Preparation method of high-thermal-conductivity polyarylene ether nitrile film

High thermal conductivity polyarylene ether nitrile films were prepared by electrospinning and hot pressing, which solved the problems of low thermal conductivity and compatibility, and achieved a balance between high thermal conductivity and mechanical properties, making them suitable for high-precision thermal conductivity applications.

CN118957882APending Publication Date: 2024-11-15UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411044155.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing polymer materials have low thermal conductivity, making it difficult to meet the application requirements of high-precision thermal conductivity fields. Furthermore, after being filled with thermally conductive fillers, they suffer from compatibility issues and a decrease in mechanical properties.

Method used

High thermal conductivity polyarylene ether nitrile films were prepared by electrospinning and hot pressing. The spinning solution was prepared by exfoliating boron nitride nanosheets and bisphenol A type polyarylene ether nitrile. After electrospinning, the solution was overlaid to form a uniformly dispersed fiber film. Then, hot pressing was performed to construct a thermally conductive network.

Benefits of technology

The thermal conductivity of polyaryletheronitrile films is improved while maintaining high strength and electrical insulation properties, making them suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957882A_ABST
    Figure CN118957882A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-thermal-conductivity polyarylene ether nitrile film. The preparation method comprises the following steps: 1) preparing a BPA-PEN spinning solution and a BNNS dispersion solution; (2) orienting the fibers through electrostatic spinning to obtain a BPA-PEN fiber membrane; 3) electrostatic spraying of the BNNS dispersion liquid on the surface of the fiber membrane is carried out, such that a BPA-PEN-coated BNNS stacked spraying fiber membrane is formed; and 4) carrying out hot pressing on the BPA-PEN-coated BNNS stack-spray fiber membrane to obtain the high-thermal-conductivity polyarylene ether nitrile film. BPA-PEN is selected as matrix resin for electrostatic spinning to realize orientation of fibers, a matrix is filled with exfoliated boron nitride nanosheets called white graphite, BNNS is electrostatically sprayed on the surfaces of the fibers, and then a fiber film obtained by repeated stack spraying is subjected to hot pressing to obtain the high-thermal-conductivity polyarylene ether nitrile film, so that construction of a thermal conductive network is further promoted, and the thermal conductivity of the high-thermal-conductivity polyarylene ether nitrile film is improved. The heat conduction path of the fiber film is improved, and the polyarylene ether nitrile film with high heat conduction coefficient and excellent comprehensive performance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material preparation, and relates to the preparation of nanocomposite materials and the study of their thermal properties, and specifically to a method for preparing a high thermal conductivity poly(arylethernitrile) film, and in particular to a method for preparing a nanofiber film by electrospinning and then hot pressing. Background Art

[0002] Due to the trend of miniaturization, automation and integration of microelectronic components and advanced mobile devices, heat dissipation has gradually become an issue that cannot be ignored. The heat generation and accumulation problems in the operation of electronic equipment and circuits may damage the system efficiency and shorten the life of electronic components by half. At the same time, a large amount of heat accumulation may cause problems such as circuit aging and leakage. Therefore, it is urgent to develop high thermal conductivity materials.

[0003] Polymers usually have the advantages of high temperature resistance, light weight, good processability and low cost, and have been widely used in electronic packaging and other fields. With the diversification of the performance requirements of polymer materials used in 5G high-frequency communications, it is often difficult for a single material to simultaneously meet the requirements of thermal conductivity, mechanical properties, dielectric properties, processability and other aspects. Therefore, composite is one of the important development trends of functional polymer materials in the future. Specifically, the heat dissipation capacity of polymer-based composite materials depends on the thermal conductivity of polymer-based composite materials. The higher the value, the more effective the heat dissipation capacity. However, the thermal conductivity constant of most polymers is only 0.1-0.5W / m·K, which greatly limits the application of polymer materials in heat transfer devices. After investigation, it was found that the main methods to improve the thermal conductivity of polymers are intrinsic improvement and filling improvement. Specifically, intrinsic thermal conductivity is mainly improved by changing the orientation, crystallization, hydrogen bonding and other force angles of polymer molecular chains; filler thermal conductivity is mainly improved by adding metals (Ag\Cu\Al, etc.), ceramics (BN\AlN\SiC\Si3N4\Al2O3, etc.), carbon materials (CNTs\GO\GNSs\GNPs\CF), etc. and mixing them into resins with specific requirements for research.

[0004] However, it is difficult to form a thermal conductive path by filling a small amount of filler into the matrix resin. Electrospinning is a promising method for preparing thermally conductive composite materials. It can arrange directional thermally conductive fillers in the fibers in a uniformly dispersed and highly oriented manner, thereby improving the thermal conductive network and increasing the thermal conductivity of the material.

[0005] Polyarylene ether nitrile (PEN) is a type of functional polymer material with excellent mechanical properties, high temperature resistance, wear resistance and corrosion resistance. In recent years, it has been widely used in military, aerospace and other fields. However, polymers conduct heat through phonon diffusion, and factors such as molecular chain entanglement, impurities, and voids make the thermal conductivity of the polymer itself very low. The low thermal conductivity limits its application in the field of high-precision thermal conductivity.

[0006] In recent years, there are few reports on the research of high thermal conductivity poly(arylether nitrile) composite materials. According to the investigation, patent CN201610454177 discloses a poly(arylether nitrile) / nano-aluminum oxide composite material and its preparation method. By changing the mass ratio of filler to matrix resin, the film is formed by casting method. The method is simple and feasible, but the formation of its thermal conductive path is not good, resulting in the highest thermal conductivity coefficient in the system being lower than 0.5W / m·K. In addition, due to the simple blending preparation, there are also problems such as poor compatibility, which leads to the destruction of mechanical properties; CN106046767A discloses a preparation technology of in-situ thermal reduction poly(arylether nitrile) / graphene oxide high thermal conductivity composite film, which uses the excellent thermal conductivity of graphene oxide to improve the thermal conductivity of the composite film (34W / m·K), and improves the comprehensive performance through hot stretching technology, but because the increase in graphene content will greatly damage the insulation of the film, it cannot be used as an interlayer dielectric in the electronic field.

[0007] Therefore, in combination with the above-mentioned problems, while improving the thermal conductivity of polyarylethernitrile, the high strength, high modulus, high decomposition temperature, high glass transition temperature and stable electrical properties of the polyarylethernitrile film can be maintained. This undoubtedly provides a method for preparing a high thermal conductivity polyarylethernitrile film with excellent comprehensive performance, which is also a problem that technical personnel in this field urgently need to solve. Summary of the invention

[0008] The purpose of the present invention is to propose a method for preparing a high thermal conductivity poly(arylethernitrile) film in view of the problems existing in the background technology. The present invention prepares a high thermal conductivity poly(arylethernitrile) film by electrospinning and hot pressing, wherein the exfoliated boron nitride nanosheets (BNNS) and bisphenol A poly(arylethernitrile) (BPA-PEN) are configured into a spinning solution, the fibers are oriented by electrospinning, the BNNS are evenly dispersed on the fibers, and the fiber film is hot pressed to further promote the construction of a thermal conductive network, thereby improving the thermal conductivity of the film. The obtained film has excellent comprehensive performance, and provides a basic theoretical and operational basis for large-scale production of the high thermal conductivity insulating poly(arylethernitrile) film with excellent performance.

[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing a high thermal conductivity poly(arylene ether nitrile) film comprises the following steps:

[0011] Step 1, preparing BPA-PEN@BNNS (bisphenol A type poly (arylene ether nitrile @ boron nitride) spray-coated fiber membrane;

[0012] 1.1 Add BPA-PEN (bisphenol A polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker and stir magnetically at 70-80°C for 1-2 hours to obtain a BPA-PEN spinning solution of 0.05 g / mL to 0.15 g / mL;

[0013] 1.2 Add BNNS (boron nitride) to DMF (N, N-dimethylformamide) and disperse by ultrasonic at room temperature for 8 to 12 hours to obtain a BNNS dispersion with a mass concentration of 0.1 g / mL to 0.3 g / mL;

[0014] 1.3 The spinning solution obtained in step 1.1 is placed in a syringe, the injection speed of the syringe pump is set to 1-3 mL / h, the applied voltage is set to 25-27 KV, the working distance between the syringe and the receiver is 15-20 cm, the rotation speed of the receiver is 200-400 rpm / min, and electrospinning is performed for 1.5 h to 2 h to obtain a BPA-PEN fiber membrane;

[0015] 1.4 Place the BNNS dispersion obtained in step 1.2 into a syringe, set the injection speed of the syringe pump to 1-3 mL / h, the applied voltage to 25-27 KV, the working distance between the syringe and the receiver to 15-20 cm, the speed of the receiver to 200-400 rpm / min, and continue electrostatic spraying on the fiber membrane obtained in step 1.3 for 1.5 h to 2 h;

[0016] 1.5 Repeat steps 1.3 to 1.4 4 to 6 times to obtain BPA-PEN@BNNS spray-coated fiber membrane;

[0017] Step 2, preparing a poly(arylene ether nitrile) hot-pressed composite film;

[0018] The BPA-PEN@BNNS spray-coated fiber membrane obtained in step 1.5 is peeled off from the aluminum foil, and then placed in a mold and hot-pressed for 10 to 20 minutes at 10 to 20 MPa and 230 to 270°C to obtain a BPA-PEN@BNNS spray-coated hot-pressed membrane; after the mold is naturally cooled to room temperature, the film is taken out to obtain the polyarylether nitrile film.

[0019] It should be noted that the process parameters listed above are obtained by the inventors through a large number of experiments. Among them, the BPA-PEN mass concentration, solution stirring time and temperature will have a direct impact on the uniformity and orientation of the fiber membrane. If they deviate from the limits of this application, the quality of the final product will not meet the expected purpose.

[0020] The present invention provides a method for preparing a high thermal conductivity poly(arylene ether nitrile) film, and its mechanism of action is as follows:

[0021] First, BPA-PEN was selected as the matrix resin for electrospinning, and a uniform and oriented fiber membrane was obtained, and then hot pressed to obtain a BPA-PEN film as a control sample; secondly, the overlapping spraying method was selected, and BPA-PEN was first electrospun to obtain a uniform and oriented fiber membrane, and then the exfoliated boron nitride nanosheets (BNNS) known as white graphite were added to fill the matrix by electrostatic spraying. During the spraying process, BNNS dispersed along the axial direction of the polymer fiber, and the distance between the fillers was reduced and overlapped to form a thermal conduction path, so the thermal conductivity and electrical properties were increased. In summary, BPA-PEN@BNNS was prepared into a fiber membrane by electrospinning, and then hot pressed to obtain a film. By changing the contact mode between the fiber membrane and BNNS, the contact distance between BNNS and BNNS was reduced, thereby improving the thermal conduction path and increasing the thermal conductivity.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention provides a method for preparing a high thermal conductivity poly(arylene ether nitrile) film, wherein BPA-PEN is selected as a matrix resin for electrostatic spinning to achieve fiber orientation, and a matrix is ​​filled with exfoliated boron nitride nanosheets (BNNS) known as white graphite. BNNS is electrostatically sprayed on the fiber surface, and then the fiber membrane obtained by repeated spraying is hot-pressed to obtain a high thermal conductivity poly(arylene ether nitrile) film, thereby further promoting the construction of a thermal conductive network, improving the thermal conductive path of the fiber membrane, and obtaining a poly(arylene ether nitrile) film with high thermal conductivity and excellent comprehensive performance.

[0024] 2. The present invention proposes a method for obtaining a high thermal conductivity poly(arylene ether nitrile) film by electrospinning and hot pressing. The preparation process is simple, the cost is low, and large-scale production and application can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0026] Figure 1 The surface of the BPA-PEN fiber membrane (a) obtained in Comparative Example 1, the surface of the BPA-PEN@BNNS mixed spray fiber membrane (b) obtained in Comparative Example 2, the surface of the fiber membrane (c) obtained in Comparative Example 3, the cross-section of the BPA-PEN fiber membrane (d) obtained in Comparative Example 1, the cross-section of the BPA-PEN@BNNS mixed spray fiber membrane (e) obtained in Comparative Example 2, and the cross-sectional morphology of the BPA-PEN@BNNS stacked spray fiber membrane (f) obtained in Example 1;

[0027] Figure 2 Out-of-plane thermal conductivity (a) and in-plane thermal conductivity (b) of the high thermal conductive films prepared in Examples 1 to 3 and the films prepared in Comparative Examples 1 to 4;

[0028] Figure 3 The breakdown strength of the high thermal conductive films prepared in Examples 1 to 3 and the films prepared in Comparative Examples 1 to 4 is characterized. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The embodiment of the invention discloses a method for preparing a high thermal conductive poly(arylene ether nitrile) film.

[0031] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0032] The technical solution of the present invention will be further described below in conjunction with specific embodiments.

[0033] Example 1

[0034] A method for preparing a high thermal conductivity poly(arylene ether nitrile) film comprises the following steps:

[0035] Step 1, preparing BPA-PEN@BNNS (bisphenol A type poly (arylene ether nitrile @ boron nitride) spray-coated fiber membrane;

[0036] 1.1 Add BPA-PEN (bisphenol A polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker and stir magnetically at 75°C for 1 h to obtain a 0.1 g / mL BPA-PEN spinning solution;

[0037] 1.2 Add BNNS (boron nitride) into DMF (N, N-dimethylformamide) and disperse by ultrasonic at room temperature for 12 hours to obtain a BNNS dispersion with a mass concentration of 0.1 g / mL;

[0038] 1.3 The spinning solution obtained in step 1.1 was placed in a syringe, the injection speed of the syringe pump was set to 2 mL / h, the applied voltage was set to 25 KV, the working distance between the syringe and the receiver was set to 18 cm, the rotation speed of the receiver was set to 200 rpm / min, and electrospinning was performed for 1.5 h to obtain a BPA-PEN fiber membrane;

[0039] 1.4 Place the BNNS dispersion obtained in step 1.2 into a syringe, set the injection speed of the syringe pump to 2 mL / h, the applied voltage to 25 KV, the working distance between the syringe and the receiver to 18 cm, the speed of the receiver to 200 rpm / min, and continue electrostatic spraying on the fiber membrane obtained in step 1.3 for 1.5 h;

[0040] 1.5 Repeat steps 1.3 to 1.4 for 4 times to obtain BPA-PEN@BNNS spray-coated fiber membrane;

[0041] Step 2, preparing a poly(arylene ether nitrile) hot-pressed composite film;

[0042] The BPA-PEN@BNNS spray-coated fiber membrane obtained in step 1.5 is peeled off from the aluminum foil, and then placed in a mold and hot-pressed at 20 MPa and 260°C for 10 minutes to obtain a BPA-PEN@BNNS spray-coated hot-pressed membrane; after the mold is naturally cooled to room temperature, the film is taken out to obtain the polyarylether nitrile film.

[0043] The high thermal conductivity poly(arylene ether nitrile) film obtained in Example 1 has an in-plane thermal conductivity of 3.26 W / m·K, an out-of-plane thermal conductivity of 0.38 W / m·K, and a breakdown strength of 92.32 KV / mm.

[0044] Example 2

[0045] Step 1, preparing BPA-PEN@BNNS (bisphenol A type poly (arylene ether nitrile @ boron nitride) spray-coated fiber membrane;

[0046] 1.1 Add BPA-PEN (bisphenol A polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker and stir magnetically at 75°C for 1 h to obtain a 0.1 g / mL BPA-PEN spinning solution;

[0047] 1.2 Add BNNS (boron nitride) into DMF (N, N-dimethylformamide) and disperse by ultrasonic at room temperature for 12 hours to obtain a BNNS dispersion with a mass concentration of 0.2 g / mL;

[0048] 1.3 The spinning solution obtained in step 1.1 was placed in a syringe, the injection speed of the syringe pump was set to 2 mL / h, the applied voltage was set to 25 KV, the working distance between the syringe and the receiver was set to 18 cm, the rotation speed of the receiver was set to 200 rpm / min, and electrospinning was performed for 1.5 h to obtain a BPA-PEN fiber membrane;

[0049] 1.4 Place the BNNS dispersion obtained in step 1.2 into a syringe, set the injection speed of the syringe pump to 2 mL / h, the applied voltage to 25 KV, the working distance between the syringe and the receiver to 18 cm, the speed of the receiver to 200 rpm / min, and continue electrostatic spraying on the fiber membrane obtained in step 1.3 for 1.5 h;

[0050] 1.5 Repeat steps 1.3 to 1.4 for 4 times to obtain BPA-PEN@BNNS spray-coated fiber membrane;

[0051] Step 2, preparing a poly(arylene ether nitrile) hot-pressed composite film;

[0052] The BPA-PEN@BNNS spray-coated fiber membrane obtained in step 1.5 is peeled off from the aluminum foil, and then placed in a mold and hot-pressed at 20 MPa and 260°C for 10 minutes to obtain a BPA-PEN@BNNS spray-coated hot-pressed membrane; after the mold is naturally cooled to room temperature, the film is taken out to obtain the polyarylether nitrile film.

[0053] The high thermal conductivity poly(arylene ether nitrile) film obtained in Example 2 has an in-plane thermal conductivity of 4.15 W / m·K, an out-of-plane thermal conductivity of 0.49 W / m·K, and a breakdown strength of 84.86 KV / mm.

[0054] Example 3

[0055] Step 1, preparing BPA-PEN@BNNS (bisphenol A type poly (arylene ether nitrile @ boron nitride) spray-coated fiber membrane;

[0056] 1.1 Add BPA-PEN (bisphenol A polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker and stir magnetically at 75°C for 1 h to obtain a 0.1 g / mL BPA-PEN spinning solution;

[0057] 1.2 Add BNNS (boron nitride) into DMF (N, N-dimethylformamide) and disperse by ultrasonic at room temperature for 12 hours to obtain a BNNS dispersion with a mass concentration of 0.3 g / mL;

[0058] 1.3 The spinning solution obtained in step 1.1 was placed in a syringe, the injection speed of the syringe pump was set to 2 mL / h, the applied voltage was set to 25 KV, the working distance between the syringe and the receiver was set to 18 cm, the rotation speed of the receiver was set to 200 rpm / min, and electrospinning was performed for 1.5 h to obtain a BPA-PEN fiber membrane;

[0059] 1.4 Place the BNNS dispersion obtained in step 1.2 into a syringe, set the injection speed of the syringe pump to 2 mL / h, the applied voltage to 25 KV, the working distance between the syringe and the receiver to 18 cm, the speed of the receiver to 200 rpm / min, and continue electrostatic spraying on the fiber membrane obtained in step 1.3 for 1.5 h;

[0060] 1.5 Repeat steps 1.3 to 1.4 twice to obtain the BPA-PEN@BNNS spray-coated fiber membrane;

[0061] Step 2, preparing a poly(arylene ether nitrile) hot-pressed composite film;

[0062] The BPA-PEN@BNNS spray-coated fiber membrane obtained in step 1.5 is peeled off from the aluminum foil, and then placed in a mold and hot-pressed at 20 MPa and 260°C for 10 minutes to obtain a BPA-PEN@BNNS spray-coated hot-pressed membrane; after the mold is naturally cooled to room temperature, the film is taken out to obtain the polyarylether nitrile film.

[0063] The high thermal conductivity poly(arylene ether nitrile) film obtained in Example 3 has an in-plane thermal conductivity of 5.98 W / m·K, an out-of-plane thermal conductivity of 0.62 W / m·K, and a breakdown strength of 69.52 KV / mm.

[0064] In addition, in order to further illustrate the excellent effects of the technical solution of the present invention, the present invention also provides the following comparative examples.

[0065] Comparative Example 1

[0066] Step 1, add BPA-PEN (bisphenol A type polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker, stir magnetically at 75° C. for 1 h to obtain a 0.1 g / mL BPA-PEN spinning solution;

[0067] Step 2, the spinning solution was placed in a syringe, the injection speed of the syringe pump was set to 2 mL / h, the applied voltage was set to 25 KV, the working distance between the syringe and the receiver was 18 cm, the rotation speed of the receiver was set to 200 rpm / min, and electrospinning was performed for 1.5 h to obtain a BPA-PEN fiber membrane;

[0068] Step 3, peeling the BPA-PEN fiber membrane from the aluminum foil, and then placing it in a mold and hot pressing it at 20 MPa and 260° C. for 10 minutes to obtain a BPA-PEN hot-pressed film; after the mold is naturally cooled to room temperature, the film is taken out to obtain a polyarylethernitrile film.

[0069] The poly(arylene ether nitrile) film obtained in Comparative Example 1 has an in-plane thermal conductivity of 0.54 W / m·K, an out-of-plane thermal conductivity of 0.067 W / m·K, and a breakdown strength of 90.45 KV / mm.

[0070] Comparative Example 2

[0071] Step 1, add BPA-PEN (bisphenol A type polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker, stir magnetically at 75° C. for 1 h to obtain a 0.1 g / mL BPA-PEN solution;

[0072] Step 2, adding BNNS (boron nitride) into DMF (N, N-dimethylformamide), and ultrasonically dispersing at room temperature for 12 hours to obtain a BNNS dispersion with a mass concentration of 0.1 g / mL;

[0073] Step 3, mixing the BPA-PEN solution and the BNNS dispersion, stirring at 75° C. for 1 h, to obtain a BPA-PEN@BNNS mixed spray spinning solution;

[0074] Step 4, placing the BPA-PEN@BNNS mixed spray spinning solution obtained in step 3 into a syringe, setting the injection speed of the syringe pump to 2 mL / h, the applied voltage to 25 KV, the working distance between the syringe and the receiver to 18 cm, the rotation speed of the receiver to 200 rpm / min, and performing electrospinning for 2.5 hours to obtain a BPA-PEN@BNNS mixed spray fiber membrane;

[0075] Step 5: peel off the obtained BPA-PEN@BNNS mixed spray fiber membrane from the aluminum foil, and then put it into a mold and hot press it at 20 MPa and 260°C for 10 minutes to obtain a BPA-PEN@BNNS mixed spray hot-pressed film; after the mold is naturally cooled to room temperature, take out the film to obtain a BPA-PEN@BNNS mixed spray fiber membrane.

[0076] The mixed spray fiber membrane obtained in Comparative Example 2 has an in-plane thermal conductivity of 2.21 W / m·K, an out-of-plane thermal conductivity of 0.21 W / m·K, and a breakdown strength of 87.23 KV / mm.

[0077] Comparative Example 3

[0078] Step 1, add BPA-PEN (bisphenol A type polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker, stir magnetically at 75° C. for 1 h to obtain a 0.1 g / mL BPA-PEN spinning solution;

[0079] Step 2, adding BNNS (boron nitride) to DMF (N, N-dimethylformamide), and ultrasonically dispersing at room temperature for 12 hours to obtain a BNNS dispersion with a mass concentration of 0.1 g / mL;

[0080] Step 3, placing the spinning solution obtained in step 1 into a syringe, setting the injection speed of the syringe pump to 2 mL / h, the applied voltage to 25 KV, the working distance between the syringe and the receiver to 18 cm, the rotation speed of the receiver to 200 rpm / min, and performing electrospinning for 1.5 h to obtain a BPA-PEN fiber membrane;

[0081] Step 4: Place the BNNS dispersion obtained in step 2 into a syringe, set the injection rate of the syringe pump to 2 mL / h, the applied voltage to 25 KV, the working distance between the syringe and the receiver to 18 cm, the speed of the receiver to 200 rpm / min, and continue electrostatic spraying on the fiber membrane obtained in step 3 for 1.5 h;

[0082] Step 5, repeat the process of steps 3 to 4 for 4 times to obtain the BPA-PEN@BNNS spray-coated fiber membrane;

[0083] Step 6: peel off the BPA-PEN@BNNS spray-coated fiber membrane obtained in step 5 from the aluminum foil to obtain a spray-coated fiber membrane.

[0084] The in-plane thermal conductivity of the spray-laid fiber membrane obtained in Comparative Example 3 is 0.47 W / m·K, the out-of-plane thermal conductivity is 0.053 W / m·K, and the breakdown strength is 10.77 KV / mm.

[0085] Comparative Example 4

[0086] Step 1, add BPA-PEN (bisphenol A type polyarylether nitrile) and DMF (N, N-dimethylformamide) into a beaker, stir magnetically at 75° C. for 1 h to obtain a 0.1 g / mL BPA-PEN solution;

[0087] Step 2, adding BNNS (boron nitride) to DMF (N, N-dimethylformamide), and ultrasonically dispersing at room temperature for 12 hours to obtain a BNNS dispersion with a mass concentration of 0.1 g / mL;

[0088] Step 3, mixing the BPA-PEN solution and the BNNS dispersion, stirring at 75° C. for 1 h, to obtain a BPA-PEN@BNNS mixed spray spinning solution;

[0089] Step 4, placing the BPA-PEN@BNNS mixed spray spinning solution obtained in step 3 into a syringe, setting the injection speed of the syringe pump to 2 mL / h, the applied voltage to 27 KV, the working distance between the syringe and the receiver to 18 cm, the rotation speed of the receiver to 200 rpm / min, and performing electrospinning for 2.5 hours to obtain a BPA-PEN@BNNS mixed spray fiber membrane;

[0090] Step 5: peel off the obtained BPA-PEN@BNNS mixed spray fiber membrane from the aluminum foil, and then put it into a mold and hot press it at 20 MPa and 260°C for 10 minutes to obtain a BPA-PEN@BNNS mixed spray hot-pressed film; after the mold is naturally cooled to room temperature, take out the film to obtain a BPA-PEN@BNNS mixed spray fiber membrane.

[0091] The mixed spray fiber membrane obtained in Comparative Example 4 has an in-plane thermal conductivity of 2.69 W / m·K, an out-of-plane thermal conductivity of 0.25 W / m·K, and a breakdown strength of 88.84 KV / mm.

[0092] Thermal conductivity: The peeled boron nitride nanosheets have a large specific surface area, and the unique layer structure can effectively reduce the interfacial thermal resistance with the matrix resin and improve the thermal conductivity efficiency; therefore, compared with comparative example 1, the thermal conductivity of Examples 1-3 is improved as a whole; compared with comparative example 2, the electrostatic spraying process of Examples 1-3 is different. The spraying method of the examples makes the BNNS oriented along the PEN, the orientation degree is increased, and the heat transfer is enhanced.

[0093] Depend on Figure 1 It can be seen that (a) BPA-PEN fiber membrane has uniform fiber thickness and high orientation; (b) BPA-PEN@BNNS mixed spray fiber membrane has defects on the fiber surface, uneven fiber diameter, and obvious BNNS agglomeration; (c) BPA-PEN@BNNS stacked spray fiber membrane, it can be seen that BNNS is well dispersed on the fiber surface, and the BNNS particle size is smaller than that of BNNS sprayed with mixed solution, and the distance between BPA-PEN and BNNS is smaller; Figures (d)-(f) are the cross-sectional morphologies of hot-pressed membranes of BPA-PEN, BPA-PEN@BNNS mixed spray and BPA-PEN@BNNS stacked spray, respectively. From (f), it can be seen that a good thermal conductivity network is formed between BPE-PEN and BNNS. These phenomena indicate that the interfacial thermal resistance between the matrix and the filler is reduced, forming an effective and complex thermal conductivity network, thereby increasing λ. In summary, compared with Example 3, the variable in Example 1 is whether or not to perform heat pressing treatment. After the heat pressing treatment, the air between the fibers is reduced, the heat conduction network is improved, and the heat transfer efficiency is effectively improved. Therefore, the thermal conductivity coefficient is improved after the heat treatment.

[0094] Compared with Comparative Example 1, the remaining embodiments all added high thermal conductivity filler BNNS to form a continuous thermal conductive network in the matrix, so the thermal conductivity coefficients were all improved.

[0095] like Figure 3 As shown, the breakdown strength of Examples 1-3 decreases with the increase of the filling amount of BNNS, which is due to the increase of the interface resistance between the matrix polymer and BNNS and the decrease of the electrical properties.

[0096] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a high thermal conductivity poly(arylene ether nitrile) film, characterized in that: The method of obtaining a high thermal conductive poly(arylene ether nitrile) film by electrospinning and hot pressing includes the following steps: Step 1, preparing BPA-PEN spinning solution and BNNS dispersion; Step 2, orienting the fibers by electrospinning to obtain a BPA-PEN fiber membrane; Step 3, electrostatically spraying the BNNS dispersion on the surface of the fiber membrane to form a BPA-PEN@BNNS spray-coated fiber membrane; Step 4: hot-press the BPA-PEN@BNNS spray-coated fiber membrane to obtain a high thermal conductivity poly(arylene ether nitrile) film.

2. The method for preparing a high thermal conductivity poly(arylene ether nitrile) film according to claim 1, characterized in that: The electrospinning process of step 2 is as follows: place the BPA-PEN spinning solution in a syringe, set the injection speed of the syringe pump to 1-3 mL / h, apply a voltage of 25-27 KV, set the working distance between the syringe and the receiver to 15-20 cm, set the rotation speed of the receiver to 200-400 rpm / min, perform electrospinning for 1.5 h to 2 h, and obtain a BPA-PEN fiber membrane.

3. The method for preparing a high thermal conductivity poly(arylene ether nitrile) film according to claim 1, characterized in that: The process of electrostatic spraying in step 3 is as follows: place the BNNS dispersion in a syringe, set the injection speed of the syringe pump to 1-3 mL / h, apply a voltage of 25-27 KV, set the working distance between the syringe and the receiver to 15-20 cm, and set the rotation speed of the receiver to 200-400 rpm / min. Electrostatic spraying is performed on the obtained BPA-PEN fiber membrane for 1.5 h to 2 h.

4. The method for preparing a high thermal conductivity poly(arylene ether nitrile) film according to claim 1, characterized in that: The hot pressing process of step 4 is as follows: the obtained BPA-PEN@BNNS spray-coated fiber membrane is peeled off, and then placed in a mold and hot pressed for 10 to 20 minutes under the conditions of 10 to 20 MPa and 230 to 270° C. to obtain a BPA-PEN@BNNS spray-coated hot-pressed membrane; after the mold is naturally cooled to room temperature, the film is taken out to obtain the polyarylether nitrile film.

5. A method for preparing a high thermal conductivity poly(arylene ether nitrile) film, characterized in that: The following steps are involved: Step 1, preparing BPA-PEN@BNNS spray-coated fiber membrane; 1.1 Add BPA-PEN to DMF and stir magnetically at 70-80°C for 1-2 hours to obtain a BPA-PEN spinning solution of 0.05 g / mL to 0.15 g / mL; 1.2 Add BNNS to DMF and disperse it ultrasonically at room temperature for 8 to 12 hours to obtain a BNNS dispersion with a mass concentration of 0.1 g / mL to 0.3 g / mL; 1.3 The spinning solution obtained in step 1.1 is placed in a syringe, the injection speed of the syringe pump is set to 1-3 mL / h, the applied voltage is set to 25-27 KV, the working distance between the syringe and the receiver is 15-20 cm, the rotation speed of the receiver is 200-400 rpm / min, and electrospinning is performed for 1.5 h to 2 h to obtain a BPA-PEN fiber membrane; 1.4 Place the BNNS dispersion obtained in step 1.2 into a syringe, set the injection speed of the syringe pump to 1-3 mL / h, the applied voltage to 25-27 KV, the working distance between the syringe and the receiver to 15-20 cm, the speed of the receiver to 200-400 rpm / min, and continue electrostatic spraying on the fiber membrane obtained in step 1.3 for 1.5 h to 2 h; 1.5 Repeat steps 1.3 to 1.4 4 to 6 times to obtain BPA-PEN@BNNS spray-coated fiber membrane; Step 2, preparing a poly(arylene ether nitrile) film; The BPA-PEN@BNNS spray-coated fiber membrane obtained in step 1 is peeled off from the aluminum foil, and then placed in a mold and hot-pressed for 10 to 20 minutes under the conditions of 10 to 20 MPa and 230 to 270° C. to obtain a BPA-PEN@BNNS spray-coated hot-pressed membrane; after the mold is naturally cooled to room temperature, the film is taken out to obtain the polyarylethernitrile film.

Citation Information

Patent Citations

  • High-heat-conductivity boron nitride / polyurethane heat-conducting composite material and preparation method thereof

    CN113861665A

  • Preparation method of insulating, heat-conducting and soaking film based on electrostatic spinning technology

    CN114717754A

  • Super-hydrophobic flexible heat-conducting film and preparation method thereof

    CN115450054A

  • Solar-driven interface water evaporation and photocatalytic dye degradation dual-functionalized composite fiber membrane as well as preparation method and application thereof

    CN118007318A