Polyfunctional organosiloxanes, compositions containing same, and methods for preparing same
By employing boron-containing Lewis acids as catalysts, the method addresses the challenges of controlling structure and crosslinking in multifunctional organosiloxanes, resulting in improved polyfunctional organohydrogensiloxanes suitable for release coating compositions.
Patent Information
- Application Number
- JP2021532474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-21
- Filing Date
- 2019-12-04
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2039-12-04
AI Technical Summary
Existing methods for producing multifunctional organosiloxanes with branched siloxane endblockers suffer from poor control over structure, molecular weight, and degree of crosslinking, leading to the production of crosslinked products.
The use of boron-containing Lewis acids as catalysts in the preparation of multifunctional organohydrogensiloxanes, which are combined with hydroxyl-terminated polydiorganosiloxanes and branched polyorganohydrogensiloxanes to form polyfunctional organohydrogensiloxanes with controlled structure and branched endblockers, allowing for improved selectivity and control over the reaction.
This method enhances the selectivity and control over the formation of polyfunctional organohydrogensiloxanes, reducing the formation of undesirable species and improving their suitability for applications such as release coating compositions.
Smart Images

Figure 0007555925000001 
Figure 0007555925000002 
Figure 0007555925000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit under 35 U.S.C. §119(e) of U.S. Provisional Application No. 62 / 783,227, filed December 21, 2018. U.S. Provisional Application No. 62 / 783,227 is incorporated herein by reference.
[0002] Polyfunctional organosiloxanes and methods for their preparation are disclosed. The polyfunctional organosiloxanes include a linear polydiorganosiloxane backbone with branched siloxane endblockers. The polyfunctional organosiloxanes are useful in curable compositions, for example as crosslinkers. [Background technology]
[0003] Methods have been proposed for producing polyfunctional organosiloxane crosslinkers having a linear polydiorganosiloxane backbone with a branched siloxane endblocker using a platinum catalyzed reaction of a branched organohydrogensiloxane with a vinyl terminated polydiorganosiloxane. These polyfunctional organosiloxane crosslinkers have a branched siloxane endblocker attached to a linear polydiorganosiloxane backbone via a divalent hydrocarbon liner. These methods suffer from the production of crosslinked products and the ability to control the structure, molecular weight, and degree of crosslinking in the product is poor. Summary of the Invention
[0004] A polyfunctional organohydrogensiloxane and a method for its preparation using a boron-containing Lewis acid as a catalyst are disclosed. The clustered functional organosiloxane can be prepared by a method including a step of functionalizing the polyfunctional organohydrogensiloxane. The polyfunctional organohydrogensiloxane and the clustered functional organosiloxane are useful in a curable composition. The polyfunctional organohydrogensiloxane can be used in a release coating composition. The clustered functional organosiloxane can be used in an adhesive composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0005] The polyfunctional organohydrogensiloxanes prepared by the methods described herein comprise a linear polydiorganosiloxane backbone with a branched siloxane endblocker. The branched siloxane endblocker is linked to the linear polydiorganosiloxane backbone via an oxygen linkage. The polyfunctional organohydrogensiloxanes can be used as crosslinkers. The polyfunctional organohydrogensiloxanes are useful in curable compositions, such as release coating compositions.
[0006] Polyfunctional organohydrogensiloxanes: 1) A) boron-containing Lewis acids; B) formula, [ka] zzzImage1zzz [wherein the subscript n is 2 to 2,000; 1 are independently selected from the group consisting of monovalent hydrocarbon groups and monovalent halogenated hydrocarbon groups; and C) formula, [ka] zzzImage2zzz wherein each subscript d is independently 0 to 995 and each R is an independently selected monovalent hydrocarbon radical, thereby preparing a product, the product comprising a polyfunctional organohydrogensiloxane and a by-product comprising H2. In step 1), the starting materials may optionally further comprise D) a solvent.
[0007] The method may optionally include one or more additional steps. The method may further include recovering the polyfunctional organohydrogensiloxane. The method may further include 2) removing H2 generated during and / or after step 1) during the formation of the polyfunctional organohydrogensiloxane, and / or 3) neutralizing residual boron-containing Lewis acid in the product. By-product H2 can be removed by any convenient means, such as stripping and / or combustion. Neutralization can be performed by E) adding a neutralizing agent to the product and then filtering the product. Steps 2) and 3) can be performed in any order. For example, if particulate by-products are present as a result of neutralization, the method may further include 4) removing particulates such as alumina after neutralization by any convenient means, such as filtration.
[0008] One or more of the process steps can be carried out at a temperature of 5° C. to 70° C., alternatively 5° C. to 65° C., alternatively 10° C. to 60° C., alternatively 15° C. to 50° C., alternatively 20° C. to 35° C., alternatively 5° C. to 30° C., alternatively 30° C. Alternatively, step 1) can be carried out at a temperature of 5° C. to 70° C., alternatively 5° C. to 65° C., alternatively 10° C. to 60° C., alternatively 15° C. to 50° C., alternatively 20° C. to 35° C., alternatively 5° C. to 30° C., alternatively 30° C. Without being bound by theory, it is believed that carrying out the process, particularly step 1), at a relatively low temperature (e.g., 90° C. or less, alternatively 80° C. or less, alternatively 70° C. or less, alternatively 50° C. or less) can result in improved reaction rate, yield, or both.
[0009] The starting materials used in step 1) of the process, or steps 1), 2), and 3) of the process, may be free of platinum group metal catalyst. As used herein, "free" includes none, or an amount undetectable by GC, or an amount insufficient to cause performance problems in release coatings prepared from the release coating compositions comprising polyfunctional organohydrogensiloxanes made by the processes described herein.
[0010] Starting Materials A) Catalyst The starting material A) in the process described herein is a boron-containing Lewis acid. The boron-containing Lewis acid may be a trivalent boron compound having at least one perfluoroaryl group per molecule, alternatively one to three perfluoroaryl groups per molecule, alternatively two to three perfluoroaryl groups per molecule, alternatively three perfluoroaryl groups per molecule. The perfluoroaryl groups may have 6 to 12 carbon atoms, alternatively 6 to 10 carbon atoms, alternatively 6 carbon atoms. A) Boron-containing Lewis acid catalysts are: (C5F4)(C6F5)2B; (C5F4)3B; (C6F5)BF2; BF(C6F5)2; B(C6F5)3; BCl2(C6F5); BCl(C6F5)2; B(C6H5)(C6F5)2; B(C6H5)2(C6F5); [C6H4(mCF3)]3B; [C6H4(pOCF3)]3B; (C6F5)B(OH)2; (C6F5)2BOH; (C6F5)2BH; (C6F5)BH2; (C7H 11 )B(C6F5)2;(C8H 14)B(C6F5); (C6F5)2B(OC2H5); or (C6F5)2B-CH2CH2Si(CH3). Alternatively, the boron-containing Lewis acid catalyst may be tris(pentafluorophenyl)borane of formula B(C6F5)3. Such boron-containing Lewis acids are commercially available, for example, from Millipore Sigma (St. Louis, Missouri, USA). The amount of starting material A) will vary depending on the type and amount of other starting materials used, but starting material A) may be present in an amount of 50 ppm to 6000 ppm based on the combined weight of starting materials A), B), and C). Alternatively, the amount may be 50 ppm to 600 ppm on the same basis.
[0011] Starting Material B) Hydroxyl-Terminated Polydiorganosiloxane The starting material B) is represented by the formula B-1): [ka] zzzImage3zzz [wherein the subscript n is 2 to 2,000; 1 are independently selected from the group consisting of monovalent hydrocarbon radicals and monovalent halogenated hydrocarbon radicals. Alternatively, the subscript n may have a value such that 2≦n≦1,000, alternatively 5≦n≦900, alternatively 5≦n≦50, alternatively 5≦n≦15. Alternatively, each R 1 may be independently selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms. Suitable alkyl groups include methyl, ethyl, and propyl (including n-propyl and isopropyl). Suitable alkenyl groups include vinyl, allyl, and hexenyl. Suitable aryl groups include phenyl. Suitable halogenated alkyl groups include chloromethyl, chloropropyl, and trifluoropropyl groups. Alternatively, each R 1may be independently selected from the group consisting of methyl, vinyl, allyl, phenyl, and trifluoropropyl.
[0012] Suitable hydroxyl-terminated polydiorganosiloxanes for use as starting material B) can be prepared by methods known in the art, such as hydrolysis and condensation of the corresponding organohalosilanes, or equilibration of cyclic polydiorganosiloxanes. An exemplary hydroxyl-terminated polydiorganosiloxane is hydroxyl-terminated polydimethylsiloxane. Suitable hydroxyl-terminated polydimethylsiloxanes are also commercially available from Gelest, Inc. (Morrisville, Pennsylvania, USA), such as DMS-S12, DMS-S14, DMS-S15, DMS-S21, DMS-S27, DMS-S41, DMS-S32, DMS-S33, DMS-S35, DMS-S42, and DMS-S45.
[0013] Starting material (C) Polyorganohydrogensiloxane The starting material C) used in the process is a branched polyorganohydrogensiloxane of formula C-1), i.e. of the formula: [ka] zzzImage4zzz wherein each subscript d is independently 0 to 995 and each R is an independently selected monovalent hydrocarbon group. Alternatively, each subscript d may be 0 to 50. Alternatively, each R may be independently selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms. Suitable alkyl groups include methyl, ethyl, and propyl (including n-propyl and isopropyl). Suitable alkenyl groups include vinyl, allyl, and hexenyl. Suitable aryl groups include phenyl. Alternatively, each R may be independently selected from the group consisting of methyl, vinyl, and phenyl, or each R may be methyl or phenyl. Alternatively, each R may be methyl. The branched polyorganohydrogensiloxane may include difunctional siloxy units, i.e., the formula (RSiO 2 / 2 ) d where each subscript d is independently from 15 to 995, or each subscript d is independently from 15 to 100.
[0014] Alternatively, when each subscript d=0, the branched polyorganohydrogensiloxane has the formula C-2): [ka] zzzImage5zzz wherein R is as described above. Suitable branched polyorganohydrogensiloxanes, such as tetrakis(dimethylsiloxy)silane, are known in the art and commercially available from Gelest, Inc. (Morrisville, Pennsylvania, USA) or Millipore Sigma (St. Louis, Missouri, USA). Suitable branched polyorganosiloxanes can be prepared by known methods, such as cohydrolysis of tetrahalosilanes with monohalosilanes, optionally with dihalosilanes, or cohydrolysis of tetraalkoxysilanes with monoalkoxysilanes, optionally with dialkoxysilanes. Methods relating to suitable branched polyorganohydrogensiloxanes and methods for their preparation are disclosed, for example, in U.S. Pat. Nos. 5,422,412 and 5,581,008.
[0015] The amounts of starting materials B) and C) will vary depending on a variety of factors, including the OH content of B) the hydroxyl-terminated polydiorganosiloxane and the silicon-bonded hydrogen (SiH) content of C) the cyclic polyorganohydrogensiloxane, but the amounts are sufficient to provide a molar ratio of SiH in starting material C) to OH in starting material B) of from 4:1 to 40:1, alternatively from 4:1 to 20:1, alternatively from 5:1 to 10:1.
[0016] Starting material D) Solvent Solvents can be used in the present method. Solvents can facilitate the introduction of certain starting materials, such as starting material A) a boron-containing Lewis acid. Solvents as used herein are those that aid in the mobilization of the starting materials but do not essentially react with any of these starting materials. Solvents may be selected based on the solubility of the starting materials and the volatility of the solvent. "Solubility" refers to the solvent being sufficient to dissolve and / or disperse the starting materials. "Volatility" refers to the vapor pressure of the solvent.
[0017] A suitable solvent may be a hydrocarbon. Suitable hydrocarbons include aromatic hydrocarbons such as benzene, toluene, or xylene, and / or aliphatic hydrocarbons such as heptane, hexane, or octane. Alternatively, the solvent may be a halogenated hydrocarbon such as dichloromethane, 1,1,1-trichloroethane, or methylene chloride.
[0018] The amount of solvent may vary depending on a variety of factors, such as the type of solvent selected, as well as the amounts and types of other starting materials selected, etc. However, the amount of solvent may range from 0.1% to 99% by weight, alternatively from 2% to 50% by weight, based on the combined weight of starting materials A), B), and C).
[0019] Starting Material E) Neutralizing Agent Starting material E) is a neutralizing agent that can be optionally used to neutralize starting material A) after the product is formed. Alumina, triphenylamine, triphenylphosphine, and phenylacetylene are suitable neutralizing agents. Neutralizing agents are known in the art and are commercially available, for example, from Millipore Sigma (St. Louis, Missouri, USA). The amount of neutralizing agent will vary depending on various factors, such as the amount of starting material A), but starting material E) may be present in an amount sufficient to provide a weight ratio of neutralizing agent to boron-containing Lewis acid (E:A ratio) of 1:1 to 1000:1. Alternatively, when the neutralizing agent is triphenylphosphine or phenylacetylene, the E:A ratio may be 1:1 to 20:1. Alternatively, when the neutralizing agent is alumina, the E:A ratio may be 100:1 to 1000:1.
[0020] Product of the Method The product of the above process includes a) a polyfunctional organohydrogensiloxane and a by-product comprising H2. The product has the unit formula a-1): [ka] zzzImage6zzz [Wherein, the groups R and R 1and the subscripts n and d are as defined above. The subscript o' is 0 to 100. The subscript n'=(o'+1). Alternatively, when the subscript o'=1, the product has the formula a-2): [ka] zzzImage7zzz [Wherein, R and R 1 and subscripts n and d are as defined above. Alternatively, when each subscript d=0, the product comprises a polyfunctional organohydrogensiloxane of formula a-3): [ka] zzzImage8zzz [In the formula, groups R, R 1 and subscript n is as defined above.
[0021] Those skilled in the art will recognize that the product may contain more than one type of polyfunctional organohydrogensiloxane. A particular species may have a linear backbone derived from more than one starting material B) in one molecule, and branched groups derived from more than three starting materials C) in one molecule, depending on various factors such as the molar ratio of starting materials B) and C) selected for the process. However, the inventors have surprisingly found that the process described herein, using a boron-containing Lewis acid as starting material A), provides higher selectivity to polyfunctional organohydrogensiloxanes of formula a-2) and / or a-3) than previous processes involving platinum-catalyzed hydrosilylation. The method can, if desired, maximize the formation of polyfunctional organohydrogensiloxanes of formula a-2) and / or a-3) by controlling the polyfunctional organohydrogensiloxane structure, thereby resulting in a product with reduced or no polyfunctional organohydrogensiloxanes of formula a-1), where subscript o'>0.For example, by controlling the ratio of starting material C) to starting material B), it is possible to obtain polyfunctional organohydrogensiloxanes of formula a-2) and / or polyfunctional organohydrogensiloxanes of formula a-3), whose molecules have two branched portions each linked via an oxygen atom at the end of one linear polydiorganosiloxane portion. For example, as the ratio of starting material C) to starting material B) decreases, the likelihood of forming species of formula a-1) with subscript o'>0 or creating crosslinked species becomes higher, which may not be desirable for certain applications, such as release coating compositions. Thus, starting materials B) and C) can be used in amounts such that the molar ratio of C):B) is >3. Alternatively, the molar ratio of SiH in starting material C) to OH in starting material B) is 4:1 to 40:1, alternatively 4:1 to 20:1, alternatively 5:1 to 10:1. The polyfunctional organohydrogensiloxanes produced by the above-mentioned methods can be used, for example, as crosslinkers or co-crosslinkers in release coating compositions.
[0022] Method for preparing clustered functional organosiloxanes Alternatively, the above-mentioned method may further comprise functionalizing the polyfunctional organohydrogensiloxane to form a clustered functional organosiloxane. Combining starting materials, the starting materials comprising: the above product, or a) a polyfunctional organohydrogensiloxane recovered therefrom; b) a hydrosilylation reaction catalyst, and The method may further include a step of combining a) starting material a) comprising a reactive species having, on average, at least one aliphatically unsaturated group per molecule capable of addition reacting with silicon-bonded hydrogen atoms of the polyfunctional organohydrogensiloxane, the starting material c) further comprising one or more curable groups per molecule. Briefly, the method may be carried out by modifying the method described in U.S. Pat. No. 9,593,209. The starting material a) described herein above may be combined with a reactive species and a hydrosilylation reaction catalyst (referred to as components c) and d, respectively) in the amounts and under the conditions described in U.S. Pat. No. 9,593,209, column 8, line 44 to column 10, line 47.
[0023] Starting material b) Hydrosilylation reaction catalyst In the method of functionalizing polyfunctional organohydrogensiloxane to form clustered functional organosiloxane, suitable hydrosilylation catalyst for starting material b) is known in the art and commercially available.Hydrosilylation catalyst includes platinum group metal catalyst.Such hydrosilylation catalyst can be a metal selected from platinum, rhodium, ruthenium, palladium, osmium and iridium. Alternatively, the hydrosilylation catalyst may be a compound of such a metal, for example, chloride tris(triphenylphosphane)rhodium(I) (Wilkinson's catalyst), rhodium diphosphine chelates such as [1,2-bis(diphenylphosphino)ethane]dichlorodirhodium or [1,2-bis(diethylphosphino)ethane]dichlorodirhodium, chloroplatinic acid (Speier's catalyst), chloroplatinic acid hexahydrate, platinum dichloride, and complexes of the above compounds with low molecular weight organopolysiloxanes or platinum compounds microencapsulated in a matrix or core-shell structure. Complexes of platinum with low molecular weight organopolysiloxanes include platinum complexes of 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane (Karstedt's catalyst) and platinum complexes of methylvinylcyclosiloxane (Ashby's catalyst). These complexes may be microencapsulated in a resin matrix. Alternatively, the hydrosilylation catalyst may comprise platinum complex of 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane.Exemplary hydrosilylation catalysts are described in U.S. Pat. Nos. 3,159,601, 3,220,972, 3,296,291, 3,419,593, 3,516,946, 3,814,730, 3,989,668, 4,784,879, 5,036,117 and 5,175,325, and European Patent No. 0347895(B).Microencapsulated hydrosilylation catalysts and their preparation methods are known in the art, as exemplified in U.S. Pat. Nos. 4,766,176 and 5,017,654. The amount used may be sufficient to provide from 1 ppm to 1,000 ppm of platinum group metal, based on the combined weight of starting materials a), b), and c).
[0024] Starting material c) Reactive species The starting material c) reactant for functionalizing the polyfunctional organohydrogensiloxane to form the clustered functional organosiloxane is represented by the formula c-1), R 4 y SiR 5 (4-y) [wherein the subscript y is 1 to 3; and each R 4 is an aliphatic unsaturated group capable of undergoing an addition reaction, and each R 5 is an organic group having a curable group. Alternatively, the subscript y may be 1 to 2. Alternatively, the subscript y may be 1. Each R 4 may be independently selected from the group consisting of alkenyl (such as vinyl, allyl, and hexenyl) and alkynyl (such as propynyl or hexynyl). 5 may be independently selected from the group consisting of organic groups having acrylate groups, alcohol groups, alkoxy groups, epoxy groups, isocyanate groups, methacrylate groups, and urethane groups. 5 may be independently selected from the group consisting of an organic group having an acrylate group, an organic group having an epoxy group, and an organic group having a methacrylate group. 5 may be an organic group having an epoxy group. Suitable silanes are known in the art and are commercially available, for example, from Dow Silicones Corporation (Midland, Michigan, USA) or Gelest, Inc. Exemplary silanes include allyltrimethoxysilane, allyltriethoxysilane, or combinations thereof.
[0025] Alternatively, the starting material c) may be an organic compound not containing a silicon atom, such as a compound represented by the formula c-2), R 6 R 7 [In the formula, each R 6 is an aliphatic unsaturated group capable of undergoing an addition reaction, and each R 7 Each R may be a curable group.6 may be independently selected from the group consisting of alkenyl (such as vinyl, allyl, and hexenyl) and alkynyl (such as propynyl or hexynyl). 7 may be independently selected from the group consisting of organic groups having an acrylate group, an alcohol group, an alkoxy group, an epoxy group, an isocyanate group, a methacrylate group, or a urethane group. 7 may be selected from the group consisting of an organic group having an acrylate group, an organic group having an epoxy group, and an organic group having a methacrylate group. 7 may be an organic group having an epoxy group. Examples of suitable compounds of formula c-2) include allyl acrylate, allyl glycidyl ether, allyl methacrylate, and combinations thereof. Alternatively, c-2) may be allyl glycidyl ether. Alternatively, c-2) may be allyl methacrylate. Suitable compounds of formula c-2) are known in the art and are commercially available, for example, from Millipore Sigma (St. Louis, Missouri, USA).
[0026] The starting materials used in the method for producing the clustered functional organosiloxane may optionally further comprise one or more additional starting materials. The additional starting materials may be the additional components disclosed in U.S. Patent No. 9,593,209 (column 10, line 48 to column 16, line 17). The additional starting materials are selected from the group consisting of fillers with or without treating agents, non-reactive resins, chain extenders, endblockers, and catalyst inhibitors.
[0027] In the above-mentioned method, a') a product containing a clustered functional organosiloxane or a masterbatch of the clustered functional organosiloxane with a filler and / or a non-reactive resin is produced. The clustered functional organosiloxane has the unit formula a'-1): [ka] zzzImage9zzz [Wherein, the groups R and R1 and subscripts n, d, n', and o' are as defined above. 8 is a hydrogen atom or a curable group, provided that at least one R 8 is a curable group. 8 The curable groups are derived from the starting material c) reactive species described above. 8 The curable group is R 4’ SiR 5 (4-y) , and R 6’ R 7 [In the formula, R 4’ and R 6’ is a divalent hydrocarbon radical produced by hydrosilylation of starting material c), and the silicon-bonded hydrogen atoms of starting material a). Alternatively, R 8 is a curable group (i.e., not hydrogen). Or, R occurs 1-3 times, or 1-2 times, or an average of 2 times per molecule. 8 becomes a curable group (other than hydrogen).
[0028] Alternatively, when the subscript o'=0, the product has the formula a'-2): [ka] zzzImage10zzz [In the formula, groups R, R 1 , and R 8 and subscripts n and d are as defined above.
[0029] Alternatively, when subscript d=0, the product has the formula a'-3): [ka] zzzImage11zzz [In the formula, groups R, R 1 , and R 8 and subscript n is as defined above.
[0030] The clustered functional organosiloxanes prepared as described above can be used, for example, as additives in adhesive compositions, such as thermal radical curing adhesive compositions.
[0031] Clustered functional organosiloxane can be used as an additive in adhesive composition, for example.Without being bound by theory, it is believed that a') clustered functional organosiloxane can provide one or more of the following effects: 1) faster curing of adhesive composition (when compared with the equivalent adhesive composition that does not contain clustered functional organosiloxane a' above), and 2) improved tensile and elongation properties of adhesive prepared by curing adhesive composition, and / or 3) improved crosslinkability of adhesive composition.
[0032] curable composition The above-described products, a) the polyfunctional organohydrogensiloxane and a') the clustered functional organosiloxane, are useful in a curable composition, the curable composition comprising: (I) one or more of the products described above: a) multifunctional organohydrogensiloxanes and a') clustered functional organosiloxanes; (II) a curing agent.
[0033] The curing agent selected depends on the type and amount of the curable substituent in the starting material (I). For example, when a) a polyfunctional organohydrogensiloxane is included in the curable composition, and / or when a') a clustered functional organosiloxane has SiH functional group in addition to the curable group introduced by the starting material c) reactive species in the method of functionalizing the polyfunctional organohydrogensiloxane as described above, the curable substituent may be SiH, for example. Alternatively, the curable substituent may be the curable group introduced by using the starting material c) to prepare a') a clustered functional organosiloxane as described above.
[0034] For example, when starting material (I) has SiH functionality, (II) the curing agent may be a hydrosilylation reaction catalyst, as exemplified by those described above for starting material b) in the method for functionalizing a polyfunctional organohydrogensiloxane described above.
[0035] For example, when the starting material (I) comprises a') clustered functional organosiloxane having radical curable groups (such as organic groups having epoxy, acrylate, or methacrylate functional groups), the curing agent may comprise a radical initiator as the curing agent (II). The radical initiator may be a thermal radical initiator, a radiation radical initiator, or a redox reagent. Thermal radical initiators include peroxides, which are known in the art and commercially available as disclosed in U.S. Pat. No. 9,593,209, column 16, line 49 to column 17, line 26. Thermal radical initiators may be used in amounts of 0.01% to 15% by weight, alternatively 0.1% to 5% by weight, alternatively 0.1% to 2% by weight, based on the total weight of all starting materials in the curable composition.
[0036] Alternatively, the radical initiator may be a radiation photoinitiator. Radiation photoinitiators are known in the art and include cationic photoinitiators such as onium salts, and radiation photoinitiators are disclosed in U.S. Pat. No. 9,593,209, column 17, line 27 to column 18, line 40. Suitable radiation photoinitiators may be present in the curable composition in an amount of 0.01% to 15% by weight, alternatively 0.1% to 10% by weight, alternatively 0.1% to 5% by weight, alternatively 0.1% to 2% by weight, based on the total weight of all starting materials in the curable composition.
[0037] Alternatively, the radical initiator may be a redox reagent such as those disclosed in US Pat. No. 9,593,209, column 21, lines 33-53.
[0038] Alternatively, when the starting material (I) comprises a') a clustered functional organosiloxane having an organic group with OH, alkoxy, or other hydrolyzable groups, the curing agent (II) may comprise a condensation reaction catalyst in an amount of 0.001% to 5% by weight based on the total weight of all starting materials in the curable composition. Exemplary condensation reaction catalysts are those disclosed in U.S. Patent No. 9,593,209, column 18, line 41 to column 19, line 15.
[0039] Alternatively, when the starting material (I) comprises a') a clustered functional organosiloxane, the curing agent (II) may comprise an organoborane amine complex. Suitable organoborane amine complexes are disclosed, for example, in U.S. Patent No. 9,593,209, column 19, line 16 to column 21, line 33.
[0040] Alternatively, when the starting material (I) comprises a') a clustered functional organosiloxane having an organic group with an isocyanate or urethane functionality, the (II) curing agent may comprise a compound having two or more carbinol groups, such as a polyol, or an amine-functional compound. Examples of such curing agents are disclosed in column 21, lines 54 to 63.
[0041] Alternatively, when starting material (I) has two or more types of curing substituents, two or more types of curing agents can be used as starting material (II) in the curable composition. For example, a combination of a radical initiator and a condensation reaction catalyst can be used when starting material (I) has both radical curing groups and condensation reaction curing groups, such as both epoxy and alkoxy. Alternatively, a combination of a hydrosilylation reaction catalyst and a condensation reaction catalyst can be used when starting material (I) has both SiH functional groups and condensation reaction curing groups such as alkoxy.
[0042] The curable composition may optionally further comprise one or more additional starting materials. These are exemplified by (III) crosslinkers, (IV) solvents, (V) adhesion promoters, (VI) colorants, (VII) reactive diluents, (VIII) corrosion inhibitors, (IX) polymerization inhibitors, (X) fillers, (XI) filler treating agents, (XII) acid acceptors, and combinations thereof. Suitable additional starting materials are described and exemplified as other optional components in U.S. Pat. No. 9,592,209, column 22, line 5 to column 29, line 8. Other additional starting materials can be added. For example, the curable composition may optionally further comprise (XIII) reactive resins and polymers, (XIV) dual cure compounds, or both. (XIII) reactive resins and polymers for starting materials are known in the art, see, for example, U.S. Pat. No. 9,670,392, column 16, line 21 to column 18, line 35.
[0043] Thermally radically curable composition The curable composition may be a thermally radically curable composition. The thermally radically curable composition can be prepared as described in U.S. Pat. No. 9,670,392 by replacing the clustered functional organosiloxane described therein as component (I) with the clustered functional organosiloxane prepared as described for starting material a') above. The thermally radically curable composition is (I) a clustered functional organosiloxane as described above as starting material a') or a product containing a clustered functional organosiloxane a'), (II) a curing agent, (a) a radical initiator, and (b) a curing agent comprising a condensation reaction catalyst; (III) a crosslinking agent; (XIII) reactive resins and polymers.
[0044] The thermal radical cure composition may further comprise (XIV) a dual cure compound, which is an organosilicon compound having both hydrolyzable groups and free radical reactive groups, (VIII) a corrosion inhibitor, and (V) an adhesion promoter, all of whose starting materials are described above.
[0045] Adhesive Composition Alternatively, the curable composition may be an adhesive composition. A) a clustered functional organosiloxane as described above as starting material a') or a product containing a clustered functional organosiloxane a'), the clustered functional organosiloxane having acrylate, epoxy and / or methacrylate functional groups; B) reactive resins and polymers; C) a condensation reaction catalyst; D) a free radical initiator.
[0046] Starting Materials B) Reactive Resins and Polymers The starting material B) in the adhesive composition is a reactive resin and polymer. The reactive resin and polymer may be the reactive resin and polymer (XIII) described above as starting materials, see U.S. Pat. No. 9,670,392. Alternatively, the reactive resin and polymer may be a polyalkoxy end-capped resin-polymer blend prepared as described in U.S. Provisional Patent Application No. 62 / 548558, filed Aug. 22, 2017. The polyalkoxy end-capped resin-polymer blend may be: i) Formula, (R 2’ 3SiO 1 / 2 ) and (SiO 4 / 2 )[where each R 2’ are independently monovalent hydrocarbon groups, provided that at least one R 2’ has aliphatic unsaturation] units in the range of 0.5:1 to 1.5:1 (R 2’ 3SiO 1 / 2 ) units (M units), (SiO 4 / 2a siloxane resin having a molar ratio (M:Q ratio) of 1,2,3,4,5,6,7,8,9,10,11,12,13,14,15,16,17,18,19,19,20,21,22,19 ii) Formula, (R 2’ 3SiO 1 / 2 ) ii and (R 2’ 2SiO 2 / 2 ) hh (D units), wherein subscript hh is 20 to 1000, and subscript ii has an average value of 2; iii) an alkoxy-functional organohydrogensiloxane oligomer having the unit formula: [ka] zzzImage12zzz (HR 22 2SiO 1 / 2 ) ppp (R 22 3SiO 1 / 2 ) qqq (HR 22 SiO 2 / 2 ) rrr (R 22 2SiO 2 / 2 ) sss (R 22 SiO 3 / 2 ) ttt (HSiO 3 / 2 ) uuu (SiO 4 / 2 ) kk [In the formula, each D 1 each independently represents a divalent hydrocarbon group having 2 to 18 carbon atoms; 22 are independently a monovalent hydrocarbon group having 1 to 18 carbon atoms or a monovalent halogenated hydrocarbon group having 1 to 18 carbon atoms (R 1 (such as those described above for R 23 are independently monovalent hydrocarbon radicals having 1 to 18 carbon atoms (R 1the subscript nnn is 0 or 1, the subscript ooo is 0, the subscripts qqq, sss, and ttt are such that 5≧qqq≧0, 5≧sss≧0, the subscript ttt is 0 or 1, the subscript kk is 0 or 1, the subscript nnn>0, and the quantity (mmm+ppp+qqq+rrr+sss+ttt+uuu+kk)≦50, with the proviso that 1 >90 mole % of the groups are linear; and iv) A hydrosilylation reaction catalyst and a reaction product of each D 1 is an alkylene group, such as ethylene, propylene, butylene, or hexylene; an arylene group, such as phenylene; or an alkylarylene group, such as [ka] zzzImage13zzz Alternatively, each D 1 is an alkylene group, such as ethylene or propylene, alternatively ethylene.
[0047] Starting material C) Condensation reaction catalyst The starting material C) in the adhesive composition described above is a condensation catalyst. The condensation catalyst may be selected from conventional condensation catalysts effective for silanol-silanol condensation reactions, including organometallic compounds, amines, and a wide range of organic and inorganic bases and acids. Organometallic compounds include tin, titanium, zinc, zirconium, hafnium, and other organic compounds. The condensation catalyst may be organotin and organotitanium compounds. Exemplary organotin compounds include a) stannous salts of carboxylic acids, such as i) dibutyltin dilaurate, ii) dimethyltin dilaurate, iii) di-(n-butyl)tin bisketonate, iv) dibutyltin diacetate, v) dibutyltin maleate, vi) dibutyltin diacetylacetonate, vii) dibutyltin dimethoxide, viii) carbomethoxyphenyltin tris-uberate, ix) dibutyltin dilaurate ... tin dioctanoate, x) dibutyltin diformate, xi) isobutyltin triceroate, xii) dimethyltin dibutyrate, xiii) dimethyltin dineodeconoate, xiv) dibutyltin dineodeconoate, xv) triethyltin tartrate, xvi) dibutyltin dibenzoate, xvii) butyltin tri-2-ethylhexanoate, xviii) dioctyltin diacetate, xix) b) stannous salts of organic carboxylic acids such as xxiv) stannous diacetate, xxv) stannous dioctanoate, xxvi) stannous diethylhexanoate, xxvii) stannous dilaurate; c) stannous salts of carboxylic acids such as xxviii) stannous octoate, xxix) stannous oleate, xxx) stannous acetate, xxxi) stannous laurate, xxxii) stannous stearate, xxxiii) stannous naphthenate, xxxiv) stannous hexanoate, xxxv) stannous succinate, xxxvi) stannous caprylate; and d) combinations of two or more of i)-xxxvi).Exemplary organotitanium compounds may be selected from the group consisting of i) tetra-n-butyl titanate, ii) tetraisopropyl titanate, iii) tetra-t-butyl titanate, iv) tetrakis(2-ethylhexyl) titanate, v) acetylacetonate titanate chelate, vi) ethylacetoacetate titanate chelate, vii) triethanolamine titanate chelate, viii) tri-n-butyl titanate, and ix) combinations of two or more of i), ii), iii), iv), v), vi), vii), and vii).
[0048] The amount of condensation reaction catalyst in the adhesive composition will vary depending on a variety of factors, such as the selection of other starting materials, whether any additional starting materials are added, and the end use of the adhesive composition. However, the condensation reaction catalyst may be present in an amount ranging from 0.01% to 25% by weight, based on the total weight of all starting materials in the adhesive composition. Alternatively, the condensation reaction catalyst may be present in an amount of 0.1% to 25%, alternatively 0.1% to 15%, alternatively 0.5% to 15%, alternatively 0.5% to 10%, alternatively 0.1% to 5%.
[0049] Starting Material D) Free Radical Initiator The starting material D) in the adhesive composition described above is a free radical initiator. The free radical initiator may include an azo compound or an organic peroxide compound. Suitable azo compounds include azobenzene, azobenzene-p-sulfonic acid, azobisdimethylvaleronitrile, azobisisobutyronitrile, and combinations thereof. Suitable organic peroxide compounds include dialkyl peroxides, diaryl peroxides, diacyl peroxides, alkyl hydroperoxides, and aryl hydroperoxides. Specific organic peroxide compounds are as described above for starting material (II). Alternatively, the organic peroxide may be exemplified by benzoyl peroxide; dibenzoyl peroxide; 4-monochlorobenzoyl peroxide; dicumyl peroxide; tert-butyl peroxybenzoate; tert-butylcumyl peroxide; tert-butyl oxide 2,5-dimethyl-2,5-di-tert-butylperoxyhexane; 2,4-dichlorobenzoyl peroxide; di-tert-butylperoxy-diisopropylbenzene; 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane; 2,5-di-tert-butylperoxyhexane-3,2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; cumyl-tert-butyl peroxide; or a combination of two or more thereof.
[0050] The amount of free radical initiator added to the adhesive composition will vary depending on a variety of factors, such as the type and amount of condensation reaction catalyst selected, as well as the selection of other starting materials in the adhesive composition, but the free radical initiator may be present in an amount of from 0.1 wt % to 5 wt %, alternatively from 0.2 wt % to 3 wt %, alternatively from 0.5 wt % to 2 wt %, based on the total weight of all starting materials in the adhesive composition.
[0051] Additional Starting Materials in the Adhesive Composition The adhesive composition described above may further comprise one or more additional starting materials (different from and added in addition to the above-mentioned starting materials A), B), C) and D). The additional starting materials may be selected from the group consisting of E) dual cure compounds, F) adhesion promoters, G) corrosion inhibitors, H) rheology modifiers, I) drying agents, J) crosslinkers, K) fillers, L) spacers, M) acid scavengers, N) silanol-functional polydiorganosiloxanes, O) fluorescent optical brighteners, P) chain transfer agents, Q) (meth)acrylate monomers, R) polyalkoxy-terminated polydiorganosiloxanes, S) colorants, and two or more of E), F), G), H), I), J), K), L), M), N), O), P), Q), R), and S).
[0052] Starting Material E) Dual Cure Compound The adhesive composition described above may optionally further comprise starting material E) a dual cure compound. The dual cure compound is an organosilicon compound having at least one hydrolyzable group and at least one free radical reactive group in one molecule. The organosilicon compound of starting material E) has the formula: 14 mm R 22 nn Six (4-mm-nn) [In the formula, R 22 is as described above, and R 14 is a curable group (such as an acrylate, epoxy, or methacrylate functional group), X is a hydrolyzable group, the subscript mm is 1-2, the subscript nn is 0-2, and the quantity (mm+nn) is 2-3.
[0053] Each X independently represents a hydrolyzable group that may be selected from an acetamido group, an acyloxy group such as acetoxy, an alkoxy group, an amido group, an amino group, an aminoxy group, an oximo group, a ketoximo group, and a methylacetamido group. X is not a hydroxyl group. Alternatively, each X may be an acetoxy group or an alkoxy group. Alternatively, each X is an alkoxy group such as methoxy, ethoxy, propoxy, or butoxy, or is methoxy.
[0054] Alternatively, the organosilicon compound starting material E) may have the unit formula: (X mm R 22 (3-mm) SiO 1 / 2 ) oo (R 14 R 22 2SiO 1 / 2 ) pp (R 22 2SiO 2 / 2 ) qq (R 22 XSiO 2 / 2 ) rr (R 14 R 22 SiO 2 / 2 ) ss (R 14 SiO 3 / 2 ) ww (R 22 SiO 3 / 2 ) tt (SiO 4 / 2 ) uu [In the formula, R 22 , R 14, and X, and the subscript mm are as described above, with the subscript oo≧0, the subscript pp≧0, the subscript qq≧0, the subscript rr≧0, the subscript ss≧0, the subscript ww≧0, the subscript tt≧0, and the subscript uu≧0, with the proviso that the quantity (oo+rr)≧1, the quantity (pp+ss+ww)≧1, and the quantity (oo+pp+qq+rr+ss+ww+tt+uu)>2. Alternatively, the subscript oo is 0-100, alternatively 0-50, alternatively 0-20, alternatively 0-10, alternatively 1-50, alternatively 1-20, or alternatively 1-10. Alternatively, the subscript pp may be 0-100, alternatively 0-50, alternatively 0-20, alternatively 0-10, alternatively 1-50, alternatively 1-20, or alternatively 1-10. Alternatively, the subscript qq is 0 to 1,000, or 0 to 500, or 0 to 200, or 0 to 100, or 1 to 500, or 1 to 200, or 1 to 100. Alternatively, the subscript rr is 0 to 100, or 0 to 50, or 0 to 20, or 0 to 10, or 1 to 50, or 1 to 20, or 1 to 10. Alternatively, the subscript ss is 0 to 100, or 0 to 50, or 0 to 20, or 0 to 10, or 1 to 50, or 1 to 20, or 1 to 10. Alternatively, the subscript ww is 0 to 100, or 0 to 50, or 0 to 20, or 0 to 10, or 1 to 50, or 1 to 20, or 1 to 10. Alternatively, the subscript tt is 0 to 1,000, or 0 to 500, or 0 to 200, or 0 to 100, or 1 to 500, or 1 to 200, or 1 to 100. Alternatively, the subscript uu is 0 to 1,000, or 0 to 500, or 0 to 200, or 0 to 100, or 1 to 500, or 1 to 200, or 1 to 100.
[0055] Examples of starting materials E) include silanes such as methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane, acryloxypropyltriethoxysilane, methacryloxypropyltriethoxysilane, methacryloxypropylmethyldimethoxysilane, acryloxypropylmethyldimethoxysilane, acryloxypropyldimethylmethoxysilane, and methacryloxypropyldimethylmethoxysilane.
[0056] The amount of the dual cure compound in the adhesive composition will vary depending on a variety of factors, such as the selection of other starting materials, whether any additional starting materials are added, and the end use of the composition. However, the dual cure compound may be present in an amount ranging from 0.01% to 25% by weight, based on the total weight of all starting materials in the adhesive composition. Alternatively, the dual cure compound may be present in an amount of 0.1% to 25%, alternatively 0.1% to 15%, alternatively 0.5% to 15%, alternatively 0.5% to 10%, alternatively 0.1% to 5%.
[0057] Starting Material F) Adhesion Promoter The adhesive composition described above may optionally further comprise F) an adhesion promoter. Suitable adhesion promoters may include transition metal chelates, hydrocarbonoxysilanes, such as alkoxysilanes, combinations of alkoxysilanes and hydroxy-functional polyorganosiloxanes, amino-functional silanes, or combinations thereof. The adhesion promoter may be represented by the formula: 15 aaa R 16 bbb Si(OR 17 ) 4-(aaa+bbb) [In the formula, each R 15 are independently monovalent organic groups having at least 3 carbon atoms; R 16 contains at least one SiC-bonding substituent having an adhesion-promoting group, such as an amino group, an epoxy group, a mercapto group, or an acrylate group; 17are independently a saturated hydrocarbon group, such as an alkyl group having 1 to 4 carbon atoms; the subscript aaa has a value ranging from 0 to 2; and the subscript bbb is either 1 or 2, with the quantity (aaa+bbb) being 3 or less. Alternatively, the adhesion promoter may comprise a partial condensate of the above-mentioned silanes. Alternatively, the adhesion promoter may comprise a combination of an alkoxysilane and a hydroxy-functional polyorganosiloxane, such as trimethoxysilyl-terminated polydimethylsiloxane, which is commercially available from Dow Silicones Corporation (Midland, Michigan, USA).
[0058] Alternatively, the adhesion promoter may comprise an unsaturated or epoxy functional compound. The adhesion promoter may comprise an unsaturated or epoxy functional alkoxysilane. For example, the functional alkoxysilane may be represented by the formula: 18 ccc Si(OR 19 ) (4-ccc) wherein the subscript ccc is 1, 2, or 3, or the subscript ccc is 1. 18 are independently monovalent organic groups, provided that at least one R 18 R is an unsaturated organic group or an epoxy-functional organic group. 18 The epoxy-functional organic groups are exemplified by 3-glycidoxypropyl and (epoxycyclohexyl)ethyl. 18 The unsaturated organic groups of R are exemplified by 3-methacryloyloxypropyl, 3-acryloyloxypropyl, and unsaturated monovalent hydrocarbon groups such as vinyl, allyl, hexenyl, undecylenyl, and the like. 19 R is independently a saturated hydrocarbon group having 1 to 4 carbon atoms, or 1 to 2 carbon atoms. 19 is exemplified by methyl, ethyl, propyl, and butyl.
[0059] Examples of suitable epoxy-functional alkoxysilanes include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, (epoxycyclohexyl)ethyldimethoxysilane, (epoxycyclohexyl)ethyldiethoxysilane, (epoxycyclohexyl)ethyltrimethoxysilane, such as β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, (epoxycyclohexyl)ethyltriethoxysilane, and combinations thereof. Examples of suitable unsaturated alkoxysilanes include vinyltrimethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, hexenyltrimethoxysilane, undecylenyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltriethoxysilane, and combinations thereof.
[0060] Alternatively, the adhesion promoter may comprise an epoxy-functional siloxane, such as the reaction product of a hydroxy-terminated polyorganosiloxane and an epoxy-functional alkoxysilane as described above, or a physical blend of a hydroxy-terminated polyorganosiloxane and an epoxy-functional alkoxysilane. The adhesion promoter may comprise a combination of an epoxy-functional alkoxysilane and an epoxy-functional siloxane. For example, the adhesion promoter is exemplified by a mixture of 3-glycidoxypropyltrimethoxysilane and a reaction product of a hydroxy-terminated methylvinylsiloxane and a 3-glycidoxypropyltrimethoxysilane, or a mixture of 3-glycidoxypropyltrimethoxysilane and a hydroxy-terminated methylvinylsiloxane, or a mixture of 3-glycidoxypropyltrimethoxysilane and a hydroxy-terminated methylvinyl / dimethylsiloxane copolymer.
[0061] Alternatively, the adhesion promoter may be H2N(CH2)2Si(OCH3)3, H2N(CH2)2Si(OCH2CH3)3, 3-aminopropyltrimethoxysilane of formula H2N(CH2)3Si(OCH2CH3)3, H2N(CH2)3Si(OCH2CH3)3, CH3NH(CH2)3Si(OCH3)3, CH3NH(CH2)3Si(OCH2CH3)3, CH3NH(CH2)5Si(OCH3)3, CH3NH(CH2)5Si(OCH2CH3)3, H2N( CH2)2NH(CH2)3Si(OCH3)3, H2N(CH2)2NH(CH2)3Si(OCH2CH3)3, CH3NH(CH2)2NH(CH2)3Si(OCH3)3, CH3NH(CH2)2NH(CH2)3Si( OCH2CH3)3, C4H9NH(CH2)2NH(CH2)3Si(OCH3)3, C4H9NH(CH2)2NH(CH2)3Si(OCH2CH3)3, H2N(CH2)2SiCH3(OCH3)2, H2N(CH2)2S iCH3(OCH2CH3)2, H2N(CH2)3SiCH3(OCH3)2, H2N(CH2)3SiCH3(OCH2CH3)2, CH3NH(CH2)3SiCH3(OCH3)2, CH3NH(CH2)3SiCH3(O CH2CH3)2, CH3NH(CH2)5SiCH3(OCH3)2, CH3NH(CH2)5SiCH3(OCH2CH3)2, H2N(CH2)2NH(CH2)3SiCH3(OCH3)2, H2N(CH2)2NH(CH 2) may include amino-functional silanes, such as amino-functional alkoxysilanes exemplified by 3SiCH3(OCH2CH3)2, CH3NH(CH2)2NH(CH2)3SiCH3(OCH3)2, CH3NH(CH2)2NH(CH2)3SiCH3(OCH2CH3)2, C4H9NH(CH2)2NH(CH2)3SiCH3(OCH3)2, C4H9NH(CH2)2NH(CH2)3SiCH3(OCH2CH3)2, and combinations thereof.
[0062] Alternatively, the adhesion promoter may comprise a transition metal chelate. Suitable transition metal chelates include titanates, zirconates such as zirconium acetylacetonate, aluminum chelates such as aluminum acetylacetonate, and combinations thereof.
[0063] Alternatively, the adhesion promoter may comprise a triazine-based compound having a functional group that reacts with starting material A), starting material B), or starting material E), if present, or two or more of these. The triazine ring may be mono-, di-, or tri-substituted, with at least one of the substituents being a reactive functional group. The functional group may be free radical reactive or condensation reactive. Examples of triazine compounds having free radical reactive functional groups include triallyl isocyanurate, diallylpropyl isocyanurate, tri-(methacryloxypropyl)isocyanurate, triallyloxytriazine, trimethacryloxytriazine, triacryloylhexahydrotriazine, and tris[2-(acryloyloxy)ethyl]isocyanurate. Examples of triazine compounds having condensation reactive groups include 2,4,6-tris(methyldimethoxysilyl)triazine, tris[3-(trimethoxysilyl)propyl]isocyanurate.
[0064] The exact amount of adhesion promoter will vary depending on a variety of factors, such as the choice and amount of other starting materials in the adhesive composition. However, when present, the adhesion promoter can be added to the adhesive composition in an amount of 0.01 to 50 parts by weight, alternatively 0.01 to 10 parts by weight, alternatively 0.01 to 5 parts by weight, based on the total weight of all starting materials in the adhesive composition. Examples of suitable adhesion promoters are described in U.S. Patent No. 9,156,948.
[0065] Starting material G) Corrosion inhibitor The adhesive composition may optionally further comprise starting material G) corrosion inhibitor. Examples of suitable corrosion inhibitors include benzotriazole, mercaptobenzothiazole, mercaptobenzotriazole, and commercially available corrosion inhibitors such as 2-mercaptobenzothiazole from Millipore Sigma, 2,5-dimercapto-1,3,4-thiadiazole derivative (CUVAN® 826) and alkyl thiadiazole (CUVAN® 484) from RT Vanderbilt (Norwalk, Connecticut, USA). Examples of suitable corrosion inhibitors are exemplified by those described in U.S. Pat. No. 9,156,948. When present, the amount of corrosion inhibitor may be 0.05% to 0.5% by weight, based on the total weight of all starting materials in the adhesive composition.
[0066] Starting Material H) Rheology Modifier The adhesive composition may optionally further comprise up to 5% by weight, alternatively 1% to 2% by weight, of starting material H) rheology modifier, based on the total weight of all starting materials in the composition. Rheology modifiers are commercially available. Examples of suitable rheology modifiers include polyamides, hydrogenated castor oil derivatives, metal soaps, microcrystalline waxes, and combinations thereof. Examples of suitable rheology modifiers are exemplified by those described in U.S. Pat. No. 9,156,948. The amount of rheology modifier will vary depending on a variety of factors, including the particular rheology modifier selected and the selection of other starting materials used in the composition. However, the amount of rheology modifier may be 0 parts by weight to 20 parts by weight, alternatively 1 part by weight to 15 parts by weight, alternatively 1 part by weight to 5 parts by weight, based on the total weight of all starting materials in the adhesive composition.
[0067] Starting Materials I) Desiccant The above-mentioned composition may optionally further comprise a starting material I) a desiccant. The desiccant captures water from various sources. For example, the desiccant may capture the by-products of the condensation reaction, such as water and alcohol. Examples of suitable desiccants are disclosed, for example, in U.S. Pat. No. 9,156,948. Examples of adsorbents suitable for the desiccant may be inorganic particulates, such as zeolites, such as chabazite, mordenite, and analcite; molecular sieves, such as alkali metal aluminosilicates, silica gel, silica magnesia gel, activated carbon, activated alumina, calcium oxide, and combinations thereof. The adsorbent may have a particle size of 10 μm or less. The adsorbent may have an average pore size sufficient to adsorb water and alcohol, for example, 10 Å (angstroms) or less.
[0068] Alternatively, the desiccant can scavenge water and / or other by-products by chemical means. The amount of silane crosslinker added to the composition (in addition to any silane crosslinker used as starting material J) is capable of functioning as a chemical desiccant. Without being bound by theory, it is believed that a chemical desiccant can be added to the dry part of a multi-part composition to keep the composition from contacting water after the parts of the composition are mixed together. For example, alkoxysilanes suitable as desiccants include vinyltrimethoxysilane, vinyltriethoxysilane, methyltrimethoxysilane, isobutyltrimethoxysilane, and combinations thereof. The amount of desiccant will vary depending on the particular desiccant selected. However, when starting material I) is a chemical desiccant, the amount may range from 0 parts by weight to 15 parts by weight, alternatively from 0 parts by weight to 10 parts by weight, alternatively from 0 parts by weight to 5 parts by weight, alternatively from 0 parts by weight to 0.5 parts by weight, based on the total weight of all starting materials in the composition.
[0069] Starting material J) - Crosslinker The above-mentioned compositions may optionally further comprise starting material J) a crosslinker. The crosslinker may comprise a silane crosslinker having hydrolyzable groups or a partial or complete hydrolysis product thereof. The crosslinker has, on average, more than two substituents in one molecule that are reactive with the hydrolyzable groups of starting material B). Examples of suitable silane crosslinkers are those having the general formula R 20 ddd Si(R 21 ) (4-ddd) [In the formula, each R 20 are independently a monovalent hydrocarbon group, such as an alkyl group; 21 is a hydrolyzable substituent, which may be the same group as X described above. Alternatively, each R 21 may be, for example, a hydrogen atom, a halogen atom, an acetamido group, an acyloxy group such as acetoxy, an alkoxy group, an amido group, an amino group, an aminoxy group, a hydroxyl group, an oximo group, a ketoximo group, or a methylacetamido group, and each instance of the subscript ii may be 0, 1, 2, or 3. For silane crosslinkers, the subscript ddd has an average value greater than 2. Alternatively, the subscript ddd may have a value in the range of 3 to 4. Alternatively, each R 21 may be independently selected from hydroxyl, alkoxy, acetoxy, amide, or oxime. Alternatively, the silane crosslinker may be selected from acyloxysilanes, alkoxysilanes, ketoximosilanes, and oximosilanes.
[0070] The silane crosslinker may include an alkoxysilane, for example, a dialkoxysilane, such as a dialkyl dialkoxysilane; a trialkoxysilane, such as an alkyl trialkoxysilane; a tetraalkoxysilane; or a partial or complete hydrolysis product thereof, or another combination thereof. Examples of suitable trialkoxysilanes include methyl trimethoxysilane, methyl triethoxysilane, ethyl trimethoxysilane, ethyl triethoxysilane, isobutyl trimethoxysilane, isobutyl triethoxysilane, and combinations thereof, or methyl trimethoxysilane. Examples of suitable tetraalkoxysilanes include tetraethoxysilane. Alternatively, the silane crosslinker may include an acyloxysilane, such as acetoxysilane. The acetoxysilanes include tetraacetoxysilane, organo triacetoxysilane, diorgano diacetoxysilane, or combinations thereof. Exemplary acetoxysilanes include, but are not limited to, tetraacetoxysilane, methyltriacetoxysilane, ethyltriacetoxysilane, vinyltriacetoxysilane, propyltriacetoxysilane, butyltriacetoxysilane, phenyltriacetoxysilane, octyltriacetoxysilane, dimethyldiacetoxysilane, phenylmethyldiacetoxysilane, vinylmethyldiacetoxysilane, diphenyldiacetoxysilane, tetraacetoxysilane, and combinations thereof. Alternatively, the crosslinker may include an organotriacetoxysilane, such as a mixture comprising methyltriacetoxysilane and ethyltriacetoxysilane. Examples of silanes suitable for starting material J) containing both alkoxy and acetoxy groups that can be used in the composition include methyldiacetoxymethoxysilane, methylacetoxydimethoxysilane, vinyldiacetoxymethoxysilane, vinylacetoxydimethoxysilane, methyldiacetoxyethoxysilane, methylacetoxydiethoxysilane, and combinations thereof.
[0071] Alternatively, the crosslinker may be H2N(CH2)2Si(OCH3)3, H2N(CH2)2Si(OCH2CH3)3, H2N(CH2)3Si(OCH3)3, H2N(CH2)3Si(OCH2CH3)3, CH3NH(CH2)3Si(OCH3)3, CH3NH(CH2)3Si(OCH2CH3)3, CH3NH(CH2)5Si(OCH3)3, CH3NH(CH2)5Si(OCH2CH3)3, H2N(CH2)2NH(CH2)3 Si(OCH3)3, H2N(CH2)2NH(CH2)3Si(OCH2CH3)3, CH3NH(CH2)2NH(CH2)3Si(OCH3)3, CH3NH(CH2)2NH(CH2)3Si(OCH2CH3)3 , C4H9NH(CH2)2NH(CH2)3Si(OCH3)3, C4H9NH(CH2)2NH(CH2)3Si(OCH2CH3)3, H2N(CH2)2SiCH3(OCH3)2, H2N(CH2)2SiCH3 (OCH2CH3)2, H2N(CH2)3SiCH3(OCH3)2, H2N(CH2)3SiCH3(OCH2CH3)2, CH3NH(CH2)3SiCH3(OCH3)2, CH3NH(CH2)3SiCH3( OCH2CH3)2, CH3NH(CH2)5SiCH3(OCH3)2, CH3NH(CH2)5SiCH3(OCH2CH3)2, H2N(CH2)2NH(CH2)3SiCH3(OCH3)2, H2N(CH2)2 The silane crosslinker may include amino functional groups such as NH(CH2)3SiCH3(OCH2CH3)2, CH3NH(CH2)2NH(CH2)3SiCH3(OCH3)2, CH3NH(CH2)2NH(CH2)3SiCH3(OCH2CH3)2, C4H9NH(CH2)2NH(CH2)3SiCH3(OCH3)2, C4H9NH(CH2)2NH(CH2)3SiCH3(OCH2CH3)2, or combinations thereof, and combinations thereof. Examples of suitable silane crosslinkers are disclosed in U.S. Pat. No. 9,156,948.
[0072] Alternatively, the crosslinker may comprise a multifunctional (meth)acrylate crosslinker, such as, for example, a di(meth)acrylate, exemplified by ethylene glycol dimethacrylate, ethylene glycol diacrylate, triethylene glycol dimethacrylate, diethylene glycol bismethacryloxycarbonate, polyethylene glycol diacrylate, tetraethylene glycol dimethacrylate, diglycerol diacrylate, diethylene glycol dimethacrylate, pentaerythritol triacrylate, trimethylolpropane triglycidyl ether, trimethylolpropane tris(2-methyl-1-aziridine)propionate, trimethylolpropane trimethacrylate, acrylate-tipped urethane-containing prepolymers, polyether diacrylates, and dimethacrylates, and combinations of two or more thereof. Suitable multifunctional (meth)acrylate crosslinkers are disclosed, for example, in U.S. Pat. No. 8,304,543, column 11, lines 46-65.
[0073] When present, the crosslinker may be added in an amount ranging from 0.1% to 10% by weight, based on the total weight of all starting materials in the adhesive composition.
[0074] Starting material K) filler The above-mentioned compositions may optionally further comprise a filler (K). The filler may comprise a reinforcing filler, an extending filler, a conductive filler, or a combination thereof. For example, the composition may optionally further comprise a starting material (K1) reinforcing filler, which, if present, may be added in an amount of 0.1% to 95% by weight, alternatively 1% to 60% by weight, based on the total weight of all starting materials in the adhesive composition. The exact amount of starting material (K1) will vary depending on various factors, such as the form of the reaction product of the composition and whether other fillers are added. Examples of suitable reinforcing fillers include reinforcing silica fillers (e.g., fumed silica, silica aerogel, silica xerogel, and precipitated silica). Fumed silica is known in the art and is commercially available, for example, fumed silica sold under the name CAB-O-SIL by Cabot Corporation (Massachusetts, USA).
[0075] The adhesive composition may optionally further comprise starting material (K2) extending filler in an amount ranging from 0.1% to 95% by weight, alternatively from 1% to 60% by weight, alternatively from 1% to 20% by weight, based on the total weight of all starting materials in the adhesive composition. Examples of extending fillers include crushed quartz, aluminum oxide, magnesium oxide, calcium carbonate (e.g., precipitated calcium carbonate), zinc oxide, talc, diatomaceous earth, iron oxide, clay, mica, chalk, titanium dioxide, zirconia, sand, carbon black, graphite, or combinations thereof. Extending fillers are known in the art and are commercially available, for example, ground silica sold under the name MIN-U-SIL by US Silica (Berkeley Springs, WV). Suitable precipitated calcium carbonates include Winnofil™ SPM from Solvay, and Ultrapflex™ and Ultrapflex™ 100 from SMI. Examples of suitable fillers are disclosed in US Pat. No. 9,156,948.
[0076] Starting material L) Spacer The adhesive composition described above may optionally further comprise a spacer (L). The spacer may comprise organic particles, inorganic particles or a combination thereof. The spacer may be thermally conductive, electrically conductive, or both. The spacer may have a desired particle size, for example, a particle size range of 25 μm to 125 μm. The spacer may comprise monodisperse beads, such as glass or polymer (e.g., polystyrene) beads. The spacer may comprise thermally conductive fillers, such as alumina, aluminum nitride, atomized metal powder, boron nitride, copper and silver. The amount of spacer varies depending on various factors, such as particle size distribution, pressure applied during use of the composition prepared by mixing the parts or the cured product prepared therefrom, temperature during use, and the desired thickness of the mixed composition or the cured product prepared therefrom. However, the composition may comprise the spacer in an amount of 0.05% to 2% by weight, alternatively 0.1% to 1% by weight, based on the total weight of all starting materials in the composition.
[0077] Starting material M) Acid scavenger The above-mentioned compositions may optionally further comprise M) an acid scavenger. Suitable acid scavengers include various inorganic and organic compounds that are basic in nature, such as magnesium oxide, calcium oxide, and combinations thereof. The composition may comprise 0% to 10% by weight of an acid scavenger, based on the total weight of all starting materials in the composition.
[0078] Starting Material N) Silanol-Functional Polydiorganosiloxane The above-described composition may optionally further comprise N) a silanol-functional polydiorganosiloxane. The starting material N) is represented by the formula: HOR 22 2SiO(R 22 2SiO) eee ((HO)R 22 SiO) fff SiR 22 2OH or formula, R3SiO(R2SiO) ggg ((HO)RSiO) hhh SiR3[wherein, R 22are as described above], or combinations thereof. The subscript eee may be zero or a positive number. Alternatively, the subscript eee has an average value of at least 2. Alternatively, the subscript eee may be from 2 to 2000. The subscript fff may be zero or a positive number. Alternatively, the subscript fff may have an average value of 0 to 2000. The subscript ggg may be zero or a positive number. Alternatively, the subscript ggg may have an average value of 0 to 2000. The subscript hhh has an average value of at least 2. Alternatively, the subscript hhh may have an average value in the range of 2 to 2000.
[0079] Starting materials N) are polydiorganosiloxanes, e.g. i) hydroxy-terminated polydimethylsiloxane; ii) hydroxy-terminated poly(dimethylsiloxane / methylphenylsiloxane); iii) trimethylsiloxy-terminated poly(dimethylsiloxane / methylhydroxysiloxane), and iv) may include a combination of two or more of i), ii), and iii).
[0080] Hydroxyl endblocked polydiorganosiloxanes suitable for use as starting material N) can be prepared by methods known in the art, such as hydrolysis and condensation of the corresponding organohalosilanes or equilibration of cyclic polydiorganosiloxanes. When added to the adhesive composition, starting material N) may be present in an amount of 0.1% to 20% by weight, alternatively 0.1% to 10% by weight, alternatively 0.1% to 5% by weight, based on the total weight of all starting materials in the adhesive composition.
[0081] Starting material O) Optical brightener The adhesive composition described above may optionally further comprise a starting material O) an optical brightener. Suitable optical brighteners are commercially available, such as 2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole), commercially available as TINOPAL OB. When added to the composition, the optical brightener may be present in an amount of 0.1% to 2% by weight, based on the total weight of all starting materials in the adhesive composition.
[0082] Starting material P) Chain transfer agent The adhesive composition described above may optionally further comprise P) a chain transfer agent. When added to the adhesive composition, the chain transfer agent may be present in an amount of 0.01% to 5% by weight, alternatively 0.01% to 2% by weight, alternatively 0.1% to 2% by weight, based on the total weight of all starting materials in the composition.
[0083] Starting Material Q) (Meth)acrylate Monomer The adhesive composition described above may optionally further comprise a starting material Q) (meth)acrylate monomer. The (meth)acrylate monomer is exemplified by methyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, isobornyl acrylate, tetrahydrofurfuryl acrylate, cyclohexylmethyl acrylate, methyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, tetrahydrofurfuryl methacrylate, and cyclohexylmethyl methacrylate. When added to the adhesive composition, the (meth)acrylate monomer may be present in an amount of 0.1% to 35% by weight, alternatively 0.1% to 25% by weight, alternatively 0.1% to 15% by weight, alternatively 0.1% to 10% by weight, based on the total weight of all starting materials in the adhesive composition.
[0084] Starting material R) polyalkoxy-terminated polydiorganosiloxane Starting material R) is a polyalkoxy-terminated polydiorganosiloxane in addition to any prepared by the preparation of starting material B) described above. Starting material R) may be a polyalkoxy-terminated polydiorganosiloxane prepared as described above for starting material B), except that it does not contain a siloxane resin. Alternatively, starting material R) may be a polyalkoxy-terminated polydiorganosiloxane prepared by a platinum-catalyzed hydrosilylation reaction.
[0085] Starting material S) Colorant The adhesive composition described above may optionally further comprise starting material S) a colorant. The colorant may be a dye or a pigment such as carbon black.
[0086] When selecting starting materials for the adhesive composition described above, certain starting materials described herein may have more than one function, so the types of starting materials may overlap. For example, certain alkoxysilanes may be useful as crosslinkers and / or adhesion promoters and / or desiccants. Certain particles may be useful as fillers and spacers. When starting materials are added to the adhesive composition, the additional starting materials are different from each other.
[0087] Method for preparing adhesive composition The adhesive composition described above can be prepared by 1) combining starting materials B)i) an organosiloxane resin, and B)ii) a polydiorganosiloxane to form a resin polymer blend (RPB). A solvent can optionally be used to homogenize the RPB. One or more of the starting materials, such as the organosiloxane resin, can be dissolved or dispersed in a solvent, such as those mentioned above, for example, an aromatic hydrocarbon, such as benzene, toluene, or xylene. The amount of solvent can be 0% to 60% by weight, alternatively 10% to 50% by weight, alternatively 20% to 40% by weight, based on the total weight of all starting materials in the adhesive composition. Starting materials B)iii) and B)iv) can be combined with the RPB to form a converted RPB, as described above. The method can further include the step of 2) combining the converted RPB, and starting materials A), C), and D) by any convenient means, such as mixing. One or more additional starting materials E)-S) as described above can be added during step 1), step 2), or both. The starting materials can be combined at 20°C to 150°C. The process can further comprise heating the starting materials in step 1), step 2), or both, at a temperature of 50°C to 150°C, alternatively 60°C to 120°C. The pressure is not critical. The process can be carried out at ambient pressure.
[0088] Release Coating Composition Alternatively, the curable composition may be a release coating composition. (i) a polyfunctional organohydrogensiloxane or a product of the above-described process that contains the above-described polyfunctional organohydrogensiloxane; (ii) a polyorganosiloxane capable of undergoing a hydrosilylation reaction and having an average of at least two silicon-bonded aliphatic unsaturated groups per molecule; (iii) a hydrosilylation reaction catalyst; and (iv) a hydrosilylation reaction inhibitor.
[0089] Starting material (ii): Polyorganosiloxane having an aliphatic unsaturated group The starting material (ii) in the release coating composition is a polyorganosiloxane having, on average, at least two silicon-bonded aliphatic unsaturated groups per molecule that are capable of undergoing a hydrosilylation reaction, or a polyorganosiloxane having, on average, at least two silicon-bonded groups per molecule and having terminal aliphatic unsaturation. This polyorganosiloxane may be linear, branched, partially branched, cyclic, resinous (i.e., having a three-dimensional network), or may contain a combination of different structures. The polyorganosiloxane has an average formula, R 13 a SiO (4-a) / 2 [wherein each R 13 is independently selected from a monovalent hydrocarbon group or a monovalent halogenated hydrocarbon group, provided that at least two of the R 13 in each molecule contain aliphatic unsaturation, and the subscript a is selected such that 0 < a ≤ 3.2]. It may have. Suitable monovalent hydrocarbon groups and monovalent halogenated hydrocarbon groups for R 13 are as described above for R 1 . The above average formula for the polyorganosiloxane is, alternatively, (R 13 3SiO 1 / 2 ) b (R 13 2SiO 2 / 2 ) c (R 13 SiO 3 / 2 ) d (SiO 4 / 2 ) e [wherein R 13are defined above, and the subscripts b, c, d, and e are each independently ≧0 to ≦1, with the proviso that the quantity (b+c+d+e)=1. One skilled in the art will understand how such M, D, T, and Q units and their mole fractions affect the subscript a in the average formula above. T units (denoted by subscript d), Q units (denoted by subscript e), or both, are typically present in the polyorganosiloxane resin, while D units, denoted by subscript c, are typically present in the polyorganosiloxane polymer (and may also be present in the polyorganosiloxane resin or branched polyorganosiloxane).
[0090] Alternatively, the starting material (i) may comprise a substantially linear, or linear, polyorganosiloxane having the average formula R 13 a’ SiO (4-a’) / 2 [In the formula, each R 13 is as defined above, and subscript a' is selected such that 1.9≦a'≦2.2.
[0091] Alternatively, at RT, the substantially linear polyorganosiloxane may be a flowable liquid or have the form of an uncured rubber. The substantially linear polyorganosiloxane may have a viscosity at 25° C. of 10 mPa·s to 30,000,000 mPa·s, alternatively 10 mPa·s to 10,000 mPa·s, alternatively 100 mPa·s to 1,000,000 mPa·s, alternatively 100 mPa·s to 100,000 mPa·s. Viscosity may be measured at RT using a Brookfield LV DV-E viscometer, i.e., RV-1 through RV-7, with a spindle appropriately selected for the viscosity of the substantially linear polyorganosiloxane.
[0092] Alternatively, (ii) when the polyorganosiloxane is substantially linear or linear, the polyorganosiloxane has the average formula: 10 R9 2SiO 1 / 2 ) aa (R 10 R 9 SiO 2 / 2 ) bb (R 10 2SiO 2 / 2 ) cc (R 9 3SiO 1 / 2 ) dd [In the formula, each R 9 are independently selected monovalent hydrocarbon radicals free of aliphatic unsaturation or monovalent halogenated hydrocarbon radicals free of aliphatic unsaturation, and each R 10 are independently selected from the group consisting of alkenyl and alkynyl, the subscript aa is 0, 1, or 2, the subscript bb is 0 or more, the subscript cc is 1 or more, and the subscript dd is 0, 1, or 2, with the proviso that the quantity (aa+dd) is ≥ 2, the quantity (aa+dd) = 2, and with the proviso that the quantity (aa+bb+cc+dd) is 3 to 2,000. Alternatively, the subscript cc is ≥ 0. Alternatively, the subscript bb is ≥ 2. Alternatively, the quantity (aa+dd) is 2 to 10, alternatively 2 to 8, alternatively 2 to 6. Alternatively, the subscript cc is 0 to 1,000, alternatively 1 to 500, alternatively 1 to 200. Alternatively, the subscript bb is 2 to 500, alternatively 2 to 200, alternatively 2 to 100.
[0093] R 9 The monovalent hydrocarbon radicals are exemplified by alkyl radicals having 1 to 6 carbon atoms, aryl radicals having 6 to 10 carbon atoms, halogenated alkyl radicals having 1 to 6 carbon atoms, halogenated aryl radicals having 6 to 10 carbon atoms, aralkyl radicals having 7 to 12 carbon atoms, or halogenated aralkyl radicals having 7 to 12 carbon atoms, where alkyl, aryl, and halogenated alkyl are as described herein. 9 are independently a monovalent hydrocarbon group free of aliphatic unsaturation. Alternatively, each R 9 is an alkyl group. Alternatively, each R 9 is independently methyl, ethyl, or propyl.9 may be the same or different. Alternatively, each R 9 is a methyl group.
[0094] R 10 The aliphatically unsaturated monovalent hydrocarbon group of R is capable of undergoing a hydrosilylation reaction. 10 Suitable aliphatically unsaturated hydrocarbon groups for are exemplified by alkenyl groups, as defined herein, exemplified by vinyl, allyl, butenyl, and hexenyl, and alkynyl groups, as defined herein, exemplified by ethynyl and propynyl. 10 may be vinyl or hexenyl. Alternatively, each R 10 is a vinyl group. The subscript in the unit formula of (ii-I) above may be sufficient such that the alkenyl or alkynyl content of the branched siloxane of (ii-I) may be from 0.1% to 1% by weight, alternatively from 0.2% to 0.5% by weight, based on the weight of the branched siloxane (ii-I).
[0095] (ii) If the polyorganosiloxane is substantially linear, or linear, the at least two aliphatically unsaturated groups can be bonded to silicon atoms at pendant positions, terminal positions, or both pendant and terminal positions. As specific examples of polyorganosiloxanes having pendant silicon-bonded aliphatically unsaturated groups, the starting material A) can have the average formula: [(CH3)3SiO 1 / 2 ]2[(CH3)2SiO 2 / 2 ] cc [(CH3)ViSiO 2 / 2 ] bbwhere the subscripts bb and cc are as defined above and Vi represents a vinyl group. With respect to this average formula, any of the methyl groups may be replaced with a different monovalent hydrocarbon group, such as an alkyl or aryl, and any of the vinyl groups may be replaced with a different aliphatically unsaturated monovalent hydrocarbon group, such as an allyl or hexenyl. Alternatively, as a specific example of a polyorganosiloxane having an average of at least two silicon-bonded aliphatically unsaturated groups per molecule, starting material (ii) may have the average formula Vi(CH3)2SiO[(CH3)2SiO] cc Si(CH3)2Vi, where the subscripts cc and Vi are defined above. The silicon-bonded vinyl terminated dimethylpolysiloxanes can be used alone or in combination with the dimethyl,methyl-vinylpolysiloxanes disclosed above. With respect to this average formula, any of the methyl groups can be replaced with a different monovalent hydrocarbon group, and any of the vinyl groups can be replaced with any terminal aliphatically unsaturated monovalent hydrocarbon group. Since the at least two silicon-bonded aliphatically unsaturated groups can be both pendant and terminal, (ii) the polyorganosiloxane can alternatively have the unit formula: [Vi(CH3)2SiO 1 / 2 ]2[(CH3)2SiO 2 / 2 ] cc [(CH3)ViSiO 2 / 2 ] bb where the subscripts bb and cc and Vi are defined above.
[0096] The substantially linear polyorganosiloxane is, for example, a dimethylpolysiloxane having both molecular chain terminals blocked by dimethylvinylsiloxy groups, a methylphenylpolysiloxane having both molecular chain terminals blocked by dimethylvinylsiloxy groups, a methylphenylsiloxane-dimethylsiloxane copolymer having both molecular chain terminals blocked by dimethylvinylsiloxy groups, a methylvinylsiloxane-methylphenylsiloxane copolymer having both molecular chain terminals blocked by dimethylvinylsiloxy groups, or a methylvinylsiloxane-diphenylsiloxane copolymer having both molecular chain terminals blocked by dimethylvinylsiloxy groups. mer, methylvinylsiloxane-methylphenylsiloxane-dimethylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxy groups, methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, methylvinylsiloxane-diphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, and methylvinylsiloxane-methylphenylsiloxane-dimethylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups.
[0097] Alternatively, the starting material (ii) may comprise a substantially linear, or linear, polyorganosiloxane selected from the group consisting of: i) dimethylvinylsiloxy-terminated polydimethylsiloxane, ii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane); iii) dimethylvinylsiloxy-terminated polymethylvinylsiloxane; iv) trimethylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane); v) trimethylsiloxy-terminated polymethylvinylsiloxane; vi) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane); vii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylphenylsiloxane); viii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / diphenylsiloxane); ix) phenyl, methyl, vinyl-siloxy terminated polydimethylsiloxanes; x) dimethylhexenylsiloxy-terminated polydimethylsiloxane, xi) dimethylhexenylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane); xii) dimethylhexenylsiloxy-terminated polymethylhexenylsiloxane, xiii) trimethylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane); xiv) trimethylsiloxy-terminated polymethylhexenyl siloxanes; xv) dimethylhexenylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane); xvi) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane) and xvii) Combinations of these.
[0098] Alternatively, A) the polyorganosiloxane may be a resinous polyorganosiloxane having the average formula R 13 a” SiO (4-a”) / 2 [In the formula, each R 13 is as defined above, and the subscript a″ is selected such that 0.5≦a″≦1.7.
[0099] Resinous polyorganosiloxanes have a branched or three-dimensional network molecular structure. At 25°C, resinous polyorganosiloxanes may be in liquid or solid form. Alternatively, resinous polyorganosiloxanes may be exemplified by polyorganosiloxanes containing only T units, polyorganosiloxanes containing T units in combination with other siloxy units (e.g., M, D, and / or Q siloxy units), or polyorganosiloxanes containing Q units in combination with other siloxy units (i.e., M, D, and / or T siloxy units). Typically, resinous polyorganosiloxanes contain T units and / or Q units. Specific examples of resinous polyorganosiloxanes include vinyl-terminated silsesquioxanes and vinyl-terminated MDQ resins.
[0100] Alternatively, starting material (ii) may include (ii-I) a branched siloxane, (ii-II) a silsesquioxane, or both (ii-I) and (ii-II). Starting materials (ii-I) and (ii-II) may be particularly useful when the composition is used in release coating applications.
[0101] The starting material (ii) may be a combination of (ii-I) a branched siloxane and (ii-II) a silsesquioxane. The combination may be a physical blend or mixture. The branched siloxane and the silsesquioxane are present in mutual amounts such that the amount of (ii-I) the branched siloxane and the amount of (ii-II) the silsesquioxane add up to a total of 100 parts by weight, based on the total weight of all starting materials in the release coating composition. The branched siloxane may be present in an amount of 50 to 100 parts by weight and the silsesquioxane may be present in an amount of 0 to 50 parts by weight. Alternatively, the branched siloxane may be present in an amount of 50 to 90 parts by weight and the silsesquioxane may be present in an amount of 10 to 50 parts by weight. Alternatively, the branched siloxane may be present in an amount of 50 to 80 parts by weight and the silsesquioxane may be present in an amount of 20 to 50 parts by weight. Alternatively, the branched siloxane may be present in an amount of 50 to 76 parts by weight and the silsesquioxane may be present in an amount of 24 to 50 parts by weight. Alternatively, the branched siloxane may be present in an amount of 50 to 70 parts by weight and the silsesquioxane may be present in an amount of 30 to 50 parts by weight. Without being bound by theory, it is believed that when the amount of silsesquioxane (ii-II) exceeds 50 parts by weight per 100 parts by weight of the combined amount of (ii-I) branched siloxane and (ii-II) silsesquioxane, the release coating formed from the composition may suffer from migration, and the silsesquioxane may migrate and become contaminated by an adherend, such as a pressure sensitive adhesive, in contact with the release coating.
[0102] The starting material (ii-I) branched siloxane has the unit formula (ii-I), (R 9 3SiO 1 / 2 ) p (R 10 R 9 2SiO 1 / 2 ) q (R 9 2SiO 2 / 2 ) r (SiO 4 / 2 ) s [In the formula, each R 9are independently a monovalent hydrocarbon group containing no aliphatic unsaturation, or a monovalent halogenated hydrocarbon group containing no aliphatic unsaturation, and each R 10 is an alkenyl or alkynyl group, both of which are as defined above, and may have the subscript p≧0, the subscript q>0, 15≧r≧995, and the subscript s>0.
[0103] In the unit formula (ii-I), the subscript p is ≧0. The subscript q is >0. Alternatively, the subscript q is ≧3. The subscript r is 15 to 995. The subscript s is >0. Alternatively, the subscript s is ≧1. Alternatively, for the subscript p, 22≧p≧0, alternatively, 20≧p≧0, alternatively, 15≧p≧0, alternatively, 10≧p≧0, alternatively, 5≧p≧0. Alternatively, for the subscript q, 22≧q>0, alternatively, 22≧q≧4, alternatively, 20≧q>0, alternatively, 15≧q>1, alternatively, 10≧q≧2, alternatively, 15≧q≧4. Alternatively, for the subscript r, 800≧r≧15, alternatively, 400≧r≧15. Alternatively, for subscript s, 10≧s>0, alternatively, 10≧s≧1, alternatively, 5≧s>0, alternatively, s=1. Alternatively, subscript s is 1 or 2. Alternatively, when subscript s=1, subscript p may be 0 and subscript q may be 4.
[0104] The branched siloxane has the formula: 9 2SiO 2 / 2 ) m wherein each subscript m is independently 2 to 100. Alternatively, the branched siloxane may have at least two polydiorganosiloxane chains of the formula: 9 2SiO 2 / 2 ) o wherein each subscript o is independently 1 to 100; attached to four polydiorganosiloxane chains of the formula (SiO 4 / 2 Alternatively, the branched siloxane may comprise at least one unit of the formula: [ka] zzzImage14zzz wherein subscript u is 0 or 1; each subscript t is independently 0 to 995, alternatively 15 to 995, alternatively 0 to 100; and each R 11 are independently selected monovalent hydrocarbon radicals, and each R 9 are independently selected monovalent hydrocarbon radicals free of aliphatic unsaturation or monovalent halogenated hydrocarbon radicals free of aliphatic unsaturation, as described above, and each R 10 is independently selected from the group consisting of alkenyl and alkynyl, as described above. Suitable branched siloxanes for starting material (ii-I) are exemplified by those disclosed in U.S. Pat. No. 6,806,339 and U.S. Patent Application Publication No. 2007 / 0289495.
[0105] Silsesquioxanes are represented by the unit formula (ii-II), (R 9 3SiO 1 / 2 ) i (R 10 R 9 2SiO 1 / 2 ) f (R 9 2SiO 2 / 2 ) g (R 9 SiO 3 / 2 ) h ([wherein, R 9 and R 10 is as above, with subscript i≧0, subscript f>0, subscript g is 15-995, and subscript h>0. Subscript i may be 0-10. Alternatively, for subscript i, 12≧i≧0, alternatively 10≧i≧0, alternatively 7≧i≧0, alternatively 5≧i≧0, alternatively 3≧i≧0.
[0106] Alternatively, the subscript f is ≧1. Alternatively, the subscript f is ≧3. Alternatively, for the subscript f, 12≧f>0, alternatively 12≧f≧3, alternatively 10≧f>0, alternatively 7≧f>1, alternatively 5≧f≧2, alternatively 7≧f≧3. Alternatively, for the subscript g, 800≧g≧15, alternatively 400≧g≧15. Alternatively, the subscript h is ≧1. Alternatively, the subscript h is 1 to 10. Alternatively, for the subscript h, 10≧h>0, alternatively 5≧h>0, alternatively h=1. Alternatively, the subscript h is 1 to 10, alternatively the subscript h is 1 or 2. Alternatively, when the subscript h=1, the subscript f may be 3 and the subscript i may be 0. The value of subscript f may be sufficient for the silsesquioxane of formula (ii-II) to have an alkenyl content of from 0.1% to 1%, alternatively from 0.2% to 0.6%, by weight, based on the weight of the silsesquioxane. Suitable silsesquioxanes for starting material (ii) are exemplified by those disclosed in U.S. Pat. No. 4,374,967.
[0107] Starting material (ii) may include a combination or two or more different polyorganosiloxanes that differ in at least one property, such as structure, molecular weight, monovalent groups bonded to silicon atoms, and content of aliphatic unsaturated groups, etc. The release coating composition may contain from 60% to 98% by weight, alternatively from 60% to 95% by weight, of starting material (ii) based on the total weight of all starting materials in the release coating composition.
[0108] Starting material (iii) hydrosilylation catalyst The hydrosilylation catalyst used as starting material (iii) in the release coating composition may be as described and exemplified above for starting material b). Alternatively, the hydrosilylation catalyst for use in the release coating composition may be selected from the group consisting of Karstedt's catalyst and Ashby's catalyst. (iii) The hydrosilylation catalyst is present in the release coating composition in a catalytic amount, i.e., an amount or quantity sufficient to promote its cure under the desired conditions. (iii) The catalytic amount of the hydrosilylation catalyst may be >0.01 ppm to 10,000 ppm, alternatively >1,000 ppm to 5,000 ppm. Alternatively, typical catalytic amounts of (iii) the hydrosilylation catalyst are 0.1 ppm to 5,000 ppm, alternatively 1 ppm to 2,000 ppm, alternatively >0 to 1,000 ppm. Alternatively, (iii) the catalytic amount of the hydrosilylation reaction catalyst can be from 0.01 ppm to 1,000 ppm, alternatively from 0.01 ppm to 100 ppm, alternatively from 20 ppm to 200 ppm, alternatively from 0.01 ppm to 50 ppm of platinum group metal, based on the combined weight of all starting materials in the release coating composition.
[0109] Starting material (iv) hydrosilylation reaction inhibitor The starting material (iv) is an inhibitor that can be used to alter the reaction rate of the release coating composition when compared to a composition containing the same starting material but without the added inhibitor. Inhibitors of the hydrosilylation curable composition include acetylenic alcohols such as methylbutynol, ethynylcyclohexanol, dimethylhexynol, and 3,5-dimethyl-1-hexyn-3-ol, 1-butyn-3-ol, 1-propyn-3-ol, 2-methyl-3-butyn-2-ol, 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3-phenyl-1-butyn-3-ol, 4-ethyl-1-octyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, and 1-ethynyl-1-cyclohexanol, and combinations thereof; cycloalkenylsiloxanes such as 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, 1,3,5,7 -methylvinylcyclosiloxanes exemplified by tetramethyl-1,3,5,7-tetrahexenylcyclotetrasiloxane, and combinations thereof; ene-yne compounds such as 3-methyl-3-penten-1-yne, 3,5-dimethyl-3-hexen-1-yne; triazoles such as benzotriazole; phosphines; mercaptans; hydrazines; amines such as tetramethylethylenediamine; dialkyl fumarates, dialkenyl fumarates, dialkoxyalkyl fumarates, maleates such as diallyl maleate; nitriles; ethers; carbon monoxide; alkenes such as cyclooctadiene, divinyltetramethyldisiloxane; alcohols such as benzyl alcohol; and combinations thereof. Alternatively, the hydrosilylation reaction inhibitor may be selected from the group consisting of acetylenic alcohols (e.g., 1-ethynyl-1-cyclohexanol), and maleates (e.g., diallyl maleate, bismaleate, or n-propyl maleate), and combinations of two or more thereof.
[0110] Alternatively, the starting material (iv) in the composition may be a silylated acetylenic compound. Without being bound by theory, it is believed that the addition of the silylated acetylenic compound reduces the yellowing of the reaction product prepared from the hydrosilylation reaction of the composition when compared to the reaction product from the hydrosilylation of a composition that does not contain the silylated acetylenic compound or a composition that contains an organic acetylenic alcohol inhibitor such as those described above.
[0111] The silylated acetylene compounds are (3-methyl-1-butyne-3-oxy)trimethylsilane, ((1,1-dimethyl-2-propynyl)oxy)trimethylsilane, bis(3-methyl-1-butyne-3-oxy)dimethylsilane, bis(3-methyl-1-butyne-3-oxy)silanemethylvinylsilane, bis((1,1-dimethyl-2-propynyl)oxy)dimethylsilane, methyl(tris(1,1-dimethyl-2-propynyloxy))silane, methyl(tris(3-methyl-1-butyne-3-oxy))silane, (3-methyl-1-butyne-3-oxy)dimethylphenylsilane, (3-methyl-1-butyne-3-oxy)dimethylhexenylsilane, (3-methyl-1-butyne-3-oxy)triethylsilane, bis(3-methyl-1- silane, (3,5-dimethyl-1-hexyne-3-oxy)trimethylsilane, (3-phenyl-1-butyne-3-oxy)diphenylmethylsilane, (3-phenyl-1-butyne-3-oxy)dimethylphenylsilane, (3-phenyl-1-butyne-3-oxy)dimethylvinylsilane, (3-phenyl-1-butyne-3-oxy)dimethylhexenylsilane, (cyclohexyl-1-ethyne-1-oxy)dimethylhexenylsilane, (cyclohexyl-1-ethyne-1-oxy)dimethylvinylsilane, (cyclohexyl-1-ethyne-1-oxy)diphenylmethylsilane, (cyclohexyl-1-ethyne-1-oxy)trimethylsilane, and combinations thereof. Alternatively, starting material (iv) is exemplified by methyl(tris(1,1-dimethyl-2-propynyloxy))silane, ((1,1-dimethyl-2-propynyl)oxy)trimethylsilane, or a combination thereof. Silylated acetylenic compounds useful as starting material (iv) can be prepared by methods known in the art, such as silylation of the above-mentioned acetylenic alcohols by reaction with chlorosilanes in the presence of an acid acceptor.
[0112] The amount of inhibitor added to the release coating composition will vary depending on a variety of factors, such as the desired pot life of the composition, whether the composition is a one-part or multi-part composition, the particular inhibitor used, the selection and amount of starting materials (i) and (ii), etc. However, if present, the amount of inhibitor may be from 0% to 1% by weight, alternatively from 0% to 5% by weight, alternatively from 0.001% to 1% by weight, alternatively from 0.01% to 0.5% by weight, alternatively from 0.0025% to 0.025% by weight, based on the total weight of all starting materials in the composition.
[0113] Additional starting materials The release coating composition may optionally further comprise one or more additional starting materials selected from (v) anchor additives, (vi) anti-mist additives, (vii) release modifiers, (viii) substantially linear or linear polyorganohydrogensiloxanes, and (ix) solvents, such as those described above for starting material D).
[0114] (v) Anchor additives The starting material (v) is an anchor additive. Suitable anchor additives are exemplified by the reaction product of vinyl alkoxysilane and epoxy functional alkoxysilane; the reaction product of vinyl acetoxysilane and epoxy functional alkoxysilane; and the combination (e.g., physical blend and / or reaction product) of polyorganosiloxane having at least one aliphatically unsaturated hydrocarbon group and at least one hydrolyzable group in one molecule with epoxy functional alkoxysilane (e.g., the combination of hydroxy-terminated vinyl functional polydimethylsiloxane and glycidoxypropyltrimethoxysilane). Alternatively, the anchor additive may comprise a polyorganosilicate resin. Suitable anchor additives and their preparation methods are disclosed, for example, in U.S. Pat. No. 9,562,149, U.S. Patent Application Publication Nos. 2003 / 0088042, 2004 / 0254274, and 2005 / 0038188, and European Patent No. 0556023. Although the exact amount of anchor additive will vary depending on a variety of factors, such as the type of substrate and whether a primer is used, the amount of anchor additive in the release coating composition may be from 0 to 2 parts by weight per 100 parts by weight of starting material (ii). Alternatively, the amount of anchor additive may be from 0.01 to 2 parts by weight per 100 parts by weight of starting material (ii).
[0115] (vi) Anti-mist additives Starting material (vi) is a mist suppressing additive, which can be added to the release coating composition to reduce or suppress silicone mist formation during the coating process, especially in high-speed coating equipment.The mist suppressing additive can be the reaction product of an organohydrogensilicon compound, an oxyalkylene compound, or an organoalkenylsiloxane having at least three silicon-bonded alkenyl groups in one molecule, and a suitable catalyst.Suitable mist suppressing additives are disclosed, for example, in U.S. Patent Application Publication No. 2011 / 0287267, U.S. Patent Nos. 8,722,153, 6,586,535, and 5,625,023.
[0116] The amount of the anti-mist additive will vary depending on a variety of factors, such as the amount and type of other starting materials selected for the release coating composition, but the amount of the anti-mist additive may be from 0% to 10% by weight, alternatively from 0.1% to 3% by weight, based on the total weight of all starting materials in the release coating composition.
[0117] (vii) Release modifier Starting material (vii) is a release modifier that can be added to the release coating composition to control (reduce) the level of release force (adhesion between the release coating and the adherend thereto, e.g., a label, including a pressure-sensitive adhesive). A release coating composition having the required release force can be formulated from a modifier-free release coating composition by adjusting the concentration of the modifier. Examples of suitable release modifiers include trimethylsiloxy-terminated dimethyl, phenylmethyl siloxanes. Alternatively, the release modifier may be a condensation reaction product of an organopolysiloxane resin having hydroxyl or alkoxy groups and a diorganopolysiloxane having at least one hydroxyl or hydrolyzable group. When used, the release modifier can be used, for example, at 0 to 85 parts by weight, alternatively 25 to 85 parts by weight, per 100 parts of starting material (ii). Examples of suitable release modifiers are disclosed, for example, in U.S. Pat. No. 8,933,177 and U.S. Patent Application Publication No. 2016 / 0053056.
[0118] (viii) Linear polyorganohydrogensiloxane Starting material (viii) is a substantially linear or linear polyorganohydrogensiloxane different from starting material (i) that can be added to the release coating composition as an additional crosslinker. The substantially linear or linear polyorganohydrogensiloxane has the unit formula: (HR 12 2SiO 1 / 2 ) v’ (HR 12 SiO 2 / 2 ) w’ (R 12 2SiO2 / 2 ) x’ (R 12 3SiO 1 / 2 ) y’ [In the formula, each R 12 are independently selected monovalent hydrocarbon radicals, subscript v' is 0, 1, or 2, subscript w' is 1 or greater, subscript x' is 0 or greater, and subscript y' is 0, 1, or 2, with the proviso that the quantity (v'+y')=2 and the quantity (v'+w')≧3. 12 The monovalent hydrocarbon group of R 1 The monovalent hydrocarbon group may be as described above. The quantity (v'+w'+x'+y') may be from 2 to 1,000. The polyorganohydrogensiloxanes are exemplified by the following: i) dimethylhydrogensiloxy-terminated poly(dimethyl / methylhydrogen)siloxane copolymers; ii) dimethylhydrogensiloxy-terminated polymethylhydrogensiloxane; iii) trimethylsiloxy-terminated poly(dimethyl / methylhydrogen)siloxane copolymers, and iv) trimethylsiloxy-terminated polymethylhydrogensiloxane, and v) A combination of two or more of i), ii), iii), iv), and v).Suitable polyorganohydrogensiloxanes are commercially available from Dow Silicones Corporation, Midland, Michigan, USA.
[0119] (ix) Solvent Starting material (x) is a solvent. Suitable solvents include the hydrocarbons described above as starting material D) in the method for producing polyfunctional organohydrogensiloxanes. Alternatively, the solvent may be selected from polyalkylsiloxanes, alcohols, ketones, glycol ethers, tetrahydrofuran, mineral spirits, naphtha, tetrahydrofuran, mineral spirits, or combinations thereof. Polyalkylsiloxanes having suitable vapor pressures can be used as solvents, including hexamethyldisiloxane, octamethyltrisiloxane, hexamethylcyclotrisiloxane, and other low molecular weight polyalkylsiloxanes, such as DOWSIL™ 200 FLUIDS and DOWSIL™ OS FLUIDS, 0.5-1.5 cSt, available from Dow Silicones Corporation (Midland, Michigan, USA).
[0120] Alternatively, the starting material (x) may comprise an organic solvent, which may be an alcohol such as methanol, ethanol, isopropanol, butanol, or n-propanol; a ketone such as acetone, methyl ethyl ketone, or methyl isobutyl ketone; an aromatic hydrocarbon such as benzene, toluene, or xylene; an aliphatic hydrocarbon (e.g., heptane, hexane, or octane); a glycol ether such as propylene glycol methyl ether, dipropylene glycol methyl ether, propylene glycol n-butyl ether, propylene glycol n-propyl ether, or ethylene glycol n-butyl ether, tetrahydrofuran, or the like; mineral spirits; naphtha; or a combination thereof.
[0121] The amount of solvent will vary depending on a variety of factors, such as the type of solvent selected, as well as the amount and type of other starting materials selected for the release coating composition. However, the amount of solvent may be from 0% to 99% by weight, alternatively from 2% to 50% by weight, based on the weight of all starting materials of the release coating composition. Solvents can be added during preparation of the release coating composition, for example, to aid in mixing and delivery. All or a portion of the solvent can be optionally removed after preparation of the release coating composition.
[0122] Other optional starting materials that may be further added to the release coating compositions described herein include, for example, reactive diluents, fragrances, preservative colorants, and fillers, such as silica, quartz, or chalk.
[0123] In selecting starting materials for the release coating composition (and other curable compositions described herein), certain starting materials described herein may have more than one function, and therefore the types of starting materials may overlap. For example, certain particulates such as carbon black may be useful as fillers, colorants such as pigments, and even flame retardants. If additional starting materials are added to the release coating composition, the additional starting materials are different from starting materials (i)-(iv) and different from each other.
[0124] Alternatively, the release coating may be free of particulates or may contain only limited amounts of particulates (e.g., fillers and / or pigments), e.g., 0% to 30% by weight of the release coating composition. Particulates may agglomerate or otherwise stick to the coater equipment used to apply the release coating. They may interfere with the optical properties, e.g., transparency, of the release coating and release liner formed therewith, if optical clarity is desired. Particulates may be detrimental to adherend adhesion.
[0125] Alternatively, the release coating composition of the present invention may be free of fluoroorganosilicone compounds. During curing, it is believed that fluoro compounds, due to their low surface tension, may rapidly migrate to the interface between the coating composition and the substrate, such as the polyorganosiloxane release coating composition / PET film interface, and may prevent the release coating (prepared by curing the release coating composition) from adhering to the substrate by creating a fluorine-containing barrier. By creating a barrier, the fluoro compounds may prevent any starting material from reacting at the interface. Furthermore, fluorosilicone compounds are usually expensive.
[0126] The stripping composition can be prepared by combining the starting materials, including (i), (ii), (iii), and (iv) above, along with any optional additional starting materials, in any order of addition, optionally via a masterbatch, and optionally under shear.
[0127] Method for coating a substrate The method for preparing a substrate coated with a curable composition includes disposing the curable composition on a substrate. The method further includes curing the curable composition on the substrate. Curing can be carried out by heating at an elevated temperature, for example, from 50° C. to 180° C., alternatively from 50° C. to 120° C., alternatively from 50° C. to 90° C., to obtain a coated substrate. One skilled in the art will be able to select an appropriate temperature depending on a variety of factors, including the choice of optional starting materials in the curable composition and substrate material of construction.
[0128] The curable composition can be disposed or distributed on the substrate in any suitable manner. Typically, the curable composition is applied in wet form by a wet coating technique. The curable composition can be applied by i) spin coating; ii) brush coating; iii) drop coating; iv) spray coating; v) dip coating; vi) roll coating; vii) flow coating; viii) slot coating; ix) gravure coating; x) Mayer bar coating; or xi) a combination of any two or more of i)-x). Typically, disposing the curable composition on the substrate results in a wet deposit on the substrate, which is then cured to obtain a coated substrate comprising a cured film formed from the curable composition on the substrate.
[0129] The substrate is not limited and may be any substrate. The cured film may be separable from the substrate or may be physically and / or chemically bonded to the substrate, depending on the choice. The substrate may be subjected to an integrated hotplate or an integrated or stand-alone oven for curing the deposit. The substrate may optionally have continuous or non-continuous shapes, sizes, dimensions, surface roughness, and other properties. The substrate may have an elevated softening point temperature. However, the curable compositions and methods are not so limited.
[0130] Alternatively, the substrate may comprise a plastic, which may be thermoset and / or thermoplastic, but may alternatively be glass, metal, paper, wood, cardboard, paperboard, silicone, or a polymeric material, or a combination thereof.
[0131] Specific examples of suitable substrates include paper substrates such as kraft paper, polyethylene-coated kraft paper (PEK-coated paper), and plain paper; polymer substrates such as polyamide (PA); polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PET), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), and liquid crystal polyester; polyolefins such as polyethylene (PE), polypropylene (PP), and polybutylene; styrene resins; polyoxymethylene (POM); polycarbonate (PC); polymethylene methacrylate (PMMA); polyvinyl chloride (PVC); polyphenylene sulfide (PPS); polyphenylene ether (PPE); polyimide (PI); polya Examples of such resins include amidoimide (PAI); polyetherimide (PEI); polysulfone (PSU); polyethersulfone; polyketone (PK); polyetherketone; polyvinyl alcohol (PVA); polyetheretherketone (PEEK); polyetherketoneketone (PEKK); polyarylate (PAR); polyethernitrile (PEN); phenolic resins; phenoxy resins; cellulose such as triacetyl cellulose, diacetyl cellulose, cellophane, etc.; fluorinated resins such as polytetrafluoroethylene; thermoplastic elastomers such as polystyrene type, polyolefin type, polyurethane type, polyester type, polyamide type, polybutadiene type, polyisoprene type, fluoro type, etc.; and copolymers and combinations thereof.
[0132] The curable composition, or wet deposit, is typically cured at elevated temperature for a period of time. The period of time is typically sufficient to effect cure, i.e., crosslinking, of the curable composition. Alternatively, the period of time may be from greater than 0 to 8 hours, alternatively from greater than 0 to 2 hours, alternatively from greater than 0 to 1 hour, alternatively from greater than 0 to 30 minutes, alternatively from greater than 0 to 15 minutes, alternatively from greater than 0 to 10 minutes, alternatively from greater than 0 to 5 minutes, or alternatively from greater than 0 to 2 minutes. The period of time will vary depending on a variety of factors, such as the presence of the elevated temperature used, the temperature selected, the desired film thickness, the absence of any water or carrier vehicle in the curable composition, etc.
[0133] The step of curing the curable composition typically has a residence time of 0.1 to 50 seconds, alternatively 1 to 10 seconds, alternatively 0.5 to 30 seconds. The residence time selected may vary depending on the choice of substrate, the temperature selected, and the line speed. As used herein, residence time refers to the time that the curable composition or wet deposit is exposed to an elevated temperature. Residence time is distinct from cure time, since there may be ongoing curing even after the curable composition, wet deposit, or partially cured reaction intermediate thereof is no longer exposed to the elevated temperatures that typically initiate curing. Alternatively, the coated article may be prepared on a conveyor belt in an oven, and the residence time may be calculated (e.g., meters / second) by dividing the length of the oven (e.g., in meters) by the line speed of the conveyor belt.
[0134] The time can be subdivided into iterations of cure, e.g., a first cure and a post cure, e.g., 1 hour for the first cure and 3 hours for the post cure. The elevated temperature can be independently selected in such iterations from any temperature above room temperature and can be the same in each iteration.
[0135] Depending on the thickness and other dimensions of the film and coated substrate, the coated substrate can be formed through an iterative process. For example, a first deposit can be formed and exposed to a first elevated temperature for a first time to obtain a partially cured deposit. A second deposit can then be placed on the partially cured deposit and exposed to a second elevated temperature for a second time to obtain a second partially cured deposit. The partially cured deposit also further cures while exposed to the second elevated temperature for a second time. A third deposit can be placed on the second partially cured deposit and exposed to a third elevated temperature for a third time to obtain a third partially cured deposit. The second partially cured deposit also further cures while exposed to the second elevated temperature for a second time. This process can be repeated, for example, 1 to 50 times, to build up the coated article as desired. The composite of partially cured layers is typically subjected to a final post-cure, for example, exposed to an elevated temperature and time as described above. Each elevated temperature and time may be selected independently and may be the same or different from each other. When the article is formed via an iterative process, each deposit may also be independently selected and may differ in the starting materials selected in the curable composition, their amounts, or both, or, alternatively, each repeating layer may be fully cured, rather than only partially cured, in such an iterative process.
[0136] Alternatively, the deposition may include a wet film. The iterative process may be wet-on-wet, depending on the curing state of the partially cured layer. Alternatively, the iterative process may be wet-on-dry.
[0137] The coated substrate comprising a film formed from the curable composition on the substrate may have a variety of dimensions, such as the relative thickness of the film and substrate. The film has a thickness that may vary depending on the end use application. The film may have a thickness of from greater than 0 to 4,000 μm, alternatively from greater than 0 to 3,000 μm, alternatively from greater than 0 to 2,000 μm, alternatively from greater than 0 to 1,000 μm, alternatively from greater than 0 to 500 μm, alternatively from greater than 0 to 250 μm. However, other thicknesses are contemplated, for example, from 0.1 to 200 μm. For example, the thickness of the film may be from 0.2 to 175 μm; alternatively, from 0.5 to 150 μm; alternatively, from 0.75 to 100 μm; alternatively, from 1 to 75 μm; alternatively, from 2 to 60 μm; alternatively, from 3 to 50 μm, alternatively, from 4 to 40 μm. Alternatively, when the substrate is plastic, the film may have a thickness of from greater than 0 to 200 μm, alternatively from greater than 0 to 150 μm, alternatively from greater than 0 to 100 μm.
[0138] If desired, the film can undergo further processing depending on its end use application. For example, the film can undergo oxide deposition (e.g., SiO2 deposition), resist deposition and patterning, etching, chemical stripping, corona or plasma stripping, metallization, or metal deposition. Such further processing techniques are well known. Such deposition can be chemical vapor deposition (such as low pressure chemical vapor deposition, plasma induced chemical vapor deposition, and plasma assisted chemical vapor deposition), physical vapor deposition, or other vacuum deposition techniques. Many such further processing techniques involve high temperatures, especially vacuum deposition, for which the film is well suited given its excellent thermal stability. However, depending on the end use of the film, the film can be used with such further processing.
[0139] The coated substrate can be used in a variety of end-use applications. For example, the coated substrate can be used in coating applications, packaging applications, adhesive applications, fiber applications, fabric or textile applications, construction applications, transportation applications, electronic applications, or electrical applications. However, the curable composition can be used in end-use applications other than preparing the coated substrate, such as preparing articles such as silicone rubber.
[0140] Alternatively, the coated substrate can be used as a release liner for a tape or adhesive, including any pressure sensitive adhesive, such as, for example, acrylic, rubber, and silicone type pressure sensitive adhesives, as well as acrylic, synthetic rubber, silicone, epoxy, and polyurethane type adhesives. Each major surface of the substrate may have a double-sided tape or film disposed thereon for an adhesive.
[0141] Alternatively, when the curable composition is formulated as a release coating composition, the release coating composition can be prepared by mixing the starting materials together, e.g., to prepare a one-part composition. However, it may be desirable to prepare the release coating composition as a multi-part composition in which the starting materials having SiH functionality (e.g., starting materials (i) and, if present, (viii)) and the hydrosilylation reaction catalyst are stored in separate parts until the parts are combined at the time of use (e.g., immediately prior to application to a substrate).
[0142] For example, a multi-part composition may include: (A) part a base part comprising: (ii) a polyorganosiloxane having an average of at least two silicon-bonded aliphatically unsaturated hydrocarbon groups per molecule; (iii) a hydrosilylation reaction catalyst; and, if present, one or more of an anchor additive and a solvent; and a curing agent part (B) comprising (ii) a polyorganosiloxane having an average of at least two silicon-bonded aliphatically unsaturated hydrocarbon groups per molecule, (i) a polyfunctional organohydrogensiloxane, and, if present, (viii) a substantially linear or linear polyorganohydrogensiloxane, an anchor additive, and a solvent. The starting material (iv) inhibitor can be added to either part (A), part (B), or both. Parts (A) and (B) can be combined in an (A):(B) weight ratio of 1:1 to 10:1, alternatively 1:1 to 5:1, alternatively 1:1 to 2:1. Parts (A) and (B) can be provided in a kit, for example, with instructions on how to combine the parts to prepare the release coating composition, how to apply the release coating composition to a substrate, and how to cure the release coating composition.
[0143] Alternatively, if an anchor additive is present, it can be incorporated into either part (A) or part (B), or can be added to a separate (third) part.
[0144] Alternatively, the release coating composition comprises: 1) ii) mixing starting materials including a polyorganosiloxane having an average of at least two silicon-bonded aliphatically unsaturated hydrocarbon groups per molecule, (i) a multifunctional organohydrogensiloxane, (iii) a hydrosilylation reaction catalyst, (iv) an inhibitor, and optionally one or more of (v) an anchor additive, (vi) a mist suppression additive, (vii) a release control agent, (viii) a linear polyorganohydrogensiloxane, and (ix) a solvent, thereby forming a release coating composition; 2) applying the mixture onto a substrate. Step 1) can be carried out by mixing parts (A) and (B) of a multi-part composition as described above.
[0145] The release coating composition can be applied to the substrate by any convenient means such as spraying, doctor blading, dipping, screen printing, or by a roll coater, for example an offset web coater, kiss coater, or etched cylinder coater.
[0146] The release coating composition of the present invention can be applied to any substrate, such as those mentioned above. Alternatively, the release coating composition can be applied to a polymeric film substrate, such as a polyester film, particularly a polyethylene terephthalate (PET) film, a polyethylene film, a polypropylene film, or a polystyrene film. Alternatively, the release coating composition can be applied to a paper substrate, including a plastic-coated paper, such as a polyethylene-coated paper, a glassine, a supercalendered paper, or a clay-coated kraft paper. Alternatively, the release coating composition can be applied to a metal foil substrate, such as an aluminum foil.
[0147] The method may further comprise the step of 3) treating the substrate, and then coating the release coating composition on the substrate. The treatment of the substrate can be carried out by any convenient means, such as plasma treatment or corona discharge treatment. Alternatively, the substrate can be treated by applying a primer. In certain cases, if the substrate is treated before coating, the adhesion of the release coating can be improved.
[0148] If the release coating composition includes a solvent, the method may further include the step of 4) removing the solvent, which may be carried out by any conventional means, such as by heating at 50° C. to 100° C. for a time sufficient to remove all or a portion of the solvent. The method may further include the step of 5) curing the release coating composition to form a release coating on the surface of the substrate. Curing may be carried out by any conventional means, such as by heating at 100° C. to 200° C.
[0149] Under production coater conditions, curing can be carried out at air temperatures of 120° C. to 150° C. with residence times of 1 to 6 seconds, alternatively 1.5 to 3 seconds. Heating in the case of steps 4) and / or 5) can be carried out in an oven, e.g., an air circulating oven or a tunnel furnace, or by passing the coated film around a heated cylinder. EXAMPLES
[0150] These examples are intended to illustrate the invention and should not be construed as limiting the scope of the invention as set forth in the claims. The starting materials in Table 1 were used in the examples herein. [Table 1]
[0151] Reference example 1. ESI-MS analysis Each sample was prepared at approximately 1000 ppm by dilution in Fisher HPLC grade MeCN. The MeCN diluted samples were analyzed by flow injection analysis, positive ion electrospray ionization MS (FIA ESI MS). The mass calibration of the instrument was verified to be error-free on the same day that the analysis was performed. The following instruments and conditions were used: ESI-MS instrument conditions Instrument: Agilent 1200UPLC system Flow rate: 0.40mL / min Injection volume: 2.5μL Mobile phase: 95% MeCN in water Positive ion ESI MS, conditions Instrument: Agilent 6520 quadrupole / time-of-flight (Q-TOF) tandem mass spectrometer Ion source: Dual electrospray ionization Mode: Positive ion-MS1 Drying gas temperature: 300℃ Drying gas flow rate: 5L / min Nebulizer pressure: 60psi Fragmenter voltage: 150V Skimmer voltage: 75V Octopole 1 RF voltage: 750V Capillary voltage: 4500V Reference mass: 121.0509, 922.0098 Acquisition mode: MS1 Mass range: 119-3200 Da Scan speed: 1 spectrum / sec
[0152] Reference Example 2. GPC The following experimental procedure was used and the samples had methyl groups. The samples were prepared as follows: Sample preparation: 10 mg / mL in eluent; solvate for 1 hour with occasional shaking; filter samples through a 0.45 μm PTFE syringe filter prior to injection. Pump: Waters515, at 1.0mL / min nominal flow rate Eluent: HPLC grade toluene Injector: Waters 717, 100 μL injection Columns: Two (300 mm x 7.5 mm) Polymer Laboratories PLgel 5 μm Mixed-C columns, preceded by a PLgel 5 μm guard column (50 mm x 7.5 mm). 45 °C Detector: Waters 2410 differential refractive index detector, 45°C Data system: Atlas8.3, Cirrus2.0 Calibration: Compared to 14 narrow polystyrene standards ranging from 580 g / mol to 2,300,000 g / mol and fitted with a third order polynomial curve.
[0153] The following experimental procedure was used and the samples had phenyl groups. Sample preparation: 10 mg / mL in eluent; solvate for 1 hour; filter solution through a 0.45 μm PTFE syringe filter prior to injection. Pump: Waters 2695, at 1.0 mL / min nominal flow rate Eluent: Certified grade THF Injector: Waters2695, 100μL injection Columns: Two (300 mm x 7.5 mm) Polymer Laboratories PLgel 5 μm Mixed-C columns, preceded by a PLgel 5 μm guard column (50 mm x 7.5 mm). 35 °C Detector: Waters 2410 differential refractive index detector, 35°C Data system: Atlas8.3, Cirrus2.0 Calibration: Compare to 16 narrow polystyrene standards ranging from 580 g / mol to 2,300,000 g / mol and fit a third order polynomial curve.
[0154] Reference example 3. 29 SiNMR Samples were prepared for analysis as follows: 3.5-4.5 g of material was dissolved in 4-4.5 g of CDCl3 for a total weight of 8-9 g. Samples were transferred to Teflon tubes (8 in. long x 13.5 mm od) with Teflon stoppers. 29 SiNMR data, 400MHz 1 The spectra were acquired on a Varian Inova NMR (mi-MR-04) spectrometer with H operating frequency and standard parameters (nt=256 and d1=13).
[0155] Reference Example 4. General Procedure for Preparation of Polyfunctional Organohydrogensiloxanes A source of SiH(MH4Q) was placed in a 1 L flask using a water-cooled condenser equipped with a mechanical stirrer, thermocouple, and N2 bubbler. 10-100 ppm of BCF (dissolved in 3-5% toluene) was initially added to the flask at a temperature between RT and 50°C. The silanol fluid (PA fluid or PB fluid) was added slowly to the flask with vigorous stirring. The reaction was recorded by pot temperature rise and gas evolution. If no gas evolution was observed, more BCF (10 ppm-100 ppm) was added to the flask. This procedure was repeated until the end of the silanol fluid addition. The pot temperature was maintained at 30°C-60°C during the course of the reaction. After the addition of the silanol fluid was completed, the mixture was maintained at 30°C-60°C for an additional 1-3 hours. The heat was then removed and neutral activated alumina (300-1000 times the weight of the BCF catalyst) was added to the flask. After stirring for 1-3 hours, the alumina was filtered off through a 0.45 μm filter membrane. Volatiles were removed by rotary evaporation (<1 mmHg) at 80°C-100°C for 60-90 minutes. The resulting product was collected and analyzed.
[0156] Table 2 shows samples produced using the general procedure in Reference Example 4. Mw was measured according to Reference Example 2, PD was measured according to Reference Example 2, and SiH% was measured according to Reference Example 3. [Table 2]
[0157] Samples 1 and 2 were evaluated by GPC analysis as described in Reference Example 2. Molecular weight averages were compared to polystyrene standards and for portions of the chromatograms as indicated. The results are shown in Table 3. [Table 3] 0
[0158] are shown in Table 4 below. M' is a compound represented by the formula (HMe2SiO 1 / 2 Q represents a monofunctional siloxane unit of the formula (SiO4 / 2 D represents a tetrafunctional siloxane unit of the formula (Me2SiO 2 / 2 D(PhMe) represents a difunctional siloxane unit of the formula (MePhSiO 2 / 2 ) represents a difunctional siloxane unit. [Table 4]
[0159] Example 5. Due to the high viscosity of the silanol fluid (DMS-S42) used in this example, heptane was used to reduce the viscosity for better mixing. Residual water was also removed by azeotropic distillation of heptane. H 4Q and 301 g of heptane were mixed in a 1 L flask using a Dean Stark fitted with a mechanical stirrer, thermocouple, and a water-cooled condenser equipped with a N2 bubbler. Approximately 90 g of heptane was removed by azeotropic distillation at 100-101°C. The pot temperature was then cooled to 60°C and 1.44 g of a 3.82% tris(pentafluorophenyl)borane (BCF) / toluene solution was added to the flask. 294.6 g of DMS-S42 was added slowly to the flask. The pot temperature was maintained at 50-60°C. After 3 hours, the heat was removed and 18.6 g of neutral activated alumina was added. After stirring for >3 hours, the alumina was filtered off through a 0.45 μm filter membrane. Volatiles were removed by rotary evaporation (<1 mmHg) at 80°C for 30 min and 100°C for 1 h. 285.4 g of viscous fluid was recovered. H% (as SiH) was: 29 It was measured to be 0.0238% based on SiNMR.
[0160] The polyfunctional organohydrogensiloxanes prepared as described above can be formulated into release coating compositions. [Table 5-1] [Table 5-2]
[0161] Reference Example 6. Release Coating Composition The inhibitor was melted in an oven at 40°C before use. The vinyl-functional polyorganosiloxane, crosslinker, and pre-melted inhibitor were thoroughly mixed at RT. The catalyst was then introduced into the mixture, which was then further mixed at RT. The amount of each starting material in the release coating composition prepared according to this Reference Example 6 is shown in Table 6 below. The amounts shown in the table are in grams. [Table 6]
[0162] Reference Example 7. (6.3) Test procedure for extractables To measure the curing performance of the release coating composition, extractables test was carried out immediately after curing.The extractables test was used to determine the amount of non-crosslinked silicone that was extractable from the release coating sample after curing in the presence of solvent.The test method used in the following examples was as follows: 1. Immediately after completion of the coating process (described above), three sample discs were cut from the coated substrate using a 1.375 inch (3.49 cm) die cutter. 2. The silicone coat weight of each sample was measured using an Oxford Instruments Lab-X 3500 Benchtop XRF analyzer. 3. Each disk was then placed into an individual 100 mL vial containing 40 mL of MIBK solvent. Tweezers were used at all times when handling the sample disks to ensure that the silicone surface of the sample was not contaminated or damaged. The solvent vial was then covered with a lid and left to sit on the laboratory bench for 30 minutes. After this period, the disks were removed from the solvent and placed silicone coated side up on a clean tissue paper. 4. The solvent was allowed to evaporate from the sample disc without wiping or blotting the sample. 5. The final coat weight of each sample disc was then determined. 6. Percent extractable was calculated using the following formula:
number
[0163] Reference Example 8.6.4 ROR Evaluation The rub-off resistance percent (ROR%) test (sometimes called anchorage index) measures the amount of cured silicone remaining after a coated substrate is subjected to surface abrasion. It indicates how strongly the cured coating film is anchored to the substrate, the higher the ROR%, the better. The ROR% is measured immediately after the coated substrate is removed from the curing oven. Two sample discs are prepared from each coated substrate, and the silicone present in each sample disc of coated substrate is then measured via an Oxford Instruments Lab-X 3500 Benchtop XRF analyzer. Each sample disc of coated substrate is then abraded in a manner similar to the "Taber method" by contacting it with felt under a load of 1.9 kg using an automated abrasion device. The ROR% is calculated as follows: ROR%=(W f / W i ) x 100 W i = Initial coat weight (before wear) W f = Final coat weight (after wear)
[0164] The release coating compositions prepared as described in Reference Example 6 were first screened by using a TA DSC-Q200 by using the test method as a heating rate of 10°C / min from 40°C to 180°C under N2 protection. The release coating compositions were then coated on UPM glassine paper at 1.3 g / m2 using a handsheet coater. 2and cured for 10 seconds at 182° C. The resulting release liner samples were evaluated for extractables and ROR by the methods of Reference Examples 7 and 8, respectively. The results are shown in Table 7. [Table 7]
[0165] Without being bound by theory, it is believed that consumers prefer short dwell times for release coating applications because shorter dwell times allow for faster line speeds and higher production efficiency. High rub-off resistance is an indication that the coating is well adhered to the substrate, and therefore it is desirable to have high rub-off resistance (high initial rub-off resistance) at short dwell times. DSC data showed that the new hyperbranched crosslinker sample 2 produced a release coating composition with a much lower peak temperature (52°C lower) than the comparative release coating containing conventional crosslinker 2, indicating that the former has much higher reactivity than the composition with conventional crosslinker 2. Higher reactivity is desirable for faster cure (lower extractables at shorter dwell times and faster line speeds). This observation was confirmed by pilot coater testing. Under the same conditions, the release coating composition containing the new hyperbranched crosslinker sample 2 had a much lower extractables than the comparative composition containing conventional crosslinker 2. However, the ROR% of the release coating containing the new hyperbranched crosslinker was worse than the comparative composition under the conditions tested in this example. Therefore, the new hyperbranched crosslinker is a good crosslinker when used alone for applications where easy and fast cure (lower extractable % at shorter residence time and faster line speed) and moderate adhesion requirements are required. When the new hyperbranched crosslinker is used as a co-crosslinker in combination with a conventional crosslinker, such as conventional crosslinker 2, both the extractable % and ROR % were improved. Thus, the new hyperbranched crosslinker is a good co-crosslinker and can improve the cure performance of release coating compositions and get both the effects of fast cure and good adhesion at the same time.
[0166] The polyfunctional organohydrogensiloxanes described above can be functionalized and formulated into adhesive compositions. The starting materials in Table 8 were used in the following examples. [Table 8-1] [Table 8-2]
[0167] Lap shear substrates used for testing adhesives made from the adhesive compositions were as follows: Alclad aluminum type AD Q-Panels 2024T3 were available from Q-Lab Corporation, 800 Canterbury Rd., Cleveland, OH 44145 USA. Polybutylene terephthalate (PBT) panels were available from Rocholl GmbH, Schwarzacher Str. 15 D-74858 Aglasterhausen, Germany.
[0168] Reference 9. Preparation and measurement of lap shear samples. 1 inch by 3 inch panels of the various substrates were cleaned with acetone. Bond lines were obtained using Spheriglass spacer beads appropriate for the application (Potters Industries Inc., 350 North Baker Drive, Canby, OR 97013-0607). Bond areas were 1 inch by 2.5 inches. 3 / 8 inch binder clips were used to hold the substrates in place during cure. Curing was performed at 100° C. and 1 hour. Testing was performed on an Instron 5566 Tensiometer (Instron, 825 University Ave., Norwood, MA 02062-2643) at 2 inches per minute.
[0169] Reference Example 10. Moving Die Rheometer (MDR) Measurements The maximum speed, time to total 90% cure (T90), final cure speed, final torque, and TS2 were measured according to the process specified in ASTM D5289-95 (2001) "Standard Test Method for Rubber Property-vulcanization Using Rotorless Cure Meters". The adhesive composition was cured for 30 minutes at 100°C and 1 arc degree using a rheometer, Premier™-MDR by Alpha Technologies (6279 Hudson Crossing Parkway, #200 Hudson, Ohio 44236, USA).
[0170] Comparative Example 11. Comparative Adhesives 11 and 12 contained methacryloxypropyl terminated linear PDMS with different filler loadings and were prepared as follows: To a mixer was added methacryloxypropyl terminated polydimethylsiloxane (TC-2000, 51.83 g) and TS-530 fumed silica. The mixture was stirred for 10 minutes. To the mixture was added EA-3013 (14.90 g), Z-6030 silane (1.54 g), triallylisocyanurate (0.39 g), a solution of 2-mercaptobenzothiazole (0.12 g) in Silquest A-186 silane (0.46 g), a solution of tri-n-butyl titanate (0.47 g) in Z-2306 (1.42 g) and A1110 (0.09 g) in Z-2306 (0.08 g). The resulting formulation was mixed until homogenous. Methylbenzoyl peroxide paste (2.24 g) was added. The resulting formulation was mixed again for 10 minutes and degassed under vacuum for 30 minutes to provide Comparative Adhesives 11 and 12. Comparative Adhesives 11 and 12 contained 6% and 9% fumed silica, respectively.
[0171] Comparative Example 12. Comparative Adhesive 13 (EA-7100), a commercial adhesive containing a dumbbell-type polydimethylsiloxane crosslinker and 17% filler, was prepared as follows: To the mixture was added MB-2030 (2897 g), SFD-120 polymer (1636 g), OS-20 fluid (271 g), and ETS-900 (also known as OFS-1579, 4.89 g). The mixture was inerted with a nitrogen purge and stirred for 10 minutes (dissolver blade = 500 rpm, scraper blade = 20 rpm). To the homogenized mixture was added butylated hydroxytoluene (1.4 g), stripped MH-1109 (98.8 g), and allyl methacrylate (233 g). The mixture was stirred (250 rpm; 20 rpm) for an additional 10 minutes at room temperature, at which point platinum catalyst (2-0707, 6.4 g) was added to the mixture. The mixture was stirred (250 rpm; 20 rpm) for an additional 10 minutes, after which the temperature was set to 60°C. The temperature was held at 60°C for 30 minutes and then cooled, and when the temperature had dropped to less than 50°C, diallyl maleate (6.4 g) was added. The mixture was then cooled to less than 30°C, after which MTM (Z-6070, 44.2 g) was added. The mixture was then heated to 60°C and held (250 rpm; 20 rpm) for 30 minutes, the temperature was increased to 85°C, and a vacuum of 5-6 Torr was applied for 40 minutes. Methacryloxypropyl-terminated dumbbell-shaped polydimethylsiloxane (PDMS) was obtained as a white viscous paste.
[0172] In a mixer, methacryloxypropyl-terminated dumbbell-shaped PDMS (2200 g), EA-3013ETM resin / polymer (593 g), 3-1719 (3 g), and Tinopal OB (0.61 g) were charged. The mixture was mixed (200 rpm; 20 rpm) for 10 minutes at 10° C. To the homogenous mixture, benzoyl peroxide paste (Perkadox L-50S-ps, 90.48 g), Z-6030 silane (60.4 g), triallyl isocyanurate (15 g), and a solution of 2-mercaptobenzothiazole (4.6 g) in A186 (aka KBM-303, 18.1 g) were added. The mixture was mixed (200 rpm; 20 rpm) again for 10 minutes at 10° C. A solution of tri-n-butyl titanate (18.7 g) in IBTMS (Z-2306, 56.7 g) and A1110 (3.4 g) in IBTMS (3.4 g) was added. The preparation was mixed again (200 rpm; 20 rpm) for 10 minutes at 10° C. and degassed under a vacuum of 200 Torr for 30 minutes at 10° C. to obtain Comparative Adhesive 13.
[0173] Example 13. Adhesives 14 and 15 containing crosslinkers prepared as described herein with different fillers were prepared as follows: In a typical synthesis, 43 g of MH4Q (Gelest) and 301 g of heptane were mixed in a 1 L flask using a Dean Stark fitted with a mechanical stirrer, thermocouple, and a water-cooled condenser equipped with a N2 bubbler. Approximately 90 g of heptane was removed by azeotropic distillation at 100-101 °C. The pot temperature was then cooled to 60 °C and 1.44 g of a 3.82% tris(pentafluorophenyl)borane (BCF) / toluene solution was added to the flask. 294.6 g of silanol fluid (DMS-S42) was slowly added to the flask. The pot temperature was maintained at 50-60 °C. After 3 hours, the heat was removed and 18.6 g of neutral activated alumina was added. After stirring for >3 h, the alumina was filtered off through a 0.45 μm filter membrane. Volatiles were removed by rotary evaporation (<1 mmHg) at 80° C. for 30 min and 100° C. for 1 h. A crosslinker sample was labeled G1Si-H and was recovered as a viscous fluid (285.4 g).
[0174] To a mixer was added G1Si-H (50.01 g), butylated hydroxytoluene (15.5 mg), allyl methacrylate (1.63 g), and optional vinyl functional monomer (0-20 mole % based on allyl methacrylate). The mixture was homogenized with stirring for 10 minutes, at which point platinum catalyst (2-0707, 0.104 g) was added. The mixture was heated at 70°C for 1 hour. The mixture was allowed to cool to 50°C and diallyl maleate (92 mg) was added. Fumed silica (TS-530) was added and the mixture was mixed thoroughly to yield a clustered functional organosiloxane, labeled Polysiloxane B.
[0175] Polysiloxane B (55.19 g), EA-3013 (14.88 g), Z-6030 silane (1.52 g), triallyl isocyanurate (0.38 g), a solution of 2-mercaptobenzothiazole (0.12 g) in Silquest A-186 silane (0.45 g), a solution of tri-n-butyl titanate (0.47 g) in Z-2306 (1.42 g) and A1110 (0.08 g) in Z-2306 (0.08 g) were mixed until homogeneous. Methylbenzoyl peroxide paste (2.26 g) was added. The preparation was mixed again for 10 minutes and degassed under vacuum for 30 minutes to give adhesives 14 and 15 with 6% and 9% fumed silica, respectively.
[0176] Example 14. Adhesive 16 containing a crosslinker prepared as described herein with 17% silica was prepared as follows: To a mixer was added MB-2030 (1672 g), SFD-120 polymer (944 g), OS-20 fluid (156.6 g), and ETS-900 (aka OFS1579, 2.81 g). The mixture was inerted with a nitrogen purge and stirred for 10 minutes (dissolver blade = 500 rpm, scraper blade = 20 rpm). To the homogenized mixture was added butylated hydroxytoluene (1.22 g), tetrakis(dimethylsilyl)silane (78.20 g), allyl methacrylate (146.0 g), and optional vinyl functional monomer (0-20 mole % based on allyl methacrylate). The mixture was stirred (250 rpm; 20 rpm) at room temperature for an additional 10 minutes at which point platinum catalyst (2-0707, 3.90 g) was added to the mixture. The mixture was stirred (250 rpm; 20 rpm) for an additional 10 minutes before the temperature was set to 60°C. The temperature was held at 60°C for 30 minutes before cooling and when the temperature had dropped below 50°C, diallyl maleate (3.69 g) was added. The mixture was then heated to 60°C and held (250 rpm; 20 rpm) for 30 minutes, the temperature was increased to 85°C and a vacuum of 5-6 Torr was applied for 40 minutes. The clustered functional organosiloxane was labeled Polysiloxane A and was obtained as a white viscous paste.
[0177] Polysiloxane A (573.5 g), EA-3013 (154.60 g), 3-1719 (0.81 g), and Tinopal OB (0.16 g) were mixed for 10 minutes at 10° C. To the homogenous mixture was added benzoyl peroxide paste (Perkadox L-50S-ps, 23.62 g), Z-6030 silane (15.74 g), triallyl isocyanurate (3.92 g), and a solution of 2-mercaptobenzothiazole (1.21 g) in Silquest A-186 silane (4.73 g). The mixture was mixed again for 10 minutes at 10° C. A solution of tri-n-butyl titanate (4.89 g) in Z-2306 (14.80 g) and A1110 (0.87 g) in Z-2306 (0.88 g) was added. The preparation was mixed again for 10 minutes at 10° C. and degassed under a vacuum of 200 Torr for 30 minutes at 10° C. to obtain Comparative Adhesive 16. The cure profile was evaluated according to the method of Reference Example 10. The results are shown in Table 9. [Table 9]
[0178] The adhesive performance of the adhesive prepared as described above was evaluated according to Reference Example 9. The results are shown in Table 10 below. Table 10, Table 11, and Table 12. Adhesion performance. [Table 10]
[0179] Table 10 shows that Adhesive 14, made from an adhesive composition containing the new clustered functional organosiloxanes described herein, had better (stronger) adhesion to both aluminum and PBT under the test conditions. [Table 11]
[0180] Table 11 shows that Adhesive 15, made from an adhesive composition containing the new clustered functional organosiloxanes described herein, had better (stronger) adhesion to both aluminum and PBT under the test conditions. [Table 12]
[0181] Industrial Applicability A new method for preparing polyfunctional organohydrogensiloxanes with branched end groups linked to linear polydiorganosiloxanes through oxygen atoms has been developed. This method provides the advantage of minimizing crosslinking by controlling the dendrimer structure as desired. For example, by controlling the ratio of branched polyorganohydrogensiloxanes to hydroxyl-terminated polydiorganosiloxanes, polyfunctional organohydrogensiloxanes can be obtained with two branched moieties linked to one linear polydiorganosiloxane end through oxygen atoms. The polyfunctional organohydrogensiloxanes can provide advantages over commercially available crosslinkers when used in release coating compositions. Alternatively, the polyfunctional organohydrogensiloxanes can be functionalized with different curable groups to form clustered functional organosiloxanes that can be used in different curable compositions. The clustered functional organosiloxanes can provide improved adhesion when adhesive compositions containing the clustered functional organosiloxanes are applied to a substrate and cured on certain substrates.
[0182] Definitions and Use of Terms The abbreviations used herein have the definitions in Table 5 below. [Table 13]
[0183] All amounts, ratios and percentages are by weight unless otherwise indicated. The amounts of all starting materials in the composition total 100% by weight. The Summary and Abstract of the Invention are incorporated herein by reference. The articles "a," "an," and "the" each refer to one or more, unless otherwise indicated by the context of the specification. The singular includes the plural unless otherwise indicated. The disclosure of a range includes the range itself and any subsumed within the range, as well as the endpoints. For example, the disclosure of a range of 2.0 to 4.0 includes not only the range 2.0 to 4.0, but also 2.1, 2.3, 3.4, 3.5, and 4.0 individually, as well as any other numbers subsumed within the range. Further, for example, the disclosure of a range of 2.0 to 4.0 also includes subsets, for example, 2.1 to 3.5, 2.3 to 3.4, 2.6 to 3.7, and 3.8 to 4.0, as well as any other subsets subsumed within that range. Similarly, a disclosure of a Markush group includes the group as a whole, as well as any individual members and subgroups subsumed therein. For example, disclosure of the Markush group "a hydrogen atom, an alkyl group, an alkenyl group, or an aryl group" includes the individual members alkyl, the subgroups alkyl and aryl, and any other individual members and subgroups subgrouped therein.
[0184] "Alkyl" means a branched or unbranched saturated monovalent hydrocarbon group. Examples of alkyl groups include methyl, ethyl, propyl (including n-propyl and / or iso-propyl), butyl (including iso-butyl, n-butyl, tert-butyl, and / or sec-butyl), pentyl (including iso-pentyl, neopentyl, and / or tert-pentyl); and n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl, as well as branched saturated monovalent hydrocarbon groups having 6 or more carbon atoms. An alkyl group has at least 1 carbon atom. Alternatively, an alkyl group may have 1 to 18 carbon atoms, alternatively 1 to 12 carbon atoms, alternatively 1 to 6 carbon atoms, alternatively 1 to 4 carbon atoms, alternatively 1 to 2 carbon atoms, or alternatively 1 carbon atom.
[0185] "Aralkyl" and "alkaryl" refer to an alkyl group having a pendant and / or terminal aryl group, or an aryl group having a pendant alkyl group, respectively. Exemplary aralkyl groups include benzyl, tolyl, xylyl, dimethylphenyl, phenylmethyl, phenylethyl, phenylpropyl, and phenylbutyl. Aralkyl groups have at least 7 carbon atoms. Monocyclic aralkyl groups may have 7 to 12 carbon atoms, alternatively 7 to 9 carbon atoms, alternatively 7 to 8 carbon atoms. Polycyclic aralkyl groups may have 7 to 17 carbon atoms, alternatively 7 to 14 carbon atoms, alternatively 9 to 10 carbon atoms.
[0186] "Alkenyl" means a branched or unbranched monovalent hydrocarbon group having a double bond. Alkenyl groups include vinyl, allyl, and hexenyl. Alkenyl groups have at least two carbon atoms. Alternatively, alkenyl groups can have 2 to 12 carbon atoms, alternatively 2 to 10 carbon atoms, alternatively 2 to 6 carbon atoms, alternatively 2 to 4 carbon atoms, or alternatively 2 carbon atoms.
[0187] "Alkynyl" means a branched or unbranched monovalent hydrocarbon group having a triple bond. Alkynyl groups include ethynyl and propynyl. Alkynyl groups have at least two carbon atoms. Alternatively, alkynyl groups can have 2 to 12 carbon atoms, alternatively 2 to 10 carbon atoms, alternatively 2 to 6 carbon atoms, alternatively 2 to 4 carbon atoms, or alternatively 2 carbon atoms.
[0188] "Aryl" means a hydrocarbon group derived from an arene by removal of a hydrogen atom from a ring carbon atom. Aryl is exemplified by, but not limited to, phenyl and naphthyl. Aryl groups have at least 5 carbon atoms. Monocyclic aryl groups may have 5 to 9 carbon atoms, alternatively 6 to 7 carbon atoms, alternatively 6 carbon atoms. Polycyclic aryl groups may have 10 to 17 carbon atoms, alternatively 10 to 14 carbon atoms, alternatively 12 to 14 carbon atoms.
[0189] "Carbocycle" and "carbocyclic" refer to a hydrocarbon ring. A carbocycle may be monocyclic or polycyclic, for example having two or more rings. A bicyclic carbocycle may be a fused, bridged, or spiropolycyclic ring. A carbocycle has at least three carbon atoms. A monocyclic carbocycle may have 3 to 9 carbon atoms, alternatively 4 to 7 carbon atoms, alternatively 5 to 6 carbon atoms. A polycyclic carbocycle may have 7 to 17 carbon atoms, alternatively 7 to 14 carbon atoms, alternatively 9 to 10 carbon atoms. A carbocycle may be saturated (e.g., cyclopentane or cyclohexane), partially unsaturated (e.g., cyclopentene or cyclohexene), or fully unsaturated (e.g., cyclopentadiene or cycloheptatriene).
[0190] "Cycloalkyl" refers to a saturated hydrocarbon group containing a carbon ring. Cycloalkyl groups are exemplified by cyclobutyl, cyclopentyl, cyclohexyl, and methylcyclohexyl. Cycloalkyl groups have at least three carbon atoms. Monocyclic cycloalkyl groups may have 3 to 9 carbon atoms, alternatively 4 to 7 carbon atoms, alternatively 5 to 6 carbon atoms. Polycyclic cycloalkyl groups may have 7 to 17 carbon atoms, alternatively 7 to 14 carbon atoms, alternatively 9 to 10 carbon atoms.
[0191] "Monovalent hydrocarbon group" means a monovalent group composed of hydrogen and carbon atoms. Monovalent hydrocarbon groups include alkyl, aralkyl, alkenyl, alkynyl, and cycloalkyl groups, as defined above.
[0192] "Monovalent halogenated hydrocarbon group" means a monovalent hydrocarbon group in which one or more hydrogen atoms bonded to a carbon atom are replaced, by formula, with a halogen atom. Halogenated hydrocarbon groups include haloalkyl groups, halogenated carbocyclic groups, and haloalkenyl groups. Halogenated alkyl groups (or haloalkyl groups) include the above alkyl or cycloalkyl groups in which one or more of the hydrogen atoms are replaced by a halogen atom, such as F or Cl. Haloalkyl groups include fluorinated alkyl and cycloalkyl groups such as trifluoromethyl (CF3), fluoromethyl, trifluoroethyl, 2-fluoropropyl, 3,3,3-trifluoropropyl, 4,4,4-trifluorobutyl, 4,4,4,3,3-pentafluorobutyl, 5,5,5,4,4,3,3-heptafluoropentyl, 6,6,6,5,5,4,4,3,3-nonafluorohexyl, 8,8,8,7,7-pentafluorooctyl, 2,2-difluorocyclopropyl, 2,3-difluorocyclobutyl, 3,4-difluorocyclohexyl, and 3,4-difluoro-5-methylcycloheptyl; and chlorinated alkyl and cycloalkyl groups such as chloromethyl, 3-chloropropyl, 2,2-dichlorocyclopropyl, and 2,3-dichlorocyclopentyl. Haloalkenyl groups include chloroallyl groups. Halogenated aryl groups include chlorobenzyl and fluorobenzyl.
[0193] The term "comprising" and its derivatives, such as "comprise" and "comprises," are used herein in their broadest sense to mean and encompass the notions of "including," "include," "consist(ing) essentially of," and "consist(ing) of." The use of "for example," "eg," "such as," and "including" to list examples does not limit the examples listed. Thus, "for example" or "such as" means "for example, but not limited to" or "such as, but not limited to," and includes other similar or equivalent examples.
[0194] Commercially available sources of starting materials include: Dow Silicones Corporation means Dow Silicones Corporation, Midland, Michigan, USA; Gelest means Gelest, Inc., Morrisville, Pennsylvania, USA; Millipore Sigma is (Sigma Aldrich), St. Louis, Missouri, USA;
[0195] Generally, as used herein, a hyphen or dash in a range of values means "to" or "through," ">" means "above" or "greater-than," "≧" means "at least" or "greater-than or equal to," "<" means "below" or "less-than," and "≦" means "at most" or "less-than or equal to." Each of the foregoing patent applications, patents, and / or patent publications is expressly incorporated herein in its entirety in one or more non-limiting embodiments on an individual basis.
[0196] It is to be understood that the scope of the appended claims is not limited to the expressions described in the detailed description and to the specific compounds, compositions, or methods, which may vary among the specific embodiments falling within the scope of the appended claims.
[0197] Release Coating Embodiments of the Invention In embodiment 1, the release coating composition comprises: Formula (i), [ka] zzzImage17zzz wherein subscript n is 2 to 2,000, each subscript d is independently 0 to 995, each R is an independently selected monovalent hydrocarbon radical, and each R 1 are independently selected from the group consisting of monovalent hydrocarbon groups and monovalent halogenated hydrocarbon groups; (ii) a polyorganosiloxane capable of undergoing a hydrosilylation reaction and having an average of at least two silicon-bonded aliphatic unsaturated groups per molecule; (iii) a hydrosilylation reaction catalyst; and (iv) a hydrosilylation reaction inhibitor.
[0198] In embodiment 2 of the release coating composition described in embodiment 1, each subscript d=0 and the polyfunctional organohydrogensiloxane has the formula: [ka] zzzImage18zzz has.
[0199] In embodiment 3, the release coating composition of embodiment 1 or embodiment 2 further comprises one or more additional starting materials selected from the group consisting of: (v) anchor additive, (vi) anti-mist additive, (vii) release control agent, (viii) linear polyorganohydrogensiloxane, and (ix) solvent.
[0200] In embodiment 4, the release coating composition of any one of embodiments 1-3, wherein starting material (ii) has the unit formula: (R 10 R 9 2SiO 1 / 2 ) aa (R 10 R 9 SiO 2 / 2 ) bb (R 10 2SiO 2 / 2 ) cc (R 9 3SiO 1 / 2 ) dd [In the formula, each R 9 are independently selected monovalent hydrocarbon radicals free of aliphatic unsaturation or monovalent halogenated hydrocarbon radicals free of aliphatic unsaturation, and each R 10 are independently selected from the group consisting of alkenyl and alkynyl, the subscript aa is 0, 1, or 2, the subscript bb is 0 or greater, the subscript cc is 1 or greater, and the subscript dd is 0, 1, or 2, with the proviso that the quantity (aa+bb) is ≥ 2, the quantity (aa+dd) = 2, and the quantity (aa+bb+cc+dd) is 3 to 2,000.
[0201] In embodiment 5, in the release coating composition described in embodiment 4, the starting material (ii) is i) dimethylvinylsiloxy-terminated polydimethylsiloxane, ii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane); iii) dimethylvinylsiloxy-terminated polymethylvinylsiloxane; iv) trimethylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane); v) trimethylsiloxy-terminated polymethylvinylsiloxane; vi) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane); vii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylphenylsiloxane); viii) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / diphenylsiloxane); ix) phenyl, methyl, vinyl-siloxy terminated polydimethylsiloxanes; x) dimethylhexenylsiloxy-terminated polydimethylsiloxane, xi) dimethylhexenylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane); xii) dimethylhexenylsiloxy-terminated polymethylhexenylsiloxane, xiii) trimethylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane); xiv) Trimethylsiloxy-terminated polymethylhexenylsiloxane xv) dimethylhexenylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane); xvi) dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylhexenylsiloxane) and xvii) substantially linear, or linear polyorganosiloxanes selected from the group consisting of combinations thereof.
[0202] In embodiment 6, the release coating composition of any one of embodiments 1-5, wherein starting material (ii) has the formula: [ka] zzzImage19zzz wherein subscript u is 0 or 1; each subscript t is independently 0 to 995, or 15 to 995; and each R 11 are independently selected monovalent hydrocarbon radicals, and each R 9 are independently selected monovalent hydrocarbon radicals free of aliphatic unsaturation or monovalent halogenated hydrocarbon radicals free of aliphatic unsaturation, as described above, and each R 10 is independently selected from the group consisting of alkenyl and alkynyl, as defined above.
[0203] In embodiment 7, the release coating composition of any one of embodiments 1-6, wherein the hydrosilylation reaction catalyst is selected from the group consisting of Karstedt's catalyst and Ashby's catalyst.
[0204] In embodiment 8, the release coating composition of any one of embodiments 1-7, wherein the hydrosilylation reaction inhibitor is selected from the group consisting of acetylenic alcohols (e.g., 1-ethynyl-1-cyclohexanol), and maleates (e.g., diallyl maleate, bismaleate, or n-propyl maleate), and combinations of two or more thereof.
[0205] In embodiment 9, the release coating composition of any one of embodiments 1-8 further comprises additional starting materials selected from the group consisting of (v) an anchor additive, (vi) an anti-mist additive, (vii) a release modifier, (viii) a substantially linear or linear polyorganohydrogensiloxane, and (ix) a solvent, and two or more of (v), (vi), (vii), (viii), and (ix).
[0206] In embodiment 10, the release coating composition of embodiment 9, wherein the anchor additive is present and comprises a polyorganosilicate resin.
[0207] In embodiment 11, the release coating composition of embodiment 9, wherein the substantially linear or linear polyorganohydrogensiloxane is present and has the unit formula: (HR 12 2SiO 1 / 2 ) v’ (HR 12 SiO 2 / 2 ) w’ (R 12 2SiO 2 / 2 ) x’ (R 12 3SiO 1 / 2 ) y’ [In the formula, each R 12 are independently selected monovalent hydrocarbon radicals, subscript v' is 0, 1, or 2, subscript w' is 1 or more, subscript x' is 0 or more, and subscript y' is 0, 1, or 2, with the proviso that the quantity (v'+y')=2, the quantity (v'+w') is 3 or more, and the quantity (v'+w'+x'+y') is 2 to 1,000.
[0208] In embodiment 12, the release coating composition of embodiment 11, wherein the polyorganohydrogensiloxane is i) dimethylhydrogensiloxy-terminated poly(dimethyl / methylhydrogen)siloxane copolymers; ii) dimethylhydrogensiloxy-terminated polymethylhydrogensiloxane; iii) trimethylsiloxy-terminated poly(dimethyl / methylhydrogen)siloxane copolymers; iv) trimethylsiloxy-terminated polymethylhydrogensiloxane, and v) is selected from the group consisting of two or more of i) to iv).
[0209] Embodiments of the Adhesive Composition of the Invention In embodiment 1, the adhesive composition comprises: A) formula, [ka] zzzImage20zzz wherein subscript n is 2 to 2,000; each subscript d is independently 0 to 995; each R is an independently selected monovalent hydrocarbon radical; and each R 1 is independently selected from the group consisting of monovalent hydrocarbon groups and monovalent halogenated hydrocarbon groups; 8 are independently selected from the group consisting of H and curable groups, provided that at least one R 8 is a curable group; and B) reactive resins and polymers; C) a condensation reaction catalyst; D) a free radical initiator.
[0210] In embodiment 2, the adhesive composition of embodiment 1, wherein each subscript d=0, and the clustered functional organosiloxane has the formula: [ka] zzzImage21zzz has.
[0211] In embodiment 3, in the adhesive composition according to embodiment 1 or embodiment 2, the starting material B) is i) Formula, (R 2’ 3SiO 1 / 2 ) and (SiO 4 / 2 )[where each R 2’ are independently monovalent hydrocarbon groups, provided that at least one R 2’ has aliphatic unsaturation], 2’ 3SiO 1 / 2 ) units (M units), (SiO 4 / 2 a siloxane resin having a molar ratio (M:Q ratio) of 0.5:1 to 1.5:1 to 1.5:1; ii) Formula, (R2’ 3SiO 1 / 2 ) ii and (RSiO 2 / 2 ) hh (D units), wherein subscript hh is 20 to 1000, and subscript ii has an average value of 2; iii) an alkoxy-functional organohydrogensiloxane oligomer having the unit formula: [ka] zzzImage22zzz (HR 22 2SiO 1 / 2 ) ppp (R 22 3SiO 1 / 2 ) qqq (HR 22 SiO 2 / 2 ) rrr (R 22 2SiO 2 / 2 ) sss (R 22 SiO 3 / 2 ) ttt (HSiO 3 / 2 ) uuu (SiO 4 / 2 ) kk [In the formula, each D 1 each independently represents a divalent hydrocarbon group having 2 to 18 carbon atoms; 22 are independently a monovalent hydrocarbon group having 1 to 18 carbon atoms or a monovalent halogenated hydrocarbon group having 1 to 18 carbon atoms (R 1 (such as those described above for R 23 are independently monovalent hydrocarbon radicals having 1 to 18 carbon atoms (R 1the subscript nnn is 0 or 1, the subscript ooo is 0, the subscripts qqq, sss, and ttt are such that 5≧qqq≧0, 5≧sss≧0, the subscript ttt is 0 or 1, the subscript kk is 0 or 1, the subscript nnn>0, and the quantity (mmm+ppp+qqq+rrr+sss+ttt+uuu+kk)≦50, with the proviso that 1 >90 mole % of the groups are linear; and iv) A polyalkoxy end-capped resin-polymer blend comprising the reaction product of a hydrosilylation catalyst.
[0212] In embodiment 4, in any one of the adhesive composition embodiments 1-3, the starting material C) is selected from the group consisting of a) stannic salts of carboxylic acids, b) tin(II) salts of organic carboxylic acids, c) stannous salts of carboxylic acids, d) organotitanium compounds, and e) combinations of two or more of a), b), c), and d) organotitanium compounds.
[0213] In embodiment 5, in the adhesive composition according to any one of embodiments 1 to 4, the starting material D) is selected from the group consisting of azo compounds and organic peroxide compounds.
[0214] In embodiment 6, the adhesive composition according to any one of embodiments 1 to 5 further comprises an additional starting material different from and added in addition to the above-mentioned starting materials A), B), C), and D), the additional starting material being selected from the group consisting of E) dual cure compounds, F) adhesion promoters, G) corrosion inhibitors, H) rheology modifiers, I) drying agents, J) crosslinkers, K) fillers, L) spacers, M) acid scavengers, N) silanol-functional polydiorganosiloxanes, O) fluorescent optical brighteners, P) chain transfer agents, Q) (meth)acrylate monomers, R) polyalkoxy-terminated polydiorganosiloxanes, S) colorants, and combinations of two or more of E), F), G), H), I), J), K), L), M), N), O), P), Q), R), and S).
[0215] In embodiment 7, the adhesive composition of embodiment 6 further comprises E) a dual cure compound selected from the group consisting of methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane, acryloxypropyltriethoxysilane, methacryloxypropyltriethoxysilane, methacryloxypropylmethyldimethoxysilane, acryloxypropylmethyldimethoxysilane, acryloxypropyldimethylmethoxysilane, methacryloxypropyldimethylmethoxysilane, and combinations of two or more thereof.
[0216] In embodiment 8, the adhesive composition according to embodiment 6 or embodiment 7 further comprises F) an adhesion promoter selected from the group consisting of β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-aminopropyltrimethoxysilane, triallyl isocyanurate, trimethoxysilyl-terminated polydimethylsiloxane, and combinations of two or more thereof.
[0217] In embodiment 9, the adhesive composition of any one of embodiments 6 to 8 further comprises G) a corrosion inhibitor, wherein the corrosion inhibitor is selected from the group consisting of 2-mercaptobenzothiazole, 2,5-dimercapto-1,3,4-thiadiazole, mercaptobenzotriazole, alkylthiadiazole, and combinations of two or more thereof.
[0218] In a tenth embodiment, the adhesive composition according to any one of the sixth to ninth embodiments comprises an alkoxysilane.
[0219] In embodiment 11, the adhesive composition of embodiment 10, wherein the alkoxysilane is selected from the group consisting of vinyltrimethoxysilane, vinyltriethoxysilane, methyltrimethoxysilane, isobutyltrimethoxysilane, and combinations of two or more thereof.
[0220] In a twelfth embodiment, the adhesive composition according to any one of the sixth to eleventh embodiments further comprises K) a filler, which comprises fumed silica.
[0221] In embodiment 13, the adhesive composition according to any one of embodiments 6 to 12 further comprises L) a spacer, the spacer comprising glass beads.
Claims
1. Unit formula, [Formula 1] wherein subscript n is 2 to 2,000; each subscript d is independently 0 to 995; subscript o′=0 to 100; subscript n′=(o′+1); each R is an independently selected monovalent hydrocarbon radical; and each R 1 is independently selected from the group consisting of monovalent hydrocarbon groups and monovalent halogenated hydrocarbon groups; 8 is a hydrogen atom or a curable group, provided that at least one R 8 is a curable group other than hydrogen.
2. The subscript o′=0 and said clustered functional organosiloxane has the formula: [chemical 2] 2. The clustered functional organosiloxane of claim 1 having the formula:
3. Each subscript d=0 and said clustered functional organosiloxane has the formula: [C3] 3. The clustered functional organosiloxane of claim 2 having the formula:
4. The subscript n is 2 to 1,000, each R is an alkyl group having 1 to 6 carbon atoms, and each R 1 is selected from the group consisting of alkyl groups having 1 to 20 carbon atoms, alkenyl groups having 2 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms, and halogenated alkyl groups having 1 to 20 carbon atoms.
5. subscript n is 5 to 50, each R is methyl, and each R 1The clustered functional organosiloxane of any one of claims 1 to 4, wherein is independently selected from the group consisting of methyl, vinyl, phenyl, and trifluoropropyl.
6. A process for preparing a product comprising the steps of: 1) A) a boron-containing Lewis acid; B) formula, [C4] wherein the subscript n is from 2 to 2,000, and each R 1 are independently selected from the group consisting of monovalent hydrocarbon groups and monovalent halogenated hydrocarbon groups; and C) formula, [C5] wherein each subscript d is independently 0 to 995 and each R is an independently selected monovalent hydrocarbon radical, thereby preparing the product, the product comprising a polyfunctional organohydrogensiloxane and a H 2 The method includes a by-product comprising:
7. The process of claim 6, carried out at a temperature of from 5°C to 70°C.
8. The subscript n is from 2 to 1,000, and each R 1 is selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and a halogenated alkyl group having 1 to 20 carbon atoms.
9. C) the polyorganohydrogensiloxane has the formula: [C6] The method according to any one of claims 6 to 8, comprising:
10. The method further comprises the step of recovering the polyfunctional organohydrogensiloxane, the method further comprising the step of 2) recovering the H generated during the formation of the polyfunctional organohydrogensiloxane during step 1) and / or thereafter. 2 10) removing any of the boron-containing Lewis acids from the organohydrogensiloxane dendrimer; 2) neutralizing any residual boron-containing Lewis acids in the organohydrogensiloxane dendrimer; and / or 3) removing any of the fine particles.
11. a) the polyfunctional organohydrogensiloxane; b) a hydrosilylation reaction catalyst; and 11. The method of any one of claims 6 to 10, further comprising the step of: c) combining with starting material a) a reactive species having, on average, at least one aliphatically unsaturated group per molecule capable of addition reacting with silicon-bonded hydrogen atoms of starting material a), and further having, on average, one or more curable groups per molecule, thereby preparing a product comprising a clustered functional organosiloxane.
12. The reactive species has the formula: 4 y SIR 5 (4-y) wherein subscript y is 1 to 3 and each R 4 is an aliphatic unsaturated group capable of undergoing the addition reaction, and each R 5 is the curable group, thereby preparing a product comprising a clustered functional polyorganosiloxane dendrimer.
13. The reactive species has the formula: 6 R 7 [In the formula, each R 6 is an aliphatic unsaturated group capable of undergoing the addition reaction, and each R 7 is the curable group.
14. 1. An adhesive composition comprising: A) Unit formula, [C7] wherein subscript n is 2 to 2,000; each subscript d is independently 0 to 995; subscript o′=0 to 100; subscript n′=(o′+1); each R is an independently selected monovalent hydrocarbon radical; and each R 1 is independently selected from the group consisting of monovalent hydrocarbon groups and monovalent halogenated hydrocarbon groups; 8 is a hydrogen atom or a curable group, provided that at least one R 8 is a curable group other than hydrogen; B) reactive resins and polymers; C) a condensation reaction catalyst; D) a free radical initiator; and and optionally, E) a dual cure compound, F) an adhesion promoter, G) a corrosion inhibitor, H) a rheology modifier, I) a drying agent, J) a crosslinker, K) a filler, L) a spacer, M) an acid scavenger, N) a silanol functional polydiorganosiloxane, O) a fluorescent optical brightener, P) a chain transfer agent, Q) a (meth)acrylate monomer, R) a polyalkoxy terminated polydiorganosiloxane, S) a colorant, and additional starting materials selected from the group consisting of two or more of E), F), G), H), I), J), K), L), M), N), O), P), Q), R), and S).
Citation Information
Patent Citations
Silicone resin composition, and cured product thereof
JP2011148981A
Method for curing silicone resin composition
JP2012121960A
Preparation process of clustered functional polyorganosiloxanes, and methods for using them.
JP2013510227A
Hydrosilyl group-containing organopolysiloxane, method for producing the same and addition-curable silicone composition
JP2017031141A