Active energy ray curable composition and method for producing matte coating film
A tailored active energy ray-curable composition with specific compounds and controlled irradiation methods addresses the balance of low gloss, stain resistance, and scratch resistance in coatings, achieving a matte finish with solvent-free application.
Patent Information
- Application Number
- JP2024506518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-18
- Filing Date
- 2023-10-12
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2043-10-12
AI Technical Summary
Existing active energy ray-curable coatings struggle to achieve a balance of low gloss, stain resistance, and scratch resistance while maintaining good viscosity, particularly in solvent-free formulations.
A specific composition of active energy ray-curable compounds, including ethylene oxide-modified 1,6-hexanediol diacrylate and ethylene oxide-modified trimethylolpropane triacrylate, combined with a matting agent of 1 to 10 μm particle size and monofunctional monomers, along with photopolymerization initiators, is used to form a matte coating film through controlled irradiation with ultraviolet and electron beams in controlled oxygen atmospheres.
The composition achieves a matte effect with low gloss, excellent stain resistance, and scratch resistance, maintaining viscosity suitable for application without the use of solvents, and can be applied as a coating agent.
Smart Images

Figure 0007556180000001 
Figure 0007556180000002 
Figure 0007556180000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an active energy ray-curable composition and a method for producing a matte coating film using the composition. [Background technology]
[0002] Generally, "decorative sheets" are used for furniture, home interiors, vehicle interior materials, etc. as a material that can be attached to the surface of a base material to give it an appearance (design) close to that of natural materials. The coating agent that constitutes the outermost layer of the decorative sheet is required to have a matte finish (sometimes called low gloss) to prevent reflection in lighting fixtures and to reproduce a wood surface, as well as scratch resistance, stain resistance, and good viscosity and other physical properties for processability to protect the base material and decorative layer. On the other hand, most of the current coating agents are two-component curing paints containing organic solvents, but in recent years, active energy ray curing type solventless paints have been attracting attention from the viewpoint of environmental friendliness. However, in solventless paints, the mechanism of matting agents orienting to the coating surface layer when the solvent evaporates, which reduces gloss, cannot be used, as in solvent-based paints, so matting agents with large particle sizes according to the film thickness must be used, which is an issue in that a sufficiently low gloss cannot be obtained. It is known to apply a coating agent containing an electron beam curable (sometimes referred to as EB curable) or ultraviolet ray curable (sometimes referred to as UV curable) matting agent onto a substrate (see, for example, Patent Document 1). Also, when curing a coating agent containing a matting agent, a method is known in which the oxygen concentration is changed in multiple stages in an oxygen-containing inert gas atmosphere, and electron beams are irradiated to cure an electron beam curable clear, thereby obtaining a sufficient matting effect and a highly weather-resistant matte decorative panel with significantly superior weather resistance (see, for example, Patent Document 2). However, even these methods are still not sufficient to provide a desired matte effect while also providing scratch resistance, stain resistance, and a viscosity that is favorable in terms of processability. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-69332 A [Patent Document 2] JP 2001-87703 A Summary of the Invention [Problem to be solved by the invention]
[0004] The problem to be solved by the present invention is to provide an active energy ray-curable composition that has a viscosity that allows it to be applied as a coating agent, low gloss that brings about a matte effect, contamination resistance, and scratch resistance, and to provide a method for producing a matte coating film using the active energy ray-curable composition. [Means for solving the problem]
[0005] The present inventors have found that an active energy ray-curable composition containing a specific amount of a specific active energy ray-curable compound, a photopolymerization initiator, and a specific amount of a matting agent having a specific particle size can solve the above problems.
[0006] That is, the present invention provides an active energy ray-curable composition containing an active energy ray-curable compound, a photopolymerization initiator, and a matting agent, the active energy ray-curable composition being characterized in that it satisfies (1) and (2). (1) As the active energy ray curable compound, the active energy ray curable compound contains 10 to 50 mass% of ethylene oxide modified 1,6-hexanediol diacrylate and 10 to 50 mass% of ethylene oxide modified trimethylolpropane triacrylate based on the total mass of the active energy ray curable compound. (2) The matting agent has a particle size of 1 to 10 μm, and is contained in an amount of 5 to 20% by mass based on the total mass of the active energy ray-curable compound. (3) The active energy ray-curable compound contains a monofunctional monomer in an amount of 1 to 30% by mass based on the total mass of the active energy ray-curable compound.
[0007] The present invention also provides the above-described active energy ray-curable composition, which contains dipentaerythritol hexaacrylate in an amount of 1 to 20 mass % based on the total mass of the active energy ray-curable compound.
[0008] The present invention also provides the above-described active energy ray-curable composition, which contains at least one (meth)acrylic oligomer selected from the group consisting of urethane (meth)acrylates, epoxy (meth)acrylates, and acrylic (meth)acrylates in an amount of 1 to 20 mass % based on the total mass of the active energy ray-curable compound.
[0009] The present invention also provides the active energy ray-curable composition described above, wherein the monofunctional monomer contains at least one selected from the group consisting of ethoxydiethylene glycol acrylate, 2-2-(phenoxyethoxy)ethyl acrylate, 2-(4-nonylphenoxy)ethyl acrylate, n-octyl acrylate, and 2-methyl-2-ethyl-1,3-dioxolan-4-ylmethyl acrylate.
[0010] The present invention also provides a method for producing a matte coating film, comprising the steps of: (I) forming a coating film of an active energy ray-curable composition on a substrate; (II) irradiating the coating film with ultraviolet light in the atmosphere; and (III) irradiating the coating film with active energy rays, in this order; wherein the active energy ray-curable composition is the active energy ray-curable composition described above. Effect of the Invention
[0011] The active energy ray-curable composition of the present invention can have a viscosity that allows it to be applied as a coating agent even without a solvent, a low gloss that provides a matte effect, and good stain resistance and scratch resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The active energy ray-curable composition of the present invention is an active energy ray-curable composition containing an active energy ray-curable compound, a photopolymerization initiator, and a matting agent, and is characterized by satisfying (1) and (2). (1) As the active energy ray curable compound, the active energy ray curable compound contains 10 to 50 mass% of ethylene oxide modified 1,6-hexanediol diacrylate and 10 to 50 mass% of ethylene oxide modified trimethylolpropane triacrylate based on the total mass of the active energy ray curable compound. (2) The matting agent has a particle size of 1 to 10 μm, and is contained in an amount of 5 to 20% by mass based on the total mass of the active energy ray-curable compound. (3) The active energy ray-curable compound contains a monofunctional monomer in an amount of 1 to 30% by mass based on the total mass of the active energy ray-curable compound.
[0013] (Matte coating film made of a cured product of an active energy ray-curable composition) The matte coating film of the present invention is a matte coating film made of a cured product of a coating agent made of an active energy ray-curable composition. Hereinafter, the coating agent made of the active energy ray-curable composition used in the present invention will be referred to as "active energy ray-curable matte coating agent". In the present invention, the term "(meth)acrylate" refers to either or both of an acrylate and a methacrylate.
[0014] (Active energy ray curable compound) The active energy ray curable compound used in the present invention must contain 10 to 50 mass% of ethylene oxide modified 1,6-hexanediol diacrylate and 10 to 50 mass% of ethylene oxide modified trimethylolpropane triacrylate, based on the total mass of the active energy ray curable compound. When the amount of ethylene oxide modified 1,6-hexanediol diacrylate is 10% by mass or more based on the total mass of the active energy ray curable compound, low gloss tends to be maintained, and when it is 50% by mass or less, scratch resistance tends to be maintained. When the amount of ethylene oxide modified trimethylolpropane triacrylate is 10% by mass or more based on the total mass of the active energy ray curable compound, scratch resistance tends to be maintained, and when it is 50% by mass or less, low gloss tends to be maintained.
[0015] In the ethylene oxide-modified 1,6-hexanediol diacrylate, the amount of alkylene oxide added in the modification is preferably 1 to 2 moles, and in the ethylene oxide-modified trimethylolpropane triacrylate, the amount of alkylene oxide added in the modification is preferably 1 to 3 moles, more preferably 2 to 3 moles.
[0016] Furthermore, the active energy ray-curable compound used in the present invention must contain a monofunctional monomer in an amount of 1 to 30% by mass based on the total mass of the active energy ray-curable compound. When the monofunctional monomer is 1% by mass or more based on the total mass of the active energy ray-curable compound, low gloss tends to be maintained, and when it is 30% by mass or less, scratch resistance tends to be maintained.
[0017] As the monofunctional monomer, ethoxydiethylene glycol acrylate, 2-2-(phenoxyethoxy)ethyl acrylate, 2-(4-nonylphenoxy)ethyl acrylate, n-octyl acrylate, and 2-methyl-2-ethyl-1,3-dioxolan-4-ylmethyl acrylate are preferred, and among these, ethoxydiethylene glycol acrylate, 2-2-(phenoxyethoxy)ethyl acrylate, and 2-(4-nonylphenoxy)ethyl acrylate are preferred. These may be used alone or in combination of two or more.
[0018] Furthermore, dipentaerythritol hexaacrylate may be contained in an amount of 1 to 20% by mass based on the total mass of the active energy ray-curable compound. When dipentaerythritol hexaacrylate is 1% by mass or more based on the total mass of the active energy ray-curable compound, stain resistance tends to be maintained, and when it is 20% by mass or less, low gloss tends to be maintained.
[0019] Furthermore, a (meth)acrylic oligomer may be used as necessary. Examples of the (meth)acrylic oligomer include urethane (meth)acrylate, acrylic (meth)acrylate, epoxy (meth)acrylate, amine-modified polyether acrylate, amine-modified epoxy acrylate, amine-modified aliphatic acrylate, amine-modified polyester acrylate, amine-modified acrylate such as amino (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, polyolefin (meth)acrylate, polystyrene (meth)acrylate, etc. Among these, urethane (meth)acrylate, epoxy (meth)acrylate, and acrylic (meth)acrylate are preferred, and urethane (meth)acrylate is more preferred in that it has a viscosity that allows it to be applied as a coating agent, low gloss, stain resistance, and scratch resistance.
[0020] The molecular weight of the (meth)acrylic oligomer is preferably in the range of 150 to 100,000 in number average molecular weight, and more preferably in the range of 200 to 10,000 in number average molecular weight.
[0021] In addition, at least one (meth)acrylic oligomer selected from the group consisting of urethane (meth)acrylate, epoxy (meth)acrylate, and acrylic (meth)acrylate is preferably contained in an amount of 1 to 20% by mass based on the total mass of the active energy ray curable compound. By containing the (meth)acrylic oligomer in an amount of 1% by mass or more based on the total mass of the active energy ray curable compound, scratch resistance tends to be maintained, and if it is contained in an amount of 20% by mass or less, viscosity suitable for application as a coating agent tends to be maintained.
[0022] (Photopolymerization initiator) The active energy ray-curable composition of the present invention generally uses a photopolymerization initiator. As the photopolymerization initiator to be used in this case, a known photopolymerization initiator may be used.
[0023] Among them, radical polymerization type photopolymerization initiators are preferred, and α-hydroxyalkyl ketone-based photopolymerization initiators are preferred, which do not color the solution when the active energy ray curable compound is dissolved and do not yellow over time. Examples of α-hydroxyalkyl ketone-based photopolymerization initiators include 1-phenyl-2-hydroxy-2-methylpropan-1-one, 1-(4-i-propylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, and 1-hydroxycyclohexyl phenyl ketone. Furthermore, phenylglyoxolate-based photopolymerization initiators are also preferred. Examples of phenylglyoxolate-based photopolymerization initiators include methylbenzoyl formate. Among them, 1-hydroxycyclohexyl phenyl ketone is preferred.
[0024] As other radical polymerization type photopolymerization initiators, monoacylphosphine oxide-based photopolymerization initiators having an absorption wavelength in the long wavelength region of ultraviolet light may be used in appropriate combination. Examples of the monoacylphosphine oxide photopolymerization initiator include monoacylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,6-dimethoxybenzoyl-diphenylphosphine oxide, 2,6-dichlorobenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoyl-phenylphosphine acid methyl ester, 2-methylbenzoyl-diphenylphosphine oxide, and pivaloylphenylphosphine acid isopropyl ester, excluding bisacylphosphine oxides that become colored when dissolved in an active energy ray-curable compound. Among these, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide is particularly preferred in that it has a UV absorption wavelength that matches the emission wavelength region of UV-LEDs having an emission wavelength of 385 nm or 395 nm, thereby obtaining suitable curability and causing less yellowing of the cured film.
[0025] The photopolymerization initiators may be used alone or in combination of two or more. The total amount of the photopolymerization initiators is preferably in the range of 0.01 to 5.0% by mass of the total amount of the active energy ray curable composition. If it is 0.01% by mass or more, good curability can be obtained. In addition, in the active energy ray curable matte coating agent used in the conventional decorative sheet, the photopolymerization initiator is generally added in an amount of 5.0 to 10.0% by mass of the total amount of the solid content of the coating agent, but in the present invention, by making it 5.0% by mass or less, the fluidity as a coating agent is maintained, and processability and workability are maintained. In addition, by the step (II) of irradiating ultraviolet rays under atmospheric conditions, the coating film surface of the matte coating film tends to be in a semi-cured state, and the fine particles of the matte agent are efficiently aligned by surface orientation, making it easy to obtain a matte effect.
[0026] Furthermore, the curing speed can be increased by adding a tertiary amine compound selected from aliphatic amine derivatives and / or benzoic acid amine derivatives as a sensitizer. Tertiary amine compounds are known to increase reactivity and prevent reaction inhibition by oxygen. Suitable tertiary amine compounds include free alkylamines such as triethylamine, methyldiethanolamine, and triethanolamine, aromatic amines such as 2-ethylhexyl-4-dimethylaminobenzoate and ethyl-4-dimethylaminobenzoate, and active energy ray polymerizable compounds such as polymeric unsaturated amines (e.g., (meth)acrylated amines), which are considered to be preferred due to their low odor, low volatility, and ability to be incorporated into the polymer matrix by curing, thereby suppressing yellowing.
[0027] The tertiary amine compound can be used in an amount of preferably 0.1 to 10% by mass, more preferably 0.3 to 3% by mass, based on the total amount of the coating material including the organic solvent.
[0028] (Matting agent with average particle size of 1 to 10 μm) The matting agent used in the present invention may be any known one having an average particle diameter of 1 to 10 μm, and may be used alone or in combination with other organic and / or inorganic particles without particular limitation. Specifically, for example, inorganic particles such as silica, titanium oxide, alumina particles (aluminum oxide), calcium carbonate, barium sulfate, and glass, organic particles such as acrylic resin, urethane resin, polycarbonate resin, silicone resin, and polystyrene resin, silicone beads, etc. may be used. As those that can be expected to have a high matting effect, silica and aluminosilicate beads as inorganic fine particles, acrylic resin beads, urethane resin beads, and silicone beads as organic fine particles are preferred. The amount of the matting agent added is preferably 5 to 20% by mass, more preferably 10 to 18% by mass, based on the total mass of the active energy ray-curable compound. If the content is 5% by mass or more, a sufficient matting effect is obtained, and if it is 20% by mass or less, the viscosity and scratch resistance that can be applied as a coating agent tend to be maintained.
[0029] (silica) The silica used in the present invention is not particularly limited as long as it has an average particle size in the range of 1 to 10 μm, and any known silica can be used. In the present invention, the average particle size is a value measured by a laser diffraction method. Specifically, amorphous silica is more preferable. Examples of the amorphous silica include diatomaceous earth and activated clay. Among the amorphous silica, dry silica, wet silica, silica gel, etc. can be used as synthetic amorphous silica. Among them, wet silica produced by neutralizing and decomposing an aqueous solution of sodium silicate with an acid or an alkali metal salt is preferable. The wet silica can also be surface-treated. The method of surface-treating the silica particles is not particularly limited and may be any known method. Examples of the wet silica include those surface-treated with wax or a silane coupling agent. The wet silica may be used by mixing a plurality of the surface-treated and non-surface-treated wet silicas.
[0030] The average particle size of the wet silica used as the matting agent is 1 to 10 μm, more preferably 1.5 to 8 μm. If the average particle size is less than 1 μm, the viscosity increases significantly and it becomes difficult to obtain a viscosity suitable for coating. If the average particle size is more than 10 μm, the effect of silica being oriented on the coating surface layer is lost, and the matte feeling becomes insufficient.
[0031] The content of silica is preferably 5 to 20% by mass, more preferably 10 to 18% by mass, based on the total mass of the active energy ray-curable compound. If the content is less than 5% by mass, a sufficient matte effect is not obtained, and if it exceeds 20% by mass, it tends to be difficult to maintain the viscosity and scratch resistance that can be applied as a coating agent, which is not preferable.
[0032] (beads) When beads are used in the present invention, there is no particular limitation and known beads can be used. Specifically, acrylic resin beads, silicone beads, glass beads, aluminosilicate beads, etc. can be used. By adding beads to the silica as the matting agent, it is possible to improve the scratch resistance of the coating surface in addition to a moderate low gloss. Although beads as the matting agent are required in larger amounts than silica, another advantage is that it is easier to fine-tune the gloss level by changing the amount of beads added. Among them, acrylic resin beads are preferred.
[0033] The active energy ray-curable composition of the present invention is preferably used without a solvent from the viewpoint of recent environmental friendliness, but an organic solvent may be added as necessary.
[0034] (Organic solvent) As the organic solvent, any solvent can be used as long as it dissolves the active energy ray-curable composition used. Examples of the solvent include aromatic hydrocarbons such as toluene and xylene; aliphatic or alicyclic hydrocarbons such as n-hexane, cyclohexane, methylcyclohexane, and ethylcyclohexane; esters such as ethyl acetate, butyl acetate, and propyl acetate; alcohols such as methanol, ethanol, isopropyl alcohol, and n-butanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alkylene glycol monoalkyl ethers such as ethylene glycol monoethyl ether and propylene glycol monomethyl ether; and ether esters such as propylene glycol monomethyl ether acetate. However, when aiming for environmental friendliness, in order to thoroughly reduce the amount of organic solvents evaporated into the atmosphere, i.e., to reduce volatile organic compounds (VOCs), it is more preferable not to contain the above organic solvents.
[0035] From the viewpoint of coatability, it is preferable that the active energy ray curable composition of the present invention is adjusted to a viscosity that can be applied in the method for producing a matte coating film of the present invention described later. The viscosity is preferably adjusted to 300 to 10,000 mPa·s, more preferably 2,000 to 10,000 mPa·s, and even more preferably 300 to 2,000 mPa·s. The active energy ray curable compounds generally have low molecular weights, and if the viscosity can be adjusted without diluting with an organic solvent, there is no need to dilute with an organic solvent. On the other hand, when a polymerizable oligomer with a high molecular weight and high viscosity is used in combination, the viscosity can be adjusted by diluting with an organic solvent or heating.
[0036] (Additives) In addition, the active energy ray-curable composition used in the present invention may contain, as necessary, a polymerization inhibitor, a leveling agent, a thixotropy imparting agent, a wax, a drying agent, a thickening agent, an anti-sagging agent, a plasticizer, a dispersant, an anti-settling agent, an antifoaming agent, an ultraviolet absorbing agent, a light stabilizer, and the like.
[0037] (Production of active energy ray-curable composition) The active energy ray-curable composition of the present invention can be produced by mixing, kneading, and dispersing the active energy ray-curable compound, the photopolymerization initiator, the matting agent, and various other additives. The active energy ray-curable composition of the present invention can be adjusted by appropriately adjusting the size of the grinding media of the dispersing machine, the packing rate of the grinding media, the dispersion treatment time, etc. As the dispersing machine, a commonly used one, for example, a roller mill, a ball mill, a pebble mill, an attritor, a sand mill, etc. can be used. When air bubbles or unexpectedly large particles are contained in the coating agent, they deteriorate the quality of the coating product, so it is preferable to remove them by filtration, etc. As the filter, a conventionally known filter can be used.
[0038] (Method of forming a matte coating film) The active energy ray-curable composition of the present invention can be used to form a coating film by a known coating or printing method. Specific examples of the coating method include a roll coater, a gravure coater, a gravure offset coater, a flexo coater, an air doctor coater, a blade coater, an air knife coater, a squeeze coater, an impregnation coater, a transfer roll coater, a kiss coater, a curtain coater, a cast coater, a spray coater, a die coater, an offset printing machine, a screen printing machine, and the like.
[0039] When the coating agent used contains an organic solvent, the matte coating film formed by the above-mentioned formation method can be obtained by drying the solvent in a drying oven or the like and then curing the coating with active energy rays to obtain a hardened coating film. However, this is not necessary when the coating agent is solvent-free.
[0040] (base material) The substrate used in the present invention can be any substrate for which a matte design is desired. For example, in the case of a decorative sheet for building materials, a general-purpose substrate sheet used for decorative sheets can be used as the substrate. There are no particular limitations on the base sheet, and a typical decorative sheet such as a sheet (film) made of a general-purpose thermoplastic resin or paper can be used. Examples of sheets (films) formed from thermoplastic resins include polyolefin resins such as polyethylene, ethylene-α-olefin copolymers, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymers, propylene-butene copolymers, ethylene-vinyl acetate copolymers, saponified ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylic acid ester copolymers, polyvinyl chloride, polyethylene terephthalate (PET), polybutylene terephthalate, polyamide, polycarbonate, polyethylene naphthalate, ionomers, acrylic acid ester polymers, and methacrylic acid ester polymers. The substrate sheet may be formed by using these resins alone or in combination of two or more.
[0041] The substrate sheet may be colored, and may contain various additives, such as fillers, matting agents, foaming agents, flame retardants, lubricants, antistatic agents, antioxidants, ultraviolet absorbers, light stabilizers, etc. The thickness of the substrate sheet can be appropriately set depending on the application and method of use of the final product, but is generally preferably 20 to 300 μm.
[0042] One or both sides of the base sheet may be subjected to a surface treatment such as corona discharge treatment, ozone treatment, plasma treatment, ionizing radiation treatment, dichromate treatment, etc. For example, when corona discharge treatment is performed, the surface tension of the base sheet surface may be set to 30 dyne or more, preferably 40 dyne or more. The surface treatment may be performed according to a conventional method for each treatment.
[0043] In addition, the types of paper base materials for decorative sheets include, for example, thin paper, plain paper, reinforced paper, paper sheets such as resin-impregnated paper, titanium paper, and the like.
[0044] The substrate may also be a wood veneer or the like that is commonly used for decorative boards. Examples of wood substrates for wood veneers include known substrates such as plywood, particle board, hardboard, and MDF that have been used as wooden substrates for decorative boards, furniture, building materials, etc. It does not matter what manufacturing method is used to obtain these known substrates. Further, examples of non-combustible materials that can be used as the substrate include perforated board building materials made from gypsum board, gypsum plate, calcium silicate plate, etc.; ceramic plates such as pottery, porcelain, stoneware, earthenware, glass, and enamel; and metal plates such as iron plate, galvanized steel plate, polyvinyl chloride sol-coated steel plate, aluminum plate, and copper plate.
[0045] (Process (I)) The active energy ray curable composition is applied to a substrate selected from the substrates described above depending on the purpose of use, and a coating film is formed on the substrate by using any of the coating methods described above.
[0046] (Step (II)) Next, the coating film is preferably irradiated with ultraviolet light in the atmosphere.
[0047] Here, ultraviolet irradiation in the atmosphere can be performed by a known method, for example, ultraviolet irradiation using a germicidal lamp, an ultraviolet fluorescent lamp, an ultraviolet light-emitting diode (UV-LED), a carbon arc, a metal halide lamp, a xenon lamp, a chemical lamp, a low-pressure mercury lamp, a high-pressure mercury lamp for copying, a medium-pressure or high-pressure mercury lamp, an ultra-high-pressure mercury lamp, an electrodeless lamp, a metal halide lamp, natural light, or the like as a light source. The cumulative dose of ultraviolet light in step (2) is 20 to 1000 mJ / cm 2 In order to maximize the effect of the present invention, it is preferable that the integrated light amount is within the range of 40 to 800 mJ / cm. 2 It is even more preferable that the range is: 20mJ / cm 2 If it is more than 1000mJ / cm, the curing efficiency is good. 2 If it is below this level, damage to the substrate due to heat generation can be prevented. By semi-curing the surface of the matte coating film of the present invention in step (II), the matte effect can be obtained more efficiently due to the surface orientation of the matte agent, and a matte effect similar to that of a solvent-based paint can be obtained even without a solvent.
[0048] (Process (III) After the step (II), the matte coating film is completely cured in the step (III) of irradiating it with active energy rays, which may be electron beams or ultraviolet rays. In the case of ultraviolet irradiation, it is more preferable to irradiate in an atmosphere with an oxygen concentration of less than 5%. Here, an atmosphere with an oxygen concentration of less than 5% means an atmosphere filled with an inert gas containing oxygen, and the oxygen concentration is less than 5%. As the inert gas, one or more of nitrogen gas, carbon dioxide gas, argon gas, etc. may be used. In addition, there is no problem if a small amount of other gases such as carbon dioxide contained in air is contained.
[0049] In an atmosphere with an oxygen concentration of less than 5%, ultraviolet rays are irradiated. The cumulative amount of ultraviolet rays in step (III) is 20 to 1000 mJ / cm. 2 In order to maximize the effect of the present invention, it is preferable that the integrated light amount is within the range of 40 to 800 mJ / cm. 2 It is even more preferable that the range is:
[0050] On the other hand, when an electron beam is used, an electron beam irradiation device is used. The irradiation dose is preferably about 10 to 230 kGy, more preferably about 10 to 100 kGy. In the case of electron beam irradiation, the oxygen concentration in the atmosphere is preferably 2% or less.
[0051] The thickness of the coating film thus obtained is preferably in the range of 0.1 to 100 μm, and most preferably in the range of 0.5 to 50 μm. By keeping the thickness in this range, the effects of the present invention can be maximized.
[0052] Furthermore, the manufacturing method of the present invention can be widely applied not only to the above-mentioned building material applications such as decorative sheets, but also to surface coating applications for furniture, musical instruments, office supplies, sporting goods, toys, and the like. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples. In the examples, "parts" and "parts by mass" refer to mass %.
[0054] The average particle size of silica was measured using a nanoparticle size distribution analyzer Nanotrac UPA EX-150 manufactured by Nikkiso Co., Ltd.
[0055] (Preparation of active energy ray-curable composition) Example 1 A total of 116.5 parts of Photomer 6184 (manufactured by IGM Resins BV) which is a urethane acrylate oligomer, 10 parts of Miramer M170 (ethoxydiethylene glycol acrylate (EOEOEA, manufactured by MIWON)) which is a monofunctional monomer, 50 parts of Miramer M202 (manufactured by MIWON) which is an ethylene oxide modified 1,6-hexanediol diacrylate, 35 parts of M3130 (manufactured by MIWON) which is an ethylene oxide modified trimethylolpropane triacrylate, 1.5 parts of 1-hydroxy-cyclohexyl-phenyl-ketone "Omnirad 184" (manufactured by BASF), and 15 parts of Nipsil E170 (average particle size: 3 μm, manufactured by Tosoh Silica Corporation) which is an organic surface-treated silica (wet silica) as a matting agent were mixed and stirred with a stirrer for 1 hour to prepare an active energy ray curable composition 1.
[0056] [Examples 2 to 14, Comparative Examples 1 to 8] According to the formulations shown in Tables 1 to 4, each active energy ray-curable composition was prepared in the same manner as in Example 1.
[0057] <Formation of coating film by step (I)> A polypropylene film (manufactured by Okamoto Corporation, 0.5 mm thick) was used as a substrate, and the active energy ray-curable compositions prepared in Examples 1 to 14 and Comparative Examples 1 to 8 were applied using a bar coater (10 μm). The coatings were then subjected to a step (II) of irradiating with ultraviolet light in the atmosphere and a step (III) of irradiating with active energy rays in accordance with Tables 1 to 4.
[0058] <Ultraviolet ray irradiation in step (II)> Using a UV irradiation device (GS Yuasa Corporation) equipped with an air-cooled high-pressure mercury lamp (output 120 W / cm x 1 lamp) and a belt conveyor, the coated material was placed on the conveyor and passed directly under the lamp (irradiation distance 11 cm) in air at a speed of 25 meters per minute to semi-cure the coating film. The UV exposure was measured at 55 mJ / cm using a UV integrating light meter (GS Yuasa Corporation's industrial UV checker UVR-N1). 2 It was confirmed that this was the case.
[0059] <Electron beam irradiation in step (III)> Next, using a curtain-type electron beam irradiation device ("Electrocurtain EC250 / 15 / 180L" manufactured by Iwasaki Electric Co., Ltd.), the coating film was irradiated with an electron beam at an exposure dose of 50 kGy to completely cure the coating film.
[0060] [Evaluation method] The active energy ray-curable composition of the present invention and the method for evaluating the prepared matte coating film will be described below.
[0061] [Evaluation item 1: Viscosity] The active energy ray-curable composition adjusted to 25° C. was measured using a digital B-type viscometer ("TVB-10M" manufactured by Toki Sangyo Co., Ltd.) with an M3 rotor at 60 rpm. (Evaluation Criteria) ◎: 300 mPa s or more, less than 2000 mPa s ○: 2000 mPa s or more, less than 10000 mPa s ×: Less than 300 mPa·s or 10,000 mPa·s or more
[0062] [Evaluation item 2: Glossiness] The completely cured matte coating film surface was measured for specular gloss in accordance with JIS Z8741 using a gloss meter (Konica Minolta's "MULTI GLOSS 268A") to measure the gloss value. The gloss value was measured under the conditions of an incident angle of 60° and a reflection angle of 60°. (Evaluation Criteria) ◎: Less than 10% ○: 10% or more but less than 20% ×: 20% or more
[0063] [Evaluation item 3: Stain resistance] In accordance with the JAS Special Plywood Stain A Test, a stain was applied to the surface of the decorative panel, and after 4 hours, the surface was wiped off with a cloth containing alcohol, after which the remaining stain was visually observed. Commercially available black marker pen was used as the stain. (Evaluation Criteria) ◎: No contaminants remain ○: Contamination remains, but it is minor and does not pose a problem for practical use. ×: Significant contaminants remain
[0064] [Evaluation item 4: Scratch resistance] The surface of the obtained coating film was evaluated using a Hoffman scratch tester (manufactured by BYK Gardner). Specifically, a scratch blade was set at an angle of 45° on the surface of the coating film, and the tester was moved. The load was gradually increased, and the load at which scratches or indentations were generated on the surface was measured. (Evaluation Criteria) ◎: Load 400g or more ○: Load 200g or more, less than 400g ×: Load less than 200g
[0065] Tables 1 to 4 show the composition of each active energy ray-curable composition and the evaluation results of the produced matte coating film. In addition, all values in the table are in parts by mass or mass %, and blank spaces indicate that no component was blended. In addition, ND in Table 4 indicates that the viscosity was too high to be evaluated.
[0066] [Table 1]
[0067] [Table 2]
[0068] [Table 3]
[0069] [Table 4]
[0070] The abbreviations in the table are as follows: Photomer 6184: Urethane acrylate oligomer manufactured by IGM Resins BV Miramer M170: Ethoxydiethylene glycol acrylate (EOEOEA) manufactured by MIWON M-101A: 2-2-(phenoxyethoxy)ethyl acrylate manufactured by Toagosei Co., Ltd. M-113: 2-(4-nonylphenoxy)ethyl acrylate manufactured by Toagosei Co., Ltd. NOAA: n-Octyl acrylate manufactured by Osaka Organic Chemical Industry Ltd. MEDOL-10: 2-Methyl-2-ethyl-1,3-dioxolan-4-ylmethyl acrylate manufactured by Osaka Organic Chemical Industry Co., Ltd. Miramer M202: MIWON ethylene oxide modified 1,6-hexanediol diacrylate Miramer M220: Tripropylene glycol diacrylate manufactured by MIWON Miramer M3130: Ethylene oxide modified trimethylolpropane triacrylate manufactured by MIWON DPA600T: Dipentaerythritol hexaacrylate manufactured by Zhangjiagang Dongya Di-Ai Biochemical Co., Ltd. Omnirad184: Photoinitiator 1-hydroxy-cyclohexyl-phenyl-ketone manufactured by BASF Nipsil E170: Silica manufactured by Tosoh Silica Corporation, average particle size 3μm Syloid ED-50: WRGrace silica, average particle size 8μm NIPGEL BY-001: Silica manufactured by Tosoh Silica Corporation, average particle size 14μm
[0071] The active energy ray-curable composition of the present invention can have a viscosity that allows it to be applied as a coating agent without using an organic solvent, while also having low gloss that brings about a matte effect, contamination resistance, and scratch resistance.
Claims
1. A step (I) of forming a coating film of an active energy ray-curable composition on a substrate; (II) a step of irradiating the coating film with ultraviolet light under atmospheric conditions; A step (III) of irradiating the coating film with an electron beam; A method for producing a matte coating film, characterized in that: The substrate is a sheet formed of a thermoplastic resin. The active energy ray-curable composition comprises A method for producing a matte coating film, comprising an active energy ray-curable composition containing an active energy ray-curable compound, a photopolymerization initiator, and a matte agent, the method being characterized in that the composition satisfies (1), (2), and (3). (1) As the active energy ray curable compound, the composition contains 10 to 50 mass % of ethylene oxide modified 1,6-hexanediol diacrylate based on the total mass of the active energy ray curable compound, and 10 to 50 mass % of ethylene oxide modified trimethylolpropane triacrylate based on the total mass of the active energy ray curable compound. (2) The matting agent has a particle size of 1 to 10 μm, and is contained in an amount of 5 to 20% by mass based on the total mass of the active energy ray-curable compound. (3) The active energy ray-curable compound contains a monofunctional monomer in an amount of 1 to 30% by mass based on the total mass of the active energy ray-curable compound.
2. 2. The method for producing a matte coating film according to claim 1, wherein the dipentaerythritol hexaacrylate is contained in an amount of 1 to 20% by mass based on the total mass of the active energy ray-curable compound.
3. The method for producing a matte coating film according to claim 1 or 2, wherein the active energy ray curable compound contains 1 to 20 mass% of at least one (meth)acrylic oligomer selected from the group consisting of urethane (meth)acrylate, epoxy (meth)acrylate, and acrylic (meth)acrylate, based on the total mass of the active energy ray curable compound.
4. The method for producing a matte coating film according to claim 1, wherein the monofunctional monomer contains at least one selected from the group consisting of ethoxydiethylene glycol acrylate, 2-2-(phenoxyethoxy)ethyl acrylate, 2-(4-nonylphenoxy)ethyl acrylate, n-octyl acrylate, and 2-methyl-2-ethyl-1,3-dioxolan-4-ylmethyl acrylate.
Citation Information
Patent Citations
Highly weather resistant matte decorative sheet and method for manufacturing the same
JP2001087703A
Active energy line curing coating composition and method for forming coating film
JP2002069332A
Method for manufacturing abrasion-resistant matte decorative material
JP2006095501A
Active energy ray-curable coating material composition, and coated article
JP2012224669A
Active energy ray-curable composition for floor material
JP2019052437A