Nitride semiconductor light emitting device
The nitride semiconductor light emitting device improves optical output by using a c-plane sapphire substrate with a thick buffer layer and controlled oxygen concentration to minimize ultraviolet light absorption, addressing the issue of oxygen-induced output reduction.
Patent Information
- Application Number
- JP2023206638
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2024-09-24
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Nitride semiconductor light-emitting devices emitting ultraviolet light with a center wavelength of 365 nm or less face a decrease in optical output due to oxygen in the buffer layer absorbing ultraviolet light.
A nitride semiconductor light emitting device is designed with a c-plane sapphire substrate, a buffer layer thicker than 500 nm, and an average oxygen concentration of 4.5×10^21 atoms/cm^3 or less, with a ratio of buffer layer oxygen concentration to substrate oxygen concentration of 3/20 or less, to minimize light absorption.
This configuration enhances the optical output of the nitride semiconductor light emitting device by reducing ultraviolet light absorption in the buffer layer.
Smart Images

Figure 0007555470000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a nitride semiconductor light emitting device. [Background technology]
[0002] Patent Document 1 discloses a semiconductor light-emitting element having an emission peak wavelength of 380 nm or more and 425 nm or less, in which the crystallinity of each semiconductor layer formed on a buffer layer is improved by adjusting the oxygen concentration distribution in the buffer layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2019 / 044173 Summary of the Invention [Problem to be solved by the invention]
[0004] A new problem has been found in nitride semiconductor light emitting devices that emit ultraviolet light with a central wavelength of 365 nm or less: oxygen contained in the buffer layer absorbs the ultraviolet light, which can lead to a decrease in optical output.
[0005] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a nitride semiconductor light-emitting device capable of improving the optical output. [Means for solving the problem]
[0006] In order to achieve the above object, the present invention provides a method for growing a semiconductor device having a c-plane as a growth plane. sapphire a substrate, a buffer layer formed on the growth surface, an n-type semiconductor layer formed on the buffer layer, an active layer formed on the n-type semiconductor layer and emitting ultraviolet light having a central wavelength of 365 nm or less, and a p-type semiconductor layer formed on the active layer, wherein the buffer layer has a thickness of more than 500 nm, and the average oxygen concentration of the buffer layer is 4.5×10 21atoms / cm 3 The following is satisfied, and sapphire The present invention provides a nitride semiconductor light emitting device, in which the ratio of the average oxygen concentration of the buffer layer to the average oxygen concentration of the substrate satisfies 3 / 20 or less. Effect of the Invention
[0007] According to the present invention, it is possible to provide a nitride semiconductor light emitting device capable of improving the optical output. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic diagram illustrating a configuration of a nitride semiconductor light emitting device according to an embodiment. [Diagram 2] 11 is a graph showing the relationship between the average oxygen concentration in the buffer layer and the optical output in an experimental example. [Diagram 3] FIG. 13 is a diagram showing the relationship between the ratio of the average oxygen concentration in the buffer layer to the average oxygen concentration in the substrate and the optical output in an experimental example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Embodiment Mode] An embodiment of the present invention will be described with reference to Fig. 1. Note that the embodiment described below is shown as a preferred specific example for carrying out the present invention, and while there are some parts that specifically exemplify various technical matters that are technically preferable, the technical scope of the present invention is not limited to this specific embodiment.
[0010] (Nitride semiconductor light emitting device 1) FIG. 1 is a schematic diagram showing the configuration of a nitride semiconductor light-emitting element 1. In FIG. 1, the dimensional ratio of the stacking direction of each semiconductor layer of the nitride semiconductor light-emitting element 1 (hereinafter also simply referred to as "light-emitting element 1") does not necessarily match the actual one. Hereinafter, the stacking direction of each semiconductor layer of the light-emitting element 1 is referred to as the up-down direction. Also, one side in the up-down direction, that is, the side on which each semiconductor layer of the substrate 2 is grown (e.g., the upper side in FIG. 1) is referred to as the upper side, and the opposite side (e.g., the lower side in FIG. 1) is referred to as the lower side. Note that the expressions up and down are for convenience, and do not limit the attitude of the light-emitting element 1 with respect to the vertical direction, for example, when the light-emitting element 1 is used.
[0011] The light-emitting element 1 constitutes, for example, a light-emitting diode (LED) or a semiconductor laser (LD: Laser Diode). In this embodiment, the light-emitting element 1 constitutes a light-emitting diode that emits light with a wavelength in the ultraviolet region. In particular, the light-emitting element 1 in this embodiment emits ultraviolet light with a central wavelength of 240 nm or more and 365 nm or less. The light-emitting element 1 can be used in the fields of, for example, sterilization (e.g., air purification, water purification, etc.), medicine (e.g., phototherapy, measurement and analysis, etc.), UV curing, etc.
[0012] The light-emitting element 1 includes a buffer layer 3, an n-type semiconductor layer 4, a compositionally graded layer 5, an active layer 6, an electron blocking layer 7, and a p-type semiconductor layer 8, which are arranged in this order on a substrate 2. The light-emitting element 1 also includes an n-side electrode 11 provided on the n-type semiconductor layer 4, and a p-side electrode 12 provided on the p-type semiconductor layer 8.
[0013] The semiconductor constituting the light emitting element 1 is, for example, Al. a Ga b In 1-a-b In this embodiment, the semiconductor constituting the light emitting element 1 can be Al. c Ga 1-cThe semiconductor material uses a binary or ternary group III nitride semiconductor represented by N (0≦c≦1). Some of these group III elements may be replaced with boron (B), thallium (Tl), etc. Also, some of the nitrogen may be replaced with phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), etc.
[0014] The substrate 2 is made of a material that transmits the light emitted by the active layer 6. In this embodiment, the substrate 2 is a sapphire (Al2O3) substrate. The growth plane 21 formed on the upper surface of the substrate 2 is a c-plane. This c-plane may have an off-angle. The off-angle of the substrate 2 is preferably 0.6° or more. If the off-angle of the substrate 2 is smaller than 0.6°, the terrace width of the step-terrace structure formed on the upper surface of the substrate 2 becomes wider, and hillocks are more likely to be formed on the upper surface of the buffer layer 3, which makes it easier for oxygen to be taken into the buffer layer 3. The off-angle of the substrate 2 is more preferably 0.9° or more and 1.1° or less. In addition, for example, an aluminum nitride (AlN) substrate or an aluminum gallium nitride (AlGaN) substrate may be used as the substrate 2.
[0015] The buffer layer 3 is formed on the substrate 2. In this embodiment, the buffer layer 3 is made up of, in order from the substrate 2 side, an AlN layer 31 made of undoped aluminum nitride, and an undoped Al p Ga 1-pThe buffer layer 3 is made of two layers, an AlGaN layer 31 and an AlGaN layer 32 formed of N (0≦p≦1). An undoped semiconductor layer means a semiconductor layer to which no impurities are intentionally added when the semiconductor layer is formed, and a semiconductor layer containing a trace amount of impurities that is inevitably included is also considered to be an undoped semiconductor layer. The total thickness of the buffer layer 3 is greater than 500 nm. This makes it easy to alleviate the lattice mismatch between the substrate 2 and the semiconductor layer formed on the buffer layer 3, and improves the crystallinity of the semiconductor layer formed on the buffer layer 3. From the viewpoint of suppressing the occurrence of cracks in the buffer layer 3, the total thickness of the buffer layer 3 is preferably 5 μm or less. The thickness of the AlN layer 31 is greater than the thickness of the AlGaN layer 32. For example, the thickness of the AlN layer 31 is 380 nm or more and 2200 nm or less, and the thickness of the AlGaN layer 32 is 80 nm or more and 120 nm or less. The Al composition ratio p of the AlGaN layer 32 is, for example, 45% or more and 65% or less. By interposing the AlGaN layer 32 between the AlN layer 31 and the n-type semiconductor layer 4, the difference in Al composition ratio between the buffer layer 3 and the n-type semiconductor layer 4 is reduced, and the propagation of dislocations to the n-type semiconductor layer 4 is suppressed, resulting in improved conductivity of the n-type semiconductor layer 4.
[0016] In a light-emitting device 1 that emits ultraviolet light with a central wavelength of 365 nm or less, if the average concentration of oxygen that is inevitably contained as an impurity in the buffer layer 3 is high, the ultraviolet light emitted from the active layer 6 is absorbed by the oxygen in the buffer layer 3, resulting in a decrease in the optical output of the light-emitting device 1. Therefore, in the light-emitting device 1 of this embodiment, the average oxygen concentration in the buffer layer 3 is set to 4.5×10 21 atoms / cm 3 Hereinafter, the average oxygen concentration of the buffer layer 3 means the average oxygen concentration at each position in the vertical direction of the buffer layer 3. The average oxygen concentration of the buffer layer 3 is 1.0×10 21 atoms / cm 3 Less than or equal to 3.5×10 is preferred 20 atoms / cm 3 Less than 3.0×10 is more preferable. 20 atoms / cm 3The following is even more preferable: The oxygen concentration of the buffer layer 3 can be adjusted by, for example, devising manufacturing conditions as described later.
[0017] Here, the sapphire substrate as the substrate 2 contains oxygen as a constituent element, and the average oxygen concentration of the buffer layer 3 is preferably smaller than the average oxygen concentration of the sapphire substrate. The ratio of the average oxygen concentration of the buffer layer 3 to the average oxygen concentration of the substrate 2 is preferably 3 / 20 or less, more preferably 13 / 100 or less, even more preferably 13 / 1000 or less, and further preferably 1 / 100 or less.
[0018] The buffer layer 3 may be a single layer or may be three or more layers. When the substrate 2 is an aluminum nitride substrate or an aluminum gallium nitride substrate, the buffer layer 3 may be composed of, for example, an AlGaN layer 32 only.
[0019] The n-type semiconductor layer 4 is formed on the buffer layer 3. The n-type semiconductor layer 4 is, for example, Al doped with n-type impurities. q Ga 1-q N (0≦q≦1). In this embodiment, silicon (Si) is used as the n-type impurity. The same applies to semiconductor layers containing n-type impurities other than the n-type semiconductor layer 4. Note that germanium (Ge), selenium (Se), tellurium (Te), etc. may also be used as the n-type impurity. The Al composition ratio q of the n-type semiconductor layer 4 is, for example, 45% or more and 65% or less. The n-type semiconductor layer 4 may have a single-layer structure or a multi-layer structure.
[0020] The compositionally graded layer 5 is formed on the n-type semiconductor layer 4. The compositionally graded layer 5 is made of Al r Ga 1-r N (0≦r≦1). The Al composition ratio at each position in the vertical direction of the composition gradient layer 5 increases toward the upper side. Note that the composition gradient layer 5 may include a region in which the Al composition ratio does not increase toward the upper side, for example, in a very small region in the vertical direction (for example, a region of 5% or less of the entire vertical direction of the composition gradient layer 5).
[0021] The compositional gradient layer 5 preferably has an Al composition ratio at its lower end that is substantially the same as (for example, within a 5% difference) the Al composition ratio at the upper end of the n-type semiconductor layer 4 adjacent to the lower side of the compositional gradient layer 5. Further, the compositional gradient layer 5 preferably has an Al composition ratio at its upper end that is substantially the same as (for example, within a 5% difference) the Al composition ratio at the lower end of the barrier layer 61 adjacent to the upper side of the compositional gradient layer 5.
[0022] The active layer 6 is formed on the compositional gradient layer 5. The active layer 6 in this embodiment has a multiple quantum well structure having a plurality of well layers 621, 622. The bandgap of the active layer 6 is adjusted so that it can emit ultraviolet light with a central wavelength of 240 nm or more and 365 nm or less. When the active layer 6 has a multiple quantum well structure as in this embodiment, from the viewpoint of improving the light output, the central wavelength of the ultraviolet light emitted by the active layer 6 is preferably 250 nm or more and 320 nm or less, and more preferably 260 nm or more and 290 nm or less. In this embodiment, the active layer 6 has three barrier layers 61 and three well layers 621, 622, and the barrier layers 61 and the well layers 621, 622 are alternately laminated. In the active layer 6, a barrier layer 61 is located at the lower end, and a well layer 622 is located at the upper end.
[0023] Each barrier layer 61 is formed of Al s Ga 1-s N (0 < s ≤ 1). The Al composition ratio s of each barrier layer 61 is, for example, 75% or more and 95% or less. Also, the film thickness of each barrier layer 61 is, for example, 2 nm or more and 50 nm or less.
[0024] The well layers 621, 622 are formed of Al t Ga 1-t N (0 < t < 1). The Al composition ratio t of each well layer 621, 622 is smaller than the Al composition ratio s of the barrier layer 61 (that is, t < s).
[0025] The three well layers 621, 622 have different configurations between the bottom well layer 621, which is the well layer disposed at the bottom, and the upper well layer 622, which is the two well layers other than the bottom well layer 621. For example, the film thickness of the bottom well layer 621 is 1 nm or more larger than the film thickness of each of the two upper well layers 622, and the Al composition ratio of the bottom well layer 621 is 2% or more larger than the Al composition ratio of each of the two upper well layers 622. In this embodiment, the upper well layer 622 has a film thickness of 2 nm to 4 nm and an Al composition ratio of 25% to 45%, and the bottom well layer 621 has a film thickness of 4 nm to 6 nm and an Al composition ratio of 35% to 55%. The difference in film thickness between the bottom well layer 621 and each upper well layer 622 can be 2 nm to 4 nm.
[0026] By making the Al composition ratio of the bottom well layer 621 larger than that of the upper well layer 622, the crystallinity of the bottom well layer 621 is improved. This is because the difference in the Al composition ratio between the bottom well layer 621 and the n-type semiconductor layer 4 is reduced. By improving the crystallinity of the bottom well layer 621, the crystallinity of each semiconductor layer of the active layer 6 formed above the bottom well layer 621 is also improved. This improves the mobility of carriers in the active layer 6 and improves the optical output. This effect becomes more pronounced as the film thickness of the bottom well layer 621 increases, but from the viewpoint of suppressing an increase in the electrical resistance value of the entire light-emitting element 1, the film thickness of the bottom well layer 621 is designed to be equal to or less than a predetermined value.
[0027] In this embodiment, the active layer 6 has a multiple quantum well structure with three well layers 621, 622, but is not limited thereto and may have a multiple quantum well structure with two or four or more well layers 621, 622. Moreover, the active layer 6 may have a single quantum well structure with only one well layer 621, 622.
[0028] The electron blocking layer 7 is formed on the active layer 6. The electron blocking layer 7 serves to improve the electron injection efficiency into the active layer 6 by suppressing the occurrence of an overflow phenomenon in which electrons leak from the active layer 6 to the p-type semiconductor layer 8 side (hereinafter also referred to as the electron blocking effect). The electron blocking layer 7 has a stacked structure in which a first layer 71 and a second layer 72 are stacked in order from the bottom side.
[0029] The first layer 71 is provided on the active layer 6. The first layer 71 is made of, for example, Al u Ga 1-u N (0 ≤ u ≤ 1). The Al composition ratio u of the first layer 71 is, for example, 90% or more, and in this embodiment, it is made of aluminum nitride. The film thickness of the first layer 71 is, for example, 0.5 nm or more and 5.0 nm or less.
[0030] The second layer 72 is made of, for example, Al v Ga 1-v N (0 < v < 1). The Al composition ratio v of the second layer 72 is smaller than the Al composition ratio u of the first layer 71 (that is, u > v), and is, for example, 70% or more and 90% or less. The film thickness of the second layer 72 is larger than the film thickness of the first layer 71, and is, for example, 15 nm or more and 100 nm or less.
[0031] Since a semiconductor layer with a larger Al composition ratio has a larger electrical resistance value, if the film thickness of the first layer 71 with a relatively high Al composition ratio is made too large, it will cause an excessive increase in the overall electrical resistance value of the light-emitting element 1. Therefore, it is preferable to make the film thickness of the first layer 71 somewhat small. On the other hand, if the film thickness of the first layer 71 is made small, the probability that electrons tunnel through the first layer 71 from the bottom side to the top side can increase. Therefore, in the light-emitting element 1 of this embodiment, by forming the second layer 72 on the first layer 71, the electrons passing through the entire electron blocking layer 7 are suppressed.
[0032] Each of the first layer 71 and the second layer 72 can be an undoped layer, a layer containing n-type impurities, a layer containing p-type impurities, or a layer containing both n-type and p-type impurities. As the p-type impurity, magnesium (Mg) can be used, but in addition to magnesium, zinc (Zn), beryllium (Be), calcium (Ca), strontium (Sr), barium (Ba), carbon (C), or the like can also be used. The same applies to the semiconductor layer containing other p-type impurities. When each electron blocking layer 7 contains impurities, the impurities contained in each electron blocking layer 7 may be contained in the whole of each electron blocking layer 7 or may be contained in a part of each electron blocking layer 7.
[0033] The p-type semiconductor layer 8 is formed on the electron blocking layer 7. The p-type semiconductor layer 8 has a smaller Al composition ratio than the electron blocking layer 7 and is Al doped with p-type impurities w Ga 1-w formed by N (0 ≦ w ≦ 1). In this embodiment, the p-type semiconductor layer 8 has a stacked structure in which a first p-type clad layer 81, a second p-type clad layer 82, and a p-type contact layer 83 are stacked in this order from the bottom.
[0034] The first p-type clad layer 81 is provided so as to be in contact with the second layer 72. The first p-type clad layer 81 is composed of Al x Ga 1-x N (0 <x ≦ 1). The Al composition ratio x of the first p-type clad layer 81 is, for example, 45% or more and 65% or less. The film thickness of the first p-type clad layer 81 is, for example, 15 nm or more and 35 nm or less.
[0035] The second p-type clad layer 82 is composed of Al containing p-type impurities y Ga 1-y N (0 <y ≦ 1). The Al composition ratio at each position in the vertical direction of the second p-type clad layer 82 becomes smaller as the position is higher. Note that the second p-type clad layer 82 may include a region where the Al composition ratio does not become smaller as it goes upward in a very small region in the stacking direction (for example, a region of 5% or less of the whole of the second p-type clad layer 82 in the stacking direction).
[0036] It is preferable that the Al composition ratio of the lower end of the second p-type cladding layer 82 is substantially the same (for example, within a difference of 5%) as the Al composition ratio of the first p-type cladding layer 81, and that the Al composition ratio of the upper end of the second p-type cladding layer 82 is substantially the same (for example, within a difference of 5%) as the Al composition ratio of the p-type contact layer 83. The film thickness of the second p-type cladding layer 82 can be, for example, not less than 2 nm and not more than 4 nm.
[0037] The p-type contact layer 83 is a layer to which the p-side electrode 12 described later is connected, and is doped with a high concentration of p-type impurities. The p-type contact layer 83 is configured to have a low Al composition ratio (e.g., 10% or less) to achieve ohmic contact with the p-side electrode 12, and from this perspective is preferably formed of p-type gallium nitride (GaN). The thickness of the p-type contact layer 83 is, for example, 10 nm or more and 25 nm or less. The p-type semiconductor layer 8 may be a single layer or multiple layers.
[0038] The n-side electrode 11 is formed on an exposed surface 41 of the n-type semiconductor layer 4 that is exposed upward from the active layer 6. The n-side electrode 11 may be, for example, a multilayer film in which titanium (Ti), aluminum, titanium, and titanium nitride (TiN) are laminated in this order on the n-type semiconductor layer 4. In addition, when the light-emitting element 1 is flip-chip mounted as described later, the n-side electrode 11 may be made of a material capable of reflecting ultraviolet light emitted by the active layer 6.
[0039] The p-side electrode 12 is formed on the upper surface of the p-type semiconductor layer 8. The p-side electrode 12 may be made of, for example, rhodium (Rh). In this embodiment, the p-side electrode 12 is a reflective electrode having a reflectance of 50% or more, preferably 60% or more, at the central wavelength of light emitted by the active layer 6, but is not limited thereto.
[0040] The light emitting element 1 is flip-chip mounted on a package substrate (not shown) for use. That is, the side of the light emitting element 1 on which the n-side electrode 11 and the p-side electrode 12 are provided in the up-down direction faces the package substrate, and each of the n-side electrode 11 and the p-side electrode 12 is mounted on the package substrate via a connection member such as a gold bump. Light is extracted from the substrate 2 side (i.e., the lower side) of the flip-chip mounted light emitting element 1.
[0041] (Method of manufacturing the nitride semiconductor light emitting element 1) Next, an example of a method for manufacturing the light emitting device 1 of this embodiment will be described. In this embodiment, a buffer layer 3, an n-type semiconductor layer 4, a composition gradient layer 5, an active layer 6, an electron block layer 7, and a p-type semiconductor layer 8 are epitaxially grown in sequence on a disk-shaped substrate 2 by metal organic chemical vapor deposition (MOCVD). That is, in this embodiment, the disk-shaped substrate 2 is placed in a chamber, and the source gases of the semiconductor layers to be formed on the substrate 2 are introduced into the chamber to form the semiconductor layers on the substrate 2. As source gases for epitaxially growing the semiconductor layers, trimethylaluminum (TMA) as an aluminum source, trimethylgallium (TMG) as a gallium source, ammonia (NH3) as a nitrogen source, tetramethylsilane (TMSi) as a silicon source, and biscyclopentadienylmagnesium (Cp2Mg) as a magnesium source can be used.
[0042] The MOCVD method is sometimes called metal organic vapor phase epitaxy (MOVPE). From the viewpoint of forming a buffer layer 3 with a thickness of more than 500 nm on the substrate 2, it is preferable to use an epitaxial growth method such as the MOCVD method, the hydride vapor phase epitaxy (HVPE) method, or the physical vapor transport (PVT) method. In this embodiment, the buffer layer 3 is not grown by the sputtering method. It is difficult to form a buffer layer 3 with a thickness of more than 500 nm by the sputtering method. However, if the buffer layer 3 with a thickness of more than 500 nm can be formed by the sputtering method, the sputtering method may be used.
[0043] In the manufacturing method of the light-emitting element 1 of this embodiment, the manufacturing conditions are designed so that the oxygen concentration of the buffer layer 3 is low as described above. For example, before forming each semiconductor layer on the substrate 2, the chamber is evacuated so that the degree of vacuum in the chamber is relatively high, so that oxygen is less likely to be contained in the buffer layer 3 to be formed. In addition, depending on the material of the chamber wall facing the space inside the chamber, oxygen may be generated from the wall in a high temperature environment where the buffer layer is formed, so the material of the chamber wall may also affect the oxygen concentration of the buffer layer 3. As illustrated above, the oxygen concentration of the buffer layer 3 can be adjusted by appropriately designing the manufacturing conditions that may affect the oxygen concentration of the buffer layer 3.
[0044] After each semiconductor layer is formed on the disk-shaped substrate 2, a mask is formed on a portion of the p-type semiconductor layer 8, i.e., on a portion other than the portion that will become the exposed surface 41 of the n-type semiconductor layer 4. Then, the region where the mask is not formed is removed by etching from the top surface of the p-type semiconductor layer 8 to the middle of the n-type semiconductor layer 4 in the vertical direction. As a result, the exposed surface 41 that is exposed toward the upper side is formed in the n-type semiconductor layer 4. After the exposed surface 41 is formed, the mask is removed.
[0045] Next, an n-side electrode 11 is formed on the exposed surface 41 of the n-type semiconductor layer 4, and a p-side electrode 12 is formed on the p-type semiconductor layer 8. The n-side electrode 11 and the p-side electrode 12 may be formed by a well-known method such as an electron beam deposition method or a sputtering method. The above-completed product is cut into pieces of desired dimensions, and a plurality of light-emitting elements 1 as shown in FIG. 1 are manufactured from one wafer.
[0046] (Functions and Effects of the Embodiments) In the light-emitting device 1 of this embodiment, the active layer 6 emits ultraviolet light with a central wavelength of 365 nm or less, and the thickness of the buffer layer 3 is greater than 500 nm. In this configuration, the relatively large thickness of the buffer layer 3 tends to reduce the lattice mismatch between the substrate 2 and the n-type semiconductor layer 4, but the problem of a decrease in the optical output of the light-emitting device 1 due to the absorption of ultraviolet light by oxygen contained in the buffer layer 3 tends to become prominent. Therefore, in this embodiment, the average oxygen concentration of the buffer layer 3 is set to 4.5×10 21 atoms / cm 3 As a result, the light output of the light-emitting element 1 can be improved. This value is supported by experimental examples described later. In addition, since the growth surface 21 of the substrate 2 is a c-plane, the oxygen concentration of the buffer layer 3 formed on the substrate 2 is reduced compared to when the growth surface 21 is an r-plane or the like.
[0047] The average oxygen concentration of the buffer layer 3 is 1.0×10 21 atoms / cm 3 The following conditions are further satisfied. This makes it possible to further improve the light output of the light-emitting element 1.
[0048] Furthermore, the substrate 2 is a sapphire substrate, and the average oxygen concentration of the buffer layer 3 is smaller than the average oxygen concentration of the substrate 2. In this way, by making the average oxygen concentration of the buffer layer 3 smaller than the average oxygen concentration of the sapphire substrate containing oxygen as a constituent element, the light output of the light-emitting element 1 can be further improved.
[0049] Moreover, the ratio of the average oxygen concentration in the buffer layer 3 to the average oxygen concentration in the substrate 2 satisfies 3 / 20 or less. This makes it possible to further improve the light output of the light-emitting element 1.
[0050] The ratio of the average oxygen concentration in the buffer layer 3 to the average oxygen concentration in the substrate 2 further satisfies 13 / 100 or less. This makes it possible to further improve the light output of the light-emitting element 1.
[0051] As described above, according to this embodiment, it is possible to provide a nitride semiconductor light emitting device capable of improving the optical output.
[0052] [Experimental Example] This experimental example is an example of evaluating the relationship between the average oxygen concentration in the buffer layer and the optical output of the wafer. Note that, among the names of components used in this experimental example, those that are the same as those used in the above embodiment represent the same components as those in the above embodiment unless otherwise specified.
[0053] First, wafers relating to Samples 1 to 4 will be described with reference to Table 1. Samples 1 to 4 are wafers having the same basic configuration as the light-emitting device in the embodiment, unless otherwise specified below.
[0054] [Table 1]
[0055] As shown in Table 1, the average oxygen concentration of the buffer layer and the thickness of the AlN layer of the buffer layer are changed between samples 1 to 4. The average oxygen concentration of the substrates of samples 1 to 4 differs slightly from each other, but this is not intentional and is within the range of individual differences.
[0056] In Table 1, the configurations common to Samples 1 to 4 are shown without distinguishing between Samples 1 to 4, and the thickness of the AlN layer, the average oxygen concentration of the substrate, and the average oxygen concentration of the AlN layer are shown for each of Samples 1 to 4. The Al composition ratio of each layer listed in Table 1 is a value estimated from the secondary ion intensity of Al measured by secondary ion mass spectrometry (SIMS). The column for composition gradient layer in Table 1 indicates that the Al composition ratio at each position in the vertical direction of the composition gradient layer gradually increases from 55% to 85% from the bottom to the top of the composition gradient layer. The column for second p-type cladding layer in Table 1 indicates that the Al composition ratio at each position in the vertical direction of the second p-type cladding layer gradually decreases from 55% to 0% from the bottom to the top of the second p-type cladding layer.
[0057] The average oxygen concentration of each layer listed in Table 1 was calculated from the measured value by SIMS. The oxygen concentration of the substrate and AlN layer in each sample was measured using a wafer grown up to the AlN layer under the same manufacturing conditions as those for manufacturing each sample. The measured oxygen concentration of each layer of the wafer by SIMS was the result of measuring the wafer from the top side. It should be noted that the AlGaN layer constituting the buffer layer has a small film thickness, making it difficult to measure the oxygen concentration accurately, but it is expected to be the same as the oxygen concentration of the AlN layer. As mentioned above, the oxygen concentration of the buffer layer may vary depending on the manufacturing environment (i.e., the temperature in the chamber, the material of the wall of the chamber, etc.), but in this experimental example, the AlN layer and AlGaN layer of each sample were manufactured in the same manufacturing environment, and the oxygen concentration of the AlN layer and the oxygen concentration of the AlGaN layer were considered to be the same. In other words, in this experimental example, the oxygen concentration of the AlN layer listed in Table 1 was considered to be the oxygen concentration of the entire buffer layer.
[0058] A current of 20 mA was then applied to each of Samples 1 to 4 while they were on the wafer, and the optical output was measured. The optical output of each sample was measured by a photodetector installed below each sample (i.e., on the substrate side). The results are shown in Figure 2. Figure 2 is a graph showing the relationship between the average oxygen concentration in the buffer layer and the optical output.
[0059] As can be seen from Fig. 2, when the average oxygen concentration in the buffer layer increases, the average oxygen concentration in the buffer layer increases by 4.5 × 10 21 atoms / cm 3 The light output gradually decreases until the average oxygen concentration reaches 4.5×10 21 atoms / cm 3 Therefore, the average oxygen concentration in the buffer layer is 4.5×10 21 atoms / cm 3 As can be seen from FIG. 2, from the viewpoint of improving the optical output, the average oxygen concentration of the buffer layer is preferably 1.0×10 21 atoms / cm 3 Less than or equal to 3.5×10 is preferred 20 atoms / cm 3 Less than 3.0×10 is more preferable. 20 atoms / cm 3 The following is even more preferred:
[0060] The results of Fig. 2 will be examined from a different perspective using Table 2 and Fig. 3. Table 2 shows the results of the average oxygen concentration of the substrate, the average oxygen concentration of the buffer layer, the ratio of the average oxygen concentration of the buffer layer to the average oxygen concentration of the substrate (hereinafter referred to as the "oxygen concentration ratio"), and the light output for each sample. Fig. 3 is a graph showing the relationship between the oxygen concentration ratio and the light output.
[0061] [Table 2]
[0062] As can be seen from Table 2 and FIG. 3, the oxygen concentration ratio is preferably 0.150 or less (i.e., 3 / 20 or less), more preferably 0.130 or less (i.e., 13 / 100 or less), even more preferably 0.013 or less (i.e., 13 / 1000 or less), and even more preferably 0.010 or less (i.e., 1 / 100 or less).
[0063] (Summary of the embodiment) Next, the technical ideas grasped from the above-described embodiment will be described by using the reference numerals and the like in the embodiment. However, the reference numerals and the like in the following description do not limit the components in the claims to the members and the like specifically shown in the embodiment.
[0064] [1] A first embodiment of the present invention comprises a substrate 2 having a growth surface 21 that is a c-plane, a buffer layer 3 formed on the growth surface 21, an n-type semiconductor layer 4 formed on the buffer layer 3, an active layer 6 formed on the n-type semiconductor layer 4 and emitting ultraviolet light having a central wavelength of 365 nm or less, and a p-type semiconductor layer 8 formed on the active layer 6, wherein the thickness of the buffer layer 3 is greater than 500 nm, and the average oxygen concentration of the buffer layer 3 is 4.5×10 21 atoms / cm 3 The nitride semiconductor light-emitting device 1 satisfies the following: This makes it possible to improve the optical output of the nitride semiconductor light emitting element 1.
[0065] [2] The second embodiment of the present invention is the first embodiment, wherein the average oxygen concentration of the buffer layer 3 is 1.0×10 21 atoms / cm 3 The following further conditions must be met: This makes it possible to further improve the optical output of the nitride semiconductor light emitting device 1.
[0066] [3] A third embodiment of the present invention is the first or second embodiment, in which the substrate 2 is a sapphire substrate, and the average oxygen concentration of the buffer layer 3 is smaller than the average oxygen concentration of the substrate 2. This makes it possible to further improve the optical output of the nitride semiconductor light emitting device 1.
[0067] [4] A fourth embodiment of the present invention is the third embodiment, in which the ratio of the average oxygen concentration of the buffer layer 3 to the average oxygen concentration of the substrate 2 satisfies 3 / 20 or less. This makes it possible to further improve the optical output of the nitride semiconductor light emitting device 1.
[0068] [5] A fifth embodiment of the present invention is the fourth embodiment, further characterized in that the ratio of the average oxygen concentration of the buffer layer 3 to the average oxygen concentration of the substrate 2 is 13 / 100 or less. This makes it possible to further improve the optical output of the nitride semiconductor light emitting device 1.
[0069] (Additional Note) Although the embodiment of the present invention has been described above, the invention according to the claims is not limited to the above embodiment. It should be noted that not all of the combinations of features described in the embodiment are essential to the means for solving the problems of the invention. The present invention can be modified appropriately without departing from the spirit of the invention. [Explanation of symbols]
[0070] 1...Nitride semiconductor light emitting device 2...Substrate 21…Growth aspect 3…Buffer layer 4...n-type semiconductor layer 6…Active layer 8...p-type semiconductor layer
Claims
1. a sapphire substrate having a c-plane as a growth surface; a buffer layer formed on the growth surface; an n-type semiconductor layer formed on the buffer layer; an active layer formed on the n-type semiconductor layer and emitting ultraviolet light having a central wavelength of 365 nm or less; a p-type semiconductor layer formed on the active layer, The thickness of the buffer layer is greater than 500 nm; The average oxygen concentration of the buffer layer is 4.5×10 21 atoms / cm 3 Satisfy the following: a ratio of an average oxygen concentration of the buffer layer to an average oxygen concentration of the sapphire substrate is 3 / 20 or less; Nitride semiconductor light emitting element.
2. The average oxygen concentration of the buffer layer is 1.0×10 21 atoms / cm 3 Additionally, The nitride semiconductor light emitting device according to claim 1 .
3. a ratio of an average value of the oxygen concentration of the buffer layer to an average value of the oxygen concentration of the sapphire substrate further satisfies 13 / 100 or less; The nitride semiconductor light emitting device according to claim 1 .
4. a ratio of an average oxygen concentration of the buffer layer to an average oxygen concentration of the sapphire substrate is further satisfied to be 1 / 100 or less; The nitride semiconductor light emitting device according to claim 3 .
5. The buffer layer has an AlN layer formed of undoped aluminum nitride and an AlGaN layer formed on the AlN layer formed of undoped Al p Ga 1-p N (0≦p≦1). The nitride semiconductor light emitting device according to claim 1 .
Citation Information
Patent Citations
Group iii nitride semiconductor light-emitting device, method for manufacturing thereof, and lamp
JP2009081406A
Nitride semiconductor crystal thin film and its deposition method, semiconductor device, and its fabrication process
JP2009231302A
Nitride semiconductor light emitting device
JP2010258096A
Substrate for growing semiconductor, semiconductor device, semiconductor light-emitting device and manufacturing method of substrate for growing semiconductor
JP2020070221A
SUBSTRATE HAVING CONDUCTIVE AlN EPITAXIAL FILM AND METHOD FOR MANUFACTURING THE SAME
JP2022084473A