Biodegradable container and plate materials and methods of their manufacture
A biodegradable container material with a cellulosic core and polyester composite surface layer addresses the need for lightweight, strong, flexible, and attractive packaging by combining cellulosic material with a polyester layer, enhancing durability and biodegradability.
Patent Information
- Application Number
- JP2021541313
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-21
- Filing Date
- 2020-01-20
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-01-20
AI Technical Summary
Existing biodegradable packaging materials, such as flower pots and food packaging, lack a combination of light weight, high strength, flexibility, resistance to water and oils, and attractive visual and tactile properties, leading to unsatisfactory performance and environmental waste.
A biodegradable container or plate material comprising a layer of cellulosic material combined with a composite surface layer containing a polyester derived from aliphatic polyols and polycarboxylic acids, particularly tricarboxylic acids, to create a structure with varying layers of polyester and polyester-free cellulose, enhancing strength and flexibility while maintaining biodegradability.
The material achieves high wet strength, resistance to water and oils, and attractive appearance, reducing waste and environmental impact by providing a durable yet biodegradable solution for packaging and containers.
Smart Images

Figure 0007555934000001 
Figure 0007555934000002 
Figure 0007555934000003
Abstract
Description
[Technical field]
[0001] The present invention relates to biodegradable container and plate materials and methods for their manufacture. In particular, the present invention relates to biodegradable container and plate materials that exhibit one or more of the following properties: light weight, high (wet) strength, a desirable degree of flexibility, good (temporary) resistance to water, oil and fat, and attractive visual and tactile properties. [Background technology]
[0002] Many products sold are sold in some form of packaging. The packaging is intended to protect the product from the external environment and to hold the product together. The packaging will be discarded at some point in its life cycle. To limit the ecological footprint of a product, it is highly desirable that the product is biobased, non-toxic, recyclable, and biodegradable if it enters the environment. Biodegradability is defined, for example, in ASTM D5511 and ASTM D5538. On the other hand, packaging materials need to be able to withstand environmental influences before being discarded, and depending on the packaged product, the packaging material may need to be able to withstand influences from one or more of moisture, liquid water, oils and fats, as well as mechanical forces for long periods of time. In addition, depending on the use, attractive visual and tactile properties may be important.
[0003] An example of a particularly complex packaging material is a flowerpot. Many plants are sold to consumers in plastic flowerpots, for example polypropylene plastic flowerpots. These flowerpots have a relatively short useful life when sold to consumers, because the plant is either removed from the pot and planted in the ground or in another container, or the plant itself has a relatively short life, for example in the case of kitchen herbs and many indoor and outdoor plants. In these cases, the pot itself or the pot with the remains of the plant is discarded. Rapid disposal therefore implies that a material is required that produces little waste and is easy to handle when discarded. On the other hand, if a plant is grown in a pot, the pot must be able to withstand not only the conditions in which the plant grows, but also the conditions that are commonly found during transportation, storage and use.
[0004] The need for a flower pot that meets the described requirements is extensively discussed in EP 3199018 A1. It is shown that the problem is solved by providing a biodegradable paper vessel, constructed by waterproofing recycled or non-recycled white cardboard or brown kraft paper, by treating the surface paper with a special resin polymer. However, this patent application does not have a description of the nature of the proposed special resin.
[0005] US Patent Publication No. 2018000017 describes a biodegradable flower pot, particularly intended for growing seedlings. The pot is particularly intended for the situation where a seedling grows in the pot and, when the seedling approaches maturity, the pot is planted in the ground together with the seedling without the need to remove the seedling from the pot. This reference describes a biodegradable flower pot provided with additives, such as wax emulsions, polyvinyl alcohol, polyvinyl acetate, or combinations thereof, to improve the tensile strength, hydrophobicity, and fungal growth resistance of the pot.
[0006] The materials proposed in this reference have several disadvantages: First, they have low solubility in water, which may contribute to imparting hydrophobicity to the flowerpot, but which may also make it difficult to form a homogeneous product.
[0007] Another example of a challenging packaging material is packaging for food products, especially packaging that comes into contact with moisture, oils or fats, or a combination thereof. This packaging needs to be able to withstand the effects of these substances over the shelf life of the packaged food product. On the other hand, the packaging is generally for single use, thus resulting in waste limitations. Summary of the Invention [Problem to be solved by the invention]
[0008] The problem underlying the present invention is to provide a biodegradable container or plate material, in particular a biodegradable packaging container, in some embodiments a biodegradable flower pot, which exhibits one or more, in particular a combination of the following properties: light weight, high (wet) strength, a desirable degree of flexibility, good (temporary) resistance to water, oil and fat, and attractive visual and tactile properties. The present invention solves this problem. [Means for solving the problem]
[0009] The biodegradable container or plate material according to the invention exhibits one or more, particularly combinations of the following properties: light weight, high (wet) strength, desirable flexibility, good (temporary) resistance to water, oil and fat, and attractive visual and tactile properties.
[0010] The present invention relates to a biodegradable container or plate material comprising a layer of cellulosic material, the layer of cellulosic material being provided with a composite surface layer comprising the cellulosic material and a polyester derived from an aliphatic polyol having 2 to 15 carbon atoms and an aliphatic polycarboxylic acid having 3 to 15 carbon atoms, wherein the polycarboxylic acid comprises at least 50% by weight of a tricarboxylic acid.
[0011] It is noted that the use of polyesters of diols and diacids in the manufacture of paper-based products is described.
[0012] WO 2018 / 067006 describes biodegradable and compostable food packaging units derived from molded pulp material, which preferably contain in the range of 0.5-20% by weight of biodegradable aliphatic polyesters such as PBS (polybutylene succinate), PHB (polyhydroxybutyrate), PHA (polyhydroxyalkanoate), PCL (polycaprolactone), PLA (polylactic acid), PGA (polyglycolic acid), PHBH (copolymer of 3-hydroxybutyrate and 3-hydroxyhexanoate) and PHBV (copolymer of 3-hydroxybutyrate and 3-hydroxyvalerate), preferably PBS (polybutylene succinate).
[0013] WO 2009 / 118377 describes biodegradable polyesters that contain units derived from at least a diacid and at least a diol, have long chain branching, and are gel-free, for use in paper-based laminate products.
[0014] US20130101865 describes the use of an aqueous dispersion of at least one biodegradable polyester as a coating for improving the barrier properties of packaging materials made from paper or paperboard, the polyester being in particular a polylactide (polylactic acid), a polycaprolactone, a block copolymer of polylactide and poly-C2-C4-alkylene glycol, a block copolymer of polycaprolactone and poly-C2-C4-alkylene glycol, or a copolyester composed of at least one aliphatic or cycloaliphatic dicarboxylic acid or one of its ester-forming derivatives and at least one aliphatic or cycloaliphatic diol component.
[0015] However, it has been found that the use of polyesters of diols and dicarboxylic acids gives poor results, especially with regard to the dry and wet strength of the resulting materials.
[0016] It is noted that WO 2012 / 140237 describes a composite material comprising a biofiller and at least 2% by weight of a polyester matrix polymer derived from an aliphatic polyol having 2 to 15 carbon atoms and an aliphatic polycarboxylic acid. This reference is directed to providing a composite material as an alternative to medium density fiberboard (MDF), high-density fiberboard (HDF), plywood, oriented strand board (OSB), particleboard, and paper-resin composites such as Formica. The material has been shown to be highly suitable as a building material due to its fire-resistant properties. The material is prepared by mixing the filler with the matrix polymer, by providing the filler in a mold and adding the matrix polymer, or by impregnating a layer of the filler with the matrix polymer. In the examples, large amounts of polymer are used. This reference does not disclose providing a biodegradable container or plate material, including a cellulosic container or plate material, with a composite surface layer comprising a cellulosic material and a polyester.
[0017] WO 2012 / 140238 describes the use of polyester polymers derived from aliphatic polyols having 2 to 15 carbon atoms and aliphatic polycarboxylic acids as coatings or in the manufacture of laminates. Again, this reference does not disclose providing a biodegradable packaging material comprising a cellulosic material provided with a composite surface layer of polyester. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention and preferred embodiments thereof along with their associated advantages will be discussed in more detail below.
[0019] The cellulosic material is provided with a composite surface layer comprising a cellulosic material and a specific polyester. The presence of the composite surface layer is a very important feature of the present invention. It means that when looking at the cross section of the biodegradable container or plate material according to the present invention, part of the material comprises the polyester and part of the material does not comprise the polyester. In other words, the composite surface layer comprising polyester can be distinguished from the layer not comprising polyester. This layer not comprising polyester can be the core layer if both sides of the material are provided with a composite surface layer comprising polyester. If only one side of the object material is provided with a composite surface layer comprising polyester, the layer not comprising polyester can also be present on one side of the object. It has been found that the combination of the composite surface layer comprising polyester and the layer not comprising polyester results in a product with desirable properties, in particular a combination of (wet) strength, barrier properties and flexibility.
[0020] In the biodegradable container or plate material according to any one of the above claims, calculated based on the sum of the composite surface layer containing polyester and the cellulosic material not containing polyester, in a cross section of the biodegradable container or plate material, 5 to 90% of the cross section is the composite surface layer containing polyester and 95 to 10% of the cross section is the cellulosic material not containing polyester, in particular 20 to 80% of the cross section is the composite surface layer containing polyester and 80 to 20% of the cross section is the cellulosic material not containing polyester, preferably 30 to 70% of the cross section is the composite surface layer containing polyester and 70 to 30% of the cross section is the cellulosic material not containing polyester.
[0021] In one embodiment, in the cross section of the biodegradable container or plate material, calculated based on the sum of the composite surface layer containing polyester and the cellulosic material not containing polyester, 1-90% of the cross section is the composite surface layer containing polyester, and 99-10% of the cross section is the cellulosic material not containing polyester. It may be preferred that 2-50% of the cross section is the composite surface layer containing polyester, and 98-50% of the cross section is the cellulosic material not containing polyester. In some embodiments, it may be preferred that 2-30% of the cross section is the composite surface layer containing polyester, and 98-70% of the cross section is the cellulosic material not containing polyester.
[0022] In addition to the layer of cellulosic material and the composite surface layer comprising cellulosic material and polyester, the biodegradable container or plate material can have further layers, such as a non-cellulose containing polyester layer.
[0023] In the biodegradable container or plate material according to the invention, the cellulosic material and the composite surface layer comprising cellulosic material and polyester are bonded at the scale of the cellulose fibers. As discussed below, the composite surface layer is provided by impregnating the cellulosic material with a liquid medium comprising polyester or polycarboxylic acid and its polyalcohol precursor. This means that the cellulosic material in the cellulose-based layer and the cellulosic material in the composite surface layer are continuous.
[0024] Thus, the starting material used in the present invention is based on a cellulose-based object, in particular a cellulose-based container, such as a box, a pot or any other container, or a cellulose-based plate material. The term "cellulosic" is intended to mean that the object comprises at least 50% by weight of cellulose material, for example derived from a source, such as virgin or used paper, virgin or used cardboard, any form of wood or other plant material, or a combination thereof. In particular, the material or container comprises at least 70% by weight, more particularly at least 80% by weight of cellulose material.
[0025] In one embodiment, the cellulosic material is derived from so-called virgin pulp, which is obtained directly from the wood pulping process. This pulp can be derived from any plant material, but mostly from wood. Wood pulp is derived from softwood trees, such as spruce, pine, fir, larch and hemlock, and hardwoods, such as eucalyptus, poplar, aspen and birch. In one embodiment, the cellulosic material includes cellulosic material derived from recycled paper, such as cellulose pulp obtained from regenerated books, papers, newspapers and periodicals, egg cartons, and other recycled paper or cardboard products. A combination of cellulose sources can also be used.
[0026] The cellulosic material may contain other components known in the art.
[0027] In one embodiment, the cellulosic material includes a compound that increases the water resistance or hydrophobicity of the material. Suitable compounds are known in the art and include, for example, alkylketene dimers (AKD) derived from fatty acids obtained by hydrolysis of animal or vegetable fats and oils, or maleated alkenes, such as iso-octadecenyl succinic anhydride (ASA).
[0028] The cellulosic material may also contain inorganic fillers to reduce consumption of more expensive components or to impart particular properties to the composite. Inorganic fillers are known in the art and include, for example, China clay, calcium carbonate, titanium dioxide, and talc.
[0029] The cellulosic material may also include a binder. Binders are known in the art. Examples include carboxymethyl cellulose (CMC), cationic and anionic hydroxyethyl cellulose (EHEC), modified starches, and dextrins.
[0030] In one embodiment, the cellulosic material contains so-called wet strength additives which help ensure that the material retains its strength when wet. Wet strength additives are known in the art and include epichlorohydrin, melamine, urea, formaldehyde, and polyimines.
[0031] In one embodiment, the cellulosic material comprises a so-called dry strength additive, also referred to as a dry strength agent for improving one or more of compressive strength, burst strength, tensile strength, and delamination resistance. Dry strength additives are known in the art. Examples include cationic starch and polyacrylamide (PAM) derivatives.
[0032] These ingredients are known in the art of manufacturing cellulosic materials, and therefore their use is within the purview of those skilled in the art and no further explanation is required.
[0033] The present invention uses polyesters derived from an aliphatic polyol having 2 to 15 carbon atoms and an aliphatic polycarboxylic acid having 3 to 15 carbon atoms, where the polycarboxylic acid comprises at least 50% by weight of a tricarboxylic acid.
[0034] The starting materials for the present invention are aliphatic polyalcohols having 2 to 15 carbon atoms and aliphatic polycarboxylic acids, where the polycarboxylic acids contain at least 50% by weight of tricarboxylic acids.
[0035] The aliphatic polyalcohols used in the present invention contain at least 2 hydroxy groups, in particular at least 3 hydroxy groups. Generally, the number of hydroxy groups is not more than 10, more in particular not more than 8, or even not more than 6, in particular 2 or 3.
[0036] The polyalcohol has from 2 to 15 carbon atoms, more particularly from 3 to 10 carbon atoms.
[0037] The polyalcohol preferably does not have any N or S heteroatoms. More particularly, the polyalcohol preferably does not contain non-carbon groups other than hydroxy groups. More particularly, the polyalcohol is an aliphatic polyalkanol containing only C, H and O atoms.
[0038] In a preferred embodiment of the present invention, the polyalcohol contains a relatively large number of hydroxy groups compared to its number of carbon atoms. For example, the ratio of the number of hydroxy groups to the number of carbon atoms ranges from 1:4 (i.e., one hydroxy group per 4 carbon atoms, or 8 carbon atoms per dialcohol) to 1:0.5 (i.e., two hydroxy groups per carbon atom). In particular, the ratio of the number of hydroxy groups to the number of carbon atoms ranges from 1:3 to 1:0.75, more particularly from 1:2 to 1:0.75. Particularly preferred polyalcohol groups are those in which the ratio ranges from 1:1.5 to 1:0.75. Compounds in which the ratio of hydroxy groups to carbon atoms is 1:1 are considered to be particularly preferred.
[0039] Examples of suitable polyalcohols include tri-alcohols selected from glycerol, sorbitol, xylitol and mannitol, and dialcohols selected from 1,2-propanediol, 1,3-propanediol and 1,2-ethanediol. The use of compounds selected from the group of glycerol, sorbitol, xylitol and mannitol is preferred, the use of glycerol being particularly preferred.
[0040] The preference for glycerol is based on the following: First, glycerol has a melting point of 20° C., which allows for easy processing, especially compared to xylitol, sorbitol, and mannitol, which all have melting points well above 90° C. Furthermore, glycerol has been found to result in high quality polymers, thus combining the use of readily available source materials with good processing conditions and high quality products. Mixtures of various types of alcohols can also be used.
[0041] The polyalcohol preferably consists of at least 50 mol%, preferably at least 70 mol%, more particularly at least 90 mol%, or even at least 95 mol% of glycerol, xylitol, sorbitol, or mannitol, in particular glycerol. In one embodiment, the polyalcohol consists essentially of glycerol.
[0042] The use of glycerol, a by-product of the production of biodiesel by transesterification of glycerides with monoalcohols, is a particular embodiment of the present invention. Suitable monoalcohols include C1-C10 monoalcohols, particularly C1-C5 monoalcohols, more particularly C1-C3 monoalcohols, especially methanol. The glycerides are mono-, di- and esters of glycerol with fatty acids, the fatty acids generally having 10-18 carbon atoms. Suitable methods for producing biodiesel with associated glycerol are known in the art.
[0043] The aliphatic polycarboxylic acid used in the present invention is an aliphatic polycarboxylic acid having 3 to 15 carbon atoms, and the polycarboxylic acid contains at least 50% by weight of a tricarboxylic acid.
[0044] The aliphatic polycarboxylic acid used in the present invention comprises at least two carboxylic acid groups, with the proviso that the polycarboxylic acid comprises at least 50% by weight of tricarboxylic acid.The aliphatic polycarboxylic acid used in the present invention in particular comprises at least three carboxylic acid groups.Generally, the number of carboxylic acid groups is not more than 10, more particularly not more than 8, or even not more than 6.
[0045] The polycarboxylic acid has from 3 to 15 carbon atoms, more particularly from 3 to 10 carbon atoms.
[0046] The polycarboxylic acid preferably does not have any N or S heteroatoms. More particularly, the polycarboxylic acid preferably does not contain any non-carbon groups other than the carboxylic acid groups. More particularly, the polycarboxylic acid is an aliphatic polycarboxylic acid containing only C, H and O atoms.
[0047] In one embodiment, dicarboxylic acid is used. When used, the dicarboxylic acid can be any dicarboxylic acid having two carboxylic acid groups, generally up to 15 carbon atoms. Examples of suitable dicarboxylic acids include itaconic acid, malic acid, succinic acid, glutaric acid, adipic acid and sebacic acid. Itaconic acid and succinic acid can be preferred.
[0048] In the present invention, a tricarboxylic acid is used. The tricarboxylic acid can be any tricarboxylic acid having three carboxylic acid groups, generally up to 15 carbon atoms. Examples include citric acid, isocitric acid, aconitic acid (both cis and trans), and 3-carboxy-cis,cis-muconic acid. The use of citric acid is considered to be preferred for reasons of both cost and availability.
[0049] Where applicable, the polycarboxylic acid may be provided wholly or partly in the form of an anhydride, for example citric anhydride.
[0050] It has been found that the use of tricarboxylic acid results in polyesters with attractive properties.Therefore, the polycarboxylic acid comprises at least 50% by weight of tricarboxylic acid, whether in combination with dicarboxylic acid, other polycarboxylic acid, and mixtures thereof.In one embodiment, the polycarboxylic acid comprises at least 70% by weight, preferably at least 90% by weight, or even at least 95% by weight, calculated based on the total amount of polycarboxylic acid.In one embodiment, the polycarboxylic acid consists essentially of tricarboxylic acid, where the term "essentially" means that other acids can be present in amounts that do not affect the properties of the material.
[0051] In another embodiment of the invention, the acid comprises at least 2% by weight, in particular at least 5% by weight, more in particular at least 10% by weight, preferably at least 30% by weight, of dicarboxylic acid, calculated on the total amount of acid.
[0052] The use of tricarboxylic acids, particularly citric acid, especially in combination with the use of tri-alcohols, such as glycerol, has been found to result in the formation of high quality composite materials.
[0053] Without being bound by theory, the inventors believe there are several reasons why the use of a triacid, especially in combination with a triol, results in the formation of a high quality composite material. First, the use of a triacid, especially in combination with a triol, creates a highly crosslinked polymer, resulting in increased strength.
[0054] Furthermore, when a triacid is used, and preferably also a triol, there is a high possibility that the acid or hydroxyl groups will physically or chemically interact with the active groups on the cellulosic material. This will result in improved bonding of the cellulosic material and the polymer, which is a very important desire in the preparation of composite materials. The degree of interaction can be controlled by the selection of the amount of triacid and trialcohol, as well as by the selection of the degree of polymerization.
[0055] The molar ratio of the polyalcohol to the polycarboxylic acid is controlled by the ratio of the number of reactive groups in the one or more alcohols used to the number of reactive groups in the one or more acids. In general, the ratio of the number of OH groups to the number of acid groups is 5:1 to 1:5. More particularly, the ratio can be 2:1 to 1:2, more particularly 1.5:1 to 1:1.5, more preferably 1.1:1 to 1:1.1. The theoretical molar ratio is 1:1.
[0056] The polymer is formed by combining the alcohol and the acid to form a liquid phase. This can be done by heating the mixture of components to a temperature at which the acid dissolves in the alcohol, especially glycerol, depending on the nature of the compounds. This can be done at a temperature ranging from, for example, 20 to 200°C, such as 40 to 200°C, for example 60 to 200°C, or 90 to 200°C, depending on the nature of the compounds. In one embodiment, the mixture can be heated and mixed at a temperature ranging from 100 to 200°C, especially 100 to 150°C, more especially 100 to 140°C, for 5 minutes to 2 hours, more especially 10 minutes to 45 minutes.
[0057] Optionally, a suitable catalyst can be used for the preparation of the polyester. Suitable catalysts for the production of polyesters are known in the art. Preferred catalysts are heavy metal-free catalysts. Useful catalysts include, but are not limited to, strong acids such as hydrochloric acid, hydroiodic acid and hydrobromic acid, sulfuric acid (H2SO4), nitric acid (HNO3), chloric acid (HClO3), boric acid, perchloric acid (HClO4), trifluoroacetic acid, and trifluoromethanesulfonic acid. Catalysts such as Zn acetate and Mn acetate can also be used, but they may be less preferred.
[0058] Optionally, after polymerization and cooling of the reaction mixture, the mixture can be (partially) neutralized with a volatile base, such as ammonia or an organic amine, to stabilize the polyester solution. Preferred amines are low odor amines, such as, but not limited to, 2-amino-2-ethyl-1,3-propanediol, 2-amino-2-methyl-1-propanol, 2-dimethylamino-2-methyl-1-propanol.
[0059] The biodegradable container or plate material comprising a layer of cellulosic material, the layer of cellulosic material being provided with a composite surface layer comprising a cellulosic material and a polyester derived from an aliphatic polyol having 2-15 carbon atoms and an aliphatic polycarboxylic acid having 3-15 carbon atoms, is generally prepared by contacting the surface of the cellulosic material with a liquid medium comprising the polyester, or its precursors, polycarboxylic acid and polyalcohol, until the cellulosic material is partially, but incompletely, impregnated with the liquid medium, followed by a curing step.
[0060] If it is intended to obtain an object comprising a layer of cellulosic material and a composite surface layer comprising cellulosic material and polyester, it is important that the manufacturing conditions are chosen such that the liquid medium does not penetrate the entirety of the cellulosic material, an effect which is controlled, inter alia, by the following parameters: the amount of liquid medium, the viscosity of the liquid medium, the absorption capacity of the cellulosic material to be impregnated with the liquid medium, and the polymerization rate of the polymer in the imbibed medium.
[0061] The viscosity of the liquid medium is determined by the degree of polymerization of the polyester in the medium and the temperature. The rate of polymerization of the polymer is determined by the presence of a catalyst and the temperature. Taking these parameters into account, it is within the skill of the art to select suitable contact conditions.
[0062] For example, a cellulosic material can be contacted with an aqueous solution of the polyester at room temperature. It is also possible to contact the cellulosic material with the polyester in liquid form at elevated temperature. It is also possible to contact the cellulosic material with a liquid comprising a polyalcohol, a polycarboxylic acid, and a polymerization catalyst under polymerization conditions.
[0063] The liquid medium comprising the polyester or polyester precursor may be applied onto the packaging by methods known in the art, such as dipping, spraying, flowing, rolling, brushing or cascading. Spraying has been found to be particularly suitable for applying a homogeneous layer of resin in small amounts, for example in the range of 1-10% by weight, and is suitable when the cellulosic material has a tendency to rapidly absorb large amounts of resin, for example when the cellulosic material has a high porosity or is relatively hydrophilic, for example when no sizing agent is used.
[0064] Immersion has proven particularly attractive for surfaces having inhomogeneous structures such as angles, corners, depressions, and protrusions.
[0065] After application of the polyester onto the cellulosic material, the resulting impregnated material is subjected to a curing step to increase the degree of polymerization of the polyester. The most important aspect of the curing step is that the polyester is at a reaction temperature, e.g., a product temperature of 80-250°C, especially 100-200°C. Curing can be carried out in heating devices known in the art, e.g., in ovens with oven temperatures of 80°C to 450°C. Various types of ovens can be used, including, but not limited to, belt ovens, convection ovens, microwave ovens, infrared ovens, induction ovens, hot air ovens, conventional baking ovens, and combinations thereof. Curing can be carried out in a single step or multiple steps depending on the desired application. Curing times range from 5 seconds to 2 hours, depending on the application and the type of oven and temperature used. It is within the skill of the art to select suitable curing conditions depending on the desired application and the desired properties.
[0066] Thus, if desired, the impregnated material may be subjected to a drying step before the curing step is carried out. The drying step, which is generally carried out at room temperature, for example at a temperature between 15° C. or 20° C. and 100° C., is carried out to remove water from the composite. The drying step may be carried out for a period of, for example, 0.25 hours to 3 days, depending on the amount of water in the composite, the thickness of the layer, and the temperature.
[0067] The amount of polyester resin present in the biodegradable container or plate material generally ranges from 0.5 to 90% by weight. It is preferred not to use more resin than is necessary to obtain a material with desired properties, since such more resin will only result in additional weight and cost. The amount of resin may be preferred to be 50% by weight or less, particularly 30% by weight or less, and in some embodiments, 20% by weight or less, or even 15% by weight or less. To obtain the effects of the present invention, generally at least 0.5% by weight, particularly at least 1% by weight, of polyester resin will be required.
[0068] As shown above, the biodegradable container or plate material according to the present invention exhibits one or more, particularly a combination of light weight, high (wet) strength, desirable flexibility, good (temporary) resistance to water, oil and fat, and attractive visual and tactile properties. This makes the biodegradable container or plate material suitable for many applications. For example, the biodegradable container or plate material can be used as a replacement for most fossil-based (single-use) plastics, for example for packaging and consumables, which together account for about 40% of the plastic market. Reducing plastic waste and reducing CO2 emissions are top priorities for the EU in environmental protection activities. New legislation is forcing industry to use replacements for fossil-based (non-biodegradable) plastics.
[0069] Particular uses for the material according to the invention include, but are not limited to, flower pots and packaging containers for fat or moisture containing materials, such as meat, fish, vegetables and other food products. In the context of using the material for food packaging, it is worth noting that the polyesters used in the present invention are safe for humans, animals and the environment.
[0070] The present invention is illustrated by, but not limited to, the following examples.
[0071] Example 1 Preparation of a solution of polyol and polycarboxylic acid polyester precursor 12 kg of tap water was heated to 90° C. in a 50 L vessel. 25 kg of citric acid monohydrate (purity >99%) was added under stirring. A solution was obtained at a temperature of 38° C. 12.5 kg of 99% pure glycerol was added to this solution. The solution was cooled to room temperature and further diluted with tap water until a water concentration of 50% was obtained. 0.5% by weight of boric acid was added as a catalyst.
[0072] Example 2 Preparation of Polyester Prepolymer Solutions 1.0 kg of glycerol (>99% purity) and 2.0 kg of citric acid (>99% purity) were placed in a stirred and heated reactor. 9 g of boric acid (0.5 m / m, >99% purity) was added. The mixture was heated to 135° C. for about 15 minutes and maintained at that temperature for 15 minutes, subsequently diluted with tap water to a water content of 50% and cooled.
[0073] Example 3 Partial impregnation of cellulose-based flower pots based on recycled paper Cylindrical molded flower pots made from cellulose fiber pulp, mainly from recycled non-printed book paper, containing 0.5% alkyl succinic anhydride, were used as starting materials. The pots were 9 cm high, 11 cm in top diameter, and 7 cm in bottom diameter. The average weight was 14.2 grams.
[0074] The pot described above was immersed for 6 seconds at room temperature in a solution of the polyester prepolymer described in Example 2. The wet pot was dried for 4 hours at room temperature and cured for 20 minutes in a ventilated oven with an internal temperature of 190° C. The temperature of the final product was 180° C. After curing, the pot weighed an average of 16.7 grams and had a polyester content of 15% by weight. A cross-section of the pot wall showed the presence of a resin-free layer between two resin-containing layers.
[0075] The table below shows the dry strength, the strength after immersion in water for 5 minutes at room temperature, and the strength after immersion in sunflower oil for 10 seconds at room temperature for the starting pots and the pots provided with polyester resin. Four pots were used per measurement. The strength was determined using a universal testing machine (UTM) (Testrometic, M350-20CT) with a plate compression test, measuring the peak force when the pots were placed upside down (bottom against top plate and top against bottom compression plate).
[0076] [Table 1]
[0077] From the table it can be seen that the impregnated pot has higher strength than the starting material.
[0078] Furthermore, the strength of the impregnated pots after immersion in water at room temperature for 5 minutes was reduced by about 30% compared to the strength of the impregnated pots before immersion in the water, and acceptable strength retention was observed, whereas the unimpregnated pots collapsed after immersion in water at room temperature for 5 minutes and did not exhibit acceptable strength retention.
[0079] The strength of the impregnated pots after immersion in sunflower oil at room temperature for 10 seconds remained unchanged, in contrast to the non-impregnated pots, which showed a 30% decrease in strength after immersion in sunflower oil at room temperature for 10 seconds compared to the pots before immersion.
[0080] The impregnated pots were stiffer than the non-impregnated pots, but still showed some flexibility (the upper edges of the pots could be moved 2-3 cm towards each other before the pot broke).
[0081] The application of the impregnation resulted in significantly improved mechanical (wet) strength for water and oil. Moreover, the color of the pot changed from off-white to an attractive light brown.
[0082] Example 4 Partial impregnation of cellulose-based flowerpots based on virgin paper As starting materials, pots were prepared with the same size, shape and weight as the pots used in Example 3. The pots were based on virgin cellulose fibers modified with 0.5 wt% alkyl succinic anhydride. The pots were 9 cm high, 11 cm in diameter at the top and 7 cm in diameter at the bottom. The pots weighed an average of 14.5 grams.
[0083] The pots were immersed for 6 seconds at room temperature in the solution of polyol and polyacid described in Example 1. The wet pots were dried for 4 hours at room temperature and cured for 20 minutes in a ventilated oven with an internal temperature of 190°C, the temperature of the final product being 180°C. After curing, the pots weighed an average of 17.7 grams, which corresponds to a polyester content of 18% by weight. A cross-section of the pot wall showed the presence of a resin-free layer between two resin-containing layers. The pots were much stiffer than the non-impregnated pots, but still showed some flexibility (the upper edges of the pots could be moved 2-3 cm towards each other before the pot broke). Furthermore, the pots had an attractive brown outer surface and very good tactile properties. The latter is probably due to the fact that the tactile properties of the virgin paper pots are better than those of the pots based on recycled paper.
[0084] The strength of the impregnated pots was about 80% higher (average 1332N) than the strength of the pots before impregnation (average 734N) and about 20% higher than the strength of the impregnated pots described in Example 3. The latter may be due to the pots having a slightly higher resin content and the virgin cellulose fibers being longer than those of the recycled paper used in Example 3.
[0085] After immersion in water or oil under the conditions described in the previous examples, the impregnated pots retained most of their strength, while the non-impregnated pots did not.
[0086] Example 5 Impregnation of flower pots based on virgin cellulose - a comparison Comparative pots were prepared by impregnating a virgin cellulose fiber pot with the solution of Example 1 under conditions such that the pot was completely impregnated with resin. The wet pot was dried at room temperature for 4 hours and cured for 20 minutes in a ventilated oven with an internal temperature of 190° C. (final product temperature 180° C.). After curing, the container weighed 41 grams and had a polyester content of about 65% by weight.
[0087] A cross section of the pot wall shows a resin-free layer. Didn't The pot was made entirely from composite materials. The pot has a good brown color, high strength, and a ceramic appearance. However, the pot has little flexibility, which may be a disadvantage in filling and emptying the pot. Moreover, the pot was very fragile. Furthermore, the relatively large weight makes the pot less attractive due to higher material and shipping costs.
[0088] Example 6 Partial impregnation of paper-based food trays A smooth rectangular small food tray (top L*W 21*14cm, bottom 17*10cm, height 5.5cm) made from high density thin walled thermoformed fabric derived from cellulose fiber regenerated from non-printed recycled paper containing 0.6% by weight alkyl succinic anhydride and weighing 20.1 grams was immersed in the solution described in Example 2 for 6 seconds at room temperature. After immersion, the wet tray was dried at room temperature for 4 hours and cured for 20 minutes in a ventilated oven with an internal temperature of 190°C (final product temperature 180°C). After curing, the bowl weighed 22.2 grams and had an estimated polyester content of 10%. A cross section of the tray wall showed the presence of a resin-free layer between two resin-containing layers. The tray was more rigid than the non-impregnated tray, but still showed some flexibility. The top layer had an attractive glossy light brown appearance.
[0089] The oil resistance of the impregnated trays was tested in a ventilated oven at 50°C for 2 hours. 10 drops of sunflower oil were placed on the bottom of the impregnated and non-impregnated trays, respectively. The impregnated trays showed good oil resistance, as no oil penetrated into or through the trays. The oil remained completely on the surface of the trays and the color of the trays remained unchanged. On the non-impregnated trays, the oil penetrated the paper immediately and a dark "wet dye" appeared on the top and bottom of the trays where the oil was applied.
[0090] Example 7 Neutralized Acid To 100 grams of the polyester solution shown in Example 2 was added 1.0 g of 2-amino-2-methyl-1-propanol, commercially available from Angus Chemie under the trade name AMP.
[0091] Cylindrical miniature flower pots similar to those described in Example 3 were treated in the same manner as described in Example 3, and similar characteristics of the material were obtained. In this case, the addition of AMP to the solution stabilized the prepolymer solution. Upon curing the pot, the base evaporates and the polyester further hardens to its final degree of polymerization.
[0092] Example 8 Comparison with polyesters based on diacids and diols Cylindrical molded flower pots made from cellulose fiber pulp, mainly from recycled non-printed book paper, containing 0.5% alkyl succinic anhydride, were used as starting materials. The pots were 8.4 cm high, 11 cm in top diameter, and 7 cm in bottom diameter. The average weight was 13.7 grams.
[0093] Two dipping solutions were prepared with the following respective compositions:
[0094] [Table 2]
[0095] [Table 3]
[0096] The pots described above were immersed in solution A or solution B for 10 seconds at room temperature. The solutions were at a temperature of 45° C. The wet pots were dried at room temperature for 1 hour and cured in a ventilated oven with an internal temperature of 190° C. for 20 minutes.
[0097] The weights of the pots after soaking and drying were as shown below. Values are the average of 6 measurements. The numbers in brackets are the percentage increase compared to the weight of the dry starting pots.
[0098] [Table 4]
[0099] Water uptake was determined after immersing the pots in water for 10 minutes. Values are the average of three measurements. Numbers in brackets are the percentage increase compared to the weight of the dry starting pots.
[0100] [Table 5]
[0101] For both the wet and dry pots, the compressive strength was determined as described in Example 3. For the dry pots, the data was the average of four measurements. For the wet pots, the data was the average of two measurements. The results were as follows:
[0102] [Table 6]
[0103] From the above comparison, it can be seen that the pots impregnated with solution B according to the invention have a higher compressive strength, both in dry and wet conditions, than the pots impregnated with comparative solution A. In addition, the pots impregnated with solution B have a lower water uptake than the pots impregnated with solution A. It should be noted that the pots impregnated with solution B have a lower resin content than the pots impregnated with solution A, making the effect obtained with the polyester according to the invention even more surprising.
Claims
1. 1. A biodegradable container or plate material comprising a layer of cellulosic material, the layer of cellulosic material being provided with a composite surface layer comprising a cellulosic material and a polyester derived from an aliphatic polyalcohol having 2 to 15 carbon atoms and an aliphatic polycarboxylic acid having 3 to 15 carbon atoms, the polycarboxylic acid comprising at least 50% by weight of a tricarboxylic acid, the cellulosic material in the layer of cellulosic material being continuous with the cellulosic material in the composite surface layer, and wherein, in a cross-section of the biodegradable container or plate material, 1 to 90% of the cross-section is the polyester-containing composite surface layer, and 99 to 10% of the cross-section is the polyester-free cellulosic material, calculated based on the sum of the polyester-containing composite surface layer and the polyester-free cellulosic material.
2. 2. The biodegradable container or plate material of claim 1, wherein the cellulosic material comprises at least 50% by weight cellulosic material.
3. 3. A biodegradable container or plate material according to claim 1 or 2, comprising one or more additives to improve one or more of hydrophobicity, dry strength and wet strength, and / or one or more fillers or binders.
4. 4. The biodegradable container or plate material according to any one of claims 1 to 3, wherein the aliphatic polyalcohol is selected from the group of tri-alcohols selected from glycerol, sorbitol, xylitol and mannitol, and dialcohols selected from 1,2-propanediol, 1,3-propanediol and 1,2-ethanediol.
5. 5. The biodegradable container or plate material according to any one of claims 1 to 4, wherein the polyalcohol consists of at least 50 mole % of glycerol, xylitol, sorbitol, or mannitol.
6. A biodegradable container or plate material according to any one of claims 1 to 5, wherein the polycarboxylic acid comprises at least 70% by weight of tricarboxylic acid, calculated on the total amount of polycarboxylic acid.
7. 7. The biodegradable container or plate material according to any one of claims 1 to 6, wherein the tricarboxylic acid is selected from the group of citric acid, isocitric acid, aconitic acid (both cis and trans), and 3-carboxy-cis,cis-muconic acid.
8. 8. The biodegradable container or plate material of any one of claims 1 to 7, wherein the aliphatic polycarboxylic acid comprises a dicarboxylic acid selected from the group of itaconic acid, malic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid.
9. 9. The biodegradable container or plate material according to claim 1, wherein in a cross section of the biodegradable container or plate material, calculated based on the sum of the polyester-containing composite surface layer and the polyester-free cellulosic material, 2 to 50% of the cross section is the polyester-containing composite surface layer, and 98 to 50% of the cross section is the polyester-free cellulosic material.
10. A biodegradable container or plate material according to any one of claims 1 to 9, wherein the amount of polyester resin present in the biodegradable container or plate material is in the range of 0.5 to 90% by weight.
11. The biodegradable container or plate material according to any one of claims 1 to 10, which is a flower pot or a packaging material.
12. A method for producing a biodegradable container or plate material according to any one of claims 1 to 11, comprising the steps of: contacting a surface of a cellulosic material with a liquid medium comprising a polyester, or a precursor thereof, of a polycarboxylic acid and a polyalcohol, until the cellulosic material is partially, but incompletely, impregnated with the liquid medium, wherein the polyester is derived from an aliphatic polyalcohol having 2 to 15 carbon atoms and an aliphatic polycarboxylic acid having 3 to 15 carbon atoms, the polycarboxylic acid comprising at least 50% by weight of a tricarboxylic acid; and Curing process The method comprising:
13. 13. The method of claim 12, wherein the step of contacting the surface of the cellulosic material with the liquid medium is carried out through immersion, spraying, flow processing, rolling, brushing, or cascading.
14. The method according to claim 12 or 13, wherein the curing step is carried out at a product temperature of from 80 to 250°C.
15. The method according to any one of claims 12 to 14, wherein a drying step is carried out before the curing step.
16. The biodegradable container or plate material of claim 2, wherein the cellulose material is obtained from virgin or used paper, virgin or used cardboard, any form of wood or other plant material, or a combination thereof.
Citation Information
Patent Citations
Biodegradable paper sheet and paper container
JP2003013391A
Biodegradable lamination sheet and processed article of the same
JP2011000743A
Biodegradable polyester, method for producing the same, and product containing the polyester
JP2011518235A
Method for Applying a Barrier on Moulded Fibrous Product and a Product Produced by Said Method
US20120276400A1
Use of an aqueous dispersion of biodegradable polyesters
US20130101865A1