Method for producing electrospun nonwoven fiber membrane

Nonwoven fibrous membranes with controlled nanofiber diameters and porosity, produced by electrospinning or electroblowing, address the challenges of traditional membrane production methods, enhancing capillary flow and protein binding in lateral flow diagnostic devices.

JP7554806B2Active Publication Date: 2024-09-20MERCK MILLIPORE LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022163021
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-07-21
Filing Date
2022-10-11
Publication Date
2024-09-20
Estimated Expiration
2038-07-20

AI Technical Summary

Technical Problem

Existing methods for producing membranes for lateral flow diagnostic devices, such as air casting, are complex, slow, and sensitive to environmental conditions, leading to variations in pore size and thickness, and result in nitrocellulose membranes with handling issues like brittleness and delamination.

Method used

The use of nonwoven fibrous membranes, specifically electrospun or electroblown membranes with nanofibers of 200 nm to 1000 nm diameter and porosity of 80% to 90%, produced by electrospinning or electroblowing polymers like PMMA and PVDF, to create membranes with consistent capillary flow and high protein binding capacity.

Benefits of technology

The nonwoven fibrous membranes provide consistent capillary flow, suitable detection bead mobility, high protein binding, and durability, enabling improved lateral flow assay sensitivity and stability, with reduced brittleness and easier handling compared to traditional nitrocellulose membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554806000080
    Figure 0007554806000080
  • Figure 0007554806000021
    Figure 0007554806000021
  • Figure 0007554806000038
    Figure 0007554806000038
Patent Text Reader

Abstract

A method for producing an improved membrane useful in an electric field lateral flow diagnostic device is provided. [Solution] A method for producing an electrospun nonwoven fibrous membrane, the membrane comprising nanofibers having an average fiber diameter of 200 nm to 1000 nm, a mean flow pore size of greater than about 1 micron, and a porosity of at least 80%, the method comprising electrospinning a polymer formulation comprising PMMA, PVDF, or a blend of PMMA and PVDF in a solvent onto a non-porous polymer film substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 62 / 535,586, filed July 21, 2017, which is hereby incorporated by reference in its entirety. [Background technology]

[0002] Lateral flow diagnostic devices require a structure through which aqueous media and nanoparticles (e.g., gold or latex beads) pass by capillary flow. This structure is typically a porous membrane and must have sufficient pore size and porosity to achieve suitable flow rates and allow nanoparticle mobility while also having sufficient protein binding capacity to allow antigen binding to the surface. Membranes for use in lateral flow diagnostic devices are traditionally produced using either air-casting or phase inversion methods. These methods are complex, slow, sensitive to environmental conditions and various process parameters such as polymer dissolution conditions (% solids, solvent composition), temperature, humidity and substrate, and can produce cross-web and down-web with variations in pore size and thickness in a similar production run.

[0003] Air casting is traditionally preferred over casting non-solvent induced phase separation (NIPS) membranes because air casting has a better ability to produce symmetric membranes with mean flow pore size (MFP) greater than 2 microns and high porosity. Air cast nitrocellulose membranes are produced on large, expensive machines at slow line speeds of about 1 ft / min by solvent evaporation in a moving web from a nitrocellulose polymer solution. Air cast nitrocellulose membranes present challenges both in production and for end users, especially in terms of nitrocellulose stability, handling, shelf life, and flammability. Also, casting nitrocellulose membranes onto non-porous films often has handling issues, including brittleness and delamination, making them difficult to use in assay production.

[0004] In lateral flow diagnostic devices, the detection particles, typically 40 nm gold or 400 nm latex beads, must migrate freely in the membrane and at the liquid front for proper assay function in forming the test and control lines. Larger MFPs and porosities are required in lateral flow diagnostic devices for fast enough capillary flow times (CFTs) and to allow detection particle bead mobility without frontal separation of the liquid bead flow. Summary of the Invention [Problem to be solved by the invention]

[0005] Thus, there is a need in the art for improved membranes useful in lateral flow diagnostic devices, and for more efficient manufacturing methods for producing such membranes. [Means for solving the problem]

[0006] Summary of the Invention In certain aspects, provided herein are nonwoven fibrous membranes suitable for use in assay development regions of lateral flow diagnostic devices. In some embodiments, the membrane comprises a nonwoven fibrous mat. In certain embodiments, the nonwoven fibrous membrane comprises nanofibers having an average fiber diameter of 200 nm to 1000 nm, the membrane having an MFP of greater than about 1.5 microns, and a porosity of at least 80% to 90%. In certain embodiments, the nonwoven fibrous membrane comprises nanofibers produced by electrospinning a polymer or blend of polymers, such as polymethacrylate (PMMA), poly(vinylidene fluoride) (PVDF), or blends thereof. In some embodiments, the nonwoven fibrous membrane comprises nanofibers produced by electroblowing.

[0007] In some aspects, provided herein is a lateral flow diagnostic device designed for detecting an analyte in a sample. In some embodiments, the lateral flow diagnostic device provided herein may include a sample port designed to receive a sample, a conjugate pad, an assay development area including a non-woven fibrous membrane, and / or an absorbent pad. In some embodiments, the conjugate pad, the non-woven fibrous membrane, and the absorbent pad are connected to each other such that they are in capillary flow communication with each other.

[0008] In certain aspects, provided herein are methods of using such lateral flow diagnostic devices to detect analytes, such as metabolites, hormones, therapeutic agents, drugs of abuse, peptides, antibodies and / or antigens, in biological samples.

[0009] Further, in some aspects, provided herein are methods of producing the nonwoven fibrous membranes, electrospun membranes, and / or electroblown membranes described herein. In some embodiments, the methods include electrospinning (e.g., needleless electrospinning) or electroblowing a polymer formulation onto a non-porous film or porous substrate. In certain embodiments, the method of producing the nonwoven fibrous membrane includes electrospinning (e.g., needleless electrospinning) a solution containing about 15%-20% PMMA and / or PVDF in the solvent N,N-dimethylacetamide (DMAC) and / or N,N-dimethylformamide (DMF). [Brief description of the drawings]

[0010] [Figure 1] 1 shows a cross-section of an exemplary lateral flow diagnostic device, in certain embodiments provided herein, the membrane in the assay deployment area is an electrospun nonwoven fiber mat membrane as disclosed herein. [Diagram 2] FIG. 1 shows an example of a prior art Hi-Flow™ Plus nitrocellulose membrane on an air-cast polyethylene terephthalate (PET) backing. [Figure 3.1]Scanning electron micrograph (SEM) of an air-cast Hi-Flow™ Plus nitrocellulose membrane. 1000× top view. [Figure 3.2] FIG. 1 shows a scanning electron micrograph (SEM) of an air-cast Hi-Flow™ Plus nitrocellulose membrane: 600× freeze-fractured cross section. [Figure 4] 1 shows an exemplary needle electrospinning process schematic: The spinning electrode is a metal syringe that also dispenses the polymer solution via a syringe pump. [Diagram 5] FIG. 1 is a schematic representation of an exemplary needleless electrospinning process, depicting a rotating wire electrode, 10 is a polymer bath, 20 is a rotating spinning electrode, 30 is a collecting substrate, 35 is a collecting electrode, 40 is a voltage source, 50 and 60 are fibers. [Figure 6] Figure 1 shows that the diameter and morphology of electrospun fibers are mainly controlled by PMMA:PVDF ratio, % solids, solvent and dew point. The productivity and uniformity of electrospun nonwoven fiber mats are controlled by four parameters: PMMA:PVDF ratio, electrospinning parameters, dew point and film substrate. The properties that affect the performance of membranes in lateral flow diagnostic devices, e.g. CFT, detection bead mobility, protein binding, protein stripping and functional assay performance, are fiber diameter / effective pore size, PMMA:PVDF ratio, surfactant treatment, mat thickness and uniformity. [Figure 7] FIG. 2 shows SEM images of high fiber quality electrospun from 15% w / v PVDF6 (Kynar® 761) in DMAC (Table 2), resulting in an average fiber diameter of 360±120 nm. [Figure 8] FIG. 1 shows an SEM of electrospun fibers from a 25% w / v solution of PVDF2 (Kynar® 711) in DMAC with an average fiber diameter of 240±55 nm and undesired beads. [Figure 9]FIG. 14 shows an SEM of larger diameter fibers (600±290 nm) electrospun from a 15% w / v solution of 20:80 PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC (Mix 2, Table 4). [Figure 10] FIG. 1 is a graph showing that for various PVDF grades (Table 2), PVDF6 (Kynar® 761) produced the highest viscosity at the lowest % w / v solution in DMAC and DMF. [Figure 11] FIG. 13 shows that for PVDF6 (Kynar® 761), DMF is a better solvent than DMAC due to its lower viscosity at the same w / v %, and the viscosity of this solution in PVDF6 is dramatically different from PVDF2 (Kynar® 711). [Figure 12] The PMMA grades (Table 3) are graphs showing that PMMA5 (BS572) produced higher solution viscosities at low w / v % in DMAC and DMF than the low molecular weight PMMA1 (V920) in DMAC. [Figure 13] 1 is a graph showing the blend viscosity of a 15% w / v solution versus blend ratio of high MW PMMA5 (BS572) and PVDF6 (Kynar® 761) with low MW PMMA1 (V920) and PVDF2 (Kynar® 711). [Figure 14] FIG. 1 is a graph showing the mixture viscosity of a 15% w / v solution versus the mixture ratio of PMMA5 (BS572) and PVDF6 (Kynar® 761) in DMAC and solution conductivity (μS / cm) on the secondary y-axis. [Figure 15] FIG. 1 shows the viscosity of solutions of increasing w / v % of PVDF6 (Kynar® 761) and PMMA as viscosity modifiers [PMMA1 (V920), PMMA5 (BS572) and PMMA4 (PRD521)] in DMAC at a ratio of 75:25 (PVDF6:PMMA), verifying that PMMA5 (BS572) had the greatest impact on viscosity at the lower w / v %. [Figure 16]FIG. 1 shows the viscosity of solutions of increasing w / v % of PVDF2 (Kynar® 711) and PMMA as viscosity modifiers [PMMA1 (V920), PMMA5 (BS572) and PMMA4 (PRD521)] in DMAC at a ratio of 75:25 (PVDF2:PMMA), verifying that PVDF6 was the choice for higher viscosity and that PMMA5 (BS572) had the greatest impact on viscosity at the lower w / v %. [Figure 17] FIG. 15 is a graph showing that 15-18 w / v% solutions of PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC with mixing ratios of 100:0, 75:25, 50:50, 25:75, and 0:100 can control the diameter of electrospun fibers. [Figure 18] FIG. 1 is a graph showing that increasing the ratio of PMMA5 (BS572) to PVDF6 (Kynar® 761) and increasing the concentration from 15 to 20% w / v results in higher viscosity. [Figure 19] FIG. 13 shows that increasing the ratio of PMMA5 (BS572) to PVDF6 (Kynar® 761) and increasing the concentration from 15-20% w / v results in larger average fiber diameters produced by electrospinning. [Figure 20] FIG. 1 shows a heterogeneous electrospun nonwoven fiber mat electrospun onto stationary Melinex® PET. [Figure 21] FIG. 13 shows SEM cross-sectional images of electrospun nonwoven fiber mat quality when electrospun on stationary Melinex® PET. [Figure 22]22 is a graph showing a plot of fiber mat thickness or productivity vs. bulk electrical resistivity of the substrate. Figure 22 shows a plot of fiber mat thickness generated from a selection of films in Table 5 (1-5, 5b-8b, 12, 17) with elevated bulk resistivity produced under identical electrospinning conditions, over the same 10 minute spinning time, and at a film width of 40 cm. This illustrates that an optimal range of bulk electrical resistivity is found at the peak of fiber mat thickness or productivity. [Figure 23] FIG. 13 shows images of electrospun nonwoven fiber mat membranes electrospun onto a fixed LDPE film (#12 in Table 5). [Figure 24] FIG. 23 shows SEM cross-sectional images of electrospun fibers on LDPE film (#12 in Table 5) with productivity of fiber mats about 90 μm thick and better fiber packing quality compared to Melinex® PET in FIG. 21 under identical electrospinning conditions. [Diagram 25] FIG. 1 shows images of a moving web at a line speed of 2 cm / min outside an ELMARCO NS1WS500U unit from Table 1 and electrospun nonwoven fibrous mat coated onto an LDPE film. [Figure 26.1] 1 shows SEM images of electrospun fibers. 2 shows SEM images of electrospun fibers on the air side. [Figure 26.2] Figure 1 shows an SEM image of electrospun fibers. Figure 2 shows an SEM image of electrospun fibers on an LDPE surface. Electrospun fibers are produced from 17% w / v PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC on a moving web of LDPE film. [Figure 27] FIG. 1 shows electrospun fiber mats produced from 17% w / v PMMA5 (BS572):PVDF6 (Kynar® 761) in a 60:40 ratio in DMAC with decreasing humidity from left to right. [Figure 28.1] FIG. 28 shows SEM images of the electrospun samples in FIG. 27 at 11.8° C. dew point out of three different dew points. [Figure 28.2]FIG. 28 shows SEM images of the electrospun samples in FIG. 27 at 3.2° C. dew point out of three different dew points. [Figure 28.3] FIG. 28 shows SEM images of the electrospun samples in FIG. 27 at 2.6° C. dew point out of three different dew points. [Figure 29] FIG. 13 shows a plot of average fiber diameter versus reduced dew point obtained by electrospinning a 17% w / v solution of PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC in ratios of 75:25, 60:40, and 50:50, collected on a moving LDPE web at reduced humidity. [Diagram 30] FIG. 13 shows a plot of the average diameter of electrospun fibers of various w / v % solutions and PMMA5 (BS572):PVDF6 (Kynar® 761) ratios at two known relative humidity % produced by the same electrospinning parameters. [Diagram 31] 1 is a graph showing the linearity of the net average thickness of the electrospun fiber mat with respect to basis weight for several conditions of voltage and line speed in Table 6. [Diagram 32] FIG. 13 shows images of the cross-web and down-web sampling areas (60×40 cm) and locations used to measure the thickness of electrospun fiber mats to determine productivity and uniformity. [Figure 33.1] 13 is a graph showing plots of net average thickness and basis weight of the solution and mat at 60 kV constant voltage for the 1 / line speed electrospinning experiments detailed in Table 6. [Figure 33.2] 3 is a graph showing a plot of net average thickness of the mat from the previously described experiment (Figure 33.1) at a constant voltage of 60 kV vs. 1 / line speed collected on a moving web of 100 μm thick LDPE film (#12 in Table 5) overlaid on a mat electrospun under identical conditions except at 100 kV on a moving web of Permastat LDPE PE700AS film (#7b in Table 5). [Diagram 34]FIG. 33 is a graph showing plots of sample thickness and uniformity versus position detailed in FIG. 32 for solutions and constant line speed for electrospinning experiments at voltages detailed in Table 6. [Diagram 35] FIG. 33 is a graph showing a plot of sample thickness and uniformity versus the position detailed in FIG. 32 for the solutions in Table 6 at 100 kV for line speed. [Figure 36.1] Figure 36 shows SEM images of the experiment in Figure 35. Figure 37 shows an SEM cross-sectional image (600x magnification) of the fiber mat produced in Figure 35 at 1.0 cm / min line speed. [Figure 36.2] Figure 36 shows SEM images of the experiment in Figure 35. Figure 37 shows an SEM cross-sectional image (magnification 2000x) of the fiber mat produced in Figure 35 at 2.0 cm / min line speed. [Figure 36.3] Figure 36 shows SEM images of the experiment in Figure 35. Figure 37 shows an SEM cross-sectional image (magnification 2000x) of the fiber mat produced in Figure 35 at 5.0 cm / min line speed. [Figure 37] FIG. 1 shows an SEM image of 733±263 nm fibers electrospun at 30 kV from 14% w / v PMMA5 (BS572):PVDF6 (Kynar® 761) in 90:10 DMAC:acetone at a ratio of 75:25 at 35° C. and 45% relative humidity. [Figure 38.1] 1 shows a plot of pore size distribution versus average diameter for air-cast nitrocellulose and electrospun nonwoven fibrous mats.1 shows a plot of pore size distribution versus average diameter for an unbacked nitrocellulose membrane (Hi-Flow™ Plus 180UB, Millipore Sigma) produced by air casting. [Figure 38.2]1 shows a plot of pore size distribution vs. average diameter for air cast nitrocellulose and electrospun nonwoven fibrous mats.1 shows a plot of pore size distribution vs. average diameter for an electrospun nonwoven fibrous mat electrospun from a 17% w / v solution of PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC in a ratio of 75:25, with an average fiber diameter of about 700 nm. [Figure 39] 13 is a graph showing a plot of CFT versus MFP with positive error bars stretched to show the maximum flow pore size for air-cast nitrocellulose and electrospun nonwoven fibrous mats with CFTs of approximately 135 to 180 seconds. [Diagram 40] 1 is a graph showing a plot of CFT against average fiber diameter illustrating the relationship between CFT and average fiber diameter. [Diagram 41] 1 is a graph showing a plot of MFP with positive error bars stretched to show maximum flow pore size versus average fiber diameter illustrating the relationship between MFP and average fiber diameter of electrospun fiber mat membranes. [Diagram 42] FIG. 1 shows four test strips tested for delamination and brittleness. Samples shown from left to right are air-cast nitrocellulose (Hi-Flow™ Plus 135) and electrospun nonwoven fiber mat membranes collected on the corona-treated side of LDPE film (delamination, brittle and as-spun), all of which passed the delamination and brittleness tests. [Figure 43.1] Figure 1 shows images of delamination and shrinkage testing of electrospun fiber mats with an average fiber diameter of about 700 nm on LDPE films after IPA / water wetting, surfactant treatment and air drying.Images of duplicate electrospun membranes die cut to 56 mm circles with an average fiber diameter of about 700 nm spun on a corona treated surface of LDPE after IPA / water wetting, surfactant treatment and air drying showing good adhesion and no shrinkage / delamination of the fiber mat. [Figure 43.2]Figure 1 shows images of delamination and shrinkage testing of electrospun fiber mats with an average fiber diameter of about 700 nm on LDPE film after IPA / water wetting, surfactant treatment and air drying. Images of duplicate electrospun membranes cut into rectangles with an average fiber diameter of about 700 nm spun onto the non-corona treated side of LDPE to delaminate after IPA / water wetting, surfactant treatment and air drying. The figures show minimal shrinkage after drying, even when intentionally delaminated from the film substrate. [Figure 44.1] FIG. 1 shows an SEM cross-sectional image of electrospun nonwoven fibers spun directly onto a conductive polyimide film (Kapton® XC, DuPont) surface containing a pressure sensitive acrylic adhesive as a way to improve adhesion. [Figure 44.2] FIG. 1 shows images of electrospun nonwoven fiber mats directly spun onto GL-187® adhesive from Lohmann Corporation (Orange, VA), which was coated onto a Permastat LDPE PE700AS film (#7b in Table 5). [Figure 44.3] FIG. 14 shows an SEM cross-sectional image of an electrospun nonwoven fiber mat directly spun onto GL-187® adhesive from Lohmann Corporation (Orange, VA), which was coated onto a Permastat LDPE PE700AS film (#7b in Table 5). [Figure 44.4] FIG. 1 shows an image of an electrospun nonwoven fiber mat electrospun onto the non-adhesive, non-corona treated side of a Permastat LDPE PE700AS film (#7b in Table 5) and transferred from there onto GL-187® adhesive from Lohmann Corporation (Orange, VA) coated onto a Permastat LDPE PE700AS film (#7b in Table 5). [Figure 44.5]Figure 5 shows an SEM cross-sectional image of an electrospun nonwoven fiber mat electrospun onto the non-adhesive, non-corona treated side of a Permastat LDPE PE700AS film (#7b in Table 5) and transferred from there onto GL-187® adhesive from Lohmann Corporation (Orange, VA) coated onto a Permastat LDPE PE700AS film (#7b in Table 5). [Figure 45.1] 1 shows images of an electrospun fiber mat on the non-adhesive side of a Kapton® XC film after IPA / water wetting, surfactant treatment and air drying. 2 shows images of a replicate sample of electrospun fibers spun on the non-adhesive side of a Kapton® XC film, where the fiber mat delaminates after IPA / water wetting, surfactant treatment and air drying. [Figure 45.2] 1 shows an image of an electrospun fiber mat on the adhesive side of a Kapton® XC film after IPA / water wetting, surfactant treatment and air drying. 2 shows an image of a replicate sample of electrospun fibers spun on the acrylic adhesive side of a Kapton® XC film, where the fiber mat remains well bonded after IPA / water wetting, surfactant treatment and air drying. [Diagram 46] FIG. 1 shows an image of a custom test stand used to measure CFT and bead mobility. [Figure 47.1] Figure 1 shows images of membranes after a latex detection bead mobility test.Images of duplicate electrospun membranes with an average fiber diameter of 632±212 nm and a CFT of about 200 seconds are shown, which passed the bead mobility test, as well as the Hi-Flow™ Plus 135 control. [Figure 47.2] Figure 1 shows images of membranes after a latex detection bead mobility test.Images of duplicate electrospun membranes with an average fiber diameter of 432±95 nm and a CFT of about 300 seconds are shown, which failed the bead mobility test with visible defects in bead mobility over the entire 4 cm length. [Figure 48.1]1 shows SEM cross-sectional images of Hi-Flow™ Plus 135 with 400 nm beads visible in cross section, and electrospun fiber mat samples with latex beads passing.14 shows SEM cross-sectional images of a Hi-Flow™ Plus 135 sample passing the latex bead mobility test with beads visible in cross section. [Figure 48.2] 1 shows SEM cross-sectional images of electrospun fiber mat samples with 400 nm beads visible in cross section, Hi-Flow™ Plus 135, and latex beads passing through.FIG. 2 shows SEM cross-sectional images of electrospun fiber samples passing the latex bead mobility test with beads visible in cross section. [Figure 49] 1 is a graph showing a plot of CFT versus average fiber diameter for electrospun nonwoven fiber mat membranes at similar net thickness of the mat. The shaded areas indicate whether the membrane passed / failed the latex bead mobility test. [Figure 50] 13 shows plots of additional samples measured for CFT versus average fiber diameter for electrospun nonwoven fiber mat membranes electrospun on a moving web of LDPE. The solution was 17% w / v PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC in a 75:25 ratio, and the fiber diameters vary because the dew point was not controlled. [Figure 51] 1 is a graph showing a plot of CFT versus average net thickness of a fiber mat for an electrospun nonwoven fiber mat having an average fiber diameter of about 700 nm. [Figure 52.1] 1 is a graph showing the correlation between CFT, relative humidity and mat thickness. A plot of CFT versus % relative humidity is shown for electrospun fibrous membranes with various mat thicknesses and a Hi-Flow™ Plus 135 nitrocellulose control. [Figure 52.2] 1 is a graph showing the correlation between CFT, relative humidity and mat thickness. FIG. 1 shows a plot of CFT versus membrane mat thickness at various equilibrium relative humidity %. [Figure 53]1 is a graph showing a plot of mat thickness versus basis weight for electrospun fibers with 75:25 PMMA:PVDF and an average fiber diameter of about 700 nm, and a Hi-Flow™ Plus 135 control. [Figure 54.1] 1 is a graph showing a plot of CFT versus wt % surfactant treatment concentration for Surfactant 1 on electrospun nonwoven fibrous mats of various thicknesses. FIG. 2 shows a plot of CFT versus wt % Surfactant 1 treatment. [Figure 54.2] 13 is a graph showing a plot of CFT versus wt% surfactant treatment concentration for Surfactant 2 on electrospun nonwoven fibrous mats of various thicknesses. FIG. 14 shows a plot of CFT versus wt% Surfactant 2 treatment. [Figure 55] 1 is a graph showing a plot of CFT versus net average thickness of fiber mats for treatments of 0.1 wt % Surfactant 1 and Surfactant 2. [Figure 56.1] 1 shows a plot of IgG binding versus wt% surfactant treatment concentration for electrospun nonwoven fiber mats of various thicknesses.FIG. 1 shows a plot of IgG binding versus wt% surfactant 1 treatment concentration. [Figure 56.2] 1 shows a plot of IgG binding versus wt% surfactant treatment concentration for electrospun nonwoven fiber mats of various thicknesses.FIG. 2 shows a plot of IgG binding versus wt% surfactant 2 treatment concentration. [Figure 57] FIG. 1 is a graph showing a plot of IgG binding versus net average thickness of approximately 700 nm PMMA:PVDF (75:25) fibers treated with various wt % of Surfactant 1 and Surfactant 2, as well as a fiber mat of a Hi-Flow™ Plus 135 control. [Figure 58.1] FIG. 9. Protein stripping quality images for samples in Table 9.1. [Figure 58.2]FIG. 9 shows images of protein stripping samples of replicate samples of electrospun nonwoven fiber mat membranes of PMMA:PVDF (70:30) treated with, from left to right, Hi-Flow™ Plus 135 control and 0.07 and 0.09% Surfactant 2 (Example 20) at the protein (IgG) dissolution conditions detailed in Table 9.2. [Figure 58.3] FIG. 9 shows images of protein stripping samples of, from left to right, duplicate Hi-Flow™ Plus 135 control and replicate samples of PMMA:PVDF (70:30) electrospun nonwoven fiber mat membranes treated with 0.07 and 0.09% Surfactant 2 (Example 20) at protein (IgG) dissolution conditions detailed in Table 9.3. [Figure 59] FIG. 1 shows fluorescence spectral intensity versus excitation (300-610 nm) and emission wavelength (320-630 nm) for Hi-Flow™ Plus 135 nitrocellulose control membrane. [Figure 60.1] Figure 1 shows fluorescence spectral intensity versus excitation (300-610 nm) and emission wavelength (320-630 nm) for one of two ratios [PMMA:PVDF membrane - Hi-Flow™ Plus 135 nitrocellulose control membrane], demonstrating that electrospun nonwoven fiber mats are less fluorescent than the nitrocellulose control. Figure 1 shows fluorescence spectral intensity versus excitation (300-610 nm) and emission wavelength (320-630 nm) for [PMMA:PVDF (75:25) membrane - Hi-Flow™ Plus 135 nitrocellulose control membrane]. [Figure 60.2] Figure 1 shows fluorescence spectral intensity versus excitation (300-610 nm) and emission wavelength (320-630 nm) for one of two ratios [PMMA:PVDF membrane - Hi-Flow™ Plus 135 nitrocellulose control membrane], demonstrating that electrospun nonwoven fiber mats are less fluorescent than the nitrocellulose control. Figure 1 shows fluorescence spectral intensity versus excitation (300-610 nm) and emission wavelength (320-630 nm) for [PMMA:PVDF (50:50) membrane - Hi-Flow™ Plus 135 nitrocellulose control membrane]. [Figure 61]FIG. 1 shows fluorescent microscopy images of Hi-Flow™ Plus 135 nitrocellulose control membrane and PMMA:PVDF (75:25) membrane with and without fluorescently labeled beads at 200× magnification, FITC mode and constant laser excitation intensity. [Figure 62] FIG. 1 shows images of electrospun PMMA membranes produced by an exemplary method provided herein having thicknesses of 21 μm, 37 μm, and 60 μm. [Figure 63] Figure 1 shows SEMs of electrospun membranes produced by the methods provided herein. Membranes are produced using the following polymers and polymer blends: PMMA, PVB, PVDF, PA, PES, NC, PMMA / PVDF, PVDF / PMMA, PMMA / PVB, PMMA / PVB / SDBS, PES / PVP, and NC / PVB / SDBS. The images illustrate the porosity, pore size, and surface morphology of the electrospun membranes. High magnification SEM shows the electrospun membrane to be bead-free and uniformly fibrous. [Figure 64] 1 shows protein attachment to electrospun membranes produced by the methods provided herein.Membranes were electrospun using PMMA, PVB and PVDF. [Figure 65] FIG. 1 shows an examination of gold nanoparticle mobility in electrospun membranes produced by the exemplary methods provided herein. [Figure 66] FIG. 1 shows latex mobility testing of electrospun membranes produced by the exemplary methods provided herein. Bead test mobility of latex beads with diameters greater than 0.4 μm was evaluated on electrospun membranes. The membranes show no flow front separation between the liquid and the latex beads. [Figure 67] Figure 1 shows an SEM of a PMMA membrane produced by an exemplary method provided herein after gold nanoparticle and latex bead mobility testing, where the particles flow along the face of the fiber through interconnected pores without any separation of the flow front as shown in the high magnification SEM. [Figure 68]1 shows protein binding of two PMMA / PVDF blend electrospun membranes with different PMMA / PVDF ratios produced by the exemplary method provided herein. The results indicate that proteins are found on the electrospun membrane and its potential properties in lateral applications. [Figure 69] FIG. 1 shows an examination of gold nanoparticle mobility in two PMMA / PVDF electrospun membranes with different PMMA / PVDF ratios produced by the exemplary methods provided herein. [Figure 70] FIG. 1 shows Hepatitis B assay of (a) 85 μm thick PVDF membrane, (b) 119 μm thick PVDF membrane, (c) 68 μm 2:1 PMMA / PVDF blend membrane, and (d) 65 μm 1:2 PMMA / PVDF blend membrane. [Figure 71.1] FIG. 1 shows a passing test result for a lateral flow test of intact Hepatitis B surface antigen (HBsAg) on ​​an electrospun nonwoven fiber mat membrane. [Figure 71.2] FIG. 1 shows a successful test result for a lateral flow test for intact Hepatitis B surface antigen (HBsAg) on ​​air-cast nitrocellulose. [Figure 72.1] FIG. 1 shows the passing of the functional test of hCG (human chorionic gonadotropin hormone) to detect pregnancy on electrospun nonwoven fiber mat membrane. [Figure 72.2] FIG. 1 shows a test pass for the hCG (human chorionic gonadotropin hormone) functional test to detect pregnancy on air-cast nitrocellulose. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] General Lateral flow diagnostic devices operate on a series of capillary beds arranged in capillary flow communication with one another. The materials used in the assay development regions in lateral flow devices require certain properties for optimal performance of the assay. These properties include consistent capillary flow, suitable detection bead mobility, suitable detection line morphology, high protein binding and durability.

[0012] In certain aspects, provided herein are nonwoven fibrous membranes (e.g., electrospun or electroblown nonwoven fibrous mat membranes) suitable for use in lateral flow diagnostic devices. In certain embodiments, the nonwoven fibrous membranes provided herein exhibit desirable properties for use in lateral flow diagnostic devices (e.g., consistent capillary flow, suitable detection bead mobility, suitable detection line morphology, high protein binding, and high durability). In certain embodiments, provided herein are lateral flow diagnostic devices comprising the nonwoven fibrous membranes provided herein, and methods of using such devices. In certain embodiments, provided herein are methods of making such nonwoven fibrous membranes using needle electrospinning, needleless electrospinning, or electroblown.

[0013] In certain embodiments, the larger diameter electrospun or electroblown fibers disclosed herein produce fiber mats that have and exhibit unique properties, such as high bulk porosity, large pore size ratings with narrow distribution, high surface area, and highly tunable protein binding. In certain embodiments, the electrospun or electroblown fiber mats disclosed herein may provide greater lateral flow assay sensitivity, enabling future applications that utilize these aforementioned properties. In some embodiments, the electrospun or electroblown fiber mats are also flexible rather than brittle, making it easier to roll or fold the mats compared to existing air-cast nitrocellulose membranes, thereby opening the door to non-planar applications.

[0014] definition For convenience, certain terms employed in the specification, examples, and appended claims are collected here.

[0015] As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.

[0016] The term "about" means within an acceptable error range as determined by one of ordinary skill in the art for a particular value, which depends in part on how the value is measured or determined, i.e., the limitations of the measurement system. For example, "about" can mean within 1 or more than 1 standard deviation, as is customary in the art. "About" can mean a range of 0-20%, 0-10%, 0-5%, or up to 1% of a given value. When the terms "about" or "approximately" are used with respect to compositions containing quantities of ingredients or conditions, such as temperature or viscosity, these values ​​include the stated value and a variation around the value of 0-10% (X±10%).

[0017] The terms "including," "includes," "having," "has," "with," and variations thereof are inclusive, as is the term "comprising." The phrase "consisting essentially of" or "consists essentially of" includes embodiments containing the specified materials or steps, as well as those including materials and steps that do not materially affect the basic and novel characteristic(s) of the embodiment.

[0018] Ranges are written in abbreviated form to avoid having to redundantly describe and explain each and every value within the range. Thus, when a range is described for a value, any suitable value within the range can be selected, and these values ​​include the upper and lower values ​​of the range. For example, a range of 0.1 to 1.0 represents the end values ​​of 0.1 and 1.0, as well as intermediate values ​​of 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and all intermediate ranges contained within 0.1 to 1.0, such as 0.2 to 0.5, 0.2 to 0.8, 0.7 to 1.0, etc.

[0019] "Nitrocellulose," also known as cellulose nitrate, is a polymer formed by nitrating cellulose with a nitrating agent, such as nitric acid.

[0020] As used herein, an "air-cast membrane" is a porous structure formed from a polymer dissolved in a solvent through a process of controlled evaporation of the solvent.

[0021] As used herein, the phrase "capillary flow porometry" is used interchangeably with the term "porometry" and is a characterization technique based on the evacuation of a wetting liquid from the pores of a sample by application of a gas at elevated pressure.

[0022] As used herein, the term "mean flow pore size" or "MFP" refers to the pore size calculated in capillary flow porometry as the midpoint from the flow pressure curve where the wetting curve meets the dry curve halfway. MFP corresponds to the pore size at which 50% of the gas flow passes through the wet membrane.

[0023] As used herein, the "maximum flow pore size" is the first bubble point measured and calculated at the pore size at which the first flow is detected through a wet membrane by capillary flow porometry.

[0024] As used herein, the term "capillary flow time" or "CFT" refers to the time it takes for a uniform liquid front to traverse 4 cm of a 1 x 4 cm strip. To measure the CFT, a 1 x 4 cm test strip is placed in a well containing 150 μL of water, and the time it takes for a uniform liquid front to traverse the entire length of 4 cm is measured as the CFT.

[0025] The "detection bead mobility test" examines the ability of a membrane to freely pass beads of a particular size through its pore structure without any separation between the liquid flow front and the bead front. Typically, in this test, colored beads are used to facilitate visualization of the bead front. A membrane passes the detection bead mobility test only if there is no visible separation between the clear liquid flow front and the colored front line of the detection beads. Typically, the detection bead mobility test is performed on a 1 x 4 cm test membrane immersed in a 25 μL solution containing latex beads of a particular size, and the solution containing the beads is allowed to flow over the top. The liquid front and bead front are observed to determine whether the test membrane passes the detection bead mobility test.

[0026] The term "porosity" is used herein to describe the size of voids in a material, which is the ratio of void volume to the total volume.

[0027] The percent porosity is calculated based on the following equation: Porosity %=[1-(basis weight / (mat thickness x polymer density))], where basis weight is in g / m 2 and the unit of polymer density is g / m 3 and the unit of mat thickness is m.

[0028] The phrase "assay development area" corresponds to an area of ​​the device designed to indicate the presence or absence of an analyte. Typically, the assay development area includes a test area that contains a binding agent that specifically binds to the analyte or a conjugate of the analyte, along with other components used in the device. The assay development area may also include a control area that contains a binding agent that specifically binds to a material used in the device, which is designed to detect whether the assay has performed as expected.

[0029] As used herein, the term "surfactant" refers to a compound that reduces the surface tension (or interfacial tension) between two liquids or between a liquid and a solid. Surfactants can function as detergents, wetting agents, emulsifiers, foaming agents, and dispersants. In some examples, surfactants are amphiphilic organic compounds, which means that they contain both hydrophobic groups (tails) and hydrophilic groups (heads). Thus, surfactants can contain both water-insoluble (or oil-soluble) and water-soluble components. When water is mixed with oil, surfactants diffuse into the water and adsorb to the interface between air and water, or between oil and water. The water-insoluble hydrophobic groups can extend from the bulk water phase into the air or oil phase, while the water-soluble head groups remain in the water phase.

[0030] Non-woven fiber membrane In certain aspects, provided herein are nonwoven fibrous membranes useful in lateral flow diagnostic devices. In certain embodiments, the nonwoven fibrous membranes provided herein are fabricated by an electrospinning process. In some embodiments, the electrospinning process is a needleless electrospinning process. In some embodiments, the electrospinning process is a needle electrospinning process. In some embodiments, the nonwoven fibrous mat is produced by an electroblowing process.

[0031] In some embodiments, the nonwoven fibrous membranes, electrospun membranes and / or electroblown membranes described herein are comprised of electrospun or electroblown nonwoven nanofibers having an average fiber diameter of 200 nm to 1000 nm. In certain embodiments, the nanofibers have an average fiber diameter of at least 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, 800 nm, 850 nm, 900 nm or 950 nm. In some embodiments, the nanofibers have an average fiber diameter of 1000 nm or less, 950 nm, 900 nm, 850 nm, 800 nm, 750 nm, 700 nm, 650 nm, 600 nm, 550 nm, 500 nm, 450 nm, 400 nm, 350 nm, 300 nm or 250 nm. In some embodiments, the nanofibers have an average fiber diameter of at least about 500 nm. In one embodiment, the nonwoven nanofibers have an average fiber diameter of 200±40 nm, 250±50 nm, 300±60 nm, 350±70 nm, 400±80 nm, 450±90 nm, 500±100 nm, 550±110 nm, 600±120 nm, 650±130 nm, 700±140 nm, 750±150 nm, 800±160 nm, 850±170 nm, 900±180 nm, 950±190 nm, or 1000±200 nm. In certain embodiments, the fibrous membranes provided herein are comprised of non-woven nanofibers, wherein at least 80%, 85%, 90%, 95%, or 99% of the nanofibers have a fiber diameter of 200±40 nm, 250±50 nm, 300±60 nm, 350±70 nm, 400±80 nm, 450±90 nm, 500±100 nm, 550±110 nm, 600±120 nm, 650±130 nm, 700±140 nm, 750±150 nm, 800±160 nm, 850±170 nm, 900±180 nm, 950±190 nm, or 1000±200 nm.In certain embodiments, the fibrous membranes provided herein are comprised of non-woven nanofibers, wherein at least 80%, 85%, 90%, 95%, or 99% of the nanofibers have a fiber diameter of about 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, 800 nm, 850 nm, 900 nm, 950 nm, or 1000 nm.

[0032] In some embodiments, the nonwoven fibrous membranes provided herein have an MFP of at least about 1 micron. In some embodiments, the nonwoven fibrous membranes provided herein have an MFP of at least about 2 microns. In certain embodiments, the nonwoven fibrous membranes provided herein have an MFP of at least about 1.0 microns, 1.2 microns, 1.3 microns, 1.4 microns, 1.5 microns, 1.6 microns, 1.7 microns, 1.8 microns, 1.9 microns, 2.0 microns, 2.1 microns, 2.2 microns, 2.3 microns, 2.4 microns, 2.5 microns, 2.6 microns, 2.7 microns, 2.8 microns, 2.9 microns, 3.0 microns, 3.5 microns, or 4.0 microns. In some embodiments, the MPF of the nonwoven fibrous membrane is 1-4 microns, 1.5-4 microns, 2-4 microns, 1-3.5 microns, 1.5-3.5 microns, 2-3.5 microns, or 2.5-3.5 microns. In certain embodiments, the nonwoven fibrous membranes provided herein have a pore size distribution as shown in Figure 38.2.

[0033] In some embodiments, the nonwoven fibrous membranes provided herein have a porosity of at least about 70%. In some embodiments, the nonwoven fibrous membranes have a porosity of at least 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, or 90%. In some embodiments, the nonwoven fibrous membranes have a porosity of 70%-95%, 70%-90%, 75%-90%, or 80%-90%.

[0034] In certain aspects, the nonwoven fibrous membranes provided herein are comprised of nanofibers that are electrospun using, for example, needle electrospinning or needleless electrospinning. In some embodiments, the nonwoven fibrous membranes provided herein are comprised of nanofibers that are electrospun using needleless electrospinning.

[0035] In some embodiments, the nonwoven fibrous membranes provided herein are comprised of nanofibers made from a polymer or blend of polymers suitable for electrospinning or electroblowing into nanofibers. Non-limiting examples of polymers or blends of polymers that can be electrospun or electroblowing into nanofibers include nylon, e.g., nylon-46, nylon-66, polyurethane (PU), polybenzimidazole, polycarbonate, polyacrylonitrile, polyvinyl alcohol, polylactic acid (PLA), polyethylene-co-vinyl acetate (PEVA), PEVA / PLA, PMMA, PMMA / tetrahydroperfluorooctyl acrylate (TAN), polyethylene oxide (PEO), collagen-PEO, polystyrene (PS), polyaniline (PANI) / PEO, PANI / PS, polyvinylcarbazole, PET, polyacrylic acid-polypropylene glycol (PPE), polystyrene-polystyrene (PS ... AA-PM), polyamide (PA), silk / PEO, polyvinylphenol (PVP), polyvinyl chloride (PVC), cellulose acetate (CA), PAA-PM / PU, polyvinyl alcohol (PVA) / silica, polyacrylamide (PAAm), polylactic acid-co-glycolic acid (PLGA), polycarrolactone (PCL), polyhydroxyethyl methacrylate (HEMA), PVDF, PVDF / PMMA, polyetherimide (PEI), polyethylene glycol (PEG), poly(ferrocenyldimethylsilane) (PFDMS), nylon 6 / montmorillonite (Mt), poly(ethylene-co-vinyl alcohol), polyacrylonitrile (PAN) / TiO 2, polycaprolactone (PCL) / metal, polyvinyl pollidone, polymeta-phenylene isophthalamide, polyethylene (PE), polypropylene (PP), nylon-12, PET, polyethylene naphthalate (PEN), polyethersulfone (PES), polyvinyl butyral (PVB), PET / PEN or blends of one or more of these polymers.

[0036] Examples of electrospinning of certain polymers into nanofibers are given in Huang et al., Composites Science and Technology, 63 (2003) 2223-2253, which is incorporated herein by reference in its entirety, particularly Table 1. In certain embodiments, the nonwoven fibrous membranes provided herein comprise nanofibers comprised of a polymer selected from PMMA, PVDF, or a blend of PMMA and PVDF. In some embodiments, the nanofibers comprise a blend of PMMA and PVDF. In some embodiments, the blend of PVDF has a weight ratio of PMMA to PVDF of 1:99 to 99:1. In some embodiments, the weight ratio of PMMA to PVDF is about 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55, 50:50, 55:45, 60:40, 65:35, 70:30, 75:25, 80:20, 85:15, or 90:10. In preferred embodiments, the blend of PMMA and PVDF has a weight ratio of PMMA to PVDF of 60:40 to 70:30. In some embodiments, the weight ratio of PMMA to PVDF is about 60:40, 61:39, 62:38, 63:37, 64:36, 65:35, 66:34, 67:33, 68:32, 69:31, or 70:30.

[0037] In certain embodiments, the nonwoven fibrous membranes provided herein have a thickness of 25 microns to 250 microns, 50 to 225 microns, 75 to 200 microns, 100 to 175 microns, or 125 to 150 microns. In some embodiments, the nonwoven fibrous membranes have a thickness of about 25 microns, 30 microns, 35 microns, 40 microns, 45 microns, 50 microns, 55 microns, 60 microns, 65 microns, 70 microns, 75 microns, 80 microns, 85 microns, 90 microns, 95 microns, 100 microns, 105 microns, 110 microns, 115 microns, 120 microns, 125 microns, 130 microns, 135 microns, 140 microns, 145 microns, 150 microns, 155 microns, 160 microns, 165 microns, 170 microns, 175 microns, 180 microns, 185 microns, 190 microns, 195 microns, or 200 microns.

[0038] In certain embodiments, the nonwoven fibrous membranes provided herein have a CFT of 75 to 300 seconds, 100 to 275 seconds, 125 to 250 seconds, 150 to 225 seconds, or 175 to 200 seconds.

[0039] In some embodiments, the nonwoven fibrous membranes provided herein pass a detection bead mobility test for beads having a size of 40-600 nm, 60-580 nm, 80-560 nm, 100-540 nm, 120-520 nm, 140-500 nm, 160-480 nm, 180-460 nm, 200-440 nm, 240-420 nm, 260-400 nm, 280-380 nm, 300-360 nm, 320-340 nm, or about 400 nm.

[0040] In yet a further embodiment, the nonwoven fibrous membranes provided herein having a thickness of about 40-60 microns have a fiber density of at least about 70-120 mg / cm 2 , 80-110mg / cm 2 or 90-100mg / cm 2 It has a protein binding capacity of

[0041] In some embodiments, the nonwoven fibrous membranes provided herein exhibit desirable characteristics such as CFT of 75-300 seconds with low deviation, favorable detection bead mobility, favorable protein stripping quality, higher and tunable protein binding, high porosity, high surface area, similar area ratio, less background autofluorescence, and the potential for lower detection limits of analytes and potentially more accurate assay quantification. Other beneficial improvements exhibited by the electrospun or electroblown fibrous membranes provided herein include stable synthetic polymers that exhibit better reproducibility in manufacturing, better stability in end user applications, longer shelf life, non-hazardous materials (compared to nitrocellulose, among others) and lower capital investment in manufacturing facilities with smaller square footage requirements than air cast facilities.

[0042] Lateral flow diagnostic devices In certain aspects, provided herein is a device comprising the nonwoven fiber membrane provided herein. In some embodiments, such a device is designed to detect an analyte in a sample. In some embodiments, the device comprises an assay development area comprising the nonwoven fiber membrane described herein.

[0043] In certain embodiments, the device is a lateral flow diagnostic device. A schematic depiction of an exemplary lateral flow diagnostic device is shown in FIG. 1. A specific description of lateral flow diagnostic devices is given, for example, in Lateral Flow Immunoassay (2009), edited by Raphael Wong and Harley Tse (eds.), Humana Press, which is incorporated herein by reference in its entirety. An additional description of lateral flow diagnostic devices is given in Sajid et al., (J Saudi Chem. Soc., (2015);(19)6:689-705), which is incorporated herein by reference in its entirety, particularly Table 2.

[0044] In certain embodiments, the lateral flow diagnostic device provided herein includes a sample port designed to receive a sample, a conjugate pad, an assay development area, and an absorbent pad. The conjugate pad, the assay development area, and the absorbent pad are connected to each other in capillary flow communication. In the lateral flow diagnostic device described herein, the assay development area is made from a non-woven fibrous membrane as described herein.

[0045] In a typical lateral flow diagnostic device, the sample pad holds excess sample fluid. When the sample pad is immersed in the sample fluid, the fluid transfers to the conjugate pad, which contains conjugates of particles and a first binding agent that specifically binds to the analyte. The conjugate pad may contain a buffer / salt / sugar matrix in dry form that provides suitable conditions for binding between the analyte and the first binding agent immobilized on the particles. The sample fluid dissolves the buffer / salt / sugar matrix as well as the particles. In a combined transport activity, the mixture of sample and conjugate flows through the porous structure. During this transport, the analyte binds to the first binding agent conjugated to the particles while also migrating through the assay development area. The assay development area has a test area and, optionally, a control area, where additional molecules are immobilized. By the time the sample-conjugate mixture reaches the control and test areas, the analyte is bound to the particles and the molecules in the test and control areas bind to the particle-first binding agent-analyte or particle-first binding agent complexes. As the fluid passes through more and more of the control and test regions, particles accumulate and the regions change color. After passing through these reaction zones, the sample fluid enters a final porous material, the absorbent pad, which acts as a waste container.

[0046] In certain lateral flow diagnostic devices described herein, the conjugate pad comprises particles conjugated to a first analyte binding agent that specifically binds to an analyte. The particles conjugated to the first analyte binding agent can be colored or chromogenic particles. Non-limiting examples of colored or chromogenic particles include gold particles or latex beads. The particles conjugated to the first analyte binding agent can be magnetic particles and aggregates, fluorescent materials or luminescent materials. The particles conjugated to the first analyte binding agent can be colloidal carbon.

[0047] In the lateral flow diagnostic device described herein, the spreading area of ​​the diagnostic device is made from the nonwoven membrane provided herein. In certain devices, the spreading area includes a test area that contains a second analyte binding agent that specifically binds to the analyte in an immobilized manner. In certain devices, the spreading area further includes a control area that includes a particle binding agent that binds to the particles and is immobilized in the control area.

[0048] The lateral flow diagnostic devices described herein can be designed to detect analytes selected from metabolites, hormones, therapeutics, drugs of abuse, peptides, antibodies, and antigens. Certain examples of analytes that can be detected using the lateral flow diagnostic devices provided herein are shown in Table 2 of the Sajid et al. reference. Further examples of analytes that can be detected using the lateral flow diagnostic devices provided herein include luteinizing hormone, human chorionic gonadotropin, cholesterol, or glucose.

[0049] In some embodiments, provided herein is a method of detecting an analyte in a sample using a lateral flow diagnostic device described herein. The analyte may be a biological sample, and the sample may be a biological sample, such as a body fluid or a tissue extract.

[0050] Non-limiting examples of biological analytes include metabolites, hormones, therapeutics, drugs of abuse, peptides, antibodies, antigens, and biological samples are body fluids. Analytes listed in Table 2 of the Sajid et al. reference can be detected by the methods provided herein. Further examples of analytes that can be detected by the methods provided herein include luteinizing hormone, human chorionic gonadotropin, cholesterol, or glucose. Still further examples of analytes that can be detected according to the methods provided herein are known or readily apparent to those skilled in the art, and such embodiments are within the scope of the methods and devices provided herein.

[0051] In certain embodiments, the methods provided herein are performed on a bodily fluid selected from amniotic fluid, aqueous humor, vitreous fluid, bile, blood, cerebrospinal fluid, chyle, endolymph, perilymph, vaginal fluid, lymph, mucus (including nasal discharge and phlegm), pericardial fluid, peritoneal fluid, pleural fluid, pus, mucosal secretions, saliva, sputum, synovial fluid, vaginal secretions, semen, blood, serum, or plasma.

[0052] In other embodiments, the methods provided herein are performed on an organ or tissue extract. Non-limiting examples of organs or tissues that can be used to generate an extract include placenta, brain, eye, pineal gland, pituitary gland, thyroid gland, parathyroid gland, thorax, heart, lung, esophagus, thymus, pleura, adrenal gland, appendix, gallbladder, urinary bladder, large intestine, small intestine, kidney, liver, pancreas, spleen, stoma, ovary, uterus, testes, skin, blood or a buffy coat sample of blood. Further examples of organs and tissues from any biological source are known to those of skill in the art, and such embodiments are within the scope of the methods provided herein.

[0053] In certain embodiments, the larger diameter electrospun fibers disclosed herein produce fiber mats that have and exhibit unique properties, such as high bulk porosity, narrowly distributed large pore size ratings, high surface area, and highly tunable protein binding. In certain embodiments, the electrospun fiber mats disclosed herein may have the potential for higher sensitivity in lateral flow assays, enabling future applications that utilize these aforementioned properties. In some embodiments, the electrospun fiber mats are also flexible rather than brittle, making it easier to roll or fold the mat compared to existing air-cast nitrocellulose membranes, thereby opening the door to non-planar applications.

[0054] How to make nonwoven fiber mats In certain aspects, methods are provided herein for producing the nonwoven fibrous membranes described herein. Specifically, the methods include electrospinning (e.g., needleless electrospinning or needle electrospinning) or electroblowing of a polymer formulation onto a non-porous film or porous substrate, followed by optional transfer to a film substrate using any adhesive method to produce the nonwoven fibrous membranes provided herein.

[0055] Electrospinning is a process of producing nanofibers from a mixture of polymers, such as a polymer solution or polymer melt. The process involves the application of an electric potential to such a polymer solution or polymer melt. Certain details of the electrospinning process for making electrospun nanofiber mats or membranes, including suitable apparatus for carrying out the electrospinning process, are described in International Patent Application Publications WO2005 / 024101, WO2006 / 131081, and WO2008 / 106903, each of which is incorporated herein by reference in its entirety.

[0056] During the electrospinning process, fibers are ejected or spun from the electrode by applying a high voltage to the spinning electrode and the polymer solution, and the fibers are charged or spun toward a collecting electrode and collected as a highly porosity nonwoven mat on the substrate between the electrodes.

[0057] The two electrospinning methods are needle and needleless electrospinning. Needle electrospinning (Figure 4) is typically set up where the spinning electrode is a metal syringe, which also dispenses the polymer solution via a syringe pump. Needle electrospinning set ups are typically done on custom lab scale or smaller commercially produced machines.

[0058] Needleless electrospinning allows for higher productivity of fiber mass / hour, and the ability to operate over larger areas and on a mobile basis to collect a continuous roll stock of nonwoven fiber mat membranes. Examples of commercial needleless electrospinning equipment include ELMARCO, sro (Liberec, Czech Republic). The ELMARCO electrospinning machine functions as a dispenser for two types of polymer solutions to the spinning electrode.

[0059] In some electrospinning processes, in a rotating wire electrode machine, the polymer solution is coated onto a spinning electrode that rotates in a coating bath (FIG. 5). ELMARCO models, NSLAB200A and NS3A1000U (listed in Table 1), feature this technology and have a maximum voltage of 82 kV and widths of 20 and 100 cm. Certain other embodiments involve a fixed unwinding wire electrode(s) for spinning, where the polymer solution is capillary dispensed via a moving head. These machines have a maximum voltage of 100 kV and widths of 50 and 160 cm. This technology is available in models NS1WS500U and NS8S1600U (also listed in Table 1).

[0060] [Table 1]

[0061] In some embodiments, the nanofiber composition is made from a single nanofiber, which is made by a single pass of a moving collector located between the spinning and collecting electrodes, and a fibrous web of nanofibers can be formed by one or more spinning electrodes operating simultaneously above / below the same moving collector.

[0062] In some embodiments, the nonwoven fibrous membranes provided herein are fabricated through an electroblowing process. An exemplary electroblowing process is provided in US Patent Publication No. 2007 / 0075015, which is incorporated herein by reference. For example, in some embodiments, the fibrous mat can be fabricated through the use of a fine fiber spinning device including a spinning beam, which includes at least one spinning beam including a spinning nozzle, a blowing gas injection nozzle, and a collector, and the spinning beam and the collector have a high voltage electrostatic joint maintained therebetween. A polymer solution including a polymer and a solvent is fed to a polymer spinning nozzle, which expels the polymer solution from the spinning nozzle under pressure while blowing the solution with a blowing gas emitted from a gas injection nozzle to form a fibrous web of fibers, and the fibrous web is collected on a moving collector in one pass under a single spinning beam. In some embodiments, a thermal calendering process can be used to reduce the thickness of the resulting medium, increase the density and stiffness, and reduce the size of the pores.

[0063] The electrospun or electroblown fiber mat membranes provided herein have a different three-dimensional morphology compared to air-cast membranes, with porosity resulting from overlapping non-woven polymeric fibers having average fiber diameters in the submicron to micron range, resulting in a proportional pore size diameter rating.

[0064] The electrospun or electroblown nonwoven fiber mat membranes provided herein have certain advantages. For example, in certain embodiments, needleless electrospinning can be scaled up to continuous roll manufacturing to produce electrospun nonwoven fiber mat membranes on nonporous substrates that can be used in lateral flow diagnostic devices. The nonwoven fiber mat membranes provided herein can be efficiently electrospun or electroblown on nonporous films or porous substrates with productivity, uniformity, and adhesion to moving substrates.

[0065] Polymer solutions, such as those disclosed herein, types, grades, mix ratios, mass percentages, solvents, and viscosities, and electrospinning conditions, such as machine type, film substrate specifications, voltage, dew point, and line speed, can be used to make a continuous roll stock of electrospun nonwoven fiber mat membranes on nonporous films. Specific blends of various polymers, such as percent solids, ratios, solvents, viscosities, and different grades of polymers can be used to produce the fiber diameters required to produce nonwoven fiber mat membranes with the desired properties, such as MFP, porosity, and thickness, for use in lateral flow diagnostic devices.

[0066] The process of producing fibers via electrospinning also has several parameters that control the fiber diameter and mat properties. In addition to the electrospinning technique, other parameters can also be controlled to obtain fibers and mats with desired properties. Figure 6 shows four parameters (PMMA:PVDF ratio, % solids, dew point, and solvent composition) that control fiber diameter and morphology. The four parameters (PMMA:PVDF ratio, electrospinning parameters, dew point, and film substrate) also contribute to the productivity and uniformity of the nonwoven fiber mat. In addition, the four parameters (fiber diameter / effective pore size, PMMA:PVDF ratio, surfactant treatment, and mat thickness and uniformity) contribute to properties that are relevant for use in lateral flow diagnostic assay applications, namely, CFT, detection bead mobility, protein binding, protein stripping, and functional assay performance. Electrospinning parameters that can be controlled during electrospinning of nanofibers include voltage, airflow, electrode distance, substrate line speed, carriage speed, dispensing orifice, and wire speed of the spinning electrode.

[0067] Polymer formulations that can be electrospun or electroblowed to produce the nonwoven fiber mat membranes provided herein include polymer melts or polymer solutions. The polymer melts or polymer solutions can include one or more polymers. For example, the polymer formulations can include nylon, e.g., nylon-46, nylon-66, polyurethane (PU), polybenzimidazole, polycarbonate, polyacrylonitrile, polyvinyl alcohol, polylactic acid (PLA), polyethylene-co-vinyl acetate (PEVA), PEVA / PLA, PMMA, PMMA / tetrahydroperfluorooctyl acrylate (TAN), polyethylene oxide (PEO), collagen-PEO, polystyrene (PS), polyaniline (PANI) / PEO, PANI / PS, polyvinylcarbazole, PET, polyacrylic acid-polypyrene methanol (PAA-PM), polyamide (PAA-PM), polystyrene-co-vinyl acetate (PS ... ), silk / PEO, polyvinylphenol (PVP), polyvinyl chloride (PVC), cellulose acetate (CA), PAA-PM / PU, polyvinyl alcohol (PVA) / silica, polyacrylamide (PAAm), polylactic acid-co-glycolic acid (PLGA), polycarrolactone (PCL), polyhydroxyethyl methacrylate (HEMA), PVDF, PVDF / PMMA, polyetherimide (PEI), polyethylene glycol (PEG), poly(ferrocenyldimethylsilane) (PFDMS), nylon 6 / montmorillonite (Mt), poly(ethylene-co-vinyl alcohol), polyacrylonitrile (PAN) / TiO 2 , polycaprolactone (PCL) / metal, polyvinyl pollidone, polymeta-phenylene isophthalamide, polyethylene (PE), polypropylene (PP), nylon-12, PET, polyethylene naphthalate (PEN), polyethersulfone (PES), polyvinyl butyral (PVB), or PET / PEN.

[0068] In a preferred embodiment, the polymer preparation used in the method of producing a nonwoven fiber mat membrane provided herein comprises PMMA, PVDF or a blend of PMMA and PVDF. In some embodiments, the blend of PVDF has a weight ratio of PMMA to PVDF of 1:99 to 99:1. In some embodiments, the weight ratio of PMMA to PVDF is about 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55, 50:50, 55:45, 60:40, 65:35, 70:30, 75:25, 80:20, 85:15 or 90:10. In a preferred embodiment, the blend of PMMA and PVDF has a weight ratio of PMMA to PVDF of 60:40 to 70:30. In some embodiments, the weight ratio of PPMA to PVDF is about 60:40, 61:39, 62:38, 63:37, 64:36, 65:35, 66:34, 67:33, 68:32, 69:31, or 70:30.

[0069] The polymer preparation comprising PMMA and / or PVDF may be a solution of PVDF and / or PMMA in a solvent selected from DMAC, DMF, or a mixture thereof. In certain embodiments, the DMAC, DMF, or mixture of DMAC and DMF may further comprise acetone.

[0070] The polymer preparation comprising PMMA and / or PVDF may contain about 5% to 20% by weight of PMMA, PVDF or blends thereof. In certain embodiments, the polymer preparation comprising PVDF and / or PMMA contains about 15%, 16%, 17%, 18%, 19% or 20% by weight of PMMA, PVDF or blends thereof. In further embodiments, the polymer preparation comprising PVDF and PMMA contains about 15%, 16%, 17%, 18%, 19% or 20% by weight of a blend of PMMA and PVDF, the blend of PMMA and PVDF may have a weight ratio between PMMA and PVDF of 60:40, 65:35, 70:30, 75:25 or 80:20, and the solvent comprises DMAC and / or DMF, and optionally further comprises acetone.

[0071] In certain embodiments, the viscosity of a solution of PMMA and / or PVDF in a solvent of DMAC and / or DMF and / or acetone is between 200 centipoise (cP) and 5000 cP, between 300 cP and 2000 cP, between 400 cP and 1000 cP, between 500 cP and 900 cP, between 600 cP and 800 cP, or between 700 cP and 800 cP.

[0072] In one aspect of the methods provided herein, the non-porous film substrate onto which the polymer is electrospun is insoluble in the electrospinning solvent and has minimal or no electrical charge. These properties of the non-porous film allow for safe moving web operations and allow for well-packed and uniform fiber mats. The non-charged film allows for moving web collection and can operate at higher voltages.

[0073] According to certain embodiments, non-porous film substrates are preferred because such substrates provide a smooth non-woven fiber mat surface and do not become electrically charged in high voltage electric fields. Also, films with low electrical resistance, crystallinity, dielectric strength, and non-polar chemistry are preferred in embodiments, and the substrate moves during fiber collection. Non-limiting examples of non-porous polymeric films suitable for use in the methods provided herein include polyethylene and carbon, polyimide and carbon, low density polyethylene (LDPE) and antistatic agent, polypropylene and antistatic agent, acrylonitrile butadiene styrene and antistatic agent, nylon, static dissipative high molecular weight polyethylene (UHMWPE), polypropylene spunbond and antistatic treatment, LDPE, polycarbonate, UHMWPE, polyvinyl chloride, PET, PMMA, PVDF, and PMMA / PVDF. For use as non-porous film substrates, antistatic or static dissipative additives, or polymer composites with conductive carbon are preferred because these substrates do not charge electrically much during electrospinning, leading to better fiber mat quality (e.g., productivity and uniformity) than electrically charged films, such as PET, PVC, PC, PMMA, and PVDF.

[0074] In certain embodiments, the nanofibers are electrospun at a voltage of 30-120 kV, 40-110 kV, 50-100 kV, 60-90 kV, or 70-80 kV.

[0075] In some embodiments, the electrode distance is 150-300 mm, 160-290 mm, 170-280 mm, 180-270 mm, 190-260 mm, 200-250 mm, 210-240 mm, or 220-230 mm.

[0076] In further embodiments, the dispensing orifice is 0.4-0.8 mm, 0.45-0.75 mm, 0.5-0.6 mm, 0.55-0.65 mm or 0.6 mm.

[0077] In certain embodiments, the carriage speed is 50-150 mm / sec, 60-140 mm / sec, 70-130 mm / sec, 80-120 mm / sec, 90-110 mm / sec, or 100 mm / sec.

[0078] In certain embodiments, the wire speed is 1-5 mm / sec, 2-4 mm / sec, or 3 mm / sec.

[0079] The air in speed of the electrospinning chamber is 60m 3 / hr~120m 3 / hr, 70m 3 / hr~110m 3 / hr, 80m 3 / hr~100m 3 / hr or 90m 3 / hr, while the air out velocity of the electrospinning chamber can be 100 m 3 / hr~140m 3 / hr, 110m 3 / hr~130m 3 / hr or 120m 3 / hr.

[0080] The temperature in the spinning chamber may be 25-50°C, 30-45°C, 35-40°C, or 40-45°C.

[0081] The relative humidity in the electrospinning chamber can be 10-35%, 15-30%, or 20-25%.

[0082] In certain embodiments, the dew point in the electrospinning chamber can be 2.0°C-6.0°C, 2.2°C-5.8°C, 2.4°C-5.6°C, 2.6°C-5.4°C, 2.8°C-5.2°C, 3.0°C-5.0°C, 3.2°C-4.8°C, 3.4°C-4.6°C, 3.6°C-4.4°C, or 3.8°C-4.2°C.

[0083] In further embodiments, the line speed is from 0.5 cm / min to 5.0 cm / min, 1.0 cm / min to 4.5 cm / min, 1.5 cm / min to 4.0 cm / min, 2.0 cm / min to 3.5 cm / min or 2.5 cm / min to 3.0 cm / min for a single wire machine, and adjusted to scale linearly for more wires.

[0084] In certain embodiments provided herein, the method includes a surfactant treatment step (e.g., treatment with one or more surfactants, e.g., surfactant 1 and surfactant 2). Typically, the surfactants used in the methods provided herein contain a lipophilic non-polar hydrocarbon group and a polar functional hydrophilic group. In some embodiments, the polar functional group can be a carboxylate, ester, amine, amide, imide, hydroxyl, ether, nitrile, phosphate, sulfate, or sulfonate. The surfactants useful in the methods provided herein can be used alone or in combination. Thus, any combination of surfactants can include anionic, cationic, nonionic, zwitterionic, amphoteric, and amphoteric electrolytic surfactants. In some embodiments, the surfactant for use in the methods provided herein can be anionic, including but not limited to sulfonates, such as alkyl sulfonates, alkylbenzenesulfonates, alphaolefinsulfonates, paraffin sulfonates and alkyl ester sulfonates; sulfates, such as alkyl sulfates, alkyl alkoxy sulfates and alkyl alkoxylated sulfates; phosphates, such as monoalkyl phosphates and dialkyl phosphates; phosphonates; carboxylates, such as fatty acids, alkyl alkoxy carboxylates, sarcosinates, isethionates and taurates. Examples of carboxylates are sodium cocoyl isethionate, sodium oleoyl methyl taurate, sodium laureth carboxylate, sodium trideceth carboxylate, sodium lauryl sarcosinate, lauroyl sarcosine and cocoyl sarcosinate. Specific examples of sulfates include sodium dodecyl sulfate (SDS), sodium lauryl sulfate, sodium laureth sulfate, sodium trideceth sulfate, sodium tridecyl sulfate, sodium cocoyl sulfate and sodium lauryl monoglyceride sulfate. Examples of sulfonate surfactants include, but are not limited to, alkyl sulfonates, aryl sulfonates, mono- and dialkyl sulfosuccinates, and mono- and dialkyl sulfosuccinamates.Examples of alkyl and aryl sulfonates are sodium tridecylbenzenesulfonate (STBS) and sodium dodecylbenzenesulfonate (SDBS). Examples of sulfosuccinates are dimethicone copolyol sulfosuccinate, diamyl sulfosuccinate, dicapryl sulfosuccinate, dicyclohexyl sulfosuccinate, diheptyl sulfosuccinate, dihexyl sulfosuccinate, diisobutyl sulfosuccinate, dioctyl sulfosuccinate, C12-15 pareth sulfosuccinate, cetearyl sulfosuccinate, cocopolyglucose sulfosuccinate, cocoyl butyl gluceth-10 sulfosuccinate, deceth-5 sulfosuccinate, deceth-6 sulfosuccinate, dihydroxyethyl sulfosuccinyl undecylenate, hydrogenated cottonseed glyceride sulfosuccinate, isodecyl sulfosuccinate, isostearyl sulfosuccinate. Sulfosuccinates include, but are not limited to, succinate, laneth-5 sulfosuccinate, laureth sulfosuccinate, laureth-12 sulfosuccinate, laureth-6 sulfosuccinate, laureth-9 sulfosuccinate, lauryl sulfosuccinate, nonoxynol-10 sulfosuccinate, oleth-3 sulfosuccinate, oleyl sulfosuccinate, PEG-10 lauryl citrate sulfosuccinate, cytocereth-14 sulfosuccinate, stearyl sulfosuccinate, tallow, tridecyl sulfosuccinate, ditridecyl sulfosuccinate, bisglycol ricin sulfosuccinate, di(1,3-dimethylbutyl) sulfosuccinate and silicone copolyol sulfosuccinate.The structure of silicone copolyol sulfosuccinate is described in U.S. Patent No. 4,717,498 and 4,849,127.Examples of sulfosuccinamates are lauramide-MEA sulfosuccinate, oleamide PEG-2 sulfosuccinate, cocamide MIPA-sulfosuccinate, cocamide PEG-3 sulfosuccinate, isostearamide MEA-sulfosuccinate, isostearamide MIPA-sulfosuccinate, lauramide MEA-sulfosuccinate, lauramide PEG-2 sulfosuccinate, lauramide PEG-5 sulfosuccinate, myristamide MEA-sulfosuccinate, oleamide MEA-sulfosuccinate, oleamide PIPA-sulfosuccinate, oleamide PEG-2 sulfosuccinate, palmitamide PEG Suitable surfactants include, but are not limited to, PEG-2 sulfosuccinate, palmitoleamide PEG-2 sulfosuccinate, PEG-4 cocamide MIPA-sulfosuccinate, ricinoleamide MEA-sulfosuccinate, stearamide MEA-sulfosuccinate, stearyl sulfosuccinamate, tallamido MEA-sulfosuccinate, tallow sulfosuccinamate, tallowamide MEA-sulfosuccinate, undecylenamide MEA-sulfosuccinate, undecylenamide PEG-2 sulfosuccinate, wheat germ amide MEA-sulfosuccinate and wheat germ amide PEG-2 sulfosuccinate. Other suitable surfactants include Hotapur SAS30 and Genapol UD-070 manufactured by Clariant Corporation.

[0085] In certain methods provided herein for producing nonwoven fiber mat membranes, electrospinning of nanofibers can be performed using needle electrospinning or needleless electrospinning. EXAMPLES

[0086] Example 1 Polymer and Solvent Selection and Electrospinning Evaluation The polymers PMMA and PVDF were used to produce electrospun fiber membranes. PVDF was supplied by Arkema and has several grades, melt viscosities or molecular weights detailed in Table 2. Kynar® Flex2850 is a PVDF / polyhexafluoropropylene copolymer P(VDF / HPA). PMMA was supplied by ALTUGLAS INTERNATIONAL and has several grades, melt viscosities or molecular weights detailed in Table 3. The solvents DMAC and DMF were used for screening because they are both solvents for PMMA and PVDF and have lower vapor pressures, making them suitable for use in the ELMARCO rotating wire electrode open pan system where rapid solvent evaporation can be an issue. Screening of PMMA and PVDF grades and solvents was performed by making 15% w / v solutions in DMF and DMAC and checking the solutions for their electrospinning qualities detailed in Tables 2 and 3. Electrospinning was performed in an ELMARCO NSLAB200A unit in Table 1.

[0087] Electrospinning parameters were ΔV of 82 kV, electrode distance 280 mm, electrode rotation 60 Hz, a fixed 50 micron Melinex® PET film collected as the substrate, and spin chamber conditions of 22-25° C. temperature and 10-30% relative humidity. Table 2 shows that PVDF6 (Kynar® 761) had the highest viscosity in DMAC and DMF, and the best fiber quality resulted from DMAC.

[0088] [Table 2]

[0089] Figure 7 shows sample SEM images of high quality electrospun fibers from 15% w / v PVDF6 (Kynar® 761) in DMAC (Table 2), resulting in an average fiber diameter of 360±120 nm. Figure 8 shows that a 25% w / v solution of PVDF2 (Kynar® 711) in DMAC (Table 2) produced fibers with an average fiber diameter of 240±55 nm and undesirable beading.

[0090] Table 3 shows that 15% w / v PMMA5 (BS572) in DMAC had a lower viscosity and showed better fiber fabrication than 15% w / v in DMF. PMMA5 (BS572) produced higher viscosity and average fiber diameter than PVDF6 (Kynar® 761) at 15% w / v in DMAC. BS572 is a pure high molecular weight (HMW) PMMA. Kynar® 761 is a PVDF with a molecular weight of about 450 kilodaltons.

[0091] [Table 3]

[0092] To generate MFPs above 2 microns, larger fiber diameters are required to produce higher pore size ratings useful for lateral flow diagnostic assays. Because PMMA5 (BS572) is the best quality fiber electrospun from DMAC of the grades tested, and PVDF6 (Kynar® 761) is the best fiber quality electrospun from DMAC, blend ratios of PMMA and PVDF6 (Kynar® 761) as a 15% w / v solution in DMAC were screened for viscosity and electrospun fiber diameter, as well as quality, and are summarized in Table 4.

[0093] [Table 4]

[0094] Figure 9 shows how a 15% w / v solution of 20:80 PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC (Mix 2, Table 4) results in large diameter fibers of 600±290 nm. These data demonstrate that the higher viscosity PMMA (BS572) can be used with varying ratios of PVDF (Kynar® 761) to control the mix viscosity and the resulting electrospun fiber diameter. Thus, blends can be used to obtain a range of average fiber diameters resulting in a range of MFPs.

[0095] Example 2 Advanced Selection of Polymers & Solvents The PMMA and PVDF grades listed in Tables 2 and 3 were further investigated for viscosity versus % w / v polymer in DMAC and DMF. Figure 10 shows that for the PVDF grades (Table 2), PVDF6 (Kynar® 761) produced the highest viscosity at the lowest % w / v solution in DMAC and DMF. Figures 10 and 11 show that for Kynar® 761, DMF is a better solvent due to its lower viscosity than DMAC, and a significant difference in solution viscosity is observed with Kynar® 711. However, based on the electrospinning evaluation, DMAC was a better solvent for electrospinning Kynar® 761, producing good quality fibers, while DMF produced fibers with beads (Figures 7 and 8). PVDF2 (Kynar® 711) produced fibers with beads (Figure 8) when electrospun at 25% w / v in DMAC or DMF. FIG. 12 shows that for PMMA grades (Table 3), PMMA5 (BS572) produced higher solution viscosity at lower w / v % in DMAC and DMF than the low molecular weight PMMA1 (V920) in DMAC. The viscosity data shows that for BS572, DMAC is a better solvent than DMF since it produces a lower viscosity at the same % w / v as DMF. PMMA5 (BS572) is also a higher quality fiber electrospun from DMAC, even at higher w / v %, better than PMMA1 (V920). Since the best solvent for PMMA and PVDF for electrospinning was DMAC, mixed viscosities at various ratios of PMMA and PVDF were evaluated for high and low MW / PMMA and PVDF viscosities. Figure 13 shows the blend viscosity of 15% w / v solutions versus blend ratios of higher MW PMMA5 (BS572) and PVDF6 (Kynar® 761) versus lower MW PMMA1 (V920) and PVDF2 (Kynar® 711), confirming that PMMA5 (BS572) and PVDF6 (Kynar® 761) produced the highest viscosity at the lowest % w / v and were the grades selected to electrospin the largest diameter fibers.FIG. 14 shows the mixed viscosity of 15% w / v solutions versus the mixing ratio of PMMA5 (BS572) and PVDF6 (Kynar® 761) in DMAC with solution conductivity (μS / cm) on the secondary y-axis. This illustrates the higher solution conductivity with PVDF6 (Kynar® 761). FIG. 15 shows the viscosity of solutions of increasing w / v % with PVDF6 (Kynar® 761) and PMMA [PMMA1 (V920), PMMA5 (BS572) and PMMA4 (PRD521)] in DMAC at a ratio of 75:25 (PVDF6:PMMA) verifying that PMMA5 (BS572) had the greatest impact on viscosity at lower w / v %. FIG. 16 shows the viscosity of solutions of increasing w / v % of PVDF2 (Kynar® 711) with PMMA [PMMA1 (V920), PMMA5 (BS572) and PMMA4 (PRD521)] as viscosity modifiers in a ratio of 75:25 (PVDF2:PMMA) verifying that PVDF6 was the choice for high viscosity and that PMMA5 (BS572) had the greatest impact on viscosity at lower w / v %. The solution viscosities above confirmed that PMMA5 (BS572) and PVDF6 (Kynar® 761) produced the highest viscosity at the lowest % w / v to electrospin fibers with the largest diameter and best quality.

[0096] Example 3 PMMA5 (BS572) and PVDF6 (Kynar® 761) Polymers in DMAC Further investigation of the viscosity and electrospun fibers was performed once PMMA5 (BS572) and PVDF6 (Kynar® 761) were proven to be available polymer grades that would produce fiber diameters with resulting MFPs for use in lateral flow diagnostic applications. Electrospinning was performed on an ELMARCO NS1WS500U unit as shown in Table 1, with fibers collected on 50 μm Melinex PET or running on a 40 cm wide 100 μm LDPE moving web. Typical electrospinning parameters were ΔV of 60-100 kV, electrode distance of 240 mm, dispensing orifice of 0.6 mm, carriage speed of 100 mm / sec, wire speed of 1-3 mm / sec, and 80 m.3 Air in / hr, 120m 3 Air out at 100 / hr and spin chamber conditions of 30-40°C and 10-30% relative humidity controlled by use of a dehumidifier. The use of a fixed wire machine with a dispensing head allows for electrospinning of higher w / v% solutions and higher viscosities with an upper viscosity limit of approximately 4,000 centipoise (cP). 15-18% solutions of increasing w / v% PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC were made at mixing ratios of 100:0, 75:25, 50:50, 25:75 and 0:100 and electrospun under the aforementioned conditions to determine the resulting average fiber diameter, as plotted in Figure 17. The data demonstrate that higher average fiber diameter is directly proportional to higher % w / v concentration and higher ratio of PMMA5 (BS572) to PVDF6 (Kynar® 761). Thus, the fiber diameter and resulting pore size rating can be adjusted depending on the polymer concentration and PMMA:PVDF ratio. Figure 18 shows that increasing the PMMA5 (BS572) to PVDF6 (Kynar® 761) ratio and increasing the concentration from 15 to 20% w / v resulted in higher viscosity. Figure 19 shows that the trend of increasing viscosity in Figure 18 also increases the resulting average fiber diameter produced by electrospinning.

[0097] Example 4 Evaluation of non-porous film substrate Typical air-cast nitrocellulose membranes are brittle and therefore cast onto non-porous films, such as Melinex® PET (DuPont Teijin Films Luxembourg SA), to provide integrity and ease of use during assembly of lateral flow diagnostic devices. Electrospun fibers were typically collected on non-woven or porous substrates that passed a voltage between the spinning and collecting electrodes and provided pores to allow the volatilized solvent to pass through. Electrospinning on non-porous substrates or films poses challenges in generating sufficient fiber mat thickness, forming a uniform coating, and causing incomplete solvent evaporation or drying the fiber mat. When attempting to electrospin a 17% w / v solution of PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC, with a viscosity of about 1500 cP, onto fixed Melinex® PET, the film becomes highly charged and the electrospun non-woven fiber mat becomes non-uniform (Figure 20). Also, the maximum thickness of the fiber mat and the quality of fiber packing are limited (Figure 21). Figure 20 shows the central area on the Melinex® PET in series with the electrodes that is not significantly covered by the fibers. Figure 20 also shows how the fibers coat the film with a pattern of electric field that tends to spread around the periphery of the film. Figure 21 shows an SEM cross-sectional image of electrospun fibers of an under-packed fiber mat on a Melinex® PET film, which is believed to be the result of the film being charged. Electrospinning was performed on an ELMARCO NS1WS500U unit in Table 1, and fibers were collected on 50 μm Melinex PET. Typical electrospinning parameters were ΔV of 100 kV, electrode distance of 240 mm, dispensing orifice of 0.6 mm, carriage speed of 100 mm / sec, wire speed of 1-3 mm / sec, spin chamber conditions of 30-40° C., and relative humidity of 10-30% controlled by the use of a dehumidifier.

[0098] Typically, the polymer film is conductive (10 1 ~10 4 ) to static dissipative (10 6 ~1012 ), antistatic (10 10 ~10 12 ), Insulation (>10 12 ) surface electrical resistivity in ohms / sq. Volume resistivity is given by sheet resistance times thickness in ohms cm. Resistivity can be measured using test method ANSI / ESD STM 11.11.

[0099] In certain embodiments, the methods provided herein include electrospinning on non-porous substrates, such as polymer films, which pose challenges of electrical resistivity, polymer chemistry, crystallinity, and solubility inherent to the polymer film. The polymer film must be insoluble in solvent electrospinning and have minimal to no charge to allow safe moving web operation and a well-packed, uniform fiber mat. Uncharged films allow for moving web collection as well as the ability to operate at higher voltages. Table 5 details the non-porous films screened for the aforementioned electrospinning conditions. The list is in order of increasing electrical resistance, with Melinex® 401 PET having the higher resistance and performing less well as an electrospun substrate (Figures 20 and 21).

[0100] [Table 5] TIFF0007554806000006.tif79162

[0101] Non-porous films with low crystallinity, low dielectric strength and non-polar chemistry, electrical resistance in the static dissipative to antistatic range are preferred substrates for electrospinning on fiber mats. Certain preferred substrates are polymeric films of LDPE, nylon, UHMWPE, or polymer composites with antistatic or static dissipative or conductive carbon. Non-porous film substrates that were poor for electrospinning exhibited high charging and included PET, PVC and PC polymers. Polymers PMMA and PVDF exhibited moderate charging under typical electrospinning conditions. Figure 22 shows a selection of films with increased bulk resistivity from Table 5, as well as the maximum thickness of a fiber mat with a 40 cm film width, produced under the same electrospinning conditions as described above, and for the same spinning time of 10 minutes. Figure 22 also shows that films 5, 5b-8b and 12 from Table 5, electrospun under the same conditions, were electrospun at approximately 10 minutes in Figure 22. 7 ~10 12 The results show that thicker mats produced films with lower or higher resistivity of Ωcm. The spinning conditions in FIG. 22 were 17% PMMA:PVDF (70:30) in DMAC, 100 kV, 240 cm distance, 2 cm / min line speed, 42° C., and 4° C. dew point, all of which produced fiber diameters of about 900 nm. Table 5 and FIG. 22 show that the bulk electrical resistivity was about 10 8 ~10 12 The Ωcm region shows the maximum productivity in terms of thickness of the nonwoven fiber mat and no film charging is observed. This finding provides a good understanding of moving web collection, fiber mat uniformity, thickness productivity, and fiber packing quality. Asymmetric currents were observed at the spinning and collecting electrodes when the substrate was excessively conductive.

[0102] Switching to LDPE (#12 in Table 5) as the non-porous substrate allows for a more uniform mat with LDPE anchoring (Figure 23) compared to Melinex® PET in Figure 20. LDPE film also allows for higher productivity of approx. 90 μm fiber mat thickness and improved fiber packing quality (Figure 24) compared to Melinex® PET in Figure 21 under identical electrospinning conditions. Similar results in terms of no film charging, productivity, improved uniformity and fiber packing occurred for film IDs #5-12 and 5b-8b in Table 5. Figure 25 shows electrospun nonwoven fiber mat coated on LDPE film using a moving web at a line speed of 2 cm / min outside an ELMARCO NS1WS500U unit in Table 1. Figures 26.1 and 26.2 show SEM images of the air and LDPE sides where similar fiber quality and diameters are observed, indicating that the resulting membrane is symmetrical in terms of pore rating on both sides.

[0103] The non-porous substrate used for fiber collection can also function as a permanent support if the fibers have high adhesion to the film surface through surface treatment methods such as corona, plasma, etching or roughening, or due to the film chemistry or solvent bonding to the substrate. For example, film #18 from Table 5 can be used, or a thin layer of 5 μm polymer that is partially soluble in the electrospinning solvent can be used for solvent bonding of the fibers to the film substrate. Alternatively, the electrospun non-woven fiber mat membrane can be removed and the membrane can be electrospun onto a film that can potentially be used as an unbacked membrane. It can also be transferred to an alternative film. As a result, this transfer option allows for the selection of the substrate film (for optical requirements, thickness, etc.) and adhesion can be achieved through, for example, lamination, adhesives and solvent bonding. Non-woven fiber mats made using electroblowing can be collected on a porous substrate, as described above for electrospinning, and then used for the assay without a backing or after transfer to a substrate film.

[0104] Example 5. Effect of Relative Humidity / Dew Point on Electrospun Fiber Diameter The diameter of the fibers produced by electrospinning is sensitive to the relative humidity or dew point in the electrospinning chamber. The higher the relative humidity or dew point, the larger the average fiber diameter for the same polymer solution in terms of w / v % and PMMA:PVDF ratio when electrospun under the same electrospinning parameters. To demonstrate this effect, experiments with a moving web were performed to show the effect of relative humidity or dew point on the average fiber diameter. The moving web experiments were performed with LDPE under the aforementioned electrospinning parameters, at a line speed of 5 cm / min, a starting temperature of 22° C., and a relative humidity of about 50%. To determine the effect of relative humidity inside the spin chamber, a dehumidifier was plumbed into the inlet of the spin chamber, turned on, and the dew point was tracked against line speed and position. Solutions of 17% w / v PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC with ratios of 75:25, 60:40 and 50:50 were electrospun and collected on a moving web with decreasing humidity to determine the effect of dew point on the average fiber diameter. The average fiber diameter was measured at various dew points calculated using SEM, showing that higher dew points produced larger average fiber diameters. Figure 27 shows images of fiber mats produced from a 60:40 PMMA:PVDF ratio as humidity decreases from left to right. Figures 28.1, 28.2 and 28.3 show SEM images of fiber quality and diameter produced at approximate dew points of 11.8°C, 3.2°C and 2.6°C. Figure 28.1 at 11.8°C shows that drying at too high a dew point fails to produce well-formed fibers, while Figures 28.2 and 28.3 show well-formed fibers with decreasing diameter with dew point. Figure 29 is a plot of the average fiber diameter obtained by electrospinning a 17% w / v solution of PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC at ratios of 75:25, 60:40, and 50:50 versus decreasing dew point, and collecting on a moving web at decreasing humidity. Figure 30 is a plot of the electrospun average fiber diameter of various w / v % solutions and PMMA5 (BS572):PVDF6 (Kynar® 761) ratios at two different relative humidities produced by the same electrospinning parameters.

[0105] 29 and 30 demonstrate that the average fiber diameter is a function of w / v %, PMMA:PVDF ratio and relative humidity or dew point, which means that the resulting MFP of the electrospun nonwoven fiber mat can be controlled through these three factors.

[0106] Example 6 Line Speed, Productivity and Mat Thickness Uniformity Electrospun nonwoven fiber mat membranes, collected on non-porous substrates, must also be productive in terms of mat thickness versus line speed and thickness uniformity to function as membranes in lateral flow diagnostic assays. As shown in Figure 6, factors that contribute to the productivities and uniformity of mat membranes are polymer solution (%, ratio), electrospinning parameters, dew point, and film substrate.

[0107] Electrospinning was performed on an ELMARCO NS1WS500U unit in Table 1, collecting fibers on a moving web of 40 cm wide 100 μm thick LDPE film (#12 in Table 5). Typical electrospinning parameters were ΔV of 60-100 kV, electrode distance of 240 mm, dispensing orifice of 0.6 mm, carriage speed of 100 mm / sec, wire speed of 1-3 mm / sec, and 80 m. 3 Air in / hr, 120m 3 / hr and spin chamber conditions were 30-40°C and 10-30% relative humidity controlled by a dehumidifier. Table 6 details a series of experiments in which the same solution (PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC at a ratio of 75:25, 17% w / v) was electrospun at different potential differences (ΔV) and at the same line speed, or at a fixed ΔV and line speeds of different substrates. Samples 072016-1 to -4 were electrospun at 60 kV and line speeds of 0.5, 1.0, 2.5 and 5.0 cm / min. Samples 072016-4 to -6 were electrospun at 5.0 cm / min and voltages of 60, 80 and 100 kV. The average thickness of the electrospun nonwoven fiber mat was measured and reported in microns (μm) by taking five micrometer measurements over a 1×4 cm sample area and subtracting the film thickness. 2 The unit weight is calculated by measuring the mass of a 1 x 4 cm strip, subtracting the mass of the film, and then multiplying it by 4 x 10 -4 m 2 The net average thickness of the electrospun fiber mat was determined by dividing by the area of ​​the fiber. FIG. 31 shows the linearity of the net average thickness of the electrospun fiber mat versus basis weight for several conditions of voltage and line speed in Table 6. Slower line speeds produced thicker mats and higher basis weights. 60 kV at reduced line speeds produced similar fiber loading slopes as fixed line speeds and increased voltages. 100 kV produced higher fiber loading than 60 kV at slower line speeds.

[0108] [Table 6]

[0109] Figure 32 is an image of the cross and down web sampling areas (60 x 40 cm) and locations used to measure thickness productivity and uniformity. Figure 33.1 is a plot of the solution and mat net average thickness and basis weight at a constant voltage of 60 kV vs 1 / line speed electrospinning experiment detailed in Table 6 collected on a moving web of 100 μm thick LDPE film (#12 in Table 5). Both the mat net average thickness and basis weight show that productivity peaks at 60 kV and a line speed of 1.0 cm / min. Figure 33.2 is a plot of the mat net average thickness from the aforementioned experiment at a constant voltage of 60 kV vs 1 / line speed collected on a moving web of 100 μm thick LDPE film (#12 in Table 5) overlaid on a mat electrospun under identical conditions except at 100 kV on a moving web of Permastat LDPE PE700AS film (#7b in Table 5). Figure 33.2 shows that at higher voltage and faster or same line speed, higher productivity or thickness can be achieved on a less resistive film (#7b vs #12 in Table 5). Figure 34 is a plot of sample thickness and uniformity vs position detailed in Figure 32 for electrospinning experiments with solutions and constant line speed vs voltage detailed in Table 6. As voltage increased, the fiber mat thickness increased and the uniformity increased to about 40 microns of mat thickness for similar cross and down web. Figure 35 is a plot of sample mat thickness and uniformity vs position detailed in Figure 32 for solutions in Table 6 at 100 kV for line speed. In this case, faster line speed or thinner mat thickness favors better cross and down web uniformity, but slower speeds allowed thicker mat collection. Figures 36.1-36.3 show SEM cross-sectional images of the samples from Figure 35, and good correlation was observed between the micrometer measured mat thickness and the observed thickness in the SEM cross-sectional images. Productivity can also be improved through the use of a machine with more spinning and collecting electrodes, such as the ELMARCO NS8S1600U shown in Table 1, in terms of mat thickness or line speed.

[0110] Example 7 Acetone as a co-solvent Table 7 details the formulation of low w / v % PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC with acetone added as a co-solvent, resulting in lower viscosity that can be used to electrospin larger diameter fibers at lower voltages of 30 kV. The use of higher vapor pressure co-solvents results in lower solution viscosity, which allows faster solvent evaporation during electrospinning, allowing for the production of larger diameter fibers, and also aids in the evaporation of the lower vapor pressure DMAC solvent, resulting in the ability to electrospin quality fibers at higher relative humidity. Figure 37 shows an SEM image of a 733±263 nm fiber sample electrospun at 30 kV from 14% w / v PMMA5 (BS572):PVDF6 (Kynar® 761) in 90:10 DMAC:acetone at 35° C. and 45% relative humidity.

[0111] [Table 7]

[0112] Example 8. Properties of electrospun nonwoven fibrous mat membranes The electrospun nonwoven fiber mat membranes provided herein have structurally different three-dimensional morphologies compared to air-cast membranes (Figure 24, compare to Figure 3.2). In the electrospun fiber mat membranes provided herein, porosity comes from overlapping nonwoven fabrics of polymer fibers with average fiber diameters in the submicron to micron range, which proportionally results in a diameter rating of pore size. Conventional lateral flow diagnostic membranes are typically constructed of nitrocellulose and are brittle. Also, because conventional lateral flow diagnostic membranes are air-cast on non-porous substrates, characterizing them is challenging with conventional membrane techniques, e.g., porometry. Typically, electrospinning produces nanofibers with average fiber diameters less than 500 nm. Electrospun nonwoven fiber mat membranes with average fiber diameters of about 500-1000 nm are provided herein, which results in a resulting MFP greater than 2 microns and a porosity greater than 85%. These parameters allow the nonwoven fiber mat membrane to be made thick enough to have desirable and useful properties for lateral flow diagnostic assays. Other techniques that produce similar fiber diameters and mats, such as solvent blowing or electric blowing, can be used to form similar lateral flow diagnostic membranes.

[0113] Some of the advantages of electrospun nonwoven fiber mats over air-cast nitrocellulose can be explained by the inherent physical properties of the membranes. Examples of comparable membrane characteristics are average fiber diameter, MFP, porosity, thickness, uniformity, shrinkage when wet and dry, mechanical strength, adhesion to substrates or ability to be transferred unbacked to a film support, CFT, surface area, ratio of internal surface area to frontal area of ​​the polymer, and properties of the base polymer.

[0114] Example 9 Porometry Capillary flow porometry, also known as porometry, is a technique based on the displacement of a wetting liquid from a sample pore by application of a gas at increasing pressure. It can be measured in normal flow direction, perpendicular to the membrane surface for unbacked membranes. Using a commercially available capillary flow porometer (Model CFP-1200AEX, Porous Materials, Inc. Ithaca, NY), a 25 mm disk of membrane and a Galwick fluid with a surface tension of 15.9 dynes / cm, flow rate versus pressure curves were measured to obtain the mean and maximum flow pore diameters. Figures 38.1 and 38.2 show plots of pore size distribution versus mean diameter for air-cast nitrocellulose and electrospun nonwoven fibrous mats. Both air-cast nitrocellulose and electrospun nonwoven fibrous mats have CFTs of 135-180 seconds, and mean and maximum flow pore diameters of approximately 3 and 3.6 microns, respectively. Figure 39 shows a plot of CFT versus MFP as measured by porometry, with positive error bars extending to the maximum flow pore diameter. Thus, membranes of two different structures with similar CFT have similar capillary flow porometry profiles.

[0115] Figure 40 is a plot of CFT vs. average fiber diameter for the same electrospun nonwoven fiber mat samples in Figure 39. Figure 41 is a plot of MFP diameter vs. average fiber diameter for electrospun fiber mats having CFTs of about 135 to 160 seconds.

[0116] Example 10 Delamination, Brittleness and Wet-Dry Shrinkage Air cast nitrocellulose membranes are inherently brittle and can delaminate from the film substrate on which they are cast. Therefore, membranes are tested for delamination and brittleness prior to quality control release. Delamination is tested using a 25 x 2.5 cm test strip membrane by folding and rolling between fingers over a 25 cm direction to observe if the membrane peels from the substrate. Brittleness is tested by folding at 45 degrees along the long axis and checking if cracks are observed. Figure 42 shows images of four test strips tested for delamination and brittleness. The samples, from left to right, show that both an air cast nitrocellulose membrane (Hi-Flow™ Plus 135) and an electrospun nonwoven fiber mat membrane collected on the corona treated side of an LDPE film (delaminated, brittle and as-spun) pass the delamination and brittleness tests. Figures 43.1 and 43.2 show images of delamination and shrinkage testing of electrospun fiber mats with an average fiber diameter of about 700 nm on LDPE film after IPA / water wetting, surfactant treatment and air drying. Figure 43.1 shows duplicate electrospun membranes with an average fiber diameter of about 700 nm spun on the corona treated side of LDPE that do not delaminate or shrink detectably after IPA / water wetting, surfactant treatment and air drying. Figure 43.2 shows rectangular cut samples of triplicate electrospun membranes on the non-corona treated side of LDPE film that exhibit only delamination and minimal shrinkage after IPA / water wetting, surfactant treatment and air drying. These experiments show that unlike air cast nitrocellulose membranes, the electrospun fibers provided herein with an average fiber diameter of about 700 nm adhere well to corona treated LDPE, exhibit minimal wet-dry shrinkage and are not brittle.

[0117] Example 11 Adhesion Due to the risks associated with adhesion, alternative methods were evaluated for adhesion of electrospun nonwoven fiber mats to nonporous substrates. Direct electrospinning onto films with adhesive layers was investigated as a promising one-step option to obtain good adhesion onto smooth nonporous films. To demonstrate the viability of this option, electrospun fibers were spun directly onto a 25 micron conductive polyimide film (Kapton® XC from DuPont USA) on a pressure sensitive acrylic adhesive side and on an adhesive-free side. Figure 44.1 is a SEM cross-sectional image showing electrospun fibers well bonded to the acrylic adhesive layer on the Kapton® film. Figures 45.1 and 45.2 show images of how the fiber mat remains well bonded to the acrylic adhesive side even after IPA / water wetting, surfactant treatment, and air drying, even as the fiber mat delaminates from the nonadhesive side. This provides a novel demonstration of electrospinning onto nonporous film substrates with a bonding adhesive. This technique can be used with alternative adhesive chemistries, custom film adhesive combinations, and the use of the commercially available acrylic adhesive GL-187® from Lohmann Corporation (Orange, VA), which is FDA approved and widely used and well accepted in the lateral flow diagnostic industry. Figures 44.2 and 44.3 are images and SEM cross-sectional images of electrospun nonwoven fiber mats spun directly onto GL-187® adhesive from Lohmann Corporation (Orange, VA), coated onto Permastat LDPE PE700AS film (#7b in Table 5). Customized adhesive thicknesses can also be used along with film and fiber mat thicknesses to match the target thicknesses of 185 and 235 microns most commonly targeted for lateral flow diagnostic assays. Alternative methods of adhering fiber mats onto films include corona or plasma treatment, surface etching or roughening, and even bilayer film combinations where the solvent can be spun onto a thin layer of polymer that is soluble when electrospun to allow vapor solvent bonding of the fibers to the substrate.Alternatively, the electrospun fibers can be spun unadhesively onto a film and the fibers can be laminated to the film with an adhesive, or the top air side can be inverted and transferred film side up. Figures 44.4 and 44.5 are images and SEM cross-sectional images of an electrospun nonwoven fiber mat spun onto the non-adhesive, non-corona treated side of a Permastat LDPE PE700AS film (#7b in Table 5) and from there transferred onto GL-187® adhesive from Lohmann Corporation (Orange, VA) coated onto a Permastat LDPE PE700AS film (#7b in Table 5).

[0118] Example 12. Characterization of electrospun fibers by SEM Electrospun fibers were imaged and the average fiber diameter was measured by SEM. Samples were prepared by coating with gold or iridium using a Cressington 208HR high resolution sputter coater. Cross sections were prepared by freeze-fracturing by immersion in liquid nitrogen and fracturing prior to sputter coating. Typical magnifications were 500-10000x using an FEI Quanta200F field emission scanning electron microscope at 3 / 5 kV. Samples at lower magnifications were imaged using a JEOL JCM-6000PLUS Benchtop SEM. The average fiber diameter and standard deviation were calculated from 10 random fiber measurements.

[0119] Example 13 Lateral Flow Diagnostic Applications (See Hi-Flow™ Plus Brochure and Document TB500EN00EM) The novel formulation and electrospinning process produces electrospun fiber mat membranes with average fiber diameters greater than 500 nm, MFP ratings greater than 2 microns, and high porosity greater than 85%. The electrospun membranes have properties comparable to, and several advantages over, commercially available air-cast nitrocellulose membranes currently used in lateral flow diagnostic assays. The electrospun nonwoven fiber mat membranes have similar or even improved stability in terms of CFT, detection bead mobility, and protein stripping quality. Advantages of the electrospun fiber mat membranes provided herein include highly reproducible fiber diameters with narrow MFP, high porosity, high surface area, higher and more tunable protein binding, less background autofluorescence, potentially lowering the detection limit of analytes, and more accurate assay quantification. Another beneficial improvement of the electrospun fiber mat membranes provided herein is the use of stable synthetic polymers that exhibit improved manufacturing reproducibility, stability in end user applications, longer shelf life, non-hazardous properties (compared to nitrocellulose), and further reduced capital investment in manufacturing facilities due to smaller square footage requirements than aircast facilities.

[0120] Example 14 Surfactant treatment and CFT Air-cast nitrocellulose is inherently hydrophobic and therefore requires treatment with a surfactant to allow wetting and aqueous capillary flow. Surfactants are commonly used to pretreat nitrocellulose membranes in lateral flow diagnostic applications. A typical treatment involves applying a dilute solution of aqueous surfactant at the end of the casting process, followed by drying to leave a coating of surfactant on the membrane to prepare for spontaneous aqueous rewetting during use. Treatment of PMMA:PVDF fiber mats can be done by wetting with 70:30 IPA:water for 2 min, soaking in the surfactant solution for 10 min with agitation, and air drying overnight at ambient temperature and relative humidity.

[0121] Example 15 CFT The CFT is an industry standardized test in which a 1x4 cm test strip is placed in a well of 150 μL of water and the CFT is measured as the time it takes for a uniform liquid front to rise a total length of 4 cm. The test water should be at 21±1°C and the relative humidity of the room should be 50±5% (MilliporeSigma test method 000764™). Typically, a useful CFT for lateral flow diagnostic assays is 75-180 seconds. In general, a faster CFT results in a lower signal strength, while a slower CFT results in a stronger signal, all other conditions remaining constant.

[0122] Example 16 Latex detection bead mobility Functional lateral flow diagnostic assays use colored detection particles to generate a signal line. One class of particles used is 400 nm diameter latex beads. Therefore, membranes used in lateral flow assays must allow these beads to pass freely through their pore structure without any separation of the bead front from the liquid front. Hi-Flow™ Plus air-cast nitrocellulose membranes have passed such tests using a test solution of 0.05% carboxylate modified 400 nm latex beads (Duke Scientific, DB1040C), 0.1% Tween surfactant in 1 mg / mL BSA in PBS buffer. Tests are performed on 1×4 cm test membranes using 25 μL of solution. Liquid is allowed to flow over the top and can only be passed with a clear liquid flow front and no visible separation of the colored line of detection beads. Gold nanoparticles of about 40 nm can also be used, but this test is not a quality control test since if the membrane can pass 400 nm latex beads, it will pass 40 nm gold particles. Figure 46 is an image of the custom test stand used to measure CFT and latex detection bead mobility. Figures 47.1 and 47.2 show images of the membrane at the end of the latex detection bead mobility test. Figure 47.1 shows a duplicate electrospun nonwoven fiber mat membrane with an average fiber diameter of 632±212 nm and a CFT of about 200 seconds, which passes the bead mobility test, as well as the Hi-Flow™ Plus 135 nitrocellulose control membrane. Figure 47.2 is an image of a duplicate electrospun membrane with an average fiber diameter of 432±95 nm and a CFT of about 300 seconds, which fails the bead mobility test with visible defects of the beads migrating the entire length of 4 cm. Figures 48.1 and 48.2 are SEM cross-sectional images of an electrospun fiber mat and beads passing through Hi-Flow™ Plus 135, showing the 400 nm beads present in the cross-section, demonstrating the presence of a minimum average fiber diameter and corresponding MFP, as well as the porosity required for the passage of 400 nm latex beads.

[0123] Example 17 CFT vs. Average Fiber Diameter for Latex Bead Mobility Observations FIG. 49 is a plot of several electrospun nonwoven fiber mats at similar net thickness of the mats and their corresponding CFT against average fiber diameter. The data demonstrates that the larger the average fiber diameter, the larger the MFP, which results in faster CFT or capillary flow. The same membrane was tested for latex bead mobility (FIGS. 47.1 and 47.2) to observe the minimum average fiber diameter required to freely pass 400 nm latex detection beads and its corresponding MFP or resulting porosity. FIG. 50 shows that the CFT is a function of average fiber diameter. In this example, a 17% w / v solution of PMMA5 (BS572):PVDF6 (Kynar® 761) in DMAC with a ratio of 75:25 was electrospun onto a moving web of LDPE, and the variable average fiber diameters were due to uncontrolled dew point (higher dew point results in higher fiber diameters).

[0124] FIG. 51 shows a plot of CFT versus average net fiber mat thickness for electrospun nonwoven fiber mats, all of which have an average fiber diameter of about 700 nm. All samples were electrospun under very similar dew points, resulting in similar fiber diameters. Mat thickness was controlled by spinning time, line speed, and voltage. CFT was measured at room temperature and 30-40% relative humidity. The slower CFT observed on thinner mats may be an effect of increased evaporation rates due to higher surface area and porosity.

[0125] Example 18 CFT vs Mat Thickness and Relative Humidity Since CFT is dependent on relative humidity, the CFT of various fiber mat thicknesses with the same average fiber diameter of about 700 nm was measured under equilibrated and carefully controlled relative humidity in a controlled humidity cabinet. Samples were equilibrated overnight at 30° C. and 10, 50, 75, and 90% relative humidity. Figure 52.1 shows plots of CFT vs. relative humidity for membranes with different net average thicknesses, including Hi-Flow™ Plus 135 net thickness 135 μm. The thinner the mat, the slower the CFT will be at lower relative humidity due to competition between capillary flow and evaporation. The data shows the sensitivity of CFT to humidity for the 135 μm thick Hi-Flow™ Plus 135 membrane. CFT release specifications and tolerances are based on testing at 21±1° C. and 50±5% relative humidity. Figure 52.2 shows plots of CFT vs. membrane mat thickness at different relative humidity, showing the sensitivity of CFT to mat thickness and humidity. The greater the thickness, closer to the net thickness of 135 μm for Hi-Flow™ Plus 135, the less sensitive the CFT is to the measured relative humidity (Figure 52.1).

[0126] Example 19 Porosity, Surface Area and Surface Area Ratio Further properties that contribute to the membrane's application for lateral flow diagnostics include porosity, surface area, and surface area ratio. The porosity percentage is calculated according to the following equation: Porosity % = [1-(basis weight / (mat thickness x polymer density))] In the formula, the units of basis weight, polymer density and mat thickness are (g / m 2 ), (g / m 3 ) and m.

[0127] m 2 The internal surface area in units of 1 / gram is determined as the BET surface area using krypton gas by Micromeritics (Norcross, GA). Surface area ratio is the ratio of internal surface area to frontal surface area and is a metric used in assay development to optimize reagent concentrations and assay conditions. Hi-Flow™ Plus membranes typically have a surface area ratio of about 100. Surface area ratios are defined as follows: Surface area ratio = BET surface area (m 2 / g)×Weight (g / m 2 ) It is calculated as follows:

[0128] Table 8 details a selection of electrospun nonwoven fiber mat membranes and Hi-Flow™ Plus 135 membranes, including data on average fiber diameter, net average thickness, basis weight, % porosity, BET surface area (SA), surface area ratio, protein binding and CFT. Protein binding is expressed as μg / cm2 per unit area with respect to the thickness of the membrane. 2 Normalizing protein binding by μg / cm 3 Calculated in units. The electrospun sample is relatively close to Hi-Flow™ Plus 135, but is thinner and therefore bendable. The fiber has a lower mat thickness / basis weight / area ratio and protein binding, but a higher percent porosity and BET SA. Figure 53 is a plot of mat thickness versus basis weight for electrospun fibers and Hi-Flow™ Plus 135 membrane. It is assumed that basis weight will be lower for fibers at similar thickness due to higher porosity and different polymer densities. However, performance in lateral flow assays depends on understanding the membrane properties. Fibers at similar thickness to air cast nitrocellulose have lower basis weight, higher porosity, higher surface area, and higher protein binding.

[0129] [Table 8]

[0130] Example 20. Effect of surfactant treatment concentration and type on CFT The effect of surfactant concentration on the CFT in the hydrophilic treatment of electrospun fiber mats was investigated using two types of surfactants, surfactant 1 and surfactant 2. Electrospun fiber mats (composed of PMMA5 (BS572):PVDF6 (Kynar® 761), ratio 75:25) of various thicknesses and average fiber diameter of about 700 nm were treated with surfactant 1 or surfactant 2 ranging from 0.02 to 0.1% w / w in water. CFT was measured for all samples at room temperature and constant relative humidity. Figure 54.1 is a plot of CFT against treatment concentration of surfactant 1 for fiber mats with various thicknesses. Figure 54.2 shows a similar plot of CFT after treatment with surfactant of surfactant 2. Both experiments demonstrate that CFT is a function of the surfactant used to hydrophilize the film and that CFT can vary slightly depending on the surfactant concentration used (higher % results in shorter CFT). Figures 54.1 and 54.2 also show that the effect of evaporation on thinner mats makes the CFT longer, resulting in shorter CFTs for thicker mats. Figure 55 is a plot of CFT versus thickness for fiber mats treated with 0.1% Surfactant 1 and Surfactant 2. Thus, surfactant 2 causes the CFT to be shorter, and the CFT on thinner mats is also longer due to competition between evaporation and capillary flow.

[0131] Example 21 Protein Binding Protein binding is an important characteristic of membranes used in lateral flow diagnostic assays. Quantitation of membrane protein binding was measured and reported in μg / cm 2 For reference, Hi-Flow™ Plus 135 nitrocellulose typically has a density of about 150 μg / cm 2 The membrane protein binding has a value of 0.1 μCi / mL. 125 It is determined using goat IgG spiked with I-(goat IgG) at a concentration of 1 mg / mL. Membrane disks were wetted thoroughly, incubated with radiolabeled goat IgG in PBS buffer for 2 hours, rinsed, and assayed for bound radioactivity and the IgG / cm of membrane was determined.2 was converted to micrograms. Figures 56.1 and 56.2 show the units in μg / cm 2 The IgG protein binding per unit is shown to depend on mat thickness and surfactant treatment. For both surfactants, protein binding decreases with higher wt% surfactant treatment. Figure 57 plots IgG binding versus net average thickness of fiber mats of about 700 nm PMMA:PVDF (75:25) fibers treated with various wt% Surfactants 1 and 2 shown in Figures 56.1 and 56.2 along with the Hi-Flow™ Plus 135 control. This plot suggests that at a fiber diameter of about 700 nm and a PMMA:PVDF ratio of 75:25, and similar mat thickness, the electrospun mats have similar protein binding as the Hi-Flow™ Plus 135 control. Fibers treated with Surfactant 2 have slightly higher protein binding than average (Figure 57). It also appears that PVDF has a higher protein binding capacity than PMMA.

[0132] Example 22 Protein Stripping Protein stripping line quality is another important attribute required for membranes used in lateral flow diagnostic assays, since line quality reflects the dissolution of the test line in the functional assay. Membrane samples were stripped using 2 mg / mL mouse IgG in PBS buffer using a Matrix™ 1600 reagent dispense module (Kinematic Automation, CA, USA) at various dispense rates in μL / cm. After drying the mats, they were stained with Ponceau S and rinsed with 1% acetic acid. The protein lines were then qualitatively evaluated against the Hi-Flow™ Plus 135 control for line width, stability, quality, and any artifacts that may adversely affect the function of the lateral flow diagnostic assay. Protein line stripping and detection lines on the assay can be optimized by varying the protein concentration and dispense rate. Table 9.1 and Figure 58.1 summarize the comparison of protein stripping quality of electrospun nonwoven fiber mat samples against the Hi-Flow™ Plus 135 control. Without significant optimization beyond varying the line speed, the electrospun fiber mat exhibited similar line quality to the commercial Hi-Flow™ Plus 135 control (Figure 58.1). Protein stripping can be optimized with detailed evaluation of dispense rate, line speed, protein concentration, and the thickness, basis weight, surface area, and protein binding capacity of the porous material. Table 9.2 and Figure 58.2 summarize the protein stripping quality as a function of protein (IgG) dissolution conditions detailed in Table 9.2 for pH and conductivity. Figure 58.2 shows, from left to right, replicate samples of Hi-Flow™ Plus 135 control and PMMA:PVDF (70:30) electrospun nonwoven fiber mat membranes treated with 0.07 and 0.09% Surfactant 2 (Example 20). The observed protein stripping line quality was 3>4>2>1 from best to worst solution. Table 9.3 and Figure 58.3 summarize the protein stripping quality as a function of protein (IgG) dissolution conditions detailed in Table 9.3 in terms of pH and conductivity.Figure 58.3 shows, from left to right, duplicate Hi-Flow™ Plus 135 control and PMMA:PVDF (70:30) electrospun nonwoven fiber mat membrane samples treated with 0.07 and 0.09% Surfactant 2 (Example 20). The protein stripping line quality observed was pH5=6>7.2>8>9 from best to worst pH. Tables 9.2 and 9.3 and Figures 58.2 and 58.3 show that the best protein stripping quality is achieved through dissolution conditions that favor the cation exchange binding mechanism.

[0133] [Table 9]

[0134] [Table 10]

[0135] [Table 11]

[0136] Example 23 Membrane Background Fluorescence Some lateral flow diagnostic assays require detection and / or quantification of fluorescently labeled detection beads, so the background fluorescence of the membrane needs to be sufficient. Solid-state fluorescence spectroscopy was performed on electrospun fiber membranes with PMMA:PVDF ratios of 75:25 and 50:50, and on Hi-Flow™ Plus 135 nitrocellulose control, which is known to have background fluorescence. The fluorescence spectroscopy was performed by photon counting intensity using a ChronosFD fluorescence lifetime spectrometer (ISS), Vinci2, and by spectral processing with Mathematica software. Excitation wavelengths of 300-610 nm and emission wavelengths of 320-630 nm were scanned in 10 nm increments with a PMT. Figure 59 shows the intensity of the fluorescence spectrum versus excitation and emission wavelengths for the Hi-Flow™ Plus 135 nitrocellulose control membrane, showing fluorescence in the emission region from about 350-500 nm. The large hypotenuse is due to Rayleigh scattering. Figures 60.1 and 60.2 show the fluorescence spectral intensity versus excitation and emission wavelengths subtracted from the Hi-Flow™ Plus 135 nitrocellulose control membrane spectrum at PMMA:PVDF ratios of 75:25 and 50:50, demonstrating that electrospun nonwoven fibers of PMMA:PVDF have less autofluorescence than nitrocellulose membranes.

[0137] Example 24 Fluorescence microscopy for detecting fluorescent beads Fluorescent microspheres and fluorescence microscopy were used to visualize the differences in terms of fluorescent bead visibility and signal intensity through the surface porosity of the two different structures in Hi-Flow™Plus135 nitrocellulose control membranes and electrospun PMMA:PVDF (75:25) membranes, as well as the differences in autofluorescence. The experiments were performed using a modification of the latex bead mobility test described above (Example 16). The fluorescent bead test solution was 0.05% fluorescent carboxylated polymer microspheres, 0.4 micron diameter, P(S / V-COOH), Ex max 480 nm, Em.Max 520 nm (FC02F Bangs Laboratories, Fishers, IN), 0.1% Tween surfactant, in 1 mg / mL BSA in PBS buffer. The solution was flowed up a 1×4 cm membrane strip and allowed to air dry before visualization under a fluorescent microscope. A Nikon Eclipse TE2000-U microscope with NIS Elements Imaging software and Ti-LAPP Modular Illumination System in bright field and FITC modes were used for the analysis (Nikon Instruments Inc. USA). Figure 61 is a collection of sample images comparing Hi-Flow™ Plus 135 nitrocellulose control membrane and electrospun PMMA:PVDF (75:25) membrane with and without fluorescent beads at 200x magnification in FITC mode and constant laser excitation intensity. The figure shows the background fluorescence of the Hi-Flow™ Plus 135 nitrocellulose control membrane, while the electrospun PMMA:PVDF (75:25) membrane has no visible fluorescence. The sample with beads shows higher visible emission fluorescence intensity through the non-woven fiber structure of the electrospun PMMA:PVDF (75:25) membrane when compared to the air-cast Hi-Flow™ Plus 135 nitrocellulose control membrane. The higher surface porosity of the electrospun nonwoven fibrous mats potentially allows for a further reduction in the detection limit in terms of fluorescence detection during functional assays.Additionally, the lack of autofluorescence of the base electrospun PMMA:PVDF (75:25) membrane makes detection and quantification easier compared to that of the air-cast Hi-Flow™ Plus 135 nitrocellulose membrane.

[0138] Example 25 Advantages of Electrospun Nanofiber and Membrane Mats FIG. 6 shows that four parameters (PMMA:PVDF ratio, % solids, dew point, and solvent composition) control fiber diameter and morphology. Four parameters (PMMA:PVDF ratio, electrospinning parameters, dew point, and film substrate) also contribute to nonwoven fiber mat productivity and uniformity. Four parameters (fiber diameter / effective pore size, PMMA:PVDF ratio, surfactant treatment, and mat thickness and uniformity) also contribute to properties relevant for use in lateral flow diagnostic applications, namely, CFT, detection bead mobility, protein binding, protein stripping, and functional assay performance. Electrospinning parameters that can be controlled during electrospinning of nanofibers include voltage, airflow, electrode distance, substrate line speed, carriage speed, dispense orifice, and wire speed of spinning electrode. Table 10 summarizes the properties of Hi-Flow™ Plus 135 air-cast nitrocellulose membrane and a typical electrospun PMMA:PVDF membrane.

[0139] [Table 12]

[0140] Example 26 Further electrospinning examples PMMA 14% in DMF was prepared by dissolving 7 g of PMMA in 43 g of DMF and stirring for 30 h at room temperature. The final solution was collected in a 10 mL plastic syringe (NANON-01A electrospinning machine, Japan) with an 18 G (gauge) needle attached and used for electrospinning. The polymer solution feed rate was varied from 1 to 5 mL / h, the applied voltage was varied from 10 to 30 kV, and the tip-to-collector (support for the membrane) distance was varied from 10 cm to 15 cm. PMMA electrospun membranes were obtained with a feed rate of 5 mL / h, a voltage of 18 kV, and a needle-to-collector distance of 15 cm. Membranes with thicknesses ranging from 20 to 120 μm were spun onto Melinex polyester backings, dried at room temperature to remove the solvent, and heat-treated at 150 °C to obtain uniform membranes. Similarly, electrospun membranes were prepared with PVDF, PVB, PA and PES. Table 11 shows the composition, electrospinning conditions and CFT of various membranes.

[0141] [Table 13] TIFF0007554806000015.tif104166

[0142] Electrospun membranes showing good adhesion to the Melinex backing were obtained by varying the solution parameters and electrospinning conditions. Figure 62 shows the dimensions of electrospun membranes with various thicknesses produced by using PMMA.

[0143] The fiber diameter and surface morphology of the electrospun membranes were characterized by a Zeiss Supra Variable Pressure Field Emission Scanning Electron microscope. The fiber diameters ranged from 200 nm to 2.7 μm. The surface profile of the membranes is shown in Figure 63. The membranes have good porosity and pore size, which is more suitable for the flow rate and allows the gold nanoparticles and latex beads mobility. The membranes also have sufficient protein binding efficiency.

[0144] Example 27 Testing of electrospun membranes Protein binding is essential for the function of membranes in lateral flow applications. The membrane should adsorb the required amount of protein to allow a visual readout of the test results. Protein stripping was performed with electrospun membranes. Membrane samples were cut (5 cm x 15 cm), pre-wet in ethanol for 1 min, immediately treated with 0.1 wt% surfactant 1 for 30 min, and dried. The protein solution was dispensed at a rate of 0.5 μl / cm. Figure 64 shows the results of protein stripping of electrospun membranes, demonstrating that proteins can be applied and bound to electrospun membranes produced by the methods described herein.

[0145] The most commonly used detection reagents in lateral flow systems are colloidal gold and latex particles. These particles are typically coupled with a variety of detection reagents and applied to the lateral flow membrane. The detection reagents allow the user to visualize the results. Gold and latex particle mobility tests were performed on electrospun PMMA and PVDF membranes. Figures 65 and 66 show the flow fronts of both gold and latex particles on PMMA and PVDF electrospun membranes, respectively. These figures show that the particles flow uniformly and without any flow front separation through the electrospun membrane.

[0146] The PMMA electrospun membranes of Figures 65 and 66 were examined under SEM to determine the flow patterns of the latex and gold nanoparticles. Figure 67 shows an SEM image of the PMMA electrospun membrane after latex and gold particle mobility testing. The particles flow along the plane of the fibers within the membrane structure and through the interconnected pores without any flow front separation.

[0147] Example 28 Electrospun Membranes Made from Polymer Blends Electrospun membranes were prepared using various polymer blends. Table 12 shows a list of the blended electrospun membranes along with the conditions used and the characteristics of the membranes produced.

[0148] To prepare a 12.5% ​​PMMA / PVDF (2:1 ratio) blend membrane, 5 g PMMA and 2.5 g PVDF were dissolved in 60 ml DMAc / acetone / THF solvent at room temperature. The electrospinning parameters were as follows: polymer solution feed rate 5 ml / hr, applied voltage 20 kV, and collector distance 15 cm. To prepare a 12.5% ​​PMMA / PVDF (1:2 ratio) blend membrane, similar conditions were used, but the amounts of PMMA and PVDF were reversed. The blend membrane was dried at room temperature to remove residual solvent from the membrane.

[0149] [Table 14] TIFF0007554806000017.tif31164

[0150] Figure 68 shows the results of protein stripping of PMMA / PVDF (2:1 ratio) and PMMA / PVDF (1:2 ratio) blend membranes. These results show that proteins can be applied to the electrospun blend membranes and that proteins bind to the electrospun membranes.

[0151] The mobility of gold and latex particles on electrospun PMMA and PVDF membranes was examined. Figure 69 shows the flow fronts of both gold and latex particles on a PMMA / PVDF blend electrospun membrane. These images show that the particles flow uniformly and without any flow front separation through the blend electrospun membrane.

[0152] Thus, a method is provided for producing highly porous electrospun membranes from a variety of polymers, PMMA, PVDF, PA, PES and PVB or combinations thereof. The membranes in electrospun process are formed from high surface area micro / nanofibers, and the membrane pore size can be controlled by blending suitable polymers in different ratios to vary the diameter of the fibers (e.g. PMMA alone was μm fibers, PMMA / PVDF was nanofibers).

[0153] The current air-casting method produces lateral flow membranes very slowly because the membrane is formed by a phase inversion method, whereas the electrospinning method provided herein produces membranes instantly. Using the methods provided herein, membranes produced from various polymers and polymer blends were evaluated. The membranes provided herein are more sensitive and facilitate detection of lower levels of analytes compared to current lateral flow membranes. Figure 70 illustrates a Hepatitis B assay, where membranes produced from various polymers and polymer blends were evaluated. ES membranes are more sensitive than current lateral flow membranes.

[0154] Example 29 Functional Lateral Flow Assay Using the Preceding Structures Electrospun nonwoven fiber mat membranes produced according to the previous examples using needleless electrospinning (summarized in Example 25) were used in fully integrated lateral flow assays and benchmarked against air-cast nitrocellulose. Examples include a lateral flow test for complete Hepatitis B surface antigen (HBsAg), as described in MilliporeSigma test method documents 00081440™ and 00081293™, and a hCG (human chorionic gonadotropin hormone) functional test to detect pregnancy.

[0155] Figure 71.2 shows a standard breakthrough test with positive test line detection at 8 ng / mL for a Hepatitis B surface antigen (HBsAg) lateral flow test using an air-cast nitrocellulose membrane. Figure 71.1 shows a similar HBsAg breakthrough test using an electrospun nonwoven fiber mat membrane produced in the previous example summarized in Example 25. The electrospun nonwoven fiber mat membrane was PMMA:PVDF (70:30) with an average fiber diameter of approximately 800 nm on a LDPE PE700AS film treated with 0.08% Surfactant 2.

[0156] Figure 72.2 shows a pass-through test with positive test line detection at 25mIU in a hCG (human chorionic gonadotropin hormone) functional test to detect pregnancy using an air cast nitrocellulose membrane. Figure 72.1 shows a similar pass-through test in a hCG (human chorionic gonadotropin hormone) functional test to detect pregnancy using an electrospun nonwoven fiber mat membrane produced in the previous example summarized in Example 25. The electrospun nonwoven fiber mat membrane was PMMA:PVDF (70:30) with an average fiber diameter of about 800 nm on a LDPE PE700AS film treated with 0.08% Surfactant 2.

[0157] Example 30 Electrically Blown Fibers A fiber mat is produced having an average fiber diameter of 500-1000 nanometers, an average flow pore rating of 1-5 microns, and a mat thickness of 100 microns, comprising a polymer ratio of about 100:0 to 0:100 between PMMA:PVDF, specifically about:10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55, 50:50, 55:45, 60:40, 65:35, 70:30, 75:25, 80:20, 85:15, or 90:10. In some embodiments, the fiber mat is produced on a porous substrate using electroblowing or electrospray spinning. The fibers are spun from a 10-20 w / w% solution of PMMA:PVDF in a solvent, such as N,N-dimethylacetamide or N,N-dimethylformamide. The resulting polymer solution is electroblown into fibers by forcing the polymer solution through a small nozzle parallel to the gas flow pressure region, where a high electric field or high voltage is maintained from the exit nozzle and a collection region above the moving porous nonwoven that collects the fibers. Conditions for electroblown fibers of 500-1000 nm diameter from the polymer solution include 1-10 mL / min solution flow from the nozzle into a gas pressure of greater than 1 bar and an electric field of 1-100 kV DC. The thickness and uniformity of the mat can be controlled by adjusting the temperature, relative humidity, dew point, nonwoven substrate, and chamber airflow. The electroblown nonwoven fiber mat is subjected to additional heat drying, calendaring, and surfactant treatments, as well as drying as a post-treatment. The electroblown nonwoven fiber mat is bonded to a non-porous substrate using the method in Example 11. The resulting electroblown fiber nonwoven mat has similar properties to previous examples made by electrospinning, summarized in Example 25. Similar properties include fiber diameter, mean flow pore size, mat thickness, capillary flow time, bead mobility, protein binding and protein stripping.

[0158] Certain aspects of an electric blowing process that can be used in the methods described herein are described in US Pat. No. 7,846,374, which is incorporated herein by reference in its entirety.

[0159] Incorporation by Reference All publications, patents, and patent applications mentioned in this specification are hereby incorporated by reference in their entirety to the same extent as if each individual publication, patent, or patent application was specifically and individually indicated to be incorporated by reference. In the case of conflicts, the present application, including any definitions herein, will control.

[0160] Equivalent form It is anticipated that those skilled in the art will recognize, or be able to ascertain using no more than routine experimentation, many equivalents to the specific embodiments described herein which equivalents are intended to be encompassed by the following claims.

Claims

1. A method for producing an electrospun nonwoven fibrous membrane by a needleless process carried out in a spinning chamber, the method being carried out by an apparatus consisting of a rotating wire electrode, a rotating spinning electrode, a collecting electrode and a collecting substrate, the membrane having a mean flow pore size of greater than about 1 micron and a porosity of at least 80%, the method comprising electrospinning a polymer preparation comprising PMMA, PVDF or a blend of PMMA and PVDF in a solvent onto a non-porous film substrate, the membrane being collected on the collecting substrate, the membrane comprising nanofibers having an average fiber diameter of 200 nm to 1000 nm.

2. The method of claim 1 , wherein the non-porous film substrate is insoluble in the solvent for the polymer formulation and does not bear an electrical charge.

3. 2. The method of claim 1, wherein the polymer preparation is 1) a melt of a polymer, or 2) a solution of a polymer, or 3) a blend of polymers.

4. 2. The method of claim 1, wherein the blend of PMMA and PVDF has a weight ratio between PMMA and PVDF of 1:99 to 99:

1.

5. 2. The method of claim 1, wherein the weight ratio of PMMA to PVDF is 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55, 50:50, 55:45, 60:40, 65:35, 70:30, 75:25, 80:20, 85:15 or 90:

10.

6. 2. The method of claim 1, wherein the polymer preparation comprises PMMA and / or PVDF dissolved in a solvent selected from N,N-dimethylacetamide (DMAC), N,N-dimethylformamide (DMF), or a mixture thereof.

7. The method of claim 6 , wherein the solvent further comprises acetone.

8. The method of claim 1, wherein the polymer formulation comprises about 5% to 20% by weight PMMA, PVDF, or a blend thereof.

9. 2. The method of claim 1, wherein the polymer preparation comprises 15%, 16%, 17%, 18%, 19% or 20% by weight of the blend of PMMA and PVDF, the ratio of PMMA to PVDF in the blend being 75:25, 60:40 or 50:50, and PMMA and / or PVDF are dissolved in a solvent selected from DMAC, DMF or mixtures thereof.

10. The method of claim 9 , wherein the solvent further comprises acetone.

11. 2. The method of claim 1, wherein the viscosity of the polymer preparation comprising PMMA and / or PVDF in the solvent of DMAC and / or DMF and / or acetone is from 200 centipoise (cP) to 5000 cP, from 300 cP to 2000 cP, from 400 cP to 1000 cP, from 500 cP to 900 cP, from 600 cP to 800 cP, or from 700 cP to 800 cP.

12. 10. The method of claim 1, wherein the non-porous polymeric film substrate comprises polyethylene and carbon, polyimide and carbon, low density polyethylene (LDPE) and antistatic agent, polypropylene and antistatic agent, acrylonitrile butadiene styrene and antistatic agent, nylon, static dissipative high molecular weight polyethylene (UHMWPE), polypropylene spunbond and antistatic treatment, LDPE, polycarbonate, UHMWPE, polyvinyl chloride, polyethylene terephthalate (PET), PMMA, PVDF, or PMMA / PVDF.

13. The non-porous polymer film substrate is 8 Ωcm~10 12 The method of claim 1 having a bulk electrical resistivity of Ω cm.

14. 10. The method of claim 1, wherein the nanofibers are electrospun at a voltage of 30-120 kV, 40-110 kV, 50-100 kV, 60-90 kV, or 70-80 kV.

15. 2. The method of claim 1, wherein the electrode distance is 150-300 mm, 160-290 mm, 170-280 mm, 180-270 mm, 190-260 mm, 200-250 mm, 210-240 mm, or 220-230 mm.

16. 2. The method of claim 1, wherein the diameter of the dispensing orifice is 0.4-0.8 mm, 0.45-0.75 mm, 0.5-0.6 mm, 0.55-0.65 mm or 0.6 mm.

17. 2. The method of claim 1, wherein the carriage speed is 50-150 mm / sec, 60-140 mm / sec, 70-130 mm / sec, 80-120 mm / sec, 90-110 mm / sec, or 100 mm / sec.

18. The method of claim 1, wherein the wire speed is 1-5 mm / sec, 2-4 mm / sec, or 3 mm / sec.

19. Air-in speed is 60m 3 / hr~120m 3 / hr, 70m 3 / hr~110m 3 / hr, 80m 3 / hr~100m 3 / hr or 90m 3 / hr, and the air out speed is 100 m 3 / hr~140m 3 / hr, 110m 3 / hr~130m 3 / hr or 120m 3 The method of claim 1, wherein the heating time is 100 min. / hr.

20. The process of claim 1, wherein the temperature in the spinning chamber is 25-50°C, 30-45°C, 35°C-40°C, or 40-45°C.

21. 2. The method of claim 1, wherein the relative humidity in the spinning chamber is 10-35%, 15-30%, or 20-25%.

22. 2. The method of claim 1, wherein the dew point in the spin chamber is 2.0°C to 6.0°C, 2.2°C to 5.8°C, 2.4°C to 5.6°C, 2.6°C to 5.4°C, 2.8°C to 5.2°C, 3.0°C to 5.0°C, 3.2°C to 4.8°C, 3.4°C to 4.6°C, 3.6°C to 4.4°C, or 3.8°C to 4.2°C.

23. 2. The method of claim 1, wherein the line speed per wire is from 0.5 cm / min to 5.0 cm / min, from 1.0 cm / min to 4.5 cm / min, from 1.5 cm / min to 4.0 cm / min, from 2.0 cm / min to 3.5 cm / min, or from 2.5 cm / min to 3.0 cm / min.

Citation Information

Patent Citations

  • Operational pressure controlling apparatus for power steering system

    JP1978055828A

  • Composite film for electrochemical device, method for producing the same, and electrochemical device provided with the same

    JP2006527911A

  • Electrolyte-containing polymers produced by the electrospinning process and high-efficiency dye-sensitized solar cells using these electrolyte-containing polymers.

    JP2012501518A

  • Method of manufacturing touch panel

    JP2013073618A

  • Polymer nanofiber structure and method for producing the same

    JP2015183334A