Cu-P co-supported zeolite, and selective reduction catalyst and exhaust gas catalyst using the same
By post-treating small-pore zeolites with phosphoric acid and an organic base, the Cu-P co-supported zeolite addresses the challenge of synthesizing zeolites with low silica-alumina ratios, achieving high thermal durability and effective catalytic performance for nitrogen oxide reduction.
Patent Information
- Application Number
- JP2020553252
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-26
- Filing Date
- 2019-10-16
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2039-10-16
AI Technical Summary
Existing methods struggle to synthesize small-pore zeolites with low silica-alumina ratios that exhibit high thermal durability and can support a large amount of catalytic metals, and the pre-blending of phosphorus with zeolites reduces ion exchange points, limiting the effectiveness of catalyst metals like copper.
A method involving the post-treatment of small-pore zeolites with a phosphoric acid and organic base solution to support extra-skeletal copper and phosphorus atoms, allowing for high thermal durability and catalytic performance by maintaining ion exchange points for copper.
The Cu-P co-supported zeolite achieves excellent thermal durability and catalytic performance, particularly in nitrogen oxide reduction, maintaining high reduction rates even in high-temperature environments.
Smart Images

Figure 0007555819000001 
Figure 0007555819000002 
Figure 0007555819000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel Cu-P co-supported zeolite, and a selective reduction catalyst and an exhaust gas catalyst using the same. [Background technology]
[0002] Zeolites have a skeletal structure with regular and uniform pore sizes, and are widely used industrially for various applications such as drying agents, dehydrating agents, adsorbents or separators for various inorganic or organic molecules that utilize differences in polarity or molecular diameter, ion exchangers, petroleum refining catalysts, petrochemical catalysts, and solid acid catalysts. The skeletal structures of various zeolites are compiled into a database by the International Zeolite Association (hereinafter sometimes abbreviated as "IZA"), and there are currently more than 200 types of zeolite skeletal structures. However, only about 10 types of zeolites are used industrially.
[0003] Zeolites are aluminosilicate crystalline materials having relatively uniform pore sizes, typically about 3-10 Angstroms in diameter, depending on the type of zeolite and the amount of cations contained in the zeolite lattice. Both synthetic and natural zeolites and their use to promote certain reactions, including the selective reaction of nitric oxide with ammonia in the presence of oxygen, are known in the art.
[0004] Also known are metal-promoted zeolite catalysts, in particular iron-promoted and copper-promoted zeolite catalysts, for selective catalytic reduction of nitrogen oxides with ammonia. Copper-promoted zeolite beta is one of the effective catalysts for selective reduction of nitrogen oxides with ammonia. For example, Patent Document 1 discloses a method for reducing nitrogen oxides (hereinafter sometimes referred to as "NOx") contained in a gas stream using Cu-supported zeolite, which exhibits good hydrothermal stability.
[0005] Furthermore, Non-Patent Document 1 describes a method of post-treating zeolite with a phosphoric acid compound in order to increase the durability and catalytic activity as a catalyst. In Non-Patent Document 1, it is discovered that by supporting phosphoric acid or diammonium hydrogen phosphate on MFI zeolite (largest pore: oxygen 10-membered ring medium-pore zeolite) and protecting the Al site, which has a relatively low heat resistance, before calcining, the heat resistance is improved and the catalytic activity in the n-butane cracking reaction after hydrothermal durability is increased compared to an untreated product.
[0006] However, Non-Patent Document 2 reports that in zeolites (small pore zeolites) whose maximum pore size is an 8-membered oxygen ring, such as CHA-type zeolites, post-treatment with a phosphoric acid compound as described in Non-Patent Document 1 above is ineffective. This is probably because the molecular diameter of phosphoric acid (about 4 Å) is larger than the pore size of small pore zeolites (CHA-type: about 3.8 Å), making it difficult for phosphoric acid to penetrate into the pores of zeolites. Non-Patent Document 3 also describes that no improvement in heat resistance was observed even when phosphoric acid-unmodified zeolites were phosphorus-modified by impregnation with diammonium hydrogen phosphate, and describes that post-treatment of zeolites using phosphoric acid compounds is ineffective in small pore zeolites.
[0007] Therefore, in small pore zeolites such as CHA-type zeolites, as shown in Patent Document 2, it has been considered to improve hydrothermal stability by adding a phosphorus compound during the synthesis of CHA-type zeolite to introduce a small amount of phosphorus atoms into the CHA framework, for example by replacing some of the framework T atoms with phosphorus atoms, thereby synthesizing a phosphorus T-atom-containing, low-phosphorus molecular sieve.
[0008] Furthermore, as shown in Patent Document 3, a method has been investigated in which a phosphonium cation is made to coexist with the ammonium cation of OSDA during synthesis, thereby incorporating phosphorus outside the framework of CHA-type zeolite, i.e., as a non-T atom, without introducing phosphorus atoms into the CHA framework containing Si and Al of CHA-type zeolite. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Special Publication No. 2010-519038 [Patent Document 2] Patent No. 6320918 [Patent Document 3] JP 2017-048106 A [Non-patent literature]
[0010] [Non-Patent Document 1] T. Blasco et al., J. Catal., 237 (2006) 267-277 [Non-Patent Document 2] February 28, 2018 "Synthesis of durable zeolite and its application to SCR catalysts" Yoji Sano, Automotive Engineers of Japan Symposium Proceedings p.43 - 47 [Non-Patent Document 3] Yoji Sano, Nao Tsunoji, Catalysts, 60 (2018) 240-246 Summary of the Invention [Problem to be solved by the invention]
[0011] However, the method described in Patent Document 2 aims to realize a phosphorus T atom-containing low phosphorus molecular sieve with a silica to alumina ratio of about 12 to 32 as shown in Table 1, but in reality, as shown in Tables 2 and 3, only CHA type zeolite with a high silica to alumina ratio of about 40 can be realized, and it is considered difficult to synthesize a zeolite with a low silica to alumina ratio that can contain more catalytic metals by this method. Moreover, even if such a zeolite with a low silica to alumina ratio can be synthesized, it is considered difficult to give it high thermal durability.
[0012] In addition, the method described in Patent Document 3 also aims to realize a CHA-type zeolite having a silica-to-alumina ratio of about 16 to 100, but in reality, as shown in Tables 1 and 2, only CHA-type zeolites with a high silica-to-alumina ratio of 22 to 24 have been realized, and it is difficult to synthesize a zeolite with a low silica-to-alumina ratio that can contain more catalytic metals by this method. Furthermore, it is unclear whether such a zeolite with a low silica-to-alumina ratio can be given high thermal durability. Moreover, the method described in Patent Document 3 requires the use of a relatively expensive phosphonium compound as a raw material, and there is a lot of room for improvement in terms of production costs and production processes.
[0013] Moreover, in the methods of Patent Documents 2 and 3, phosphorus is added before the catalytic metal such as copper is supported on the zeolite surface, so that some of the ion exchange points based on Al in the zeolite framework are protected by the phosphorus added in advance. Such protected sites cannot act as ion exchange points for copper, and as a result, sufficient ion exchange ability cannot be exhibited when the catalytic metal such as copper is supported on the zeolite surface, and as a result, a large amount of catalytic metal cannot be supported. Therefore, the methods of Patent Documents 2 and 3 are insufficient in improving NOx purification performance after hydrothermal durability as expected.
[0014] The present invention has been made in view of the above problems, and an object of the present invention is to provide a high-performance Cu-P co-supported zeolite having excellent thermal durability and catalytic performance, in which extraskeletal copper atoms and extraskeletal phosphorus atoms are supported on a small pore zeolite. Another object of the present invention is to provide a selective reduction catalyst molded body and an exhaust gas catalyst, which are excellent in catalytic performance and which use the high-performance Cu-P co-supported zeolite.
[0015] In addition to the objectives stated here, the present invention can also be positioned as another objective of achieving effects that are derived from the various components shown in the description of the embodiments of the invention described below, and that cannot be obtained by conventional techniques. [Means for solving the problem]
[0016] As a result of intensive research to solve the above problems, the present inventors have found that a specific Cu-P co-supported zeolite, in which extraskeletal copper atoms and extraskeletal phosphorus atoms are supported on a small pore zeolite, has excellent thermal durability and catalytic performance, and have completed the present invention. That is, the present invention provides various specific embodiments as shown below.
[0017] <1> The present invention comprises at least a small pore zeolite and an extra-framework copper atom and an extra-framework phosphorus atom supported on the small pore zeolite, The silica-alumina ratio (SiO2 / Al2O3) is 7 or more and 20 or less, The ratio of copper atoms to T atoms (Cu / T) is 0.005 or more and 0.060 or less, The ratio of phosphorus atoms to T atoms (P / T) is 0.005 or more and 0.060 or less, The ratio of phosphorus atoms to copper atoms (P / Cu) is 0.1 or more and 3 or less; Cu-P co-loaded zeolite.
[0018] <2> The small pore zeolite has an 8-membered oxygen ring structure. the above <1> The Cu-P co-supported zeolite described in . <3> The small pore zeolite has at least one framework structure selected from the group consisting of CHA, AEI, and ERI, as determined by powder X-ray diffraction measurement. the above <1> or <2> The Cu-P co-supported zeolite described in . <4> The small pore zeolite has a crystallite size of 10 nm or more and 50 nm or less as measured by powder X-ray diffraction. the above <1> ~ <3> The Cu-P co-supported zeolite according to any one of the above. <5> The small pore zeolite has a crystallite size of 15 nm or more and 100 nm or less as measured by powder X-ray diffraction. the above <1> ~ <3> The Cu-P co-supported zeolite according to any one of the preceding claims. <6> Average particle size D between 0.01μm and 20μm 50 have the above <1> ~ <5> The Cu-P co-supported zeolite according to any one of the preceding claims.
[0019] <7> the above <1> ~ <6> The present invention comprises at least the Cu-P co-supported zeolite according to any one of the above claims. Selective reduction catalyst. <8> the above <1> ~ <6> A composition comprising the Cu-P co-supported zeolite according to any one of claims 1 to 5, which is formed into a predetermined shape. Selective reduction catalyst molded body. <9> The present invention comprises at least a support and a catalyst layer provided on at least one surface of the support, The catalyst layer is <1> ~ <6> The present invention is characterized by containing at least the Cu-P co-supported zeolite according to any one of the above. Exhaust gas catalyst. Effect of the Invention
[0020] According to the present invention, a high-performance Cu-P co-supported zeolite having excellent thermal durability and catalytic performance can be realized by supporting extraskeletal copper atoms and extraskeletal phosphorus atoms on a small pore zeolite. By using this Cu-P co-supported zeolite, a selective reduction catalyst, an exhaust gas catalyst, and the like having excellent purification performance can be realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments of the present invention will be described in detail. The following embodiments are examples (representative examples) of the present invention, and the present invention is not limited to these. The present invention can be modified as desired without departing from the scope of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the values before and after the "~" are included. For example, the expression of a numerical range such as "1 to 100" includes both the upper limit "100" and the lower limit "1". The same applies to the expression of other numerical ranges.
[0022] The Cu-P co-supported zeolite of this embodiment contains at least a small pore zeolite and extraskeletal copper atoms and extraskeletal phosphorus atoms supported on the small pore zeolite, and is characterized in that it has a silica-alumina ratio (SiO2 / Al2O3) of 7 or more and 20 or less, a ratio of copper atoms to T atoms (Cu / T) of 0.005 or more and 0.060 or less, a ratio of phosphorus atoms to T atoms (P / T) of 0.005 or more and 0.060 or less, and a ratio of phosphorus atoms to copper atoms (P / Cu) of 0.1 or more and 3 or less.
[0023] As described above, it was previously believed that a Cu-P co-supported zeolite with such a composition could not be obtained by post-treatment of zeolite using a phosphoric acid compound, and even if it was realized, it was believed that excellent thermal durability and catalytic performance could not be obtained. This is because it was believed to be difficult to co-support extra-framework copper atoms and extra-framework phosphorus atoms on a small pore zeolite. The reasons for this are as follows.
[0024] In the first place, in the past, it was thought in the industry that it would be difficult to make phosphoric acid penetrate into the pores of small-pore zeolite and support phosphorus on the pore surface because phosphoric acid (about 4 Å) is larger than the pores of small-pore zeolite (e.g., CHA: about 3.8 Å). However, according to the findings of the present inventors, in an environment above room temperature (25°C), the pores of small-pore zeolite become larger or smaller due to atomic and molecular vibration, so it is possible to make phosphoric acid penetrate into the pores of small-pore zeolite and support it on the pore surface. In particular, since the Al-O bond is an ionic bond, it has more flexibility in bond length and bond angle than the Si-O covalent bond. In addition, if the treatment temperature is increased during treatment to promote atomic and molecular vibration, phosphoric acid is promoted in the pores of small-pore zeolite. That is, phosphorus can be permeated into the zeolite by setting the temperature when the catalyst coated with Cu-P co-supported zeolite is calcined or when it is subjected to hydrothermal durability treatment to, for example, preferably 350° C. or higher, more preferably 400° C. or higher, and even more preferably 450° C. or higher. Also, when the silica-alumina ratio (SiO2 / Al2O3, molar ratio, hereinafter sometimes referred to as "SAR") of the small pore zeolite is low (when Al is high), Al is easily removed from the framework by dealuminization, and the pore size of the pores increases accordingly, making it easier for phosphoric acid to penetrate into the pores of the small pore zeolite.
[0025] On the other hand, when a phosphorus loading process is performed by impregnating a Cu-loaded small-pore zeolite with a strongly acidic aqueous solution of phosphoric acid, the Cu adsorbed on the acid sites of the zeolite is dissolved by the phosphoric acid and flows out. It is also possible to weaken the acidity of phosphoric acid by using diammonium hydrogen phosphate instead of phosphoric acid, but the free ammonia molecules generated from diammonium hydrogen phosphate coordinate to copper to form soluble copper ammine complexes, which also cause copper dissolution and flow. This flow of Cu during the P loading process is thought to be one of the factors that ultimately reduces the catalyst performance. The flow of Cu here refers to the solubilization and migration of Cu in the zeolite and / or the dissolution of Cu into the aqueous phase of the slurry when the honeycomb is applied.
[0026] In response to this, the present inventors have found that, for example, in the P loading step, if a treatment solution containing at least phosphoric acid and an organic base, i.e., an aqueous phosphoric acid solution neutralized in advance with an organic amine that is unlikely to form a complex with copper, is used, the flow of Cu during the above-mentioned P loading treatment is suppressed, and as a result, P can be co-loaded with high efficiency while maintaining the Cu loaded on the zeolite surface with high efficiency. In addition, the inventors have also found that, since P is loaded after Cu loading, protection of the ion exchange points by phosphorus, which occurred in the prior art, is unlikely to occur, and therefore sufficient co-loading of Cu and P can be achieved. More specifically, the form of copper loaded on the ion exchange points in the zeolite can be Cu, 2+ is bonded to two ion exchange sites, and Cu(OH) + is known to be bonded to one ion exchange point (non-patent literature, J. Song et al., ACS Catal. 7 (2017) 8214-8227). Of these, the former has excellent hydrothermal durability, but the latter is inferior, so the latter is inappropriate as an active site structure for automotive catalyst materials that are used under harsh conditions, and catalyst materials are required to produce a large amount of the former. On the other hand, in order to create the former structure, a structure called Paired Al is required. This refers to a structure in which there are two ion exchange points based on framework Al within the reach of the copper atom. Specifically, it refers to a structure in which one or two Si atoms are between two framework Al atoms. In this Paired Al structure, it is known that the ratio of (Paired Al) / (framework Al) is larger the more framework Al there is (the smaller the SAR is) (non-patent literature C.Paolucci et al., J.Am.Chem.Soc. 138 (2016) 6028-6048). From these viewpoints, in order to obtain a material having a larger amount of the former structure, it is desirable to first add copper to a zeolite with a relatively high framework Al content (low SAR) to give it a large amount of the former structure, and then protect the excess framework Al with phosphorus to improve hydrothermal durability.
[0027] As described above, the present inventors have found for the first time that it is possible to co-support extraskeletal copper atoms and extraskeletal phosphorus atoms on small pore zeolite by post-treatment of the zeolite with a phosphoric acid compound, and have also found for the first time that the obtained Cu-P co-supported zeolite has a novel composition and exhibits excellent thermal durability and catalytic performance. Hereinafter, a more detailed description will be given with an example of a suitable method for producing the Cu-P co-supported zeolite.
[0028] [Production of Cu-P co-supported zeolite] An example of a method for producing the Cu-P co-supported zeolite of this embodiment, i.e., a Cu-P co-supported zeolite containing at least a small pore zeolite and an extraskeletal copper atom and an extraskeletal phosphorus atom supported on the small pore zeolite, includes a production method including at least a step (S11) of preparing a Cu-supported zeolite and a P-supporting step (S21) of applying a treatment liquid containing at least phosphoric acid and an organic base to the Cu-supported zeolite.
[0029] According to this method for producing Cu-P co-supported zeolite, although it is a post-supporting method of a phosphate compound, which has been evaluated as being ineffective for small pore zeolites in the prior art in the industry, it is possible to co-support copper and phosphorus in the desired loading amounts. Therefore, it is possible to obtain a high-performance Cu-P co-supported zeolite that has excellent thermal durability and suppresses deterioration of catalytic performance, with a small environmental impact, and through a simpler process at relatively low cost.
[0030] The reason why such an effect is achieved is not clear, but according to the findings of the present inventors, it is presumed to be as follows. However, the effects are not limited to these. In the first place, in the past, in the industry, it was thought that it was difficult to make phosphoric acid penetrate into the pores of small-pore zeolite and support phosphorus on the pore surface because phosphoric acid (about 4 Å) is larger than the pores of small-pore zeolite (e.g., CHA: about 3.8 Å). However, according to the findings of the present inventors, in an environment above room temperature (25°C), the pores of small-pore zeolite become larger or smaller due to atomic and molecular vibration, so it is possible to make phosphoric acid penetrate into the pores of small-pore zeolite and support it on the pore surface. In particular, since the Al-O bond is an ionic bond, it has more flexibility in bond length and bond angle than the Si-O covalent bond. In addition, if the treatment temperature is increased during treatment to promote atomic and molecular vibration, the penetration of phosphoric acid into the pores of small-pore zeolite is further promoted. That is, phosphorus can be permeated into the zeolite by setting the temperature when the catalyst coated with Cu-P co-supported zeolite is calcined or subjected to hydrothermal durability treatment to, for example, preferably 350° C. or higher, more preferably 400° C. or higher, and even more preferably 450° C. or higher. Furthermore, when the silica-alumina ratio of small pore zeolite is low (when the content of Al is high), Al is easily removed from the framework by dealuminization, and the pore size of the pores increases accordingly, making it easier for phosphoric acid to penetrate into the pores of the small pore zeolite.
[0031] In addition, in the above-mentioned manufacturing method, since the P-loading process is performed using a pre-neutralized phosphoric acid aqueous solution, sufficient Cu and P can be co-loaded, and a high-performance Cu-P co-loaded zeolite can be obtained, the calcination process of the Cu-loaded zeolite and the Cu-P co-loaded zeolite and the high-temperature drying process at 200°C or higher are not required after the Cu-loading process, specifically, until the P-loading process and the catalyst layer coating process. Therefore, the above-mentioned manufacturing method can omit the calcination process and the high-temperature drying process that were previously required, and in this case, it is positioned as a mass production method with high industrial usefulness that has a small environmental load and can obtain a Cu-P co-loaded zeolite at a relatively low cost through a simpler process. Further details will be described below.
[0032] [Preparation step of Cu-supported zeolite (S11)] In this step, a Cu-supported zeolite containing at least a small pore zeolite and extraskeletal copper atoms supported on the small pore zeolite is prepared. A commercially available Cu-supported zeolite can be used here, and a desired Cu-supported zeolite can be prepared as needed by supporting Cu on a zeolite that does not support Cu.
[0033] The small pore zeolite not carrying Cu used as a raw material is so-called small pore zeolite. Its type is not particularly limited, but it is preferable that it has an 8-membered oxygen ring structure. Specifically, it is preferable that it has at least one of the crystal structures CHA, AEI, and ERI in powder X-ray diffraction measurement.
[0034] In addition, the small pore zeolite not supporting Cu is not particularly limited, but from the viewpoint of the penetration of phosphoric acid, etc., it is preferable that the crystallite diameter is 10 nm or more and 50 nm or less in powder X-ray diffraction measurement, more preferably 15 nm or more and 50 nm or less, even more preferably 15 nm or more and 45 nm or less, and particularly preferably 15 nm or more and 35 nm or less. Among small pore zeolites, zeolite species (e.g., AEI and ERI) that tend to have a larger crystallite diameter than CHA etc. due to the framework structure are preferably those having a crystallite diameter of 15 nm or more and 100 nm or less in powder X-ray diffraction measurement, more preferably 20 nm or more and 90 nm or less, even more preferably 25 nm or more and 85 nm or less, and particularly preferably 30 nm or more and 80 nm or less.
[0035] Furthermore, the small pore zeolite not supporting Cu is not particularly limited, but from the viewpoint of the penetration of phosphoric acid, etc., it is preferable to use an aluminosilicate having a silica-alumina ratio of 7 or more and 20 or less, preferably 8 or more and 19 or less, more preferably 9 or more and 18 or less, even more preferably 10 or more and 17 or less, particularly preferably 11 or more and less than 16, and most preferably 12 or more and less than 16. As described above, by using such a small pore zeolite having a relatively high framework Al content (low SAR), first supporting copper on this small pore zeolite with low SAR, and then protecting the excess framework Al with phosphorus, it is possible to exhibit higher hydrothermal durability.
[0036] The small pore zeolite not supporting Cu and the small pore zeolite supporting Cu, which have the above-mentioned physical properties, are commercially available, and can be synthesized or prepared by a conventionally known method as required. For example, the small pore zeolite is synthesized by a conventionally known method (S12), and the small pore zeolite is dissolved in NH + Type and / or H + After ion-exchanging the zeolite with a zeolite matrix (S13), copper is supported on the small pore zeolite (S14), thereby obtaining small pore zeolite not supporting Cu or small pore zeolite supporting Cu. Each step will be described in detail below.
[0037] <Zeolite synthesis (S12)> As a method for synthesizing (S12) a small pore zeolite, there is widely known a method that includes at least a step of preparing a mixture containing a Si-Al element source and / or an Al element source containing at least an aluminosilicate having a silica-alumina ratio of 2 or more but less than 20, a Si element source (excluding those corresponding to the Si-Al element source), an alkali metal source, an organic structure directing agent, and water, and a synthesis step of synthesizing the small pore zeolite by hydrothermal treatment of the mixture.
[0038] In the mixture preparation step, a mixture containing a Si-Al element source and / or an Al element source, a Si element source, an alkali metal source, an organic structure directing agent (hereinafter sometimes abbreviated as "SDA"), and water is prepared.
[0039] As the Si-Al element source used as the raw material, any known source can be used without any particular limitation as long as it contains at least an aluminosilicate with a silica-alumina ratio of 2 or more and less than 20. The type of the source is not particularly limited. Here, the aluminosilicate has a structure in which a part of the silicon atoms in the silicate is replaced with an aluminum atom. The silica-alumina ratio is preferably 5 or more and less than 20, more preferably 7 or more and less than 18. In this specification, the silica-alumina ratio means a value obtained by fluorescent X-ray analysis. Specifically, a sample obtained by pressurizing about 5 g of a sample with 20 t was measured using Axios (Spectolys), and the SAR was calculated from the mass% of Al2O3 and SiO2 obtained.
[0040] As such an aluminosilicate, an aluminosilicate represented by the following general formula (I) is preferably used. xM2O·Al2O3·mSiO2·nH2O ···(I) (In the formula (I), M represents an alkali metal element, x is a number satisfying 0≦x≦1.0, m is a number satisfying 2≦m<20, and n is a number satisfying 5≦n≦15.)
[0041] In the general formula (I), examples of the alkali metal element include Li, Na, Ka, Rb, Cs, etc., and among these, Na and K are preferred, and Na is more preferred. The aluminosilicate may contain other elements in addition to Si and Al, such as Ga, Fe, B, Ti, Zr, Sn, Zn, etc. In addition, in the general formula (I), 0≦x≦0.6 is preferable, and 0.1≦x≦0.5 is more preferable. On the other hand, in the general formula (I), m is preferably 5≦m<20, and more preferably 7≦m<18. In the general formula (I), n is preferably 6≦n≦15, and more preferably 7≦n≦15.
[0042] Among aluminosilicates having an SAR of 2 or more and less than 20, aluminosilicates in a solid powder form at room temperature and normal pressure (25°C, 1 atm) are preferably used from the viewpoints of handling and diffusibility. In this specification, the term "powder-like" refers to a powder (a powder containing primary particles and / or aggregates (secondary particles) formed by agglomeration of primary particles) and granules formed by granulating primary particles or secondary particles. The shape of each particle of the powdered aluminosilicate is not particularly limited, and may be, for example, spherical, ellipsoidal, crushed, flat, or irregular.
[0043] The average particle diameter of the powdered aluminosilicate (D 50 ) is not particularly limited, but is preferably 0.01 to 500 μm, and more preferably 0.1 to 20 μm. In this specification, the average particle diameter D 50 means the median diameter measured by a laser diffraction particle size distribution analyzer (for example, the laser diffraction particle size distribution analyzer SALD-3100 manufactured by Shimadzu Corporation).
[0044] In addition, as the aluminosilicate having an SAR of 2 or more and less than 20, an aluminosilicate having an amorphous crystal structure as determined by powder X-ray diffraction or an aluminosilicate having an FAU structure is preferably used. Here, the fact that the crystal structure as determined by powder X-ray diffraction is amorphous means that there is no clear peak showing a specific plane index in the X-ray diffraction pattern. As such an amorphous aluminosilicate, commercially available synthetic aluminum silicate can be used.
[0045] Such an aluminosilicate having an SAR of 2 or more and less than 20 can be synthesized by a method known in the art, and the synthesized product can be used as the Si-Al element source. For example, a water-soluble silicate and a water-soluble aluminum salt are reacted under the following conditions: the ratio (Si / Al) of silicon atoms in the water-soluble silicate to aluminum atoms in the water-soluble aluminum salt is 1.0 to 11 (preferably 2.5 to 10.8), the liquid temperature is 20 to 90°C (preferably 40 to 70°C), the pH is 3.8 to 5.0 (preferably 4.0 to 4.7), the reaction liquid concentration (SiO2+Al2O3) is 70 to 250 g / L (preferably 100 to 180 g / L), and the reaction method is a continuous reaction; the aluminum silicate is separated from the resulting reaction liquid into a solid-liquid separation, washed, and dried, thereby obtaining an aluminosilicate having an SAR of 2 or more and less than 20. In this case, aluminum chloride, aluminum nitrate, aluminum sulfate, sodium aluminate, etc. are preferably used as the water-soluble aluminum salt. As the water-soluble silicate, an alkali metal silicate such as sodium silicate or potassium silicate is preferably used. As the sodium silicate, sodium silicate No. 1, No. 2, No. 3, No. 4, sodium metasilicate, sodium orthosilicate, etc. are preferably used. The aluminosilicate having a silica-alumina ratio of 2 or more and less than 20, which serves as a source of Si-Al elements, can be used alone or in any combination and ratio of two or more.
[0046] Examples of the Al element source used as a raw material include, but are not limited to, aluminum hydroxide, sodium aluminate, aluminum sulfate, pseudoboehmite, boehmite, metallic aluminum, and aluminum isopropoxide.
[0047] The Al element source may be used alone or in any combination and ratio of two or more kinds.
[0048] Examples of the Si element source used as a raw material include, but are not limited to, precipitated silica, colloidal silica, fumed silica, silica gel, sodium silicate (sodium metasilicate, sodium orthosilicate, sodium silicate No. 1, No. 2, No. 3, No. 4, etc.), alkoxysilanes such as tetraethoxysilane (TEOS) and trimethylethoxysilane (TMEOS), etc. However, in this specification, aluminosilicates with SAR of 2 or more and less than 20 correspond to the above-mentioned Si-Al element source and are not included in this Si element source.
[0049] The Si element source may be used alone or in any combination and ratio of two or more kinds.
[0050] Examples of the alkali metal source include alkali metal hydroxides such as LiOH, NaOH, KOH, CsOH, and RbOH, aluminates of these alkali metals, and the above-mentioned Si-Al element source and alkali components contained in the Si element source. Among these, NaOH and KOH are preferably used. In addition, the alkali metal in the mixture can also function as an inorganic structure directing agent, so that an aluminosilicate with excellent crystallinity tends to be easily obtained.
[0051] The alkali metal sources can be used alone or in any combination and ratio of two or more kinds.
[0052] As the organic structure directing agent, for example, at least one selected from the group consisting of primary amines, secondary amines, tertiary amines, and quaternary ammonium salts is used. Specifically, AEI type zeolite includes hydroxide salts, carbonate salts, halides, sulfate salts, etc., in which quaternary ammonium such as 1,1,3,5-tetramethylpiperidinium and tetraethylammonium is used as the cation. In addition, ERI type zeolite includes hydroxide salts, carbonate salts, halides, sulfate salts, etc., in which quaternary ammonium such as hexamethonium, tetrapropylammonium, tetraethylammonium, and dimethyldiethylammonium is used as the cation. Further, the CHA type zeolite includes hydroxide salts, halides, carbonate salts, sulfate salts, methyl carbonate salts, and sulfate salts of adamantanamine derivatives such as N,N,N-trialkyladamantaammonium as the cation; benzylamine derivatives such as N,N,N-trialkylbenzylammonium ion, cyclohexylamine derivatives such as N,N,N-trialkylcyclohexylammonium ion and N,N,N-methyldiethylcyclohexylammonium ion, quinuclidinol derivatives such as N-alkyl-3-quinuclidinol ion, or aminonorbornane derivatives such as N,N,N-trialkylexoaminonorbornane, tetramethylammonium ion, ethyltrimethylammonium ion, diethyldimethylammonium ion, triethylmethylammonium ion, tetraethylammonium ion, and other alkylamine derivatives having 1 to 2 carbon atoms as the cation; but is not particularly limited thereto. The above cations may be accompanied by anions that are generally not detrimental to the formation of the aluminosilicate. Such anions include Cl. - , Br - , I - Examples of the ions include, but are not limited to, halogen ions such as those mentioned above, hydroxide ions, acetates, sulfates, carboxylates, etc. Among these, hydroxide ions are preferably used.
[0053] Among these, as an organic structure directing agent suitable for the synthesis of CHA type zeolite, at least one selected from the group consisting of N,N,N-trimethyladamantane ammonium hydroxide (hereinafter sometimes abbreviated as "TMAdaOH"), N,N,N-trimethyladamantane ammonium halide, N,N,N-trimethyladamantane ammonium carbonate, N,N,N-trimethyladamantane ammonium methyl carbonate salt, N,N,N-trimethyladamantane ammonium hydrochloride, and N,N,N-trimethyladamantane ammonium sulfate is preferred. As an organic structure directing agent suitable for the synthesis of AEI type zeolite, 1,1,3,5-tetramethylpiperidinium is preferred, and as an organic structure directing agent suitable for the synthesis of ERI type zeolite, a combination of hexamethonium and tetraalkylammonium is preferred.
[0054] The organic structure directing agents may be used alone or in any combination and ratio of two or more kinds.
[0055] In the step of preparing the mixture, a mixture (slurry) containing the above-mentioned Si-Al element source and / or Al source, the Si element source, the alkali metal source, the organic structure directing agent, and water is prepared. At this time, wet mixing can be performed using a known mixer or stirrer, such as a ball mill, a bead mill, a media stirring mill, a homogenizer, etc., if necessary. When stirring, it is usually preferable to perform the stirring at a rotation speed of about 30 to 2000 rpm, more preferably 50 to 1000 rpm.
[0056] At this time, the content of water in the mixture can be appropriately set in consideration of reactivity, handling, etc., and is not particularly limited, but the water-silica ratio (H2O / SiO2 molar ratio) of the mixture is usually 5 to 100, preferably 6 to 50, more preferably 7 to 40. When the water-silica ratio is within the above-mentioned preferred range, stirring during preparation of the mixture or during crystallization by hydrothermal synthesis becomes easy, and the handling is improved, and the generation of by-products and impurity crystals is suppressed, so that a high yield tends to be obtained. The water used here may be tap water, RO water, deionized water, distilled water, industrial water, pure water, ultrapure water, etc., depending on the desired performance. In addition, the method of blending water into the mixture may be blended separately from each of the above-mentioned components, or it may be mixed with each component in advance and blended as an aqueous solution or dispersion of each component.
[0057] The silica-alumina ratio in the mixture can also be appropriately set, and is not particularly limited, but is usually 5 to 80, preferably 8 to less than 75, and more preferably 10 to less than 70. When the silica-alumina ratio is within the above preferred range, dense crystals are easily obtained, and an aluminosilicate having excellent thermal durability in a high-temperature environment or after exposure to high temperatures tends to be easily obtained. More specifically, for the synthesis of CHA-type zeolite, the silica-alumina ratio in the mixture is preferably 5 to 50, more preferably 8 to less than 45, and even more preferably 10 to less than 40. For the synthesis of AEI-type zeolite, the silica-alumina ratio in the mixture is preferably 15 to 80, more preferably 20 to less than 75, and even more preferably 25 to less than 70. For the synthesis of ERI-type zeolite, the silica-alumina ratio in the mixture is preferably 5 to 50, more preferably 8 to less than 45, and even more preferably 10 to less than 40.
[0058] On the other hand, the hydroxide ion / silica ratio (OH - / SiO2 molar ratio) can also be set appropriately and is not particularly limited, but is usually 0.10 to 0.90, preferably 0.15 to 0.80, and more preferably 0.20 to 0.75. When the hydroxide ion / silica ratio is within the above preferred range, crystallization tends to proceed easily, and an aluminosilicate having excellent thermal durability in a high-temperature environment or after exposure to high temperatures tends to be obtained. More specifically, for the synthesis of CHA-type zeolite, the hydroxide ion / silica ratio in the mixture is preferably 0.10 to 0.90, more preferably 0.15 to 0.50, and even more preferably 0.20 to 0.40. For the synthesis of AEI-type zeolite, the hydroxide ion / silica ratio in the mixture is preferably 0.30 to 0.90, more preferably 0.40 to 0.85, and even more preferably 0.50 to 0.80. In the synthesis of ERI-type zeolite, the hydroxide ion / silica ratio in the mixture is 0.10 or more and 0.90 or less, preferably 0.15 or more and 0.80 or less, and more preferably 0.20 or more and 0.70 or less.
[0059] The content of the alkali metal in the mixture can also be appropriately set, and is not particularly limited, but the molar ratio of the alkali metal (M) in terms of oxide, i.e., the alkali metal oxide / silica ratio (MO / SiO2 molar ratio), is usually 0.01 to 0.50, preferably 0.05 to 0.30. When the alkali metal oxide / silica ratio is within the above preferred range, crystallization due to mineralization is promoted, and the generation of by-products and impurity crystals is suppressed, tending to easily obtain a high yield.
[0060] On the other hand, the organic structure directing agent / silica ratio (organic structure directing agent / SiO2 molar ratio) in the mixture can also be set appropriately, and is not particularly limited, but is usually 0.05 to 0.70, preferably 0.07 to 0.60, and more preferably 0.09 to 0.55. When the organic structure directing agent / silica ratio is within the above preferred range, crystallization tends to proceed easily, and an aluminosilicate having excellent thermal durability in a high-temperature environment or after exposure to high temperatures tends to be easily obtained at low cost. More specifically, for the synthesis of CHA-type zeolite, the organic structure directing agent / silica ratio in the mixture is 0.05 to 0.40, preferably 0.07 to 0.30, and more preferably 0.09 to 0.25. For the synthesis of AEI-type zeolite, the organic structure directing agent / silica ratio in the mixture is 0.05 to 0.40, preferably 0.07 to 0.30, and more preferably 0.09 to 0.25. In the synthesis of ERI-type zeolite, the organic structure directing agent / silica ratio in the mixture is 0.20 or more and 0.70 or less, preferably 0.30 or more and 0.65 or less, and more preferably 0.40 or more and 0.60 or less.
[0061] The above mixture may further contain seed crystals (seed crystals) of an aluminosilicate having a desired skeletal structure from the viewpoint of promoting crystallization. By blending seed crystals, crystallization of the desired skeletal structure is promoted, and a high-quality aluminosilicate tends to be easily obtained. The seed crystals used here are not particularly limited as long as they have a desired skeletal structure. For example, seed crystals of an aluminosilicate having at least one of the skeletal structures CHA, AEI, and ERI can be used. The silica-alumina ratio of the seed crystals is arbitrary, but is preferably the same as or similar to the silica-alumina ratio of the mixture, and from this viewpoint, the silica-alumina ratio of the seed crystals is preferably 5 or more and 80 or less, more preferably 8 or more and less than 75, and even more preferably 10 or more and less than 70. The silica-alumina ratio of the seed crystals can also be appropriately set according to the zeolite having the desired skeletal structure, and the preferred range is the same as that described above.
[0062] The seed crystals used here can be not only separately synthesized aluminosilicates, but also commercially available aluminosilicates. Naturally produced aluminosilicates can be used, and aluminosilicates synthesized according to the present invention can also be used as seed crystals. The cation type of the seed crystals is not particularly limited, and for example, sodium type, potassium type, ammonium type, proton type, etc. can be used.
[0063] The particle size of the seed crystal used here (D 50 ) is not particularly limited, but from the viewpoint of promoting crystallization of the desired crystal structure, it is desirable that it is relatively small, and is usually 0.5 nm to 5 μm, preferably 1 nm to 3 μm, and more preferably 2 nm to 1 μm. The amount of the seed crystals to be mixed can be appropriately set according to the desired crystallinity, and is not particularly limited, but is preferably 0.05 to 30 mass%, more preferably 0.1 to 20 mass%, and even more preferably 0.5 to 10 mass%, based on the mass of SiO2 in the mixture.
[0064] In the hydrothermal treatment step of the mixture, the above-mentioned mixture is heated in a reaction vessel to carry out hydrothermal synthesis, thereby obtaining a crystallized aluminosilicate.
[0065] The reaction vessel used in this hydrothermal synthesis can be any known sealed pressure vessel that can be used in hydrothermal synthesis, and the type is not particularly limited. For example, a sealed heat-resistant and pressure-resistant vessel such as an autoclave equipped with a stirring device, a heat source, a pressure gauge, and a safety valve is preferably used. The crystallization of the aluminosilicate may be performed with the above-mentioned mixture (raw material composition) left to stand, but from the viewpoint of increasing the uniformity of the obtained aluminosilicate, it is preferable to perform the crystallization while stirring and mixing the above-mentioned mixture (raw material composition). At this time, it is usually preferable to perform the crystallization at a rotation speed of about 30 to 2000 rpm, more preferably 50 to 1000 rpm.
[0066] The treatment temperature (reaction temperature) of the hydrothermal synthesis is not particularly limited, but from the viewpoint of the crystallinity of the obtained aluminosilicate, economic efficiency, etc., it is usually 100° C. or more and 200° C. or less, preferably 120° C. or more and 190° C. or less, and more preferably 125° C. or more and 180° C. or less. The treatment temperature may be appropriately set depending on the zeolite of the desired framework structure, and for example, for CHA-type and AEI-type zeolites, 150° C. or more and 180° C. or less is particularly preferred, and for example, for ERI-type zeolites, 100° C. or more and 150° C. or less is particularly preferred.
[0067] The treatment time (reaction time) of the hydrothermal synthesis is not particularly limited as long as it is long enough to allow crystallization. From the viewpoints of the crystallinity of the resulting aluminosilicate and economic efficiency, the treatment time is usually from 1 hour to 20 days, preferably from 4 hours to 10 days, and more preferably from 12 hours to 8 days.
[0068] The treatment pressure for the hydrothermal synthesis is not particularly limited, and the autogenous pressure generated when the mixture charged in the reaction vessel is heated to the above-mentioned temperature range is sufficient. At this time, an inert gas such as nitrogen or argon may be introduced into the vessel as necessary.
[0069] By carrying out such hydrothermal treatment, a crystallized aluminosilicate can be obtained. At this time, if necessary, a solid-liquid separation treatment, a water washing treatment, a drying treatment for removing moisture in air at a temperature of about 50 to 150°C, etc. may be carried out according to a conventional method.
[0070] The aluminosilicate thus obtained may contain a structure-directing agent, an alkali metal, etc., in the pores, etc. Therefore, it is preferable to carry out a removal step to remove them as necessary. The organic structure-directing agent, the alkali metal, etc., can be removed according to a conventional method, and the method is not particularly limited. For example, liquid-phase treatment using an acidic aqueous solution, liquid-phase treatment using an aqueous solution containing ammonium ions, liquid-phase treatment using a chemical solution containing a decomposition component of the organic structure-directing agent, exchange treatment using a resin, etc., baking treatment, etc. can be carried out. These treatments can be carried out in any combination. Among these, the organic structure-directing agent, the alkali metal, etc. are preferably removed by baking treatment from the viewpoint of production efficiency, etc.
[0071] The treatment temperature (calcination temperature) in the calcination treatment can be appropriately set depending on the raw materials used, etc., and is not particularly limited, but from the viewpoint of maintaining crystallinity and reducing the remaining proportion of the structure directing agent, alkali metal, etc., the treatment temperature is usually 300° C. or higher and 1000° C. or lower, preferably 400° C. or higher and 900° C. or lower, more preferably 430° C. or higher and 800° C. or lower, and further preferably 480° C. or higher and 750° C. or lower. The calcination treatment is preferably carried out in an oxygen-containing atmosphere, for example, in the air.
[0072] The treatment time (calcination time) in the calcination treatment can be appropriately set depending on the treatment temperature, economic efficiency, etc., and is not particularly limited, but is usually 0.5 hours or more and 72 hours or less, preferably 1 hour or more and 48 hours or less, and more preferably 3 hours or more and 40 hours or less.
[0073] <Ion exchange (S13)> After crystallization, the aluminosilicate may have metal ions, such as alkali metal ions, on its ion exchange sites. Depending on the desired performance, an ion exchange step may be carried out. In this ion exchange step, ammonium ions (NH4 + ) and protons (H +) can be ion-exchanged with non-metallic cations such as ammonium ions. For example, by performing a liquid-phase treatment using an aqueous solution containing ammonium ions such as an aqueous ammonium nitrate solution or an aqueous ammonium chloride solution on the aluminosilicate, it can be ion-exchanged into the ammonium form. Further, after ion-exchanging the aluminosilicate with ammonia and then performing a firing treatment, it can be ion-exchanged into the proton form. In the above production method, from the viewpoint of omitting the firing treatment and the high-temperature drying treatment using a neutralized treatment liquid in the P-supporting treatment, it is preferable that it is in the ammonium ion (NH4 + ) form. The aluminosilicate thus obtained can be further treated, if necessary, such as reducing the acid amount. The treatment for reducing the acid amount may be performed, for example, by silylation, steam treatment, dicarboxylic acid treatment, etc. These treatments for reducing the acid amount and changing the composition may be performed according to conventional methods.
[0074] <Cu supported (S14)> Here, a Cu-supported zeolite is obtained by supporting Cu on the above-described aluminosilicate (without Cu supported). The Cu-supporting treatment may be performed according to a conventional method. By supporting Cu in this way, it can function as a catalyst in various applications. Further, if necessary, transition metal elements other than Cu, such as iron (Fe) and tungsten (W), can also be supported.
[0075] The supporting treatment of transition metals such as Cu may be carried out according to a conventional method. For example, the above-mentioned aluminosilicate may be contacted with a simple substance or compound of a transition metal, or a transition metal ion. The supporting method of the transition metal may be any method in which the transition metal is held at least in the ion exchange sites or pores of the aluminosilicate. The transition metal may be supplied as an inorganic acid salt of the transition metal, for example, a sulfate, a nitrate, an acetate, a chloride, an oxide, a composite oxide, and a complex salt of the transition metal. Among these, in the above-mentioned manufacturing method, since a neutralized treatment liquid is used in the P supporting treatment, it is preferable to supply the transition metal as a strong acid inorganic salt such as a sulfate or a nitrate. Specific methods include, but are not limited to, an ion exchange method, an evaporation to dryness method, a precipitation supporting method, a physical mixing method, a framework replacement method, and an impregnation supporting method. After the supporting treatment of the transition metal, if necessary, a solid-liquid separation treatment, a water washing treatment, and a drying treatment for removing moisture at a temperature of about 50 to 150 ° C. in the air may be carried out according to a conventional method.
[0076] If necessary, platinum group elements (PGM: platinum group metals) such as platinum, palladium, rhodium, and iridium may be supported on the aluminosilicate. The method of supporting the precious metal elements and platinum group elements can be applied by known methods and is not particularly limited. For example, a solution of a salt containing the precious metal elements and platinum group elements is prepared, the aluminosilicate is impregnated with this salt-containing solution, and then calcined, whereby the precious metal elements and platinum group elements can be supported. The salt-containing solution is not particularly limited, but is preferably a nitrate solution, a dinitrodiamine nitrate solution, an aqueous chloride solution, or the like. The calcination treatment is also not particularly limited, but is preferably performed at 350°C to 1000°C for about 1 to 12 hours. Prior to the high-temperature calcination, it is preferable to perform reduced pressure drying using a vacuum dryer or the like, and a drying treatment at about 50°C to 180°C for about 1 to 48 hours.
[0077] Next, the Cu-unsupported zeolite and Cu-supported zeolite thus prepared will be described. The Cu-unsupported zeolite and Cu-supported zeolite are crystalline aluminosilicates classified by various structure codes in IZA. Preferably, the crystalline aluminosilicates are classified by at least one structure code of CHA, AEI, and ERI. These crystalline zeolites have a structure in which the main framework metal atoms are aluminum (Al) and silicon (Si), and a network of these and oxygen (O) is formed. The structure is characterized by X-ray diffraction data.
[0078] The particle diameters of Cu-unsupported zeolite and Cu-supported zeolite are not particularly limited because they may vary depending on synthesis conditions, etc., but from the viewpoints of surface area, handleability, etc., their average particle diameters (D 50 ) is preferably from 0.01 μm to 20 μm, and more preferably from 0.02 to 20 μm.
[0079] The silica-alumina ratio of Cu-unsupported zeolite or Cu-supported zeolite can be appropriately set and is not particularly limited, but from the viewpoint of thermal durability, catalytic activity, and the like in a high-temperature environment or after exposure to high temperatures, it is preferably from 7 to 20, more preferably from 8 to 19, even more preferably from 9 to 18, particularly preferably from 10 to 17, especially preferably from 11 to less than 16, and most preferably from 12 to less than 16. By using an aluminosilicate with a silica-alumina ratio within the above-mentioned preferred numerical range, it tends to be easier to obtain a catalyst or catalyst carrier in which thermal durability and catalytic activity are well-balanced at a high level.
[0080] On the other hand, the Cu content in the Cu-supported small pore zeolite is not particularly limited, but is preferably 0.1 to 10 mass % and more preferably 0.5 to 8 mass % based on the total amount.
[0081] Furthermore, the atomic ratio of transition metal to aluminum (transition metal / aluminum) in the Cu-supported small pore zeolite is not particularly limited, but is preferably 0.01 to 1.0, more preferably 0.05 to 0.7, and even more preferably 0.1 to 0.5.
[0082] [P loading step (S21)] Here, P is co-supported on the Cu-supported small pore zeolite. The method of supporting phosphorus is to prepare a treatment liquid containing at least phosphoric acid and an organic base in advance (S22) and apply the treatment liquid to the Cu-supported small pore zeolite. By co-supporting Cu and P in this way, the thermal durability of the catalyst in various applications can be improved. Examples of catalyst applications include, but are not limited to, exhaust gas purification catalysts, catalysts for producing lower olefins from alcohols and ketones, cracking catalysts, dewaxing catalysts, isomerization catalysts, etc. In particular, Cu-P co-supported zeolite can maintain relatively high adsorption performance and catalytic performance even in a high-temperature environment or after exposure to high temperatures, and is highly useful as a nitrogen oxide reduction catalyst. In addition, transition metal elements other than Cu, such as iron (Fe) and tungsten (W), can also be supported as necessary.
[0083] (Preparation of processing solution S22) The composition and physical properties of the treatment liquid used here are not particularly limited as long as it contains at least phosphoric acid and an organic base. Here, phosphoric acid means orthophosphoric acid. If necessary, phosphoric acids such as pyrophosphoric acid may be used in combination. From the viewpoint of increasing the phosphorus carrying efficiency, an aqueous solution containing at least phosphoric acid, an organic base, and water is preferably used as the treatment liquid.
[0084] As described above, in the above-mentioned manufacturing method, a phosphoric acid aqueous solution that has been neutralized in advance is used, so to speak, and therefore the flow of Cu during the above-mentioned P loading treatment is suppressed, and as a result, Cu loaded on the zeolite is maintained at a high efficiency while P is co-loaded at a high efficiency. From this viewpoint, the pH of the treatment solution is not particularly limited, but is preferably 4 to 9, and more preferably 5 to 8.
[0085] The organic base is not particularly limited in type as long as it can realize a phosphoric acid aqueous solution that has been neutralized in advance, and can be appropriately selected from known organic bases. If the organic base is a molecule or ion that is easily coordinated with Cu, it may complex Cu, and if the organic base is a strong base, it may promote the production of copper hydroxide. From this perspective, the organic base is preferably a water-soluble monocyclic compound with a pKa (25°C) of 5 to 9, more preferably a pKa (25°C) of 6 to 8.5.
[0086] Suitable examples of organic bases include water-soluble heterocyclic compounds.Such heterocyclic compounds include 5-membered or 6-membered heterocyclic compounds, and 6-membered heterocyclic compounds are more preferred.Specific examples of organic bases include, but are not limited to, pyridine, 2-picoline, 3-picoline, 4-picoline, 2,6-dimethylpyridine, N-methylmorpholine, N-ethylmorpholine, imidazole, morpholine, etc.
[0087] The P loading treatment may be carried out under the usual conditions. For example, the Cu-loaded small pore zeolite may be impregnated with the above-mentioned treatment solution and brought into contact with the Cu-loaded small pore zeolite. The heat treatment temperature after the P loading treatment is not particularly limited as long as it is at room temperature (25°C) or higher, but is preferably at 40°C or higher, more preferably at 60°C or higher, and even more preferably at 80°C or higher, and the upper limit temperature is not particularly limited, but is generally 180°C or lower, and is preferably 150°C or lower.
[0088] The Cu-P co-supported zeolite of the present embodiment thus obtained contains at least a small pore zeolite and extraskeletal copper atoms and extraskeletal phosphorus atoms supported on the small pore zeolite, and since Cu and P are co-supported on the zeolite with high efficiency, the thermal durability is enhanced and excellent catalytic performance is exhibited.
[0089] Here, from the viewpoint of thermal durability and catalytic performance, the silica-alumina ratio of the Cu-P co-supported zeolite of this embodiment is preferably 7 or more and 20 or less, more preferably 8 or more and 19 or less, even more preferably 9 or more and 18 or less, particularly preferably 10 or more and 17 or less, particularly preferably 11 or more and less than 16, and most preferably 12 or more and less than 16. The SAR value of the Cu-P co-supported zeolite can be appropriately adjusted depending on the SAR of the small pore zeolite used, the SAR and amounts of the Si-Al element source and Si element source used during the synthesis of the small pore zeolite, the synthesis temperature, time, etc.
[0090] In addition, in the Cu-P co-supported zeolite of this embodiment, the ratio of copper atoms to T atoms (Cu / T) is preferably 0.005 to 0.060 from the viewpoint of thermal durability and catalytic performance, more preferably 0.010 to 0.060, even more preferably 0.020 to 0.055, and particularly preferably 0.030 to 0.050. If the Cu content is high, low-temperature performance tends to improve, but if it is too high, high-temperature performance tends to decrease, so it may be appropriately adjusted according to the desired performance. Here, T atoms refer to tetrahedral atoms present in the zeolite framework, and in this specification, refer to the sum of Si atoms and Al atoms. The value of Cu / T of the Cu-P co-supported zeolite can be adjusted to a desired value by appropriately adjusting the amount of Cu salt blended and the supporting time during the Cu supporting process according to the SAR of the small pore diameter zeolite used.
[0091] Furthermore, in the Cu-P co-supported zeolite of this embodiment, the ratio of phosphorus atoms to T atoms (P / T) is preferably 0.005 to 0.060 from the viewpoint of thermal durability and catalytic performance, more preferably 0.010 to 0.060, and even more preferably 0.011 to 0.050. If the P content is high, low temperature performance tends to improve, but if it is too high, high temperature performance and low temperature performance tend to decrease, so it may be appropriately adjusted according to the desired performance. The P / T value of the Cu-P co-supported zeolite can be adjusted to a desired value by appropriately adjusting the amount of phosphoric acid blended during the P support treatment and the support time, etc., depending on the SAR of the small pore diameter zeolite used. For example, in the case of Cu-P co-supported CHA-type zeolite, P / T is particularly preferably 0.020 to 0.055, and most preferably 0.030 to 0.050.
[0092] On the other hand, in the Cu-P co-supported zeolite of this embodiment, the ratio of phosphorus atoms to copper atoms (P / Cu) is preferably 0.1 to 3 for the reasons described above, more preferably 0.3 to 2.5, even more preferably 0.5 to 2.0, and particularly preferably 0.6 to 1.5. When P / Cu is 1.0 or more, the excess Al in the framework of the Cu-supported zeolite is highly protected by phosphorus, and there is a tendency for particularly remarkable hydrothermal durability to be exhibited. The P / Cu value of the Cu-P co-supported zeolite can be adjusted to a desired value by appropriately adjusting the amount and supporting time of the Cu salt during the Cu-supporting treatment and the amount and supporting time of the phosphoric acid during the P-supporting treatment according to the SAR of the small pore diameter zeolite used. For example, in the case of Cu-P co-supported CHA-type zeolite, P / Cu is particularly preferably 0.7 or more and 1.5 or less, more particularly preferably 1.0 or more and 1.5 or less, and most preferably 1.1 or more and 1.5 or less.
[0093] In addition, the Cu-P co-supported zeolite of this embodiment preferably has a crystallite diameter of 10 nm to 100 nm in powder X-ray diffraction measurement from the viewpoint of thermal durability and catalytic performance, more preferably 12 nm to 80 nm, even more preferably 15 nm to 70 nm, and particularly preferably 20 nm to 60 nm. The crystallite diameter of the Cu-P co-supported zeolite may be appropriately set according to the zeolite of the desired framework structure by setting the treatment temperature. For example, in the case of Cu-P co-supported CHA-type zeolite, from the viewpoint of thermal durability and catalytic performance, it is particularly preferable that the crystallite diameter is 10 nm to 50 nm in powder X-ray diffraction measurement, more particularly preferably 15 nm to 50 nm, particularly preferably 15 nm to 45 nm, and most preferably 15 nm to 35 nm.
[0094] Furthermore, the particle size of the Cu-P co-supported zeolite of this embodiment is not particularly limited because it may vary depending on synthesis conditions, etc., but from the viewpoint of surface area, handleability, etc., these average particle sizes (D 50 ) is preferably from 0.01 μm to 20 μm, and more preferably from 0.02 to 20 μm.
[0095] After the P loading treatment, if necessary, solid-liquid separation treatment, water washing treatment, drying treatment for removing water and organic bases in air at a temperature of about 50 to 150° C., etc. can be carried out in accordance with a conventional method. In this case, the composition of the Cu-P co-loaded zeolite from which water and organic bases have been removed is preferably that represented by the following formula (I) from the viewpoint of catalytic activity, etc. SiO2·xAl2O3·yCuO·zP2O5···(I) (In the formula, 0.05≦x≦0.14, 0.005≦y≦0.06, and 0.005≦z≦0.06.)
[0096] Here, the Cu-P co-supported zeolite after the P-supporting treatment can be further subjected to a calcination treatment at 350°C or higher or a high-temperature drying treatment at 200°C or higher, if necessary. However, the above-mentioned manufacturing method has an advantage in terms of process in that such a calcination treatment or high-temperature drying treatment is not essential. That is, this Cu-P co-supported zeolite can be used as it is as a raw material for catalyst slurry, and in this case, since one or two or more calcination processes can be omitted compared to the conventional method, the environmental load is small, and it is possible to mass-supply Cu-P co-supported zeolite at a relatively low cost using a simpler process.
[0097] [Application] As described above in detail, the Cu-P co-supported zeolite of this embodiment can be suitably used in applications such as adsorbents, separation agents, ion exchangers, adsorbents, catalysts, and catalyst carriers. In particular, the Cu-P co-supported zeolite of this embodiment has excellent thermal durability and can maintain relatively high adsorption and catalytic performance even in high-temperature environments or after exposure to high temperatures, so it can be particularly suitably used in applications where it is used in high-temperature environments or exposed to high temperatures. Examples of adsorbents used in high-temperature atmospheres include, but are not limited to, water adsorbents, hydrocarbon adsorbents, and nitrogen oxide adsorbents. Examples of catalysts used in high-temperature and high-humidity atmospheres include, but are not limited to, exhaust gas purification catalysts or catalyst carriers thereof for purifying exhaust gases from diesel automobiles, gasoline automobiles, jet engines, boilers, gas turbines, etc., and nitrogen oxide catalysts or catalyst carriers thereof (nitrogen oxide direct decomposition catalysts, nitrogen oxide reduction catalysts, catalyst carriers thereof, etc.).
[0098] In addition, Cu-P co-supported zeolite is particularly useful as a catalyst for purifying exhaust gas, and is particularly suitable for use as a selective reduction catalyst (SCR catalyst) using ammonia, urea, organic amines, etc. as a reducing agent. That is, Cu-P co-supported zeolite has excellent thermal durability, so it can maintain a high reduction rate of nitrogen oxides even at high temperatures of 400°C to 600°C after hydrothermal durability treatment. In contrast, the reduction rate of nitrogen oxides of conventionally known copper-supported zeolites is significantly reduced at the same high temperature range. As is clear from these comparisons, the above-mentioned Cu-P co-supported zeolite has a particularly remarkable effect in that it shows a high reduction rate at high temperatures when used as an SCR catalyst.
[0099] The hydrothermal durability treatment means an aging treatment of a catalyst performed to exhibit stable catalytic performance in practical use. In this specification, when evaluating the reduction rate of nitrogen oxides, a treatment is performed at 650°C for 100 hours or at 750°C for 40 hours in a water vapor environment with a moisture content of 10% by volume. The reduction rate of nitrogen oxides after hydrothermal durability treatment at 650°C is preferably 65% or more at 500°C, more preferably 70% or more, more preferably 75% or more, more preferably 80% or more, and most preferably 85% or more. The reduction rate of nitrogen oxides after hydrothermal durability treatment at 750°C is preferably 65% or more at 500°C, more preferably 70% or more, more preferably 75% or more, more preferably 78% or more, and most preferably 80% or more.
[0100] In a preferred embodiment, the above-mentioned Cu-P co-supported zeolite exhibits a nitrogen oxide reduction rate equivalent to that of conventionally known copper-supported zeolites even in a low temperature range of 150°C or higher and lower than 400°C. Specifically, the reduction rate of nitrogen oxides after hydrothermal and hydrothermal durability treatment at 650°C is preferably 70% or higher at 200°C, more preferably 75% or higher, even more preferably 80% or higher, particularly preferably 83% or higher, and most preferably 86% or higher. The reduction rate of nitrogen oxides after hydrothermal durability treatment at 750°C is preferably 65% or higher at 200°C, more preferably 70% or higher, even more preferably 76% or higher, particularly preferably 78% or higher, and most preferably 80% or higher.
[0101] [Exhaust gas purification catalyst, exhaust gas purification device, and exhaust gas purification method] When used as a catalyst for purifying exhaust gas or a catalyst carrier thereof, the Cu-P co-supported zeolite of this embodiment can be used as it is in the form of powder. In addition, for example, the powder can be molded into any shape to be used as a granular or pellet-shaped molded body. In addition, various known dispersing devices, kneading devices, and molding devices can be used when preparing the molded body. Furthermore, the Cu-P co-supported zeolite of this embodiment can be supported (supported) on a catalyst carrier such as a ceramic monolith carrier made of cordierite, silicon carbide, silicon nitride, etc., a metal honeycomb carrier or wire mesh carrier made of stainless steel, or a steel wool-like knit wire carrier. In addition, these can be used alone or in any combination and ratio of two or more. When the Cu-P co-supported zeolite is supported on a catalyst carrier, various known coating methods, wash coat methods, and zone coat methods can be applied.
[0102] The Cu-P co-supported zeolite of this embodiment can be used by blending it into the catalyst layer of a catalytic converter for purifying exhaust gas. For example, it can be implemented by providing a catalyst layer containing the Cu-P co-supported zeolite of this embodiment on a catalyst carrier such as a monolithic carrier. In addition, the catalyst area of the catalytic converter for purifying exhaust gas may be a single layer having only one catalyst layer, or a laminate consisting of two or more catalyst layers. Furthermore, it may be any laminate combining one or more catalyst layers with one or more other layers known in the industry. For example, in the case where the catalytic converter for purifying exhaust gas has a multi-layer structure having at least an oxygen storage layer and a catalyst layer on a catalyst carrier, at least the Cu-P co-supported zeolite of this embodiment can be contained in the catalyst layer to provide a catalytic converter for purifying exhaust gas with excellent heat resistance and three-way purification performance. Considering the trend of strengthening exhaust gas regulations, the layer structure is preferably two or more layers.
[0103] The method of forming the catalyst layer may be performed according to a conventional method, and is not particularly limited. For example, the Cu-P co-supported zeolite of this embodiment, an aqueous medium, and, if necessary, a binder known in the art, other catalysts, co-catalyst particles, OSC material, base material particles, additives, etc. are mixed in a desired mixing ratio to prepare a catalyst slurry (slurry-like mixture), and the obtained slurry-like mixture can be applied to the surface of the catalyst support, dried, and fired. At this time, if necessary, an acid or base can be mixed to adjust the pH, or a surfactant or a dispersion resin can be mixed to adjust the viscosity or improve the slurry dispersibility. In addition, as a method of mixing the slurry, crushing and mixing using a ball mill or the like can be applied, but other crushing or mixing methods can also be applied.
[0104] The method of applying the slurry mixture to the catalyst carrier may be performed according to a conventional method, and is not particularly limited. Various known coating methods, wash coat methods, and zone coat methods can be applied. After applying the slurry mixture, it is possible to obtain a catalytic converter for purifying exhaust gas, which includes a catalyst layer containing the Cu-P co-supported zeolite of this embodiment, by performing drying and firing according to a conventional method.
[0105] The above-mentioned catalytic converter for purifying exhaust gas can be arranged in the exhaust system of various engines. The number and the location of the catalytic converter for purifying exhaust gas can be appropriately designed according to the exhaust gas regulations. For example, when the exhaust gas regulations are strict, the number of installation locations can be set to two or more, and the installation locations can be arranged under the floor position immediately behind the catalyst downstream of the exhaust system. And, according to the catalytic composition containing the Cu-P co-supported zeolite of this embodiment and the catalytic converter for purifying exhaust gas, it can exhibit excellent effects in the purification reaction of CO, HC, and NOx even in a high temperature environment. That is, according to the Cu-P co-supported zeolite of this embodiment, it is possible to purify the exhaust gas by contacting it with exhaust gas containing at least one selected from the group consisting of HC, CO, and NOx. EXAMPLES
[0106] The features of the present invention will be described in more detail below with reference to test examples, examples and comparative examples, but the present invention is not limited by these. That is, the materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. In addition, the values of various manufacturing conditions and evaluation results in the following examples have the meaning of preferred upper limit values or preferred lower limit values in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper limit value or lower limit value and the values of the following examples or the values of the examples.
[0107] Example 1 <Preparation of the mixture> To 1,220.0 g of an aqueous solution of 25% N,N,N-trimethyladamantammonium hydroxide (hereinafter sometimes referred to as "25% aqueous solution of TMAdaOH"), 1,710 g of pure water, 590 g of solid powder amorphous synthetic aluminum silicate as a Si-Al element source (manufactured by Kyowa Chemical Industry Co., Ltd., synthetic aluminum silicate, trade name: Kyoward (registered trademark) 700SEN-S, SAR: 9.7), 880.0 g of colloidal silica as a Si element source (manufactured by Nissan Chemical Industries, Ltd., trade name: Snowtex (registered trademark) 40, SiO2 content: 39.7% by mass), 74.0 g of sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Corporation, content 97% or more), and 31.0 g of chabazite seed crystals (SAR 16) were added and thoroughly mixed to obtain a raw material composition (mixture). The composition of the raw material composition was SiO2:0.053Al2O3:0.119TMAdaOH:0.095Na2O:15.1H2O in molar ratio.
[0108] <Synthesis of CHA-type aluminosilicate> This raw material composition (mixture) was put into a 5,000 cc stainless steel autoclave and sealed, and then while stirring at 300 rpm, the temperature was raised to 170 °C and held for 55 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, the obtained solid phase was washed with a sufficient amount of water, and dried at 105 °C to obtain a product. When powder X-ray diffraction analysis was performed, it was confirmed that the product was a pure CHA-type aluminosilicate, that is, a single phase of chabazite-type synthetic zeolite. When fluorescence X-ray analysis was performed, the silica-alumina ratio (SiO2 / Al2O3) of the CHA-type aluminosilicate of Example 1 obtained was 15.5.
[0109] <Firing and ion exchange of CHA-type aluminosilicate> The CHA-type aluminosilicate of Example 1 obtained was fired at 600 °C, and then ion exchange was repeated twice using an ammonium nitrate aqueous solution containing the same amount of ammonium nitrate and 10 times the amount of water, and then washed with a sufficient amount of pure water and dried at 120 °C to obtain an NH4 + -type CHA-type aluminosilicate (NH4 + -type CHA-type zeolite).
[0110] <Cu-supported, P-supported> The obtained NH4 of Example 1 + 170 g of the CHA-type aluminosilicate of the NH4 type was impregnated with a mixture of 41 g of a 50% aqueous solution of copper nitrate trihydrate and 45 g of water, and then dried at 100 to 120 °C. To this, a mixture of 12 g of 85% phosphoric acid, 17 g of morpholine, and 35 g of water (treatment solution, pH = 7.5) was impregnated in an environment at 25 °C and dried again at 100 to 120 °C to obtain the Cu-P co-supported CHA-type aluminosilicate (Cu-P co-supported CHA-type zeolite) of Example 1. The supported amount of Cu in terms of solid content measured by X-ray fluorescence analysis was 3.4% by mass, and the supported amount of P was 2.2% by mass. <Manufacture of honeycomb laminated catalyst> Thereafter, except for using the obtained Cu-P co-supported CHA-type aluminosilicate of Example 1, the honeycomb laminated catalyst of Example 1 was obtained in the same manner as in Example 1.
[0111] (Example 2) <Preparation of mixture> To 930.0 g of a 25% aqueous solution of TMAdaOH, 2,080 g of pure water, 826 g of solid powder amorphous synthetic aluminum silicate (manufactured by Kyowa Chemical Industry Co., Ltd., synthetic aluminum silicate, trade name: Kyoward (registered trademark) 700PEL, SAR: 10.0) as a Si-Al element source, 320.0 g of colloidal silica (manufactured by Nissan Chemical Industries, Ltd., trade name: Snowtex (registered trademark) 40, SiO2 content ratio: 39.7%) as a Si element source, 133.0 g of 48% sodium hydroxide (manufactured by Kanto Chemical Co., Inc.), and 23.0 g of chabazite seed crystals (SAR10) were added and thoroughly mixed to obtain a raw material composition (mixture). The composition of the raw material composition was, in molar ratio, SiO2:0.081Al2O3:0.100TMAdaOH:0.100Na2O:16.0H2O.
[0112] <Synthesis of CHA-type aluminosilicate> This raw material composition (mixture) was put into a 5,000 cc stainless steel autoclave and sealed. Then, while stirring at 300 rpm, the temperature was raised to 160 °C and held for 48 hours, and then held at 170 °C for 24 hours. After this hydrothermal treatment, the product was subjected to solid-liquid separation. The obtained solid phase was washed with a sufficient amount of water and dried at 105 °C to obtain the product. When powder X-ray diffraction analysis was performed, it was confirmed that the product was a single phase of pure CHA-type aluminosilicate, that is, chabazite-type synthetic zeolite. When X-ray fluorescence analysis was performed, the silica-alumina ratio (SiO2 / Al2O3) of the CHA-type aluminosilicate obtained in Example 2 was 11.3.
[0113] <Ion Exchange of CHA-Type Aluminosilicate> The same procedure as in Example 1 was carried out except that the CHA-type aluminosilicate obtained in Example 2 was used.
[0114] <Cu Loading, P Loading> To 120 g of the obtained NH4 + type CHA-type aluminosilicate, a mixed solution of 34.6 g of 50% copper nitrate trihydrate aqueous solution and 26 g of water was impregnated, and then dried at 105 °C. To this, a mixture of 8 g of 85% phosphoric acid, 12 g of morpholine, and 40 g of water (treatment solution, pH = 7.6) was impregnated in an environment at 25 °C and dried again at 100 to 120 °C to obtain the Cu-P co-loaded CHA-type aluminosilicate (Cu-P co-loaded CHA-type zeolite) of Example 2. The Cu loading amount in terms of solid content measured by X-ray fluorescence analysis was 3.7 mass%, and the P loading amount was 2.0 mass%.
[0115] <Manufacture of Honeycomb Monolith Catalyst> Thereafter, the honeycomb monolith catalyst of Example 2 was obtained in the same manner as in Example 1 except that the Cu-P co-loaded CHA-type aluminosilicate obtained in Example 2 was used.
[0116] (Comparative Example 1) <Preparation of Mixture> To 560.0 g of a 25% aqueous solution of TMAdaOH, 3,735 g of pure water, 52.0 g of solid powdered sodium aluminate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as an Al element source, 109.0 g of a sodium silicate solution (manufactured by Nippon Chemical Industry Co., Ltd., J Sodium Silicate No. 3) as a Si element source, 305.0 g of precipitated silica (manufactured by Tosoh Silica Corporation, trade name: Nipsil (registered trademark) ER), and 10.0 g of chabazite seed crystals (SAR13) were added and thoroughly mixed to obtain a raw material composition (mixture). The composition of the raw material composition was, in molar ratio, SiO2:0.053 Al2O3:0.125 TMAdaOH:0.095 Na2O:44.0 H2O.
[0117] <Synthesis of CHA-Type Aluminosilicate> This raw material composition (mixture) was put into a 5,000 cc stainless steel autoclave and sealed, and then while stirring at 300 rpm, the temperature was raised to 160 °C and held for 96 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, the obtained solid phase was washed with a sufficient amount of water, and dried at 105 °C to obtain a product. When powder X-ray diffraction analysis was performed, it was confirmed that the product was a single phase of pure CHA-type aluminosilicate, that is, chabazite-type synthetic zeolite. When fluorescence X-ray analysis was performed, the silica-alumina ratio (SiO2 / Al2O3) of the CHA-type aluminosilicate of Comparative Example 1 obtained was 16.3.
[0118] <Ion Exchange of CHA-Type Aluminosilicate> It was carried out in the same manner as in Example 1 except that the CHA-type aluminosilicate of Comparative Example 1 obtained was used.
[0119] <Cu Loading and High-Temperature Drying Treatment> To 160 g of the obtained NH4 + type CHA-type aluminosilicate, 84 g of a 25% aqueous solution of copper(II) nitrate trihydrate was impregnated, then dried at 105 °C, and further subjected to a high-temperature drying treatment at 200 °C for 16 hours to obtain a Cu-loaded CHA-type aluminosilicate (Cu-loaded CHA-type zeolite) of Comparative Example 1. The Cu loading amount in terms of solid content measured by fluorescence X-ray analysis was 3.9 mass%.
[0120] <Manufacture of Honeycomb Structured Catalyst> Thereafter, a honeycomb structured catalyst of Comparative Example 1 was obtained in the same manner as in Example 1, except that the Cu-supported CHA-type aluminosilicate of Comparative Example 1 obtained was used.
[0121] (Comparative Example 2) <Preparation of Mixture> To 1,125.0 g of a 25% aqueous solution of TMAdaOH, 2,990 g of pure water, 630 g of solid powder amorphous synthetic aluminosilicate as a Si—Al element source (manufactured by Kyowa Chemical Industry Co., Ltd., synthetic aluminosilicate, trade name: Kyoward (registered trademark) 700SL, SAR: 9.7), 340.0 g of precipitated silica as a Si element source (manufactured by Tosoh Silica Corporation, trade name: Nipsil (registered trademark) ER), 85.0 g of sodium hydroxide (content 97% or more), and 30.0 g of chabazite seed crystals (SAR 13) were added and thoroughly mixed to obtain a raw material composition (mixture). The composition of the raw material composition was SiO2:0.059Al2O3:0.109TMAdaOH:0.100Na2O:18.1H2O in terms of molar ratio.
[0122] <Synthesis of CHA-Type Aluminosilicate> This raw material composition (mixture) was put into a 5,000 cc stainless steel autoclave and sealed, and then while stirring at 300 rpm, the temperature was raised to 160° C. and held for 48 hours, and then further held at 170° C. for 48 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, and the obtained solid phase was washed with a sufficient amount of water and dried at 105° C. to obtain a product. As a result of powder X-ray diffraction analysis, it was confirmed that the product was a single phase of pure CHA-type aluminosilicate, that is, chabazite-type synthetic zeolite. As a result of fluorescent X-ray analysis, the silica-alumina ratio (SiO2 / Al2O3) of the CHA-type aluminosilicate of Comparative Example 2 obtained was 15.4.
[0123] <Ion Exchange of CHA-Type Aluminosilicate> The same procedure as in Example 1 was carried out, except that the CHA-type aluminosilicate of Comparative Example 2 obtained was used.
[0124] <Cu Loading and Calcination Treatment> The obtained NH₄ of Comparative Example 2 + 220 g of the CHA-type aluminosilicate of the NH₄ type of Comparative Example 2 was impregnated with 46 g of an aqueous solution of 25% copper nitrate trihydrate and 64 g of water, dried at 105 °C, and further calcined at 500 °C for 4 hours to obtain the Cu-supported CHA-type aluminosilicate (Cu-supported CHA-type zeolite) of Comparative Example 2.
[0125] <Manufacture of honeycomb laminated catalyst> Thereafter, a honeycomb laminated catalyst of Comparative Example 2 was obtained in the same manner as in Example 1 except that the obtained Cu-supported CHA-type aluminosilicate of Comparative Example 2 was used.
[0126] (Comparative Example 3) <Cu loading> The NH₄ of Example 2 + 120 g of the CHA-type aluminosilicate of the NH₄ type of Example 2 was impregnated with a mixed solution of 34.6 g of an aqueous solution of 50% copper nitrate trihydrate and 26 g of water, and then dried at 100 - 120 °C. This was impregnated with a mixed solution of 12.0 g of morpholine and 48 g of water (pH 11.0) and dried again at 100 - 120 °C to obtain the Cu-supported CHA-type aluminosilicate (Cu-supported CHA-type zeolite) of Comparative Example 3.
[0127] <Manufacture of honeycomb laminated catalyst> Thereafter, a honeycomb laminated catalyst of Comparative Example 3 was obtained in the same manner as in Example 1 except that the obtained Cu-supported CHA-type aluminosilicate of Comparative Example 3 was used.
[0128] <Laboratory measurement of nitrogen oxide reduction efficiency> The honeycomb laminated catalyst (a laminated catalyst in which Cu-supported CHA-type aluminosilicate was applied to a honeycomb carrier) was cut into a cylindrical shape with a diameter of 25.4 mmφ×length of 50 mm to prepare each measurement sample, which was then placed in an electric furnace (product name OXK-600X, manufactured by Kyoei Electric Furnace Manufacturing Co., Ltd.) connected to a gas humidifier (product name RMG-1000, manufactured by J-Science Lab Co., Ltd.) and subjected to hydrothermal durability by holding at 650°C for 100 hours or at 750°C for 40 hours under a flow rate of 70 L / min of air containing 10% water vapor. The samples after hydrothermal durability were set in a catalyst evaluation device (product name SIGU-2000, manufactured by Horiba, Ltd.), and the gas composition was analyzed with an automobile exhaust gas measurement device (product name MEXA-6000FT, manufactured by Horiba, Ltd.) to measure the nitrogen oxide reduction efficiency in a steady air flow of a model gas. Here, a model gas containing 210 ppm NO, 40 ppm NO2, 250 ppm NH3, 4% H2O, 10% O2, and the balance N2 was used. Measurements were performed in the temperature range of 170°C to 500°C, with a space velocity of SV = 59,000 h -1 So I went.
[0129] The results are shown in Table 1. [Table 1]
[0130] Example 3 <Preparation of the mixture> 1,270.0 g of 1,1,3,5-tetramethylpiperidinium hydroxide 20% aqueous solution (Sachem, hereinafter sometimes referred to as "TMPOH 20% aqueous solution") was added with 1,060 g of pure water, 166.0 g of FAU type zeolite (Zeolyst, trade name: CBV-712, SAR10.9) as a Si-Al element source, and 1,830.0 g of J sodium silicate No. 3 solution (Nippon Chemical Industry, SiO2 content: 29.0 mass%) as a Si element source, and mixed thoroughly to obtain a raw material composition (mixture). The composition of the raw material composition was SiO2: 0.016Al2O3: 0.152TMPOH: 0.261Na2O: 16.7H2O in molar ratio.
[0131] <Synthesis of AEI-Type Aluminosilicate> This raw material composition (mixture) was put into a 5,000 cc stainless steel autoclave and sealed. Then, while stirring at 200 rpm, the temperature was raised to 150 °C and held for 96 hours, and further raised to 160 °C and held for 24 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, the obtained solid phase was washed with a sufficient amount of water, and dried at 105 °C to obtain the product. When powder X-ray diffraction analysis was performed, it was confirmed that the product was a single phase of pure AEI-type aluminosilicate. When fluorescence X-ray analysis was performed, the silica-alumina ratio (SiO2 / Al2O3) of the AEI-type aluminosilicate of Example 3 obtained was 14.3.
[0132] <Firing and Ion Exchange of AEI-Type Aluminosilicate> After firing the obtained AEI-type aluminosilicate of Example 3 at 594 °C, ion exchange was repeated twice using an ammonium nitrate aqueous solution containing the same amount of ammonium nitrate and 10 times the amount of water, then washed with a sufficient amount of pure water, and dried at 120 °C to obtain an NH4 + -type AEI-type aluminosilicate (NH4 + -type AEI-type zeolite).
[0133] <Cu-Supported, P-Supported> 149 g of the obtained NH4 + -type AEI-type aluminosilicate was impregnated with a mixture of 39.5 g of a 50% aqueous solution of copper(II) nitrate trihydrate and 35 g of water, and then dried at 100 - 120 °C. This was impregnated with a mixture of 6 g of 85% phosphoric acid, 12 g of morpholine, and 62 g of water (treatment solution, pH = 7.5) in an environment at 25 °C, and dried again at 100 - 120 °C to obtain the Cu-P co-supported AEI-type aluminosilicate (Cu-P co-supported AEI-type zeolite) of Example 3. The supported amount of Cu in terms of solid content measured by fluorescence X-ray analysis was 3.9 mass%, and the supported amount of P was 1.2 mass%.
[0134] <Manufacture of Honeycomb-Laminated Catalyst> The obtained Cu-P co-supported AEI type aluminosilicate of Example 3 was wet-coated onto a honeycomb carrier to give a loading ratio of 180 g per 1 L of honeycomb carrier, and then fired at 500°C to obtain a honeycomb laminated catalyst of Example 3, in which a catalyst layer containing Cu-P co-supported AEI type aluminosilicate was provided on a honeycomb carrier.
[0135] Comparative Example 4 NH4 obtained in the same manner as in Example 3 + A Cu-supported AEI type aluminosilicate was used, and the addition of phosphoric acid was omitted during Cu support to not support P. The same procedure as in Example 3 was carried out to obtain a Cu-supported AEI type aluminosilicate (Cu-supported AEI type zeolite) of Comparative Example 4. The amount of Cu supported in terms of solid content measured by fluorescent X-ray analysis was 4.0 mass%. Moreover, a honeycomb laminated catalyst of Comparative Example 4 was obtained by the same procedure as in Example 3, except that the Cu-supported AEI type aluminosilicate of Comparative Example 4 was used.
[0136] The honeycomb laminated catalysts of Example 3 and Comparative Example 4 were subjected to performance evaluation in the same manner as in Example 1. Table 2 shows the results. [Table 2]
[0137] Example 4 <Preparation of the mixture> To 2,050.0 g of an aqueous solution of tetrapropylammonium hydroxide (40% aqueous solution, hereinafter sometimes referred to as "40% aqueous TPAOH solution"), 700 g of pure water, 107 g of solid powder aluminum hydroxide (manufactured by Sigma-Aldrich), which is an Al element source, and 650.0 g of amorphous silica (manufactured by Tosoh Silica Corporation, trade name: Nipsil (registered trademark) E200A, SiO2 content: 93.8% by mass), which is an Si element source, were added and thoroughly mixed, and then held at 95 °C for 24 hours. To this, 250.0 g of pure water, a solution prepared by dissolving hexamethonium chloride dihydrate (manufactured by Tokyo Chemical Industry Co., Ltd.) in 630.0 g of pure water, and a solution prepared by dissolving 60.0 g of potassium hydroxide (manufactured by Fujifilm Wako Pure Chemical Corporation, content 85% or more) in 130.0 g of pure water were each added and thoroughly mixed to obtain a raw material composition (mixture). The composition of the raw material composition was, in molar ratio, SiO2:0.060 Al2O3:0.397 TPAOH:0.105 hexamethonium:0.046 K2O:16.6 H2O.
[0138] <Synthesis of ERI-type aluminosilicate> This raw material composition (mixture) was charged into a 5,000 cc stainless steel autoclave and sealed, and then heated to 125 °C while stirring at 70 rpm and held for 120 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, the obtained solid phase was washed with a sufficient amount of water, and dried at 105 °C to obtain a product. When powder X-ray diffraction analysis was performed, it was confirmed that the product was a single phase of pure ERI-type aluminosilicate. When fluorescence X-ray analysis was performed, the silica-alumina ratio (SiO2 / Al2O3) of the ERI-type aluminosilicate of Example 4 obtained was 14.3.
[0139] <Firing and ion exchange of ERI-type aluminosilicate> The obtained ERI-type aluminosilicate of Example 4 was fired at 550 °C, and then ion exchange was repeated three times using an ammonium nitrate aqueous solution containing 1.5 times the amount of ammonium nitrate and 10 times the amount of water, and then washed with a sufficient amount of pure water and dried at 120 °C to obtain an NH4 + type ERI-type aluminosilicate (NH4 + type ERI-type zeolite).
[0140] <Cu-supported, P-supported> The obtained NH4 + 132 g of the NH4 type ERI-type aluminosilicate was impregnated with a mixture of 26.3 g of a 50% aqueous solution of copper nitrate trihydrate and 40 g of water, and then dried at 100 - 120 °C. This was impregnated with a mixture of 3.1 g of 85% phosphoric acid, 9.3 g of morpholine, and 49.3 g of water (treatment solution, pH = 7.6) in an environment at 25 °C, and dried again at 100 - 120 °C to obtain the Cu-P co-supported ERI-type aluminosilicate (Cu-P co-supported ERI-type zeolite) of Example 4. The supported amount of Cu in terms of solid content measured by X-ray fluorescence analysis was 2.8 mass%, and the supported amount of P was 1.3 mass%.
[0141] <Manufacture of honeycomb laminated catalyst> The obtained Cu-P co-supported ERI-type aluminosilicate of Example 4 was wet-coated on a honeycomb carrier at a loading ratio of 180 g per liter of the honeycomb carrier, and then calcined at 500 °C to obtain the honeycomb laminated catalyst of Example 4 in which a catalyst layer containing the Cu-P co-supported ERI-type aluminosilicate was provided on the honeycomb carrier.
[0142] (Comparative Example 5) The NH4 type ERI-type aluminosilicate obtained in Example 4 was used, and Cu-supported ERI-type aluminosilicate (Cu-supported ERI-type zeolite) of Comparative Example 5 was obtained in the same manner as in Example 4 except that the addition of phosphoric acid was omitted during Cu loading and P loading was not performed. The supported amount of Cu in terms of solid content measured by X-ray fluorescence analysis was 2.9 mass%. Also, the honeycomb laminated catalyst of Comparative Example 5 was obtained in the same manner as in Example 4 except that the Cu-supported ERI-type aluminosilicate of this Comparative Example 5 was used. + Performance evaluation was carried out on the honeycomb laminated catalysts of Example 4 and Comparative Example 5 in the same manner as in Example 1. The results are shown in Table 3.
[0143]
Table 3
Industrial Applicability
[0144] The Cu-P co-supported zeolite of the present invention has excellent thermal durability and can maintain relatively high adsorption and catalytic performances even in a high-temperature environment or after exposure to high temperatures, and therefore can be widely and effectively used in applications such as adsorbents, separators, ion exchangers, adsorbents, catalysts, catalyst carriers, etc. In particular, the Cu-P co-supported zeolite of the present invention can be particularly effectively used as exhaust gas purification catalysts or catalyst carriers thereof, nitrogen oxide catalysts or catalyst carriers thereof, etc., for purifying exhaust gases from diesel automobiles, gasoline automobiles, jet engines, boilers, gas turbines, etc., which are exposed to harsh operating environments.
Claims
1. The present invention comprises at least a small pore zeolite and an extra-framework copper atom and an extra-framework phosphorus atom supported on the small pore zeolite, The small pore zeolite has a framework structure of CHA as measured by powder X-ray diffraction, The small pore zeolite has a crystallite size of 15 nm or more and 100 nm or less as measured by powder X-ray diffraction, Silica-alumina ratio (SiO 2 / Al 2 O 3 ) is 7 or more and 20 or less, The ratio of copper atoms to T atoms (Cu / T) is 0.005 or more and 0.060 or less, the ratio of phosphorus atoms to T atoms (P / T) is 0.005 or more and 0.060 or less; The ratio of phosphorus atoms to copper atoms (P / Cu) is 1.0 or more and 1.5 or less; Cu-P co-supported zeolite.
2. The present invention comprises at least a small pore zeolite and an extra-framework copper atom and an extra-framework phosphorus atom supported on the small pore zeolite, The small pore zeolite has a framework structure of CHA as measured by powder X-ray diffraction, having an average particle size D50 of 0.01 μm or more and 20 μm or less; Silica-alumina ratio (SiO 2 / Al 2 O 3 ) is 7 or more and 20 or less, The ratio of copper atoms to T atoms (Cu / T) is 0.005 or more and 0.060 or less, the ratio of phosphorus atoms to T atoms (P / T) is 0.005 or more and 0.060 or less; The ratio of phosphorus atoms to copper atoms (P / Cu) is 1.0 or more and 1.5 or less; Cu-P co-supported zeolite.
3. The small pore zeolite has an 8-membered oxygen ring structure. The Cu-P co-supported zeolite according to claim 1 or 2.
4. A catalyst comprising at least the Cu-P co-supported zeolite according to any one of claims 1 to 3. Selective reduction catalyst.
5. A composition comprising the Cu-P co-supported zeolite according to any one of claims 1 to 3, which is formed into a predetermined shape. Selective reduction catalyst molded body.
6. The present invention comprises at least a support and a catalyst layer provided on at least one surface of the support, The catalyst layer contains at least the Cu-P co-supported zeolite according to any one of claims 1 to 3. Exhaust gas catalyst.
Citation Information
Patent Citations
Phase locked oscillation circuit
JP1988020918A
Copper CHA zeolite catalysts
JP2010519038A
AEI zeolite containing phosphorus, and method for producing the same
JP2015134698A
CHA type zeolite comprising phosphorus and method for producing the same
JP2017048106A
NOx SELECTIVE REDUCTION CATALYST AND NOx PURIFICATION METHOD USING THE SAME
JP2018020295A