Moisture and oxygen barrier laminate
A laminate with an inorganic barrier and protective layer on a light-transmissive substrate maintains moisture and oxygen barrier properties post-retort and bending, addressing the deterioration issue in existing laminates.
Patent Information
- Application Number
- JP2023535498
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-13
- Filing Date
- 2021-12-23
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2041-12-23
AI Technical Summary
Barrier laminates used for food packaging deteriorate in barrier properties due to separation or tearing during retort processes or bending, necessitating a laminate that maintains excellent moisture and oxygen barrier properties under deformation.
A laminate structure comprising an inorganic barrier layer and a protective layer sequentially formed on a light-transmissive substrate, which maintains moisture and oxygen permeability after retort processes and bending tests, with specific parameters for the substrate and layers to ensure adhesion and performance.
The laminate exhibits excellent moisture and oxygen barrier properties with maintained adhesion after retort processes and bending tests, with moisture permeability of 1.00g/m²/day or less and oxygen permeability of 0.50cc/m²/day or less, even after rigorous testing.
Smart Images

Figure 0007554362000001 
Figure 0007554362000002
Abstract
Description
[Technical field]
[0001] [Cross-reference to related applications] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0004783 filed on January 13, 2021, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a laminate having moisture and oxygen barrier properties. [Background technology]
[0003] 2. Description of the Related Art Barrier laminates in which an inorganic thin film such as aluminum oxide is formed on the surface of a plastic substrate are used for packaging a variety of products such as food and electronic devices.
[0004] In particular, food packaging barrier laminates have a problem in that when they are subjected to a retort process in which food is sterilized at high temperatures or deformation such as bending, the barrier properties deteriorate due to separation or tearing between layers.
[0005] Therefore, there is a need for a laminate that can maintain excellent barrier properties even when subjected to deformation such as retort heat treatment or bending. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a barrier laminate that exhibits excellent moisture and oxygen permeability even after a retort process for sterilizing food at high temperatures and a Gelbo flex test. [Means for solving the problem]
[0007] Hereinafter, a moisture and oxygen barrier laminate according to an embodiment of the present invention will be described.
[0008] Unless otherwise defined herein, all technical and scientific terms have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. The terms used in the description of the present invention are merely for the purpose of effectively describing a specific embodiment and are not intended to limit the present invention.
[0009] As used herein, the singular forms "a," "an," and "the" include the plural forms unless the context clearly indicates otherwise.
[0010] As used herein, the meaning of "comprising" is to embody certain features, regions, constants, steps, operations, elements, components and / or ingredients, and does not exclude the presence or inclusion of other particular features, regions, constants, steps, operations, elements, components and / or groups.
[0011] Since the present invention can be modified in various ways and can have various forms, specific embodiments are described in detail below. However, this is not intended to limit the present invention to the specific disclosed embodiments, and it should be understood that the present invention includes all modifications, equivalents, and alternatives within the above-mentioned concept and technical scope.
[0012] In this specification, when the location of two parts is described using, for example, "on," "upper," "lower," "adjacent," etc., one or more other parts may be located between the two parts, unless the words "immediately" or "directly" are used.
[0013] In this specification, when a temporal relationship is described using, for example, "after," "following," "next to," "before," etc., this can also include non-consecutive relationships, unless the words "immediately" or "directly" are used.
[0014] As used herein, the term "at least one" should be understood to include all possible combinations of one or more of the associated items.
[0015] According to one embodiment of the present invention, the present invention is directed to a light-transmitting substrate having an inorganic barrier layer and a protective layer formed in sequence on one side thereof, and a moisture transmission rate (WVTR) change of 1.00 g / m 2 before and after retort treatment at a temperature of 135° C. for 1 hour. 2 The present invention provides a moisture and oxygen barrier laminate having a moisture and oxygen barrier strength of 0.1 to 100% by weight per unit area (Tmax) of 0.1 to 100% by weight per unit area (Tmax).
[0016] As a result of the inventors' continued research, it has been discovered that a moisture and oxygen barrier laminate includes an inorganic barrier layer and a protective layer formed in this order on one side of a light-transmitting substrate, and the change in moisture transmission rate (WVTR) before and after retort treatment for one hour at a temperature of 135°C is 1.00 g / m 2 *day or less, 0.80g / m 2 *day or less, 0.60g / m 2 *day or less, 0.50g / m 2 *day or less, or 0.01-0.40g / m 2 *It was confirmed that the moisture and oxygen permeability was well maintained and excellent interlayer adhesion was observed not only during the retort process, in which food is sterilized at high temperatures, but also after the Gelbo Flex test.
[0017] According to another embodiment of the present invention, a light-transmitting substrate is provided with an inorganic barrier layer and a protective layer formed in sequence on one surface of the substrate, and the change in moisture transmission rate (WVTR) before and after 50 twists using a Gelbo flex tester is 0.70 g / m 2 The laminate has a moisture and oxygen barrier property of less than 0.1*day.
[0018] The moisture and oxygen barrier laminate was subjected to 50 twists using a Gelbo flex tester, and the change in moisture transmission rate (WVTR) was 0.70 g / m 2 *day or less, 0.68g / m 2 *day or less, 0.65g / m 2 *day or less, or 0.01-0.62g / m 2In addition, by satisfying such moisture permeability, the moisture and oxygen permeability can be well maintained even after the Gelbo flex test, and excellent interlayer adhesion can be exhibited.
[0019] The moisture and oxygen barrier laminate was subjected to a retort treatment at a temperature of 135° C. for 1 hour, and the change in oxygen transmission rate (OTR) was 0.50 cc / m 2 *day or less, 0.40cc / m 2 *day or less, 0.30cc / m 2 *Day or less, or 0.01~0.25cc / m 2 *day.
[0020] The moisture and oxygen barrier laminate was subjected to 50 twists using a Gelbo flex tester, and the change in oxygen transmission rate (OTR) was 1.00 cc / m 2 *day or less, 0.90cc / m 2 *day or less, 0.80cc / m 2 *day or less, 0.70cc / m 2 *Day or less or 0.01~0.65cc / m 2 *day.
[0021] By satisfying the above-mentioned numerical ranges, the moisture and oxygen barrier laminate can maintain high moisture and oxygen permeability and exhibit excellent interlayer adhesion even after undergoing a retort process in which food is sterilized at high temperatures and a Gelbo flex test.
[0022] The change in the moisture permeability and oxygen permeability is controlled by, but is not limited to, the type of light-transmitting substrate, the in-plane retardation (Re), the shrinkage rate, or the composition of the protective layer.
[0023] The retort treatment may be carried out, for example, by using a retort evaluation device (KYUNGHAN PRS-03-IH) to perform sterilization at 135° C. for 1 hour.
[0024] The Gelbo Flex test can be performed using a Kelbo Flex Tester (model: G0005, manufacturer: IDM Instruments) according to the standard test method of ASTM F392. For example, the moisture and oxygen barrier laminate can be attached to the mandrel of the Kelbo Flex Tester, and the test settings can provide a 440 degree twisting motion in the first 90 mm of the stroke followed by a 65 mm straight horizontal motion, and the bending speed can be set to 50 cycles per minute and stroked for 50 cycles.
[0025] Furthermore, the moisture permeability before and after the retort treatment and Gelbo flex test can be measured using a moisture permeability analyzer (model name: AQUATRAN 2 WVTR Analyzer, manufacturer: Mocon) under conditions of 40°C and relative humidity of 90% according to the standard test method of ASTM F1249.
[0026] In addition, the oxygen transmission rate before and after the retort treatment and the Gelbo flex test can be measured under conditions of 23°C and 0% relative humidity in accordance with the standard test method of ASTM D3985 using an oxygen transmission rate analyzer (model name: OX-Tran 2 / 21 OTR Analyzer, manufacturer: Mocon).
[0027] The moisture and oxygen barrier laminate according to an embodiment of the present invention may have a structure including an inorganic barrier layer and a protective layer sequentially formed on one surface of a light-transmitting substrate.
[0028] The moisture and oxygen barrier laminate may have a structure including an inorganic barrier layer and a protective layer formed in that order on both sides of the light-transmitting substrate.
[0029] The light-transmitting substrate included in the moisture and oxygen barrier laminate according to an embodiment of the present invention may be a plastic film having transparency and flexibility.
[0030] The light-transmitting substrate may have a transmittance of 50% or more, 70% or more, 80% or more, or 90% or more at wavelengths of 300 nm or more.
[0031] Specifically, the light-transmitting substrate may be a plastic film containing one or more polymers selected from the group consisting of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), cycloolefin polymer (COP), cycloolefin copolymer (COC), polycarbonate (PC), and poly(methyl methacrylate) (PMMA).
[0032] Among these, a polyethylene terephthalate film is suitable for use as the light-transmitting substrate since it has both transparency and flexibility and is also excellent in strength.
[0033] The polyethylene terephthalate film may have an in-plane retardation (Re) value of, for example, 120 to 300 nm, 130 to 280 nm, 140 to 250 nm, or 150 to 200 nm. If the polyethylene terephthalate film does not satisfy the above-mentioned in-plane retardation value, the moisture permeability, oxygen permeability, and adhesive strength properties of the laminate after the retort process and the Gelbo flex test may rapidly deteriorate.
[0034] The polyethylene terephthalate film has, for example, a retardation in the thickness direction (R th ) value may be 100 nm or more and 1,000 nm or less, 200 nm or more and 800 nm or less, 300 nm or more and 700 nm or less, or 400 nm or more and 600 nm or less. If the polyethylene terephthalate film does not satisfy the above-mentioned thickness direction retardation value, the moisture permeability, oxygen permeability and adhesive strength properties of the laminate after the retort process and the Gelbo flex test may be rapidly deteriorated.
[0035] The retardation is determined by the refractive index (n x ), the refractive index in the fast axis direction perpendicular to the slow axis direction (n y ), the refractive index in the thickness direction of the polyethylene terephthalate film (n z ) and the thickness d (unit: nm) of the polyethylene terephthalate film into the following mathematical formulas 1 and 2, respectively.
[0036] [Formula 1] Re = (n x -n y ) X d
[0037] [Formula 2] R th =(n z -n y ) X d
[0038] Moreover, such retardation can be a value measured using, for example, a phase difference measuring device (KOBRA-WPR, measuring wavelength: 590 nm).
[0039] Alternatively, the polyethylene terephthalate film may have two axial refractive indices (n x ,n y ) is determined by the Abbe refractive index system (NAR-4T). Here, the axis showing a larger refractive index is defined as the slow axis. The thickness of the polyethylene terephthalate film is measured, for example, using an electric micrometer, and the refractive index difference (n x -n y ) and calculate the refractive index difference (n x -n y The retardation (Re) can be calculated by multiplying the thickness d (nm) of the polyethylene terephthalate film by the refractive index (R) of the film.
[0040] The refractive index difference of the polyethylene terephthalate film (nx -n y ) may be 0.010 to 0.030, 0.013 to 0.028, or 0.015 to 0.025. x -n y ) is not satisfied, the moisture permeability, oxygen permeability and adhesive strength properties of the laminate after the retort process and the Gelbo flex test may rapidly deteriorate.
[0041] In addition, such retardation was measured by cutting the polyethylene terephthalate film into a strip-shaped test piece having a full width in the transverse direction (TD), and then measuring the in-plane retardation (Re) and the retardation in the thickness direction (R th ) can be measured, respectively.
[0042] Here, the average in-plane retardation (Re) measured at 100 mm intervals in the width direction of the polyethylene terephthalate film may be 120 to 300 nm, 130 to 280 nm, 140 to 250 nm, or 150 to 200 nm. The standard deviation of the in-plane retardation (Re) measured at each of the above-mentioned measurement points may be 7.0 to 15.0, 8.0 to 14.0, 9.0 to 12.0, 9.5 to 11.0, or 10.0 to 10.3.
[0043] The retardation in the thickness direction (R th The average value of the retardation in the thickness direction (R th ) may be 10.0 to 40.0, 15.0 to 35.0, 20.0 to 30.0, or 25.0 to 30.0.
[0044] Meanwhile, the polyethylene terephthalate film may have a shrinkage percentage in the machine direction (MD) of 0.5% to 2.0%, 0.7% to 1.8%, or 1.0% to 1.5% after being maintained at 150° C. for 30 minutes and measured according to ASTM D 2305. Also, the shrinkage percentage in the transverse direction (TD) may be 0.0% to 1.0%, 0.0% to 0.8%, or 0.0% to 0.5%.
[0045] If the polyethylene terephthalate film does not satisfy the above-mentioned shrinkage ratios in the machine direction (MD) and the transverse direction (TD), the moisture permeability, oxygen permeability and adhesive strength properties of the laminate after the retort process and the Gelbo flex test may rapidly deteriorate.
[0046] The shrinkage rate in the machine direction (MD) and the shrinkage rate in the transverse direction (TD) are measured in accordance with ASTM D 2305 by measuring the change in size after placing the sample in a hot air oven maintained at 150°C for 30 minutes, and the shrinkage rate can be calculated by the following formula.
[0047] Shrinkage rate (%) = (film length before heat treatment - film length after maintaining at 150°C for 30 minutes) / film length before heat treatment x 100
[0048] The light-transmitting substrate may have a thickness of 5 μm to 300 μm, 5 μm to 250 μm, or 10 μm to 250 μm, or 10 μm to 200 μm, or 10 μm to 150 μm, or 10 μm to 100 μm, or 10 μm to 50 μm. In order to achieve an appropriate strength as a substrate, the thickness of the light-transmitting substrate is preferably 5 μm or more. However, if the substrate is too thick, the flexibility may decrease. Therefore, the thickness of the light-transmitting substrate is preferably 300 μm or less.
[0049] The light-transmitting substrate may be surface-treated to improve the wettability of the surface or the adhesion to the inorganic barrier layer, etc. Non-limiting examples of the surface treatment may include plasma treatment, corona treatment, glow discharge treatment, etc.
[0050] On the other hand, the inorganic barrier layer is a thin film made of an inorganic material, and is laminated on one surface of the light-transmitting substrate.
[0051] The inorganic barrier layer is transparent, and can enable the moisture and oxygen barrier laminate to exhibit moisture and oxygen barrier properties.
[0052] Such an inorganic barrier layer is made of one or more inorganic substances selected from the group consisting of silicon oxide, silicon oxynitride, silicon nitride, aluminum oxide, and aluminum nitride.
[0053] The inorganic barrier layer may have a thickness of 1 nm to 200 nm, 1 nm to 150 nm, 5 nm to 150 nm, 5 nm to 100 nm, or 10 nm to 100 nm. In order to achieve appropriate physical properties as a barrier layer, the inorganic barrier layer is preferably 1 nm or more in thickness. However, if the inorganic barrier layer is too thick, curling due to stress may occur, or even slight bending may cause cracks. Therefore, the inorganic barrier layer is preferably 200 nm or less in thickness.
[0054] The inorganic barrier layer can be formed on the light-transmitting substrate by a conventional method. For example, the lamination method of the inorganic barrier layer can be selected from physical vapor deposition (PVD) and chemical vapor deposition (CVD) as a more appropriate method.
[0055] Preferably, the deposition method of the inorganic barrier layer can be selected from evaporation methods such as thermal evaporation and electron-beam evaporation; or sputtering.
[0056] As an example, the evaporation method is the most basic method for forming a thin film, in which a metal or nonmetal source is heated, evaporated, and condensed on the surface of a substrate at a low temperature to form a thin film. According to one embodiment of the invention, among the evaporation methods, thermal evaporation can be preferably selected as a method for depositing the inorganic barrier layer. The thermal evaporation is performed at an initial vacuum of 10°C. -4 This method requires a vapor pressure of about 1 / 2 torr, and heats the source by passing electricity through a boat carrying the source to be evaporated and using the resistance heat generated by the boat. The deposition rate in thermal evaporation can be changed by adjusting the amount of current supplied to the filament. In addition, an oxide film (AlO x ,SiO x etc.) can be formed.
[0057] As another example, the sputtering method is preferably used since it has excellent reproducibility and can easily form a dense thin film over a large area. Preferably, reactive sputtering using an inorganic target and reactive oxygen (e.g., oxygen) is used as a method for laminating the inorganic barrier layer. In the reactive sputtering method, the reactive gas is additionally introduced into the system in addition to argon (Ar) as a plasma generating gas. In the reactive sputtering method, it is preferable to precisely control the amount of the reactive gas in the system using a device such as a plasma emission monitor or a mass flow controller. This is because the stoichiometric ratio of the inorganic thin film to be formed must be consistent. By adjusting the amount of the reactive gas introduced, stable film formation is possible, and the inorganic barrier layer having excellent barrier properties can be formed.
[0058] Meanwhile, the protective layer is laminated on the inorganic barrier layer, and the protective layer can minimize cracks or interlayer separation of the inorganic barrier layer due to deformation such as bending.
[0059] The protective layer may contain one or more resins selected from the group consisting of alkyd resins, melamine resins, acrylic resins, urethane resins, polyester resins, phenolic resins, amino resins, fluorine resins, epoxy resins, and isocyanate resins.
[0060] In addition, the protective layer may further include a silane coupling agent that can improve adhesion to the inorganic barrier layer.
[0061] The protective layer may be formed on the inorganic barrier layer by a conventional method in the technical field to which the present invention pertains.
[0062] For example, the protective layer may be laminated by a wet coating method, such as a bar coating method, a spin coating method, a roller coating method, a spray coating method, an air knife coating method, a flow coating method, a curtain coating method, a direct gravure coating method, or a slit reverse coating method.
[0063] As another example, the protective layer can be laminated onto the inorganic barrier layer using an adhesive or adhesive film.
[0064] The protective layer may have a thickness of 1 nm to 1000 nm, 5 nm to 1000 nm, 5 nm to 800 nm, 10 nm to 800 nm, 50 nm to 700 nm, 100 nm to 700 nm, 200 nm to 600 nm, or 400 nm to 600 nm. In order to achieve appropriate physical properties as a protective layer, the thickness of the protective layer is preferably 1 nm or more. However, if the protective layer is too thick, flexibility is reduced and curling due to stress may occur. Therefore, the thickness of the protective layer is preferably 1000 nm or less.
[0065] In the moisture and oxygen barrier laminate according to one embodiment, one or more films selected from the group consisting of a nylon film and an unstretched polypropylene film may be further formed on the protective layer.
[0066] The nylon film may be a biaxially oriented nylon film, which can complement the impact resistance of the moisture and oxygen barrier laminate, and the unoriented polypropylene film can complement the heat resistance of the laminate.
[0067] For example, the moisture and oxygen barrier laminate may be formed by forming only an unstretched polypropylene film on a protective layer, or by forming a nylon film and an unstretched polypropylene film sequentially on the protective layer, and the layers may be bonded together by bonding with a urethane adhesive or the like.
[0068] The moisture and oxygen barrier laminate according to the embodiment can be used as a food packaging material. The laminate can also be applied to various electronic elements such as liquid crystal display elements, solar cells, touch panels, organic EL elements, organic TFTs, organic semiconductor sensors, organic light-emitting devices, film capacitors, inorganic EL elements, and color filters, or can be used as packaging materials for the electronic elements. Effect of the Invention
[0069] The moisture and oxygen barrier laminate of the present invention can exhibit excellent moisture and oxygen barrier properties while maintaining excellent interlayer adhesion even after undergoing a retort process in which food is sterilized at high temperatures and a Gelbo flex test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0070] In the following, preferred examples are presented to aid in understanding of the present invention. However, the following examples are for illustrating the present invention and are not intended to limit the present invention.
[0071] <Example 1> (1) Preparation of the composition for forming the protective layer A composition for forming a protective layer was prepared by mixing a urethane resin (Takelac WPB-341A, manufactured by Mitsui Chemicals, Inc.), pure water, and isopropyl alcohol in a weight ratio of 30:55:15.
[0072] (2) Adhesive manufacturing The adhesive was produced by mixing a polyester-based two-component adhesive, a base component (product name: TM-585-60K, solid content 60% by weight), a hardener component (product name: CAT-10, solid content 75% by weight), and ethyl acetate in a weight ratio of 36:4:60.
[0073] (3) Manufacturing of moisture and oxygen barrier laminate A polyethylene terephthalate (PET1) film shown in Table 1 below was prepared as a light-transmitting substrate. Aluminum oxide was deposited on the PET1 film to a thickness of 10 nm using a thermal deposition device equipped with an aluminum target to form an inorganic barrier layer. The composition for forming a protective layer was applied on the inorganic barrier layer using a Mayer bar (WIRE BAR) in a dry coating amount of 0.5 g / m. 2 After coating so as to obtain a coating solution having a thickness of 100 nm, the coating solution was dried at 100° C. for 12 seconds to form a protective layer having a thickness of 500 nm.
[0074] The adhesive was applied to a thickness of 3 μm on the protective layer, and then dried at 100° C. for 20 seconds. A 15 μm-thick nylon film (CNH-02, KOLON) was laminated (inserted) on the dried adhesive-coated surface using a laminator. The adhesive was applied to a thickness of 3 μm on the nylon film, and then dried at 100° C. for 20 seconds. A 70 μm-thick unstretched polypropylene film (CPR-HS, FILMAX) was laminated (inserted) on the dried adhesive-coated surface using a laminator to produce a moisture- and oxygen-barrier laminate.
[0075] <Comparative Examples 1 to 3> A moisture and oxygen barrier laminate was produced in the same manner as in Example 1, except that one of the PET2 to PET4 films in Table 1 below was used instead of the PET1 film.
[0076] Meanwhile, the methods for measuring the shrinkage rate and the in-plane retardation (Re) in Table 1 are as follows.
[0077] (a) Shrinkage measurement The shrinkage in the machine direction (MD) and the shrinkage in the transverse direction (TD) of the polyethylene terephthalate (PET) films used in the examples and comparative examples were measured according to the ASTM D 2305 standard.
[0078] Specifically, a polyethylene terephthalate film was cut into a size of 200 mm wide and 200 mm long, and then left for 30 minutes in a hot air oven maintained at 150°C, after which the change in size was measured.
[0079] Shrinkage rate (%) = (film length before heat treatment - film length after maintaining at 150°C for 30 minutes) / film length before heat treatment x 100
[0080] (b) Retardation measurement A strip-shaped test piece having a length of 50 mm in the machine direction (MD) and a length of 100 mm in the transverse direction (TD) was cut out from the polyethylene terephthalate (PET) film used in each of the Examples and Comparative Examples. Next, the in-plane retardation (Re) and the thickness direction retardation (R) at 590 nm were measured at 10 measurement points at intervals of 100 mm in the transverse direction using a parallel Nicol rotation type phase difference meter (Oji Scientific Instruments, KOBRA-WPR, Japan). th ) were measured, and the in-plane retardation (Re) and the retardation in the thickness direction (R th ) were calculated.
[0081] [Table 1]
[0082] <Test Example> (1) Moisture permeability evaluation 50 cm of moisture and oxygen barrier laminates of the Examples and Comparative Examples 2 After mounting the sample on a moisture permeability analyzer (model: AQUATRAN 2 WVTR Analyzer, manufacturer: Mocon), the moisture permeability (g / m2) was measured under conditions of 40°C and 90% relative humidity in accordance with the standard test method of ASTM F1249. 2 *day) was measured.
[0083] (2) Oxygen permeability evaluation 50 cm of moisture and oxygen barrier laminates of the Examples and Comparative Examples 2 After mounting the sample on an oxygen transmission rate analyzer (model name: OX-Tran 2 / 21 OTR Analyzer, manufacturer: Mocon), the oxygen transmission rate (cc / m 2) was measured under conditions of 23°C and 0% relative humidity in accordance with the standard test method of ASTM D3985. 2 *day) was measured.
[0084] (3) Adhesion strength evaluation In the moisture and oxygen barrier laminates of the Examples and Comparative Examples, an adhesive was dry-coated to a thickness of 3 μm on the protective layer on which the nylon film and the unstretched polypropylene film were not formed, and then only the unstretched polypropylene film was laminated on top of that, and the resulting mixture was aged at 45° C. for one day to prepare a test sample.
[0085] Two sheets of double-sided tape were attached to the measurement plate of a peel tester (model name: AR-1000, manufacturer: ChemInstruments), and then the test sample cut to a width of 1.5 cm was attached to the plate. A 180° peel test was performed according to the standard test method of ASTM D3330 to obtain the adhesive strength (gf / 15 mm).
[0086] (4) Evaluation of moisture permeability, oxygen permeability and adhesive strength after retort treatment The moisture and oxygen barrier laminates of the examples and comparative examples were subjected to a retort treatment, specifically, sterilization was performed at 135° C. for 1 hour using a retort evaluation device (KYUNGHAN PRS-03-IH).
[0087] Thereafter, the retorted moisture and oxygen barrier laminate was collected and re-evaluated for (1) moisture permeability, (2) oxygen permeability, and (3) adhesive strength.
[0088] (5) Moisture permeability and oxygen permeability evaluation after Gelbo Flex test The moisture and oxygen barrier laminates of the examples and comparative examples were subjected to a Gelbo Flex test. Specifically, the test was performed according to the standard test method of ASTM F392 using a Gelbo Flex tester (model name: G0005, manufacturer: IDM Instruments), and the moisture and oxygen barrier laminate was attached to the mandrel of the Gelbo Flex tester. The test settings provided a 440 degree twisting motion in the first 90 mm of the stroke, followed by a 65 mm straight horizontal motion. At this time, the bending speed was set to 50 cycles per minute.
[0089] Thereafter, the moisture and oxygen barrier laminates that had been subjected to the Gelbo Flex test were collected and re-evaluated for the (1) moisture permeability evaluation and (2) oxygen permeability evaluation.
[0090] [Table 2]
[0091] Referring to Table 2, the moisture and oxygen barrier laminate of the above example had excellent initial moisture barrier properties, oxygen barrier properties and adhesive strength, and in particular, the changes in moisture permeability, oxygen permeability and adhesive strength before and after the retort treatment and the Gelbo flex test were significantly small. This confirmed that even after the retort treatment and the Gelbo flex test, the laminate exhibited excellent moisture and oxygen barrier properties while maintaining excellent interlayer adhesion.
[0092] In contrast, the moisture and oxygen barrier laminates of the comparative examples not only had inferior initial moisture barrier properties, oxygen barrier properties and adhesive strength compared to the examples, but also showed a rapid deterioration in the above properties after retort treatment and Gelbo flex test.
Claims
1. The optically transparent substrate includes an inorganic barrier layer and a protective layer formed in that order on one side of the substrate, the light-transmitting substrate is a polyethylene terephthalate film, The polyethylene terephthalate film has an in-plane retardation (Re) value of 120 to 300 nm, The polyethylene terephthalate film has a retardation (R th ) value in the thickness direction of 100 nm or more and 1,000 nm or less, the difference (n x -n y ) between the refractive index (n x ) in the in-plane slow axis direction and the refractive index (n y ) in the in-plane fast axis direction of the polyethylene terephthalate film is 0.010 to 0.030; The polyethylene terephthalate film is maintained at 150° C. for 30 minutes, and then has a shrinkage rate of 0.5% to 2.0% in the machine direction (MD) and a shrinkage rate of 0.0% to 1.0% in the transverse direction (TD), as measured according to ASTM D 2305; A nylon film and an unstretched polypropylene film are further formed on the protective layer; The change in moisture transmission rate (WVTR) before and after retort treatment for 1 hour at a temperature of 135° C. is 1.00 g / m 2 * days or less.
2. The optically transparent substrate includes an inorganic barrier layer and a protective layer formed in that order on one side of the substrate, the light-transmitting substrate is a polyethylene terephthalate film, The polyethylene terephthalate film has an in-plane retardation (Re) value of 120 to 300 nm, The polyethylene terephthalate film has a retardation (R th ) value in the thickness direction of 100 nm or more and 1,000 nm or less, the difference (n x -n y ) between the refractive index (n x ) in the in-plane slow axis direction and the refractive index (n y ) in the in-plane fast axis direction of the polyethylene terephthalate film is 0.010 to 0.030; The polyethylene terephthalate film is maintained at 150° C. for 30 minutes, and then has a shrinkage rate of 0.5% to 2.0% in the machine direction (MD) and a shrinkage rate of 0.0% to 1.0% in the transverse direction (TD), as measured according to ASTM D 2305; A nylon film and an unstretched polypropylene film are further formed on the protective layer; The change in moisture transmission rate (WVTR) before and after 50 repeated twists using a Gelbo flex tester was 0.70 g / m 2 * days or less.
3. The change in oxygen transmission rate (OTR) of the laminate before and after retort treatment for 1 hour at a temperature of 135° C. is 0.50 cc / m 2 3. The moisture and oxygen barrier laminate according to claim 1, wherein the moisture and oxygen barrier properties are not more than 100%.
4. The laminate was subjected to 50 repeated twists using a Gelbo flex tester, and the change in moisture transmission rate (WVTR) was 0.70 g / m 2 2. The moisture and oxygen barrier laminate according to claim 1, wherein the moisture and oxygen barrier properties are not more than 100%.
5. The laminate was twisted 50 times using a Gelbo flex tester, and the change in oxygen transmission rate (OTR) was 1.00 cc / m 2 3. The moisture and oxygen barrier laminate according to claim 1, wherein the moisture and oxygen barrier properties are not more than 100%.
6. 2. The moisture and oxygen barrier laminate according to claim 1, wherein the polyethylene terephthalate film has an average in-plane retardation (Re) of 120 to 300 nm and a standard deviation of 7.0 to 15.0, the in-plane retardation being measured at intervals of 100 mm in the width direction.
7. 3. The moisture and oxygen barrier laminate according to claim 1, wherein the inorganic barrier layer is made of one or more inorganic substances selected from the group consisting of silicon oxide, silicon oxynitride, silicon nitride, aluminum oxide, and aluminum nitride.
8. 3. The moisture and oxygen barrier laminate according to claim 1, wherein the protective layer contains one or more resins selected from the group consisting of alkyd resins, melamine resins, acrylic resins, urethane resins, polyester resins, phenolic resins, amino resins, fluorine resins, epoxy resins and isocyanate resins.
9. 3. The moisture and oxygen barrier laminate according to claim 1, wherein the light-transmitting substrate has a thickness of 5 μm to 100 μm.
10. 3. The moisture and oxygen barrier laminate according to claim 1, wherein the inorganic barrier layer has a thickness of 1 nm to 200 nm.
11. 3. The moisture and oxygen barrier laminate according to claim 1, wherein the protective layer has a thickness of 1 nm to 1000 nm.
Citation Information
Patent Citations
Polyester film
JP2005097560A
Pouch for retort
JP2005178805A
Gas barrier vapor deposition film, and laminate, packaging material and packaging body using the gas barrier vapor deposition film
JP2020049942A
Gas barrier multilayer film and method for producing the same
US20170036833A1
Gas barrier multilayer film and method for producing same
WO2015163413A1