Direct reduced iron manufacturing equipment and manufacturing method
The method and equipment for direct reduced iron production optimize carbon content and reduction efficiency by using an autothermal reformer and methane generation, separating reduction and cooling zones, and controlling gas parameters, addressing the challenges of external thermal reformers and maintaining high-quality iron production.
Patent Information
- Application Number
- JP2021539817
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-23
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-04-23
AI Technical Summary
Existing direct reduction ironmaking methods require expensive alloy tubes for external thermal reformers, suffer from carbon precipitation and metal dusting issues, and struggle to maintain optimal carbon content and reduction efficiency without increasing equipment costs and downtime.
A method and equipment that eliminates the need for external thermal reformers by using an autothermal reformer, adjusting hydrocarbon concentration, gas pressure, and temperature to control carbon content and reduction efficiency, incorporating a methane generator to recycle carbon within the system, and separating reduction and cooling zones to optimize carbon addition.
This approach reduces equipment costs, minimizes maintenance, enhances reduction efficiency, and maintains high carbon content in reduced iron, addressing issues like carbon precipitation and metal dusting while improving thermal efficiency and reducing emissions.
Smart Images

Figure 0007555125000002 
Figure 0007555125000003 
Figure 0007555125000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a direct reduced iron (DRI) manufacturing facility and method, which does not use an externally heated reformer, can adjust the carbon content of the reduced iron over a wide range independent of the conditions in the reduction zone, and can efficiently carry out reforming and reduction without causing problems such as metal dusting in a circulation gas preheater, and also relates to a direct reduced iron manufacturing facility and method in which hydrogen is supplied as a main reducing agent to reduce iron oxide. [Background technology]
[0002] In addition to the blast furnace ironmaking process, there is also a method called the direct reduction ironmaking process as a method for producing metallic iron in a vertical reduction furnace (shaft furnace) by reducing iron oxide raw materials (raw materials) such as iron lump ore or fired pellets made from iron ore powder.
[0003] Direct reduction ironmaking processes are typified by the Midrex process shown in Patent Document 1 and the HYL process shown in Patent Document 2. These processes involve introducing a reducing gas containing hydrogen (H2) and carbon monoxide (CO) as main components into a vertical reduction furnace to reduce iron oxide in the solid phase, thereby producing solid metallic iron.
[0004] The reducing gas, which is mainly composed of hydrogen and carbon monoxide, is introduced into the vertical reduction furnace and reacts with iron oxide in the reduction zone, and some of it removes oxygen from the iron oxide to produce water vapor (H2O) and carbon dioxide (CO2).
[0005] In the Midrex process, the gas discharged from the vertical reduction furnace (top gas) is cleaned and cooled in a scrubber. After that, a portion of the gas is pressurized, and new hydrocarbon-containing gas is added to the gas, which is then reformed in the reformer for recycling.
[0006] In the HYL process, a portion of the top gas that has been similarly de-dusted and cooled is mixed with newly reformed gas made from steam and hydrocarbon-containing gas, heated in an external combustion type circulating gas heater (reheater), and introduced into a vertical reduction furnace for circulating use.
[0007] When the produced reduced iron is cooled and discharged, a cooling zone is provided below the reduction zone, and a gas for cooling (cooling gas) is introduced into the cooling zone to cool the reduced iron. The cooling gas used for this cooling is discharged from the middle part of the vertical reduction furnace below the reducing gas inlet part of the vertical reduction furnace, where it is cleaned of dust and cooled in a scrubber, then pressurized and recycled.
[0008] In either case, to produce the reducing gas, the gas is reformed by heating it to over 900°C in an externally heated reformer filled with a catalyst. The reformer tubes used in these externally heated reformers require expensive alloy tubes because they are exposed to high temperatures above the reformed gas temperature.
[0009] In the Midrex process, a circulating gas containing carbon dioxide and water vapor is mixed with a hydrocarbon-containing gas under low pressure, for example, at a pressure of 350 kPa(A) or less, and after preheating, the mixture is passed through an externally heated reformer to produce reformed gas.
[0010] As mentioned above, the Midrex process uses a low reforming pressure of about 350 kPa (A), so carbon does not deposit on the reformer catalyst and reforming can be performed in a unit operation until the gas reduction degree (R-Value = (H2 + CO) / (H2O + CO2)) reaches 10 to 12 or more, which is necessary to achieve efficient reduction of iron oxide.
[0011] In the HYL method, steam and a hydrocarbon-containing gas are mixed under high pressure, for example at a pressure of 700 kPa (A) or more, preheated, and then passed through an externally heated reformer to produce a reformed gas.
[0012] In the case of the HYL method, because of the high pressure, in order to prevent carbon deposition in the externally heated reformer, the reforming is carried out with excess steam, for example, a mixed gas with an S / C (Steam / Carbon) ratio of 3 or more, and the excess steam components after reforming are removed. For this purpose, the gas is first cooled, some of the steam components are removed, and then it is reheated.
[0013] Therefore, the HYL process requires both an externally heated reformer and an externally fired circulation gas heater (reheater).
[0014] In either case, very expensive alloys must be used for the tubes of the externally heated reformer or the external combustion type circulating gas heater, resulting in a large initial investment.
[0015] In addition, in some cases, the tubes need to be replaced within a short period of time due to damage caused by metal dusting caused by carbon deposition on the surface of the alloy tubes.Even if such damage does not occur within such a short period of time, the tubes need to be replaced every 5 to 10 years due to high heat loads, and the replacement costs and opportunity loss due to production stoppages associated with the replacement have become problems.
[0016] In the case of low-pressure operation as in the Midrex process, the problems of carbon deposition and metal dusting are avoided, but as mentioned above, the reformer tubes need to be replaced every 5 to 10 years, and because of the low pressure, the carbon content of the reduced iron is at most around 3%, and generally remains at around 1.5% to 2%.
[0017] In recent years, hydrogen reduction has been considered as a means of reducing CO2 emissions from the steelmaking process. However, when directly reducing iron oxide with hydrogen alone, it is impossible to add carbon to the reduced iron product because there is no carbon source.
[0018] On the other hand, in the steelmaking process, an appropriate amount of carbon in the molten iron is essential to maintain the quality of the final product and to keep the solidification temperature low. In addition, current electric furnace reduced iron melting is aimed at shortening the melting time by oxygen blowing, reducing electricity consumption, and improving product quality, so the carbon content in reduced iron is desired to be 2% or more, preferably 3% or more. [Prior art documents] [Patent documents]
[0019] [Patent Document 1] U.S. Pat. No. 3,764,123 [Patent Document 2] U.S. Pat. No. 4,336,063 [Patent Document 3] U.S. Patent No. 5,858,057 Summary of the Invention [Problem to be solved by the invention]
[0020] In view of the above technical background, as disclosed in Patent Document 3, a method represented by the HYL ZR method is proposed that does not use an externally heated reformer, which requires a large initial investment, thereby reducing the initial investment amount and the replacement cost of the externally heated reformer tube.
[0021] In this method, it is proposed that the oxidizing gases H2O and CO2 are removed from the top gas discharged from a vertical reduction furnace, and the resulting gas is mixed with a hydrocarbon-containing gas and water vapor, and then the resulting mixture is heated to about 850°C to 1000°C for circulating use.
[0022] It has also been proposed to mix oxygen into the heated mixed gas, heat it to about 900°C to 1150°C using the heat of partial combustion, and then feed it into the furnace.
[0023] In this method, gas reforming to a degree of reduction suitable for efficient iron reduction (for example, R-value 10 or more) and reduction of iron oxide with the reformed gas are carried out in one furnace. That is, in this method, the required heat is provided by preheating the circulating gas and the heat of partial combustion of mixed oxygen.
[0024] Therefore, the mixed gas is heated to the above-mentioned temperature range (approximately 850°C to 1000°C) in an external combustion type circulating gas preheater (preheater), and then oxygen is mixed in and the temperature is raised to approximately 900°C to 1150°C using the heat of partial combustion.
[0025] The gas heated by this preheater is a gas in which a hydrocarbon-containing gas and an appropriate amount of H2O have been added again to a gas mainly composed of CO and H2 from which most of the CO2 and H2O have been removed as described above.
[0026] The main components of this gas are CO, H2, and CH4, and this gas has a strong carburizing property. Therefore, it has been reported that when this gas is heated in a preheater to a high temperature, for example, 850°C or higher as disclosed in Patent Document 3, it causes problems such as carbon deposition on the tube surface of the preheater and carburization and metal dusting on the ferroalloy.
[0027] Here, the reforming reaction is a reaction in which the volume increases, as typified by CH4+H2O=CO+3H2 and CH4+CO2=2CO+2H2, and in order to cause this reforming reaction under high pressure conditions (e.g., 700 kPa(A) or higher), a higher hydrocarbon gas partial pressure is required. Therefore, it is necessary to mix a large amount of hydrocarbon-containing gas, and heating this high-pressure hydrocarbon gas to a high temperature can cause problems such as carbon deposition, carburization on ferroalloys, and metal dusting.
[0028] In order to avoid this problem, it is effective to lower the circulating gas pressure in the preheater and at the same time lower the hydrocarbon concentration, or to lower the preheating temperature of the circulating gas, but this has the following problems.
[0029] Patent Document 3 proposes increasing the carbon content of reduced iron by causing a carbon precipitation reaction, which occurs simultaneously with reforming, to occur on the metallic iron of the reduced iron in the furnace.
[0030] However, if the carbon precipitation problem in the preheater is avoided by lowering the gas pressure and the hydrocarbon concentration, the carbon precipitation reaction on the metallic iron surface and the carburization reaction with the metallic iron in the reducing furnace are also suppressed, resulting in a decrease in the carbon content in the product reduced iron.
[0031] On the other hand, if the circulation gas preheating temperature is lowered to avoid the problems of carbon deposition in the preheater and carburization and metal dusting on the ferroalloy, the amount of heat that can be provided by preheating decreases. In order to compensate for this, it becomes necessary to mix a large amount of oxygen- and hydrocarbon-containing gas in the downstream, and the temperature of the gas introduced into the reducing furnace increases.
[0032] In this way, when the temperature at which the raw materials are charged into the reduction furnace is raised to a high temperature, for example, from 900°C to about 1150°C as disclosed in Patent Document 3 or higher, problems such as pulverization in the furnace, fusion (clustering) of reduced iron particles, and damage to refractories by pulverized iron can occur depending on the raw materials.
[0033] Conversely, if the temperature at which the fuel is fed into the reduction furnace is suppressed to a level that does not cause problems such as fusion within the furnace, the temperature after the reforming reaction in the furnace will also fall, and the degree of reduction of the reformed gas will also decrease, making it difficult to efficiently reduce the iron oxide.
[0034] In view of the above circumstances, an object of the present invention is to provide a process for producing reduced iron by reduction with carbon monoxide and / or hydrogen, which does not use an externally heated reformer, which is independent of the reduction conditions and, for example, can adjust the carbon content in the reduced iron to a desired amount without decreasing it even in hydrogen reduction, which can maintain high temperature and degree of reduction of the reducing gas after reforming in the reducing furnace while maintaining the gas temperature at the inlet of the reducing furnace at a temperature that does not cause pulverization in the furnace, fusion (clustering) between reduced iron, damage to refractories by pulverized iron, etc., and which can solve the problems of carbon deposition in an externally fired circulating gas preheater (preheater) and carburization and metal dusting on ferroalloy, and which has high equipment reliability and is capable of producing high quality reduced iron with good reduction efficiency.
[0035] Another object of the present invention is to provide a process for producing direct reduced iron containing the amount of carbon components required for the steelmaking process, by externally compensating for only the amount of carbon consumed by circulating the carbon components within the system, even when hydrogen is used as the main raw material for the reducing gas required for the direct reduced iron production process. [Means for solving the problem]
[0036] The first feature of the facility and method is that it produces direct reduced iron (Cold DRI) by reducing iron oxide raw material in a vertical reduction furnace and then cooling it, and that it has the following features: it can adjust the hydrocarbon concentration in a cooling gas to 50% or more, preferably 70% or more, and adjust the flow rate of the cooling gas introduced into the reduction furnace, and it has a cooling gas aftercooler to adjust the inlet temperature of at least a part of the cooling gas to the inlet temperature of the reduction furnace, preferably a chiller-type aftercooler (cooling gas chiller) that can cool to wet-bulb atmospheric temperature +3 to 4°C or less, or an aftercooler that introduces a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like to supply a low-temperature cooling gas to the reduction furnace.
[0037] A second feature of this facility and method is that it produces direct reduced iron (Cold DRI) by reducing iron oxide raw material in a vertical reduction furnace and then cooling it, in which the hydrocarbon concentration in the cooling gas is adjusted to 50% or more, preferably 70% or more, and the reduction zone and the cooling zone are separated from each other, and the two zones are connected by a chute through which the reduced iron falls, and are also connected by a separate gas duct so that the cooling gas can be introduced from the cooling zone to at least one of the reduction zone and the circulation gas line without impeding the descent of the reduced iron.
[0038] A third feature of the equipment and method is that it produces direct reduced iron (Cold DRI) by reducing iron oxide raw material in a vertical reduction furnace and then cooling the reduced iron, and that it provides an intermediate cooling zone between the reduction zone and the cooling zone, arranges two cooling gas loops, and adjusts the outlet temperature of the upper cooling gas (intermediate cooling zone) to be higher than the outlet temperature of the lower cooling gas (cooling zone).
[0039] A fourth feature of the equipment and method for producing direct reduced iron (DRI) by reducing iron oxide raw material in a vertical reduction furnace is that the equipment and method include a moisture adjustment device such as a scrubber that adjusts moisture by removing a portion of moisture (HO), which is an oxidizing component, from the top gas discharged from the vertical reduction furnace, a first gas mixing device that pressurizes the moisture-adjusted gas in order to circulate it, and can adjust the inlet gas temperature, outlet gas temperature, and reduction degree of the outlet gas of a downstream autothermal reformer (autothermal reformer) so that they are within appropriate ranges, and an autothermal reformer that reforms the circulation gas in which the oxygen-containing gas and the hydrocarbon-containing gas are mixed, using its own energy, to increase the reduction degree of the gas.
[0040] A fifth feature of the equipment and method for producing direct reduced iron (DRI) by reducing iron oxide raw material in the vertical reduction furnace is that it has a second gas mixing device that mixes an oxygen-containing gas and a hydrocarbon-containing gas downstream of the autothermal reformer in order to further reform the gas fed into the reduction furnace in the vertical reduction furnace, improve the degree of reduction, and increase the temperature of the reducing gas.
[0041] A sixth feature of the equipment and method for producing direct reduced iron (DRI) by reducing iron oxide raw material in the above-mentioned vertical reduction furnace is that it has a CO2 remover that removes water vapor from the top gas discharged from the vertical reduction furnace and removes part or all of carbon dioxide (CO2), another oxidizing component, and has equipment that can adjust the CO2 concentration at the inlet of the autothermal reformer.
[0042] A seventh feature of the equipment and method for producing direct reduced iron (DRI) by reducing an iron oxide raw material in the above-mentioned vertical reduction furnace is that the gas pressure at the inlet of the autothermal reformer is adjusted to less than 600 kPa (A), preferably less than 500 kPa (A), and more preferably less than 350 kPa (A) in order to avoid carbon deposition problems in the autothermal reformer, thereby producing a reformed gas with a high degree of reduction and avoiding the problem of carbon deposition in the autothermal reformer.
[0043] An eighth feature of the equipment and method for producing direct reduced iron (DRI) by reducing iron oxide raw materials in the above-mentioned vertical reduction furnace is that it has a heat exchanger that preheats the circulating gas before mixing the circulating gas with an oxygen-containing gas, and that the temperature of the circulating gas after preheating is set to less than 850°C, preferably less than 700°C, and more preferably less than 550°C in order to eliminate problems due to carbon deposition and carburization in the heat exchanger.
[0044] A ninth feature of the equipment and method for producing direct reduced iron (DRI) by reducing an iron oxide raw material in the above-mentioned vertical reduction furnace is that the amount of oxygen-containing gas and the amount of hydrocarbon-containing gas to be mixed are adjusted so that the gas temperature at the inlet of the autothermal reformer is adjusted to 1500°C or less, preferably 1400°C or less, and the gas temperature at the outlet is adjusted to 700°C or more, preferably 750°C or more, more preferably 800°C or more.
[0045] A tenth feature of the equipment and method for producing direct reduced iron (DRI) by reducing an iron oxide raw material in the above-mentioned vertical reduction furnace is that the gas temperature at the inlet of the autothermal reformer is adjusted to 1500°C or less, preferably 1400°C or less, and the amount of oxygen-containing gas and the amount of hydrocarbon-containing gas mixed are adjusted so that the gas temperature at the outlet is 700°C or more, preferably 750°C or more, more preferably 800°C or more, and the inlet gas of the vertical reduction furnace has a desired reduction degree, and the autothermal reformer is provided in multiple stages.
[0046] An eleventh feature of the equipment and method for producing direct reduced iron (DRI) by reducing iron oxide raw material in the vertical reduction furnace is that it includes a methane generator that reacts carbon dioxide and hydrogen in the presence of a catalyst to produce methane, generates methane using carbon dioxide recovered by a CO2 remover and hydrogen introduced from outside the system, and uses the generated methane as a hydrocarbon gas for producing the reducing gas or as a hydrocarbon gas to be mixed with a cooling gas for cooling the reduced iron.
[0047] More specifically, the present invention has the following configuration.
[0048] One embodiment of the present invention is an equipment for reducing an iron oxide raw material in a vertical reduction furnace, and then cooling it to produce and discharge direct reduced iron (Cold DRI). The Cold DRI production equipment includes a vertical reduction furnace (shaft furnace) for reducing the iron oxide raw material, a cooling gas scrubber (direct contact type water-cooled cooling gas cooler) for removing dust and cooling the cooling gas for cooling the reduced iron, a cooling gas compressor, and a cooling gas aftercooler, preferably a chiller type aftercooler or an aftercooler that introduces a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like to supply a low-temperature cooling gas to the reduction furnace.
[0049] The cooling gas aftercooler, preferably a chiller-type aftercooler or an aftercooler which introduces a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like to supply a low-temperature cooling gas to a reducing furnace, is an aftercooler which can adjust the temperature of at least a part of the cooling gas to be introduced into the furnace to atmospheric wet-bulb temperature +3 to 4°C or lower, for example, 35°C or lower.
[0050] In another form of Cold DRI production equipment, the reduction zone and the cooling zone of the vertical reduction furnace are separated from each other, and a gas duct (cooling gas connection duct) capable of introducing a cooling gas into at least one of the reduction zone and the circulation gas line is provided in addition to the chute for lowering the reduced iron. The cooling gas introduced into the circulation gas line is preferably mixed with at least one of the reducing gas introduced into the circulation gas line, particularly into the vertical reduction furnace, and the gas flowing upstream of the reformer provided in the reduced iron production equipment. Note that this reformer includes not only an autothermal reformer but also an externally heated reformer.
[0051] In another type of Cold DRI manufacturing equipment, an intermediate cooling zone is provided between the reduction zone and the cooling zone, and the intermediate cooling zone and the cooling zone each have a gas loop. The temperature and flow rate of the cooling gas in the upper gas loop provided in the intermediate cooling zone and the lower gas loop provided in the cooling zone can be controlled separately.
[0052] In a preferred embodiment of the Cold DRI production facility, a dry cooling gas culverter and a cooling gas heat exchanger such as a hydrocarbon-containing gas preheater and a boiler are provided to recover heat from the high-temperature outlet cooling gas.
[0053] In addition, a dry booster is installed in the intermediate cooling zone.
[0054] Another type of reduced iron production equipment includes a vertical reduction furnace (shaft furnace) that reduces iron oxide raw material, a top gas scrubber that removes dust, cools, and removes moisture from the gas (top gas) discharged from the shaft furnace after reduction, and adjusts it; a circulating gas compressor; a first gas mixing device that mixes a high-concentration oxygen-containing gas such as pure oxygen and a hydrocarbon-containing gas; an autothermal reformer that reforms the gas; a cooling gas scrubber that removes dust and cools the cooling gas used to cool the reduced iron; and a cooling gas compressor.
[0055] In a preferred embodiment of a direct reduced iron production facility, a second gas mixing device is provided that mixes a high-concentration oxygen-containing gas and a hydrocarbon-containing gas downstream of the autothermal reformer so as to promote in-situ reforming in the vertical reduction furnace.
[0056] A more preferred form of direct reduced iron production facility is equipped with a CO2 remover that removes water vapor from the top gas discharged from the vertical reduction furnace and also removes some or all of carbon dioxide (CO2), another oxidizing component, from the top gas, thereby adjusting the CO2 concentration at the inlet of the autothermal reformer.
[0057] A more preferred embodiment of the direct reduced iron production facility includes an autothermal reformer in which the oxidation reaction and the reforming reaction proceed in a single reformer.
[0058] A more preferred embodiment of the direct reduced iron production facility is equipped with an autothermal reformer arranged in a U-shape or V-shape, with used catalyst discharged from the bottom and new catalyst filled from the top, making catalyst replacement easy. Also, a more preferred embodiment of the direct reduced iron production facility is equipped in the front stage with a similar inert catalyst packed bed filled with alumina balls or the like capable of removing fine solids such as soot and dust, in order to reduce the frequency of catalyst replacement.
[0059] In a further preferred embodiment of a direct reduced iron manufacturing facility, a heat exchanger (at least one of a top gas heat recovery heat exchanger and a circulation gas preheater (preheater)) is provided to exchange heat between the top gas and the gas at the outlet of the CO remover in order to adjust the preheat temperature of the circulation gas.
[0060] In a further preferred embodiment of a direct reduced iron production facility, a reformed gas cooler is provided for adjusting the temperature of the gas introduced into the furnace so as to prevent problems such as powdering in the furnace, fusion (clustering) of reduced iron particles, and damage to refractories due to powdered iron depending on the raw materials.
[0061] In a further preferred embodiment of the direct reduced iron production facility, a reformed gas mixer is provided for mixing the cooled reformed gas and the hydrocarbon gas into the furnace input gas line.
[0062] In a further preferred embodiment of the direct reduced iron production facility, a methane generator is provided which has a reactor for producing methane from CO2 and hydrogen and mixes hydrogen with at least a portion of the carbon dioxide recovered by the CO2 remover to produce methane. At least a portion of the methane produced in the methane generator can be used as a hydrocarbon gas for producing a reducing gas or as a hydrocarbon gas to be mixed with a cooling gas for cooling the reduced iron.
[0063] The present invention also relates to a method for producing direct reduced iron by contacting an iron oxide raw material with a reducing gas in a vertical reduction furnace. The method for producing direct reduced iron includes a moisture adjustment step of adjusting the top gas discharged from the vertical reduction furnace by removing a portion of the moisture, a gas mixing step of mixing the moisture-adjusted gas with an oxygen-containing gas and a hydrocarbon-containing gas, and a reformed gas production step of reforming the mixed gas with its own energy to produce a reformed gas. Effect of the Invention
[0064] In a facility for producing directly reduced iron (Cold DRI) by reducing and cooling iron oxide raw materials in a vertical reduction furnace, the hydrocarbon concentration in the cooling gas is set to 50% or more, preferably 70% or more, and the inlet temperature of this cooling gas into the reduction furnace is lowered by a cooling gas aftercooler, preferably a chiller-type aftercooler (cooling gas chiller) or an aftercooler that introduces a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like to supply low-temperature cooling gas to the reduction furnace, and at the same time, the flow rate of the cooling gas input into the furnace is reduced, thereby making it possible to cool reduced iron to a desired temperature and increase the cooling gas outlet temperature.
[0065] As a result, the reduced high-temperature reduced iron comes into contact with sufficiently heated hydrocarbon gas in the upper part of the cooling zone, and regardless of the reduction conditions, it is possible to increase the carbon content in the reduced iron to 3% or more even in the case of hydrogen reduction, when the pressure in the reduction zone is low, and when the hydrocarbon partial pressure is low.
[0066] In other words, by adjusting the temperature and flow rate of the cooling gas, the carbon content of the reduced iron can be controlled without being largely dependent on the gas composition and pressure in the reduction zone. This makes it possible to supply reduced iron with an optimal temperature and carbon content according to the transport equipment to the electric furnace and the operating conditions of the electric furnace, regardless of the production method and conditions of the reformed gas.
[0067] In addition, when the reduction zone and the cooling zone are separated from each other, a gas duct (a gas duct for the reduction zone or a gas duct for the circulation gas line) is arranged so that cooling gas can be introduced from the cooling zone to the reduction zone or the circulation gas line, separately from the descent chute for reduced iron.
[0068] The cooling gas is heated by exchanging heat with the reduced iron in the cooling zone to cool the reduced iron. At least a part of the heated cooling gas is introduced into the reduction zone through the gas duct for the reduction zone, so that the cooling gas can be introduced into the reduction zone without impeding the descent of the reduced iron through the descent chute for the reduced iron.
[0069] This heated cooling gas is further heat exchanged with the reduced iron in a region below the reducing gas introduction portion of the reduction zone, and is heated to approximately the same temperature as the reduced iron.
[0070] As a result, the sufficiently heated cooling gas containing a hydrocarbon gas as a main component comes into contact with the high-temperature reduced iron in a region below the reducing gas inlet portion, making it possible to increase the carbon content in the reduced iron in the same manner as in the above case.
[0071] After that, the cooling gas rises in the reduction zone, but since its temperature is already sufficiently high, the reduction does not stagnate due to the cooling effect of the rising cooling gas, and efficient reduction is not hindered.
[0072] In addition, when a part of this heated cooling gas is introduced into the circulation gas line without being cooled by a direct contact type water-cooling type cooling gas cooler, the following effects are obtained.
[0073] A hydrocarbon-containing gas is introduced into the cooling gas loop to maintain the hydrocarbon gas concentration in the cooling gas, but to maintain a constant pressure, it is necessary to extract from the system an amount of cooling gas equivalent to the amount of hydrocarbon-containing gas introduced into the cooling gas and the volume increase in the cooling zone.
[0074] In this case, if the cooling gas is cooled and then returned to the circulation gas line, the low-temperature cooling gas will be mixed into the circulation gas, reducing the total thermal efficiency and reduction efficiency. However, if the heated cooling gas is returned to the circulation gas line without being cooled in a direct contact water-cooled cooling gas cooler, the thermal efficiency will not decrease.
[0075] Furthermore, since most of the hydrocarbon gas required for reduction can be preheated without the need to install a separate preheater, the equipment costs for an external preheater for the hydrocarbon-containing gas can also be reduced.
[0076] When most of the cooling gas introduced into the cooling zone is introduced directly into the reduction zone and mixed into the circulation gas line (reduction furnace input gas (reducing gas) and / or circulation gas) without cooling, most of the hydrocarbon-containing gas required for the entire process can be preheated through the cooling zone and used. In addition, the amount of circulation cooling gas that is extracted from the cooling zone, cooled, and then reintroduced into the cooling zone is significantly reduced. In other words, it becomes close to a one-through process.
[0077] Therefore, most of the cooling gas is the newly introduced hydrocarbon-containing gas, so the size of the cooling gas compressor that pressurizes the circulating cooling gas can be reduced and the required power can be reduced. In addition, the amount of cooling gas to be cooled is reduced, so water consumption can also be reduced.
[0078] Furthermore, the hydrocarbon concentration in the circulating cooling gas is increased, and the carbon content in the reduced iron can be increased.
[0079] In addition, the temperature at the cooling zone inlet will depend greatly on the temperature of the newly introduced hydrocarbon-containing gas. However, since this hydrocarbon-containing gas is in most cases supplied at high pressure from a natural gas supply station, reducing the pressure of this high-pressure natural gas and mixing it will have the effect of lowering the temperature at the cooling zone inlet through adiabatic expansion.
[0080] When an intermediate cooling zone is provided between the reduction zone and the cooling zone and a gas loop is provided for each of the intermediate cooling zone and the cooling zone, the gas temperature and gas flow rate at the reducing furnace inlet of the upper intermediate cooling zone and the gas temperature and gas flow rate at the reducing furnace inlet of the lower cooling zone are controlled individually.
[0081] In this case, the gas outlet temperature of the intermediate cooling zone can be increased by setting the gas inlet temperature of the intermediate cooling zone higher and the flow rate lower, while the gas inlet temperature of the lower cooling zone can be set lower and the flow rate higher, allowing the reduced iron to be cooled to a desired temperature.
[0082] Therefore, in the upper part of the intermediate cooling zone, the high-temperature cooling gas mainly composed of hydrocarbon gas comes into contact with the high-temperature reduced iron, which makes it possible to similarly increase the carbon content in the reduced iron.
[0083] Furthermore, when hydrogen is used as the reducing gas, no CO2 is emitted from the hydrogen reduction, and most of the reactions of the hydrocarbons introduced into the cooling zone are hydrocarbon cracking reactions, and the carbon in the hydrocarbons is added to the reduced iron, making it possible to significantly reduce CO2 emissions from the reduced iron production facility.
[0084] In addition, in a facility for producing reduced iron by introducing a reducing gas into a vertical reduction furnace, a part of the moisture, which is an oxidizing component, is removed from the top gas discharged from the vertical reduction furnace to adjust the moisture content of the circulating gas, which is then mixed with an oxygen-containing gas and a hydrocarbon-containing gas and introduced into an autothermal reformer, thereby producing the reformed gas required for the reduction of iron oxide.
[0085] This eliminates the need for an externally heated reformer, which requires expensive alloy tubes, and allows for a significant reduction in initial investment.
[0086] At this time, by adjusting the mixing amount of the oxygen-containing gas and the hydrocarbon-containing gas in the first gas mixing device, the inlet gas temperature, outlet gas temperature, and reduction degree of the outlet gas of the autothermal reformer can be adjusted within appropriate ranges.
[0087] In addition, by mixing the circulating gas with a high-concentration oxygen-containing gas rather than with an oxidizing agent such as moisture or carbon dioxide before introducing it into the autothermal reformer, the total heat content of the circulating gas is increased, eliminating the need to preheat the circulating gas to a high temperature (for example, 850°C or higher).
[0088] Therefore, expensive alloy tubes are not required in the preheater, and problems such as clogging caused by carbon deposition and carburization, metal dusting, and damage caused by high heat load are eliminated, so the frequency of tube replacement is reduced, and the initial investment and maintenance costs can be significantly reduced. In addition, downtime of the direct reduced iron production facility due to maintenance is reduced, and opportunity losses due to the stoppage of reduced iron production can be significantly reduced.
[0089] In addition, since an externally heated reformer is not used, and instead heat is recovered from the circulating gas and heat generated by the internal combustion of high-concentration oxygen-containing gas such as pure oxygen is used, the total thermal efficiency is improved, which leads to reduced operating costs. In addition, combustion equipment such as a blower for reformer combustion, the reformer and its exhaust gas treatment equipment are no longer required, allowing for a significant reduction in initial investment costs.
[0090] In addition, in a typical direct reduced iron manufacturing facility, the site area occupied by the externally heated reformer (reformer), combustion equipment, exhaust gas treatment equipment, and exhaust gas heat recovery equipment (off-gas preheater) accounts for approximately 70% or more of the total process equipment excluding utility equipment and material handling. By being able to eliminate these, the required site area can be reduced to 30% or less.
[0091] In addition, since most of the required gas reforming is carried out in the autothermal reformer, it is possible to increase the degree of reduction of the gas at the inlet of the reduction furnace.
[0092] At this time, the rate of gas reforming (in-situ reforming) in the reduction furnace can be reduced, so there is no need to excessively increase the furnace inlet temperature in order to maintain a high temperature after gas reforming in the reduction furnace.
[0093] Therefore, it is possible to maintain the inlet temperature of the reduction furnace within a temperature range that does not cause problems such as pulverization and fusion (clusters) of reduced iron in the furnace and damage to refractories due to pulverized iron, and to maintain high degrees of reduction and temperatures after gas reforming in the reduction zone.
[0094] In addition, when excess CO and H2-containing gas is generated, it can be effectively utilized not only as a fuel for combustion but also as a chemical raw material for the production of methanol, etc.
[0095] On the other hand, if the properties of the iron oxide raw material are good and problems such as powdering, fusion (clustering), and damage to refractories due to powdered iron in the furnace are unlikely to occur, it is possible to further mix an oxygen-containing gas and a hydrocarbon-containing gas with the gas reformed by the autothermal reformer, thereby raising the temperature of the gas at the inlet of the reduction furnace and enabling a large amount of gas reforming (in-situ reforming) to be performed due to the catalytic effect of metallic iron in the furnace. This increases both the temperature and the degree of reduction of the reduced gas after reforming in the furnace, enabling more efficient reduction of iron oxide.
[0096] At this time, a carbon deposition reaction occurs on the reduced iron, but since there is no equipment using the alloy after mixing with the hydrocarbon-containing gas, problems associated with carbon deposition and carburization on the alloy metal surface do not occur.
[0097] On the other hand, the carbon precipitation reaction on the reduced iron is beneficial because it leads to an increase in the carbon content of the product reduced iron, and is also preferable from the viewpoint of product quality.
[0098] In addition, by adjusting the moisture content of the circulating gas by adjusting the gas pressure and temperature at the outlet of the moisture adjustment device and removing most of the CO2 with a CO2 remover, and adjusting the amount of CO2 component along with the moisture in the circulating gas, most of the required reformed gas can be produced using oxygen and hydrocarbon gas. This makes it possible to further lower the preheating temperature of the circulating gas required for reforming, and further reduce the thermal load on the preheater.
[0099] Therefore, the preheater can be made cheaper and problems with the preheater can be eliminated.
[0100] In addition, there will be no more flue gas from the externally heated reformer and the amount of combustion required in the preheater can be reduced, so there is an advantage in that the CO2 removed from the top gas can be effectively utilized in oil fields, etc., significantly reducing CO2 emissions from the reduced iron production facility.
[0101] In addition, in a reduced iron production facility that reduces and cools iron oxide raw materials in a vertical reduction furnace to produce direct reduced iron (Cold DRI), the reduced iron production facility is equipped with the cooling gas system and the autothermal reformer, and can adjust the carbon content in the reduced iron to a desired level without decreasing the carbon content, without using an externally heated reformer, and can maintain high temperatures and a high degree of reduction of the reducing gas after reforming in the reduction furnace while maintaining the gas temperature at the inlet of the reduction furnace at a level that does not cause pulverization in the furnace, fusion (clustering) between the reduced iron particles, or damage to refractories due to pulverized iron, and can also solve the problems of carbon deposition in an external combustion type circulating gas preheater (preheater) and carburization and metal dusting on the ferroalloy. This realizes a process that is inexpensive, has high facility reliability, and is highly efficient in reducing iron production, and can produce high-quality reduced iron.
[0102] In addition, in a facility that produces direct reduced iron (Cold DRI) by reducing iron oxide raw materials in a vertical reduction furnace, hydrogen is added to at least a portion of the carbon dioxide recovered in the reduced iron production facility equipped with the above-mentioned CO2 remover to produce methane, and at least a portion of the produced methane is used as a hydrocarbon gas for producing a reducing gas or as a hydrocarbon gas to be mixed with a cooling gas for cooling the reduced iron. This makes it possible to reuse carbon dioxide within the reduced iron production facility without the need for separate carbon dioxide storage or carbon dioxide utilization facilities.
[0103] In addition, since the reducing gas produced from methane consists of hydrogen and carbon monoxide, it is possible to realize the same reduction as currently possible without the problems that arise when reduction is performed using only hydrogen, such as reduction disintegration, a temperature drop in the reduction zone, and carbon deficiency in the reduced iron. In this case, carbon is added directly to the reduced iron from the carbon monoxide and methane during reduction, so that hot reduced iron having the desired carbon content can be produced even when the reduced iron is directly discharged from the hot state.
[0104] Furthermore, if the recovered carbon dioxide is mixed with as much hydrogen as possible to generate methane and reuse it in the system, the amount of carbon components required to be replenished in the production of reduced iron will be only the amount of carbon in the reduced iron taken out of the system, the amount of carbon components in the exhaust gas, and the amount of carbon components dissolved in the water system and degassed. Therefore, it is sufficient to replenish the amount of hydrocarbon gas equal to the amount of carbon components discharged out of the system, and a large amount of hydrocarbon gas is not required. In other words, even when hydrogen is supplied as the main raw material for the reducing gas, by recycling the carbon components in the system, it is possible to produce direct reduced iron, whether hot or cold, which can solve the problems associated with directly reducing iron oxide with hydrogen.
[0105] It is also possible to recover and replenish carbon dioxide emitted in the downstream steelmaking process. In this case, most of the carbon components can be recycled, realizing a hydrogen reduction ironmaking process that produces reduced iron with the desired carbon components. [Brief description of the drawings]
[0106] [Figure 1] FIG. 1 is a diagram illustrating a process flow according to a first embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram illustrating a process flow of a second embodiment of the present invention in which a reduction zone and a cooling zone are separated. [Diagram 3] FIG. 11 is a diagram illustrating a process flow of a modified example of the second embodiment of the present invention. [Figure 4] FIG. 11 is a diagram illustrating a process flow of a third embodiment of the present invention in which the gas loop for a cooling gas is divided into two gas loops. [Diagram 5]FIG. 11 is a diagram illustrating a process flow of a fourth embodiment of the present invention in which CO2 and hydrogen are mixed to generate methane, and the methane is used for reduction and cooling of reduced iron. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0107] Hereinafter, a direct reduced iron manufacturing system and a direct reduced iron manufacturing method according to the present invention will be described with reference to the accompanying drawings.
[0108] First, a direct reduced iron production facility 30a according to a first embodiment of the present invention will be described with reference to FIG.
[0109] The direct reduced iron manufacturing equipment 30a of the present embodiment 1 includes a vertical reduction furnace (shaft furnace) 1, a reduction zone 2, a heat exchanger 3, a moisture adjustment device (top gas scrubber) 4, a circulation gas compressor 5, a CO2 remover 6, a first gas mixing device 7a, a first hydrocarbon-containing gas mixing device 7b, an autothermal reformer 8, a second gas mixing device 9, a reformed gas cooler 10, a reformed gas mixer 11, a cooling zone 12, a cooling gas scrubber 13, a cooling gas compressor 14, a cooling gas aftercooler 15, hydrocarbon-containing gas lines A1, A2, A3, A4, A5, and oxygen-containing gas lines B1, B2.
[0110] The vertical reduction furnace 1 reduces the iron oxide raw material by contacting it with a reducing gas, and is equipped with a reduction zone 2 and a cooling zone 12. The heat exchanger 3 is composed of a top gas heat recovery heat exchanger 3a and a circulation gas preheater (preheater) 3b. The top gas heat recovery heat exchanger 3a recovers heat from the top gas and adjusts the preheat temperature of the circulation gas by heat exchange between the gas (top gas) discharged from the shaft furnace 1 after reduction and the outlet gas of the CO2 remover 6. The preheater 3b is a preheater for further adjusting the temperature of the circulation gas as necessary. The heat exchanger 3 is provided between the vertical reduction furnace 1 and the first gas mixer 7a. The moisture adjustment device (top gas scrubber) 4 removes dust from the top gas, cools it, and removes moisture from it to adjust the moisture. The circulation gas compressor 5 is a boost compressor for gas circulation to circulate the top gas. The CO2 remover 6 removes some or all of the carbon dioxide from the top gas.
[0111] The first gas mixing device (oxygen partial combustion equipment) 7a mixes a high-concentration oxygen-containing gas such as pure oxygen with a hydrocarbon-containing gas, which has been subjected to partial oxidation and combustion, into a gas from which moisture and CO2 have been removed and the acidic gas components have been reduced. The first hydrocarbon-containing gas mixing device 7b mixes the hydrocarbon-containing gas. The first gas mixing device 7a and the first hydrocarbon-containing gas mixing device 7b adjust the amount of the oxygen-containing gas B1 and the hydrocarbon-containing gas A1, A2 added by the first gas mixing device 7a and the first hydrocarbon-containing gas mixing device 7b, thereby adjusting the inlet temperature, outlet temperature, and outlet gas reduction degree of the autothermal reformer 8. Therefore, the first hydrocarbon-containing gas mixing device 7b is provided as necessary when the amount of the hydrocarbon-containing gas is insufficient when the first gas mixing device 7a mixes the hydrocarbon-containing gas A1.
[0112] The autothermal reformer 8 reforms a mixed gas obtained by mixing the oxygen-containing gas B1 and the hydrocarbon-containing gases A1 and A2 in the first gas mixer 7a and the first hydrocarbon-containing gas mixer 7b with the gas from which moisture and carbon dioxide have been removed from the top gas, using the energy of the mixed gas. The autothermal reformer 8 is preferably arranged in a U-shape or a V-shape. This allows the used catalyst to be discharged from the lower part and new catalyst to be filled from the upper part, making it easy to replace the catalyst. In addition, it is more preferable that the autothermal reformer 8 is provided with a similar inert catalyst packed bed filled with alumina balls or the like capable of removing fine solids such as soot, in the front stage. This makes it possible to reduce the frequency of catalyst replacement. In addition, it is preferable that the autothermal reformer 8 is configured to allow the oxidation reaction and the reforming reaction to proceed in one reformer.
[0113] The second gas mixing device 9 mixes the gas discharged from the autothermal reformer 8 with an oxygen-containing gas B2 and a hydrocarbon-containing gas A3, partially oxidizes and burns the gas, and further adjusts the temperature rise and hydrocarbon concentration of the gas at the inlet of the reducing furnace 1 in order to perform an appropriate amount of reforming in the reducing furnace.
[0114] The reformed gas cooler 10 adjusts the temperature of the gas introduced into the furnace according to the raw material so as to prevent problems such as pulverization in the furnace, fusion (cluster) between reduced irons, and damage to refractories due to pulverized iron. The reformed gas mixer 11 mixes the cooled reformed gas and hydrocarbon-containing gas into the furnace input gas line.
[0115] Furthermore, the direct reduced iron manufacturing equipment 30a is provided with a cooling gas loop 23 that circulates a cooling gas for cooling the reduced iron in the cooling zone 12 in order to manufacture cooled direct reduced iron (Cold DRI). The cooling gas scrubber 13, the cooling gas compressor 14, and the cooling gas aftercooler 15 are provided in the cooling gas loop 23. The cooling gas loop 23 is provided with a flow rate adjusting means (not shown) that adjusts the flow rate of the cooling gas, so that the flow rate of the cooling gas introduced into the reduction furnace 1 can be adjusted.
[0116] The cooling gas scrubber 13 is a water-cooled direct contact type cooler, and removes dust and cools the cooling gas for cooling the reduced iron discharged from the reduction furnace 1. The cooling gas aftercooler 15 adjusts the temperature of the cooling gas, and is provided on the outlet side of the cooling gas compressor 14. For example, the cooling gas aftercooler 15 lowers the inlet temperature of the cooling gas, and the flow rate adjustment means reduces the total flow rate of the cooling gas, thereby increasing the outlet temperature of the cooling gas and adjusting the amount of carbon in the reduced iron. The cooling gas aftercooler 15 is preferably a chiller-type aftercooler or an aftercooler that introduces a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like to supply a low-temperature cooling gas to the reduction furnace, and is particularly preferably capable of cooling to a wet-bulb atmospheric temperature +3 to 4°C or lower.
[0117] The details of the first embodiment will be described below.
[0118] In the direct reduced iron production facility 30a equipped with the above-mentioned equipment, direct reduced iron is produced by contacting the oxidized iron raw material with a reducing gas in the vertical reduction furnace 1. The gas obtained by reducing the oxidized iron raw material fed from the top of the vertical reduction furnace 1 is discharged from the top of the furnace as top gas.
[0119] This top gas is cleaned of dust and cooled in a top gas scrubber 4, and the majority of the moisture is removed to adjust the moisture content (moisture adjustment process). The gas with the moisture content adjusted is pressurized in a circulation gas compressor 5 and the CO2 is removed in a CO2 remover 6 (CO2 removal process). The CO2 component is also adjusted along with the moisture, and the total amount of oxidizing gas components is adjusted.
[0120] The moisture content is adjusted by adjusting the amount or temperature of water supplied to the top gas scrubber 4 to adjust the gas temperature, by adjusting the outlet pressure to adjust the gas pressure, and by adjusting the saturated water vapor pressure in the circulating gas.
[0121] The CO2 remover 6 may be a PSA (pressure swing absorption) type device or a chemical absorption method. In either case, in order to achieve the target CO2 removal rate, it may be necessary to first increase the pressure and then reduce the pressure after removing the CO2. It is even better to use a rotary pressure reducer for the pressure reduction and physically connect the shaft of the rotary pressure reducer to the shaft of the circulating gas compressor 5 to reduce the power required for pressure increase.
[0122] The gas in which the oxidizing components have been adjusted by removing moisture (H2O) and carbon dioxide (CO2) and the main components are CO and H2 is preheated as necessary in a top gas heat recovery heat exchanger 3a and a preheater 3b (preheating process), and then in a first gas mixing device 7a, a high-concentration oxygen-containing gas B1 having an oxygen concentration higher than the oxygen concentration in the atmosphere, such as pure oxygen, and a hydrocarbon-containing gas A1, such as natural gas, are mixed (first gas mixing process) and partially oxidized and combusted with oxygen.
[0123] This produces a mixed gas of oxidizing gases of H2O and CO2, reducing gases of hydrogen (H2) and carbon monoxide (CO), and hydrocarbon gas, and also heats the mixed gas by the heat generated by the oxidation reaction.
[0124] The heated mixed gas is further mixed with a required amount of hydrocarbon-containing gas A2 in a first hydrocarbon-containing gas mixing device 7b and introduced into an autothermal reformer 8, where the hydrocarbons and oxidizing gas are reformed using the mixed gas's own energy to produce a reduced gas with a high degree of reduction (reformed gas production process).
[0125] Here, the preheat temperature of the circulating gas, the amount of high-concentration oxygen-containing gas B1 to be mixed, and the amounts of hydrocarbon-containing gases A1 and A2 can be determined based on the amount of reforming gas required for the reduction of the iron oxide raw material, the degree of reduction and temperature of the reforming gas, and the gas temperatures at the inlet and outlet of the autothermal reformer 8.
[0126] For example, when a large amount of reducing gas to be input into the reduction furnace is required, the preheating temperature of the circulating gas in the preheater 3b is set to a low value, oxygen-containing gas B1 is mixed up to the upper limit of the gas temperature at the inlet of the autothermal reformer 8, and hydrocarbon-containing gases A1 and A2 corresponding to that are mixed, thereby making it possible to produce a larger amount of reducing gas.
[0127] On the other hand, when it is desired to reduce the amount of reducing gas introduced into the reducing furnace in order to reduce the excess top gas, the preheating temperature of the circulating gas is set as high as possible within a range in which problems due to carbon deposition and carburization do not occur in the top gas heat recovery heat exchanger 3a and the preheater 3b, for example, within a range of less than 850°C, preferably less than 700°C, and more preferably less than 550°C, thereby reducing the amount of oxygen that can be mixed and reducing the amount of reducing gas newly produced.
[0128] In addition, in the first gas mixing device 7a, the top gas is mixed with a hydrocarbon-containing gas A1 and a high-concentration oxygen-containing gas B1 and partially combusted in a ratio that does not generate soot, and further, in the first hydrocarbon-containing gas mixing device 7b, a hydrocarbon-containing gas A2 is mixed as necessary, and the gas temperature at the inlet of the autothermal reformer 8 is adjusted to an allowable temperature, for example, 1500°C or less, preferably 1400°C or less.
[0129] At the same time, the hydrocarbon-containing gases A1, A2 and the high-concentration oxygen-containing gas B1 are adjusted within a range in which carbon deposition does not occur within the autothermal reformer 8 and the gas temperature at the outlet of the autothermal reformer 8 is 700°C or higher, preferably 750°C or higher, and more preferably 800°C or higher.
[0130] If the reduction degree of the reformed gas at the outlet of the autothermal reformer 8 under these conditions does not satisfy the condition of a predetermined reduction degree, for example, 7 or more, preferably 8 or more, the first gas mixer 7a, the first hydrocarbon-containing gas mixer 7b and the autothermal reformer 8 are made into a multi-stage. Then, the gas whose temperature has been lowered by the reforming reaction at the outlet of the first-stage autothermal reformer is further mixed with a high-concentration oxygen-containing gas and a hydrocarbon-containing gas, and introduced into the next autothermal reformer, and this process is repeated to adjust the reduction degree of the gas at the outlet of the last autothermal reformer, so that the reduction degree and temperature of the gas at the inlet of the vertical reduction furnace 1 become the desired degree and temperature.
[0131] In addition, since the carbon deposition and carburization reaction in the top gas heat recovery heat exchanger 3a and the preheater 3b and the carbon deposition reaction in the autothermal reformer 8 depend on the HO and CO concentrations in the circulating gas, the gas pressure, and the gas temperature, these problems can be solved by adjusting each of these within an appropriate range.
[0132] For example, the moisture concentration is adjusted by adjusting the pressure and temperature of the outlet gas of the top gas scrubber 4. Alternatively, a water-cooled cooler may be provided directly at the outlet of the circulation gas compressor 5 to adjust the moisture concentration. The CO2 concentration is adjusted by a CO2 remover. The gas pressure is adjusted by adjusting the outlet pressure of the top gas scrubber 4 by adjusting the amount of gas discharged outside the system. The inlet pressure of the autothermal reformer 8 is adjusted to an appropriate pressure by adjusting the outlet pressure of the top gas scrubber 4. The preheat temperature of the gas may be increased by, for example, recovering a certain amount of heat from the top gas in the top gas heat recovery heat exchanger 3a, and adjusting the amount of combustion of the external combustion type preheater 3b to a desired temperature within a range in which carbon deposition does not occur.
[0133] If the gas introduced into the autothermal reformer 8 has a pressure of 600 kPa(A) or more, carbon will easily precipitate on the catalyst of the autothermal reformer 8 unless a large amount of excess oxidizing gas is present, and therefore it is not possible to avoid the carbon precipitation problem and obtain a reformed gas with a specified degree of reduction.
[0134] Therefore, in the direct reduced iron production equipment 30a according to the first embodiment of the present invention, in order to prevent carbon deposition in the autothermal reformer 8 and to obtain a reducing gas with a desired degree of reduction, the pressure of the gas introduced into the autothermal reformer 8 is adjusted to less than 600 kPa (A), preferably less than 500 kPa (A), and more preferably less than 350 kPa (A).
[0135] In the above explanation, the first gas mixing device 7a, the first hydrocarbon-containing gas mixing device 7b, and the autothermal reformer 8 are installed separately, but the present invention is not limited to this. If an autothermal reformer 8 that can perform oxidation reactions and reforming reactions in a single reformer is used, there is no need to mix the hydrocarbon gases A1, A2 separately in the first gas mixing device 7a and the first hydrocarbon-containing gas mixing device 7b, and it is sufficient to mix all of the required amounts of the high-concentration oxygen-containing gas B1 and the hydrocarbon-containing gases A1, A2 in the autothermal reformer 8.
[0136] At this time, the gas temperature at the inlet of the autothermal reformer 8 also drops, making it possible to adjust the temperature over a wide range.
[0137] The reformed gas produced under the above conditions is further mixed with high-concentration oxygen-containing gas B2 and hydrocarbon-containing gas A3 in the second gas mixing device 9 (second gas mixing step), and then further mixed with hydrocarbon-containing gas A4 in the downstream, thereby increasing the temperature of the furnace inlet gas and reforming it (in-situ reforming) due to the catalytic effect of metallic iron in the furnace. This further increases the degree of gas reduction in the furnace, and makes it possible to carry out the reduction reaction of iron oxide at a high temperature.
[0138] In addition, it is preferable to provide a reformed gas mixer 11 for performing the necessary hydrocarbon mixing to prevent the inside of the furnace from becoming partially overheated due to the exothermic CH4 production reaction in addition to the reforming reaction in the furnace, thereby enabling further mixing of the hydrocarbon-containing gas A4.
[0139] Even if the gas temperature at the inlet of the vertical reduction furnace 1 is in the range of about 1000°C, depending on the raw material, when the reformed gas is introduced into the reduction furnace 1, the reduced iron may fuse together in the furnace, forming clusters that cause discharge problems or pulverizing in the furnace. In this case, a reformed gas cooler 10 may be provided to control the temperature.
[0140] On the other hand, when the raw material has excellent cluster characteristics, the amount of high-concentration oxygen-containing gas B2 and hydrocarbon-containing gas A3 fed to the second gas mixing device 9 can be increased to increase the amount of partial combustion of oxygen and also increase the amount of hydrocarbon gas, thereby further promoting an increase in the furnace temperature and the reforming reaction (in-situ reforming) in the furnace.
[0141] In this case, if the amount of the hydrocarbon-containing gas A4 from the reforming gas mixer 11 is increased and the concentration of the hydrocarbon gas in the reducing gas (furnace introduction gas) introduced into the reducing furnace 1 is raised, the carbon precipitation reaction is promoted as well as the reforming reaction, and the carbon concentration of the reduced iron can be improved.
[0142] At this time, a carbon precipitation reaction occurs on the reduced iron, but since no equipment using alloys is present after the hydrocarbon-containing gas A4 is mixed, problems such as damage to equipment due to carbon precipitation and carburization do not occur, and on the other hand, the carbon content of the product reduced iron increases, which is also preferable from the standpoint of product quality.
[0143] However, in the case where the reducing gas pressure is low as in the first embodiment, the partial pressure of the hydrocarbon gas required for reforming in the reduction furnace is low. Also, in order to maintain high productivity, it is not preferable to mix an excess of hydrocarbon gas. Therefore, since the partial pressure of the hydrocarbon is low, the carbon deposition reaction on the reduced iron in the reduction zone 2 is unlikely to occur, and the carbon content in the reduced iron at the outlet side of the reduction zone 2 remains at approximately 1.5% to 2%.
[0144] On the other hand, in the present embodiment 1, the amount of carbon added in the cooling zone 12 is adjustable without being greatly dependent on the state of the reduction zone 2 as described above, and therefore, it is possible to adjust the amount of carbon in the discharged reduced iron as described below.
[0145] The main carbon deposition reaction in the vertical reduction furnace 1 is a hydrocarbon cracking reaction, and the reaction is highly dependent on the hydrocarbon gas partial pressure and temperature.
[0146] In the first embodiment, the cooling gas discharged from the cooling zone 12 of the reduction furnace 1 is subjected to dust removal and cooling in a cooling gas scrubber (a direct contact type water-cooled cooling gas cooler) 13 through a cooling gas loop 23, and then the pressure of the cooling gas is increased in a cooling gas compressor 14. Thereafter, a part of the gas is introduced into the cooling zone 12 as it is, and the other part of the gas is further cooled in a cooling gas aftercooler 15.
[0147] In order to bring gas having a high partial pressure of hydrocarbons into contact with reduced iron at a high temperature, the hydrocarbon concentration of the circulating cooling gas is set to 50% or more, preferably 70% or more, and a cooling gas aftercooler 15, preferably a chiller-type aftercooler or an aftercooler that introduces a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like to supply low-temperature cooling gas to the reducing furnace, is provided on the outlet side of the cooling gas compressor 14.
[0148] In typical Cold DRI production facilities, the flow rate of cooling gas is adjusted so that the discharge temperature of the reduced iron remains below 50°C to 55°C to prevent problems caused by reoxidation of the reduced iron.
[0149] However, the inlet temperature of the cooling gas to the reducing furnace 1 is approximately 40°C due to the increase in pressure, even when the water spray cooling type cooling gas compressor 14 is used. As described above, a large amount of cooling gas is required because the temperature difference between the cooling gas and the controlled discharge temperature of reduced iron is small, and the discharge temperature of the cooling gas from the reducing furnace is inevitably low, at approximately 400°C.
[0150] As mentioned above, the main component of the cooling gas is hydrocarbons, and efforts are made to make the partial pressure of the hydrocarbon gas in contact with the reduced iron as high as possible. However, if the gas temperature is around 400°C, the reduced iron will be cooled the moment it comes into contact with the hot reduced iron, and the cracking reaction of the hydrocarbon gas will not occur sufficiently.
[0151] In addition, even if a part of this cooling gas is raised to the reduction zone 2, the gas always has a low temperature and flows through the center of the reduction furnace. Therefore, the temperature does not reach a high enough temperature to cause the carbon deposition reaction. In addition, the carbon deposition reaction does not occur, and the reduction reaction is stagnated.
[0152] On the other hand, as in the present embodiment 1, by providing a cooling gas aftercooler 15, preferably a chiller-type aftercooler or an aftercooler that cools the cooling gas by mixing it with a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like, on the outlet side of the cooling gas compressor 14, and lowering the inlet temperature of at least a part of the cooling gas into the reducing furnace 1, it becomes possible to increase the temperature difference from the desired discharge temperature of reduced iron (usually about 50°C to 55°C or less), and therefore it becomes possible to cool to the desired discharge temperature of reduced iron even with a small amount of cooling gas. The inlet temperature of this cooling gas into the reducing furnace 1 is preferably 35°C or less.
[0153] At this time, the total flow rate of the cooling gas required to cool the reduced iron is reduced, and the total heat capacity of the cooling gas is reduced, so that the temperature on the outlet side of the cooling zone 12 is inevitably increased.
[0154] Therefore, in the first embodiment, the high-temperature cooling gas comes into contact with the reduced iron in the upper part of the cooling zone 12. In this portion, the partial pressure of the hydrocarbon gas is high and the temperature is high, so that the cracking reaction of the hydrocarbon gas is promoted and the amount of carbon in the reduced iron can be increased. In addition, by cooling the cooling gas, the amount of moisture contained in the cooling gas is reduced, which prevents the consumption of carbon in the reduced iron by moisture. In addition, since the cooling gas outlet temperature becomes high, for example, by providing a heat recovery device such as a boiler in the cooling gas loop 23, efficient heat recovery from the cooling gas is possible.
[0155] In other words, even if the problems of carbon precipitation in an external combustion type circulating gas preheater, carburization and metal dusting on ferroalloys are avoided and the gas temperature at the inlet of the reduction furnace is maintained at a temperature that does not cause pulverization in the furnace, fusion (clustering) of reduced iron particles, or damage to refractories due to pulverized iron, it is possible to adjust the carbon content in the reduced iron to, for example, 3% or more by adjusting the inlet temperature and flow rate of the cooling gas regardless of these conditions.
[0156] An example of the conditions for producing direct reduced iron in the first embodiment will be shown below.
[0157] The moisture content in the circulating gas is adjusted by setting the preheating temperature of the circulating gas to approximately 450°C, the outlet pressure of the top gas scrubber 4 to 50 kPa (A), and the outlet temperature to 45°C, and the pressure of the gas introduced into the autothermal reformer 8 after removing CO2 using a dry process gas compressor 5 is controlled to approximately 250 kPa (A) to 350 kPa (A).
[0158] In the first gas mixer 7a and the first hydrocarbon-containing gas mixer 7b, when the hydrocarbon-containing gas A1, the high-concentration oxygen-containing gas B1 and the hydrocarbon-containing gas A2 are mixed and partially combusted so that the reformed gas at the outlet of the autothermal reformer 8 has an R-Value of about 10, the inlet temperature of the autothermal reformer 8 becomes 1500°C or lower, and the outlet gas temperature becomes about 950°C. At this time, the hydrocarbon gas ratio (CO2+H2O) / CH4 of the oxidizing substances at the outlet side of the autothermal reformer 8 can be maintained at a ratio at which carbon deposition does not occur on the catalyst.
[0159] Further, when a hydrocarbon-containing gas A3 and a high-concentration oxygen-containing gas B2 are added to this in a second gas mixing device 9 and fed into the reduction furnace 1 at about 920°C, reforming (in-situ reforming) and a carbon deposition reaction occur in the furnace, and the gas after the reforming and carbon deposition reaction has a temperature of about 780°C and a good quality reduced gas with a reduction degree of about 13 can be obtained.
[0160] Under the above-mentioned example conditions, the concentration of the hydrocarbon gas in the gas introduced into the furnace is sufficient at about 5 to 8% or less. In other words, since a large amount of excess hydrocarbon-containing gas is not required, the amount of gas introduced into the furnace required per reduced iron is smaller than that in high-pressure operation, and the pressure loss in the reducing furnace 1 is almost the same as that in operation at a circulation gas pressure of 700 kPa(A) or more, for example, and the disadvantage of an increase in pressure loss, which is one of the disadvantages of low-pressure gas operation, is not significant.
[0161] Furthermore, since productivity, i.e., the required reduction reaction time, depends more on temperature than on pressure, not lowering the temperature of the reducing gas after the in-furnace reforming and carbon deposition reaction contributes greatly to the reduction reaction rate, i.e., high productivity.
[0162] Under these production conditions, most of the reforming reaction is completed in advance in the autothermal reformer 8, so the temperature drop due to the in-furnace reforming reaction (in-situ reforming) is small, and the gas temperature after the reforming and carbon deposition reaction is about 780°C.
[0163] On the other hand, when most of the reforming reaction (in-situ reforming) is carried out in the furnace under high pressure conditions, the endothermic reaction causes a significant drop in the gas temperature in the furnace, and the productivity also drops significantly.
[0164] Therefore, a large vertical reduction furnace is required despite the high pressure reduction, and the size of the vertical reduction furnace cannot be significantly reduced compared to the vertical reduction furnace under these conditions, and the advantage of reduced equipment size, which is an advantage of high pressure gas operation, cannot be enjoyed.
[0165] Moreover, the carbon content in the product under these conditions can be adjusted in the cooling zone 12.
[0166] In this example, the temperature of the entire amount of cooling gas is adjusted to 35° C. or less, preferably 25° C. or less, by a chiller-type cooling gas aftercooler 15, and the amount of cooling gas is adjusted so that the discharge temperature of reduced iron becomes a desired temperature, for example, 50° C. or less.
[0167] At this time, the difference between the discharge temperature of the reduced iron (usually about 50°C) and the inlet temperature of the cooling gas at the reduction furnace 1 is 25°C, which is more than twice the temperature difference of 10°C when the cooling gas temperature is about 40°C.
[0168] Therefore, the amount of cooling gas required is significantly reduced, the temperature of the cooling gas at the outlet of the reduction furnace is increased, and it becomes possible to adjust the carbon content in the reduced iron to 3% or more.
[0169] As described above, as shown in this example, the present embodiment 1 is superior to the high-pressure gas conditions from the overall viewpoints of the carbon deposition problem, pressure loss in the furnace, fluidization phenomenon in the furnace, productivity, equipment reliability, equipment size, and product quality.
[0170] Next, a direct reduced iron production facility 30b according to another embodiment 2 of the present invention will be described with reference to FIG.
[0171] The direct reduced iron manufacturing equipment 30b of the present embodiment 2 includes a vertical reduction furnace (shaft furnace) 1, a reduction zone 2, a heat exchanger 3, a moisture regulator (top gas scrubber) 4, a circulation gas compressor 5, a CO2 remover 6, a first gas mixer 7a, a first hydrocarbon-containing gas mixer 7b, an autothermal reformer 8, a second gas mixer 9, a reformed gas cooler 10, a reformed gas mixer 11, a cooling zone 12, a cooling gas scrubber (direct contact type water-cooled cooling gas cooler) 13, a cooling gas compressor 14, a cooling gas aftercooler 15, a hydrocarbon-containing gas line A1, A2, A3, A4, A5, and an oxygen-containing gas line B1, B2, similar to the direct reduced iron manufacturing equipment 30a of the present embodiment 1. The heat exchanger 3 includes a top gas heat recovery heat exchanger 3a and a circulation gas preheater (preheater) 3b. The same components as those in the first embodiment are designated by the same reference numerals and the description thereof will be omitted.
[0172] In the direct reduced iron manufacturing equipment 30b of the second embodiment, the reduction zone 2 and the cooling zone 12 are configured as separate furnaces independent of each other so that a desired high-temperature cooling gas can be extracted and introduced into the reduction zone 2. The reduction zone 2 and the cooling zone 12 are connected by a chute 22 that drops the reduced iron into the cooling zone 12.
[0173] Furthermore, in order to produce cooled direct reduced iron (Cold DRI), the direct reduced iron manufacturing equipment 30b is provided with a cooling gas loop 23 that circulates a cooling gas that cools the reduced iron in the cooling zone 12. The cooling gas loop 23 is provided with cooling gas dust collectors 17, 18 that remove dust from the cooling gas discharged from the cooling zone 12, and a cooling gas heat exchanger (boiler) 19 that recovers heat from the cooling gas and cools the cooling gas. The cooling gas dust collectors 17, 18 are configured as dry dust collectors.
[0174] By dividing the reduction zone 2 and the cooling zone 12 into separate furnaces as in the present embodiment 2, the ducts connecting the upper part of the reduction furnace 1 and the cooling zone 12 can be easily constructed using refractory materials, and high-temperature cooling gas can be extracted without causing any equipment problems.
[0175] In this way, the cooling gas, which is mainly composed of hydrocarbons preheated to a high temperature, can be brought into contact with the reduced metallic iron, so that the carbon content of the reduced iron can be easily increased.
[0176] Furthermore, when the cooling gas is introduced into the reduction zone 2 as an upward flow in the furnace, it is further heated in the lower region of the reduction zone 2 and heated to almost the same temperature as the reduced iron, making it possible to further increase the carbon content of the reduced iron regardless of the surrounding gas pressure.
[0177] In addition, since the cooling gas introduced into the reduction zone 2 has been sufficiently heated, the cooling effect due to the upward flow of the cooling gas in the reduction zone 2 is eliminated, and reduction stagnation in the reduction zone 2 is not caused.
[0178] In addition, there is a sufficient residence time in the lower part of the reduction zone 2, so sufficient carburization can be expected from the viewpoint of reaction time.
[0179] In addition, when heat is recovered from the cooling gas by increasing the outlet temperature of the cooling gas, the heat recovery efficiency is improved. For example, heat may be recovered in a boiler 19 via dry dust collectors 17 and 18 to generate power. In this case, the steam temperature can be raised to a high level, so the power generation efficiency is improved dramatically. In addition, instead of using the boiler 19, the circulating gas or the hydrocarbon-containing gas may be preheated.
[0180] On the other hand, if the cooling gas is introduced directly from the cooling zone to the reduction zone through a direct reduced iron descent chute, problems such as poor descent of the reduced iron and damage to equipment due to vibration of the chute can occur.
[0181] However, in the direct reduced iron manufacturing equipment 30b of the present embodiment 2, in addition to the chute 22 connecting the reduction zone 2, into which the reduced iron descends, and the cooling zone 12, a gas duct 16a for the reduction zone that passes a cooling gas to the reduction zone 2 is separately provided. This gas duct 16a for the reduction zone is connected from the upper part of the cooling zone 12 to the lower part of the reduction zone 2. In the present embodiment 2, the gas duct 16a for the reduction zone constitutes the gas duct (cooling gas connecting duct) 16.
[0182] This allows most of the cooling gas to be introduced into the reduction zone 2 via the gas duct 16a for the reduction zone without impeding the descent of reduced iron. That is, the amount of cooling gas directly introduced from the cooling zone 12 to the reduction zone 2 is not limited by reasons such as poor descent of reduced iron, and can be adjusted by the amount of the hydrocarbon-containing gas A5 introduced into the cooling gas loop 23.
[0183] As a result, in this embodiment 2, by introducing a sufficiently preheated cooling gas into the reduction zone 2 as needed, it is possible to increase the carbon content in the reduced iron without causing reduction stagnation in the reduction zone 2, and it is also possible to maintain stable operation without impeding the descent of the reduced iron, and it is also possible to improve the total thermal efficiency.
[0184] Next, a direct reduced iron manufacturing facility 30b according to a modification of the second embodiment will be described with reference to Fig. 3. In this modification, the cooling gas connection duct 16 is composed of a gas duct 16a for the reduction zone and a gas duct 16b for the circulation gas line, which returns a part of the cooling gas extracted from the cooling zone 12 to the circulation gas line. The gas duct 16b for the circulation gas line is connected to the cooling zone 12 or the cooling gas loop 23 and the circulation gas line. Specifically, the gas duct 16b for the circulation gas line is provided by branching off from the gas duct 16a for the reduction zone, and is connected to the downstream of the autothermal reformer 8, for example, the reformed gas mixer 11, and / or the upstream of the autothermal reformer 8, for example, the first hydrocarbon-containing gas mixer 7b. As a result, a portion of the cooling gas is returned downstream of the autothermal reformer 8, for example to the reformed gas mixer 11, and / or returned upstream of the autothermal reformer 8, for example to the first hydrocarbon-containing gas mixing device 7b, and mixed with the reducing gas introduced into the reducing furnace 1 and / or the gas flowing upstream of the autothermal reformer 8.
[0185] In this way, the preheated cooling gas may be returned to the circulation gas line without being cooled, and used as a part or a substitute for the hydrocarbon-containing gases A2 and A4. If this makes the supply lines for the hydrocarbon-containing gases A2 and A4 unnecessary, the supply lines for the hydrocarbon-containing gases A2 and A4 may be omitted. In addition, if the gas duct 16b for the circulation gas line is directly connected to the circulation gas line, the first hydrocarbon-containing gas mixing device 7b and the like may not be provided.
[0186] Furthermore, the gas duct 16b for the circulation gas line may take any form as long as the cooling gas discharged from the reduction furnace 1 can be returned to the circulation gas line without passing through the direct contact type water-cooled cooling gas cooler 13. For example, after dust has been removed by the cooling gas dust removers 17 and 18 and from the upstream of the cooling gas scrubber 13, the cooling gas may be mixed with the reducing gas introduced into the reduction furnace 1 in the same manner as above and / or the gas flowing upstream of the autothermal reformer 8. In this case, since dust has already been removed, there is no need to install a new dust remover.
[0187] By providing the gas duct 16b for the circulation gas line in this manner, the hydrocarbon-containing gas required for reduction can be obtained from the preheated cooling gas, and there is no need to install a separate preheater for preheating the hydrocarbon-containing gas, thereby reducing the equipment costs for an external preheater for the hydrocarbon-containing gas.
[0188] In addition, by directly introducing most of the cooling gas introduced into the cooling zone 12 into the reduction zone 2 or extracting it into the circulation gas line (reduction furnace input gas (reducing gas) and / or circulation gas) without directly cooling it with water, the amount of circulating cooling gas that is extracted from the cooling zone 12, cooled, and then reintroduced into the cooling zone 12 is significantly reduced.
[0189] Therefore, most of the cooling gas flowing through the cooling zone 12 becomes the newly introduced hydrocarbon-containing gas A5, and when the pressure of the hydrocarbon-containing gas A5 is high and it is introduced from the outlet side of the cooling gas compressor 14, the size of the cooling gas compressor 14 that pressurizes the circulating cooling gas can be reduced and the required power can be reduced. In addition, the amount of cooling gas to be cooled is reduced, so the amount of water consumed can also be reduced.
[0190] Furthermore, the hydrocarbon concentration in the circulating cooling gas is increased, and the carbon content in the reduced iron can be increased.
[0191] In addition, the temperature at the inlet of the cooling zone 12 will depend on the temperature of the newly introduced hydrocarbon-containing gas A5. However, since this hydrocarbon-containing gas A5 is in most cases supplied at high pressure from a natural gas supply station, reducing the pressure of this high-pressure natural gas and mixing it will have the effect of lowering the temperature at the inlet of the cooling zone 12 through adiabatic expansion.
[0192] Next, a direct reduced iron production facility 30c according to another embodiment 3 of the present invention will be described with reference to FIG.
[0193] The direct reduced iron production equipment 30c of the present embodiment 3 includes a vertical reduction furnace (shaft furnace) 1, a reduction zone 2, a heat exchanger 3, a moisture regulator (top gas scrubber) 4, a circulation gas compressor 5, a CO2 remover 6, a first gas mixer 7a, a first hydrocarbon-containing gas mixer 7b, an autothermal reformer 8, a second gas mixer 9, a reformed gas cooler 10, a reformed gas mixer 11, a cooling zone 12, a cooling gas scrubber (direct contact type water-cooled cooling gas cooler) 13, a cooling gas compressor 14, a cooling gas aftercooler 15, a hydrocarbon-containing gas line A1, A2, A3, A4, A5, and an oxygen-containing gas line B1, B2, similar to the direct reduced iron production equipment 30a, 30b of the embodiments 1 and 2. The heat exchanger 3 includes a top gas heat recovery heat exchanger 3a and a circulation gas preheater (preheater) 3b. The same components as those in the first and second embodiments are designated by the same reference numerals and their explanations are omitted.
[0194] In the present embodiment 3, the cooling zone 12 is different from that in the embodiment 2. Specifically, the structure is similar to that of the reduction furnace 1 in the embodiment 1 in which the reduction zone 2 and the cooling zone 12 are integrated, but an intermediate cooling zone 21 is provided between the reduction zone 2 and the cooling zone 12.
[0195] In the third embodiment, the direct reduced iron manufacturing equipment 30c is provided with a cooling gas loop 23 that circulates a cooling gas for cooling the reduced iron in the cooling zone 12 and the intermediate cooling zone 21 in order to manufacture cooled direct reduced iron (Cold DRI). The cooling gas loop 23 is provided in each of the intermediate cooling zone 21 and the cooling zone 12. Specifically, the cooling gas loop 23 has an upper cooling gas loop 231 and a lower cooling gas loop 232, and the upper cooling gas loop 231 is provided in the intermediate cooling zone 21 and the lower cooling gas loop 232 is provided in the cooling zone 12.
[0196] The upper cooling gas loop 231 is equipped with cooling gas dust removers 17 and 18 that remove dust from the cooling gas discharged from the intermediate cooling zone 21, a cooling gas heat exchanger (boiler) 19 that cools the cooling gas, and an intermediate cooling gas compressor 20 that pressurizes the cooling gas.
[0197] The intermediate cooling gas compressor 20 is configured as a dry type booster. The cooling gas discharged from the intermediate cooling zone 21 is subjected to dust removal by the cooling gas dust removers 17 and 18, and then cooled by heat recovery in the cooling gas heat exchanger 19. Thereafter, the cooling gas is pressurized by the intermediate cooling gas compressor 20 and introduced into the intermediate cooling zone 21.
[0198] This upper cooling gas loop 231 is a high-temperature gas loop, and the flow rate is adjusted so that, for example, the temperature of the cooling gas at the cooling gas inlet of the reduction furnace 1 is set to about 150° C. to 200° C., and the temperature of the cooling gas at the cooling gas outlet of the reduction furnace 1 is close to the temperature of the reduced iron immediately after reduction, for example, about 700° C. This makes it possible to enjoy the advantages of a high-temperature cooling gas in the same way as in the case where the reduction zone 2 and the cooling zone 12 are separated into separate furnaces.
[0199] Here, by making the cooling gas outlet part a refractory structure, there is no need for a metal structure such as an alloy, and problems such as carburization and metal dusting in the metal structure do not occur.
[0200] The lower cooling gas loop 232 includes a cooling gas scrubber 13, a cooling gas compressor 14, and a cooling gas aftercooler 15 similar to those in the embodiment 1. The cooling gas discharged from the cooling zone 12 is subjected to dust removal and cooling in the cooling gas scrubber 13, and then pressurized in the cooling gas compressor 14. Then, the cooling gas is cooled in the cooling gas aftercooler 15 and introduced into the cooling zone 12.
[0201] The lower cooling gas loop 232 is a low-temperature gas loop whose temperature is lower than that of the cooling gas in the upper cooling gas loop 231, and controls the discharge temperature of the reduced iron to a desired temperature. At this time, since the reduced iron has already been cooled in the intermediate cooling zone 21, it is possible to cool it to the desired temperature with a smaller flow rate of cooling gas than in the case where the intermediate cooling zone 21 is not provided.
[0202] The required flow rate can be further reduced by providing an aftercooler 15, preferably a chiller-type aftercooler or an aftercooler that introduces a hydrocarbon-containing gas cooled by its own adiabatic expansion or the like, on the outlet side of the cooling gas compressor 14 to supply low-temperature cooling gas to the reduction furnace.
[0203] In this manner, by adjusting the temperature and flow rate of each of the upper cooling gas loop 231 and the lower cooling gas loop 232, the discharge temperature of the reduced iron and the carbon content of the reduced iron can be arbitrarily controlled in the same manner as in the previous embodiment.
[0204] Next, a direct reduced iron production facility 30d according to another embodiment 4 of the present invention will be described with reference to FIG.
[0205] The direct reduced iron manufacturing equipment 30d of the present embodiment 4 includes a vertical reduction furnace (shaft furnace) 1, a reduction zone 2, a heat exchanger 3, a moisture regulator (top gas scrubber) 4, a circulation gas compressor 5, a CO2 remover 6, a first gas mixer 7a, a first hydrocarbon-containing gas mixer 7b, an autothermal reformer 8, a second gas mixer 9, a reformed gas cooler 10, a reformed gas mixer 11, a cooling zone 12, a cooling gas scrubber (direct contact type water-cooled cooling gas cooler) 13, a cooling gas compressor 14, a cooling gas aftercooler 15, a hydrocarbon-containing gas line A1, A2, A3, A4, A5, and an oxygen-containing gas line B1, B2, similar to the direct reduced iron manufacturing equipment 30a of the present embodiment 1. The heat exchanger 3 includes a top gas heat recovery heat exchanger 3a and a circulation gas preheater (preheater) 3b. The same components as those in the first embodiment are designated by the same reference numerals and the description thereof will be omitted.
[0206] Moreover, the direct reduced iron manufacturing equipment 30d of the fourth embodiment includes a methane generator 24 downstream of the CO2 remover 6. A gas (not shown in FIG. 1) mainly composed of CO2 separated and removed by the CO2 remover 6 and a hydrogen-containing gas C1 mainly composed of hydrogen that is separately produced are introduced into the methane generator 24. Then, in the methane generator 24, the gas mainly composed of CO2 and the hydrogen-containing gas C1 mainly composed of hydrogen are mixed to generate methane.
[0207] The gas mainly composed of methane produced in the methane generator 24 is mixed with the hydrocarbon-containing gases A1, A2, A3, A4, and A5 required in the direct reduced iron production equipment 30d and used as at least a part of those hydrocarbon-containing gases.
[0208] As in the fourth embodiment, carbon monoxide introduced into the reduction furnace 2 reduces iron oxide to generate carbon dioxide, and most of the carbon dioxide contained in the circulating gas is separated by the CO2 remover 6.
[0209] This separated gas containing carbon dioxide as a main component is mixed with a hydrogen-containing gas C1 containing hydrogen as a main component, which is separately produced, and methane is produced in the methane production device 24 by the following reaction or the like in the presence of a catalyst. CO2+4H2=CH4+2H2O
[0210] In this way, methane (CH4) is regenerated by reacting the carbon monoxide produced by the reforming reaction of hydrocarbons with the carbon dioxide produced by the reduction reaction of the carbon monoxide with iron oxide and the hydrogen in the hydrogen-containing gas C1, which is mainly composed of hydrogen, with the methane being recycled as the hydrocarbon-containing gases A1, A2, A3, A4, and A5 required in the direct reduced iron production facility 30d. This makes it possible to recycle and reuse the carbon components contained in the reduced iron and discharged to the outside of the system, as well as trace amounts of carbon components contained in the gas leaking to the outside of the system, and trace amounts of carbon components that are dissolved in the cooling water system and discharged by being degassed.
[0211] As described above, most of the consumed carbon components are taken out as carbon components in the reduced iron, so by replenishing a hydrocarbon gas containing an amount of carbon equal to the amount of carbon in the reduced iron, it is possible to reduce iron oxide without emitting carbon dioxide and by replenishing a small amount of hydrocarbon gas.
[0212] Furthermore, by similarly capturing the carbon dioxide that is generated during decarburization in the steelmaking process and mixing it with hydrogen to produce and use methane, it will be possible to recycle most of the carbon.
[0213] By recycling carbon as described above, hydrogen becomes the main reducing agent raw material introduced from outside the system to the direct reduced iron production facility 30d. On the other hand, the reduction of iron oxide itself is carried out with reducing gas containing carbon monoxide and hydrogen generated by the methane generation reaction of hydrogen and carbon dioxide and the reforming of methane and oxygen. This enables reduction similar to the conventional direct reduction reaction using hydrocarbons, and eliminates various problems that occur when direct reduction is performed with hydrogen. In addition, carburization of the reduced iron does not depend on the cooling process by hydrocarbons and occurs during the reduction process. Therefore, even if the direct reduced iron is discharged while hot, the required carbon is contained in the direct reduced iron, and various problems in downstream processes caused by a lack of carbon components are eliminated.
[0214] Although the first to fourth embodiments of the present invention have been described above with reference to the drawings, the present invention is not limited to the first to fourth embodiments, and various modifications are possible without departing from the spirit of the present invention.
[0215] For example, in the first to fourth embodiments, a single reforming and reducing gas circulation loop using the autothermal reformer 8 for one vertical reducing furnace 1 has been described, but it may be used in combination with other gas circulation loops.
[0216] That is, by extracting a part of the top gas or circulating gas from an existing reduced iron production facility, producing a reformed gas by applying the present invention, and combining the reformed gas with the existing furnace inlet gas, it is possible to increase the amount of reducing gas that can be introduced into the vertical reduction furnace, and thus the production capacity of the existing reduced iron production facility can be improved.
[0217] Conversely, a reformer employed in the Midrex process or the HYL process may be used as an auxiliary to the present invention to produce reformed gas, and both gases may be introduced into the vertical reduction furnace.
[0218] In the above-mentioned first to fourth embodiments, the amount of water vapor in the circulating gas is adjusted by adjusting the saturated vapor pressure of water vapor through the outlet pressure and temperature of the moisture adjusting device (top gas scrubber) 4. However, the water vapor component may also be adjusted by installing an aftercooler or a water vapor mixing device on the outlet side of the circulating gas compressor 5 or the CO2 remover 6.
[0219] In addition, a portion of the gas from the first gas mixing device 7a or the second gas mixing device 9 may be introduced into a packed tower or fluidized bed of solid hydrocarbons such as waste plastics or coal, and the solid hydrocarbons or coal may be thermally decomposed or partially oxidized with an oxygen-containing gas to generate hydrogen, carbon monoxide, and a hydrocarbon-containing gas, which may be utilized as a hydrocarbon-containing reducing gas.
[0220] When waste plastic is used, the amount of hydrocarbon-containing gas required can be reduced, and waste plastic sticks can also be treated at the same time, making this method extremely effective in areas where hydrocarbon-containing gas is expensive or where waste plastic treatment is necessary.
[0221] In addition, a portion of the top gas may be branched off before being mixed with the oxygen-containing gas, and the oxygen-containing gas and steam may be introduced as necessary into a facility for treating solid hydrocarbons such as waste plastics, where the solid hydrocarbons are partially oxidized and thermally decomposed to generate hydrogen, carbon monoxide, and a hydrocarbon-containing gas, which may be used as a hydrocarbon-containing reducing gas.
[0222] In addition, various measures can be taken according to the requirements of downstream electric furnaces, or in cases where there is no downstream electric furnace and direct reduced iron is exported.
[0223] For example, when melting reduced iron at room temperature in an electric furnace because the raw material handling equipment of the electric furnace is designed for room temperature, it is desirable to increase the amount of oxygen blown into the electric furnace as much as possible to increase productivity, so reduced iron with a high carbon content is desirable.
[0224] In this case, as described above, the inlet temperature of the cooling gas to the reduction furnace 1 is lowered as much as possible using the cooling gas aftercooler 15 or the like so that the temperature of the reduced iron becomes room temperature, while the flow rate of the cooling gas is reduced to increase the outlet temperature of the cooling zone 12, and the carbon amount in the reduced iron is increased by the hydrocarbon-containing gas preheated to a high temperature, making it possible to produce and supply reduced iron with a high carbon content at room temperature.
[0225] Furthermore, the cooling gas aftercooler, which is a system for introducing low-temperature cooling gas, may be a chiller-type aftercooler alone, or may be a mixer-type aftercooler that mixes a hydrocarbon-containing gas cooled by its own adiabatic expansion, etc. Also, a system may be used in which both a chiller-type aftercooler and a hydrocarbon-containing gas mixer-type aftercooler are used, for example, to mix a circulating cooling gas cooled by the chiller-type aftercooler with a further low-temperature hydrocarbon-containing gas, and introduce the cooling gas cooled by the mixer-type aftercooler into the cooling zone.
[0226] 1 to 5, the hydrocarbon-containing gas A5 is introduced into the cooling gas aftercooler 15, but it may be introduced from an appropriate position on the inlet side or outlet side of the cooling gas compressor 14 depending on the gas pressure and the desired cooling gas temperature. Furthermore, depending on the configuration of the cooling aftercooler 15 and the temperature of the hydrocarbon-containing gas to be introduced, the gas may be introduced into the inlet side or outlet side of the chiller-type aftercooler. Furthermore, if a low-temperature hydrocarbon-gas-containing gas mixer (mixer-type aftercooler) is provided, the gas may be introduced into the mixer.
[0227] 1 to 5, a part of the cooling gas is cooled by the cooling gas aftercooler 15, and the cooled cooling gas and the uncooled cooling gas are separately introduced into the cooling zone 12. However, this is not limited to the configuration, and all of the cooling gas may be cooled by the cooling gas aftercooler 15 and introduced into the cooling zone 12. Also, the cooled cooling gas and the uncooled cooling gas may be mixed and introduced into the cooling zone 12.
[0228] Furthermore, when a large amount of cooling gas is extracted to the reduction zone 2 or the circulation gas line as described above, it is necessary to supply a large amount of hydrocarbon-containing gas to the cooling zone 12, and the required cooling gas circulation air volume is reduced. Therefore, most or all of the circulating cooling gas from the cooling gas compressor 14 may be supplied to the cooling zone 12 without passing through the cooling gas aftercooler 15, and only the hydrocarbon-containing gas or a hydrocarbon-containing gas mixed with a small amount of the circulating cooling gas may be supplied from the bottom of the cooling zone 12 via the cooling gas aftercooler 15.
[0229] In addition, the reduction zone 2 and the cooling zone 12 may be separated and a high-temperature cooling gas may be introduced into the reduction zone 2, or the cooling zone 12 may be divided and an intermediate cooling zone 21 may be provided so that the high-temperature cooling gas comes into contact with the high-temperature reduced iron.
[0230] On the other hand, when the transport equipment is of high-temperature specification, for example, capable of melting reduced iron at 500°C or higher, if the reduced iron contains too much carbon, a decarburization process is required after complete melting in the electric furnace, which actually reduces the productivity of the electric furnace.
[0231] In this case, if the supply of cooling gas is completely stopped and the introduction of high-concentration hydrocarbon-containing gas into the cooling zone 12 and the reduction zone 2 is prevented, the cracking reaction of the hydrocarbon gas will not occur, and high-temperature reduced iron with a low carbon content can be produced and supplied.
[0232] In addition, when the reduction zone 2 and the cooling zone 12 are separated as shown in FIG. 2, the reduced iron may be discharged directly from the reduction zone 2.
[0233] In addition, when producing hot briquette iron (HBI) for transporting the direct reduced iron by sea, a hot briquette machine can be placed downstream of the vertical reduction furnace 1 and the high-temperature reduced iron can be directly supplied from the reduction zone 2 to the briquette machine to produce HBI.
[0234] Furthermore, when reduced iron of an intermediate temperature is required, it is possible to increase the inlet temperature of the cooling gas to some extent and increase the amount of the cooling gas, for example, by allowing a part of the cooling gas to bypass the aftercooler 15. In this case, the outlet temperature of the cooling zone 12 becomes intermediate, and intermediate-temperature reduced iron containing intermediate carbon can be produced and supplied.
[0235] The carbon amount in the reduced iron can be adjusted regardless of the manufacturing method and conditions of the reformed gas, so that an autothermal reformer may not be used, for example, by modifying an existing direct reduced iron manufacturing facility. Specifically, the configurations of the cooling zone 12, intermediate cooling zone 21, and cooling gas loop 23 in the above-mentioned embodiments 1 to 4 may be incorporated into an existing direct reduced iron manufacturing facility equipped with an externally heated reformer (reformer) or an external combustion type circulation gas preheater (preheater). This makes it possible to easily adjust the carbon amount contained in the reduced iron produced, even in an existing direct reduced iron manufacturing facility, and to obtain high quality reduced iron.
[0236] In addition, when the heated cooling gas is mixed in the first hydrocarbon-containing gas mixing device 7b, by making the first hydrocarbon-containing gas mixing device 7b an ejector type, a high-temperature booster is not required, resulting in a system that is simple in terms of equipment and highly reliable.
[0237] Furthermore, it is even more advantageous to pass the mixture through a high-temperature dust remover such as a ceramic filter before mixing, since this will prevent catalytic problems caused by reduced iron powder and the like in the autothermal reformer 8.
[0238] The cooling gas loop 23 of the present invention may be combined with a hydrogen reduction ironmaking facility. That is, the reduction of iron oxide is carried out with hydrogen, and carbon can be added to the reduced iron by hydrocarbons in the cooling zone 12 and the lower part of the reduction zone 2.
[0239] In this case, the reduction of iron oxide is carried out with hydrogen, so no carbon dioxide is generated. Also, the carburization reaction in the cooling zone 12 is as follows: CH4=C+2H2 No carbon dioxide is generated by the carburization reaction, and only a small amount of carbon dioxide is generated by the reforming of a small amount of hydrocarbons introduced into the reduction zone 2.
[0240] This solves the problem of the required amount of carbon in reduced iron, which was a major drawback of hydrogen reduction ironmaking, and also achieves the intended goal of significantly reducing the amount of carbon dioxide generated to a level roughly equivalent to that achieved by hydrogen-only reduced ironmaking processes.
[0241] In addition, the gas duct 16b for the circulation gas line for mixing the cooling gas extracted from the reduction furnace 1 with the circulation gas may be applied not only to the above-mentioned embodiment 2 but also to the above-mentioned embodiment 1, 3, or 4. When applied to embodiment 1 or 4, the gas duct 16b for the circulation gas line may be provided between the cooling gas outlet of the cooling zone 12 and the direct contact type water-cooled cooling gas cooler 13. When applied to embodiment 3, the gas duct 16b for the circulation gas line may be provided between the cooling gas outlet of the cooling zone 12 and the direct contact type water-cooled cooling gas cooler 13, and in the case of the intermediate cooling zone 21, since no equipment for direct water cooling is provided, at either one or both of any positions of the cooling gas loop 231. In these embodiments 1, 3, and 4, the gas duct 16b for the circulation gas line constitutes the gas duct 16.
[0242] Moreover, the methane generator 24 is not limited to the above-mentioned fourth embodiment, but may be applied to the above-mentioned second or third embodiment.
[0243] In addition, since the methane production reaction is an exothermic reaction in the methane generator 24, cooling is necessary, but by performing this cooling with the circulating gas, it is possible to preheat the circulating gas. In addition, when a CO2 remover that requires a regeneration heat source is used, by using the cooling heat of the methane generator 24 as the heat source, for example, steam is generated by cooling during methane production, and the steam is used to regenerate the CO2 capture liquid, thereby enabling efficient separation and capture of CO2 and regeneration of methane.
[0244] In addition, the direct reduced iron manufacturing equipment 30a, 30b, 30c, and 30d of the above-mentioned embodiments 1 to 4 are provided with the second gas mixer 9, the reformed gas cooler 10, the reformed gas mixer 11, and the cooling gas aftercooler 15, but these are not essential components and may be provided as necessary. In addition, the heat exchanger 3 may include at least one of a top gas heat recovery heat exchanger 3a and a circulation gas preheater (preheater 3b). In addition, the line for introducing the hydrocarbon-containing gas A5 shown in Figures 1 to 5 into the cooling gas loop 23 is not limited to the position shown in Figures 1 to 5, and may be any position in the cooling gas loop 23. [Explanation of symbols]
[0245] 1 Vertical reduction furnace 2 Reduction Zone 3 Heat exchanger 3a Top gas heat recovery heat exchanger 3b Circulation gas preheater (preheater) 4. Moisture control device (top gas scrubber) 5. Circulation Gas Compressor 6. CO2 Remover 7a First gas mixing device 7b First hydrocarbon-containing gas mixing device 8 Autothermal Reformer 9 Second gas mixing device 10 Reformed gas cooler 11 Reformed gas mixer 12 Cooling Zone 13 Cooling gas scrubber (direct contact water-cooled cooling gas cooler) 14 Cooling gas compressor 15 Cooling gas aftercooler 16 Gas duct (cooling gas connection duct) 16a Gas duct for reduction zone 16b Gas duct for circulation gas line 17 Cooling gas dust collector 18 Cooling gas dust collector 19 Cooling gas heat exchanger (boiler) 20 Intermediate Cooling Gas Compressor 21 Intermediate Cooling Zone 22 SHOTS 23 Cooling gas loop 231 Upper cooling gas loop 232 Lower cooling gas loop 24 Methane Generator 30a, 30b, 30c, 30d Direct reduced iron manufacturing equipment A1, A2, A3, A4, A5 Hydrocarbon-containing gases B1, B2 High-concentration oxygen-containing gas C1 Hydrogen-containing gas
Claims
1. A direct reduced iron manufacturing facility for manufacturing direct reduced iron by contacting an iron oxide raw material with a reducing gas in a vertical reduction furnace, A CO 2 removal system for removing a part or all of carbon dioxide from the gas discharged from the vertical reduction furnace 2 Remover and The CO 2 a methane generator that mixes the gas mainly composed of carbon dioxide separated and recovered by the remover with a hydrogen-containing gas to generate methane; a cooling gas loop for circulating a cooling gas for cooling the reduced iron produced in the vertical reduction furnace, The generated methane is utilized in the direct reduced iron production facility, The vertical reduction furnace has a reduction zone and a cooling zone, the cooling gas loop can lower a temperature of the cooling gas at an inlet of the reduction furnace, thereby reducing a flow rate of the cooling gas introduced into the vertical reduction furnace, and can adjust a concentration of a hydrocarbon-containing gas in the cooling gas, and the cooling gas aftercooler is provided on an outlet side of a cooling gas compressor.
2. A direct reduced iron manufacturing facility as described in claim 1, characterized in that the reduction zone and the cooling zone are configured as furnaces independent of each other and are connected by a chute that lowers reduced iron into the cooling zone and a gas duct for the reduction zone that passes cooling gas into the reduction zone.
3. 3. The direct reduced iron manufacturing facility according to claim 1, wherein at least a part of the cooling gas introduced into the cooling zone has a temperature of 35° C. or less at an inlet of the vertical reduction furnace, and a hydrocarbon concentration of the cooling gas at the inlet of the reduction furnace is 50% or more.
4. A reformer for producing a reducing gas is provided, 4. The direct reduced iron manufacturing facility according to claim 1, wherein the cooling gas extracted from the cooling zone of the vertical reduction furnace is mixed with at least one of the reducing gas to be introduced into the vertical reduction furnace and the gas flowing upstream of the reformer without passing through a direct contact type water-cooled cooling gas cooler.
5. A direct reduced iron manufacturing facility for producing direct reduced iron by contacting an iron oxide raw material with a reducing gas in a vertical reduction furnace, comprising: a CO 2 remover that removes a part or all of carbon dioxide from the gas discharged from the vertical reduction furnace; a methane generator that mixes a gas mainly composed of carbon dioxide separated and recovered by the CO 2 remover with a hydrogen-containing gas to generate methane; a moisture adjusting device for adjusting moisture from the gas discharged from the vertical reduction furnace; a first gas mixing device for mixing an oxygen-containing gas and a hydrocarbon-containing gas with the gas from which the moisture has been adjusted by the moisture adjusting device and from which carbon dioxide has been removed by the CO 2 remover; an autothermal reformer that reforms the mixed gas produced in the first gas mixing device by its own energy; The generated methane is utilized in the direct reduced iron production facility, The first gas mixing device adjusts the amounts of the oxygen-containing gas and the hydrocarbon-containing gas to be mixed, so that the gas temperature at the inlet of the autothermal reformer, the gas temperature at the outlet, and the reduction degree of the gas at the outlet are adjusted to be within appropriate ranges; 1. A direct reduced iron production facility, comprising: a gas temperature at an outlet of the autothermal reformer being adjusted to 700° C. or higher; and a pressure at which gas is introduced into the autothermal reformer being adjusted to less than 600 kPA (A).
6. 6. The direct reduced iron production facility according to claim 5, further comprising a second gas mixing device for mixing an oxygen-containing gas and a hydrocarbon-containing gas with the gas discharged from the autothermal reformer.
7. The autothermal reformer has multiple stages, 7. The direct reduced iron production facility according to claim 5 or 6, wherein the degree of reduction of the gas at the outlet of the final stage autothermal reformer is 7 or more.
8. A method for producing direct reduced iron, comprising contacting an iron oxide raw material with a reducing gas in a vertical reduction furnace having a reduction zone and a cooling zone in a direct reduced iron production facility, the method comprising: removing a part or all of the carbon dioxide from the gas discharged from the vertical reduction furnace; and mixing the separated and recovered gas mainly composed of carbon dioxide with a hydrogen-containing gas to produce methane. The generated methane is utilized in the direct reduced iron production facility, the direct reduced iron manufacturing facility includes a cooling gas loop that cools the reduced iron produced in the vertical reduction furnace, a cooling gas aftercooler provided on the outlet side of a cooling gas compressor, the cooling gas loop can lower the temperature of the cooling gas at the inlet of the reduction furnace, thereby reducing the flow rate of the cooling gas introduced into the vertical reduction furnace and adjusting the concentration of a hydrocarbon-containing gas in the cooling gas.
9. A method for producing direct reduced iron, comprising contacting an iron oxide raw material with a reducing gas in a vertical reduction furnace in a direct reduced iron production facility, the method comprising: removing a part or all of carbon dioxide from the gas discharged from the vertical reduction furnace by a CO 2 remover; and mixing the separated and recovered gas mainly composed of carbon dioxide with a hydrogen-containing gas to produce methane. The generated methane is utilized in the direct reduced iron production facility, The direct reduced iron manufacturing facility includes a moisture adjusting device for adjusting moisture from the gas discharged from the vertical reduction furnace, a first gas mixing device for mixing an oxygen-containing gas and a hydrocarbon-containing gas with the gas from which moisture has been adjusted by the moisture adjusting device and from which carbon dioxide has been removed by the CO 2 remover, and an autothermal reformer for reforming the mixed gas produced by the first gas mixing device by its own energy, The first gas mixing device adjusts the amounts of the oxygen-containing gas and the hydrocarbon-containing gas to be mixed so that the gas temperature at the inlet of the autothermal reformer, the gas temperature at the outlet, and the reduction degree of the gas at the outlet are within appropriate ranges; A method for producing direct reduced iron, comprising adjusting a temperature of a gas at an outlet of the autothermal reformer to 700°C or higher, and adjusting a pressure of the gas introduced into the autothermal reformer to less than 600 kPA (A).
Citation Information
Patent Citations
JP1972002901B1
Control of reduced iron discharge in vertical reducing furnace
JP1979084816A
Method and apparatus for direct reduction iron making
JP1980113819A
Method for direct reduction ironmaking, and apparatus for production of reducing gas therefor
JP2012007213A
Blast furnace operation method
JP2014005510A