Manufacturing method and device for multi-stage hot press-formed part, and hot press-formed part manufactured by the same

The multi-step hot press forming method addresses the limitations of single-step processes by using rapid heating and controlled cooling to produce complex shapes with improved strength and productivity, reducing heating furnace length and costs.

JP7554904B2Active Publication Date: 2024-09-20POHANG IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023504042
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-24
Filing Date
2021-06-28
Publication Date
2024-09-20
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

Conventional hot press forming methods are limited to single-step processes, making it difficult to manufacture complex shapes and incur additional costs due to the need for specialized heating furnaces and rapid cooling of high-temperature materials, which complicates multi-stage forming processes.

Method used

A method and apparatus for multi-step hot press forming that includes a heating stage, notching, blanking, molding, and trimming processes using a single press with multiple molds, employing rapid heating methods like induction or resistance heating to achieve uniform temperature distribution and minimize cooling during transfer, allowing for the production of complex shapes with improved productivity and strength.

Benefits of technology

The method enables the stable supply of high-temperature materials at fast cycle times, facilitating the production of complex shapes with enhanced strength properties, such as a tensile strength of 1300 MPa or more, while reducing the length and cost of heating equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554904000017
    Figure 0007554904000017
  • Figure 0007554904000013
    Figure 0007554904000013
  • Figure 0007554904000025
    Figure 0007554904000025
Patent Text Reader

Abstract

The present invention provides a method and device for manufacturing a multi-stage hot press-formed part, which includes: a heating step for heating a strip material; a transport step for transporting the heated strip material using a processing device in which a number of dies, including one or more dies selected from among notching dies and blanking dies, a forming die, and a trimming die, are attached to one press; one or more of a notching step for cutting a part of the material using the notching dies to obtain a notched material in a form connected to a web portion of the strip, and a blanking step for cutting a part of the material using the blanking dies to obtain a blank material in a form separated from the strip; a forming step for transporting the material that has undergone one or more of the notching and blanking steps, positioning it near the forming die, and then forming the material using the forming die; and a trimming step for removing the peripheral portion of the unnecessary material from the final product shape using the trimming die.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for manufacturing a multi-stage hot press-formed part, which has improved one or more of productivity and formability. [Background technology]

[0002] In response to the demand for lighter vehicle weight and improved safety, the application of high-strength steel using hot press forming is being actively promoted. In general, in the hot press forming method, a blank with a shape designed for forming a part is prepared, heated to a high temperature, and then inserted into a die attached to a press. Then, the press slide is lowered to the bottom dead center to form the blank, and the formed part is quenched in the die by maintaining it at the bottom dead center for a certain period of time. After being sufficiently cooled in this manner, the slide is raised and the product is taken out, and the part is manufactured. In addition, the parts manufactured in this manner generally undergo a process of cutting off some unnecessary edges and holes on the inside from the final part shape, and are manufactured into the final part shape. The process of cutting the product after such forming is performed by laser trimming or mechanical trimming using a trimming die / press, since the formed product has high strength.

[0003] The above-mentioned general hot press forming has a limitation that the final part must be produced in one forming operation, and has a drawback that it is not possible to produce part shapes that are difficult to produce in one forming operation. In order to solve this problem, a method of using indirect hot press forming has been applied in which a part is formed into an intermediate stage shape at room temperature, and then the preformed part is heated and hot press formed into a final part shape. However, such indirect hot press forming has a drawback in that it requires an additional process of forming into an intermediate stage shape and a special heating furnace capable of heating the formed part, which adds various production costs.

[0004] Meanwhile, in general cold press forming, a common approach is to form the final part through a multi-stage forming process. As a method of cold press forming, forming is divided into several steps using several presses and dies, or a method of forming by placing a multi-stage die in one press is used. Meanwhile, as a method of forming by placing a multi-stage die in one press, a transfer method of forming in which separate blanks are put into a die and formed in multiple stages, and a progressive method of forming in which a continuously connected strip-shaped material is fed and formed in multiple stages are generally used.

[0005] However, unlike cold press forming, hot press forming has a special restriction that a high-temperature material must be rapidly cooled to ensure high strength, so it is not easy to apply the above-mentioned multi-stage forming method. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Korean Patent Publication No. 2006-0054479 Summary of the Invention [Problem to be solved by the invention]

[0007] According to one aspect of the present invention, there is provided a method and apparatus for manufacturing a multi-stage hot press-formed part, which has improved one or more of productivity and formability.

[0008] According to another aspect of the present invention, a formed member having excellent strength characteristics while having a complex shape that could not be obtained by a conventional single-step hot press forming method can be provided.

[0009] The object of the present invention is not limited to the above. Anyone having ordinary knowledge in the technical field to which the present invention belongs will have no difficulty in understanding further object of the present invention from the entire contents of the specification of the present invention. [Means for solving the problem]

[0010] One aspect of the present invention is A heating stage in which the strip material is heated; a transfer step of transferring the heated strip material using a processing device having a number of dies, including one or more dies of a notch die and a blanking die, a forming die, and a trimming die, attached to one press; one or more steps of: a cutting step of cutting a part of the material using the cutting die to obtain a notched material connected to the web portion of the strip; and a blanking step of cutting a part of the material using the blanking die to obtain a blanked material separated from the strip; a molding step of transferring the blank that has been subjected to one or more of the notching step and the blanking step, positioning the blank near the molding die, and molding the blank using the molding die; and a trimming step in which the trimming die is used to remove the peripheral portion of the unnecessary material from the final product shape; The present invention provides a method for producing a multi-stage hot press formed part, comprising the steps of:

[0011] Another aspect of the present invention is A feed section for continuously feeding strip material; A heating section for heating the supplied strip material; A processing section including a processing device to which a number of dies including one or more of a notch die and a blanking die, a molding die, and a trimming die are attached to one press; and a transfer section for transferring the strip material heated in the heating section to the processing section; The present invention provides a multi-stage hot press formed part manufacturing apparatus, comprising:

[0012] Another aspect of the present invention is A hot press-molded member manufactured by the above-mentioned method for manufacturing a multi-stage hot press-molded member, Provided is a hot press formed part that includes an undercut shape and has a tensile strength of 1300 MPa or more. Effect of the Invention

[0013] According to one aspect of the present invention, it is possible to provide a manufacturing method and apparatus for a hot press-formed part for multi-stage processes, which can stably heat and supply strip material at a fast cycle time and has improved productivity.

[0014] Alternatively, according to another aspect of the present invention, by forming a strip material through multiple steps, it is possible to relatively easily provide a complex shape as compared with a single-step hot press forming.

[0015] According to another aspect of the present invention, a formed member having excellent strength characteristics while having a complex shape that could not be obtained by a conventional single-step hot press forming method can be provided.

[0016] The various yet significant advantages and effects of the present invention are not limited to the above, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0017] [Figure 1] 1 is a diagram showing an exemplary multi-stage hot press forming apparatus according to the present invention; [Diagram 2] 1A shows the temperature distribution when a material with a constant width is electrically heated, and FIG. 1B shows the temperature distribution when a material with a variable width is electrically heated. [Diagram 3] 4 is a graph showing the operation method of an exemplary mechanical press of the present invention in terms of the relationship between stroke and crank angle. [Figure 4]1 is a graph showing the temperature change of a material over time when applying a typical progressive method in an exemplary notch stage of the present invention. [Diagram 5] 10 is a graph showing the temperature change of the material over time in an exemplary notching step of the present invention, in which the notching upper die and the notching lower die are in contact with the strip material only during the cutting process. [Figure 6] 1 is a graph illustrating the temperature change of the material over time for Example 14. [Figure 7] 1 is a graph illustrating the temperature change of the material over time for Example 15. [Figure 8] 1 is a graph illustrating the temperature change of the material over time for Example 16. [Figure 9] 1 is a graph showing a change in thickness reduction rate when an exemplary molding process of the present invention is performed in a single process. [Figure 10] 1 is a graph showing a change in thickness reduction rate when an exemplary molding process of the present invention is performed in two stages. [Figure 11] 1 is a diagram illustrating an exemplary multi-step hot press forming method according to the present invention. [Figure 12] 1 is a diagram showing changes in a material during an exemplary multi-step process of the present invention. [Figure 13] 1 illustrates an exemplary notching or blanking method of the present invention. [Figure 14] 1 is a diagram illustrating an exemplary notch or blanking method using a push bar according to the present invention. [Figure 15] 1 illustrates an exemplary method of increasing mold contact time of the present invention. [Figure 16] 1 illustrates an exemplary method of increasing mold contact time of the present invention. [Figure 17] 1 illustrates an exemplary method of increasing mold contact time of the present invention. [Figure 18]FIG. 1 is a drawing showing the structure of an exemplary hot press-formed member of the present invention, in which (a) is a perspective view of the formed member and (b) is a side view of the formed member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Since hot press forming requires rapid cooling of high-temperature materials to ensure high strength, it is difficult to apply a multi-stage forming method. Therefore, a method has been recently studied in which a blank is heated using galvanized hot press forming steel, then inserted into a multi-stage die attached to a mechanical servo press, where it is rapidly cooled to a relatively low temperature, pierced, and finally trimmed. However, this method requires that the heating furnace has sufficient performance to supply the heated blank at the speed required by the press.

[0019] For example, if pressing is performed at a speed of 15 SPM (15 strokes per minute), this means that a furnace capable of supplying a heated blank every 4 seconds is required.Normal hot press forming cycle times are also around 16 seconds, which means that the work can be considered to be performed quite quickly, but this means that a furnace capable of supplying a heated blank every 16 seconds is required.

[0020] Now, if the cycle time is 4 seconds, the heated blanks must be fed at a speed four times faster than when the cycle time is 16 seconds. Since the material is not heated to the desired temperature unless it stays in the heating furnace for the required time, four times as many blanks must be fed into the heating furnace to heat at a speed four times faster. Therefore, it can be arithmetically estimated that the length of the heating furnace must be four times longer to achieve this. For example, a normal heating furnace is about 30 m long, but to heat at a speed four times faster as described above, the length of the heating furnace must be about 120 m, or four heating furnaces each 30 m long must be installed in parallel.

[0021] However, since the length of the heating furnace is a major obstacle in terms of space and cost, it is also possible to utilize equipment that can rapidly heat the blanks rather than the heating furnace with the general atmosphere described above.

[0022] In response to this, the inventors have conducted extensive research and found that it is technically not easy to heat a shaped blank quickly and uniformly. Thus, the inventors have continued their research and have invented a multi-stage hot press forming apparatus and method that stably supplies high-temperature material at a high speed compatible with a short cycle time and has improved formability.

[0023] In addition, general hot press forming includes a process of maintaining the press at the bottom dead center for a certain period of time after forming and maintaining the die in a closed state to perform cooling. However, in the case of a multi-stage process, since multiple stages of processes need to be performed in sequence, cooling is not performed in only one die, but in multiple stages of dies. Therefore, the multi-stage hot press forming method of the present invention requires a process design that takes into account the influence of various process factors, such as press speed and number of steps, on cooling. Therefore, the present inventors have designed an optimal multi-stage process in consideration of various process factors.

[0024] [Manufacturing method for hot press-formed parts for multi-stage processes] One aspect of the present invention is A heating stage in which the strip material is heated; a transfer step of transferring the heated strip material using a processing device having a number of dies, including one or more dies of a notch die and a blanking die, a forming die, and a trimming die, attached to one press; one or more steps of: a cutting step of cutting a part of the material using the cutting die to obtain a notched material connected to the web portion of the strip; and a blanking step of cutting a part of the material using the blanking die to obtain a blanked material separated from the strip; a molding step of transferring the blank that has been subjected to one or more of the notching step and the blanking step, positioning the blank near the molding die, and molding the blank using the molding die; and a trimming step in which the trimming die is used to remove the peripheral portion of the unnecessary material from the final product shape; The present invention provides a method for producing a multi-stage hot press formed part, comprising the steps of:

[0025] According to one aspect of the present invention, the method may include a heating step of heating the strip material, and the strip material may be heated in a temperature range of 850 to 960°C. According to one aspect of the present invention, the heating method may be rapid heating, and the heating rate may be in the range of 12 to 200°C / s. Meanwhile, preferably, the lower limit of the heating rate may be 13°C / s, and more preferably, the lower limit of the heating rate may be 30°C / s. Also, the upper limit of the heating rate may be 100°C / s, and more preferably, the upper limit of the heating rate may be 80°C / s. Also, the heating temperature may be a value measured based on a temperature change based on any one point on the surface of the strip material.

[0026] According to one aspect of the present invention, various methods can be used for rapid heating, such as induction heating, resistance heating, infrared heating, etc. By heating a strip material having a uniform width using the above-mentioned rapid heating methods, a more uniform temperature distribution can be ensured compared to the conventional method of heating a blanking material having a shape, and thus the heated strip material can be stably supplied at a fast cycle time.

[0027] On the other hand, in the conventional method of heating blank material, since it is difficult to perform uniform heating, an atmosphere heating furnace is almost always used. However, in order to supply blanks heated in a short cycle time of a multi-stage process, the length of the heating furnace becomes excessively long. Here, in the present invention, it has been found that the above-mentioned problem can be solved by applying a rapid heating method to a strip material itself with a constant width.

[0028] For example, if the cycle time is 4 seconds (based on a pitch of 500mm designed for the multi-stage process described below), and if a method of rapid heating to the final temperature in 16 seconds is used, the length of the strip material involved in the heating process is calculated to be around 2m. Therefore, it is expected that the heating space can be significantly reduced compared to the conventional blank heating method exemplified above, where the heating furnace length is 120m or four heating furnaces are arranged in parallel, each 30m long.

[0029] That is, according to one aspect of the present invention, the ratio (L / S) of the total heating device effective length (L) to the cycle time (S) can be, but is not particularly limited to, in the range of 0.25 to 4. By satisfying the above-mentioned range, it is possible to provide a hot press forming method that stably supplies material at a fast cycle time and has improved formability.

[0030] In this case, the above-mentioned total effective length of the heating device (L) refers to the length of the part directly used for heating the material, and is expressed in units of m. For example, in the case of a heating furnace, it means the internal length of the heating furnace, and in the case of high-frequency heating, it can mean the length of the high-frequency coil used for heating. That is, even if one or more of the series and parallel types are included, it means the effective length of all the heating devices. Specifically, if four 30m heating furnaces are arranged in parallel, the total effective length of the heating device corresponds to 120m [=30m x 4]. The above-mentioned cycle time means the time it takes for one cycle to be performed in a multi-stage process, and is expressed in units of sec (seconds).

[0031] Meanwhile, according to one aspect of the present invention, the strip material can be a plated steel sheet including a base steel sheet and a plating layer provided on the base steel sheet. That is, an aluminum-plated steel sheet or an aluminum alloy-plated steel sheet can be used to sufficiently alloy the plating layer and prevent melting and volatilization of the plating layer when a rapid heating method is applied to the strip material.

[0032] According to one aspect of the present invention, the base steel sheet may have a composition including, by weight percent, C: 0.1-0.5%, Si: 0.1-2%, Mn: 0.5-3%, Cr: 0.01-0.5%, Al: 0.001-1.0%, P: 0.05% or less, S: 0.02% or less, N: 0.02% or less, B: 0.002-0.005%, the balance being Fe and other inevitable impurities, but the base steel sheet is not limited to such a composition. In addition, the plating layer may be used by alloying a plated material produced by hot-dip plating so as to have a composition including, by weight percent, Si: 5-11%, Fe: 4.5% or less, the balance being Al and other inevitable impurities, but the plating layer is not limited to such a composition. That is, as a non-limiting example of the present invention, an aluminum-plated steel sheet or an aluminum alloy-plated steel sheet satisfying the above-mentioned composition may be used.

[0033] According to one aspect of the present invention, the strip material can be an aluminum-plated steel sheet or an aluminum alloy-plated steel sheet having an Fe content of 5% by weight or more, preferably 5 to 60% by weight (more preferably 30 to 60% by weight) in the surface portion of the plating layer. In this case, the surface portion of the plating layer means a region within 2 μm from the surface of the plating layer. Meanwhile, by using a strip material having an Fe content in the surface portion of the plating layer that satisfies the above-mentioned range, high-temperature heating can be performed while ensuring a sufficient alloying time when rapid heating is applied.

[0034] According to one aspect of the present invention, the method may further include a step of continuously supplying the prepared strip material to the heating unit prior to the heating step. The strip material may be continuously supplied to the heating unit in the form of a strip material having a uniform width by an uncoiler, the strip material being prepared in a coil shape. Here, the strip material having a uniform width refers to a strip material having a uniform width measured in a direction perpendicular to the transport direction of the strip material based on the surface of the strip material.

[0035] According to one aspect of the present invention, the term "continuously supplying" may mean that the strip material is supplied to the heating section at a constant speed, except for a moment when the material is stopped for a while to consider a subsequent process.

[0036] According to one aspect of the present invention, a processing device is provided in which a number of dies including one or more of a notching die and a blanking die, a forming die, and a trimming die are attached to a single press, and the processing device includes a strip material transfer step for transferring the heated strip material.

[0037] According to one aspect of the present invention, the heated strip material can be continuously transferred to the processing device, and the above description of "continuously supplying" can be applied to the meaning of "continuously transferring" except that the heated strip material is transferred to the processing device.

[0038] According to one aspect of the present invention, since it is preferable to minimize cooling of the strip material heated during the above-mentioned transport step, the above-mentioned transport step of the strip material can be performed in a heat-retaining chamber. That is, by transporting the strip material in the above-mentioned heat-retaining chamber, it is possible to prevent heat loss and ensure easy processability in the processing equipment.

[0039] According to one aspect of the present invention, the temperature of the heat-retaining chamber may be maintained within a temperature range of Ts-200°C or more and Ts+50°C or less, based on the surface temperature (Ts) of the strip material supplied to the heat-retaining chamber. By controlling the temperature of the heat-retaining chamber to Ts-200°C or more, it is possible to minimize cooling of the strip material during the transfer process and ensure easy processability in a processing device, and by controlling the temperature of the heat-retaining chamber to Ts+50°C or less, it is possible to prevent further temperature rise during the transfer process. Meanwhile, in order to further improve the above-mentioned easy processability and the effect of preventing further temperature rise during the transfer process, the temperature of the heat-retaining chamber may be preferably 900°C or more and Ts+50°C or less, more preferably in the range of 900 to 1,010°C.

[0040] In this case, the surface temperature (Ts) of the strip material fed into the heat-retaining chamber may be in the range of heating temperatures generally used in the art, and is not particularly limited in the present specification. However, as a non-limiting example, the surface temperature (Ts) of the strip material may be in the range of 850 to 960°C.

[0041] Meanwhile, according to one aspect of the present invention, in the one press, at least one of the notch die and the blanking die and the forming die may be installed at a distance from each other by a designed pitch amount in the transport direction of the strip material. For example, in the case where only the notch die (or only the blanking die) is included, the notch die (or the blanking die) may be installed first in the transport direction of the strip material in the one press, and then the forming die may be installed at a distance from the notch die (or the blanking die) by a designed pitch amount. Alternatively, in the case where all of the notch die and the blanking die are included, the notch die, the blanking die, and the forming die may be installed in the transport direction of the strip material in the one press, and at this time, the distance between two dies adjacent to each other in the transport direction may be the designed pitch amount.

[0042] According to one aspect of the present invention, the forming die and the trimming die can be attached to the one press at a designed pitch from each other in the transport direction of the strip material. That is, in the one press, the notching die (and / or blanking die) and the forming die can be attached in order in the transport direction of the strip material in the same manner as described above, and the trimming die can be attached at a designed pitch from the forming die.

[0043] Alternatively, as described below, when one or more of a piercing step and a flanging step are further included, a piercing die (and / or a flanging die) may be further installed between the forming die and the trimming die in the material conveying direction in one press. For example, when a piercing step is further included, a notch die (and / or a blanking die), a forming die, a piercing die, and a trimming die may be installed in this order in the material conveying direction in one press.

[0044] According to one aspect of the present invention, in addition to the above-mentioned piercing and flanging steps, additional processing steps that are generally applicable in the art may be further included according to the purpose of the present invention. Accordingly, additional processing dies corresponding to the above-mentioned additional processing steps may be attached to the one press as needed.

[0045] In this case, according to one aspect of the present invention, in one press, two dies adjacent to each other in the transport direction of the strip material may be disposed at a designed pitch between them. For example, if a piercing step is further included, in one press, a piercing die may be attached at a designed pitch from the forming die, and a trimming die may be attached at a designed pitch from the piercing die.

[0046] Alternatively, according to one aspect of the present invention, when one or more steps of the notching and blanking steps, the forming step, one or more steps of the piercing and flanging steps (however, the piercing and flanging steps can be omitted), and one or more steps of the trimming step are divided into two or more multi-stage processes as described below, a number of dies provided for the steps divided into the multi-stage processes may be attached at intervals of a designed pitch amount from each other in a transport direction of the strip material in one press. In this case, in one press, a first die of a step performed in the multi-stage process may be attached at an interval of a designed pitch amount from the die of the previous step in the transport direction of the strip material. Also, a last die of a step performed in the multi-stage process may be attached at an interval of a designed pitch amount from the die of the immediately following step in the transport direction of the strip material.

[0047] For example, when the forming step is performed in a multi-stage process of two stages, the primary forming die and the secondary forming die may be attached to one press at an interval of a pitch amount designed in the transport direction of the strip material. In this case, the primary forming die may be attached to one press at an interval of a pitch amount designed in the transport direction of the strip material from a notching die (if a notching step is included) used in the immediately preceding stage. Also, the secondary forming die, which is the last die in the forming step performed in the multi-stage process, may be attached to one press at an interval of a pitch amount designed in the transport direction of the strip material from a piercing die (if a piercing step is included) used in the immediately following stage.

[0048] According to one aspect of the present invention, for a number of dies, each pitch amount designed between two dies adjacent to each other in the transport direction of the strip material may be the same. Meanwhile, Fig. 1 shows a transport direction X of the strip material, and shows a designed pitch amount 50 between two dies adjacent to each other in the transport direction X. The designed pitch amount may mean the distance between two adjacent dies measured based on the center of each die (a point that is 1 / 2 the length of one die along the transport direction of the material).

[0049] According to one aspect of the present invention, multiple dies attached to one press can all move in conjunction with the press movement of the single press. That is, the upper and lower dies for each die attached to one press can be mated in conjunction with the press movement of the single press. That is, mating of each die attached to the press can be performed when the press slide descends and stops at the bottom dead center of the press.

[0050] Therefore, by controlling the pitch amounts designed for two adjacent dies in the material transfer direction to be the same as described above, the material transfer between the dies can be consistently controlled when the material is processed by the progressive method, which corresponds to one example of the present invention. This ensures improved productivity and processability, and makes it easy to perform multi-stage processes.

[0051] That is, according to one aspect of the present invention, after one closing between the press upper plate (press slide) and the press lower plate (press bolster) due to the press movement of one press, the workpiece can be transferred in the workpiece transfer direction by the designed pitch amount.

[0052] According to one aspect of the present invention, the method may include one or more of the following steps: a cutting step, in which a portion of the material is cut using the cutting die to obtain a notched material in a form connected to the web portion of the strip; and a blanking step, in which a portion of the material is cut using the blanking die to obtain a blank material in a form separated from the strip.

[0053] In the cutting or blanking step, the upper and lower dies of the dies are mated to each other, so that unnecessary portions can be removed in advance from the material and processed into a desired shape. In this case, the material processed into a desired shape obtained by the cutting step may be a cut-out material connected to the strip by a web portion. Also, the material processed into a desired shape obtained by the blanking step may be a blank material separated from the strip.

[0054] According to one aspect of the present invention, a heated mold may be used in one or more of the notching and blanking steps, and the initial temperature of one or more of the notching and blanking molds may be 50° C. or higher, but is not particularly limited thereto. Meanwhile, the higher the temperature of the mold, the better the effect of suppressing cooling, so the upper limit of the initial temperature of the mold does not need to be separately limited. However, preferably, the upper limit of the initial temperature of the mold may be equal to or lower than the heating temperature of the strip material. That is, a notching mold heated in the notching step and / or a blanking mold heated in the blanking step may be used. Generally, in order to process the material in the notching and blanking steps, it is essential that the upper and lower molds of the mold are in contact with each other. Therefore, by using a heated mold in the notching and blanking steps, the strip material heated to a high temperature is prevented from coming into contact with a cold mold, and rapid cooling of the material is suppressed, and easy formability in the subsequent process can be ensured.

[0055] According to one aspect of the present invention, in order to suppress cooling of the strip material, the initial temperature of at least one of the notch mold and the blanking mold may be 400° C. or more, and more preferably 500° C. or more. The initial temperature of the mold means the initial temperature of the mold at the time when the material is put into the mold. Meanwhile, since the higher the temperature of the mold, the better the effect of suppressing cooling, the upper limit of the initial temperature of the mold does not need to be separately limited. However, preferably, the upper limit of the initial temperature of the mold may be equal to or lower than the heating temperature of the strip material. In this way, by controlling the initial temperature of the mold to 400° C. or more, easy formability in the molding step, which is a subsequent process, can be ensured. In addition, by controlling the initial temperatures of the notch and blanking molds to be equal to or lower than the heating temperature of the strip material, additional heating due to contact during notching and blanking can be prevented.

[0056] According to one aspect of the present invention, the surface temperature of the material immediately after one or more of the notching and blanking steps may be controlled to 700°C or more, more preferably 712°C or more. Meanwhile, the upper limit of the surface temperature is not particularly limited, but it may be preferably equal to or lower than the heating temperature of the strip material. In this case, the surface temperature of the material is a value measured based on the point at which the contact between the mold and the material ends immediately after one or more of the notching and blanking steps. Meanwhile, by satisfying the above-mentioned range, excellent formability in the subsequent process and prevention of additional heating can be achieved at the same time.

[0057] On the other hand, as can be seen from Figures 11 and 13, in the case of the progressive method, the strip material 200 transferred to the processing device 41 is generally maintained at the normal material transfer height level 110a, and while contacting the notched upper die 61a, it descends in accordance with the movement of the upper die 61a while in contact with the notched upper die 61a. In this way, while the strip material 200 descends while in contact with the notched upper die 61a, it also comes into contact with the notched lower die 61b near the bottom dead center 110b of the slide, cutting off a part of the strip material 200, thereby notching it. Next, the notched material rises again while in contact with the notched upper die 61a to the original transfer height level.

[0058] 4, which shows exemplary experimental results reflecting the above, it can be seen that the temperature of the material drops rapidly in the section where the contact of the notch upper die begins. Here, the inventors further discovered that if the strip material comes into contact with the die only when it is cut, the time the strip material contacts the upper die of the die can be minimized, thereby reducing cooling. In addition, although not shown separately in the drawings, in the same manner as in the notch step described above, in the blanking step, the time the material contacts the upper die of the blanking die can be minimized, thereby reducing cooling.

[0059] That is, according to one aspect of the present invention, in the above-mentioned cutting and blanking steps, the strip material fed into the processing device can be controlled so that it descends from the material transfer height level to the press bottom dead point without contacting the upper die of the mold, and the strip material comes into contact with the upper die (or upper die surface) and lower die (or lower die surface) of the mold only during the cutting process.

[0060] For example, in the case where the cutting step or blanking step is included, in the cutting step (or blanking step), the strip material fed into the processing device can be controlled so that it descends from the material transport height level to the press bottom dead point without contacting the notched upper die (or blanking upper die) and the strip material comes into contact with the notched upper die and the notched lower die (or the blanking upper die and the blanking lower die) only during the cutting process.

[0061] Alternatively, if all of the above cutting and blanking steps are included, the cutting step can be performed in the same manner as described above, followed by the blanking step, except that it presupposes a cut-out material.

[0062] According to one aspect of the present invention, in the notching step (or blanking step), when the strip material is raised after the cutting process, the strip material can be separated from the notching (or blanking) lower die and raised to the transfer height level of the strip material without contacting the notching (or blanking) upper die, similar to the above-mentioned lowering step. In this way, by controlling the notching (or blanking) upper die and the notching (or blanking) lower die to come into contact with the strip material only at the time of cutting the strip material in the notching step (or blanking step), excessive cooling in the notching step (or blanking step) can be suppressed, thereby ensuring easy formability in the subsequent forming step.

[0063] 1 showing an exemplary multi-stage hot press forming apparatus of the present invention, when only the notch die is included among the notch die and the blanking die, a notch upper die 61a and a notch lower die 61b are shown, and when only the blanking die is included, a blanking upper die 61a and a blanking lower die 61b are shown. However, the drawings of the case where both the notch die and the blanking die are included are omitted.

[0064] In the above-mentioned notching and blanking steps, there may be various methods for the strip material to come into contact with the upper and lower dies of the die only during the cutting process. For example, as shown in Fig. 14, a push bar 11 operated by a spring may be provided as a protruding structure on the surface of the notching upper die (or blanking upper die) that contacts the strip material. In this case, the push bar may be disposed on the surface of the notching upper die (or blanking upper die) that contacts the strip material so as to correspond to the portion that will be removed from the material during the subsequent process.

[0065] That is, according to one aspect of the present invention, the push bar 11 can lower and raise the notched upper die (or blanking upper die) while pushing the blank 200 so as to contact a portion of the blank 200 that will be removed in a subsequent process. Thus, when the press is lowered and raised, the surface of the notched upper die (or blanking upper die) that contacts the strip material can be controlled so as not to contact the strip material in an area other than where the push bar is provided. For example, the portion of the strip material that will be removed in a subsequent process can correspond to a guide bar or guide pin that guides the strip to transport the strip.

[0066] Meanwhile, according to one aspect of the present invention, the inventors have further discovered that as the time during which the processing device remains near the bottom dead center of the press (i.e., the maintenance time near the bottom dead center of the press) becomes longer, the time for the upper and lower dies of the mold to close increases, and thus the cooling rate of the material can also be increased.

[0067] Figure 3 shows the stroke of the slide along the crank angle in the operation method of the exemplary mechanical press motion of the present invention. Figure 3(a) corresponds to a general crank motion method, and Figure 3(b) corresponds to other motion methods such as link, knuckle, servo, etc. It can be seen that there is a difference in the maintenance time of the slide near the bottom dead center depending on the above-mentioned method, and in the case of the motion method of Figure 3(b), the proportion of the maintenance time near the bottom dead center is higher than that of the motion method of Figure 3(a).

[0068] Therefore, according to one aspect of the present invention, the press motion of the processing device may be performed by any method selected from the group consisting of a link motion method, a knuckle motion method, and a servo motion method, but is not limited thereto.

[0069] Alternatively, according to one aspect of the present invention, the press motion of the processing device may have a maintenance time ratio near the bottom dead center within one stroke of 4 to 30%, more preferably 10 to 30%, where the maintenance time ratio near the bottom dead center means the ratio of time the press stays at a point 1 mm upward from the bottom dead center.

[0070] According to one aspect of the present invention, when the ratio of the above-mentioned maintenance time is 4% or more, the minimum die contact time for cooling is ensured, thereby preventing an increase in the number of processes for ensuring physical properties. In addition, this prevents an increase in the final part extraction time, ensures the critical cooling rate, and easily ensures the desired physical properties. In addition, when the ratio of the above-mentioned maintenance time is 30% or less, unnecessary maintenance time near the bottom dead center is reduced, thereby ensuring sufficient process time for the up and down movement of the press slide and the transport of the strip, thereby ensuring a stable process.

[0071] According to one aspect of the present invention, one or more of the notching and blanking steps may be performed in one step or may be divided into two or more steps to be performed in a multi-step process.

[0072] According to one aspect of the present invention, the method may further include a molding step of transferring a material that has undergone one or more of the cutting step and the blanking step and positioning it near the molding die, and then molding the material using the molding die (i.e., by mating an upper mold and a lower mold of the molding die).

[0073] According to one aspect of the present invention, the molding step may be performed in one step or may be performed in two or more steps as a multi-step process.

[0074] According to one aspect of the present invention, although not particularly limited thereto, in the above-mentioned molding step, the molding step may be performed in a multi-step process of two or more steps so as to form an undercut shape (the contents described below apply equally to the undercut shape).

[0075] According to one aspect of the present invention, when the above-mentioned molding step is performed in a multi-step process of two or more steps, the molding direction of the material in any one molding step may be different from the molding direction of the material in the other molding steps. For example, the molding direction of the material in the first molding step may be different from the molding direction of the material in the additional molding step for forming an undercut shape after the first molding step. In this case, the molding directions being different from each other means that they are not parallel.

[0076] As a non-limiting example of the present invention, a burring portion may be formed in a forming direction perpendicular to the surface of the material in a first forming step, and then a bending process may be performed on the material in a forming step after the first forming step (e.g., a second forming step). At this time, the bending process may be performed so as to be at an angle of 90° or less with respect to the forming direction in the first forming step, so that the forming direction in the first forming step and the forming direction in the second forming step may be different from each other.

[0077] In this case, according to one aspect of the present invention, since the burring portion cannot be cooled by additional die contact after a single bending process, the process can be designed so that the bending process is performed after sufficient cooling is performed when the burring portion is formed in the molding stage.

[0078] That is, according to one aspect of the present invention, a material is processed in a primary molding step to form a molded portion such as a burring portion, and a bending process is performed on the material in a post-primary molding step to form a bent portion (i.e., a portion formed by connecting a flat portion and a side portion) as described below in the material.

[0079] Meanwhile, as another non-limiting example of the present invention, a material may be molded in a first molding step using a molding die to include a flat portion A having a first surface direction S based on the surface of the material and a side portion B having a second surface direction P different from the first surface direction. Then, in a molding step after the first molding step (e.g., a second molding step), pressure may be applied to the side portion to mold the material to include a portion in which the angle D between the first surface direction S and the second surface direction P is within 90°.

[0080] According to one aspect of the present invention, by including a forming step performed in two or more processes in which the forming directions are different from each other as described above, it is possible to provide a hot press-formed part having an undercut shape as described below.

[0081] That is, by including a forming step performed in a multi-step process of two or more steps according to one aspect of the present invention, it is possible to easily form an undercut shape that could not be produced by a conventional technique in which the forming step is performed in a single step. Therefore, according to the present invention, even if the final product includes the above-mentioned undercut shape, it is possible to easily produce a formed part having an overall tensile strength of 1,300 MPa or more by applying a hot press forming method.

[0082] According to one aspect of the present invention, when the notching step or blanking step is included, when the notching die or blanking die is transferred to the vicinity of the molding die, the notched material (or blanking material) may be transferred by the designed pitch amount from the notching die (or blanking die) to the vicinity of the molding die in accordance with the designed pitch amount between the molding die and the notched die (or blanking die). In this case, the vicinity of the molding die may refer to the space where molding is performed between the upper molding die and the lower molding die.

[0083] According to one aspect of the present invention, the forming step may be followed by one or more of a piercing step of removing unnecessary portions such as holes from the formed material and a flanging step of forming a flange from the formed material. That is, one or more of the piercing step and the flanging step may be provided between the forming step and a trimming step described below.

[0084] That is, according to one aspect of the present invention, in the piercing step, the molded material is transferred and positioned near the piercing die, and then unnecessary portions such as holes can be removed from the molded material using the piercing die (i.e., by mating an upper mold and a lower mold of the piercing die). In this case, the vicinity of the piercing die may refer to a space where piercing is performed between the upper piercing die and the lower piercing die.

[0085] In addition, in the flanging step, the molded material (or the piercing step and the flanging step are both included, and in this case, the term "pierced material" refers to a material that has been pierced in sequence) is transferred and positioned near the flanging die, and then the pierced material is processed to form a flange portion using the flanging die (i.e., by mating an upper mold and a lower mold of the flanging die). In this case, the term "near the flanging die" may refer to the space where flanging is performed between the upper flanging die and the lower flanging die.

[0086] Meanwhile, according to one aspect of the present invention, when all of the above-mentioned piercing and flanging steps are included, the order of the piercing and flanging steps is not particularly limited as long as they are performed between the molding step and the trimming step, and piercing-flanging may be performed in that order, or flanging-piercing may be performed.

[0087] According to one aspect of the present invention, when a material is transferred from the vicinity of a molding die to the vicinity of a piercing die (or a flanging die), the molded material can be transferred by a designed pitch amount so as to correspond to the pitch amount designed between the molding die and the piercing die (or the flanging die) and placed in the vicinity of the piercing die (or the flanging die). Meanwhile, when the material is transferred from the piercing die to the flanging die in a manner similar to the above-mentioned method, in a case where both the piercing step and the flanging step are included, the material can be transferred in the same manner as the above-mentioned method.

[0088] According to one aspect of the present invention, one or more of the piercing and flanging steps may be performed in one step, or may be divided into two or more steps to be performed in a multi-step process, or one or more of the piercing and flanging steps may be omitted as necessary.

[0089] According to one aspect of the present invention, a trimming step can be included in which an unnecessary peripheral portion of the material is removed from the final product shape using the trimming die, and a material having a desired product shape can be finally obtained by such a trimming step.

[0090] According to one aspect of the present invention, in the trimming step, a molded material (however, in the case where one or more of the above-mentioned piercing and flanging steps are further included, this means a material that has undergone one or more of the piercing and flanging steps) is transferred and positioned near the trimming die, and unnecessary peripheral parts are removed from the material using the trimming die, thereby manufacturing a material having a final product shape. Here, the trimming step may be performed by mating the upper and lower dies of the trimming die with respect to the material transferred near the trimming die (the space where trimming is performed between the upper and lower trimming dies).

[0091] According to one aspect of the present invention, when transferring the material from the molding stage to the trimming stage, the material can be transferred from the die in the previous stage (previous stage) to the vicinity of the die in the subsequent stage (following stage) by a designed pitch amount, so as to correspond to the pitch amount designed for two dies adjacent to each other in the transfer direction of the material.

[0092] According to one aspect of the present invention, the trimming step may be performed in one step or may be divided into two or more steps to be performed as a multi-step process.

[0093] According to one aspect of the present invention, one or more of the notching and blanking steps, the forming step, and the trimming step (including the above-mentioned piercing and flanging steps when the step further includes one or more of the above-mentioned steps) may be divided into two or more steps and performed as a multi-stage process. By performing each step in a multi-stage process, not only can the moldability be improved more than when each step is performed in a single process, but the effect of preventing cracks in the final product can be improved by reducing the thickness reduction rate in each step.

[0094] According to one aspect of the present invention, the method may further include a step of cooling the trimmed product in its final shape to room temperature.

[0095] Furthermore, according to one aspect of the present invention, one or more of the notching step and blanking step, the molding step, and the trimming step (including the above-mentioned piercing step and flanging step when the molding step further includes one or more of the above-mentioned steps) may further include a step of cooling the mold. For example, when the molding step is performed in a multi-step process by dividing it into two or more steps, the secondary molding step may further include a step of cooling the secondary molding mold.

[0096] Meanwhile, in a conventional hot press forming method, forming is completed in one process, and immediately after forming, the material is quenched while being maintained in the same mold for a certain period of time to ensure strength, whereas in the technology of the present invention, cooling is performed through multiple steps such as notching, blanking, forming, piercing, flanging, and / or trimming.

[0097] Here, according to one aspect of the present invention, as a result of thorough investigation into whether the physical properties of a material can be ensured through the above-mentioned multi-stage process, the inventors further discovered that the cooling speed of a material, which can determine whether the physical properties of the material can be ensured, can be determined by the pressing speed (SPM), the number of processes until the final product is removed, the maintenance time near the bottom dead center to close the upper and lower dies in one process, and the relational equation of the slide stroke, etc.

[0098] That is, according to one aspect of the present invention, a multi-stage process can be carried out with a number of steps equal to or greater than the minimum number of steps determined by the following relational expression 1. This makes it possible to obtain a product having desired physical properties. [Equation 1] N=ROUNDUP{T / [(60 / SPM)×(f / 100)]} (In the above Relational Formula 1, N represents the minimum number of steps required from the forming stage excluding the notching step and the blanking step, SPM stands for strokes per minute (SPM) of the press. f is the percentage of time that the stroke is maintained near the bottom dead center, T is a value calculated from the following relational expression 2 when 0.8≦t<1.5, and is a value calculated from the following relational expression 3 when 1.5≦t, ROUNDUP indicates the value in {} rounded up to the nearest integer.) [Equation 2] T=t [Equation 3] T = 5 × t-6 (In the above relations 2 and 3, t is the thickness of the material, and its unit is mm.)

[0099] Moreover, according to one aspect of the present invention, when the above f satisfies 0.8≦t<1.5, it satisfies the following relational expression 4, and when the above f satisfies 1.5≦t, it satisfies the following relational expression 5. [Equation 4] 0.8×t+2.6≦f [Equation 5] 4.4×t-2.8≦f (In the above relations 4 and 5, t is the thickness of the material, and its unit is mm.)

[0100] According to one aspect of the present invention, the thicker the material is, the more difficult it is to cool it, and therefore the longer the contact time with the die is required. Therefore, the thicker the material is, the greater the pressing motion that has a higher maintenance rate at the bottom dead center can be selected.

[0101] Alternatively, according to one aspect of the present invention, the contact time with the die can be approached by increasing the number of steps, but too many steps with little die contact in one step increases the possibility of different phases occurring as the air cooling time increases. Therefore, most preferably, the proportion of time that the press slide remains near the bottom dead center in one step needs to be increased. In addition, the contact time with the die is influenced not only by the proportion of time that the slide remains near the bottom dead center, but also by the time required for one step, i.e., the press motion speed (SPM).

[0102] Therefore, according to one aspect of the present invention, a multi-stage process is performed with more than the minimum number of steps calculated from the above relational expression 1, and the minimum f value according to the material thickness expressed by the above relational expressions 4 and 5 is ensured, thereby obtaining a final product with the desired strength.

[0103] According to one aspect of the present invention, it is necessary to suppress cooling of the material in the notching and blanking steps, while accelerating cooling in the multi-step process after the notching and blanking steps (i.e., from the molding step) to ensure a temperature of Ms or less in the final product. Therefore, it is necessary to increase the contact time with the mold for fast cooling, and the following method can be used to achieve this.

[0104] In a typical progressive method, the position of the strip material rises in conjunction with the rise of the press upper die, and it waits for transfer to the next stage. However, in this case, the molded product (or material) is cooled by contacting the upper and lower dies of the die only while the press slide remains near the bottom dead center, and as the press slide rises, the molded product also rises and separates from the upper and lower dies of the die, so it is only cooled to the air cooling level.

[0105] Here, the inventors have intensively studied a preferred embodiment of the multi-stage process, and as a result, since the strip material is not transferred while the slide upper plate (press slide) is rising, the press slide rises from the press bottom dead point to a certain height level, and the material (or formed product) can be kept near the press bottom dead point until the strip material reaches the transfer stage, as shown in Figures 15 to 17. In this way, when the press slide rises, the material is kept near the press bottom dead point, and then the position information of the press slide is used to raise the material just before the strip transfer stage, and it has been further discovered that faster cooling can be ensured.

[0106] 15 to 17 show the press motion of an exemplary processing device 41 of the present invention. That is, according to one aspect of the present invention, as shown in FIG. 15, when a material is input to the processing device 41, the press slide 6a descends to the press bottom dead point 120b to process the material. Next, as shown in FIG. 16, the material remains near the press bottom dead point 120b while the press slide 6a is rising. Finally, as shown in FIG. 17, by utilizing the position information of the press slide, when the press slide rises to a point 120a where it does not interfere with the transfer of the material, a method can be applied in which the material located near the press bottom dead point 120b is raised.

[0107] According to one aspect of the present invention, the method of lifting the workpiece described above is shown in FIG. 17. Specifically, when the press slide 6a is lifted and reaches a point 120a where the transfer of the workpiece does not interfere, the workpiece can be lifted from near the bottom dead point of the press to the transfer point 120a by a cylindrical workpiece position control unit 600 that controls the workpiece to separate from the lower dies 61b, 62b, 63b, and 64b of the dies used in each stage.

[0108] At this time, according to one aspect of the present invention, the material position control unit 600 may be provided on the surface of the press lower plate (i.e., the press bolster) on the side where the die is provided. More specifically, the material position control unit 600 may be provided on both ends of one die (i.e., any one of the lower dies 61b, 62b, 63b, and 64b) in the material transfer direction. Alternatively, as shown in FIG. 17, one material position control unit 600 may be provided between two adjacent dies.

[0109] According to one aspect of the present invention, when the molding step is performed in two or more steps, in order to prevent the molded part from being excessively cooled and cracking from occurring, the molding step may further include a step of heating one or more additional molding dies other than the primary molding die used in the primary molding step.

[0110] Alternatively, according to one aspect of the present invention, one or more of the piercing and flanging steps and / or the trimming step may further include a step of heating one or more dies in each step to prevent cracks from occurring due to excessive cooling of the processed area.

[0111] The three-dimensional structure of the material after passing through the multi-stage process according to the exemplary progressive method of the present invention is shown in FIG. 12(a). Specifically, the cut-out material 210 after passing through the notch stage as the first process has a shape connected to the strip by the web portion 300. Next, the molded material 220 after passing through the molding stage as the second process forms a three-dimensional structure. At this time, a side view of the three-dimensional structure is shown in FIG. 12(b). Also, the shape of the pierced material 230 after passing through the piercing stage as the third process is shown, and unnecessary holes are removed from the material. Also, the shape of the trimmed material 240 after passing through the trimming stage as the fourth process is shown, and unnecessary peripheral portions 400 are removed by performing the trimming stage. By performing all the above-mentioned processes, the final product (250 in FIG. 11) taken out of the processing device is obtained.

[0112] In addition, although not shown in the drawings, in the case of including a blanking step of obtaining a blanking material separated from the strip by a transfer method described below, the material may be processed in the same manner, except that a blank separated from the strip so as not to include the strip web portion is formed and then the subsequent process is performed in the same manner as in the above-mentioned Fig. 12. In this case, the shape of the material may be formed in the same manner as in the case of using a conventional method in the art.

[0113] Meanwhile, according to one aspect of the present invention, in the progressive method, a material guide portion is formed in the web portion 300 and is operated to transport the material. The strip web portion 300 is a portion that is not actually molded and is removed from the final product shape in the trimming step. Therefore, the web portion 300 is heated to a low temperature during the processing process or cooled faster than the portion of the material that is processed in the cutting step, thereby enabling smooth transport of the material.

[0114] That is, according to one aspect of the present invention, in the cutting step, the web portion of the material can be cooled faster than the formed portion of the material.

[0115] Alternatively, according to one aspect of the present invention, in the cutting step, the web portion of the material can be controlled to a lower temperature than the molding portion of the material. In this manner, in order to control the temperature of the web portion of the material to be lower than the other portions, only a portion of the cutout mold that corresponds to the web portion of the material can be controlled to a lower temperature than the other portions.

[0116] In addition, in the hot press forming method for multi-step processes according to one aspect of the present invention, it is required to rapidly heat the strip material to achieve uniform heating, and to minimize the contact time with the die in one or more of the notching and blanking steps for the high-temperature strip material, thereby minimizing temperature drop. Meanwhile, in the forming step, piercing step, flanging step, trimming step, etc. after one or more of the notching and blanking steps (however, one or more of the piercing and flanging steps may be omitted), it is required to maximize the contact time of the material with the die to ensure fast cooling. In this way, when the conflicting requirements are carried out to the final step in a progressive manner, one or more of the notching and blanking steps, and the forming step, piercing step, flanging step, and trimming step are all carried out at the same transfer point, making it difficult to achieve different goals.

[0117] Here, as a result of intensive research, the inventors have further discovered that, in order to satisfy the above-mentioned conflicting requirements in each step, using the progressive method has many advantages in the heating step, the notching step, and the blanking step, and that using the transfer method in the molding step, the piercing step, the flanging step, and the trimming step allows for longer control of contact with the mold.

[0118] According to one aspect of the present invention, it has been confirmed that applying a composite method in which the heating step, the notching step, and the blanking step are performed in a progressive manner, and the molding step, the piercing step, the flanging step, and the trimming step are performed in a transfer manner, is more advantageous in ensuring physical properties.

[0119] That is, according to one aspect of the present invention, the multi-stage hot press forming method includes a blanking step in which the blanking die is used to cut a portion of the heated strip material fed into the processing device to obtain a blank material separated from the strip, and a transfer method using a pincer-shaped transfer means can be applied when transferring the material from the die in the previous stage (previous stage) to the vicinity of the die in the subsequent stage (following stage) based on two dies adjacent to each other in the material transfer direction in one press.

[0120] For example, when transferring a material from a blanking stage to a forming stage, and when transferring a material from a forming stage to the next stage (piercing stage, flanging stage or trimming stage), a pliers-like transfer means can be used to transfer the material located near the die of the previous stage to the vicinity of the die of the next stage.

[0121] [Manufacturing equipment for hot press forming parts for multi-stage processes] Another aspect of the present invention is A feed section for continuously feeding strip material; A heating section for heating the supplied strip material; A processing section including a processing device to which a number of dies including one or more of a notch die and a blanking die, a molding die, and a trimming die are attached to one press; and a transfer section for transferring the strip material heated in the heating section to the processing section; The present invention provides a multi-stage hot press formed part manufacturing apparatus, comprising:

[0122] In addition, the above-mentioned description of the manufacturing method for the multi-stage hot press-formed part can be applied to the manufacturing apparatus for the multi-stage hot press-formed part.

[0123] Specifically, the structure of an exemplary multi-stage hot press-formed part manufacturing apparatus of the present invention is shown in Figure 1, and the multi-stage hot press-formed part manufacturing apparatus 100 includes a supply section 1; a heating section 2; a transfer section 3; and a processing section 4.

[0124] According to one aspect of the present invention, the supply unit 1 continuously supplies the strip material 200. In this case, the supply unit 1 can continuously supply the coiled material 10 to the heating unit 2 in the form of a strip material having a uniform width by an uncoiler.

[0125] According to one aspect of the present invention, the heating section 2 can heat the strip material supplied from the supply section by using the heating device 21. In this case, the rapid heating method described above can be applied, and various rapid heating devices such as high-frequency heating, electrical heating, and infrared heating can be used.

[0126] According to one aspect of the present invention, the transfer unit 3 can transfer the strip material 200 heated in the heating unit 2 to the processing unit 4. At this time, the transfer of the strip material 200 can be performed within a heat-retaining chamber 31. Meanwhile, the above description can be similarly applied to the heat-retaining chamber.

[0127] According to one aspect of the present invention, the processing unit 4 may include a processing device 41 in which one or more dies 61a, 61b of a notching die and a blanking die, a forming die 62a, 62b, and a trimming die 64a, 64b are attached to one press 6; 6a, 6b. Meanwhile, as described above in the molding method, one or more dies of a piercing die and a flanging die may be further attached between the forming die and the trimming die.

[0128] According to one aspect of the present invention, the single press 6 may include a press slide corresponding to the upper plate 6a of the press and a press bolster corresponding to the lower plate 6b of the press. In this case, the lower plate 6b of the press may be provided to correspond to the upper plate 6a of the press.

[0129] According to one aspect of the present invention, the processing device 41 may further include separate mold temperature controllers 5a and 5b for controlling the temperature of each of the above-mentioned molds, and the mold temperature controllers may be provided between the molds and the press, that is, on the press side in contact with each mold.

[0130] According to one aspect of the present invention, when a heated die is used for the notch die and / or the blanking die, a separate temperature controller 51a, 51b for the notch die and / or the blanking die for controlling the temperature of the die may be included. In this case, the temperature controller 51a, 51b may be provided between the die 61a, 61b and the press 6a, 6b.

[0131] Furthermore, according to one aspect of the present invention, a temperature control section for each die can be provided between each die and the press, similar to the method described above (for example, temperature control sections 52a, 52b of the molding die, temperature control sections 53a, 53b of the piercing die or flanging die, temperature control sections 54a, 54b of the trimming die; see FIG. 1(b)).

[0132] According to one aspect of the present invention, as described above, the notch upper die or the blanking upper die may be provided with a spring-operated push bar 11 as a structure protruding from the surface of the side that contacts the strip material (see FIG. 14). Meanwhile, the above description can be applied to the push bar in the same manner.

[0133] According to one aspect of the present invention, as described above, a cylindrical material position control unit 600 can be provided on the surface of the press lower plate (i.e., the press bolster) on the side where the die is provided. The above description can be applied to the material position control unit 600 in the same manner.

[0134] According to one aspect of the present invention, the processing device may include blanking dies as the multiple dies, and may further include a pliers-like transfer means for transferring the material from a previous stage die to the vicinity of a subsequent stage die based on two dies adjacent to each other in a transfer direction of the material in one press. In this case, the pliers-like transfer means is an example in which a transfer method is applied, and the above description may be similarly applied.

[0135] In addition, since the manufacturing device for a hot press-formed member for multi-stage processes according to one aspect of the present invention can be similarly applied to the above-mentioned manufacturing method for a formed member, it is possible to use, for example, a processing device that can perform multi-stage processes with more than the minimum number of processes calculated from the above-mentioned Relational Formula 1. For example, in the above-mentioned processing device, the number of multiple dies attached to one press can be more than the minimum number of processes calculated from the above-mentioned Relational Formula 1. Alternatively, it is possible to use a processing device that satisfies the above-mentioned Relational Formulas 4 and 5 by utilizing information on the thickness (corresponding to t in Relational Formulas 4 and 5) of the material fed into the processing device.

[0136] [Hot press forming parts] Another aspect of the present invention is As a hot press-formed part manufactured by the above-mentioned method for manufacturing a hot press-formed part for multi-stage processes, Provided is a hot press formed part that includes an undercut shape and has a tensile strength of 1300 MPa or more.

[0137] According to one aspect of the present invention, the undercut shape has the same meaning as the term used in the art. Therefore, the undercut shape may include various shapes that are commonly interpreted in the art. For example, the molded shape of the hot press molded part may include a convex or concave part on the side, or a burring part or the like formed on the side, so that the molded product cannot be molded or removed by vertical movement of the mold alone.

[0138] As a non-limiting example of the present invention, various forms of the hot press-formed member are shown in FIG. 18. The hot press-formed member according to one aspect of the present invention may include a planar portion A having a first surface direction S, and a side portion B having a second surface direction P different from the first surface direction. In this case, the hot press-formed member may have one or more planar portions and / or one or more side portions. Meanwhile, the hot press-formed member may have any planar portion A and any side portion B connected to each other, and since the planar portion A and the side portion B have different surface directions, the planar portion A and the side portion B may be connected to each other to provide a bent portion.

[0139] For example, in the case of a hat shape as shown in FIG. 18, a first side portion and a second side portion may be connected to both ends of one flat portion, respectively (i.e., a first side portion may be connected to one end of both ends of the one flat portion, and a second side portion may be connected to the other end). Also, an additional first flat portion may be connected to an end of the first side portion other than the side connected to the flat portion, and an additional second flat portion may be connected to an end of the second side portion other than the side connected to the flat portion (however, this is not limited thereto, and additional flat portions and / or side portions may be further included). Thus, as a non-limiting example of the present invention, the hot press formed member may be composed of three flat portions A and two side portions B as shown in FIG. 18.

[0140] On the other hand, a non-limiting example of an undercut shape of the present invention may include a portion in which the narrower angle D formed by the first surface direction S of any planar portion A and the second surface direction P of any side portion B is within 90°, as shown in the side view of the molded member in (b) of Figure 18.

[0141] Alternatively, as yet another non-limiting example of the undercut shape of the present invention, as shown in the perspective view of the molded member in Fig. 18(a), one or more of any of the flat portions A and any of the side portions B may include an additional molded portion C (e.g., including a burring portion, etc.). In this case, the molded member may include a bent portion formed by connecting any of the flat portions A and any of the side portions B. Therefore, the molded portion C may also be provided on the surface of the side portion in the second surface direction.

[0142] According to one aspect of the present invention, the undercut shape may be manufactured by a manufacturing method in which the above-mentioned molding step is performed in a multi-step process of two or more steps, and a molding direction of the material in one molding step is different from a molding direction of the material in another molding step. Specifically, the undercut shape may mean including two or more parts having different molding directions, and in this case, the above description of the molding direction may be applied in the same manner.

[0143] For example, as described above, when a burring portion is formed in the primary molding step and then bending is performed in the secondary molding step, since the molding directions in the primary molding step and the secondary molding step are different from each other, an undercut shape that cannot be formed when the molding step is performed in a single process can be formed.

[0144] Alternatively, in another example, the material may be processed to include a flat portion and a side portion in the first molding step, and then pressure may be applied to the material in a direction perpendicular to the surface of the side portion in the second molding step, forming an undercut shape in which the angle between the flat portion and the side portion is within 90°.

[0145] Meanwhile, according to one aspect of the present invention, the hot-formed part may have an overall tensile strength of 1,300 MPa or more even if it includes an undercut shape, and the upper limit is not particularly limited because the higher the strength characteristics, the better the properties are. However, as a non-limiting example, the upper limit may be 2,000 MPa.

[0146] (Example) The present invention will be described in more detail below with reference to examples. However, it should be noted that the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention, as the scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.

[0147] (Experimental Example 1) Strip materials with a constant width and blank materials with variable widths were prepared, and each material was subjected to electrical heating at a heating rate of 50°C / s. The material used was an alloyed plated steel sheet with an Fe content of 30 wt% at the surface of the plated layer (within 2 μm from the surface of the plated layer) obtained by alloying a base steel sheet with a composition (by weight) of C: 0.22%, Si: 0.3%, Mn: 1.2%, Cr: 0.2%, Al: 0.03%, P: 0.01%, S: 0.001%, N: 0.003%, B: 0.003%, with the balance being Fe and other unavoidable impurities, by immersing the plated steel sheet in a plating bath of Al-Si9%-Fe3%.

[0148] The temperature distribution result when the strip material with a constant width was electrically heated is shown in Figure 2(a) as Example 1, and the temperature distribution result when the strip material with a non-constant width was electrically heated is shown in Figure 2(b) as Comparative Example 1.

[0149] As can be seen by comparing the temperature distribution results in Figure 2 above, in Comparative Example 1, a larger temperature difference occurred between the narrow and wide areas of the material as shown in Figure 2(b) compared to Figure 2(a). Therefore, in the case of Example 1 using a strip material with a constant width as shown in Figure 2(a), it was confirmed that more uniform heating could be easily performed by applying rapid heating compared to Comparative Example 1 using a blank with an inconsistent width.

[0150] (Experimental Example 2) A prepared strip material having a thickness of 1.4 mm was rapidly heated to 920°C at a heating rate of 50°C / s using an electric heating method in which the effective length of the heating device was 2 m and the cycle time was 4 seconds. The strip material was the same alloyed plated steel sheet used in the above Experimental Example 1. The heated strip material was then passed through a heating chamber at 900°C and transferred to a processing device. The transferred strip material was operated at 15 SPM using a press motion of the crank motion type shown in FIG. 3(a). Example 2 was a case in which a notch was made using a cold notch die with an initial temperature of 25°C, and Example 3 was a case in which a notch was made using a heated notch die with an initial temperature of 500°C. A graph of the temperature change of the material over time in the notch stage for Examples 2 and 3 is shown in FIG. 4 below.

[0151] In the case of Example 2, by using a cold notch die, the material was cooled very quickly from the time when the notch upper die descended and made contact. Meanwhile, in the case of Example 3, by using a heated notch die with an initial die temperature of 50°C or more, excessive cooling was suppressed when the notch upper die descended and made contact with the material. That is, in Example 3, by suppressing excessive cooling compared to Example 2, the temperature of the material after the notch step was controlled to 700°C or more. As a result, the elongation rate of the material after the notch step was 50% or more, which was ensured at a level that allowed the molding process to be performed in the subsequent process, and it was confirmed that the moldability in the subsequent process was superior.

[0152] (Experimental Example 3) A strip material having a thickness of 1 mm was used, and the strip material was processed in the same manner as in Experimental Example 2 described above, except that the temperature of the initial notch die was changed as shown in Table 1 below. At this time, the surface temperature of the material was measured based on the point at which the contact of the notch die with the material ended during the notching stage, and the results are shown in Table 1.

[0153] Meanwhile, in order to confirm the effect of the temperature of the notch mold on the possibility of further molding, the elongation of the material obtained after the notch step was measured, and the possibility of further molding was evaluated according to the following criteria. ×: Elongation rate less than 50% ○: Elongation rate 50% or more

[0154] In this case, in Comparative Example 2, when the blank itself, rather than the strip material, was rapidly heated, the surface temperature of the material was measured and shown in Table 1 below, and the possibility of further forming was measured in the same manner as described above.

[0155] Further, the temperature uniformity for the material was measured in the same manner as in the above-mentioned Experimental Example 1, and was evaluated according to the following criteria. ×: When the temperature difference generated by the material is 50℃ or more ○: When the temperature difference generated by the material is less than 50℃

[0156] [Table 1]

[0157] As shown in Table 1 above, in Comparative Example 2, a high surface temperature of the material was ensured by heating the blank itself, but due to the uneven temperature distribution caused by the shape of the blanking material having an inconsistent width, there were parts where the temperature of the material after the blanking stage was too low, making further forming impossible.

[0158] On the other hand, in the cases of Examples 4 to 11 in which the strip material was rapidly heated, it was confirmed that the temperature uniformity of the material was superior to that of Comparative Example 2 above.

[0159] On the other hand, in Examples 8 to 11, in which the initial temperature of the notch die was 400°C or higher, the temperature of the material after notching was higher than in Examples 4 to 7, in which the initial temperature of the notch die was less than 400°C, and the desired level of elongation could be secured, thereby enabling further molding.

[0160] (Experimental Example 4) The strip material was notched in the same manner as in Experimental Example 2, except that a link-type press motion as shown in Fig. 3(b) was used, and a push bar was provided on the surface of the notch upper die that contacts the strip material and controlled to operate with a spring so that the notch upper die and the notch lower die would come into contact with the strip material only in the cutting process at the notch stage. Example 12 shows a case where the initial temperature of the notch die was 25°C, and Example 13 shows a case where the initial temperature of the notch die was 500°C, and a graph of the temperature change of the material over time at the notch stage is shown in Fig. 5.

[0161] Meanwhile, by comparing Figures 4 and 5, it was confirmed that in Examples 12 and 13, the cooling of the material was significantly reduced as the contact time with the notched upper die was reduced compared to Examples 2 and 3. In this way, when the press was lowered and raised, the notched upper die was lowered and raised without contacting the strip material, and the notched upper / lower dies were brought into contact with the strip material only during the cutting process, so that the surface temperature of the material after the notching step could be controlled to be higher. As a result, it was confirmed that a high elongation rate of the material of 50% or more could be secured, and better formability was confirmed in subsequent processes.

[0162] (Experimental Example 5) As a strip material having a thickness of 1.4 mm, a steel plate having the same composition as that used in the above-mentioned Experimental Example 1 was rapidly heated to 920°C at a heating rate of 50°C / s using an electric heating method. The heated strip material was then transferred to a processing device in a heat-retaining chamber at 900°C. The transferred strip material was operated at 15 SPM using a press motion that satisfied the motion method and the maintenance ratio near the bottom dead center in one stroke shown in Table 2 below, and the notching process, forming process, piercing process, and trimming process of the HAT-shaped part were performed. At this time, in the notching process, a notching die that satisfied the initial temperature in Table 2 below was used, and a push bar was used to control so that the notching upper die and the notching lower die came into contact with the strip material only in the cutting process.

[0163] For Examples 14 to 16 which met the experimental conditions in Table 2 below, the formability, the presence or absence of martensite (Ms) phase, and strength properties were evaluated, and the results are shown in Table 2 below.

[0164] In this case, the formability was evaluated according to the same criteria as in Experimental Example 3 described above, and the strength properties of the product were evaluated based on the forming and cooling analysis method that took into account the phase transformation of the material. When the martensite phase fraction of the final product was 99% or more and the tensile strength was 1,300 MPa or more, it was indicated with an "O" and when the martensite phase fraction of the final product was 90% or less, it was indicated with an "X".

[0165] [Table 2]

[0166] For Examples 14 to 16 in Table 2, the temperature changes of the materials over time during the multi-stage process are shown in Figures 6 to 8, respectively. At this time, the temperature changes of the materials are shown as temperature changes on the surface, based on the points that will become the parts in the final parts indicated by circles in Figures 6 to 8.

[0167] In the case of Comparative Example 3, in which the multi-stage process was carried out under the same conditions as in Examples 14 to 16, except for applying the conventional method of rapidly heating the blank material, the blank material had an uneven width, which resulted in uneven temperature distribution, resulting in the formation of areas where the temperature of the material was too low after the blanking stage, making further molding impossible.

[0168] Meanwhile, it was confirmed that Example 14 had better formability than Comparative Example 3. However, the contact time with the die was somewhat short, and as can be seen from Fig. 6, the cooling rate was low, so sufficient martensite of 99% or more was not secured.

[0169] On the other hand, in the case of Example 15, as can be seen from Fig. 7, the temperature drop is somewhat reduced in the 0 to 4 second section corresponding to the notching stage, and the formability is superior to that of Example 14. However, sufficient martensite of 99% or more was not secured because the contact time between the die and the formed product was somewhat short.

[0170] In addition, in the case of Example 16, as can be seen from FIG. 8, not only is there little temperature drop at the cutting stage, and the moldability is excellent, but the strength characteristics of the product are also excellent.

[0171] Specifically, in Example 16, the proportion of time during which the upper and lower dies of the die remained in a closed state at the bottom dead center of the press was higher than in Examples 14 and 15, ensuring a fast cooling rate of the material throughout the entire process. Therefore, after a total of 16 seconds of multi-stage processing, the temperature of the material was kept below 400°C, which is the Ms temperature, ensuring a critical cooling rate, and thus ensuring a sufficient martensite phase after the multi-stage processing, resulting in a product having desired strength characteristics.

[0172] (Experimental Example 6) In manufacturing the notched material manufactured by the method of Experimental Example 2, the case where the notching step was performed in a single step as shown in Figure 9(a) was taken as Example 17, and the thickness reduction rate at this time was shown in Figure 9(b). Similarly, the case where the notching step was performed in two steps as shown in Figure 10(a) was taken as Example 18, and the thickness reduction rate at this time was shown in Figure 10(b).

[0173] In the case of Example 18, by dividing the notching step into two steps, it was confirmed that the thickness reduction rate of the final part was reduced more than in Example 17, in which the notching step was performed in a single process, and thus the effect of preventing crack generation was superior.

[0174] (Experimental Example 7) For several thicknesses of material having the same composition as in Experimental Example 2 described above, the press movement speed SPM, the percentage of time that the slide remains near the bottom dead center in one process, whether the material extracted is kept below the Ms temperature depending on the variation in the minimum required number of processes from the forming stage excluding notching, whether a stable martensite phase is maintained, and the physical properties of the product are evaluated as shown in Table 3 below.

[0175] In this case, the formability was evaluated according to the same criteria as in the above-mentioned Experimental Example 2, and the presence or absence of the stable martensite phase was evaluated according to the same criteria as in the above-mentioned Experimental Example 5, with a martensite phase of 99% or more being evaluated as "OK" and a martensite phase of 90% or less being evaluated as "NOK." The product strength was evaluated as "OK" as mentioned above, and a tensile strength of 1300 MPa or more was evaluated as "○," and other cases were evaluated as "×."

[0176] [Table 3] JPEG0007554904000004.jpg144162

[0177] As shown in Table 3 above, in the case of Comparative Example 4 in which the conventional method of rapidly heating a blank material was applied, the temperature non-uniformity of the material generated in the heating step caused poor moldability and the physical properties of the final product were not ensured, despite the conditions being such that the physical properties could be ensured as seen in Example 20.

[0178] On the other hand, Examples 19, 21 to 23, 26, 29, 32 and 33 have superior formability compared to Comparative Example 4, but are smaller than the minimum f value calculated from the material thickness according to the above-mentioned Relational Formulas 4 and 5, and other phases are generated, so that physical properties could not be secured. Also, Examples 25, 28 and 34 satisfy the minimum f value calculated from the material thickness according to the above-mentioned Relational Formulas 4 and 5, but are smaller than the minimum number of steps (N) calculated from Relational Formula 1. As a result, the temperature could not reach below Ms when removed, and there was room for other phases other than martensite to be generated in the air-cooling process after removal under conditions of a temperature of Ms or higher. Therefore, when the above-mentioned Relational Formulas 4 and 5 are not satisfied or Relational Formula 1 is not satisfied, it was necessary to solve the problem by performing more steps than the minimum required steps (N) by adding a cooling process, etc., and then removing the product.

[0179] On the other hand, Examples 20, 24, 27, 30, 31, 35 and 36 are cases in which the minimum f value calculated from the material thickness according to the above-mentioned Relational Formulas 4 and 5 is satisfied, and a multi-stage process was carried out in which the number of steps (N) or more was equal to or greater than the minimum number of steps calculated from the above-mentioned Relational Formula 1. As a result, the temperature was kept below the Ms temperature when the material was removed from the multi-stage process, no phase other than martensite was generated, and a product with sufficient martensite phase was obtained, ensuring the physical properties of the final product.

[0180] (Experimental Example 8) In Examples 37 and 38, the blanking step was carried out in the same manner as in Experimental Example 2 described above, except that the blanking step was used to produce a blank material separated from the strip instead of the notching step, and then the forming, piercing, and trimming steps were carried out. In this case, a pliers-like transfer means was used when transferring the material between two dies adjacent to each other in the transfer direction.

[0181] In the case of Example 37, a cold blanking die with an initial temperature of 25°C was used, which allowed the material to cool very quickly, whereas in the case of Example 38, in which the initial temperature was 500°C, a heated blanking die was used, which prevented excessive cooling when the blanking upper die descended and came into contact with the material.

[0182] In other words, in Example 38, by suppressing excessive cooling compared to Example 37, the temperature of the blank material was 700°C or higher after the blanking stage was completed, and a material with an elongation rate of 50% or more was secured, and superior formability was confirmed in the subsequent processes after the blanking stage. [Explanation of symbols]

[0183] 100 Manufacturing equipment for hot press-formed parts for multi-stage processes 1 Supply section 10. Material arranged in coils 11 Push Bar 2 Heating section 21 Strip material heating device 3 Transfer section 31 Heating chamber 4 Processing section 41 Processing equipment 5a, 5b Mold temperature control section 50 Designed pitch amount X Direction of strip material transport 51a, 51b Temperature control section for notch die or blanking die 52a, 52b Temperature control unit of molding die 53a, 53b Temperature control section of piercing die or flanging die 54a, 54b Temperature control unit for trimming die 6 Press 6a Press top plate (press slide) 6b Press lower plate (press bolster) 61a, 61b Notch or blanking dies 62a, 62b Molding mold 63a, 63b Piercing or flanging dies 64a, 64b Trimming mold 110a Strip material transfer height level 110b Near the bottom dead center of the press slide 120a Location that does not interfere with the transport of materials 120b Near the bottom dead point of the press 200 Materials 210 Cut-out material 220 Molded Material 230 Pierced Material 240 Trimmed Material 250 Finished products taken out 300 Web Section 400 Unnecessary fringe 600 Material position control unit A flat part B Side part C Molded parts (burring parts, etc.) S 1st surface direction P 2nd surface direction D Narrow side angle between the first and second plane directions

Claims

1. a heating step for heating the strip material; A processing device in which a number of dies including one or more of a notching die and a blanking die, a forming die, and a trimming die are attached to one press, and a transfer step of transferring the heated strip material; a cutting step of cutting a part of the material using the cutting die to obtain a cut-out material connected to the web portion of the strip, and a blanking step of cutting a part of the material using the blanking die to obtain a blank material separated from the strip; a molding step of transferring the blank that has been subjected to one or more of the notching step and the blanking step, positioning the blank near the molding die, and molding the blank using the molding die; and A trimming step of removing a peripheral portion of unnecessary material from a final product shape using the trimming die; When a material is fed into the processing device, the press slide descends to the press bottom dead point to process the material, and then while the press slide is rising, the material remains near the press bottom dead point. Then, using position information about the press slide, when the press slide reaches a point where it does not interfere with the transfer of the material, the material positioned near the press bottom dead point is raised. This is a method for manufacturing a hot press-formed part for multi-stage processes.

2. 2. The method of claim 1, wherein the transport step is performed in a heat-retaining chamber in which the heated strip material is maintained at a temperature within a range of Ts-200°C to Ts+50°C based on a surface temperature (Ts) of the strip material fed to the heat-retaining chamber.

3. In the one press, two adjacent dies are arranged at an interval of a designed pitch between them in a material transfer direction, 3. The method for manufacturing a hot press-formed part for multi-stage processes according to claim 1 or 2, wherein the material is transferred in the material transfer direction by the designed pitch amount each time one stroke is performed by the press movement.

4. The method for manufacturing a multi-stage hot press-formed member according to any one of claims 1 to 3, wherein an initial temperature of the notch die and an initial temperature of the blanking die are 400°C or higher.

5. 5. The method for producing a hot press-formed part for multi-stage processes according to claim 1, wherein one or more of the notching step and the blanking step; the forming step; and one or more of the trimming step are divided into two or more steps and performed in a multi-stage process.

6. 6. A method for manufacturing a hot press-formed part for multi-stage processes according to claim 1, wherein in the notching and blanking steps, the strip material fed into the processing device is controlled so that it descends from the transfer height level of the strip material to the press bottom dead point without contacting the upper die of the die, and the strip material comes into contact with the upper and lower die surfaces of the die only in the cutting process.

7. The press motion of the processing device has a maintenance time near the bottom dead center within one stroke of 4 to 30%; 7. The method for producing a hot press-formed part for multi-stage processes according to claim 1, wherein the proportion of the maintenance time near the bottom dead center is the proportion of the time the press remains at a point 1 mm above the bottom dead center of the press.

8. 8. The method for manufacturing a multi-stage hot press-formed part according to claim 1, further comprising, between the forming step and the trimming step, one or more steps of a piercing step for removing unnecessary holes from the formed material and a flanging step for forming a flange portion from the formed material.

9. The method for producing a hot press-formed member for multi-stage processes according to any one of claims 1 to 8, wherein the multi-stage processes are performed with a minimum number of steps or more obtained by the following relational expression 1. [Relationship 1] N=ROUNDUP {T / [(60 / SPM)×(f / 100)]} (In the above-mentioned relational expression 1, N represents the minimum number of steps required from the forming stage excluding the notching step and the blanking step, SPM stands for strokes per minute (SPM) of the press. f represents the percentage of time during one stroke that the stroke is maintained near the bottom dead center, T represents a value calculated from the following Relation 2 when 0.8≦t<1.5, and represents a value calculated from the following Relation 3 when 1.5≦t, ROUNDUP indicates the value in {} rounded up to the nearest whole number.) [Relationship 2] T = t [Relationship 3] T = 5 x t - 6 (In the above Relational Formulas 2 and 3, t is the thickness of the material, and is expressed in mm.)

10. The method for producing a multi-stage hot press-formed member according to claim 9, wherein f satisfies the following relational expression 4 when 0.8≦t<1.5 is satisfied, and satisfies the following relational expression 5 when 1.5≦t is satisfied. [Relationship 4] 0.8×t+2.6≦f [Relationship 5] 4.4×t−2.8≦f (In the above Relational Formulas 4 and 5, t is the thickness of the material, and is expressed in mm.)

11. A blanking step of cutting a part of the heated strip material introduced into the processing device using the blanking die to obtain a blank material separated from the strip, A method for manufacturing a multi-stage hot press-formed part according to any one of claims 1 to 10, wherein a pliers-shaped transfer means is used to transfer the material from the previous stage die to the vicinity of the next stage die based on two dies adjacent to each other in the material transfer direction in the one press.

12. a supply section for continuously supplying strip material; a heating section for heating the supplied strip material; A processing section including a processing device to which a number of dies including one or more of a notch die and a blanking die, a molding die, and a trimming die are attached to one press; and A transfer section that transfers the strip material heated in the heating section to the processing section; When a material is fed into the processing device, the press slide descends to the press bottom dead point to process the material, and then the material remains near the press bottom dead point while the press slide rises. Then, using position information about the press slide, when the press slide reaches a point where it does not interfere with the transfer of the material, the material positioned near the press bottom dead point is raised. This is an apparatus for manufacturing hot press-formed parts for multi-stage processes.

13. The processing device further includes a temperature control unit that controls an initial temperature of at least one of the notch die and the blanking die to 400° C. or higher; The manufacturing apparatus for a multi-stage hot press-formed part according to claim 12, wherein the temperature control unit is provided between at least one of a notch die and a blanking die and a press.

14. A manufacturing device for multi-stage hot press-formed parts as described in claim 12 or 13, comprising a structure protruding from a surface of the upper die of one or more of the notching die and blanking die that contacts the strip material, the structure being a push bar operated by a spring.

15. the one press includes a press slide and a press bolster; The manufacturing apparatus for a multi-stage hot press-formed member according to any one of claims 12 to 14, wherein a cylindrical material position control unit is provided on a surface of the press bolster on which a die is provided.

16. A hot press-molded member manufactured by the method for manufacturing a multi-stage hot press-molded member according to any one of claims 1 to 11, A hot press-formed member having an undercut shape and a tensile strength of 1300 MPa or more.

Citation Information

Patent Citations

  • Transfer press machine

    JP2007144495A

  • Method for manufacturing magnesium alloy material

    JP2012166232A

  • Hot press forming device and hot press forming method

    JP2013163209A

  • Press molding article of extrusion material

    JP2014159038A

  • Press molding article, hot press molding method, and hot press molding apparatus

    JP2014208374A