How to Repair or Recycle Elastomer Film

A polymer latex composition with carboxylated and oxirane-functional components allows for self-healing and recyclability of elastomeric films, addressing the non-repairable and non-recyclable issues of crosslinked films, enhancing durability and reducing waste.

JP7554333B2Active Publication Date: 2024-09-19SYNTHOMER SDN BHD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023166618
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2024-09-19
Estimated Expiration
2039-05-17

AI Technical Summary

Technical Problem

Elastomeric films, such as examination gloves, are typically crosslinked irreversibly, making them non-recyclable and non-repairable due to the lack of self-healing properties, leading to waste and failure of articles containing them.

Method used

The use of a polymer latex comprising carboxylated conjugated diene nitrile latex polymer and oxirane-functional latex polymer, prepared by free radical emulsion polymerization, which allows for self-healing and recyclability through a combination of specific monomer compositions and heating or annealing processes.

Benefits of technology

The method enables the repair and recycling of elastomeric films by promoting self-healing and maintaining mechanical properties, reducing waste and extending the lifespan of articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554333000007
    Figure 0007554333000007
  • Figure 0007554333000013
    Figure 0007554333000013
  • Figure 0007554333000015
    Figure 0007554333000015
Patent Text Reader

Abstract

To provide a method for repairing or recycling elastomeric films or articles containing the elastomeric films made using a specific polymer latex, and to provide a specific polymer latex for making elastomeric films repairable and recyclable.SOLUTION: The repairable and recyclable elastomer film is made from a polymer latex containing: particles of carboxylated conjugated diene-nitrile latex polymer (a), which can be obtained by free radical emulsion polymerization of a mixture of ethylenic unsaturated monomers, and particles of latex polymer (b) containing at least one oxirane functional group. Here, the monomer composition of latex polymer (a) is different from that of latex polymer (b).SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for repairing or recycling elastomeric films, and in particular, but not exclusively, to repairing or recycling elastomeric films using thermal reprocessing. Additionally, the present invention relates to the use of specific polymer latexes to make elastomeric films made from aqueous dispersions of polymer latex particles repairable and recyclable, and to enable self-healing of the films. [Background technology]

[0002] According to current industry standards, elastomeric films, especially for dip-molded applications such as examination gloves, are made from compounds containing carboxylated acrylonitrile butadiene latex (XNBR). In order to obtain the mechanical strength required for the intended use of these elastomeric films, some crosslinking of the film needs to be achieved during the preparation of the elastomeric films.

[0003] To obtain such crosslinked elastomeric films, several different concepts are available in the prior art. One possibility is that the compound for making the elastomeric film contains a conventional sulfur vulcanization system, such as sulfur in combination with accelerators such as thiurams and carbamates and zinc oxide.

[0004] Since sulfur vulcanization systems can cause allergic reactions, alternative concepts have been developed to make latex films curable. Another possibility is to include a crosslinker component in the compound, such as a polyvalent cation (e.g. zinc oxide) or other polyfunctional organic compounds suitable for reacting with functional groups on the latex particles, to achieve chemical crosslinking. Furthermore, if the polymer latex has a sufficient amount of self-crosslinking groups, such as N-methylol amide groups, sulfur vulcanization systems and / or crosslinkers can be avoided altogether.

[0005] All these different concepts result in crosslinked elastomeric films, where the crosslinking is essentially irreversible, so that these elastomeric films cannot be easily recycled and do not exhibit self-healing properties to make them repairable. For example, due to the lack of self-healing properties of the film, if any type of defect occurs during the production of the elastomeric film, such as a pinhole, these products must be discarded, resulting in waste that cannot be reused. Furthermore, if such an elastomeric film ruptures during its use, this cannot be repaired, resulting in irreversible disposal of the elastomeric film and, in turn, failure of the article containing such an elastomeric film.

[0006] Thus, a need exists in the industry for elastomeric films that have inherent self-healing properties and can potentially be recycled to reduce unusable waste of such elastomeric films and to avoid eventual failure of articles containing such elastomeric films.

[0007] WO 2017 / 209596 discloses a polymer latex for dip molding applications that includes two different types of latex particles: one type of latex particle is carboxylated, while the second type of latex particle contains oxirane functional groups.

[0008] It is therefore an object of the present invention to provide a method for repairing or recycling elastomeric films and to select a particular polymer latex to make the elastomeric film obtained therefrom repairable and recyclable. Summary of the Invention

[0009] The inventors have surprisingly discovered an elastomeric film made from a polymer latex comprising: (a) particles of a carboxylated conjugated diene nitrile latex polymer (a) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising: - 15-99% by weight of conjugated dienes; - 1 to 80% by weight of a monomer selected from ethylenically unsaturated nitrile compounds; - 0.05 to 10% by weight of ethylenically unsaturated carboxylic acids and / or their salts; - 0-50% by weight of vinyl aromatic monomers; - 0-65% by weight of alkyl esters of ethylenically unsaturated acids; Weight percentages are based on total monomers in the mixture. In combination or in collaboration, (b) particles of a latex polymer (b) containing at least one oxirane functional group; the monomer composition of the latex polymer (a) is different from the monomer composition of the latex polymer (b); The elastomeric film has self-healing properties and can therefore be repaired and recycled, which was not possible with previous sulfur vulcanized elastomeric films known from the prior art.

[0010] According to one aspect, the present invention relates to a method for repairing an elastomeric film or an article comprising an elastomeric film by the following steps; a) providing a damaged elastomeric film or an article including a damaged elastomeric film, wherein said damaged elastomeric film has at least a surface to be reconnected; b) rejoining the damaged film surface; and c) heating or annealing the damaged elastomeric film while holding the rejoined surfaces of the damaged film in intimate contact at a temperature between 40°C and 200°C; wherein the elastomeric film is made from a polymer latex comprising: (a) Particles of a carboxylated conjugated diene nitrile latex polymer (a) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising: - 15-99% by weight of conjugated dienes; - 1 to 80% by weight of a monomer selected from ethylenically unsaturated nitrile compounds; - 0.05 to 10% by weight of ethylenically unsaturated carboxylic acids and / or their salts; - 0-50% by weight of vinyl aromatic monomers; - 0-65% by weight of alkyl esters of ethylenically unsaturated acids; Weight percentages are based on total monomers in the mixture. In combination or in collaboration, (b) particles of a latex polymer (b) containing at least one oxirane functional group; Here, the monomer composition of the latex polymer (a) is different from the monomer composition of the latex polymer (b).

[0011] According to a further aspect, the present invention relates to a method for recycling an elastomeric film or an article comprising an elastomeric film, comprising cutting, shredding or grinding said elastomeric film or article to form particles of elastomer, optionally blending the obtained particles with particles of virgin elastomer and forming a recycled film or recycled article by exposing the particles to a pressure of 1-20 MPa and a temperature of 40°C-200°C, wherein the elastomeric film is made from a polymer latex comprising: (a) particles of a carboxylated conjugated diene nitrile latex polymer (a) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising: - 15-99% by weight of conjugated dienes; - 1 to 80% by weight of a monomer selected from ethylenically unsaturated nitrile compounds; - 0.05 to 10% by weight of ethylenically unsaturated carboxylic acids and / or their salts; - 0-50% by weight of vinyl aromatic monomers; - 0-65% by weight of alkyl esters of ethylenically unsaturated acids; Weight percentages are based on total monomers in the mixture. In combination or in collaboration, (b) particles of a latex polymer (b) containing at least one oxirane functional group; Here, the monomer composition of the latex polymer (a) is different from the monomer composition of the latex polymer (b).

[0012] According to a further aspect, the present invention also relates to the use of a polymer latex comprising: (a) particles of a carboxylated conjugated diene nitrile latex polymer (a) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising: - 15-99% by weight of conjugated dienes; - 1 to 80% by weight of a monomer selected from ethylenically unsaturated nitrile compounds; - 0.05 to 10% by weight of ethylenically unsaturated carboxylic acids and / or their salts; - 0-50% by weight of vinyl aromatic monomers; - 0-65% by weight of alkyl esters of ethylenically unsaturated acids; Weight percentages are based on total monomers in the mixture. In combination or in collaboration, (b) particles of a latex polymer (b) containing at least one oxirane functional group; Here, the monomer composition of the latex polymer (a) is different from the monomer composition of the latex polymer (b), The elastomeric films obtained from the above polymer latexes are capable of self-healing, repairability and / or recyclability. [Brief description of the drawings]

[0013] [Figure 1]FIG. 1 shows a dumbbell-shaped sample cut from the film using a cutter. [Diagram 2] FIG. 2 shows a dumbbell-shaped sample strained to 1%. [Diagram 3] FIG. 3 shows a dumbbell-shaped sample sustained at 1% strain. [Figure 4] FIG. 4 shows the results of the stress relaxation experiment obtained in Example 9. [Diagram 5] FIG. 5 shows the results of the stress relaxation experiment obtained in Example 10. [Figure 6] FIG. 6 shows the results of the stress relaxation experiment obtained in Example 11. [Figure 7] FIG. 7 shows the tensile test results obtained in Example 22. [Figure 8] FIG. 8 shows the tensile test results obtained in Example 23. [Figure 9] FIG. 9 shows the results of the tensile test obtained in Example 24. [Figure 10] FIG. 10 shows the results of the tensile test obtained in Example 25. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Polymer latexes used to create self-healing, repairable and / or recyclable elastomeric films Polymer latexes used in accordance with one embodiment of the present invention to impart self-healing properties to elastomeric films obtained therefrom, rendering said elastomeric films repairable and / or recyclable, include: (a) particles of a carboxylated conjugated diene nitrile latex polymer (a) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising: - 15-99% by weight of conjugated dienes; - 1 to 80% by weight of a monomer selected from ethylenically unsaturated nitrile compounds; - 0.05 to 10% by weight of ethylenically unsaturated carboxylic acids and / or their salts; - 0-50% by weight of vinyl aromatic monomers; - 0-65% by weight of alkyl esters of ethylenically unsaturated acids; Weight percentages are based on total monomers in the mixture. In combination or in collaboration, (b) particles of a latex polymer (b) containing at least one oxirane functional group; Here, the monomer composition of the latex polymer (a) is different from the monomer composition of the latex polymer (b).

[0015] The term "in combination or association" encompasses not only latexes in which latex polymer (a) and latex polymer (b) exhibit any kind of chemical or physical interaction between the particles of latex polymer (a) and latex polymer (b), but also latexes in which latex polymer (a) and latex polymer (b) are present as a physical mixture, such as a blend of both latex polymers. According to the present invention, the combination or association of particles of said latex polymer (a) with particles of said latex polymer (b) can be achieved, for example, by one of the following means: (i) a mixture of ethylenically unsaturated monomers for a latex polymer (a) is polymerized in the presence of oxirane-functional latex particles (b) in a free radical emulsion polymerization; (ii) preforming a polymer latex comprising particles of latex polymer (a) and a polymer latex comprising particles of latex polymer (b), followed by combining both latices; and (iii) a mixture of ethylenically unsaturated monomers for latex polymer (a) is polymerized in the presence of oxirane-functional latex particles (b) in a free radical emulsion polymerization to form a first polymer latex, a second polymer latex comprising particles of latex polymer (b) is preformed, and subsequently both latexes are combined, wherein the latex comprising oxirane-functional latex particles (b) present in the polymerization of the mixture of ethylenically unsaturated monomers for latex polymer (a) and the second polymer latex comprising particles of component (b) are the same or different.

[0016] The term "the monomer composition of latex polymer (a) is different from the monomer composition of latex polymer (b)" encompasses either the monomers used to prepare latex polymer (a) are different from the monomers for preparing latex polymer (b), or the monomers are the same but used in different relative amounts when preparing latex polymer (a) and latex polymer (b).

[0017] The polymer latex of the present invention may include: (a) particles of a carboxylated conjugated diene nitrile latex polymer (a) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising: - 15-99% by weight of conjugated dienes; - 1 to 80% by weight of a monomer selected from ethylenically unsaturated nitrile compounds; - 0.05 to 10% by weight of ethylenically unsaturated carboxylic acids and / or their salts; - 0-50% by weight of vinyl aromatic monomers; - 0-65% by weight of alkyl esters of ethylenically unsaturated acids; - 0 to 5% by weight, preferably 0 to 3% by weight, of ethylenically unsaturated monomers having oxirane functions; The weight percentages are based on the total monomers in the mixture of latex polymer (a), In combination or in collaboration, (b) Particles of latex polymer (b) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising more than 5% by weight, preferably at least 10% by weight, more preferably at least 15% by weight, of ethylenically unsaturated monomers having oxirane functionality, based on the total monomers in the mixture for latex polymer (b).

[0018] (b) a latex polymer containing at least one oxirane functional group; The latex polymer (b) used in accordance with the present invention can be prepared by any suitable free radical emulsion polymerization method known in the art. Suitable process parameters are those discussed below for the emulsion polymerization process for the preparation of latex polymer (a).

[0019] The unsaturated monomers and their relative amounts used for the preparation of latex polymer (b) are not particularly important, as long as the monomer mixture contains at least one ethylenically unsaturated monomer with oxirane functionality.According to the present invention, the oxirane-functional ethylenically unsaturated monomer may be monofunctional with respect to oxirane functionality and does not contain an oligomeric or polymeric backbone.In particular, the number average molecular weight of the oxirane-functional ethylenically unsaturated monomer is less than 280 Daltons.

[0020] Suitable oxirane-functional ethylenically unsaturated monomers include glycidyl (meth)acrylate, allyl glycidyl ether, vinyl glycidyl ether, vinylcyclohexene oxide, limonene oxide, 2-ethyl glycidyl acrylate, 2-ethyl glycidyl methacrylate, 2-(n-propyl)glycidyl acrylate, 2-(n-propyl)glycidyl methacrylate, 2-(n-butyl)glycidyl acrylate, 2-(n-butyl)glycidyl methacrylate, glycidyl methyl methacrylate, glycidyl acrylate, (3',4'-epoxyheptyl)-2-ethyl acrylate, (3',4'-epoxyheptyl)-2-ethyl methacrylate, and the like. The epoxy group may be selected from the group consisting of acrylate, (6',7'-epoxyheptyl)acrylate, (6',7'-epoxyheptyl)methacrylate, allyl-3,4-epoxyheptyl ether, 6,7-epoxyheptyl allyl ether, vinyl-3,4-epoxyheptyl ether, 3,4-epoxyheptyl vinyl ether, 6,7-epoxyheptyl vinyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, 3-vinylcyclohexene oxide, α-methylglycidyl methacrylate, 3,4-epoxycyclohexylmethyl(meth)acrylate and combinations thereof. Glycidyl(meth)acrylate is particularly preferred.

[0021] The oxirane-functional latex polymer (b) according to the present invention may contain structural units derived from an ethylenically unsaturated oxirane-functional monomer in an amount of 1 to 80% by weight, preferably 20 to 70% by weight, more preferably 25 to 65% by weight, and most preferably 35 to 65% by weight, based on the total weight of monomers for the oxirane-functional latex particle (b). Thus, the lower limit of the amount of the ethylenically unsaturated oxirane-functional monomer may be 1% by weight, or 5% by weight, or 10% by weight, or 12% by weight, or 14% by weight, or 16% by weight, or 18% by weight, or 20% by weight, or 22% by weight, or 24% by weight, or 26% by weight, or 28% by weight, or 30% by weight, or 32% by weight, or 34% by weight, or 35% by weight, based on the total weight of monomers for the oxirane-functional latex particle (b). Thus, the upper limit for the amount of ethylenically unsaturated oxirane-functional monomer may be 80%, or 75%, or 73%, or 70%, or 68%, or 65%, or 62%, or 60%, or 58%, or 56%, or 54%, or 52%, or 50% by weight based on the total weight of monomers in the oxirane-functional latex particles (b). One of ordinary skill in the art will understand that any range formed by any of the explicitly disclosed lower and upper limits is expressly encompassed herein.

[0022] Suitable additional monomers for the preparation of the oxirane-functional latex polymer (b) according to the present invention can be selected from: - Ethylenically unsaturated nitrile compounds; - vinyl aromatic monomers; - alkyl esters of ethylenically unsaturated acids; - hydroxyalkyl esters of ethylenically unsaturated acids; - amides of ethylenically unsaturated acids; - ethylenically unsaturated acids; - ethylenically unsaturated sulfonic acid monomers and / or ethylenically unsaturated phosphorus-containing acid monomers; - vinyl carboxylates; - conjugated dienes; - a monomer having at least two ethylenically unsaturated groups; and - A combination of them.

[0023] Examples of ethylenically unsaturated nitrile monomers that can be used to prepare the oxirane-functional latex polymer (b) according to the present invention include polymerizable unsaturated aliphatic nitrile monomers containing from 2 to 4 carbon atoms in a linear or branched arrangement, which may be substituted with either an acetyl group or an additional nitrile group. Such nitrile monomers include acrylonitrile, methacrylonitrile, α-cyanoethyl acrylonitrile, fumaronitrile, and combinations thereof, with acrylonitrile being most preferred.

[0024] Representative examples of vinyl aromatic monomers include, for example, styrene, alpha-methylstyrene, p-methylstyrene, t-butylstyrene, and vinyltoluene. Preferably, the vinyl aromatic monomer is selected from styrene, alpha-methylstyrene, and combinations thereof.

[0025] Esters of (meth)acrylic acid that can be used to prepare oxirane-functional latex particles (b) according to the present invention include n-, iso-, or tert-alkyl esters of acrylic or (meth)acrylic acid, where the alkyl group has 1 to 20 carbon atoms, reaction products of glycidyl esters of neoacids (such as versatic, neodecanoic, or pivalic acid) with methacrylic acid, and hydroxyalkyl (meth)acrylate and alkoxyalkyl (meth)acrylate monomers.

[0026] Generally, the preferred alkyl esters of (meth)acrylic acid are 1 -C 20 Alkyl (meth)acrylate, preferably C 1 -C 10Can be selected from alkyl (meth)acrylate. Examples of such acrylate monomers include n-butyl acrylate, secondary butyl acrylate, methyl acrylate, ethyl acrylate, hexyl acrylate, tert-butyl acrylate, 2-ethyl-hexyl acrylate, isooctyl acrylate, 4-methyl-2-pentyl acrylate, 2-methylbutyl acrylate, methyl methacrylate, butyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, ethyl methacrylate, isopropyl methacrylate, hexyl methacrylate, cyclohexyl methacrylate and cetyl methacrylate. Particularly preferred is to select (meth)acrylic acid ester from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate and combinations thereof.

[0027] Hydroxyalkyl (meth)acrylate monomers that can be used to prepare the oxirane-functional latex polymer (b) according to the present invention include hydroxyalkyl acrylate and methacrylate monomers based on ethylene oxide, propylene oxide and higher alkylene oxides or mixtures thereof. Examples are hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate and hydroxybutyl acrylate. Preferably, the hydroxyalkyl (meth)acrylate monomer is selected from 2-hydroxyethyl (meth)acrylate.

[0028] Amides of ethylenically unsaturated acids that can be used to prepare the oxirane-functional latex polymer (b) of the present invention include acrylamide, methacrylamide, and diacetone acrylamide.The preferred amide monomer is (meth)acrylamide.

[0029] Vinyl ester monomers that can be used to prepare the oxirane-functional latex polymer (b) according to the present invention include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl benzoate, vinyl-2-ethylhexanoate, vinyl stearate, and vinyl esters of versatic acid. The most preferred vinyl ester is vinyl acetate.

[0030] Ethylenically unsaturated carboxylic acid monomers suitable for preparing the oxirane-functional latex polymer (b) according to the present invention include mono- and di-carboxylic acid monomers, as well as monoesters of dicarboxylic acids. In the practice of the present invention, it is preferred to use ethylenically unsaturated aliphatic mono- or di-carboxylic acids or anhydrides containing 3 to 5 carbon atoms. Examples of mono-carboxylic acid monomers include acrylic acid, methacrylic acid, crotonic acid, and examples of di-carboxylic acid monomers include fumaric acid, itaconic acid, maleic acid, and maleic anhydride. Examples of other suitable ethylenically unsaturated acids include vinyl acetic acid, vinyl lactic acid, vinyl sulfonic acid, 2-methyl-2-propene-1-sulfonic acid, styrene sulfonic acid, acrylamidomethylpropane sulfonic acid, and salts thereof. Preferably, the ethylenically unsaturated carboxylic acid monomer is selected from (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, and combinations thereof.

[0031] Conjugated diene monomers suitable for preparing the oxirane-functional latex polymer (b) according to the present invention include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl -6-methylene-1,7-octadiene, 7-methyl-3-methylene-1,6-octadiene, 1,3,7-octatriene, 2-ethyl-1,3-butadiene, 2-amyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatriene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, and 1,3-cyclohexadiene are preferred conjugated dienes. 1,3-butadiene, isoprene, and combinations thereof are preferred conjugated dienes.

[0032] Additionally, monomers having at least two ethylenically unsaturated groups can be used in the preparation of the oxirane-functional latex polymer (b). Suitable difunctional monomers (herein known as multifunctional monomers) capable of providing internal crosslinking and branching in the polymer may be selected from divinylbenzene and diacrylates and di(meth)acrylates. Examples are ethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and dipropylene glycol di(meth)acrylate. The monomers having at least two ethylenically unsaturated groups are preferably selected from divinylbenzene, 1,2-ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, and 1,6-hexanediol di(meth)acrylate.

[0033] The oxirane functional latex polymer (b) according to the present invention can include structural units derived from: - 0-50% by weight, preferably 0-30% by weight, more preferably 0-20% by weight of an ethylenically unsaturated nitrile compound, preferably acrylonitrile; - 0-95% by weight, preferably 0-70% by weight, more preferably 0-50% by weight of a vinyl aromatic monomer, preferably styrene; - 0 to 95% by weight, preferably 5 to 95% by weight, more preferably 20 to 95% by weight of C 1 ~C 8 Alkyl (meth)acrylate; - 0 to 10% by weight, preferably 0 to 7% by weight, more preferably 0.01 to 7% by weight of an ethylenically unsaturated acid, preferably (meth)acrylic acid; - 0 to 10% by weight, preferably 0 to 8% by weight, more preferably 0 to 6% by weight, of ethylenically unsaturated compounds having silane, sulfonate, sulfonic acid, phosphate, amide and / or N-methylolamide groups; - 0 to 50% by weight, preferably 0 to 40% by weight, more preferably 0 to 20% by weight of vinyl carboxylate, preferably vinyl acetate; - 1 to 80% by weight, preferably 20 to 70% by weight, more preferably 25 to 65% by weight, most preferably 35 to 65% by weight of structural units derived from ethylenically unsaturated oxirane-functional monomers.

[0034] Alternatively, the oxirane functional latex polymer (b) according to the present invention can comprise structural units derived from: - 2 to 95% by weight, preferably 10 to 95% by weight, more preferably 20 to 95% by weight of a conjugated diene, preferably chosen from butadiene, isoprene and combinations thereof, more preferably butadiene; - 1 to 50% by weight, preferably 5 to 50% by weight, more preferably 5 to 40% by weight of a monomer chosen from ethylenically unsaturated nitrile compounds, preferably acrylonitrile; - 0-95% by weight, preferably 0-90% by weight, more preferably 0-70% by weight of a vinyl aromatic monomer, preferably styrene; - 0 to 95% by weight, preferably 0 to 90% by weight, more preferably 0 to 70% by weight of C 1 ~C 8 Alkyl (meth)acrylate; - 0 to 10% by weight, preferably 0 to 8% by weight, more preferably 0 to 7% by weight of an ethylenically unsaturated acid, preferably (meth)acrylic acid; - 0 to 10% by weight, preferably 0 to 8% by weight, more preferably 0 to 6% by weight of ethylenically unsaturated compounds containing silane, sulfonate, sulfonic acid, phosphate, amide and / or N-methylolamide groups; - 1 to 80% by weight, preferably 20 to 70% by weight, more preferably 25 to 65% by weight, most preferably 35 to 65% by weight of structural units derived from ethylenically unsaturated oxirane-functional monomers.

[0035] According to the present invention, the amount of monomers as defined above for the preparation of the latex polymer (b) may total up to 100% by weight.

[0036] The glass transition temperature (midpoint temperature Tmg) of the oxirane-functional latex polymer (b) according to the present invention may be from -50°C to 50°C, preferably from -40°C to 40°C, more preferably from -30°C to 30°C, even more preferably from -25°C to 25°C, and most preferably from -22°C to 22°C, as measured by DSC according to ASTM D3418-03. Thus, the lower limit of the Tmg range may be -50, -45, -40, -38, -36, -34, -32, -30, -29, -28, -27, -26, -25, -24, -23, or -22°C. The upper limit of the Tmg range may be 50, 45, 40, 38, 36, 34, 32, 30, 29, 28, 27, 26, 25, 24, 23, or 22°C. One of ordinary skill in the art will understand that any range formed by any of the explicitly disclosed lower and upper limits is expressly encompassed herein.

[0037] The z-average particle size of the oxirane functional latex particles (b) according to the present invention, whether used as a latex added during the polymerization of the latex polymer (a) or as a preformed latex blended with the latex polymer (a), as measured by dynamic light scattering (DLS) on a Malvern Zetasizer Nano S (ZEN1600), is preferably 5-90 nm, more preferably 15-85 nm, more preferably 20-80 nm. Thus, the lower limit of the z-average particle size can be 5 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, or 20 nm, while the upper limit can be 90 nm, 85 nm, 80 nm, 75 nm, 70 nm, 65 nm, 60 nm, 55 nm, 50 nm, 45 nm, 40 nm, 38 nm, 36 nm, 34 nm, 32 nm, or 30 nm. One of ordinary skill in the art will understand that any range formed by any of the explicitly disclosed lower and upper limits is expressly encompassed herein.

[0038] Those skilled in the art will understand that the oxirane-functional latex polymer (b) of the present invention can be used as particles present in the emulsion polymerization of the latex polymer (A), e.g., as seed particles, or can be blended with a preformed latex polymer (a), whereby the preformed latex polymer (a) can be made by emulsion polymerization, e.g., with or without the oxirane-functional latex polymer (b) of the present invention as particles present in the emulsion polymerization as seed particles. Those skilled in the art will also understand that the oxirane-functional latex particles (b) used as particles present in the emulsion polymerization of the preformed latex polymer (a) and the oxirane-functional latex polymer (b) blended with the preformed latex polymer (a) can be the same or different.

[0039] Latex polymer (a) According to the present invention, the mixture of ethylenically unsaturated monomers for preparing the latex polymer (a) comprises: - 15 to 99% by weight of conjugated dienes, - 1 to 80% by weight of a monomer selected from ethylenically unsaturated nitrile compounds, - 0.05 to 10% by weight of an ethylenically unsaturated carboxylic acid and / or a salt thereof, - 0 to 50% by weight of vinyl aromatic monomers; and - 0-65% by weight of alkyl esters of ethylenically unsaturated acids; The weight percentages are based on total monomers used in the emulsion polymerization.

[0040] In the mixture of ethylenically unsaturated monomers, additional ethylenically unsaturated monomers may be present and are selected from: - hydroxyalkyl esters of ethylenically unsaturated acids; - amides of ethylenically unsaturated acids; - vinyl carboxylates; - monomers having at least two ethylenically unsaturated groups; - ethylenically unsaturated silanes; - oxirane-functional ethylenically unsaturated compounds; and - A combination of them.

[0041] According to the present invention, the mixture of ethylenically unsaturated monomers for preparing the latex polymer (a) may be free of oxirane-functional monomers.

[0042] Conjugated diene monomers suitable for preparing the latex polymer (a) according to the present invention include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7- Conjugated diene monomers selected from octadiene, 7-methyl-3-methylene-1,6-octadiene, 1,3,7-octatriene, 2-ethyl-1,3-butadiene, 2-amyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatriene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, myrcene, ocimene and farnacene. 1,3-butadiene, isoprene and combinations thereof are preferred conjugated dienes. 1,3-butadiene is the most preferred diene. Typically, the amount of conjugated diene monomer is 15-99 wt%, preferably 20-99 wt%, more preferably 30-75 wt%, and most preferably 40-70 wt% based on the total weight of monomers. Thus, the conjugated diene may be present in an amount of at least 15 wt%, at least 20 wt%, at least 22 wt%, at least 24 wt%, at least 26 wt%, at least 28 wt%, at least 30 wt%, at least 32 wt%, at least 34 wt%, at least 36 wt%, at least 38 wt%, or at least 40 wt% based on the total weight of ethylenically unsaturated monomers for the latex polymer (a).

[0043] Thus, conjugated diene monomer can be used in amounts of 95% or less, 90% or less, 85% or less, 80% or less, 78% or less, 76% or less, 74% or less, 72% or less, 70% or less, 68% or less, 66% or less, 64% or less, 62% or less, 60% or less, 58% or less, or 56% or less by weight. One of ordinary skill in the art would understand that any range between any of the explicitly disclosed lower and upper limits is disclosed herein.

[0044] Unsaturated nitrile monomers that can be used to make the particles of latex polymer (a) include polymerizable unsaturated aliphatic nitrile monomers containing 2 to 4 carbon atoms in a linear or branched arrangement, which may be substituted with either an acetyl group or an additional nitrile group. Such nitrile monomers include acrylonitrile, methacrylonitrile, α-cyanoethyl acrylonitrile, fumaronitrile, and combinations thereof, with acrylonitrile being most preferred. These nitrile monomers may be included in an amount of 1 to 80% by weight, preferably 10 to 70% by weight, or 1 to 60% by weight, and more preferably 15 to 50% by weight, even more preferably 20 to 50% by weight, and most preferably 23 to 43% by weight, based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a).

[0045] Thus, the unsaturated nitrile may be present in an amount of at least 1 weight percent, 5 weight percent, at least 10 weight percent, at least 12 weight percent, at least 14 weight percent, at least 16 weight percent, at least 18 weight percent, at least 20 weight percent, at least 22 weight percent, at least 24 weight percent, at least 26 weight percent, at least 28 weight percent, at least 30 weight percent, at least 32 weight percent, at least 34 weight percent, at least 36 weight percent, at least 38 weight percent, or at least 40 weight percent based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a).

[0046] Thus, the unsaturated nitrile monomer can be used in amounts of 80% or less, 75% or less, 73% or less, 70% or less, 68% or less, 66% or less, 64% or less, 62% or less, 60% or less, 58% or less, 56% or less, 54% or less, 52% or less, 50% or less, 48% or less, 46% or less, or 44% or less by weight. One of ordinary skill in the art would understand that any range between any of the explicitly disclosed lower and upper limits is disclosed herein.

[0047] The ethylenically unsaturated carboxylic acid or its salt can be selected from monocarboxylic and dicarboxylic acid monomers and their anhydrides, and partial esters of polycarboxylic acids. To carry out the present invention, it is preferable to use ethylenically unsaturated aliphatic mono- or dicarboxylic acids or anhydrides containing 3 to 5 carbon atoms. Examples of monocarboxylic acid monomers include acrylic acid, methacrylic acid, and crotonic acid, and examples of dicarboxylic acid monomers include fumaric acid, itaconic acid, maleic acid, cis-cyclohexene-1,2-dicarboxylic acid, dimethyl maleic acid, bromomaleic acid, 2,3-dichloromaleic acid, and (2-dodecen-1-yl)succinic acid. Examples of polycarboxylic acid partial esters include monomethyl maleate, monomethyl fumarate, monoethyl maleate, monoethyl fumarate, monopropyl maleate, monopropyl fumarate, monobutyl maleate, monobutyl fumarate, mono(2-ethylhexyl) maleate, and mono(2-ethylhexyl) fumarate. Examples of other suitable ethylenically unsaturated acids include vinyl acetic acid, vinyl lactic acid, vinyl sulfonic acid, 2-methyl-2-propene-1-sulfonic acid, styrene sulfonic acid, acrylamidomethylpropane sulfonic acid, and salts thereof. (Meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, and combinations thereof are particularly preferred.

[0048] The use of ethylenically unsaturated carboxylic acid monomers affects the properties of the polymer dispersion and the film produced therefrom. This determines the type and amount of these monomers. Typically, such amount is 0.05 to 10 wt%, in particular 0.1 to 10 wt% or 0.05 to 7 wt%, preferably 0.1 to 9 wt%, more preferably 0.1 to 8 wt%, even more preferably 1 to 7 wt%, and most preferably 2 to 7 wt%, based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a). Thus, the ethylenically unsaturated carboxylic acid monomer may be present in an amount of at least 0.01 wt%, at least 0.05 wt%, at least 0.1 wt%, at least 0.3 wt%, at least 0.5 wt%, at least 0.7 wt%, at least 0.9 wt%, at least 1 wt%, at least 1.2 wt%, at least 1.4 wt%, at least 1.6 wt%, at least 1.8 wt%, at least 2 wt%, at least 2.5 wt%, or at least 3 wt%. Similarly, the ethylenically unsaturated carboxylic acid monomer may be present in an amount of 10% or less, 9.5% or less, 9% or less, 8.5% or less, 8% or less, 7.5% or less, 7% or less, 6.5% or less, 6% or less, 5.5% or less, or 5% or less by weight based on the total weight of the ethylenically unsaturated monomers for latex polymer (a). One of ordinary skill in the art will understand that any range defined by an explicitly disclosed lower limit and an explicitly disclosed upper limit is herein disclosed.

[0049] Representative examples of vinyl aromatic monomers include, for example, styrene, α-methylstyrene, vinyltoluene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, vinylnaphthalene, vinyltoluene, vinylxylene, 2-vinylpyridine, 4-vinylpyridine, 1,1-diphenylethylene, substituted 1,1-diphenylethylene, 1,2-diphenylethylene and substituted 1,2-diphenylethylene. Mixtures of one or more vinyl aromatic compounds can also be used. Preferred monomers are styrene and α-methylstyrene. The vinyl aromatic compound can be used in the range of 0-50 wt%, preferably 0-40 wt%, more preferably 0-25 wt%, even more preferably 0-15 wt%, and most preferably 0-10 wt%, based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a). Thus, the vinyl aromatic compound can be present in an amount of 35 wt% or less, 30 wt% or less, 25 wt% or less, 20 wt% or less, 18 wt% or less, 16 wt% or less, 14 wt% or less, 12 wt% or less, 10 wt% or less, 8 wt% or less, 6 wt% or less, 4 wt% or less, 2 wt% or less, or 1 wt% or less, based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a). The vinyl aromatic compound may also be completely absent.

[0050] Furthermore, the mixture of ethylenically unsaturated monomers for the latex polymer (a) according to the present invention can contain additional ethylenically unsaturated monomers different from the monomers specified above. These monomers can be selected from esters of (meth)acrylic acid, vinyl esters, and amides of ethylenically unsaturated acids, or ethylenically unsaturated silane compounds.

[0051] Vinyl ester monomers that can be used according to the present invention include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl benzoate, vinyl-2-ethylhexanoate, vinyl stearate, and vinyl esters of Versatic acid. The most preferred vinyl ester monomer for use in the present invention is vinyl acetate. Typically, the vinyl ester monomer can be present in an amount of 18% by weight or less, 16% by weight or less, 14% by weight or less, 12% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, 4% by weight or less, 2% by weight or less, or 1% by weight or less, based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a).

[0052] Examples of suitable ethylenically unsaturated silane compounds can be selected from triethoxyvinylsilane and 3-methacryloxypropyltrimethoxysilane. The ethylenically unsaturated silane compound can be present in an amount of 0.05-5.0% by weight, preferably 0.3-2.0% by weight, more preferably 0.3-1.0% by weight, based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a).

[0053] Esters of (meth)acrylic acid that can be used in accordance with the present invention include n-, iso-, or tert-alkyl esters of acrylic or (meth)acrylic acid, in which the alkyl group has 1 to 20 carbon atoms, reaction products of glycidyl esters of neo acids (such as versatic, neodecanoic, or pivalic acid) with methacrylic acid, and hydroxyalkyl (meth)acrylate and alkoxyalkyl (meth)acrylate monomers.

[0054] Generally, the preferred alkyl esters of (meth)acrylic acid are 1 -C 10 Alkyl (meth)acrylate, preferably C 1 -C 8Can be selected from alkyl (meth)acrylate. Examples of such acrylate monomers include n-butyl acrylate, secondary butyl acrylate, ethyl acrylate, hexyl acrylate, tert-butyl acrylate, 2-ethyl-hexyl acrylate, isooctyl acrylate, 4-methyl-2-pentyl acrylate, 2-methylbutyl acrylate, methyl methacrylate, butyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, ethyl methacrylate, isopropyl methacrylate, hexyl methacrylate, cyclohexyl methacrylate and cetyl methacrylate. Methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate and combinations thereof are preferred.

[0055] Typically, the alkyl (meth)acrylate monomer can be present in an amount of 18% by weight or less, 16% by weight or less, 14% by weight or less, 12% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, 4% by weight or less, 2% by weight or less, or 1% by weight or less, based on the total weight of ethylenically unsaturated monomers for latex polymer (a).

[0056] Hydroxyalkyl (meth)acrylate monomers that can be used to prepare the polymer latex according to the present invention include hydroxyalkyl acrylate and hydroxyalkyl methacrylate monomers based on ethylene oxide, propylene oxide and higher alkylene oxides or mixtures thereof. Examples are hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate and hydroxybutyl acrylate. Preferably, the hydroxyalkyl (meth)acrylic monomer is 2-hydroxyethyl (meth)acrylate. Typically, the hydroxyalkyl (meth)acrylate monomer can be present in an amount of 18% by weight or less, 16% by weight or less, 14% by weight or less, 12% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, 4% by weight or less, 2% by weight or less, or 1% by weight or less based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a).

[0057] The alkoxyalkyl (meth)acrylate monomers that can be used in the present invention include methoxyethyl methacrylate, ethoxyethyl methacrylate, methoxyethyl methacrylate, ethoxyethyl acrylate, butoxyethyl methacrylate, methoxybutyl acrylate and methoxyethoxyethyl acrylate.Preferred alkoxyalkyl (meth)acrylate monomers are ethoxyethyl acrylate and methoxyethyl acrylate.Typically, the alkoxyethyl alkyl (meth)acrylate monomers can be present in an amount of 18% by weight or less, 16% by weight or less, 14% by weight or less, 12% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, 4% by weight or less, 2% by weight or less, or 1% by weight or less based on the total weight of the ethylenically unsaturated monomers for latex polymer (a).

[0058] The amides of ethylenically unsaturated acids that can be used to prepare the polymer latex according to the present invention include acrylamide, methacrylamide, and diacetone acrylamide. The preferred amide monomer is (meth)acrylamide. To introduce functional groups capable of self-crosslinking during heat treatment into the polymer particles of the present invention, monomers containing N-methylol amide groups may be employed. Suitable monomers are N-methylol (meth)acrylamide, N-methoxymethyl-(meth)acrylamide, Nn-butoxy-methyl-(meth)acrylamide, N-iso-butoxy-methyl-(meth)acrylamide, N-acetoxymethyl-(meth)acrylamide, N(-2,2-dimethoxy-1-hydroxyethyl)acrylamide. Typically, the amide of an ethylenically unsaturated acid can be present in an amount of 18% by weight or less, 16% by weight or less, 14% by weight or less, 12% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, 4% by weight or less, 2% by weight or less, or 1% by weight or less, based on the total weight of the ethylenically unsaturated monomers for the latex polymer (a).

[0059] Furthermore, monomers having at least two ethylenically unsaturated groups can be present in the monomer mixture for the preparation of the polymer latex of the present invention in an amount of 0 to 6.0% by weight, preferably 0.1 to 3.5% by weight, based on the total weight of the ethylenically unsaturated monomers. Typically, these monomers can be present in an amount of 6% by weight or less, 4% by weight or less, 2% by weight or less, 1% by weight or less, based on the total weight of the ethylenically unsaturated monomers. Suitable difunctional monomers (known herein as multifunctional monomers) capable of providing internal crosslinking and branching in the polymer may be selected from divinylbenzene and diacrylates and di(meth)acrylates. Examples are ethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and dipropylene glycol di(meth)acrylate. The monomer having at least two ethylenically unsaturated groups is preferably selected from divinylbenzene, 1,2-ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, and 1,6-hexanediol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate.

[0060] Suitable oxirane functional monomers for use in preparing the latex polymer (a) are those described above for the oxirane functional latex polymer (b), including preferred embodiments. When used, the oxirane functional monomer is preferably present in an amount of up to 5% by weight, more preferably up to 3% by weight, based on the total amount of monomers used in preparing the latex polymer (a). However, as noted above, it is most preferred that the latex polymer (a) does not contain oxirane functionality.

[0061] The mixture of ethylenically unsaturated monomers for the latex polymer (a) may include: - 20-99% by weight of a conjugated diene, preferably selected from butadiene, isoprene and combinations thereof, more preferably butadiene; - 1 to 60% by weight of a monomer selected from ethylenically unsaturated nitrile compounds, preferably acrylonitrile; - 0 to 40% by weight of a vinyl aromatic monomer, preferably styrene; - C 1 ~C 8 Alkyl (meth)acrylate 0-25% by weight; - 0.05 to 7% by weight of an ethylenically unsaturated acid, preferably (meth)acrylic acid; - 0-10% by weight of vinyl esters; - 0-10% by weight of ethylenically unsaturated compounds containing silane, amide and / or N-methylolamide groups; The weight percentages are based on total monomers present in the mixture.

[0062] According to the present invention, the amount of the above-defined monomers for the preparation of the latex polymer (a) may total up to 100% by weight.

[0063] According to the present invention, the mixture of ethylenically unsaturated monomers polymerized in the free radical emulsion polymerization may also include: (a) 15-90% by weight isoprene; (b) 1 to 80% by weight of acrylonitrile; (c) 0.01 to 10% by weight, preferably 0.05 to 10% by weight, of at least one ethylenically unsaturated acid; (d) 0 to 40% by weight of at least one aromatic vinyl compound; and (e) 0 to 20% by weight of at least one further ethylenically unsaturated compound different from any of the compounds (a) to (d). The ranges for components (a) and / or (b) can be selected from the ranges for (a) conjugated diene and (b) unsaturated nitrile described above. Similarly, the specific embodiments and amounts for components (c), (d) and / or (e) can be selected from those described above for components (c), (d) and the additional polymer.

[0064] The z-average particle size of the latex particles (a) of the present invention measured by dynamic light scattering (DLS) using Zetasizer Nano S (ZEN1600) manufactured by Malvern Instruments is preferably 70 to 1000 nm, more preferably 80 to 1000 nm, more preferably 90 to 1000 nm, 100 to 1000 nm, more preferably 110 to 600 nm, more preferably 120 to 500 nm. Therefore, the lower limit of the z-average particle size of the latex particles (a) can be 70 nm, 80 nm, 90 nm, 100 nm, 105 nm, 110 nm, or 120 nm, and the upper limit of the z-average particle size can be 900 nm, 800 nm, 700 nm, 600 nm, 500 nm, 400 nm, 350 nm, 300 nm, 270 nm, 250 nm, 230 nm, 210 nm, or 200 nm. One of ordinary skill in the art will understand that any range formed by any of the explicitly disclosed lower and upper limits is expressly encompassed herein.

[0065] According to the present invention it is particularly preferred that the z-average particle size of the latex polymer (a) is greater than the z-average particle size of the latex polymer (b).

[0066] Method for preparing the polymer latex of the present invention: The latex polymer (a) according to the present invention can be prepared by any emulsion polymerization method known to those skilled in the art, provided that the monomer mixtures defined herein are used. The methods described in EP-A-792891 are particularly suitable.

[0067] In the emulsion polymerization to prepare the latex polymer (a) of the present invention, a seed latex may be employed. Preferably, the seed latex is the latex polymer (b) as described above, including all the disclosed variations. Alternatively, any other seed particles known to those skilled in the art may be used. However, if the latex polymer (b) is not used as a seed particle, the particles of the latex polymer (b) must be incorporated into the polymer latex of the present invention in any other suitable manner, such as by mixing a preformed latex containing particles of the latex polymer (a) with a preformed latex containing particles of the latex polymer (b).

[0068] The seed latex particles are preferably present in an amount of 0.01 to 10, preferably 1 to 5 parts by weight based on 100 parts by weight of all ethylenically unsaturated monomers used in the polymer latex, including those used to make the seed particles, such as oxirane-functional latex particles (b). Thus, the lower limit of the amount of seed latex particles can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5 parts by weight. The upper limit of the above amount can be 10, 9, 8, 7, 6, 5.5, 5, 4.5, 4, 3.8, 3.6, 3.4, 3.3, 3.2, 3.1 or 3 parts by weight. One of ordinary skill in the art will recognize that any range formed by any of the explicitly disclosed lower and upper limits is expressly encompassed herein.

[0069] The above-mentioned process for the preparation of the polymer latex can be carried out in the presence or absence of one or more emulsifiers, in the presence or absence of one or more colloids and in the presence of one or more initiators at temperatures between 0 and 130° C., preferably between 0 and 100° C., particularly preferably between 5 and 70° C. and very particularly preferably between 5 and 60° C., including all values ​​and subvalues ​​therebetween, in particular 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120 and 125° C.

[0070] The initiator that can be used in carrying out the present invention includes water-soluble and / or oil-soluble initiators that are effective for polymerization purposes.Representative initiators are well known in the art and include, for example, azo compounds (e.g., AIBN, AMBN, and cyanovaleric acid) and inorganic peroxy compounds (e.g., hydrogen peroxide, sodium, potassium, and ammonium peroxydisulfates, peroxycarbonates, and peroxyborates), as well as organic peroxy compounds (e.g., alkyl hydroperoxides, dialkyl peroxides, acyl hydroperoxides, and diacyl peroxides), and esters (e.g., tert-butyl perbenzoate), as well as combinations of inorganic and organic initiators.

[0071] The initiator is used in an amount sufficient to initiate the polymerization reaction at the desired rate. Generally, an amount of initiator of 0.01 to 5 weight percent, preferably 0.1 to 4 weight percent, based on the weight of the total polymer, is sufficient. Most preferably, the amount of initiator is 0.01 to 2 weight percent, based on the total weight of the polymer. The amount of initiator includes all values ​​and subvalues ​​therebetween, particularly including 0.01, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 4 and 4.5 weight percent, based on the total weight of the polymer.

[0072] The inorganic and organic peroxy compounds mentioned above may also be used alone or in combination with one or more suitable reducing agents, as is well known in the art. Examples of such reducing agents that may be mentioned are sulfur dioxide, alkali metal disulfites, alkali metal and ammonium hydrogen sulfites, thiosulfates, dithionites and formaldehyde sulfoxylates, as well as hydroxylamine hydrochloride, hydrazine sulfate, iron(II) sulfate, copper naphthanate, glucose, sulfonic acid compounds such as sodium methanesulfonate, amine compounds such as dimethylaniline, and ascorbic acid. More preferred is the use of the proprietary sodium salts of organic sulfinic acid derivatives, such as Bruggolite® FF6 or Bruggolite® FF6M. The amount of reducing agent is preferably between 0.03 and 10 parts by weight per part by weight of polymerization initiator.

[0073] Suitable surfactants or emulsifiers for stabilizing latex particles include conventional surfactants for polymerization processes. Surfactants can be added to the aqueous phase and / or the monomer phase. In a seeded process, an effective amount of surfactant is an amount selected to support colloidal stabilization of the particles, minimizing interparticle contact and preventing coagulation. In a non-seeded process, an effective amount of surfactant is an amount selected to affect particle size.

[0074] Representative surfactants include saturated and ethylenically unsaturated sulfonic acids or salts thereof (including unsaturated hydrocarbon sulfonic acids and their salts, such as vinyl sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid), aromatic hydrocarbon acids (such as p-styrene sulfonic acid, isopropenyl benzene sulfonic acid, and vinyloxybenzene sulfonic acid and their salts), sulfoalkyl esters of acrylic and methacrylic acid (such as sulfoethyl methacrylate and sulfopropyl methacrylate and their salts), 2-acrylamido-2-methylpropane sulfonic acid and their salts, alkylated diphenyloxide disulfonates, sodium dodecylbenzene sulfonate, dihexyl ester of sodium sulfosuccinate, sodium alkyl esters of sulfonic acid, ethoxylated alkylphenols and ethoxylated alcohols, and fatty alcohol (poly)ether sulfates.

[0075] The type and amount of surfactant is typically governed by the number of particles, their size and their composition. Typically, surfactants are used in an amount of 0-20, preferably 0-10, more preferably 0-5% by weight, based on the total weight of monomers. The amount of surfactant includes all values ​​and subvalues ​​therebetween, in particular 0, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18 and 19% by weight, based on the total weight of monomers. According to one embodiment of the present invention, the polymerization is carried out without the use of surfactants.

[0076] Instead of or in addition to the above surfactants, various protective colloids can also be used. Suitable colloids include partially acetylated polyvinyl alcohol, casein, hydroxyethyl starch, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polysaccharides and polyhydroxy compounds such as degraded polysaccharides, polyethylene glycol and gum arabic. Preferred protective colloids are carboxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl cellulose. In general, these protective colloids are used in a content of 0 to 10, preferably 0 to 5, more preferably 0 to 2 parts by weight, based on the total weight of the monomers. The amount of protective colloid includes all values ​​and subvalues ​​therebetween, in particular 1, 2, 3, 4, 5, 6, 7, 8 and 9% by weight, based on the total weight of the monomers.

[0077] Those skilled in the art will understand the types and amounts of polar functional monomers, surfactants and protective colloids that are selected to make the polymer latex of the present invention suitable for dip molding applications. Thus, the polymer latex composition of the present invention contains 30 mmol / l CaCl 2 It is preferred that the composition has a certain maximum electrolyte stability, determined as the critical freezing concentration (CFC) of less than 25 mmol / l, preferably less than 25 mmol / l, more preferably less than 20 mmol / l, and most preferably less than 10 mmol / l (measured for 0.1% total solids of the composition at pH 10 and 23° C.).

[0078] If the electrolyte is too stable, it will be difficult to coagulate the polymer latex in the dip molding process, resulting in either no continuous film of polymer latex being formed on the former or the resulting product having an uneven thickness.

[0079] It is within the routine of a person skilled in the art to appropriately adjust the electrolyte stability of the polymer latex.The electrolyte stability depends on certain different factors, such as the amount and selection of monomers used to make the polymer latex, especially the monomers containing polar functional groups, and the selection and amount of stabilizing system, such as the emulsion polymerization method to make the polymer latex.The stabilizing system can contain surfactants and / or protective colloids.

[0080] Depending on the monomers selected and their relative amounts to make the polymer latex of the present invention, one skilled in the art can adjust the stabilization system to achieve electrolyte stability according to the present invention.

[0081] Since there are so many different influences on electrolyte stability, adjustments are best made by trial and error experimentation, but this can be easily done without undue effort using the test methods for electrolyte stability as disclosed above.

[0082] It is often recommended to further carry out the emulsion polymerization in the presence of buffer substances and chelating agents. Suitable substances are, for example, alkali metal carbonates and hydrogen carbonates, alkali metal phosphates and pyrophosphates (buffer substances) and alkali metal salts of ethylenediaminetetraacetic acid (EDTA) or hydroxyl-2-ethylenediaminetriacetic acid (HEEDTA) as chelating agents. The amount of buffer substances and chelating agents is usually 0.001-1.0% by weight, based on the total amount of monomers.

[0083] In addition, it may be advantageous to use chain transfer agents (regulators) in the emulsion polymerization. Typical agents are, for example, thioesters, 2-mercaptoethanol, 3-mercaptopropionic acid and C 1 -C 12The organic sulfur compounds are alkyl mercaptans, with n-dodecyl mercaptan and t-dodecyl mercaptan being preferred. The amount of chain transfer agent, if present, is usually 0.05-3.0% by weight, preferably 0.2-2.0% by weight, based on the total weight of the monomers used.

[0084] Additionally, it may be beneficial to introduce partial neutralization into the polymerization process. Those skilled in the art will appreciate that by appropriate selection of this parameter the necessary control may be achieved.

[0085] Various other additives and ingredients can be added to prepare the latex composition of the present invention. Such additives include, for example, defoamers, wetting agents, thickeners, plasticizers, fillers, pigments, dispersants, optical brighteners, antioxidants, biocides, and metal chelating agents. Known defoamers include silicone oils and acetylene glycol. Commonly known wetting agents include alkylphenol ethoxylates, alkali metal dialkyl sulfosuccinates, acetylene glycol, and alkali metal alkyl sulfates. Typical thickeners include polyacrylates, polyacrylamides, xanthan gum, modified cellulose, or granular thickeners such as silicas and clays. Typical plasticizers include mineral oils, liquid polybutenes, liquid polyacrylates, and lanolin. Titanium dioxide (TiO 2 ), calcium carbonate and clay are typically used fillers.

[0086] In another embodiment of the present invention, a polymer latex containing particles of latex polymer (a) and a polymer latex containing particles of latex polymer (b) are preformed, and then both latexes are combined. The emulsion polymerization for preparing the preformed latexes containing latex polymer (a) and latex polymer (b), respectively, can be carried out in the same manner as described above for preparing the latex containing latex polymer (a), including all the modifications disclosed.

[0087] The polymer latex of the present invention may comprise 50-99% by weight, preferably 60-98% by weight, more preferably 65-97% by weight, and most preferably 70-96% by weight of latex polymer (a) particles based on the total weight of latex particles in the composition, and 1-50% by weight, preferably 2-40% by weight, more preferably 3-35% by weight, and most preferably 4-30% by weight of oxirane-functional latex polymer (b) based on the total weight of latex particles in the composition. Thus, the lower limit of the amount of latex polymer (a) particles may be 50% by weight, or 55% by weight, or 58% by weight, or 60% by weight, or 62% by weight, or 63% by weight, or 64% by weight, or 65% by weight, or 66% by weight, or 67% by weight, or 68% by weight, or 69% by weight, or 70% by weight, based on the total weight of latex particles in the composition. The upper limit for the amount of particles of latex polymer (a) can be 99% by weight, or 98% by weight, or 97% by weight, or 96% by weight, or 95% by weight, or 94% by weight, or 93% by weight, or 92% by weight, or 91% by weight, or 90% by weight, or 89% by weight, or 88% by weight, or 87% by weight, or 86% by weight, or 85% by weight, or 84% by weight, or 83% by weight, or 82% by weight, or 81% by weight, or 80% by weight, based on the total weight of the latex particles in the composition. The lower limit of the amount of particles of latex polymer (b) may be 1% by weight, or 1% by weight, or 1% by weight, or 1% by weight, or 5% by weight, or 6% by weight, or 7% by weight, or 8% by weight, or 9% by weight, or 10% by weight, or 11% by weight, or 12% by weight, or 13% by weight, or 14% by weight, or 15% by weight, or 16% by weight, or 17% by weight, or 18% by weight, or 19% by weight, or 20% by weight. The upper limit of the amount of particles of latex polymer (b) may be 50% by weight, or 45% by weight, or 42% by weight, or 40% by weight, or 38% by weight, or 37% by weight, or 36% by weight, or 35% by weight, or 34% by weight, or 33% by weight, or 32% by weight, or 31% by weight, or 30% by weight, based on the total weight of the latex particles in the composition.One of ordinary skill in the art will understand that any range formed by any of the explicitly disclosed lower and upper limits is expressly encompassed herein.

[0088] For the preparation of the polymer latex of the present invention, a mixture of ethylenically unsaturated monomers for latex polymer (a) can be polymerized in the presence of particles of oxirane-functional latex polymer (b) in a free radical emulsion polymerization to form a first polymer latex (e.g., particles of oxirane-functional latex polymer (b) can be present as seed particles), and a second polymer latex containing particles of latex polymer (b) can be preformed, followed by combining both latexes, where the oxirane-functional latex polymer (b) present during the polymerization of latex polymer (a) and the second polymer latex containing particles of latex polymer (b) can be the same or different. Each emulsion polymerization to form the first and second latexes can be carried out in the same manner as described above for the preparation of the latex containing latex polymer (a), including all the modifications disclosed.

[0089] In the above case, the polymer latex of the present invention can include particles of latex polymer (a) in an amount of 50-99% by weight, preferably 60-98, more preferably 65-97, and most preferably 70-96% by weight, based on the total weight of the latex particles in the composition, the latex polymer (a) is prepared in the presence of the oxirane-functional latex polymer (b) in an amount of 0.01-10, preferably 1-5 parts by weight, based on 100 parts by weight of the total ethylenically unsaturated monomers in the polymer latex (a) including those for making the oxirane-functional latex polymer (b) present during the polymerization of the latex polymer (a), and the polymer latex of the present invention can include second oxirane-functional latex particles (b) in an amount of 1-50% by weight, preferably 2-40, more preferably 3-35, and most preferably 4-30% by weight, based on the total weight of the latex particles in the composition.

[0090] Thus, the lower limit of the amount of oxirane functional latex polymer (b) for the preparation of the first latex can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5 parts by weight. The upper limit of the amount can be 10, 9, 8, 7, 6, 5.5, 5, 4.5, 4, 3.8, 3.6, 3.4, 3.3, 3.2, 3.1, or 3 parts by weight. Those skilled in the art will understand that any range formed by any of the explicitly disclosed lower and upper limits is expressly included herein.

[0091] Thus, the lower limit for the amount of particles of latex polymer (a) can be 50% by weight, or 55% by weight, or 58% by weight, or 60% by weight, or 62% by weight, or 63% by weight, or 64% by weight, or 65% by weight, or 66% by weight, or 67% by weight, or 68% by weight, or 69% by weight, or 70% by weight, based on the total weight of latex particles in the composition. The upper limit for the amount of particles of latex polymer (a) can be 99% by weight, or 98% by weight, or 97% by weight, or 96% by weight, or 95% by weight, or 94% by weight, or 93% by weight, or 92% by weight, or 91% by weight, or 90% by weight, or 89% by weight, or 88% by weight, or 87% by weight, or 86% by weight, or 85% by weight, or 84% by weight, or 83% by weight, or 82% by weight, or 81% by weight, or 80% by weight, based on the total weight of the latex particles in the composition. The lower limit of the amount of particles of the second latex polymer (b) can be 1%, or 1%, or 1%, or 1%, or 5%, or 6%, or 7%, or 8%, or 9%, or 10%, or 11%, or 12%, or 13%, or 14%, or 15%, or 16%, or 17%, or 18%, or 19%, or 20% by weight based on the total weight of the latex particles in the composition. The upper limit of the amount of particles of the second latex polymer (b) can be 50%, or 45%, or 42%, or 40%, or 38%, or 37%, or 36%, or 35%, or 34%, or 33%, or 32%, or 31%, or 30% by weight based on the total weight of the latex particles in the composition. One of ordinary skill in the art will understand that any range formed by any of the explicitly disclosed lower and upper limits is expressly encompassed herein.

[0092] Compounded latex composition for the production of dip-molded articles: The polymer latexes used to make elastomeric films are particularly suitable for the dip molding process. Thus, the polymer latexes are compounded to produce a curable polymer latex compound composition that can be used directly in the dip molding process. For dipping to make thin disposable gloves, it is desirable to adjust the pH of the compounded polymer latex composition by a pH adjuster to a range of pH 7 to 13, preferably 10.5 to 13, more preferably 11 to 12, in order to obtain reproducible good physical film properties. For making unsupported and / or supported reusable gloves, it is desirable to adjust the pH of the compounded polymer latex composition by a pH adjuster to a range of pH 8 to 10, preferably 8.5 to 9.5. The compounded polymer latex composition comprises the polymer latex of the present invention, optionally a pH adjuster, preferably ammonia or an alkali hydroxide, and optionally an antioxidant, a pigment, TiO 2 The compositions contain the usual additives used in these compositions selected from fillers and dispersing agents.

[0093] Alternatively, instead of blending the polymer latex of the present invention, a polymer latex containing the latex polymer (a) as defined above may be blended in the same manner as described above, and during or after the blending step, a polymer latex containing the oxirane-functional latex polymer (b) as defined above may be added to provide the blended latex composition of the present invention. Also, a polymer latex containing the oxirane-functional latex polymer (b) as defined above may be blended in the same manner as described above, and during or after the blending step, a polymer latex (a) as defined above may be added to provide the blended latex composition of the present invention. Of course, all variations in the latex polymer (a), the oxirane-functional latex polymer (b), and their relative amounts based on the total amount of latex polymers as described above may be used.

[0094] However, it is particularly advantageous that sulfur vulcanization systems and crosslinkers, and optionally ZnO, can be avoided entirely, while the polymer latex compounds used according to the present invention are still capable of curing to provide dip-molded articles having the necessary tensile and self-healing properties to make them repairable and / or recyclable.

[0095] How to make a dip molded part: In the method of making a dip-molded latex article according to the present invention, a clean mold having the desired shape of the final article is first immersed in a coagulant bath containing a solution of a metal salt. The coagulant is usually used as a solution in water, alcohol or a mixture thereof. As specific examples of coagulants, the metal salts can be metal halides such as calcium chloride, magnesium chloride, barium chloride, zinc chloride and aluminum chloride; metal nitrates such as calcium nitrate, barium nitrate and zinc nitrate; metal sulfates such as calcium sulfate, magnesium sulfate and aluminum sulfate; and acetates such as calcium acetate, barium acetate and zinc acetate. Most preferred are calcium chloride and calcium nitrate. The coagulant solution may contain additives to improve the wetting behavior of the former.

[0096] The mold is then removed from the bath and optionally dried. The treated mold is then immersed in a compounded latex composition according to the invention, which causes a thin film of latex to solidify on the mold surface. It is known in the art that the thickness of such an immersed film can be influenced by the concentration of the compounded latex and / or the length of time the salt-coated mold is in contact with the compounded latex. Alternatively, it is also possible to obtain a latex film by performing multiple immersion steps, in particular two immersion steps, one after the other.

[0097] The former is then removed from the latex composition and optionally immersed in a water bath, for example to extract polar components from the composition and to wash the coagulated latex film.

[0098] The latex coated former is then optionally dried at a temperature below 80°C.

[0099] Finally, the latex coated mold is heat treated at temperatures between 40 and 180 °C to obtain the desired mechanical properties of the final film product. The final latex film is then removed from the mold. The duration of the heat treatment depends on the temperature and is typically between 1 and 60 minutes. The higher the temperature, the shorter the treatment time required.

[0100] The present inventors have surprisingly discovered that when using the polymer latex of the present invention, the dip molding process can be carried out more economically. In particular, it has been discovered that the duration between forming the compounded latex composition according to the present invention and carrying out the dip molding step (aging period) can be significantly reduced to 180 minutes or less, as compared to compounds made from standard latexes, which require aging periods well in excess of 180 minutes.

[0101] Furthermore, the inventors have found that the temperature of the heat treatment step can be significantly reduced within the range of 40° C. to less than 120° C. without compromising the mechanical properties of the final dip-molded article. Conventional latexes require temperatures of 120° C. or higher to achieve the desired mechanical properties. Thus, when using the polymer latexes of the present invention, the dip-molding process becomes less time-consuming, less energy-intensive, and more economical.

[0102] Therefore, according to the invention, it is preferred that - In the compounding step (a) (i) the polymer latex according to the present invention is formulated without adding ZnO by adjusting the pH to the range of 10.5-13, preferably 11-12; or (ii) a polymer latex comprising particles of latex polymer (a) as defined above is formulated by adjusting the pH to the range of 10.5 to 13, preferably 11 to 12, without the addition of ZnO, followed by the addition of preformed particles of latex polymer (b) as defined above; or (iii) a polymer latex containing particles of polymer (b) as defined above is formulated by adjusting the pH to the range of 10.5 to 13, preferably 11 to 12, without the addition of ZnO, followed by the addition of preformed particles of latex polymer (a) as defined above; and The compounded latex composition obtained thereby is free of sulfur vulcanizing agents and sulfur vulcanization accelerators and ZnO, and is aged for less than 180 minutes, preferably from 10 minutes to 150 minutes, more preferably from 20 minutes to 120 minutes, and most preferably from 30 minutes to 90 minutes, before being used in the immersion step d); and / or In the heat treatment step h), the latex-coated mold is heat treated at a temperature of 40°C to 120°C, preferably 60°C to 100°C, more preferably 70°C to 90°C.

[0103] The final heat-treated polymer latex film has a tensile strength of at least about 7 MPa and an elongation at break of at least about 300%, preferably a tensile strength of at least about 10 MPa and an elongation at break of at least about 350%, more preferably a tensile strength of at least about 15 MPa and an elongation at break of at least about 400%, and even more preferably a tensile strength of at least about 20 MPa and an elongation at break of at least about 500%. These mechanical properties were measured according to ISO 37-77 (5th edition 2011-12-150).

[0104] This method can be used for any latex article that can be made by dip molding processes known in the art.

[0105] The articles used in the repair or recycling methods according to the invention may be selected from health care devices formed from or including elastomeric films, such as surgical gloves, examination gloves, condoms, catheters, or all different kinds of industrial and household gloves.

[0106] Method for repairing an elastomeric film or an article including an elastomeric film The items formed from the elastomeric film are collected, sorted, and optionally sterilized for handling purposes. Items that are damaged but not to the point of being unable to be reused are separated, and the damaged surfaces are optionally further cleaned. This cleaning can be by washing with hydrogen peroxide or other sterilizing liquid, or by passing under a carbon dioxide air stream or UV light to ensure that no pathogens are present. At the location of the damage, the surfaces of the damaged film that were separated from each other are brought together so that they are in contact with each other (e.g., if there is a hole, the edges of the hole are brought into contact), the surfaces are heated so that the elastomeric film softens, the surfaces are sealed together to repair the damage, and then the surfaces are cooled, resulting in a repaired or self-healed surface. The heating may be performed while applying pressure to the contact areas of the damaged surfaces.

[0107] Method for recycling an elastomeric film or an article containing said elastomeric film The elastomeric materials, such as gloves, are collected and, if necessary, sorted so that nitrile-containing materials are collected together while other materials are discarded or sent to an alternative recycling or reprocessing facility. The collected materials are then washed and decontaminated as necessary, similar to what is done for the repair / self-healing process. The materials are then ground to a particle size of 2 mm or less average diameter, preferably 1 mm or less average diameter, and ideally to a particle size in the range of 0.15-0.75, more preferably 0.2-0.3 average diameter. The grinding or grinding process can be carried out below room temperature or under cold conditions to allow for easy processing and to maintain the material as particles before further processing. Cold conditions avoid recombination of particles until required. The materials can be stored at room temperature or under conditions that avoid recombination of particles until required. The materials may be further ground before being fed to a blender where the materials are blended with other materials (e.g., particles of virgin elastomeric material, and conventional processing aids and additives). In the absence of a blending step, the material is fed directly into a heat treatment system where the particles / crumbs are hot pressed, two-roll milled, calendered, or extruded under pressure and heat, i.e., at temperatures above 40° C., to impart flow into the material until it reaches its glass transition temperature, at which stage it can also be formed into the required final shape. After this, the material is cooled, if necessary, in a mold or as part of the extrusion process to produce the final product formed from the recycled material.

[0108] The invention will now be further described with reference to the following examples.

[0109] Determination of physical parameters: The dispersions were characterized by measuring the total solids content (TSC), pH value, gel content, viscosity (Brookfield LVT) and z-average particle size. Additionally, the final films were tested for tensile properties.

[0110] Determination of Total Solids Content (TSC): The determination of total solids was based on gravimetric method. 1-2 g of dispersion was placed in a weighed aluminum dish on an analytical balance. The dish was stored at 120°C in a circulating air oven for 1 hour until a constant mass was reached. After cooling to room temperature, the final weight was remeasured. The solids content was calculated as follows:

number

[0111] Measurement of pH value: The pH value was determined according to DIN ISO 976. After applying a two-point calibration with a buffer solution, the electrode of a Schott CG840 pH meter was immersed in the dispersion at 23° C. and the constant value on the display was recorded as the pH value.

[0112] Viscosity measurement: Latex viscosity was measured at 23°C using a Brookfield LVT viscometer. Approximately 220 ml of liquid (without air bubbles) was filled into a 250 ml beaker and the viscometer spindle was immersed up to the mark on the spindle. The viscometer was then switched on and the values ​​recorded after approximately 1 minute until they became constant. The viscosity range determines the choice of spindle and rotation speed and the factors in the recorded values ​​for calculating the viscosity. Information on the spindle and revolutions per minute used is given in brackets for Examples 1, 2 and 8.

[0113] Measurement of particle size (PS): The z-average particle size was measured using dynamic light scattering with a Malvern Zetasizer Nano S (ZEN1600). The latex sample was diluted with deionized water to the turbidity level specified in the manual and transferred to a test cuvette. The cuvette was gently mixed to homogenize the sample and the cuvette was placed in the measurement instrument. The value was recorded as the z-average particle size generated by the software.

[0114] Dipping film preparation: Nitrile latex with or without compounding materials of the desired pH value was stirred at room temperature for 3 hours and then immersed in coagulant as follows: A ceramic spade was washed with a stone sieve and then thoroughly rinsed with deionized water before being dried in an air circulating oven set at 65-70°C (spade temperature, 55-60°C) until dry. A solution of coagulant was prepared by dissolving calcium nitrate (18% by weight) and calcium carbonate (2% by weight) in deionized water. The dry spade was then immersed in a salt solution, removed, and then dried in an air circulating oven set at 70-75°C (spade temperature, 60-65°C) until dry. The salt-coated spade was then immersed in the desired compounded latex (having a total solids content of 18% by weight and aged at room temperature for 24 hours after compounding) for a dwell time of 5 seconds, after which it was removed and the latex-coated spade was placed in an air circulating oven set at 100°C for 1 minute to gel the film.

[0115] The thus gelled film was then washed for 1 minute in a tank of deionized water set at 50-60°C, followed by curing for 20 minutes in an air circulating oven set at 120°C, after which the thus cured / vulcanized film was cooled and removed from the spade and aged for 22 hours in an air circulating oven set at 100°C. Finally, the cured glove was peeled off the spade by hand and a typical dry film thickness was 0.056-0.066 mm. Gloves prepared from the above latex were tested for their tensile strength properties and stress relaxation behavior.

[0116] Measurement of tensile strength properties of glove samples: The tensile properties of the vulcanized or regenerated gloves were tested according to ISO 37-77 (5th edition 2011-12-15). Dumbbell specimens were cut from gloves prepared from each latex compound using an ISO 37-2 type cutter (narrow width = 4 mm, narrow length = 25 mm, total length = 75 mm, dumbbell thickness is shown in the results table) and tested with a Hounsfield HK10KS tensile meter equipped with an H500LC extensometer at an extension rate of 500 mm / min.

[0117] Preparation of recycled glove film: Specimens for tensile testing were prepared by recombining cut-up samples of the dipped film made from the original compounded latex, the small piece mixture was placed between two polished steel plates and then hot pressed at 13.8 MPa (2000 psi) for the time period specified in each example (typically 5 minutes) and at the temperature specified in each example (typically 100, 120, 150 or 180°C), after which it was cooled to room temperature and then dumbbell shaped specimens were cut out using a cutter as specified in ISO 37-77 (5th Edition, 2011-12-15), ISO 37-2 type die cutter.

[0118] Measurement of stress relaxation properties: The stress relaxation properties of the elastomeric films were performed on dumbbell specimens cut from gloves prepared from each latex compound using an ASTM D412 Type C cutter (narrow width = 6 mm, narrow length = 33 mm, total length = 115 mm, dumbbell thicknesses are given in the results table). Tests were performed on a DMA Q800 Dynamic Mechanical Analyzer supplied by TA Instruments, which was operated in the "stress relaxation mode", i.e., surface tension mode, in which the specimens were strained to a value of 1% and the initial stress value was recorded (G 0 ) The stress values ​​were then recorded as a function of the time the sample was held at 1% strain (G t ).

[0119] In the examples, the following abbreviations are used: BA = n-Butyl acrylate MAA = methacrylic acid Bd = butadiene ACN = acrylonitrile GMA = glycidyl methacrylate tDDM = tert-dodecyl mercaptan Na 4 EDTA = tetrasodium salt of ethylenediaminetetraacetic acid tBHP = tert-butyl hydroperoxide TSC = Total Solids Content PS = particle size ZnO = zinc oxide ZDEC = zinc diethyldithiocarbamate

[0120] Below, all parts and percentages are by weight unless otherwise stated. EXAMPLES

[0121] Example 1: Preparation of Carboxylated Nitrile Latex An autoclave purged with nitrogen was charged with 2 parts by weight of oxirane-free seed latex (average particle size 36 nm) and 80 parts by weight of water (based on 100 parts by weight of monomers containing the seed latex) and heated to 30° C. Then, 0.01 parts by weight of Na dissolved in 2 parts by weight of water was added. 4 EDTA and 0.005 parts by weight of Bruggolite® FF6 were added, followed by 0.08 parts by weight of sodium persulfate dissolved in 2 parts by weight of water. Monomers (35 parts by weight of acrylonitrile, 58 parts by weight of butadiene, 5 parts by weight of methacrylic acid) were then added over 4 hours along with 0.6 parts by weight of tDDM. Over 10 hours, 2.2 parts by weight of sodium dodecylbenzenesulfonate, 0.2 parts by weight of tetrasodium pyrophosphate, and 22 parts by weight of water were added. A coactivator feed of 0.13 parts by weight of Bruggolite® FF6 in 8 parts by weight of water was added over 9 hours. The temperature was maintained at 30° C. until 95% conversion and a total solids content of 45%. The polymerization was briefly stopped by the addition of 0.08 parts by weight of a 5% aqueous solution of diethylhydroxylamine. The pH was adjusted to 7.5 with potassium hydroxide (5% aqueous solution) and residual monomer was removed by vacuum distillation at 60° C. 0.5 parts by weight of Wingstay L type antioxidant (60% dispersion in water) was added to the raw latex and the pH was adjusted to 8.2 by the addition of a 5% aqueous solution of potassium hydroxide.

[0122] For Example 1, the following characterization results were obtained: TSC=44.9wt% pH=8.2 Viscosity=38mPas(1 / 60) Particle size, P z =121nm

[0123] Example 2: Preparation of Oxirane-Functional Latex A nitrogen purged autoclave was charged with 2.0 parts by weight of diphenyl oxide disulfonate dissolved in 185 parts by weight of water per 100 parts by weight of monomer and heated to a temperature of 70° C. 0.1 parts by weight of tDDM and 0.05 parts by weight of Na4EDTA were added to the initial charge along with 0.7 parts by weight of ammonium peroxodisulfate (12% solution in water) added in portionwise addition. Then, a solution of 45.4 parts by weight of butadiene, 14.6 parts by weight of acrylonitrile, and 5.0 parts by weight of diphenyl oxide disulfonate dissolved in 50 parts by weight of water was added over 6.5 hours. The addition of 40 parts by weight of GMA was started after 1 hour and added over 6.5 hours. After the addition of the above monomers, the temperature was maintained at 70° C. The polymerization was maintained to 99% conversion. The reaction mixture was cooled to room temperature and sieved through a filter screen (90 μm).

[0124] For Example 2, the following characterization results were obtained: TSC=37.7wt% pH=7.1 Viscosity=15mPas(1 / 60) Particle size, P z =39nm

[0125] Example 3: (Comparison) A portion of the oxirane-free XNBR latex of Example 1 was adjusted to a pH value of 10 using an aqueous solution of potassium hydroxide and compounded with 1 phr of zinc oxide, 1 phr of titanium dioxide, 0.8 phr of sulfur, and 0.7 phr of ZDEC. The mixture was then adjusted to a concentration of 18 wt. % solids and stirred for 3 hours.

[0126] Example 4: To a portion of Example 1 (an oxirane-free XNBR latex) was added a portion of Example 2 (an oxirane-functional latex) such that the blend ratio was 90:10 by wet weight of Example 1:Example 2.

[0127] Preparation of dip-coated samples: Example 5: (Comparison) The dried, salt-coated spades were then immersed in the compounded latex solution of Example 3 for a 5 second dwell time, followed by gelling at 100°C for 1 minute, washing with deionized water (in a tank set at 50-60°C) for 1 minute, and then drying and curing / vulcanization in an air circulating oven set at 120°C for 20 minutes to ensure complete drying and crosslinking.

[0128] Example 6: The blend of Example 4 was adjusted to a pH value of 10 using potassium hydroxide solution and the blend was stirred for 3 hours after which a dry salt coated spade was immersed and treated according to the procedure given in Example 5.

[0129] Example 7: The blend of Example 4 was adjusted to a pH value of 10.0 using a solution of potassium hydroxide and combined with zinc oxide (1 phr), and the blend was then stirred for 3 hours before immersing a dry salt-coated spade and treating according to the procedure given in Example 5.

[0130] Example 8: The blend of Example 4 was adjusted to a pH value of 11.5 using potassium hydroxide solution, and the blend was then stirred for 3 hours before immersing a dry salt-coated spade and treating according to the procedure set forth in Example 5.

[0131] Stress relaxation experiment A number of samples were tested for stress relaxation as a function of time, the samples being prepared according to the "Preparation of Immersed Films" section above.

[0132] Example 9: The dried and cured film obtained from Example 5 (comparative) was then cut into multiple dumbbell-shaped specimens (length 25±0.8 mm, width 6 mm, thickness 0.056-0.066 mm) using a preform cutter (see FIG. 1).

[0133] The dumbbells were then clamped in the jaws of a DMA Q800 dynamic mechanical analyzer supplied by TA Instruments, and the specimens were allowed to equilibrate at the test temperature for 5 minutes before being strained to 1% to obtain the initial stress value G. 0 The strain was maintained at 1% and then measured as a function of time (G t ) and the stress values ​​were monitored for typically 1200 seconds (see FIG. 3).

[0134] Typical test temperatures selected were 100, 120, 150 and 180°C. Stress relaxation is defined as Stress relaxation = G t / G 0 The results obtained in Example 9 are shown in Figure 4, with the thickness of the test specimens shown in brackets on the plot. t / G 0 It should be noted that the graph is drawn at e = 1 / e (= 0.63). Reference:http: / / web.mit.edu / course / 3 / 3.11 / www / modules / visco.pdfHYPERLINK "http: / / web.mit.edu / course / 3 / 3.11 / www / modules / visco.pdf" The time elapsed until the stress reached the 1 / e value is shown in Table 1 below. The stress relaxation values ​​at 120°C and 100°C did not fall below the 1 / e value.

[0135] Example 10: This was an exact repeat of Example 9, except that Example 6 was substituted for Example 5. The results are shown in FIG. The results of the stress relaxation experiment are shown in Figure 5 and Table 3. The data show that the 100°C data did not fall below the 1 / e value. Furthermore, in contrast to Example 9, the data followed an increasing trend with temperature.

[0136] Example 11: This was an exact repeat of Example 9, except that Example 8 was substituted for Example 5. The results are shown in FIG. The data showed that for the zinc oxide-free elastomer systems formulated at pH 11.5, the rate of change of stress relaxation values ​​decreased in the order 180>>150>120>100 °C, with all data sets reaching the 1 / e value.

[0137] Table 1 [Table 1]

[0138] This data shows the reworkability of the elastomeric film made according to the present invention. It is believed that this data can be interpreted as the crosslinks being broken in the examples of the present invention compared to the comparative examples, and then the polymer system can move on a microscopic scale to relieve the applied stress. This effect is more pronounced at higher temperatures. The elastomeric film made without ZnO also shows this effect at lower temperatures. This result is evidence of the self-healing properties of the elastomeric film described herein.

[0139] Recycling of elastomer films Several elastomeric films were recycled and the tensile strength values ​​of the original elastomeric films were compared to the tensile strength values ​​of the recycled films.

[0140] Examples 12: (Comparison) and 13-15 Specimens for tensile testing were cut from films prepared according to Examples 5-8 using a Type 2 dumbbell cutter die as specified in ISO 37 (5th edition, 2011-12-15). The dumbbell ends were placed in the jaws of a Hounsfield HK10KS tensile meter fitted with an H500LC extensometer and subjected to a strain rate of 500 mm / min. Values ​​of stress were automatically reported by the instrument software as modulus values ​​at given strains (typically 100, 300 and 500% strain). The results are reported in Table 2.

[0141] Table 2 [Table 2]

[0142] Recycling of elastomer films A recyclable elastomeric film is defined herein as one that, when cut into pieces, can be reassembled upon exposure of the pieces to low temperatures, typically below 100°C for 1 minute or preferably at 80°C for 5 minutes, under an applied pressure of 13.8 MPa (2000 psi), which then demonstrates an elongation to break of greater than 90% and a tensile strength of greater than 1.5 MPa according to the following test procedure.

[0143] Example 16: (Comparison) Specimens for tensile testing were prepared by rejoining cut samples of dipped films made from compounded latex of Example 5 (comparative) (the original film was prepared according to the procedure of Example 5), annealing the mixture of small pieces between two polished steel plates, followed by hot pressing at 13.8 MPa (2000 psi) for 1 minute and 100°C, cooling to room temperature, and then cutting dumbbell-shaped specimens using a type 2 die cutter as specified in ISO 37 (5th edition, 2011-12-15). Both ends of the dumbbell were placed in the jaws of a Hounsfield HK10KS tensile meter fitted with an H500LC extensometer and subjected to a strain rate of 500 mm / min. Stress values ​​were automatically reported by the instrument software as modulus values ​​at given strains (typically 100, 300 and 500% strain). The results are reported in Table 3.

[0144] Example 17: This was an exact repeat of Example 16, except that Example 6 was substituted for Example 5. The results are reported in Table 3.

[0145] Example 18: (Comparison) This was an exact repeat of Example 16, except that the dumbbell samples were annealed at 13.8 MPa (2000 psi) and 80° C. for 5 minutes, cooled to room temperature, and both ends of the dumbbell were placed in the jaws of a Hounsfield HK10KS tensile meter fitted with an H500LC extensometer and subjected to a strain rate of 500 mm / min. Stress values ​​were automatically reported by the instrument software as modulus values ​​at given strains (typically 100, 300 and 500% strain). The results are reported in Table 3.

[0146] Example 19: This was an exact repeat of Example 18, except that Example 6 was replaced with Example 3. The results are shown in Table 5.

[0147] Example 20: This was an exact repeat of Example 18, except that Example 8 was substituted for Example 5. The results are shown in Table 3.

[0148] Table 3 [Table 3] where F = specimen failure / breakage.

[0149] Table 3 shows that both comparative examples (16 and 18) failed (dumbbell break) at less than 100% strain and all exhibited tensile strengths less than 1.5 MPa and elongations at break less than 90 strain. Thus, the comparative examples did not demonstrate the ability to self-heal at the annealing temperatures used.

[0150] Examples 17 and 19 (no zinc oxide, pH 10.0) exhibited tensile strengths of over 3 MPa and elongations at break of over 200% after annealing at 100° C. for 1 minute or at 80° C. for 5 minutes, i.e., the films produced from these dipped gloves were recyclable films.

[0151] Example 20 demonstrated that increasing the pH to 11.5 increased the tensile strength and modulus while decreasing the elongation to break to 139%. Thus, the film produced from this dipped glove was a recyclable film.

[0152] Measurement of tensile properties after repair of elastomeric films: The nitrile latex with or without the compounding materials at the desired pH value was stirred at room temperature for 3 hours and then cast onto a Petri dish. The cast latex film on the surface of the Petri dish was then placed in a circulating air oven at 25° C. for 3 days. The resulting film was then annealed in an air circulating oven at 90° C. for 24 hours to ensure complete drying and any desired crosslinking had occurred.

[0153] The cast film was carefully removed from the glass Petri dish and cut into dumbbell shapes using a 3 mm "D" cutter (see FIG. 1). One dumbbell was left uncut (to act as a control sample) and the other was cut in half at the midpoint of the dumbbell (see FIG. 2). Marks were placed on the top surface of each cut half for reference, if necessary. The freshly cut surfaces of the dumbbell were then immediately pressed together for 60 seconds (see FIG. 3), the cut pieces were placed on a glass plate, and these rejoined pieces on the glass plate were then placed in an air circulating oven at 180° C. for 30 minutes (to simulate a non-pressurized dry rubber heat treatment process). The freshly cut surfaces of the dumbbell were also immediately pressed together for 60 seconds, pressure was maintained by placing the "tabs" of a wooden fastener on the rejoined pieces, and subsequently heat treated in an oven at 180° C. for 30 minutes. This was intended to simulate a low pressure dry rubber hot pressing process.

[0154] Example 21: (Comparison) A portion of the oxirane-free XNBR latex of Example 1 was adjusted to a pH value of 10 using an aqueous solution of potassium hydroxide and compounded with 1 phr of zinc oxide, 0.8 phr of sulfur, and 0.7 phr of ZDEC. The compound was then stirred for 3 hours and then cast onto a glass Petri dish and dried at room temperature (25° C.) for 3 days. The resulting film was removed from the glass Petri dish and annealed in a 90° C. oven for 24 hours to ensure complete drying and crosslinking.

[0155] Here, a film that has been cut into two halves and then the two halves held together is said to be self-healing if it is able to exhibit tensile strength when the two halves thus joined are subsequently separated.

[0156] The two dumbbell samples (cut and rejoined, and uncut) were then subjected to stress-strain analysis to measure the tensile properties of the elastomer before and after it was cut and rejoined; i.e., to measure the degree of self-healing of the cut film. Tensile properties were tested according to ASTM D412-06a using 3 mm type "D" dumbbell specimens with typical film thicknesses of 1.0-1.4 mm ± 0.01 cut from the cast latex film for tensile testing. Film thickness (mm) was measured using a thickness gauge (Model Studenroth, Sylvac, Type 12.5 mm / 0.001).

[0157] Tensile stress-elongation curves were recorded using a ZwickRoell Z005TN Proline tensometer equipped with a long stroke extensometer. Samples were elongated at a rate of 500 mm / min at a temperature of 23 ± 2 °C and a relative humidity of 50 ± 5%. The tensile strength data reported here correspond to the maximum tensile stress observed while stretching the dumbbells to break. The ultimate elongation values ​​reported correspond to the elongation at which break occurred. The elastic modulus values ​​reported, M 100 , M 300 and M. 500 corresponds to the stress required to reach an elongation of 100%, 300% or 500% of the original length, respectively.

[0158] Preparation of dumbbell specimens and comparison of uncut and self-healing specimens: Example 22: The dried and cured film from Example 21 was then cut into multiple dumbbell samples using a "D" cutter (see FIG. 1). One dumbbell remained uncut, while the other was cut in half using a sharp blade applied to the narrow part of the dumbbell (see FIG. 2). The cut dumbbell was then immediately rejoined by pressing the cut surfaces together and manually for 60 seconds (see FIG. 3). The dumbbell thus rejoined was then annealed for 30 minutes in an air circulating oven maintained at 180° C. The self-healing dumbbell was then subjected to tensile testing to measure the extent of recovery of tensile properties by comparison with the results obtained for uncut dumbbells obtained from the same cast film. The results are shown in Table 4 and FIG.

[0159] Example 23: To the dispensed Example 1 (oxirane-free XNBR latex), dispensed Example 2 (oxirane-functional latex) was added such that the blend ratio was 90:10 by wet weight of Example 1:Example 2. The blend was adjusted to a pH value of 10 using potassium hydroxide solution and stirred for 3 hours before being cast into a glass Petri dish and dried at room temperature (25° C.) for 3 days. The resulting film was removed from the glass Petri dish and annealed in a 90° C. oven for 24 hours to ensure complete drying and crosslinking. The film was then cut into dumbbells and tested as in Example 22. The results are shown in Table 4 and FIG.

[0160] Example 24: This was a repeat of Example 23, except that 1 phr of zinc oxide was added to the latex at pH 10 and stirred for 3 hours before casting. The film was then cut into dumbbells and tested as in Example 22. The results are shown in Table 4 and FIG.

[0161] Example 25: This was a repeat of Example 23, except that the pH value was adjusted to 11.5. The films were then cut into dumbbells and tested as in Example 22. The results are shown in Table 4 and FIG.

[0162] Table 4 [Table 4]

[0163] Example 26: To a portion of Example 1 (an oxirane-free XNBR latex) was added a portion of Example 2 (an oxirane-functional latex) such that the blend ratio was 90:10 by wet weight of Example 1:Example 2.

[0164] The blend was adjusted to a pH value of 5 using aqueous potassium hydroxide, stirred for 3 hours, and then cast onto a glass Petri dish and dried at room temperature (25°C) for 3 days. The resulting film was removed from the glass plate and annealed in an oven at 90°C for 24 hours to ensure complete drying and cross-linking. The dried and cured film was then cut into multiple dumbbell samples using a "D" cutter. One dumbbell remained uncut while the other was cut in half using a sharp blade applied to the narrow part of the dumbbell. The cut dumbbells were then immediately rejoined by holding the cut surfaces together and manually pressing for 60 seconds, following which the prongs of a wooden clothespin were applied to maintain intimate contact of the two surfaces and the rejoined dumbbells were annealed for 30 minutes in an air circulating oven maintained at 180°C. The results are shown in Table 5.

[0165] Example 27: This was a repeat of Example 26, except that the pH value was adjusted to 10. The results are shown in Table 5.

[0166] Example 28: This was a repeat of Example 26, except that the pH was adjusted to 11. The results are shown in Table 5.

[0167] Example 29: This was a repeat of Example 26, except that the pH was adjusted to 11.5. The results are shown in Table 5.

[0168] Table 5 [Table 5]

Claims

1. A method for recycling an elastomeric film or an article comprising said elastomeric film, comprising cutting, shredding or grinding said elastomeric film or article to form particles of elastomer, optionally blending the resulting particles with particles of virgin elastomer, and exposing the particles to a pressure of 1-20 MPa and a temperature of 40° C.-200° C. to form a recycled film or article: wherein the elastomeric film is made from a polymer latex comprising: (a) Particles of a carboxylated conjugated diene nitrile latex polymer (a) obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising: 15-95% by weight of conjugated dienes; 1 to 80% by weight of monomers chosen from ethylenically unsaturated nitrile compounds; 0.05 to 10% by weight of ethylenically unsaturated carboxylic acids and / or salts thereof; 0 to 50% by weight of vinyl aromatic monomers; 0 to 65% by weight of alkyl esters of ethylenically unsaturated acids; Weight percentages are based on total monomers in the mixture. In combination or in collaboration, (b) particles of a latex polymer (b) containing at least one oxirane functional group; Here, the monomer composition of the latex polymer (a) is different from the monomer composition of the latex polymer (b).

2. The process according to claim 1, wherein the temperature is between 60°C and 200°C and / or the pressure is between 12 and 15 MPa.

3. The method according to any one of claims 1 to 2, wherein a) the conjugated diene is selected from butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, myrcene, ocimene, farnacene, and combinations thereof; b) the ethylenically unsaturated nitrile compound is selected from (meth)acrylonitrile, α-cyanoethyl acrylonitrile, fumaronitrile, α-chloronitrile, and combinations thereof; c) the ethylenically unsaturated carboxylic acid and its salt are selected from the following: monocarboxylic acids and their salts; - ethylenically unsaturated polycarboxylic acids, their anhydrides and their salts; - partial esters of polycarboxylic acids and their salts; d) the vinyl aromatic monomer is selected from styrene, alpha-methylstyrene, vinyltoluene, and combinations thereof; e) the alkyl ester of an ethylenically unsaturated acid is selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl methacylate, n-butyl (meth)acrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, and combinations thereof; The mixture of ethylenically unsaturated monomers for the latex polymer (I) optionally includes ethylenically unsaturated monomers selected from: f) hydroxyalkyl esters of ethylenically unsaturated acids; g) amides of ethylenically unsaturated acids; h) vinyl carboxylate; i) a monomer having at least two ethylenically unsaturated groups; j) ethylenically unsaturated silanes; and combinations thereof.

4. The method of any one of claims 1 to 3, wherein the mixture of ethylenically unsaturated monomers for the latex polymer (a) comprises: 20-95% by weight of conjugated dienes; - 1 to 60% by weight of monomers chosen from ethylenically unsaturated nitrile compounds; 0 to 40% by weight of vinyl aromatic monomers; - C 1 ~C 8 Alkyl (meth)acrylate 0 to 25% by weight; 0.05 to 7% by weight of ethylenically unsaturated acids; 0 to 10% by weight of vinyl esters; - 0 to 10% by weight of ethylenically unsaturated compounds containing silane, amide and / or N-methylolamide groups; The weight percentages are based on total monomers in the mixture.

5. The method of any one of claims 1 to 4, wherein the oxirane-functional latex polymer (b) comprises structural units derived from ethylenically unsaturated oxirane-functional monomers in an amount of from 1 to 80 weight percent, based on the total weight of monomers of the oxirane-functional latex particles (b).

6. The method of any one of claims 1 to 5, wherein the oxirane-functional latex polymer (b) comprises structural units derived from: (I) - 0 to 50% by weight of monomers chosen from ethylenically unsaturated nitrile compounds; - 0 to 95% by weight of vinyl aromatic monomers; 0 to 95% by weight of C 1 ~C 8 Alkyl (meth)acrylate; - 0 to 10% by weight of an ethylenically unsaturated acid; - 0 to 10% by weight of ethylenically unsaturated compounds containing silane, sulfonate, sulfonic acid, amide and / or N-methylolamide groups; 0 to 50% by weight of vinyl carboxylates; - 1 to 80% by weight of structural units derived from ethylenically unsaturated oxirane-functional monomers; or (II) - 2 to 95% by weight of conjugated dienes; - 1 to 50% by weight of monomers chosen from ethylenically unsaturated nitrile compounds; - 0 to 95% by weight of vinyl aromatic monomers; 0 to 95% by weight of C 1 ~C 8 Alkyl (meth)acrylate; - 0 to 10% by weight of an ethylenically unsaturated acid; - 0 to 10% by weight of ethylenically unsaturated compounds containing silane, sulfonate, sulfonic acid, amide and / or N-methylolamide groups; - 1 to 80% by weight of structural units derived from ethylenically unsaturated oxirane-functional monomers.

7. The method according to any one of claims 1 to 6, wherein in preparing the polymer latex, (i) a mixture of ethylenically unsaturated monomers for the latex polymer (a) is polymerized in the presence of particles of the oxirane-functional latex polymer (b) in a free radical emulsion polymerization; or (ii) a polymer latex comprising particles of latex polymer (a) and a polymer latex comprising particles of latex polymer (b) are preformed and then both latexes are combined; or (iii) A mixture of ethylenically unsaturated monomers for latex polymer (a) is polymerized in the presence of particles of oxirane functional latex polymer (b) in a free radical emulsion polymerization to form a first polymer latex, a second polymer latex comprising particles of latex polymer (b) is preformed, and subsequently both latices are combined, wherein the latex comprising oxirane functional latex particles (b) to form the first polymer latex and the second polymer latex comprising particles of latex polymer (b) are the same or different.

8. 8. The method of any one of claims 1 to 7, wherein the z-average particle size of the oxirane-functional latex particles (b) is from 5 to 90 nm as measured by dynamic light scattering with a Malvern Zetasizer Nano S (ZEN1600).

9. The method of any one of claims 1 to 8, wherein the elastomeric film or the article comprising the elastomeric film is made from a compounded latex composition comprising a polymer latex as defined in any one of claims 1 and 3 to 8, which does not contain a sulfur vulcanizing agent and an accelerator for sulfur vulcanization, and optionally undergoes one or more treatments of the following characteristics: - the compounded latex composition does not contain ZnO; The pH of the compounded latex composition is 10.5-13.

10. 10. The method of claim 9, wherein the article is made by a dip molding process comprising: a) providing a compounded latex composition according to claim 9; b) immersing a form having the desired shape of the final article in a coagulant bath containing a solution of metal salts; c) removing the form from the coagulant bath and optionally drying the form; d) immersing the former treated in steps b) and c) into the compounded latex composition of step a); e) coagulating the latex film on the surface of the mold; f) removing the latex coated former from the compounded latex composition and optionally immersing the latex coated former in a water bath; g) Optionally drying the latex coated former; h) heat treating the latex coated mold obtained from step e) or f) at a temperature of 40° C. to 180° C.; and i) Removing the latex article from the mold.

11. The method of any one of claims 1 to 10, wherein the article comprising the elastomeric film is selected from surgical gloves, examination gloves, condoms, catheters, industrial gloves, fabric-bearing gloves, and household gloves.

Citation Information

Patent Citations

  • Polymer Latex for Dip Molding Applications

    JP2019523796A

  • Method for reclaiming used-up rubber of latex

    KR1020120080753A