Manufacturing method of polytetrafluoroethylene resin tube

The described method addresses the challenge of producing thin-walled PTFE resin tubes with high strength and yield by combining extrusion molding with PTFE dispersion application and firings, resulting in pinhole-free tubes with enhanced structural integrity.

JP7555561B2Active Publication Date: 2024-09-25CHUKOH CHEM IND LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020088944
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-21
Publication Date
2024-09-25
Estimated Expiration
2040-05-21

AI Technical Summary

Technical Problem

Existing methods for manufacturing polytetrafluoroethylene (PTFE) resin tubes struggle to produce thin-walled tubes with high strength and yield, as they often result in pinholes or require excessive thermal deterioration.

Method used

A method involving extrusion molding of PTFE fine powder followed by first and second firings, with an intermediate application of PTFE dispersion to the outer surface of the first tubular precursor to form a two-layer structure, thereby avoiding stretching and minimizing pinholes.

Benefits of technology

This method enables the high-yield production of thin-walled PTFE resin tubes with improved strength and integrity by eliminating pinholes through the use of PTFE dispersion to fill and reinforce the extruded product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555561000003
    Figure 0007555561000003
  • Figure 0007555561000004
    Figure 0007555561000004
  • Figure 0007555561000005
    Figure 0007555561000005
Patent Text Reader

Abstract

To provide a high-yield method for manufacturing a thin-wall polytetrafluoroethylene resin tube.SOLUTION: A method for manufacturing polytetrafluoroethylene resin tube including: extrusion-molding a mixture including polytetrafluoroethylene fine powder to obtain a tube-shaped extrusion-molded article; performing first burning to the extrusion-molded article to obtain a first tube-shaped precursor; applying polytetrafluoroethylne dispersion to the external surface of the first tube-shaped precursor to obtain a second tube-shaped precursor; and performing second burning to the second tube-shaped precursor.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polytetrafluoroethylene resin tube. [Background technology]

[0002] Polytetrafluoroethylene (PTFE) resin tubes are used in a wide range of fields due to their excellent lubricity, chemical resistance, and heat resistance. As devices in which tubes are used become smaller, there is a growing demand for smaller outer diameters and larger inner diameters at the same time. Such demands can be met, for example, by making the tubes thinner.

[0003] Among the methods for manufacturing PTFE resin tubes, the dip coating-baking method, which uses a PTFE resin dispersion, is suitable for manufacturing thin-walled tubes, but the tubes obtained by this method tend to lack strength.

[0004] On the other hand, although the tubes obtained by extrusion molding can be expected to have high strength, it is difficult to manufacture thin-walled tubes by extrusion molding. For example, when a thin-walled tube is manufactured by extruding a resin paste, the resulting tube is prone to pinholes.

[0005] Patent Document 1 (JP Patent Publication 2006-205680A) describes adjusting the wall thickness to a moderately high value in order to improve the strength of a PTFE resin tube obtained by a dip coating-sintering method. Although the wall thickness can be adjusted by simply repeating coating and sintering alternately, there is a problem that repeated sintering will cause excessive thermal deterioration of the resin. As a means for solving this problem, Patent Document 1 employs a method for obtaining a PTFE thin-walled tube adjusted to a desired wall thickness while reducing the number of times of overcoating. Specifically, a sintered layer of pure PTFE resin dispersion is formed as the inner layer, and a sintered layer of PTFE resin dispersion containing a thickener is formed as the outer layer. The coating thickness of the dispersion on the outer periphery of the inner layer can be adjusted by adjusting the amount of thickener added to the dispersion used to form the outer layer. By increasing the thickness of one coating, the number of times of overcoating can be reduced.

[0006] Patent Document 2 (International Publication WO2008 / 102878) describes a method for producing a PTFE molded article by extrusion molding, in which a PTFE powder, which is a primary particle rather than a secondary particle, is used in a dispersion liquid to obtain a molded article having a thickness of 50 μm or less.

[0007] Patent Document 3 (JP Patent Publication 10-337405A) describes a method for producing a fluororesin tube in which a porous structure layer and a non-porous structure layer are integrated in the thickness direction, in which a fluororesin tube is stretched in at least one axial direction to form an orientation, an aqueous suspension of a fluororesin is applied to the outer surface or inner surface of the tube, and the tube is fired while fixed in the stretching axial direction. The tube obtained by extruding a mixture of a fluororesin material powder and a liquid lubricant into a tube and then removing the liquid lubricant by heating is stretched in at least one axial direction to make it porous. The suspension applied to one surface is fired to form a non-porous layer. Since the porous structure layer and the non-porous structure layer are integrated in the thickness direction, when used as a membrane material in a device for vacuum degassing medicines, etc., it exhibits excellent degassing efficiency and prevents the treatment liquid from penetrating the tube. It is expected that the tube will need to have a certain wall thickness, for example, a wall thickness of 0.1 mm or more, to function as a membrane material for degassing.

[0008] Patent Document 4 (JP Patent Publication No. 2007-237597) describes that by using a PTFE resin with an absorbed dose of ionizing radiation of 200 to 4000 Gy, a thin PTFE tube with a wall thickness of 7 to 50 μm can be obtained. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2006-205680 A [Patent Document 2] International Publication WO2008 / 102878 [Patent Document 3] Japanese Patent Application Publication No. 10-337405 [Patent Document 4] JP 2007-237597 A Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a method for producing a thin-walled polytetrafluoroethylene resin tube with high yield. [Means for solving the problem]

[0011] A method for producing a polytetrafluoroethylene resin tube includes extruding a mixture containing polytetrafluoroethylene fine powder to obtain a tubular extrusion product, and performing a first firing process on the extrusion product without performing a stretching process to obtain a first tubular precursor. After the first firing, without any further processing, The method includes applying a polytetrafluoroethylene dispersion to an outer surface of the first tubular precursor to obtain a second tubular precursor, and subjecting the second tubular precursor to a second firing. Effect of the Invention

[0012] According to the above-mentioned manufacturing method, a thin-walled polytetrafluoroethylene resin tube can be manufactured with a high yield. [Brief description of the drawings]

[0013] [Figure 1] FIG. 4 is a cross-sectional view that illustrates an example of a method for manufacturing a fluororesin tube. [Diagram 2] FIG. 2 is a perspective view showing an example of a PTFE resin tube. [Diagram 3] FIG. 3 is a cross-sectional view taken along imaginary plane III-III′ shown in FIG. 2 . [Figure 4] FIG. 4 is a cross-sectional view taken along imaginary plane IV-IV′ shown in FIG. 2 . [Diagram 5] FIG. 2 is a schematic cross-sectional view of an example of a first tubular precursor. [Figure 6] FIG. 1 is a schematic cross-sectional view of an example extruder. [Figure 7] FIG. 4 is a schematic cross-sectional view of another example of an extruder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A method for producing a polytetrafluoroethylene resin tube according to an embodiment of the invention includes extruding a mixture containing polytetrafluoroethylene fine powder to obtain a tubular extrusion product, subjecting the extrusion product to a first firing to obtain a first tubular precursor, applying a polytetrafluoroethylene dispersion to an outer surface of the first tubular precursor to obtain a second tubular precursor, and subjecting the second tubular precursor to a second firing.

[0015] Thin-walled tubes obtained by extruding a material containing tetrafluoroethylene resin, i.e., polytetrafluoroethylene (PTFE) resin, into a thin-walled tube and then baking the resulting extrusion are prone to pinholes. Pinholes can be filled by applying a PTFE dispersion to the outer surface of the tube and then baking it. It is preferable to apply the dispersion to the side surface along the length of the tube. This allows high-yield production of thin-walled tubes.

[0016] That is, a mixture containing a first polytetrafluoroethylene powder (first PTFE powder) is extruded to obtain a tubular extrusion product, the extrusion product is subjected to a first firing to obtain a first tubular precursor, a dispersion liquid containing a second polytetrafluoroethylene powder (second PTFE powder) is applied to the outer surface of the first tubular precursor to obtain a second tubular precursor, and the second tubular precursor is subjected to a second firing, thereby producing a thin-walled pinholeless tube with a high yield.

[0017] As the PTFE fine powder, materials commonly used for extrusion molding of PTFE molded products can be used. Fine powder is obtained by coagulating and drying an aqueous dispersion obtained by emulsion polymerization. For example, the fine powder may be mainly composed of primary particles generated by polymerization that have aggregated to form secondary particles with a particle size of about 100 μm.

[0018] The PTFE fine powder is preferably a powder of only PTFE, without including any fillers or additives, etc. In other words, the PTFE fine powder is preferably made of PTFE. The PTFE fine powder is preferably a virgin PTFE powder.

[0019] The PTFE fine powder may be irradiated with ionizing radiation at an absorbed dose of 200 Gy or more and 4000 Gy or less. By irradiating the above amount of ionizing radiation, the pressure during extrusion molding can be reduced. An absorbed dose of 200 Gy or more can reduce the extrusion pressure. If the absorbed dose is 4000 Gy or less, the mechanical strength of the extrusion molded product will not decrease. Ionizing radiation includes electromagnetic waves such as X-rays and gamma rays, charged particles such as beta rays, positrons, electrons, alpha rays, protons, deuterons, heavy ions, mesons, and other uncharged elementary particles, either alone or in combination.

[0020] For example, a paste-like mixture can be obtained by mixing an extrusion aid such as a lubricant with PTFE fine powder. A tubular extrusion molded product can be obtained by extruding the mixture containing the PTFE fine powder into a tube shape. A PTFE molded product having a single-layer tube shape, i.e., a first tubular precursor, can be obtained by baking the extrusion molded product (first baking).

[0021] Examples of extrusion aids include the commonly used solvent naphtha (e.g., registered trademark: Isoper E, manufactured by Exxon Chemical Co.), white oil, and liquid paraffin having 6 to 12 carbon atoms (e.g., registered trademark: Cactus Normal Paraffin N-10, manufactured by Japan Energy Corporation).

[0022] The mixture obtained by mixing the PTFE fine powder and the extrusion aid may be aged before being subjected to extrusion molding. The aged mixture may be compressed to produce a compression molded body (billet). By compressing, air in the PTFE fine powder can be removed, and the uniformity of the extrusion molded product can be improved. The shape of the compression molded body is not particularly limited, but may be, for example, a cylindrical shape. The compression molded body is placed in an extruder and extrusion molding is performed.

[0023] It is desirable to carry out the extrusion molding under conditions that result in a wall thickness of 20 μm or less of the extrusion molding obtained. It is more preferable to carry out the extrusion molding under conditions that result in a wall thickness of 15 μm or less, and even more preferable to carry out the extrusion molding under conditions that result in a wall thickness of 10 μm or less. The thinner the wall thickness, the more likely pinholes tend to occur, but the pinholes can be filled by applying a PTFE dispersion in a later step.

[0024] During extrusion molding, heating may be performed. For example, extrusion molding may be performed while heating by setting the temperature of the mold (e.g., die or die) of the extruder to 40° C. or higher and 95° C. or higher. It is preferable to heat the mold to 50° C. or higher and 60° C. or lower.

[0025] The baking temperature in the baking (first baking) of the extrusion molded product is not particularly limited. It is preferable to bake at a temperature exceeding the melting point of PTFE, 390° C., for example, at a temperature of 400° C. or higher.

[0026] It is preferable to crystallize the PTFE resin by drying the extrusion molded product prior to sintering. Although drying can remove the auxiliary agent, typical extrusion auxiliary agents volatilize at about 200°C, and therefore will volatilize during sintering even if they are not removed in advance.

[0027] A core wire may be used in the extrusion molding. By performing extrusion molding so that the outer periphery of the core wire is covered with a mixture containing PTFE fine powder, a tubular extrusion molded product can be formed on the core wire. In addition, by subjecting the extrusion molded product on the core wire to firing (first firing) as it is, a first tubular precursor in a form in which the core wire is covered can be obtained. If the core wire is covered, it becomes easier to adopt a continuous coating method when applying the PTFE dispersion to the outer surface of the first tubular precursor.

[0028] The core wire may be, for example, a metal wire made of a metal such as copper or aluminum, or a core material made of resin. The diameter of the core wire may be appropriately changed depending on the desired inner diameter of the tube.

[0029] It is desirable to complete the first baking without performing any other treatment on the extrusion molded product obtained using PTFE fine powder. For example, if an unbaked extrusion molded product is stretched, the tube may tear from a pinhole or further pinholes may occur. In particular, if the tube is stretched in the radial direction to expand the tube diameter, the tube may tear along the longitudinal direction. In the tube obtained by extrusion molding, the resin is oriented along the extrusion direction. Even in a thin-walled tube, the strength in the longitudinal direction is ensured by the orientation, but the strength in the direction crossing it is weak. In the part with a pinhole, the orientation is irregular, and the tube is likely to tear by stretching in any direction. Therefore, it is desirable not to perform a stretching treatment on the extrusion molded product before the first baking. Even after the first baking, the above-mentioned problems may occur if the tube is stretched.

[0030] The PTFE dispersion contains a dispersion medium and PTFE powder in the dispersion medium. As the PTFE dispersion, a material that is generally used in a method for forming a resin tube by coating, such as a dip coating method, can be used. For example, the PTFE dispersion is an aqueous dispersion liquid in which PTFE powder is dispersed in an aqueous dispersion medium by emulsion polymerization. The PTFE dispersion can be a suspension containing PTFE powder.

[0031] The PTFE powder contained in the PTFE dispersion is preferably a powder of PTFE only, without any fillers or additives. That is, the PTFE dispersion is preferably one in which a powder made of PTFE is dispersed in a dispersion medium. The PTFE dispersion is preferably a dispersion of virgin PTFE.

[0032] The dispersion medium may be, for example, water, etc. The composition of the PTFE dispersion is not particularly limited, and for example, a dispersion liquid or suspension having a composition commonly used in techniques such as dip coating can be used.

[0033] The second tubular precursor is obtained by applying the PTFE dispersion to the outer surface of the first tubular precursor. It is preferable to apply the PTFE dispersion to the entire outer surface of the first tubular precursor. To apply the PTFE dispersion, for example, the first tubular precursor can be immersed in the PTFE dispersion. Specifically, it is preferable to adopt a dip coating method using the first tubular precursor formed on a core wire. In the dip coating method, a uniform coating thickness can be formed by passing the core wire together with the first tubular precursor through the PTFE dispersion and pulling it up at a constant speed.

[0034] The second tubular precursor obtained by applying the PTFE dispersion to the first tubular precursor is fired. In this way, a pinhole-less resin tube in which the pinholes are closed is obtained. In addition, a two-layered PTFE resin tube is obtained by firing the second tubular precursor obtained by applying the PTFE dispersion to the entire outer surface of the first tubular precursor.

[0035] After applying the PTFE dispersion once and then baking, the outer surface of the obtained tube may be further coated with the PTFE dispersion and then baked. By alternately repeating the application of the dispersion and the baking, the wall thickness of the tube can be adjusted to a desired thickness.

[0036] Alternatively, after applying and baking the PTFE dispersion, a filler-containing dispersion liquid containing a composite material containing PTFE powder and a filler may be applied and baked (third baking). As the filler, for example, an imide resin powder can be mixed with the PTFE powder. By forming an outer layer using a mixed powder of PTFE powder and imide resin powder, the abrasion resistance of the outer surface of the tube can be improved. In addition, by including a conductive material such as a carbon material as the filler, electrical properties can be imparted to the tube. However, the dispersion liquid directly applied to the outer surface of the first tubular precursor is a PTFE dispersion containing no filler.

[0037] After the first firing of the extrusion molded product obtained using the PTFE fine powder, it is preferable to apply the PTFE dispersion to the first tubular precursor without performing any other treatment. For example, if the first tubular precursor is stretched, the tube may tear from the pinhole as in the case of the extrusion molded product before firing, or further pinholes may occur. Therefore, it is preferable not to perform a stretching treatment on the first tubular precursor.

[0038] After the first firing, it is desirable to only cool the first tubular precursor to a temperature suitable for applying the PTFE dispersion, and then apply the PTFE dispersion to the first tubular precursor. For example, the extrusion molding is formed on the core wire during extrusion molding, and the same core wire is used throughout the process until the application of the PTFE dispersion is performed. The core wire on which the first tubular precursor after the first firing is formed is sent out as it is and immersed in the PTFE dispersion, so that the process from the first firing to the application of the dispersion liquid may be performed continuously. Alternatively, after the first firing, the first tubular precursor may be temporarily wound up on, for example, a winding roll. The roll on which the first tubular precursor is wound may be used as a supply roll to start applying the dispersion liquid again.

[0039] A specific example of a method for producing a fluororesin tube will be described with reference to the drawings. Fig. 1 is a cross-sectional view that shows a schematic example of a method for producing a fluororesin tube. In this example, a first tubular precursor is formed on a core wire by extrusion molding, and then the first tubular precursor is held on the same core wire and the PTFE dispersion is applied by dip coating.

[0040] An extrusion die 51 provided in an extrusion molding machine 50 is filled with an admixture 20 containing PTFE fine powder. The admixture 20 is a mixture of PTFE fine powder and other materials such as an extrusion aid. The admixture 20 may be, for example, a paste containing PTFE fine powder. Alternatively, the admixture 20 may be a compression molded body (billet) containing PTFE fine powder.

[0041] The core wire 4 is fed into the inside of the extrusion die 51. The core wire 4 passes through the inside of the extrusion die 51 and is drawn out from the discharge port 52 of the extrusion die 51 to the outside.

[0042] As the extrusion ram 53 is moved toward the discharge port 52, the mixture 20 is compressed and extruded from the discharge port 52 together with the core wire 4. In this manner, a tubular extrusion product 21 covering the outer periphery of the core wire 4 is obtained.

[0043] The inner tube diameter of the extrusion molded product 21 can be controlled by adjusting the wire diameter of the core wire 4. When the core wire 4 is not used, for example, a core pin can be placed in the extrusion die 51, and the inner tube diameter can be controlled by the diameter of the core pin. The outer diameter of the extrusion molded product 21 can be controlled by adjusting the aperture of the discharge port 52 of the extrusion die 51. In order to control the outer diameter, for example, a sizing die of appropriate dimensions may be used. The wall thickness of the extrusion molded product can be controlled by adjusting the wire diameter (or core pin diameter) of the core wire 4 and the aperture (or die dimensions) of the discharge port 52.

[0044] The extrusion molded product 21 on the core wire 4 is supplied to a drying furnace 61 and dried there (first drying). Drying the extrusion molded product 21 promotes crystallization of the PTFE resin. The extrusion molded product 21 is then supplied to a heating furnace 62 and subjected to a first baking there. By the first baking, a first tubular precursor 22 is obtained in a form in which the core wire 4 is covered.

[0045] The first tubular precursor 22 on the core wire 4 is supplied to the dispersion liquid 30 in the bath 71 via the cooling device 63. The dispersion liquid 30 is a PTFE dispersion. The cooling means by the cooling device 63 is not particularly limited and may include, for example, air cooling and water cooling. The cooling device 63 may be omitted, and instead, the arrangement and number of guide rollers 90 may be set so that the distance from the heating furnace 62 to the bath 71 is long, thereby increasing the heat dissipation time. In addition, the arrangement and number of guide rollers 90 are not limited to those shown in FIG. 1.

[0046] The first tubular precursor 22 (and the core wire 4 therein) is immersed in the dispersion liquid 30 and then pulled up. The dispersion liquid 30 is applied to the outer surface of the first tubular precursor 22 via the dip coating, and a second tubular precursor 10 including the first tubular precursor 22 and a dispersed PTFE coating 31 covering the outer periphery thereof is obtained. At this time, part of the dispersion liquid 30 fills the pinholes generated in the first tubular precursor 22.

[0047] The second tubular precursor 10, which includes the first tubular precursor 22 covering the outer periphery of the core wire 4 and the dispersed PTFE coating 31 further covering the outer periphery of the first tubular precursor 22, is successively fed to a drying furnace 81 and a heating furnace 82, and is subjected to drying (second drying) and second baking. Through the second baking, a two-layered PTFE resin tube 1 including an inner layer 2 and an outer layer 3 is obtained. The inner layer 2 corresponds to the first tubular precursor 22 that is reheated by the second baking.

[0048] The PTFE resin tube 1 on the core wire 4 is supplied to a take-up roll 91 via a cooling device 83. The means of cooling by the cooling device 83 is not particularly limited and may include, for example, air cooling and water cooling. The cooling device 83 may be omitted, and instead, the arrangement and number of guide rollers 90 may be set so that the distance from the heating furnace 82 to the take-up roll 91 is long, thereby increasing the heat dissipation time. In addition, the arrangement and number of guide rollers 90 are not limited to those shown in FIG. 1. The PTFE resin tube 1 is taken up by the take-up roll 91 while still including the core wire 4.

[0049] By removing the core wire 4 when in use, the PTFE resin tube 1 can be used with a hollow structure. For example, a PTFE resin tube 1 having a structure as shown in Figs. 2 to 4 can be obtained. Fig. 2 is a perspective view showing an example of a PTFE resin tube. Figs. 3 and 4 are cross-sectional views taken along imaginary planes III-III' and IV-IV' shown in Fig. 2, respectively.

[0050] The PTFE resin tube 1 shown in Fig. 2 has a hollow cylindrical shape. In this example, the PTFE resin tube 1 has a two-layer structure in which an inner layer 2 and an outer layer 3 are laminated in the radial direction of the cylinder. As shown in Fig. 3, the inner layer 2 and the outer layer 3 may each have a circular cross section in a portion along the longitudinal direction of the PTFE resin tube 1. On the other hand, as shown in Fig. 4, the cross section of the inner layer 2 may not be a perfect circle in other portions. A protrusion 33, which is part of the outer layer 3, may fit into the portion where the inner layer 2 is missing.

[0051] The protrusions 33 are formed from the dispersion liquid 30 filled in the pinholes generated in the first tubular precursor 22. FIG. 5 shows a cross-sectional view of the first tubular precursor before the dispersion liquid 30 is applied. Specifically, FIG. 5 is a cross-sectional view of the first tubular precursor 22 when passing through position A shown in FIG. 1, including the pinhole 23. When the first tubular precursor 22 passes through the dispersion liquid 30 containing the second PTFE powder, the dispersion liquid (PTFE dispersion) adheres to the outer periphery of the first tubular precursor 22 and a part of it enters the pinhole 23. The dispersion liquid that entered the pinhole 23 becomes the protrusions 33 by the second baking, and the pinhole 23 is blocked.

[0052] The above example is an example of the manufacture of a PTFE resin tube having a two-layer structure, but the embodiment is not limited to the above example. For example, the number of times of application of the dispersion liquid 30 and the subsequent baking are not limited to one as shown in FIG. 1, and may be performed two or more times. In addition, after the second baking, a dispersion liquid having a composition different from the dispersion liquid 30, such as a dispersion liquid containing a filler, may be further applied to the outer surface of the outer layer 3 and baked to manufacture a PTFE resin tube having a three-layer structure. In addition, after the first baking, the core wire 4 and the first tubular precursor 22 may be temporarily wound on a roll, and this may be used as a supply roll to supply the dispersion liquid 30 again. In addition, extrusion molding and coating with a PTFE dispersion may be performed without using the core wire 4.

[0053] When the core wire 4 is not used, for example, an extruder having a structure shown in Fig. 6 can be used. Fig. 6 is a schematic cross-sectional view of one example of an extruder.

[0054] The extrusion molding machine of the illustrated example has a cylinder 51a and a die 51c disposed below the cylinder 51a via a seal ring 51b. A die 51d having a band heater 54 wound around its outer periphery is disposed below the die 51c. A mandrel 55 is disposed inside the cylinder 51a via a ram 53a and a ram head 53b. A core pin 51e is connected to the bottom of the mandrel 55. In general, a centering bush 56 is inserted into the tip (lower end) of the die 51d.

[0055] The inclination angle (θ) of the central portion of the die 51c may be, for example, 30° or more and 60° or less. When molding with a high reduction ratio (RR), the inclination angle (θ) is preferably 10° or more and 20° or less. The die portion may be heated by a band heater 54 or the like to, for example, 50° C. or more and 60° C. or less.

[0056] In an extruder having such a configuration, as shown in FIG. 6, when the cross-sectional area of ​​the cylinder-mandrel portion is S1 and the cross-sectional area of ​​the die-core pin is S2, the above RR is S1 / S2, and the higher the RR, the greater the drawing ratio.

[0057] FIG. 7 is a schematic cross-sectional view of an extrusion molding machine of another example. FIG. 7 may correspond to a more detailed view of the extrusion molding machine 50 shown in FIG. 1. In FIG. 7, the same members as those in FIG. 6 are described by using the same reference numerals. The extrusion molding machine does not have a core pin, but has a guide tube 57. The core wire 4 is inserted into the guide tube 57. A clearance is provided between the straight portion of the die 51d and the guide tube 57. The extrusion molding machine may further have two divided cylindrical frames 58a, 58b and an annular clamp 59 for fixing the frames 58a, 58b on the outer periphery of the cylinder 51a and the die 51c.

[0058] It can be confirmed that a tube with a two-layer structure has been obtained as follows. The tube is cut at a cross section that intersects the main axis of the tube to expose the cross section. The cross section of the tube is observed under an optical microscope. The inner layer of the tube is formed from PTFE fine powder suitable for extrusion molding, and the outer layer is formed from PTFE powder for PTFE dispersion suitable for coating and baking of a dispersion liquid. The PTFE fine powder and the PTFE powder for dispersion may differ in at least one of particle size, transparency, molecular weight, etc. In such a case, the inner layer and the outer layer can be distinguished by observing the cross section of the tube.

[0059] The tube may be cut and observed while still attached to the core wire, or the core wire may be removed before cutting and observing the tube. Since the tube is prone to crushing without the core wire, it is desirable to at least cut the tube with the core wire still attached.

[0060] The cross section observed differs depending on the position of the cut surface. When the cut surface intersects the position where the pinhole occurred in the first tubular precursor, a cross section in which the cross section of the inner layer 2 is not a complete ring, and a protrusion 33 is formed on the inner surface of the outer layer 3, as in Fig. 4, can be observed. When the cut surface does not intersect any position where a pinhole occurred, a cross section of the tube in which both the cross sections of the inner layer 2 and the outer layer 3 are complete rings, as in Fig. 3, can be observed.

[0061] The resin material forming each layer of the tube can be identified as follows: It is possible to confirm that the resin material is PTFE by measuring the melting point using a differential scanning calorimeter (DSC).

[0062] The presence or absence of pinholes in PTFE resin tubes can be confirmed as follows. For tubes with the core wire still covered, use a spark tester to check for electrical conduction between the outer diameter and the core wire. If electrical conduction is confirmed, it is determined that there is a pinhole. For tubes that do not contain a core wire, seal one end of the tube and introduce air from the other end, then check for leaks underwater. If air leakage is confirmed, it is determined that there is a pinhole.

[0063] [Example] <Manufacturing> In this example, extrusion molding and a first baking were performed with reference to Patent Document 4 (JP Patent Publication 2007-237597A), and the obtained first tubular precursor was molded, and a PTFE dispersion was applied to the outer surface of the molded product, and a second baking was performed to produce a PTFE resin tube. The embodiment is not limited to this example. For example, as a method for obtaining a thin-walled extrusion product during extrusion molding, other methods such as a method using a resin suitable for thin-walled extrusion instead of irradiating with gamma rays or a method using a fluororesin auxiliary may be used.

[0064] Example 1 A PTFE resin tube was produced by the same method as that described with reference to Fig. 1. The details are as follows.

[0065] The PTFE fine powder used was PTFE 640-J manufactured by Chemours, Inc. This resin was irradiated with gamma rays from a Co60 (ionizing radiation) source at an absorbed dose of 3000 Gy.

[0066] As the PTFE dispersion, AD-912 manufactured by Asahi Glass Co., Ltd. was used.

[0067] Next, 21 parts by mass of naphtha was added to 100 parts by mass of the resin powder (PTFE fine powder) irradiated with ionizing radiation, and then mixed at room temperature using a turbular mixer. Next, this mixture was molded into a cylindrical shape using a pre-molding machine, and then fed into a paste extruder equipped with a φ2.6 (mm) die and a φ2.58 (mm) core pin (tip), and extrusion molded. The obtained extrusion molded product was subjected to a first drying at 180°C to 200°C and a first firing at 380°C to 400°C.

[0068] The first tubular precursor obtained by the first baking was cooled, and then the outer surface of the first tubular precursor was coated with a PTFE dispersion by dip coating.

[0069] The PTFE dispersion was adjusted to 54 wt% by adding a surfactant and distilled water, and was pulled up at a constant speed. The obtained second tubular precursor was then subjected to a second drying at 140°C to 180°C and a second baking at 380°C to 400°C. The obtained two-layered polytetrafluoroethylene resin tube was cooled and then wound up on a roll.

[0070] Example 2 First, Teflon (registered trademark) 640-J manufactured by Mitsui DuPont Fluorochemicals was used as the PTFE fine powder. This resin was irradiated with gamma rays from Co60 (ionizing radiation) at an absorbed dose of 3000 Gy. Next, 21 parts by mass of naphtha was added to 100 parts by mass of the resin powder irradiated with ionizing radiation, and then mixed at room temperature using a turbular mixer. Next, this mixture was molded into a cylindrical shape using a pre-molding machine, and then fed into an extruder equipped with a φ2.6 (mm) die and a guide tube (tip), and a silver-plated copper wire with an outer diameter of φ2.58 (mm) was passed through the inner diameter of the guide tube as a core material, and pulled in synchronization with the extrusion, and the extrusion aid was removed in a heating furnace set at 180°C to 200°C (first drying). Next, it was passed through a heating furnace set at 380°C to 400°C and baked to obtain a molded product in which a PTFE layer was coated on the core wire (first baking). Thereafter, the molded product was cut to a fixed length, and the silver-plated copper wire serving as the core material was pulled from both ends, stretched, and pulled out from the coated PTFE layer to obtain a tube with an inner diameter of φ2.58 mm and a wall thickness of 7 μm to 8 μm.

[0071] Next, a PTFE dispersion was applied to the outer surface of the obtained tube, and a second drying and a second baking were performed under the same conditions as in Example 1. The obtained polytetrafluoroethylene resin tube having a two-layer structure was cooled and then wound up on a roll.

[0072] Comparative Example 1 A PTFE resin tube was produced by performing only extrusion molding. That is, after the extrusion molding was baked, the PTFE dispersion was not applied to the obtained tubular molding. In detail, a mixture containing PTFE fine powder prepared by the same procedure as in Example 1 was used, and extrusion molding, first drying, and first baking were performed under the same conditions as in Example 1. The tubular molding obtained by the first baking was wound up on a roll as it was.

[0073] Comparative Example 2 Before the first baking, the extrusion molded product was stretched. In detail, extrusion molding was performed under the same conditions as in Example 1, and the obtained extrusion molded product was subjected to a first drying and then stretched twice in the axial direction. The procedures after the first baking were performed under the same conditions as in Example 1, except that the extrusion molded product after stretching was used.

[0074] The manufacturing conditions of the PTFE resin tubes in Examples 1-2 and Comparative Example 1-2 are summarized in Table 1 below. Specifically, the size of the extrusion die, the diameter of the core wire, and whether or not the PTFE dispersion was applied are shown. Note that since no core wire was used in Example 1 and Comparative Example 1-2, the diameter of the core wire is indicated with "-". Furthermore, since no core pin was used in Example 2, the size of the core pin is indicated with "-".

[0075] [Table 1]

[0076] <Evaluation> (Check the tube thickness) The wall thickness of each tube produced in Example 1-2 and Comparative Example 1-2 was measured as follows. The tube was cut at a cross section intersecting the main axis of the tube to expose the cross section. The cross section was observed under an optical microscope to measure the wall thickness.

[0077] (Check for pinholes) The presence or absence of pinholes was confirmed for each of the tubes manufactured in Examples 1-2 and Comparative Examples 1-2 by the method described above. Specifically, for Example 1 and Comparative Examples 1 and 2, a method of checking for the presence or absence of air leakage in water was adopted, and for Example 2, a method using a spark tester was adopted.

[0078] Table 2 below summarizes the confirmed tube wall thickness and the presence or absence of pinholes.

[0079] [Table 2]

[0080] As shown in Table 4, thin-walled tubes were obtained in Example 1-2 and Comparative Example 1-2. The PTFE resin tube produced in Example 1-2 had no pinholes. On the other hand, the tubes produced in Comparative Examples 1 and 2 contained pinholes.

[0081] According to the above-described embodiment, a method for producing a polytetrafluoroethylene resin tube is provided. This method includes obtaining a tubular extrusion product by extrusion molding of a mixture containing PTFE fine powder, performing a first firing on the extrusion product to obtain a first tubular precursor, applying a PTFE dispersion to the outer surface of the first tubular precursor to obtain a second tubular precursor, and performing a second firing on the second tubular precursor. This method can produce a thin-walled polytetrafluoroethylene resin tube with a high yield.

[0082] The present invention is not limited to the above-mentioned embodiment, and can be modified in various ways without departing from the gist of the present invention. The embodiments may be combined as appropriate, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention. The invention as originally claimed in the present application is set forth below. [1] A method for producing a polytetrafluoroethylene resin tube, comprising the steps of: Obtaining a tubular extrusion molded product by extruding a mixture containing polytetrafluoroethylene fine powder; performing a first firing on the extrusion molded product to obtain a first tubular precursor; applying a polytetrafluoroethylene dispersion to an outer surface of the first tubular precursor to obtain a second tubular precursor; and subjecting the second tubular precursor to a second firing. [2] The method according to [1], wherein the extrusion-molded product has a wall thickness of 20 μm or less. [Explanation of symbols]

[0083] Reference Signs List 1...PTFE resin tube, 2...inner layer, 3...outer layer, 4...core wire, 10...second tubular precursor, 20...mixture, 21...extrusion molded product, 22...first tubular precursor, 23...pinhole, 30...dispersion, 31...dispersed PTFE coating, 33...projection, 50...extrusion molding machine, 51...extrusion die, 51a...cylinder, 51b...seal ring, 51c...die, 51d...die, 51e...core pin, 52 ...discharge port, 53...extrusion ram, 53a...ram, 53b...ram head, 54...band heater, 55...mandrel, 56...centering bush, 57...guide tube, 58a...frame, 58b...frame, 59...clamp, 61...drying furnace, 62...heating furnace, 63...cooling device, 71...bath, 81...drying furnace, 82...heating furnace, 83...cooling device, 90...guide roller, 91...winding roll.

Claims

1. A method for producing a polytetrafluoroethylene resin tube, comprising the steps of: Obtaining a tubular extrusion molded product by extruding a mixture containing polytetrafluoroethylene fine powder; performing a first baking process on the extrusion molded product without performing a stretching process to obtain a first tubular precursor; After the first baking, a polytetrafluoroethylene dispersion is applied to an outer surface of the first tubular precursor without any additional treatment to obtain a second tubular precursor; and subjecting the second tubular precursor to a second firing.

2. The method of claim 1 , wherein the extrusion has a wall thickness of 20 μm or less.

Citation Information

Patent Citations

  • Porous tube of polytetrafluoroethylene and its manufacture

    JP1998323923A

  • Fluororesin tube, production of the tube and deaerating method and deaerating device using the tube

    JP1998337405A

  • Thin and multi-layered tube

    JP2006205680A

  • Tube made of polytetrafluoroethylene

    JP2007237597A

  • Tube

    JP2012092901A