Method for manufacturing a semiconductor device

The use of multiple oxide layers with controlled oxygen diffusion and CAAC-OS in semiconductor devices addresses variations and reliability issues, enhancing electrical performance and integration capabilities while reducing power consumption.

JP7555906B2Active Publication Date: 2024-09-25SEMICON ENERGY LAB CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021510575
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-19
Publication Date
2024-09-25
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Existing semiconductor devices using oxide semiconductors face challenges with variations in transistor characteristics, reliability, electrical performance, miniaturization, integration, and power consumption, particularly due to issues with oxygen diffusion and impurity incorporation.

Method used

A manufacturing method involving the formation of multiple oxide layers with controlled oxygen diffusion and impurity suppression, using CAAC-OS (c-axis aligned crystalline oxide semiconductor) to reduce variations and enhance reliability, electrical characteristics, and integration capabilities.

Benefits of technology

The method results in semiconductor devices with reduced transistor characteristic variations, improved reliability, enhanced electrical performance, increased on-current, and potential for miniaturization and high integration, while maintaining low power consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555906000001
    Figure 0007555906000001
  • Figure 0007555906000002
    Figure 0007555906000002
  • Figure 0007555906000003
    Figure 0007555906000003
Patent Text Reader

Abstract

A semiconductor device is provided in which variation of transistor characteristics is low. A first insulation body, a first oxide film, a second oxide film, a first electroconductive film, a first insulation film, and a second electroconductive film are formed, in the stated order, on a substrate, and processed in island shapes to form a first oxide, a second oxide, a first electroconductive layer, a first insulation layer, and a second electroconductive layer; during the processing, a layer is formed covering the first oxide, the second oxide, the first electroconductive layer, the first insulation layer, and the second electroconductive layer, and the second electroconductive layer and the layer are removed; a second insulation layer is formed contacting the side surfaces of the first oxide, the second oxide, the first electroconductive layer, and the first insulation layer, and a second insulation body is formed thereon; and an opening reaching the second oxide is formed in the first electroconductive layer, the first insulation layer, the second insulation layer, and the second insulation body.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] 1. Field of the Invention An embodiment of the present invention relates to a transistor, a semiconductor device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of a semiconductor device. Another embodiment of the present invention relates to a semiconductor wafer and a module.

[0002] In this specification and the like, a semiconductor device refers to any device that can function by utilizing semiconductor characteristics. Semiconductor elements such as transistors, semiconductor circuits, arithmetic devices, and memory devices are all embodiments of semiconductor devices. Display devices (such as liquid crystal display devices and light-emitting display devices), projection devices, lighting devices, electro-optical devices, power storage devices, memory devices, semiconductor circuits, imaging devices, electronic devices, and the like may be considered to include semiconductor devices.

[0003] Note that one aspect of the present invention is not limited to the above technical field. One aspect of the invention disclosed in the present specification etc. relates to an object, a method, or a manufacturing method. Another aspect of the present invention relates to a process, a machine, a manufacture, or a composition of matter. [Background technology]

[0004] Technology that constructs transistors using semiconductor thin films formed on substrates with insulating surfaces is attracting attention. Such transistors are widely used in electronic devices such as integrated circuits (ICs) and image display devices (also simply referred to as display devices). Silicon-based semiconductor materials are widely known as semiconductor thin films that can be used in transistors, but oxide semiconductors are also attracting attention as other materials.

[0005] In oxide semiconductors, c-axis aligned crystalline (CAAC) structures and nanocrystalline (nc) structures, which are neither single crystal nor amorphous, have been found (see Non-Patent Documents 1 and 2).

[0006] Non-Patent Documents 1 and 2 disclose techniques for manufacturing a transistor using an oxide semiconductor having a CAAC structure. [Prior art documents] [Non-patent literature]

[0007] [Non-Patent Document 1] S. Yamazaki et al., “SID Symposium Digest of Technical Papers”, 2012, volume 43, issue 1, p.183-186 [Non-Patent Document 2] S. Yamazaki et al., “Japanese Journal of Applied Physics”, 2014, volume 53, Number 4S, p.04ED18-1-04ED18-10 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of one embodiment of the present invention is to provide a semiconductor device with little variation in transistor characteristics. Another object of one embodiment of the present invention is to provide a semiconductor device with high reliability. Another object of one embodiment of the present invention is to provide a semiconductor device having good electrical characteristics. Another object of one embodiment of the present invention is to provide a semiconductor device with large on-state current. Another object of one embodiment of the present invention is to provide a semiconductor device that can be miniaturized or highly integrated. Another object of one embodiment of the present invention is to provide a semiconductor device with low power consumption.

[0009] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these will become apparent from the description of the specification, drawings, claims, etc., and it is possible to extract problems other than these from the description of the specification, drawings, claims, etc. [Means for solving the problem]

[0010] One embodiment of the present invention includes forming a first insulator, a first oxide film, a second oxide film, a first conductive film, a first insulating film, and a second conductive film in this order on a substrate, processing the first oxide film, the second oxide film, the first conductive film, the first insulating film, and the second conductive film into an island shape to form a first oxide, a second oxide, a first conductive layer, a first insulating layer, and a second conductive layer, forming a layer covering the first oxide, the second oxide, the first conductive layer, the first insulating layer, and the second conductive layer in the processing, removing the second conductive layer, and forming a second insulating film on the first insulator, the first oxide, the second oxide, the first conductive layer, and the first insulating layer, and anisotropically etching the second insulating film to form the first oxide, the second oxide, and the second conductive layer. A method for manufacturing a semiconductor device includes forming a first conductive layer and a second insulating layer in contact with a side surface of the first insulating layer, forming a second insulator on the first insulator, first oxide, second oxide, first conductive layer, first insulating layer, and second insulating layer, and forming openings in the first conductive layer, first insulating layer, second insulating layer, and second insulator reaching the second oxide, and in forming the openings, a first conductor and a second conductor are formed from the first conductive layer, a third insulator and a fourth insulator are formed from the first insulating layer, a fifth insulator and a sixth insulator are formed from the second insulating layer, and forming a third oxide, a seventh insulator on the third oxide, and a third conductor on the seventh insulator in the openings.

[0011] In the above, the second conductive layer and the layer are preferably removed by dry etching. Also, in the above, it is preferable that the layer contains a main component of the second conductive layer.

[0012] In the above, it is preferable that an eighth insulator is formed on the second insulator, the third oxide, the seventh insulator, and the third conductor by using a sputtering method in an atmosphere containing oxygen.

[0013] In the above, the third to sixth insulators are preferably capable of suppressing oxygen diffusion more than the second insulator. Also, in the above, the first oxide is preferably capable of suppressing oxygen diffusion more than the second oxide.

[0014] In the above, it is preferable to carry out a heat treatment at a temperature of 400° C. or more and 600° C. or less after the formation of the second oxide film. Effect of the Invention

[0015] According to one embodiment of the present invention, a semiconductor device with little variation in transistor characteristics can be provided. According to one embodiment of the present invention, a semiconductor device with high reliability can be provided. According to one embodiment of the present invention, a semiconductor device with good electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device with large on-state current can be provided. According to one embodiment of the present invention, a semiconductor device that can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a semiconductor device with low power consumption can be provided.

[0016] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not need to have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract effects other than these from the description in the specification, drawings, claims, etc. [Brief description of the drawings]

[0017] Fig. 1A is a top view of a semiconductor device according to one embodiment of the present invention, and Figs. 1B to 1D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. FIG. 2 is a cross-sectional view of a semiconductor device according to an embodiment of the present invention. 3A and 3B are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Fig. 4A is a diagram explaining the classification of crystal structures. Fig. 4B is a diagram explaining the XRD spectrum of quartz glass. Fig. 4C is a diagram explaining the XRD spectrum of crystalline IGZO. Fig. 4D is a diagram explaining the ultrafine electron beam diffraction pattern of crystalline IGZO. Fig. 5A is a top view of a semiconductor device according to one embodiment of the present invention, and Figs. 5B to 5D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. 6A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 6B to 6D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 7A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 7B to 7D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 8A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 8B to 8D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 9A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 9B to 9D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 10A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 10B to 10D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 11A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 11B to 11D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 12A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 12B to 12D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 13A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 13B to 13D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 14A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 14B to 14D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 15A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIG 15B to FIG 15D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 16A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 16B to 16D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 17A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 17B to 17D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 18A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 18B to 18D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 19A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 19B to 19D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 20A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 20B to 20D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 21A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 21B to 21D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 22A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 22B to 22D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 23A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 23B to 23D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 24A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 24B to 24D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 25A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 25B to 25D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 26A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 26B to 26D are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. 27A and 27B are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Fig. 28A is a top view of a semiconductor device according to one embodiment of the present invention, and Fig. 28B to Fig. 28D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. Fig. 29A is a top view of a semiconductor device according to one embodiment of the present invention, and Fig. 29B to Fig. 29D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. Fig. 30A is a top view of a semiconductor device according to one embodiment of the present invention, and Fig. 30B to Fig. 30D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. Fig. 31A is a top view of a semiconductor device according to one embodiment of the present invention, and Figs. 31B to 31D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. Fig. 32A is a top view of a semiconductor device according to one embodiment of the present invention, and Figs. 32B to 32D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. Fig. 33A is a top view of a semiconductor device according to one embodiment of the present invention, and Fig. 33B to Fig. 33D are cross-sectional views of the semiconductor device according to one embodiment of the present invention. 34A and 34B are cross-sectional views of a semiconductor device according to one embodiment of the present invention. FIG. 35 is a cross-sectional view illustrating a configuration of a memory device according to one embodiment of the present invention. FIG. 36 is a cross-sectional view illustrating a configuration of a memory device according to one embodiment of the present invention. FIG. 37 is a cross-sectional view of a semiconductor device according to one embodiment of the present invention. 38A and 38B are cross-sectional views of a semiconductor device according to one embodiment of the present invention. FIG. 39 is a cross-sectional view of a semiconductor device according to one embodiment of the present invention. FIG. 40 is a cross-sectional view of a semiconductor device according to one embodiment of the present invention. 41A is a block diagram illustrating a configuration example of a storage device according to one embodiment of the present invention, and FIG 41B is a schematic diagram illustrating a configuration example of a storage device according to one embodiment of the present invention. 42A to 42H are circuit diagrams illustrating configuration examples of a memory device according to one embodiment of the present invention. FIG. 43 is a diagram showing various storage devices by hierarchy. 44A and 44B are schematic diagrams of a semiconductor device according to one embodiment of the present invention. 45A and 45B are diagrams illustrating an example of an electronic component. 46A to 46E are schematic diagrams of a memory device according to one embodiment of the present invention. 47A to 47H are diagrams showing electronic devices according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments will be described with reference to the drawings. However, it will be easily understood by those skilled in the art that the embodiments can be implemented in many different ways, and that the modes and details can be changed in various ways without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the following embodiments.

[0019] In addition, in the drawings, the size, thickness of layers, or areas may be exaggerated for clarity. Therefore, the drawings are not necessarily limited to the scale. The drawings are schematic illustrations of ideal examples, and are not limited to the shapes or values ​​shown in the drawings. For example, in an actual manufacturing process, layers, resist masks, etc. may be unintentionally thinned by etching or other processes, but this may not be reflected in the drawings to facilitate understanding. In addition, in the drawings, the same reference numerals are used in common between different drawings for the same parts or parts having similar functions, and repeated explanations may be omitted. In addition, when referring to similar functions, the same hatch pattern may be used and no particular reference numeral may be attached.

[0020] In order to facilitate understanding of the invention, particularly in top views (also called "plan views") and perspective views, some components may be omitted from the drawings. Also, some hidden lines may be omitted from the drawings.

[0021] In addition, in this specification, ordinal numbers such as first, second, etc. are used for convenience and do not indicate the order of steps or stacking. Therefore, for example, "first" can be appropriately replaced with "second" or "third" for explanation. In addition, the ordinal numbers described in this specification and the like may not match the ordinal numbers used to specify one embodiment of the present invention.

[0022] In addition, in this specification, the terms "above" and "below" indicating the arrangement are used for convenience in order to explain the positional relationship between the components with reference to the drawings. In addition, the positional relationship between the components changes as appropriate depending on the direction in which each component is depicted. Therefore, the terms are not limited to those described in the specification, and can be rephrased appropriately depending on the situation.

[0023] For example, when it is explicitly stated in this specification that X and Y are connected, the case where X and Y are electrically connected, the case where X and Y are functionally connected, and the case where X and Y are directly connected are considered to be disclosed in this specification. Therefore, it is not limited to a specific connection relationship, for example, a connection relationship shown in a figure or text, and a connection relationship other than that shown in a figure or text is also considered to be disclosed in the figure or text. Here, X and Y are objects (for example, a device, an element, a circuit, wiring, an electrode, a terminal, a conductive film, a layer, etc.).

[0024] In this specification, a transistor is an element having at least three terminals including a gate, a drain, and a source. A region where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode) (hereinafter, also referred to as a channel formation region) is provided, and a current can flow between the source and the drain through the channel formation region. In this specification, a channel formation region refers to a region through which a current mainly flows.

[0025] Furthermore, the functions of the source and drain may be interchanged when transistors of different polarities are used, when the direction of current changes during circuit operation, etc. For this reason, in this specification and the like, the terms source and drain may be used interchangeably.

[0026] The channel length refers to, for example, a region where the semiconductor (or a portion in the semiconductor through which current flows when the transistor is on) and the gate electrode overlap in a top view of a transistor, or a distance between the source (source region or source electrode) and the drain (drain region or drain electrode) in a channel formation region. Note that the channel length of one transistor does not necessarily have the same value in all regions. That is, the channel length of one transistor may not be fixed to one value. Therefore, in this specification, the channel length is defined as any one value, maximum value, minimum value, or average value in the channel formation region.

[0027] The channel width refers to, for example, the length of a channel formation region in a vertical direction based on the channel length direction in a region where a semiconductor (or a portion in the semiconductor through which current flows when the transistor is on) and a gate electrode overlap in a top view of a transistor, or in a channel formation region. Note that the channel width does not necessarily have the same value in all regions in one transistor. In other words, the channel width of one transistor may not be determined to a single value. Therefore, in this specification, the channel width is defined as any one value, maximum value, minimum value, or average value in the channel formation region.

[0028] In this specification and the like, depending on the structure of a transistor, the channel width in a region where a channel is actually formed (hereinafter also referred to as an "effective channel width") may differ from the channel width shown in a top view of the transistor (hereinafter also referred to as an "apparent channel width"). For example, when a gate electrode covers a side surface of a semiconductor, the effective channel width may be larger than the apparent channel width, and the influence of this may not be negligible. For example, in a fine transistor in which a gate electrode covers a side surface of a semiconductor, the proportion of a channel formation region formed on the side surface of the semiconductor may be large. In that case, the effective channel width is larger than the apparent channel width.

[0029] In such a case, it may be difficult to estimate the effective channel width by actual measurement. For example, in order to estimate the effective channel width from the design value, it is necessary to assume that the shape of the semiconductor is known. Therefore, if the shape of the semiconductor is not precisely known, it is difficult to accurately measure the effective channel width.

[0030] In this specification, when simply described as a channel width, it may refer to an apparent channel width. Alternatively, when simply described as a channel width, it may refer to an effective channel width. Note that the values ​​of the channel length, channel width, effective channel width, apparent channel width, etc. can be determined by analyzing a cross-sectional TEM image, etc.

[0031] Note that impurities in a semiconductor refer to, for example, anything other than the main components constituting the semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity. The inclusion of impurities can, for example, increase the density of defect states in the semiconductor or reduce the crystallinity. When the semiconductor is an oxide semiconductor, impurities that change the characteristics of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor, such as hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Note that water can also function as an impurity. For example, the inclusion of impurities can cause oxygen deficiencies (V O :oxygen vacancy) may be formed.

[0032] In this specification and the like, silicon oxynitride refers to a material having a composition that contains more oxygen than nitrogen, and silicon nitride oxide refers to a material having a composition that contains more nitrogen than oxygen.

[0033] In this specification and the like, the term "insulator" can be replaced with an insulating film or an insulating layer, the term "conductor" can be replaced with a conductive film or a conductive layer, and the term "semiconductor" can be replaced with a semiconductor film or a semiconductor layer.

[0034] In addition, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes the case of -5 degrees or more and 5 degrees or less. "Approximately parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. "Perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes the case of 85 degrees or more and 95 degrees or less. "Approximately perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.

[0035] In this specification and the like, the term "metal oxide" refers to an oxide of a metal in a broad sense. Metal oxides are classified into oxide insulators, oxide conductors (including transparent oxide conductors), oxide semiconductors (also referred to as oxide semiconductors or simply OS), and the like. For example, when a metal oxide is used for a semiconductor layer of a transistor, the metal oxide may be referred to as an oxide semiconductor. In other words, an OS transistor can be rephrased as a transistor having a metal oxide or an oxide semiconductor.

[0036] In this specification and the like, normally off means that when no potential is applied to the gate or when a ground potential is applied to the gate, the drain current flowing through the transistor per 1 μm of channel width is 1×10 -20 A or less, 1×10 at 85℃ -18 A or less, or 1×10 at 125°C -16 This means that it is A or lower.

[0037] (Embodiment 1) In this embodiment, an example of a semiconductor device including a transistor 200 according to one embodiment of the present invention and a manufacturing method thereof will be described with reference to FIGS.

[0038] <Example of semiconductor device configuration> A configuration of a semiconductor device having a transistor 200 will be described with reference to FIG. 1. FIGS. 1A to 1D are a top view and a cross-sectional view of a semiconductor device having a transistor 200. FIG. 1A is a top view of the semiconductor device. FIGS. 1B to 1D are cross-sectional views of the semiconductor device. FIG. 1B is a cross-sectional view of a portion indicated by a dashed line A1-A2 in FIG. 1A, and is also a cross-sectional view of the transistor 200 in the channel length direction. FIG. 1C is a cross-sectional view of a portion indicated by a dashed line A3-A4 in FIG. 1A, and is also a cross-sectional view of the transistor 200 in the channel width direction. FIG. 1D is a cross-sectional view of a portion indicated by a dashed line A5-A6 in FIG. 1A. Note that some elements are omitted from the top view of FIG. 1A for clarity.

[0039] The semiconductor device of one embodiment of the present invention includes an insulator 211 on a substrate (not shown), an insulator 212 on the insulator 211, an insulator 214 on the insulator 212, a transistor 200 on the insulator 214, an insulator 280 on the transistor 200, an insulator 282 on the insulator 280, an insulator 283 on the insulator 282, and an insulator 284 on the insulator 283. The insulators 211, 212, 214, 280, 282, 283, and 284 function as interlayer films. The semiconductor device also includes a conductor 240 (conductor 240a and conductor 240b) that is electrically connected to the transistor 200 and functions as a plug. Note that an insulator 241 (insulator 241a and insulator 241b) is provided in contact with a side surface of the conductor 240 that functions as a plug. Moreover, a conductor 246 (conductor 246a and conductor 246b) that is electrically connected to the conductor 240 and functions as wiring is provided on the insulator 284 and on the conductor 240. Furthermore, an insulator 286 is provided on the conductor 246 and on the insulator 284.

[0040] Insulator 241a is provided in contact with the inner walls of the openings of insulators 271, 280, 282, 283, and 284, a first conductor of conductor 240a is provided in contact with the side surface of insulator 241a, and a second conductor of conductor 240a is provided further inward. Insulator 241b is provided in contact with the inner walls of the openings of insulators 271, 280, 282, 283, and 284, a first conductor of conductor 240b is provided in contact with the side surface of insulator 241b, and a second conductor of conductor 240b is provided further inward. Here, the height of the top surface of conductor 240 and the height of the top surface of insulator 284 in the region overlapping with conductor 246 can be made to be approximately the same. Note that, although the transistor 200 shows a structure in which the first conductor of the conductor 240 and the second conductor of the conductor 240 are stacked, the present invention is not limited to this. For example, the conductor 240 may be provided as a single layer or a stacked structure of three or more layers. When the structure has a stacked structure, the structures may be distinguished by giving ordinal numbers in the order of formation.

[0041] [Transistor 200] As shown in FIGS. 1A to 1D , the transistor 200 includes an insulator 216 on an insulator 214, a conductor 205 (conductor 205a and conductor 205b) disposed so as to be embedded in the insulator 216, an insulator 222 on the insulator 216 and on the conductor 205, an insulator 224 on the insulator 222, an oxide 230a on the insulator 224, an oxide 230b on the oxide 230a, an oxide 243 (oxide 243a and oxide 243b) and an oxide 230c on the oxide 230b, a conductor 242a on the oxide 243a, and a conductor 242b on the oxide 243a. The oxide 230c has an insulator 271a on the oxide 242a, a conductor 242b on the oxide 243b, an insulator 271b on the conductor 242b, an oxide 230d on the oxide 230c, an insulator 250 on the oxide 230d, a conductor 260 (conductor 260a and conductor 260b) located on the insulator 250 and overlapping with a part of the oxide 230c, an insulator 272a in contact with the side of the oxide 230b, the side of the oxide 243a, and the side of the conductor 242a, and an insulator 272b in contact with the side of the oxide 230b, the side of the oxide 243b, and the side of the conductor 242b. The oxide 230c also has a side of the oxide 243a in contact with the side of the oxide 243b, the side of the conductor 242a, and the side of the conductor 242b. 1B and 1C, the upper surface of the conductor 260 is disposed so as to be substantially flush with the upper surfaces of the insulator 250, the oxide 230d, and the oxide 230c. The insulator 282 contacts the upper surfaces of the conductor 260, the insulator 250, the oxide 230d, the oxide 230c, and the insulator 280.

[0042] In the following, the insulator 271a and the insulator 271b may be collectively referred to as the insulator 271. Furthermore, the insulator 272a and the insulator 272b may be collectively referred to as the insulator 272. Furthermore, the conductor 242a and the conductor 242b may be collectively referred to as the conductor 242.

[0043] An opening is provided in the insulator 280, reaching the oxide 230b. The oxide 230c, the oxide 230d, the insulator 250, and the conductor 260 are disposed in the opening. In addition, in the channel length direction of the transistor 200, the conductor 260, the insulator 250, the oxide 230d, and the oxide 230c are provided between the conductor 242a and the oxide 243a and between the conductor 242b and the oxide 243b. The insulator 250 has a region in contact with the side surface of the conductor 260 and a region in contact with the bottom surface of the conductor 260. In addition, in the region overlapping with the oxide 230b, the oxide 230c has a region in contact with the oxide 230b, a region facing the side surface of the conductor 260 through the oxide 230d and the insulator 250, and a region overlapping with the bottom surface of the conductor 260 through the oxide 230d and the insulator 250.

[0044] The oxide 230 preferably includes an oxide 230a arranged on the insulator 224, an oxide 230b arranged on the oxide 230a, an oxide 230c arranged on the oxide 230b and at least a part of which is in contact with the oxide 230b, and an oxide 230d arranged on the oxide 230c. By having the oxide 230a below the oxide 230b, it is possible to suppress the diffusion of impurities from structures formed below the oxide 230a to the oxide 230b. Also, by having the oxide 230d on the oxide 230c, it is possible to suppress the diffusion of impurities from structures formed above the oxide 230d to the oxide 230c.

[0045] Note that, in the transistor 200, the oxide 230 has a structure in which four layers of the oxide 230a, the oxide 230b, the oxide 230c, and the oxide 230d are stacked, but the present invention is not limited to this. For example, the oxide 230 may have a single layer of the oxide 230b, a two-layer structure of the oxide 230a and the oxide 230b, a two-layer structure of the oxide 230b and the oxide 230c, a three-layer structure of the oxide 230a, the oxide 230b, and the oxide 230c, or a stacked structure of five or more layers. Alternatively, each of the oxide 230a, the oxide 230b, the oxide 230c, and the oxide 230d may have a stacked structure.

[0046] The conductor 260 functions as a first gate (also referred to as a top gate) electrode, and the conductor 205 functions as a second gate (also referred to as a back gate) electrode. The insulator 250 functions as a first gate insulator, and the insulator 224 functions as a second gate insulator. The conductor 242a functions as one of a source or a drain, and the conductor 242b functions as the other of the source or the drain. At least a part of a region of the oxide 230 that overlaps with the conductor 260 functions as a channel formation region.

[0047] Here, an enlarged view of the vicinity of the channel formation region in FIG. 1B is shown in FIG. 2. As shown in FIG. 2, the oxide 230 has a region 234 that functions as a channel formation region of the transistor 200, and regions 236 (regions 236a and 236b) that function as a source region or drain region and are provided to sandwich the region 234. At least a portion of the region 234 overlaps with the conductor 260. A conductor 242 is provided on the oxide 230b, and a lower resistance region is formed near the conductor 242 in the region 236.

[0048] The region 236 functioning as a source region or drain region is a region with a low oxygen concentration or an increased carrier concentration and low resistance due to the inclusion of impurities such as hydrogen, nitrogen, and metal elements. That is, the region 236 is a region with a high carrier concentration and low resistance compared to the region 234. The region 234 functioning as a channel formation region is a high-resistance region with a low carrier concentration because it has a higher oxygen concentration or a lower impurity concentration than the region 236. A region may be formed between the region 234 and the region 236, in which the oxygen concentration is equal to or higher than the oxygen concentration of the region 236 and equal to or lower than the oxygen concentration of the region 234.

[0049] 2, the width of the region 234 in the channel length direction coincides with the conductor 260; however, this is not limited to this embodiment of the present invention. The width of the region 234 may be shorter than the conductor 260, or the width of the region 234 may be longer than the conductor 260.

[0050] In addition, it may be difficult to clearly detect the boundaries between the regions in the oxide 230. The concentrations of metal elements, hydrogen, nitrogen, and other impurity elements detected in each region may not only vary stepwise from region to region, but may also vary continuously within each region. In other words, it is sufficient that the concentrations of metal elements, hydrogen, nitrogen, and other impurity elements decrease in the region closer to the channel formation region.

[0051] In the transistor 200, it is preferable to use a metal oxide that functions as a semiconductor (hereinafter also referred to as an oxide semiconductor) for the oxide 230 (the oxide 230a, the oxide 230b, the oxide 230c, and the oxide 230d) including a channel formation region.

[0052] In addition, the metal oxide functioning as a semiconductor preferably has a band gap of 2 eV or more, more preferably 2.5 eV or more. By using a metal oxide having a wide band gap in this way, the off-state current of a transistor can be reduced.

[0053] As the oxide 230, for example, a metal oxide such as an In-M-Zn oxide having indium, an element M, and zinc (the element M is one or more selected from aluminum, gallium, yttrium, tin, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, magnesium, etc.) may be used. Alternatively, as the oxide 230, an In-Ga oxide, an In-Zn oxide, or an indium oxide may be used.

[0054] Here, it is preferable that the atomic ratio of In to element M in the metal oxide used for oxide 230b or oxide 230c is greater than the atomic ratio of In to element M in the metal oxide used for oxide 230a or oxide 230d.

[0055] In this manner, by arranging oxide 230a below oxide 230b or oxide 230c, the diffusion of impurities and oxygen from structures formed below oxide 230a to oxide 230b or oxide 230c can be suppressed.

[0056] Moreover, by disposing the oxide 230d on the oxide 230b or the oxide 230c, it is possible to suppress the diffusion of impurities from a structure formed above the oxide 230d to the oxide 230b or the oxide 230c. Moreover, by disposing the oxide 230d on the oxide 230b or the oxide 230c, it is possible to suppress the upward diffusion of oxygen from the oxide 230b or the oxide 230c.

[0057] In addition, since the oxides 230a to 230d have a common element other than oxygen (as a main component), the defect state density at each interface between the oxides 230a, 230b, 230c, and 230d can be reduced. In this case, the main path of carriers is the oxide 230b, the oxide 230c, or the vicinity thereof, for example, the interface between the oxide 230b and the oxide 230c. Since the defect state density at the interface between the oxide 230b and the oxide 230c can be reduced, the effect of interface scattering on carrier conduction is small, and a high on-current can be obtained.

[0058] It is preferable that the oxide 230b and the oxide 230c each have crystallinity. In particular, it is preferable to use a c-axis aligned crystalline oxide semiconductor (CAAC-OS) as the oxide 230b and the oxide 230c. Also, the oxide 230d may have crystallinity.

[0059] CAAC-OS has a c-axis orientation and a distorted crystal structure in which multiple nanocrystals are connected in the ab-plane direction. The distortion refers to a portion where the lattice orientation changes between a region with a uniform lattice arrangement and a region with a different uniform lattice arrangement in the region where multiple nanocrystals are connected.

[0060] Nanocrystals are basically hexagonal, but may be non-regular hexagonal. In addition, the lattice arrangement may be pentagonal or heptagonal due to the distortion. In CAAC-OS, it is difficult to confirm clear grain boundaries even near the distortion. In other words, it is found that the formation of grain boundaries is suppressed by the distortion of the lattice arrangement. This is because CAAC-OS can tolerate distortion due to the lack of dense arrangement of oxygen atoms in the ab-plane direction and the change in the bond distance between atoms due to the substitution of metal elements.

[0061] A crystal structure in which clear grain boundaries are observed is called polycrystal. The grain boundaries are likely to become recombination centers, trap carriers, and cause a decrease in the on-current of a transistor or a decrease in field-effect mobility. Therefore, CAAC-OS in which clear grain boundaries are not observed is one of the crystalline oxides having a crystal structure suitable for a semiconductor layer of a transistor. In order to form a CAAC-OS, a structure containing Zn is preferable. For example, In-Zn oxide and In-Ga-Zn oxide are suitable because they can suppress the occurrence of grain boundaries more than In oxide.

[0062] CAAC-OS also tends to have a layered crystal structure (also referred to as a layered structure) in which a layer containing indium and oxygen (hereinafter, In layer) and a layer containing element M, zinc, and oxygen (hereinafter, (M, Zn) layer) are stacked. Note that indium and element M can be substituted for each other, and when element M in an (M, Zn) layer is substituted for indium, it can also be expressed as an (In, M, Zn) layer. When indium in an In layer is substituted for element M, it can also be expressed as an (In, M) layer.

[0063] As described above, the CAAC-OS is a metal oxide having a highly crystalline and dense structure and having few impurities and defects (oxygen vacancies Vo, etc.). In particular, by performing heat treatment at a temperature (e.g., 400° C. or higher and 600° C. or lower) at which the metal oxide does not polycrystallize after formation of the metal oxide, the CAAC-OS can have a more crystalline and dense structure. In this way, the density of the CAAC-OS can be increased, and the diffusion of impurities or oxygen in the CAAC-OS can be further reduced.

[0064] On the other hand, it is difficult to identify clear grain boundaries in CAAC-OS, so it is unlikely that the electron mobility will decrease due to grain boundaries. Therefore, metal oxides with CAAC-OS have stable physical properties. Therefore, metal oxides with CAAC-OS are resistant to heat and highly reliable.

[0065] Here, in a transistor using an oxide semiconductor, if impurities and oxygen vacancies exist in a region in which a channel is formed in the oxide semiconductor, the electrical characteristics are likely to fluctuate and the reliability may be reduced. In addition, hydrogen near the oxygen vacancies is called a defect in which hydrogen enters the oxygen vacancy (hereinafter, V OH) and generate electrons that serve as carriers. For this reason, if oxygen vacancies are included in a region in the oxide semiconductor in which a channel is formed, the transistor is likely to have normally-on characteristics (a channel exists even when no voltage is applied to the gate electrode, and a current flows through the transistor). Therefore, impurities and oxygen vacancies are preferably reduced as much as possible in the region in the oxide semiconductor in which a channel is formed. In other words, it is preferable that the carrier concentration is reduced in the region in the oxide semiconductor in which a channel is formed, and the region is made i-type (intrinsic) or substantially i-type.

[0066] In response to this, an insulator containing oxygen that is desorbed by heating (hereinafter may be referred to as excess oxygen) may be provided near the oxide semiconductor, and heat treatment may be performed to supply oxygen from the insulator to the oxide semiconductor. However, if an excessive amount of oxygen is supplied to the source or drain region, the carrier density in the source or drain region may be reduced, which may cause a decrease in the on-state current or the field-effect mobility of the transistor 200. Furthermore, the amount of oxygen supplied to the source or drain region varies within the substrate plane, which may cause variations in the characteristics of a semiconductor device having the transistor.

[0067] Therefore, in the oxide semiconductor, the region 234 functioning as a channel formation region preferably has a reduced carrier concentration and is i-type or substantially i-type, while the region 236 functioning as a source or drain region preferably has a high carrier concentration and is n-type. In other words, it is preferable to supply oxygen to the oxide semiconductor region 234 and prevent an excessive amount of oxygen from being supplied to the region 236.

[0068] Therefore, in the present embodiment, oxygen is diffused from the insulator 280 containing excess oxygen to the oxide 230c via the insulator 224, and the oxygen is supplied from the oxide 230c to the oxide 230b. This makes it possible to selectively supply oxygen to the oxide 230c which occupies most of the region 234, and to the region of the oxide 230b in contact with the oxide 230c.

[0069] Here, the behavior of oxygen when the transistor 200 according to this embodiment is subjected to heat treatment will be described with reference to FIG. 3. FIG. 3A is an enlarged cross-sectional view corresponding to FIG. 1C, and FIG. 3B is an enlarged cross-sectional view corresponding to FIG. 1D. That is, the oxide 230b and a part of the oxide 230c shown in FIG. 3A are regions where a channel is formed, and the oxide 230b shown in FIG. 3B is a region that functions as a source region or a drain region. Note that the arrows in FIG. 3A and FIG. 3B indicate the main diffusion direction of oxygen.

[0070] 3A and 3B, the excess oxygen contained in the insulator 280 diffuses from the interface between the insulator 280 and the insulator 224 into the insulator 224. Furthermore, as shown in FIG. 3A, the excess oxygen contained in the insulator 224 diffuses from the interface between the insulator 224 and the oxide 230c into the oxide 230c. Furthermore, the excess oxygen contained in the oxide 230c diffuses from the interface between the oxide 230c and the oxide 230b into the oxide 230b. In this way, the excess oxygen contained in the insulator 280 is supplied to the region 234 that functions as the channel formation region of the transistor 200.

[0071] In addition, by using the CAAC-OS having the dense structure as described above as the oxide 230b, the diffusion of impurities and oxygen in the oxide 230b can be reduced, and thus the diffusion of oxygen supplied to the region 234 of the oxide 230b to the region 236 of the oxide 230b can be reduced.

[0072] Here, a process of forming the oxide 230b and the like in an island shape is sandwiched between the formation of the insulator 224 and the formation of the insulator 280 on the insulator 224. For this reason, by-products generated in the process of forming the oxide 230b and the like in an island shape may be deposited in a layer on the insulator 224, and if the insulator 280 is formed on the layer of by-products, the amount of oxygen diffusing from the insulator 280 to the insulator 224 may be reduced. Therefore, it is preferable to perform an etching process to remove the layer of by-products before the insulator 280 is formed. Details of the etching process will be described later.

[0073] In addition, a part of the excess oxygen diffused into the oxide 230c also diffuses into the oxide 230d. Since oxygen is less likely to diffuse into the oxide 230d than into the oxide 230c, the diffusion of oxygen into the insulator 250 is relatively suppressed. This makes it possible to suppress the oxidation of the conductor 260 via the insulator 250.

[0074] 3A and 3B, the oxide 230b overlaps with the insulator 224 via the oxide 230a, which has low oxygen permeability. Therefore, the excess oxygen contained in the insulator 224 is less likely to diffuse into the oxide 230a than the oxide 230c. Therefore, the diffusion of the excess oxygen contained in the insulator 224 from the lower surface of the oxide 230b is relatively suppressed.

[0075] 3B, the insulator 272b is disposed in contact with the side surfaces of the oxide 230a, the oxide 230b, the oxide 243b, the conductor 242b, and the insulator 271b, and the insulator 271b is disposed on the upper surface of the conductor 242b. That is, the oxide 230a, the oxide 230b, the oxide 243b, and the conductor 242b are separated from the insulator 280 by the insulator 271b and the insulator 272b, which are difficult to diffuse oxygen. This makes it possible to suppress the excess oxygen contained in the insulator 280 from diffusing directly into the oxide 230a, the oxide 230b, the oxide 243b, and the conductor 242b. Note that, although only the conductor 242b side (region 236b side) shown in FIG. 3B is mentioned above, the conductor 242a side (region 236a side) can also suppress the diffusion of excess oxygen in the same manner.

[0076] In this manner, oxygen is selectively supplied to the oxide semiconductor region 234 to make it i-type or substantially i-type, and oxygen diffusion to the region 236 functioning as a source or drain region is suppressed, thereby maintaining the n-type structure. This can suppress fluctuations in the electrical characteristics of the transistor 200 and variations in the electrical characteristics of the transistor 200 within the substrate surface.

[0077] By adopting the above-mentioned configuration, it is possible to provide a semiconductor device with less variation in transistor characteristics, a highly reliable semiconductor device, and a semiconductor device having good electrical characteristics.

[0078] In addition, in a cross-sectional view in the channel length direction of the transistor, it is preferable to provide a groove in the oxide 230b and fill the groove with the oxide 230c. In this case, the oxide 230c is arranged so as to cover the inner wall (side wall and bottom surface) of the groove. In addition, it is preferable that the film thickness of the oxide 230c is approximately the same as the depth of the groove.

[0079] With this configuration, even if a damaged region is formed on the surface of the oxide 230b at the bottom of the opening when forming the opening for embedding the conductor 260, the damaged region can be removed, thereby suppressing defects in the electrical characteristics of the transistor 200 caused by the damaged region.

[0080] In FIG. 1 and other figures, the side of the opening in which the conductor 260 and the like are embedded is approximately perpendicular to the surface on which the oxide 230b is formed, including the groove of the oxide 230b, but this embodiment is not limited to this. For example, the bottom of the opening may be in a U-shape with a gentle curve. Also, for example, the side of the opening may be inclined with respect to the surface on which the oxide 230b is formed.

[0081] 1C, in a cross-sectional view in the channel width direction of the transistor 200, a curved surface may be formed between the side surface of the oxide 230b and the top surface of the oxide 230b. In other words, the end of the side surface and the end of the top surface may be curved (hereinafter also referred to as rounded).

[0082] The radius of curvature of the curved surface is preferably greater than 0 nm and smaller than the thickness of the oxide 230b in the region overlapping with the conductor 242, or smaller than half the length of the region not having the curved surface. Specifically, the radius of curvature of the curved surface is greater than 0 nm and less than 20 nm, preferably greater than 1 nm and less than 15 nm, and more preferably greater than 2 nm and less than 10 nm. By forming the curved surface in this shape, the coverage of the groove portion by the insulator 250 and the conductor 260 formed in a later process can be improved. In addition, the length of the region not having the curved surface can be prevented from decreasing, and the on-current and mobility of the transistor 200 can be suppressed from decreasing. Therefore, a semiconductor device having good electrical characteristics can be provided.

[0083] The oxide 230 preferably has a laminated structure of a plurality of oxide layers with different chemical compositions. Specifically, in the metal oxide used for the oxide 230a, the atomic ratio of element M to the metal element that is the main component is preferably greater than the atomic ratio of element M to the metal element that is the main component in the metal oxide used for the oxide 230b. In addition, in the metal oxide used for the oxide 230a, the atomic ratio of element M to In is preferably greater than the atomic ratio of element M to In in the metal oxide used for the oxide 230b. In addition, in the metal oxide used for the oxide 230b, the atomic ratio of In to element M is preferably greater than the atomic ratio of In to element M in the metal oxide used for the oxide 230a.

[0084] In order to make the oxide 230c the main path of carriers, the atomic ratio of indium to the main metal element in the oxide 230c is preferably larger than the atomic ratio of indium to the main metal element in the oxide 230b. By using a metal oxide with a high indium content in the channel formation region, the on-current of the transistor can be increased. Therefore, by making the atomic ratio of indium to the main metal element in the oxide 230c larger than the atomic ratio of indium to the main metal element in the oxide 230b, the oxide 230c can be made the main path of carriers.

[0085] In addition, the conduction band minimum of the oxide 230c is preferably farther from the vacuum level than the conduction band minimums of the oxides 230a and 230b. In other words, the electron affinity of the oxide 230c is preferably greater than the electron affinity of the oxides 230a and 230b. In this case, the main carrier path is the oxide 230c.

[0086] Specifically, the oxide 230c may be a metal oxide, indium oxide, or the like having a composition of In:M:Zn=4:2:3 [atomic ratio] or a composition close thereto, In:M:Zn=5:1:3 [atomic ratio] or a composition close thereto, or In:M:Zn=10:1:3 [atomic ratio] or a composition close thereto.

[0087] An example of a parameter for evaluating the reliability of a transistor is the shift voltage (Vsh) measured in a +GBT (Gate Bias Temperature) stress test of the transistor. The shift voltage (Vsh) is defined as the Vg at which the tangent to the maximum slope of the drain current (Id)-gate voltage (Vg) curve of the transistor intersects with the line of Id=1pA. The amount of change in Vsh is expressed as ΔVsh.

[0088] In a +GBT stress test of a transistor, ΔVsh may shift in the negative direction over time. Also, ΔVsh may not fluctuate in the negative direction (e.g., in the negative direction), but may exhibit behavior in which it fluctuates in both the negative and positive directions. Note that in this specification and the like, the above behavior may be referred to as the jagged behavior of ΔVsh in a +GBT stress test.

[0089] By using a metal oxide that does not contain element M as a main component or a metal oxide with a low ratio of element M for oxide 230c, for example, it is possible to reduce ΔVsh, suppress the jagged behavior of ΔVsh, and improve the reliability of the transistor.

[0090] Moreover, the oxide 230b and the oxide 230c are preferably crystalline oxides such as CAAC-OS. Crystalline oxides such as CAAC-OS have few impurities and defects (such as oxygen vacancies) and have a dense structure with high crystallinity. This makes it possible to suppress the extraction of oxygen from the oxide 230b by the source electrode or the drain electrode. As a result, even when heat treatment is performed, the extraction of oxygen from the oxide 230b can be reduced, so that the transistor 200 is stable against high temperatures (so-called thermal budget) in the manufacturing process.

[0091] In addition, it is preferable to use a CAAC-OS as the oxide 230c, and it is preferable that the c-axis of the crystal of the oxide 230c is oriented in a direction approximately perpendicular to the surface on which the oxide 230c is formed or the upper surface of the oxide 230c. The CAAC-OS has a property of easily moving oxygen in a direction perpendicular to the c-axis. Therefore, oxygen in the oxide 230c can be efficiently supplied to the oxide 230b.

[0092] Moreover, the oxide 230d preferably contains at least one of the metal elements constituting the metal oxide used in the oxide 230c, and more preferably contains all of the metal elements. For example, the oxide 230c may be In-M-Zn oxide, In-Zn oxide, or indium oxide, and the oxide 230d may be In-M-Zn oxide, M-Zn oxide, or an oxide of element M. This can reduce the defect state density at the interface between the oxide 230c and the oxide 230d.

[0093] In addition, the conduction band minimum of the oxide 230d is preferably closer to the vacuum level than the conduction band minimum of the oxide 230c. In other words, the electron affinity of the oxide 230d is preferably smaller than that of the oxide 230c. In this case, the oxide 230d is preferably made of a metal oxide that can be used for the oxide 230a or the oxide 230b. In this case, the main carrier path is the oxide 230c.

[0094] Specifically, a metal oxide or indium oxide having a composition of In:M:Zn=4:2:3 [atomic ratio] or a composition close thereto, In:M:Zn=5:1:3 [atomic ratio] or a composition close thereto, or In:M:Zn=10:1:3 [atomic ratio] or a composition close thereto may be used as oxide 230c, and a metal oxide or oxide of element M having a composition of In:M:Zn=1:3:4 [atomic ratio] or a composition close thereto, M:Zn=2:1 [atomic ratio] or a composition close thereto, or M:Zn=2:5 [atomic ratio] or a composition close thereto may be used as oxide 230d.

[0095] Moreover, the oxide 230d is preferably a metal oxide that suppresses the diffusion or permeation of oxygen more than the oxide 230c. By providing the oxide 230d between the insulator 250 and the oxide 230c, it is possible to suppress the diffusion of oxygen contained in the insulator 280 into the insulator 250. Therefore, the oxygen can be efficiently supplied to the oxide 230b via the oxide 230c.

[0096] In addition, by making the atomic ratio of In to the main component metal element in the metal oxide used for the oxide 230d smaller than the atomic ratio of In to the main component metal element in the metal oxide used for the oxide 230c, it is possible to suppress the diffusion of In to the insulator 250 side. Since the insulator 250 functions as a gate insulator, if In gets mixed into the insulator 250, the transistor characteristics will be poor. Therefore, by providing the oxide 230d between the oxide 230c and the insulator 250, it is possible to provide a highly reliable semiconductor device.

[0097] Here, the conduction band minimum changes gradually at the junctions of the oxides 230a, 230b, 230c, and 230d. In other words, the conduction band minimum at the junctions of the oxides 230a, 230b, 230c, and 230d can be said to change continuously or to be a continuous junction. To achieve this, it is preferable to reduce the defect level density of the mixed layers formed at the interface between the oxides 230a and 230b, the interface between the oxides 230b and 230c, and the interface between the oxides 230c and 230d.

[0098] Specifically, the oxide 230a and the oxide 230b, the oxide 230b and the oxide 230c, and the oxide 230c and the oxide 230d have a common element other than oxygen as a main component, thereby forming a mixed layer with a low density of defect states. For example, when the oxide 230b is an In-M-Zn oxide, the oxide 230a, the oxide 230c, and the oxide 230d may be appropriately selected from In-M-Zn oxide, M-Zn oxide, an oxide of element M, In-Zn oxide, indium oxide, and the like.

[0099] Specifically, the oxide 230a may be a metal oxide having a composition of In:M:Zn=1:3:4 [atomic ratio] or a composition close thereto, or In:M:Zn=1:1:0.5 [atomic ratio] or a composition close thereto. The oxide 230b may be a metal oxide having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition close thereto, or In:M:Zn=4:2:3 [atomic ratio] or a composition close thereto. The oxide 230c may be a metal oxide having a composition of In:M:Zn=4:2:3 [atomic ratio] or a composition close thereto, In:M:Zn=5:1:3 [atomic ratio] or a composition close thereto, or In:M:Zn=10:1:3 [atomic ratio] or a composition close thereto, or an indium oxide. The composition close thereto includes a range of ±30% of the desired atomic ratio. It is preferable to use gallium as the element M. In addition, as the oxide 230d, a metal oxide having a composition of In:M:Zn=1:3:4 [atomic ratio] or a composition close thereto, a composition of M:Zn=2:1 [atomic ratio] or a composition close thereto, or a composition of M:Zn=2:5 [atomic ratio] or a composition close thereto, or an oxide of the element M may be used.

[0100] In addition, when a metal oxide film is formed by a sputtering method, the above atomic ratio is not limited to the atomic ratio of the formed metal oxide film, but may be the atomic ratio of a sputtering target used to form the metal oxide film.

[0101] By configuring the oxide 230a, the oxide 230b, the oxide 230c, and the oxide 230d as described above, it is possible to reduce the defect state density at the interface between the oxide 230a and the oxide 230b, the interface between the oxide 230b and the oxide 230c, and the interface between the oxide 230c and the oxide 230d. As a result, the effect of interface scattering on carrier conduction is reduced, and the transistor 200 can obtain a large on-current and high frequency characteristics.

[0102] Note that the oxide 230c may be provided for each transistor 200. That is, the oxide 230c of one transistor 200 and the oxide 230c of another transistor 200 adjacent to the transistor 200 may not be in contact with each other. Furthermore, the oxide 230c of one transistor 200 and the oxide 230c of another transistor 200 adjacent to the transistor 200 may be separated from each other. In other words, a configuration in which the oxide 230c is not provided between the transistor 200 and the transistor 200 adjacent to the transistor 200 may be used.

[0103] In a semiconductor device in which a plurality of transistors 200 are arranged in the channel width direction, the above-described structure allows the oxide 230c to be provided independently in each of the transistors 200. This makes it possible to prevent a parasitic transistor from being generated between a transistor 200 and a transistor 200 adjacent to the transistor 200, thereby preventing the above-described leakage path from being generated. This makes it possible to provide a semiconductor device that has favorable electrical characteristics and can be miniaturized or highly integrated.

[0104] For example, when the distance between the side end of the oxide 230c of the transistor 200 and the side end of the oxide 230c of the transistor 200 adjacent to the transistor 200, which face each other in the channel width direction of the transistor 200, is expressed as L1, L1 is set to be larger than 0 nm. Also, when the distance between the side end of the oxide 230a of the transistor 200 and the side end of the oxide 230a of the transistor 200 adjacent to the transistor 200, which face each other in the channel width direction of the transistor 200, is expressed as L2, the value of the ratio of L1 to L2 (L1 / L2) is preferably larger than 0 and smaller than 1, more preferably 0.1 or more and 0.9 or less, and even more preferably 0.2 or more and 0.8 or less. Note that L2 may be the distance between the side end of the oxide 230b of the transistor 200 and the side end of the oxide 230b of the transistor 200 adjacent to the transistor 200, which face each other.

[0105] By reducing the ratio of L1 to L2 (L1 / L2) described above, even if a misalignment occurs in a region where oxide 230c is not located between transistor 200 and a transistor 200 adjacent to said transistor 200, oxide 230c of transistor 200 can be separated from oxide 230c of a transistor 200 adjacent to said transistor 200.

[0106] Furthermore, by increasing the ratio of L1 to L2 (L1 / L2), even if the distance between transistor 200 and the adjacent transistor 200 is narrowed, the minimum processing dimension width can be secured, thereby enabling further miniaturization or high integration of the semiconductor device.

[0107] Note that the conductor 260 and the insulator 250 may be shared between adjacent transistors 200. That is, the conductor 260 of one transistor 200 has a region provided contiguous with the conductor 260 of another transistor 200 adjacent to the transistor 200. The insulator 250 of one transistor 200 has a region provided contiguous with the insulator 250 of another transistor 200 adjacent to the transistor 200.

[0108] With the above structure, the oxide 230d has a region in contact with the insulator 224 between the transistor 200 and another transistor 200 adjacent to the transistor 200. Note that the oxide 230c and the oxide 230d of the transistor 200 may be separated from the oxide 230c and the oxide 230d of the transistor 200 adjacent to the transistor 200.

[0109] The insulators 211, 212, 214, 271, 272, 282, 283, 284, and 286 preferably function as barrier insulating films that suppress the diffusion of impurities such as water and hydrogen from the substrate side or from above the transistor 200 to the transistor 200. Therefore, the insulators 211, 212, 214, 271, 272, 282, 283, 284, and 286 are preferably made of an insulating material that has a function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (NO, NO, NO, etc.), and copper atoms (through which the above impurities are difficult to permeate). Alternatively, it is preferable to use an insulating material that has a function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms, oxygen molecules, etc.) (through which the above oxygen is difficult to permeate).

[0110] In this specification, a barrier insulating film refers to an insulating film having a barrier property. In this specification, the barrier property means a function of suppressing the diffusion of a corresponding substance (also called low permeability) or a function of capturing and fixing a corresponding substance (also called gettering).

[0111] For example, it is preferable to use silicon nitride or the like as the insulators 211, 212, 283, and 284, and aluminum oxide or the like as the insulators 214, 271, 272, and 282. This can suppress impurities such as water and hydrogen from diffusing from the substrate side to the transistor 200 side through the insulators 211, 212, and 214. Alternatively, it can suppress oxygen contained in the insulator 224 or the like from diffusing to the substrate side through the insulators 211, 212, and 214. It can also suppress impurities such as water and hydrogen from diffusing from the insulator 280, the conductor 246, and the like to the oxide 230. In this way, it is preferable to have a structure in which transistor 200 is surrounded by insulators 211, 212, 214, 271, 272, 282, 283, and 284, which have the function of suppressing the diffusion of impurities such as water and hydrogen, and oxygen.

[0112] In addition, it may be preferable to reduce the resistivity of the insulators 211, 284, and 286. For example, it is preferable to reduce the resistivity of the insulators 211, 284, and 286 to approximately 1×10 13 By setting the resistivity at Ωcm, the insulator 211, the insulator 284, and the insulator 286 may be able to reduce charge-up of the conductor 205, the conductor 242, the conductor 260, or the conductor 246 in a process using plasma or the like in a semiconductor device manufacturing process. 10 Ωcm or more 1×10 15 Ωcm or less.

[0113] Note that the insulator 211 or the insulator 212 is not necessarily provided, and the insulator 283 or the insulator 284 is not necessarily provided. For example, the insulator 212 and the insulator 284 may be formed by a CVD method using a compound gas that does not contain hydrogen atoms or has a small amount of hydrogen atoms.

[0114] The insulator 216 and the insulator 280 preferably have a lower dielectric constant than the insulator 214. By using a material with a low dielectric constant as an interlayer film, the parasitic capacitance generated between wirings can be reduced. For example, silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide to which fluorine has been added, silicon oxide to which carbon has been added, silicon oxide to which carbon and nitrogen have been added, silicon oxide having vacancies, or the like may be used as the insulator 216 and the insulator 280 as appropriate.

[0115] The conductor 205 may function as a second gate electrode. In this case, the threshold voltage (Vth) of the transistor 200 can be controlled by changing the potential applied to the conductor 205 independently of the potential applied to the conductor 260. In particular, applying a negative potential to the conductor 205 can increase the Vth of the transistor 200 and reduce the off-current. Therefore, applying a negative potential to the conductor 205 can reduce the drain current when the potential applied to the conductor 260 is 0 V, compared to not applying a negative potential.

[0116] The conductor 205 is disposed so as to overlap the oxide 230 and the conductor 260. In addition, the conductor 205 is preferably embedded in the insulator 214 or the insulator 216.

[0117] As shown in FIG. 1A, the conductor 205 is preferably provided larger than the size of the region of the oxide 230 that does not overlap with the conductor 242a and the conductor 242b. In particular, as shown in FIG. 1C, the conductor 205 preferably extends in a region outside the end of the oxide 230a and the oxide 230b that intersects with the channel width direction. In other words, outside the side surface of the oxide 230 in the channel width direction, the conductor 205 and the conductor 260 preferably overlap with each other via an insulator. With this configuration, the channel formation region of the oxide 230 can be electrically surrounded by the electric field of the conductor 260 that functions as the first gate electrode and the electric field of the conductor 205 that functions as the second gate electrode. In this specification, a structure of a transistor in which the channel formation region is electrically surrounded by the electric fields of the first gate and the second gate is called a surrounded channel (S-channel) structure.

[0118] In this specification and the like, a transistor with an S-channel structure refers to a transistor structure in which a channel formation region is electrically surrounded by the electric fields of one and the other of a pair of gate electrodes. The S-channel structure disclosed in this specification and the like is different from a fin type structure and a planar type structure. By adopting the S-channel structure, it is possible to improve resistance to the short channel effect, in other words, to make a transistor in which the short channel effect is unlikely to occur.

[0119] 1C, the conductor 205 is extended to function as wiring. However, the present invention is not limited to this, and a conductor functioning as wiring may be provided below the conductor 205. Also, it is not necessary to provide one conductor 205 for each transistor. For example, the conductor 205 may be shared by multiple transistors.

[0120] Note that, in the transistor 200, the conductor 205 has a structure in which the conductor 205a and the conductor 205b are stacked, but the present invention is not limited to this. For example, the conductor 205 may have a single layer or a stacked structure of three or more layers. When the structure has a stacked structure, the structures may be distinguished by giving ordinal numbers to the order of formation.

[0121] Here, the conductor 205a is preferably made of a conductive material having a function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (NO, NO, NO, etc.), copper atoms, etc. Alternatively, it is preferably made of a conductive material having a function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms, oxygen molecules, etc.).

[0122] By using a conductive material having a function of suppressing the diffusion of oxygen for the conductor 205a, it is possible to suppress the conductor 205b from being oxidized and its conductivity from decreasing. As the conductive material having a function of suppressing the diffusion of oxygen, for example, tantalum, tantalum nitride, ruthenium, ruthenium oxide, etc. are preferably used. Therefore, the conductor 205a may be a single layer or a multilayer of the above conductive material. For example, the conductor 205a may be a multilayer of tantalum, tantalum nitride, ruthenium, or ruthenium oxide, and titanium or titanium nitride.

[0123] The conductor 205b is preferably made of a conductive material containing tungsten, copper, or aluminum as a main component. Although the conductor 205b is illustrated as a single layer, it may have a laminated structure, for example, a laminate of titanium or titanium nitride and the conductive material.

[0124] Insulator 222 and insulator 224 function as gate insulators.

[0125] The insulator 222 preferably has a function of suppressing the diffusion of hydrogen (e.g., at least one of hydrogen atoms, hydrogen molecules, etc.). The insulator 222 preferably has a function of suppressing the diffusion of oxygen (e.g., at least one of oxygen atoms, oxygen molecules, etc.). For example, the insulator 222 preferably has a function of suppressing the diffusion of one or both of hydrogen and oxygen more than the insulator 224.

[0126] The insulator 222 may be an insulator containing an oxide of one or both of aluminum and hafnium, which are insulating materials. As the insulator, it is preferable to use aluminum oxide, hafnium oxide, an oxide containing aluminum and hafnium (hafnium aluminate), or the like. When the insulator 222 is formed using such a material, the insulator 222 functions as a layer that suppresses the release of oxygen from the oxide 230 to the substrate side and the diffusion of impurities such as hydrogen from the periphery of the transistor 200 to the oxide 230. Thus, by providing the insulator 222, it is possible to suppress the diffusion of impurities such as hydrogen into the inside of the transistor 200 and the generation of oxygen vacancies in the oxide 230. In addition, it is possible to suppress the reaction of the conductor 205 with the insulator 224 and the oxygen contained in the oxide 230.

[0127] Alternatively, for example, aluminum oxide, bismuth oxide, germanium oxide, niobium oxide, silicon oxide, titanium oxide, tungsten oxide, yttrium oxide, or zirconium oxide may be added to the insulator. Alternatively, these insulators may be nitrided. The insulator 222 may be formed by stacking silicon oxide, silicon oxynitride, or silicon nitride on these insulators.

[0128] The insulator 222 may be a single layer or a multilayer of insulators containing so-called high-k materials, such as aluminum oxide, hafnium oxide, tantalum oxide, zirconium oxide, lead zirconate titanate (PZT), strontium titanate (SrTiO3), (Ba,Sr)TiO3 (BST), etc. As transistors become smaller and more highly integrated, problems such as leakage current may occur due to the thinning of the gate insulator. By using a high-k material for the insulator that functions as the gate insulator, it is possible to reduce the gate potential during transistor operation while maintaining the physical film thickness.

[0129] It is preferable that the insulator 224 in contact with the oxide 230 release oxygen by heating. For example, the insulator 224 may be made of silicon oxide, silicon oxynitride, or the like as appropriate. By providing an insulator containing oxygen in contact with the oxide 230, oxygen vacancies in the oxide 230 can be reduced and the reliability of the transistor 200 can be improved.

[0130] Specifically, it is preferable to use an oxide material from which some oxygen is released by heating, in other words, an insulator material having an excess oxygen region, as the insulator 224. An oxide material from which oxygen is released by heating is an oxide material from which the amount of released oxygen molecules is 1.0×10 18 molecules / cm 3 More than 1.0×10 19 molecules / cm 3 More preferably, 2.0×10 19 molecules / cm 3 or more than 3.0×10 20 molecules / cm 3 The oxide film is one having the above-mentioned properties. The surface temperature of the film during the TDS analysis is preferably in the range of 100° C. or more and 700° C. or less, or 100° C. or more and 400° C. or less.

[0131] In addition, the oxide 230 may be brought into contact with an insulator having the excess oxygen region and subjected to one or more of heat treatment, microwave treatment, and RF treatment. By carrying out such treatment, water or hydrogen in the oxide 230 can be removed. For example, in the oxide 230, defects in which hydrogen has entered an oxygen vacancy (V O A reaction occurs in which the bond of V O H→V O A reaction of "H + H" occurs, resulting in dehydrogenation. Some of the hydrogen generated at this time may combine with oxygen to form HO, which may be removed from the oxide 230 or an insulator in the vicinity of the oxide 230. Some of the hydrogen may also diffuse or be captured (also called gettering) by the conductor 242.

[0132] The microwave treatment is preferably performed using, for example, a device having a power source for generating high-density plasma or a device having a power source for applying RF to the substrate side. For example, high-density oxygen radicals can be generated by using a gas containing oxygen and high-density plasma, and the oxygen radicals generated by the high-density plasma can be efficiently introduced into the oxide 230 or an insulator near the oxide 230 by applying RF to the substrate side. The microwave treatment may be performed under a pressure of 133 Pa or more, preferably 200 Pa or more, and more preferably 400 Pa or more. For example, oxygen and argon are used as gases to be introduced into the microwave treatment device, and the oxygen flow rate ratio (O2 / (O2+Ar)) is 50% or less, preferably 10% or more and 30% or less.

[0133] In addition, in the manufacturing process of the transistor 200, it is preferable to perform heat treatment while the surface of the oxide 230 is exposed. The heat treatment may be performed, for example, at a temperature of 100° C. or higher and 600° C. or lower, more preferably 350° C. or higher and 400° C. or lower. Note that the heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing an oxidizing gas at 10 ppm or higher, 1% or higher, or 10% or higher. For example, the heat treatment is preferably performed in an oxygen atmosphere. This supplies oxygen to the oxide 230 to reduce oxygen deficiencies (VO ) can be reduced. The heat treatment may be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas in order to compensate for the desorbed oxygen after the heat treatment in a nitrogen gas or inert gas atmosphere. Alternatively, the heat treatment may be performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas in order to compensate for the desorbed oxygen. Alternatively, the heat treatment may be performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas in succession to a heat treatment in a nitrogen gas or inert gas atmosphere.

[0134] In addition, by subjecting the oxide 230 to an oxygen addition treatment, the oxygen vacancies in the oxide 230 are repaired by the supplied oxygen. In other words, O In addition, the reaction of the hydrogen remaining in the oxide 230 with the oxygen supplied can be promoted, and the hydrogen can be removed as H2O (dehydrated). As a result, the hydrogen remaining in the oxide 230 recombines with the oxygen vacancies to form V O The formation of H can be suppressed.

[0135] The insulator 222 and the insulator 224 may have a laminated structure of two or more layers. In this case, the laminated structure is not limited to being made of the same material, and may be made of different materials.

[0136] Preferably, oxide 243 (oxide 243a and oxide 243b) is provided on oxide 230b.

[0137] The oxide 243 (oxide 243a and oxide 243b) preferably has a function of suppressing oxygen permeation. By disposing the oxide 243 having a function of suppressing oxygen permeation between the conductor 242 functioning as a source electrode or a drain electrode and the oxide 230b, the electrical resistance between the conductor 242 and the oxide 230b is reduced, which is preferable. With such a structure, the electrical characteristics and reliability of the transistor 200 can be improved. Note that if the electrical resistance between the conductor 242 and the oxide 230b can be sufficiently reduced, the oxide 243 may not be provided.

[0138] A metal oxide having element M may be used as the oxide 243. In particular, the element M may be aluminum, gallium, yttrium, or tin. The oxide 243 preferably has a higher concentration of element M than the oxide 230b. Gallium oxide may be used as the oxide 243. A metal oxide such as In-M-Zn oxide may be used as the oxide 243. Specifically, in the metal oxide used for the oxide 243, the atomic ratio of element M to In is preferably greater than the atomic ratio of element M to In in the metal oxide used for the oxide 230b. The film thickness of the oxide 243 is preferably 0.5 nm or more and 5 nm or less, more preferably 1 nm or more and 3 nm or less, and even more preferably 1 nm or more and 2 nm or less. The oxide 243 is preferably crystalline. When the oxide 243 is crystalline, the release of oxygen in the oxide 230 can be suitably suppressed. For example, if the oxide 243 has a crystal structure such as a hexagonal crystal structure, the release of oxygen in the oxide 230 may be suppressed.

[0139] The conductor 242a is provided over the oxide 243a, and the conductor 242b is provided over the oxide 243b. The conductor 242a and the conductor 242b function as a source electrode and a drain electrode of the transistor 200, respectively.

[0140] As the conductor 242 (conductor 242a and conductor 242b), for example, a nitride containing tantalum, a nitride containing titanium, a nitride containing molybdenum, a nitride containing tungsten, a nitride containing tantalum and aluminum, a nitride containing titanium and aluminum, or the like is preferably used. In one embodiment of the present invention, a nitride containing tantalum is particularly preferable. Also, for example, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, an oxide containing lanthanum and nickel, or the like may be used. These materials are preferable because they are conductive materials that are difficult to oxidize, or materials that maintain their conductivity even when they absorb oxygen.

[0141] If the oxide 243 is not provided, contact between the conductor 242 and the oxide 230b or the oxide 230c may cause oxygen in the oxide 230b or the oxide 230c to diffuse into the conductor 242, resulting in the oxidation of the conductor 242. The oxidation of the conductor 242 is likely to result in a decrease in the conductivity of the conductor 242. The diffusion of oxygen in the oxide 230b or the oxide 230c into the conductor 242 can be rephrased as the conductor 242 absorbing the oxygen in the oxide 230b or the oxide 230c.

[0142] In addition, oxygen in the oxide 230b or the oxide 230c may diffuse into the conductor 242a and the conductor 242b, forming layers between the conductor 242a and the oxide 230b, between the conductor 242b and the oxide 230b, or between the conductor 242a and the oxide 230c, and between the conductor 242b and the oxide 230c. Since the layer contains more oxygen than the conductor 242a or the conductor 242b, the layer is presumed to have insulating properties. In this case, the three-layer structure of the conductor 242a or the conductor 242b, the layer, and the oxide 230b or the oxide 230c can be regarded as a three-layer structure made of a metal-insulator-semiconductor, and can be regarded as a MIS (Metal-Insulator-Semiconductor) structure or a diode junction structure mainly based on the MIS structure.

[0143] Note that hydrogen contained in the oxide 230b, the oxide 230c, etc. may diffuse into the conductor 242a or the conductor 242b. In particular, by using a nitride containing tantalum for the conductor 242a and the conductor 242b, hydrogen contained in the oxide 230b, the oxide 230c, etc. may easily diffuse into the conductor 242a or the conductor 242b, and the diffused hydrogen may combine with nitrogen contained in the conductor 242a or the conductor 242b. In other words, hydrogen contained in the oxide 230b, the oxide 230c, etc. may be absorbed by the conductor 242a or the conductor 242b.

[0144] Furthermore, there may be a curved surface between the side surface of the conductor 242 and the top surface of the conductor 242. That is, the end of the side surface and the end of the top surface may be curved. The curved surface has a radius of curvature of, for example, 3 nm to 10 nm, preferably 5 nm to 6 nm, at the end of the conductor 242. The lack of corners at the end improves the coverage of the film in the subsequent film formation process.

[0145] The insulator 272 is provided to cover the side surfaces of the oxide 230a, the oxide 230b, the oxide 243, the conductor 242, and the insulator 271, and preferably functions as a barrier insulating film against at least oxygen. Therefore, the insulator 272 preferably has a function of suppressing the diffusion of oxygen. For example, the insulator 272 preferably has a function of suppressing the diffusion of oxygen more than the insulator 280. As the insulator 272, for example, a film containing an oxide of one or both of aluminum and hafnium may be formed.

[0146] The insulator 271 is provided in contact with the upper surface of the conductor 242 and preferably functions as a barrier insulating film against oxygen, similar to the insulator 272. Therefore, the insulator 271 also preferably has a function of suppressing the diffusion of oxygen. For example, the insulator 271 preferably has a function of suppressing the diffusion of oxygen more than the insulator 280. As the insulator 271, for example, an insulator containing an oxide of one or both of aluminum and hafnium may be formed. As the insulator 271, for example, an insulator containing silicon nitride may be used.

[0147] By providing the insulator 271 and the insulator 272 as described above, the oxide 230a, the oxide 230b, the oxide 243, and the conductor 242 can be separated from the insulator 280. Therefore, it is possible to suppress the direct diffusion of oxygen from the insulator 280 to the oxide 230a, the oxide 230b, the oxide 243, and the conductor 242. This makes it possible to prevent the carrier density of the source region and the drain region of the oxide 230 from being reduced due to the supply of excess oxygen to the source region and the drain region. In addition, it is possible to suppress the conductor 242 from being excessively oxidized, which increases the resistivity and reduces the on-current.

[0148] 1, the insulators 271 and 272 are shown as separate insulating films in contact with each other, but this embodiment is not limited to this. If the same material is used for the insulators 271 and 272, the boundary between the insulators 271 and 272 may not be clear, and the insulators 271 and 272 may be observed as a single insulating film.

[0149] The insulator 250 functions as a gate insulator. The insulator 250 is preferably disposed in contact with the upper surface of the oxide 230d. The insulator 250 can be made of silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide doped with fluorine, silicon oxide doped with carbon, silicon oxide doped with carbon and nitrogen, silicon oxide having vacancies, or the like. In particular, silicon oxide and silicon oxynitride are preferable because they are stable against heat.

[0150] The insulator 250 is preferably formed using an insulator that releases oxygen when heated, similar to the insulator 224. By providing the insulator that releases oxygen when heated as the insulator 250 in contact with the upper surface of the oxide 230d, oxygen can be effectively supplied to the channel formation region of the oxide 230b, and oxygen vacancies in the channel formation region of the oxide 230b can be reduced. Therefore, a transistor with suppressed fluctuations in electrical characteristics, stable electrical characteristics, and improved reliability can be provided. Furthermore, similar to the insulator 224, it is preferable that the concentration of impurities such as water and hydrogen in the insulator 250 is reduced. The thickness of the insulator 250 is preferably 1 nm or more and 20 nm or less.

[0151] In addition, although the insulator 250 is illustrated as a single layer in FIG. 1B and FIG. 1C, it may be a laminated structure of two or more layers. When the insulator 250 is a laminated structure of two layers, it is preferable that the lower layer of the insulator 250 is formed using an insulator that releases oxygen when heated, and the upper layer of the insulator 250 is formed using an insulator that has a function of suppressing the diffusion of oxygen. By adopting such a configuration, it is possible to suppress the diffusion of oxygen contained in the lower layer of the insulator 250 to the conductor 260. In other words, it is possible to suppress the decrease in the amount of oxygen supplied to the oxide 230. In addition, it is possible to suppress the oxidation of the conductor 260 due to the oxygen contained in the lower layer of the insulator 250. For example, the lower layer of the insulator 250 can be provided using a material that can be used for the insulator 250 described above, and the upper layer of the insulator 250 can be provided using a material similar to that of the insulator 222.

[0152] When silicon oxide or silicon oxynitride is used for the lower layer of the insulator 250, the upper layer of the insulator 250 may be made of an insulating material that is a high-k material with a high dielectric constant. By forming the gate insulator into a laminated structure of the lower layer of the insulator 250 and the upper layer of the insulator 250, it is possible to obtain a laminated structure that is stable against heat and has a high dielectric constant. Therefore, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical film thickness of the gate insulator. In addition, it is possible to reduce the equivalent oxide thickness (EOT) of the insulator that functions as the gate insulator.

[0153] Specifically, the upper layer of the insulator 250 may be a metal oxide containing one or more of hafnium, aluminum, gallium, yttrium, zirconium, tungsten, titanium, tantalum, nickel, germanium, magnesium, etc., or a metal oxide that can be used as the oxide 230. In particular, it is preferable to use an insulator containing an oxide of one or both of aluminum and hafnium.

[0154] Furthermore, a metal oxide may be provided between the insulator 250 and the conductor 260. The metal oxide preferably suppresses the diffusion of oxygen from the insulator 250 to the conductor 260. By providing a metal oxide that suppresses the diffusion of oxygen, the diffusion of oxygen from the insulator 250 to the conductor 260 is suppressed. In other words, a decrease in the amount of oxygen supplied to the oxide 230 can be suppressed. Furthermore, oxidation of the conductor 260 due to oxygen from the insulator 250 can be suppressed.

[0155] It is preferable that the metal oxide has a function as a part of the first gate electrode. For example, the metal oxide that can be used as the oxide 230 can be used as the metal oxide. In this case, the electric resistance value of the metal oxide can be reduced to make it a conductor by forming the conductor 260a by a sputtering method. This can be called an OC (Oxide Conductor) electrode.

[0156] By including the metal oxide, the on-current of the transistor 200 can be improved without weakening the effect of the electric field from the conductor 260. Furthermore, by maintaining a distance between the conductor 260 and the oxide 230 due to the physical thickness of the insulator 250 and the metal oxide, it is possible to suppress leakage current between the conductor 260 and the oxide 230. Furthermore, by providing a stacked structure of the insulator 250 and the metal oxide, it is possible to easily and appropriately adjust the physical distance between the conductor 260 and the oxide 230 and the electric field strength applied from the conductor 260 to the oxide 230.

[0157] The conductor 260 functions as a first gate electrode of the transistor 200. The conductor 260 preferably includes a conductor 260a and a conductor 260b disposed on the conductor 260a. For example, the conductor 260a is preferably disposed so as to surround the bottom and side surfaces of the conductor 260b. As shown in FIG. 1B and FIG. 1C, the upper surface of the conductor 260 is substantially aligned with the upper surface of the insulator 250 and the upper surface of the oxide 230c. Note that, although the conductor 260 is shown as a two-layer structure of the conductor 260a and the conductor 260b in FIG. 1B and FIG. 1C, the conductor 260 may be a single-layer structure or a stacked structure of three or more layers.

[0158] The conductor 260a is preferably made of a conductive material having a function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules, copper atoms, etc. Alternatively, it is preferably made of a conductive material having a function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms, oxygen molecules, etc.).

[0159] Furthermore, since the conductor 260a has a function of suppressing the diffusion of oxygen, it is possible to suppress a decrease in conductivity due to oxidation of the conductor 260b caused by oxygen contained in the insulator 250. As a conductive material having a function of suppressing the diffusion of oxygen, it is preferable to use, for example, tantalum, tantalum nitride, ruthenium, ruthenium oxide, or the like.

[0160] In addition, since the conductor 260 also functions as wiring, it is preferable to use a conductor with high conductivity. For example, the conductor 260b can be a conductive material mainly composed of tungsten, copper, or aluminum. The conductor 260b may also have a laminated structure, for example, a laminated structure of titanium or titanium nitride and the above-mentioned conductive material.

[0161] Moreover, in the transistor 200, the conductor 260 is formed in a self-aligned manner so as to fill an opening formed in the insulator 280 or the like. By forming the conductor 260 in this manner, the conductor 260 can be reliably disposed in the region between the conductor 242a and the conductor 242b without alignment.

[0162] As shown in FIG. 1C, in the channel width direction of the transistor 200, the height of the bottom surface of the conductor 260 in the region where the conductor 260 and the oxide 230b do not overlap is preferably lower than the height of the bottom surface of the oxide 230b when the bottom surface of the insulator 222 is used as a reference. The conductor 260, which functions as a gate electrode, is configured to cover the side and upper surface of the channel formation region of the oxide 230b via the insulator 250 or the like, so that the electric field of the conductor 260 can be easily applied to the entire channel formation region of the oxide 230b. This makes it possible to increase the on-current of the transistor 200 and improve the frequency characteristics. When the bottom surface of the insulator 222 is used as a reference, the difference between the height of the bottom surface of the conductor 260 in the region where the oxide 230a and the oxide 230b do not overlap with the conductor 260 and the height of the bottom surface of the oxide 230b is 0 nm or more and 100 nm or less, preferably 3 nm or more and 50 nm or less, and more preferably 5 nm or more and 20 nm or less.

[0163] The insulator 280 is provided on the insulator 224, the oxide 230, the conductor 242, and the insulator 271. In addition, the upper surface of the insulator 280 may be planarized.

[0164] The insulator 280 that functions as an interlayer film preferably has a low dielectric constant. By using a material with a low dielectric constant as the interlayer film, the parasitic capacitance that occurs between wirings can be reduced. The insulator 280 is preferably formed using, for example, the same material as the insulator 216. In particular, silicon oxide and silicon oxynitride are preferable because they are thermally stable. In particular, materials such as silicon oxide, silicon oxynitride, and silicon oxide having vacancies are preferable because they can easily form a region containing oxygen that is desorbed by heating.

[0165] The concentration of impurities such as water and hydrogen in the insulator 280 is preferably reduced. The insulator 280 preferably has a low hydrogen concentration and an excess oxygen region or excess oxygen, and may be formed using, for example, a material similar to that of the insulator 216. The insulator 280 may have a structure in which the above materials are stacked, for example, a stacked structure of silicon oxide formed by a sputtering method and silicon oxynitride formed by a chemical vapor deposition (CVD) method. Silicon nitride may also be stacked on top of that.

[0166] The insulator 282 or the insulator 283 preferably functions as a barrier insulating film that suppresses diffusion of impurities such as water and hydrogen from above into the insulator 280. The insulator 282 or the insulator 283 preferably functions as a barrier insulating film that suppresses oxygen transmission. The insulator 282 and the insulator 283 may be, for example, an insulator such as aluminum oxide, silicon nitride, or silicon nitride oxide. For example, the insulator 282 may be made of aluminum oxide, which has a high blocking property against oxygen, and the insulator 283 may be made of silicon nitride, which has a high blocking property against hydrogen.

[0167] The conductor 240a and the conductor 240b are preferably made of a conductive material containing tungsten, copper, or aluminum as a main component. The conductor 240a and the conductor 240b may have a layered structure.

[0168] In addition, when the conductor 240 has a laminated structure, it is preferable to use a conductive material having a function of suppressing the permeation of impurities such as water and hydrogen for the conductor in contact with the insulator 284, the insulator 283, the insulator 282, the insulator 280, and the insulator 271. For example, it is preferable to use tantalum, tantalum nitride, titanium, titanium nitride, ruthenium, ruthenium oxide, etc. In addition, the conductive material having a function of suppressing the permeation of impurities such as water and hydrogen may be used in a single layer or a laminated layer. In addition, it is possible to suppress impurities such as water and hydrogen contained in layers above the insulator 284 from being mixed into the oxide 230 through the conductor 240a and the conductor 240b.

[0169] As the insulator 241a and the insulator 241b, for example, an insulator such as silicon nitride, aluminum oxide, or silicon nitride oxide may be used. The insulator 241a and the insulator 241b are provided in contact with the insulator 284, the insulator 283, the insulator 282, and the insulator 271, and therefore can prevent impurities such as water and hydrogen contained in the insulator 280 from being mixed into the oxide 230 through the conductor 240a and the conductor 240b. In particular, silicon nitride is preferable because it has a high blocking property against hydrogen. In addition, it can prevent the oxygen contained in the insulator 280 from being absorbed by the conductor 240a and the conductor 240b.

[0170] Conductors 246 (conductors 246a and 246b) may be disposed in contact with the upper surface of conductor 240a and the upper surface of conductor 240b to function as wiring. Conductor 246 is preferably made of a conductive material containing tungsten, copper, or aluminum as a main component. The conductor may have a laminated structure, for example, a laminate of titanium or titanium nitride and the above conductive material. The conductor may be formed so as to be embedded in an opening provided in an insulator.

[0171] The insulator 286 is provided on the conductor 246 and on the insulator 284. As a result, the upper surface and the side surface of the conductor 246 contact the insulator 286, and the lower surface of the conductor 246 contacts the insulator 284. In other words, the conductor 246 can be configured to be wrapped in the insulators 284 and 286. With such a configuration, it is possible to suppress the permeation of oxygen from the outside and prevent oxidation of the conductor 246. This is also preferable because it is possible to prevent impurities such as water and hydrogen from diffusing to the outside from the conductor 246.

[0172] <Materials for semiconductor devices> The following describes constituent materials that can be used in the semiconductor device.

[0173] <<Substrate>> The substrate on which the transistor 200 is formed may be, for example, an insulating substrate, a semiconductor substrate, or a conductive substrate. Examples of insulating substrates include a glass substrate, a quartz substrate, a sapphire substrate, a stabilized zirconia substrate (such as an yttria stabilized zirconia substrate), and a resin substrate. Examples of semiconductor substrates include a semiconductor substrate made of silicon or germanium, or a compound semiconductor substrate made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Examples of semiconductor substrates include a semiconductor substrate having an insulating region inside the semiconductor substrate, such as an SOI (Silicon On Insulator) substrate. Examples of conductive substrates include a graphite substrate, a metal substrate, an alloy substrate, and a conductive resin substrate. Examples of substrates include a substrate having a metal nitride, a substrate having a metal oxide, and the like. Examples of substrates include a substrate having a conductor or semiconductor provided on an insulating substrate, a substrate having a conductor or insulator provided on a semiconductor substrate, and a substrate having a semiconductor or insulator provided on a conductive substrate. Alternatively, a substrate provided with elements may be used. The elements provided on the substrate include a capacitor element, a resistor element, a switch element, a light-emitting element, a memory element, and the like.

[0174] <<Insulators>> Examples of the insulator include oxides, nitrides, oxynitrides, nitride oxides, metal oxides, metal oxynitrides, and metal nitride oxides, each of which has insulating properties.

[0175] For example, as transistors become smaller and more highly integrated, problems such as leakage current can occur due to thinner gate insulators. By using a high-k material for the insulator that functions as the gate insulator, it is possible to reduce the voltage required for transistor operation while maintaining the physical film thickness. On the other hand, by using a material with a low dielectric constant for the insulator that functions as the interlayer film, it is possible to reduce the parasitic capacitance that occurs between wiring. Therefore, it is best to select materials according to the function of the insulator.

[0176] Further, examples of insulators with a high relative dielectric constant include gallium oxide, hafnium oxide, zirconium oxide, oxides having aluminum and hafnium, oxynitrides having aluminum and hafnium, oxides having silicon and hafnium, oxynitrides having silicon and hafnium, and nitrides having silicon and hafnium.

[0177] Examples of insulators with a low dielectric constant include silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide with fluorine added, silicon oxide with carbon added, silicon oxide with carbon and nitrogen added, silicon oxide with voids, or resin.

[0178] In addition, the transistor using metal oxide can have stable electrical characteristics by being surrounded by an insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen. As the insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen, for example, an insulator containing boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, or tantalum may be used in a single layer or a stacked layer. Specifically, as the insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, and metal nitrides such as aluminum nitride, silicon nitride oxide, and silicon nitride can be used.

[0179] The insulator that functions as the gate insulator is preferably an insulator having a region containing oxygen that is released by heating. For example, by using a structure in which silicon oxide or silicon oxynitride having a region containing oxygen that is released by heating is in contact with the oxide 230, oxygen vacancies in the oxide 230 can be compensated for.

[0180] <<Conductors>> As the conductor, it is preferable to use a metal element selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing the above-mentioned metal elements as a component, or an alloy combining the above-mentioned metal elements. For example, it is preferable to use tantalum nitride, titanium nitride, tungsten, nitride containing titanium and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel, etc. In addition, tantalum nitride, titanium nitride, nitride containing titanium and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel are conductive materials that are difficult to oxidize, or materials that maintain conductivity even when oxygen is absorbed, so they are preferable. Furthermore, a semiconductor having high electrical conductivity, typified by polycrystalline silicon containing an impurity element such as phosphorus, or a silicide such as nickel silicide may be used.

[0181] A plurality of conductive layers formed of the above-mentioned materials may be stacked. For example, a stacked structure may be formed by combining the above-mentioned material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-mentioned material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-mentioned material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.

[0182] In addition, when an oxide is used for the channel formation region of a transistor, a conductor functioning as a gate electrode preferably has a stacked structure in which a material containing a metal element and a conductive material containing oxygen are combined. In this case, the conductive material containing oxygen is preferably provided on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen released from the conductive material is easily supplied to the channel formation region.

[0183] In particular, it is preferable to use a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed as a conductor functioning as a gate electrode. A conductive material containing the above-mentioned metal element and nitrogen may also be used. For example, a conductive material containing nitrogen, such as titanium nitride or tantalum nitride, may also be used. Indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide to which silicon is added may also be used. Indium gallium zinc oxide containing nitrogen may also be used. By using such a material, hydrogen contained in the metal oxide in which the channel is formed may be captured. Alternatively, hydrogen mixed in from an external insulator may be captured.

[0184] <<Metal oxides>> It is preferable to use a metal oxide that functions as a semiconductor (oxide semiconductor) as the oxide 230. Hereinafter, metal oxides that can be applied to the oxide 230 according to the present invention will be described.

[0185] The metal oxide preferably contains at least indium or zinc. In particular, it is preferable that the metal oxide contains indium and zinc. In addition to these, it is preferable that the metal oxide contains aluminum, gallium, yttrium, tin, etc. In addition, it may contain one or more elements selected from boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, magnesium, etc.

[0186] Here, the case where the metal oxide is an In-M-Zn oxide having indium, element M, and zinc is considered. The element M is aluminum, gallium, yttrium, or tin. Other elements applicable to the element M include boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, magnesium, etc. However, there are cases where the element M may be a combination of multiple elements mentioned above.

[0187] In this specification and the like, metal oxides containing nitrogen may also be collectively referred to as metal oxides. Furthermore, metal oxides containing nitrogen may also be referred to as metal oxynitrides.

[0188] [Metal oxide structures] Oxide semiconductors (metal oxides) are classified into single-crystal oxide semiconductors and other non-single-crystal oxide semiconductors, such as CAAC-OS, polycrystalline oxide semiconductors, nanocrystalline oxide semiconductors (nc-OS), amorphous-like oxide semiconductors (a-like OS), and amorphous oxide semiconductors.

[0189] The nc-OS has periodic atomic arrangement in a microscopic region (for example, a region of 1 nm to 10 nm, particularly a region of 1 nm to 3 nm). In addition, the nc-OS does not show regularity in the crystal orientation between different nanocrystals. Therefore, no orientation is seen throughout the film. Therefore, depending on the analysis method, the nc-OS may be indistinguishable from an a-like OS or an amorphous oxide semiconductor.

[0190] In-Ga-Zn oxide (hereinafter referred to as IGZO), a type of metal oxide containing indium, gallium, and zinc, may have a stable structure when made into the above-mentioned nanocrystals. In particular, since IGZO tends to have difficulty in crystal growth in the atmosphere, it may be structurally more stable when made into small crystals (for example, the above-mentioned nanocrystals) rather than large crystals (here, crystals of several mm or several cm).

[0191] The a-like OS is a metal oxide having a structure between the nc-OS and an amorphous oxide semiconductor. The a-like OS has a pore or low-density region. That is, the a-like OS has lower crystallinity than the nc-OS and CAAC-OS.

[0192] Oxide semiconductors (metal oxides) have a variety of structures and each structure has different characteristics. The oxide semiconductor of one embodiment of the present invention may include two or more of an amorphous oxide semiconductor, a polycrystalline oxide semiconductor, an a-like OS, an nc-OS, and a CAAC-OS.

[0193] As an alternative to the oxide semiconductor, a cloud-aligned composite (CAC)-OS may be used.

[0194] CAC-OS has a conductive function in a part of the material and an insulating function in a part of the material, and the material as a whole has a function as a semiconductor. When CAC-OS or CAC-metal oxide is used in the active layer of a transistor, the conductive function is a function of flowing electrons (or holes) that become carriers, and the insulating function is a function of not flowing electrons that become carriers. By making the conductive function and the insulating function act complementarily, it is possible to impart a switching function (on / off function) to CAC-OS or CAC-metal oxide. By separating the respective functions in CAC-OS or CAC-metal oxide, it is possible to maximize both functions.

[0195] Moreover, the CAC-OS or CAC-metal oxide has a conductive region and an insulating region. The conductive region has the above-mentioned conductive function, and the insulating region has the above-mentioned insulating function. In addition, in the material, the conductive region and the insulating region may be separated at the nanoparticle level. In addition, the conductive region and the insulating region may be unevenly distributed in the material. In addition, the conductive region may be observed to be connected in a cloud shape with a blurred periphery.

[0196] In addition, in the CAC-OS or CAC-metal oxide, the conductive regions and the insulating regions may each be dispersed in the material with a size of 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm.

[0197] In addition, the CAC-OS or CAC-metal oxide is composed of components having different band gaps. For example, the CAC-OS or CAC-metal oxide is composed of a component having a wide gap due to an insulating region and a component having a narrow gap due to a conductive region. In this configuration, when carriers are caused to flow, the carriers mainly flow in the component having the narrow gap. In addition, the component having the narrow gap acts complementarily on the component having the wide gap, and carriers also flow in the component having the wide gap in conjunction with the component having the narrow gap. Therefore, when the above CAC-OS or CAC-metal oxide is used in the channel formation region of a transistor, a high current driving force in the on state of the transistor, that is, a large on-current and a high field effect mobility can be obtained.

[0198] That is, CAC-OS or CAC-metal oxide can also be called a matrix composite or a metal matrix composite.

[0199] In addition, when focusing on the crystal structure, oxide semiconductors may be classified differently from the above. Here, the classification of crystal structures in oxide semiconductors will be described with reference to FIG. 4A. FIG. 4A is a diagram for explaining the classification of crystal structures of oxide semiconductors, typically IGZO (metal oxide containing In, Ga, and Zn).

[0200] As shown in FIG. 4A, IGZO is broadly classified into Amorphous, Crystalline, and Crystal. Amorphous includes completely amorphous. Crystalline includes c-axis aligned crystalline (CAAC), nanocrystalline (nc), and cloud-aligned composite (CAC). Crystalline excludes single crystal, poly crystal, and completely amorphous. Crystal includes single crystal and poly crystal.

[0201] The structure in the bold frame shown in FIG. 4A is an intermediate state between Amorphous and Crystal, and belongs to a new boundary region (New crystalline phase). This structure is in the boundary region between Amorphous and Crystal. In other words, this structure can be said to be a structure that is completely different from Amorphous, which is energetically unstable, or Crystal.

[0202] The crystal structure of the film or substrate can be evaluated using an X-ray diffraction (XRD) image. Figures 4B and 4C show XRD spectra of quartz glass and IGZO (also called crystalline IGZO) having a crystal structure classified as Crystalline. Figure 4B shows the XRD spectrum of quartz glass, and Figure 4C shows the XRD spectrum of crystalline IGZO. The composition of the crystalline IGZO shown in Figure 4C is approximately In:Ga:Zn=4:2:3 [atomic ratio]. The thickness of the crystalline IGZO shown in Figure 4C is 500 nm.

[0203] As shown by the arrows in Figure 4B, the shape of the peak in the XRD spectrum of silica glass is almost symmetrical. On the other hand, as shown by the arrows in Figure 4C, the shape of the peak in the XRD spectrum of crystalline IGZO is asymmetrical. The asymmetric shape of the peak in the XRD spectrum clearly indicates the presence of crystals. In other words, if the shape of the peak in the XRD spectrum is not symmetrical, it cannot be said to be amorphous. Note that Figure 4C clearly shows the crystal phase (IGZO crystal phase) at or near 2θ=31°. It is presumed that the reason why the shape of the peak in the XRD spectrum is asymmetrical is due to the crystal phase (microcrystals).

[0204] Specifically, the XRD spectrum of crystalline IGZO shown in FIG. 4C has a peak at or near 2θ=34°. Microcrystals have a peak at or near 2θ=31°. When an oxide semiconductor film is evaluated using an X-ray diffraction image, the width of the spectrum on the lower angle side is wider than the peak at or near 2θ=34°, as shown in FIG. 4C. This suggests that the oxide semiconductor film contains microcrystals having a peak at or near 2θ=31°.

[0205] The crystal structure of the film can be evaluated from the diffraction pattern (also called the nanobeam electron diffraction pattern) observed by nanobeam electron diffraction (NBED). Figure 4D shows the diffraction pattern of an IGZO film formed at room temperature on the substrate. The IGZO film shown in Figure 4D was formed by sputtering using an oxide target with an In:Ga:Zn=1:1:1 [atomic ratio]. In the nanobeam electron diffraction method, electron diffraction was performed with a probe diameter of 1 nm.

[0206] As shown in Figure 4D, a spot-like pattern, not a halo, is observed in the diffraction pattern of the IGZO film deposited at room temperature. Therefore, it is presumed that the IGZO film deposited at room temperature is in an intermediate state, neither crystalline nor amorphous, and it cannot be concluded that it is in an amorphous state.

[0207] [impurities] Here, the influence of each impurity in the metal oxide will be described.

[0208] When impurities are mixed into an oxide semiconductor, defect states or oxygen vacancies may be formed. Thus, when impurities are mixed into a channel formation region of an oxide semiconductor, the electrical characteristics of a transistor using the oxide semiconductor are likely to fluctuate, and the reliability may be reduced. Furthermore, when oxygen vacancies are included in the channel formation region, the transistor is likely to have normally-on characteristics (characteristics in which a channel exists and a current flows through the transistor even when no voltage is applied to the gate electrode).

[0209] A transistor using a metal oxide is likely to have normally-on characteristics due to impurities and oxygen vacancies in the metal oxide, and when the transistor is operated in a state where the metal oxide contains excess oxygen that exceeds an appropriate amount, the valence of the excess oxygen atom changes, causing the electrical characteristics of the transistor to change, which may result in poor reliability.

[0210] Therefore, it is preferable to use a metal oxide with a low carrier concentration in the channel formation region of a transistor. In order to reduce the carrier concentration of the metal oxide, it is sufficient to reduce the impurity concentration in the metal oxide and reduce the density of defect states. In this specification and the like, a low impurity concentration and a low density of defect states are referred to as high purity intrinsic or substantially high purity intrinsic. Note that in this specification and the like, a metal oxide with a carrier concentration of 1×10 16 cm -3 The following cases are defined as substantially high purity and authentic:

[0211] The carrier concentration of the metal oxide in the channel formation region is 1×10 18 cm -3 It is preferable that the value is less than 1×10 17 cm -3 More preferably, it is 1×10 16 cm -3 More preferably, it is 1×10 13 cm -3 More preferably, it is less than 1×10 12 cm -3 The lower limit of the carrier concentration of the metal oxide in the channel formation region is not particularly limited, but is preferably, for example, 1×10 -9 cm -3 It can be said that:

[0212] Examples of impurities in metal oxides include hydrogen, nitrogen, alkali metals, alkaline earth metals, iron, nickel, and silicon. In particular, hydrogen contained in metal oxides reacts with oxygen that bonds with metal atoms to form water, which may cause oxygen vacancies in the metal oxide. If oxygen vacancies are present in the channel formation region in the metal oxide, the transistor may have normally-on characteristics. Furthermore, if hydrogen enters an oxygen vacancy in the metal oxide, the oxygen vacancy and hydrogen combine to form a V O H may be formed. A defect in which hydrogen enters an oxygen vacancy (V OHydrogen can function as a donor and generate electrons, which are carriers. In addition, some of the hydrogen can bond with oxygen, which is bonded to metal atoms, to generate electrons, which are carriers. Therefore, transistors using metal oxides that contain a lot of hydrogen tend to have normally-on characteristics. In addition, hydrogen in metal oxides is easily mobile due to stresses such as heat and electric fields, so if metal oxides contain a lot of hydrogen, the reliability of the transistor may deteriorate.

[0213] In one embodiment of the present invention, V in oxide 230 O It is preferable to reduce H as much as possible and make it high-purity intrinsic or substantially high-purity intrinsic. O In order to obtain a metal oxide with a sufficiently reduced amount of H, it is important to remove impurities such as water and hydrogen from the metal oxide (sometimes referred to as dehydration or dehydrogenation treatment) and to supply oxygen to the metal oxide to compensate for the oxygen deficiency (sometimes referred to as oxygen addition treatment). O By using a metal oxide in which impurities such as H are sufficiently reduced for the channel formation region of a transistor, stable electrical characteristics can be obtained.

[0214] A defect in which hydrogen has entered an oxygen vacancy (V O H) can function as a donor for the metal oxide. However, it is difficult to quantitatively evaluate the defect. Therefore, in the case of metal oxides, the carrier concentration may be used instead of the donor concentration. Therefore, in this specification, the carrier concentration assuming a state in which no electric field is applied may be used as a parameter of the metal oxide instead of the donor concentration. In other words, the "carrier concentration" described in this specification may be rephrased as the "donor concentration". In addition, the "carrier concentration" described in this specification may be rephrased as the "carrier density".

[0215] Therefore, it is preferable that hydrogen in the metal oxide is reduced as much as possible. Specifically, the hydrogen concentration in the metal oxide obtained by secondary ion mass spectrometry (SIMS) is 1×10 20 atoms / cm 3 Less than 1 x 10 19 atoms / cm 3 less than 5×10 18 atoms / cm 3 less than 1×10 18 atoms / cm 3 By using a metal oxide in which impurities such as hydrogen are sufficiently reduced for a channel formation region of a transistor, stable electrical characteristics can be obtained.

[0216] The defect levels may include trap levels. Charges trapped in the trap levels of metal oxides take a long time to disappear, and may behave as if they were fixed charges. Therefore, a transistor having a channel formation region made of a metal oxide with a high density of trap levels may have unstable electrical characteristics.

[0217] Furthermore, when impurities are present in a channel formation region of an oxide semiconductor, the crystallinity of the channel formation region may be reduced, or the crystallinity of an oxide provided in contact with the channel formation region may be reduced. When the crystallinity of the channel formation region is low, the stability or reliability of the transistor tends to be degraded. When the crystallinity of an oxide provided in contact with the channel formation region is low, an interface state may be formed, which may degrade the stability or reliability of the transistor.

[0218] Therefore, in order to improve the stability or reliability of a transistor, it is effective to reduce the concentration of impurities in the channel formation region of the oxide semiconductor and in its vicinity. Examples of impurities include hydrogen, nitrogen, alkali metals, alkaline earth metals, iron, nickel, silicon, and the like.

[0219] Specifically, the concentration of the impurities in the channel formation region of the oxide semiconductor and its vicinity, which is obtained by SIMS, is set to 1×10 18 atoms / cm 3 Less than or equal to 2 x 10 16 atoms / cm 3 or less. Alternatively, the concentration of the impurity in the channel formation region of the oxide semiconductor and its vicinity, which is obtained by elemental analysis using EDX, is set to 1.0 atomic % or less. Note that when an oxide containing element M is used as the oxide semiconductor, the concentration ratio of the impurity to element M in the channel formation region of the oxide semiconductor and its vicinity is set to less than 0.10, preferably less than 0.05. Here, the concentration of element M used in calculating the concentration ratio may be the concentration in the same region as the region where the concentration of the impurity is calculated, or may be the concentration in the oxide semiconductor.

[0220] Furthermore, since a metal oxide with a reduced impurity concentration has a low defect state density, the trap state density may also be low.

[0221] In addition, when impurities and oxygen vacancies are present in a channel formation region of a transistor including an oxide semiconductor, the resistance of the oxide semiconductor may be reduced and the electrical characteristics may be easily changed, resulting in reduced reliability.

[0222] For example, silicon has a higher bond energy with oxygen than indium and zinc. For example, when an In-M-Zn oxide is used as an oxide semiconductor, if silicon is mixed into the oxide semiconductor, oxygen contained in the oxide semiconductor may be taken by silicon, resulting in oxygen vacancies being formed near indium or zinc.

[0223] In a transistor using an oxide semiconductor for a channel formation region, when a low-resistance region is formed in the channel formation region, a leakage current (parasitic channel) between the source electrode and the drain electrode of the transistor is likely to occur in the low-resistance region. In addition, the parasitic channel is likely to cause defects in the transistor characteristics, such as a normally-on transistor, an increase in leakage current, and a shift in threshold voltage due to application of stress. In addition, if the processing precision of the transistor is low, the parasitic channel varies from transistor to transistor, causing variation in the transistor characteristics.

[0224] Therefore, it is preferable that the impurities and oxygen vacancies be reduced as much as possible in the channel formation region of the oxide semiconductor and its vicinity.

[0225] <<Other semiconductor materials>> The semiconductor material that can be used for the oxide 230 is not limited to the above-mentioned metal oxides. A semiconductor material having a band gap (a semiconductor material that is not a zero-gap semiconductor) may be used for the oxide 230. For example, a semiconductor of a single element such as silicon, a compound semiconductor such as gallium arsenide, or a layered material (also called an atomic layer material, a two-dimensional material, etc.) that functions as a semiconductor is preferably used for the semiconductor material. In particular, it is preferable to use a layered material that functions as a semiconductor for the semiconductor material.

[0226] Here, in this specification and the like, the layered material is a general term for a group of materials having a layered crystal structure. The layered crystal structure is a structure in which layers formed by covalent bonds or ionic bonds are stacked via bonds weaker than covalent bonds or ionic bonds, such as van der Waals forces. The layered material has high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-current can be provided.

[0227] Layered materials include graphene, silicene, and chalcogenides. Chalcogenides are compounds that contain chalcogen. Chalcogen is a general term for elements in group 16, including oxygen, sulfur, selenium, tellurium, polonium, and livermorium. Chalcogenides include transition metal chalcogenides and group 13 chalcogenides.

[0228] It is preferable to use, for example, a transition metal chalcogenide that functions as a semiconductor as the oxide 230. Specific examples of transition metal chalcogenides that can be used as the oxide 230 include molybdenum sulfide (representatively MoS2), molybdenum selenide (representatively MoSe2), molybdenum tellurium (representatively MoTe2), tungsten sulfide (representatively WS2), tungsten selenide (representatively WSe2), tungsten tellurium (representatively WTe2), hafnium sulfide (representatively HfS2), hafnium selenide (representatively HfSe2), zirconium sulfide (representatively ZrS2), and zirconium selenide (representatively ZrSe2).

[0229] <Modifications of the semiconductor device> An example of a semiconductor device according to one embodiment of the present invention will be described below with reference to FIGS. 5A to 5D. FIG.

[0230] Fig. 5A shows a top view of the semiconductor device. Fig. 5B is a cross-sectional view corresponding to the portion indicated by the dashed line A1-A2 in Fig. 5A. Fig. 5C is a cross-sectional view corresponding to the portion indicated by the dashed line A3-A4 in Fig. 5A. Fig. 5D is a cross-sectional view corresponding to the portion indicated by the dashed line A5-A6 in Fig. 5A. In the top view of Fig. 5A, some elements are omitted for clarity.

[0231] 5A to 5D, structures having the same functions as those of the structures constituting the semiconductor device shown in <Configuration example of semiconductor device> are denoted by the same reference numerals. Note that, in this section, the materials described in detail in <Configuration example of semiconductor device> can be used as the materials constituting the semiconductor device.

[0232] <<Modification 1 of the semiconductor device>> The semiconductor device shown in Figures 5A to 5D is a modified example of the semiconductor device shown in Figures 1A to 1D. The semiconductor device shown in Figures 5A to 5D is different from the semiconductor device shown in Figures 1A to 1D in the shapes of the insulators 280, 282, 283, and 284. Also, the semiconductor device is different in that it has the insulators 274 and 287.

[0233] 5A to 5D, the insulators 212, 214, 216, 222, 224, 280, and 282 are patterned, and the insulator 287 is provided in contact with the side surfaces of the insulators 212, 214, 216, 222, 224, 280, and 282. The insulators 283 and 284 are structured to cover the insulators 212, 214, 216, 222, 224, 280, 282, and 287. That is, the insulator 283 is in contact with the upper surface of the insulator 282, the upper surface and side surfaces of the insulator 287, and the upper surface of the insulator 211, and the insulator 284 is in contact with the upper surface and side surfaces of the insulator 283. As a result, the insulators 214, 216, 222, 224, 280, 282, and 287, including the oxide 230, are isolated from the outside by the insulators 283 and 284, and the insulator 211. In other words, the transistor 200 is disposed within a region sealed by the insulators 283 and 284, and the insulator 211.

[0234] For example, it is preferable to form the insulators 212, 214, 287, and 282 using a material having a function of capturing and fixing hydrogen, and to form the insulators 211, 283, and 284 using a material having a function of suppressing the diffusion of hydrogen and oxygen. Typically, the insulators 212, 214, 287, and 282 can be made of aluminum oxide. Typically, the insulators 211, 283, and 284 can be made of silicon nitride.

[0235] With this configuration, it is possible to prevent hydrogen contained outside the sealed region from entering the sealed region.

[0236] 5A to 5D, the insulator 211, the insulator 283, and the insulator 284 are each provided as a single layer, but the present invention is not limited to this. For example, each of the insulator 211, the insulator 283, and the insulator 284 may be provided as a stacked structure of two or more layers.

[0237] The insulator 274 functions as an interlayer film. The insulator 274 preferably has a lower dielectric constant than the insulator 214. By using a material with a low dielectric constant as the interlayer film, parasitic capacitance generated between wirings can be reduced. The insulator 274 can be provided using, for example, a material similar to that of the insulator 280.

[0238] <Method for manufacturing semiconductor device> Next, a manufacturing method of the semiconductor device of one embodiment of the present invention shown in FIGS. 5A to 5D will be described with reference to FIGS. 6A to 26A, FIGS. 6B to 26B, FIGS. 6C to 26C, and FIGS. 6D to 26D.

[0239] 6A to 26A are top views. FIG. 6B to 26B are cross-sectional views corresponding to the portion indicated by the dashed line A1-A2 in FIG. 6A to 26A, and are cross-sectional views in the channel length direction of the transistor 200. FIG. 6C to 26C are cross-sectional views corresponding to the portion indicated by the dashed line A3-A4 in FIG. 6A to 26A, and are cross-sectional views in the channel width direction of the transistor 200. FIG. 6D to 26D are cross-sectional views of the portion indicated by the dashed line A5-A6 in FIG. 6A to 26A. Note that some elements are omitted in the top views in FIG. 6A to 26A for clarity.

[0240] First, a substrate (not shown) is prepared, and the insulator 211 is formed on the substrate. The insulator 211 can be formed by a sputtering method, a CVD method, a molecular beam epitaxy (MBE) method, a pulsed laser deposition (PLD) method, an atomic layer deposition (ALD) method, or the like.

[0241] CVD methods can be classified into plasma enhanced CVD (PECVD), which uses plasma, thermal CVD (TCVD), which uses heat, photo CVD (Photo CVD), etc. They can also be further divided into metal CVD (MCVD) and metal organic CVD (MOCVD), depending on the source gas used.

[0242] The plasma CVD method can obtain a high-quality film at a relatively low temperature. Moreover, the thermal CVD method is a film formation method that can reduce plasma damage to the object to be processed because it does not use plasma. For example, wiring, electrodes, elements (transistors, capacitive elements, etc.) included in a semiconductor device may be charged up by receiving electric charge from plasma. At this time, the wiring, electrodes, elements, etc. included in the semiconductor device may be destroyed by the accumulated electric charge. On the other hand, in the case of the thermal CVD method that does not use plasma, such plasma damage does not occur, so the yield of the semiconductor device can be increased. Furthermore, in the thermal CVD method, plasma damage does not occur during film formation, so a film with few defects can be obtained.

[0243] As the ALD method, a thermal ALD method in which a reaction between a precursor and a reactant is carried out using only thermal energy, a plasma enhanced ALD method in which a plasma excited reactant is used, or the like can be used.

[0244] In addition, the ALD method utilizes the self-regulating nature of atoms to deposit atoms one layer at a time, and thus has the following advantages: extremely thin films can be formed; films can be formed on structures with high aspect ratios; films can be formed with fewer defects such as pinholes; films can be formed with excellent coverage; and films can be formed at low temperatures. In the PEALD method, the use of plasma can be preferable because it allows films to be formed at lower temperatures. Note that some precursors used in the ALD method contain impurities such as carbon. For this reason, films formed by the ALD method may contain more impurities such as carbon than films formed by other film formation methods. Note that the amount of impurities can be quantified using X-ray photoelectron spectroscopy (XPS).

[0245] The CVD method and the ALD method are different from the film formation method in which particles emitted from a target or the like are deposited, and are film formation methods in which a film is formed by a reaction on the surface of a workpiece. Therefore, they are film formation methods that are not easily affected by the shape of the workpiece and have good step coverage. In particular, the ALD method has excellent step coverage and excellent thickness uniformity, so it is suitable for coating the surface of an opening with a high aspect ratio. However, since the ALD method has a relatively slow film formation speed, it may be preferable to use it in combination with other film formation methods such as the CVD method, which has a fast film formation speed.

[0246] In the CVD method and the ALD method, the composition of the film obtained can be controlled by the flow rate ratio of the raw material gases. For example, in the CVD method and the ALD method, a film of any composition can be formed by changing the flow rate ratio of the raw material gases. In addition, for example, in the CVD method and the ALD method, a film whose composition changes continuously can be formed by changing the flow rate ratio of the raw material gases while forming the film. When forming a film while changing the flow rate ratio of the raw material gases, the time required for film formation can be shortened compared to the case of forming a film using multiple film formation chambers because no time is required for transportation and pressure adjustment. Therefore, the productivity of semiconductor devices can be increased in some cases.

[0247] In this embodiment, the insulator 211 is formed of silicon nitride by CVD.

[0248] Next, the insulator 212 is deposited over the insulator 211. The insulator 212 can be deposited by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, a silicon nitride film is deposited as the insulator 212 by a sputtering method.

[0249] In this way, by using an insulator such as silicon nitride through which copper does not easily permeate as insulator 211 and insulator 212, even if a metal that easily diffuses, such as copper, is used for a conductor in a layer below insulator 211 (not shown), it is possible to suppress the metal from diffusing upward through insulator 211 and insulator 212. Furthermore, by using an insulator such as silicon nitride through which impurities such as water and hydrogen do not easily permeate, it is possible to suppress the diffusion of impurities such as water and hydrogen contained in the layer below insulator 211.

[0250] Next, the insulator 214 is deposited over the insulator 212. The insulator 214 can be deposited by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, aluminum oxide is used as the insulator 214.

[0251] It is preferable that the hydrogen concentration of the insulator 212 is lower than that of the insulator 211, and the hydrogen concentration of the insulator 214 is lower than that of the insulator 212. By forming a silicon nitride film as the insulator 212 by a sputtering method, it is possible to form silicon nitride having a lower hydrogen concentration than the insulator 211 formed by forming a silicon nitride film by a CVD method. Furthermore, by using aluminum oxide as the insulator 214, it is possible to form a hydrogen concentration lower than that of the insulator 212.

[0252] In a subsequent process, the transistor 200 is formed on the insulator 214, and it is preferable that the film close to the transistor 200 has a relatively low hydrogen concentration, and it is preferable that the film with a relatively high hydrogen concentration is placed away from the transistor 200.

[0253] Next, the insulator 216 is deposited over the insulator 214. The insulator 216 can be deposited by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, silicon oxide or silicon oxynitride is used as the insulator 216. The insulator 216 is preferably deposited by a deposition method using a gas in which hydrogen atoms are reduced or removed. This allows the hydrogen concentration in the insulator 216 to be reduced.

[0254] Next, an opening is formed in the insulator 216, reaching the insulator 214. The opening may be, for example, a groove or a slit. The opening may be an area where an opening is formed. The opening may be formed by wet etching, but dry etching is preferable for fine processing. For the insulator 214, it is preferable to select an insulator that functions as an etching stopper film when etching the insulator 216 to form a groove. For example, when silicon oxide or silicon oxynitride is used for the insulator 216 that forms the groove, the insulator 214 may be silicon nitride, aluminum oxide, or hafnium oxide.

[0255] As the dry etching apparatus, a capacitively coupled plasma (CCP) etching apparatus having parallel plate electrodes can be used. The capacitively coupled plasma etching apparatus having parallel plate electrodes can be configured to apply a high frequency voltage to one of the parallel plate electrodes. Alternatively, it can be configured to apply a plurality of different high frequency voltages to one of the parallel plate electrodes. Alternatively, it can be configured to apply a high frequency voltage of the same frequency to each of the parallel plate electrodes. Alternatively, it can be configured to apply high frequency voltages of different frequencies to each of the parallel plate electrodes. Alternatively, a dry etching apparatus having a high density plasma source can be used. As the dry etching apparatus having a high density plasma source, for example, an inductively coupled plasma (ICP) etching apparatus or the like can be used.

[0256] After the opening is formed, a conductive film that becomes the conductor 205a is formed. The conductive film preferably contains a conductor that has a function of suppressing oxygen permeation. For example, tantalum nitride, tungsten nitride, titanium nitride, or the like can be used. Alternatively, the conductive film may be a stacked film of a conductor that has a function of suppressing oxygen permeation and tantalum, tungsten, titanium, molybdenum, aluminum, copper, or a molybdenum-tungsten alloy. The conductive film can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.

[0257] In this embodiment, the conductive film that becomes the conductor 205a has a multi-layer structure. First, a tantalum nitride film is formed by sputtering, and titanium nitride is laminated on the tantalum nitride. By using such a metal nitride as the lower layer of the conductor 205b, even if a metal that easily diffuses, such as copper, is used for the conductive film that becomes the conductor 205b described later, the metal can be prevented from diffusing out of the conductor 205a.

[0258] Next, a conductive film that becomes the conductor 205b is formed. The conductive film can be formed by a plating method, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, etc. In this embodiment, a low-resistance conductive material such as copper is formed as the conductive film that becomes the conductor 205b.

[0259] Next, a CMP process is performed to remove the conductive film that will become the conductor 205a and a portion of the conductive film that will become the conductor 205b, exposing the insulator 216. As a result, the conductor 205a and the conductor 205b remain only in the openings. This makes it possible to form a conductor 205 with a flat upper surface (see FIGS. 6A to 6D). Note that the CMP process may remove a portion of the insulator 216.

[0260] In the above description, the conductor 205 is formed so as to be embedded in the opening of the insulator 216, but the present embodiment is not limited to this. For example, the conductor 205 may be formed on the insulator 214, the insulator 216 may be formed on the conductor 205, and the insulator 216 may be subjected to CMP treatment to remove a part of the insulator 216 and expose the surface of the conductor 205.

[0261] Next, the insulator 222 is formed on the insulator 216 and the conductor 205. As the insulator 222, an insulator containing one or both of an oxide of aluminum and hafnium may be formed. Note that as the insulator containing one or both of an oxide of aluminum and hafnium, it is preferable to use aluminum oxide, hafnium oxide, an oxide containing aluminum and hafnium (hafnium aluminate), or the like. The insulator containing one or both of an oxide of aluminum and hafnium has a barrier property against oxygen, hydrogen, and water. When the insulator 222 has a barrier property against hydrogen and water, the hydrogen and water contained in the structure provided around the transistor 200 are prevented from diffusing into the inside of the transistor 200 through the insulator 222, and the generation of oxygen vacancies in the oxide 230 can be suppressed.

[0262] The insulator 222 can be formed by sputtering, CVD, MBE, PLD, ALD, or the like.

[0263] It is preferable to carry out a heat treatment subsequently. The heat treatment may be carried out at 250°C or higher and 650°C or lower, preferably 300°C or higher and 500°C or lower, and more preferably 320°C or higher and 450°C or lower. The heat treatment may be carried out in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing 10 ppm or higher, 1% or higher, or 10% or higher of an oxidizing gas. For example, when the heat treatment is carried out in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas may be about 20%. The heat treatment may be carried out under reduced pressure. Alternatively, the heat treatment may be carried out in an atmosphere of nitrogen gas or an inert gas, and then in an atmosphere containing 10 ppm or higher, 1% or higher, or 10% or higher of an oxidizing gas to compensate for the desorbed oxygen.

[0264] In addition, it is preferable that the gas used in the heat treatment is highly purified. For example, the amount of moisture contained in the gas used in the heat treatment is 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By performing the heat treatment using a highly purified gas, it is possible to prevent moisture and the like from being taken into the insulator 222 as much as possible.

[0265] In this embodiment, after the insulator 222 is formed, heat treatment is performed at a flow rate ratio of nitrogen gas and oxygen gas of 4 slm:1 slm at a temperature of 400° C. for one hour. The heat treatment can remove impurities such as water and hydrogen contained in the insulator 222. When an oxide containing hafnium is used as the insulator 222, the heat treatment can improve the crystallinity of the insulator 222. The heat treatment can also be performed at a timing such as after the insulator 224 is formed.

[0266] Next, the insulator 224 is formed on the insulator 222. The insulator 224 can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, a silicon oxide or silicon oxynitride film is formed as the insulator 224 by a CVD method. The insulator 224 is preferably formed by a film formation method using a gas in which hydrogen atoms are reduced or removed. This allows the hydrogen concentration of the insulator 224 to be reduced. Since the insulator 224 becomes the insulator 224 in contact with the oxide 230a in a later process, it is preferable that the hydrogen concentration be reduced in this manner.

[0267] Here, in order to form an excess oxygen region in the insulator 224, a plasma treatment including oxygen may be performed under reduced pressure. For the plasma treatment including oxygen, it is preferable to use an apparatus having a power source that generates high density plasma using, for example, microwaves. Alternatively, the apparatus may have a power source that applies RF (Radio Frequency) to the substrate side. By using high density plasma, high density oxygen radicals can be generated, and by applying RF to the substrate side, the oxygen radicals generated by the high density plasma can be efficiently guided into the insulator 224. Alternatively, after performing a plasma treatment including an inert gas using this apparatus, a plasma treatment including oxygen may be performed to compensate for the desorbed oxygen. Note that impurities such as water and hydrogen contained in the insulator 224 can be removed by appropriately selecting the conditions for the plasma treatment. In that case, heat treatment does not need to be performed.

[0268] Here, after forming an aluminum oxide film on the insulator 224 by, for example, a sputtering method, a CMP process may be performed until the insulator 224 is reached. The CMP process can planarize and smooth the surface of the insulator 224. By disposing the aluminum oxide on the insulator 224 and performing the CMP process, it becomes easy to detect the end point of the CMP process. In addition, the CMP process may polish a part of the insulator 224, and the thickness of the insulator 224 may become thin, but the thickness may be adjusted when the insulator 224 is formed. By planarizing and smoothing the surface of the insulator 224, it may be possible to prevent a deterioration in the coverage rate of the oxide to be formed later and to prevent a decrease in the yield of the semiconductor device. In addition, it is preferable to form an aluminum oxide film on the insulator 224 by a sputtering method, since oxygen can be added to the insulator 224.

[0269] Next, oxide film 230A and oxide film 230B are sequentially formed on insulator 224 (see FIGS. 6A to 6D). Note that oxide film 230A and oxide film 230B are preferably formed successively without being exposed to the air environment. By forming the films without exposing them to the air, it is possible to prevent impurities or moisture from the air environment from adhering to oxide film 230A and oxide film 230B, and it is possible to keep the vicinity of the interface between oxide film 230A and oxide film 230B clean.

[0270] The oxide film 230A and the oxide film 230B can be formed by using a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.

[0271] For example, when the oxide film 230A and the oxide film 230B are formed by sputtering, oxygen or a mixed gas of oxygen and a rare gas is used as the sputtering gas. By increasing the ratio of oxygen contained in the sputtering gas, the excess oxygen in the oxide film to be formed can be increased. In addition, when the oxide film is formed by sputtering, the above-mentioned In-M-Zn oxide target can be used.

[0272] In particular, during the formation of the oxide film 230A, a portion of the oxygen contained in the sputtering gas may be supplied to the insulator 224. Therefore, the ratio of oxygen contained in the sputtering gas may be set to 70% or more, preferably 80% or more, and more preferably 100%.

[0273] When the oxide film 230B is formed by a sputtering method, an oxygen-excessive oxide semiconductor is formed when the ratio of oxygen contained in the sputtering gas is more than 30% and less than or equal to 100%, preferably 70% to 100%. A transistor using an oxygen-excessive oxide semiconductor for a channel formation region can have relatively high reliability. However, one embodiment of the present invention is not limited thereto. When the oxide film 230B is formed by a sputtering method, an oxygen-deficient oxide semiconductor is formed when the ratio of oxygen contained in the sputtering gas is more than or equal to 1% and less than or equal to 30%, preferably 5% to 20%,. A transistor using an oxygen-deficient oxide semiconductor for a channel formation region can have relatively high field-effect mobility. When the oxide film is formed while the substrate is heated, the crystallinity of the oxide film can be improved.

[0274] In this embodiment, the oxide film 230A is formed by sputtering using an oxide target with an atomic ratio of In:Ga:Zn=1:3:4. The oxide film 230B is formed by sputtering using an oxide target with an atomic ratio of In:Ga:Zn=4:2:4.1. Each oxide film may be formed according to the characteristics required for the oxide 230a and the oxide 230b by appropriately selecting the film formation conditions and atomic ratio.

[0275] Next, the oxide film 243A is formed on the oxide film 230B (see FIGS. 6A to 6D). The oxide film 243A can be formed by sputtering, CVD, MBE, PLD, ALD, or the like. The atomic ratio of Ga to In in the oxide film 243A is preferably greater than the atomic ratio of Ga to In in the oxide film 230B. In this embodiment, the oxide film 243A is formed by sputtering using an oxide target with an atomic ratio of In:Ga:Zn=1:3:4.

[0276] It is preferable to form the insulator 222, the insulator 224, the oxide film 230A, the oxide film 230B, and the oxide film 243A without exposing them to the atmosphere, for example, by using a multi-chamber type film forming apparatus.

[0277] Next, it is preferable to perform a heat treatment. The heat treatment may be performed in a temperature range in which the oxide film 230A, the oxide film 230B, and the oxide film 243A are not polycrystallized, and may be performed at 250°C to 650°C, preferably 400°C to 600°C. The heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas may be about 20%. The heat treatment may be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere of nitrogen gas or an inert gas, and then in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas to compensate for the desorbed oxygen.

[0278] In addition, the gas used in the heat treatment is preferably highly purified. For example, the amount of moisture contained in the gas used in the heat treatment may be 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By using a highly purified gas to perform the heat treatment, it is possible to prevent moisture and the like from being taken into the oxide film 230A, the oxide film 230B, and the oxide film 243A as much as possible.

[0279] In this embodiment, the heat treatment is performed in a nitrogen atmosphere at 550° C. for 1 hour, followed by another heat treatment in an oxygen atmosphere at 550° C. for 1 hour. This heat treatment can remove impurities such as water and hydrogen from the oxide film 230A, the oxide film 230B, and the oxide film 243A. Furthermore, this heat treatment can improve the crystallinity of the oxide film 230B, resulting in a denser and more compact structure. This can reduce the diffusion of oxygen or impurities in the oxide film 230B.

[0280] Next, the conductive film 242A is formed on the oxide film 243A (see FIGS. 6A to 6D). The conductive film 242A can be formed by sputtering, CVD, MBE, PLD, ALD, or the like. For example, tantalum nitride may be formed as the conductive film 242A by sputtering. Note that heat treatment may be performed before the conductive film 242A is formed. The heat treatment may be performed under reduced pressure, and the conductive film 242A may be formed continuously without exposure to the air. By performing such treatment, moisture and hydrogen adsorbed on the surface of the oxide film 243A can be removed, and the moisture concentration and hydrogen concentration in the oxide film 230A, the oxide film 230B, and the oxide film 243A can be further reduced. The temperature of the heat treatment is preferably 100° C. or higher and 400° C. or lower. In this embodiment, the temperature of the heat treatment is set to 200° C.

[0281] Next, the insulating film 271A is formed on the conductive film 242A (see FIGS. 6A to 6D). The insulating film 271A can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. The insulating film 271A is preferably an insulating film having a function of suppressing oxygen permeation. For example, the insulating film 271A may be formed of aluminum oxide, hafnium oxide, silicon nitride, or the like by a sputtering method or an ALD method.

[0282] Next, a conductive film 248A is formed over the insulating film 271A (see FIGS. 6A to 6D). The conductive film 248A can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. The conductive film 248A may be, for example, a conductive film similar to the conductive film 242A.

[0283] Next, the oxide film 230A, the oxide film 230B, the oxide film 243A, the conductive film 242A, the insulating film 271A, and the conductive film 248A are processed into an island shape by using a lithography method to form the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 (see FIGS. 7A to 7D). This processing can be performed using a dry etching method or a wet etching method. Processing using the dry etching method is suitable for fine processing. The oxide film 230A, the oxide film 230B, the oxide film 243A, the conductive film 242A, the insulating film 271A, and the conductive film 248A may be processed under different conditions. In this process, the thickness of the region of the insulator 224 that does not overlap with the oxide 230a may be thin.

[0284] In the lithography method, first, the resist is exposed through a mask. Next, the exposed area is removed or left using a developer to form a resist mask. Next, a conductor, a semiconductor, an insulator, or the like can be processed into a desired shape by etching through the resist mask. For example, a resist mask may be formed by exposing the resist using KrF excimer laser light, ArF excimer laser light, EUV (Extreme Ultraviolet) light, or the like. Also, a liquid immersion technique may be used in which a liquid (e.g., water) is filled between the substrate and the projection lens and exposure is performed. Also, an electron beam or an ion beam may be used instead of the light described above. When an electron beam or an ion beam is used, a mask is not required. The resist mask can be removed by performing a dry etching process such as ashing, a wet etching process, a wet etching process after a dry etching process, or a dry etching process after a wet etching process.

[0285] Furthermore, a hard mask made of an insulator or a conductor may be used under the resist mask. When using a hard mask, an insulating film or a conductive film that is to be a hard mask material is formed on the conductive film 242A, a resist mask is formed thereon, and the hard mask material is etched to form a hard mask of a desired shape. Etching of the conductive film 242A and the like may be performed after removing the resist mask, or may be performed while leaving the resist mask. In the latter case, the resist mask may disappear during etching. After etching of the conductive film 242A and the like, the hard mask may be removed by etching. On the other hand, if the material of the hard mask does not affect a later process or can be used in a later process, it is not necessarily necessary to remove the hard mask. In this embodiment, the insulating layer 271B and the conductive layer 248 are used as the hard mask.

[0286] Here, since the insulating layer 271B and the conductive layer 248 function as a mask for the conductive layer 242B, the conductive layer 242B does not have a curved surface between the side surface and the top surface, as shown in FIGS. 7B to 7D. As a result, the conductors 242a and 242b shown in FIGS. 5B and 5D have angular ends where the side surface and the top surface intersect. The angular end where the side surface and the top surface of the conductor 242 intersect increases the cross-sectional area of ​​the conductor 242 compared to when the end has a curved surface. This reduces the resistance of the conductor 242, and therefore the on-current of the transistor 200 can be increased.

[0287] Moreover, the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 are formed so as to at least partially overlap with the conductor 205. Moreover, it is preferable that the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 are approximately perpendicular to the upper surface of the insulator 222. Since the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 are approximately perpendicular to the upper surface of the insulator 222, it is possible to reduce the area and increase the density when providing a plurality of transistors 200. Alternatively, the angle between the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 and the upper surface of the insulator 222 may be low. In this case, the angle between the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 and the upper surface of the insulator 222 is preferably 60 degrees or more and less than 70 degrees. By adopting such a shape, the coverage of the insulating film 272A and the like can be improved in the subsequent steps, and defects such as voids can be reduced.

[0288] Here, during etching of the oxide 230a and the oxide 230b, a layer 247 may be formed covering the insulator 224, the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 (see FIGS. 7A to 7D). The layer 247 is a layer formed when a part of the conductive layer 248 is etched, floats up in the chamber, and is deposited again. Thus, the layer 247 is an oxide containing the main component of the conductive layer 248. For example, when tantalum nitride is used for the conductive layer 248, the layer 247 is an oxide containing tantalum.

[0289] Next, the layer 247 formed to cover the insulator 224, the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248 is removed (see FIGS. 8A to 8D). The layer 247 may be removed by a dry etching method or a wet etching method. The conductive layer 248 may be removed at the same time as the layer 247 is removed.

[0290] In this manner, by removing the layer 247 that covered the insulator 224, the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, the insulating layer 271B, and the conductive layer 248, the insulator 280 to be formed in a later process can be disposed in contact with the upper surface of the insulator 224. This allows oxygen to diffuse from the insulator 280 to the insulator 224 as shown in FIG. 3, so that oxygen can be efficiently supplied to the channel formation region of the oxide 230.

[0291] 8 shows the case where the layer 247 is completely removed, but as shown in FIG. 27A, the layer 247A may remain in contact with the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, and the insulating layer 271B. Here, FIG. 27A is an enlarged view of the area corresponding to FIG. 8D. That is, the layer 247A is formed in the sidewall shape of the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, and the insulating layer 271B.

[0292] Even when the layer 247A is formed, the upper surface of the insulator 224 is exposed, so that the insulator 280 formed in a later step can be disposed in contact with the upper surface of the insulator 224. Therefore, oxygen can be efficiently supplied from the insulator 280 through the insulator 224 to the channel formation region of the oxide 230.

[0293] If the manufacturing process of the transistor 200 is continued while the layer 247A remains, the insulator 272b will be formed covering the layer 247A, as shown in Fig. 27B. Here, Fig. 27B is an enlarged view of the area corresponding to Fig. 5D. In this manner, the layer 247A is formed in contact with the side surface of the oxide 230b, and the insulator 272 is formed covering the layer 247, thereby making it possible to suppress the diffusion of oxygen from the insulator 280 to the side surface of the oxide 230b.

[0294] Next, the insulating film 272A is formed over the insulator 224, the oxide 230a, the oxide 230b, the oxide layer 243B, the conductive layer 242B, and the insulating layer 271B (see FIGS. 9A to 9D). The insulating film 272A can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, aluminum oxide is formed as the insulating film 272A by a sputtering method. For example, by forming the insulating film 272A by an RF sputtering method using an aluminum oxide target in an oxygen-free atmosphere, the insulating film 272A can be formed without adding excess oxygen to the oxide 230b.

[0295] Furthermore, by forming the insulating film 272A using the ALD method, it is possible to form a film that is dense, has fewer defects such as cracks and pinholes, and has a uniform thickness.

[0296] Next, the insulating film 272A is anisotropically etched to remove the insulating film 272A on the insulating layer 271B and the insulating film 272A on the insulator 224 (see FIGS. 10A to 10D). If the conductive layer 248 remains in the process shown in FIG. 8, it can be removed by the anisotropic etching. As a result, the insulating layer 272B is formed in contact with the side surfaces of the oxide 230a, the side surfaces of the oxide 230b, the side surfaces of the oxide layer 243B, the side surfaces of the conductive layer 242B, and the side surfaces of the insulating layer 271B. In this process, the film thickness of the exposed region of the insulator 224 may be thinner than the film thickness of the region of the insulator 224 that overlaps with the insulating layer 272B.

[0297] In this manner, the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B can be covered with the insulating layer 272B and the insulating layer 271B, which have the function of suppressing the diffusion of oxygen. This makes it possible to prevent oxygen from diffusing directly from the insulator 280 to the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B when the insulator 280 is formed on the insulating layer 272B and the insulating layer 271B in a later process and oxygen is diffused from the insulator 280.

[0298] Next, an insulating film to be the insulator 280 is formed on the insulator 224, the insulating layer 272B, and the insulating layer 271B. The insulating film can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. For example, a silicon oxide film may be formed as the insulating film by a sputtering method, and a silicon oxide film may be formed thereon by a PEALD method or a thermal ALD method. In addition, the insulating film is preferably formed by a film forming method using a gas in which hydrogen atoms are reduced or removed. This makes it possible to reduce the hydrogen concentration of the insulator 280. Note that a heat treatment may be performed before the insulating film is formed. The heat treatment may be performed under reduced pressure, and the insulating film may be formed continuously without exposure to the atmosphere. By carrying out such a treatment, it is possible to remove moisture and hydrogen adsorbed on the surfaces of the insulator 224, the insulating layer 272B, and the insulating layer 271B, and further to reduce the moisture concentration and hydrogen concentration in the oxide 230a, the oxide 230b, the oxide layer 243B, and the insulator 224. The above-mentioned heat treatment conditions can be used for the heat treatment.

[0299] Next, the insulating film is subjected to CMP processing to form an insulator 280 with a flat upper surface (see FIGS. 11A to 11D). As with the insulator 224, an aluminum oxide film may be formed on the insulator 280 by, for example, a sputtering method, and CMP may be performed until the aluminum oxide reaches the insulator 280.

[0300] Here, a microwave treatment may be performed. The microwave treatment is preferably performed in an oxygen-containing atmosphere under reduced pressure. By performing the microwave treatment, an electric field due to microwaves is applied to the insulator 280, the oxide 230b, the oxide 230a, etc., and the V in the oxide 230b and the oxide 230a is increased. O H is oxygen deficiency (V O ) and hydrogen (H). At this time, some of the hydrogen that is separated may combine with oxygen contained in the insulator 280 and be removed as water molecules. Also, some of the hydrogen may be gettered to the conductor 242 via the insulating layer 272B and the insulating layer 271B.

[0301] After the microwave treatment, a heat treatment may be performed while maintaining the reduced pressure. By performing such a treatment, hydrogen in the insulator 280, the oxide 230b, and the oxide 230a can be efficiently removed. Note that the heat treatment temperature is preferably 300° C. or higher and 500° C. or lower.

[0302] Furthermore, by performing microwave treatment, the film quality of the insulator 280 can be modified, thereby suppressing the diffusion of hydrogen, water, impurities, etc. Therefore, it is possible to suppress the diffusion of hydrogen, water, impurities, etc. into the oxide 230 through the insulator 280 in a post-process after the formation of the insulator 280, or by heat treatment, etc.

[0303] Next, a part of the insulator 280, a part of the insulating layer 271B, a part of the insulating layer 272B, a part of the conductive layer 242B, a part of the oxide layer 243B, and a part of the oxide 230b are processed to form an opening that reaches the oxide 230b. The opening is preferably formed so as to overlap the conductor 205. By forming the opening, the insulator 271a, the insulator 271b, the insulator 272a, the insulator 272b, the conductor 242a, the conductor 242b, the oxide 243a, and the oxide 243b are formed (see FIGS. 12A to 12D).

[0304] When forming the opening, the upper part of the oxide 230b is removed. By removing a part of the oxide 230b, a groove is formed in the oxide 230b. Depending on the depth of the groove, the groove may be formed in the process of forming the opening, or may be formed in a process different from the process of forming the opening.

[0305] In addition, a part of the insulator 280, a part of the insulating layer 271B, a part of the insulating layer 272B, a part of the conductive layer 242B, a part of the oxide layer 243B, and a part of the oxide 230b can be processed by dry etching or wet etching. Processing by the dry etching method is suitable for fine processing. In addition, the processing may be performed under different conditions. For example, a part of the insulator 280 may be processed by dry etching, a part of the insulating layer 271B and a part of the insulating layer 272B may be processed by wet etching, and a part of the oxide layer 243B, a part of the conductive layer 242B, and a part of the oxide 230b may be processed by dry etching. In addition, processing of a part of the oxide layer 243B and a part of the conductive layer 242B and processing of a part of the oxide 230b may be performed under different conditions.

[0306] Here, when a part of the oxide 230b is removed by dry etching to form a groove, it is preferable to perform the process by increasing the bias power. For example, the power density of the bias power is set to 0.02 W / cm 2 Above 0.03W / cm 2 It is preferable to set it to 0.06 W / cm or more. 2 It is more preferable that the dry etching time is set to be equal to or longer than that. The dry etching time may be appropriately set according to the depth of the groove.

[0307] Here, it is preferable to remove impurities attached to the surfaces of the oxide 230a, the oxide 230b, etc. or diffused therein. It is also preferable to remove damaged areas formed on the surface of the oxide 230b by the dry etching. The impurities include those originating from components contained in the insulator 280, a part of the insulating layer 271B, a part of the insulating layer 272B, and the conductive layer 242B, components contained in the members used in the device used to form the opening, and components contained in the gas or liquid used in the etching. The impurities include, for example, aluminum, silicon, tantalum, fluorine, and chlorine.

[0308] In particular, impurities such as aluminum or silicon inhibit the oxide 230b or the oxide 230c formed in a later step from becoming a CAAC-OS. Therefore, it is preferable that impurity elements such as aluminum or silicon that inhibit the CAAC-OS formation are reduced or removed. For example, the concentration of aluminum atoms at the interface between the oxide 230b and the oxide 230c formed in a later step and in the vicinity thereof may be 5.0 atomic % or less, preferably 2.0 atomic % or less, more preferably 1.5 atomic % or less, even more preferably 1.0 atomic % or less, and even more preferably less than 0.3 atomic %.

[0309] In addition, the region of the metal oxide in which the CAAC-OS formation is inhibited by impurities such as aluminum or silicon and which becomes an amorphous-like oxide semiconductor (a-like OS) is sometimes called a non-CAAC region. In the non-CAAC region, the density of the crystal structure is reduced, so the V O A large amount of H is formed, which makes the transistor more likely to be normally on. Therefore, it is preferable that the non-CAAC regions of the oxide 230b and the oxide 230c are reduced or removed.

[0310] In contrast, it is preferable that the oxide 230b and the oxide 230c have a layered CAAC structure. In particular, it is preferable that the oxide 230b and the oxide 230c have a CAAC structure up to the drain lower end. Here, in the transistor 200, the conductor 242a or the conductor 242b and its vicinity function as the drain. In other words, it is preferable that either one or both of the oxide 230b and the oxide 230c near the lower end of the conductor 242a (conductor 242b) have a CAAC structure. In this way, even at the drain end that significantly affects the drain breakdown voltage, the damaged region of the oxide 230b is removed, and by having the CAAC structure, the fluctuation of the electrical characteristics of the transistor 200 can be further suppressed. In addition, the reliability of the transistor 200 can be improved.

[0311] In order to remove the above-mentioned impurities, a cleaning process is performed. The cleaning method includes wet cleaning using a cleaning solution, plasma processing using plasma, cleaning by heat treatment, and the like, and the above cleaning methods may be combined appropriately. Note that the above-mentioned grooves may become deeper due to the cleaning process.

[0312] For wet cleaning, a cleaning process may be performed using an aqueous solution of ammonia water, oxalic acid, phosphoric acid, hydrofluoric acid, or the like diluted with carbonated water or pure water, pure water, carbonated water, or the like. Alternatively, ultrasonic cleaning may be performed using these aqueous solutions, pure water, or carbonated water. Alternatively, these cleaning methods may be combined as appropriate.

[0313] In this specification, an aqueous solution obtained by diluting commercially available hydrofluoric acid with pure water may be called diluted hydrofluoric acid, and an aqueous solution obtained by diluting commercially available ammonia water with pure water may be called diluted ammonia water. The concentration and temperature of the aqueous solution may be appropriately adjusted depending on the impurities to be removed and the configuration of the semiconductor device to be cleaned. The ammonia concentration of the diluted ammonia water may be 0.01% or more and 5% or less, preferably 0.1% or more and 0.5% or less. The hydrogen fluoride concentration of the diluted hydrofluoric acid may be 0.01 ppm or more and 100 ppm or less, preferably 0.1 ppm or more and 10 ppm or less.

[0314] In addition, it is preferable to use a frequency of 200 kHz or more, and more preferably 900 kHz or more, for ultrasonic cleaning. By using such a frequency, damage to the oxide 230b and the like can be reduced.

[0315] The above cleaning process may be performed multiple times, and the cleaning solution may be changed for each cleaning process. For example, a first cleaning process may be performed using diluted hydrofluoric acid or diluted ammonia water, and a second cleaning process may be performed using pure water or carbonated water.

[0316] In the present embodiment, as the cleaning process, wet cleaning is performed using diluted hydrofluoric acid, followed by wet cleaning using pure water or carbonated water. By performing this cleaning process, impurities attached to the surfaces of the oxide 230a, the oxide 230b, etc. or diffused inside can be removed. Furthermore, the crystallinity of the oxide 230c formed on the oxide 230b can be improved.

[0317] In the past, processing such as dry etching or the above-mentioned cleaning process may result in the thickness of insulator 224 in the area that overlaps with the opening but does not overlap with oxide 230b and insulator 272 being thinner than the thickness of insulator 224 in the area that overlaps with oxide 230b.

[0318] After the etching or cleaning, a heat treatment may be performed. The heat treatment may be performed at a temperature of 100° C. to 450° C., preferably 350° C. to 400° C. The heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. For example, the heat treatment is preferably performed in an oxygen atmosphere. This supplies oxygen to the oxide 230a and the oxide 230b, thereby reducing the oxygen vacancy V. O It is possible to reduce the amount of oxide 230c formed in the grooves of the oxide 230b. In addition, by carrying out such a heat treatment, the crystallinity of the oxide 230b can be improved, and the crystallinity of the oxide 230c formed in the grooves of the oxide 230b can also be improved. The heat treatment may be carried out under reduced pressure. Alternatively, after the heat treatment in an oxygen atmosphere, the heat treatment may be carried out continuously in a nitrogen atmosphere without exposure to the air.

[0319] Next, the oxide film 230C is formed (see FIGS. 13A to 13D). A heat treatment may be performed before the formation of the oxide film 230C. The heat treatment is preferably performed under reduced pressure, and the oxide film 230C is continuously formed without exposure to the atmosphere. The heat treatment is also preferably performed in an atmosphere containing oxygen. By performing such a treatment, moisture and hydrogen adsorbed on the surface of the oxide 230b can be removed, and the moisture concentration and hydrogen concentration in the oxide 230a and the oxide 230b can be further reduced. The temperature of the heat treatment is preferably 100° C. or more and 400° C. or less. In this embodiment, the temperature of the heat treatment is 200° C.

[0320] Here, it is preferable that the oxide film 230C is provided so as to be in contact with at least the inner wall of the groove formed in the oxide 230b, a part of the side surface of the oxide 243, a part of the side surface of the conductor 242, a part of the side surface of the insulator 271, and a part of the side surface of the insulator 280. By being surrounded by the oxide 243, the insulator 271, the insulator 272, and the oxide film 230C, the decrease in conductivity of the conductor 242 due to oxidation in the subsequent steps can be suppressed.

[0321] The oxide film 230C can be formed by sputtering, CVD, MBE, PLD, ALD, or the like. The oxide film 230C may be formed by the same film formation method as the oxide film 230A or the oxide film 230B according to the desired characteristics of the oxide film 230C. In this embodiment, the oxide film 230C is formed by sputtering using an oxide target with In:Ga:Zn=4:2:3 [atomic ratio], an oxide target with In:Ga:Zn=5:1:3 [atomic ratio], an oxide target with In:Ga:Zn=10:1:3 [atomic ratio], or an indium oxide target.

[0322] When the oxide film 230C is formed, some of the oxygen contained in the sputtering gas may be supplied to the oxide 230a and the oxide 230b. Alternatively, when the oxide film 230C is formed, some of the oxygen contained in the sputtering gas may be supplied to the insulator 280. Therefore, the proportion of oxygen contained in the sputtering gas for the oxide film 230C may be 70% or more, preferably 80% or more, and more preferably 100%. Furthermore, by forming the oxide film 230C in an atmosphere containing a large amount of oxygen in this manner, it becomes easier to make the oxide film 230C into a CAAC-OS.

[0323] The oxide film 230C is preferably formed while heating the substrate. At this time, by setting the substrate temperature to 200° C. or higher, oxygen vacancies in the oxide film 230C and the oxide 230b can be reduced. By forming the oxide film 230C while heating the substrate, the crystallinity of the oxide film 230C and the oxide 230b can be improved.

[0324] Next, a mask is formed by lithography on the oxide film 230C. Note that as the mask, a hard mask or a resist mask may be used.

[0325] Next, the above mask is used to selectively remove a portion of the oxide film 230C (see FIGS. 14A, 14C, and 14D). The portion of the oxide film 230C may be removed by wet etching or the like. This process can remove a portion of the oxide film 230C located between the transistors 200 adjacent to each other in the channel width direction.

[0326] In the above process, in the region where part of oxide film 230C has been removed, the surfaces of insulator 224 and insulator 280 are exposed. At this time, the film thickness of insulator 224 and the film thickness of insulator 280 in the region may become thin. Also, insulator 224 in the region may be removed, exposing the surface of insulator 222. The process of forming the mask may also serve as a process of removing part of oxide film 230C.

[0327] Next, the mask is removed (see FIGS. 14A, 14C, and 14D). The mask may be removed by etching or the like.

[0328] Next, an oxide film 230D is formed (see FIGS. 15A to 15D). It is preferable that the oxide film 230D is formed continuously from the oxide film 230C without exposure to the atmosphere.

[0329] The oxide film 230D can be formed by sputtering, CVD, MBE, PLD, ALD, or the like. The oxide film 230D may be formed by the same film formation method as the oxide film 230A or the oxide film 230B according to the characteristics required for the oxide film 230D. In this embodiment, the oxide film 230D is formed by sputtering using an oxide target with an atomic ratio of In:Ga:Zn=1:3:4.

[0330] When the oxide film 230D is formed, some of the oxygen contained in the sputtering gas may be supplied to the oxide film 230C. Alternatively, when the oxide film 230D is formed, some of the oxygen contained in the sputtering gas may be supplied to the insulator 280. Therefore, the ratio of oxygen contained in the sputtering gas for the oxide film 230D may be 70% or more, preferably 80% or more, and more preferably 100%.

[0331] Next, the insulating film 250A is formed (see FIGS. 15A to 15D). A heat treatment may be performed before the formation of the insulating film 250A. The heat treatment may be performed under reduced pressure, and the insulating film 250A may be formed continuously without exposure to the atmosphere. The heat treatment is preferably performed in an atmosphere containing oxygen. By performing such a treatment, moisture and hydrogen adsorbed on the surface of the oxide film 230C can be removed, and the moisture concentration and hydrogen concentration in the oxide 230a, the oxide 230b, and the oxide film 230C can be further reduced. The temperature of the heat treatment is preferably 100° C. or higher and 400° C. or lower.

[0332] The insulating film 250A can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. The insulating film 250A is preferably formed by a film formation method using a gas in which hydrogen atoms are reduced or removed. This allows the hydrogen concentration of the insulating film 250A to be reduced. Since the insulating film 250A becomes the insulator 250 that contacts the oxide 230d in a later process, it is preferable that the hydrogen concentration is reduced in this manner.

[0333] When the insulator 250 has a two-layer laminated structure, it is preferable to continuously deposit the insulating film that will be the lower layer of the insulator 250 and the insulating film that will be the upper layer of the insulator 250 without exposing them to the atmospheric environment. By depositing the films without exposing them to the atmosphere, it is possible to prevent impurities or moisture from the atmospheric environment from adhering to the insulating film that will be the lower layer of the insulator 250 and the insulating film that will be the upper layer of the insulator 250, and it is possible to keep the vicinity of the interface between the insulating film that will be the lower layer of the insulator 250 and the insulating film that will be the upper layer of the insulator 250 clean.

[0334] Here, after the insulating film 250A is formed, a microwave treatment may be performed under an oxygen-containing atmosphere and reduced pressure. By performing the microwave treatment, an electric field due to microwaves is applied to the insulating film 250A, the oxide film 230D, the oxide film 230C, the oxide 230b, the oxide 230a, etc., and V in the oxide film 230C, the oxide 230b, and the oxide 230a is increased. O H to V O and hydrogen. At this time, some of the hydrogen separated may combine with oxygen to become H2O, which may be removed from the insulating film 250A, the oxide film 230D, the oxide film 230C, the oxide 230b, and the oxide 230a. Also, some of the hydrogen may be gettered to the conductor 242 (the conductor 242a and the conductor 242b). In this way, by performing microwave processing, the hydrogen concentrations in the insulating film 250A, the oxide film 230D, the oxide film 230C, the oxide 230b, and the oxide 230a can be reduced. Also, the V in the oxide 230a, the oxide 230b, and the oxide film 230C can be reduced. O H to V O V that can exist after splitting into and hydrogenO Oxygen is supplied to V O can be repaired or compensated for.

[0335] Also, a heat treatment may be performed while maintaining the reduced pressure state after the microwave treatment. By performing such a treatment, hydrogen in the insulating film 250A, the oxide film 230D, the oxide film 230C, the oxide 230b, and the oxide 230a can be efficiently removed. Also, some of the hydrogen may be gettered to the conductor 242 (the conductor 242a and the conductor 242b). Alternatively, a step of performing a heat treatment may be repeated multiple times while maintaining the reduced pressure state after the microwave treatment. By repeatedly performing the heat treatment, hydrogen in the insulating film 250A, the oxide film 230C, the oxide 230b, and the oxide 230a can be more efficiently removed. Note that the heat treatment temperature is preferably 300° C. or more and 500° C. or less.

[0336] Furthermore, by performing microwave processing to modify the film quality of the insulating film 250A, it is possible to suppress the diffusion of hydrogen, water, impurities, etc. Therefore, it is possible to suppress the diffusion of hydrogen, water, impurities, etc. into the oxide 230b, the oxide 230a, etc. through the insulator 250 by a post-process such as film formation of a conductive film that becomes the conductor 260, or a post-treatment such as heat treatment.

[0337] Next, the conductive film 260A and the conductive film 260B are formed in this order (see FIGS. 16A to 16D). The conductive film 260A and the conductive film 260B can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, the conductive film 260A is formed by an ALD method, and the conductive film 260B is formed by a CVD method.

[0338] Next, the oxide film 230C, the oxide film 230D, the insulating film 250A, the conductive film 260A, and the conductive film 260B are polished by CMP until the insulator 280 is exposed, thereby forming the oxide 230c, the oxide 230d, the insulator 250, and the conductor 260 (the conductor 260a and the conductor 260b) (see FIGS. 17A to 17D). As a result, the oxide 230c is arranged so as to cover the opening that reaches the oxide 230b and the inner wall (side wall and bottom surface) of the groove of the oxide 230b. The oxide 230d is arranged so as to cover the opening and the inner wall of the groove through the oxide 230c. The insulator 250 is arranged so as to cover the opening and the inner wall of the groove through the oxide 230d. The conductor 260 is arranged so as to fill the opening and the groove through the oxide 230c, the oxide 230d, and the insulator 250.

[0339] Next, heat treatment may be performed under the same conditions as the above heat treatment. In this embodiment, the treatment is performed in a nitrogen atmosphere at a temperature of 400° C. for 1 hour. The heat treatment can reduce the moisture and hydrogen concentrations in the insulators 250 and 280. Note that after the heat treatment, the insulator 282 may be formed without exposure to the air.

[0340] Next, the insulator 282 is formed on the oxide 230c, the insulator 250, the conductor 260, and the insulator 280 (see FIGS. 18A to 18D). The insulator 282 can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. As the insulator 282, for example, it is preferable to form a film of aluminum oxide by a sputtering method. By forming the insulator 282 in an atmosphere containing oxygen by a sputtering method, oxygen can be added to the insulator 280 while forming the film. This allows the insulator 280 to contain excess oxygen. At this time, it is preferable to form the insulator 282 while heating the substrate. Moreover, it is preferable to form the insulator 282 in contact with the upper surface of the conductor 260, because this can suppress the oxygen contained in the insulator 280 from being absorbed by the conductor 260 in a subsequent heat treatment.

[0341] Next, a part of the insulator 282, a part of the insulator 280, a part of the insulator 224, a part of the insulator 222, a part of the insulator 216, a part of the insulator 214, and a part of the insulator 212 are processed to form an opening that reaches the insulator 211 (see FIGS. 19A to 19D). The opening may be formed so as to surround the transistor 200. Alternatively, the opening may be formed so as to surround a plurality of transistors 200. Thus, in the opening, a part of the side surface of the insulator 282, a part of the side surface of the insulator 280, a part of the side surface of the insulator 224, a part of the side surface of the insulator 222, a part of the side surface of the insulator 216, a part of the side surface of the insulator 214, and a part of the side surface of the insulator 212 are exposed.

[0342] A dry etching method or a wet etching method can be used for processing a part of the insulator 282, a part of the insulator 280, a part of the insulator 224, a part of the insulator 222, a part of the insulator 216, a part of the insulator 214, and a part of the insulator 212. Processing by the dry etching method is suitable for fine processing. In addition, the processing may be performed under different conditions.

[0343] Next, the insulator 287A is formed to cover the insulators 282, 280, 224, 222, 216, 214, and 212 (see FIGS. 20A to 20D). The insulator 287A is preferably formed under the same conditions as those for the insulator 282. For example, the insulator 287A can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.

[0344] Specifically, it is preferable to form the insulator 287A by, for example, a film of aluminum oxide by a sputtering method. By forming the insulator 287A in an oxygen-containing atmosphere using a sputtering method, oxygen can be added to the insulator 280 while the film is being formed. At this time, it is preferable to form the insulator 287A while heating the substrate. In addition, since the insulator 282 is formed in contact with the upper surface of the conductor 260, it is possible to suppress the oxygen contained in the insulator 280 from being absorbed by the conductor 260 during the film formation process of the insulator 287A.

[0345] Next, an anisotropic etching process is performed on insulator 287A to form insulator 287 on the sides of insulator 282, insulator 280, insulator 224, insulator 222, insulator 216, insulator 214 and insulator 212 (see Figures 21A to 21D).

[0346] Here, a side end of insulator 282 contacts the upper end of insulator 287, and a side end of insulator 214 contacts the lower end of insulator 287, thereby forming a structure that seals transistor 200 and insulator 280.

[0347] The anisotropic etching is preferably a dry etching process, which can remove the insulating film formed on a surface approximately parallel to the substrate surface and form the insulator 287 in a self-aligned manner.

[0348] Next, the insulator 283 is formed to cover the insulator 282, the insulator 287, and the insulator 211 (see FIGS. 22A to 22D). The insulator 283 can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. The insulator 283 may be a multi-layered structure. For example, a silicon nitride film may be formed by a sputtering method, and a silicon nitride film may be formed on the silicon nitride by a CVD method. As shown in FIG. 22, the insulator 283 contacts the insulator 211 at the bottom of the opening. That is, the upper and side surfaces of the transistor 200 are surrounded by the insulator 283, and the lower surface is surrounded by the insulator 211. In this manner, the transistor 200 is surrounded by the insulator 283 and the insulator 211, which have high barrier properties, to prevent moisture and hydrogen from entering from the outside.

[0349] Next, the insulator 284 may be formed on the insulator 283 (see FIGS. 23A to 23D). Note that the insulator 284 is preferably formed using a film formation method with high film-forming properties. For example, the insulator 284 can be formed using a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. Note that the insulator 284 is preferably formed using the same material as the insulators 212 and 283.

[0350] Specifically, a silicon nitride film may be formed by a CVD method. In particular, the insulator 284 may be formed by a CVD method using a compound gas that does not contain hydrogen atoms or that contains a small amount of hydrogen atoms.

[0351] Next, an insulating film that becomes the insulator 274 is formed on the insulator 284. The insulating film that becomes the insulator 274 can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. For example, a silicon oxide film can be formed by a CVD method. In addition, the insulating film that becomes the insulator 274 is preferably formed by a film formation method using a gas in which hydrogen atoms are reduced or removed as described above. This allows the hydrogen concentration in the insulating film that becomes the insulator 274 to be reduced.

[0352] Next, the insulating film that will become the insulator 274 is subjected to CMP processing to form the insulator 274 with a flat upper surface (see FIGS. 24A to 24D).

[0353] Next, heat treatment may be performed. In this embodiment, the treatment is performed in a nitrogen atmosphere at a temperature of 400° C. for one hour. As shown in FIG. 4, the heat treatment allows oxygen added by the formation of the insulator 282 to diffuse into the insulator 280 and the insulator 224, and can be selectively supplied to the oxide 230b and the channel formation region of the oxide 230c via the oxide 230c. Furthermore, the diffusion of oxygen into the source region or drain region of the oxide 230b can be reduced. Note that the heat treatment may be performed not only after the formation of the insulator 274, but also after the formation of the insulator 282 or the insulator 284.

[0354] Next, openings are formed in the insulators 271, 280, 282, 283, and 284, reaching the conductor 242 (see FIGS. 25A to 25D). The openings may be formed by using a lithography method. Note that, although the shape of the openings is circular in top view in FIG. 25A, the shape is not limited to this. For example, the openings may be substantially circular such as an ellipse, polygonal such as a rectangle, or polygonal such as a rectangle with rounded corners in top view.

[0355] Next, an insulating film that will become the insulator 241 is formed, and the insulating film is anisotropically etched to form the insulator 241 (insulator 241a and insulator 241b) (see Figures 25A to 25D). The insulating film that will become the insulator 241 can be formed using a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. As the insulating film that will become the insulator 241, it is preferable to use an insulating film that has a function of suppressing oxygen permeation. For example, it is preferable to form an aluminum oxide film using the ALD method. Alternatively, it is preferable to form a silicon nitride film using the PEALD method. Silicon nitride is preferable because it has high blocking properties against hydrogen.

[0356] Moreover, for example, a dry etching method may be used as the anisotropic etching of the insulating film that becomes the insulator 241. By providing the insulator 241 on the sidewall of the opening, it is possible to suppress the permeation of oxygen from the outside and prevent the oxidation of the conductor 240a and the conductor 240b to be formed next. It is also possible to prevent impurities such as water and hydrogen from diffusing to the outside from the conductor 240a and the conductor 240b.

[0357] Next, a conductive film that becomes the conductor 240a and the conductor 240b is formed. The conductive film that becomes the conductor 240a and the conductor 240b is preferably a laminated structure including a conductor that has a function of suppressing the permeation of impurities such as water and hydrogen. For example, it can be a laminated structure of tantalum nitride, titanium nitride, or the like, and tungsten, molybdenum, copper, or the like. The conductive film that becomes the conductor 240 can be formed by using a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.

[0358] Next, a CMP process is performed to remove parts of the conductive film that will become the conductors 240a and 240b, exposing the upper surfaces of the insulators 284 and 274. As a result, the conductive film remains only in the openings, forming the conductors 240a and 240b with flat upper surfaces (see FIGS. 25A to 25D). Note that the CMP process may remove parts of the upper surfaces of the insulators 284 and 274.

[0359] Next, a conductive film is formed to become the conductor 246. The conductive film to become the conductor 246 can be formed by sputtering, CVD, MBE, PLD, ALD, or the like.

[0360] Next, the conductive film that becomes the conductor 246 is processed by lithography to form the conductor 246a in contact with the top surface of the conductor 240a and the conductor 246b in contact with the top surface of the conductor 240b. At this time, a part of the insulator 284 in the region where the conductor 246a and the conductor 246b do not overlap with the insulator 284 may be removed (see FIGS. 26A to 26D).

[0361] Next, the insulator 286 is formed on the conductor 246 and the insulator 284 (see FIGS. 5A to 5D). The insulator 286 can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. The insulator 286 may also be a multi-layered structure. For example, a silicon nitride film may be formed by a sputtering method, and a silicon nitride film may be formed on the silicon nitride by a CVD method.

[0362] Through the above steps, a semiconductor device including the transistor 200 shown in Figures 5A to 5D can be manufactured. As shown in Figures 6A to 26A, 6B to 26B, 6C to 26C, and 6D to 26D, the transistor 200 can be manufactured by using the method for manufacturing a semiconductor device described in this embodiment. Note that when a semiconductor device including the transistor 200 shown in Figures 1A to 1D is manufactured, the semiconductor device may be manufactured without performing the steps shown in Figures 19 to 24.

[0363] <<Modification 2 of Semiconductor Device>> The semiconductor device shown in Figures 28A to 28D is a modified example of the semiconductor device shown in Figures 1A to 1D. The semiconductor device shown in Figures 28A to 28D differs from the semiconductor device shown in Figures 1A to 1D in that it does not have an insulator 271 (insulator 271a and insulator 271b).

[0364] When the insulator 271 is not provided, a curved surface may exist between the side surface of the conductor 242 and the top surface of the conductor 242. In other words, the end of the side surface and the end of the top surface may be curved. The curved surface has a radius of curvature of, for example, 3 nm or more and 10 nm or less, preferably 5 nm or more and 6 nm or less, at the end of the conductor 242. By not having corners at the end, the coverage of the film in the subsequent film formation process is improved.

[0365] Next, a manufacturing method of the semiconductor device of one embodiment of the present invention shown in FIGS. 28A to 28D will be described with reference to FIGS. 29A to 33A, FIGS. 29B to 33B, FIGS. 29C to 33C, and FIGS. 29D to 33D.

[0366] 29A to 33A are top views. FIG. 29B to 33B are cross-sectional views corresponding to a portion indicated by a dashed line A1-A2 in FIG. 29A to 33A, and are cross-sectional views in the channel length direction of the transistor 200. FIG. 29C to 33C are cross-sectional views corresponding to a portion indicated by a dashed line A3-A4 in FIG. 29A to 33A, and are cross-sectional views in the channel width direction of the transistor 200. FIG. 29D to 33D are cross-sectional views of a portion indicated by a dashed line A5-A6 in FIG. 29A to 33A. Note that some elements are omitted in the top views of FIG. 29A to 33A for clarity. Note that a description of the same parts as those in <Manufacturing method of semiconductor device> is omitted.

[0367] First, a substrate (not shown) is prepared, and then insulators 211, 212, and 214 are deposited in that order on the substrate, conductor 205 and insulator 216 are formed on insulator 214, insulator 222 is deposited on conductor 205 and insulator 216, insulator 224 is deposited on insulator 222, oxide film 230A and oxide film 230B are deposited in that order on insulator 224, oxide film 243A is deposited on oxide film 230B, and conductive film 242A is deposited on oxide film 243A (see Figures 29A to 29D).

[0368] Note that in the semiconductor device shown in Figures 28A to 28D, the process up to forming the conductive film 242A is similar to the process shown in <Method for manufacturing a semiconductor device>, and therefore detailed description of the process up to forming the conductive film 242A will be omitted.

[0369] Next, the oxide film 230A, the oxide film 230B, the oxide film 243A, and the conductive film 242A are processed into islands by using a lithography method to form the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B (see Figs. 30A to 30D). This processing can be performed by a dry etching method or a wet etching method. Processing by the dry etching method is suitable for fine processing. The oxide film 230A, the oxide film 230B, the oxide film 243A, and the conductive film 242A may be processed under different conditions. In this process, the thickness of the region of the insulator 224 that does not overlap with the oxide 230a may become thin.

[0370] A curved surface is provided between the side surface of the conductive layer 242B and the top surface of the conductive layer 242B. In other words, it is preferable that the end of the side surface and the end of the top surface are curved. For example, the curved surface has a radius of curvature of 3 nm or more and 10 nm or less, preferably 5 nm or more and 6 nm or less, at the end of the conductive layer 242B. By not having corners at the end, the coverage of the film in the subsequent film formation process is improved.

[0371] The oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B are formed so that at least a portion of them overlaps with the conductor 205. The side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B are preferably approximately perpendicular to the upper surface of the insulator 222. When the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B are approximately perpendicular to the upper surface of the insulator 222, a reduction in area and a high density can be achieved when providing a plurality of transistors 200. Alternatively, the angle between the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B and the upper surface of the insulator 222 may be low. In this case, the angle between the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B and the upper surface of the insulator 222 is preferably 60 degrees or more and less than 70 degrees. By using such a shape, the coverage of the insulating film 272A and the like can be improved in the subsequent steps, and defects such as voids can be reduced.

[0372] Here, during etching of the oxide 230a and the oxide 230b, a layer 247 may be formed covering the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B (see FIGS. 30A to 30D). The layer 247 is formed when a part of the conductive layer 242B is etched, floats up in the chamber, and is deposited again. Thus, the layer 247 is an oxide containing the main component of the conductive layer 242B. For example, when tantalum nitride is used for the conductive layer 242B, the layer 247 is an oxide containing tantalum.

[0373] Next, the layer 247 formed to cover the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B is removed (see FIGS. 31A to 31D). The layer 247 may be removed by dry etching or wet etching. The conductive layer 242B may be removed at the same time as the layer 247 is removed.

[0374] In this manner, by removing the layer 247 that covered the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B, the insulator 280 to be formed in a later step can be disposed in contact with the upper surface of the insulator 224. This allows oxygen to be diffused from the insulator 280 to the insulator 224 as shown in FIG. 3, so that oxygen can be efficiently supplied to the channel formation region of the oxide 230.

[0375] Although FIG. 31 shows the case where the layer 247 is completely removed, the layer 247 may remain in contact with the side surfaces of the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B.

[0376] Next, the insulating film 272A is formed over the oxide 230a, the oxide 230b, the oxide layer 243B, and the conductive layer 242B (see FIGS. 32A to 32D). The insulating film 272A can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, aluminum oxide is formed as the insulating film 272A by a sputtering method. For example, by forming the insulating film 272A by an RF sputtering method using an aluminum oxide target in an oxygen-free atmosphere, the insulating film 272A can be formed without adding excess oxygen to the oxide 230b.

[0377] Furthermore, by forming the insulating film 272A using the ALD method, it is possible to form a film that is dense, has fewer defects such as cracks and pinholes, and has a uniform thickness.

[0378] Next, the insulating film 272A is anisotropically etched to remove the insulating film 272A on the conductive layer 242B and the insulating film 272A on the insulator 224 (see FIGS. 33A to 33D). As a result, the insulating layer 272B is formed in contact with the side surfaces of the oxide 230a, the side surfaces of the oxide 230b, the side surfaces of the oxide layer 243B, and the side surfaces of the conductive layer 242B. Note that in this process, the film thickness of the exposed region of the insulator 224 may be thinner than the film thickness of the region of the insulator 224 that overlaps with the insulating layer 272B.

[0379] Note that in the semiconductor device shown in FIGS. 28A to 28D, the steps after the anisotropic etching are similar to the steps shown in <Method for manufacturing a semiconductor device>, and therefore detailed description of the steps after the anisotropic etching will be omitted.

[0380] <Applications of semiconductor devices> 34A and 34B, an example of a semiconductor device including a transistor 200 according to one embodiment of the present invention, which is different from those described in the above <Structural Example of Semiconductor Device> and the above <Modification of Semiconductor Device>, will be described below. Note that in the semiconductor device shown in FIG. 34A and FIG. 34B, structures having the same functions as those of the semiconductor device shown in <<Modification of Semiconductor Device 1>> (see FIG. 5A to FIG. 5D) are denoted by the same reference numerals. Note that in this section, the materials described in detail in the <Structural Example of Semiconductor Device> and <Modification of Semiconductor Device> can be used as the materials for forming the transistor 200.

[0381] 34A and 34B show a configuration in which a plurality of transistors 200_1 to 200_n are encapsulated by an insulator 283 and an insulator 211. Note that although the transistors 200_1 to 200_n appear to be aligned in the channel length direction in FIGS. 34A and 34B, this is not the only possible arrangement. The transistors 200_1 to 200_n may be aligned in the channel width direction or may be arranged in a matrix. Furthermore, the transistors 200_1 to 200_n may be arranged without any regularity depending on the design.

[0382] 34A, a portion where the insulator 283 and the insulator 211 contact each other (hereinafter, may be referred to as a sealing portion 265) is formed outside the plurality of transistors 200_1 to 200_n. The sealing portion 265 is formed so as to surround the plurality of transistors 200_1 to 200_n. With this structure, the plurality of transistors 200_1 to 200_n can be enclosed by the insulator 283 and the insulator 211. Thus, a plurality of transistor groups surrounded by the sealing portion 265 are provided on the substrate.

[0383] Also, dicing lines (which may be called scribe lines, division lines, or cutting lines) may be provided overlapping the sealing portion 265. Since the substrate is divided along the dicing lines, a group of transistors surrounded by the sealing portion 265 is taken out as one chip.

[0384] In addition, although Fig. 34A shows an example in which the plurality of transistors 200_1 to 200_n are surrounded by one sealing portion 265, the present invention is not limited to this. As shown in Fig. 34B, the plurality of transistors 200_1 to 200_n may be surrounded by a plurality of sealing portions. In Fig. 34B, the plurality of transistors 200_1 to 200_n are surrounded by a sealing portion 265a and further surrounded by an outer sealing portion 265b.

[0385] In this manner, by using a structure in which the multiple transistors 200_1 to 200_n are surrounded by multiple sealing portions, the number of areas in which the insulator 283 and the insulator 211 are in contact with each other increases, thereby improving the adhesion between the insulator 283 and the insulator 211. This makes it possible to more reliably seal the multiple transistors 200_1 to 200_n.

[0386] In this case, a dicing line may be provided so as to overlap sealing portion 265a or sealing portion 265b, or a dicing line may be provided between sealing portion 265a and sealing portion 265b.

[0387] According to one embodiment of the present invention, a semiconductor device with little variation in transistor characteristics can be provided. According to one embodiment of the present invention, a semiconductor device with high reliability can be provided. According to one embodiment of the present invention, a semiconductor device with good electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device with large on-state current can be provided. According to one embodiment of the present invention, a semiconductor device that can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a semiconductor device with low power consumption can be provided.

[0388] The structures, methods, and the like described in this embodiment mode can be used in appropriate combination with structures, methods, and the like described in other embodiment modes or examples.

[0389] (Embodiment 2) In this embodiment mode, one mode of a semiconductor device will be described with reference to FIGS.

[0390] [Storage device 1] 35 illustrates an example of a semiconductor device (memory device) according to one embodiment of the present invention. In the semiconductor device of one embodiment of the present invention, a transistor 200 is provided above a transistor 300, and a capacitor 100 is provided above the transistors 300 and 200. Note that the transistor 200 described in the above embodiment can be used as the transistor 200.

[0391] The transistor 200 is a transistor in which a channel is formed in a semiconductor layer including an oxide semiconductor. Since the off-state current of the transistor 200 is small, stored data can be retained for a long time by using the transistor 200 in a memory device. In other words, a refresh operation is not required or the frequency of the refresh operation is extremely low, so that the power consumption of the memory device can be sufficiently reduced.

[0392] 35, a wiring 1001 is electrically connected to a source of a transistor 300, and a wiring 1002 is electrically connected to a drain of the transistor 300. A wiring 1003 is electrically connected to one of a source and a drain of the transistor 200, a wiring 1004 is electrically connected to a first gate of the transistor 200, and a wiring 1006 is electrically connected to a second gate of the transistor 200. The gate of the transistor 300 and the other of the source and drain of the transistor 200 are electrically connected to one electrode of the capacitor 100, and a wiring 1005 is electrically connected to the other electrode of the capacitor 100.

[0393] Moreover, the memory device shown in FIG. 35 can be arranged in a matrix to form a memory cell array.

[0394] <Transistor 300> The transistor 300 is provided on a substrate 311 and includes a conductor 316 functioning as a gate, an insulator 315 functioning as a gate insulator, a semiconductor region 313 formed of a part of the substrate 311, and a low-resistance region 314a and a low-resistance region 314b functioning as a source region or a drain region. The transistor 300 may be either a p-channel type or an n-channel type.

[0395] Here, in the transistor 300 shown in FIG. 35, a semiconductor region 313 (a part of a substrate 311) in which a channel is formed has a convex shape. A conductor 316 is provided so as to cover the side and top surface of the semiconductor region 313 via an insulator 315. Note that the conductor 316 may be made of a material that adjusts the work function. Such a transistor 300 is also called a FIN type transistor because it uses a convex portion of a semiconductor substrate. Note that an insulator that contacts the upper part of the convex portion and functions as a mask for forming the convex portion may be provided. Note that, although a case where a convex portion is formed by processing a part of a semiconductor substrate has been shown here, a semiconductor film having a convex shape may be formed by processing an SOI substrate.

[0396] Note that the transistor 300 illustrated in FIG. 35 is just an example, and the present invention is not limited to this structure. An appropriate transistor may be used depending on the circuit configuration and driving method.

[0397] <Capacitive element 100> The capacitor 100 is provided above the transistor 200. The capacitor 100 includes a conductor 110 that functions as a first electrode, a conductor 120 that functions as a second electrode, and an insulator 130 that functions as a dielectric. Here, the insulator 130 is preferably an insulator that can be used as the insulator 286 described in the above embodiment.

[0398] For example, the conductor 112 over the conductor 240 and the conductor 110 can be formed at the same time. Note that the conductor 112 functions as a plug or a wiring electrically connected to the capacitor 100, the transistor 200, or the transistor 300.

[0399] 35, the conductor 112 and the conductor 110 are shown to have a single-layer structure, but are not limited to this configuration and may have a laminated structure of two or more layers. For example, a conductor having barrier properties and a conductor having high adhesion to the conductor having high conductivity may be formed between a conductor having barrier properties and a conductor having high conductivity.

[0400] The insulator 130 can be made of, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, aluminum oxynitride, aluminum nitride oxide, aluminum nitride, hafnium oxide, hafnium oxynitride, hafnium nitride oxide, hafnium nitride, or the like, and can be provided as a stacked layer or a single layer.

[0401] For example, it is preferable to use a laminated structure of a material with high dielectric strength, such as silicon oxynitride, and a high dielectric constant (high-k) material for the insulator 130. With this configuration, the capacitance element 100 can ensure sufficient capacitance by having an insulator with high dielectric constant (high-k), and the capacitance element 100 can have improved dielectric strength by having an insulator with high dielectric strength, thereby suppressing electrostatic breakdown of the capacitance element 100.

[0402] Examples of high dielectric constant (high-k) material insulators (materials with a high relative dielectric constant) include gallium oxide, hafnium oxide, zirconium oxide, oxides having aluminum and hafnium, oxynitrides having aluminum and hafnium, oxides having silicon and hafnium, oxynitrides having silicon and hafnium, and nitrides having silicon and hafnium.

[0403] On the other hand, materials with high dielectric strength (materials with low dielectric constant) include silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, silicon oxide or resin with voids, etc.

[0404] <Wiring layer> Between each structure, a wiring layer having an interlayer film, wiring, plugs, etc. may be provided. Also, a plurality of wiring layers may be provided according to the design. Here, a conductor having a function as a plug or wiring may be collectively given the same symbol as a plurality of structures. Also, in this specification, the wiring and the plug electrically connected to the wiring may be integrated. That is, there are cases where a part of the conductor functions as the wiring, and cases where a part of the conductor functions as the plug.

[0405] For example, an insulator 320, an insulator 322, an insulator 324, and an insulator 326 are stacked in this order as an interlayer film over the transistor 300. A conductor 328, a conductor 330, and the like that are electrically connected to the capacitor 100 or the transistor 200 are embedded in the insulator 320, the insulator 322, the insulator 324, and the insulator 326. The conductor 328 and the conductor 330 function as plugs or wirings.

[0406] The insulator functioning as an interlayer film may also function as a planarizing film that covers the uneven shape underneath. For example, the top surface of the insulator 322 may be planarized by a planarization process using a chemical mechanical polishing (CMP) method or the like to enhance flatness.

[0407] A wiring layer may be provided on the insulator 326 and the conductor 330. For example, in Fig. 35, an insulator 350, an insulator 352, and an insulator 354 are stacked in this order. Furthermore, a conductor 356 is formed in the insulator 350, the insulator 352, and the insulator 354. The conductor 356 functions as a plug or a wiring.

[0408] Similarly, a conductor 218, a conductor constituting the transistor 200 (conductor 205), and the like are embedded in the insulators 210, 211, 212, 214, and 216. Note that the conductor 218 functions as a plug or wiring electrically connected to the capacitor 100 or the transistor 300. Furthermore, an insulator 150 is provided over the conductor 120 and the insulator 130.

[0409] Here, similarly to the insulator 241 shown in the above embodiment, the insulator 217 is provided in contact with the side surface of the conductor 218 functioning as a plug. The insulator 217 is provided in contact with the inner wall of the opening formed in the insulators 210, 211, 212, 214, and 216. That is, the insulator 217 is provided between the conductor 218 and the insulators 210, 211, 212, 214, and 216. Note that the conductor 205 can be formed in parallel with the conductor 218, and therefore the insulator 217 may be formed in contact with the side surface of the conductor 205.

[0410] As the insulator 217, for example, an insulator such as silicon nitride, aluminum oxide, or silicon nitride oxide may be used. Since the insulator 217 is provided in contact with the insulators 211, 212, 214, and 222, it is possible to prevent impurities such as water or hydrogen from the insulator 210 or the insulator 216 from being mixed into the oxide 230 through the conductor 218. In particular, silicon nitride is preferable because it has a high blocking property against hydrogen. In addition, it is possible to prevent oxygen contained in the insulator 210 or the insulator 216 from being absorbed by the conductor 218.

[0411] The insulator 217 can be formed by a method similar to that of the insulator 241. For example, a silicon nitride film is formed by a PEALD method, and an opening reaching the conductor 356 is formed by anisotropic etching.

[0412] Examples of insulators that can be used as the interlayer film include insulating oxides, nitrides, oxynitrides, nitride oxides, metal oxides, metal oxynitrides, and metal nitride oxides.

[0413] For example, by using a material with a low dielectric constant for the insulator that functions as an interlayer film, the parasitic capacitance generated between wirings can be reduced. Therefore, it is advisable to select a material according to the function of the insulator.

[0414] For example, the insulator 150, the insulator 210, the insulator 352, the insulator 354, etc. preferably have an insulator with a low relative dielectric constant. For example, the insulator preferably has silicon oxynitride, silicon nitride, silicon oxide to which fluorine has been added, silicon oxide to which carbon has been added, silicon oxide to which carbon and nitrogen have been added, silicon oxide having voids, or resin. Alternatively, the insulator preferably has a laminated structure of silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide to which fluorine has been added, silicon oxide to which carbon has been added, silicon oxide to which carbon and nitrogen has been added, or silicon oxide having voids, and resin. Silicon oxide and silicon oxynitride are thermally stable, and therefore can be combined with a resin to form a laminated structure that is thermally stable and has a low relative dielectric constant. Examples of the resin include polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, and acrylic.

[0415] Furthermore, when a transistor using an oxide semiconductor is surrounded by an insulator that has a function of suppressing the permeation of impurities such as hydrogen and oxygen, the electrical characteristics of the transistor can be stabilized. Therefore, the insulators 214, 211, 212, and 350 can be made of insulators that have a function of suppressing the permeation of impurities such as hydrogen and oxygen.

[0416] As an insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen, for example, an insulator containing boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, or tantalum may be used in a single layer or a stacked layer. Specifically, as an insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, or tantalum oxide, silicon nitride oxide, or silicon nitride may be used.

[0417] Conductors that can be used for wiring and plugs include materials containing one or more metal elements selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, etc. Also, semiconductors with high electrical conductivity, typified by polycrystalline silicon containing impurity elements such as phosphorus, and silicides such as nickel silicide may be used.

[0418] For example, the conductor 328, the conductor 330, the conductor 356, the conductor 218, the conductor 112, etc. can be formed of a single layer or a stack of conductive materials such as metal materials, alloy materials, metal nitride materials, or metal oxide materials formed from the above materials. It is preferable to use a high melting point material such as tungsten or molybdenum that has both heat resistance and conductivity, and it is preferable to use tungsten. Alternatively, it is preferable to form the conductor from a low resistance conductive material such as aluminum or copper. By using a low resistance conductive material, the wiring resistance can be reduced.

[0419] <Wiring or plug of layer provided with oxide semiconductor> Note that when an oxide semiconductor is used for the transistor 200, an insulator having an excess oxygen region may be provided near the oxide semiconductor. In that case, an insulator having a barrier property is preferably provided between the insulator having the excess oxygen region and a conductor provided in the insulator having the excess oxygen region.

[0420] 35, for example, an insulator 241 may be provided between the insulator 224 and the insulator 280 having excess oxygen and the conductor 240. By providing the insulator 241 in contact with the insulator 222, the insulator 282, the insulator 283, and the insulator 284, the insulator 224 and the transistor 200 can be sealed with an insulator having barrier properties.

[0421] In other words, the insulator 241 can prevent excess oxygen contained in the insulator 224 and the insulator 280 from being absorbed by the conductor 240. Furthermore, the insulator 241 can prevent hydrogen, which is an impurity, from diffusing into the transistor 200 through the conductor 240.

[0422] As the insulator 241, an insulating material having a function of suppressing the diffusion of impurities such as water or hydrogen, and oxygen, may be used. For example, it is preferable to use silicon nitride, silicon nitride oxide, aluminum oxide, or hafnium oxide. In particular, silicon nitride is preferable because it has a high blocking property against hydrogen. In addition, other metal oxides such as magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, or tantalum oxide may be used.

[0423] As in the above embodiment, the transistor 200 is preferably sealed with the insulators 211, 212, 214, 287, 282, 283, and 284. Such a structure can reduce the intrusion of hydrogen contained in the insulators 274, 150, and the like into the insulator 280 and the like.

[0424] Here, the conductor 240 penetrates the insulators 284, 283, and 282, and the conductor 218 penetrates the insulators 214, 212, and 211, but as described above, the insulator 241 is provided in contact with the conductor 240, and the insulator 217 is provided in contact with the conductor 218. This makes it possible to reduce hydrogen that is mixed into the inside of the insulators 211, 212, 214, 287, 282, 283, and 284 through the conductors 240 and 218. In this way, the transistor 200 can be more reliably sealed with the insulators 211, 212, 214, 287, 282, 283, 284, 241, and 217, and it is possible to reduce impurities such as hydrogen contained in the insulators 274 and the like from the outside.

[0425] Furthermore, as described in the above embodiment, the insulators 216, 224, 280, 250, and 274 are preferably formed by a film formation method using a gas in which hydrogen atoms are reduced or removed, thereby reducing the hydrogen concentrations in the insulators 216, 224, 280, 250, and 274.

[0426] In this manner, the hydrogen concentration in the silicon-based insulating film in the vicinity of the transistor 200 can be reduced, and the hydrogen concentration in the oxide 230 can be reduced.

[0427] <Dicing line> In the following, a dicing line (sometimes called a scribe line, a dividing line, or a cutting line) that is provided when a large-area substrate is divided into individual semiconductor elements to extract multiple semiconductor devices in chip form will be described. As a dividing method, for example, first, grooves (dicing lines) for dividing the semiconductor elements are formed in the substrate, and then the substrate is cut along the dicing lines to divide (split) the substrate into multiple semiconductor devices.

[0428] 35, for example, it is preferable to design the region where the insulator 283 and the insulator 211 contact each other so as to overlap the dicing line. That is, openings are provided in the insulators 282, 280, 224, 222, 216, 214, and 212 near the region that will become the dicing line provided on the outer edge of the memory cell having the multiple transistors 200.

[0429] That is, the insulator 211 and the insulator 283 are in contact with each other through the openings provided in the insulators 282, 280, 224, 222, 216, 214, and 212. Also, openings may be provided in the insulators 282, 280, 224, 222, 216, and 214, and the insulators 212 and 283 may be in contact with each other. For example, the insulators 212 and 283 may be formed using the same material and the same method. By providing the insulators 212 and 283 using the same material and the same method, the adhesion can be improved. For example, it is preferable to use silicon nitride.

[0430] With this structure, the transistor 200 can be surrounded by the insulator 211, the insulator 212, the insulator 214, the insulator 287, the insulator 282, the insulator 283, and the insulator 284. At least one of the insulators 211, 212, 214, the insulator 287, the insulator 282, the insulator 283, and the insulator 284 has a function of suppressing diffusion of oxygen, hydrogen, and water. Therefore, even if the substrate is divided into a plurality of chips by dividing the substrate into each circuit region in which the semiconductor element shown in this embodiment is formed, impurities such as hydrogen or water can be prevented from entering from the side direction of the divided substrate and diffusing into the transistor 200.

[0431] This structure can prevent excess oxygen in the insulator 280 and the insulator 224 from diffusing to the outside. Therefore, the excess oxygen in the insulator 280 and the insulator 224 is efficiently supplied to the oxide in which a channel is formed in the transistor 200. The oxygen can reduce oxygen vacancies in the oxide in which a channel is formed in the transistor 200. As a result, the oxide in which a channel is formed in the transistor 200 can be an oxide semiconductor with low density of defect states and stable characteristics. That is, fluctuations in the electrical characteristics of the transistor 200 can be suppressed and reliability can be improved.

[0432] In the memory device shown in Fig. 35, the shape of the capacitor 100 is a planar type, but the memory device shown in this embodiment is not limited to this. For example, the shape of the capacitor 100 may be a cylindrical type as shown in Fig. 36. In the memory device shown in Fig. 36, the configuration below the insulator 150 is similar to that of the semiconductor device shown in Fig. 35.

[0433] 36 includes an insulator 150 on an insulator 130, an insulator 142 on the insulator 150, a conductor 115 disposed in an opening formed in the insulator 150 and the insulator 142, an insulator 145 on the conductor 115 and the insulator 142, a conductor 125 on the insulator 145, and an insulator 152 on the conductor 125 and the insulator 145. Here, at least a portion of the conductor 115, the insulator 145, and the conductor 125 are disposed in the opening formed in the insulator 150 and the insulator 142.

[0434] The conductor 115 functions as the lower electrode of the capacitance element 100, the conductor 125 functions as the upper electrode of the capacitance element 100, and the insulator 145 functions as the dielectric of the capacitance element 100. The capacitance element 100 has a configuration in which the upper electrode and the lower electrode face each other across the dielectric not only on the bottom surface but also on the side surface in the openings of the insulators 150 and 142, and the capacitance per unit area can be increased. Therefore, the deeper the opening is, the larger the capacitance of the capacitance element 100 can be. Increasing the capacitance per unit area of ​​the capacitance element 100 in this way can promote miniaturization or high integration of semiconductor devices.

[0435] The insulator 152 may be made of an insulator that can be used for the insulator 280. The insulator 142 preferably functions as an etching stopper when forming an opening in the insulator 150, and may be made of an insulator that can be used for the insulator 214.

[0436] The shape of the openings formed in the insulator 150 and the insulator 142 when viewed from above may be a rectangle, a polygon other than a rectangle, a polygon with curved corners, or a circle including an ellipse. Here, it is preferable that the area of ​​the opening overlapping with the transistor 200 is large when viewed from above. With such a configuration, the occupation area of ​​a semiconductor device including the capacitor 100 and the transistor 200 can be reduced.

[0437] The conductor 115 is disposed in contact with the insulator 142 and an opening formed in the insulator 150. The upper surface of the conductor 115 preferably approximately coincides with the upper surface of the insulator 142. The lower surface of the conductor 115 is in contact with the conductor 110 through the opening of the insulator 130. The conductor 115 is preferably formed by an ALD method, a CVD method, or the like, and may be, for example, a conductor that can be used for the conductor 205.

[0438] The insulator 145 is disposed so as to cover the conductor 115 and the insulator 142. For example, the insulator 145 is preferably formed by an ALD method, a CVD method, or the like. The insulator 145 may be formed using, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, zirconium oxide, aluminum oxide, aluminum oxynitride, aluminum nitride oxide, aluminum nitride, hafnium oxide, hafnium oxynitride, hafnium nitride oxide, hafnium nitride, or the like, and can be provided as a stacked layer or a single layer. For example, the insulator 145 can be an insulating film stacked in this order of zirconium oxide, aluminum oxide, and zirconium oxide.

[0439] Moreover, it is preferable to use a material with high dielectric strength, such as silicon oxynitride, or a high dielectric constant (high-k) material for the insulator 145. Alternatively, a laminated structure of a material with high dielectric strength and a material with high dielectric constant (high-k) may be used.

[0440] Examples of insulators made of high dielectric constant (high-k) materials (materials with high relative dielectric constant) include gallium oxide, hafnium oxide, zirconium oxide, oxides having aluminum and hafnium, oxynitrides having aluminum and hafnium, oxides having silicon and hafnium, oxynitrides having silicon and hafnium, and nitrides having silicon and hafnium. By using such high-k materials, the capacitance of the capacitance element 100 can be sufficiently secured even if the insulator 145 is made thick. By making the insulator 145 thick, the leakage current occurring between the conductor 115 and the conductor 125 can be suppressed.

[0441] On the other hand, materials with high dielectric strength include silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, silicon oxide with vacancies, and resin. For example, silicon nitride (SiN x ), silicon oxide (SiO x), and silicon nitride (SiN x ) in that order can be used. By using such an insulator having a high dielectric strength, the dielectric strength is improved, and electrostatic breakdown of the capacitor 100 can be suppressed.

[0442] The conductor 125 is disposed so as to fill the openings formed in the insulator 142 and the insulator 150. The conductor 125 is electrically connected to the wiring 1005 via the conductor 140 and the conductor 153. The conductor 125 is preferably formed by an ALD method, a CVD method, or the like, and may be formed using a conductor that can be used for the conductor 205, for example.

[0443] The conductor 153 is provided over the insulator 154 and is covered with the insulator 156. The conductor 153 may be any conductor that can be used for the conductor 112, and the insulator 156 may be any insulator that can be used for the insulator 152. Here, the conductor 153 is in contact with the top surface of the conductor 140 and functions as a terminal of the capacitor 100, the transistor 200, or the transistor 300.

[0444] [Storage device 2] An example of a semiconductor device (memory device) according to one embodiment of the present invention is illustrated in FIG.

[0445] <Memory device configuration example> Fig. 37 is a cross-sectional view of a semiconductor device including a memory device 290. The memory device 290 shown in Fig. 37 includes a capacitor device 292 in addition to the transistor 200 shown in Fig. 1A to Fig. 1D. Fig. 37 corresponds to a cross-sectional view of the transistor 200 in the channel length direction.

[0446] The capacitance device 292 includes a conductor 242b, an insulator 271b provided on the conductor 242b, an insulator 272b provided in contact with a side surface of the conductor 242b, and a conductor 294 provided to cover the insulator 271b and the insulator 272b. That is, the capacitance device 292 configures an MIM (Metal-Insulator-Metal) capacitance. Note that one of a pair of electrodes included in the capacitance device 292, that is, the conductor 242b, can also serve as a source electrode of a transistor. In addition, a dielectric layer included in the capacitance device 292 can also serve as a protective layer provided in the transistor, that is, the insulator 271 and the insulator 272. Therefore, a part of the manufacturing process of the transistor can be used in the manufacturing process of the capacitance device 292, so that a semiconductor device with high productivity can be obtained. In addition, one of a pair of electrodes of the capacitor 292, that is, the conductor 242b, also serves as a source electrode of the transistor, so that the area in which the transistor and the capacitor are arranged can be reduced.

[0447] Note that the conductor 294 may be made of, for example, a material that can be used for the conductor 242.

[0448] <Modifications of memory device> An example of a semiconductor device having a transistor 200 according to one embodiment of the present invention and a capacitor device 292, which is different from those shown in the above <Configuration Example of Memory Device>, will be described below with reference to Figs. 38A, 38B, 39, and 40. Note that in the semiconductor device shown in Figs. 38A, 38B, 39, and 40, structures having the same functions as those of the semiconductor device shown in the above embodiment and <Configuration Example of Memory Device> (see Fig. 37) are denoted by the same reference numerals. Note that in this section, the materials for the transistor 200 and the capacitor device 292 can be the materials described in detail in the above embodiment and <Configuration Example of Memory Device>.

[0449] <<Memory Device Variation 1>> Below, an example of a semiconductor device 600 including a transistor 200a, a transistor 200b, a capacitor device 292a, and a capacitor device 292b according to one embodiment of the present invention will be described with reference to FIG. 38A.

[0450] 38A is a cross-sectional view in the channel length direction of a semiconductor device 600 including a transistor 200a, a transistor 200b, a capacitance device 292a, and a capacitance device 292b. Here, the capacitance device 292a includes a conductor 242a, an insulator 271a provided on the conductor 242a, an insulator 272a provided in contact with a side surface of the conductor 242a, and a conductor 294a provided to cover the insulator 271a and the insulator 272a. The capacitance device 292b includes a conductor 242b, an insulator 271b provided on the conductor 242b, an insulator 272b provided in contact with a side surface of the conductor 242b, and a conductor 294b provided to cover the insulator 271b and the insulator 272b.

[0451] As shown in FIG. 38A, the semiconductor device 600 has a linear symmetrical configuration with the dashed line A3-A4 as the axis of symmetry. The conductor 242c serves as one of the source electrode or drain electrode of the transistor 200a and one of the source electrode or drain electrode of the transistor 200b. An insulator 271c is provided on the conductor 242c. The conductor 246 functions as wiring, and the conductor 240 functions as a plug to connect the transistor 200a and the transistor 200b. In this way, by configuring the two transistors, the two capacitance devices, and the wiring and the plugs as described above, a semiconductor device that can be miniaturized or highly integrated can be provided.

[0452] The configuration examples of the semiconductor device illustrated in FIGS. 1A to 1D and 37 can be referred to for the configurations and effects of the transistor 200a, the transistor 200b, the capacitance device 292a, and the capacitance device 292b.

[0453] <<Memory Device Modification 2>> In the above, the transistor 200a, the transistor 200b, the capacitance device 292a, and the capacitance device 292b are given as examples of the configuration of the semiconductor device, but the semiconductor device shown in this embodiment is not limited to this. For example, as shown in FIG. 38B, a configuration may be adopted in which a semiconductor device 600 and a semiconductor device having a similar configuration to the semiconductor device 600 are connected via a capacitance portion. In this specification, a semiconductor device having the transistor 200a, the transistor 200b, the capacitance device 292a, and the capacitance device 292b is referred to as a cell. For the configurations of the transistor 200a, the transistor 200b, the capacitance device 292a, and the capacitance device 292b, the above description of the transistor 200a, the transistor 200b, the capacitance device 292a, and the capacitance device 292b can be referred to.

[0454] FIG. 38B is a cross-sectional view of a semiconductor device 600 having a transistor 200a, a transistor 200b, a capacitance device 292a, and a capacitance device 292b, and a cell having a similar configuration to the semiconductor device 600, connected via a capacitance portion.

[0455] As shown in FIG. 38B, the conductor 294b functioning as one electrode of the capacitance device 292b of the semiconductor device 600 is configured to also serve as one electrode of the capacitance device of the semiconductor device 601 having the same configuration as the semiconductor device 600. Although not shown, the conductor 294a functioning as one electrode of the capacitance device 292a of the semiconductor device 600 also serves as one electrode of the capacitance device of the semiconductor device adjacent to the left side of the semiconductor device 600, that is, in FIG. 38B, in the A1 direction. The same configuration is also applied to the right side of the semiconductor device 601, that is, in FIG. 38B, in the A2 direction. That is, a cell array (also called a memory device layer) can be configured. By configuring the cell array in this way, the interval between adjacent cells can be reduced, so that the projection area of ​​the cell array can be reduced, and high integration is possible. Also, by arranging the cell array configuration shown in FIG. 38B in a matrix, a matrix-shaped cell array can be configured.

[0456] As described above, by forming transistor 200a, transistor 200b, capacitance device 292a, and capacitance device 292b in the configuration shown in this embodiment, the cell area can be reduced, and miniaturization or high integration of a semiconductor device having a cell array can be achieved.

[0457] Moreover, the cell array may be configured not only in a plane but also in a stacked configuration. Fig. 39 shows a cross-sectional view of a configuration in which the cell array 610 is stacked in n layers. As shown in Fig. 39, by stacking a plurality of cell arrays (cell arrays 610_1 to 610_n), the cells can be integrated and arranged without increasing the area occupied by the cell arrays. In other words, a 3D cell array can be configured.

[0458] <Memory Device Modification 3> FIG. 40 shows an example in which a memory unit 470 includes a transistor layer 413 including a transistor 200T and four memory device layers 415 (memory device layers 415_1 to 415_4).

[0459] Each of the memory device layers 415_1 to 415_4 includes a plurality of memory devices 420.

[0460] The memory device 420 is electrically connected to a memory device 420 in a different memory device layer 415 and a transistor 200T in a transistor layer 413 via a conductor 424 and a conductor 205.

[0461] The memory unit 470 is sealed by the insulator 211, the insulator 212, the insulator 214, the insulator 287, the insulator 282, the insulator 283, and the insulator 284 (for convenience, hereinafter, referred to as a sealing structure). The insulator 274 is provided around the insulator 284. Furthermore, the conductor 440 is provided on the insulator 274, the insulator 284, the insulator 283, and the insulator 211, and is electrically connected to the element layer 411.

[0462] Further, an insulator 280 is provided inside the sealing structure. The insulator 280 has a function of releasing oxygen when heated. Alternatively, the insulator 280 has an excess oxygen region.

[0463] Note that the insulators 211, 283, and 284 are preferably made of a material having a high blocking property against hydrogen. The insulators 214, 282, and 287 are preferably made of a material having a function of capturing hydrogen or fixing hydrogen.

[0464] For example, the material having a high blocking property against hydrogen includes silicon nitride, silicon oxynitride, etc. Furthermore, the material having a function of capturing or fixing hydrogen includes aluminum oxide, hafnium oxide, and oxide containing aluminum and hafnium (hafnium aluminate), etc.

[0465] Note that the crystal structure of the materials used for the insulators 211, 212, 214, 287, 282, 283, and 284 is not particularly limited, and may be an amorphous or crystalline structure. For example, an amorphous aluminum oxide film is preferably used as a material having a function of capturing or fixing hydrogen. Amorphous aluminum oxide may be capable of capturing and fixing a larger amount of hydrogen than aluminum oxide with high crystallinity.

[0466] In addition, the insulator 282 and the insulator 214 are preferably provided between the transistor layer 413 and the memory device layer 415 or between each memory device layer 415. In addition, the insulator 296 is preferably provided between the insulator 282 and the insulator 214. The insulator 296 can be made of a material similar to that of the insulator 283 and the insulator 284. Alternatively, silicon oxide or silicon oxynitride can be used. Alternatively, a known insulating material can be used.

[0467] Here, the following model can be considered for the diffusion of excess oxygen in the insulator 280 and hydrogen in the oxide semiconductor in contact with the insulator 280.

[0468] Hydrogen present in the oxide semiconductor diffuses to other structures through the insulator 280 in contact with the oxide semiconductor. In the diffusion of hydrogen, excess oxygen in the insulator 280 reacts with hydrogen in the oxide semiconductor to form an OH bond, and the hydrogen diffuses through the insulator 280. When the hydrogen atom having the OH bond reaches a material (typically the insulator 282) having a function of capturing or fixing hydrogen, the hydrogen atom reacts with an oxygen atom bonded to an atom (e.g., a metal atom, etc.) in the insulator 282, and is captured or fixed in the insulator 282. On the other hand, it is presumed that the oxygen atom of the excess oxygen having the OH bond remains in the insulator 280 as excess oxygen. In other words, there is a high probability that the excess oxygen in the insulator 280 plays a bridging role in the diffusion of hydrogen.

[0469] In order to satisfy the above model, the manufacturing process of the semiconductor device is one of the important factors.

[0470] As an example, the insulator 280 containing excess oxygen is formed in an oxide semiconductor, and then the insulator 282 is formed. After that, heat treatment is preferably performed. Specifically, the heat treatment is performed in an atmosphere containing oxygen, an atmosphere containing nitrogen, or an atmosphere containing a mixture of oxygen and nitrogen at a temperature of 350° C. or higher, preferably 400° C. or higher. The heat treatment time is 1 hour or longer, preferably 4 hours or longer, and more preferably 8 hours or longer.

[0471] By the above heat treatment, hydrogen in the oxide semiconductor can diffuse outward through the insulators 280, 282, and 287. That is, the absolute amount of hydrogen present in and near the oxide semiconductor can be reduced.

[0472] After the heat treatment, the insulators 283 and 284 are formed. The insulators 283 and 284 are made of materials having a high blocking property against hydrogen, and therefore can prevent hydrogen that has diffused to the outside or hydrogen present on the outside from entering the inside, specifically, the oxide semiconductor or the insulator 280.

[0473] Note that the above heat treatment is performed after the insulator 282 is formed, but is not limited thereto. For example, the heat treatment may be performed after the transistor layer 413 is formed or after the memory device layers 415_1 to 415_3 are formed. When hydrogen is diffused outward by the heat treatment, hydrogen is diffused upward or laterally of the transistor layer 413. Similarly, when the heat treatment is performed after the memory device layers 415_1 to 415_3 are formed, hydrogen is diffused upward or laterally.

[0474] By using the above manufacturing process, the insulator 211 and the insulator 283 are bonded to each other, thereby forming the above-described sealing structure.

[0475] As described above, by using the above structure and manufacturing process, a semiconductor device including an oxide semiconductor in which the hydrogen concentration is reduced can be provided. Therefore, a semiconductor device with high reliability can be provided. According to one embodiment of the present invention, a semiconductor device with good electrical characteristics can be provided.

[0476] The structures, methods, and the like described in this embodiment mode can be used in appropriate combination with structures, methods, and the like described in other embodiment modes or examples.

[0477] (Embodiment 3) In this embodiment, a transistor including an oxide as a semiconductor (hereinafter may be referred to as an OS transistor) and a memory device including a capacitor (hereinafter may be referred to as an OS memory device) according to one embodiment of the present invention will be described with reference to FIGS. 41A, 41B, and 42A to 42H. The OS memory device is a memory device including at least a capacitor and an OS transistor that controls charging and discharging of the capacitor. Since the off-state current of the OS transistor is extremely small, the OS memory device has excellent retention characteristics and can function as a nonvolatile memory.

[0478] <Storage device configuration example> 41A shows an example of the configuration of an OS memory device. The memory device 1400 includes a peripheral circuit 1411 and a memory cell array 1470. The peripheral circuit 1411 includes a row circuit 1420, a column circuit 1430, an output circuit 1440, and a control logic circuit 1460.

[0479] The column circuit 1430 includes, for example, a column decoder, a precharge circuit, a sense amplifier, a write circuit, and the like. The precharge circuit has a function of precharging the wiring. The sense amplifier has a function of amplifying a data signal read from a memory cell. Note that the above wiring is a wiring connected to a memory cell included in the memory cell array 1470, and will be described in detail later. The amplified data signal is output to the outside of the memory device 1400 as a data signal RDATA via the output circuit 1440. The row circuit 1420 includes, for example, a row decoder, a word line driver circuit, and the like, and can select a row to be accessed.

[0480] A low power supply voltage (VSS), a high power supply voltage (VDD) for the peripheral circuit 1411, and a high power supply voltage (VIL) for the memory cell array 1470 are supplied to the memory device 1400 from the outside as power supply voltages. In addition, control signals (CE, WE, RE), an address signal ADDR, and a data signal WDATA are input from the outside to the memory device 1400. The address signal ADDR is input to a row decoder and a column decoder, and the data signal WDATA is input to a write circuit.

[0481] The control logic circuit 1460 processes control signals (CE, WE, RE) input from the outside to generate control signals for the row decoder and column decoder. The control signal CE is a chip enable signal, the control signal WE is a write enable signal, and the control signal RE is a read enable signal. The signals processed by the control logic circuit 1460 are not limited to these, and other control signals may be input as necessary.

[0482] The memory cell array 1470 has a plurality of memory cells MC arranged in a matrix and a plurality of wirings. The number of wirings connecting the memory cell array 1470 and the row circuit 1420 is determined by the configuration of the memory cells MC, the number of memory cells MC in one column, etc. The number of wirings connecting the memory cell array 1470 and the column circuit 1430 is determined by the configuration of the memory cells MC, the number of memory cells MC in one row, etc.

[0483] 41A shows an example in which the peripheral circuit 1411 and the memory cell array 1470 are formed on the same plane, but the present embodiment is not limited to this. For example, as shown in FIG. 41B, the memory cell array 1470 may be provided so as to overlap a part of the peripheral circuit 1411. For example, a sense amplifier may be provided so as to overlap the memory cell array 1470 below.

[0484] 42A to 42H will be used to explain examples of the configuration of a memory cell that can be applied to the above-mentioned memory cell MC.

[0485] [DOSRAM] 42A to 42C show circuit configuration examples of a DRAM memory cell. In this specification and the like, a DRAM using a memory cell with one OS transistor and one capacitor may be called a DOSRAM (Dynamic Oxide Semiconductor Random Access Memory). The memory cell 1471 shown in FIG. 42A includes a transistor M1 and a capacitor CA. Note that the transistor M1 includes a gate (sometimes called a top gate) and a back gate.

[0486] A first terminal of the transistor M1 is connected to a first terminal of the capacitance element CA, a second terminal of the transistor M1 is connected to a wiring BIL, a gate of the transistor M1 is connected to a wiring WOL, a back gate of the transistor M1 is connected to a wiring BGL, and a second terminal of the capacitance element CA is connected to a wiring CAL.

[0487] The wiring BIL functions as a bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitor CA. When writing and reading data, it is preferable to apply a low-level potential to the wiring CAL. The wiring BGL functions as a wiring for applying a potential to the back gate of the transistor M1. The threshold voltage of the transistor M1 can be increased or decreased by applying an arbitrary potential to the wiring BGL.

[0488] Here, the memory cell 1471 shown in Fig. 42A corresponds to the memory device shown in Fig. 37. That is, the transistor M1 corresponds to the transistor 200, and the capacitance element CA corresponds to the capacitance device 292.

[0489] The memory cell MC is not limited to the memory cell 1471, and the circuit configuration can be changed. For example, the memory cell MC may be configured such that the back gate of the transistor M1 is connected to the wiring WOL instead of the wiring BGL, as in the memory cell 1472 shown in FIG. 42B. For example, the memory cell MC may be configured as a single-gate transistor, that is, a memory cell configured with a transistor M1 without a back gate, as in the memory cell 1473 shown in FIG. 42C.

[0490] When the semiconductor device described in the above embodiment is used for the memory cell 1471 or the like, the transistor 200 can be used as the transistor M1, and the capacitor 100 can be used as the capacitor CA. By using an OS transistor as the transistor M1, the leakage current of the transistor M1 can be made very small. That is, written data can be held by the transistor M1 for a long time, so that the frequency of refreshing the memory cell can be reduced. In addition, the refresh operation of the memory cell can be made unnecessary. Furthermore, since the leakage current is very small, multi-valued data or analog data can be held in the memory cell 1471, the memory cell 1472, and the memory cell 1473.

[0491] Furthermore, in the DOSRAM, if a sense amplifier is provided so as to overlap under the memory cell array 1470 as described above, the bit line can be shortened. This reduces the bit line capacitance and the storage capacitance of the memory cell.

[0492] [NOSRAM] 42D to 42G show circuit configuration examples of a gain cell type memory cell having two transistors and one capacitor. A memory cell 1474 shown in FIG. 42D includes a transistor M2, a transistor M3, and a capacitor CB. The transistor M2 has a top gate (sometimes simply referred to as a gate) and a back gate. In this specification and the like, a storage device having a gain cell type memory cell using an OS transistor as the transistor M2 may be referred to as a nonvolatile oxide semiconductor RAM (NOSRAM).

[0493] A first terminal of the transistor M2 is connected to a first terminal of the capacitance element CB, a second terminal of the transistor M2 is connected to the wiring WBL, a gate of the transistor M2 is connected to the wiring WOL, and a back gate of the transistor M2 is connected to the wiring BGL. A second terminal of the capacitance element CB is connected to the wiring CAL. A first terminal of the transistor M3 is connected to the wiring RBL, a second terminal of the transistor M3 is connected to the wiring SL, and a gate of the transistor M3 is connected to the first terminal of the capacitance element CB.

[0494] The wiring WBL functions as a write bit line, the wiring RBL functions as a read bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CB. When writing data, while holding data, and when reading data, it is preferable to apply a low-level potential to the wiring CAL. The wiring BGL functions as a wiring for applying a potential to the back gate of the transistor M2. By applying an arbitrary potential to the wiring BGL, the threshold voltage of the transistor M2 can be increased or decreased.

[0495] Here, the memory cell 1474 shown in Fig. 42D corresponds to the memory device shown in Fig. 35. That is, the transistor M2 corresponds to the transistor 200, the capacitor CB corresponds to the capacitor 100, the transistor M3 corresponds to the transistor 300, the wiring WBL corresponds to the wiring 1003, the wiring WOL corresponds to the wiring 1004, the wiring BGL corresponds to the wiring 1006, the wiring CAL corresponds to the wiring 1005, the wiring RBL corresponds to the wiring 1002, and the wiring SL corresponds to the wiring 1001.

[0496] Moreover, the memory cell MC is not limited to the memory cell 1474, and the circuit configuration can be changed as appropriate. For example, the memory cell MC may be configured such that the back gate of the transistor M2 is connected to the wiring WOL instead of the wiring BGL, as in the memory cell 1475 shown in FIG. 42E. For example, the memory cell MC may be configured such that the transistor M2 has a single gate structure, that is, a transistor M2 without a back gate, as in the memory cell 1476 shown in FIG. 42F. For example, the memory cell MC may be configured such that the wiring WBL and the wiring RBL are combined into a single wiring BIL, as in the memory cell 1477 shown in FIG. 42G.

[0497] When the semiconductor device described in the above embodiment is used for the memory cell 1474 or the like, the transistor 200 can be used as the transistor M2, the transistor 300 can be used as the transistor M3, and the capacitor CB can be used as the capacitor CB. By using an OS transistor as the transistor M2, the leakage current of the transistor M2 can be made very small. As a result, written data can be held by the transistor M2 for a long time, so that the frequency of refreshing the memory cell can be reduced. In addition, the refresh operation of the memory cell can be made unnecessary. In addition, since the leakage current is very small, multi-level data or analog data can be held in the memory cell 1474. The same applies to the memory cells 1475 to 1477.

[0498] Note that the transistor M3 may be a transistor having silicon in a channel formation region (hereinafter, may be referred to as a Si transistor). The conductivity type of the Si transistor may be an n-channel type or a p-channel type. The Si transistor may have a higher field-effect mobility than an OS transistor. Therefore, a Si transistor may be used as the transistor M3 functioning as a read transistor. By using a Si transistor as the transistor M3, the transistor M2 can be stacked on the transistor M3, thereby reducing the area occupied by the memory cell and achieving high integration of the memory device.

[0499] In addition, the transistor M3 may be an OS transistor. When the transistors M2 and M3 are OS transistors, the memory cell array 1470 can be configured as a circuit using only n-type transistors.

[0500] FIG. 42H shows an example of a gain cell type memory cell having three transistors and one capacitor. A memory cell 1478 shown in FIG. 42H includes transistors M4 to M6 and a capacitor CC. The capacitor CC is provided as appropriate. The memory cell 1478 is electrically connected to a wiring BIL, a wiring RWL, a wiring WWL, a wiring BGL, and a wiring GNDL. The wiring GNDL is a wiring that applies a low-level potential. Note that the memory cell 1478 may be electrically connected to a wiring RBL and a wiring WBL instead of the wiring BIL.

[0501] The transistor M4 is an OS transistor having a backgate, and the backgate is electrically connected to the wiring BGL. The backgate and the gate of the transistor M4 may be electrically connected to each other. Alternatively, the transistor M4 does not necessarily have to have a backgate.

[0502] Note that the transistors M5 and M6 may be n-channel Si transistors or p-channel Si transistors, or the transistors M4 to M6 may be OS transistors. In this case, the memory cell array 1470 can be configured as a circuit using only n-type transistors.

[0503] When the semiconductor device described in the above embodiment is used for the memory cell 1478, the transistor 200 can be used as the transistor M4, the transistors M5 and M6 can be used as the transistors M5 and M6, and the capacitor 100 can be used as the capacitor CC. By using an OS transistor as the transistor M4, the leakage current of the transistor M4 can be made extremely small.

[0504] Note that the configurations of the peripheral circuit 1411, the memory cell array 1470, and the like shown in this embodiment are not limited to those described above. The arrangement or functions of these circuits, wirings connected to the circuits, circuit elements, and the like may be changed, deleted, or added as necessary.

[0505] Generally, various storage devices (memories) are used in semiconductor devices such as computers depending on the purpose. Figure 43 shows various storage devices by hierarchy. The higher the storage device, the faster the access speed is required, and the lower the storage device, the larger the storage capacity and the higher the recording density are required. Figure 43 shows, from the top layer, memories embedded as registers in arithmetic processing devices such as CPUs, SRAMs (Static Random Access Memory), DRAMs (Dynamic Random Access Memory), and 3D NAND memories.

[0506] The memory embedded as a register in a processor such as a CPU is used for temporary storage of calculation results, and is accessed frequently by the processor. Therefore, a faster operating speed is required rather than a larger memory capacity. The register also has the function of storing setting information for the processor.

[0507] SRAM is used, for example, in caches. A cache has the function of storing a copy of some of the information stored in the main memory. By storing a copy of frequently used data in the cache, the speed of accessing the data can be increased.

[0508] DRAM is used, for example, as a main memory. The main memory has a function of storing programs and data read from storage. The recording density of DRAM is approximately 0.1 to 0.3 Gbit / mm 2 It is.

[0509] 3D NAND memory is used, for example, in storage. Storage has the function of holding data that needs to be stored for a long time and various programs used in processing units. Therefore, storage requires a larger memory capacity and a higher recording density than the operating speed. The recording density of memory devices used in storage is approximately 0.6 to 6.0 Gbit / mm 2 It is.

[0510] The storage device of one embodiment of the present invention has a high operating speed and can retain data for a long period of time. The storage device of one embodiment of the present invention can be suitably used as a storage device located in a boundary area 901 including both a hierarchical level where a cache is located and a hierarchical level where a main memory is located. The storage device of one embodiment of the present invention can be suitably used as a storage device located in a boundary area 902 including both a hierarchical level where a main memory is located and a hierarchical level where a storage is located.

[0511] The structure described in this embodiment mode can be used in appropriate combination with structures described in other embodiment modes or examples.

[0512] (Embodiment 4) In this embodiment, an example of a chip 1200 on which the semiconductor device of the present invention is mounted is shown with reference to Figures 44A and 44B. A plurality of circuits (systems) are mounted on the chip 1200. A technology for integrating a plurality of circuits (systems) on a single chip in this manner is sometimes called a system on chip (SoC).

[0513] As shown in FIG. 44A, the chip 1200 includes a CPU 1211, a GPU 1212, one or more analog computing units 1213, one or more memory controllers 1214, one or more interfaces 1215, one or more network circuits 1216, and the like.

[0514] Chip 1200 is provided with bumps (not shown) and is connected to a first surface of a printed circuit board (PCB) 1201 as shown in Fig. 44B. In addition, a plurality of bumps 1202 are provided on the back side of the first surface of PCB 1201 and are connected to a motherboard 1203.

[0515] The motherboard 1203 may be provided with storage devices such as a DRAM 1221 and a flash memory 1222. For example, the DRAM 1221 may be the DOSRAM described in the above embodiment. For example, the flash memory 1222 may be the NOSRAM described in the above embodiment.

[0516] The CPU 1211 preferably has a plurality of CPU cores. The GPU 1212 preferably has a plurality of GPU cores. The CPU 1211 and the GPU 1212 may each have a memory for temporarily storing data. Alternatively, a memory common to the CPU 1211 and the GPU 1212 may be provided in the chip 1200. The memory may be the above-mentioned NOSRAM or DOSRAM. The GPU 1212 is suitable for parallel calculation of a large amount of data, and may be used for image processing and multiplication and accumulation. By providing the GPU 1212 with an image processing circuit or a multiplication and accumulation circuit using the oxide semiconductor of the present invention, it becomes possible to perform image processing and multiplication and accumulation with low power consumption.

[0517] In addition, by providing the CPU 1211 and GPU 1212 on the same chip, the wiring between the CPU 1211 and GPU 1212 can be shortened, and data transfer from the CPU 1211 to the GPU 1212, data transfer between the memories of the CPU 1211 and GPU 1212, and transfer of calculation results from the GPU 1212 to the CPU 1211 after calculation in the GPU 1212 can be performed quickly.

[0518] The analog calculation unit 1213 has one or both of an A / D (analog / digital) conversion circuit and a D / A (digital / analog) conversion circuit. The analog calculation unit 1213 may also be provided with the above-mentioned product-sum calculation circuit.

[0519] The memory controller 1214 has a circuit that functions as a controller for the DRAM 1221 and a circuit that functions as an interface for the flash memory 1222 .

[0520] The interface 1215 has an interface circuit with externally connected devices such as a display device, a speaker, a microphone, a camera, and a controller. The controller includes a mouse, a keyboard, a game controller, etc. As such an interface, a USB (Universal Serial Bus), an HDMI (registered trademark) (High-Definition Multimedia Interface), etc. can be used.

[0521] The network circuit 1216 includes a network circuit such as a LAN (Local Area Network), and may also include a circuit for network security.

[0522] The above circuits (systems) can be formed in the same manufacturing process in the chip 1200. Therefore, even if the number of circuits required for the chip 1200 increases, there is no need to increase the manufacturing process, and the chip 1200 can be manufactured at low cost.

[0523] A PCB 1201 on which a chip 1200 having a GPU 1212 is provided, a motherboard 1203 on which a DRAM 1221 and a flash memory 1222 are provided can be referred to as a GPU module 1204.

[0524] The GPU module 1204 has the chip 1200 using SoC technology, so that its size can be reduced. In addition, since it excels in image processing, it is suitable for use in portable electronic devices such as smartphones, tablet terminals, laptop PCs, and portable (portable) game consoles. In addition, a multiply-and-accumulate circuit using the GPU 1212 can execute techniques such as deep neural networks (DNN), convolutional neural networks (CNN), recurrent neural networks (RNN), autoencoders, deep Boltzmann machines (DBM), and deep belief networks (DBN), so that the chip 1200 can be used as an AI chip, and the GPU module 1204 can be used as an AI system module.

[0525] The structure described in this embodiment mode can be used in appropriate combination with structures described in other embodiment modes or examples.

[0526] (Embodiment 5) This embodiment mode describes an example of an electronic component or electronic device in which the memory device or the like described in the above embodiment mode is incorporated.

[0527] <Electronic components> First, an example of an electronic component incorporating a memory device 720 will be described with reference to FIGS. 45A and 45B.

[0528] FIG. 45A shows a perspective view of electronic component 700 and a substrate (mounting substrate 704) on which electronic component 700 is mounted. Electronic component 700 shown in FIG. 45A has memory device 720 in mold 711. FIG. 45A omits a portion of electronic component 700 in order to show the inside of electronic component 700. Electronic component 700 has lands 712 on the outside of mold 711. Lands 712 are electrically connected to electrode pads 713, and electrode pads 713 are electrically connected to memory device 720 by wires 714. Electronic component 700 is mounted on, for example, a printed circuit board 702. A plurality of such electronic components are combined and electrically connected on printed circuit board 702 to complete mounting substrate 704.

[0529] The memory device 720 includes a driver circuit layer 721 and a memory circuit layer 722 .

[0530] 45B shows a perspective view of electronic component 730. Electronic component 730 is an example of a SiP (System in package) or MCM (Multi Chip Module). Electronic component 730 has an interposer 731 provided on a package substrate 732 (printed circuit board), and a semiconductor device 735 and a plurality of memory devices 720 provided on interposer 731.

[0531] In the electronic component 730, an example is shown in which the storage device 720 is used as a high bandwidth memory (HBM). Also, the semiconductor device 735 can be an integrated circuit (semiconductor device) such as a CPU, a GPU, or an FPGA.

[0532] The package substrate 732 may be a ceramic substrate, a plastic substrate, a glass epoxy substrate, etc. The interposer 731 may be a silicon interposer, a resin interposer, etc.

[0533] The interposer 731 has a plurality of wirings and functions to electrically connect a plurality of integrated circuits having different terminal pitches. The plurality of wirings are provided in a single layer or multiple layers. The interposer 731 also functions to electrically connect the integrated circuits provided on the interposer 731 to electrodes provided on the package substrate 732. For these reasons, the interposer may be called a "rewiring substrate" or an "intermediate substrate." In addition, a through electrode may be provided in the interposer 731, and the integrated circuits and the package substrate 732 may be electrically connected using the through electrode. In addition, in a silicon interposer, a TSV (Through Silicon Via) may be used as the through electrode.

[0534] It is preferable to use a silicon interposer as the interposer 731. Since a silicon interposer does not require an active element, it can be manufactured at a lower cost than an integrated circuit. On the other hand, since the wiring of the silicon interposer can be formed by a semiconductor process, it is easy to form fine wiring, which is difficult to form with a resin interposer.

[0535] In HBM, many wirings need to be connected to realize a wide memory bandwidth. For this reason, the interposer that mounts HBM requires fine and high-density wiring. Therefore, it is preferable to use a silicon interposer for the interposer that mounts HBM.

[0536] In addition, in SiPs and MCMs that use silicon interposers, reliability is less likely to decrease due to differences in the expansion coefficient between the integrated circuit and the interposer. In addition, because the surface of the silicon interposer is highly flat, connection defects are less likely to occur between the integrated circuit mounted on the silicon interposer and the silicon interposer. In particular, it is preferable to use silicon interposers in 2.5D packages (2.5-dimensional mounting) in which multiple integrated circuits are arranged side by side on the interposer.

[0537] A heat sink (heat dissipation plate) may be provided so as to overlap the electronic component 730. When providing a heat sink, it is preferable to align the height of an integrated circuit provided on the interposer 731. For example, in the electronic component 730 shown in this embodiment, it is preferable to align the height of the memory device 720 and the height of the semiconductor device 735.

[0538] In order to mount the electronic component 730 on another substrate, electrodes 733 may be provided on the bottom of the package substrate 732. FIG. 45B shows an example in which the electrodes 733 are formed of solder balls. By providing solder balls in a matrix on the bottom of the package substrate 732, BGA (Ball Grid Array) mounting can be realized. The electrodes 733 may also be formed of conductive pins. By providing conductive pins in a matrix on the bottom of the package substrate 732, PGA (Pin Grid Array) mounting can be realized.

[0539] The electronic component 730 can be mounted on other substrates using various mounting methods, including but not limited to BGA and PGA, such as Staggered Pin Grid Array (SPGA), Land Grid Array (LGA), Quad Flat Package (QFP), Quad Flat J-leaded package (QFJ), and Quad Flat Non-leaded package (QFN).

[0540] This embodiment mode can be implemented in appropriate combination with structures described in other embodiment modes or examples.

[0541] (Embodiment 6) In this embodiment, an application example of a storage device using the semiconductor device described in the previous embodiment will be described. The semiconductor device described in the previous embodiment can be applied to storage devices of various electronic devices (e.g., information terminals, computers, smartphones, electronic book terminals, digital cameras (including video cameras), recording and reproducing devices, navigation systems, and the like). Note that the computer here includes a large computer such as a server system, in addition to tablet computers, notebook computers, and desktop computers. Alternatively, the semiconductor device described in the previous embodiment can be applied to various removable storage devices such as memory cards (e.g., SD cards), USB memories, and SSDs (solid state drives). FIGS. 46A to 46E are schematic diagrams showing some configuration examples of removable storage devices. For example, the semiconductor device described in the previous embodiment is processed into a packaged memory chip and used in various storage devices and removable memories.

[0542] 46A is a schematic diagram of a USB memory. A USB memory 1100 has a housing 1101, a cap 1102, a USB connector 1103, and a board 1104. The board 1104 is housed in the housing 1101. For example, a memory chip 1105 and a controller chip 1106 are attached to the board 1104. The semiconductor device described in the above embodiment can be incorporated in the memory chip 1105 or the like.

[0543] FIG. 46B is a schematic diagram of the appearance of an SD card, and FIG. 46C is a schematic diagram of the internal structure of the SD card. The SD card 1110 has a housing 1111, a connector 1112, and a substrate 1113. The substrate 1113 is housed in the housing 1111. For example, a memory chip 1114 and a controller chip 1115 are attached to the substrate 1113. The capacity of the SD card 1110 can be increased by providing a memory chip 1114 on the back side of the substrate 1113 as well. In addition, a wireless chip having a wireless communication function may be provided on the substrate 1113. This makes it possible to read and write data from and to the memory chip 1114 by wireless communication between the host device and the SD card 1110. The semiconductor device shown in the above embodiment can be incorporated into the memory chip 1114 or the like.

[0544] FIG. 46D is a schematic diagram of the appearance of an SSD, and FIG. 46E is a schematic diagram of the internal structure of the SSD. SSD 1150 has a housing 1151, a connector 1152, and a board 1153. Board 1153 is housed in housing 1151. For example, memory chip 1154, memory chip 1155, and controller chip 1156 are attached to board 1153. Memory chip 1155 is a work memory for controller chip 1156, and may be, for example, a DOSRAM chip. By providing memory chip 1154 on the back side of board 1153, the capacity of SSD 1150 can be increased. The semiconductor device shown in the previous embodiment can be incorporated into memory chip 1154 or the like.

[0545] This embodiment mode can be implemented in appropriate combination with structures described in other embodiment modes or examples.

[0546] (Embodiment 7) The semiconductor device according to one embodiment of the present invention can be used for a processor such as a CPU or a GPU, or a chip. Specific examples of electronic devices including a processor such as a CPU or a GPU, or a chip according to one embodiment of the present invention are shown in FIG.

[0547] <Electronic equipment and systems> The GPU or chip according to one embodiment of the present invention can be mounted on various electronic devices. Examples of electronic devices include electronic devices with relatively large screens, such as television devices, monitors for desktop or notebook information terminals, digital signage, large game machines such as pachinko machines, digital cameras, digital video cameras, digital photo frames, electronic book readers, mobile phones, portable game machines, portable information terminals, and audio playback devices. Moreover, by providing the GPU or chip according to one embodiment of the present invention in an electronic device, it is possible to mount artificial intelligence on the electronic device.

[0548] The electronic device of one embodiment of the present invention may have an antenna. By receiving a signal through the antenna, images, information, and the like can be displayed on a display portion. In addition, when the electronic device has an antenna and a secondary battery, the antenna may be used for contactless power transmission.

[0549] An electronic device according to one embodiment of the present invention may have a sensor (including a function of measuring force, displacement, position, velocity, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared rays).

[0550] An electronic device according to one embodiment of the present invention can have various functions. For example, the electronic device can have a function of displaying various information (still images, videos, text images, etc.) on a display unit, a touch panel function, a function of displaying a calendar, date, or time, a function of executing various software (programs), a wireless communication function, a function of reading out a program or data recorded in a recording medium, etc. Examples of electronic devices are shown in Figs. 47A to 47H.

[0551] [Information terminal] 47A illustrates a mobile phone (smartphone), which is a type of information terminal. The information terminal 5100 includes a housing 5101 and a display unit 5102. As an input interface, a touch panel is provided on the display unit 5102, and buttons are provided on the housing 5101.

[0552] By applying the chip of one embodiment of the present invention, the information terminal 5100 can execute applications using artificial intelligence. Examples of applications using artificial intelligence include an application that recognizes a conversation and displays the conversation content on the display unit 5102, an application that recognizes characters, figures, and the like input by a user to a touch panel provided in the display unit 5102 and displays them on the display unit 5102, and an application that performs biometric authentication such as fingerprints and voiceprints.

[0553] 47B illustrates a notebook type information terminal 5200. The notebook type information terminal 5200 includes a main body 5201 of the information terminal, a display unit 5202, and a keyboard 5203.

[0554] The notebook type information terminal 5200 can execute an application using artificial intelligence by applying a chip according to one embodiment of the present invention, similar to the above-described information terminal 5100. Examples of applications using artificial intelligence include design support software, text correction software, and automatic menu generation software. In addition, the notebook type information terminal 5200 can be used to develop new artificial intelligence.

[0555] In the above description, a smartphone and a notebook type information terminal are illustrated in Fig. 47A and Fig. 47B as examples of electronic devices, but information terminals other than smartphones and notebook type information terminals can also be applied. Examples of information terminals other than smartphones and notebook type information terminals include PDAs (Personal Digital Assistants), desktop type information terminals, and workstations.

[0556] [Game consoles] FIG. 47C illustrates a portable game machine 5300 which is an example of a game machine. The portable game machine 5300 includes a housing 5301, a housing 5302, a housing 5303, a display unit 5304, a connection unit 5305, an operation key 5306, and the like. The housing 5302 and the housing 5303 can be detached from the housing 5301. When the connection unit 5305 of the housing 5301 is attached to another housing (not shown), a video displayed on the display unit 5304 can be displayed on another video device (not shown). In this case, the housing 5302 and the housing 5303 can each function as an operation unit. This allows a plurality of players to play a game at the same time. The chips described in the above embodiments can be incorporated in the chips provided on the substrates of the housings 5301, 5302, and 5303.

[0557] 47D shows an example of a game machine, a stationary game machine 5400. A controller 5402 is connected to the stationary game machine 5400 wirelessly or via a wire.

[0558] A game machine with low power consumption can be realized by applying a GPU or a chip of one embodiment of the present invention to a game machine such as a portable game machine 5300 or a stationary game machine 5400. Furthermore, low power consumption can reduce heat generation from a circuit, and therefore the influence of heat generation on the circuit itself, peripheral circuits, and modules can be reduced.

[0559] Furthermore, by applying a GPU or a chip of one embodiment of the present invention to the portable game console 5300, the portable game console 5300 can have artificial intelligence.

[0560] Originally, the expression of the progress of a game, the behavior of creatures appearing in the game, and phenomena occurring in the game are determined by the program of the game, but by applying artificial intelligence to the portable game device 5300, it becomes possible to express things that are not limited to the program of the game. For example, it becomes possible to express things such as changes in the questions asked by the player, the progress of the game, the time, and the behavior of people appearing in the game.

[0561] In addition, when playing a game on the portable game console 5300 that requires multiple players, the game players can be personified using ...

Claims

1. forming a first insulator, a first oxide film, a second oxide film, a first conductive film, a first insulating film, and a second conductive film in this order on a substrate; processing the first oxide film, the second oxide film, the first conductive film, the first insulating film, and the second conductive film into an island shape to form a first oxide, a second oxide, a first conductive layer, a first insulating layer, and a second conductive layer; In the process, a layer having an oxide containing a main component of the second conductive film is formed to cover the first oxide, the second oxide, the first conductive layer, the first insulating layer, and the second conductive layer; removing the second conductive layer and the layer; depositing a second insulating film on the first insulator, the first oxide, the second oxide, the first conductive layer, and the first insulating layer; anisotropically etching the second insulating film to form a second insulating layer in contact with a side surface of the first oxide, the second oxide, the first conductive layer, and the first insulating layer; forming a second insulator over the first insulator, the first oxide, the second oxide, the first conductive layer, the first insulating layer, and the second insulating layer; forming an opening through the first conductive layer, the first insulating layer, the second insulating layer, and the second insulator to reach the second oxide; In forming the opening, a first conductor and a second conductor are formed from the first conductive layer, a third insulator and a fourth insulator are formed from the first insulating layer, and a fifth insulator and a sixth insulator are formed from the second insulating layer; forming a third oxide in the opening, a seventh insulator on the third oxide, and a third conductor on the seventh insulator.

2. A method of forming a first insulator, a first oxide film, a second oxide film, a first conductive film, a first insulating film, and a second conductive film on a substrate in this order; processing the first oxide film, the second oxide film, the first conductive film, the first insulating film, and the second conductive film into an island shape to form a first oxide, a second oxide, a first conductive layer, a first insulating layer, and a second conductive layer; In the process, a layer having an oxide containing a main component of the second conductive film is formed to cover the first oxide, the second oxide, the first conductive layer, the first insulating layer, and the second conductive layer; removing the second conductive layer and the layer; During the removal, the layer is left in contact with sides of the first oxide, the second oxide, the first conductive layer, and the first insulating layer; depositing a second insulating film on the first insulator, the first oxide, the second oxide, the first conductive layer, and the first insulating layer; anisotropically etching the second insulating film to form a second insulating layer in contact with the first oxide, the second oxide, the first conductive layer, and the layer in contact with a side of the first insulating layer; forming a second insulator over the first insulator, the first oxide, the second oxide, the first conductive layer, the first insulating layer, and the second insulating layer; forming an opening through the first conductive layer, the first insulating layer, the second insulating layer, and the second insulator to reach the second oxide; In forming the opening, a first conductor and a second conductor are formed from the first conductive layer, a third insulator and a fourth insulator are formed from the first insulating layer, and a fifth insulator and a sixth insulator are formed from the second insulating layer; forming a third oxide in the opening, a seventh insulator on the third oxide, and a third conductor on the seventh insulator.

3. In claim 1 or 2, The method for manufacturing a semiconductor device, wherein the second conductive layer and the layer are removed by dry etching.

4. In any one of claims 1 to 3, A method for manufacturing a semiconductor device, comprising: depositing an eighth insulator over the second insulator, the third oxide, the seventh insulator, and the third conductor by a sputtering method in an atmosphere containing oxygen.

5. In any one of claims 1 to 4, A method for manufacturing a semiconductor device, wherein the third insulator, the second insulator, and the sixth insulator can suppress oxygen diffusion more than the second insulator.

6. In any one of claims 1 to 5, A method for manufacturing a semiconductor device, wherein the first oxide is more effective at suppressing oxygen diffusion than the second oxide.

7. In any one of claims 1 to 6, a heat treatment at a temperature of 400° C. or more and 600° C. or less after the formation of the second oxide film;

8. In any one of claims 1 to 7, the first insulator has a first region in contact with the first oxide and a second region not in contact with the first oxide; the thickness of the second region is less than the thickness of the first region; A method for manufacturing a semiconductor device, wherein the third oxide has a region in contact with a top surface of the second region, a region in contact with a side surface of the first region, a region in contact with a side surface of the first oxide, and a region in contact with a side surface of the second oxide.

Citation Information

Patent Citations

  • Thin film transistor

    JP2012084857A

  • Semiconductor device, and method of manufacturing the same

    JP2018107447A

  • Semiconductor device and semiconductor device manufacturing method

    JP2018121049A

  • Semiconductor device

    JP2019024128A

  • Semiconductor device and method for manufacturing semiconductor device

    WO2018178793A1