temperature is 600°C, the sintering time is 5 hours, and the heating rate is 5°C / min.

[0105] Step S2: Conductive carbon black and cyanamide were weighed in a mass ratio of 5:1, ultrasonically dispersed in ethanol for 5 minutes, and stirred in an oil bath at 60° C. until evaporated to dryness to obtain a coating layer precursor.

[0106] Step S3: Weigh the core material and the coating layer precursor in a mass ratio of 20:1, grind and mix them for 30 minutes in an environment with a dew point of ≤-40°C, and then heat them in an Ar (ventilation rate of 10m 3 / h) protection, the mixture was kept at 400° C. in a sintering furnace for 4 h, then heated to 700° C. at a rate of 10° C. / min and kept for 3 h to obtain the lithium-rich lithium ferrite material of this comparative example.

[0107] Comparative Example 2

[0108] Step S1: According to the molar ratio of Li, Fe and the first doping element Ti of 5.5:1:0.001, lithium oxide, iron oxide Fe2O3 and titanium dioxide are weighed respectively, placed in a ball mill, and mixed at a speed of 300 rpm for 3 hours with a ball-to-material ratio of 5:1. Microwave sintering is performed under vacuum to obtain the core material, wherein the microwave sintering power is 1 kW, the sintering temperature is 600°C, the sintering time is 5 hours, and the heating rate is 5°C / min.

[0109] Step S2: weigh the core material and conductive carbon black in a mass ratio of 20:1, grind and mix them for 30 min in an environment with a dew point of ≤-40°C, and then stir in an atmosphere of Ar (ventilation rate of 10 m 3 / h) protection, the mixture was kept at 400° C. in a sintering furnace for 4 h, then heated to 700° C. at a rate of 10° C. / min and kept for 3 h to obtain the lithium-rich lithium ferrite material of this comparative example.

[0110] Comparative Example 3

[0111] Step S1: lithium oxide and iron oxide Fe2O3 were weighed respectively according to a molar ratio of Li to Fe of 5.5:1, placed in a ball mill, mixed at a speed of 300 rpm for 3 hours with a ball-to-material ratio of 5:1, and microwave sintered under vacuum to obtain a core material, wherein the microwave sintering power was 1 kW, the sintering temperature was 600°C, the sintering time was 5 hours, and the heating rate was 5°C / min.

[0112] Step S2: weigh the core material and conductive carbon black in a mass ratio of 20:1, grind and mix them for 30 min in an environment with a dew point of ≤-40°C, and then stir in an atmosphere of Ar (ventilation rate of 10 m 3 / h) protection, the mixture was kept at 400° C. in a sintering furnace for 4 h, then heated to 700° C. at a rate of 10° C. / min and kept for 3 h to obtain the lithium-rich lithium ferrite material of this comparative example.

[0113] Test example

[0114] 1. Power-off test

[0115] The above-mentioned lithium ferrite-rich material, polyvinylidene fluoride (PVDF), and conductive carbon black (SP) were mixed and ground in a mass ratio of 8:1:1, and then coated on aluminum foil as the positive electrode of a lithium-ion battery. A button battery of model CR2032 was assembled in a glove box filled with argon, wherein the battery negative electrode was a metal lithium sheet, the separator was a polypropylene microporous membrane, the electrolyte was a 1 mol / L LiPF6 solution, and the electrolyte solvent was ethylene carbonate (EC): vinylene carbonate (DMC): ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1. The measurement voltage range of the button battery was 2V~4.5V, and the charge and discharge current was 0.05C. The capacity of the button battery was tested.

[0116] 2. Stability Test

[0117] A lithium-rich lithium ferrite material with a mass of m1 was added to N-methyl-2-pyrrolidone (NMP) and ultrasonically dispersed for 1 minute. After centrifugal drying, it was placed in a 30% humidity environment. After being placed for 24 hours, the mass was measured to be m2. The stability coefficient was calculated according to the stability coefficient λ = m2 / m1.

[0118] 3. Gas production test

[0119] Preparation of soft-pack batteries: The above-mentioned lithium-rich lithium ferrite material, lithium iron phosphate material, polyvinylidene fluoride, graphene oxide (GO), conductive carbon black (SP), and carbon nanotubes (SWCNTs) are mixed in a planetary mixer at a mass ratio of 2:94.5:2:0.48:1:0.02, and coated on both sides of aluminum foil using a coater as a positive electrode sheet; graphite, conductive carbon black (SP), carbon nanotubes (SWCNTs), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) are mixed evenly at a mass ratio of 96.5:0.48:0.02:2:1, and coated on both sides of copper foil as a negative electrode sheet; a polypropylene microporous membrane is used as a thin film, and a soft-pack battery cell is assembled by stacking, and then sealed with an aluminum shell; the electrolyte is a 1 mol / L LiPF6 solution, and the electrolyte solvent is ethylene carbonate (EC): vinylene carbonate (DMC): ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1.

[0120] A soft pack battery was prepared by adding lithium iron oxide (LiFePO4) material to lithium iron phosphate material at a dosage of 2%. After the filling was completed, the battery was connected to the bottom of the balance with a thin wire and the battery was completely immersed in water. The mass was recorded as m3 (g). The battery was then subjected to a 0.05C low current formation. After completion, the mass was measured in the same way as m4 (g). The gas production was calculated according to the gas production ΔV = (m3-m4) / 10. The unit of ΔV is cubic centimeters (cm 3 ).

[0121] The test results are shown in Table 1.

[0122] Table 1

[0123]

[0124]

[0125] As shown in Table 1, the present invention can significantly reduce gas production while ensuring stability and lithium replenishment capacity by introducing the first doping element and the second doping element. Comparing Examples 1-12 and Examples 14-16, it can be seen that by adjusting the amount of raw material added, the ratio of each component in the lithium-rich lithium ferrite material can be adjusted, thereby further reducing gas production, improving stability and lithium replenishment capacity. In addition, comparing Example 13 with Example 1, it can be seen that if the temperature of the first sintering treatment is too high or the time is too long, it will lead to overburning, which is prone to carbon thermal reaction and reduces purity, which is not conducive to improving performance.

[0126] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.

Claims

1. A lithium-rich lithium iron oxide material, characterized in that: It includes a core and a coating layer coated on the surface of the core, the material of the core is lithium iron-rich lithium doped with a first doping element, and the material of the coating layer is a carbon material doped with a second doping element; wherein the first doping element includes at least one of Ti, W, Ni, Ce, and Co, and the second doping element includes at least one of B, N, S, O, and P.

2. The lithium-rich lithium iron oxide material according to claim 1, characterized in that: The first doping element includes at least one of Ti, W, Ni, and Ce; and / or the second doping element includes at least one of N, S, and O.

3. The lithium-rich lithium iron oxide material according to claim 1 or 2, characterized in that: The D50 particle size of the lithium-rich lithium iron oxide material is 3 to 8 μm; and / or, the thickness of the coating layer is 1 to 20 nm; and / or, in the material of the core, the molar ratio of iron to the first doping element is 1:(0.001 to 0.0021); and / or, in the material of the coating layer, the molar ratio of carbon to the second doping element is (4 to 9):(0.2 to 0.5). Preferably, the chemical formula of the core is Li5Fe (1-x) M x O4, wherein M is the first doping element, 0.001≤x≤0.

002.

4. A method for preparing the lithium-rich lithium iron oxide material according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step S1, performing a first mixed grinding of a lithium source, an iron source and a first doping material, and performing a first sintering treatment to obtain a core material; Step S2, mixing and dispersing the carbon source and the second doping material in a solvent, and heating and stirring until the solvent evaporates to obtain a coating layer precursor; Step S3, performing a second mixed grinding of the core material and the coating layer precursor, and performing a second sintering treatment to obtain the lithium-rich lithium ferrite material; The first doping material contains a first doping element, and the second doping material contains a second doping element. The first doping element includes at least one element of Ti, W, Ni, Ce, and Co, and the second doping element includes at least one element of B, N, S, O, and P.

5. The preparation method according to claim 4, characterized in that: In step S1, the first doping material includes at least one of TiO2, WO3, NiO, CeO2, and Co2O3; and / or, in step S3, the second doping material includes at least one of cyanamide, glutathione, sodium borohydride, and phytic acid.

6. The preparation method according to claim 4 or 5, characterized in that: In step S1, the lithium source includes at least one of Li2O, LiOH, Li2C2O4, and Li2CO3; and / or, the iron source includes at least one of Fe2O3, Fe2(C2O4)3, and Fe(NO3)3; and / or, in step S2, the carbon source includes at least one of conductive carbon black, acetylene black, graphite, and graphene.

7. The preparation method according to claim 4 or 5, characterized in that: In step S1, the molar ratio of the lithium element in the lithium source, the iron element in the iron source and the first doping element in the first doping material is (5.5-6): 1: (0.001~0.0021); and / or, in step S2, the mass ratio of the carbon source to the second doping material is (5~10):1; and / or, in step S3, the mass ratio of the core material to the coating layer precursor is (20~50):

1.

8. The preparation method according to claim 4 or 5, characterized in that: In step S1, the first sintering treatment is carried out by microwave assisted heating, the temperature is 600-800°C, the time is 5-10h, the microwave power is 1-3kW, and the heating rate is 5-10°C / min; and / or, in step S2, the solvent includes at least one of water, ethanol, and acetone, and the heating temperature is 60-100°C; and / or, in step S3, the second sintering treatment is carried out under an inert atmosphere, which includes a first stage sintering and a second stage sintering; wherein the temperature of the first stage sintering is 400-600°C, and the time is 4-6h; the temperature of the second stage sintering is 700-850°C, and the time is 3-5h; the inert atmosphere is at least one of Ar and He.

9. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode active material and a lithium supplement, wherein the lithium supplement comprises the lithium-rich lithium ferrite material according to any one of claims 1 to 3 or the lithium-rich lithium ferrite material prepared by the preparation method according to any one of claims 4 to 8.

10. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, an electrolyte, a separator and a negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Preparation method for N-doped carbon-covered positive electrode material

    CN108682828A

  • Preparation method of non-metal doped carbon / ferrous sulfide compound

    CN113644283A

  • N-Cat-Li5FeO4 composite lithium supplement additive and preparation and application thereof in lithium ion battery

    CN115148962A

  • N-C (at) Li5FeO4-XNy lithium supplement agent and preparation and application thereof

    CN115148963A

  • Boron-doped carbon-coated nickel nano material, lithium-sulfur battery positive active material with high cycle stability, preparation method of lithium-sulfur battery positive active material and lithium-sulfur battery

    CN115395004A

Cited By

  • Lithium supplement material for positive electrode of lithium ion battery, positive electrode plate of lithium ion battery and lithium ion battery

    CN116565171A

  • Positive lithium supplement agent, preparation method, positive pole piece and secondary battery

    CN119481006A

  • Lithium supplementing agent for positive electrode, preparation method, positive electrode sheet, and secondary battery

    CN119481006B

  • Non-gas-production type lithium-rich lithium ferrite positive electrode lithium supplementing material and preparation method and application of non-gas-production type lithium-rich lithium ferrite positive electrode lithium supplementing material

    CN119786607A

  • A non-gas-producing lithium-rich lithium iron ferrite cathode material, its preparation method and application

    CN119786607B