Method for passivating the surface of tinplate and electrolytic system for carrying out the method - Patents.com

A trivalent chromium electrolyte-based method with a heat treatment process forms a pure chromium oxide passivation layer on tinplate, addressing environmental hazards and enhancing adhesion and corrosion resistance while preventing tin oxide growth.

JP7554805B2Active Publication Date: 2024-09-20THYSSENKRUPP RASSELSTEIN
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022155876
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-04
Filing Date
2022-09-29
Publication Date
2024-09-20
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

Existing electrolytic methods for passivating tinplate surfaces using chromium-containing electrolytes pose environmental and health hazards due to the use of chromium-VI, and they fail to prevent the growth of a tin oxide layer in oxygen-containing environments, compromising the adhesion of organic coatings.

Method used

A method using a trivalent chromium compound-based electrolyte without organic complexing agents, followed by a heat treatment to convert chromium hydroxide to chromium oxide, forming a pure chromium oxide passivation layer that prevents oxygen penetration and enhances adhesion to organic coatings.

Benefits of technology

The method achieves a chromium oxide passivation layer with high resistance to oxidation and excellent adhesion to organic coatings, complying with environmental regulations and reducing tin oxide growth, thereby ensuring long-term corrosion resistance and coating integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554805000005
    Figure 0007554805000005
  • Figure 0007554805000004
    Figure 0007554805000004
Patent Text Reader

Abstract

To provide a method of passivating a surface of a tin plate, including electrolytic deposition of a passivation layer including chromium oxide / chromium hydroxide onto the surface.SOLUTION: Electrolytic deposition of a passivation layer can at least partially be carried out in an electrolytic solution including a trivalent chromium compound, at least one kind of a salt for enhancing electric conductivity, and at least one kind of an acid or a base for adjusting pH to an intended value, and not including an organic complexing agent and a buffer agent, In order to increase the amount of chromium oxide in the passivation layer, a passivated tin plate is subjected to thermal processing whereby it is kept at a processing temperature of 100°C or higher for a processing time of at least 0.5 seconds.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for passivating the surface of tinplate by electrolytic deposition of a chromium oxide-containing passivation layer on the surface of tinplate, and to an electrolytic system for electrolytic deposition of a chromium oxide-containing passivation layer on the surface of tinplate. [Background technology]

[0002] Steel sheets electrolytically coated with passivation layers of chromium and chromium oxide / hydroxide are known from the state of the art for the production of packages. They are known as tin-free steels (TFS) or electrolytic chromium coated steels (ECCS) and are an alternative to tinplate. These tin-free steel sheets are particularly characterized by good adhesion to lacquers or organic coatings (such as polymeric coatings made of PP or PET). Despite the low thickness of the passivation layers of chromium and chromium oxide / hydroxide, which is generally less than 20 nm, these chromium-coated steel sheets show good corrosion resistance and good formability in forming processes, for example in deep drawing and drawing-ironing processes for the production of packages.

[0003] Tin-plated steel sheets (tinplate) are usually provided with a passivation layer after electrolytic tin plating to prevent oxidation of the tin surface to atmospheric oxygen. Suitable passivation layers have proven to be chromium-containing layers which can be electrolytically deposited on the tin surface of the tinplate from an electrolyte containing chromium (VI). These chromium-containing passivation layers consist of metallic chromium and chromium oxide. Chromium oxide here is understood to include all compounds of chromium and oxygen, including chromium hydroxide.

[0004] For the production of electrolytic chromium coated steel (ECCS) and for the passivation of tinplate surfaces, electrolytic coating methods are known from the prior art, by which a passivation layer containing metallic chromium and chromium oxide / hydroxide can be applied to strip-like substrates (uncoated steel or tinplate) in a strip coating line using an electrolyte containing chromium-VI. However, these coating methods have considerable drawbacks due to the environmental and health-harmful properties of the chromium-VI-containing electrolytes used in the electrolytic methods, and will have to be replaced by alternative coating methods in the foreseeable future, since the use of materials containing chromium-VI will be banned in the future.

[0005] For this reason, electrolytic coating methods have already been developed in the state of the art, which make it possible to dispense with the use of electrolytes containing chromium-VI. For example, methods for the electrolytic passivation of strip-shaped steel sheets, in particular strip-shaped blackplate or tinplate, with a chromium metal oxide (Cr-CrOx) layer are known from US Pat. No. 5,399,623 and US Pat. No. 5,499,633, in which the steel sheets connected as cathodes in a strip coating line pass at high strip speeds of more than 100 m / min through a single electrolyte containing trivalent chromium compounds (in particular Cr-III sulfates) as well as complexing agents and conductivity-increasing salts, and free of buffers such as chlorides and boric acid.

[0006] Organic compounds, especially formates, preferably sodium or potassium formate, are used as complexing agents. The electrolyte may contain sulfuric acid to set the preferred pH value in the range of 2.5-3.5. The passivation layers of chromium metal and chromium oxide can be deposited in layers in successive electrolytic cells (each of which is filled with the same electrolyte) or in a successive coil coating line.

[0007] It was observed that the electrolytically deposited passivation layer can contain chromium sulfate and chromium carbide in addition to the components chromium metal and chromium oxide / hydroxide, and that the proportion of these components in the total coating weight of the passivation layer depends very substantially on the current density set in the electrolytic cell. It was found that three ranges (regime I, regime II, and regime III) are formed as a function of the current density, in the first range (regime I) with low current densities up to a first current density threshold, no chromium-containing deposits yet occur on the steel substrate, in the second range (regime II) with moderate current densities there is a linear relationship between the current density and the coating weight of the deposited passivation layer, and at current densities above the second current density threshold (regime III) partial decomposition of the applied passivation layer occurs, as a result of which the coating weight of chromium of the passivation layer in this regime first decreases as the current density increases and then settles to a constant value at higher current densities. Here, in the region with moderate current density (regime II), essentially metallic chromium is deposited on the steel substrate with a weight percentage of up to 80% (based on the total weight of the passivation layer), and above a second current density threshold (regime III), the passivation layer contains a higher percentage of chromium oxide, which in the region of higher current density accounts for 1 / 4 to 1 / 3 of the total coating weight of the passivation layer. The value of the current density threshold that separates the ranges (regimes I to III) from one another depends on the strip speed at which the steel sheet moves through the electrolyte.

[0008] For good passivation of the tinplate surface against oxidation in oxygen-containing environments and for the formation of good adhesion of organic coatings, such as lacquers or thermoplastics, in particular for the lamination of plastic films made of PET, PP, PE or mixtures thereof, a proportion of chromium oxide as high as possible in the chromium-containing passivation layer is advantageous.

[0009] From US Pat. No. 5,399,513 a method is known for passivating the surface of tinplate by deposition of a passivation layer consisting at least essentially of chromium oxide and chromium hydroxide, for which purpose an aqueous solution of an electrolyte is used which contains a trivalent chromium compound free of organic substances, in particular free of organic complexing agents. Due to the use of an aqueous electrolyte, the deposited passivation layer has a high chromium hydroxide content in addition to chromium oxide. However, the chromium hydroxide content of the passivation layer allows atmospheric oxygen to diffuse through the passivation layer if the passivated tinplate is stored for long periods in an air atmosphere. The diffusion of atmospheric oxygen through the passivation layer leads to the formation of a harmful tin oxide layer on the tin surface of the tinplate, which consists essentially of divalent tin oxide (SnO). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] WO2015 / 177314 [Patent Document 2] WO2015 / 177315 [Patent Document 3] EP3722464A1 Summary of the Invention

[0011] The problem of the present invention is therefore to provide an efficient and cost-effective electrolytic method for passivating the surface of tinplate with a chromium oxide-containing passivation layer based on an electrolyte containing a trivalent chromium compound, which is able to prevent the growth of a tin oxide layer on the tin surface of the tinplate in an oxygen-containing atmosphere or in air. In any case, the use of substances containing chromium-VI, even as intermediate products of the electrolytic method, should be avoided so as to be able to fully comply with the legal requirements regarding the prohibition of substances containing chromium-VI. The tinplate coated according to the present method should be as resistant as possible to oxidation in oxygen-containing environments, in particular in atmospheric oxygen, and should have good adhesion properties to organic coatings such as organic lacquers and polymer coatings (in particular polymer films made of, for example, PET, PE or PP).

[0012] The method according to the invention involves electrolytic deposition of a chromium oxide-containing passivation layer on a tin-plated steel strip (tinplate strip) from an electrolyte that contains a trivalent chromium compound, at least one salt for increasing the electrical conductivity, and at least one acid or base for adjusting the pH value to the desired value, free of organic complexing agents and free of buffers, and after electrolytic deposition of the passivation layer, the passivated tinplate is subjected to a heat treatment in which the passivated tinplate is maintained at a treatment temperature of at least 100° C. for a treatment time of at least 0.5 seconds. The heat treatment of the passivated tinplate is carried out immediately after the electrolytic deposition of the passivation layer in order to remove the chromium hydroxide components contained in the passivation layer from the passivation layer, which makes the passivation layer impermeable to oxygen and prevents the growth of a tin oxide layer on the tin surface of the tinplate. In the case of tinplate that has been heat-treated according to the invention after deposition of the passivation layer, after storage in an oxygen-containing atmosphere for at least 4 weeks, the passivation layer is maintained at a temperature of 70 C / m 2 A tin oxide layer with a tin oxide overlay of less than 55 C / m is present under the passivation layer. Preferably, the tin oxide layer overlay after at least 4 weeks of storage has a melting point of less than 55 C / m 2 More preferably, it is less than 40 C / m 2 Less than 20C / m 2 ~60C / m 2This allows the entire tin oxide overlay to consist of divalent tin oxide (SnO), produced by natural oxidation of the tin surface in atmospheric oxygen, and tetravalent tin oxide (SnO2), produced by targeted anodic oxidation prior to the electrolytic deposition of the passivation layer. Preferably, the tetravalent tin oxide has a viscosity in the range of 40 C / m 2 less than 30 C / m 2 has an overlay of less than

[0013] Since in the method according to the invention no substances containing chromium VI are used, even as intermediates, the process is completely free of substances containing chromium VI and therefore does not harm the environment or human health when the process is carried out.

[0014] Due to the use of an organic complexing agent-free (in particular formate-free) electrolyte for the electrolytic deposition of the passivation layer or at least the upper layer of the passivation layer, and due to the subsequent heat treatment of the tinplate provided with the passivation layer, the passivation layer consists at least essentially of pure chromium oxide, with the exception of unavoidable impurities (which may in particular be residues of chromium hydroxide and chromium sulfate (if chromium(III) sulfate is used as the trivalent chromium compound in the electrolyte), or comprises at least one upper layer of pure chromium oxide. A passivation layer or an upper layer of a passivation layer consisting of pure chromium oxide, on the one hand, forms a very good barrier against the penetration of oxygen and, on the other hand, provides good adhesion to organic coatings, such as organic lacquers or polymer films made from PET, PP or PE.

[0015] Reference to chromium oxide means all (trivalent) oxide forms of chromium (CrOx). Reference to chromium hydroxide means all hydrated forms of chromium oxide, in particular chromium(III) hydroxide and chromium(III) oxide hydrate, as well as mixtures thereof.

[0016] After the heat treatment according to the invention, the electrolytically applied passivation layer has a chromium oxide content as high as possible. Preferably, the weight fraction of chromium oxide is more than 95%. On the one hand, this ensures good passivation of the tinplate surface against oxidation, and on the other hand provides good properties for organic coatings, such as organic lacquers or polymer layers made of thermoplastics such as PET, PE or PP.

[0017] For the electrolytic deposition of the passivation layer, the tinplate strip is connected as a cathode and is contacted with the electrolyte in at least one electrolytic cell for a predefined electrolysis time. The electrolysis time is preferably in the range of 0.3-5.0 seconds, particularly preferably between 0.6 and 1.5 seconds. For this purpose, the tinplate strip passes at a predefined speed in succession through at least one electrolytic cell or through several electrolytic cells arranged one behind the other in the running direction of the strip, the strip speed being preferably at least 100 m / min, even more preferably between 200 m / min and 750 m / min. High speeds can ensure a high efficiency of the process.

[0018] The thickness or coating weight of the electrolytically deposited passivation layer can be controlled by the electrolysis time and therefore by the stripping speed. Preferably, the electrolysis time is such that the deposited chromium oxide is at least 3 mg / m2 in terms of chromium. 2 , preferably 8 mg / m 2 ~12mg / m 2 These preferred coating weights of the passivation layer provide sufficient oxidation and corrosion resistance of the tinplate for packaging applications and also provide a good adhesion base for organic coatings such as lacquers or thermoplastic films.

[0019] Thus, in order to improve the corrosion resistance and form a barrier against sulfur-containing materials, in particular sulfate or sulfite-containing contents of the package, it is possible to provide, after the passivation layer has been electrolytically applied, a coating of an organic material, in particular a coating of a polymer film of a thermoplastic resin, in particular PET, PE, PP or mixtures thereof, which adheres well to the chromium oxide layer of the passivation layer, by coating the surface of the passivation layer with an organic coating or by providing a plastic layer of a thermoplastic resin, such as PET, PP and / or PE.

[0020] To ensure that the method is completely free of chromium-VI-containing substances, a suitable anode is selected for the electrolytic deposition of the passivation layer and placed in the electrolytic cell or cells respectively to prevent oxidation of chromium-(III) from the trivalent chromium compounds of the electrolyte to chromium-(VI). Anodes free of steel and stainless steel, having an outer surface or passivation layer of metal oxide (especially iridium oxide) or mixed metal oxide (especially iridium-tantalum oxide), have been found to be particularly suitable for this purpose. Preferably, the anode is free of stainless steel and platinum. By using such an anode, a coating containing only trivalent chromium oxide and / or hydroxide, in particular Cr2O3 and / or Cr(OH)3, can be deposited on the tinplate.

[0021] To carry out the method according to the invention, at least one electrolytic cell filled with a first electrolyte solution, or a plurality of electrolytic cells arranged in series, where at least one cell is filled with the first electrolyte solution and the remaining cells are filled with the first electrolyte solution or with another electrolyte solution containing a trivalent chromium compound and having a different composition from the first electrolyte solution; the first electrolyte comprises an electrolytic cell containing a trivalent chromium compound, at least one salt for increasing electrical conductivity, and at least one acid or base for adjusting the pH to a desired value, but not containing an organic complexing agent and not containing a buffer; a conveying device for conveying the strip tinplate in a running direction at a predetermined speed, preferably above 100 m / min, through at least one electrolytic cell, or through several electrolytic cells in succession, for electrolytic deposition of a passivation layer from a first electrolyte and optionally from another electrolyte on the surface of the tinplate; a heating device arranged downstream of the electrolytic cell or cells in the direction of travel and designed to heat the passivated tinplate to a predetermined treatment temperature of at least 100°C for a predetermined treatment time of at least 0.5 seconds; An electrolytic system including:

[0022] In one embodiment, the electrolysis system according to the invention comprises several electrolytic cells arranged in succession, of which at least the last one in the running direction of the strip is filled with a first electrolyte, and the preceding ones with another electrolyte which contains, in addition to a trivalent chromium compound, at least one salt for increasing the electrical conductivity and at least one acid or base for setting the desired pH value and an organic complexing agent. In particular, formates, preferably sodium or potassium formate, can be used as complexing agents. The temperatures of the electrolytes in the individual electrolytic cells can also be selected to be different. This embodiment makes it possible to deposit a chromium oxide-containing passivation layer on the surface of the tinplate with several layers having different compositions.

[0023] In particular, this embodiment of the electrolysis system can be used to produce a passivation layer having a lower layer of metallic chromium and chromium oxide / hydroxide and possibly chromium carbide and an upper layer of pure chromium oxide. The individual layers of the passivation layer are deposited on the tin surface of the tinplate in the individual electrolysis cells of the electrolysis system arranged one behind the other. Differences in the composition and / or temperature of the electrolyte in the individual electrolysis cells result in different compositions of the layers of the passivation layer, which in particular differ from one another in the weight proportion of chromium oxide.

[0024] Using the heating device, the chromium hydroxide components of the passivation layer or at least the chromium hydroxide components of the upper layer of the passivation layer can be converted into chromium oxide, so that the passivation layer consists entirely of pure chromium oxide or at least the upper layer of the passivation layer essentially only comprises chromium oxide, in particular does not comprise metallic chromium and at most has unavoidable residual chromium hydroxide. The heating device is preferably arranged immediately downstream of the electrolytic cell or immediately downstream of the last cell of the electrolytic cells, as viewed in the running direction of the strip. This allows the heat treatment of the passivation layer to be carried out immediately after the completion of the electrolytic application of the passivation layer, within a short time interval, for example less than 10 seconds.

[0025] The electrolysis system according to the invention can be advantageously arranged immediately downstream of an electrolytic tinning line in which a tinplate steel substrate is electrolytically provided with a tin layer. Thus, providing the tinplate surface of the tinplate with a passivation layer can be carried out immediately after the electrolytic tinning of the steel substrate without the need to roll up the tinplate strip. The tinplate steel substrate can thus be fed as a steel strip at a predefined stripping speed through a tinning line for tinning and further fed at the same stripping speed by a transport device immediately after tinning through the electrolysis system according to the invention. However, it is also possible to first wind the tinplate steel strip into a coil and then feed the coil to the transport device of the electrolysis system according to the invention for unwinding and transporting the tinplate steel strip.

[0026] The heating device may be designed as a continuous furnace with a heating section having a preferred length of at least 3 m. The heating device may also comprise an induction heater. The electrolysis system according to the invention may also comprise a further heating device arranged upstream of the (first) electrolytic cell or upstream of the electrolytic cells, seen in the running direction of the strip. This further heating device, preferably designed as an induction heater, can be used to at least partially melt the tin layer of the tinplate provided in the tinning line by heating the tinplate strip in the further heating device to a temperature above the melting point of tin.

[0027] The electrolyte preferably has an electrolyte temperature in the range of 20°C to 80°C, particularly preferably in the range of 30°C to 65°C, in particular 40°C to 60°C. At these temperatures, the electrolytic deposition of the chromium oxide-containing passivation layer is very efficient. When the electrolyte temperature or the temperature of the electrolyte or the temperature in the electrolytic cell is mentioned, in each case the average temperature averaged over the entire volume of the electrolytic cell is meant. Generally, in the electrolytic cell there is a temperature gradient with an increasing temperature from top to bottom. If several electrolytic cells are used, the electrolyte temperature in each electrolytic cell may be different, which may affect the composition of the layer of the passivation layer deposited in each electrolytic cell. For example, at electrolyte temperatures below 40°C, a layer with a higher chromium oxide content is deposited compared to electrolytic cells with higher electrolyte temperatures. It is therefore advantageous in the method according to the invention to set the electrolyte temperature of the last electrolytic cell below 40°C in order to maximize the chromium oxide content of the upper layer of the passivation layer.

[0028] The first electrolyte, filled in at least one, preferably the last electrolytic cell in the direction of travel, contains, in addition to a trivalent chromium compound and solvent water, at least one conductivity-improving salt and at least one acid or base for setting a suitable pH value, and is preferably chloride ion-free and buffer-free, in particular borate buffer-free.

[0029] The trivalent chromium compounds in the electrolyte are preferably basic Cr(III) sulfate (Cr2(SO4)3), Cr(III) nitrate (Cr(NO3)3), Cr(III) oxalate (CrC2O4), Cr(III) acetate (C 12 H 36 ClCrO 22 Cr(III) formate (Cr(OOCH)3) or mixtures thereof. The concentration of the trivalent chromium compound in the electrolyte is preferably at least 10 g / L, particularly preferably greater than 15 g / L, and especially preferably equal to or greater than 20 g / L.

[0030] To increase the electrical conductivity, the electrolyte contains at least one salt, preferably an alkali metal sulfate, in particular potassium sulfate or sodium sulfate.

[0031] A very efficient deposition of the passivation layer containing chromium oxide and chromium hydroxide is achieved if the pH of the electrolyte (measured at a temperature of 20 ° C) is in the range of 2.3 to 5.0, preferably between 2.5 and 3.5. The desired pH can be adjusted by adding an acid or a base to the electrolyte. When using basic Cr(III) sulfate as the trivalent chromium compound, sulfuric acid or an acid mixture containing sulfuric acid is particularly suitable for adjusting to the desired pH.

[0032] A particularly preferred composition of the electrolyte contains basic Cr(III) sulfate (Cr2(SO4)3) as the trivalent chromium compound, sodium sulfate as the conductivity enhancing salt, and sulfuric acid for setting the preferred pH in the range of 2.5 to 3.5.

[0033] In addition to the trivalent chromium-containing substance, at least one salt for increasing the electrical conductivity, and at least one acid or base for adjusting the pH value, the electrolyte contains no other components other than the solvent water, which ensures a simple and inexpensive preparation of the electrolyte and leads to the deposition of a passivation layer that consists at least substantially only of chromium oxide and chromium hydroxide, and otherwise contains only unavoidable impurities such as chromium sulfate (when Cr-(III) sulfate is used as the trivalent chromium compound).

[0034] In the method according to the invention, the chromium hydroxide component contained in the electrodeposited passivation layer is removed from the passivation layer by subjecting the passivated tinplate to a heat treatment at a treatment temperature of 100° C. or higher and maintained for a treatment time of at least 0.5 seconds, so that the water of the hydrated chromium oxide evaporates and the chromium hydroxide is converted to chromium oxide.

[0035] The treatment time is preferably between 0.5 seconds and 30 minutes, more preferably between 1.0 seconds and 1 minute. In order to prevent melting of the tin surface of the tinplate, the treatment temperature is preferably between 150°C and the melting temperature of tin (232°C). In particular, the heat treatment is carried out immediately after electrolytic deposition of a passivation layer on the tinplate strip by passing the tinplate strip through a furnace at a strip speed at which the tinplate strip passes through an electrolytic cell. At high strip speeds, preferably above 100 m / min and up to 900 m / min, very short treatment times of a few seconds or even less than 1 second are obtained, depending on the length of the furnace, which is preferably between 5 and 30 m in the running direction of the strip. For very short treatment times of less than 1 second, higher treatment temperatures are selected, which can be, for example, between 170°C and 230°C. If the temperature of the electrolyte in the last electrolytic cell seen in the strip running direction is relatively high, for example in the range of 50°C or higher, then very short treatment times of less than 1 second are sufficient even for lower treatment temperatures below 150°C, since the passivated tinplate strip has this temperature and only needs to be heated to the (maximum) treatment temperature for the heat treatment in a short time.

[0036] A particularly fast and efficient heating of the passivated tinplate to the (maximum) treatment temperature can be achieved by induction heating in an induction coil. Heating rates of 100 K / s to 700 K / s can be achieved, which allows the passivated tinplate to be heated from the electrolyte temperature of the last electrolytic cell to the (maximum) treatment temperature.

[0037] However, if necessary, it is also possible to carry out a heat treatment of the passivated tinplate after cutting the tinplate strip into several sheets in an oven or by IR irradiation of the passivated tinplate. By using an oven, longer treatment times of several minutes can be selected, which allows the use of lower treatment temperatures in the range of 100 ° C to 150 ° C.

[0038] In order to prevent oxygen diffusion through the passivation layer while it is still wet after deposition of the passivation layer, the heat treatment is preferably carried out immediately after the electrolytic deposition of the passivation layer, i.e. immediately after leaving the last electrolytic bath. After the completion of the deposition of the passivation layer, i.e. between leaving the last electrolytic bath and reaching the treatment temperature, there is preferably an intermediate time of maximum 10 seconds.

[0039] In a preferred embodiment of the method, a tin oxide layer consisting essentially of tetravalent tin oxide (SnO2) is produced on the surface of the tinplate prior to the electrolytic deposition of the passivation layer by placing the tinplate as an anode in an aqueous, in particular basic electrolyte containing phosphates, borates, sulfates or carbonates. The formation of a tetravalent tin oxide layer, which is more inert to further oxidation in an oxygen atmosphere than divalent tin oxide, minimizes the inevitable growth of an oxide layer on the tin surface of the tinplate in an oxygen-containing atmosphere and improves the marbling resistance of the tinplate to sulfur-containing substances, such as the sulfur content of packages manufactured from the tinplate. On the one hand, the stoichiometry of the tin oxide layer and the ratio of divalent and tetravalent tin oxides can be controlled by targeted anodic oxidation, and on the other hand, a uniform distribution of the tin oxide layer on the surface of the tinplate is achieved.

[0040] Advantageously, before the electrolytic provision of a passivation layer is carried out in the electrolytic system according to the invention, anodization is carried out in the electrolytic line in which the electrolytic provision of a passivation layer is carried out, i.e. by passing the tinplate strip through a first electrolytic cell which is connected upstream of the electrolytic cell with the trivalent chromium electrolyte and which is filled with a basic electrolyte, so that the tinplate strip is connected as an anode in the electrolytic cell with the basic electrolyte and as a cathode in the subsequent electrolytic cell with the trivalent chromium electrolyte.

[0041] The basic electrolyte may be, for example, an aqueous solution of sodium carbonate having a concentration in the range of 1% to 10% by weight, preferably having a temperature in the range of 30 to 60° C. and a pH value in the range of 7 to 11, particularly in the case of sodium carbonate, with a pH value between 10 and 11. The current density in the first electrolytic cell, where the anodic oxidation takes place, is preferably 0.1 to 10 A / dm 2 Within the range of 0.2 to 3 A / dm 2 The anodization time, i.e. the time during which the tinplate is in effective electrolytic contact with the basic electrolyte, is preferably less than 5 seconds, preferably in the range of 0.1 to 1.0 seconds, and can be suitably adapted to the strip speed at which the tinplate strip passes through the electrolytic system.

[0042] As a result of the anodization, a tin oxide layer (SnO2) is provided on the not yet passivated tin surface of the tinplate, which preferably has a temperature of 10-40 C / m 2 In particular, 30 C / m 2 Less than 10~28C / m 2 The overlay of the tin oxide layer on the sample can be determined coulometrically with a chronoamperometric measurement method by measuring the applied tin oxide layer with a working electrode made of the material to be measured and previously degreased, a counter electrode made of a carbon rod and a Ag / AgCl reference electrode in 47% hydrobromic acid (HBr) diluted to a 0.01 n solution (0.01 mol / l) in water and thoroughly degassed with inert gas (e.g. N2), the ... the counter electrode made of a carbon rod and a Ag / AgCl reference electrode in 47% hydrobromic acid (HBr) diluted to a 0.01 n solution (0.01 mol / l) in water and thoroughly degassed with inert gas (e.g. N2), the overlay of the tin oxide layer on the 2 The amount of charge in coulombs (determined from the product of the cathodic current A and the reduction time t) required to completely reduce the tin oxide layer at current densities in the range of C / m 2 The charge per unit area at is the ratio of the charge in Coulombs (C) to the area of ​​the sample (m 2 ) (according to Annex D of the proposed European Standard EN10202:2001).

[0043] Prior to anodization, the tin layer of the tinplate can be optionally partially melted by heating the tinplate to a temperature above the melting point of tin (232°C). Preferably, the heating is inductive so that only the portion of the tin layer facing the steel substrate can be melted and metallic tin remains on the surface of the tin layer. The melted areas of the tin layer form an iron-tin alloy layer with the iron atoms of the steel substrate, which forms a barrier against corrosion.

[0044] The tinplate produced by the method according to the invention has the following layer structure (in this order): Steel substrates (especially once (SR) or twice (DR) cold-rolled steel sheets with a thickness of 0.5 mm or less), Optional: 0.1 to 2 g / m2 in tin equivalent 2 an iron-tin alloy layer having a coating weight in the range of Especially 0.5 to 5 g / m 2 Free (metallic) tin having a coating weight in the range of Especially from SnO2, especially 10~30C / m 2 Tin oxide having a charge density in the range of In particular, chromium equivalent is 3 to 12 mg / m 2 A chromium oxide-containing passivation layer having a coating weight in the range of

[0045] The chromium oxide passivation layer can be a pure chromium oxide layer, except for unavoidable impurities. However, the passivation layer can also consist of several superimposed layers of different composition, whereby the individual layers can contain metallic chromium, chromium oxide and / or chromium hydroxide, and possibly chromium carbide, whose chromium oxide content differs from one another. In particular, the passivation layer may comprise a lower layer of metallic chromium and chromium oxide / hydroxide, and possibly chromium carbide, and an upper layer of pure chromium oxide. This allows the individual layers of the passivation layer to be deposited on the tin surface of the tinplate in individual electrolytic cells of the electrolytic system according to the invention, which are arranged one behind the other, the individual electrolytic cells being filled with electrolytes of different composition and / or having different electrolyte temperatures. The difference in composition and / or temperature of the electrolyte in the individual electrolytic cells results in different compositions of the individual layers of the passivation layer.

[0046] The top layer of the electrolytically deposited passivation layer advantageously comprises only chromium oxide and chromium hydroxide, the chromium hydroxide being converted into chromium oxide by the heat treatment in the method according to the invention, so that the top layer of the tinplate according to the invention consists essentially of at least pure chromium oxide after the heat treatment, with the exception of unavoidable impurities and residual chromium hydroxide.

[0047] Thus, the method according to the invention can be used to produce tinplate having a chromium oxide-containing passivation layer, the passivation layer having at least one overlayer, which consists essentially only of trivalent chromium oxide and in particular does not contain chromium hydroxide other than residual components. Preferably, at least the overlayer of the passivation layer has a chromium oxide content of more than 95%, more preferably more than 98%. Preferably, the passivation layer or the overlayer at least substantially only comprises compounds of chromium and oxygen, in which chromium is present in trivalent form, in particular as Cr2O3 and / or Cr(OH)3.

[0048] The tinplate according to the invention is characterized by high corrosion resistance, good marbling resistance to sulfur-containing materials and good adhesion to organic coatings such as lacquers or polymer coatings.

[0049] In addition to the chromium oxide and chromium hydroxide residues, the passivation layer or an overlying layer may still contain residual chromium sulfate (e.g., as the starting chromium compound in the electrolytic deposition process when using Cr-(III) sulfate as the trivalent chromium compound in the electrolyte), except for unavoidable impurities.

[0050] In an advantageous embodiment, the passivation layer of the tinplate according to the invention is composed of at least a bottom layer facing the surface of the tinplate and a top layer forming the surface of the passivated tinplate, the bottom layer comprising metallic chromium and chromium oxide / hydroxide and optionally chromium carbide, and the top layer consisting of pure chromium oxide, with the exception of said residual components of chromium hydroxide and chromium sulfate as well as other unavoidable impurities.

[0051] The good corrosion resistance of the tinplate according to the invention is due to the fact that the passivation layer has a thickness of at least 3 mg / m2 calculated as chromium. 2 , preferably 5 mg / m 2 ~15mg / m 2 This can be achieved when the coating has a total coating weight of

[0052] The invention will now be described in more detail by way of examples with reference to the accompanying drawings, in which: Figure 1 illustrates the invention by way of example only and does not limit the invention in terms of the scope of protection defined by the appended claims. [Brief description of the drawings]

[0053] [Figure 1] 1A shows a schematic representation of two different embodiments of an electrolysis system according to the invention for carrying out a method according to the invention, where FIG. 1A shows a first embodiment having an electrolysis cell filled with a trivalent chromium electrolyte and FIG. 1B shows a second embodiment having two electrolysis cells each filled with a trivalent chromium electrolyte of different composition. [Diagram 2] 2A and 2B are schematic cross-sectional views of embodiments of tinplate according to the present invention, where FIG. 2A shows an embodiment having a single passivation layer and FIG. 2B shows an embodiment having a double passivation layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0054] Figures 1A and 1B show diagrammatically different embodiments of an electrolysis system for carrying out the method according to the invention. The electrolysis system in Figure 1A comprises three cells 1a, 1b, 1c arranged adjacent to each other or one after the other in the strip running direction, the first cell 1a being filled with a basic electrolyte BE, the middle cell 1b with a rinsing solution Sp and the last cell 1c with a first electrolyte E1.

[0055] The basic electrolyte BE consists of an aqueous soda solution (sodium carbonate solution with a concentration of 1-10% by weight and a pH value of 10-11). The rinsing solution Sp consists of distilled or demineralized water.

[0056] The first electrolytic solution E1 is an aqueous solution of a trivalent chromium compound, further containing a salt for increasing the electrical conductivity and an acid for adjusting the pH to a desired value between 2.5 and 3.5, and containing no organic complexing agent and no buffering agent. In a preferred embodiment, the first electrolytic solution E1 is composed of a trivalent chromium compound (particularly, Cr-(III) sulfate), a salt (e.g., potassium sulfate or sodium sulfate), an acid (e.g., sulfuric acid), and water as a solvent, and does not contain any other components. The first electrolytic solution E1 does not contain any organic components, particularly does not contain any organic complexing agent such as a formate salt, and does not contain any buffering agent such as boric acid, and does not contain any halide. An example of the composition of the first electrolytic solution E1 is shown in Table 1. The concentration of the trivalent chromium compound in the first electrolytic solution E1 is preferably at least 10 g / L, and particularly preferably 20 g / L or more. The temperature of the first electrolytic solution E1 is preferably 25°C to 70°C.

[0057] The cathode pair KP is placed in the first tank 1a and the anode pair AP is placed in the last tank 1c. The anode pair AP does not include stainless steel and platinum, but includes a coating of a metal oxide such as iridium oxide or a mixed metal oxide such as tantalum-iridium oxide. The anode of the AP anode pair may also be made entirely of a metal oxide or mixed metal oxide. An electric current may be applied to the cathode of the cathode pair KP and the anode of the anode pair AP.

[0058] Tin-plated steel strip (tinplate strip, hereinafter also referred to as strip B) is continuously fed through the baths 1a-1c. The strip B is drawn through the baths 1a-1c in the strip running direction v by a conveying device, not shown here, at a predefined strip speed, preferably above 100 m / min, in particular in the range from 100 to 750 m / min. A current roller S is arranged above the baths 1a-1c, via which the belt B can be switched as an anode or a cathode. In each electrolytic bath and above the baths 1a-1c, a deflection roller U is also arranged, around which the strip B is guided, by means of which the strip B is fed through the baths 1a-1c. The strip B is guided between the opposing cathodes of the cathode pair KP and between the two anodes of the anode pair AP.

[0059] A first heating device H1 is arranged downstream of the last tank 1c and a second heating device H2 is arranged upstream of the first tank. Each of the heating devices H1 and H2 can be a continuous furnace in which the strip B is heated to a given temperature and held at this temperature for a holding time. The holding time is determined by the strip speed and the length of the continuous furnace. The heating devices H1 and H2 can preferably also include an induction coil for the induction heating of the strip. The first heating device H1 is configured to rapidly heat the strip B to a temperature between 100 ° C and 232 ° C over a treatment time of at least 0.5 seconds. The second heating device H2 is configured to heat the strip B to a temperature above the melting point of tin (232 ° C).

[0060] In preparation for the electrolysis process, the strip B is first degreased, rinsed, pickled and rinsed again, then passes first through the second heating device H2, then successively through the baths 1a-1c and finally through the first heating device H1.

[0061] In the second heating device H2, the tin coating of the tinplate strip B is at least partially melted by heating to a temperature above the melting point of tin. The melting of the tin coating produces a dense iron-tin alloy layer at the interface between the steel substrate and the tin coating of the tinplate, the composition of which depends on the temperature and which may comprise FeSn and FeSn2 or mixtures thereof. Preferably, the tin coating is only partially melted, leaving a layer of free metallic tin on the surface. This can be anodized in the first bath 1a.

[0062] For this purpose, the strip B in the first bath 1a is connected as an anode and, depending on the strip speed, receives a current of 0.1 to 10 A / dm 2 in the range of 0.2 to 3 A / dm 2 A current density between 0.01 and 0.1 is generated by the cathode pair KP. At the corresponding current density, a tin oxide layer consisting essentially of at least tetravalent tin oxide (SnO2) is formed on the tin surface of the tinplate due to electrolytic interaction with the basic electrolyte BE. The thickness of the tin oxide layer electrolytically generated in the first tank 1a depends on the strip speed and the current density. The first tank 1a can also be passed without a current, so that no (tetravalent) tin oxide layer is formed on the tin surface of the tinplate strip B.

[0063] The strip B then passes through a central tank 1b with a rinsing solution Sp in order to rinse the strip, which is then dried by a drying device not shown here.

[0064] In the following cell 1c, strip B is connected as the cathode and the anode of the anode pair AP supplies 15 A / dm 2 Above 20A / dm 2 ~40A / dm 2A current density in the range of 0.5 to 2.0 seconds is generated. At this current density, a chromium oxide-containing passivation layer P is deposited on the (oxidized) surface of the tinplate strip B, which in addition to chromium oxide may contain unavoidable impurities of chromium hydroxide and chromium sulfate. The weight of the chromium oxide-containing layer can be controlled by the electrolysis time in the last bath 1c, which in turn can be controlled by the stripping speed and the current density. The higher the stripping speed, the higher the minimum current density required for the electrolytic deposition of the chromium oxide-containing layer. The electrolysis time in the last bath is 0.5 to 2.0 seconds, depending on the stripping speed. Preferably, in the last bath 1c, a chromium oxide-containing passivation layer P is deposited in a concentration of 3 to 12 mg / m 2 is deposited on the (oxidized) surface of tinplate strip B with a chromium-related coating weight of

[0065] The electrodeposited passivation layer P consists essentially of chromium oxide and chromium hydroxide, in particular with a weight proportion of chromium oxide and chromium hydroxide of at least 90%, preferably more than 95%, with respect to the total coating weight of the passivation layer. In case Cr-(III) sulfate is used as the chromium compound in the first electrolyte E1, in addition to chromium oxide and chromium hydroxide, the passivation layer may still contain unavoidable impurities such as residual chromium sulfate.

[0066] In order to minimize the amount of chromium hydroxide in the passivation layer, the passivated strip B is passed through a first heating device H1, in which a treatment temperature above 100 ° C, in particular in the range of 100 ° C to 230 ° C, is maintained for a treatment time of at least 0.5 seconds. In order to prevent melting of the tin layer, the treatment temperature must not exceed the melting point of tin (232 ° C). The treatment time depends on the strip speed and the length of the first heating device H1, which can range from 3 m to 30 m. With induction heating, the length of the heating device can also be reduced. After the heat treatment in the first heating device, the weight percentage of chromium oxide to the total coating weight of the passivation layer is preferably at least 95%, even more preferably more than 98%.

[0067] Figure 2A shows diagrammatically a cross-section of a tinplate strip B that can be produced using the electrolytic system of Figure 1A. The strip B, consisting of a steel substrate S, an iron-tin alloy layer (FeSn / FeSn2), a metallic tin layer (Sn) and a (tetravalent) tin oxide layer (SnO2), is provided on one side with a passivation layer P consisting essentially of pure chromium oxide. The strip B can also comprise corresponding passivation layers P on both sides.

[0068] After heat treatment in the first heating device H1, the strip B with the dried passivation layer P can be rinsed, dried and oiled (e.g. DOS). After this, the passivated strip B can further be provided with an organic coating. The organic coating is provided in a known manner on the surface of the chromium oxide passivation layer, for example by lacquering or laminating a plastic film. The chromium oxide surface of the passivation layer provides a good adhesion base for the organic material of the organic coating. The organic coating can be, for example, an organic lacquer or a polymer film made of a thermoplastic polymer such as PET, PE, PP or mixtures thereof. The organic coating can be provided, for example, by a coil coating method or a sheet method, in which the coated strip is first divided into a plurality of sheets by a sheet method, which are then coated with an organic coating or laminated with a polymer film.

[0069] FIG. 1B shows a second embodiment of an electrolysis system comprising four tanks 1a, 1b, 1c, 1d arranged one behind the other in the running direction of the strip. The two front tanks 1a, 1b in the running direction of the strip correspond to the tanks 1a and 1b in the embodiment of FIG. 1A and are filled with a basic electrolyte BE and a rinsing solution Sp. Downstream of the second tank 1b there is a third tank 1c filled with a second electrolyte E2. Next to the third tank 1c in the running direction v of the strip there is a fourth tank 1d filled with a first electrolyte E1. An example of the composition of the first electrolyte E1 and the second electrolyte E2 is shown in Table 1.

[0070] TIFF0007554805000001.tif163170

[0071] The composition of the first and second electrolytes E1, E2 differs in that the first electrolyte E1 (as in the embodiment of FIG. 1A) does not contain any organic components, in particular does not contain any organic complexing agent, whereas the second electrolyte E2 contains an organic complexing agent in addition to a trivalent chromium compound, a conductivity enhancing salt, an acid and water as solvent. In particular, a formate, for example sodium formate or potassium formate, is used as the organic complexing agent.

[0072] Due to the different compositions of the electrolytes E1 and E2 filling the two downstream tanks 1c and 1d, several layers containing chromium oxide are electrolytically deposited on the surface of the tinplate strip B in these last two tanks 1c and 1d, which differ from each other with respect to their composition. Here, in tank 1c, a lower layer L1 of the passivation layer P is deposited from the second electrolyte E2, and in the last tank 1d, an upper layer L2 is deposited from the first electrolyte E1. The lower layer L1 deposited in tank 1c from the second electrolyte E2 comprises chromium oxide / hydroxide as well as metallic chromium and chromium carbide. On the other hand, the upper layer L2 consists essentially of chromium oxide / hydroxide. The weight proportion of chromium oxide and chromium hydroxide is therefore lower in the lower layer L1 deposited in the upstream tank 1c than in the upper layer L2 deposited on the surface of the tinplate strip B in the last tank 1d, as viewed in the strip running direction. The passivation layer P deposited in the last two baths 1c, 1d is therefore composed of a lower layer L1 facing the steel substrate S and an upper layer L2 deposited on top of the lower layer L1, the compositions of the lower and upper layers differing with respect to the weight percentages of chromium oxide and chromium hydroxide as well as the weight percentages of metallic chromium and chromium carbide. In particular, the upper layer L2 has a high weight percentage of chromium oxide / hydroxide and does not contain metallic chromium. In the lower layer, a weight percentage between 10% and 50% can be attributed to metallic chromium, and the rest to chromium oxide / hydroxide and chromium carbide.

[0073] Figure 2A shows a schematic cross-sectional view of a tinplate strip B with a passivation layer P that can be produced using the electrolytic system of Figure 1B. In comparison with the embodiment of Figure 2A, the passivation layer P on the surface of the passivated tinplate strip is composed of two layers, namely a lower layer L1 and an upper layer L2, which differ from each other in terms of composition, in particular in terms of the weight percentages of chromium metal and chromium oxide / hydroxide, with the upper layer L2 having a higher weight percentage of chromium oxide / hydroxide.

[0074] As in the embodiment of Figure 1A, in the electrolytic system of Figure 1B, after the passivation layer P is applied to the surface of the tinplate strip B, a heat treatment is performed in a first heating device H1 in order to remove the chromium hydroxide from the passivation layer P, in particular from the top layer L2, by drying and conversion to chromium oxide. After the heat treatment, at least the top layer L2 consists essentially of pure chromium oxide, the weight percentage of chromium oxide relative to the total coating weight of the passivation layer P, excluding unavoidable impurities, being at least 95%, preferably more than 98%. EXAMPLES

[0075] Example 1 To determine the growth of tin oxide on the tin surface of passivated tin sheets electrolytically coated with a passivation layer containing chromium oxide based on an electrolyte containing a trivalent chromium compound, the tin sheets were passivated in the laboratory by electrolytic deposition of a passivation layer containing chromium oxide and then subjected to a heat treatment according to the invention. The samples were subsequently stored for 6 weeks in an oxygen-containing atmosphere (air) in a climate chamber at 40° C. and 80% humidity. Before the start and during the storage period, the amount of the tin oxide layer formed on the tin surface of the tinplate samples by oxidation with atmospheric oxygen was recorded. The amount of the tin oxide layer formed by oxidation to atmospheric oxygen was determined by coulometry.

[0076] For comparison, the same samples without heat treatment were exposed to the same storage conditions in a climatic chamber after electrolytic deposition of the passivation layer P, and the amount of tin oxide formed on the tin surface of the tinplate samples by oxidation by atmospheric oxygen before and during storage was also recorded coulometrically for these comparative samples.

[0077] The method and material parameters of the tested tinplate samples from the laboratory tests are shown in Table 2.

[0078] To prepare the test specimens, 1.4 g / m2 was applied to both sides. 2 A partially melted unpassivated tinplate specimen having a tin coating of 2.5 A / dm2 was placed in a 5% soda solution. 2 The electrodes were cathodically degreased after an anodizing time of 30 seconds at a current density of 2 A / dm2 and then rinsed with fully demineralized water. 2 After cathodic degreasing at a current density of 1000 s, a chromium oxide-containing passivation layer P was electrolytically formed on the tinplate sample from the first electrolyte E1 in Table 1, which was adjusted to pH=3.2 by adding sulfuric acid, at a temperature of 35°C and an electrolysis time of 0.5 to 1.0 seconds. The coating weight of the electrolytically deposited passivation layer P in terms of chromium is shown in Table 2 as "chromium support (Cr)".

[0079] The tinplate samples provided with the passivation layer P were then subjected to a heat treatment according to the invention in an oven at a temperature of 200° C. for 600 seconds, which heat treatment was not carried out on the comparative specimens of table 2 (specimen numbers 1a, 1b, 2a, 2b, 3a and 4a).

[0080] The samples heat treated according to the invention and the comparative samples were then stored for 6 weeks in a climatic chamber in the presence of atmospheric oxygen at 40° C. and 80% humidity. At the start of the storage and at two-week intervals, the amount of tin oxide layer (SnO2) formed on the tin surface of the tinplate samples during each storage period was determined by coulometry. Table 2 shows the initial amount of tin oxide layer (SnO2) present on the surface before the samples were stored and the amount of tin oxide layer (SnO2) recorded after storage periods of 2, 4 and 6 weeks. The last column of Table 2 shows the difference between the amount of tin oxide layer (SnO2) after 6 weeks of storage in the climatic chamber and the initial amount of tin oxide layer (SnO2).

[0081] From the last column of Table 2, it can be seen that the samples according to the invention (samples 1c, 2c, 3b and 4b) which have been subjected to a heat treatment according to the invention after the electrolytic deposition of the passivation layer P have a significantly lower tin oxide growth compared to the control samples (samples 1a, 1b, 2a, 2b, 3a and 4a) which have not been subjected to a heat treatment. The heat treatment of the passivated tinplate samples according to the invention therefore significantly reduces the tin oxide growth in an oxygen-containing atmosphere if the tinplate samples are stored for longer periods. In comparison, an inhibition of tin oxide growth of more than 50% can be seen in the samples treated according to the invention compared to the control samples.

[0082] Example 2 In plant tests, 2.4 g / m2 was used on both sides. 2 A tinplate strip with a tin coating of about 10 ... 2 A passivation layer P containing chromium oxide was electrolytically deposited on the tin surface of the tinplate with a coating weight (chromium support) of 1000 g / m2. After deposition of the passivation layer, the tinplate samples according to the invention (samples no. 2 to 5 in Table 3) were cooled to room temperature and heat treated in the first heating device H1 at a treatment temperature of 187° C. for different treatment times between 10 s and 120 s. The first heating device H1 was used to heat the tinplate samples. This heat treatment was not carried out on the comparative sample (sample no. 1 in Table 3). The tinplate strip was then cut into sheets and the initial amount of tin oxide on the tin surface of the samples thus produced was recorded by coulometry. The tinplate samples were stored for 4 weeks in a climate chamber at 40° C. and 80% humidity in air and the amount of tin oxide formed on the tin surface of the samples during storage, due to oxidation by atmospheric oxygen, was recorded by coulometry at intervals of 2 weeks.

[0083] Table 3 summarizes the results of the plant tests. The comparative sample (sample no. 1) was exposed to 11 C / m on the tin surface at the start of the climate chamber storage. 2This oxide occupancy rate was 44 C / m after two weeks. 2 After 4 weeks, it increased to 60C / m 2 increased to.

[0084] In contrast, the tinplate samples heat treated according to the invention (samples no. 2 to 5 in Table 3) already show a low tin oxide layer at the beginning of the climatic chamber storage, and the growth of the tin oxide layer during storage in the climatic chamber is significantly lower for the samples according to the invention, whereby the inhibition of tin oxide growth is higher at longer treatment times. For example, samples no. 4 and 5, heat treated at 187°C for treatment times of 60 s (sample no. 4) and 120 s (sample no. 5), respectively, show a tin oxide layer growth rate of 40 C / m after 4 weeks of storage in the climatic chamber. 2 Shows a tin oxide overlay of less than 40 C / m 2 Such tin oxide overlays of less than 41 C / m are preferred both visually and from the standpoint of lacquer adhesion and paintability. 2 ~69C / m 2 Tinplate with a tin oxide coating of 69 C / m shows adequate adhesion to organic coatings, but is not optimal as it has a pale yellow discoloured surface. 2 Tin oxide coatings exceeding this thickness can cause complete failure of the material, especially delamination of the organic coating, due to poor adhesion to the passivated tinplate surface.

[0085] The method according to the present invention can significantly reduce the growth of tin oxide on the tin surface of electrolytically passivated tinplate from trivalent chromium electrolyte, resulting in better adhesion of organic coatings and a desirable visual appearance of the surface.

[0086] TIFF0007554805000002.tif254170

[0087] TIFF0007554805000003.tif254170

Claims

1. 1. A method for passivating a tinplate surface by applying a passivation layer comprising chromium oxide onto the tinplate surface, comprising: the passivation layer is obtained at least in part by electrolytic deposition of a chromium oxide- and chromium hydroxide-containing passivation layer from an electrolyte (E) which contains a trivalent chromium compound, at least one salt for increasing the electrical conductivity and at least one acid or base for adjusting the desired pH value, is free of organic complexing agents and is free of buffers, 4. A method according to claim 3, characterized in that immediately after said electrolytic deposition of said passivation layer and within an intermediate time not exceeding 10 seconds after completion of the deposition of said passivation layer, the passivated tinplate is subjected to a heat treatment at a treatment temperature not less than 100° C., maintained for a treatment time of at least 0.5 seconds, in order to remove chromium hydroxide from said passivation layer.

2. The method of claim 1, wherein the treatment time is between 0.5 seconds and 30 minutes.

3. The method of claim 1, wherein the processing temperature is from 150°C to 232°C.

4. 4. The method according to claim 1, wherein for the heat treatment, the passivated tinplate is inductively heated to the treatment temperature.

5. 4. The method according to claim 1, wherein the electrolyte (E) has an average temperature in the range of 20° C. to 80° C., the passivated tinplate immediately after completion of the electrolytic deposition of the passivation layer has a tinplate temperature equal to the average temperature of the electrolyte (E), and for the heat treatment, the tinplate is heated starting from the tinplate temperature up to the treatment temperature.

6. A method according to any one of the preceding claims, in which the passivated tinplate is heated to the treatment temperature immediately after completion of the electrolytic deposition of the passivation layer at a heating rate of 100 to 700 K / s.

7. 4. The method according to claim 1, wherein the electrolyte (E) consists of the trivalent chromium compound, the at least one salt and the at least one acid or base, and a solvent.

8. 4. The method according to claim 1, wherein after the heat treatment, the passivation layer consists of trivalent chromium oxide, except for unavoidable by-products comprising residues of chromium sulfate and chromium hydroxide.

9. 4. The method according to claim 1, wherein the passivation layer obtained from the electrolyte (E) has a weight percentage of chromium oxide and chromium hydroxide of more than 95%, the remainder of the passivation layer being formed by unavoidable by-products including chromium sulfate.

10. 4. The method according to claim 1, wherein for the electrolytic deposition of the passivation layer, the tinplate passes at a speed (v) in the running direction through at least one electrolytic cell (1) or through several electrolytic cells (1a, 1b, 1c) arranged one after the other in said running direction, said speed (v) being at least 100 m / min.

11. 11. The method according to claim 10, wherein the electrolysis time (t) during which the tinplate is in effective electrolytic contact with the electrolyte (E) in the one electrolytic cell (1) or in each of the plurality of electrolytic cells (1a, 1b, 1c) is less than 1.0 second.

12. The total electrolysis time (t G 11. The method of claim 10, wherein the time t1 is between 0.5 seconds and 2.0 seconds.

13. 11. The method according to claim 10, wherein for the electrolytic deposition of the passivation layer, the tinplate passes at a speed (v) in a running direction through several electrolytic cells (1a, 1b, 1c) arranged one after the other in said running direction, and at least the last electrolytic cell (1c) in said running direction contains an electrolyte (E) consisting of the trivalent chromium compound, the at least one salt and the at least one acid or base and a solvent.

14. The passivation layer obtained from the electrolyte (E) has a chromium content of at least 3 mg / m 2 13. The method of claim 1, wherein the chromium oxide and chromium hydroxide have a total coating weight of

15. Tetravalent tin oxide (SnO 2 2. The method of claim 1, wherein a tin oxide layer consisting of a tin oxide film of 0.1% by weight of tin is formed on the surface of the tinplate prior to the electrolytic deposition of the passivation layer by placing the tinplate as an anode in an aqueous electrolyte containing a phosphate, borate, sulfate or carbonate.

16. 1. An electrolytic system for electrolytically passivating a tinplate surface by depositing a chromium oxide-containing passivation layer on said surface, comprising: at least one electrolytic cell (1) filled with a first electrolytic solution (E) comprising a trivalent chromium compound, at least one salt for increasing the electrical conductivity, at least one acid or base for adjusting the desired pH value, without organic complexing agents and without buffering agents, or A plurality of electrolytic cells (1a, 1b, 1c) arranged in series, at least one of which (1c) is filled with the first electrolytic solution (E), and the remaining electrolytic cells (1a, 1b) are filled with the first electrolytic solution (E) or with another electrolytic solution (E') containing a trivalent chromium compound and having a composition different from that of the first electrolytic solution (E); a conveying device for conveying the strip tinplate through the at least one electrolytic cell (1) or through the electrolytic cells (1a, 1b, 1c) in succession at a predetermined speed (v) in a running direction for electrolytic deposition of a passivation layer containing chromium oxide and chromium hydroxide from the first electrolyte (E) and optionally from the further electrolyte (E') on the surface of the tinplate, a heating device arranged immediately downstream of said electrolytic cell (1) in the direction of travel or immediately after the last electrolytic cell (1c) of said plurality of electrolytic cells (1a, 1b, 1c) and designed to heat the passivated tinplate to a predetermined treatment temperature of at least 100° C. for a predetermined treatment time of at least 0.5 seconds in order to remove chromium hydroxide from the passivation layer; Electrolysis system comprising:

17. 17. The electrolysis system according to claim 16, wherein the heating device is designed as a continuous furnace with a heating section having a length of at least 3 m.

18. 18. The electrolysis system of claim 16 or 17, wherein the heating device comprises an induction heater.

Citation Information

Patent Citations

  • Method for passivating the surface of a black plate or a tin plate and electrolysis system for carrying out the method

    EP3722464A1

  • FR02687693A1

  • Method of passivating surface of black plate or tin plate and electrolysis system for executing the method

    JP2020172701A

  • Method for producing tinplate and product produced therewith

    WO2014006031A1

  • Method for plating a moving metal strip and coated metal strip produced thereby

    WO2015177314A1