Method for producing solid biofuel
The method of high-pressure molding and controlled pressure adjustment in the production of biomass solids addresses the low char yield issue, resulting in a biofuel with a char yield of 25% or more, suitable for coal coke substitution.
Patent Information
- Application Number
- JP2020160689
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-25
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Conventional biomass solids have a low char yield due to high volatile content, making them unsuitable as a partial substitute for coal coke in applications requiring high char yield.
A manufacturing method involving high-pressure molding and controlled pressure adjustment during heating and cooling to produce a biomass solid with a char yield of 25% or more, utilizing a process that includes initial pressures of 8 MPa or more, constant updating of maximum pressure, and maintaining back pressure during cooling.
The resulting solid biofuel achieves a char yield of 25% or more, enabling longer burning time and suitability as a substitute for coal coke.
Smart Images

Figure 0007555067000002 
Figure 0007555067000007 
Figure 0007555067000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid biofuel and a method for producing the same, and more particularly to a solid biofuel that can be used as an alternative fuel to coal coke and as a material raw material, and a method for producing the same. [Background technology]
[0002] Biofuels made from biomass that can partially replace coal coke in foundry and steelmaking are highly anticipated as renewable resources and can reduce greenhouse gas emissions due to their carbon-neutral properties.
[0003] In particular, coal coke used in foundry and steel manufacturing is subjected to high stress because it collides with other coal when it is fed into the furnace and falls a long distance into the furnace, etc. Therefore, a considerable hardness was also required for biomass fuel.
[0004] For example, Patent Document 1 discloses an invention for a biomass solid that can be mixed with coal coke and used as a biomass fuel, which is made of a pre-semi-carbonized or semi-carbonized solid material that is formed by heating and pressurizing a biomass raw material resulting from photosynthesis, and is characterized by having a maximum compressive strength of 60 to 200 MPa and a calorific value of 18 to 23 MJ / kg. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2006 / 078023 Summary of the Invention [Problem to be solved by the invention]
[0006] Coal coke is composed almost entirely of carbon, and has a char yield of approximately 100%. On the other hand, conventional biomass solids, including those described in Patent Document 1, have a char yield of only about 22%. This is because biomass solids contain a large amount of volatile matter because the raw materials are not carbonized. In other words, the release of volatile matter could not be suppressed inside the solid, resulting in a low char yield. However, there was a strong demand for biomass solids with a high char yield to be used as a partial substitute for coal coke. [Means for solving the problem]
[0007] The present invention has been conceived in view of the above problems, and provides a biomass solid (hereinafter referred to as "solid biofuel") that has a char yield higher than that of the raw material, the char yield being 25 mass% or more. )of A method of manufacture is provided.
[0009] In addition, the method for producing a solid biofuel according to the present invention comprises the steps of: A process of placing a raw material obtained by chipping biomass resulting from photosynthesis into a molding space, applying an initial pressure of 8 MPa or more, and heating and pressurizing the raw material until the molding start temperature and the molding start pressure, which are greater than the initial pressure, are reached; a molding process for maintaining the maximum molding pressure at the molding start pressure for a predetermined time while adjusting the volume of the molding space so as to constantly update the maximum molding pressure from the molding start pressure; A step of cooling the molding space while adjusting the pressure in the molding space so that the volume of the molding space is equal to or smaller than the volume of the molding space at the start of cooling, The maximum molding pressure in the molding step is higher than 30 MPa. Effect of the Invention
[0010] The solid biofuel of the present invention has a char yield higher than that of the raw material, and the char yield is 25% by mass or more. This value could not be achieved with conventional biomass solids, and the solid biofuel can burn for a longer period of time than conventional biomass solids. [Brief description of the drawings]
[0011] [Figure 1] 4 is a graph showing the progress of temperature and pressure in the manufacturing method according to the present invention. [Diagram 2] 1 is a graph showing the progress of temperature and pressure when the initial pressure is higher than 30 MPa. [Diagram 3] 1 is a graph showing the progress of temperature and pressure when the initial pressure is lower than 30 MPa. [Figure 4] 1 is a graph showing the progress of temperature and pressure when forced pressurization is performed in a heating and pressurizing process. [Diagram 5] 13 is a graph showing the progress of temperature and pressure when a pressurizing method in which the maximum pressure is constantly updated and a forced pressurizing method are combined in a heating and pressurizing process. [Figure 6] 1 is a graph showing the relationship between back pressure (Back pressure [MPa]) and char yield (Char yield [%]). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The solid biofuel and its production method according to the present invention will be described below with reference to the drawings and examples. Note that the following description illustrates one embodiment of the present invention and one example, and the present invention is not limited to the following description. The following description can be modified within the scope of the present invention. In addition, the char yield means the ratio of non-volatile matter excluding the components that have volatilized from the solid biofuel. Specifically, it corresponds to the total of the fixed carbon content, ash content, etc.
[0013] The solid biofuel of the present invention is made only from biomass resulting from photosynthesis. Here, biomass can be considered to have a general definition of "renewable organic resources derived from living organisms, excluding fossil resources." In addition, "biomass resulting from photosynthesis" includes biomass such as woody materials, herbaceous plants, agricultural crops, and kitchen waste.
[0014] Suitable woody materials include wood, dead leaves, or waste materials such as forest residues, pruning and leaf cuttings, driftwood, and paper. Suitable herbaceous materials include bamboo and kenaf. Suitable agricultural products include non-edible parts such as Chinese stalks, sesame stalks, potato vines, and rice husks. Suitable kitchen waste materials include coffee grounds, used tea leaves, and soybean lees.
[0015] In addition, the solid biofuel according to the present invention is made by subjecting the raw material to a semi-carbonized state. Here, the "non-semi-carbonized state" raw material refers to a raw material on a completely dry basis. Also, the "completely dry basis" refers to a ratio in which the mass of the measurement subject after desorption of moisture is taken as 100 (the same applies below).
[0016] <Molding equipment> The solid biofuel of the present invention can be molded by a molding device capable of heating while adjusting the applied pressure. The molding device is provided with a molding chamber, and by moving at least one wall of the molding chamber, the volume of the molding chamber is reduced and pressure is applied to the raw material in the molding chamber. Hereinafter, the pressure of the molding chamber refers to the pressure applied to maintain or reduce the volume of the molding chamber. In other words, adjusting the pressure in the direction of reducing the volume of the molding chamber means that pressure is applied to the molding chamber. Also, even if the volume of the molding chamber is kept constant, pressure is applied to the molding chamber when the raw material inside expands. In either case, it can be said that the volume of the molding chamber is adjusted.
[0017] <Chipping process> The solid biofuel according to the present invention can be obtained by processes including a chipping process, a heating and pressurizing process, a molding process, and a cooling process, as described below. These processes will be described below and then further explained in detail using figures (<Explanation using graphs>). First, the raw material is cut into a predetermined size. Specifically, it is preferable that the size is about several mm to several cm. This may be called a process of chipping the raw material biomass. The raw material obtained in this way may be called "raw material obtained by chipping biomass resulting from photosynthesis". Furthermore, a process of adjusting the moisture content of the raw material to 25% or less is included.
[0018] <Heat and pressure process> Next, these raw materials are put into a molding space (molding chamber of molding equipment) where pressure and heat can be applied, and heated to a molding start temperature Tt (for example, 190°C) under the condition of an initial loading pressure ILP (Initial Loading Pressure) of 8 MPa or more. The pressure at the molding start temperature is the molding start pressure Pt. The molding start pressure Pt is set to a pressure higher than the initial pressure ILP. A temperature rise rate Trop of about 10°C / min is usually used, but is not limited to this rate. A molding start temperature Tt of 190°C is suitable, but it can be selected in the range of 180°C to 210°C.
[0019] In the heating and pressurizing step, a method of heating and pressurizing while constantly updating the maximum pressure can be preferably used. The "method of heating and pressurizing while constantly updating the maximum pressure" is a method of heating the raw material when the raw material expands due to heating and the pressure in the molding space increases without lowering the pressure below the increased pressure.
[0020] More specifically, the pressure from a short time ago is set as the maximum pressure Pm, and if the current pressure is higher than Pm, the current pressure is set as the new maximum pressure Pm. The molding device is controlled so that the maximum pressure Pm is always applied to the molding space. Therefore, if the temperature of the raw material increases due to heating, and the pressure in the molding space increases as a result, the volume of the molding space can remain constant.
[0021] However, if the pressure decreases from the maximum pressure Pm before the short time, the molding device operates to reduce the volume of the molding space and maintain the maximum pressure Pm before the short time. In other words, the volume of the molding space is adjusted so that the maximum pressure is always maintained. The short time may be determined by the machine time of the molding device, and a range of, for example, 0.01 seconds to 3 seconds can be suitably used.
[0022] The pressurization in the heating and pressurizing step may be performed by forcibly increasing the pressure in the molding space at a predetermined pressure increase rate. For example, when it is desired to heat the raw material in a molding space of a certain volume and increase the pressure in the molding space faster than the pressure increase caused by heating, heating can be performed while forcibly applying pressure. Note that, here, forcibly applying pressure means applying a force in a direction to forcibly reduce the molding space. In addition, the pressure increase rate at this time is not limited to a linear proportional relationship between time and pressure. For example, the pressure increase rate may be such that the pressure increases quadratically with respect to time.
[0023] In addition, the pressurization in the heating and pressurizing step may be a combination of a method of heating and pressurizing while constantly updating the maximum pressure and a method of heating and pressurizing while forcibly applying pressure. For example, heating and pressurizing may be performed while constantly forcibly applying pressure until the middle of the temperature rise, and then heating and pressurizing may be performed while updating the maximum pressure from that point on.
[0024] In the method for producing a solid biofuel according to the present invention, the solid biofuel is molded at a "maximum molding pressure Pmx" (described later) higher than 30 MPa. Therefore, the molding start pressure Pt is higher than 30 MPa, or the maximum molding pressure Pmx exceeds 30 MPa in the molding process (described later). In addition, in the heating and pressurizing process and the molding process (described later), a pressure higher than the initial pressure ILP is called back pressure (BP). In the method for producing a solid biofuel according to the present invention, it is also necessary to have a back pressure. In other words, no matter what procedure is used for the heating and pressurizing process, the molding start pressure will be higher than the initial pressure.
[0025] <Molding process> When the molding start temperature Tt is reached, the molding space is maintained for a predetermined time while constantly updating the maximum pressure. Here, the pressure in the molding space during the molding process is called the "molding pressure." The molding pressure may be understood as the pressure applied to the raw material in the molding space.
[0026] "While constantly updating the maximum pressure" is the same as explained in the <Heating and Pressurizing Process>. In other words, the pressure from a short time ago is set as the maximum pressure Pm, and if the current pressure is higher than Pm, the current pressure is set as the new maximum pressure Pm. The molding device controls the volume of the molding space so that the maximum pressure Pm is always applied to the molding space.
[0027] The highest pressure during the molding process is called the "maximum molding pressure Pmx." Pressure control is performed while constantly updating the maximum pressure, so the maximum molding pressure Pmx is the pressure at the end of the molding process (at the start of the cooling process described below).
[0028] The "predetermined time" for the molding process is preferably from one minute to several hours. The "predetermined time" may also be called the "molding time." The molding time is a time that is set in advance.
[0029] The temperature of the molding space in the molding process is called the "molding temperature". The molding temperature may be understood as the temperature of the raw material in the molding space. The molding temperature is usually controlled to maintain the molding start temperature Tt. However, the molding temperature may be forcibly changed (by heating or cooling the molding device) during the molding time. In addition, when internal heat is generated in the pressurized raw material and the temperature in the molding space rises, it may be cooled to a constant temperature, or temperature control may be performed to maintain the increased temperature as it is. However, in the method for producing solid biofuel according to the present invention, even if the molding temperature changes, the molding pressure is always controlled to update the maximum pressure. The raw material in the molding space that has undergone the molding process is called a molded product.
[0030] In the molding process, by constantly updating the maximum pressure, it is possible to achieve the effect of softening and resinification even when there is insufficient heating by thermal conduction and the temperature inside the molded product is low. In addition, if the maximum molding pressure Pmx is maintained for a long period of time (about 60 minutes), the temperature inside the molded product will rise by thermal conduction, and most of the inside of the molded product will be softened and resinified. These effects remain even when the molded product is cooled and becomes solid biofuel.
[0031] <Cooling process> After the molding time has elapsed since the start of molding in the molding process, the process moves to the cooling process, in which the temperature in the molding space is cooled at a predetermined rate.
[0032] In the cooling process, rapid unloading is not preferable because it may cause cracks in the molded product. Cooling is performed while maintaining the size (volume) of the molding space at the start of cooling. The volume of the molded product decreases as the temperature decreases. As a result, the pressure on the molding space also decreases. In the cooling process of the present invention, cooling is performed while controlling the pressure so that the volume of the molding space is at least equal to or less than the molding space at the start of cooling. That is, in the cooling process, the molding space is controlled to maintain the molding space at the start of cooling or to be smaller than the molding space at the start of cooling so that pressure is applied to the molded product.
[0033] In particular, it is preferable to cool the mold space while maintaining the pressure (maximum molding pressure Pmx) at the start of cooling. In this type of cooling, the molding device is controlled to reduce the volume of the mold space to compensate for the pressure reduction that accompanies the volume reduction of the molded product due to the temperature drop. The molded product at the end of the cooling process becomes solid biofuel.
[0034] <Graphic explanation> The steps described above are specifically shown in Figure 1. Figure 1 can also be said to represent the operating program of the molding device. Referring to Figure 1, the horizontal axis represents time, the left vertical axis represents the temperature of the molding space, and the right vertical axis represents the pressure of the molding space. The units of temperature that are preferably used are "℃: Celsius" or "K: Kelvin". The unit of pressure that can be preferably used is MPa.
[0035] Time t0 is the processing start time. The initial temperature Ts at the processing start time is usually room temperature. The molding device heats up to the molding start temperature Tt at time t2, maintains the temperature Tt from time t2 to time t4, and then cools at a constant temperature drop rate until time t5. Therefore, the heating and pressurizing process is from time t0 to time t2, the molding process is from time t2 to time t4, and the cooling process is from time t4 to time t5.
[0036] At the start of processing time t0, an initial pressure ILP is applied to the molding space. Figure 1 shows that the temperature of the raw material in the molding space rises from time t1, which is halfway through the heating and pressurizing process, and the pressure increases. In the heating and pressurizing process, the volume of the molding space is adjusted to constantly update the maximum pressure. Since most raw materials expand in volume when heated, it is sufficient for the molding space to maintain the volume at the time of the initial pressure ILP. However, if the volume temporarily decreases due to heating, the pressure is controlled so that the volume of the molding space decreases to compensate for the decrease in pressure caused by the decrease in volume.
[0037] When the heating and pressurizing process is performed by adjusting the molding space so as to constantly update the maximum pressure, the transition from the heating and pressurizing process to the molding process is determined by whether or not the molding start temperature Tt has been reached. In this case, the molding start pressure Pt becomes a pressure that is determined by the natural course of events.
[0038] In Figure 1, the pressure at time t2 is the molding start pressure Pt. During the molding process (from time t2 to time t4), pressure control is performed to constantly update the maximum pressure. If an expansion change occurs inside the molded product under the heating and pressurizing conditions, the pressure in the molding space will rise. Figure 1 shows that such a change occurred at time t3.
[0039] The molding pressure is always maintained as the maximum pressure because the molding space is controlled so that the maximum pressure is updated. In other words, even if the volume of the molded product shrinks, the molding space is controlled to become smaller so that the pressure is maintained. In the heating and pressurizing process, the molding space is controlled so that pressure is applied to the raw material during heating, so the molding start pressure Pt is always greater than the initial pressure ILP (back pressure: BP).
[0040] In Fig. 1, an example is shown in which the molding temperature in the molding process is controlled to maintain the molding start temperature Tt. However, as explained in <Molding process>, the temperature may be forcibly changed.
[0041] The molding process is time-controlled, i.e., the time between time t2 and time t4 is preset.
[0042] After the molding process is completed, the process proceeds to the cooling process (time t4 to time t5). The pressure at the start of cooling is the maximum molding pressure Pmx. In the present invention, by setting this maximum molding pressure Pmx to 30 MPa or more, a solid biofuel with a char yield of more than 25% can be obtained.
[0043] When cooling is performed while maintaining the molding space at the start of cooling, the pressure in the molding space decreases as the volume of the molded product decreases or the internal pressure of the molded product decreases. This pressure decrease is called "constant molding space cooling." In the present invention, cooling is performed while applying a pressure equal to or greater than the constant molding space cooling. In Figure 1, it is sufficient if there is a pressure reduction line (a line showing the relationship between time and pressure in the molding space) in the gray area. If there is a pressure reduction line in this area, it can be said that the molding space is cooled with a pressure that will result in a molding space with a volume equal to or less than that of the molding space at the start of cooling.
[0044] In particular, in the present invention, a preferred embodiment is cooling while controlling the molding space so as to maintain the maximum molding pressure Pmx at the start of cooling. In FIG. 1, this is a reduced pressure line indicated by the reference symbol 12. The reduced pressure line indicating constant cooling of the molding space is indicated by the reference symbol 10. The reduced pressure line 12 adjusts the molding space so that the temperature is cooled to near room temperature (Ts in FIG. 1) and the maximum molding pressure Pmx is maintained until just before the end of the processing. Then, the load is released all at once at the end of the processing (time t5). Note that cooling while controlling the molding space so as to maintain the maximum molding pressure Pmx does not mean cooling while constantly updating the maximum pressure.
[0045] In the present invention, other pressure reduction lines may be used in addition to pressure reduction line 12, as long as they are in the grey region (e.g., pressure reduction lines 14, 16, etc.). Cooling may also be performed while applying a pressure equal to or greater than the maximum molding pressure Pmx at the start of cooling (pressure reduction line 18, etc.). There is no particular upper limit to the region in which pressure reduction lines equal to or greater than the maximum molding pressure Pmx at the start of cooling exist, and this may be the limit of the molding device. In the figure, the white arrow indicates that a pressure equal to or greater than the maximum molding pressure Pmx is also acceptable.
[0046] Fig. 2 shows one embodiment of the heating and pressing step. In the present invention, it is necessary that the maximum molding pressure Pmx is greater than 30 MPa, and this is achieved by setting the initial pressure ILP to 30 MPa or more. As shown in Fig. 3, even if the initial pressure ILP is less than 30 MPa, it may be lower than 30 MPa as long as it can exceed 30 MPa through the subsequent heating and pressing step and molding step. In either case, the pressurization in the heating and pressing step is performed so as to constantly update the maximum pressure. Therefore, the molding step is performed while applying back pressure.
[0047] Fig. 4 shows a case where pressure is forcibly applied from the initial pressure ILP to the molding start pressure. In this case, since the molding start pressure Pt is also preset, the molding start pressure can be reliably set to a pressure exceeding 30 MPa, and back pressure can also be applied.
[0048] 5 shows a case where pressure is always forcibly applied from the outside in the beginning of the heating and pressurizing step (from time t0 to time t6), but from time t6 onwards, pressure is applied so as to update the maximum pressure. In this way, in the present invention, the heating and pressurizing step may be carried out by combining the method of forcibly applying pressure and the method of applying pressure while constantly updating the maximum pressure.
[0049] The solid biofuel according to the present invention is molded through the above-mentioned steps. The solid biofuel according to the present invention is characterized in that it has a char yield higher than that of conventionally obtained solid biomass materials. In the examples described later, a char yield of 25 mass% or more is obtained, which is a value that conventional biomass solid materials could not achieve.
[0050] Next, we will explain the measurement methods of some indicators. Note that the following is an example of the measurement method, and it can be modified as long as the measurement principle is the same.
[0051] <Carbon mass fraction> This is the amount of carbon in a sample. It is measured on a completely dry basis. The standards that govern this measurement are "ISO16948: Solid biofuels - Determination of total carbon, hydrogen, and nitrogen content" and "JIS M 8813 Coal and coke - Methods for elemental analysis."
[0052] The measurement principle is to combust an analytical sample in an oxygen atmosphere and measure the mass of carbon dioxide in the exhaust gas to determine the carbon mass fraction.
[0053] For example, when the carbon mass fraction of cedar, a raw material biomass, was measured, it was 51.3 mass% (total dry basis). In other words, on a total dry basis, it can be said that about half of the total mass is carbon.
[0054] The mass ratio of the solid biofuel to the raw material, which will be described later, i.e., the carbon mass fraction, is shown in Table 1. Here, the mass of the raw material is m0, the mass of the solid biofuel is m, and the mass ratio (%) is calculated as m / m0 x 100.
[0055] [Table 1]
[0056] The carbon mass fraction of the solid biofuel can be said to be the same as the carbon mass fraction of the raw biomass.
[0057] <Volatile content of raw materials> This is the ratio of volatile matter in raw materials. It is measured on a completely dry basis. This measurement is regulated by "JIS M 8812 Coal and coke - Methods of proximate analysis."
[0058] The measurement principle is to subtract the moisture content of the analytical sample from the mass loss when a crucible with a lid containing the analytical sample is placed in an atmosphere of 900±20℃ for 7 minutes, and calculate the mass m VM The mass of the analytical sample minus the water content is m0. VM Ratio of m VM / m0×100 is calculated as the mass fraction of volatile matter VM [%] (volatile matter rate) on a completely dry basis.
[0059] This measurement makes it possible to determine the percentage of volatile matter other than water in the raw material. For example, when the raw material was cedar, the volatile matter percentage was found to be 81.6% by mass.
[0060] <Ash content of raw materials> Ash is the residue left over from burning raw materials. It may consist of elements other than carbon, oxygen, and hydrogen. Its measurement is regulated by "JIS M 8812 Coal and coke - Industrial analysis method".
[0061] The measurement principle is to heat and burn the analytical sample to 815°C in an air atmosphere, and measure the mass of the remaining ash m ASH The mass of the analytical sample minus the water content is taken as m0, and m ASH Ratio of m ASH / m0×100 is the mass fraction A [%] of ash on a completely dry basis (ash content).
[0062] This measurement allows us to determine the percentage of ash in the raw material. For example, when the raw material was cedar, the ash percentage was found to be 0.40%.
[0063] <Fixed carbon fraction of raw materials> The standard governing this measurement is "JIS M 8812 Coal and coke - Proximate analysis method."
[0064] The measurement principle is that the fixed carbon fraction on a completely dry basis is calculated using the measured VM [%] and A [%] using equation (1). FC[%]=100-VM[%]-A[%] ···(1)
[0065] From equation (1), the fixed carbon fraction is calculated by subtracting the volatile fraction VM and the ash fraction A from the total. When the raw material was measured using cedar, the fixed carbon fraction was found to be approximately 18% by mass. EXAMPLES
[0066] An example of the solid biofuel according to the present invention is shown below. The raw material biomass was derived from Japanese cedar. This biomass was dried in advance to a moisture content of about 10% by mass. Next, the biomass was pulverized with a cutter mill for 25 seconds, and then classified into particles of 53 to 150 μm using a sieve shaker.
[0067] 50 mg of classified biomass was placed in a cylinder with an inner diameter of 4 mm, the bottom of which was closed with a metal mold, and a metal mold similar to the bottom was inserted from the top. A predetermined pressure (22 to 70 MPa) was applied to the biomass with a hydraulic jack. This was the initial pressure.
[0068] The pressure is applied to the biomass until the entire production process is completed.
[0069] With pressure applied, the cylinder was covered with an electric tubular furnace and heated to the set temperature (190°C). In the process of heating to the set temperature, the pressure inside the cylinder rose from the initial value, but the pressure was not removed and the increased state was maintained.
[0070] After reaching the set temperature, the set temperature and increased pressure (maximum molding pressure: 30-100 MPa) were maintained for 1 minute and 15 seconds.
[0071] After that, the electric tubular furnace was removed and cooling was continued in that state. The difference between the maximum molding pressure at the start of cooling and the initial pressure was taken as the pack pressure BP. The maximum molding pressure at the start of cooling was also maintained during the cooling process. In other words, if a reduction in pressure occurred due to cooling, pressure was immediately increased to maintain the maximum molding pressure.
[0072] During the cooling process, the cooling was deemed to be complete when the thermometer reading fell below 50°C, i.e., the treatment was completed. The pressure applied to the biomass was released, and the solid biofuel was removed.
[0073] The char yield of the solid biofuel was measured as follows. First, the atmosphere in the measurement chamber was an inert (nitrogen) atmosphere, and nitrogen was supplied to the measurement chamber at 150 cc / min. The analysis sample in the molded state was heated from room temperature to the set temperature of 107°C at a heating rate of 10°C / min, and after reaching the set temperature, it was held for 30 minutes to release moisture. This was judged to be in a completely dry state.
[0074] After the specified time had elapsed, the temperature was further increased at 10°C / min to the set temperature of 900°C, and then held at 900°C for 10 minutes to release the volatile matter. The mass remaining at this point was the mass of the non-volatile matter. The char yield (%) on a completely dry basis was calculated from the ratio of this to the mass of the analysis sample before measurement excluding moisture.
[0075] The char yield [%] for solid biofuel (molding temperature 190°C) is shown in Figure 6. Referring to Figure 6, the horizontal axis is back pressure BP (MPa) and the vertical axis is char yield (%). The black circles are samples when back pressure was applied at an initial pressure of 44 MPa, and are solid biofuels according to the present invention. The black diamonds are samples when back pressure BP was applied at an initial pressure of 22 MPa. For all samples, the heating and pressurizing step and molding step were carried out using a pressurizing method that constantly updates the maximum pressure. Furthermore, for all samples, the maximum molding pressure exceeded 30 MPa in the molding step, and back pressure could be obtained, and they are solid biofuels according to the present invention.
[0076] The black squares are samples with an initial pressure of 44 MPa, and a pressurizing method in which the maximum pressure is constantly updated, as in the manufacturing method according to the present invention, was used, but no back pressure BP was applied, and they are comparative examples. The molding temperature of this sample was 110°C, but the raw material did not expand, and back pressure did not occur even when the heating and pressurizing process and the molding process were performed using a pressurizing method in which the maximum pressure is constantly updated. In other words, in the heating and pressurizing process, the molding space was controlled to shrink so that the initial pressure ILP was maintained. In the subsequent molding process, the molding space was also maintained so that the initial pressure ILP was maintained. In other words, even if the pressure of the molded product in the molding space changed to be lower, the molding space was controlled to shrink, and the pressure in the molding space was maintained at the initial pressure ILP. In the cooling process, the molding space was controlled to become smaller so that the initial pressure ILP was maintained.
[0077] The white circles and white squares are samples in which the chipped raw material was solidified at an initial pressure of 44 MPa and then processing proceeded without applying pressure. In other words, these are samples to which the manufacturing method of the present invention was not applied. Therefore, in the heating and pressurizing process, the white circles were heated to the molding start temperature of 190°C, and the white squares were heated to the molding start temperature of 110°C without applying pressure. In the molding process, the molding start temperature was maintained without applying pressure, and no pressure was applied in the subsequent cooling process. The white circles and white squares are also comparative examples. The char yield of the raw material was 16%.
[0078] 6, all of the solid biofuels according to the present invention to which back pressure could be applied had a char yield of over 24%. More specifically, the samples with black diamonds and an initial pressure of 22 MPa had char yields of 25.5% to 26.3% when the back pressure BP was around 10 MPa. The samples with black circles and an initial pressure of 44 MPa had char yields of 27.4%, 28.3%, and 28.4% when the back pressure BP was 18.9 MPa, 33.9 MPa, and 51.0 MPa, respectively.
[0079] On the other hand, the samples indicated by the white circles, white squares, and black squares are considered to be representative of conventional solid biofuels, and none of them had a char yield of 25%. In other words, the solid biofuel of the present invention had a char yield that was higher than that of conventional solid biofuels.
[0080] In particular, the sample marked with black squares was subjected to constant maximum pressure updates throughout the heating and pressurizing process and molding process. However, at a molding start temperature of 110°C, back pressure did not occur. This shows that even with the same raw materials, back pressure may not be applied depending on differences in conditions such as the molding start temperature, resulting in different solid biofuels.
[0081] Such solid biofuels with a high char yield are closer to coke and can be used as a substitute for coke. [Industrial Applicability]
[0082] The present invention can be suitably used for solid biofuel that uses biomass as fuel.
Claims
1. A step of placing a raw material obtained by chipping biomass resulting from photosynthesis into a molding space, applying an initial pressure of 8 MPa or more, and heating and pressurizing the raw material until the molding start temperature and the molding start pressure, which are greater than the initial pressure, are reached; a molding process for maintaining the maximum molding pressure at the molding start pressure for a predetermined time while adjusting the volume of the molding space so as to constantly update the maximum molding pressure from the molding start pressure; A step of cooling the molding space while adjusting the pressure in the molding space so that the volume of the molding space is equal to or smaller than the volume of the molding space at the start of cooling, A method for producing a solid biofuel, wherein the maximum molding pressure in the molding step is higher than 30 MPa.
2. The cooling step includes:
2. The method for producing a solid biofuel according to claim 1, further comprising a step of cooling the molding space while adjusting the volume of the molding space so that a pressure equal to or higher than the maximum molding pressure is maintained.
3. 3. The method for producing a solid biofuel according to claim 1 or 2, characterized in that in the step of heating and pressurizing, the heating and pressurizing is performed while constantly updating the maximum molding pressure.
4. The heating and pressurizing step includes a step of heating the molded product while constantly updating a maximum molding pressure; 3. The method for producing a solid biofuel according to claim 1 or 2, further comprising a step of heating the mixture while forcibly increasing the pressure at a predetermined rate.
5. 3. The method for producing a solid biofuel according to claim 1 or 2, wherein the step of heating and pressurizing comprises a step of heating while forcibly increasing the pressure at a predetermined rate.
Citation Information
Patent Citations
Method for molding waste wood crumbles and solid fuel or molded coal molded thereby
JP2006315316A
Apparatus for producing biocoke and method for producing the same
JP2008274107A
Biocoke production process and production apparatus
JP2010100807A
Fuel, and method for manufacturing fuel
JP2010138253A
Biocoke production apparatus and method
JP2012246414A