Stabilization of laser-patterned organic thin-film solar cells

Nanoporous plasma polymer layers, like SiOCH, stabilize laser-patterned protrusions in organic thin-film solar cells, addressing adhesion and short circuit issues, enabling roll-to-roll processing and enhancing module durability.

JP7555341B2Active Publication Date: 2024-09-24HELIATEK GMBH +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021534305
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-14
Filing Date
2019-12-16
Publication Date
2024-09-24
Estimated Expiration
2039-12-16

AI Technical Summary

Technical Problem

Existing methods for stabilizing protrusions caused by laser patterning in organic thin-film solar cells, such as UV crosslinking layers, can outgas and cause adhesion issues, while roll-to-roll processes require uniform coating and are not suitable for large-area modules, leading to short circuits and reduced service life.

Method used

The use of nanoporous plasma polymer-based stabilization layers, such as SiOCH, deposited via PECVD, to stabilize laser-patterned protrusions, allowing for subsequent sealing and protection during manufacturing processes.

Benefits of technology

Prevents short circuits and ensures mechanical protection, enabling roll-to-roll processing and extended service life by providing a flexible, water vapor barrier that protects the organic stack from adhesive interactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555341000006
    Figure 0007555341000006
  • Figure 0007555341000004
    Figure 0007555341000004
  • Figure 0007555341000001
    Figure 0007555341000001
Patent Text Reader

Abstract

During laser patterning of organic thin film solar cell components, protrusions that exceed the stack height by several times can occur. The present invention describes a technique for stabilizing the laser-patterned protrusions to allow further processing of the preform, followed by introduction into the encapsulation of the OPV component.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention describes a method for producing a layer for stabilizing protrusions in laser-patterned organic thin-film solar cells (OPVs) and a stabilization layer for laser-patterned organic thin-film solar cells. [Background technology]

[0002] An organic thin-film solar cell module consists of a stack on a substrate, which contains two electrodes, one of which is placed on the substrate and the other electrode is placed away from the substrate as a counter electrode. Between the two electrodes an organic laminate is arranged. Organic thin-film solar cell modules can be produced, for example, by evaporating materials, printing polymers or processing from a liquid. The principle structure of organic photoactive components is disclosed, for example, in WO2004083958 and WO2011138021.

[0003] The inventors understand small molecules to be absorber materials that contain a well-defined number of monomers, typically 10 or less, have a well-defined mass, typically 1500 g / mol or less, preferably 1200 g / mol or less, and do not have undefined, possibly reactive groups at the end of the molecular chain, so that they may be present in the polymer as a by-product of a polymerization chain reaction. The advantage of these absorber materials in the small molecule system is their evaporability in vacuum and the associated possibility of purification by gradient sublimation, which allows the production of arbitrarily complex multilayer systems by sequential evaporation of different pure materials. Moreover, these absorber materials allow photoactive heterojunctions, for example bulk heterojunctions.

[0004] The photoactive layers in the stack of the cell may contain only one acceptor absorber material, only one donor absorber material, or a combination of multiple absorber materials of different and / or the same type, which contribute to the formation of excitons. Additionally, materials may be added to the absorber layers to improve the absorption properties.

[0005] Furthermore, the organic stack between the electrodes does not have to consist of only photoactive (absorber) layers. To build a multi-cell system, further layers, such as transport layers, preferably doped transport layers between the individual photoactive (absorber) layers / (absorber) layer systems and between the organic photoactive (absorber) layer systems and the electrodes, can be introduced into the stack. This allows an optimal positioning of the photoactive layers with respect to the field strength distribution of the optical field.

[0006] Organic thin-film photovoltaic modules (organic solar cells or organic photodetectors) need to be adequately protected by encapsulation, since direct contact with air and / or oxygen and / or water significantly reduces their service life. The encapsulation can be achieved by a barrier film or by a direct encapsulant.

[0007] The laser-treated organic thin-film solar cell module is patterned by laser processing. This method is / can also be used for the connection of individual solar cell strings on the module and for the electrical isolation of the solar module, especially in a roll-to-roll process. The connection of the organic thin-film solar cell strings to the module can be realized by laser connections (P1, P2, P3, P4), the principle of which is described, for example, in DE 10 2016 118 177 A1.

[0008] This leads to so-called laser scribe protrusions, especially during the patterning of the electrodes, which can exceed the height of the flat laminate of the stack of organic thin-film photovoltaic modules by many times. At organic laminate thicknesses of about 100-400 nm, protrusions with a height of more than 2 μm have already been measured. These can damage the module if it is rolled up without a cover layer, or damage the organic layers by the adhesive used if it is subsequently sealed.

[0009] DE 10 2015116418 A1 proposes printing a UV-crosslinked layer as a winding protection layer, which is applied in liquid form on a silicon basis in order to prevent folding or crimping of protrusions from causing short circuits in further method steps, for example when winding up the module.

[0010] US 2008 / 0102206 A1 discloses a method for producing a multi-layer coating in one method step by varying process parameters.

[0011] Gebhard, M. et al.: Laser structuring of flexible organic solar cells. Laser Technik Journal 1013, H.1, S.25-28. describes P1, P2, and P3 laser patterning for the fabrication of polymer solar cells. Summary of the Invention [Problem to be solved by the invention]

[0012] Shortcomings of the prior art The printed UV crosslinked layer proposed in DE 102015116418 A1 can still produce gas after crosslinking, which can impair the adhesion of the subsequent encapsulation. Furthermore, peeling of the counter electrode was rarely observed. Also, placing the liquid material on the underlying organic stack is undesirable, as it can attack the organics, i.e. the organic laminate placed between the electrodes, leading to a reduced service life and performance of the organic solar cell. For roll-to-roll processes for the production of large-area modules, simply covering the organics, as used for small laboratory samples, is not sufficient, as this can lead to short circuits. Furthermore, for roll-to-roll processes, the process parameters must be kept constant with a certain variation range in order to apply the material uniformly.

[0013] The method disclosed in US 2008 / 0102206 A1 is not suitable for the production of large area modules by the roll-to-roll method, since according to the method in the chamber, during this method step, the plasma mixture changes in the chamber (strong fluctuation of parameters), which results in the application of several different coating layers. This can only be used in "fixed" chambers, but not if the object to be coated moves in the chamber. The method described in US 2008 / 0102206 A1 has the problem of realizing a water barrier in the scope of use as an encapsulant. Furthermore, the coatings produced by the method described in US 2008 / 0102206 A1 cannot be used as wound protective layers, since these parameters allow a rather hard coating.

[0014] The technical problem on which the invention is based was, on the one hand, to stabilize the protrusions resulting from the laser patterning of the layers of the solar cell, thus eliminating the drawbacks identified in the prior art, and, on the other hand, to enable sealing and encapsulation with a thin layer that can be integrated in a roll-to-roll process. Usability is particularly important for small molecule-based OPVs. After the application of this layer, an encapsulant can be applied to the smooth surface. Furthermore, it is important that this layer itself allows the winding of the semi-finished product and does not adversely affect the subsequent winding and unwinding of the finished product.

[0015] The inventors understand a semi-finished product to be an OPV module that has not yet been encapsulated. The finished product will be encapsulated and equipped with the terminals required for operation. The challenge of encapsulation is to provide a barrier against environmental influences, e.g. water / water vapor, so as to extend the service life of the OPV module. [Means for solving the problem]

[0016] The technical problem of stabilizing the protrusions generated by the laser treatment is solved by a stabilization layer based on a nanoporous plasma polymer, for example SiOCH.

[0017] Nanoporous materials consist of a regular framework with a regular porous structure. The size of the pores is in the nanometer range. According to IUPAC (International Union of Pure and Applied Chemistry), nanoporous materials are divided into three groups: microporous materials with a size of less than 2 nm, mesoporous materials with a size of 2-50 nm, and macroporous materials with a size of more than 50 nm.

[0018] An encapsulant can then be applied to this stabilizing layer, which may require prior planarization.

[0019] The deposition of the SiOCH layer can be done by a Plasma Enhanced Chemical Vapor Deposition (PECVD) method, for example the Hollow Cathode PECVD (arcPECVD) method, via the HMDSO precursor or the Bistrimethylsilimethane (BTMSM) precursor or the Tetraethylorthosilicate (TEOS) precursor or the Tetramethylsilane (TMS) precursor or the Hexamethyldisilazane (HMDSN) precursor (further precursors (precursor materials) are possible). The use of microwave PECVD methods is known from the manufacturing field for the encapsulation of OLEDs (organic light emitting diodes). In the manufacture of OLEDs, no laser patterning of layers is necessary or known, so that a flat topography is obtained for the OLEDs and the encapsulation can be realized directly by thin film encapsulation (TFE), for example performed by microwave PECVD deposition. In the manufacture of OLEDs, plasma polymers with low dielectric constant k (Low-k materials) have been proposed as one of the barrier materials.

[0020] The method according to the invention differs from the microwave PECVD methods used in the OLED field, which are mainly oxidative in nature and affect the organic content of the layer by the use of a DC power source, allowing the deposition of layers up to 500 nm or up to about 1 or 2 μm thick, which is thicker than a direct SiN encapsulant, which is typically about 100 nm thick.

[0021] In order to use a layer for stabilization of laser-patterned projections, it is particularly important that this layer has nanoporous properties, so that the stabilization layer can also be rolled up in further manufacturing processes. The manufacturing parameters known in the prior art do not result in nanoporous and flexible layers, but rather inflexible layers that are very stable. Only by extensive testing and adjusting the parameters could a nanoporous and flexible layer be produced that overcomes the disadvantages of the prior art.

[0022] SiOCH is a silicon oxide (SiOx) that acquires organic properties due to its carbon content, which affects its chemical structure and its polymeric, partially cross-linked chain structure. The material is more elastic and flexible than SiOx, making it a nanoporous material with flexible and elastic properties.

[0023] The technical challenge to stabilization and sealing of the laser patterned protrusions (A, B) is solved by the application of a plasma polymer layer and subsequent sealing, which includes the following steps: 1. Providing a laser patterned OPV on a substrate, the OPV including at least an organic stack and a substrate electrode pattern; 2. Installing a stabilization layer; 3. Depositing an optional planarization layer; 4. Installing the sealant.

[0024] Providing a laser patterned OPV includes at least the following steps. 1. Providing a substrate (1); 2. Providing a substrate electrode (2) and patterning the substrate electrode (2); 3. Depositing the layers of an organic solar cell, including the transport layers and the photoactive absorber layer, called stack (3), including the patterning of the organic stack; 4. Providing the counter electrode (4).

[0025] Ideally, the stabilization layer comprises a SiOCH material or a material similar to SiOCH that has nanoporous properties.

[0026] This provides stabilization of the laser patterned protrusions for subsequent encapsulation and as a wrap-around protective layer during manufacturing.

[0027] The use of other plasma polymers is possible if this has no effect on the organics of the thin-film solar module (damage, reduction in service life), is a transparent material with long-term stability and has sufficient mechanical stability, i.e. adhesion and flexibility, or thermal expansion properties so that no additional stresses arise due to the different expansion of different materials (organics and stabilization layers).

[0028] Ideally, the stabilization layer can protect the organic stack of the solar cell from unintended interactions with the barrier film adhesive when the entire module is subsequently encapsulated with the barrier film and adhesive.

[0029] Ideally, the stabilizing layer allows for winding and unwinding during subsequent process steps for producing the finished product in a roll-to-roll process and / or during winding of the finished product. Effect of the Invention

[0030] The technical problem was solved to stabilize the laser treated protrusions of the organic stack so that the module could be subsequently sealed. This leads to: a) Short circuits caused by folding back or folding back of protrusions after laser patterning are prevented. b) A closed planar feature is provided so that a subsequent encapsulant, such as a thin film encapsulant, can be applied to the planar feature required for the encapsulation process. c) Ensuring sufficient mechanical protection of the organic solar cells, for example after application of the stabilization layer and any planarization layer, to allow winding and unwinding during the roll-to-roll process. d) During the subsequent encapsulation of the entire module with a barrier film and adhesive, the stabilization layer according to the invention can better protect the organic stack of the solar cell from unintended interactions with the barrier film adhesive.

[0031] The use of PECVD hollow cathode deposition and the resulting SiOCH layer results in a more elastic structure than a silicon nitride barrier layer (SiN), even at the high layer thicknesses required to cover the laser-patterned protrusions, and also provides a water vapor barrier, which improves water vapor protection in the next process steps and prevents / reduces outgassing of materials used during encapsulation in the organic stack. [Brief description of the drawings]

[0032] [Figure 1] FIG. 1 shows an exemplary configuration of a laser-patterned organic solar cell having protrusions (A) (and (B)) that require stabilization and planarization for encapsulation, including a stabilization layer (5) according to the present invention, an optional planarization layer (6), and an encapsulant (7). [Diagram 2] The size of the laser patterned protrusions is shown in relation to the stabilizing layer (5) and optional planarizing layer (6) and encapsulant (7). [Diagram 3] The size of the laser patterned protrusions is shown in relation to the stabilizing layer (5) and optional planarizing layer (6) and encapsulant (7). [Figure 4] The size of the laser patterned protrusions is shown in relation to the stabilizing layer (5) and optional planarizing layer (6) and encapsulant (7). [Diagram 5]The size of the laser patterned protrusions is shown in relation to the stabilizing layer (5) and optional planarizing layer (6) and encapsulant (7). [Figure 6] 1 shows experimental physical results of laser patterned OPV with and without a stabilization layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The manufacture of organic solar cell modules by roll-to-roll technology involves the provision of a substrate on which a first electrode (substrate electrode) is deposited and then patterned, and an organic stack deposited between the first electrode and a second electrode (counter electrode), comprising an absorber layer and both (partially) doped and undoped transport layers, followed by the deposition of the second electrode (counter electrode).

[0034] According to the invention, a nanoporous plasma polymer based stabilizing layer is applied to the above laminate to protect the laser patterned protrusions.

[0035] Stabilization is performed in preparation for subsequent encapsulation by a method that includes the following process steps. a) Providing an organic stack of a solar cell with P3 patterning. b) applying a stabilizing layer (5) followed by an encapsulant (7);

[0036] The stabilization layer (5) comprises a nanoporous plasma polymer comprising at least one precursor selected from the group of tetramethylsilane (TMS), hexamethyldisiloxane (HMDSO), tetraethylorthosilicate (TEOS), hexamethyldisilazane (HMDSN), silane (SiH4), triethoxysilane (TriEOS), tetramethoxysilane (TMOS), and trimethoxysilane (TriMOS).

[0037] According to one embodiment, the stabilization layer (5) has a thickness greater than 100 nm, preferably greater than 150 nm, particularly preferably greater than 200 nm, very particularly preferably greater than 300 nm and more particularly preferably greater than 500 nm.

[0038] According to one embodiment of the invention, the stabilization layer (5) contains at least 2 at.% silicon or titanium, at least 2 at.% oxygen or nitrogen, and at least 2 at.% carbon.

[0039] According to one embodiment of the invention, the stabilization layer (5) comprises a carbon content greater than 15 at.%, preferably greater than 20 at.%, particularly preferably greater than 25 at.%.

[0040] According to one embodiment, the stabilization layer (5) may be configured as a gradient, with the carbon content varying across the thickness of the layer by at least about 2 at.%, preferably at least about 4 at.%, particularly preferably by more than about 6 at.%.

[0041] In the production of nanoporous plasma polymers, a reactive gas selected from nitrogen and / or oxygen is used.

[0042] In other embodiments, the stabilization layer includes a material similar to SiOCH, such as, for example, SiONCH, SiNCH, or the like.

[0043] These are produced by using precursors selected from the group above in combination with nitrogen as the reactive gas.

[0044] Additionally / alternatively, a titanium-containing layer may be used as the stabilization layer, which can be produced using titanium-containing monomers such as titanium propoxide, tetraisopropoxyl orthotitanate (TIPT), or TiCl4.

[0045] In other embodiments, tetramethylaluminum, trimethylaluminum have been proposed as stabilizing layers that can be produced using Al2O3 in combination with N2O.

[0046] Furthermore, during the production, an inert gas is used, selected from the group of noble gases, such as argon, xenon, neon, preferably argon.

[0047] After extensive testing, the inventors have adjusted the parameters for the manufacture of the stabilization layer, which in unfavourable cases, when using the parameters known in the prior art, results in a stabilization layer that is so strong that it causes the electrode to peel off from the organic stack during winding.

[0048] According to the invention, the ratio of reactive gas to precursor is greater than 4, preferably greater than 6, and less than 20, preferably less than 12, particularly preferably less than 10. If the ratio is too low, the layer stress in the stabilization layer becomes too large.

[0049] According to the invention, the coating pressure is less than 50 Pa, preferably less than 10 Pa, particularly preferably less than 5 Pa.

[0050] According to the present invention, the plasma power per 1 sccm of precursor monomer is 100 W / sccm or less, preferably in the range of 15 to 80 W / sccm, more preferably in the range of 30 to 80 W / sccm, and particularly preferably in the range of 40 to 50 W / sccm.

[0051] The subsequent encapsulation (7) can be performed by a barrier film or a direct encapsulant, which can be achieved by known methods.

[0052] If the protrusions are very large, it may be necessary to apply a planarizing layer after stabilization to ensure sealing on a flat surface.

[0053] The planarization layer (6) can be achieved, for example, by providing a printed UV crosslinking layer as proposed in DE 102015116418 A1 or by another material, thereby providing a flat surface.

[0054] When sealing with a direct sealant, it may be beneficial to use other precursors, which can alter the pore size.

[0055] Furthermore, the encapsulation of the module can also be performed with at least one PECVD_layer or ALD (atomic layer deposition) layer. EXAMPLES

[0056] In a contemplated embodiment, the fabrication involves producing organic solar cells having organic layers made of small molecule based materials in a roll-to-roll coating apparatus.

[0057] Example 1 The solar cell module is characterized by a SiOCH deposition including rolling and unrolling and includes the following method steps: 1. Fabricating organic solar cells in a roll-to-roll coating equipment up to cathode deposition, followed by winding up the solar cell film. 2. Transporting under nitrogen to another roll-to-roll PECVD apparatus capable of operating at lower pressure. 3. Unrolling the solar cell film and P3 laser patterning. 4. Depositing a planarization layer as a wraparound protection layer. 5. Sealing with a barrier film.

[0058] Example 2 The solar cell module is characterized by a roll-in and roll-out free SiOCH deposition and comprises the following method steps: 1. Fabricating organic solar cells up to cathode deposition and P3 laser patterning in a roll-to-roll coating equipment. 2. Subsequently, deposit a planarization layer in an integrated PECVD tool / chamber (Caution: pressure regulation is required). 3. The next step is sealing with a barrier film.

[0059] Figure 6 shows the normalized efficiency during life testing of organic tandem solar cells (opaque or transparent) with SiOCH stabilization layer compared to the current configuration without SiOCH stabilization layer and using barrier layers (barrier films) with different adhesives (epoxy vs. acrylic) as encapsulants. The lines represent respectively with stabilization layer followed by encapsulation with barrier film with epoxy adhesive (filled circles), ▲ without stabilization layer followed by encapsulation with barrier film with epoxy adhesive (filled triangles), with stabilization layer followed by encapsulation with barrier film with acrylic adhesive (open circles), △ without stabilization layer followed by encapsulation with barrier film with acrylic adhesive (open triangles).

[0060] The service life is the same in both cases (with or without the stabilizing layer) or is slightly improved when an epoxy adhesive is used.

[0061] Example 3 The solar cell module is separated by SiOCH deposition in a full process thin film encapsulation including rolling and unrolling, and includes the following method steps: 1. Fabricating organic solar cells in a roll-to-roll coating equipment up to cathode deposition, followed by winding up the solar cell film. 2. Transporting under nitrogen to another PECVD apparatus capable of operating at lower pressure. 3. Unrolling the solar cell film and P3 laser patterning. 4. Depositing a planarization layer and a barrier layer or a corresponding barrier stack.

[0062] Example 4 The solar cell module is separated by SiOCH deposition in a full process thin film encapsulation including rolling and unrolling, and includes the following method steps: 1. Fabricating organic solar cells up to cathode deposition and P3 laser patterning in a roll-to-roll coating equipment. 2. Subsequent deposition of a planarization layer (pressure regulation is required in this case) and a barrier sealing layer or a corresponding barrier stack in an integrated PECVD apparatus / chamber. [Explanation of symbols]

[0063] 1 Board 2 1st electrode / substrate electrode 3 Organic matter 4 Second electrode / counter electrode 5 Stabilization layer 6 Planarization layer 7. Encapsulating material P1, P2, P3, P4 Laser Patterning A, B Laser patterning of the counter electrode and protrusions caused by patterning of the OPV

Claims

1. 1. A method for stabilizing and encapsulating a laser patterned organic thin film solar cell (OPV) in a roll-to-roll process, comprising: a. providing a laser patterned OPV on a substrate (1) by depositing a substrate electrode on said substrate electrode (2), laser patterning said substrate electrode (2), depositing a stack (3) on said substrate electrode (2), laser patterning said stack (3), and depositing a counter electrode (4); b. after step a), providing a stabilization layer (5), said stabilization layer (5) having nanoporous and flexible properties and comprising at least silicon, oxygen or nitrogen and carbon, said nanoporous and flexible stabilization layer (5) having a pore size of less than 2 nm and / or between 2 and 50 nm; c. after step b), providing a planarization layer (6); d. after step c), placing a sealant (7), A method characterized in that said stabilization layer (5) is applied by a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.

2. 2. A method according to claim 1, characterized in that the patterning of the counter electrode (4) is performed in step a).

3. 2. The method according to claim 1, characterized in that the patterning of the counter electrode (4) is performed between steps b) and c), and that after the patterning of the counter electrode (4) a further stabilization layer (5) is applied.

4. 2. A method according to claim 1, characterized in that the patterning of the counter electrode (4) follows immediately after step c) and that before step d) a further stabilisation layer (5) is applied.

5. Method according to any one of claims 1 to 4, characterized in that the stabilisation layer (5) is applied by hollow cathode or magnetron PECVD.

6. a. the stabilization layer (5) is formed using one or more precursors selected from the group of tetramethylsilane (TMS), hexamethyldisiloxane (HMDSO), tetraethylorthosilicate (TEOS), hexamethyldisilazane (HMDSN), silane (SiH4), triethoxysilane (TriEOS), tetramethoxysilane (TMOS), and trimethoxysilane (TriMOS); b. formed using a reactive gas selected from nitrogen and / or oxygen; c) The method according to any one of claims 1 to 5, characterized in that it is formed using an inert gas selected from the group of noble gases.

7. The method according to claim 1, wherein the coating pressure of the roll-to-roll coating apparatus is less than 50 Pa.

8. 7. The method of claim 6, wherein the ratio of reactant gas to precursor is greater than 2 and less than 20.

9. 7. The method of claim 6, wherein the ratio of reactant gas to precursor is greater than 2 and less than 10.

10. The method according to any one of claims 1 to 9, characterized in that the plasma power per sccm of precursor is less than or equal to 100 W / sccm.

11. The planarization layer is realized by printing a UV crosslinked layer or by PECVD using a precursor, The precursor is at least one precursor selected from the group consisting of tetramethylsilane (TMS), hexamethyldisiloxane (HMDSO), tetraethylorthosilicate (TEOS), hexamethyldisilazane (HMDSN), silane (SiH4), triethoxysilane (TriEOS), tetramethoxysilane (TMOS), and trimethoxysilane (TriMOS). The method according to any one of claims 1 to 10, characterized in that

12. 1. A stabilization layer (5) for stabilizing laser treated protrusions (A) of a laser patterned OPV, formed using at least one precursor selected from the group of tetramethylsilane (TMS), hexamethyldisiloxane (HMDSO), tetraethylorthosilicate (TEOS), hexamethyldisilazane (HMDSN), silane (SiH4), triethoxysilane (TriEOS), tetramethoxysilane (TMOS), and trimethoxysilane (TriMOS), the stabilization layer (5) having nanoporous and flexible properties and comprising at least silicon or titanium, oxygen or nitrogen, and carbon, the nanoporous and flexible stabilization layer (5) having a pore size of less than 2 nm and / or between 2 and 50 nm.

13. A stabilization layer (5) as described in claim 12, characterized in that the thickness of the stabilization layer (5) is greater than 100 nm.

14. 14. The stabilization layer (5) according to claim 12 or 13, characterized in that the carbon content is greater than 15 at.%.

15. A thin-film solar cell component comprising a stabilization layer (5) made according to the method of claim 1 and having laser-patterned protrusions.

16. 10. The method of claim 1, wherein the PECVD process comprises a hollow cathode PECVD process.

Citation Information

Patent Citations

  • Film solar battery of wide spectrum absorption

    CN202167502U

  • Optical electromotive device and manufacturing method

    JP2003115598A

  • Solar cell, multilayer substrate for solar cell, and manufacturing method thereof

    JP2012023070A

  • Manufacturing method of organic optical device

    JP2012190612A

  • Substrate equipped with organic functional layer and method for producing the same

    JP2015157370A