Polyphenylene ether melt spun fiber and its manufacturing method, and paper and fabric

A high-content polyphenylene ether melt-spun fiber production method using a specific resin composition with controlled glass transition temperatures addresses spinning challenges, resulting in fibers with enhanced mechanical strength and flame retardance for applications in papers and fabrics.

JP7554392B2Active Publication Date: 2024-09-20TOYOBO MC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021562464
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-03
Filing Date
2020-09-18
Publication Date
2024-09-20
Estimated Expiration
2040-09-18

AI Technical Summary

Technical Problem

Existing methods for producing polyphenylene ether melt-spun fibers face challenges in achieving high polyphenylene ether content due to high melt viscosity, leading to difficulties in spinning and drawing, poor spinnability, and inadequate mechanical properties.

Method used

A method involving a raw resin composition with a high content of polyphenylene ether components, specifically 95% by mass or more, with a glass transition temperature between 180°C and 205°C, combined with a low Tg component to enhance fluidity and spinnability, allowing for melt spinning and production of fibers with improved mechanical strength and flame retardance.

Benefits of technology

The method enables the production of polyphenylene ether melt-spun fibers with high mechanical strength, heat resistance, and flame retardance, suitable for applications in papers and fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554392000009
    Figure 0007554392000009
  • Figure 0007554392000001
    Figure 0007554392000001
  • Figure 0007554392000006
    Figure 0007554392000006
Patent Text Reader

Abstract

An objective of the present invention is to provide: polyphenylene ether melt-spun fibers that can be melt-spun even when the fibers have a high polyphenylene ether content, and that have superior properties in terms of mechanical strength and the like; a method for manufacturing the same; a paper; and a textile. The present invention pertains to polyphenylene ether melt-spun fibers characterized by having a polyphenylene ether component content of 95 mass% or more in terms of the total components forming the fibers, and a glass transition temperature of 180°C to 205°C, inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polyphenylene ether melt-spun fibers having a high content of polyphenylene ether components and a method for producing the same, as well as paper and fabric. [Background technology]

[0002] Polyphenylene ether (hereinafter sometimes referred to as PPE) has excellent heat resistance, flame retardancy, strength, chemical resistance, etc., and molded articles made from polyphenylene ether are used in a wide range of fields. However, polyphenylene ether generally has a high melt viscosity, so melt molding is difficult when polyphenylene ether is used alone or when the polyphenylene ether content is high. In particular, when melt spinning to make fibers, the melt viscosity has a large effect on the spinning and drawing state after extrusion from the nozzle, and this has been accompanied by many difficulties compared to normal injection molding.

[0003] Known melt-spun fibers containing polyphenylene ether include those obtained by melt-spinning a polymer alloy of a non-crystalline thermoplastic resin such as polyphenylene ether and a crystalline thermoplastic resin such as polypropylene (see, for example, Patent Document 1), fibers containing polyphenylene ether and a processing aid and a flame retardant containing linear low-density polyethylene, petroleum resin, or a combination thereof (see, for example, Patent Document 2), and fibers made of a polyphenylene ether-based resin composition made of polyphenylene ether and a copolymer having a functional group reactive with polyphenylene ether (see, for example, Patent Document 3). Also known are various molding compositions containing two types of polyphenylene ether resins having specific intrinsic viscosities (see, for example, Patent Document 4). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-190156 A [Patent Document 2] Special Publication No. 2017-502179 [Patent Document 3] JP 2008-138294 A [Patent Document 4] Special Publication No. 2003-531234 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in Patent Documents 1 and 2, crystalline thermoplastic resins such as polypropylene, processing aids, etc. are added to polyphenylene ether to improve processability, and the polyphenylene ether content is low, so the excellent characteristics of polyphenylene ether cannot be fully utilized. Furthermore, in Patent Document 3, although the polyphenylene ether content is high, only thick fibers with a diameter of 0.14 mm are obtained, and it is considered that the fluidity of polyphenylene ether is not sufficiently improved or the spinnability is insufficient. In general, in order to obtain thin fibers, it is necessary to achieve both fluidity and spinnability, and it is extremely difficult to achieve both with a high polyphenylene ether content. In addition, the fiber obtained in the specific example of Patent Document 3 has a low elongation of 20%, which raises concerns about its handleability. In Patent Document 4, a polyphenylene ether blend with high fluidity is obtained by including two kinds of polyphenylene ether resins with different intrinsic viscosities, but in the specific examples, the polyphenylene ether is included in an amount of about 75% by weight or less in the composition, and there are no specific examples of the case where the polyphenylene ether is included in a higher content. In addition, in the specific examples in Patent Document 4, a large amount of flame retardant and glass fiber is included, thereby achieving both flame retardancy and fluidity and physical and mechanical properties, but it is difficult to make such a resin composition into fibers.

[0006] An object of the present invention is to provide a polyphenylene ether melt spun fiber which can be melt spun even when the polyphenylene ether content is high and which has excellent properties such as mechanical strength, a method for producing the same, and paper and fabric formed from the polyphenylene ether melt spun fiber. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted extensive research into polyphenylene ether melt spun fibers and have found that the above-mentioned problems can be solved by the following polyphenylene ether melt spun fibers and production methods thereof, as well as paper and fabric, and have thus completed the present invention.

[0008] Specifically, the present invention relates to a polyphenylene ether melt-spun fiber characterized in that the content of the polyphenylene ether component is 95 mass% or more of all components forming the fiber and the glass transition temperature is 180°C or higher and 205°C or lower.

[0009] The polyphenylene ether melt spun fiber preferably has a single fiber fineness of 1.0 dtex or more and 100 dtex or less.

[0010] The polyphenylene ether melt-spun fiber preferably has a maximum elongation of 25% or more and 120% or less.

[0011] The polyphenylene ether melt spun fibers are preferably staple fibers.

[0012] The short fibers are preferably flame-retardant short fibers.

[0013] The present invention also relates to paper formed from said polyphenylene ether melt spun fibers.

[0014] The paper is preferably flame-retardant paper.

[0015] The present invention also relates to a fabric formed from the polyphenylene ether melt spun fibers.

[0016] The fabric is preferably a flame-retardant fabric.

[0017] The present invention also provides a method for producing polyphenylene ether melt spun fibers, comprising the steps of: A step of melt-extruding a raw material resin composition containing a polyphenylene ether component having a glass transition temperature of less than 170°C and a polyphenylene ether component having a glass transition temperature of 180°C or higher; The molten raw material resin composition is discharged from a spinning nozzle to spin the composition, The present invention relates to a method for producing polyphenylene ether melt spun fibers, wherein the content of polyphenylene ether components in the obtained polyphenylene ether melt spun fibers is 95 mass % or more of all components forming the fibers.

[0018] The content of the polyphenylene ether component having a glass transition temperature of less than 170° C. is preferably 5% by mass or more in the polyphenylene ether component contained in the raw material resin composition.

[0019] The spinning speed is preferably 100 to 1000 m / min.

[0020] The temperature of the spinning nozzle is preferably 280 to 320°C.

[0021] It is preferable to perform spinning by introducing an inert gas into the region immediately below the spinning nozzle. Effect of the Invention

[0022] The present invention provides polyphenylene ether melt spun fibers containing a high content of polyphenylene ether components, and paper and fabric formed from the polyphenylene ether melt spun fibers. The polyphenylene ether melt spun fibers of the present invention have excellent mechanical strength, flame retardancy, heat resistance, chemical resistance, etc., because they contain a high content of polyphenylene ether components.

[0023] Furthermore, according to the production method of the present invention, a raw material resin composition containing a polyphenylene ether component having a glass transition temperature of less than 170°C and a polyphenylene ether component having a glass transition temperature of 180°C or higher is used, which improves fluidity and spinnability to the extent that melt spinning is possible, making it possible to produce polyphenylene ether melt-spun fibers containing a high content of polyphenylene ether component. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a method for producing polyphenylene ether melt-spun fibers of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] 1. Polyphenylene ether melt spun fiber The polyphenylene ether melt spun fiber of the present invention is characterized in that the content of the polyphenylene ether component is 95 mass% or more of all components forming the fiber, and the glass transition temperature is 180°C or more and 205°C or less.

[0026] In the present invention, the content of the polyphenylene ether component is 95% by mass or more, preferably 98% by mass or more, and more preferably substantially composed of only the polyphenylene ether component (100% by mass) in all the components forming the fiber. When the content of the polyphenylene ether component in the polyphenylene ether melt spun fiber is within the above range, the obtained fiber is excellent not only in mechanical strength but also in heat resistance, chemical resistance, flame retardancy, etc.

[0027] The polyphenylene ether is, for example, a compound represented by the following general formula (1): [ka] (In the formula, R 1 , R 2 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, R 3 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent. Examples of the repeating unit include those having the following repeating units:

[0028] R in the general formula (1) 1 , R 2 Examples of the alkyl group include a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, an octyl group, or a decyl group, an aryl group having 6 to 10 carbon atoms, such as a phenyl group, a 4-methylphenyl group, a 1-naphthyl group, or a 2-naphthyl group, and an aralkyl group having 7 to 10 carbon atoms, such as a benzyl group, a 2-phenylethyl group, or a 1-phenylethyl group.

[0029] When the hydrocarbon group has a substituent, examples of the substituent include a halogen atom such as a fluorine atom, an alkoxy group such as a methoxy group, etc. Specific examples of the hydrocarbon group having a substituent include a trifluoromethyl group, etc.

[0030] Among these, R 1 , R 2 is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom.

[0031] R in the general formula (1) 3Examples of the alkyl group include alkyl groups having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, an octyl group, and a decyl group; aryl groups having 6 to 10 carbon atoms, such as a phenyl group, a 4-methylphenyl group, a 1-naphthyl group, and a 2-naphthyl group; and aralkyl groups having 7 to 10 carbon atoms, such as a benzyl group, a 2-phenylethyl group, and a 1-phenylethyl group.

[0032] When the hydrocarbon group has a substituent, examples of the substituent include a halogen atom such as a fluorine atom, and an alkoxy group such as a methoxy group. Specific examples of the hydrocarbon group having a substituent include a trifluoromethyl group.

[0033] Among these, R 3 As the alkyl group, a methyl group is preferable.

[0034] Specific examples of the repeating unit of the general formula (1) include repeating units derived from 2,6-dimethyl-1,4-phenylene ether, 2,6-diethyl-1,4-phenylene ether, 2-methyl-6-ethyl-1,4-phenylene ether, and 2,6-dipropyl-1,4-phenylene ether. Among these, the repeating unit derived from 2,6-dimethyl-1,4-phenylene ether is preferred.

[0035] The polyphenylene ether is preferably a homopolymer having a repeating unit of the general formula (1) or a copolymer containing two or more different repeating units of the general formula (1). The polyphenylene ether may contain a repeating unit other than the general formula (1) as long as the effect of the present invention is not impaired. The content of such a repeating unit other than the general formula (1) is not particularly limited as long as the effect of the present invention is not impaired, but for example, it is preferably about 5 mol % or less in the copolymer, and more preferably it is not contained at all.

[0036] The polyphenylene ether melt spun fiber of the present invention may contain a resin component other than the polyphenylene ether component. Examples of the resin component other than the polyphenylene ether component include styrene, polyethylene, polypropylene, polyamides such as polyamide 4, polyamide 6, polyamide 10, polyamide 11, polyamide 66, polyamide 6T, and polyamide 6T / 11, polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polycarbonates. However, the content of the resin component is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 0% by mass or less, based on the total components forming the fiber.

[0037] Furthermore, additives such as lubricants, plasticizers, antioxidants, UV absorbers, dulling agents, and antistatic agents can be added to the polyphenylene ether melt spun fibers of the present invention within the range that does not impair the effects of the present invention. However, the amount of such additives added is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably none (0% by mass) of all the components forming the fiber.

[0038] The method for producing the polyphenylene ether melt spun fiber of the present invention is not particularly limited, and for example, the polyphenylene ether melt spun fiber can be produced by the method for producing the polyphenylene ether melt spun fiber described below.

[0039] The glass transition temperature of the polyphenylene ether melt spun fiber is 180° C. or more and 205° C. or less, and preferably 190° C. or more and 205° C. or less. When the glass transition temperature is in the above range, it is possible to achieve a good balance between melt processability and heat resistance.

[0040] The polyphenylene ether melt spun fiber has a maximum stress of 0.8 cN / dtex or more and 1.8 cN / dtex or less, and more preferably 0.9 cN / dtex or more and 1.5 cN / dtex or less. The polyphenylene ether melt spun fiber has a maximum elongation of 25% or more and 120% or less, and more preferably 50% or more and 95% or less, from the viewpoint of handling. The maximum stress and maximum elongation can be measured by the method described in the Examples.

[0041] The single-filament fineness of the polyphenylene ether melt-spun fiber is preferably 1.0 dtex or more and 100 dtex or less, more preferably 1.0 dtex or more and 50 dtex or less, and even more preferably 1.0 dtex or more and 30 dtex or less, for general heat-resistant filters, heat-resistant woven fabrics, etc. Such single-filament fineness can be appropriately set depending on the application. In the present invention, very fine fibers of 30 dtex or less can also be obtained.

[0042] The polyphenylene ether melt spun fibers have excellent high temperature stability. The polyphenylene ether melt spun fibers may be long fibers or short fibers.

[0043] 2. Method for producing polyphenylene ether melt-spun fibers The method for producing polyphenylene ether melt spun fibers of the present invention includes the steps of melt extruding a raw material resin composition containing a polyphenylene ether component having a glass transition temperature of less than 170° C. (hereinafter also referred to as a low Tg polyphenylene ether component) and a polyphenylene ether component having a glass transition temperature of 180° C. or higher (hereinafter also referred to as a high Tg polyphenylene ether component); The molten raw material resin composition is discharged from a spinning nozzle to spin the composition, The content of the polyphenylene ether component in the obtained polyphenylene ether melt-spun fiber is characterized by being 95 mass % or more of all components forming the fiber.

[0044] Generally, polyphenylene ether has a high melt viscosity, and it has been considered difficult to melt spin the polyphenylene ether alone or in the case where the polyphenylene ether is contained in a high content. In the present invention, a raw material resin composition containing a polyphenylene ether component having a glass transition temperature of less than 170°C and a polyphenylene ether component having a glass transition temperature of 180°C or more is used, so that the fluidity and spinnability are improved to such an extent that melt spinning is possible, and it is also possible to produce melt spun fibers. Each of the components of the present invention will be described below.

[0045] The raw material polyphenylene ether may be a homopolymer having a repeating unit of the general formula (1), a copolymer containing two or more different repeating units of the general formula (1), or a copolymer having a repeating unit of the general formula (1) and a repeating unit other than the general formula (1). The content of the repeating unit other than the general formula (1) in the copolymer may be as described above. Among these, a homopolymer having a repeating unit of the general formula (1) is preferred.

[0046] Specific examples of homopolymers having a repeating unit of the general formula (1) include poly(2,6-dimethyl-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dipropyl-1,4-phenylene ether), and the like. Among these, poly(2,6-dimethyl-1,4-phenylene ether) is preferred.

[0047] As the poly(2,6-dimethyl-1,4-phenylene ether), commercially available products can also be suitably used. Specific examples include PPO640, PPO646, and PPOSA120 manufactured by SABIC Innovative Plastic, and ZYLON S201A and ZYLON S202A manufactured by Asahi Kasei Chemicals Corporation.

[0048] The glass transition temperature of the high Tg polyphenylene ether component as the raw material is 180° C. or higher, preferably 200° C. or higher, and more preferably 210° C. or higher. The upper limit of the glass transition temperature is not particularly limited, but is preferably 230° C. or lower. When the glass transition temperature of the high Tg polyphenylene ether component as the raw material is in the above range, polyphenylene ether melt-spun fibers having high heat resistance can be obtained, which is preferable.

[0049] The glass transition temperature of the low Tg polyphenylene ether component as the raw material is less than 170° C., preferably 165° C. or less, and more preferably 160° C. or less. The lower limit of the glass transition temperature is not particularly limited, but is preferably 150° C. or more. When the glass transition temperature of the low Tg polyphenylene ether component as the raw material is in the above range, the melt viscosity of the raw material resin composition is reduced, and the flowability and spinnability are improved.

[0050] In the polyphenylene ether component contained in the raw material resin composition, the content of the high Tg polyphenylene ether component is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. The upper limit of the content of the high Tg polyphenylene ether component is preferably 95% by mass or less. In the present invention, it is preferable to contain a polyphenylene ether component having a high glass transition temperature (i.e., a high molecular weight) in the above range, since the obtained polyphenylene ether melt spun fiber has excellent mechanical strength, heat resistance, chemical resistance, flame retardancy, etc.

[0051] The content of the low Tg polyphenylene ether component is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less, based on the polyphenylene ether component contained in the raw resin composition. The lower limit of the content of the low Tg polyphenylene ether component is preferably 5% by mass or more. In the present invention, it is preferable to include a polyphenylene ether component having a low glass transition temperature (i.e., a low molecular weight) in the above range, since this tends to reduce the melt viscosity of the raw resin composition and improve the flowability and spinnability.

[0052] The raw resin composition may contain resin components and additives other than the polyphenylene ether component together with the polyphenylene ether component. The resin components and additives other than the polyphenylene ether component are as described above. The content of the resin components and additives other than the polyphenylene ether component in the raw resin composition is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably none (0% by mass).

[0053] The melt extrusion can be carried out by a method that can be generally used in this field, for example, by using an extruder equipped with a cylinder and a screw. As the extruder equipped with a cylinder and a screw, a single screw extruder or a twin screw extruder that can be generally used in this field can be used. When the raw material resin is in a powder form, it is preferable to use a twin screw extruder.

[0054] The screw speed and screw shape are not particularly limited, and any speed and shape that can be generally used in this field can be appropriately adopted.

[0055] If the temperature inside the cylinder is too low, the fluidity of the resin is poor, and if it is too high, the fluidity is improved, but foaming phenomenon occurs due to thermal decomposition of the resin, so it is necessary to select a processing temperature that balances these two. The temperature inside the cylinder is preferably, for example, 250 to 320°C, and more preferably 280 to 300°C. By setting the temperature inside the cylinder within the above range, foaming phenomenon can be suppressed, which is preferable.

[0056] The spinning nozzle is not particularly limited, and any nozzle commonly used in this field can be used.

[0057] The temperature of the spinning nozzle is preferably from 280 to 320°C, and more preferably from 290 to 310°C, from the viewpoint of spinnability.

[0058] The spinning speed can be appropriately set depending on the required fineness, etc., but in order to stably obtain fine fibers, it is preferably about 100 to 1000 m / min, and more preferably about 100 to 800 m / min.

[0059] The single hole output rate of the spinning nozzle is preferably 1.0 g / min or less, more preferably 0.7 g / min or less, even more preferably 0.5 g / min or less, and particularly preferably 0.3 g / min or less. The lower limit of the single hole output rate is not particularly limited, but is preferably 0.05 g / min or more, more preferably 0.1 g / min or more, and even more preferably 0.12 g / min or more. By setting the single hole output rate within the above range, it is preferable to obtain a polyphenylene ether fiber with a fineness.

[0060] An example of the production of polyphenylene ether melt spun fibers will be described with reference to FIG. 1. The raw resin composition is fed from a hopper 1 in FIG. 1 into an extruder 2 equipped with a cylinder and a screw, and the molten raw resin composition is metered at a discharge speed by a gear pump 3, passes through a filter medium 4 made of fine sand, and is discharged from a spinning nozzle 5 to obtain melt spun fibers. It is also preferable to install a filter 6 made of a metal nonwoven fabric on the filter medium 4. By installing the filter 6, foreign matter can be removed in advance, and clogging of the filter medium 4 can be prevented, which is preferable.

[0061] From the viewpoint of preventing nozzle clogging due to oxidative crosslinking, it is preferable to provide a heat-retaining space 7 directly below the spinning nozzle 5 and introduce 8 an inert gas such as nitrogen into this region for spinning, and it is more preferable to introduce an inert gas heated by a heating torch 9. The temperature of the heated inert gas is preferably 100 to 500°C, and more preferably 200 to 400°C.

[0062] The single-filament fineness of the polyphenylene ether melt-spun fiber obtained by the production method of the present invention can be appropriately set according to the use of the fiber. For example, the single-filament fineness of the polyphenylene ether melt-spun fiber is preferably 1.0 dtex or more and 100 dtex or less, more preferably 1.0 dtex or more and 50 dtex or less, and even more preferably 1.0 dtex or more and 30 dtex or less, for general heat-resistant filters, heat-resistant woven fabrics, etc. Furthermore, according to the production method of the present invention, very fine fibers of 30 dtex or less can be obtained. This is because the present invention uses a raw material resin composition containing a polyphenylene ether component having a glass transition temperature of less than 170°C and a polyphenylene ether component having a glass transition temperature of 180°C or more, and therefore the fluidity and spinnability are improved to a degree that melt spinning is possible, making it possible to produce melt-spun fibers, and further making it possible to produce melt-spun fibers having the above single-filament fineness.

[0063] 3. Polyphenylene ether melt-spun staple fiber The polyphenylene ether melt spun staple fibers of the present invention can be obtained, for example, by doubling the polyphenylene ether melt spun fibers to form a tow, and cutting the resulting fiber.

[0064] The length of the polyphenylene ether melt-spun short fibers of the present invention is not particularly limited and can be appropriately adjusted depending on the application, but is usually 1 to 500 mm, preferably 3 to 400 mm, and more preferably 5 to 300 mm.

[0065] The tensile strength of the polyphenylene ether melt-spun short fiber of the present invention is not particularly limited, but is usually 0.8 to 60 cN / dtex, preferably 0.85 to 50 cN / dtex, and more preferably 0.9 to 40 cN / dtex. The tensile strength is measured in accordance with JIS L1013 8.5.1.

[0066] The tensile elongation of the polyphenylene ether melt spun short fiber of the present invention is not particularly limited, but is usually 30 to 180%, preferably 40 to 160%, and more preferably 60 to 150%. The tensile elongation is measured in accordance with JIS L1013 8.5.1.

[0067] The equilibrium moisture content of the polyphenylene ether melt-spun short fibers of the present invention is not particularly limited, but is usually 0.01 to 1.5%, preferably 0.02 to 1.2%, and more preferably 0.03 to 1.0%. The equilibrium moisture content is measured in accordance with JIS L1013.

[0068] The high temperature shrinkage of the polyphenylene ether melt spun short fiber of the present invention at 190°C is not particularly limited, but is usually 0.1 to 6%, preferably 0.3 to 5%, and more preferably 0.5 to 4%. The method for measuring the high temperature shrinkage at 190°C is described in the Examples.

[0069] The polyphenylene ether melt-spun staple fibers of the present invention are preferably flame-retardant staple fibers.

[0070] The flame-retardant short fibers can be obtained by subjecting the polyphenylene ether melt-spun short fibers to a flame-retardant treatment, for example, by heat-treating the polyphenylene ether melt-spun short fibers in air at 120 to 240°C for 1 to 30 hours to make them infusible (infusible treatment), and then heat-treating them in air at 260 to 400°C for 0.1 to 10 hours to make them flame-retardant (flame-retardant treatment).

[0071] In the infusibility treatment, the polyphenylene ether melt spun short fibers are treated in air at 120 to 240°C for 1 to 30 hours. Here, "in air" refers to an environment that is not particularly adjusted. The treatment temperature is 120 to 240°C, preferably 140 to 230°C, and more preferably 160 to 220°C. The treatment time is 1 to 30 hours, preferably 1.5 to 25 hours, and more preferably 2 to 20 hours. By setting the treatment time and temperature as described above, the polyphenylene ether melt spun short fibers do not melt in the subsequent flame retardant treatment, and an appropriate flame retardant treatment can be performed.

[0072] After the infusibility treatment, a flame-retardant treatment is performed in air at 260 to 400°C for 0.1 to 10 hours. "In air" refers to an environment that is not particularly adjusted. The treatment temperature is 260 to 400°C, preferably 270 to 380°C, and more preferably 280 to 360°C. The treatment time is 0.1 to 10 hours, preferably 0.3 to 8 hours, and more preferably 0.5 to 6 hours. By setting the treatment time and temperature as described above, a C=O bond structure is formed in the polyphenylene ether melt spun short fibers, and flame-retardant short fibers exhibiting extremely high flame retardancy, flame resistance, heat resistance, etc. are obtained.

[0073] The fineness of the flame-retardant staple fiber is not particularly limited and can be appropriately determined depending on the purpose for which the fiber is used, but for example, it is preferably 100 dtex or less, more preferably 95 dtex or less, and even more preferably 90 dtex or less. The fineness within the above range is preferable because it can be processed into various shapes such as woven fabrics, knitted fabrics, staple fiber nonwoven fabrics, paper, and cloth. In addition, the lower limit of the fineness is not particularly limited, but it is preferably 0.1 dtex or more, and more preferably 0.2 dtex or more.

[0074] The tensile strength of the flame-retardant short fiber is preferably 0.8 cN / dtex or more, more preferably 0.85 cN / dtex or more, and even more preferably 0.90 cN / dtex or more. The tensile strength in the above range is preferable because it improves the handleability of the fiber. The upper limit of the tensile strength is not particularly limited, but is preferably 50 cN / dtex or less, and more preferably 40 cN / dtex or less.

[0075] The polyphenylene ether melt spun staple fibers of the present invention can be used, for example, in paper, fabrics, heat-resistant binders, C / C composites, CFRP matrix resins, industrial brushes, and brake materials.

[0076] Paper formed from polyphenylene ether melt-spun fibers The paper of the present invention is formed from the polyphenylene ether melt spun fibers. The paper can be manufactured by a general method, for example, by a wet papermaking method. In the wet papermaking method, for example, an aqueous slurry containing the polyphenylene ether melt spun fibers is prepared, and then this aqueous slurry is subjected to a normal papermaking process. The aqueous slurry may contain a binder (for example, a water-soluble polymer fiber such as a polyvinyl alcohol fiber, or a heat-adhesive polymer fiber such as a polyethylene terephthalate fiber (PET fiber)). If necessary, the fibers used may be subjected to a beating process. In addition, in order to improve the uniformity and pressure adhesion of the paper, a heat pressing process may be added after the papermaking process.

[0077] The length of the polyphenylene ether melt spun fibers used in the production of paper is not particularly limited, but from the viewpoint of ensuring sufficient quality as paper, the length is preferably 0.5 mm or more, more preferably 1 mm or more, and is preferably 100 mm or less, more preferably 80 mm or less.

[0078] Depending on the purpose, the paper of the present invention may contain other fibers, various additives such as paper strength improvers, fixing agents, defoamers, dyes, ultraviolet absorbers, flame retardants, etc., and various fillers such as talc, kaolin, calcium carbonate, titanium dioxide, etc. These raw materials are often added to the aqueous slurry, but may also be attached by appropriate coating or the like.

[0079] Examples of other fibers include general-purpose fibers such as polyolefin fibers, polyester fibers, polyamide fibers, cellulose fibers, and polysulfone fibers; and heat-resistant fibers such as aromatic para-aramid, polyaryl ketone fibers, and polysulfone fibers.

[0080] The proportion of the polyphenylene ether melt spun fibers contained in the paper of the present invention is, for example, 50 to 100 mass%, preferably 55 to 98 mass%, more preferably 60 to 95 mass%, and even more preferably 65 to 90 mass%, from the viewpoints of mechanical strength, flame retardancy, heat resistance, high-temperature stability, chemical resistance, and the like.

[0081] The basis weight of the paper of the present invention is not particularly limited and can be appropriately adjusted depending on the application of the paper, but is usually 5 to 800 g / cm 2 and preferably 7 to 700 g / cm 2 , more preferably 10 to 600 g / cm 2 It is.

[0082] The tensile strength of the paper of the present invention is not particularly limited, but is usually 1 to 300 N / cm, preferably 3 to 250 N / cm, and more preferably 5 to 200 N / cm. The tensile strength is measured in accordance with JIS L1013 8.5.1.

[0083] The tensile elongation of the paper of the present invention is not particularly limited, but is usually 0.1 to 100%, preferably 0.3 to 90%, and more preferably 0.5 to 80%. The tensile elongation is measured in accordance with JIS L1013 8.5.1.

[0084] The LOI value of the paper of the present invention is not particularly limited, but is usually from 25 to 80, preferably from 27 to 75, and more preferably from 30 to 70. The LOI value is measured in accordance with JIS L 1091 E method.

[0085] The dielectric constant of the paper of the present invention is not particularly limited, but is usually from 1.0 to 2.9, preferably from 1.1 to 2.8, and more preferably from 1.2 to 2.7.

[0086] The equilibrium moisture content of the paper of the present invention is not particularly limited, but is usually 0.01 to 1.5%, preferably 0.02 to 1.2%, and more preferably 0.03 to 1.0%. The equilibrium moisture content is measured in accordance with JIS L1013.

[0087] The high temperature shrinkage of the paper of the present invention at 190° C. is not particularly limited, but is usually 0.1 to 20%, preferably 0.2 to 15%, and more preferably 0.3 to 10%. The method for measuring the high temperature shrinkage at 190° C. is described in the Examples.

[0088] The paper of the present invention is preferably a flame-retardant paper, which can be produced by the above-mentioned method using polyphenylene ether melt-spun fibers that have been subjected to the above-mentioned flame-retardant treatment.

[0089] The flame-resistant paper preferably has a weight loss rate difference of 5.0% or less between 150°C and 400°C, more preferably 4.0% or less, and even more preferably 3.5% or less. The weight loss rate difference within the above range is preferable because it suppresses polymer degradation and improves durability. The weight loss rate difference is preferably 0%, but usually there is a weight loss of about 0.1% or more, and may be about 0.15% or more.

[0090] The specific gravity of the flame-resistant paper is preferably 1.2 or more, more preferably 1.25 or more, and even more preferably 1.3 or more. The specific gravity being within the above range is preferable because the flame-resistant properties of the paper are sufficiently improved and the flame resistance is improved. The upper limit of the specific gravity is not particularly limited, but is preferably 2.0 or less, and more preferably 1.8 or less.

[0091] The LOI value of the flame-retardant paper is preferably 30 or more, more preferably more than 30, even more preferably 32 or more, and particularly preferably 35 or more. The LOI value being in the above range is preferable because the flame retardancy of the obtained flame-retardant paper is excellent. Here, the LOI value means the limiting oxygen index, and the higher the LOI value, the better the flame retardancy. Therefore, the higher the LOI value, the more preferable it is, and the upper limit is not particularly limited.

[0092] The tensile elongation of the flame-resistant paper is preferably 5% or more, more preferably 7% or more, and even more preferably 10% or more. The tensile elongation in the above range is preferable because it can improve processability. The upper limit of the tensile strength is not particularly limited, but is preferably 100% or less, and more preferably 80% or less.

[0093] The strength retention of the flame-resistant paper at 400°C is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more. The strength retention at 400°C in the above range is preferable because it provides high durability when used at high temperatures. The upper limit of the strength retention at 400°C is not particularly limited, but is preferably 100% or less, and more preferably 99% or less. Here, the strength retention at 400°C refers to the strength retention after heat treatment at 400°C for 10 minutes.

[0094] The elongation retention of the flame-resistant paper at 400°C is preferably 40% or more, more preferably 50% or more, and even more preferably 55% or more. The elongation retention at 400°C in the above range is preferable because it provides high durability when used at high temperatures. The upper limit of the elongation retention at 400°C is not particularly limited, but is preferably 100% or less, and more preferably 99% or less. Here, the elongation retention at 400°C refers to the elongation retention after heat treatment at 400°C for 10 minutes.

[0095] The paper of the present invention can be used, for example, as a heat insulating material, a sound absorbing material, a heat resistant filter, a heat resistant insulating paper, an electromagnetic wave shielding material, and the like.

[0096] <Fabrics formed from polyphenylene ether melt-spun fibers> The fabric of the present invention is formed from the polyphenylene ether melt-spun fibers. The fabric may further include one or more fibers selected from the group consisting of wholly aromatic polyester fibers, polybenzoxazole (PBO) fibers, polybenzimidazole (PBI) fibers, polybenzothiazole (PBTZ) fibers, polyimide (PI) fibers, polysulfonamide (PSA) fibers, polyetheretherketone (PEEK) fibers, polyetherimide (PEI) fibers, polyarylate (PAr) fibers, melamine fibers, phenolic fibers, fluorine-based fibers, polyphenylene sulfide (PPS) fibers, cellulose fibers, polyolefin fibers, acrylic fibers, rayon fibers, cotton fibers, animal hair fibers, polyurethane fibers, polyvinyl chloride fibers, polyvinylidene chloride fibers, acetate fibers, and polycarbonate fibers.

[0097] The proportion of the polyphenylene ether melt spun fibers contained in the fabric of the present invention is, for example, 50 to 100 mass%, preferably 55 to 98 mass%, more preferably 60 to 95 mass%, and even more preferably 65 to 90 mass%, from the viewpoints of mechanical strength, flame retardancy, heat resistance, high temperature stability, chemical resistance, and the like.

[0098] The fabric of the present invention may contain additives such as flame retardants, ultraviolet absorbing agents, reflectors, organic dyes, organic pigments, and inorganic pigments, as necessary.

[0099] The fabric of the present invention can be produced by a general method, for example, a method in which the spun yarn of the above-mentioned fiber is blended to obtain a spun yarn, and then the yarn is woven into a twill weave, plain weave, or other weave using a rapier loom or the like using a single or double yarn.

[0100] The basis weight of the fabric of the present invention is not particularly limited and can be appropriately adjusted depending on the application of the fabric, but is usually 10 to 3000 g / cm. 2 and preferably 20 to 2500 g / cm 2 , more preferably 30 to 2000 g / cm 2 It is.

[0101] The LOI value of the fabric of the present invention is not particularly limited, but is usually from 25 to 80, preferably from 27 to 75, and more preferably from 30 to 70. The LOI value is measured in accordance with JIS L 1091 E method.

[0102] The high temperature shrinkage of the fabric of the present invention at 190° C. is not particularly limited, but is usually 0.1 to 20%, preferably 0.2 to 15%, and more preferably 0.3 to 10%. The method for measuring the high temperature shrinkage at 190° C. is as described in the Examples.

[0103] The fabric of the present invention is preferably a flame-retardant fabric. The flame-retardant fabric may be produced by using polyphenylene ether melt-spun fibers that have been subjected to the flame-retardant treatment by the above-mentioned method, or may be produced by using the polyphenylene ether melt-spun fibers to produce a fabric by the above-mentioned method, and then subjecting the produced fabric to the flame-retardant treatment.

[0104] The flame-resistant fabric preferably has a weight loss rate difference of 5.0% or less between 150°C and 400°C, more preferably 4.0% or less, and even more preferably 3.5% or less. The weight loss rate difference within the above range is preferable because it suppresses degradation of the polymer and improves durability. The weight loss rate difference is preferably 0%, but usually there is a weight loss of about 0.1% or more, and may be about 0.15% or more.

[0105] The specific gravity of the flame-resistant fabric is preferably 1.2 or more, more preferably 1.25 or more, and even more preferably 1.3 or more. The specific gravity being within the above range is preferable because the flame resistance of the fabric is sufficiently advanced and the flame resistance is improved. The upper limit of the specific gravity is not particularly limited, but is preferably 2.0 or less, and more preferably 1.8 or less.

[0106] The LOI value of the flame-resistant fabric is preferably 30 or more, more preferably more than 30, even more preferably 32 or more, and particularly preferably 35 or more. The LOI value in the above range is preferable because the flame retardancy of the obtained flame-resistant fabric is excellent. Here, the LOI value means the limiting oxygen index, and the larger the LOI value, the better the flame retardancy. Therefore, the larger the LOI value, the more preferable it is, and the upper limit value is not particularly limited.

[0107] The tensile elongation of the flame-resistant fabric is preferably 5% or more, more preferably 7% or more, and even more preferably 10% or more. The tensile elongation in the above range is preferable because it can improve processability. The upper limit of the tensile strength is not particularly limited, but is preferably 100% or less, and more preferably 80% or less.

[0108] The strength retention of the flame-resistant fabric at 400°C is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more. The strength retention at 400°C in the above range is preferable because it provides high durability when used at high temperatures. The upper limit of the strength retention at 400°C is not particularly limited, but is preferably 100% or less, and more preferably 99% or less. Here, the strength retention at 400°C refers to the strength retention after heat treatment at 400°C for 10 minutes.

[0109] The elongation retention of the flame-resistant fabric at 400°C is preferably 40% or more, more preferably 50% or more, and even more preferably 55% or more. The elongation retention at 400°C in the above range is preferable because it provides high durability when used at high temperatures. The upper limit of the elongation retention at 400°C is not particularly limited, but is preferably 100% or less, and more preferably 99% or less. Here, the elongation retention at 400°C refers to the elongation retention after heat treatment at 400°C for 10 minutes.

[0110] The fabric of the present invention can be used, for example, as a heat insulating material, workwear (for firefighters, racers, and pilots), heat-resistant gloves, disaster prevention hoods, interior materials for transport equipment, heat-resistant clothing, and electromagnetic wave shielding materials. EXAMPLES

[0111] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The methods for evaluating physical properties and the like in the following examples are as follows.

[0112] (1) Fineness, single yarn fineness The measurement was performed according to the method described in JIS L-1095 9.4.1. The single yarn fineness was calculated by dividing the fineness by the number of filaments.

[0113] (2) Maximum stress and maximum elongation Measurements were made in accordance with JIS L1013 8.5.1. The stress at the maximum load was taken as the maximum point stress, and the elongation at the maximum load was taken as the maximum point elongation.

[0114] (3) Glass transition temperature Using a differential scanning calorimeter (model: DSC-Q100) manufactured by TA Instruments, 2 mg of fiber was measured in a nitrogen atmosphere from 30°C to 250°C at a heating rate of 10°C / min. The glass transition temperature (Tg) was determined as the temperature at the intersection of the extension of the baseline below the glass transition temperature and the tangent showing the maximum slope at the transition section.

[0115] <Polyphenylene ether melt-spun fiber> Example 1 A mixture of 90 parts by mass of poly(2,6-dimethyl-1,4-phenylene ether) (PPO640, glass transition temperature (Tg): 221°C, manufactured by SABIC Innovative Plastic) and 10 parts by mass of poly(2,6-dimethyl-1,4-phenylene ether) (PPOSA120, glass transition temperature (Tg): 159°C, manufactured by SABIC Innovative Plastic) was extruded using a twin-screw extruder (product name: KZW15TW-30MG) manufactured by Technovel Co., Ltd. The twin-screw extruder has four cylinder zones, and the cylinders are named cylinders 1, 2, 3, and 4 from the hopper side, respectively, and the cylinders 1 to 4 and the cylinder head part were set to 280°C, and the screw rotation speed was set to 200 rpm.

[0116] A gear pump was installed downstream of the extruder to measure the polymer discharge rate, and the polymer was extruded through a metal nonwoven filter (product name: NF-07, manufactured by Nippon Seisen Co., Ltd.) to a nozzle (nozzle hole diameter: 0.5 mm, nozzle hole land length: 1 mm, number of nozzle holes: 24) (total discharge amount: 5.8 g / min, single hole discharge amount: 0.242 g / min). A surface heater was placed directly below the nozzle, and the nozzle temperature was set to 300°C. A 60 mm heat retention space was provided directly below the nozzle, and nitrogen heated to 300°C was continuously introduced into this area. The polymer discharged from the nozzle was wound up at a spinning speed of 100 m / min. The fineness of the obtained melt spun fiber was 577.1 dtex, the single yarn fineness was 24.0 dtex, the maximum point stress was 0.93 cN / dtex, the maximum point elongation was 93.9%, and the glass transition temperature was 203°C. The physical properties of the obtained fibers are shown in Table 1.

[0117] Examples 2 to 7 Melt spun fibers were obtained in the same manner as in Example 1, except that the composition of the raw resin composition, the screw rotation speed, the nozzle shape, and the spinning conditions were changed as shown in Table 1. The fiber properties of the obtained fibers are shown in Table 1.

[0118] Comparative Example 1 In Comparative Example 1, melt spun fibers were produced in the same manner as in Example 7, except that only poly(2,6-dimethyl-1,4-phenylene ether) (PPO640, glass transition temperature (Tg): 221°C, manufactured by SABIC Innovative Plastic) was used. However, the viscosity was too high to extrude the polymer from the gear pump, resulting in destruction of the gear pump.

[0119] Comparative Example 2 A mixture of 80 parts by mass of poly(2,6-dimethyl-1,4-phenylene ether) (PPO640, manufactured by SABIC Innovative Plastic) and 20 parts by mass of polystyrene (679, manufactured by PS Japan Co., Ltd.) was used, and melt spinning was performed in the same manner as in Example 1, except that the nozzle shape and spinning conditions were changed as shown in Table 1. However, spinnability was very poor, and it was only by increasing the single-hole output rate to 0.242 g / min that a fiber with a single yarn fineness of 78.4 dtex could be obtained at a spinning speed of 30 m / min. The fiber properties of the obtained fiber are shown in Table 1.

[0120] [Table 1]

[0121] In Table 1, "PPE(646)" stands for poly(2,6-dimethyl-1,4-phenylene ether) (PPO646, glass transition temperature (Tg): 221°C, manufactured by SABIC Innovative Plastic), "PPE(640)" stands for poly(2,6-dimethyl-1,4-phenylene ether) (PPO640, glass transition temperature (Tg): 220°C, manufactured by SABIC Innovative Plastic), "PPE(SA120)" stands for poly(2,6-dimethyl-1,4-phenylene ether) (PPOSA120, glass transition temperature (Tg): 159°C, manufactured by SABIC Innovative Plastic), and "PS(679)" stands for polystyrene (679, manufactured by PS Japan Co., Ltd.).

[0122] As shown in Table 1, in the examples of the present invention, although the polyphenylene ether content is high, melt spun fibers were obtained because low Tg polyphenylene ether was used as the raw material. The melt spun fibers obtained in the examples were excellent in maximum point stress and maximum point elongation. In addition, in Examples 2 to 5, thin fibers with a single yarn fineness of 15 dtex or less were obtained, and further, in Example 5, a very thin fiber with a single yarn fineness of 3.4 dtex was obtained by setting the spinning speed to 700 m / min.

[0123] In contrast, melt spun fibers could not be obtained in Comparative Example 1. This is believed to be because Comparative Example 1 did not contain low Tg polyphenylene ether, and therefore the melt viscosity was too high to extrude the polymer from the gear pump. In Comparative Example 2, despite the incorporation of polystyrene in poly(2,6-dimethyl-1,4-phenylene ether), spinnability was very poor and only very thick fibers could be obtained. Moreover, the obtained fibers had low strength, elongation, and glass transition temperature.

[0124] <Polyphenylene ether melt-spun short fibers> Example 8 The melt spun fibers obtained in Example 1 were doubling to form a tow, which was then cut into short fibers having a fiber length of 50 mm using a guillotine cutter.

[0125] (1) Tensile strength and elongation Measurements were made in accordance with JIS L1013 8.5.1. The stress at the maximum load was taken as the tensile strength, and the elongation at the maximum load was taken as the tensile elongation.

[0126] (2) High temperature shrinkage rate The fiber length (X cm) of a 5 cm-long short fiber cut out without fixing the ends was measured after it was placed in an air thermostatic chamber kept at 190°C for 10 minutes, after which the fiber length was calculated using the following formula. However, if it is not possible to obtain a 5 cm-long short fiber, the length may be changed as appropriate. High temperature shrinkage rate (%) = <x 5>×100 (When 5 cm short fibers cannot be obtained, <X / length before treatment> × 100)

[0127] (3) Equilibrium moisture content In accordance with JIS L1013, the sample was dried to absolute dryness in an atmosphere of 120 °C, then adjusted for 72 hours at a temperature of 20 °C and a relative humidity of 65% RH, and the moisture content contained in the sample with respect to the mass of the sample in the absolute dry state was calculated and expressed as a percentage (%).

[0128]

Table 2

[0129] <Flame-resistant short fibers> Example 9 The melt-spun fibers obtained in Example 1 were combined into a bundle and made into a tow shape, and then cut into 50 mm fiber lengths with a guillotine cutter to obtain short fibers. The obtained short fibers were heat-treated in an air atmosphere in the order of 200 °C × 120 min, 210 °C × 20 min, 220 °C × 20 min, 250 °C × 120 min, 280 °C × 120 min, and 320 °C × 120 min to produce flame-resistant short fibers.

[0130] (1) Tensile strength, elongation at break Measured in accordance with JIS L1013 8.5.1. The stress at the maximum load was defined as the tensile strength, and the elongation rate at the maximum load was defined as the elongation at break.

[0131] (2) High-temperature shrinkage rate The flame-resistant short fibers cut into 5 cm were held in an air thermostat maintained at 190 °C for 10 minutes without fixing the ends, and then calculated using the following formula from the fiber length (X cm). However, when 5 cm flame-resistant short fibers cannot be obtained, the length may be appropriately changed for measurement. High-temperature shrinkage rate (%) = <x 5>×100 (When the 5 cm flame-retardant short fibers cannot be obtained, <X / length before treatment> × 100)

[0132] (3) Equilibrium moisture content In accordance with JIS L1013, after the sample was dried to absolute dryness in an atmosphere of 120 °C, it was adjusted for 72 hours at a temperature of 20 °C and a relative humidity of 65% RH, and the moisture content contained in the sample with respect to the mass of the sample in the absolute dry state was calculated and expressed as a percentage (%).

[0133] (4) Generated gas Measured in accordance with STM E662.

[0134] (5) Smoke generation amount Measured in accordance with BSS 7239.

[0135]

Table 3

[0136] <Paper formed from polyphenylene ether melt-spun fibers> Example 10 The melt-spun fibers obtained in Example 1 were combined into a bundle and cut into short fibers with a fiber length of 5 mm using a guillotine cutter. Wet papermaking was performed using the obtained short fibers. During papermaking, the surfactant "Maker Surfactant MK-37" manufactured by Meisei Chemical Industry Co., Ltd. was used. The obtained paper sheet was placed on an aluminum foil and washed with approximately 5 L of ion-exchanged water using a spray. Then, it was sandwiched between aluminum foils and calendered at a temperature of 210 °C, a linear pressure of 30 kg / cm (calculated as a 25 cm width), and a roller speed of 1.0 m / min to produce paper (basis weight: 320 g / cm 2 ).

[0137] (1) Tensile strength, elongation at break Measured in accordance with JIS L1013 8.5.1. Using a sample with a width of 25 mm and a length of 100 mm, the distance between chucks was 50 mm, and the tensile speed was 100 mm / min. The elongation at break was defined as the elongation when the strength was maximum.

[0138] (2) LOI value Measurements were made in accordance with JIS L 1091 E. The oxygen index was determined when the flame continued to burn for 50 mm or more, and the heat source for the igniter was propane gas.

[0139] (3) Dielectric constant A 50 μm thick sample was measured using a dielectric constant measuring device manufactured by AET Corporation in accordance with JIS C2565 using the cavity resonator method (TM mode). The frequency was 10 GHz. The sample size was 3 mm wide and 80 mm long.

[0140] (4) Equilibrium moisture content In accordance with JIS L1013, the samples were dried in an atmosphere at 120°C, and then conditioned at a temperature of 20°C and a relative humidity of 65%RH for 72 hours. The moisture content of the samples relative to the mass of the samples in the dried state was calculated and expressed as a percentage (%).

[0141] (5) High temperature shrinkage rate The length of the paper (X cm) after cutting the paper into a 10 cm square and leaving the ends unfixed in an air thermostatic chamber kept at 190°C for 10 minutes was calculated using the following formula. High temperature shrinkage rate (%) = <x 10>×100

[0142] [Table 4]

[0143] <Flame-retardant paper> Example 11 The paper produced in Example 10 was heat-treated in an air atmosphere in the following order: 200°C x 120 min, 210°C x 20 min, 220°C x 20 min, 250°C x 120 min, 280°C x 120 min, and 320°C x 120 min to produce flame-resistant paper.

[0144] (1) Tensile strength and elongation Measurements were made in accordance with JIS L1013 8.5.1. Samples 25 mm wide and 100 mm long were used, with a chuck distance of 50 mm and a tensile speed of 100 mm / min. The tensile elongation was defined as the elongation at which the strength was at its maximum.

[0145] (2) Gas generated Measured in accordance with STM E662.

[0146] (3) Amount of smoke produced Measured in accordance with BSS 7239.

[0147] (4) LOI value Measurements were made in accordance with JIS L 1091 E. The oxygen index was determined when the flame continued to burn for 50 mm or more, and the heat source for the igniter was propane gas.

[0148] (5) Dielectric constant A 50 μm thick sample was measured using a dielectric constant measuring device manufactured by AET Corporation in accordance with JIS C2565 using the cavity resonator method (TM mode). The frequency was 10 GHz. The sample size was 3 mm wide and 80 mm long.

[0149] (6) Equilibrium moisture content In accordance with JIS L1013, the samples were dried in an atmosphere at 120°C, and then conditioned at a temperature of 20°C and a relative humidity of 65%RH for 72 hours. The moisture content of the samples relative to the mass of the samples in the dried state was calculated and expressed as a percentage (%).

[0150] (7) High temperature shrinkage rate The flame-retardant paper was cut into 10 cm square pieces and left in an air thermostatic chamber kept at 190°C for 10 minutes without fixing the ends. The paper length (X cm) was then calculated using the following formula. High temperature shrinkage rate (%) = <x 10>×100

[0151] [Table 5]

[0152] <Fabrics formed from polyphenylene ether melt-spun fibers> Example 12 The melt-spun fibers obtained in Example 1 were woven to obtain a fabric with a basis weight of 150 g / m 2 Thus, a plain weave fabric of 100 g was obtained.

[0153] (1) LOI value Measurements were made in accordance with JIS L 1091 E. The oxygen index was determined when the flame continued to burn for 50 mm or more, and the heat source for the igniter was propane gas.

[0154] (2) High temperature shrinkage rate The fabric was cut into a 10 cm square and held in an air thermostatic chamber kept at 190° C. for 10 minutes without fixing the ends. The fabric length (X cm) was then calculated using the following formula. High temperature shrinkage rate (%) = <x 10>×100

[0155] [Table 6]

[0156] <Flame resistant fabric> Example 13 The plain weave fabric produced in Example 12 was heat treated in an air atmosphere in the following order: 200°C x 120 min, 210°C x 20 min, 220°C x 20 min, 250°C x 120 min, 280°C x 120 min, and 320°C x 120 min to produce a flame-resistant fabric.

[0157] (1) Gas generated Measured in accordance with STM E662.

[0158] (2) Amount of smoke produced Measured in accordance with BSS 7239.

[0159] (3) LOI value Measurements were made in accordance with JIS L 1091 E. The oxygen index was determined when the flame continued to burn for 50 mm or more, and the heat source for the igniter was propane gas.

[0160] (4) High temperature shrinkage rate The flame-resistant fabric was cut into a 10 cm square and held in an air thermostatic chamber kept at 190°C for 10 minutes without fixing the ends. The fabric length (X cm) was calculated using the following formula. High temperature shrinkage rate (%) = <x 10>×100

[0161] [Table 7] [Explanation of symbols]

[0162] 1 Hopper 2. Extruder 3 Gear pump 4. Filters 5. Spinning nozzle 6 Filter media 7. Insulation space 8. Introduction of inert gas 9 Heating Torch< / x> < / x> < / x> < / x> < / x> < / x>

Claims

1. A polyphenylene ether melt-spun fiber, characterized in that the content of the polyphenylene ether component is 95% by mass or more of all components forming the fiber, and the glass transition temperature is 180° C. or more and 205° C. or less, The polyphenylene ether melt spun fiber is a flame-retardant staple fiber.

2. 2. The polyphenylene ether melt spun fiber according to claim 1, wherein the single fiber fineness is 1.0 dtex or more and 100 dtex or less.

3. 3. The polyphenylene ether melt spun fiber according to claim 1, wherein the maximum point elongation is 25% or more and 120% or less.

4. A paper formed from the polyphenylene ether melt-spun fibers of any one of claims 1 to 3.

5. 5. The paper according to claim 4, characterized in that the paper is a flame retardant paper.

6. A fabric formed from the polyphenylene ether melt spun fibers of any one of claims 1 to 3.

7. The fabric of claim 6, wherein the fabric is a flame retardant fabric.

8. 1. A method for producing polyphenylene ether melt spun fibers, comprising the steps of: A step of melt-extruding a raw material resin composition containing a polyphenylene ether component having a glass transition temperature of less than 170° C. and a polyphenylene ether component having a glass transition temperature of 180° C. or more; The molten raw material resin composition is discharged from a spinning nozzle to spin the composition, A method for producing polyphenylene ether melt spun fibers, characterized in that the content of polyphenylene ether components in the obtained polyphenylene ether melt spun fibers is 95 mass % or more of all components forming the fibers.

9. 9. The method for producing polyphenylene ether melt spun fibers according to claim 8, wherein the content of the polyphenylene ether component having a glass transition temperature of less than 170°C is 5 mass% or more in the polyphenylene ether component contained in the raw material resin composition.

10. The method for producing polyphenylene ether melt spun fibers according to claim 8 or 9, characterized in that the spinning speed is 100 to 1000 m / min.

11. The method for producing polyphenylene ether melt spun fibers according to any one of claims 8 to 10, characterized in that the temperature of the spinning nozzle is 280 to 320°C.

12. The method for producing polyphenylene ether melt spun fibers according to any one of claims 8 to 11, characterized in that spinning is carried out while introducing an inert gas into the region immediately below the spinning nozzle.

Citation Information

Patent Citations

  • Polyphenylene ether formulation with high fluidity

    JP2003531234A

  • Fiber, fiber assembly and molding of fiber assembly

    JP2004190156A

  • Ultrafine polyphenylene ether fiber and its fiber aggregate

    JP2008069478A

  • Fiber, fiber structure, and method for producing them

    JP2008138294A

  • Poly(phenylene ether) fiber, method of production, and article made from same

    JP2017502179A