Glass shatter prevention sheet

The glass shatter prevention sheet with an uneven synthetic resin film and adhesive layer addresses the challenges of existing methods by providing effective glass protection and easy removal, ensuring safety and sunlight transmission during typhoons.

JP7555794B2Active Publication Date: 2024-09-25SEIREN CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020185672
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2020-11-06
Publication Date
2024-09-25
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

Existing glass shatter prevention methods, such as adhesive tapes and cardboard coverings, are either ineffective, time-consuming, or pose safety risks during typhoons, and removable adhesive tapes are difficult to peel off due to smooth surfaces.

Method used

A glass shatter prevention sheet with a synthetic resin film having an uneven surface and an acrylic or urethane adhesive layer, featuring protrusions and recesses to facilitate easy peeling and enhance adhesion, ensuring effective glass protection and ease of removal.

Benefits of technology

The sheet effectively prevents glass scattering during disasters by allowing easy peeling and reducing manual effort, maintaining sunlight transmission, and ensuring safety during and after the event.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555794000002
    Figure 0007555794000002
  • Figure 0007555794000003
    Figure 0007555794000003
  • Figure 0007555794000001
    Figure 0007555794000001
Patent Text Reader

Abstract

To provide a scattering prevention sheet capable of, in addition to an effect of preventing scattering of glass at the time of disaster such as typhoon or the like, easily floating an edge part that becomes a reason of peeling and easy to peel.SOLUTION: The glass scattering prevention sheet of the present invention is a glass scattering prevention sheet laminated with a synthetic resin film and an adhesive resin layer, and an uneven surface is formed on the surface of the synthetic resin film, and the adhesive resin layer is made of at least one resin selected from the group consisting of acrylic and urethane systems, and has an unevenness on the surface of the layer, and the convex height formed on the surface of the synthetic resin film is 10 μm or larger, and, a cross section of the convex is 6000 to 50000 μm2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet for preventing glass from shattering, which is temporarily attached to prevent glass from breaking and shattering due to a disaster such as a typhoon, and which can be easily removed. [Background technology]

[0002] During a typhoon, strong winds can blow debris into residential window glass, which can break and shatter, creating a dangerous situation. To avoid this danger, thin masking tape is temporarily applied in a grid or stripe pattern in preparation for a typhoon to prevent the glass from shattering and limit the damage from spreading if it does break. However, the shatter-proofing effect is not achieved in areas where the tape is not applied. Applying the tape to the entire surface is time-consuming and expensive, and is not suitable for preparing for imminent situations before a typhoon. Another method is to cover the entire window glass by taping the edges of cardboard, but this blocks sunlight from entering the window, making the room dark and dangerous in the event of a power outage.

[0003] Additionally, adhesive sheets that can be affixed to the entire window glass to prevent glass from shattering are commercially available, but because they are designed to be left in place, they have strong adhesive properties and cannot be repositioned, meaning they cannot be removed after the typhoon has passed.

[0004] Therefore, a removable adhesive tape for preventing glass shattering that can be easily removed after a typhoon has passed has been proposed in Patent Document 1. However, such a smooth adhesive tape is difficult to remove because there is no catch, and a considerable amount of finger strength is required to manually remove the adhesive tape that has been applied to a wide area of ​​window glass. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-17835 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above-mentioned problems, and relates to a sheet for preventing glass from shattering, which not only has the effect of preventing glass from shattering during disasters such as typhoons, but also has edges that are easy to lift and peel off when peeled off. [Means for solving the problem]

[0007] The present invention relates to a glass shatterproof sheet in which a synthetic resin film and an adhesive resin layer are laminated, and the synthetic resin film has a surface irregularity formed thereon, the adhesive resin layer is made of at least one resin selected from the group consisting of acrylic and urethane resins, and the layer surface has a surface irregularity formed thereon, the height of the protrusions formed on the surface of the synthetic resin film is 10 μm or more, and the cross-sectional area of ​​the protrusions is 6000 to 50000 μm. 2 This is a glass shatterproof sheet. The adhesive strength of the adhesive resin layer to glass is preferably 0.90 to 1.80 N / 25 mm. Effect of the Invention

[0008] According to the present invention, in addition to the effect of preventing glass from shattering in the event of a disaster such as a typhoon, it is possible to provide a glass shatterproof sheet in which the surface of the synthetic resin film and the surface of the adhesive resin layer are uneven, making it easy to lift the edge that triggers peeling, and which is easy to peel off because a fine gap is formed between the glass and the sheet, so that resistance when peeling is weak. Also, when attaching the sheet to a window glass, the unevenness on the surface of the adhesive resin layer makes it easy to release air pockets, making the attachment work easy. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic cross-sectional view showing a glass shatterproof sheet according to an embodiment of the present invention. [Diagram 2] 1 is a schematic enlarged cross-sectional view showing the concept of the cross-sectional area of ​​a convex portion of a glass shatterproof sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The glass shatterproof sheet of the present invention will be described below with reference to the drawings. However, the present invention is not intended to be limited to the configuration described below. In the drawings, layers constituting the glass shatterproof sheet of the present invention are illustrated, but the thickness and size of each layer are appropriately changed to facilitate explanation, and do not accurately reflect the actual thickness size relationship (scale).

[0011] 1, the adhesive sheet 1 for preventing glass from shattering of the present invention is formed by laminating a synthetic resin film 2 and an adhesive resin layer 3, with unevenness formed on the surface of the synthetic resin film 2, and also on the surface of the adhesive resin layer 3, i.e., the adhesive surface to be bonded to glass. In one embodiment, the adhesive sheet is used by attaching the surface of the adhesive resin layer 3 to a window glass 4.

[0012] As the synthetic resin film 2, other synthetic resins such as polyester, polyvinyl chloride, polyethylene, polypropylene, polycarbonate, etc. can be used, but polyethylene is preferred in terms of film strength, economy, post-use disposal, and ease of forming unevenness. In addition, a colorless or colored translucent or transparent film is preferred to allow sunlight into the room, and specifically, a light transmittance of 70% or more for the visible light wavelength range of 400 to 700 nm is preferred. If the transmittance is less than 70%, the room will be dark because insufficient sunlight will enter the room, and if a power outage occurs due to a typhoon, there is a risk of injury even indoors.

[0013] Furthermore, the shape of the projections and recesses formed on the surface of the synthetic resin film 2 is not limited as long as it allows easy peeling. For example, the shape may be a regular shape such as a lattice, dots, or stripes, or a random shape such as letters or symbols. The projections and recesses formed on the synthetic resin film 2 can be formed by various methods, but embossing is preferred from the standpoint of ease of processing and economic efficiency.

[0014] The unevenness formed on the synthetic resin film 2 is such that the cross-sectional area of ​​the protrusions 5 is 6000 to 50000 μm 2 The height of the protrusions 5 is designed to be 10 μm or more. The height of the protrusions 5 is preferably 35 μm or more. The cross-sectional area of ​​the protrusions 5 is preferably 6000 μm or more. 2 If the cross-sectional area of ​​the protrusions 5 is less than 50,000 μm or the height of the protrusions 5 is less than 10 μm, it becomes difficult to lift the end portion, which serves as a trigger for peeling. 2 If it is larger, even if you try to press it with your hand to make it stick to the window glass when attaching it, the convex parts will hinder the sheet from adhering sufficiently, causing wrinkles, and the wrinkled parts will not be able to achieve shatterproof performance and may be easily peeled off by strong winds. The cross-sectional area of ​​the convex parts 5 is determined by placing the glass shatterproof sheet 1 on a flat surface, observing the cross-section of the glass shatterproof sheet with an electron microscope (magnification: 100 times), and averaging the values ​​measured for the cross-sectional areas 6 (areas surrounded by dotted lines in Figure 2) of 20 randomly selected convex parts 5. The height of the convex parts 5 is determined by observing the cross-section with an electron microscope (magnification: 100 times), and averaging the values ​​measured for the heights of 20 randomly selected convex parts.

[0015] The thickness of the synthetic resin film 2 is preferably 50 to 200 μm. If it is less than 50 μm, the film may break when the window glass breaks, making it difficult to obtain shatterproof effects, and if it is thicker than 200 μm, it is too heavy and may cause injury if the worker loses balance during work. The thickness is determined by observing the cross section with an electron microscope (magnification: 100 times) and averaging the values ​​measured at 20 randomly selected points. The synthetic resin film 2 can be formed by an inflation method or a T-die method, but the T-die method is preferred from the viewpoint of ease of forming projections and recesses.

[0016] An adhesive resin layer 3 is laminated on the back surface of a synthetic resin film 2 to produce an adhesive sheet 1 for preventing glass from scattering. It is preferable to subject the back surface onto which the adhesive resin layer 3 is laminated to a known treatment method such as corona discharge treatment or plasma surface treatment, since this makes it easier to apply the adhesive resin layer 3. Furthermore, corona discharge treatment is preferable because it is highly effective in roughening and activating the surface.

[0017] The adhesive resin layer 3 can be made of at least one resin selected from the group consisting of acrylic and urethane resins, which is easy to attach to the window glass, is not easily affected by rain, and is unlikely to leave any adhesive residue on the window glass when peeled off after use. When durability against wind and rain is more important, acrylic resins are preferred. When ease of peeling is more important, urethane resins are preferred.

[0018] In addition, the adhesive strength of the adhesive resin layer of the glass shatterproof sheet to glass is preferably 0.90 to 1.80 N / 25 mm. If it is less than 0.90 N / 25 mm, it may peel off when exposed to strong winds and rain, and shatterproof performance may be difficult to obtain. If it is stronger than 1.80 N / 25 mm, there is resistance when peeling it off, making it difficult to work with, and there is a risk that the window glass may come off from the frame or break. The adhesive strength is measured according to JIS A5759 6.9 Adhesion Test 6.9.3 Test Method a) 180° Peel Test after the glass shatterproof sheet is attached by hand.

[0019] When an acrylic resin is used, examples of the resin include a homopolymer (main monomer) having an acrylic acid ester as the main monomer unit, and an acrylic copolymer selected from a copolymer with a comonomer. If necessary, a crosslinking agent such as an isocyanate, amine, or acid anhydride, or an adhesion improver such as a petroleum resin, a phenolic resin, a rosin resin, or a silane coupling agent can be added. On the other hand, urethane resins are generally obtained by reacting polyols with polyisocyanate compounds. Examples of polyols include polyether polyols, polyester polyols, polycarbonate polyols, and polycaprolactone polyols. Examples of polyisocyanate compounds include diphenylmethane diisocyanate, tolylene diisocyanate, and hexamethylene diisocyanate. If necessary, adhesion improvers such as petroleum resins, phenolic resins, rosin resins, and silane coupling agents can be added.

[0020] In order to let sunlight into the room, a colorless or colored, translucent or transparent adhesive is preferable, and specifically, the light transmittance of the visible light wavelength region of 400 to 700 nm is preferably 70% or more. If it is less than 70%, the room will be dark because not enough sunlight will enter the room, and if there is a power outage due to a typhoon, there is a risk of injury even indoors.

[0021] The method for laminating the adhesive resin layer 3 may be a conventionally known method, and is not particularly limited. For example, a method may be used in which an adhesive resin dissolved in a solvent is coated onto the synthetic resin film 2 using a gravure coating method, a roll coating method, a knife coating method, a bar coating method, or the like, and then the adhesive resin is heated to evaporate the solvent.

[0022] The thickness of the adhesive resin layer 3 is preferably 10 to 30 μm. If it is less than 10 μm, the adhesive strength obtained is low and it may peel off in strong winds and rain. If it is thicker than 30 μm, it will fill the shape of the recesses on the back surface, making it difficult to peel off from the window glass and there is a risk that the adhesive will remain on the glass. The thickness is determined by observing the cross section with an electron microscope (magnification: 100 times) and averaging the values ​​measured at 20 randomly selected points.

[0023] In the glass shatterproof sheet 1 of the present invention, unevenness is formed on the surface of the synthetic resin film 2, and further unevenness is formed on the surface of the adhesive resin layer 3. In detail, convex parts 5 are formed on the surface side of the synthetic resin film 2, and it is preferable that concave parts 7 smaller than the convex parts 5 on the surface side are formed on the surface opposite to the convex parts, i.e., the surface of the adhesive resin layer 3. If the concave parts 7 on the surface of the adhesive resin layer 3 are large, the area in contact with the glass 4 becomes small, and there is a risk of peeling or the shatterproof effect not being obtained. Furthermore, the adhesion strength with the glass is easily affected by the way the sheet is pressed when attached, so there is a risk of the effect varying depending on the installer.

[0024] The depth of the recesses in the adhesive resin layer 3 is preferably 7 μm or more. If it is less than 7 μm, the adhesion to the window glass will be nearly the entire surface, making it difficult to peel off from the window glass after use, and air that has entered during the application process will be difficult to escape, making it difficult to obtain shatterproof performance in the area where air has entered. The recess depth is determined by observing the cross section with an electron microscope (magnification: 100 times) and averaging the values ​​measured for the depth of 20 randomly selected recesses.

[0025] It is preferable to form the unevenness so that when the adhesive resin layer 3 is attached to the glass 4, the proportion of the area where the adhesive resin layer is attached, i.e., the adhesion area rate, is 70 to 90%. If it is less than 70%, there is a risk that it may peel off or the shatterproof effect may not be obtained. If it exceeds 90%, air is trapped during the attachment work and the layer is likely to wrinkle, and the part with air trapped therein does not easily obtain shatterproof performance, and it is also difficult to peel off from the window glass.

[0026] To form the convex portions 5 on the surface of the synthetic resin film 2 and further form the concave portions 7 on the surface of the adhesive resin layer 3, the following manufacturing method may be used.

[0027] For example, there is a method in which the synthetic resin film 2 is embossed after or simultaneously with the molding, and then the adhesive resin layer 3 is laminated. The case of embossing after molding of the synthetic resin film 2 will be described in detail. The synthetic resin film 2 is embossed by passing it between a cooling roll engraved with unevenness and an elastic roll whose surface is made of an elastic body while being pressurized, and then the adhesive resin layer 3 is laminated by the above-mentioned method. In the case of embossing simultaneously with the molding of the synthetic resin film 2, when the molten resin is molded into a film shape and cooled, it is embossed by passing it between a cooling roll engraved with unevenness and an elastic roll, and then the adhesive resin layer 3 is laminated. From the viewpoints of economy and processability, the method of embossing simultaneously with molding is preferable. The elastic body of the elastic roll can be natural rubber, chloroprene rubber, nitrile rubber, or silicone rubber, but it is preferable to use silicone rubber in terms of heat resistance and abrasion resistance.

[0028] Furthermore, the size of the protrusions 5 can be formed to any desired size by adjusting the depth of the depressions engraved on the cooling roll and by adjusting the pressure applied by the cooling roll and the elastic roll. Furthermore, to form recesses 7 on the back side that are smaller than the protrusions 5 on the front side, molding is performed with the cooling roll side engraved with the recesses and protrusions as the front side and the elastic roll side as the back side. In order to make the recesses 7 smaller, a roll with high hardness is used as the elastic roll. If the hardness is low, the elastic roll will also deform to match the recesses and protrusions of the cooling roll, making it easier for the recesses 7 on the back side to become large. If the hardness is high, the elastic roll will also be less likely to deform, making it easier for small recesses 7 to be formed. The size of the protrusions 5 and recesses 7 can be adjusted by adjusting the hardness of the elastic roll and the pressure applied to the cooling roll and elastic roll.

[0029] The glass shatterproof sheet 1 preferably has a light transmittance of 70% or more for the wavelength of 400 to 700 nm. If the light transmittance is less than 70%, sufficient sunlight will not enter the room, making it dark, and if a power outage occurs due to a typhoon, there is a risk of injury even indoors. EXAMPLES

[0030] The glass shatterproof sheet of the present invention will be specifically described with reference to the following examples and comparative examples, but the present invention is not limited thereto. Measurements and evaluations of physical properties in the examples and comparative examples were carried out by the following methods.

[0031] <Cross-sectional area of ​​convex part> The cross section of the glass shatterproof sheet when placed on a flat surface was observed under an electron microscope (magnification: 100x), and the cross-sectional areas of 20 randomly selected protrusions were measured and averaged.

[0032] <Adhesive strength of adhesive resin layer> JIS A5759 6.9 Adhesive strength test 6.9.3 Test method a) The adhesive strength of the adhesive resin layer of the glass shatterproof sheet was measured according to the 180° peel test. The glass shatterproof sheet was attached by pressing the entire sheet with hands without using any tools.

[0033] <Glass shatterproof performance> The glass shatterproof sheet cut to a width of 840 mm and a length of 1906 mm was attached to a plate glass with a width of 864 mm and a length of 1930 mm and a nominal thickness of 5 mm, with the center aligned, pressed by hand, and left to stand for 4 days in the test environment of JIS A5759 6.1.1. The number of test pieces was 4. A shot bag test was conducted using a test device conforming to JIS A5759 6.11.2 and a test method conforming to JIS A5759 6.11.3. If the glass shatterproof performance against impact breakage specified in JIS A5759 5.4h)1) was met, it was marked as ◯, and if it was not met, it was marked as ×.

[0034] <Evaluation of peeling: Ease of peeling the sheet> In the same manner as in the glass shatterproof performance test, the sheet was applied to glass and then peeled off by hand, and a sensory evaluation was conducted on the ease of gripping the sheet and the burden of peeling it off. The evaluation criteria were as follows, and the results were averaged by 10 female testers in their 30s to 50s. ○: There is an opening for peeling, the sheet is easy to grasp, and the burden of peeling is small. △: There is an opportunity to peel it off, but it is a little difficult to grasp the sheet and there is a little strain in peeling it off. ×: There was no trigger for peeling, making it difficult to grasp the sheet and causing a large burden to peel it off.

[0035] [Example 1] Molten polyethylene was molded into a film and passed between a cooling roll engraved with a grid of square pyramidal depressions with sides of 1.0 mm and an elastic roll to form convex portions on the surface of the polyethylene film (Hayashi Ichiji Co., Ltd., High Grain Film Natural L-LDPE). A mixture of 100 parts by mass of acrylic adhesive (Lion Specialty Chemicals Co., Ltd., AS-415) and 4.5 parts by mass of isocyanate crosslinking agent (Lion Specialty Chemicals Co., Ltd., B-45) was added to the film by roll coating to a thickness of 20 μm, laminating an adhesive resin layer and obtaining a glass shatterproof sheet as shown in Figure 1. The polyethylene film was 100 μm thick and the cross-sectional area of ​​the convex portions was 24753 μm. 2The measurement results and evaluation results of each physical property are shown in Table 1.

[0036] [Example 2] The cross-sectional area of ​​the convex part is 46488μm 2 A glass shatterproof sheet was obtained by processing in the same manner as in Example 1, except that the depth of the indentations engraved on the cooling roll was adjusted and formed so as to become 100%. The measurement results and evaluation results of each physical property are shown in Table 1.

[0037] [Example 3] Convex cross-sectional area: 7063μm 2 A glass shatterproof sheet was obtained by processing in the same manner as in Example 1, except that the depth of the indentations engraved on the cooling roll was adjusted and formed so as to become 100%. The measurement results and evaluation results of each physical property are shown in Table 1.

[0038] [Example 4] A glass shatterproof sheet was obtained in the same manner as in Example 1, except that the adhesive was a mixture of 100 parts by mass of a urethane adhesive (Vinezone U-250, manufactured by Lion Specialty Chemicals Co., Ltd.) and 3.7 parts by mass of an isocyanate crosslinking agent (B-45, manufactured by Lion Specialty Chemicals Co., Ltd.). The measurement results and evaluation results of each physical property are shown in Table 1.

[0039] [Comparative Example 1] Convex cross-sectional area: 96μm 2 A glass shatterproof sheet was obtained by processing in the same manner as in Example 1, except that the composition was adjusted and molded so that the thickness was 100 μm or more. The measurement results and evaluation results of each physical property are shown in Table 1.

[0040] [Comparative Example 2] Convex cross-sectional area: 127406μm 2 A glass shatterproof sheet was obtained by processing in the same manner as in Example 1, except that the composition was adjusted and molded so that the thickness was 100 μm or more. The measurement results and evaluation results of each physical property are shown in Table 1.

[0041] [Comparative Example 3] Table 1 shows the measurement and evaluation results of each physical property of a window film for buildings (Wincos, Architectural Film 1501UH, manufactured by Lintec Corporation) made of a polyester film coated with an acrylic adhesive.

[0042] [Table 1]

[0043] As shown in Table 1, the glass shatterproof sheets according to the examples had glass shatterproof performance, low peeling resistance, and were easy to peel off. In contrast, the glass shatterproof sheets according to the comparative examples had poor glass shatterproof performance or were difficult to peel off because of high peeling resistance. [Explanation of symbols]

[0044] 1. Glass shatterproof sheet 2. Synthetic resin film 3 Adhesive resin layer 4. Glass 5 Convex 6. Convex cross-sectional area 7 Recess

Claims

1. A glass shatterproof sheet having a synthetic resin film and an adhesive resin layer laminated thereon, The synthetic resin film has a surface having irregularities formed thereon, the adhesive resin layer is made of at least one resin selected from the group consisting of acrylic and urethane resins, and has an uneven surface; The height of the protrusions formed on the surface of the synthetic resin film is 10 μm or more, and the cross-sectional area of ​​the protrusions is 6,000 to 50,000 μm. 2 This is a sheet to prevent glass from shattering.

2. 2. The glass shatterproof sheet according to claim 1, wherein the adhesive resin layer has an adhesive strength with glass of 0.90 to 1.80 N / 25 mm.

Citation Information

Patent Citations

  • JP1975156560U

  • Strippable, pressure-sensitive adhesive tape roll for prevention of breaking and scattering of glass

    JP1998017835A

  • Film for scattering prevention and method for producing the same

    JP2009255351A

  • Scattering prevention sheet, el element equipped with the same, and el light-emitting device equipped with the el element as light-emitting source

    JP2011082032A

  • Window sticking film

    JP2015098119A