Laminated film and its manufacturing method

The sputtering method for gallium nitride film formation addresses misaligned growth on rough substrates by controlling gas composition and energy, resulting in a highly oriented and dense laminated film for semiconductor applications.

JP7556197B2Active Publication Date: 2024-09-26TOSOH CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020005715
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-17
Publication Date
2024-09-26
Estimated Expiration
2040-01-17

AI Technical Summary

Technical Problem

Existing methods for growing gallium nitride thin films on substrates with rough or porous surfaces result in misaligned crystal growth, leading to non-dense films with low crystallinity and poor adhesion.

Method used

A sputtering method using a gallium nitride target is employed to control gas composition and energy during film formation, achieving high crystallinity and density by controlling crystal orientation and substrate alignment.

Benefits of technology

The method produces a laminated film with high coverage and improved crystallinity, suitable for semiconductor devices like LEDs and power devices, even on rough substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556197000001
    Figure 0007556197000001
Patent Text Reader

Abstract

To provide a gallium nitride film and a method for producing the film by a sputtering process using a gallium nitride target.SOLUTION: Using a sputtering process using a gallium nitride sintered body with a reduced oxygen content as the main component of a sputtering target, film deposition conditions are optimized, to deposit a gallium nitride film on a porous substrate with large surface roughness.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Gallium nitride has attracted attention as a raw material for the light-emitting layer of blue light-emitting diodes (LEDs) and blue laser diodes (LDs). In recent years, it has been used in various applications such as white LEDs and blue LDs in the form of thin films and substrates, and is also attracting attention as a material for power devices in the future. Currently, gallium nitride thin films are generally manufactured by the metal-organic chemical vapor deposition (MOCVD) method. The MOCVD method is a method in which the vapor of the raw material is contained in a carrier gas and transported to the surface of a substrate, where the raw material is decomposed by reacting with the heated substrate to grow crystals. Another method is the hydride vapor phase epitaxy (HVPE) method, which is used for single crystal growth.

[0002] Conventionally, epitaxial growth of gallium nitride-based materials has been a technique that can only grow extremely smooth and dense films with an Ra of 1 nm, and the mechanism is that in MOCVD and HVPE methods, nuclei first form and grow into islands, which then densify and grow into a film shape. However, for example, on substrates with rough or porous surfaces, the crystals do not orient during island growth, and furthermore, the growth of the islands does not match during the densification process, making it difficult to obtain a dense film.

[0003] Meanwhile, sputtering is another method for producing thin films other than MOCVD and HVPE. This method involves physically colliding positive ions such as Ar ions with a target placed at the cathode, releasing the material that makes up the target with the collision energy, and depositing a film with approximately the same composition as the target material on a substrate placed opposite. There are two types of sputtering: direct current sputtering (DC sputtering) and radio frequency sputtering (RF sputtering).

[0004] Furthermore, Patent Document 2 proposes a sintered body of gallium nitride with a low oxygen content, but there is no description of growing a thin film using the same on a porous substrate or a substrate with a rough surface. Further investigation into the film formation conditions and further reduction in the oxygen content of gallium nitride were necessary. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-147271 A [Patent Document 2] JP 2014-159368 A [Non-patent literature]

[0006] [Non-Patent Document 1] Applied Physics Letters 97, 141902 (2010) [Non-Patent Document 2] Japanese Journal of Applied Physics 53, 11RC01 (2014) Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a laminated film including a gallium nitride-based film that has the necessary crystal phase with a substrate and has high crystallinity and density by controlling the gas composition and energy during sputtering using a sputtering method using a gallium nitride-based target, and a method for producing the film. [Means for solving the problem]

[0008] In view of this background, the inventors conducted extensive research and, as a result, thoroughly investigated the sputtering film formation conditions and discovered conditions under which the crystal orientation in the film can be controlled by controlling the sputtering energy, thereby obtaining a laminated film containing a highly dense substrate and a gallium nitride film with a high coverage, thereby completing the present invention.

[0009] That is, the aspects of the present invention are as follows. (1) A laminated film comprising a substrate and a gallium nitride film, the laminated film being characterized in that the surface roughness (Ra) of the film surface of the gallium nitride film is 100 nm or more and 5000 nm or less, and when the intensity of the (0002) plane and the intensity of the (10-11) plane in X-ray diffraction measurement are I(0002) and I(10-11), respectively, the intensity ratio I(0002) / I(10-11) is 3 or more. (2) The laminated film according to (1), characterized in that the surface roughness (Ra) of the gallium nitride film is 100 nm or more and 5000 nm or less, and the half width at half maximum of the 2θ / ω scan of the (0002) plane is 10° or less. (3) The laminated film according to (1) or (2), characterized in that the coverage of the substrate per unit area is 80% or more. (4) The laminated film according to any one of (1) to (3), wherein the substrate has a surface roughness (Ra) of 100 nm or more. (5) The method for producing a laminated film according to any one of (1) to (4), characterized in that sputtering is performed on a substrate using a sputtering target mainly composed of gallium nitride, with a sputtering gas pressure of less than 0.4 Pa during film formation. (6) A sputtering target mainly composed of gallium nitride was used, and the sputtering power density during film formation was set at 1 W / cm 2 The method for producing a laminated film according to (5), characterized in that sputtering is performed in the above manner.

[0010] The present invention will be described in detail below, but the present invention is not limited to the following embodiments.

[0011] The gallium nitride-based film in the laminated film of the present invention is a thin film whose main component is gallium nitride, and generally refers to a film containing 25 at% or more of gallium as a composition. In the present invention, the gallium nitride-based film may contain indium or aluminum, which are homologous elements, or silicon or the like as a dopant to exhibit electrical conductivity or semiconductor properties.

[0012] It is preferable that the crystal phase of the gallium nitride film has a hexagonal structure, which may enable semiconductor devices to exhibit higher performance than conventional devices.

[0013] In addition, regarding the crystal growth orientation, cubic crystals are expressed as (hkl) and hexagonal crystals as (hklm).

[0014] The surface roughness (Ra) of the gallium nitride film is 100 nm or more and 5000 nm or less, preferably 100 nm or more and 2000 nm or less, and particularly preferably 1000 nm or less. The surface roughness (Ra) here refers to the arithmetic mean roughness obtained when measuring 5 mm with a tactile surface roughness meter.

[0015] In a gallium nitride based film, when the intensity of the (0002) plane and the intensity of the (10-11) plane in an X-ray diffraction measurement are I(0002) and I(10-11), respectively, the intensity ratio I(0002) / I(10-11) is 3 or more, and more preferably 7 or more. This makes it possible to eliminate various problems that occur when fabricating various devices.

[0016] The crystalline phase of the gallium nitride film is hexagonal, and the half-width at half maximum of the ω scan preferably has a peak of 10° or less, more preferably 7° or less, and particularly preferably 5° or less. This results in a film with uniform crystals, improving performance in various applications. The half-width at half maximum of the ω scan to be measured targets at least one of the (0002) plane or the (000-2) plane as the crystal orientation, and both are referred to as (0002) plane. The ω scan measurement method is a method for precisely measuring the orientation of the crystal axis, so it is necessary to use an XRD device with a movable range in the ω direction on the measurement sample side.

[0017] The thickness of the gallium nitride film is preferably 10 nm or more, more preferably 100 nm or more, and even more preferably 300 nm or more, which makes it possible to obtain a thin film with a predetermined crystallinity.

[0018] Examples of the substrate in the laminate film of the present invention include glass substrates including alkali-free glass and quartz, polymeric film substrates made of resin, ceramic or metal substrates, and substrates such as carbon and graphene, with carbon being particularly preferred.

[0019] Furthermore, the laminated film of the present invention preferably has a substrate coverage of 80% or more, more preferably 90% or more, even more preferably 99% or more, and even more preferably 100%.

[0020] The surface roughness (Ra) of the substrate is preferably 100 nm or more, and more preferably 200 nm or more. By making such a material available, it becomes possible to deal with inexpensive substrates.

[0021] The thickness of the substrate is preferably 0.1 mm or more, more preferably 0.5 mm or more, and even more preferably 1 mm or more.

[0022] The laminated film of the present invention may further include a gallium nitride film, an aluminum gallium nitride film, an aluminum nitride film, or the like, in addition to the substrate and the gallium nitride-based film.

[0023] Next, the method for producing the laminated film of the present invention and the film obtained will be described.

[0024] The laminated film of the present invention is formed by sputtering a substrate using a sputtering target containing gallium nitride as a main component at a sputtering gas pressure of less than 0.4 Pa during film formation.

[0025] The sputtering method can be appropriately selected from DC sputtering, RF sputtering, AC sputtering, DC magnetron sputtering, RF magnetron sputtering, ion beam sputtering, etc., and among these, DC magnetron sputtering and RF magnetron sputtering are preferred because they are capable of forming a film uniformly over a large area and at high speed.

[0026] The gas pressure during sputtering is less than 0.4 Pa, preferably 0.3 Pa or less, more preferably 0.1 Pa or less, and even more preferably 0.08 Pa or less. The lower the gas pressure during sputtering, the easier it is for particles emitted from the sputtering target to reach the substrate with high energy and to be epitaxially rearranged. This makes it possible to obtain a hexagonal gallium nitride film. In addition, in order to obtain a high coverage, it is preferable that other crystal phases are not mixed in.

[0027] In order to improve the crystallinity of the entire film, the sputtering target used preferably has an oxygen content of less than 3 at%, more preferably 1 at% or less. High purity is also preferable, and the content of metal impurities is preferably less than 0.1 wt%, more preferably less than 0.01 wt%. The impurities in this case do not include intentionally added indium, aluminum, etc. The area of ​​the sputtering target is 18 cm 2 More preferably, 100 cm 2 That's it. The larger the target area, the more stable the discharge becomes, making it possible to perform sputtering at lower gas pressure and lower power density. Furthermore, the uniformity of the film thickness and quality also improves.

[0028] The degree of vacuum in the deposition equipment before deposition was 3×10 -5 Pa or less, and 1×10 -5 It is more preferable to set the vacuum level at a level lower than 1 Pa. By setting the vacuum level at a lower pressure, residual gas is less likely to be mixed in as an impurity during film formation, improving the crystallinity of the thin film. It is preferable to perform a baking process on the device in order to remove residual gas.

[0029] It is also preferable to pretreat the substrate before film formation. By carrying out the pretreatment, obstacles to adhesion on the substrate surface are removed, enabling epitaxial growth. Examples of pretreatment methods include reverse sputtering, acid treatment, and UV treatment, but reverse sputtering is preferable from the viewpoint of preventing re-adhesion of impurities after treatment. Reverse sputtering is a method of cleaning the surface by colliding plasma atoms with the substrate side, not the sputtering target side. By utilizing this mechanism, the surface of the substrate is cleaned and sent to the film formation chamber without exposure to the outside air, making it possible to form a film while maintaining the cleanliness of the substrate surface. In carrying out reverse sputtering, it is preferable to carry out the treatment separately from the film formation chamber in order to prevent reverse sputtered impurities from adhering to the film formation chamber. Argon, nitrogen, oxygen, etc. can be used as the gas species for the reverse sputtering treatment. The treatment time is preferably 30 seconds or more and 900 seconds or less, more preferably 60 seconds or more and 300 seconds or less. As a result, it is possible to remove impurities on the surface and obtain a preferable surface state.

[0030] It is also preferable to form the film without heating the substrate, since heating the substrate increases the time required for film formation and reduces throughput.

[0031] The gas used is mainly nitrogen. It is preferable to deposit the film with some argon, which is commonly used, added. This will worsen the surface roughness (Ra). The partial pressure ratio of nitrogen / (nitrogen + argon) is preferably 0.7 or more and 0.9 or less.

[0032] The power density during discharge is 1W / cm 2 More than 20W / cm 2 It is preferable that the power consumption is less than 1.5 W / cm 2 More than 10W / cm 2 More preferably, it is 2.5 W / cm or less. 2 More than 5W / cm 2 It is more preferable that the power density is less than 20 W / cm. The power density is calculated by dividing the power applied during discharge by the area of ​​the sputtering target. 2If the power is higher than this, the sputtering target mainly made of gallium nitride generally has a low density, and the power applied to the target causes coarse polycrystalline particles to peel off from the sputtering target, which is not preferable. 2 If the thickness is less than 100 nm, the plasma is not stable, making discharge difficult, and the film formation rate is reduced, lowering the film productivity, which is not preferable. Furthermore, the energy during sputtering is low, and the adhesive strength during film formation is reduced.

[0033] It is also possible to laminate another gallium nitride film on the prepared gallium nitride film by a different method, for example, by depositing a gallium nitride film by MOCVD on a gallium nitride film deposited by sputtering.

[0034] The laminated film of the present invention is preferably used as a semiconductor element composed of a plurality of functional parts. For example, it is used as a light emitting element such as an LED, a laser diode, a power device such as a transistor, etc. Furthermore, the semiconductor element is preferably used in various electronic devices. Effect of the Invention

[0035] The laminated film of the present invention has a high orientation and coverage even when the substrate surface is rough, and is a hexagonal crystal, so that it can be suitably used for light emitting elements such as LEDs and elements for power devices. EXAMPLES

[0036] The present invention will be specifically described using the following examples, but the present invention is not limited to these examples.

[0037] (Methods for confirming crystal planes, measuring half-width at half maximum, and measuring intensity ratio) For normal measurements, a general powder X-ray diffractometer (device name: Ultima III, manufactured by Rigaku Corporation) was used. The conditions for XRD measurement were as follows:

[0038] Radiation source: CuKα radiation (λ=0.15418nm) Measurement mode: 2θ / θ scan Measurement interval: 0.01° Divergence slit: 0.5deg Scattering slit: 0.5deg Receiving slit: 0.3mm Measurement time: 1.0 seconds Measurement range: 2θ=20°~80° XRD analysis software (product name: JADE7, manufactured by MID) was used for the identification analysis of the XRD pattern. The gallium nitride crystal plane was confirmed with reference to JCPDS No. 00-050-0792 for the hexagonal crystal, and JCPDS No. 00-052-0791 for the cubic crystal. When it was difficult to identify the crystal phase from the XRD pattern, a time-of-flight atomic scattering surface analyzer (TOFLAS-3000, manufactured by Pascal) was used to make the judgment. The half-widths of the (0002) plane for the hexagonal crystal and the (111) plane for the cubic crystal were measured, and the intensity ratios of I(0002) and I(10-11) for the hexagonal crystal and I(111) / I(220) for the cubic crystal were calculated using the following formula.

[0039] Intensity ratio = I(0002) / I(10-11) (hexagonal) When no peak corresponding to the denominator was detected, the background peak intensity at 36 to 37° was regarded as the denominator peak and calculations were performed.

[0040] For high-precision measurements, the following configuration was used with an XRD device (Bruker D8 DISCOVER) under conditions of 40 kV, 40 mA, HIGH RESOLUTION mode, a Ge(220) monochromator was used to remove CuKα2, and ω-scan was performed.

[0041] Radiation source: CuKα radiation (λ=0.15418nm) Measurement mode: ω scan Measurement interval: 0.01° Measurement time: 0.5 seconds Measurement range: ω=0°~35° (Measurement of surface roughness (Ra)) The measurements were carried out using a tactile surface roughness tester.

[0042] (Oxygen content measurement in target) The target material was pyrolyzed, and the oxygen content was measured by the thermal conductivity method using an oxygen / nitrogen / hydrogen analyzer (manufactured by Leco).

[0043] (Thin film thickness measurement) The thickness of the formed thin film was measured by measuring the step between the substrate and the film using a laser microscope VK-X250 / 260.

[0044] (Method of measuring coverage) The coverage rate of gallium nitride was measured using SEM-EDS at 100x magnification, with the substrate surface photographed over the entire field of view, and the rate at which the gallium nitride film was present was calculated.

[0045] Coverage rate = area occupied by gallium nitride / field of view However, sunken holes where EDS measurement is difficult are excluded from the field of view.

[0046] Examples 1 to 3 The substrate used was a carbon substrate measuring 10 mm square.

[0047] A sputtering film formation test was carried out under the conditions shown in Table 1 using a gallium nitride sputtering target (purity 99.99 wt%) in a magnetron sputtering device.

[0048] The target-substrate distance during film formation was set to 150 mm, and the ultimate vacuum was increased by baking treatment inside the chamber prior to film formation.

[0049] At the start of sputtering, the shutter on the substrate side was closed and nitrogen gas was used to ignite the plasma, and pre-sputtering was performed for 10 minutes under the same conditions as for film formation, and film formation was performed after stabilizing the discharge. The distance between the shutter and the substrate was 5 mm. The shutter size was 3 inches φ.

[0050] By performing film deposition under the above conditions, we succeeded in producing a dense, highly crystalline hexagonal gallium nitride thin film, as shown in Table 1.

[0051] Comparative Example 1 When a film was formed under the conditions in Table 1, such as increasing the sputtering gas pressure, the coverage rate deteriorated and a film with the desired characteristics could not be obtained.

[0052] [Table 1] [Industrial Applicability]

[0053] The gallium nitride based film of the present invention can be suitably used for the following:

Claims

1. A laminated film comprising a carbon substrate and a gallium nitride film, the laminated film being characterized in that the surface roughness (Ra) of the film surface of the gallium nitride film is 100 nm or more and 5000 nm or less, and when the intensities of the (0002) plane and the (10-11) plane in X-ray diffraction measurement are I(0002) and I(10-11), respectively, the intensity ratio I(0002) / I(10-11) is 3 or more, and the surface roughness (Ra) of the substrate is 100 nm or more.

2. 2. The laminated film according to claim 1, wherein the surface roughness (Ra) of the gallium nitride based film is 100 nm or more and 5000 nm or less, and the half width at half maximum of the 2θ / ω scan of the (0002) plane is 10° or less.

3. 3. The laminated film according to claim 1, wherein the coverage of the substrate per unit area is 80% or more.

4. 4. The laminated film according to claim 1, wherein the gallium nitride film has a thickness of 10 nm or more.

5. A method for manufacturing a laminated film described in any one of claims 1 to 4, characterized in that sputtering is performed on a carbon substrate using a sputtering target mainly composed of gallium nitride, with the sputtering gas pressure during film formation being less than 0.4 Pa.

6. A sputtering target mainly composed of gallium nitride was used, and the sputtering power density during film formation was set to 1 W / cm 2 6. The method for producing a laminated film according to claim 5, wherein sputtering is performed using the above method.

Citation Information

Patent Citations

  • Production of aluminum nitride thin film

    JP1996002999A

  • Nitride semiconductor substrate and method for manufacturing nitride semiconductor substrate

    JP2005112641A

  • Gallium Nitride Light Emitting Device on Diamond

    JP2008528420A

  • Substrate manufacturing method and group-iii nitride semiconductor crystal

    JP2009147271A

  • Gallium nitride sintered body or gallium nitride molded article, and method for producing the same

    JP2014159368A