Water-dispersed composition for heat-sealing agent, and heat-sealing material

JP7554609B2Active Publication Date: 2024-09-20NIPPON A & L INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020148635
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-10
Filing Date
2020-09-04
Publication Date
2024-09-20
Estimated Expiration
2040-09-04

AI Technical Summary

Technical Problem

Existing heat sealing technologies fail to adequately balance heat sealability and blocking resistance without using lamination, which poses challenges for recyclability and environmental sustainability.

Method used

An aqueous dispersion composition comprising an aliphatic conjugated diene copolymer latex with specific properties and polyolefin powder is used to form a heat-sealing layer, enhancing both heat sealability and blocking resistance.

Benefits of technology

The composition improves heat sealability and blocking resistance of the heat seal layer, facilitating recyclability and reducing environmental impact by eliminating the need for lamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554609000003
    Figure 0007554609000003
  • Figure 0007554609000001
    Figure 0007554609000001
  • Figure 0007554609000002
    Figure 0007554609000002
Patent Text Reader

Abstract

To provide a water dispersion composition for a heat sealant that has excellent heat sealability and blocking resistance of a heat seal layer without using a lamination process.SOLUTION: A water dispersion composition for a heat sealant contains an aliphatic conjugated diene copolymer latex with a toluene insoluble matter of 60 mass% or less and a glass transition temperature of 10°C or higher and a polyolefin powder with an MFR (melt mass flow rate) (190°C / 2.16 kg) of 30-150 g / 10 min as measured by JIS K-7210.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-dispersed composition for a heat-sealing agent, and a heat-sealing material. [Background technology]

[0002] The method of bonding (i.e., heat sealing) paper, film, etc. by overlapping them and applying heat and pressure is used for various applications including packaging materials. As a means for imparting heat sealability to paper, film, etc., for example, a method of forming so-called laminated paper laminated with polyolefin resin, or a method of applying, laminating, or internally adding a polymeric compound such as a copolymer containing vinyl chloride or vinylidene chloride to a substrate such as paper or film to impart heat sealability is widely used due to ease of production and low production costs.

[0003] However, in recent years, due to the global trend towards reducing the use of plastics and saving resources, efforts have been made to reuse waste paper, but in the case of laminated paper, etc., from the viewpoint of biodegradability and during the process of making recycled paper, the laminated parts remain in the ecosystem, or remain undisintegrated during recycling, making it difficult to remove the residual residue. Therefore, there has been a demand for the development of a technology to replace lamination that allows for recovery, regeneration, and other recycling.

[0004] Patent Document 1 describes an invention that can impart heat sealability, recyclability (recovery and recycling), and even water and oil resistance, by using a paint that contains an acrylic dispersion and a styrene-butadiene dispersion in a specific ratio, which improves heat sealability.

[0005] Patent Document 2 discloses that the heat sealability can be improved by using a coating liquid containing as a main component an acrylic emulsion having heat sealability.

[0006] Patent Document 3 shows that the low-temperature heat sealability and water resistance can be improved by using an aqueous resin dispersion containing resin particles A and resin particles B having specified glass transition temperatures and particle sizes. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2002-13095 A [Patent Document 2] JP 2015-155582 A [Patent Document 3] JP 2016-216533 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, although the means described in the above-mentioned patent publications are effective in terms of recyclability, they are still insufficient in terms of satisfying both the requirements for heat sealability and the blocking resistance of the heat seal layer.

[0009] An object of the present invention is to provide an aqueous dispersion composition for a heat-sealing material, which can improve the heat sealability and the blocking resistance of a heat-sealing layer without using a lamination process. [Means for solving the problem]

[0010] The present invention provides an aqueous dispersion composition for a heat-sealing material, comprising an aliphatic conjugated diene copolymer latex having a toluene-insoluble content of 60% by mass or less and a glass transition temperature of 10°C or more, and a polyolefin powder having an MFR (melt mass flow rate) (190°C / 2.16 kg) of 30 to 150 g / 10 min, as measured according to JIS K-7210.

[0011] The present invention also provides a heat-sealing material, which comprises a substrate and a heat-sealing layer obtained by applying the water-dispersed composition for a heat-sealing material of the present invention to the substrate and drying the applied composition. Effect of the Invention

[0012] According to the present invention, it is possible to provide an aqueous dispersion composition for a heat-sealing material, which can improve the heat sealability and the blocking resistance of a heat-sealable layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The water dispersion composition for a heat sealing material according to this embodiment contains an aliphatic conjugated diene copolymer latex having a toluene-insoluble content of 60% by mass or less and a glass transition temperature of 10°C or more, and a polyolefin powder having an MFR (melt mass flow rate) (190°C / 2.16 kg) measured according to JIS K-7210 of 30 to 150 g / 10 min.

[0014] The aliphatic conjugated diene copolymer latex is a copolymer latex having structural units derived from an aliphatic conjugated diene monomer and structural units derived from other copolymerizable monomers, and is obtained, for example, by emulsion polymerization of an aliphatic conjugated diene monomer and other copolymerizable monomers.

[0015] Examples of the aliphatic conjugated diene monomer include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadiene, and substituted and side-chain conjugated hexadienes. These can be used alone or in combination of two or more. In this embodiment, it is preferable to use 1,3-butadiene from the viewpoints of industrial ease of production, availability, and cost.

[0016] As the other copolymerizable monomer, from the viewpoints of heat sealability and blocking resistance of the heat seal layer, ethylenically unsaturated carboxylic acid monomers and alkenyl aromatic monomers are preferred.

[0017] Examples of the ethylenically unsaturated carboxylic acid monomer include monocarboxylic acid monomers such as acrylic acid, methacrylic acid, and crotonic acid, dicarboxylic acid monomers such as maleic acid, fumaric acid, and itaconic acid, and anhydrides thereof. These monomers can be used alone or in combination of two or more.

[0018] Examples of the alkenyl aromatic monomer include styrene, α-methylstyrene, methyl-α-methylstyrene, vinyltoluene, and divinylbenzene. These may be used alone or in combination of two or more. In this embodiment, it is preferable to use styrene from the viewpoints of industrial ease of production, availability, and cost.

[0019] Examples of copolymerizable monomers other than ethylenically unsaturated carboxylic acid monomers and alkenyl aromatic monomers include vinyl cyanide monomers, unsaturated carboxylic acid alkyl ester monomers, unsaturated monomers containing a hydroxyalkyl group, unsaturated carboxylic acid amide monomers, etc. These monomers can be used alone or in combination of two or more.

[0020] Examples of vinyl cyanide monomers include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, and α-ethylacrylonitrile. These may be used alone or in combination of two or more. In the present embodiment, it is preferable to use acrylonitrile or methacrylonitrile from the viewpoints of industrial ease of production, availability, and cost.

[0021] Examples of the unsaturated carboxylic acid alkyl ester monomer include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, glycidyl methacrylate, dimethyl fumarate, diethyl fumarate, dimethyl maleate, diethyl maleate, dimethyl itaconate, monomethyl fumarate, monoethyl fumarate, and 2-ethylhexyl acrylate. These can be used alone or in combination of two or more. In this embodiment, it is preferable to use methyl methacrylate from the viewpoints of industrial ease of production, availability, and cost.

[0022] Examples of unsaturated monomers containing a hydroxyalkyl group include β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, 3-chloro-2-hydroxypropyl methacrylate, di-(ethylene glycol) maleate, di-(ethylene glycol) itaconate, 2-hydroxyethyl maleate, bis(2-hydroxyethyl) maleate, and 2-hydroxyethyl methyl fumarate. These can be used alone or in combination of two or more.

[0023] Examples of the unsaturated carboxylic acid amide monomer include acrylamide, methacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, and N,N-dimethylacrylamide. These can be used alone or in combination of two or more.

[0024] In addition to the above monomers, monomers that are typically used in emulsion polymerization, such as ethylene, propylene, vinyl acetate, vinyl propionate, vinyl chloride, and vinylidene chloride, can also be used.

[0025] The content of the structural unit derived from the aliphatic conjugated diene monomer in the copolymer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. Also, it is preferably 32% by mass or less, more preferably 30% by mass or less, and even more preferably 28% by mass or less. By setting it in the above range, the film-forming property of the aqueous dispersion composition for a heat-sealing agent and the blocking resistance of the heat-sealing layer tend to be excellent.

[0026] The content of structural units derived from ethylenically unsaturated carboxylic acid monomers in the copolymer is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2.5% by mass or less. By setting it in the above range, the heat sealability and the disintegrability of the heat seal material tend to be excellent. In addition, from the viewpoint of the dispersion stability of the copolymer latex, it is preferably 0.1% by mass or more, and more preferably 0.5% by mass or more.

[0027] The content of the structural unit derived from the alkenyl aromatic monomer in the copolymer is preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 65% ​​by mass or more. Also, it is preferably 95% by mass or less, more preferably 85% by mass or less, and even more preferably 75% by mass or less. By keeping it in the above range, the blocking resistance of the heat seal layer tends to be excellent.

[0028] The content of structural units derived from other copolymerizable monomers other than the ethylenically unsaturated carboxylic acid monomer and the alkenyl aromatic monomer in the copolymer is preferably from 0% by mass to 40% by mass.

[0029] In addition to the monomer components constituting the copolymer, an emulsifier (surfactant), a polymerization initiator, and, if necessary, a chain transfer agent, a reducing agent, and the like can be blended into the reaction system of the emulsion polymerization according to this embodiment.

[0030] Examples of emulsifiers include sulfate esters of higher alcohols and alkylbenzene sulfonates. Phosphonates, alkyl diphenyl ether disulfonates, aliphatic sulfonates, aliphatic carbamide Abietinates, dehydroabietic acids, formalin condensates of naphthalenesulfonic acid, non-ionic Anionic surfactants such as sulfate ester salts of carboxylic surfactants, polyethylene glycol Noniolic acid such as alkyl ester type, alkyl phenyl ether type, and alkyl ether type These may be used alone or in combination of two or more. It can be used.

[0031] Examples of the chain transfer agent include alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, t-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-stearyl mercaptan; xanthogen compounds such as dimethyl xanthogen disulfide and diisopropyl xanthogen disulfide; thiuram compounds such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, and tetramethylthiuram monosulfide; and 2,6-di-t-butyl-4-methylphenol. phenolic compounds such as styrenated phenol; allyl compounds such as allyl alcohol; halogenated hydrocarbon compounds such as dichloromethane, dibromomethane, and carbon tetrabromide; vinyl ethers such as α-benzyloxystyrene, α-benzyloxyacrylonitrile, and α-benzyloxyacrylamide; and chain transfer agents such as triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, thiomalic acid, 2-ethylhexyl thioglycolate, terpinolene, and α-methylstyrene dimer. These can be used alone or in combination of two or more. The amount of the chain transfer agent can be appropriately adjusted in consideration of the combination with other additives, etc.

[0032] In addition, in order to control the molecular weight and crosslinked structure of the copolymer, the reaction system according to this embodiment can contain saturated hydrocarbons such as pentane, hexane, heptane, octane, cyclohexane, and cycloheptane; unsaturated hydrocarbons such as pentene, hexene, heptene, cyclopentene, cyclohexene, cycloheptene, 4-methylcyclohexene, and 1-methylcyclohexene; and aromatic hydrocarbons such as benzene, toluene, and xylene. These can be used alone or in combination of two or more. Of these, it is preferable to use cyclohexene and toluene.

[0033] Furthermore, the reaction system according to the present embodiment may contain additives such as electrolytes, oxygen scavengers, chelating agents, dispersants, defoamers, antioxidants, preservatives, antibacterial agents, flame retardants, ultraviolet absorbing agents, etc. The types and amounts of these additives may be appropriately selected and used.

[0034] The average particle size of the aliphatic conjugated diene copolymer latex is preferably 250 nm or less, more preferably 220 nm or less. If it exceeds 250 nm, the film-forming property of the water-dispersed composition for heat-sealing agents tends to decrease. Also, it is preferably 70 nm or more, more preferably 80 nm or more. If it is less than 70 nm, the dispersion stability of the copolymer latex tends to decrease or the viscosity tends to increase. The average particle size can be adjusted, for example, by changing the amount of water or emulsifier when preparing the copolymer latex. The average particle size is measured by dynamic light scattering using a photon correlation method in accordance with JIS Z8826.

[0035] The toluene insoluble content of the aliphatic conjugated diene copolymer latex is 60% by mass or less, preferably 50% by mass or less, and more preferably 40% by mass or less. If it exceeds 60% by mass, the heat sealability decreases. From the viewpoint of the surface strength of the heat seal layer, it is preferably 2% by mass or more, and more preferably 5% by mass or more. The toluene insoluble content can be adjusted, for example, by changing the amount of the chain transfer agent. The toluene insoluble content is measured by the method described in the Examples.

[0036] The glass transition temperature (Tg) of the aliphatic conjugated diene copolymer latex is 10° C. or higher, preferably 20° C. or higher, and more preferably 25° C. or higher. If it is lower than 10° C., the blocking resistance of the heat seal layer decreases. From the viewpoint of the film-forming property of the water-dispersed composition for a heat sealant, it is preferably 80° C. or lower, and more preferably 70° C. or lower. The glass transition temperature is measured by the method described in the Examples.

[0037] The aliphatic conjugated diene copolymer latex may be blended with functional additives such as dispersants, preservatives, antioxidants, printability improvers, surfactants, viscosity modifiers, etc., as necessary. The types and amounts of these additives may be appropriately selected and used.

[0038] Examples of polyolefin powders include polypropylene powder and polyethylene powder, and these can be used alone or in combination of two or more. Among these, polyethylene powder is preferred.

[0039] The polyolefin powder has a median particle size of preferably 5 to 150 μm, more preferably 10 to 120 μm, and even more preferably 15 to 100 μm. If it exceeds 150 μm, the coatability of the water dispersion composition for a heat-sealing material tends to decrease, and if it is less than 5 μm, handling tends to become difficult.

[0040] The polyolefin powder has a melt mass flow rate (190°C / 2.16 kg) of 30 to 150 g / 10 min, preferably 50 to 120 g / 10 min, as measured by the method described in JIS K-7210. If it is less than 30 g / 10 min, the heat sealability is reduced. If it exceeds 150 g / 10 min, the yield of the polyolefin powder is reduced.

[0041] The water dispersion composition for heat-sealing material according to the present embodiment contains a copolymer latex and a polyolefin powder, and preferably contains 10 to 100 parts by weight, more preferably 15 to 80 parts by weight, and even more preferably 20 to 60 parts by weight of the polyolefin powder per 100 parts by weight (solid content equivalent) of the aliphatic conjugated diene copolymer latex. If the amount of the polyolefin powder is less than 10 parts by weight, the heat sealability tends to decrease, and if it exceeds 100 parts by weight, the coatability of the water dispersion composition for heat-sealing material tends to decrease.

[0042] The water dispersion composition for a heat-sealing material may contain functional additives such as dispersants, preservatives, antiaging agents, printability improvers, surfactants, viscosity adjusters, etc. The types and amounts of these additives may be appropriately selected and used.

[0043] The heat-sealing material of the present embodiment has a heat-sealing layer formed by applying the aqueous dispersion composition for a heat-sealing material of the present embodiment to a substrate and drying the applied composition. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. Furthermore, unless otherwise specified, % and parts are based on mass.

[0045] <Measurement of toluene insoluble matter of aliphatic conjugated diene copolymer latex> A copolymer latex film is prepared in an atmosphere with a temperature of 40°C and a humidity of 85%. Approximately 1 g of the latex film is then weighed out and designated as Xg. This is then placed in 400 ml of toluene and allowed to swell and dissolve for 48 hours. This is then filtered through a weighed 300 mesh stainless steel mesh, after which the toluene is evaporated and dried. The weight of the mesh is subtracted from the dried weight, and the dried weight of the sample is then weighed and designated as Yg. Insoluble in toluene (mass%) = Y / X x 100

[0046] <Measurement of glass transition temperature (Tg) of aliphatic conjugated diene copolymer latex> The copolymer latex is cast onto a glass plate and dried at 70°C for 4 hours to produce a film, which is then packed into an aluminum pan and set into a differential scanning calorimeter (DSC6200: Seiko Instruments Inc.). The apparatus is cooled in advance to a temperature about 50°C lower than the expected Tg, and then the temperature is increased at a heating rate of 10°C / min to plot a DSC curve.

[0047] In the present invention, the glass transition temperature refers to, in a differential curve of a DSC measurement chart, (a) the temperature at the top of the peak when there is one peak, (b) the temperature at the top of the peak with the largest area when there are two or more peaks, (c) the temperature at the top of the peak when there is a peak top but the shape is broad, (d) the temperature at the center of a broad (trapezoidal) peak when there is no peak top, or (e) the temperature obtained based on the criteria (c) or (d) when there are two or more peaks and the shape of the part with the largest area falls under (c) or (d), respectively.

[0048] <Measurement of average particle size of aliphatic conjugated diene copolymer latex> The average particle size of each copolymer latex was measured by dynamic light scattering using a photon correlation method in accordance with JIS Z8826. FPAR-1000 (manufactured by Otsuka Electronics) was used for the measurement.

[0049] <Measurement of MFR (Melt Mass Flow Rate) of Polyolefin Powder> The method described in JIS K7210 (190°C / 2.16 kg) was followed.

[0050] <Production of Aliphatic Conjugated Diene Copolymer Latex> The materials shown in Table 1 were mixed in the amounts (unit: parts by mass) shown in the same table and reacted to synthesize copolymer latexes A1 to A3. Specific synthesis procedures are shown below.

[0051] 10% by mass of each monomer shown in Table 1, an emulsifier, a polymerization initiator, a chain transfer agent, and polymerization water were charged into a pressure-resistant polymerization reactor, and after thorough stirring, the remaining components of each monomer shown in Table 1 were continuously added over 360 minutes from the point when the temperature inside the reactor reached 65°C. The temperature inside the polymerization reactor was then raised to 80°C, and polymerization was terminated when the polymerization conversion rate exceeded 95%. Next, the pH of the obtained copolymer latex was adjusted to 9.0 with NaOH to obtain copolymer latexes A1 to A3.

[0052] The components in Table 1 are represented by the following abbreviations. BDE: 1,3-butadiene STY: Styrene HEA: Hydroxyethyl acrylate FA: Fumaric acid AA: Acrylic acid EML: Sodium dodecylbenzenesulfonate (Kao Corporation, Neopelex G-15) (anionic emulsifier) TDM: t-dodecyl mercaptan (chain transfer agent)

[0053] [Table 1]

[0054] <Preparation of Water-Dispersed Composition for Heat-Sealing Agent> The aliphatic conjugated diene copolymer latex shown in Table 1 and the polyethylene powder shown in Table 2 were mixed according to the formulation shown in Table 3, and the solid content was adjusted to 50% by weight and the viscosity to 1000±500 mPa s using a thickener and water, to obtain aqueous dispersion compositions for heat-sealing agents of Examples 1 to 5 and Comparative Examples 1 to 5.

[0055] [Table 2]

[0056] [Table 3]

[0057] <How to evaluate coatability> The water-dispersed composition for heat sealant was applied to commercially available wood-free paper (basis weight 65 g / m 2 ) was coated with a wire bar (#20) and dried at 130°C for 1 minute, after which the presence or absence of streaks (coating streaks) on the coated surface was visually evaluated. (Excellent) 〇 > △ > × (Poor)

[0058] <How to evaluate heat sealability> A water-dispersed composition for heat sealant was applied to synthetic paper Yupo (Yupo Corporation) at a coating weight of 20 g / m on one side. 2 The coated surfaces were then overlapped and heat sealed using a heat seal tester TP-701A manufactured by Tester Sangyo Co., Ltd. at a heat seal width of 10 mm, a sealing temperature of 120°C, a sealing pressure of 1.3 MPa, and 10 seconds. The adhesive strength was then measured using a T-peel test.

[0059] <Method for evaluating blocking resistance> The water-dispersed composition for heat sealant was applied to a PET film using a wire bar (#20), dried at 130°C for 1 minute, cut into 1 cm-wide strips, and aligned and pasted on a mount. Black Kent paper was placed on top of the strips, and pressed between hot rolls at 100°C using a laboratory test heat calendar. After peeling off the black Kent paper, the state of fiber adhesion was visually evaluated. Those with less fiber adhesion had excellent blocking resistance. Those with more fiber adhesion had poor blocking resistance, and were relatively evaluated as follows: (Excellent) ◎ > 〇 > △ > × (Poor)

Claims

1. A water-dispersed composition for a heat-sealing material, comprising: an aliphatic conjugated diene copolymer latex having a toluene-insoluble content of 60% by mass or less and a glass transition temperature of 10°C or more; and a polyolefin powder having an MFR (melt mass flow rate) (190°C / 2.16 kg) measured according to JIS K-7210 of 30 to 150 g / 10 min, the aliphatic conjugated diene copolymer latex contains 5 to 32 mass% of structural units derived from an aliphatic conjugated diene monomer, 0.1 to 5 mass% of structural units derived from an ethylenically unsaturated carboxylic acid monomer, 55 to 85 mass% of structural units derived from an alkenyl aromatic monomer, and 0 to 40 mass% of structural units derived from other copolymerizable monomers other than an ethylenically unsaturated carboxylic acid monomer and an alkenyl aromatic monomer; The composition contains 10 to 100 parts by weight of a polyolefin powder relative to 100 parts by weight (solid content equivalent) of an aliphatic conjugated diene copolymer latex, The water-dispersible composition for a heat-sealing material contains 44 parts by weight or more (in terms of solid content) of an aliphatic conjugated diene copolymer latex per 100 parts by weight (in terms of solid content) of the water-dispersible composition for a heat-sealing material.

2. The aqueous dispersion composition for a heat sealant according to claim 1, wherein the aliphatic conjugated diene copolymer latex contains 15 to 32 mass% of structural units derived from an aliphatic conjugated diene monomer, 0.1 to 5 mass% of structural units derived from an ethylenically unsaturated carboxylic acid monomer, 55 to 75 mass% of structural units derived from an alkenyl aromatic monomer, and 0 to 40 mass% of structural units derived from other copolymerizable monomers other than an ethylenically unsaturated carboxylic acid monomer and an alkenyl aromatic monomer.

3. An aqueous dispersion composition for a heat-sealing agent as described in claim 1 or 2, containing 20 parts by weight or more of polyolefin-based powder per 100 parts by weight (converted into solid content) of the aqueous dispersion composition for a heat-sealing agent.

4. The water-dispersed composition for a heat-sealing material according to any one of claims 1 to 3, wherein the polyolefin-based powder is a polyethylene powder.

5. A heat-sealing material comprising a substrate and a heat-sealing layer obtained by applying the aqueous dispersion composition for a heat-sealing material according to any one of claims 1 to 4 and drying the applied composition.

Citation Information

Patent Citations

  • Copolymer latex and composition for coating paper

    JP1998204218A

  • Water-resistant and oil-resistant paper usable for for bag making, or the like

    JP2002013095A

  • Base paper for press bonding paper

    JP2002302895A

  • Aqueous dispersion composition and method for producing the same

    JP2006282723A

  • Diene-based copolymer latex composition for corrugated cardboard adhesive

    JP2007091994A