Optical Devices
The liquid crystal element film with a spacer, alignment film, and adhesive layer addresses the challenge of maintaining cell gap and adhesion in flexible substrates, achieving stable and uniform optical performance under high pressure and temperature conditions.
Patent Information
- Application Number
- JP2022575240
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-29
- Filing Date
- 2021-07-02
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2041-07-02
AI Technical Summary
Existing methods for maintaining cell gap and adhesion between base layers in liquid crystal cells using flexible substrates are prone to defects due to the low modulus of adhesive layers, leading to issues like cell gap collapse and poor electro-optical properties under high temperature and pressure conditions.
A liquid crystal element film structure is developed with a spacer and alignment film on the second base layer, combined with an adhesive layer having both liquid crystal alignment and adhesive forces, and an intermediate layer with controlled thickness and modulus to ensure structural stability and uniformity.
The solution maintains cell gap and adhesion, minimizing defects and ensuring structural stability and uniform quality, even under high temperature and pressure, thus enhancing the electro-optical properties of the optical device.
Smart Images

Figure 0007556191000008 
Figure 0007556191000011 
Figure 0007556191000006
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0084734 filed on July 9, 2020, and Korean Patent Application No. 10-2020-0142095 filed on October 29, 2020, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present application relates to optical devices. [Background technology]
[0003] For the long-term stability and large-area scalability of liquid crystal film cells that use flexible substrates, it is important to maintain the cell gap between the first substrate layer (or "upper substrate layer") and the second substrate layer (or "lower substrate layer") and to provide adhesive strength between the first substrate layer and the second substrate layer.
[0004] Non-Patent Document 1 discloses a technique of forming a pillar- or wall-shaped organic film pattern with the height of the cell gap on one substrate layer and fixing it to the substrate layer on the opposite side using an adhesive. However, this technique requires that the adhesive be located only on the pillar or wall surface, and the technique of micro-stamping the adhesive on the pillar or wall surface is highly difficult to process, difficult to control the thickness and area of the adhesive, and highly likely that the adhesive will be pushed out when the upper and lower substrate layers are bonded, which may contaminate the alignment film or the liquid crystal. Non-Patent Document 1: "Tight Bonding of Two Plastic Substrates for Flexible LCDs" SID Symposium Digest, 38, pp. 653-656 (2007) Summary of the Invention [Problem to be solved by the invention]
[0005] In order to maintain the cell gap of the liquid crystal cell and ensure the adhesive strength between the first and second substrate layers, it is possible to form a spacer and an alignment film on the second substrate layer, and then form an adhesive layer having both liquid crystal alignment and adhesive strength on the first substrate layer, and then bond them together. However, this structure is vulnerable to external pressure due to the very low modulus of the adhesive layer, and it is difficult to obtain good quality in the high-temperature and high-pressure autoclave process. Specifically, if the structural stability of the liquid crystal cell is not ensured during the autoclave process, the cell gap collapses and the liquid crystal flow / concentration failure occurs, which causes a deterioration in the electro-optical properties and appearance uniformity of the liquid crystal cell.
[0006] The objective of the present application is to provide an optical device in which the cell gap of a liquid crystal cell is appropriately maintained, the first base layer and the second base layer are maintained with excellent adhesion, defects such as pressing and concentration are minimized, and structural stability and good quality uniformity are ensured. [Means for solving the problem]
[0007] In the present specification, when the measurement temperature affects the results of the physical properties, the physical properties are those measured at room temperature unless otherwise specified. The term "room temperature" refers to a natural temperature that is not heated or cooled, and is usually a temperature within the range of about 10°C to 30°C, or about 23°C or about 25°C. Furthermore, unless otherwise specified in the present specification, the unit of temperature is °C.
[0008] In the present specification, when the measurement pressure affects the results of any physical property mentioned, the physical property is measured at normal pressure unless otherwise specified. The term "normal pressure" refers to the natural pressure without pressure or reduction, and is usually about 1 atmosphere.
[0009] The present application relates to an optical device, the optical device including a liquid crystal element film.
[0010] Fig. 1 is a cross-sectional view of an exemplary liquid crystal element film included in the optical device of the present application. As shown in Fig. 1, the liquid crystal element film 10 included in the optical device includes a first substrate layer (or referred to as "upper substrate layer") 11a, a second substrate layer (or referred to as "lower substrate layer") 11b disposed opposite to the first substrate layer, and the liquid crystal layer 16 located between the first and second substrate layers.
[0011] The first base layer 11a and the second base layer 11b may be, for example, an inorganic film made of glass or a plastic film. The plastic film may be, but is not limited to, a PEN (polyethylene-naphthalate), PI (polyimide), COP (cycloolefin polymer), TAC (tri-acetyl-cellulose), PET (polyethyleneterephthalate), or PC (polycarbonate) film. If necessary, the base layer may have a coating layer of gold, silver, or a silicon compound such as silicon dioxide or silicon monoxide, or a functional layer such as an anti-reflection layer.
[0012] For example, the first and second substrate layers may each have a thickness of about 10 μm to about 1,000 μm. For example, the substrate layers may each have a thickness of about 20 μm or more, 40 μm or more, 60 μm or more, 80 μm or more, 100 μm or more, 120 μm or more, 140 μm or more, 160 μm or more, or about 180 μm or more, and may each have a thickness of about 900 μm or less, 800 μm or less, 700 μm or less, 600 μm or less, 500 μm or less, or about 400 μm or less. When the thickness of the substrate layer satisfies the above range, when a liquid crystal element film including the substrate layer is bonded to an outer substrate described below to manufacture an optical device, defects in appearance such as wrinkles can be reduced.
[0013] The liquid crystal element film includes at least a liquid crystal layer containing a liquid crystal compound.
[0014] The liquid crystal compound may be a liquid crystal compound whose alignment direction can be changed by application of an external action. In this specification, the term "external action" may mean any external factor that can affect the behavior of a substance contained in the liquid crystal layer, such as an external voltage. Therefore, a state without an external action may mean a state in which an external voltage or the like is not applied.
[0015] The type and properties of the liquid crystal compound may be appropriately selected in consideration of the object of the present application. In one example, the liquid crystal compound may be a nematic liquid crystal or a smectic liquid crystal. Nematic liquid crystal refers to a liquid crystal in which rod-shaped liquid crystal molecules are arranged in parallel to the long axis direction of the liquid crystal molecules without any regularity in position, and smectic liquid crystal refers to a liquid crystal in which rod-shaped liquid crystal molecules are regularly arranged to form a layered structure and are regularly arranged in parallel to the long axis direction. According to one embodiment of the present application, the liquid crystal compound may be a nematic liquid crystal compound.
[0016] Nematic liquid crystal compounds may be selected to have a clearing point or a phase transition point in said range, i.e., a nematic to isotropic phase transition point, of, for example, about 40° C. or higher, 50° C. or higher, 60° C. or higher, 70° C. or higher, 80° C. or higher, 90° C. or higher, 100° C. or higher, or about 110° C. or higher. In one example, the clearing point or phase transition point may be about 160° C. or lower, 150° C. or lower, or about 140° C. or lower.
[0017] The liquid crystal compound may be a non-reactive liquid crystal compound. The non-reactive liquid crystal compound may mean a liquid crystal compound that does not have a polymerizable group. The polymerizable group may include, but is not limited to, an acryloyl group, an acryloyloxy group, a methacryloyl group, a methacryloyloxy group, a carboxyl group, a hydroxyl group, a vinyl group, or an epoxy group, and may include a known functional group known as a polymerizable group.
[0018] The liquid crystal compound may have a positive or negative dielectric anisotropy. The absolute value of the dielectric anisotropy of the liquid crystal compound may be appropriately selected in consideration of the object of the present application. The term "dielectric anisotropy (Δε)" may mean the difference (ε / / -ε⊥) between the horizontal dielectric constant (ε / / ) and the vertical dielectric constant (ε⊥) of the liquid crystal. In this specification, the term horizontal dielectric constant (ε / / ) means a dielectric constant value measured along the direction of the electric field in a state where a voltage is applied so that the direction of the electric field caused by the applied voltage and the director of the liquid crystal compound are substantially horizontal, and the vertical dielectric constant (ε⊥) means a dielectric constant value measured along the direction of the electric field in a state where a voltage is applied so that the direction of the electric field caused by the applied voltage and the director of the liquid crystal compound are substantially perpendicular. The anisotropy of the dielectric constant of the liquid crystal molecules may be within a range of 5 to 25.
[0019] The refractive index anisotropy of the liquid crystal compound may be appropriately selected in consideration of the object of the present application. In this specification, the term "refractive index anisotropy" may mean the difference between the extraordinary refractive index and the ordinary refractive index of the liquid crystal compound. The refractive index anisotropy of the liquid crystal compound may be, for example, 0.01 to 0.3. The refractive index anisotropy may be 0.01 or more, 0.05 or more, or 0.07 or more, or 0.3 or less, 0.2 or less, 0.15 or less, or 0.13 or less.
[0020] The liquid crystal layer may further include a dichroic dye. When the liquid crystal layer includes a dichroic dye, even if the liquid crystal element film includes an adhesive layer, the liquid crystal element film is less affected by the variation in cell gap during the bonding process of the outer substrate, so that the thickness of the intermediate layer for ensuring the structural stability and quality uniformity of the liquid crystal element film can be relatively thin.
[0021] The dichroic dye can control the light transmittance variable property of the liquid crystal layer. In this specification, the term "dye" refers to a substance that can intensively absorb and / or transform light in at least a part or all of the visible light range, for example, a wavelength range of 400 nm to 700 nm, and the term "dichroic dye" refers to a substance that can anisotropically absorb light in at least a part or all of the visible light range.
[0022] The liquid crystal layer including the liquid crystal compound and the dichroic dye may be a GHLC layer (Guest Host Liquid Crystal Layer). In this specification, the term "GHLC layer (Guest Host Liquid Crystal Layer)" refers to a functional layer that is arranged with the dichroic dye by the arrangement of the liquid crystal compound and exhibits anisotropic light absorption characteristics in the alignment direction of the dichroic dye and in the direction perpendicular to the alignment direction. For example, the dichroic dye is a material whose light absorption rate changes depending on the polarization direction, and if it has a high absorption rate for light polarized in the long axis direction, it can be called a p-type dye, and if it has a high absorption rate for light polarized in the short axis direction, it can be called an n-type dye. In one example, when a p-type dye is used, polarized light vibrating in the long axis direction of the dye is absorbed, and polarized light vibrating in the short axis direction of the dye can be transmitted with little absorption. Hereinafter, unless otherwise specified, the dichroic dye is assumed to be a p-type dye.
[0023] As the dichroic dye, for example, a known dye that is known to have a property of being aligned according to the alignment state of the liquid crystal compound due to the so-called guest-host effect may be selected and used. Examples of such dichroic dyes include azo dyes, anthraquinone dyes, methine dyes, azomethine dyes, merocyanine dyes, naphthoquinone dyes, tetrazine dyes, phenylene dyes, chitalylene dyes, benzothiadiazole dyes, diketopyrrolopyrrole dyes, squaraine dyes, and pyromethene dyes, but the dyes applicable in the present application are not limited to the above.
[0024] The dichroic dye may have a dichroic ratio, i.e., the absorption of light polarized parallel to the long axis of the dichroic dye divided by the absorption of light polarized parallel to the direction perpendicular to the long axis, of 5 or more, 6 or more, or 7 or more. The dye may satisfy the dichroic ratio at least at some wavelengths or at any wavelength within the wavelength range of the visible light region, for example, within a wavelength range of about 380 nm to 700 nm or about 400 nm to 700 nm. The upper limit of the dichroic ratio may be, for example, about 20 or less, 18 or less, 16 or less, or 14 or less.
[0025] The content of the dichroic dye in the liquid crystal layer may be appropriately selected in consideration of the object of the present application. For example, the content of the dichroic dye in the liquid crystal layer may be 0.2 wt% or more. The content of the dichroic dye may be specifically 0.5 wt% or more, 1 wt% or more, 2 wt% or more, or 3 wt% or more. The upper limit of the content of the dichroic dye may be, for example, 10 wt% or less, 9 wt% or less, 8 wt% or less, 6 wt% or less, or 5 wt% or less. If the content of the dichroic dye in the liquid crystal layer is too small, it is difficult to exhibit the desired transmittance variable characteristics, and it is insufficient to reduce the thickness of the intermediate layer for reducing the variation of the cell gap that may occur during the bonding process of the outer substrate. On the other hand, if the content of the dichroic dye in the liquid crystal layer is too large, precipitation may occur. Therefore, it may be advantageous for the content of the dichroic dye to be within the above range.
[0026] The thickness of the liquid crystal layer is not particularly limited, and for example, the thickness of the liquid crystal layer may be about 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.5 μm or more, 1 μm or more, 1.5 μm or more, 2 μm or more, 2.5 μm or more, 3 μm or more, 3.5 μm or more, 4 μm or more, 4.5 μm or more, 5 μm or more, 5.5 μm or more, 6 μm or more, 6.5 μm or more, 7 μm or more, 7.5 μm or more, 8 μm or more, 8.5 μm or more, 9 μm or more, or 9.5 μm or more. The upper limit of the thickness of the liquid crystal layer is not particularly limited, and may generally be about 30 μm or less, 25 μm or less, 20 μm or less, or 15 μm or less.
[0027] The liquid crystal layer may be switched between a first alignment state and a second alignment state different from the first alignment state. The switching may be controlled by application of external energy such as a voltage. For example, the liquid crystal layer may be maintained in one of the first and second alignment states in the absence of an applied voltage, and may be switched to the other alignment state by application of a voltage.
[0028] In one example, the first alignment state may be a twisted alignment state, i.e., the liquid crystal layer may be switched between a twisted alignment and an alignment state different from the twisted alignment through application of external energy.
[0029] In one example, the liquid crystal layer may switch between a twisted and a homeotropic state, in one example, the liquid crystal layer may be in a homeotropic state with no voltage applied, and in a twisted state with a voltage applied.
[0030] In this specification, the term "vertical alignment state" refers to a state in which the directors of the liquid crystal compound in the liquid crystal layer are aligned approximately perpendicular to the plane of the liquid crystal layer, and for example, the angle that the directors of the liquid crystal compound make with respect to the plane of the liquid crystal layer can be, for example, within a range of approximately 80 degrees to 100 degrees or 85 degrees to 95 degrees, or can be approximately 90 degrees.
[0031] In the present specification, the term "twisted alignment state" may refer to a helical structure in which the directors of the liquid crystal compounds are aligned in layers while twisting along a virtual helical axis in the liquid crystal layer. The twisted alignment state may be embodied as a vertical, horizontal or tilted alignment state. That is, the vertical twist alignment mode is a state in which the individual liquid crystal compounds are aligned vertically and twisted along a helical axis to form layers, the horizontal twist alignment mode is a state in which the individual liquid crystal compounds are aligned horizontally and twisted along a helical axis to form layers, and the tilted twist alignment mode is a state in which the individual liquid crystal compounds are aligned in a tilted state and twisted along a helical axis to form layers. According to the present application, the twisted alignment state may be a twisted alignment state in a horizontal alignment state.
[0032] The ratio d / p of the thickness d to the pitch p of the liquid crystal layer in the twisted alignment state may be 20 or less, and the lower limit may be 0.5 or more. When the ratio d / p of the thickness d to the pitch p in the twisted alignment state is within the above range, the optical device can exhibit excellent light transmittance variable characteristics even without a polarizer. In general, when the ratio d / p is 0.7 or more and less than 2.5, it can be called STN (Super Twisted Nematic) mode, and when the ratio d / p is 2.5 or more, it can be called HTN (Highly Twisted Nematic) driving mode.
[0033] The pitch p of the liquid crystal layer may be measured by a method using a wedge cell, specifically, the method described in Simple method for accurate measurements of the cholesteric pitch using a stripe-wedge Grandjean-Cano cell by D. Podolskyy et al. (Liquid Crystals, Vol. 35, No. 7, July 2008, 789-791). The ratio d / p can be achieved by introducing an appropriate amount of chiral dopant into the liquid crystal layer.
[0034] The liquid crystal layer may further include a chiral dopant. When the liquid crystal layer includes a chiral agent, a twisted alignment state may be realized. The chiral agent (or chiral dopant) that may be included in the liquid crystal layer may be used without any particular limitation as long as it can induce a desired twisting without impairing the liquid crystal property, for example, nematic regularity. The chiral agent for inducing rotation in a liquid crystal compound must at least include chirality in its molecular structure. Examples of the chiral agent include a compound having one or more asymmetric carbons, a compound having an asymmetric point on a heteroatom such as a chiral amine or chiral sulfoxide, or a compound having an axially asymmetric, optically active site such as cumulene or binaphthol. The chiral agent may be, for example, a low molecular weight compound having a molecular weight of 1,500 or less. As the chiral agent, commercially available chiral nematic liquid crystals, such as commercially available chiral dopant liquid crystal S-811 from Merck and LC756 from BASF, may be used.
[0035] The application ratio of the chiral dopant is selected so as to achieve the desired ratio d / p. In general, the content (wt%) of the chiral dopant can be calculated by the formula 100 / HTP (Helixcal Twisting power)×pitch p (nm). The HTP represents the strength of the twist of the chiral dopant, and the content of the chiral dopant may be determined by taking into account the desired pitch with reference to the formula.
[0036] The liquid crystal element film 10 may include a spacer 14 for maintaining a distance between the first and second base layers. The distance between the first base layer and the second base layer may be maintained by the spacer 14. A liquid crystal layer may be present in an area where no spacer is present between the first base layer and the second base layer.
[0037] The spacer may be a patterned spacer. The spacer may have a column shape or a partition wall shape. The partition wall may divide the space between the second base layer and the first base layer into two or more spaces. In the area where the spacer is not present, other films or other layers present in the second base layer may be exposed. For example, the conductive layer may be exposed in the area where the spacer is not present. The alignment film may cover the spacer and the conductive layer exposed in the area where the spacer is not present. In the liquid crystal element film in which the first base layer and the second base layer are bonded, the alignment film present on the top of the spacer of the second base layer and the adhesive layer of the first base layer may be in contact with each other.
[0038] In the region where no spacer is present between the first base material layer and the second base material layer, a liquid crystal compound and the above-mentioned additives, such as a dichroic dye, a chiral agent, etc., may be present. The shape of the spacer is not particularly limited, and may be applied without limitation to have multiple faces such as a circle, an ellipse, or other polygonal shapes.
[0039] The spacer may include a curable resin. The type of the curable resin is not particularly limited, and may be, for example, a thermosetting resin or a photocurable resin, such as an ultraviolet curable resin. As the thermosetting resin, for example, a silicone resin, a silicon resin, a furan resin, a polyurethane resin, an epoxy resin, an amino resin, a phenol resin, a urea resin, a polyester resin, or a melamine resin may be used, but is not limited thereto. As the ultraviolet curable resin, a representative acrylic polymer, for example, a polyester acrylate polymer, a polystyrene acrylate polymer, an epoxy acrylate polymer, a polyurethane acrylate polymer, or a polybutadiene acrylate polymer, a silicone acrylate polymer, or an alkyl acrylate polymer may be used, but is not limited thereto.
[0040] The spacer may be formed by a patterning process. For example, the spacer may be formed by a photolithography process. The photolithography process may include a process of applying a curable resin composition onto a substrate layer or a conductive layer, and then irradiating the curable resin composition with ultraviolet light through a pattern mask. The pattern mask may be patterned into an ultraviolet light transmitting region and an ultraviolet light blocking region. The photolithography process may further include a process of washing the curable resin composition irradiated with ultraviolet light. The region irradiated with ultraviolet light is cured, and the region not irradiated with ultraviolet light remains in a liquid state, so that the region is removed through a washing process to perform patterning into a partition wall shape. In the photolithography process, in order to easily separate the resin composition from the pattern mask after ultraviolet light irradiation, a release treatment may be performed on the pattern mask, or a release paper may be placed between the layer of the resin composition and the pattern mask.
[0041] The width (line width), interval (pitch), thickness, and area of the spacer may be appropriately selected within a range that does not impair the object of the present application. For example, the width (line width) of the spacer may be in the range of 10 μm to 500 μm, or in the range of 10 μm to 50 μm. The interval (pitch) of the spacer may be in the range of 10 μm to 1000 μm, or in the range of 100 μm to 1000 μm. The area of the spacer may be about 5% or more, or 50% or less, with respect to the total area of the second base layer being 100%. When the area of the spacer is within the above range, it may be advantageous to ensure excellent electro-optical characteristics while appropriately ensuring the adhesive force between the first base layer and the second base layer. The thickness of the spacer may be, for example, in the range of 1 μm to 30 μm or 3 μm to 20 μm.
[0042] The spacer may have an optical density measured within a range of 1.1 to 4. The optical density can be determined by measuring the transmittance (unit: %) of the spacer and then substituting the measured transmittance into a formula for optical density (optical density=-log10(T), where T is the transmittance). Meanwhile, the method for measuring the transmittance of the spacer is not particularly limited, and may be measured by a known method. As an example, the transmittance of the spacer may be measured using 341C manufactured by X-rite.
[0043] In an optical device capable of adjusting the transmittance, color, and / or reflectance of light, the area where the spacer is present becomes an optically inactive area. In the present application, by applying spacers having the above-mentioned optical density, it is possible to prevent the occurrence of light leakage during operation of the device and ensure uniform optical performance.
[0044] As an example, the liquid crystal element film 10 may further include a conductive layer 12. The conductive layers may be formed on the first and second base layers 11a and 11b, respectively. The conductive layers may be formed on the surfaces of the base layers facing the liquid crystal layer 16.
[0045] The conductive layer 12 is a component for applying a voltage to the liquid crystal layer, and may be a known conductive layer without any particular limitation. Examples of the conductive layer include conductive polymers, conductive metals, conductive nanowires, metal oxides such as ITO (Indium Tin Oxide), carbon nanotubes, and graphene. Examples of conductive layers applicable to the present application are not limited to the above, and all types of conductive layers known to be applicable to liquid crystal element films in this field may be used.
[0046] As an example, the liquid crystal element film may further include an adhesive layer located between the liquid crystal layer 16 and the conductive layer 12 located on the surface of the first base layer 11a facing the liquid crystal layer.
[0047] The pressure-sensitive adhesive layer may be optically transparent. The pressure-sensitive adhesive layer may have an average transmittance of about 80% or more, 85% or more, 90% or more, or 95% or more in the visible light region, for example, in the wavelength range of 380 nm to 780 nm.
[0048] The adhesive layer may be a liquid crystal aligning adhesive layer. The adhesive layer may be, for example, a vertically aligning adhesive layer or a horizontally aligning adhesive layer. In this specification, the term "vertically aligning adhesive" may mean an adhesive having an adhesive force capable of imparting a vertical alignment force to adjacent liquid crystal compounds and bonding a first base layer and a second base layer. In this specification, the term "horizontally aligning adhesive" may mean an adhesive having an adhesive force capable of imparting a horizontal alignment force to adjacent liquid crystal compounds and bonding a first base layer and a second base layer. The pretilt angle of the adjacent liquid crystal compounds relative to the vertically aligning adhesive may be within a range of 80 degrees to 90 degrees, 85 degrees to 90 degrees, or about 87 degrees to 90 degrees, and the pretilt angle of the adjacent liquid crystal compounds relative to the horizontally aligning adhesive may be within a range of 0 degrees to 10 degrees, 0 degrees to 5 degrees, or 0 degrees to 3 degrees.
[0049] In this specification, the pretilt angle may refer to the angle that the director of the liquid crystal compound makes with respect to the liquid crystal alignment adhesive or alignment film and a plane horizontal thereto when no voltage is applied. In this specification, the director of the liquid crystal compound may refer to the optical axis or slow axis of the liquid crystal layer. Alternatively, the director of the liquid crystal compound may refer to the long axis direction when the liquid crystal compound is rod-shaped, and may refer to the axis parallel to the normal direction of the disc plane when the liquid crystal compound is discotic.
[0050] The thickness of the adhesive layer may be, for example, within a range of 3 μm to 15 μm. When the thickness of the adhesive layer is within this range, it can be advantageous in minimizing defects such as pressure-sensitive adhesive pressing or concentration when used in the manufacture of a liquid crystal element film while ensuring adhesion between the first base layer and the second base layer.
[0051] The adhesive layer may be made of various types of adhesives known in the industry as OCA (Optically Clear Adhesive). The adhesive may be different from OCR (Optically Clear Resin) type adhesives that are cured after the objects are bonded, in that the adhesive is cured before the objects are bonded. The adhesive may be, for example, an acrylic, silicone, epoxy, or urethane adhesive.
[0052] The adhesive layer may include a cured product of an adhesive resin. In one example, the adhesive layer may include a silicone-based adhesive. The silicone-based adhesive may include a cured product of a curable silicone compound as an adhesive resin.
[0053] The type of the curable silicone compound is not particularly limited, and for example, a heat-curable silicone compound or an ultraviolet-curable silicone compound may be used. The curable silicone compound may also be called an adhesive resin.
[0054] In one example, the curable silicone compound may be an addition-curable silicone compound.
[0055] Specifically, the addition curing silicone compound includes, but is not limited to, (1) an organopolysiloxane containing two or more alkenyl groups in the molecule and (2) an organopolysiloxane containing two or more silicon-bonded hydrogen atoms in the molecule. The silicone compound may form a cured product by addition reaction in the presence of a catalyst described later, for example.
[0056] More specific examples of the organopolysiloxane (1) that can be used in the present application include dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with trimethylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, and RSiO 1 / 2 Siloxane units represented by R12R2SiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R12R2SiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R1R2SiO 2 / 2 and the siloxane unit represented by RSiO 3 / 2 Siloxane units represented by RSiO 3 / 2 Examples of the organopolysiloxane copolymers include those containing siloxane units represented by the formula (I) and mixtures of two or more of the above, but are not limited thereto. In the above, R1 is a hydrocarbon group other than an alkenyl group, and specifically may be an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group, an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group, an aralkyl group such as a benzyl group or a phenethyl group, or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group, etc. In addition, in the above, R2 is an alkenyl group, and specifically may be a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, or a heptenyl group, etc.
[0057] More specific examples of the organopolysiloxane (2) that can be used in the present application include methylhydrogenpolysiloxanes capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogen copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogensiloxane-methylphenylsiloxane copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, dimethylsiloxane-methylphenylsiloxane copolymers capped with dimethylhydrogensiloxane groups at both molecular chain terminals, methylphenylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, and RSiO 1 / 2 Siloxane units represented by R12HSiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R12HSiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R1HSiO 2 / 2 Siloxane units represented by RSiO 3 / 2 Siloxane units represented by HSiO 3 / 2 and mixtures of two or more of the above, but are not limited thereto. In the above, R1 is a hydrocarbon group other than an alkenyl group, and specifically may be an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group, an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group, an aralkyl group such as a benzyl group or a phenethyl group, or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group.
[0058] When the adhesive layer is a vertically oriented adhesive layer, the surface energy may be 16 mN / m or less. The lower limit of the surface energy may be, for example, 5 mN / m or more. When the adhesive layer is a horizontally oriented adhesive layer, the surface energy may be more than 16 mN / m. The upper limit of the surface energy may be, for example, 50 mN / m or less. The surface energy may be measured using a Drop Shape Analyzer (Drop Shape Analyzer, KRUSS's DSA100 product). Specifically, deionized water with a known surface tension is dropped on the surface of the adhesive, the contact angle is measured, and the process is repeated five times to obtain the average value of the five contact angles obtained. Similarly, diiodomethane with a known surface tension is dropped on the surface of the adhesive, the contact angle is measured, and the process is repeated five times to obtain the average value of the five contact angles obtained. Then, the surface energy was calculated by substituting the value (Strom value) related to the surface tension of the solvent using the average contact angle for deionized water and diiodomethane obtained by the Owens-Wendt-Rabel-Kaelble method. The surface energy (γsurface) of the sample can be calculated by considering the dispersion force between nonpolar molecules and the interaction force between polar molecules (γsurface = γdispersion + γpolar), and the ratio of the polar term (γolar) in the surface energy γsurface can be defined as the polarity of the surface.
[0059] The first and second base layers of the liquid crystal element film may be attached to each other by an adhesive layer. Specifically, the adhesive layer of the first base layer and the spacer of the second base layer may be attached to each other. When an alignment film is formed on the spacer of the second base layer, a region of the alignment film corresponding to the spacer may be attached to the adhesive layer of the first base layer.
[0060] For example, the adhesive layer may have a storage modulus of 10 MPa or less. As another example, the storage modulus may be about 9.5 MPa or less, 9 MPa or less, 8.5 MPa or less, or about 2 MPa or less, and may be about 0.005 MPa or more, 0.006 MPa or more, 0.007 MPa or more, 0.008 MPa or more, 0.009 MPa or more, 0.01 MPa or more, 0.005 MPa or more, or about 0.1 MPa or more. In order to overcome the physical property limitations of the liquid crystal element film, outer substrates can be bonded to both sides of the liquid crystal element film via an intermediate layer, but due to the low modulus of the adhesive layer, it is vulnerable to external pressure, and defects such as collapse of the cell gap, flow and concentration of liquid crystal may occur during the bonding process. According to the present invention, the defects can be minimized by controlling the thickness of the intermediate layer included in the optical device as described below, and the structural stability and uniformity of the quality of the optical device can be ensured.
[0061] As an example, the liquid crystal element film may further include an alignment film 15. The alignment film may be a vertical alignment film or a horizontal alignment film. In this specification, the term "horizontal alignment film" may mean a layer containing an alignment material that imparts a horizontal alignment force to a liquid crystal compound present in an adjacent liquid crystal layer. In this specification, the term "vertical alignment film" may mean a layer containing an alignment material that imparts a vertical alignment force to a liquid crystal compound present in an adjacent liquid crystal layer. The pretilt angle of the adjacent liquid crystal compound relative to the vertical alignment film may be within a range of 80 degrees to 90 degrees, 85 degrees to 90 degrees, or about 87 degrees to 90 degrees, and the pretilt angle of the adjacent liquid crystal compound relative to the horizontal alignment film may be within a range of 0 degrees to 10 degrees, 0 degrees to 5 degrees, or 0 degrees to 3 degrees. Unlike the adhesive layer, the alignment film may not have an adhesive force that bonds the first base layer and the second base layer. In one example, the alignment film may have a peel force close to 0 with respect to the first base layer in the state of the liquid crystal element film of FIG. 1.
[0062] The alignment film may be a rubbing alignment film or a photo-alignment film. The alignment direction of the alignment film may be the rubbing direction in the case of a rubbing alignment film, and the direction of the irradiated polarized light in the case of a photo-alignment film, and such an alignment direction may be confirmed by a detection method using an absorbing linear polarizer. Specifically, the alignment direction may be confirmed by arranging an absorbing linear polarizer on one side of the liquid crystal layer in a state where the liquid crystal compound contained in the liquid crystal layer is horizontally aligned, and measuring the transmittance while rotating the polarizer 360 degrees. In the above state, when light is irradiated to the liquid crystal layer or the absorbing linear polarizer side and the brightness (transmittance) is measured on the other side, the transmittance tends to be low when the absorption axis or transmission axis coincides with the alignment direction of the liquid crystal alignment film, and the alignment direction may be confirmed through a simulation that reflects the refractive index anisotropy of the applied liquid crystal compound. A method for confirming the alignment direction depending on the mode of the liquid crystal layer is well known, and in this application, the alignment direction of the alignment film may be confirmed by such a well-known method.
[0063] The alignment film may be made of a polyimide compound, a poly(vinyl alcohol) compound, a poly(amic acid) compound, a polystyrene compound, a polyamide compound, a polyoxyethylene compound, or the like, which is a known material that exhibits alignment ability through rubbing alignment. Examples of such materials include polyimide compounds, polyamic acid compounds, polynorbornene compounds, phenylmaleimide copolymer compounds, polyvinylcinamate compounds, polyazobenzene compounds, polyethyleneimide compounds, polyvinylalcohol compounds, polyamide compounds, polyethylene compounds, polystyrene compounds, polyphenylenephthalamide compounds, polyester compounds, CMPI (chloromethylated The material may include, but is not limited to, one or more selected from the group consisting of known substances that can exhibit alignment ability upon light irradiation, such as a polyimide compound, a PVCI (polyvinylcinnamate) compound, and a polymethylmethacrylate compound.
[0064] As an example, the alignment film 15 may be located on the conductive layer 12 located on the surface of the second base layer 11b facing the liquid crystal layer. Specifically, when the adhesive layer 13 is located between the conductive layer 12 located on the surface of the first base layer 11a and the liquid crystal layer, the alignment film may be located on the conductive layer 12 located on the surface of the second base layer 11b. In this case, the spacer 14 may be formed in a patterned structure on the conductive layer 12 located on the surface of the second base layer 11b, and the alignment film may be located on the conductive layer on which the patterned spacer is formed. A liquid crystal element film 10 having a structure as shown in FIG. 1 may be manufactured by bonding a base layer having an adhesive layer formed on a conductive layer and a base layer having a spacer and an alignment film formed on a conductive layer. Meanwhile, since the adhesive layer located between the conductive layer 12 located on the surface of the first base layer 11a and the liquid crystal layer may have liquid crystal alignment properties, an alignment film may not be included on the surface of the first base layer facing the liquid crystal layer.
[0065] The structure in which the conductive layer formed on the first base layer is in contact with the spacer formed on the second base layer via the adhesive layer as described above can improve the adhesive strength between the elements constituting the liquid crystal element film, and therefore can prevent peeling between the elements constituting the liquid crystal element film and improve structural stability.
[0066] For example, the sheet may further include a sealant 17 that can adhere the first base material layer and the second base material layer while maintaining the gap between the first base material layer and the second base material layer. The material of the sealant is not particularly limited and may be any known material.
[0067] The optical device of the present application includes the above-mentioned liquid crystal element film. FIG. 2 is a cross-sectional view of an optical device according to an example of the present application. As shown in FIG. 2, the exemplary optical device 100 of the present application includes a first outer substrate 20a, a second outer substrate 20b arranged opposite to the first outer substrate, the liquid crystal element film 10 located between the first and second outer substrates, and an intermediate layer 30 located between the first outer substrate and the liquid crystal element film and between the liquid crystal element film and the second outer substrate. The expressions "first" and "second" do not define the front-back or top-bottom relationship of the outer substrates.
[0068] For example, the first and second outer substrates may each independently be an inorganic substrate or a plastic substrate.
[0069] The inorganic substrate is not particularly limited, and may be a known inorganic substrate. As an example, a glass substrate having excellent light transmittance may be used as the inorganic substrate. As the glass substrate, for example, a soda lime glass substrate, a general reinforced glass substrate, a borosilicate glass substrate, or an alkali-free glass substrate may be used, but is not limited thereto.
[0070] Examples of the plastic substrate include, but are not limited to, cellulose films such as TAC (triacetyl cellulose) or DAC (diacetyl cellulose), COP (cycloolefin copolymer) films such as norbornene derivatives, acrylic films such as PAR (Polyacrylate) or PMMA (poly(methyl methacrylate)), PC (polycarbonate) films, polyolefin films such as PE (polyethylene) or PP (polypropylene), PVA (polyvinyl alcohol) films, PI (polyimide) films, PSF (polysulfone) films, PPS (polyphenylsulfone film) or PES (poly ether sulfone) films, and other sulfone-based films, PEEK (polyetheretherketon), PEI (polyetherimide) films, PEN (polyethylenenaphthalate film) or PET (polyethyleneterephtalate) films, and other polyester-based films, and fluororesin films.
[0071] The first and second outer substrates 20a and 20b may have a coating layer of gold, silver, or a silicon compound such as silicon dioxide or silicon monoxide, or a functional layer such as an anti-reflection layer, if necessary.
[0072] The thickness of the first and second outer substrates 20a and 20b is not particularly limited and may be, for example, about 0.3 mm or more. In other examples, the thickness may be about 0.5 mm or more, 1 mm or more, 1.5 mm or more, or about 2 mm or more, or about 10 mm or less, 9 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, 5 mm or less, 4 mm or less, or about 3 mm or less.
[0073] For example, the first and second outer substrates 20a and 20b may be flat or curved. For example, the first and second outer substrates may be flat and curved at the same time, or one may be flat and the other may be curved.
[0074] When both of the above surfaces have a curved shape, the respective curvatures or radii of curvature may be the same or different.
[0075] In this specification, the curvature or radius of curvature may be measured by a method known in the art, for example, by using a non-contact device such as a 2D Profile Laser Sensor, a Chromatic confocal line sensor, or a 3D Measuring Confocal Microscopy. Methods for measuring the curvature or radius of curvature using such devices are well known.
[0076] In addition, for the first and second outer substrates, for example, when the curvature or radius of curvature of the front and back surfaces are different, the curvature or radius of curvature of the opposing surfaces, i.e., in the case of the first outer substrate, the curvature or radius of curvature of the surface opposing the second outer substrate, and in the case of the second outer substrate, the curvature or radius of curvature of the surface opposing the first outer substrate, may be the basis. In addition, when the curvature or radius of curvature of the surface is not constant and there are different portions, the maximum curvature or radius of curvature may be the basis, the minimum curvature or radius of curvature may be the basis, or the average curvature or radius of curvature may be the basis.
[0077] The first and second outer substrates 20a and 20b may have a difference in curvature or radius of curvature of about 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, or about 1%. The difference in curvature or radius of curvature may be a large curvature or radius of curvature C. L The smaller curvature or radius of curvature is called C S When this happens, 100×(CL -C S ) / C S The value is calculated by the formula: In addition, the lower limit of the difference in the curvature or radius of curvature is not particularly limited. Since the difference in the curvature or radius of curvature of the first and second outer substrates may be the same, the difference in the curvature or radius of curvature may be equal to or greater than about 0%.
[0078] The control of the curvature or radius of curvature as described above is useful in a structure in which a liquid crystal element film and / or a polarizer described later contacts an intermediate layer, such as the optical device of the present application. That is, if the curvature or radius of curvature exceeds 10%, when the outer substrate contacts the liquid crystal element film and / or the polarizer at the intermediate layer described later, a problem may occur in which the bonded outer substrate spreads due to a decrease in adhesion force. However, when controlled within 10%, the problem of the bonded outer substrate spreading due to a decrease in adhesion force can be efficiently prevented.
[0079] The first and second outer substrates may have the same sign of curvature. In other words, the first and second outer substrates may be curved in the same direction. That is, in this case, the center of curvature of the first outer substrate and the center of curvature of the second outer substrate are both present in the same portion of the upper and lower portions of the first and second outer substrates.
[0080] When the first and second outer substrates are bent in the same direction, the first and second outer substrates can be more efficiently bonded with the intermediate layer, and the adhesion strength between the first and second outer substrates and the liquid crystal element film and / or polarizer after bonding can be more efficiently prevented from decreasing.
[0081] The curvature or the radius of curvature of each of the first and second outer substrates 20a and 20b is not particularly limited. In one example, the first and second outer substrates may each have a radius of curvature of about 100R or more, 200R or more, 300R or more, 400R or more, 500R or more, 600R or more, 700R or more, 800R or more, or about 900R or more, or about 10,000R or less, 9,000R or less, 8,000R or less, 7,000R or less, 6,000R or less, 5,000R or less, 4,000R or less, 3,000R or less, 2,000R or less, 1,900R or less, 1,8000R or less, 1,7000R or less, 1,6000R or less, 1,5000R or less, 1,400R or less, 1,300R or less, 1,200R or less, 1,100R or less, or about 1,050R or less. In the above, R means the degree of curvature of a circle with a radius of 1 mm. Thus, for example, 100R in the above is the degree of curvature of a circle with a radius of 100 mm, or the radius of curvature for that circle.
[0082] The first and second outer substrates may have the same or different radii of curvature within the range. In one example, when the first and second outer substrates have different radii of curvature, the substrate having the larger curvature may have a radius of curvature within the range.
[0083] In one example, when the curvatures of the first and second outer substrates are different from each other, the substrate having the larger curvature may be the substrate that is disposed more in the direction of gravity when the optical device is used.
[0084] By controlling the curvature or radius of curvature of the first and second outer substrates as described above, even if the adhesion force of the intermediate layer described below decreases, the resultant force, which is the sum of the restoring force and gravity, acts to prevent spreading.
[0085] An optical device according to one example of the present application includes a liquid crystal element film 10 located between the first and second outer substrates 20a, 20b, and intermediate layers 30 located between the first outer substrate and the liquid crystal element film, and between the liquid crystal element film and the second outer substrate, respectively.
[0086] As an example, the intermediate layer has a sum of total thickness (total thickness) of 1,600 μm or more. As another example, the intermediate layer may have a sum of total thickness of about 1,650 μm or more, 1,700 μm or more, 1,750 μm or more, 1,800 μm or more, 1,850 μm or more, 1,900 μm or more, 1,950 μm, 2,000 μm or more, 2,100 μm or more, 2,150 μm or more, or about 2,200 μm or more, and may be about 6,000 μm or less, 5,900 μm or less, 5,800 μm or less, 5,700 μm or less, 5,600 μm or less, 5,500 μm or less, 5,400 μm or less, 5,300 μm or less, 5,200 μm or less, 5,100 μm or less, or about 5,000 μm or less.
[0087] Each of the intermediate layers may have a single layer structure of one intermediate layer, or may be a laminate of two or more sub-intermediate layers. The thickness and number of the sub-intermediate layers may be controlled in consideration of the desired thickness of the intermediate layer.
[0088] The sum of the total thicknesses of the intermediate layers means the sum of the thicknesses of the intermediate layers present between the first outer substrate and the liquid crystal element film and between the second outer substrate and the liquid crystal element film.
[0089] As one specific example, the sum of the thickness of the sub-intermediate layer laminate located between the first outer substrate and the liquid crystal element film and the thickness of the sub-intermediate layer laminate located between the second outer substrate and the liquid crystal element film is 1,600 μm or more in total, as shown in Figure 2. As another specific example, the sum of the thickness of the intermediate layer that is a single layer between the first outer substrate and the liquid crystal element film and the thickness of the intermediate layer that is a single layer between the second outer substrate and the liquid crystal element film is 1,600 μm or more in total.
[0090] In order to overcome the physical property limitations of the liquid crystal element film, outer substrates can be bonded to both sides of the liquid crystal element film via an intermediate layer, but due to the low modulus of the adhesive layer, it is vulnerable to external pressure, and defects such as collapse of the cell gap, flow and concentration of liquid crystals can occur during the bonding process. By controlling the thickness of the intermediate layer included in the optical device within the above range, the above defects can be minimized and the structural stability and uniform appearance characteristics of the optical device can be ensured.
[0091] If the sum of the total thicknesses of the intermediate layers is less than 1,600 μm, the liquid crystal element film of the optical device may have poor appearance such as pressing defects as shown in Figure 3, weak concentration defects as shown in Figure 4, or strong concentration defects as shown in Figure 5, which may degrade the quality of the optical device. On the other hand, if the sum of the total thicknesses of the intermediate layers exceeds 6,000 μm, the electro-optical properties such as the transmittance properties of the optical device may be degraded.
[0092] For example, a total thickness Ta of the intermediate layer located between the first outer substrate and the liquid crystal element film and a total thickness Tb of the intermediate layer located between the second outer substrate and the liquid crystal element film may be within a range of 200 to 3,000 μm. As another example, the Ta and Tb may be about 210 μm or more, 220 μm or more, 230 μm or more, 240 μm or more, 250 μm or more, 260 μm or more, 270 μm or more, 280 μm or more, 290 μm or more, 300 μm or more, 310 μm or more, 320 μm or more, 330 μm or more, 340 μm or more, 350 μm or more, or about 300 μm or more, and may be about 2,950 μm or less, 2,900 μm or less, 2,850 μm or less, 2,800 μm or less, 2,750 μm or less, 2,700 μm or less, 2,650 μm or less, or about 2,600 μm or less, respectively.
[0093] The sum of the total thicknesses Ta of the intermediate layers between the first outer substrate and the liquid crystal element film means the sum of the total thicknesses of all the intermediate layers between the first outer substrate and the liquid crystal element film, and the sum of the total thicknesses Tb of the intermediate layers between the second outer substrate and the liquid crystal element film means the sum of the thicknesses of all the intermediate layers between the second outer substrate and the liquid crystal element film. Therefore, when a liquid crystal display includes a first polarizer located between a first outer substrate and a liquid crystal element film, and a second polarizer located between the second outer substrate and a liquid crystal element film, and an intermediate layer is included between the first polarizer and the liquid crystal element film and between the second polarizer and the liquid crystal element film, the sum of the total thicknesses Ta of the intermediate layers located between the first outer substrate and the liquid crystal element film means the sum of the thicknesses of the intermediate layer located between the first outer substrate and the first polarizer, and the intermediate layer located between the first polarizer and the liquid crystal element film, and the sum of the total thicknesses Tb of the intermediate layers located between the second outer substrate and the liquid crystal element film means the sum of the thicknesses of the intermediate layer located between the second outer substrate and the second polarizer, and the intermediate layer located between the second polarizer and the liquid crystal element film.
[0094] When the total thickness Ta of the intermediate layer located between the first outer substrate and the liquid crystal element film and the total thickness Tb of the intermediate layer located between the second outer substrate and the liquid crystal element film are each in the range of 200 to 3,000 μm, it may be more advantageous in improving appearance defects of the liquid crystal element film.
[0095] As an example, a thickness ratio Ta / Tb of a total thickness Tb of the intermediate layer 30 located between the second outer substrate 20b and the liquid crystal element film 10 to a total thickness Ta of the intermediate layer 30 located between the first outer substrate 20a and the liquid crystal element film 10 may be within a range of 0.1 to 10. As another example, the thickness ratio Ta / Tb may be about 0.12 or more, about 0.13 or more, or about 0.14 or more, and may be about 9.5 or less, 9.0 or less, 8.5 or less, 8.0 or less, 7.5 or less, or about 7.0 or less. When the thickness ratio is within a range of 0.1 to 10, it is possible to more effectively improve the appearance defect of the liquid crystal element film.
[0096] As one example, the intermediate layer 30 may have a Young's modulus (E) in the range of 0.1 MPa to 100 MPa. As another example, the Young's modulus E of the intermediate layer may be about 0.2 MPa or more, 0.4 MPa or more, 0.6 MPa or more, 0.8 MPa or more, 1 MPa or more, 5 MPa or more, or about 10 MPa or more, or about 95 MPa or less, 80 MPa or less, 75 MPa or less, 70 MPa or less, 65 MPa or less, 60 MPa or less, 55 MPa or less, or about 50 MPa or less.
[0097] The Young's modulus E can be measured, for example, by the method specified in ASTM D882, by cutting the film in the shape specified in the standard and using equipment capable of measuring a stress-strain curve (capable of simultaneously measuring force and length), such as a universal testing machine (UTM). By selecting the intermediate layer to have the above Young's modulus, an optical device with better durability can be provided.
[0098] As an example, the intermediate layer 30 in the present application may have a thermal expansion coefficient of 2,000 ppm / K or less. In other examples, the thermal expansion coefficient may be about 1,900 ppm / K or less, 1,700 ppm / K or less, 1,600 ppm / K or less, or about 1,500 ppm / K or less, or about 10 ppm / K or more, 20 ppm / K or more, 30 ppm / K or more, 40 ppm / K or more, 50 ppm / K or more, 60 ppm / K or more, 70 ppm / K or more, 80 ppm / K or more, 90 ppm / K or more, 100 ppm / K or more, 200 ppm / K or more, 300 ppm / K or more, 400 ppm / K or more, 500 ppm / K or more, 600 ppm / K or more, 700 ppm / K or more, or about 800 ppm / K or more. The thermal expansion coefficient of the intermediate layer can be measured, for example, according to the standard of ASTM D696, by cutting the intermediate layer in a shape specified in the standard, measuring the change in length per unit temperature, and calculating the thermal expansion coefficient, which can be measured by a known method such as TMA (ThermoMechanic Analysis). By selecting the intermediate layer to have the above-mentioned thermal expansion coefficient, an optical device with better durability can be provided.
[0099] The intermediate layer is not particularly limited, and may be a known adhesive layer that satisfies the above-mentioned physical properties, such as Young's modulus and thermal expansion coefficient, etc. For example, the intermediate layer may be a thermoplastic polyurethane adhesive layer, a polyamide adhesive layer, a polyester adhesive layer, an EVA (Ethylene Vinyl Acetate) adhesive layer, an acrylic adhesive layer, a silicone adhesive layer, or a polyolefin adhesive layer that satisfies the above-mentioned physical properties.
[0100] As an example, the optical device according to the present application may include a first polarizer located between the first outer substrate and the liquid crystal element film, and a second polarizer located between the second outer substrate and the liquid crystal element film. In this specification, the term polarizer means a film, sheet, or element having a polarizing function. A polarizer is a functional element that can extract light vibrating in one direction from incident light vibrating in various directions.
[0101] The first polarizer and the second polarizer may be an absorptive polarizer or a reflective polarizer, respectively. In this specification, the absorptive polarizer means an element that exhibits selective transmission and absorption characteristics for incident light. For example, the polarizer may transmit light that vibrates in one direction from incident light that vibrates in various directions, and absorb light that vibrates in the remaining directions. In this specification, the reflective polarizer means an element that exhibits selective transmission and reflection characteristics for incident light. For example, the polarizer may transmit light that vibrates in one direction from incident light that vibrates in various directions, and reflect light that vibrates in the remaining directions. According to one embodiment of the present application, the polarizer may be an absorptive polarizer.
[0102] The first polarizer and the second polarizer may each be a linear polarizer. In this specification, a linear polarizer means that the selectively transmitted light is linearly polarized light that vibrates in one direction, and the selectively absorbed or reflected light is linearly polarized light that vibrates in a direction perpendicular to the vibration direction of the linearly polarized light. In the case of an absorptive linear polarizer, the light transmission axis and the light absorption axis may be perpendicular to each other. In the case of a reflective linear polarizer, the light transmission axis and the light reflection axis may be perpendicular to each other.
[0103] In one example, the first polarizer and the second polarizer may each be a polymer stretched film dyed with iodine or an anisotropic dye. The polymer stretched film may be a PVA (polyvinyl alcohol) stretched film. In another example, the first polarizer and the second polarizer may each be a guest-host type polarizer having a liquid crystal polymerized in an oriented state as a host and an anisotropic dye aligned by the orientation of the liquid crystal as a guest. In another example, the first polarizer and the second polarizer may each be a thermotropic liquid crystal film or a lyotropic liquid crystal film.
[0104] A protective film, an anti-reflection film, a retardation film, an adhesive layer, an adhesive layer, a surface treatment layer, etc. may be further formed on one or both sides of the first polarizer and the second polarizer. The retardation film may be, for example, a quarter-wave plate or a half-wave plate. The quarter-wave plate may have an in-plane retardation value in the range of about 100 nm to 180 nm, or 100 nm to 150 nm, for light with a wavelength of 550 nm. The half-wave plate may have an in-plane retardation value in the range of about 200 nm to 300 nm, or 250 nm to 300 nm, for light with a wavelength of 550 nm. The retardation film may be, for example, a polymer stretched film or a liquid crystal polymerized film.
[0105] The transmittance of the first polarizer and the second polarizer for light with a wavelength of 550 nm may be within a range of 40% to 50%. The transmittance may refer to the single transmittance of the polarizer for light with a wavelength of 550 nm. The single transmittance of the polarizer may be measured, for example, using a spectrometer (V7100, manufactured by Jasco). For example, the air may be set as the baseline in a state where a polarizer sample (not including upper and lower protective films) is attached to the instrument, and the axis of the polarizer sample is aligned vertically and horizontally with the axis of the reference polarizer, and then the single transmittance may be calculated.
[0106] The light transmission axis of the first polarizer and the light transmission axis of the second polarizer may be perpendicular to each other. Specifically, the angle between the light transmission axis of the first polarizer and the light transmission axis of the second polarizer may be within a range of 80 degrees to 100 degrees or 85 degrees to 95 degrees. When the light transmission axis of the first polarizer and the light transmission axis of the second polarizer are perpendicular to each other, light leakage may occur depending on the distance between the first polarizer and the second polarizer.
[0107] According to the present application, the intermediate layer may include an intermediate layer located between the first polarizer and the liquid crystal element film and between the second polarizer and the liquid crystal element film, respectively, and having a thickness of 380 μm or less. That is, the thickness of the intermediate layer located between the first polarizer and the liquid crystal element film and the intermediate layer located between the second polarizer and the liquid crystal element film may each be 380 μm or less. This can minimize the separation distance between the first polarizer and the second polarizer, thereby reducing light leakage and ensuring the structural safety of the liquid crystal element film. The lower limit of the thickness of the intermediate layer located between the first polarizer and the liquid crystal element film and the intermediate layer located between the second polarizer and the liquid crystal element film may each be 10 μm or more.
[0108] In one example, the thickness of the intermediate layer located between the first outer substrate and the first polarizer and the intermediate layer located between the second outer substrate and the second polarizer may be in the range of 400 μm to 3,000 μm. In another example, the thickness of the intermediate layer located between the first outer substrate and the first polarizer and the intermediate layer located between the second outer substrate and the second polarizer may be about 400 μm or more, 500 μm or more, 600 μm or more, 700 μm or more, 800 μm or more, 900 μm or more, 1,000 μm or more, or 1,100 μm or more, and may be about 3,000 μm or less, 2,800 μm or less, 2,600 μm or less, 2,400 μm or less, about 2,200 μm or less, about 2,000 μm or less, about 1,800 μm or less, about 1,600 μm or less, or about 1,400 μm or less. When the thicknesses of the intermediate layer located between the first outer substrate and the first polarizer and the intermediate layer located between the second outer substrate and the second polarizer are within the above ranges, respectively, it may be advantageous to ensure structural stability and uniform appearance characteristics without appearance defects during the outer substrate bonding process without impairing the electro-optical properties of the optical device.
[0109] According to another embodiment of the present application, an optical device may include a first outer substrate, a second outer substrate disposed opposite to the first outer substrate, a liquid crystal element film disposed between the first and second outer substrates, and intermediate layers respectively disposed between the first outer substrate and the liquid crystal element film, between the liquid crystal element film and the second outer substrate, and at an outer portion of the liquid crystal element film, wherein the intermediate layers respectively disposed between the first outer substrate and the liquid crystal element film, and between the liquid crystal element film and the second outer substrate have a sum of total thicknesses of 1,600 μm or more, and the liquid crystal element film may be encapsulated between the first outer substrate and the liquid crystal element film, between the liquid crystal element film and the second outer substrate, and at an outer portion of the liquid crystal element film, between the first outer substrate and the second outer substrate.
[0110] According to yet another embodiment of the present application, an optical device includes a first outer substrate, a second outer substrate disposed opposite to the first outer substrate, a liquid crystal element film disposed between the first and second outer substrates, a first polarizer disposed between the first outer substrate and the liquid crystal element film, a second polarizer disposed between the second outer substrate and the liquid crystal element film, and intermediate layers respectively disposed between the first outer substrate and the first polarizer, between the first polarizer and the liquid crystal element film, between the liquid crystal element film and the second polarizer, between the second polarizer and the second outer substrate, and at an outer portion of the liquid crystal element film. The intermediate layers located between the first outer substrate and the first polarizer, between the first polarizer and the liquid crystal element film, between the liquid crystal element film and the second polarizer, and between the second polarizer and the second outer substrate may have a sum of total thicknesses of 1,600 μm or more, and the liquid crystal element film may be encapsulated between the first outer substrate and the second outer substrate by intermediate layers located between the first outer substrate and the first polarizer, between the first polarizer and the liquid crystal element film, between the liquid crystal element film and the second polarizer, between the second polarizer and the second outer substrate, and on the outer portion of the liquid crystal element film, respectively.
[0111] In the present application, the term "outer portion of the liquid crystal element film" may refer to a side portion surrounding the liquid crystal element film. Alternatively, the term "encapsulation" in the present application may refer to covering the front surface of the liquid crystal element film and / or the polarizer as an intermediate layer. For example, the structure may be realized by laminating an outer substrate, an intermediate layer, a liquid crystal element film, an intermediate layer, and an outer substrate according to a desired structure, positioning an intermediate layer on the outer portion of the liquid crystal element film, and then pressing in a vacuum state. This encapsulation structure significantly improves the durability and weather resistance of the optical device, and as a result, it can be stably applied to outdoor applications such as sunroofs.
[0112] The method for manufacturing the optical device of the present application is not particularly limited. In one example, the optical device may be manufactured through an autoclave process for the above-mentioned encapsulation.
[0113] For example, the method for manufacturing the optical device may include encapsulating the liquid crystal element film and / or the polarizer between the first and second outer substrates through an autoclave process using an intermediate layer.
[0114] The autoclave process may be performed by disposing the intermediate layer, the liquid crystal element film and / or the polarizer between the outer substrates according to a desired encapsulation structure, and applying heat and pressure.
[0115] As an example, when a laminate in which a first outer substrate 20a, an intermediate layer 30, a liquid crystal element film 10, an intermediate layer 30, and a second outer substrate 20b are arranged in the above order, and an intermediate layer 30 is also arranged on the outer portion of the liquid crystal element film, is heated / pressurized in an autoclave process, an optical device as shown in Fig. 2 can be formed. As another example, when a laminate in which a first outer substrate 20a, an intermediate layer 30, a first polarizer 40, an intermediate layer 30, a liquid crystal element film 10, an intermediate layer 30, a second polarizer 40, an intermediate layer 30, and a second outer substrate 20b are arranged in the above order, and an intermediate layer 30 is also arranged on the outer portions of the liquid crystal element film and the polarizer, is heated / pressurized in an autoclave process, an optical device as shown in Fig. 6, Fig. 7, or Fig. 8 can be formed.
[0116] The conditions of the autoclave process are not particularly limited, and may be performed at an appropriate temperature and pressure depending on the type of intermediate layer applied. The temperature of the typical autoclave process is about 80°C or more, 90°C or more, or 100°C or more, and the pressure is 2 atm or more, but is not limited thereto. The upper limit of the process temperature may be about 200°C or less, 190°C or less, 180°C or less, or 170°C or less, and the upper limit of the process pressure may be about 10 atm or less, 9 atm or less, 8 atm or less, 7 atm or less, or 6 atm or less.
[0117] Such optical devices may be used for various purposes, for example, in eyewear such as sunglasses and eyewear for AR (Argumented Reality) or VR (Virtual Reality), the exterior walls of buildings, and sunroofs for vehicles.
[0118] In one example, the optical device may itself be a sunroof for a vehicle.
[0119] For example, the optical device or vehicle sunroof may be mounted in an automobile including a vehicle body having at least one opening formed therein. Effect of the Invention
[0120] The optical device of the present application properly maintains the cell gap of the liquid crystal element film, has excellent adhesion between the upper and lower substrates, and minimizes defects such as pressing and concentration during the bonding process of the outer substrates, thereby ensuring structural stability and good quality uniformity. [Brief description of the drawings]
[0121] [Figure 1] FIG. 2 is a cross-sectional view of an exemplary liquid crystal element film of the present application. [Diagram 2] 1 is a cross-sectional view of an exemplary optical device of the present application. [Diagram 3] This is an image of an optical device in which a liquid crystal element film has become defective due to external pressure. [Figure 4] This is an image of an optical device in which a weak concentration defect has occurred in the liquid crystal element film due to external pressure. [Diagram 5] This is an image of an optical device in which a strong concentration defect has occurred in the liquid crystal element film due to external pressure. [Figure 6] FIG. 2 is a cross-sectional view of an optical device manufactured in Example 1 of the present application. [Figure 7] FIG. 2 is a cross-sectional view of an optical device manufactured in Example 2 of the present application. [Figure 8] FIG. 2 is a cross-sectional view of an optical device manufactured in Example 3 of the present application. [Figure 9] FIG. 2 is a cross-sectional view of an optical device manufactured in Comparative Example 1 or Comparative Example 2 of the present application. [Figure 10] 1 shows photographed images of the optical devices manufactured in Example 1 and Example 2. [Figure 11] 1 shows the results of measuring the transmittance of the optical devices manufactured in Example 1 and Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0122] Hereinafter, the present application will be described in detail with reference to examples, but the scope of the present application is not limited to the following examples.
[0123] Measurement example 1. Storage modulus measurement The storage modulus was measured using DMA Q800 manufactured by TA Corp. Specifically, the storage modulus was recorded in Multi-Frequency-Strain mode under the conditions of a temperature of 25° C., a force of 0.01 N, and a ramp rate of 3° / min.
[0124] Manufacturing of liquid crystal element films A polycarbonate film (Keiwa) with a thickness of about 100 μm and a horizontal x vertical area of 600 mm x 300 mm was prepared as the first base layer. ITO (indium-tin-oxide) was vapor-deposited on the first base layer to a thickness of 50 nm to form a conductive layer. An adhesive composition (KR-3700, Shin-Etsu) was bar-coated on the conductive layer, and then dried at about 150° C. for about 5 minutes to form an adhesive layer with a thickness of about 10 μm. The storage modulus of the adhesive layer was about 0.1 MPa. The combination of the first base layer, the conductive layer, and the adhesive layer is called the upper laminate.
[0125] A polycarbonate film (Keiwa) with a thickness of about 100 μm and a horizontal x vertical area of 600 mm x 300 mm was prepared as the second base layer. ITO (indium-tin-oxide) was vapor-deposited to a thickness of 50 nm on the second base layer to form a conductive layer. An acrylic resin composition (KAD-03, Minutec) was coated on the conductive layer, and then a honeycomb-type spacer was formed by photolithography. The pitch of the regular hexagons (closed shape) constituting the honeycomb was about 450 μm, the height was about 12 μm, and the line width was about 30 μm. The area of the closed shape (regular hexagon) formed by the spacer was about 2.14 mm. 2 A vertical alignment film (Nissan, SE-5661) was coated on the spacer to a thickness of about 300 nm, and then rubbed in one direction. The combination of the second substrate layer, the conductive layer, the spacer, and the vertical alignment film is called the lower laminate.
[0126] A liquid crystal composition was coated on the vertical alignment film of the lower laminate to form a liquid crystal layer, and then the adhesive layer of the upper laminate was laminated opposite the liquid crystal composition coated surface to prepare a liquid crystal element film. The liquid crystal composition included a liquid crystal compound (Merck, MAT-16-568) and a chiral dopant (HCCH, S811), and the pitch p of the liquid crystal layer formed as above was about 20 μm.
[0127] Optical Device Manufacturing Example 1 A laminate was manufactured by sequentially disposing intermediate layers on all the outer peripheries of the liquid crystal element film, which sequentially included a first outer substrate, a first intermediate layer, a first polarizer, a second intermediate layer, the manufactured liquid crystal element film, a third intermediate layer, a second polarizer, a fourth intermediate layer, and a second outer substrate. The second outer substrate was disposed in the direction of gravity compared to the first outer substrate.
[0128] The first polarizer and the second polarizer were PVA polarizers, and were arranged so that the light transmission axis of the first polarizer and the light transmission axis of the second polarizer were at about 90 degrees. The first outer substrate was a glass substrate having a thickness of about 3 mm, an area of 300 mm x 300 mm (horizontal x vertical), and a curvature radius of about 2,470R. The second outer substrate was a glass substrate having a thickness of about 3 mm, an area of 300 mm x 300 mm (horizontal x vertical), and a curvature radius of about 2,400R.
[0129] The second and third intermediate layers are each a single layer of TPU (Argotec) with a thickness of approximately 380 μm. The first and fourth intermediate layers are each a laminate of three TPU (Argotec) layers with a thickness of approximately 380 μm. The TPU layer (Argotec) has a thermal expansion coefficient of 307 ppm / K and a storage modulus of 8 to 15 MPa. The intermediate layers disposed on the outer periphery of the liquid crystal element film are also formed from the same material as the first to fourth intermediate layers.
[0130] The laminate was subjected to an autoclave process at a temperature of about 110° C. and a pressure of about 2 atm to produce an optical device having the structure shown in Fig. 6. In the optical device of Example 1, the second intermediate layer and the third intermediate layer each had a thickness of about 380 μm, and the total thickness of the intermediate layers was about 3,040 μm.
[0131] Example 2 Except for changing the first and fourth intermediate layers to single layers of TPU (Argotec) having a thickness of about 380 μm, and changing the second and third intermediate layers to laminates of three TPU layers (Argotec) each having a thickness of about 380 μm, the same process as in Example 1 was carried out to fabricate an optical device having the structure shown in Fig. 7. In the optical device of Example 2, the total thickness of the intermediate layers was about 3,040 μm.
[0132] Example 3 Except for changing the first and fourth intermediate layers to single layers of TPU (Argotec) having a thickness of about 380 μm, and changing the second and third intermediate layers to laminates of two TPU layers (Argotec) each having a thickness of about 380 μm, the same process as in Example 1 was carried out to fabricate an optical device having the structure shown in Fig. 8. In the optical device of Example 3, the total thickness of the intermediate layers was about 2,280 μm.
[0133] Comparative Example 1 Except for changing the first intermediate layer, the second intermediate layer, the third intermediate layer, and the fourth intermediate layer to a single TPU layer (Argotec) having a thickness of about 380 μm, the same process as in Example 1 was carried out to fabricate an optical device having the structure shown in Fig. 9. In the optical device of Comparative Example 1, the total thickness of the intermediate layers was about 1,520 μm.
[0134] Comparative Example 2 Except for changing the first and fourth intermediate layers to single layers of TPU (Argotec) having a thickness of about 150 μm, and changing the second and third intermediate layers to single layers of TPU (Argotec) having a thickness of about 380 μm, the same process as in Example 1 was carried out to fabricate an optical device having the structure shown in Fig. 9. In the optical device of Comparative Example 2, the total thickness of the intermediate layers was about 1,060 μm.
[0135] Evaluation example 1: Appearance defect evaluation method The appearance defects were measured using an optical microscope (Olympus, BX51-N33MB) to see whether the appearance defects as shown in Figs. 3 to 5 were observed in the optical devices manufactured in the examples and comparative examples. The optical devices manufactured in Examples 1, 2, and 3 did not show appearance defects such as pressing defects, weak concentration defects, and strong concentration defects as shown in Figs. 3 to 5. In contrast, the optical devices manufactured in Comparative Examples 1 and 2 showed appearance defects such as pressing defects, weak concentration defects, and strong concentration defects in the liquid crystal element film due to external pressure. Therefore, it can be confirmed that the optical devices manufactured in Examples 1, 2, and 3, in which the total thickness of the intermediate layer is 1,600 μm or more, have excellent appearance even when manufactured by a high-temperature and high-pressure autoclave process, compared to the optical devices manufactured in Comparative Examples 1 and 2, in which the total thickness of the intermediate layer is less than 1,600 μm.
[0136] Evaluation example 2: Light leakage observation Fig. 10 is a photograph (Olympus, BX51-N33MB) of the optical devices manufactured in Example 1 and Example 2 taken in a state where no voltage is applied. Fig. 10(a) and (b) are images of Example 1 and Example 2, respectively, in a state where no voltage is applied, and Fig. 10(c) and (d) are images of Example 1 and Example 2, respectively, in a state where a voltage of 50 V is applied. From Fig. 10(a) and (b), it can be observed that Example 1 has less light leakage in a state where no voltage is applied compared to Example 2.
[0137] Evaluation example 3: Electro-optical characteristic evaluation The optical devices manufactured in Example 1 and Example 2 were measured for transmittance in all directions (azimuth angles 0° to 360°) at a polar angle of 60°, and the results are shown in FIG. 11. The transmittance was measured using a haze meter (CA-2500, manufactured by Konica Minolta) in a state where no voltage was applied to the optical device. The transmittance is the average transmittance for light with wavelengths of 380 nm to 780 nm, and the lower the transmittance, the less the light leakage. In FIG. 11, the relative transmittance means the relative transmittance when the backlight light amount is 100%. The azimuth angle of 0° is parallel to the rubbing axis of the alignment film of the liquid crystal element film. Example 1 and Example 2 each showed the maximum transmittance at an azimuth angle of 110°, with Example 1 having a transmittance of 5.51% at an azimuth angle of 110° and Example 2 having a transmittance of 6.03% at an azimuth angle of 110°. Furthermore, Example 1 and Example 2 showed the greatest difference in transmittance at an azimuth angle of 60°, with Example 1 having a transmittance of 3.17% at an azimuth angle of 60° and Example 2 having a transmittance of 4.04% at an azimuth angle of 60°.
Claims
1. A first outer substrate; a second outer substrate disposed opposite to the first outer substrate; a liquid crystal element film disposed between the first outer substrate and the second outer substrate; an intermediate layer located between the first outer substrate and a liquid crystal element film, and between the liquid crystal element film and a second outer substrate; a first polarizer disposed between the first outer substrate and the liquid crystal element film, and a second polarizer disposed between the second outer substrate and the liquid crystal element film; the intermediate layer is located between the first polarizer and the liquid crystal element film, and between the second polarizer and the liquid crystal element film, and includes an intermediate layer having a thickness of 380 μm or less; The total thickness of the intermediate layers is 1,600 μm or more, The liquid crystal element film includes a first base layer and a second base material layer disposed opposite the first base material layer; a liquid crystal layer located between the first base material layer and the second base material layer; a conductive layer located on a surface of the first base material layer and a surface of the second base material layer facing the liquid crystal layer; the conductive layer is located on a surface of the first base layer facing the liquid crystal layer, and an adhesive layer is located between the conductive layer and the liquid crystal layer; the liquid crystal element film does not include an alignment film on a surface of the first base layer facing the liquid crystal layer, The pressure-sensitive adhesive layer has a storage modulus of 10 MPa or less. Optical devices.
2. The liquid crystal element film is The optical device of claim 1 , further comprising: a patterned spacer that maintains a spacing between the first substrate layer and the second substrate layer.
3. The liquid crystal element film is characterized in that the first base material layer and the second base material layer are each independently a PEN (polyethylene-naphthalate) film, a PI (polyimide) film, a COP (cyclo-olefin polymer) film, a TAC (tri-acetyl-cellulose) film, a PET (polyethyleneterephthalate) film, or a PC (polycarbonate) film. The optical device according to claim 1 or 2.
4. The optical device according to any one of claims 1 to 3, wherein the liquid crystal element film further comprises an alignment film located on the conductive layer located on the surface of the second substrate layer facing the liquid crystal layer.
5. The optical device according to claim 4 dependent on claim 2, wherein the spacers are formed on the conductive layer, and the alignment film is located on the conductive layer on which the spacers are formed.
6. The optical device according to any one of claims 1 to 5, wherein the liquid crystal layer of the liquid crystal element film comprises a dichroic dye guest.
7. 7. The optical device according to claim 1, wherein the liquid crystal element film is capable of switching between first and second alignment states.
8. The optical device according to claim 1 , wherein the first outer substrate and the second outer substrate are glass substrates.
9. The optical device according to any one of claims 1 to 8, wherein a total thickness Ta of the intermediate layer located between the first outer substrate and the liquid crystal element film and a total thickness Tb of the intermediate layer located between the second outer substrate and the liquid crystal element film are each within a range of 200 to 3,000 μm.
10. The optical device of any one of claims 1 to 9, wherein a thickness ratio Ta / Tb of a total thickness Tb of an intermediate layer located between the second outer substrate and the liquid crystal element film to a total thickness Ta of the intermediate layer located between the first outer substrate and the liquid crystal element film is within a range of 0.1 to 10.
11. 11. The optical device according to claim 1, wherein the intermediate layer has a Young's modulus in the range of 0.1 MPa to 100 MPa.
12. The optical device according to any one of claims 1 to 11, wherein the intermediate layer has a thermal expansion coefficient of 2,000 ppm / K or less.
13. 13. The optical device according to claim 1, wherein the intermediate layer is a thermoplastic polyurethane adhesive layer, a polyamide adhesive layer, a polyester adhesive layer, an EVA (Ethylene Vinyl Acetate) adhesive layer, an acrylic adhesive layer, a silicone adhesive layer, or a polyolefin adhesive layer.
14. The optical device according to any one of claims 1 to 13, wherein the light transmission axis of the first polarizer and the light transmission axis of the second polarizer are perpendicular to each other.
15. 15. A motor vehicle comprising a body having one or more openings formed therein, and an optical device according to any one of claims 1 to 14 attached to said openings.
Citation Information
Patent Citations
PDLC grating of lcd equipment and making method
CN101424814A
Liquid crystal display device and its production
JP1999242228A
Display device with spacer and seal, and method of manufacturing same
JP2007504502A
Dimming device and manufacturing method of the same
JP2020030355A
Light control device, transparent display device including the same, and method of manufacturing the same
US20170090237A1