Solid powder cosmetics
Cellulose powder with specific properties addresses the moldability and impact resistance issues in solid powder cosmetics, enhancing both smoothness and softness.
Patent Information
- Application Number
- JP2022112171
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-13
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2042-07-13
AI Technical Summary
Conventional solid powder cosmetics face challenges in achieving both impact resistance and a smooth, soft feel due to weak binding forces between powder particles, leading to poor moldability and cracking issues.
Incorporation of cellulose powder with specific particle size and aspect ratio, along with additives, to enhance moldability and impact resistance while providing a smooth and soft texture.
The use of cellulose powder with fine fibrous cellulose improves moldability and impact resistance, resulting in a solid powder cosmetic that is both smooth and soft to the touch.
Smart Images

Figure 0007555079000009 
Figure 0007555079000006 
Figure 0007555079000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid powder cosmetic preparation. [Background technology]
[0002] Conventionally, solid powder cosmetics such as foundations and eye shadows are produced by a press molding method in which the cosmetic composition is filled in a container and compressed to solidify. Since the amount of oil in solid powder cosmetics is relatively small, the bonding force between the powder particles is weak and the cosmetics do not solidify easily. Therefore, the press pressure is increased to mold the cosmetics, but the molded products produced in this way have a hard, powdery feel.
[0003] Therefore, in solid powder cosmetics, elastic spherical resin powders such as silicone elastomers and polyurethanes are sometimes used to obtain a moist, smooth, and soft feel. However, when a large amount of this resin powder is blended, the solid powder cosmetics have poor moldability and are easily broken by impact. Thus, there is a certain degree of difficulty in producing a solid powder cosmetic that combines smoothness and impact resistance.
[0004] In Patent Document 1, the average crushing strength is 0.2 to 1 kg / mm 2 30-90% by weight of organic powder consisting of acylated taurine polyvalent metal salt of the above, and elastic modulus of 1-100 kg / cm 2 The above-mentioned difficulties are resolved by using a film-forming polymer of the above-mentioned type. Patent Document 2 focuses on oil-soluble rice bran extract, which has excellent moisturizing properties, and proposes a powder cosmetic in which oil-soluble rice bran extract is blended in a specific ratio with an oil agent contained in the powder cosmetic. Although this powder cosmetic is a powder, it is smooth and frictionless when applied, and the powder adheres to the skin, providing a unique feel of smooth, soft skin after application, while reducing damage when dropped. Also, Reference 3 proposes a makeup cosmetic containing cellulose granules. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-80325 A [Patent Document 2] Patent Publication No. 2021-98674 [Patent Document 3] International Publication No. 2018 / 194050 Summary of the Invention [Problem to be solved by the invention]
[0006] The technologies described in the above-mentioned Patent Documents 1 and 2 both focus not on the powder contained in solid powder cosmetics, but on ingredients other than the powder, such as film-forming polymers and oil-soluble rice bran extracts, and by mixing these ingredients, impact resistance and a smooth feel are imparted to the solid powder cosmetics. In contrast, the inventor of the present invention has focused on powder, and has been engaged in research into powder that can be added to solid powder cosmetics to impart impact resistance and a smooth feel. [Means for solving the problem]
[0007] As a result of intensive research, the inventors have found that a solid powder cosmetic containing cellulose powder can solve the above-mentioned problems, and have completed the following invention. Note that the cellulose granules described in the cited document 3 are different from the cellulose powder of the present invention.
[0008] (First aspect) The cellulose powder has an average particle size of 1 to 25 μm and an aspect ratio of 0.6 to 0.9. The cellulose powder is an aggregate containing an additive and fine fibrous cellulose having an average fiber width of 1 to 500 nm. A solid powder cosmetic preparation characterized by:
[0009] The cellulose powder contained in the above-mentioned solid powder cosmetic contains fine fibrous cellulose. As the name suggests, fine fibrous cellulose is made of long, thin fibers, so the cellulose powder containing fine fibrous cellulose is not spherical, but has a shape that is distorted from a spherical shape. The distorted shape can be expressed, for example, by the above-mentioned aspect ratio range. A solid powder cosmetic containing cellulose powder within the above-mentioned average particle size range and aspect ratio range can have both resistance to impact (impact resistance) and a feeling of use such as smoothness, moistness, and softness. The reason why the solid powder cosmetic containing the cellulose powder can achieve both impact resistance and a feeling of use is probably as follows.
[0010] In order to improve the drawbacks of conventional solid powder cosmetics, such as hardness and powdery texture, the incorporation of elastic spherical particles has been investigated. Elastic spherical particles are soft, and the rolling effect of the spherical particles gives them a moist feel and smooth stretchability. However, because they undergo elastic deformation during compression molding, when the pressure is released after molding, they exert a force that causes them to return to their original shape, making them difficult to mold and also resulting in poor impact resistance after molding.
[0011] In contrast, the cellulose particles used in the present invention are presumed to increase the contact area between particles by plastic deformation when compressed, improving the moldability and impact resistance of the solid powder cosmetic. Even without deformation due to pressure, the cellulose powder used in the present invention includes particles with distorted shapes, has a larger specific surface area than general spherical particles, and because the powder is non-spherical, it is assumed that when mixed with cosmetic ingredients, it is aligned in random directions, increasing the contact points between the ingredients, thereby reducing the impact resistance and causing less damage due to external forces.
[0012] In addition, when a dispersion of fine fibrous cellulose is dried as is, the fibers become strongly and randomly bound together by hydrogen bonds. On the other hand, when a cellulose powder containing fine fibrous cellulose and additives (e.g., hydrophilic water-retaining agents) is dried, the additives moderately inhibit the formation of hydrogen bonds between the cellulose fibers, adding softness, resulting in a moist feel and improving moldability through plastic deformation.
[0013] In addition to the first embodiment, the following embodiment is also preferred.
[0014] (Second aspect) The cellulose powder is formed by agglomeration of the fine fibrous cellulose. A solid powder cosmetic according to a first embodiment.
[0015] (Third aspect) The powder containing the cellulose powder is 60 to 99.9% by mass, and the oil content is 0.1 to 40% by mass. A solid powder cosmetic according to a first embodiment.
[0016] (Fourth aspect) The additive is glycerin. A solid powder cosmetic according to a first embodiment.
[0017] (Fifth aspect) The cellulose powder has a moisture content of 1 to 15% in an atmosphere with a humidity of 50%. A solid powder cosmetic according to a first embodiment.
[0018] (Sixth aspect) The cellulose powder has a bulk density of 0.5 g / cm 3 Below is the A solid powder cosmetic according to a first embodiment.
[0019] (Seventh aspect) The cellulose powder has a specific surface area of 1.0 m 2 / g or more, A solid powder cosmetic according to a first embodiment.
[0020] (Eighth aspect) The cellulose powder is contained in an amount of 1 to 99% by mass. A solid powder cosmetic according to a first embodiment.
[0021] (Ninth aspect) The cellulose powder has a pulp viscosity of cellulose of 1.0 to 7.0 mPa s. A solid powder cosmetic according to a first embodiment.
[0022] (Tenth Aspect) It is a base makeup cosmetic product. A solid powder cosmetic according to a first embodiment. Effect of the Invention
[0023] According to the present invention, a solid powder cosmetic preparation that is resistant to impact (impact resistance) and has a smooth texture can be obtained. [Brief description of the drawings]
[0024] [Figure 1] 1 is an SEM image of cellulose powder A. [Diagram 2] 1 is an SEM image of cellulose powder B. [Diagram 3] 1 is an SEM image of cellulose powder C. [Figure 4] 1 is an SEM image of cellulose powder D. [Diagram 5] 1 is an SEM image of silicone powder. [Figure 6] 1 is an SEM image of silica powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Next, an embodiment of the present invention will be described. Note that the embodiment is an example of the present invention. The scope of the present invention is not limited to the scope of the embodiment.
[0026] The solid powder cosmetic of this embodiment contains cellulose powder having an average particle size of 1 to 25 μm and an aspect ratio of 0.6 to 0.9, and the cellulose powder is characterized in that the cellulose powder is an aggregate containing additives and fine fibrous cellulose having an average fiber width of 1 to 500 nm. The composition of the solid powder cosmetic is described below.
[0027] (Fine fibrous cellulose) The cellulose powder contained in the solid powder cosmetic of this embodiment contains fine fibrous cellulose (also known as "CNF"). This fine fibrous cellulose can be obtained by defibrating (refining) raw pulp.
[0028] As the raw material pulp for fine fibrous cellulose, one or more types can be selected from, for example, wood pulp made from broadleaf trees, coniferous trees, etc.; non-wood pulp made from straw, bagasse, cotton, hemp, bast fiber, etc.; and deionized paper pulp (DIP) made from recycled waste paper, broke paper, etc.
[0029] However, it is preferable to use wood pulp rather than non-wood pulp or waste paper pulp, because it is possible to avoid the inclusion of impurities as much as possible and obtain a high content of alkali-insoluble α-cellulose among the cellulose components. By treating with alkali, it is possible to remove alkali-soluble components and increase the purity of the cellulose.
[0030] As the wood pulp, for example, one or more types can be selected from chemical pulps such as hardwood kraft pulp (LKP) and softwood kraft pulp (NKP), and mechanical pulp (TMP), and the like.
[0031] The hardwood kraft pulp may be bleached hardwood kraft pulp, unbleached hardwood kraft pulp, or semi-bleached hardwood kraft pulp. Similarly, the softwood kraft pulp may be bleached softwood kraft pulp, unbleached softwood kraft pulp, or semi-bleached softwood kraft pulp.
[0032] As the mechanical pulp, for example, one or more types can be selected and used from stone ground pulp (SGP), pressurized stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermo-ground pulp (TGP), ground pulp (GP), thermo-mechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), refiner mechanical pulp (RMP), bleached thermo-mechanical pulp (BTMP), etc. However, in order to avoid the inclusion of impurities other than the above-mentioned cellulose, it is particularly preferable to use chemical pulp such as hardwood kraft pulp (LKP) and softwood kraft pulp (NKP).
[0033] Prior to defibration of the fine fibrous cellulose, it may be pretreated by a chemical method, for example, hydrolysis of polysaccharides with an acid (acid treatment), hydrolysis of polysaccharides with an enzyme (enzyme treatment), swelling of polysaccharides with an alkali (alkali treatment), oxidation of polysaccharides with an oxidizing agent (oxidation treatment), reduction of polysaccharides with a reducing agent (reduction treatment), etc.
[0034] When the pulp is treated with alkali prior to defibration, some of the hydroxyl groups in the hemicellulose and cellulose contained in the pulp are dissociated and the molecules are anionized, weakening intra- and intermolecular hydrogen bonds and promoting the dispersion of the cellulose fibers during defibration.
[0035] Examples of the alkali used in the alkali treatment include organic alkalis such as sodium hydroxide, lithium hydroxide, potassium hydroxide, an aqueous ammonia solution, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, and benzyltrimethylammonium hydroxide. However, from the viewpoint of production costs, it is preferable to use sodium hydroxide.
[0036] By subjecting the fine fibrous cellulose to an enzyme treatment, acid treatment, or oxidation treatment prior to defibration, it is possible to lower the water retention of the fine fibrous cellulose, increase the degree of crystallinity, and increase the homogeneity. In this regard, when the water retention of the fine fibrous cellulose is low, it becomes easier to dehydrate, and the dehydration of the dispersion of the fine fibrous cellulose (hereinafter also referred to as "slurry") is improved.
[0037] When raw pulp is treated with an enzyme, acid or oxidation, the amorphous regions of hemicellulose and cellulose contained in the pulp are decomposed. Decomposing the amorphous regions can reduce the energy required for finely pulp treatment, and can improve the homogeneity and dispersibility of cellulose fibers. When cellulose fibers have excellent homogeneity and dispersibility, the cellulose powder produced from fine fibrous cellulose tends to have less variation in particle size and is homogeneous. When the particle size of the cellulose powder varies greatly, the cellulose powder may not be sufficiently dispersed in the solid powder cosmetic and may be unevenly distributed. Therefore, the degree of decomposition of the amorphous regions of hemicellulose and cellulose contained in the pulp is one of the important factors. However, since pretreatment reduces the aspect ratio of the fine fibrous cellulose and may produce a cellulose powder that is not within the desired average particle size, it is preferable to avoid excessive pretreatment.
[0038] The raw material pulp can be defibrated by beating the raw material pulp using, for example, a homogenizer such as a beater, a high-pressure homogenizer, or a high-pressure homogenizer, a stone mill-type friction machine such as a grinder or a grinding machine, a single-shaft kneader, a multi-shaft kneader, a kneader refiner, a jet mill, etc. However, it is preferable to use a refiner or a jet mill.
[0039] The raw material pulp is preferably defibrated so that the average fiber diameter, average fiber length, water retention, degree of crystallinity, coefficient of variation of fiber diameter distribution, peak value in the pseudo-particle size distribution curve, pulp viscosity, and B-type viscosity of the dispersion (slurry) of the obtained fine fibrous cellulose attain the desired values or evaluations shown below.
[0040] The average fiber diameter (average fiber width; average diameter of a single fiber) of the fine fibrous cellulose is preferably 1 to 500 nm, more preferably 3 to 500 nm, and particularly preferably 10 to 100 nm. If the average fiber diameter of the fine fibrous cellulose is less than 1 nm, the fine fibrous cellulose becomes highly viscous when made into a slurry, making it difficult to dry the fine fibrous cellulose to produce cellulose powder, and depending on the production method, the cellulose may dissolve, making it difficult to maintain the fibrous shape.
[0041] On the other hand, if the average fiber diameter of the fine fibrous cellulose exceeds 500 nm, the average particle diameter of the cellulose powder will become larger and the shape will become more distorted, such as more rod-like or flat, and there is a risk that the solid powder cosmetic containing the cellulose powder will be rough or prone to a foreign body sensation.
[0042] The average fiber diameter of the fine fibrous cellulose can be adjusted, for example, by the selection of raw pulp, pretreatment, defibration, etc.
[0043] The method for measuring the average fiber diameter of the fine fibrous cellulose is as follows. First, 100 ml of an aqueous dispersion (slurry) of fine fibrous cellulose with a solid content concentration of 0.01 to 0.1% by mass is filtered through a Teflon (registered trademark) membrane filter, and the solvent is replaced once with 100 ml of ethanol and three times with 20 ml of t-butanol. Next, the sample is freeze-dried and osmium-coated to obtain a sample. This sample is observed using an electron microscope SEM image at a magnification of 3000 to 30000 times depending on the width of the fibers that constitute it. Specifically, two diagonal lines are drawn on the observed image, and three straight lines passing through the intersection of the diagonal lines are arbitrarily drawn. Furthermore, the widths of a total of 100 fibers that intersect with these three straight lines are visually measured. The median diameter of the measured values is taken as the average fiber diameter.
[0044] The average fiber length of the fine fibrous cellulose (average length of a single fiber) is preferably 0.3 to 200 μm, more preferably 0.4 to 200 μm, and particularly preferably 0.5 to 200 μm. If the average fiber length of the fine fibrous cellulose is less than 0.3 μm, the fibers will not be well aggregated, making it difficult to produce a cellulose powder having a desired average particle size, and there is a risk that a cellulose powder having a small particle size or a large amount of aggregated bundle-shaped particles will be produced.
[0045] On the other hand, when the average fiber length of fine fibrous cellulose exceeds 200 μm, it tends to become a powder with various shapes, which causes non-uniformity in particle shape and particle size.
[0046] The average fiber length of the fine fibrous cellulose can be adjusted, for example, by selecting the raw pulp, pre-treating it, defibrating it, and the like.
[0047] The average fiber length of the fine fibrous cellulose is measured in the same manner as in the case of the average fiber diameter, by visually measuring the length of each fiber. The median length of the measured values is taken as the average fiber length.
[0048] The aspect ratio of the fine fibrous cellulose is preferably 50 to 200,000, more preferably 50 to 10,000. If the aspect ratio is below 50, it is difficult to obtain cellulose powder with a desired average particle size. On the other hand, if the aspect ratio is above 200,000, the circularity of the cellulose powder becomes small, and the smoothness of the solid powder cosmetic may be impaired.
[0049] The lower limit of the crystallinity of the fine fibrous cellulose is preferably at least 50, more preferably at least 60, and particularly preferably at least 70, and the upper limit is preferably no more than 100, more preferably no more than 95, and particularly preferably no more than 90. If the crystallinity is less than 50, the strength of the cellulose powder is low, and a solid powder cosmetic preparation having excellent impact resistance may not be obtained.
[0050] The water retention of the fine fibrous cellulose is preferably 500% or less, more preferably 300% to 480%, unless chemically modified. If the water retention of the fine fibrous cellulose is below 300%, the fine fibrous cellulose is not defibrated to the desired size, and as a result, particles of the desired shape and size may not be obtained.
[0051] On the other hand, if the water retention of the fine fibrous cellulose exceeds 500%, the water retention capacity of the fine fibrous cellulose itself becomes high, and the drying process of the fine fibrous cellulose takes a long time.
[0052] The water retention of the fine fibrous cellulose can be adjusted, for example, by the selection of raw pulp, pretreatment, defibration, etc.
[0053] The water retention of the fine fibrous cellulose is a value measured in accordance with JAPAN TAPPI No. 26 (2000).
[0054] The pulp viscosity of the fine fibrous cellulose is preferably 1.0 to 7.0 mPa·s, more preferably 1.5 to 6.5 mPa·s, and particularly preferably 2.0 to 6.0 mPa·s. The degree of polymerization of the fine fibrous cellulose used in the cellulose powder is preferably 150 to 1250, more preferably 250 to 1150. The pulp viscosity is the viscosity of the solution after dissolving cellulose in a copper ethylenediamine liquid, and the higher the pulp viscosity, the higher the degree of polymerization of cellulose. The pulp viscosity is also related to the strength and rigidity of the cellulose fiber. If the degree of polymerization is too high, the cellulose powder becomes hard, and even if an additive is mixed, the resulting solid powder cosmetic has a rough texture. On the other hand, if the degree of polymerization is too low, the strength of the fiber itself is lost, and the plastic force required for the cellulose powder used in the present invention becomes excessive, making it difficult to control the moldability of the cosmetic itself. The degree of polymerization of the fine fibrous cellulose can be adjusted, for example, by selecting the raw pulp, pre-treating, defibrating, etc. If the pulp viscosity is within the above-mentioned range, the particles have good plasticity, and a solid powder cosmetic having impact resistance and smoothness can be obtained.
[0055] The fine fibrous cellulose obtained by defibration can be dispersed in an aqueous medium to prepare a dispersion (slurry) if necessary. The aqueous medium is particularly preferably entirely water (aqueous solution). However, the aqueous medium may be partially other liquids that are compatible with water. As the other liquids, for example, lower alcohols having 3 or less carbon atoms can be used.
[0056] The dispersion of fine fibrous cellulose (slurry, 2.0% by mass based on solid content) preferably has a Brookfield viscosity of 400 mPa·s to 100,000 mPa·s, more preferably 500 to 50,000 mPa·s. If the Brookfield viscosity of the dispersion is within the above range, the slurry can be supplied to the drying device in the drying step without clogging.
[0057] The B-type viscosity of the dispersion of fine fibrous cellulose is a value measured in accordance with JIS-Z8803 (2011) "Method of measuring viscosity of liquids." B-type viscosity is the resistance torque when the dispersion is stirred, and the higher the viscosity, the more energy is required for stirring.
[0058] The cellulose fibers can be defibrated by the following defibration devices and methods. The defibration can be performed by using one or more means selected from homogenizers such as high-pressure homogenizers and high-pressure homogenizers, grinders, grinders, and other mill-type friction machines, refiners such as conical refiners and disk refiners, and various bacteria. However, it is preferable to defibrate the cellulose fibers using a water flow, particularly a high-pressure water flow, and a device or method for finely pulverizing the fibers. This device or method provides very high dimensional uniformity and dispersion uniformity for the fine fibrous cellulose obtained. In contrast, for example, when a grinder that grinds between rotating grindstones is used, it is difficult to uniformly pulverize the cellulose fibers, and in some cases, there is a risk that some fiber lumps will remain undisintegrated.
[0059] An example of a grinder used to defibrate cellulose fibers is the Masscolloider manufactured by Masuko Sangyo Co., Ltd. An example of a device for pulverizing with a high-pressure water flow is the Starburst (registered trademark) manufactured by Sugino Machine Co., Ltd., or the Nanovater (registered trademark) manufactured by Yoshida Kikai Kogyo Co., Ltd. An example of a high-speed rotary homogenizer used to defibrate cellulose fibers is the Clearmix-11S manufactured by M Technique Co., Ltd.
[0060] The solid powder cosmetic of the present embodiment contains cellulose powder, but may also contain a powder Y other than cellulose powder. In this specification, the term may be simply referred to as "powder" or "powder containing cellulose powder" as a concept including cellulose powder and powder Y other than cellulose powder.
[0061] (Cellulose powder) The cellulose powder of the present embodiment is an aggregate formed by drying fine fibrous cellulose, but when viewed microscopically, some are formed by drying fine fibrous cellulose as a single unit (for example, formed by a single thread entangled within the thread or formed by drying), and some are formed by agglomerating multiple fine fibrous celluloses during drying to form aggregates. Fine fibrous cellulose is produced from raw pulp, and when dried, the fibers wrinkle and shrink, so the cellulose powder formed has an uneven shape that is difficult to describe, for example, a shape like an aggregate of dried fine fibrous cellulose, a shape of confetti, or a shape like one or more sheets of paper such as Japanese writing paper that have been crumpled and rolled up. The cellulose powder is white, pale yellow, cream, pale orange, or a mixture of these colors. In particular, white or pale yellow cellulose powder is preferable as one composition of a solid powder cosmetic because it is not noticeable.
[0062] The cellulose powder of the present embodiment preferably contains 50% by mass or more of fine fibrous cellulose, more preferably 60% by mass or more, and even more preferably 70% by mass or more, and the upper limit may be 100% by mass. If the mass percentage of fine fibrous cellulose in the cellulose powder is less than 50% by mass, the cellulose powder may not have the desired average particle size and aspect ratio.
[0063] In addition, the cellulose powder has a surface that is uneven due to fine wrinkles formed on the surface, and light irradiated from the outside hits the unevenness and is diffusely reflected at various angles. Therefore, the surface of the cellulose powder lacks luster, and solid powder cosmetics containing the cellulose powder have reduced shine.
[0064] Furthermore, since the cellulose powder of the present embodiment is produced, for example, by drying, multiple pieces of dried and wrinkled fine fibrous cellulose may become entangled to form unevenness on the surface. The way in which fine fibrous cellulose dries varies, and the cellulose powder formed becomes particles consisting of a single piece of dried fine fibrous cellulose or a plurality of pieces of aggregated cellulose.
[0065] The cellulose powder contained in the solid powder cosmetic of this embodiment has an average particle size of preferably 1 to 25 μm, more preferably 2 to 24 μm, and even more preferably 3 to 23 μm, and an aspect ratio of preferably 0.6 to 0.90, and more preferably 0.6 to 0.85. If the average particle size and aspect ratio of the cellulose powder are within the above-mentioned ranges, the solid powder cosmetic has impact resistance and smoothness. To achieve both impact resistance and smoothness, it is desirable that both the average particle size and the aspect ratio are within the above-mentioned ranges, and it is not preferable that either one of them is outside the above-mentioned range. For example, even if the average particle size of the cellulose powder is within the above-mentioned range, if the aspect ratio exceeds the above-mentioned range, the impact resistance of the solid powder cosmetic may be impaired. Furthermore, even if the aspect ratio of the cellulose powder is within the above-mentioned range, if the average particle size exceeds the above-mentioned range, the smoothness of the solid powder cosmetic may be impaired. The aspect ratio of the cellulose powder is the value obtained by dividing the minor axis diameter of the cellulose powder by the major axis diameter of the cellulose powder.
[0066] The moisture content of the cellulose powder in an atmosphere with a humidity of 50% is preferably 1 to 15%, more preferably 3 to 10%. If the moisture content of the cellulose powder is within the above-mentioned range, the impact resistance of the solid powder cosmetic will be further improved. The moisture content of the cellulose powder can be adjusted by the concentration of fine fibrous cellulose in the fine fibrous cellulose dispersion liquid, which is the raw material of the cellulose powder, the drying time, the average fiber width of the fine fibrous cellulose, etc. However, according to the drying method described below, it may be difficult to adjust the moisture content of the cellulose powder to be smaller than the lower limit of the above-mentioned range. In addition, if the moisture content of the cellulose powder exceeds the above-mentioned range, the solid powder cosmetic may deteriorate with long-term use.
[0067] The bulk density of cellulose powder is 0.5 g / cm 3 or less, preferably 0.1 to 0.5 g / cm 3 , more preferably 0.1 to 0.4 g / cm 3 The bulk density of the cellulose powder is 0.5 g / cm 3If it exceeds this value, the adhesion of the solid powder cosmetic will be poor (the adhesion feeling means the feeling that the solid powder cosmetic is sufficiently adhered to the target of application, such as the skin), the moist feeling will be difficult to feel, and the solid powder cosmetic will be difficult to pick up with a puff.
[0068] The circularity of the cellulose powder is preferably 0.5 to 0.9, more preferably 0.6 to 0.85. If the circularity of the cellulose powder is within the above range, the resulting solid powder cosmetic has excellent impact resistance and smoothness. If the circularity is less than 0.5, the smoothness decreases, and if it exceeds 0.9, the impact resistance may decrease.
[0069] The aspect ratio and circularity can be measured using a Morphologi 4 manufactured by Malvern Panalytical. 3 was collected in a sample cartridge and dispersed on a glass plate using a dispersion unit, and then the particle count was 20,000, as determined by static image analysis.
[0070] The compressive strength (10% strength) of the cellulose powder is preferably 5 MPa or less, more preferably 0.5 to 5 MPa. If the compressive strength of the cellulose powder exceeds 5 MPa, the powder feels hard and rough, and lacks smoothness.
[0071] The specific surface area of the cellulose powder is preferably 1.0 m 2 / g or more, more preferably 1.0 to 10m 2 / g, more preferably 1.5 to 8m 2 / g. The specific surface area is 1.0 m 2 If the surface roughness of the cellulose powder is less than 1 / g, the surface roughness of the cellulose powder is small, resulting in poor adhesion of the solid powder cosmetic and noticeable dryness and powderiness.
[0072] (Additives) In order to improve the dispersibility of the cellulose powder produced through the above-mentioned drying process in the composition of the solid powder cosmetic, and to impart the effect of preventing the skin from drying and the effect of imparting moisture (emollient effect), additives may be contained in the cellulose powder. This is because, if the cellulose powder is left to stand after production, it may aggregate with each other. One of the causes of this is thought to be the polarity of the cellulose molecules that make up the cellulose powder. Therefore, the cellulose powder may not be dispersed overall in the solid powder cosmetic and may be unevenly distributed. Therefore, by containing an additive in the cellulose powder, the polarity of the cellulose molecules in the cellulose powder is masked, making the cellulose powder less likely to aggregate with each other and easier to disperse throughout the solid powder cosmetic. The additive in the present invention may be any additive capable of masking the polarity of cellulose molecules or physically preventing strong aggregation of cellulose fibers during drying, and is preferably a hydrophilic material considering that it is mixed in advance with the cellulose fiber dispersion, and is more preferably a hydrophilic material having an OH group (hydroxyl group), a CO group (carbonyl group), or a COOH group (carboxyl group). Since the cellulose powder in this form is hydrophilic, the inclusion of the additive, which is a hydrophilic material, keeps the moisture content of the cellulose powder within a desired range, and the solid powder cosmetic has excellent impact resistance.
[0073] The additive may be one or more selected from the group consisting of polyhydric alcohols, polysaccharides, water-soluble polymers, and surfactants. The content of the additive in the cellulose powder is preferably 1 to 49% by mass, more preferably 2 to 48% by mass. If the content is too high, the cellulose powder becomes sticky and loses its lightness, resulting in a poor feel on the skin. On the other hand, if the content is too low, the dispersion effect and emollient effect may not be achieved.
[0074] As the additive, the polyhydric alcohol may be a polyhydric alcohol having 2 to 6 carbon atoms and 2 to 3 oxygen atoms. Specifically, glycerin, diglycerin, propylene glycol, 1,3-butylene glycol, 1,2-pentanediol, dipropylene glycol, 1,2-hexanediol, heptanediol, ethylene glycol, diethylene glycol, 1,3-propanediol, 3-methyl-1,3-butanediol, etc. may be used, but are not limited thereto. In particular, glycerin is preferred from the viewpoint of thickening and dispersibility of composite particles.
[0075] Examples of polysaccharides that can be used include, but are not limited to, quince seed, veegum, xanthan gum, hyaluronate, etc. Hyaluronate is particularly preferred from the viewpoint of thickening properties and dispersibility of cellulose powder.
[0076] Examples of the water-soluble polymer include polyvinyl alcohol, polyvinylpyrrolidone, carboxyvinyl polymer, polyethylene glycol, homopolymers or copolymers having a monomer with a phosphorylcholine group as a constituent monomer, homopolymers or copolymers having a monomer with a sugar residue as a constituent monomer, and homopolymers or copolymers having a monomer with an amino acid residue as a constituent monomer.Specific examples include, but are not limited to, copolymers of alkyl (meth)acrylate and polymethacryloyloxyethyl phosphorylcholine, copolymers of alkyl (meth)acrylate and methacryloyloxyethyl glucoside, and copolymers of alkyl (meth)acrylate and methacryloyl-L-lysine.In particular, polyvinylpyrrolidone is preferred from the viewpoint of thickening and dispersibility of cellulose powder.
[0077] Examples of surfactants include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. In particular, nonionic surfactants are preferred to eliminate the effects of ionic bonds. On the other hand, if a cationic surfactant is added to anionic cellulose fibers, the cellulose fibers may be excessively aggregated during powder production (drying), making it difficult to control the shape of the powder.
[0078] Examples of nonionic surfactants include polyoxyalkylene alkyl ethers, glycerin alkyl ethers, glycerin fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, and their alkylene glycol adducts, polyalkylene glycol fatty acid esters, polyglycerin-modified silicones, and polyether-modified silicones. Examples of anionic surfactants include alkyl phosphates, polyoxyalkylene alkyl ether phosphates, sulfonates, alkyl sulfates, and polyaspartates. Examples of cationic surfactants include alkylamine salts and alkyltrimethylammonium salts. Examples of amphoteric surfactants include hydrogenated lecithin, carbobetaine-type amphoteric surfactants, sulfobetaine-type amphoteric surfactants, and amino acid-type amphoteric surfactants.
[0079] (Inorganic fine particles) The cellulose powder may contain inorganic fine particles. The inorganic fine particles can impart various functions to the cellulose powder, and for example, metallic inorganic fine particles have the effect of diffusing and reflecting incident light. By including such inorganic fine particles in the cellulose powder, it is expected that the effect of suppressing irradiation of ultraviolet rays and the effect of suppressing shine on the skin of the application area can be achieved.
[0080] The content of inorganic fine particles in the cellulose powder may be set at an upper limit of 49% by mass, preferably 45% by mass or less, and at a lower limit of 0% by mass, preferably 5% by mass or more. If the content exceeds 49% by mass, the specific gravity of the cellulose powder increases by the amount of the inorganic fine particles contained, and dispersibility in the solid powder cosmetic may be impaired. On the other hand, if the content is 5% by mass or more, the effect of diffuse reflection of incident light is sufficiently exhibited.
[0081] The upper limit of the primary particle diameter of the inorganic fine particles is preferably 10 μm, more preferably 5 μm or less, and more preferably 1 μm or less. If the primary particle diameter of the inorganic fine particles exceeds 10 μm, the inorganic fine particles are difficult to support by the fine fibrous cellulose. The lower limit of the primary particle diameter of the inorganic fine particles is not particularly limited, but is preferably 1 nm, more preferably 2 nm or more, and more preferably 3 nm or more. If the primary particle diameter of the inorganic fine particles is 1 nm or more, when the inorganic fine particles are mixed with the raw material slurry for producing cellulose powder, the inorganic fine particles are easily dispersed and cling to the fine fibrous cellulose.
[0082] The primary particle size of the inorganic fine particles can be measured by observation under an electron microscope, and the average value of the obtained particle sizes is taken as the measured value.
[0083] The inorganic fine particles can be used as they are, but it is preferable to subject them to hydrophilic treatment, since it makes them more compatible with the raw material slurry used to produce the cellulose powder. The surface treatment agent used for the hydrophilic treatment has the effect of suppressing the surface activity of the inorganic fine particles, improving the dispersibility of the inorganic fine particles, and improving transparency and squeaking. The surface treatment agent for the inorganic fine particles is not particularly limited as long as it is a treatment agent that can be dispersed in the raw material slurry, but it is preferable to use one that contains silicic anhydride or hydrated silicic acid.
[0084] The inorganic fine particles are not particularly limited and known inorganic fine particles can be used, for example, barium titanate, lead zirconate titanate, silicon carbide, silicon nitride, aluminum nitride, alumina, zirconia, zircon, titanium oxide, zinc oxide, iron oxide, cerium oxide, etc. In order to improve the effect of suppressing ultraviolet irradiation and the effect of suppressing skin shine, for example, one or a combination of two or more selected from the group consisting of titanium oxide, zinc oxide, iron oxide, and cerium oxide can be used. In particular, when the inorganic fine particles are titanium oxide, it is preferable because the effect of suppressing ultraviolet irradiation is improved.
[0085] The shape of the inorganic fine particles that can be contained in the cellulose powder is not particularly limited, but can be, for example, spherical, rod-like, needle-like, spindle-like, plate-like, polygonal, or the like.
[0086] The inorganic fine particles may be attached to the surface of the fine fibrous cellulose in the cellulose powder, or may be encapsulated in the fine fibrous cellulose. If the inorganic fine particles are encapsulated in the fine fibrous cellulose, the inorganic fine particles can be supported not only on the surface of the cellulose powder but also inside, and the cellulose powder is preferably diffusely reflected even when the incident light is irradiated from various angles. Here, the encapsulation can be defined as a state in which a part of the surface of the inorganic fine particles is covered with the fine fibrous cellulose, or a state in which the inorganic fine particles are covered with the fine fibrous cellulose when the cellulose powder is observed from the outside and cannot be observed from the outside.
[0087] The inorganic fine particles can be added to the fine fibrous cellulose dispersion before drying, and may be mixed uniformly.
[0088] The solid powder cosmetic of the present invention preferably contains 1 to 99% by mass of cellulose powder, more preferably 3 to 60% by mass, and even more preferably 5 to 40% by mass. If the cellulose powder is less than 1% by mass, the solid powder cosmetic will have poor impact resistance.
[0089] (Production of cellulose powder) The cellulose powder can be produced by drying fine fibrous cellulose in a drying process. Specifically, the cellulose powder can be produced by freeze-drying the fine fibrous cellulose as a raw material, drying under reduced pressure, drying by heating (for example, a drying method using hot drying), spray drying, or a method using spray-type freeze-drying under reduced pressure, which is a drying method for the cellulose powder of this embodiment. In particular, the cellulose powder produced by the heating drying method or spray drying method has an average particle size and aspect ratio suitable for use as a composition for the solid powder cosmetic of this embodiment.
[0090] Among the heat drying techniques, the drum drying method for producing cellulose powder makes it possible to obtain a dried product that is less likely to aggregate and is easily dispersed, even for fine fibrous cellulose that is relatively highly concentrated or has poor fluidity. One example of the production of cellulose powder by the drum drying method is as follows.
[0091] The fine fibrous cellulose can be supplied to a drum dryer in a slurry (aqueous dispersion) state, for example, where the drying process is performed. In this case, the content of the fine fibrous cellulose (absolute dry mass%) is 1 mass% or more, preferably 1.5 mass%, more preferably 2.0 mass%. The content is 10 mass% or less, preferably 7 mass%, more preferably 5 mass%. If the content exceeds 10 mass%, the viscosity of the slurry is too high and the handling property is poor. On the other hand, if the content is less than 1 mass%, a lot of energy and time are consumed to remove the moisture, which is not economical.
[0092] The drum dryer used in the drying process by the drum drying method may be a known one. For example, the "John Milder JM-T type" manufactured by Johnson Boiler Co., Ltd. can be used. As the drum dryer, an internal rotation drum dryer can be preferably used. If an internal rotation drum dryer is used, a gentle drying process is performed, and a dried body with a relatively small specific surface area is obtained. The drying process can be performed under normal pressure.
[0093] Regarding the operating conditions of the drum dryer, the surface temperature of the inner surface of the drum is 80 to 200°C, preferably 90 to 190°C. At this surface temperature, a dried body with strong cohesive force can be obtained. If the surface temperature exceeds 200°C, some of the fibers of the fine fibrous cellulose may be thermally denatured. On the other hand, if the surface temperature is less than 80°C, not only will it take a long time to remove the moisture, but the particles will have a very high moisture content. The rotation speed of the drum dryer can be, for example, 0.5 rpm or more and 2 rpm or less, depending on the inner diameter of the drum and the amount of slurry added. The time for drying with the drum dryer depends on the amount of slurry added, but if it is 1 second to 60 seconds, the dried body will be sufficiently dried, and even if it is dried for a longer time, the moisture content of the dried body will not be further reduced.
[0094] An example of an apparatus used for producing cellulose powder by the spray drying method is a spray dryer (Pris' "P-260"). Cellulose powder can be produced by supplying a slurry of fine fibrous cellulose to the spray dryer. The spray dryer may be, for example, a two-fluid nozzle type having two 90-type nozzles. The conditions for spray drying may be, for example, 20 kg / h of the slurry of fine fibrous cellulose, an inlet temperature of the drying air of 200°C, an outlet temperature of 100°C, and a spray air pressure of 0.6 MPa, but are not limited thereto.
[0095] When producing cellulose powder containing the above-mentioned additives, the additives are mixed with a slurry of fine fibrous cellulose, which is the raw material for production, to form a mixture, and this mixture is then fed to a drying device (e.g., a drum dryer or a spray drying device) used in a heat drying technique or a spray drying technique.
[0096] (Oil content) The solid powder cosmetic of the present embodiment may contain oil. By containing oil in the solid powder cosmetic, moldability is improved and impact resistance is excellent, but since the solid powder cosmetic contains cellulose powder, good impact resistance can be obtained even with a smaller amount of oil than conventional cosmetics.
[0097] The oil may be any of various origins, such as animal oil, vegetable oil, synthetic oil, etc., and may be in any of various forms, such as solid oil, semi-solid oil, liquid oil, volatile oil, etc.
[0098] The oil may be one or a combination of two or more selected from the group consisting of hydrocarbons, oils and fats, waxes, hardened oils, ester oils, fatty acids, silicone oils, fluorine-based oils, lanolin derivatives, and oil-soluble ultraviolet absorbers.
[0099] More specifically, for example, hydrocarbons such as liquid paraffin, squalane, petrolatum, paraffin wax, ceresin wax, microcrystalline wax, Japan wax, and montan wax; oils and fats such as olive oil, castor oil, jojoba oil, mink oil, and macadamia nut oil; waxes such as beeswax, lanolin, carnauba wax, candelilla wax, and veronica wax; esters such as isostearyl isostearate, cetyl isooctanoate, isopropyl myristate, isopropyl palmitate, octyldodecyl myristate, glyceryl trioctanoate, glyceryl tribehenate, pentaerythritol rosinate, diisostearyl malate, dilinoleyl dimer dilinoleate, and neopentyl glycol dioctanoate; silicones such as silicone gels composed of crosslinked silicones and solvents, such as fluorine-modified silicones, etc.; fluorine-based oils such as perfluoropolyether, perfluorodecane, and perfluorooctane; lanolin derivatives such as lanolin acetate, lanolin fatty acid isopropyl, and lanolin alcohol; lipophilic surfactants having an HLB value of 8 or less, such as sorbitan isostearate, sorbitan sesquiisostearate, polyglyceryl-2 isostearate, and polyglyceryl-2 diisostearate; and oil-soluble ultraviolet absorbers such as ethylhexyl methoxycinnamate, ethylhexyl dimethyl PABA, diethylamino hydroxybenzoyl hexyl benzoate, ethylhexyl triazone, and bisethylhexyloxyphenol methoxyphenyl triazine, which can be used alone or in combination of two or more of the above. Furthermore, among these, when one or more selected from high-viscosity ester oils having a viscosity of 1,000 to 50,000 mPa s at 25°C, such as diisostearyl malate and dilinoleyl dimer dilinoleate, and lipophilic surfactants, such as sorbitan sesquiisostearate and polyglyceryl-2 diisostearate, are used in combination, the moldability and moist feel can be further improved.
[0100] The content of oil in the solid powder cosmetic of this embodiment is preferably 0.1 to 40% by mass, more preferably 0.1 to 25% by mass, and particularly preferably 1 to 15% by mass. If the oil content is less than 0.1% by mass, moldability may decrease. On the other hand, if the oil content is more than 40% by mass, the cosmetic is less likely to be removed by a cosmetic puff such as a sponge, making it difficult to spread the cosmetic on the skin. Since the solid powder cosmetic of this embodiment contains cellulose powder, moldability can be maintained with a smaller amount of oil than the normal amount of oil, and the cosmetic can be made to be excellent in puff removal and ease of spreading.
[0101] (Other powder Y) The solid powder cosmetic of this embodiment can be blended with powder Y other than the cellulose powder. When the powder Y is included, the sticky feeling of the cosmetic film can be further suppressed, and when the solid powder cosmetic of this embodiment is used as a base makeup cosmetic, the covering power and the finish feeling can be made as desired. The powder Y other than the cellulose powder has an average particle diameter of 0.01 to 200 μm.
[0102] The powder Y other than the cellulose powder is not limited by, for example, its shape (e.g., spherical, plate-like, spindle-like, needle-like, etc.), its particle size, its particle structure (e.g., porous, non-porous, etc.), etc. In addition, the powder Y other than the cellulose powder may be one or a combination of two or more selected from inorganic color pigments, inorganic body pigments, inorganic fine particle powders, glittering powders, organic body pigments, and organic color pigments.
[0103] Specific examples of the powder Y other than the cellulose powder include inorganic coloring pigments such as titanium oxide, zinc oxide, zirconium oxide, red iron oxide, yellow iron oxide, black iron oxide, carbon black, chromium hydroxide, ferric malt, and ultramarine; inorganic body pigments such as mica, sericite, talc, kaolin, synthetic phlogopite, silicic acid anhydride (silica), magnesium carbonate, calcium carbonate, aluminum hydroxide, alumina, aluminum silicate, magnesium silicate, aluminum magnesium silicate, silicon carbide, barium sulfate, calcium silicate, zeolite, calcined calcium sulfate (calcined gypsum), calcium phosphate, hydroxyapatite, and boron nitride; inorganic fine particle powders such as titanium oxide, zinc oxide, and cerium oxide having an average primary particle size of 100 nm or less; luster powders such as bismuth oxychloride, mica titanium, iron oxide-coated mica, iron oxide-coated mica titanium, organic pigment-coated mica titanium, and aluminum powder; magnesium stearate, zinc stearate, N-acyl lysine, polyurethane, polystyrene, nylon, polymethyl methacrylate, and the like. cellulose, polymethylsilsesquioxane powder, organopolysiloxane elastomer powder, cellulose other than the above-mentioned cellulose powder, crystalline cellulose, polyethylene, crosslinked polymethyl (meth)acrylate, polyester, copolymer of styrene and acrylic acid, benzoguanamine, tetrafluoroethylene, organic pigments such as cellulose acetate; Red No. 201, Red No. 202, Red No. 204, Red No. 205, Red No. 220, Red No. 226, Red No. 228, Red No. 405, Orange No. 203, Orange No. 2 and organic pigments such as Red No. 04, Yellow No. 205, Yellow No. 401, and Blue No. 404; water-soluble dye lakes such as Red No. 3, Red No. 104, Red No. 106, Red No. 227, Red No. 230, Red No. 401, Red No. 505, Orange No. 205, Yellow No. 4, Yellow No. 5, Yellow No. 202, Yellow No. 203, Green No. 3, and Blue No. 1 (zirconium lake, barium lake, aluminum lake, etc.); and organic coloring pigments such as natural dyes and their lakes.
[0104] The powder Y other than the cellulose powder is preferably one that has been subjected to a surface hydrophobic treatment in terms of feel when used and cosmetic durability. Examples of such surface hydrophobic treatment include baking treatment with silicone such as methylhydrogenpolysiloxane and (dimethicone / methicone) copolymer, fatty acid treatment such as stearic acid, fatty acid metal soap treatment such as aluminum stearate and zinc stearate, acylated amino acid treatment, lipoamino acid treatment which is a mixed treatment of acylated amino acid (salt) and fatty acid (salt), fluorine treatment such as perfluoroalkyl phosphate, silylation treatment such as trimethylsilane, and acid ester treatment such as isostearyl sebacate.
[0105] In the solid powder cosmetic of this embodiment, it is preferable to contain an inorganic filler pigment that has been surface-hydrophobized, in order to improve the feel of use, such as the cosmetic durability and the ease of application and spreadability on the skin. A preferred inorganic filler pigment constituting the surface-hydrophobized inorganic filler pigment is a plate-like powder having a volume average particle size of 1 to 50 μm. Specific examples of the plate-like powder include talc, sericite, mica, synthetic phlogopite, and boron nitride. The surface hydrophobization treatment of the surface-hydrophobized inorganic filler pigment is preferably an acid ester treatment, an acylated amino acid treatment, or a lipoamino acid treatment, since these treatments are excellent in moldability, moist feeling, and cosmetic durability. Preferred specific examples of the surface hydrophobization treatment include isostearyl sebacate treatment, which is an acidic ester treatment, aluminum stearoyl glutamate treatment, which is an acylated amino acid treatment, and a combined treatment of palmitoyl proline / magnesium palmitoyl glutamate / sodium palmitoyl sarcosine / aluminum palmitate, which is a lipoamino acid treatment.
[0106] Among the powders Y other than the above-mentioned cellulose powders, particularly spherical inorganic and organic powders, such as spherical silica, polyurethane, polystyrene, nylon, polymethyl methacrylate, polymethyl silsesquioxane powder, organopolysiloxane elastomer powder, cellulose other than the above-mentioned cellulose powders, crystalline cellulose, cellulose acetate, etc., can be used to effectively conceal irregularities such as pores and fine wrinkles, resulting in a preferable finish.
[0107] The content of the powder containing the cellulose powder (i.e., the combination of the cellulose powder and the powder Y other than cellulose powder) is preferably 60 to 99.9% by mass, more preferably 70 to 99% by mass, and particularly preferably 80 to 95% by mass, based on the total amount of the solid powder cosmetic. If the content of the powder containing the cellulose powder is less than 60% by mass, the powder is difficult to remove onto a cosmetic puff such as a sponge, and the cosmetic film formed tends to be sticky.
[0108] When the solid powder cosmetic of the present embodiment contains a plate-shaped inorganic filler pigment, the content of the plate-shaped inorganic filler pigment is preferably 1 to 95% by mass, more preferably 5 to 90% by mass, and particularly preferably 10 to 85% by mass, based on the total amount of the solid powder cosmetic. Here, the plate-shaped refers to a particle shape in which, for example, the aspect ratio (length / thickness) is calculated by observing the particles using a SEM (scanning electron microscope) and measuring the thickness and length of each cross section. When the content of the plate-shaped inorganic filler pigment is low, the adhesion (adhesion to the skin) tends to be poor. On the other hand, when a large amount of the plate-shaped inorganic filler pigment is contained, there is a concern that the moldability and drop strength may be impaired. However, in the solid powder cosmetic of the present embodiment, even if the plate-shaped inorganic filler pigment is blended in an amount exceeding 70% by mass, the cellulose powder improves the moldability, so that the moldability and drop strength are excellent.
[0109] When the solid powder cosmetic of the present embodiment contains spherical inorganic powder and / or organic powder, the content of the spherical inorganic powder and / or organic powder is preferably 1 to 40 mass%, more preferably 3 to 35 mass%, and particularly preferably 5 to 30 mass% relative to the total amount of the solid powder cosmetic. Here, spherical refers to a shape having a circularity of 0.8 to 1, as determined by, for example, the static image analysis method described above. If the content is too low, the effect of hiding unevenness is poor, and if the content is too high, moldability is reduced.
[0110] (Moisturizer) The solid powder cosmetic of the present embodiment may contain a moisturizing agent. As the moisturizing agent, for example, one or a combination of two or more of polyhydric alcohols, sugars, sugar alcohols, amino acids, peptides, water-soluble polymers, etc. may be used. In addition, as the moisturizing agent, for example, glycerin, diglycerin, propylene glycol, 1,3-butylene glycol, 1,2-pentanediol, dipropylene glycol, 1,3-propanediol, 1,2-hexanediol, heptanediol, 1,2-octanediol, ethylhexylglycerin, xylitol, sorbitol, maltitol, chondroitin sulfate, hyaluronic acid, collagen, sodium lactate, dl-pyrrolidone carboxylate, Rosa roxburghii extract, Achillea millefolium extract, Melilot extract, etc. may be used.
[0111] (others) The solid powder cosmetic of the present embodiment may contain, in addition to the powders, oils, and moisturizers described above, various ingredients that are typically contained in cosmetics, such as water-soluble ultraviolet absorbers, preservatives, antibacterial agents, fragrances, antioxidants, pH adjusters, chelating agents, cooling agents, anti-inflammatory agents, skin-beautifying ingredients, vitamins, amino acids, nucleic acids, and inclusion compounds.
[0112] (Applications, etc.) The solid powder cosmetic of the present embodiment is particularly suitable for use as a makeup cosmetic, such as pressed powder (solid white powder), powder foundation, wet / dry foundation, wet cake foundation, powder eye shadow, blusher, face color, eyebrow ink, and the like. EXAMPLES
[0113] The results of various tests carried out are shown below. The cellulose powder, silicone powder, and silica powder used in the test examples and reference examples were obtained as follows. Not chemically modified The fine fibrous cellulose used was "ELLEX (registered trademark)-S" manufactured by Daio Paper Co., Ltd., and the glycerin used was special grade manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0114] (Cellulose powder A) Fine fibrous cellulose was mixed to a solid content of 70% by mass and glycerin was mixed to a solid content of 30% by mass to obtain a fine fibrous cellulose aqueous dispersion with a concentration of 3.0%. The aqueous dispersion was spray-dried using a spray dryer (Pris Co., Ltd. "P-260") to obtain cellulose powder A. The average particle size of cellulose powder A was 13.5 μm. An SEM image of cellulose powder A is shown in FIG. 1.
[0115] (Cellulose powder B) Fine fibrous cellulose was mixed with water to a solid content of 70% by mass and glycerin was mixed with water to a solid content of 30% by mass to obtain a fine fibrous cellulose aqueous dispersion. The aqueous dispersion was dried in a double drum dryer (Johnson Boiler's "John Milder JM-T type") at a drum rotation speed of 3 rpm and a drum surface temperature of 135°C to obtain a dried body, which was then pulverized to obtain cellulose powder B. An SEM image of cellulose powder B is shown in Figure 2.
[0116] (Cellulose powder C) As cellulose powder C, Fujifilm Wako Pure Chemical Industries, Ltd.'s product "Wako First-class Cellulose, Powder, 38 μm (400 mesh) passing" was used. Note that the cellulose raw material of cellulose powder C is not the fine fibrous cellulose used in the present invention. An SEM image of cellulose powder C is shown in FIG. 3.
[0117] (Cellulose powder D) "CELLULOBEADS" manufactured by Daito Kasei Kogyo Co., Ltd. was used as cellulose powder D. The cellulose raw material of cellulose powder D is not the fine fibrous cellulose used in the present invention. An SEM image of cellulose powder D is shown in FIG.
[0118] (Cellulose powder E) The fine fibrous cellulose was dispersed in water to a concentration of 3.0% based on the solid content to obtain a fine fibrous cellulose aqueous dispersion. No additives were added. The aqueous dispersion was spray-dried using a spray dryer (Pris Co., Ltd. "P-260") to obtain cellulose powder E.
[0119] (Silicone powder) The silicone powder used was "KSP-100" manufactured by Shin-Etsu Chemical Co., Ltd. Figure 5 shows an SEM image of the silicone powder.
[0120] (Silica powder) The silica powder used was "CHIFFONSIL P-3R" manufactured by JGC Catalysts and Chemicals Co., Ltd. Figure 6 shows an SEM image of the silica powder.
[0121] The physical properties of the powder obtained were measured. The measured physical properties are shown in Table 1. The physical properties were measured according to the following procedure.
[0122] The bulk density was measured by the static method according to JIS-K-5101-12-1 (2004).
[0123] The moisture content was measured by leaving 5 g of powder for 24 hours using the heat drying method, and determining the weight before and after drying. More specifically, the powder that had been left for 24 hours or more under a humidity of 50% (i.e., the powder before drying) was used, and dried at a temperature of 105°C for 24 hours to obtain the powder after drying. The moisture content was calculated from the weight of the powder before drying and the weight of the powder after drying using the following formula [Equation 1]. [Number 1] (Moisture content (%)) = [((Weight of powder before drying) - (Weight of powder after drying)) / (Weight of powder after drying)] x 100
[0124] The compressive strength was measured using a micro component strength evaluation device, Micro Autograph "MST-I", manufactured by Shimadzu Corporation, in accordance with JIS R1639-5 "Fine ceramics - Measurement methods for granule characteristics - Part 5: Single granule crushing strength".
[0125] The specific surface area (BET multipoint method) was measured using a specific surface area measuring device, "TriStar II 3020 N2 gas" manufactured by Shimadzu Corporation.
[0126] The cumulative distribution of equivalent circle diameter (number basis, cumulative 50% diameter), cumulative distribution of equivalent circle diameter (volume basis, cumulative 50% diameter), aspect ratio, and circularity were measured using the Morphologi 4 product of Spectris Corporation.
[0127] The mode diameter (most frequent diameter), median diameter (cumulative 50% diameter), average particle diameter, cumulative 10% diameter, and cumulative 90% diameter were measured using a measuring device conforming to ISO-13320 (2009), specifically, the laser diffraction / scattering type particle size distribution measuring device (particle size distribution) "LA-960V2", using a dry method without removing the moisture adhering to the cellulose powder.
[0128] The pulp viscosity and average degree of polymerization of cellulose were measured for each of the obtained cellulose powders A to D. The pulp viscosity was a value measured in accordance with TAPPI T 230. The average degree of polymerization of cellulose refers to the viscosity average degree of polymerization measured in accordance with JIS-K6726.
[0129] [Table 1]
[0130] (Test Examples and Reference Examples) The powders obtained as described above were blended in the blending ratios shown in Tables 2 and 3. Specifically, for Test Examples 1 and 2 and Reference Examples 1 to 3 in Table 2, any one of the powders of Component Nos. 1 to 5 and Component Nos. 6 to 13 were mixed using a sample mill (Kyoritsu Riko Co., Ltd. product "SK-M10") at 10,000 rpm (scale 50) for 10 seconds to obtain a mixture that was an intermediate product. Next, Component Nos. 15 to 19, which had been mixed in advance and uniformly, were mixed with the above-mentioned mixture and further mixed for 30 seconds using the sample mill to obtain powder compositions for Test Examples 1 and 2 and Reference Examples 1 to 3, respectively.
[0131] For Test Example 3 and Reference Examples 4 to 7 in Table 3, any one of the powders of Component Nos. 1 to 4 and Component Nos. 5 to 13 were mixed using a sample mill (Kyoritsu Riko Co., Ltd. product "SK-M10") at 10,000 rpm (scale 50) for 10 seconds to obtain a mixture that was an intermediate product. Next, Component Nos. 14 to 19 (Component Nos. 14 to 20 for Reference Example 7) that had been mixed uniformly in advance were mixed with the above-mentioned mixture and further mixed for 30 seconds using the above-mentioned sample mill to obtain powder compositions for Test Example 3 and Reference Examples 4 to 7, respectively.
[0132] [Table 2]
[0133] [Table 3]
[0134] Each of the powder compositions obtained by the above-mentioned operating procedures was filled into an aluminum metal dish having a diameter of 54 mmφ, and pressed using a press (a semi-automatic press "SSPP (hydraulic cylinder diameter 80 mmφ)" manufactured by Sanshin Seiki Co., Ltd.) at the press pressure shown in Table 4 to obtain Test Examples 1 to 3 and Reference Examples 1 to 7. The hardness of the obtained Test Examples 1 to 3 and Reference Examples 1 to 7 was measured. The hardness was measured using an "Olsen Hardness Tester" manufactured by Ueshima Seisakusho, which is a constant-load indentation hardness tester, under the condition of a load of 1 pound (=453.59 g). The hardness measurement results are shown in Table 4.
[0135] [Table 4]
[0136] (Performance evaluation test) Performance evaluation tests were conducted on the test examples and reference examples. The test items for the performance evaluation tests were drop strength, ease of removal onto a puff, smoothness when applied to the skin, moist feeling when applied to the skin, and adhesion to the skin. The results of the performance evaluation tests are shown in Table 5.
[0137] [Table 5]
[0138] The drop strength test was carried out according to the following procedure. (1) From a height of 30 cm above a horizontally placed concrete block plane, the test example or reference example was allowed to freely fall with the flat surface of the test example or reference example kept horizontal, causing it to collide with the concrete block plane. (2) The above procedure (1) was repeated until the test example or reference example cracked. (3) If the test example or reference example broke after 11 or more trials under (1) and (2) above, it was judged as A, if it was 8 to 10, it was judged as B, if it was 5 to 7, it was judged as C, and if it was 4 or less, it was judged as D. Regarding the notation of drop strength in Table 5, for example, if the test example or reference example broke after 10 trials, it was judged as "B(10)", etc.
[0139] The tests for ease of removal onto the puff, smoothness when applied to the skin, moist feeling when applied to the skin, and adhesion to the skin were carried out as follows. A panel of 10 female specialists used the test sample and the reference sample and evaluated them.
[0140] Specifically, participants were asked to rate the ease of removal onto the puff, the smoothness when applied to the skin, the moist feeling when applied to the skin, and the adhesion to the skin on a three-point scale: good (a score of 2), neutral (a score of 1), and bad (a score of 0). The average score was calculated, and an A was given if the average score was 1.5 or higher, a B if it was 1.2 or higher but less than 1.5, a C if it was 0.5 or higher but less than 1.2, and a D if it was less than 0.5.
[0141] The results in Table 5 reveal the following. Comparing Test Examples 1 and 2 and Reference Examples 1 to 3, which have the same powder amount (90% by mass) and the same total amount of oil and moisturizer (10% by mass), Test Example 1, which contains cellulose powder A, was excellent in all items, whereas Reference Example 1, which contains commercially available spherical cellulose, and Reference Example 3, which contains commercially available spherical silica, were significantly inferior in the items of ease of removal onto puff, moist feeling upon application, and adhesion to skin. Reference Example 2, which contains silicone elastomer, an elastic powder, had cosmetic performance such as moist feeling equivalent to Test Example 1, but its drop strength was significantly inferior to Test Example 1. Test Example 2, which contains cellulose powder B with a larger average particle size, was excellent in drop strength, but was slightly inferior to Test Example 1 in the items of ease of removal onto puff, smoothness upon application, moist feeling upon application, and adhesion to skin.
[0142] Comparing Test Example 3 and Reference Examples 4 to 7, which have the same powder amount (95.95% by mass) and the same total amount of oil and moisturizer (4.05% by mass), Test Example 3 was excellent in all items even when the total amount of oil and moisturizer was small, whereas Reference Examples 4 to 6 all had insufficient drop strength. On the other hand, Reference Example 4, which contains commercially available cellulose powder C, had poor drop strength and was slightly inferior in moist feeling, etc. Furthermore, Reference Example 6, which contains cellulose particles E produced from fine fibrous cellulose without additives, had poor drop strength and was slightly inferior in smoothness, moist feeling, etc.
[0143] Reference Example 7 uses cellulose powder E, which does not contain any additives and is made of aggregates containing fine fibrous cellulose, and although the drop strength is improved, the smoothness and the feeling of attachment to the skin are inferior. Note that the glycerin contained in Reference Example 7 is added to the mixture, which is the intermediate product, as one component of the moisturizing agent, and does not constitute the aggregates. [Industrial Applicability]
[0144] The present invention can be used as a cosmetic material such as a primer, face powder, foundation, or base makeup cosmetic material.
Claims
1. The cellulose powder has an average particle size of 1 to 25 μm and an aspect ratio of 0.6 to 0.
9. The cellulose powder is an aggregate containing an additive and chemically unmodified fine fibrous cellulose having an average fiber width of 1 to 500 nm and an average fiber length of 0.3 to 20 μm, and has a specific surface area of 1.0 m 2 / g or more, the additive is one or a combination of two or more selected from the group consisting of polyhydric alcohols, polysaccharides, water-soluble polymers, and surfactants, and the content of the additive in the cellulose powder is 1 to 49% by mass, The powder containing the cellulose powder is contained in an amount of 70 to 99% by mass, The cellulose powder is contained in an amount of 3 to 60% by mass. A solid powder cosmetic preparation characterized by:
2. The cellulose powder is formed by agglomeration of the fine fibrous cellulose. The solid powder cosmetic according to claim 1.
3. Contains 0.1 to 25 mass% oil, The solid powder cosmetic according to claim 1.
4. The additive is a polyhydric alcohol. The solid powder cosmetic according to claim 1.
5. The cellulose powder has a moisture content of 1 to 15% in an atmosphere with a humidity of 50%. The solid powder cosmetic according to claim 1.
6. The cellulose powder has a bulk density of 0.5 g / cm 3 Below is the The solid powder cosmetic according to claim 1.
7. The cellulose powder has a pulp viscosity of cellulose of 1.0 to 7.0 mPa·s. The solid powder cosmetic according to claim 1.
8. It is a base makeup cosmetic product. The solid powder cosmetic according to claim 1.
Citation Information
Patent Citations
Solid powdery cosmetic containing organic powder
JP2002080325A
Cosmetic
JP2017048181A
Solid powder cosmetic
JP2017186323A
Powder cosmetic
JP2021098674A
Makeup cosmetic
WO2018194050A1