Image display device
A double-sided adhesive sheet with a base material, having a thicker adhesive layer on the transparent plate side and a thinner layer on the panel side, addresses deformation issues in image display panels, enhancing adhesion and reducing pressure marks.
Patent Information
- Application Number
- JP2020014199
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-30
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-01-30
AI Technical Summary
Image display panels using flexible substrates deform locally during pressure processing, leading to permanent pressure marks, while rigid substrates are resistant to deformation but difficult to bond effectively with transparent plates, resulting in air bubble formation and poor adhesion.
A double-sided adhesive sheet with a base material is used, featuring a thicker first adhesive layer on the transparent plate side and a thinner second layer on the panel side, to absorb pressure and reduce deformation marks.
The solution effectively reduces pressure marks and air bubbles, ensuring strong adhesion and improved durability of the image display device by absorbing pressure and maintaining panel integrity.
Smart Images

Figure 0007555710000003 
Figure 0007555710000004 
Figure 0007555710000005
Abstract
Description
[Technical field]
[0001] The present invention , painting This invention relates to image display devices. [Background technology]
[0002] Liquid crystal display devices and organic electroluminescence display devices are widely used as various image display devices such as mobile phones, smartphones, car navigation devices, personal computer monitors, televisions, etc. In order to prevent damage to the image display panel due to impact from the outer surface, a front transparent plate (also called a "cover window" or the like) such as a transparent resin plate or glass plate may be provided on the viewing side of the image display panel.
[0003] A colored layer (decorative printed layer) for decoration or light shielding purposes may be formed on the periphery of the front transparent plate. When a pressure sensitive adhesive is attached to a transparent member having a decorative printed layer, air bubbles are likely to form around the printed step portion. For this reason, a method has been adopted in which a thick adhesive sheet is used to provide step absorption properties and suppress defects such as air bubble inclusion (e.g., Patent Document 1). As the brightness of display devices increases, there is a tendency for the decorative printed layer to become thicker in order to improve light shielding properties, and accordingly, thicker and softer adhesive sheets are being used to attach the front transparent plate.
[0004] Patent Document 2 proposes using an adhesive sheet with a base film, in which adhesive layers having a predetermined thickness are laminated on both sides of a base film, as an adhesive sheet for attaching a cover window to the polarizing plate of a liquid crystal panel equipped with an in-cell or on-cell touch sensor.
[0005] Conventionally, the mainstream image display device was a liquid crystal display device that placed polarizing plates on the front and back of a liquid crystal cell that had a liquid crystal layer sandwiched between two glass substrates, and combined with a light source such as a backlight. In recent years, organic electroluminescence (EL) display devices, which have electrodes and a light-emitting layer on a resin film substrate such as a polyimide film, have been put to practical use. Since organic EL displays are self-emitting and do not require a light source, it is possible to make the screen thinner, curved, and flexible. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2013 / 161666 [Patent Document 2] JP 2017-160416 A Summary of the Invention [Problem to be solved by the invention]
[0007] In forming an image display device, pressure processing such as heat pressing or pressure bonding may be performed when or after bonding the image display panel and the front transparent plate. In an image display panel using a rigid substrate such as a glass substrate, the substrate is not easily deformed, so the image display panel hardly deforms even when localized pressure is applied. On the other hand, in an image display panel using a flexible substrate, the substrate deforms locally when a large pressure is applied locally to the connection points of the components during pressure processing. If the localized deformation does not recover after the pressure is released and remains as a "pressure mark," this can be a defect in the image display. [Means for solving the problem]
[0008] By using a double-sided adhesive sheet with a substrate, in which an adhesive layer is provided on both sides of a film substrate, to bond the image display panel to the front transparent plate, it is possible to suppress indentations caused by deformation of the image display panel due to localized pressure application from the back side.
[0009] The present invention Used in the formation of image display devices The pressure-sensitive adhesive sheet is a substrate-attached double-sided pressure-sensitive adhesive sheet having a first pressure-sensitive adhesive layer on one main surface of a transparent film substrate and a second pressure-sensitive adhesive layer on the other main surface of the substrate, the first pressure-sensitive adhesive layer being thicker than the second pressure-sensitive adhesive layer.
[0010] The thickness of the first pressure-sensitive adhesive layer is preferably 80 μm or more, and the thickness of the second pressure-sensitive adhesive layer is preferably 150 μm or less. The thickness of the transparent film substrate is preferably 15 to 150 μm. The front retardation of the transparent film substrate is preferably 50 nm or less.
[0011] The double-sided adhesive sheet with substrate is Includes touch sensor On the visible side of the image display panel Does not include touch sensor The adhesive can be used to form an image display device having a front transparent plate disposed thereon, in which the first adhesive layer is bonded to the front transparent plate and the second adhesive layer is bonded to an image display panel.
[0012] The image display panel may be an organic EL display device including an organic EL cell. The organic EL cell may include electrodes and an organic light-emitting layer on a resin film substrate. Effect of the Invention
[0013] By bonding the image display cell and the front transparent plate via the substrate-attached pressure-sensitive adhesive sheet of the present invention, it is possible to reduce the remaining marks caused by pressure applied from the back surface side. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a cross-sectional view showing an example of a laminate structure of a double-sided pressure-sensitive adhesive sheet with a substrate. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of the configuration of an image display device. [Diagram 3] FIG. 2 is a cross-sectional view showing an example of a laminated structure of an optical film with a pressure-sensitive adhesive sheet. [Figure 4] FIG. 2 is a cross-sectional view showing an example of a laminated structure of an optical film with a pressure-sensitive adhesive sheet. [Diagram 5] FIG. 2 is a schematic diagram showing the arrangement of samples in an impact resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Fig. 1 is a cross-sectional view of a double-sided pressure-sensitive adhesive sheet with a substrate. The double-sided pressure-sensitive adhesive sheet with a substrate 15 comprises a first pressure-sensitive adhesive layer 51 on one main surface of a transparent film substrate 59, and a second pressure-sensitive adhesive layer 53 on the other main surface of the transparent film substrate 59. In the embodiment shown in Fig. 1, release films 21, 23 are temporarily attached to the surfaces of the pressure-sensitive adhesive layers 51, 53. Fig. 2 is a cross-sectional view showing an example of the configuration of an image display device in which a front transparent plate 7 is fixed to the viewing side surface of an image display panel using the double-sided pressure-sensitive adhesive sheet with a substrate 15.
[0016] [Image display panel] In an image display device 201 shown in FIG. 2, an image display panel 10 includes an image display cell 6 such as a liquid crystal cell or an organic EL cell.
[0017] The image display cell 6 includes a functional layer for image display and a substrate supporting the functional layer. For example, in a liquid crystal cell, a liquid crystal layer is provided between two transparent substrates, and the amount of light passing through the polarizing plate is adjusted by changing the orientation state of the liquid crystal to change the polarization state of the transmitted light. In an organic EL cell, a pair of electrodes is provided on the substrate, and the amount of light emitted by the organic light emitting layer provided between the electrodes is adjusted.
[0018] The substrate of the image display cell 6 may be a rigid substrate such as glass, or a flexible substrate such as a resin film. By using a resin film substrate, it is possible to reduce the thickness and weight. In addition, by using a resin film substrate, it is possible to form a curved display or a flexible display.
[0019] As an image display cell using a film substrate, there are top-emission type or bottom-emission type organic EL cells. A top-emission type organic EL cell has a metal electrode, an organic light-emitting layer, and a transparent electrode in this order on a substrate, and emits light from the transparent electrode side (opposite side to the substrate). A bottom-emission type organic EL cell has a transparent electrode, an organic light-emitting layer, and a metal electrode in this order on a substrate, and emits light from the substrate side. The organic light-emitting layer may have an electron transport layer, a hole transport layer, and the like, in addition to an organic layer that functions as a light-emitting layer itself. A transparent substrate is used in a bottom-emission type organic EL cell. A substrate does not necessarily have to be transparent in a top-emission type organic EL cell.
[0020] A reinforcing substrate 9 may be provided on the back surface of the image display cell 6 for the purpose of protecting and reinforcing the substrate. A metal plate, a glass plate, a resin film, or the like is used as the reinforcing substrate 9. The thickness of the reinforcing substrate is, for example, about 10 to 200 μm.
[0021] A flexible printed circuit board (FPC) 95 is connected to the outer peripheral edge of the image display cell 6. The FPC 95 is bent so as to wrap around the back surface of the image display cell 6, and is connected to a main substrate 90 arranged on the back surface of the image display cell. In FIG. 2, the FPC and the main substrate are connected by inserting a terminal of the FPC 95 into a connector 91 provided on the main substrate 90. The FPC may be connected to the main substrate by soldering or the like. The FPC and the main substrate may also be connected via lead wires. At the connection points of the FPC, the thickness of the connector and soldered portion may be locally large, and a convex portion may be formed.
[0022] An optical film 3 may be disposed on the viewing side surface of the image display cell 6 via a pressure-sensitive adhesive layer 4. An example of the optical film 3 disposed on the viewing side surface of the image display cell 6 is a polarizing plate. The polarizing plate includes a polarizer, and generally, a transparent film is laminated on both sides of the polarizer as a polarizer protective film. The polarizer protective film on one or both sides of the polarizer may be omitted.
[0023] The polarizing plate may have an optically functional film laminated on one or both surfaces of the polarizer via an appropriate adhesive layer or pressure-sensitive adhesive layer as necessary. Examples of the optically functional film include a retardation plate, a viewing angle widening film, a viewing angle limiting (anti-peeping) film, a brightness enhancing film, etc.
[0024] When the image display cell 6 is an organic EL cell, the metal electrode of the organic EL cell is light reflective, so when external light enters the organic EL cell, the light is reflected by the metal electrode, and the reflected light is seen from the outside as a mirror. By disposing a circular polarizing plate as the optical film 3 on the viewing side surface of the organic EL cell, the reflected light at the metal electrode is prevented from being re-emitted to the outside, improving the visibility and design of the screen.
[0025] The image display panel 10 may be an in-cell or on-cell type image display panel with a touch sensor having a built-in touch sensor. When the image display panel 10 has a touch sensor function, it is not necessary to provide a separate touch sensor on the viewing side of the image display panel 10. Therefore, in the image display device 201, the front transparent plate 7 is attached to the viewing side surface of the image display panel 10 via a double-sided adhesive sheet 15 with a substrate.
[0026] [Front transparent plate] The front transparent plate 7 has a printed layer 76 provided on the periphery of one surface of a transparent flat plate 71. By disposing the front transparent plate on the viewing side surface of the image display panel, damage to the image display panel 10 due to impact from the outer surface can be prevented. In addition, by providing the printed layer 76, wiring members such as the FPC 95 are not visible from the outside, improving the design of the image display device.
[0027] The transparent plate 71 may be a transparent resin plate such as an acrylic resin or a polycarbonate resin, or a glass plate. The transparent plate 71 may be either rigid or flexible. From the viewpoint of improving protection for the image display panel 10, the transparent plate 71 is preferably a rigid substrate, and the thickness of the transparent plate 71 is preferably 200 μm or more, and more preferably 300 μm or more. The thickness of the printing layer 76 is about 10 to 100 μm.
[0028] [Double-sided adhesive sheet with substrate] As shown in FIG. 2, in the substrate-attached double-sided adhesive sheet 15, a first adhesive layer 51 provided on one main surface of a transparent film substrate 59 is bonded to a front transparent plate 7, and a second adhesive layer 53 bonded to the other main surface of the transparent film substrate 59 is bonded to an image display panel 10.
[0029] In the adhesive sheet 15, the adhesive strength of the first adhesive layer 51 to glass is preferably 2N / 10mm or more, more preferably 4N / 10mm or more, and even more preferably 5N / 10mm or more. When the adhesive strength is in the above range, peeling of the adhesive sheet from the adherend can be prevented when stress due to distortion or impact due to dropping or the like occurs. It is preferable that the second adhesive layer 53 also has high adhesive strength, like the first adhesive layer. The adhesive strength is determined by a peel test using a glass plate as the adherend, with a tensile speed of 300mm / min and a peel angle of 180°. Unless otherwise specified, the adhesive strength is measured at 25°C.
[0030] The total light transmittance of the adhesive sheet 15 is preferably 85% or more, and more preferably 90% or more. The haze of the adhesive sheet 15 is preferably 1% or less. The thickness of the adhesive sheet 15 (the total thickness of the transparent film substrate 59 and the adhesive layers 51, 53) is preferably 120 to 1000 μm, more preferably 150 to 500 μm, and even more preferably 180 to 400 μm.
[0031] The adhesive sheet 15 preferably has ultraviolet shielding properties. When the adhesive sheet 15 has ultraviolet shielding properties, deterioration of the organic layer (for example, organic light-emitting layer) included in the polarizing plate 3 and the image display cell 6 of the image display panel 10 due to ultraviolet rays can be suppressed. The transmittance of the adhesive sheet 15 at a wavelength of 380 nm is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less. In order to impart ultraviolet shielding properties to the adhesive sheet 15, it is sufficient to impart ultraviolet shielding properties to any one or more of the first adhesive layer 51, the transparent film substrate 59, and the second adhesive layer 53. For example, ultraviolet shielding properties can be imparted by using a resin material having ultraviolet shielding properties, such as transparent polyimide or polyethylene naphthalate, as the transparent film substrate 59. In addition, an ultraviolet absorber may be included in any one or more of the transparent film substrate 59 and the adhesive layers 51 and 53.
[0032] <Transparent film substrate> A transparent resin film is used as the transparent film substrate 59. The total light transmittance of the transparent film substrate 59 is preferably 85% or more, and more preferably 90% or more. The resin material constituting the transparent film substrate 59 is not particularly limited as long as it has transparency, and examples thereof include polyesters such as polyethylene terephthalate and polyethylene naphthalate; polyolefins such as polyethylene and polypropylene; cyclic polyolefins such as norbornene-based polymers; cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose; acrylic polymers; styrene-based polymers; polycarbonate, polyamide, polyimide, polyether ether ketone, and the like.
[0033] The transparent film substrate 59 may have a functional layer such as an easy-adhesion layer or an antistatic layer on the surface. The transparent film substrate 59 may have a function as a touch sensor. When the transparent film substrate 59 has a function as a touch sensor, an electrode for position detection is provided on the surface of the film. On the other hand, when the image display panel 10 has a touch sensor function, it is not necessary to provide a touch sensor on the viewing side of the image display panel 10. Therefore, the transparent film substrate 59 may not have an electrode for position detection.
[0034] By disposing the transparent film substrate between the two adhesive layers 51, 53, the elasticity of the adhesive sheet 15 as a whole is increased, and the restoring force against deformation is increased. Therefore, even if the image display panel 10 is deformed by pressure from the rear side of the image display panel, the plastic deformation of the adhesive sheet 15 is small, and the restoring force of the film substrate can reduce the remaining of the pressed mark. The thickness of the transparent film substrate 59 is preferably about 15 to 150 μm, more preferably 25 to 120 μm, and further preferably 35 to 100 μm.
[0035] From the viewpoint of suppressing rainbow coloring (iris phenomenon) when the screen of an image display device is viewed, the transparent film substrate 59 preferably has optical isotropy. The front retardation of the transparent film substrate 59 at a wavelength of 590 nm is preferably 50 nm or less, more preferably 30 nm or less, further preferably 10 nm or less, and particularly preferably 5 nm or less.
[0036] <Adhesive layer> The thickness of first pressure-sensitive adhesive layer 51 is greater than the thickness of second pressure-sensitive adhesive layer 53. The thickness of second pressure-sensitive adhesive layer 53 is preferably 0.2 to 0.85 times the thickness of first pressure-sensitive adhesive layer 51, more preferably 0.3 to 0.8 times, and even more preferably 0.4 to 0.75 times.
[0037] The relatively large thickness of the first adhesive layer 51 tends to enhance the step absorbency with respect to the printed layer 76 of the front transparent plate 7. From the viewpoint of ensuring step absorbency and impact resistance, the thickness of the first adhesive layer 51 is preferably 80 μm or more. The thickness of the first adhesive layer 51 may be 100 μm or more or 120 μm or more. When the first adhesive layer 51 is bonded to a front transparent plate having the printed layer 76, the thickness of the first adhesive layer 51 is preferably greater than the thickness of the printed layer 76.
[0038] The upper limit of the thickness of first pressure-sensitive adhesive layer 51 is not particularly limited, but from the viewpoints of productivity, processing dimensional stability, and the like, it is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 250 μm or less.
[0039] The relatively small thickness of the second adhesive layer 53 reduces plastic deformation due to pressure from the image display panel 10 side. Even if the image display panel 10 is deformed by pressure from the back surface side, the adhesive sheet 15 is less plastically deformed, so that the remaining impression can be reduced.
[0040] From the viewpoint of reducing plastic deformation and reducing imprints, the thickness of second pressure-sensitive adhesive layer 53 is preferably 150 μm or less, and more preferably 120 μm or less. The thickness of second pressure-sensitive adhesive layer 53 may be 100 μm or less or 80 μm or less. From the viewpoint of imparting impact resistance, the thickness of second pressure-sensitive adhesive layer 53 is preferably 30 μm or more, and more preferably 50 μm or more.
[0041] When an image display panel and a front transparent plate are bonded together via a single-layer substrate-less adhesive sheet, if the thickness of the adhesive sheet is small, the step absorbency for the printing step of the front transparent plate is insufficient, and if the thickness of the adhesive sheet is large, the adhesive sheet undergoes large plastic deformation, so that a pressing mark due to pressing from the panel side is likely to remain. A substrate-attached adhesive sheet having a transparent film substrate 59 between two adhesive layers 51, 53 can ensure step absorbency by the relatively thick first adhesive layer 51. In addition, the relatively thin second adhesive layer 53 undergoes small plastic deformation, and the elastic restoring force of the transparent film substrate 59 makes it easy for the second adhesive layer 53 to recover from deformation due to pressing from the back side, so that the remaining of pressing marks can be suppressed.
[0042] From the viewpoint of increasing the adhesive retention when the pressure-sensitive adhesive sheet 15 is attached to an adherend and ensuring dimensional stability during processing, the shear storage modulus G' of the first pressure-sensitive adhesive layer 51 at 25°C is 25℃ is preferably 0.16 MPa or more, more preferably 0.18 MPa or more, further preferably 0.20 MPa or more, and particularly preferably 0.21 MPa or more.
[0043] On the other hand, in order to ensure wettability by providing an appropriate viscosity, and to provide step absorbency and cushioning against impacts such as being dropped, the first pressure-sensitive adhesive layer 51 has a G' 25℃ is preferably 0.5 MPa or less, more preferably 0.4 MPa or less, further preferably 0.3 MPa or less, particularly preferably 0.28 MPa or less.
[0044] From the viewpoint of imparting step absorbency to the pressure-sensitive adhesive sheet 15, the loss tangent tanδ of the first pressure-sensitive adhesive layer 51 at 70° C. 70℃ is preferably 0.25 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. 70℃ may be 0.40 or more, 0.45 or more, 0.50 or more, or 0.55 or more. 70℃ is preferably 1.0 or less, more preferably 0.9 or less, and even more preferably 0.85 or less. 70℃ may be 0.80 or less, 0.75 or less, or 0.70 or less.
[0045] The peak top value of tan δ of the first pressure-sensitive adhesive layer 51 is preferably 1.5 or more, more preferably 1.6 or more, and even more preferably 1.7 or more. A pressure-sensitive adhesive having a large peak top value of tan δ tends to have a large viscous behavior and excellent impact resistance. The upper limit of the peak top value of tan δ of the first pressure-sensitive adhesive layer 51 is not particularly limited, but is generally 3.0 or less. From the viewpoint of adhesive retention, the peak top value of tan δ is preferably 2.7 or less, and more preferably 2.5 or less.
[0046] The glass transition temperature of the first pressure-sensitive adhesive layer 51 is preferably −3° C. or lower, more preferably −4° C. or lower. The glass transition temperature of the first pressure-sensitive adhesive layer 51 is preferably −20° C. or higher, more preferably −15° C. or higher, and even more preferably −13° C. or higher. When the glass transition temperature is within the above range, the pressure-sensitive adhesive has appropriate viscosity even in a low temperature range, and peeling of the adherend due to impact such as dropping tends to be suppressed.
[0047] The shear storage modulus G', loss tangent tan δ, and glass transition temperature are determined by viscoelasticity measurements at a frequency of 1 Hz. Tan δ is the ratio G" / G' of the storage modulus G' to the loss modulus G", and the glass transition temperature is the temperature at which tan δ is maximized (peak top temperature). The storage modulus G' corresponds to the portion stored as elastic energy when the material is deformed, and is an index of the degree of hardness. The larger the storage modulus, the higher the adhesive retention and the more likely it is that peeling due to distortion will be suppressed. The loss modulus G" corresponds to the portion of the lost energy dissipated due to internal friction when the material is deformed, and indicates the degree of viscosity. The larger the tan δ, the stronger the tendency for viscosity, the more liquid-like the deformation behavior, and the smaller the rebound elastic energy.
[0048] G' 25℃ From the viewpoint of ensuring processing stability by setting the pressure sensitive adhesive to 0.16 MPa or more and imparting appropriate flexibility for imparting step absorbency, the gel fraction of the pressure sensitive adhesive is preferably 30 to 80%, more preferably 35 to 70%. The gel fraction may be 40% or more or 45% or more, and may be 65% or less, or 60% or less.
[0049] The gel fraction of an adhesive can be determined as the insoluble portion in a solvent such as ethyl acetate, specifically, the weight fraction (unit: weight %) of the insoluble portion after immersing the adhesive in ethyl acetate for 7 days at 23°C relative to the sample before immersion. In general, the gel fraction of a polymer is equal to the degree of crosslinking, and the more crosslinked portions in the polymer, the higher the gel fraction. The gel fraction (amount of crosslinked structure introduced) can be adjusted to a desired range by the method of introducing the crosslinked structure, the type and amount of the crosslinking agent, etc.
[0050] There are no particular limitations on the second pressure-sensitive adhesive layer 53 as long as it is a transparent pressure-sensitive adhesive layer having the above-mentioned thickness. The pressure-sensitive adhesive of the first pressure-sensitive adhesive layer 51 and the pressure-sensitive adhesive of the second pressure-sensitive adhesive layer 53 may be the same or different. From the viewpoint of enhancing adhesive retention, dimensional stability, and impact resistance, the second pressure-sensitive adhesive layer 53 has a shear storage modulus G' at 25°C of 100% or more. 25℃ , Loss tangent tanδ at 70℃ 70℃ It is preferable that the peak top value of tan δ, the glass transition temperature, and the gel fraction for first pressure-sensitive adhesive layer 51 are within the ranges mentioned above.
[0051] <Adhesive composition> The composition of the adhesive constituting the first adhesive layer 51 and the second adhesive layer 53 is not particularly limited, and an adhesive having a base polymer such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyvinyl ether, a vinyl acetate / vinyl chloride copolymer, a modified polyolefin, an epoxy polymer, a fluorine polymer, or a rubber-based polymer such as natural rubber or synthetic rubber can be appropriately selected and used. In particular, an acrylic adhesive containing an acrylic base polymer into which a crosslinked structure has been introduced is preferably used, since it has excellent optical transparency, exhibits adhesive properties such as appropriate wettability, cohesiveness, and adhesion, and is also excellent in weather resistance and heat resistance.
[0052] The acrylic base polymer contains an alkyl (meth)acrylate ester as a main constituent monomer component. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.
[0053] The (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 1 to 20. The (meth)acrylic acid alkyl ester may have an alkyl group that is branched or may have a cyclic alkyl group.
[0054] Specific examples of (meth)acrylic acid alkyl esters having a chain alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, and isooctyl (meth)acrylate. Examples of acrylates include acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, isotridodecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, and nonadecyl (meth)acrylate.
[0055] Specific examples of (meth)acrylic acid alkyl esters having an alicyclic alkyl group include (meth)acrylic acid cycloalkyl esters such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring such as isobornyl (meth)acrylate; and (meth)acrylic acid esters having a tricyclic or higher aliphatic hydrocarbon ring such as dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.
[0056] The amount of (meth)acrylic acid alkyl ester relative to the total amount of monomer components constituting the acrylic base polymer is preferably 50% by weight or more, more preferably 55% by weight or more, and even more preferably 60% by weight or more. From the viewpoint of setting the glass transition temperature (Tg) in an appropriate range, the amount of (meth)acrylic acid alkyl ester having a chain alkyl group having 4 to 10 carbon atoms relative to the total amount of the monomer components constituting the acrylic base polymer is preferably 40% by weight or more, more preferably 50% by weight or more, and even more preferably 55% by weight or more. The monomer components constituting the acrylic base polymer are those excluding monomers (such as polyfunctional (meth)acrylates and urethane (meth)acrylates described below) used to form a crosslinked structure and crosslinking agents from all monomer components constituting the polymer.
[0057] The acrylic base polymer may contain a hydroxyl group-containing monomer or a carboxyl group-containing monomer as a constituent monomer component. When a crosslinking structure is introduced by an isocyanate crosslinking agent, the hydroxyl group becomes a reaction site with the isocyanate group, and when a crosslinking structure is introduced by an epoxy crosslinking agent, the carboxyl group becomes a reaction site with the epoxy group.
[0058] Examples of the hydroxyl group-containing monomer include (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl (meth)acrylate. When a crosslinked structure due to a urethane-based segment is introduced into the acrylic base polymer, it is preferable that the acrylic base polymer contains a (meth)acrylic acid ester having a hydroxyalkyl group having 4 to 8 carbon atoms as a constituent monomer component, from the viewpoint of high compatibility with the urethane-based segment and improving the transparency of the pressure-sensitive adhesive.
[0059] By having the acrylic base polymer contain a hydroxyl group-containing monomer as a constituent monomer component, the transparency of the adhesive is improved and opacity in a high temperature and high humidity environment tends to be suppressed. In addition, the hydroxyl group of the hydroxyl group-containing monomer can form a physical crosslink by hydrogen bonding with the acrylic polymer or the crosslinked segment. Therefore, by increasing the ratio of the hydroxyl group-containing monomer in the monomer components constituting the acrylic base polymer, the cohesive force is increased and the G' 25℃ The amount of the hydroxyl group-containing monomer relative to the total amount of monomer components constituting the acrylic base polymer is preferably from 5 to 30% by weight, more preferably from 8 to 25% by weight, and even more preferably from 10 to 20% by weight.
[0060] Examples of the carboxy group-containing monomer include acrylic monomers such as (meth)acrylic acid, carboxyethyl (meth)acrylate, and carboxypentyl (meth)acrylate, as well as itaconic acid, maleic acid, fumaric acid, and crotonic acid.
[0061] The acrylic base polymer may contain a nitrogen-containing monomer as a constituent monomer component. Examples of the nitrogen-containing monomer include vinyl monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinyl carboxylic acid amides, and N-vinylcaprolactam, and cyano group-containing acrylic monomers such as acrylonitrile and methacrylonitrile. Among these, N-vinylpyrrolidone is preferred because it has a high effect of improving adhesive strength by improving cohesive strength.
[0062] By containing highly polar monomers such as hydroxyl group-containing monomers, carboxyl group-containing monomers and nitrogen-containing monomers as constituent monomer components in the acrylic base polymer, the cohesive strength of the pressure-sensitive adhesive is increased, and the G' 25℃ The amount of the highly polar monomer increases, and the adhesive retention tends to improve. On the other hand, if the content of the highly polar monomer is excessively large, the glass transition temperature increases, and impact resistance may decrease. Therefore, the amount of the highly polar monomer (the total of the hydroxyl group-containing monomer, the carboxyl group-containing monomer, and the nitrogen-containing monomer) relative to the total amount of the monomer components constituting the acrylic base polymer is preferably 15 to 45% by weight, more preferably 20 to 40% by weight, and even more preferably 25 to 37% by weight. In particular, it is preferable that the total of the hydroxyl group-containing monomer and the nitrogen-containing monomer is within the above range. The amount of the nitrogen-containing monomer relative to the total amount of the monomer components constituting the acrylic base polymer is preferably 7 to 30% by weight, more preferably 10 to 25% by weight, and even more preferably 12 to 22% by weight.
[0063] The acrylic base polymer may contain, as monomer components other than those mentioned above, vinyl monomers such as acid anhydride group-containing monomers, caprolactone adducts of (meth)acrylic acid, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, vinyl acetate, vinyl propionate, styrene, and α-methylstyrene; cyano group-containing acrylic monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing monomers such as glycidyl (meth)acrylate; glycol-based acrylic ester monomers such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; and acrylic ester monomers such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, silicone (meth)acrylate, and 2-methoxyethyl (meth)acrylate.
[0064] Of the above monomer components, the acrylic base polymer preferably has the highest content of (meth)acrylic acid alkyl ester. The characteristics of the adhesive are easily influenced by the type of monomer (main monomer) that is the most abundant among the constituent monomers of the base polymer. For example, when the main monomer is a (meth)acrylic acid alkyl ester having a chain alkyl group with 6 or less carbon atoms, tan δ 70℃ In particular, when butyl acrylate or other C4 alkyl esters of acrylic acid are the main monomers, tanδ 70℃ tends to be large. The amount of the (meth)acrylic acid alkyl ester having a chain alkyl group having 6 or less carbon atoms relative to the total amount of the monomer components constituting the acrylic base polymer is preferably 40 to 85% by weight, more preferably 45 to 80% by weight, and even more preferably 50 to 75% by weight. In particular, it is preferable that the content of butyl acrylate as a constituent monomer component is in the above range.
[0065] The theoretical Tg of the acrylic base polymer is preferably -50°C or higher. The theoretical Tg of the acrylic base polymer is preferably -10°C or lower, more preferably -20°C or lower, and even more preferably -25°C or lower. The theoretical Tg is the glass transition temperature Tg of the homopolymer of the constituent monomer component of the acrylic base polymer. i and the weight fraction W of each monomer component i It is calculated using the following Fox formula: 1 / Tg=Σ(W i / Tg i )
[0066] Tg is the glass transition temperature of the polymer (unit: K), W i is the weight fraction of the monomer component i constituting the segment (copolymerization ratio by weight), Tg i is the glass transition temperature (unit: K) of the homopolymer of monomer component i. The glass transition temperature of the homopolymer can be the value described in Polymer Handbook, 3rd Edition (John Wiley & Sons, Inc., 1989). For the Tg of the homopolymer of a monomer not described in the above literature, the peak top temperature of the loss tangent (tan δ) measured by dynamic viscoelasticity measurement can be used.
[0067] A polymer having a crosslinked structure introduced therein can be obtained, for example, by (1) a method in which a polymer having a functional group capable of reacting with a crosslinking agent is polymerized, and then a crosslinking agent is added to react the polymer with the crosslinking agent; and (2) a method in which a branched structure (crosslinked structure) is introduced by including a multifunctional compound in the polymerization components of the polymer, etc. These methods may be used in combination to introduce multiple types of crosslinked structures into the base polymer.
[0068] Specific examples of the crosslinking agent in the above method (1) of reacting the base polymer with the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, carbodiimide-based crosslinking agents, and metal chelate-based crosslinking agents. Among them, isocyanate-based crosslinking agents and epoxy-based crosslinking agents are preferred because they have high reactivity with the hydroxyl groups and carboxyl groups of the base polymer and are easy to introduce a crosslinked structure. These crosslinking agents react with functional groups such as hydroxyl groups and carboxyl groups introduced into the base polymer to form a crosslinked structure. In an acid-free adhesive in which the base polymer does not contain a carboxyl group, it is preferred to use an isocyanate-based crosslinking agent to form a crosslinked structure by reacting the hydroxyl groups in the base polymer with the isocyanate crosslinking agent.
[0069] As the isocyanate crosslinking agent, a polyisocyanate having two or more isocyanate groups in one molecule is used. Examples of the isocyanate crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate; trimethylolpropane / Examples of the isocyanate adduct include tolylene diisocyanate trimer adduct (e.g., Tosoh's "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (e.g., Tosoh's "Coronate HL"), xylylene diisocyanate trimethylolpropane adduct (e.g., Mitsui Chemicals' "Takenate D110N"), and hexamethylene diisocyanate isocyanurate (e.g., Tosoh's "Coronate HX"). In addition, by using a urethane prepolymer having an isocyanate group at the end as the isocyanate crosslinking agent, a crosslinked structure by a urethane segment can be introduced.
[0070] In the above method (2) of including a polyfunctional compound in the polymerization components of the base polymer, the monomer components constituting the acrylic base polymer and the polyfunctional compound for introducing a crosslinking structure may be reacted in their entirety at once, or the polymerization may be carried out in multiple stages. As a method of carrying out polymerization in multiple stages, a method is preferred in which a monofunctional monomer constituting the base polymer is polymerized (preliminary polymerization) to prepare a partial polymer (prepolymer composition), and a polyfunctional compound such as a polyfunctional (meth)acrylate is added to the prepolymer composition to polymerize the prepolymer composition and the polyfunctional monomer (main polymerization). The prepolymer composition is a partial polymer containing a polymer with a low degree of polymerization and an unreacted monomer.
[0071] By carrying out prepolymerization of the components of the acrylic base polymer, branching points (crosslinking points) due to the polyfunctional compound can be uniformly introduced into the base polymer. In addition, a mixture (adhesive composition) of a low molecular weight polymer or a partially polymerized product and an unpolymerized monomer component can be applied onto a substrate, and then main polymerization can be carried out on the substrate to form a pressure-sensitive adhesive layer. Since low-polymerization compositions such as prepolymer compositions have low viscosity and excellent applicability, the method of carrying out main polymerization on a substrate after applying a pressure-sensitive adhesive composition, which is a mixture of a prepolymer composition and a polyfunctional compound, can improve the productivity of the pressure-sensitive adhesive layer and make the thickness of the pressure-sensitive adhesive layer uniform.
[0072] The polyfunctional compound used for introducing the crosslinked structure may be a compound containing two or more polymerizable functional groups (ethylenically unsaturated groups) having an unsaturated double bond in one molecule. As the polyfunctional compound, a polyfunctional (meth)acrylate is preferred because it is easily copolymerized with the monomer component of the acrylic base polymer. When introducing a branched (crosslinked) structure by active energy ray polymerization (photopolymerization), a polyfunctional acrylate is preferred.
[0073] Examples of polyfunctional (meth)acrylates include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, bisphenol A ethylene oxide modified di(meth)acrylate, bisphenol A propylene oxide modified di(meth)acrylate, alkanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol dimethacrylate. Examples of the di(meth)acrylate include pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, dipentaerythritol hexa(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin di(meth)acrylate, epoxy (meth)acrylate, butadiene (meth)acrylate, and isoprene (meth)acrylate.
[0074] By using a urethane (meth)acrylate having a (meth)acryloyl group at the end of the urethane chain as the multifunctional (meth)acrylate, a crosslinked structure due to the urethane-based segment can be introduced. By crosslinking the acrylic-based base polymer with the urethane-based segment, a pressure-sensitive adhesive that can achieve both a low glass transition temperature and high adhesive retention is easily obtained. The urethane-based segment is a molecular chain having a urethane bond, and both ends of the urethane-based segment are covalently bonded to the acrylic-based base polymer, thereby introducing a crosslinked structure due to the urethane-based segment. The urethane-based segment is typically obtained by reacting a diol with a diisocyanate and contains a polyurethane chain.
[0075] The molecular weight of the polyurethane chain in the urethane-based segment is preferably 5,000 to 30,000, more preferably 6,000 to 23,000, and even more preferably 7,000 to 20,000. The larger the molecular weight of the polyurethane chain in the urethane-based segment, the longer the distance between crosslinking points. If the molecular weight of the polyurethane chain is within the above range, the polymer into which the crosslinked structure is introduced has appropriate cohesiveness and fluidity, so that it is possible to achieve both adhesive strength, step absorbency, and impact resistance.
[0076] When the molecular weight of the polyurethane chain is too small and the distance between crosslinking points is short, the tan δ decreases with an increase in cohesive force, and the step absorption and impact resistance tend to decrease. On the other hand, when the molecular weight of the polyurethane chain is too large and the distance between crosslinking points is long, the storage modulus is small and the adhesive retention may be insufficient. Even when the molecular weight of the polyurethane chain is large, the storage modulus can be increased by increasing the amount of urethane-based segments to increase the gel fraction. However, since polyurethane chains with large molecular weights have low compatibility with acrylic polymers, the haze of the adhesive may increase and the transparency may decrease with an increase in the amount of urethane-based segments.
[0077] When the amount of the urethane-based segment is excessively large, the viscosity of the adhesive decreases with an increase in the gel fraction, and the step absorption and impact resistance may decrease. In addition, when the amount of the urethane-based segment is excessively large, the transparency of the adhesive may decrease and the haze may increase. Therefore, the amount of the urethane-based segment in the base polymer is preferably 10 parts by weight or less, more preferably 7 parts by weight or less, and even more preferably 5 parts by weight or less, relative to 100 parts by weight of the acrylic polymer. On the other hand, from the viewpoint of increasing the gel fraction and providing adhesive retention, the amount of the urethane-based segment in the base polymer is preferably 0.3 parts by weight or more, more preferably 0.4 parts by weight or more, and even more preferably 0.5 parts by weight or more, relative to 100 parts by weight of the acrylic polymer. The amount of the urethane-based segment in the base polymer may be 4 parts by weight or less or 3 parts by weight or less, or 0.7 parts by weight or more, or 1 part by weight or more, relative to 100 parts by weight of the acrylic polymer.
[0078] Diols used to form polyurethane chains include low molecular weight diols such as ethylene glycol, diethylene glycol, propylene glycol, butylene glycol, and hexamethylene glycol; and high molecular weight polyols such as polyester polyols, polyether polyols, polycarbonate polyols, acrylic polyols, epoxy polyols, and caprolactone polyols.
[0079] The diisocyanate used to form the polyurethane chain may be either an aromatic diisocyanate or an aliphatic diisocyanate. As the diisocyanate, a derivative of an isocyanate compound may be used. Examples of the derivative of an isocyanate compound include a dimer of polyisocyanate, a trimer of isocyanate (isocyanurate), polymeric MDI, an adduct with trimethylolpropane, a biuret modified product, an allophanate modified product, and a urea modified product. As the diisocyanate component, a urethane prepolymer having an isocyanate group at the end may be used.
[0080] Among the exemplified polyurethane chains, it is preferable to include polyether urethane having polyether polyol as a diol component and / or polyester urethane having polyester polyol as a diol component, since it has high compatibility with acrylic polymers. In particular, when a crosslinked structure is introduced by polyester urethane, the storage modulus at room temperature tends to increase, and the adhesive retention and processability tend to improve. One reason for this is that polyester has a more rigid molecular structure than polyether and the like. When a crosslinked structure is introduced by a rigid segment, the movement of the polymer is restricted, so the storage modulus is increased, while the distance between the crosslinked points of the polymer is maintained, so it is thought that impact resistance and step absorption are exhibited.
[0081] A crosslinked structure due to a urethane-based segment can be introduced into the acrylic polymer by using a compound having a functional group copolymerizable with a monomer component constituting the acrylic polymer at the end of the polyurethane chain, or a compound having a functional group reactive with a carboxyl group, hydroxyl group, etc. contained in the acrylic polymer at the end of the polyurethane chain. It is preferable to introduce a crosslinked structure due to a urethane-based segment by using a urethane di(meth)acrylate having (meth)acryloyl groups at both ends of the polyurethane chain as the above-mentioned polyfunctional (meth)acrylate, since it is easy to uniformly introduce crosslinking points into the acrylic polymer and the compatibility between the acrylic polymer and the urethane-based segment is excellent.
[0082] A urethane di(meth)acrylate having (meth)acryloyl groups at both ends can be obtained, for example, by using a (meth)acrylic compound having a hydroxyl group in addition to a diol component in polyurethane polymerization. From the viewpoint of controlling the chain length (molecular weight) of the urethane-based segment, it is preferable to react a diol with a diisocyanate so that there is an excess of isocyanate to synthesize an isocyanate-terminated polyurethane, and then add a (meth)acrylic compound having a hydroxyl group to react the terminal isocyanate group of the polyurethane with the hydroxyl group of the (meth)acrylic compound.
[0083] Polyhydric alcohol and polyisocyanate compound are reacted so that the polyisocyanate compound is in excess, thereby obtaining polyurethane chains having isocyanate groups at the ends. In order to obtain isocyanate-terminated polyurethane, diol components and diisocyanate components may be used so that the NCO / OH (equivalent ratio) is preferably 1.1 to 2.0, more preferably 1.15 to 1.5. The diol component and diisocyanate component may be mixed in approximately equal amounts and reacted, and then the diisocyanate component may be added.
[0084] Examples of the (meth)acrylic compound having a hydroxyl group include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxymethylacrylamide, and hydroxyethylacrylamide.
[0085] As the urethane (meth)acrylate, commercially available products sold by companies such as Arakawa Chemical Industries, Ltd., Shin-Nakamura Chemical Industry Co., Ltd., Toa Gosei Co., Ltd., Kyoeisha Chemical Co., Ltd., Nippon Kayaku Co., Ltd., Nippon Synthetic Chemical Industry Co., Ltd., Negami Chemical Industries, Ltd., Daicel Allnex Co., Ltd., etc. The weight average molecular weight of the urethane (meth)acrylate is preferably 5,000 to 30,000, more preferably 6,000 to 23,000, and even more preferably 7,000 to 20,000.
[0086] The glass transition temperature of the urethane (meth)acrylate is preferably 0° C. or lower, more preferably −10° C. or lower, and even more preferably −20° C. or lower. By using a urethane (meth)acrylate with a low Tg, even if a crosslinked structure is introduced by a urethane-based segment to increase the cohesive strength of the base polymer, a pressure-sensitive adhesive having excellent low-temperature adhesive strength can be obtained. The lower limit of the glass transition temperature of the urethane (meth)acrylate is not particularly limited, but from the viewpoint of obtaining a pressure-sensitive adhesive having excellent high-temperature retention, it is preferably −100° C. or higher, more preferably −90° C. or higher, and even more preferably −80° C. or higher.
[0087] When a crosslinked structure due to a urethane-based segment is introduced into an acrylic polymer using a urethane (meth)acrylate, the glass transition temperature of the urethane-based segment of the base polymer is approximately equal to the glass transition temperature of the urethane (meth)acrylate.
[0088] <Adhesive composition> An adhesive layer is formed by applying an adhesive composition containing a base polymer onto a substrate, and then drying the solvent and / or crosslinking / curing the base polymer as necessary.
[0089] The base polymer can be prepared by a known polymerization method such as solution polymerization, photopolymerization (UV polymerization), bulk polymerization, emulsion polymerization, etc. In terms of the transparency, water resistance, cost, etc. of the adhesive, solution polymerization or photopolymerization is preferred. Since photopolymerization can prepare a polymer without using a solvent, it is not necessary to dry and remove the solvent when forming the adhesive layer, and a thick adhesive layer can be formed uniformly.
[0090] In preparing the base polymer, a polymerization initiator such as a photopolymerization initiator or a thermal polymerization initiator may be used depending on the type of polymerization reaction. As the photopolymerization initiator, a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, a thioxanthone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, or the like may be used. As the thermal polymerization initiator, an azo-based initiator, a peroxide-based initiator, or a redox-based initiator in which a peroxide and a reducing agent are combined (for example, a combination of a persulfate and sodium hydrogen sulfite, a combination of a peroxide and sodium ascorbate, or the like) may be used.
[0091] In order to adjust the molecular weight of the base polymer, a chain transfer agent may be used. Examples of the chain transfer agent include thiols such as α-thioglycerol, lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, and 2,3-dimercapto-1-propanol, and α-methylstyrene dimer.
[0092] When a polyfunctional monomer is used in addition to a monofunctional monomer as a monomer component forming a base polymer, the monofunctional monomer may be polymerized first to form a prepolymer composition with a low degree of polymerization (preliminary polymerization), and then the polyfunctional monomer may be added to the syrup of the prepolymer composition to polymerize the prepolymer and the polyfunctional monomer (main polymerization). In this way, by performing prepolymerization, branch points resulting from the polyfunctional monomer component can be uniformly introduced into the base polymer. In addition, a mixture (adhesive composition) of a prepolymer composition and an unpolymerized monomer component may be applied onto a substrate, and then main polymerization may be performed on the substrate to form a pressure-sensitive adhesive layer. Since the prepolymer composition has low viscosity and excellent coatability, the method of performing main polymerization on a substrate after applying a pressure-sensitive adhesive composition, which is a mixture of a prepolymer composition and an unpolymerized monomer, can increase the productivity of the pressure-sensitive adhesive layer and make the thickness of the pressure-sensitive adhesive layer uniform.
[0093] The prepolymer composition can be prepared, for example, by partially polymerizing (preliminarily polymerizing) a composition (referred to as a "prepolymer-forming composition") obtained by mixing a monomer component constituting an acrylic base polymer with a polymerization initiator. The monomer in the prepolymer-forming composition is preferably a monofunctional monomer such as a (meth)acrylic acid alkyl ester or a polar group-containing monomer among the monomer components constituting the acrylic polymer. The prepolymer-forming composition may contain a polyfunctional monomer. For example, a part of the polyfunctional monomer component that is the raw material of the base polymer may be contained in the prepolymer-forming composition, and the remaining part of the polyfunctional monomer component may be added after polymerization of the prepolymer to be subjected to the main polymerization.
[0094] The prepolymer forming composition may contain a chain transfer agent or the like as necessary in addition to the monomer and the polymerization initiator. The polymerization method of the prepolymer is not particularly limited, but from the viewpoint of adjusting the reaction time to set the molecular weight (polymerization rate) of the prepolymer in a desired range, polymerization by irradiation with active light such as UV light is preferred. The polymerization initiator and chain transfer agent used in the preliminary polymerization are not particularly limited, and for example, the above-mentioned photopolymerization initiator and chain transfer agent can be used.
[0095] The polymerization rate of the prepolymer is not particularly limited, but is preferably 3 to 50% by weight, more preferably 5 to 40% by weight, from the viewpoint of obtaining a viscosity suitable for application onto a substrate. The polymerization rate of the prepolymer can be adjusted to a desired range by adjusting the type and amount of photopolymerization initiator, the irradiation intensity and irradiation time of active light such as UV light, etc. The polymerization rate of the prepolymer is calculated from the weight before and after heating at 130°C for 3 hours using the following formula. The polymerization rate of the pressure-sensitive adhesive is also calculated using the same method. Polymerization rate (%) = weight after drying / weight before drying x 100
[0096] The prepolymer composition is mixed with the remaining monomer components constituting the acrylic base polymer (post-added monomer), and, if necessary, a polymerization initiator, a chain transfer agent, a silane coupling agent, a crosslinking agent, etc. to form a pressure-sensitive adhesive composition. The post-added monomer preferably contains a polyfunctional monomer. When a crosslinked structure is introduced by a urethane-based segment using urethane di(meth)acrylate, it is preferable to add urethane di(meth)acrylate as a post-added monomer.
[0097] The photopolymerization initiator and the chain transfer agent used in the main polymerization are not particularly limited, and for example, the above-mentioned photopolymerization initiator and the chain transfer agent can be used. When the polymerization initiator in the preliminary polymerization remains in the prepolymer composition without being deactivated, the addition of the polymerization initiator for the main polymerization can be omitted.
[0098] In the main polymerization, it is preferable to adjust the molecular weight by including a chain transfer agent in the pressure-sensitive adhesive composition. The chain transfer agent used in the main polymerization is not particularly limited, and for example, the above-mentioned chain transfer agents can be used. The amount of the chain transfer agent in the pressure-sensitive adhesive composition is preferably 0.001 to 2 parts by weight, more preferably 0.005 to 1 part by weight, and even more preferably 0.01 to 0.5 parts by weight, relative to 100 parts by weight of the base polymer constituents. In addition, when the chain transfer agent used in the preliminary polymerization remains in the prepolymer composition without being deactivated, the addition of the chain transfer agent to the pressure-sensitive adhesive composition may be omitted.
[0099] The chain transfer agent accepts radicals from the growing polymer chain to terminate the polymer growth, and the chain transfer agent that has accepted the radicals attacks the monomer to restart polymerization. By using a chain transfer agent, it is possible to suppress the increase in molecular weight of the polymer without decreasing the radical concentration in the reaction system.
[0100] When the ratio of monofunctional monomer to polyfunctional monomer is constant, the larger the molecular weight, the higher the probability that one polymer chain contains a crosslinking point (branching point) due to the polyfunctional monomer, and therefore the gel fraction tends to be larger. By using a chain transfer agent to suppress the elongation of the polymer, the molecular weight of the polymer tends to be smaller, and the increase in the gel fraction tends to be suppressed. Therefore, by including a chain transfer agent in the adhesive composition, an adhesive having a large tan δ and excellent step absorbency is easily formed.
[0101] (UV absorber) An ultraviolet absorbing agent may be used to impart ultraviolet absorbing properties to the adhesive layers 51 and 53. Examples of ultraviolet absorbing agents include benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, triazine-based ultraviolet absorbing agents, salicylate-based ultraviolet absorbing agents, and cyanoacrylate-based ultraviolet absorbing agents. Triazine-based ultraviolet absorbing agents and benzotriazole-based ultraviolet absorbing agents are preferred because they have high ultraviolet absorbing properties and excellent compatibility with acrylic polymers, and it is easy to obtain a highly transparent acrylic adhesive. Among these, triazine-based ultraviolet absorbing agents containing a hydroxyl group and benzotriazole-based ultraviolet absorbing agents having one benzotriazole skeleton in one molecule are preferred.
[0102] Commercially available products may be used as the ultraviolet absorber. Commercially available triazine-based ultraviolet absorbers include the reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hydroxyphenyl and [(alkyloxy)methyl]oxirane (BASF's "TINUVIN 400"), the reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and (2-ethylhexyl)-glycidic acid ester (BASF's "TINUVIN 405"), (2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (BASF's "TINUVIN 460"), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol (BASF's "TINUVIN 577"), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (BASF's "TINUVIN 479"), 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (BASF's "Tinosorb S"), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (ADEKA's "ADK STAB LA-46"), and the like.
[0103] Commercially available benzotriazole UV absorbers include 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF's "TINUVIN 928"), 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (BASF's "TINUVIN PS"), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (BASF's "TINUVIN 900"), and 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF's "TINUVIN 928"), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (BASF "TINUVIN 571"), 2-(2H-benzotriazol-2-yl)-p-cresol (BASF "TINUVIN P"), 2-(2H-benzotriazol-2-yl)-4-6-bis(1-methyl-1-phenylethyl)phenol (BASF "TINUVIN 234"), 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (BASF "TINUVIN 326"), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol (BASF "TINUVIN 328"), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF "TINUVIN 329"), benzenepropanoic acid and 3-(2H-benzotriazol-2-yl)-5-(1,Examples of such compounds include esters of 1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (BASF's "TINUVIN 384-2"), reaction products of methyl-3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate and polyethylene glycol (BASF's "TINUVIN 1 130"), reaction products of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol 300 (BASF's "TINUVIN 213"), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimido-methyl)-5-methylphenyl]benzotriazole (Sumitomo Chemical's "Sumisorb 250"), etc.
[0104] When an ultraviolet absorber is added to the pressure-sensitive adhesive composition, the amount added is usually about 0.05 to 10 parts by weight, and preferably 0.1 to 5 parts by weight, per 100 parts by weight of the base polymer. By setting the content of the ultraviolet absorber within the above range, it is possible to improve the ultraviolet shielding property of the pressure-sensitive adhesive layer while suppressing a decrease in transparency due to bleeding out of the ultraviolet absorber, etc.
[0105] (Oligomer) The pressure-sensitive adhesive composition may contain various oligomers for the purpose of adjusting the adhesive strength, viscosity, etc. As the oligomer, for example, one having a weight average molecular weight of about 1000 to 30000 is used. As the oligomer, an acrylic oligomer is preferable because it has excellent compatibility with the acrylic base polymer.
[0106] The acrylic oligomer contains an alkyl (meth)acrylate ester as a main constituent monomer component. Among them, those containing an alkyl (meth)acrylate ester having a chain alkyl group (chain alkyl (meth)acrylate) and an alkyl (meth)acrylate ester having an alicyclic alkyl group (alicyclic alkyl (meth)acrylate) as a constituent monomer component are preferred. Specific examples of the chain alkyl (meth)acrylate and the alicyclic alkyl (meth)acrylate are as exemplified above as the constituent monomers of the acrylic polymer.
[0107] The glass transition temperature of the acrylic oligomer is preferably 20°C or higher, more preferably 40°C or higher. The glass transition temperature of the acrylic oligomer may be 60°C or higher, 80°C or higher, 100°C or higher, or 110°C or higher. The adhesive retention of the pressure-sensitive adhesive tends to be improved by using a low Tg acrylic base polymer with a crosslinked structure introduced and a high Tg acrylic oligomer in combination. The upper limit of the glass transition temperature of the acrylic oligomer is not particularly limited, but is generally 200°C or lower, preferably 180°C or lower, and more preferably 160°C or lower. The glass transition temperature of the acrylic oligomer is calculated by the above-mentioned Fox formula.
[0108] Among the exemplified (meth)acrylic acid alkyl esters, methyl methacrylate is preferred as the chain alkyl (meth)acrylate because it has a high glass transition temperature and excellent compatibility with the base polymer. As the alicyclic alkyl (meth)acrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate, cyclohexyl acrylate, and cyclohexyl methacrylate are preferred. That is, the acrylic oligomer preferably contains, as a constituent monomer component, one or more selected from the group consisting of dicyclopentanyl acrylate, dicyclopentanyl methacrylate, cyclohexyl acrylate, and cyclohexyl methacrylate, and methyl methacrylate.
[0109] The amount of the alicyclic alkyl (meth)acrylate relative to the total amount of the monomer components constituting the acrylic oligomer is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, and even more preferably 30 to 70% by weight. The amount of the chain alkyl (meth)acrylate relative to the total amount of the monomer components constituting the acrylic oligomer is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, and even more preferably 30 to 70% by weight.
[0110] The weight average molecular weight of the acrylic oligomer is preferably from 1000 to 30000, more preferably from 1500 to 10000, and further preferably from 2000 to 8000. By using an acrylic oligomer having a molecular weight within this range, the adhesive strength and adhesive retention strength of the pressure-sensitive adhesive tend to be improved.
[0111] The acrylic oligomer can be obtained by polymerizing the above-mentioned monomer components by various polymerization methods. Various polymerization initiators may be used in the polymerization of the acrylic oligomer. In addition, a chain transfer agent may be used for the purpose of adjusting the molecular weight.
[0112] When the pressure-sensitive adhesive composition contains an oligomer component such as an acrylic oligomer, the content thereof is preferably 0.5 to 20 parts by weight, more preferably 1 to 15 parts by weight, and even more preferably 2 to 10 parts by weight, relative to 100 parts by weight of the base polymer. When the content of the oligomer in the pressure-sensitive adhesive composition is within the above range, the adhesiveness at high temperatures and the high-temperature holding power tend to be improved.
[0113] (Silane coupling agent) For the purpose of adjusting the adhesive strength, a silane coupling agent may be added to the adhesive composition. When a silane coupling agent is added to the adhesive composition, the amount added is usually about 0.01 to 5.0 parts by weight, and preferably about 0.03 to 2.0 parts by weight, per 100 parts by weight of the base polymer.
[0114] (Other additives) In addition to the above-exemplified components, the pressure-sensitive adhesive composition may contain additives such as a tackifier, a plasticizer, a softener, an anti-deterioration agent, a filler, a colorant, an antioxidant, a surfactant, and an antistatic agent.
[0115] <Formation of adhesive layer> When the adhesive composition is photocurable, the adhesive composition is applied onto a supporting substrate, and then photocured by irradiation with ultraviolet light and / or short-wavelength visible light to form an adhesive layer. When photocuring, it is preferable to attach a cover sheet to the surface of the coating layer and irradiate the adhesive composition with light while sandwiching the adhesive composition between the two sheets to prevent polymerization inhibition by oxygen.
[0116] Any suitable substrate may be used as the substrate and cover sheet used to form the adhesive layer. The substrate and cover sheet may be a release film having a release layer on the surface that contacts the adhesive layer. The transparent film substrate 59 of the adhesive sheet 15 may be used as the substrate or cover sheet.
[0117] Examples of methods for applying the pressure-sensitive adhesive composition include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.
[0118] The adhesive composition applied in a layer on the substrate is irradiated with actinic rays to carry out the main polymerization, in which the unreacted monomer components in the prepolymer composition react with the polyfunctional compound such as urethane di(meth)acrylate to obtain a polymer with a crosslinked structure.
[0119] The active light may be selected depending on the type of polymerizable component, the type of photopolymerization initiator, etc., and generally, ultraviolet light and / or short-wavelength visible light is used. The cumulative light amount of the irradiated light is 100 to 5000 mJ / cm. 2The light source for the light irradiation is not particularly limited as long as it can irradiate light in the wavelength range to which the photopolymerization initiator contained in the pressure-sensitive adhesive composition has sensitivity, and an LED light source, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a xenon lamp, etc. are preferably used. If a large amount of unreacted monomer remains, the G' of the pressure-sensitive adhesive layer becomes large. 25℃ The adhesion retention may decrease due to a decrease in the molecular weight of the adhesive. Therefore, the polymerization rate of the adhesive after the main polymerization is preferably 95% or more, more preferably 97% or more, even more preferably 98% or more, and particularly preferably 99% or more. In order to increase the polymerization rate, the adhesive layer may be heated to volatilize the remaining monomers, unreacted polymerization initiator, etc.
[0120] As described above, the gel fraction of the adhesive is preferably 30 to 80%, more preferably 35 to 70%. By having a gel fraction of 30% or more, the adhesive retention strength of the adhesive is increased, and the adhesive is less likely to have chipped glue or misaligned between members during processing, resulting in excellent processability and processing dimensional stability. In addition, by having a gel fraction of 80% or less, excellent step absorbency can be achieved.
[0121] The weight average molecular weight of the sol content of the adhesive is preferably 150,000 to 450,000, more preferably 180,000 to 420,000. The sol content is a soluble portion obtained by extracting the base polymer with tetrahydrofuran (hereinafter, THF). Since it is difficult to measure the molecular weight of each polymer chain of a crosslinked polymer (gel content), the molecular weight of the sol content (non-crosslinked polymer) is an index representing the degree of extension of the polymer chain. If the molecular weight of the sol content is excessively large, the glass transition temperature may increase and the impact resistance may decrease. On the other hand, if the molecular weight of the sol content is excessively small, the adhesive retention force may decrease.
[0122] <Preparation of double-sided adhesive sheet with substrate> A substrate-attached double-sided pressure-sensitive adhesive sheet is obtained by laminating first pressure-sensitive adhesive layer 51 and second pressure-sensitive adhesive layer 53 on the front and back of transparent film substrate 59. As described above, when forming the pressure-sensitive adhesive layer, a pressure-sensitive adhesive composition may be applied onto transparent film substrate 59 to form a laminate of the transparent film substrate and the pressure-sensitive adhesive layer.
[0123] By laminating release films 21, 23 to the surfaces of first pressure-sensitive adhesive layer 51 and second pressure-sensitive adhesive layer 53, a substrate-attached double-sided pressure-sensitive adhesive sheet with release films temporarily attached to both sides is obtained, as shown in Fig. 1. The release films used as the substrate or cover sheet when forming the pressure-sensitive adhesive layers may be used as release films 21, 23 as they are.
[0124] [Formation of image display device] As described above, the adhesive sheet 15 is suitably used for bonding the front transparent plate 7 to the viewing side surface of the image display panel 10 in the formation of an image display device. The order of bonding is not particularly limited, and the adhesive sheet 15 may be bonded to the image display panel 10 first, or the adhesive sheet 15 may be bonded to the front transparent plate 7 first. Moreover, the two may be bonded simultaneously. After bonding the second adhesive layer 53 and the polarizing plate 3, the polarizing plate 3 and the image display cell 6 may be bonded via the adhesive layer 4.
[0125] The substrate-attached double-sided pressure-sensitive adhesive sheet 15 can be used as a pressure-sensitive adhesive film in which the second pressure-sensitive adhesive layer 53 is fixed to an optical film such as a polarizing plate, in addition to the form in which release films are temporarily attached to the pressure-sensitive adhesive layers 51 and 53 as shown in Fig. 1. For example, in the form shown in Fig. 3, a release film 21 is temporarily attached to the surface of the first pressure-sensitive adhesive layer 51, and an optical film 3 is fixed to the second pressure-sensitive adhesive layer 53. In the form shown in Fig. 4, a pressure-sensitive adhesive layer 4 is further provided on the polarizing plate 3, and a release film 24 is temporarily attached thereon.
[0126] After the image display panel 10 and the front transparent plate 7 are bonded together via the adhesive sheet 15, pressure processing such as heat pressing and pressure bonding is performed. At this time, if there are partially thick protrusions such as FPC connection points, a large pressure is applied locally from the back surface side of the image display panel, deforming the image display panel 10. As described above, by bonding the image display panel 10 and the front transparent plate 7 together via the double-sided adhesive sheet 15 with a substrate, the plastic deformation of the adhesive sheet 15 is small and a restoring force against the deformation acts, so that the remaining impression caused by the pressure from the back surface side can be reduced. EXAMPLES
[0127] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0128] [Preparation of acrylic oligomer] 60 parts by weight of dicyclopentanyl methacrylate (DCPMA), 40 parts by weight of methyl methacrylate (MMA), 3.5 parts by weight of α-thioglycerol as a chain transfer agent, and 100 parts by weight of toluene as a polymerization solvent were mixed and stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) was added as a thermal polymerization initiator, and the mixture was reacted at 70°C for 2 hours, and then heated to 80°C and reacted for 2 hours. Thereafter, the reaction liquid was heated to 130°C, and the toluene, chain transfer agent, and unreacted monomers were dried and removed to obtain a solid acrylic oligomer. The weight average molecular weight of the acrylic oligomer was 5100.
[0129] [Preparation of prepolymer composition] <Prepolymer composition 1> As monomer components for forming a prepolymer, 70 parts by weight of butyl acrylate (BA), 17 parts by weight of N-vinyl-2-pyrrolidone (NVP), and 13 parts by weight of 4-hydroxybutyl acrylate (4HBA), as well as photopolymerization initiators (0.05 parts by weight of BASF's "Irgacure 184" and 0.05 parts by weight of BASF's "Irgacure 651") were mixed, and polymerization was carried out by irradiating with ultraviolet light until the viscosity (BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 20 Pa s, obtaining prepolymer composition 1 (polymerization rate: approximately 9%).
[0130] <Prepolymer composition 2> The monomer components for forming the prepolymer were changed to 2-ethylhexyl acrylate (2EHA): 68 parts by weight, NVP: 17 parts by weight, and 4-hydroxybutyl acrylate (4HBA): 17 parts by weight, and polymerization was carried out in the same manner as above, to obtain prepolymer composition 2.
[0131] [Preparation of photocurable adhesive composition] <Adhesive composition A> To 100 parts by weight of the above prepolymer composition 1, 2 parts by weight of polyester urethane diacrylate having a weight average molecular weight of 12,500 ("Art Resin UN-350" manufactured by Negami Chemical Industries), 5 parts by weight of the above acrylic oligomer, 0.05 parts by weight of "Irgacure 184" and 0.55 parts by weight of "Irgacure 651" as photopolymerization initiators, 0.07 parts by weight of α-methylstyrene dimer ("Nofumer MSD" manufactured by NOF Corp.) as a chain transfer agent, and 0.3 parts by weight of "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd. as a silane coupling agent were added, and these were then mixed uniformly to prepare adhesive composition A.
[0132] <Adhesive composition B> 0.70 parts by weight of an ultraviolet absorber (BASF's "Tinosorb S") was added, and 0.05 parts by weight of BASF's "Irgacure 184", 0.05 parts by weight of BASF's "Irgacure 651", and 0.40 parts by weight of BASF's "Irgacure 819" were added as photopolymerization initiators. Except for these changes, pressure-sensitive adhesive composition B was prepared in the same manner as pressure-sensitive adhesive composition A.
[0133] <Adhesive composition C> A pressure-sensitive adhesive composition C was prepared in the same manner as for the preparation of pressure-sensitive adhesive composition B, except that the amount of the chain transfer agent was changed to 0.03 parts by weight.
[0134] <Adhesive composition D> An adhesive composition D was prepared in the same manner as in the preparation of adhesive composition B, except that 0.1 parts by weight of hexanediol diacrylate (HDDA) was used as the polyfunctional monomer instead of polyester urethane diacrylate.
[0135] <Adhesive composition E> To 100 parts by weight of the above prepolymer composition 2, 0.1 part by weight of HDDA, 5 parts by weight of the above acrylic oligomer, 0.04 parts by weight of "Irgacure 184", 0.04 parts by weight of "Irgacure 651", and 0.12 parts by weight of "Irgacure 819" as photopolymerization initiators, and 0.3 parts by weight of a silane coupling agent were added, and then these were mixed uniformly to prepare adhesive composition E.
[0136] [Preparation of adhesive layer] <Adhesive layer A1> A 75 μm thick polyethylene terephthalate (PET) film with a silicone-based release layer on the surface was used as a substrate, and the above-mentioned photocurable adhesive composition was applied to the substrate to a thickness of 150 μm to form a coating layer. A 75 μm thick PET film with one side treated with silicone release was attached as a cover sheet to the coating layer. This laminate was laminated from the cover sheet side with an irradiation intensity of 5 mW / cm2 on the irradiation surface directly under the lamp. 2The adhesive layer was then photocured by irradiating it with ultraviolet rays using a black light whose position was adjusted so that the adhesive layer was in the range of 100 to 200 μm in thickness and 99% in polymerization rate.
[0137] <Adhesive layer A2~A4> Adhesive layers A2, A3, and A4 were prepared in the same manner as adhesive layer A1, except that the thickness of the adhesive layer was changed to 150 μm, 100 μm, and 70 μm.
[0138] <Adhesive layer B1~B4, C2, C3, D2, D3, E1~E3> Except for changing the type and thickness of the adhesive composition as shown in Table 1, adhesive layers were prepared in the same manner as for adhesive layer A1.
[0139] [Evaluation of adhesive layer] For each of the pressure-sensitive adhesive layers, the glass transition temperature, storage modulus, loss tangent, gel fraction and molecular weight of the sol fraction were measured by the following methods.
[0140] <Storage modulus, loss tangent and glass transition temperature> The release films (substrate and cover sheet) on both sides were peeled off and the adhesive layer was laminated to a thickness of about 1.5 mm to prepare a measurement sample. Dynamic viscoelasticity measurements were performed under the following conditions using Rheometric Scientific's "Advanced Rheometric Expansion System (ARES)". (Measurement conditions) Deformation mode: Torsion Measurement frequency: 1Hz Heating rate: 5℃ / min Shape: Parallel plate 7.9mmφ
[0141] From the measurement results, the shear storage modulus G' at 25°C 25℃ , and loss tangent tanδ at 70°C 70℃ The temperature at which the loss tangent (tan δ) became maximum (peak top temperature) was determined as the glass transition temperature of the pressure-sensitive adhesive layer.
[0142] <Gel fraction> About 0.2 g of adhesive was scraped off from the adhesive layer, wrapped in a porous polytetrafluoroethylene membrane ("NTF-1122" manufactured by Nitto Denko) with a pore diameter of 0.2 μm cut to a size of 100 mm × 100 mm, and the opening of the wrapping was tied with a string. The weight of the adhesive sample (B) was calculated by subtracting the total weight (A) of the porous polytetrafluoroethylene membrane and the string measured in advance from the weight of this sample. The adhesive sample wrapped in the porous polytetrafluoroethylene membrane was immersed in about 50 mL of ethyl acetate at 23 ° C for 7 days, and the sol component of the adhesive was eluted outside the porous polytetrafluoroethylene membrane. After immersion, the adhesive wrapped in the porous polytetrafluoroethylene membrane was taken out, dried at 130 ° C for 2 hours, and allowed to cool for about 20 minutes, and then the dry weight (C) was measured. The gel fraction of the adhesive was calculated by the following formula. Gel fraction (%) = 100 × (CA) / B
[0143] <Weight average molecular weight of sol content> Approximately 0.2 g of adhesive was scraped off from the adhesive layer and immersed in a 10 mM tetrahydrofuran phosphate solution for 12 hours to extract the sol content. The amount of tetrahydrofuran phosphate solution was adjusted so that the sol content of the solution after extraction was 0.1 wt%, taking into account the gel fraction of the adhesive. The filtrate obtained by filtering the solution after extraction through a 0.45 μm membrane filter was used as a sample and subjected to GPC (gel permeation chromatography) analysis using a Tosoh GPC device (product name "HLC-8120GPC") under the following conditions to calculate the weight average molecular weight Mw of the sol content. (Measurement conditions) Column: Tosoh Corporation, G7000HXL+GMHXL+GMHXL Column size: 7.8mmφ×30cm (total column length: 90cm) Column temperature: 40℃ Flow rate: 0.8mL / min Injection volume: 100μL Eluent: Tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene
[0144] Table 1 shows the composition and thickness of each pressure-sensitive adhesive layer (pressure-sensitive adhesive composition), as well as the evaluation results.
[0145] [Table 1]
[0146] [Example 1] Adhesive layer A2 was bonded to one main surface of a 50 μm thick cyclic olefin polymer (COP) film ("ZEONORFILM ZF16" manufactured by Zeon Corporation; front retardation 3 nm) as a first adhesive layer, and adhesive layer A3 was bonded to the other main surface as a second adhesive layer to produce a double-sided adhesive sheet with a film substrate in which adhesive layers were laminated on both sides of the film substrate.
[0147] [Example 2] A double-sided pressure-sensitive adhesive sheet with a film substrate was prepared in the same manner as in Example 1, except that a 50 μm-thick biaxially oriented polyethylene terephthalate (PET) film (Toray's "Lumirror S10"; front retardation 920 nm) was used as the film substrate.
[0148] [Examples 3 to 9, Comparative Examples 3 to 5] The type of film substrate and the type of adhesive layer were changed as shown in Table 2 to prepare double-sided adhesive sheets with a film substrate.
[0149] [Comparative Examples 1, 2, 6, 7] The single pressure-sensitive adhesive layers A1, B1, E1, and E3 were used as substrate-less pressure-sensitive adhesive sheets.
[0150] [evaluation] The pressure-sensitive adhesive sheets of the Examples and Comparative Examples were evaluated for adhesive strength, step absorbency, drop impact resistance, and impression by the following methods.
[0151] <Adhesive strength> The release film was peeled off from the second adhesive layer, a 50 μm thick PET film was attached, and the sample was cut to a width of 10 mm and a length of 100 mm. The release film was then peeled off from the first adhesive layer and pressed onto a glass plate with a 5 kg roller to prepare a sample for measuring adhesive strength. In Comparative Examples 1, 2, 6, and 7, which used a substrate-less single-layer adhesive sheet, the release film on one side was peeled off and a PET film was attached, and then the release film on the other side was peeled off and a glass plate was attached (the same applies to the other evaluations that follow).
[0152] The adhesive strength measurement sample was kept in an environment of 25°C for 30 minutes, and then the test piece was peeled from the glass plate using a tensile tester at a tensile speed of 300 mm / min and a peel angle of 180° to measure the peel strength.
[0153] <Haze> The release film was peeled off from the second adhesive layer and laminated to an 800 μm thick alkali-free glass (total light transmittance 92%, haze 0.4%), and the release film was peeled off from the first adhesive layer to obtain a test piece, which was then used to measure haze using a haze meter ("HM-150" manufactured by Murakami Color Research Laboratory). The haze of the adhesive sheet was determined by subtracting the haze of the alkali-free glass (0.4%) from the measured value.
[0154] <Gap absorption> The adhesive sheet was cut to a size of 75 mm x 45 mm, the release film was peeled off from the second adhesive layer, and the sheet was laminated to the center of a 125 μm thick PET film cut to 100 mm x 50 mm using a roll laminator (pressure between rolls: 0.2 MPa, feed rate: 100 mm / min). Then, the release film was peeled off from the first adhesive layer, and a 500 μm thick glass plate (100 mm x 50 mm) with black ink (printing thickness: 25 μm or 40 μm) printed in a frame shape on the periphery was laminated to the glass plate using a roll laminator (pressure between rolls: 0.2 MPa, feed rate: 100 mm / min). The ink printing area of the glass plate was 5 mm from both ends in the short side direction and 15 mm from both ends in the long side direction, and the black ink layer was in contact with the area 5 mm from the ends of the four sides of the adhesive sheet. After this sample was treated in an autoclave (50°C, 0.5 MPa) for 30 minutes, the vicinity of the boundary of the black ink printed area was observed with a digital microscope at a magnification of 20 times to confirm the presence or absence of air bubbles. The step absorbency of each sample with a black ink printing thickness of 25 μm and 40 μm was evaluated according to the following criteria. ◎: No air bubbles were observed around the entire circumference ○: Air bubbles were found in one of the four corners, but no air bubbles were found on any of the four sides. ×: Air bubbles are found in two or more of the four corners or one or more of the four sides.
[0155] <Impact resistance> The adhesive sheet was cut into a size of 75 mm x 45 mm, the release film was peeled off from the second adhesive layer, and the sheet was laminated to the center of a 500 μm thick glass plate (100 mm x 70 mm) using a roll laminator (roll pressure: 0.2 MPa, feed speed: 100 mm / min). Then, the release film was peeled off from the first adhesive layer, and a 500 μm thick glass plate (50 mm x 100 mm) with a 30 μm thick black ink printed in a frame shape on the periphery was laminated by vacuum pressure bonding (surface pressure 0.3 MPa, pressure 100 Pa). The ink printing area of the glass plate was 5 mm from both ends in the short side direction and 15 mm from both ends in the long side direction, and the black ink layer was in contact with the area 5 mm from the ends of the four sides of the adhesive sheet. This sample was treated in an autoclave (50 ° C, 0.5 MPa) for 30 minutes.
[0156] 5, both ends of the short side of the test sample 85 were placed on tables 83 arranged at an interval of 60 mm so that the glass plate 7 on which the printed layer 76 was provided was on the lower side, and the upper surface of the end of the glass plate 8 on which the printed layer was not provided was fixed to the table 83 with adhesive tape (not shown). The test sample 85 fixed to the table 83 with adhesive tape was kept in an environment of -5°C for 24 hours, and then, within 40 seconds after being taken out to room temperature, a metal ball 87 having a mass of 11 g was dropped onto the glass plate 7 from a height of 300 mm to perform an impact resistance test.
[0157] In the impact resistance test, a cylindrical guide 89 was used to keep the drop position of the metal ball constant, and a metal ball 87 was dropped at a position 10 mm away in both the short side and long side directions from the corners of the inner edge of the frame of the printed area of the printed layer 76. Two tests were performed, and a rating of ◯ was given to cases where the glass plate did not peel off in either test, and a rating of × was given to cases where the glass plate peeled off in either or both of the two tests.
[0158] <Indentation test> The release film was peeled off from the second adhesive layer, and the film was attached to a 50 μm thick PET film using a roll laminator (pressure between rolls: 0.2 MPa, feed rate: 100 mm / min). Then, the release film was peeled off from the first adhesive layer, and the film was attached to a 500 μm thick glass plate using a roll laminator (pressure between rolls: 0.2 MPa, feed rate: 100 mm / min). This sample was treated in an autoclave (50° C., 0.5 MPa) for 30 minutes.
[0159] Using SAICAS manufactured by Daipla Wintes, a steel ball indenter with a diameter of 1 mm was pressed into the PET film side of the above sample at a pressing speed of 5 μm / s until the vertical load reached 1 N, and after holding for 180 seconds, the indenter was lifted at a speed of 5 μm / s. Six hours after the test, the surface shape of the PET film was measured using a non-contact interference microscope (WYKO), and the depth of the indentation on the sample was determined and evaluated according to the following criteria. ◎: Depth of indentation is 3μm or less ○: Depth of indentation is greater than 3 μm and less than 4 μm ×: The depth of the indentation is greater than 4 μm
[0160] [Evaluation Results] The layer structure and evaluation results of each pressure-sensitive adhesive sheet are shown in Tables 1 and 2. The numbers in parentheses for the first pressure-sensitive adhesive layer, the film substrate, and the second pressure-sensitive adhesive layer in Table 2 are the thicknesses of each layer (unit: μm).
[0161] [Table 2]
[0162] The substrate-attached double-sided pressure-sensitive adhesive sheets of Examples 1 to 4, in which a relatively thicker pressure-sensitive adhesive layer was provided on the viewing side of the transparent film substrate and a relatively thinner pressure-sensitive adhesive layer was provided on the image display panel side of the transparent film substrate, exhibited excellent step absorbency and good characteristics, with little remaining imprints due to deformation when an indenter was pressed into the second pressure-sensitive adhesive layer side. On the other hand, the substrate-less double-sided pressure-sensitive adhesive sheet of Comparative Example 1, which was made of a 220 μm-thick pressure-sensitive adhesive layer A1, exhibited good step absorbency, but was prone to leaving imprints due to deformation when an indenter was pressed into the pressure-sensitive adhesive layer, resulting in poor imprint quality.
[0163] Similar trends were observed in comparing Examples 5 and 6, in which the adhesive composition was changed, with Comparative Example 2, and in comparing Example 9 with Comparative Example 6. Examples 7 and 8, in which the adhesive composition was changed, also showed good characteristics, such as excellent step absorbency and little residual pressure marks, like the other examples.
[0164] The substrate-attached double-sided adhesive sheets of Comparative Examples 3 to 5, in which a 220 μm-thick adhesive layer B1 was provided as a second adhesive layer on one main surface of the film substrate and relatively thinner adhesive layers B2, B3, B4 were provided as first adhesive layers on the other main surface of the film substrate, exhibited imprint defects, similar to the substrate-less adhesive sheet of Comparative Example 2 consisting of adhesive layer B2.
[0165] The substrate-less adhesive sheet of Comparative Example 7 consisting of an adhesive layer E3 with a thickness of 100 μm gave good results in the imprint test, but the adhesive sheet was poor in level difference absorbency due to its small thickness.
[0166] From the above results, it can be seen that by using a substrate-attached double-sided adhesive sheet having a relatively thick adhesive layer as the first adhesive layer on the viewing side of the transparent film substrate and a relatively thin adhesive layer as the second adhesive layer on the image display panel side of the transparent film substrate, it is possible to achieve excellent step absorption properties for printing steps in the front transparent plate and to suppress defects caused by pressure marks due to pressure from the image display panel side. [Explanation of symbols]
[0167] 51,53 Adhesive layer 21,23 Release film 59 Transparent film substrate 15 Double-sided adhesive sheet with substrate 3 Optical film (polarizing plate) 4 Adhesive layer 6 Image display cells 10 Image display panel 7 Front transparent plate 9 Reinforcement substrate 95 FPC 91 Main Board 92 Connector 201 Image display device
Claims
1. An image display device in which an image display panel and a front transparent plate arranged on a viewing side surface of the image display panel are bonded together via an adhesive sheet, the pressure-sensitive adhesive sheet comprises a transparent film substrate; a first pressure-sensitive adhesive layer bonded to a first main surface of the transparent film substrate; and a second pressure-sensitive adhesive layer bonded to a second main surface of the transparent film substrate, the first adhesive layer is bonded to the front transparent plate, and the second adhesive layer is bonded to the image display panel; the thickness of the first pressure-sensitive adhesive layer is greater than the thickness of the second pressure-sensitive adhesive layer, the second pressure-sensitive adhesive layer has an adhesive strength to glass of 2 N / 10 mm or more as determined by a peel test at a temperature of 25° C., a tensile speed of 300 mm / min, and a peel angle of 180°; The image display device, wherein the image display panel includes a touch sensor, and the front transparent plate does not include a touch sensor.
2. The image display device according to claim 1 , wherein the first pressure-sensitive adhesive layer has a thickness of 80 μm or more.
3. The image display device according to claim 1 , wherein the second pressure-sensitive adhesive layer has a thickness of 150 μm or less.
4. 4. The image display device according to claim 1, wherein the transparent film substrate has a thickness of 15 to 150 μm.
5. 5. The image display device according to claim 1, wherein the transparent film substrate has an in-plane retardation of 50 nm or less.
6. The image display device according to any one of claims 1 to 5, wherein the first pressure-sensitive adhesive layer has a shear storage modulus at a temperature of 25°C of 0.16 MPa or more.
7. The image display device according to any one of claims 1 to 6, wherein the first pressure-sensitive adhesive layer has a loss tangent at a temperature of 70°C of 0.25 or more.
8. The image display device according to any one of claims 1 to 7, wherein the first pressure-sensitive adhesive layer has a glass transition temperature of -3°C or lower.
9. The image display device according to any one of claims 1 to 8, wherein the first pressure-sensitive adhesive layer contains an acrylic polymer having a crosslinked structure.
10. The image display device according to claim 9, wherein the first pressure-sensitive adhesive layer has a gel fraction of 30 to 80%.
11. The image display device according to claim 9 , wherein the first pressure-sensitive adhesive layer has a polymerization rate of 95% or more.
12. 12. The image display device according to claim 9, wherein a crosslinked structure due to a urethane segment is introduced into the acrylic polymer.
13. The image display device according to any one of claims 1 to 12, wherein the first pressure-sensitive adhesive layer has an adhesive strength to glass of 2 N / 10 mm or more as determined by a peel test at a temperature of 25°C, a tensile speed of 300 mm / min, and a peel angle of 180°.
14. The image display device according to any one of claims 1 to 13, wherein the image display panel comprises a polarizing plate on a viewing side surface of an image display cell, the polarizing plate being attached to the second pressure-sensitive adhesive layer.
15. 15. The image display device according to claim 1, wherein the image display panel includes an organic EL cell.
16. The image display device according to claim 15 , wherein the organic EL cell comprises an electrode and an organic light-emitting layer on a resin film substrate.
Citation Information
Patent Citations
Double-sided pressure-sensitive adhesive tape
JP2009155503A
Double-sided pressure-sensitive adhesive tape for panel fixing
JP2012017386A
Double-sided adhesive sheet and touch panel display device containing the same
JP2014502292A
Pressure sensitive adhesive sheet and bonded body using the same
JP2016000774A
Adhesive sheet for optical use, polarizing film with adhesive layer, and liquid crystal display device
JP2017160416A