Negative photosensitive resin composition
A novolac type phenolic resin composition with specific structural units and ethylenically unsaturated polyimide/polybenzoxazole improves alkali solubility and chemical resistance, addressing issues in existing negative photosensitive resins for organic EL displays, ensuring fine pixel division and extended display lifespan.
Patent Information
- Application Number
- JP2023033915
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-05-16
- Filing Date
- 2023-03-06
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2043-03-06
AI Technical Summary
Existing negative photosensitive resin compositions for organic EL displays suffer from issues such as low alkaline solubility, low-temperature curability, residue generation, and poor chemical resistance, which hinder the formation of fine pixel dividing layers and reduce the lifespan of the displays.
A novolac type phenolic resin composition with specific molar ratios of structural units derived from m-cresol, benzaldehyde, and salicylaldehyde, combined with ethylenically unsaturated group-containing polyimide or polybenzoxazole, enhances alkali solubility, allows low-temperature curing, and improves chemical resistance.
The composition achieves high alkali solubility, suppresses film formation defects, and provides a cured film with excellent chemical resistance, enabling fine pixel division layers without residue and extending the lifespan of organic EL displays.
Smart Images

Figure 0007556419000003 
Figure 0007556419000005 
Figure 0007556419000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative photosensitive resin composition, a cured film, and a resist film. [Background technology]
[0002] Organic EL displays have been attracting attention as the next generation of flat panel displays. Organic EL displays are self-luminous display devices that utilize electroluminescence from organic compounds, and are capable of displaying images with a wide viewing angle and high response speed. They can also be made thinner and lighter. In recent years, as organic EL displays have become more highly precise, there has been a demand for further miniaturization of light-emitting elements.
[0003] In an organic EL display, the element emits light using the energy generated by the recombination of electrons injected from the cathode and holes injected from the anode. Therefore, if a substance that forms an energy level that inhibits the recombination of electrons and holes is present, the light-emitting efficiency of the light-emitting element decreases, and the life of the organic EL display decreases. On the other hand, in order to divide the pixels of the light-emitting element, an insulating layer called a pixel division layer is generally formed between the transparent electrode on the light extraction side and the metal electrode on the opposite side. Since this pixel division layer is formed in a position adjacent to the light-emitting element, degassing or outflow of ion components from the pixel division layer can be one of the factors that shorten the life of the organic EL display. For this reason, the pixel division layer is required to be heat-resistant and durable.
[0004] From the viewpoint of high heat resistance, a positive-type photosensitive resin composition using polyimide or polybenzoxazole is used as the material for the pixel division layer (for example, Patent Document 1). However, the pixel division layer using the positive-type photosensitive resin composition contains a naphthoquinone diazide compound as a photosensitizer, and therefore degassing occurs from the pixel division layer, which is one of the factors that shorten the life of the organic EL display. Therefore, a method for forming a pixel division layer using a negative photosensitive resin composition that does not use naphthoquinone diazide has been studied (for example, Patent Document 2). However, the negative resist described in Patent Document 2 does not provide sufficient alkaline developability and low-temperature curing property, and has problems such as generation of residue (scum) after development, sagging of the division layer after heat treatment, and low solvent resistance.
[0005] As described above, with the trend toward higher definition organic EL displays, there is a demand for a photosensitive resin composition that is capable of drawing finer pixel division layers without generating residues and that has low-temperature curing properties and chemical resistance. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] US Patent Application Publication No. 2002 / 162998 [Patent Document 2] International Publication No. 2017 / 159876 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a curable composition which is alkali-soluble, can suppress the occurrence of film formation defects, can be cured at low temperatures, and can give a cured film having excellent chemical resistance. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and have found that a negative-type photosensitive resin composition using a combination of a novolac-type phenolic resin composition having a specific structural unit and at least one of an ethylenically unsaturated group-containing polyimide and an ethylenically unsaturated group-containing polybenzoxazole has high alkaline solubility in unexposed areas, can suppress the occurrence of film formation defects, can be cured at low temperatures after development, and can give a cured film having excellent chemical resistance, thereby completing the present invention.
[0009] That is, the present invention relates to a negative type photosensitive resin composition containing the following components (A) to (D): (A) A novolak-type phenolic resin in which the molar ratio [(a1):(a2):(a3)] of a structural unit (a1) derived from m-cresol, a structural unit (a2) derived from benzaldehyde, and a structural unit (a3) derived from salicylaldehyde is 1.0:0.4-0.8:0.3-0.6. (B) one or more resins selected from the group consisting of ethylenically unsaturated group-containing polyimides, ethylenically unsaturated group-containing polyimide precursors, ethylenically unsaturated group-containing polybenzoxazoles, and ethylenically unsaturated group-containing polybenzoxazole precursors; (C) Photosensitizer (D) Solvent
[0010] The present invention further relates to a cured film obtained from the negative type photosensitive resin composition. The present invention further relates to a resist film obtained from the negative photosensitive resin composition. Effect of the Invention
[0011] According to the present invention, there is provided a curable composition which has alkali solubility, can suppress the occurrence of film formation defects, can be cured at low temperatures, and can give a cured film having excellent chemical resistance. [Brief description of the drawings]
[0012] [Figure 1] 1 is a GPC chart of the novolak phenolic resin obtained in Synthesis Example 1. [Diagram 2] 1 is a GPC chart of the novolak phenolic resin obtained in Synthesis Example 2. [Diagram 3] 1 is a GPC chart of the novolak phenolic resin obtained in Synthesis Example 3. [Figure 4] 1 is a GPC chart of the novolak phenolic resin obtained in Synthesis Example 4. [Diagram 5] 1 is a GPC chart of the novolak-type phenolic resin obtained in Preparation Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes an embodiment of the invention. In this specification, "x to y" represents a numerical range of "not less than x and not more than y." The upper and lower limit values described in relation to the numerical ranges can be combined in any combination. In addition, any combination of two or more of the individual aspects of the present invention described below is also an aspect of the present invention.
[0014] [Negative-type photosensitive resin composition] A negative photosensitive resin composition according to one embodiment of the present invention contains the following components (A) to (D). (A) A novolak-type phenolic resin in which the molar ratio [(a1):(a2):(a3)] of a structural unit (a1) derived from m-cresol, a structural unit (a2) derived from benzaldehyde, and a structural unit (a3) derived from salicylaldehyde is 1.0:0.4-0.8:0.3-0.6. (B) one or more resins selected from the group consisting of ethylenically unsaturated group-containing polyimides, ethylenically unsaturated group-containing polyimide precursors, ethylenically unsaturated group-containing polybenzoxazoles, and ethylenically unsaturated group-containing polybenzoxazole precursors; (C) Photosensitizer (D) Solvent
[0015] In this embodiment, the novolac type phenolic resin (A) and the resin (B) are used in combination to improve the compatibility of the two resins. This makes it possible to suppress the occurrence of film formation defects. In addition, the resin composition has high alkali solubility in the non-exposed areas, can be cured at low temperatures after development, and can provide a cured film with excellent chemical resistance. The components of the negative photosensitive resin composition will be described below.
[0016] Ingredient (A) The novolac phenolic resin which is component (A) has a molar ratio of the structural unit (a1) derived from m-cresol, the structural unit (a2) derived from benzaldehyde, and the structural unit (a3) derived from salicylaldehyde [(a1):(a2):(a3)] of 1.0:0.4-0.8:0.3-0.6.
[0017] The molar ratio of the structural unit (a1) derived from m-cresol, the structural unit (a2) derived from benzaldehyde, and the structural unit (a3) derived from salicylaldehyde contained in component (A) [(a1):(a2):(a3)] is preferably 1.0:0.5-0.7:0.3-0.5, and more preferably 1.0:0.55-0.65:0.35-0.45, from the viewpoint of obtaining a cured film that has high sensitivity and chemical resistance when cured at low temperature.
[0018] Component (A) may contain structural units other than the structural unit (a1) derived from m-cresol, the structural unit (a2) derived from benzaldehyde, and the structural unit (a3) derived from salicylaldehyde. Examples of structural units other than (a1) to (a3) include structural units derived from phenols and aldehydes other than m-cresol, benzaldehyde, and salicylaldehyde.
[0019] Examples of the phenols include phenol, o-cresol, p-cresol, 2,3-xylenol, 2,5-xylenol, 3,4-xylenol, 3,5-xylenol, 2,3,5-trimethylphenol, and 3,4,5-trimethylphenol.
[0020] Examples of the aldehydes include formalin, paraformaldehyde, acetaldehyde, chloroacetaldehyde, 4-hydroxybenzaldehyde, and 3-hydroxybenzaldehyde.
[0021] From the viewpoint of obtaining a cured film that has high sensitivity and chemical resistance when cured at low temperature, the total content of the structural units (a1), (a2) and (a3) in component (A) is preferably 30 mass % or more, more preferably 50 mass % or more, and even more preferably 90 mass % or more. The total content of the structural units (a1), (a2) and (a3) may be substantially 100% by mass, which means that structural units other than the structural units (a1), (a2) and (a3) are inevitably contained.
[0022] The weight average molecular weight of the novolac phenolic resin, which is component (A), is preferably 1000 or more, more preferably 1,500 or more. It is also preferably 7,000 or less, more preferably 6,000 or less, and even more preferably 5,000 or less. A weight average molecular weight of 1000 or more is preferable because of high heat resistance. On the other hand, a weight average molecular weight of 7,000 or less is preferable because of high sensitivity. In this specification, the weight average molecular weight is measured according to the conditions described in the examples.
[0023] The novolak type phenolic resin, which is the component (A), preferably has an area ratio of components having a molecular weight of less than 500 of 3.0 or less as measured by gel permeation chromatography. % By reducing the amount of low-molecular-weight components having a molecular weight of less than 500 in the novolac phenolic resin, the alkali solubility can be further increased. The lower limit of the component having a molecular weight of less than 500 in the novolac phenolic resin is not particularly limited, but is, for example, 0.0 mass % or more, 0.1 mass % or more, or 0.3 mass % or more. The proportion of components having a molecular weight of less than 500 in the novolak phenolic resin is less than 3.0% by mass is confirmed by gel permeation chromatography (GPC) measurement described in the Examples.
[0024] The amount of components having a molecular weight of less than 500 in the novolac phenolic resin can be reduced to less than 3.0% by mass, for example, by further reprecipitating the novolac phenolic resin obtained by the manufacturing method described below. Specifically, the novolac phenolic resin is dissolved in a good solvent (e.g., methyl isobutyl ketone), and then a poor solvent (e.g., heptane) is added to reprecipitate the novolac phenolic resin. By carrying out this operation multiple times, the amount of components having a molecular weight of less than 500 can be reduced to less than 3.0% by mass.
[0025] Component (A) is obtained by polycondensing m-cresol, benzaldehyde, and salicylaldehyde in an organic solvent in a molar ratio (m-cresol:benzaldehyde:salicylaldehyde) range of 1.0:0.4-0.8:0.3-0.6 using an acid catalyst.
[0026] The molar ratio of m-cresol, benzaldehyde, and salicylaldehyde in the organic solvent (m-cresol:benzaldehyde:salicylaldehyde) is preferably in the range of 1.0:0.5-0.7:0.3-0.5, and more preferably 1.0:0.55-0.65:0.35-0.45, from the viewpoint of obtaining a cured film that has high sensitivity and chemical resistance when cured at low temperature.
[0027] The molar ratio of benzaldehyde is preferably smaller than the molar ratio of salicylaldehyde, i.e., it is preferable that the molar ratio satisfies benzaldehyde<salicylaldehyde.
[0028] When m-cresol, benzaldehyde, and salicylaldehyde are polycondensed in an organic solvent to obtain a novolak-type phenolic resin as component (A), as described above, phenols and aldehydes other than m-cresol, benzaldehyde, and salicylaldehyde may be contained in the organic solvent.
[0029] The proportion of the total mass of m-cresol, benzaldehyde, and salicylaldehyde in the organic solvent to the total mass of all starting materials that can become structural units constituting component (A) is preferably 30 mass % or more, more preferably 50 mass % or more, and even more preferably substantially 100 mass %, from the viewpoint of obtaining a cured film that has high sensitivity and chemical resistance when cured at a low temperature.
[0030] Examples of organic solvents used in producing component (A) include methanol, ethanol, 1-propanol, 2-propanol, butanol, hexanol, ethylene glycol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, methyl ethyl ketone, methyl isobutyl ketone, toluene, and the like. Among these, one or more selected from ethanol, 1-propanol, and 2-propanol are preferred, and ethanol is more preferred.
[0031] From the viewpoint of uniformity of the reaction, the amount of the organic solvent used is preferably 20 parts by mass or more, more preferably 50 parts by mass or more, relative to 100 parts by mass of the raw material for deriving the structural unit constituting component (A), and is preferably 500 parts by mass or less, more preferably 300 parts by mass or less.
[0032] Examples of the acid catalyst used in producing component (A) include inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, boric acid, etc., and organic acids such as oxalic acid, acetic acid, paratoluenesulfonic acid, etc. Among these, inorganic acids and paratoluenesulfonic acid are preferred in order to further promote the reaction, and paratoluenesulfonic acid is more preferred. The amount of the acid catalyst to be added is not particularly limited, but is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, relative to 100 parts by mass of the raw material for deriving the structural unit constituting component (A), and is preferably 150 parts by mass or less, more preferably 100 parts by mass or less.
[0033] The reaction temperature during polycondensation of the raw material of component (A) is preferably 30° C. or higher, more preferably 40° C. or higher, in order to promote the reaction and efficiently increase the molecular weight, and is preferably 100° C. or lower, more preferably 80° C. or lower. The reaction time is preferably 4 hours or more, more preferably 12 hours or more, and is preferably 32 hours or less, more preferably 24 hours or less.
[0034] ·Component (B) Component (B) is one or more resins selected from ethylenically unsaturated group-containing polyimide, ethylenically unsaturated group-containing polyimide precursor, ethylenically unsaturated group-containing polybenzoxazole, and ethylenically unsaturated group-containing polybenzoxazole precursor. Component (B) is a polyimide, a polyimide precursor, a polybenzoxazole, or a polybenzoxazole precursor to which an ethylenically unsaturated group has been introduced. Component (B) can be any resin that has been used in conventional photosensitive resin compositions.
[0035] <Polyimide and polyimide precursor> Examples of the polyimide precursor include those obtained by reacting a tetracarboxylic acid, a corresponding tetracarboxylic dianhydride, or a tetracarboxylic diester dichloride, etc., with a diamine, a corresponding diisocyanate compound, or a trimethylsilylated diamine, etc., and have a tetracarboxylic acid and / or a derivative residue thereof and a diamine and / or a derivative residue thereof. Examples of the polyimide precursor include polyamic acid, polyamic acid ester, polyamic acid amide, and polyisoimide.
[0036] Examples of polyimides include those obtained by dehydrating and ring-closing the above-mentioned polyamic acid, polyamic acid ester, polyamic acid amide, or polyisoimide through heating or a reaction using an acid, a base, or the like, and have a residue of a tetracarboxylic acid and / or a derivative thereof, and a residue of a diamine and / or a derivative thereof. The tetracarboxylic dianhydride used in the synthesis of the polyimide is preferably pyromellitic anhydride from the viewpoint of heat resistance.The diamine used in the synthesis of the polyimide is preferably 4,4-diaminodiphenyl ether from the viewpoint of heat resistance.
[0037] The unsaturated group-containing polyimide and the unsaturated group-containing polyimide precursor used in the present invention have the above-mentioned polyimide or polyimide precursor and an ethylenically unsaturated group as a radical polymerizable group. By having an ethylenically unsaturated group, the sensitivity during exposure can be improved. The unsaturated group-containing polyimide and the unsaturated group-containing polyimide precursor are preferably obtained by reacting a part of the phenolic hydroxyl group and / or carboxyl group of the polyimide and the polyimide precursor with a compound having an ethylenically unsaturated group described later. The above reaction makes it possible to introduce an ethylenically unsaturated group into the resin.
[0038] <Polybenzoxazole and polybenzoxazole precursor> The polybenzoxazole precursor may be, for example, a product obtained by reacting a dicarboxylic acid, a corresponding dicarboxylic acid dichloride or a dicarboxylic acid active diester, etc., with a bisaminophenol compound, etc., as a diamine, and has a dicarboxylic acid and / or a derivative residue thereof and a bisaminophenol compound and / or a derivative residue thereof. The polybenzoxazole precursor may be, for example, a polyhydroxyamide.
[0039] Examples of polybenzoxazoles include those obtained by dehydrating and ring-closing a dicarboxylic acid and a bisaminophenol compound as a diamine through a reaction using polyphosphoric acid, and those obtained by dehydrating and ring-closing the above-mentioned polyhydroxyamide through heating or a reaction using phosphoric anhydride, a base, a carbodiimide compound, or the like, and have a dicarboxylic acid and / or a derivative residue thereof and a bisaminophenol compound and / or a derivative residue thereof. The bisaminophenol used in the synthesis of polybenzoxazole is preferably 3,3-hydroxybenzidine from the viewpoint of heat resistance.The dicarboxylic acid used in the synthesis of polybenzoxazole is preferably 4,4-biphenyldicarboxylic acid from the viewpoint of heat resistance.
[0040] The ethylenically unsaturated group-containing polybenzoxazole and ethylenically unsaturated group-containing polybenzoxazole precursor used in the present invention have an ethylenically unsaturated group as a radical polymerizable group. By having an ethylenically unsaturated group, the sensitivity during exposure can be improved. The ethylenically unsaturated group-containing polybenzoxazole and ethylenically unsaturated group-containing polybenzoxazole precursor are preferably obtained by reacting a part of the phenolic hydroxyl group and / or carboxyl group of the polybenzoxazole and polybenzoxazole precursor with a compound having an ethylenically unsaturated group described below. The above reaction makes it possible to introduce an ethylenically unsaturated group into the resin.
[0041] <Compound having an ethylenically unsaturated group> Examples of compounds having an ethylenically unsaturated group include isocyanate compounds, isothiocyanate compounds, epoxy compounds, aldehyde compounds, thioaldehyde compounds, ketone compounds, thioketone compounds, acetate compounds, carboxylic acid chlorides, carboxylic acid anhydrides, carboxylic acid active ester compounds, carboxylic acid compounds, alkyl halide compounds, alkyl azide compounds, alkyl triflate compounds, alkyl mesylate compounds, alkyl tosylate compounds, and alkyl cyanide compounds.
[0042] <Method for synthesizing polyimide, polybenzoxazole, polyimide precursor, or polybenzoxazole precursor> Polyimide, polyimide precursor, polybenzoxazole or polybenzoxazole precursor can be synthesized by a known method. For example, a specific method is to first dissolve diamines or bisaminophenol compounds in a reaction solvent, and gradually add substantially equimolar amounts of carboxylic acid anhydrides to this solution. Using a mechanical stirrer, the mixed solution is stirred at a temperature of preferably 0 to 200°C, more preferably 40 to 150°C, preferably for 0.5 to 50 hours, more preferably 2 to 24 hours. When a terminal blocking agent is used, after adding the carboxylic acid anhydrides, the mixture is stirred at a predetermined temperature for a predetermined time, and then the terminal blocking agent is gradually added and stirred.
[0043] The reaction solvent used in the polymerization reaction may be a polar solvent that can dissolve the diamines or bisaminophenol compounds and carboxylic anhydrides that are raw materials. Examples of the reaction solvent include amides such as N,N-dimethylformamide, N,N-dimethylacetamide, or N-methyl-2-pyrrolidone, cyclic esters such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, or α-methyl-γ-butyrolactone, carbonates such as ethylene carbonate or propylene carbonate, glycols such as triethylene glycol, phenols such as m-cresol or p-cresol, or other solvents such as acetophenone, 1,3-dimethyl-2-imidazolidinone, sulfolane, and dimethyl sulfoxide. The amount of the reaction solvent is preferably from 100 to 1,900 parts by mass, and more preferably from 150 to 950 parts by mass, based on 100 parts by mass of the total of the diamines or bisaminophenol compounds and the carboxylic acid anhydrides.
[0044] It is preferable that one or more selected from polyimide, polybenzoxazole, polyimide precursor, and polybenzoxazole precursor are precipitated in a poor solvent for one or more selected from polyimide, polybenzoxazole, polyimide precursor, and polybenzoxazole precursor, such as methanol or water, after the polymerization reaction is completed, and then washed and dried. By carrying out the reprecipitation treatment, low molecular weight components and the like can be removed, and the mechanical properties of the cured film are significantly improved.
[0045] <Method for synthesizing ethylenically unsaturated group-containing polyimide, ethylenically unsaturated group-containing polyimide precursor, ethylenically unsaturated group-containing polybenzoxazole, or ethylenically unsaturated group-containing polybenzoxazole precursor> The ethylenically unsaturated group-containing polyimide, the ethylenically unsaturated group-containing polyimide precursor, the ethylenically unsaturated group-containing polybenzoxazole, or the ethylenically unsaturated group-containing polybenzoxazole precursor can be synthesized by a known method. As conditions for the reaction of further introducing an ethylenically unsaturated group into polyimide, polybenzoxazole, polyimide precursor, or polybenzoxazole precursor, it is preferable to sufficiently replace the atmosphere in a reaction vessel with nitrogen under air or by bubbling, degassing under reduced pressure, or the like, and then add polyimide, polyimide precursor, polybenzoxazole, or polybenzoxazole precursor and a compound having an ethylenically unsaturated group in a reaction solvent and react for 30 to 500 minutes at 20 to 110° C. Furthermore, a polymerization inhibitor such as a phenol compound, an acid catalyst, or a base catalyst may be used as necessary.
[0046] Regarding component (B), for specific descriptions of polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, ethylenically unsaturated group-containing polyimide, ethylenically unsaturated group-containing polyimide precursor, ethylenically unsaturated group-containing polybenzoxazole, and ethylenically unsaturated group-containing polybenzoxazole precursor, the contents of
[0074] to
[0210] in WO 2017 / 159876 may be referred to as appropriate.
[0047] The weight average molecular weight of component (B) is preferably 5,000 or more, more preferably 10,000 or more. Also, it is preferably 50,000 or less, more preferably 40,000 or less. If the weight average molecular weight is 5,000 or more, it is preferred because it has high heat resistance. On the other hand, if the weight average molecular weight is 50,000 or less, it is preferred from the viewpoint of solvent solubility.
[0048] The amount of component (B) is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, relative to 100 parts by mass of component (A) in order to obtain good sensitivity and a desired pattern, and is preferably 2,000 parts by mass or less, more preferably 1,000 parts by mass or less.
[0049] ·Component (C) Component (C) is a photosensitizer. The negative photosensitive resin composition of the present invention preferably contains, as the photosensitizer, one or more selected from a photoacid generator, a photopolymerization initiator, and a radical polymerizable compound.
[0050] [Photoacid generator] The photoacid generator refers to a compound that generates an acid by bond cleavage upon exposure. By including the photoacid generator, the curing of the exposed portion is promoted, and the sensitivity can be improved. In addition, the photoacid generator that can improve the crosslink density after thermal curing of the negative photosensitive resin composition and improve the chemical resistance of the cured film is not particularly limited, and a known photoacid generator can be used. For example, an organic halogen compound, a sulfonic acid ester, an onium salt, a diazonium salt, and a disulfone compound can be mentioned.
[0051] Specific examples of the photoacid generator include the following. haloalkyl group-containing s-triazine derivatives such as tris(trichloromethyl)-s-triazine, tris(tribromomethyl)-s-triazine, tris(dibromomethyl)-s-triazine, 2,4-bis(tribromomethyl)-6-p-methoxyphenyl-s-triazine, and (2-[2-(5-methylfuran-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine);
[0052] Halogen-substituted paraffinic hydrocarbon compounds such as 1,2,3,4-tetrabromobutane, 1,1,2,2-tetrabromoethane, carbon tetrabromide, and iodoform; halogen-substituted cycloparaffinic hydrocarbon compounds such as hexabromocyclohexane, hexachlorocyclohexane, and hexabromocyclododecane;
[0053] Benzene derivatives containing haloalkyl groups, such as bis(trichloromethyl)benzene and bis(tribromomethyl)benzene; sulfone compounds containing haloalkyl groups, such as tribromomethyl phenyl sulfone and trichloromethyl phenyl sulfone; halogen-containing sulfolane compounds, such as 2,3-dibromosulfolane; isocyanurate compounds containing haloalkyl groups, such as tris(2,3-dibromopropyl)isocyanurate;
[0054] Sulfonium salts such as triphenylsulfonium chloride, diphenyl-4-methylphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium methanesulfonate, triphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium p-toluenesulfonate, triphenylsulfonium tetrafluoroborate, triphenylsulfonium hexafluoroarsenate, and triphenylsulfonium hexafluorophosphonate;
[0055] iodonium salts such as diphenyliodonium trifluoromethanesulfonate, diphenyliodonium p-toluenesulfonate, diphenyliodonium tetrafluoroborate, diphenyliodonium hexafluoroarsenate, and diphenyliodonium hexafluorophosphonate;
[0056] Methyl p-toluenesulfonate, Ethyl p-toluenesulfonate, p-Toluenesulfonate sulfonate compounds such as butyl methanesulfonate, phenyl p-toluenesulfonate, 1,2,3-tris(p-toluenesulfonyloxy)benzene, p-toluenesulfonic acid benzoin ester, methyl methanesulfonate, ethyl methanesulfonate, butyl methanesulfonate, 1,2,3-tris(methanesulfonyloxy)benzene, phenyl methanesulfonate, methanesulfonic acid benzoin ester, methyl trifluoromethanesulfonate, ethyl trifluoromethanesulfonate, butyl trifluoromethanesulfonate, 1,2,3-tris(trifluoromethanesulfonyloxy)benzene, phenyl trifluoromethanesulfonate, and trifluoromethanesulfonic acid benzoin ester; disulfone compounds such as diphenyl disulfone;
[0057] Bis(phenylsulfonyl)diazomethane, bis(2,4-dimethylphenylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, cyclohexylsulfonyl-(2-methoxyphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(3-methoxyphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(4-methoxyphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2-methoxyphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(3-methoxyphenylsulfonyl)diazomethane phenyl)diazomethane, cyclopentylsulfonyl-(4-methoxyphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(2-fluorophenylsulfonyl)diazomethane, cyclohexylsulfonyl-(3-fluorophenylsulfonyl)diazomethane, cyclohexylsulfonyl-(4-fluorophenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2-fluorophenylsulfonyl)diazomethane, cyclopentylsulfonyl-(3-fluorophenylsulfonyl)diazomethane, cyclopentylsulfonyl- (4-Fluorophenylsulfonyl)diazomethane, cyclohexylsulfonyl-(2-chlorophenylsulfonyl)diazomethane, cyclohexylsulfonyl-(3-chlorophenylsulfonyl)diazomethane, cyclohexylsulfonyl-(4-chlorophenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2-chlorophenylsulfonyl)diazomethane, cyclopentylsulfonyl-(3-chlorophenylsulfonyl)diazomethane, cyclopentylsulfonyl-(4-chlorophenylsulfonyl)diazomethane, cyclohexyl cyclohexylsulfonyl-(2-trifluoromethylphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(3-trifluoromethylphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(4-trifluoromethylphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2-trifluoromethylphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(3-trifluoromethylphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(4-trifluoromethylphenylsulfonyl)diazomethane,Cyclohexylsulfonyl-(2-trifluoromethoxyphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(3-trifluoromethoxyphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(4-trifluoromethoxyphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2-trifluoromethoxyphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(3-trifluoromethoxyphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(4-trifluoromethoxyphenylsulfonyl)diazomethane cyclohexylsulfonyl-(2,4,6-trimethylphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(2,3,4-trimethylphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(2,4,6-triethylphenylsulfonyl)diazomethane, cyclohexylsulfonyl-(2,3,4-triethylphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2,4,6-trimethylphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2,3,4- (trimethylphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2,4,6-triethylphenylsulfonyl)diazomethane, cyclopentylsulfonyl-(2,3,4-triethylphenylsulfonyl)diazomethane, phenylsulfonyl-(2-methoxyphenylsulfonyl)diazomethane, phenylsulfonyl-(3-methoxyphenylsulfonyl)diazomethane, phenylsulfonyl-(4-methoxyphenylsulfonyl)diazomethane, bis(2-methoxyphenylsulfonyl)diazomethane, bis(3-methoxyphenylsulfonyl)diazomethane phenylsulfonyl)diazomethane, bis(4-methoxyphenylsulfonyl)diazomethane, phenylsulfonyl-(2,4,6-trimethylphenylsulfonyl)diazomethane, phenylsulfonyl-(2,3,4-trimethylphenylsulfonyl)diazomethane, phenylsulfonyl-(2,4,6-triethylphenylsulfonyl)diazomethane, phenylsulfonyl-(2,3,4-triethylphenylsulfonyl)diazomethane, 2,4-dimethylphenylsulfonyl-(2,4,6-trimethylphenylsulfonyl)diazomethane,Sulfone diazide compounds such as 2,4-dimethylphenylsulfonyl-(2,3,4-trimethylphenylsulfonyl)diazomethane, phenylsulfonyl-(2-fluorophenylsulfonyl)diazomethane, phenylsulfonyl-(3-fluorophenylsulfonyl)diazomethane, and phenylsulfonyl-(4-fluorophenylsulfonyl)diazomethane;
[0058] o-Nitrobenzyl ester compounds such as o-nitrobenzyl-p-toluenesulfonate; Sulfonhydrazide compounds such as N,N'-di(phenylsulfonyl)hydrazide; sulfonium salts which are salts of sulfonium cations such as triarylsulfonium and triaralkylsulfonium with sulfonates such as fluoroalkanesulfonates, arenesulfonates and alkanesulfonates;
[0059] iodonium salts which are salts of iodonium cations such as diaryliodonium and sulfonates such as fluoroalkanesulfonates, arenesulfonates, and alkanesulfonates; bissulfonyldiazomethane compounds such as bis(alkylsulfonyl)diazomethane, bis(cycloalkylsulfonyl)diazomethane, bis(perfluoroalkylsulfonyl)diazomethane, bis(arylsulfonyl)diazomethane, and bis(aralkylsulfonyl)diazomethane;
[0060] N-sulfonyloxyimide compounds comprising a combination of a dicarboxylic acid imide compound and a sulfonate such as a fluoroalkanesulfonate, an arenesulfonate, or an alkane sulfonate; Benzoin sulfonate compounds such as benzoin tosylate, benzoin mesylate, and benzoin butanesulfonate; Polyhydroxyarene sulfonate compounds in which all of the hydroxy groups of a polyhydroxyarene compound have been substituted with sulfonates such as fluoroalkanesulfonates, arenesulfonates, and alkanesulfonates;
[0061] Nitrobenzyl sulfonate compounds such as (poly)nitrobenzyl fluoroalkanesulfonate, (poly)nitrobenzyl arenesulfonate, and (poly)nitrobenzyl alkanesulfonate; Fluoroalkanebenzyl sulfonate compounds such as (poly)fluoroalkanebenzyl fluoroalkanesulfonate, (poly)fluoroalkanebenzyl arenesulfonate, and (poly)fluoroalkanebenzyl alkanesulfonate;
[0062] Bis(arylsulfonyl)alkane compounds; bis-O-(arylsulfonyl)-α-dialkylglyoximes, bis-O-(arylsulfonyl)-α-dicycloalkylglyoximes, bis-O-(arylsulfonyl)-α-diarylglyoximes, bis-O-(alkylsulfonyl)-α-dialkylglyoximes, bis-O-(alkylsulfonyl)-α-dicycloalkylglyoximes, bis-O-(alkylsulfonyl)-α-diarylglyoximes, bis-O-(fluoroalkylsulfonyl)-α-dialkylglyoximes, bis-O-(fluoroalkylsulfonyl)-α-dicycloalkylglyoximes, bis-O-(fluoroalkylsulfonyl)-α-diarylglyoximes, Oxime compounds such as bis-O-(arylsulfonyl)-α-dialkylnioxime, bis-O-(arylsulfonyl)-α-dicycloalkylnioxime, bis-O-(arylsulfonyl)-α-diarylnioxime, bis-O-(alkylsulfonyl)-α-dialkylnioxime, bis-O-(alkylsulfonyl)-α-dicycloalkylnioxime, bis-O-(alkylsulfonyl)-α-diarylnioxime, bis-O-(fluoroalkylsulfonyl)-α-dialkylnioxime, bis-O-(fluoroalkylsulfonyl)-α-dicycloalkylnioxime, and bis-O-(fluoroalkylsulfonyl)-α-diarylnioxime;
[0063] Modified oxime compounds such as arylsulfonyloxyiminoarylacetonitrile, alkylsulfonyloxyiminoarylacetonitrile, fluoroalkylsulfonyloxyiminoarylacetonitrile, ((arylsulfonyl)oxyimino-thiophen-ylidene)arylacetonitrile, ((alkylsulfonyl)oxyimino-thiophen-ylidene)arylacetonitrile, ((fluoroalkylsulfonyl)oxyimino-thiophen-ylidene)arylacetonitrile, bis(arylsulfonyloxyimino)arylenediacetonitrile, bis(alkylsulfonyloxyimino)arylenediacetonitrile, bis(fluoroalkylsulfonyloxyimino)arylenediacetonitrile, arylfluoroalkanone-O-(alkylsulfonyl)oxime, arylfluoroalkanone-O-(arylsulfonyl)oxime, and arylfluoroalkanone-O-(fluoroalkylsulfonyl)oxime.
[0064] The photoacid generator may be used alone or in combination of two or more kinds. The amount of the photoacid generator is preferably 0.1 parts by mass or more, more preferably 5 parts by mass or more, relative to 100 parts by mass of component (A), in order to obtain good sensitivity and a desired pattern, and is preferably 20 parts by mass or less, more preferably 15 parts by mass or less.
[0065] [Photopolymerization initiator] A photopolymerization initiator is a compound that generates radicals by bond cleavage and / or reaction upon exposure to light. By including a photopolymerization initiator, the exposed portion of the film of the negative photosensitive resin composition becomes insoluble in an alkaline developer, thereby forming a negative pattern. In addition, the curing of the exposed portion is promoted, thereby improving the sensitivity.
[0066] The photopolymerization initiator is not particularly limited, and a known photopolymerization initiator can be used. Examples of the photopolymerization initiator include benzyl ketal-based photopolymerization initiators, α-hydroxyketone-based photopolymerization initiators, α-aminoketone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, oxime ester-based photopolymerization initiators, acridine-based photopolymerization initiators, titanocene-based photopolymerization initiators, benzophenone-based photopolymerization initiators, acetophenone-based photopolymerization initiators, aromatic ketoester-based photopolymerization initiators, and benzoic acid ester-based photopolymerization initiators.
[0067] The photopolymerization initiator may be used alone or in combination of two or more kinds. The amount of the photopolymerization initiator is preferably 0.1 parts by mass or more, more preferably 5 parts by mass or more, relative to 100 parts by mass of component (A), in order to obtain good sensitivity and a desired pattern, and is preferably 20 parts by mass or less, more preferably 15 parts by mass or less.
[0068] [Radical polymerizable compounds] The radical polymerizable compound refers to a compound having a plurality of ethylenically unsaturated groups in the molecule. By including the radical polymerizable compound, the curing of the exposed part is promoted, and the sensitivity during exposure can be improved. In addition, the crosslinking density after thermal curing is improved, and the hardness of the cured film can be improved.
[0069] The radical polymerizable compound is not particularly limited, and any known radical polymerizable compound can be used, but a compound having a (meth)acrylic group, which is easily subjected to radical polymerization, is preferred. From the viewpoint of improving the sensitivity during exposure and the hardness of the cured film, a compound having two or more (meth)acrylic groups in the molecule is more preferred.
[0070] Examples of the radical polymerizable compound include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane di(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, ditri ... diolpropane tetra(meth)acrylate, 1,3-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, ethoxylated glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate (Meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol nona(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, pentapentaerythritol undeca(meth)acrylate acrylate, pentaerythritol dodeca(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-(3-(meth)acryloxy-2-hydroxypropoxy)phenyl]propane, 1,3,5-tris((meth)acryloxyethyl)isocyanuric acid, 1,3-bis((meth)acryloxyethyl)isocyanuric acid, 9,9-bis[4-(2-(meth)acryloxyethoxy)phenyl]fluorene, 9,9-bis[4-(3-(meth)acryloxypropoxy)phenyl]fluorene or 9,9-bis(4-(meth)acryloxyphenyl)fluorene or an acid-modified product thereof, an ethylene oxide-modified product thereof, or a propylene oxide-modified product thereof.
[0071] The amount of the radical polymerizable compound is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 5 parts by mass or more, based on 100 parts by mass of component (A). When the content is within the above range, the sensitivity during exposure can be improved. On the other hand, the content of the radical polymerizable compound is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 25 parts by mass or less, and particularly preferably 20 parts by mass or less.
[0072] The photosensitizer, which is the component (C), may be used alone or in combination of two or more. For example, a photopolymerization initiator and a radical polymerizable compound may be blended at the same time.
[0073] ·Component (D) Examples of the solvent that is component (D) include polar aprotic solvents such as N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethylsulfoxide, ethers such as tetrahydrofuran, dioxane, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, ketones such as acetone, methyl ethyl ketone, and diisobutyl ketone, esters such as ethyl acetate, butyl acetate, isobutyl acetate, propyl acetate, propylene glycol monomethyl ether acetate, and 3-methyl-3-methoxybutyl acetate, alcohols such as ethyl lactate, methyl lactate, diacetone alcohol, and 3-methyl-3-methoxybutanol, and aromatic hydrocarbons such as toluene and xylene. These solvents may be used alone or in combination of two or more.
[0074] The amount of component (D) in the negative photosensitive resin composition of the present embodiment is preferably an amount such that the solid content in the composition is 5% by mass or more, since the fluidity of the composition allows a uniform coating to be obtained by a coating method such as spin coating, and is preferably an amount such that the solid content in the composition is 65% by mass or less.
[0075] ·others In one embodiment, the negative photosensitive resin composition may contain various additives in addition to the above-mentioned components (A) to (D) within the range that does not impair the effects of the present invention. Examples of the additives include fillers, pigments, surfactants such as leveling agents, adhesion improvers, and dissolution promoters.
[0076] In one embodiment, an organic base compound may be included to neutralize the acid generated from the photoacid generator (component (C)) upon exposure. When the negative type photosensitive resin composition includes an organic base compound, it is possible to obtain an effect of preventing dimensional fluctuation of the resist pattern caused by migration of the acid generated from the photoacid generator.
[0077] Specific examples of the organic base compound include pyrimidine compounds such as pyrimidine, (poly)aminopyrimidine, (poly)hydroxypyrimidine, (poly)amino(poly)hydroxypyrimidine, (poly)amino(poly)alkylpyrimidine, (poly)amino(poly)alkoxypyrimidine, (poly)hydroxy(poly)alkylpyrimidine, (poly)hydroxy(poly)alkoxypyrimidine; pyridine compounds such as pyridine, (poly)alkylpyridine, dialkylaminopyridine; hydroxyalkyl group-containing amine compounds such as polyalkanolamine, tri(hydroxyalkyl)aminoalkane, bis(hydroxyalkyl)iminotris(hydroxyalkyl)alkane; and aminoaryl compounds such as aminophenol. The organic base compounds may be used alone or in combination of two or more.
[0078] The content of the organic base compound in the negative photosensitive resin composition is preferably 0.1 mol% or more, more preferably 1 mol% or more, and is preferably 100 mol% or less, more preferably 50 mol% or less, based on 1 mol of the photoacid generator.
[0079] The negative type photosensitive resin composition of the present embodiment can be prepared by stirring and mixing the above-mentioned components (A) to (D) and, if necessary, various additives, in a conventional manner to prepare a homogeneous liquid. When solid materials such as fillers and pigments are blended into the composition, they are preferably dispersed and mixed using a dispersing device such as a dissolver, homogenizer, triple roll mill, etc. In addition, the composition can be filtered using a mesh filter, membrane filter, etc. to remove coarse particles and impurities.
[0080] [Hardened film / resist film] A cured film according to one embodiment of the present invention can be obtained by curing the above-mentioned negative type photosensitive resin composition according to the present invention. Specifically, the negative photosensitive resin composition of the present invention is applied onto an object to be subjected to photolithography, and then prebaked to obtain a film of the photosensitive resin composition (photosensitive film) from which the solvent has been removed.
[0081] Examples of the coating method include spin coating, roll coating, flow coating, dip coating, spray coating, doctor blade coating, etc. Pre-baking may be performed, for example, by heating at a temperature of 60° C. to 150° C. for a period of 30 seconds to 600 seconds.
[0082] By exposing the photosensitive film, the solubility of the exposed area in an alkaline developer is significantly reduced. Examples of light sources used for exposure include infrared light, visible light, ultraviolet light, far ultraviolet light, X-rays, and electron beams. Among these light sources, ultraviolet light is preferred, and g-rays (wavelength 436 nm) and i-rays (wavelength 365 nm) from a high-pressure mercury lamp are suitable. After exposure, the film is heated at about 100° C. to promote the crosslinking reaction between components (A), (B) and (C) through the catalytic reaction of the acid generated by the exposure.
[0083] The photosensitive film obtained from the negative photosensitive resin composition of the present invention has high alkali solubility, and therefore the difference in alkali solubility between the exposed area and the photosensitive film is large, which enables patterning with high resolution. Therefore, the photosensitive film can be suitably used as a resist film.
[0084] Examples of alkaline developers used for development after exposure include alkaline aqueous solutions of inorganic alkaline substances such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and aqueous ammonia; primary amines such as ethylamine and n-propylamine; secondary amines such as diethylamine and di-n-butylamine; tertiary amines such as triethylamine and methyldiethylamine; alcohol amines such as dimethylethanolamine and triethanolamine; quaternary ammonium salts such as tetramethylammonium hydroxide and tetraethylammonium hydroxide; and cyclic amines such as pyrrole and pyridine. The alkaline developer may be used by appropriately adding alcohol, a surfactant, etc., if necessary. The alkaline concentration of the alkaline developer is usually preferably in the range of 2 to 5% by mass, and a 2.38% by mass aqueous solution of tetramethylammonium hydroxide is generally used.
[0085] After development with an alkaline developer, a cured film in which the exposed areas are crosslinked can be obtained by heating at a low temperature, for example, from 150° C. to 200° C. The cured film of this embodiment has excellent chemical resistance. The cured film of the present embodiment can be used, for example, as a pixel dividing layer in a display device such as an organic EL display. EXAMPLES
[0086] The present invention will be described in more detail below with reference to specific examples. The weight average molecular weight (Mw) of the synthesized resin was measured under the following GPC measurement conditions. [GPC measurement conditions] Measurement equipment: Tosoh Corporation "HLC-8220 GPC" Column: Showa Denko K.K. "Shodex KF802": 8.0mmΦ×300mm +Showa Denko KF802: 8.0mmΦ×300mm +Showa Denko KF803: 8.0mmΦ×300mm +Showa Denko KF804: 8.0mmΦ×300mm Column temperature: 40℃ Detector: RI (differential refractometer) Data processing: Tosoh Corporation "GPC-8020 Model II Version 4.30" Developing solvent: Tetrahydrofuran Flow rate: 1.0mL / min Sample: 0.5% by mass of tetrahydrofuran solution (resin solid content equivalent) filtered through a microfilter Injection volume: 0.1mL Standard sample: monodisperse polystyrene as follows (Standard sample: monodisperse polystyrene) "A-500" manufactured by Tosoh Corporation "A-2500" manufactured by Tosoh Corporation "A-5000" manufactured by Tosoh Corporation "F-1" manufactured by Tosoh Corporation "F-2" manufactured by Tosoh Corporation "F-4" manufactured by Tosoh Corporation "F-10" manufactured by Tosoh Corporation "F-20" manufactured by Tosoh Corporation
[0087] [Component (A)] Synthesis Example 1 (Synthesis of Novolac-type Phenolic Resin (A-1)) In a 2000mL four-neck flask equipped with a cooling tube, 164g (1.52mol) of m-cresol, 103g (0.97mol) of benzaldehyde, 74g (0.61mol) of salicylaldehyde, and 8g of paratoluenesulfonic acid were charged and dissolved in 300g of ethanol as a reaction solvent. The mixture was then heated to 80°C using a mantle heater and stirred under reflux for 16 hours to react. After the reaction, ethyl acetate and water were added and the mixture was washed five times by separation. The solvent was removed from the remaining resin solution under reduced pressure, and the mixture was dried in vacuum to obtain 281g of a pale red powder of novolac-type phenolic resin (A1). The Mw of the novolak phenolic resin (A-1) was 3100. The GPC chart of the novolak phenolic resin (A-1) is shown in FIG.
[0088] Synthesis Example 2 (Synthesis of Novolac-type Phenolic Resin (A-2)) Except for changing the amounts of the starting materials to 164 g (1.52 mol) of m-cresol, 80 g (0.75 mol) of benzaldehyde, and 92 g (0.75 mol) of salicylaldehyde, the same procedure as in Synthesis Example 1 was repeated to obtain 280 g of powder of novolac type phenolic resin (A-2). The Mw of the novolac type phenolic resin (A-2) was 2,370. The GPC chart of the novolak phenolic resin (A-2) is shown in FIG.
[0089] Synthesis Example 3 (Synthesis of Novolac-type Phenolic Resin (A-3)) Except for changing the amounts of the starting materials to 164 g (1.52 mol) of m-cresol, 117 g (1.10 mol) of benzaldehyde, and 58 g (0.47 mol) of salicylaldehyde, the same procedure as in Synthesis Example 1 was repeated to obtain 279 g of powder of novolac type phenolic resin (A-3). The Mw of the novolac type phenolic resin (A-3) was 2,700. The GPC chart of the novolak phenolic resin (A-3) is shown in FIG.
[0090] Synthesis Example 4 (Synthesis of Novolac-type Phenolic Resin (A-4)) Except for using 250 g of ethanol, 30 g of 1-propanol and 15 g of 2-propanol as the reaction solvent, 282 g of powder of novolak type phenolic resin (A5) was obtained in the same manner as in Synthesis Example 1. The Mw of the novolak type phenolic resin (A-4) was 3,200. The GPC chart of the novolak phenolic resin (A-4) is shown in FIG.
[0091] Comparative Synthesis Example 1 (Synthesis of Novolac-type Phenolic Resin (A-5)) Under a dry nitrogen stream, 70.29g (0.65mol) of m-cresol, 37.85g (0.35mol) of anisole as a reaction promoter, and 0.62g (0.005mol) of oxalic acid dihydrate were charged into a 2000mL three-neck flask equipped with a cooling tube, and dissolved in 198.85g of methyl isobutyl ketone (MIBK), and then 243.49g (3.00mol) of 37% by mass formaldehyde aqueous solution was added, and the mixture was heated to 95°C with a mantle heater, and the reaction liquid was stirred and reacted for 5 hours while refluxing. The temperature was then raised to 180°C, and water and MIBK were distilled out of the system. The temperature was then further raised to 195°C, and unreacted monomers were distilled out under a reduced pressure of 150 torr (2.0 kPa). The obtained resin solid was dissolved again in MIBK, water was added, and separation washing was performed five times. The MIBK was removed under reduced pressure at 60°C using an evaporator, and then vacuum drying was performed to obtain 212 g of a pale red powder of novolac-type phenolic resin (A-5). The Mw of the novolac-type phenolic resin (A-5) was 5,500.
[0092] Comparative Synthesis Example 2 (Synthesis of Novolac-type Phenolic Resin (A-6)) Except for changing the amounts of the starting materials to 164 g (1.52 mol) of m-cresol, 39 g (0.38 mol) of benzaldehyde, and 137 g (1.13 mol) of salicylaldehyde, the same procedure as in Synthesis Example 1 was repeated to obtain 284 g of powder of novolac type phenolic resin (A-6). The Mw of the novolac type phenolic resin (A-6) was 4,700.
[0093] [Component (B)] Synthesis Example 5 (Synthesis of ethylenically unsaturated group-containing polyimide precursor (B-1)) Under a dry nitrogen stream, 125 g (0.023 mol) of pyromellitic anhydride and 115 g (0.023 mol) of 4,4-diaminodiphenyl ether were dissolved in 1602 g of N-methyl-2-pyrrolidone in a 2000 mL four-neck flask equipped with a cooling tube, and the mixture was stirred at 100°C for 4 hours to react. After the reaction was completed, the solution was poured into 2000 g of water, and the precipitate of the polymer solid was collected by filtration. The polymer solid was dried in a vacuum dryer at 80°C for 72 hours to obtain a polymer solid powder. 32.8 g of the obtained solid powder was dissolved in 76.5 g of 3-methoxy-n-butyl acetate. After cooling this mixed solution to 0°C, a solution of 3.2 g of 2-methacryloxyethyl isocyanate dissolved in 3.2 g of 3-methoxy-n-butyl acetate was added dropwise. After the dropwise addition was completed, the mixture was stirred at 80°C for 1 hour to obtain an ethylenically unsaturated group-containing polymer solution. After the reaction was completed, the obtained solution was poured into 1000 g of water, and the precipitate of the ethylenically unsaturated group-containing polymer solid was collected by filtration. The precipitate of the polymer solid was collected by filtration. The ethylenically unsaturated group-containing polymer solid was dried in a vacuum dryer at 80°C for 72 hours to obtain a polymer powder of an ethylenically unsaturated group-containing polyimide precursor (B-1).
[0094] [Negative-type photosensitive resin composition] Example 1 A negative photosensitive resin composition (F-1) was obtained by dissolving 4.2 g of the phenol novolak resin (A-1) powder obtained in Synthesis Example 1 as component (A), 1.8 g of the ethylenically unsaturated group-containing polyimide precursor polymer (B-1) powder obtained in Synthesis Example 5 as component (B), and 4.0 g of a radical polymerizable compound solution (dipentaerythritol hexaacrylate: manufactured by Nippon Kayaku Co., Ltd.) and 0.9 g of a photopolymerization initiator solution (NCI-831: manufactured by ADEKA Corporation) as component (C) in 98 g of γ-butyrolactone as component (D).
[0095] Examples 2 to 4, Comparative Examples 1 to 3 In Examples 2 to 4 and Comparative Examples 1 and 2, negative photosensitive resin compositions (F-2) to (F-6) were obtained in the same manner as in Example 1, except that phenol novolak resin (A-2) to (A-6) powders shown in Table 1 were used as component (A). In Comparative Example 3, a negative photosensitive resin composition (F-7) was obtained in the same manner as in Example 1, except that the phenol novolak resin shown in Table 1 was not included as component (A).
[0096] [evaluation] The negative photosensitive resin compositions prepared in the Examples and Comparative Examples were used to evaluate the alkali solubility before exposure, the chemical resistance of the cured film, and the hardness of the cured film. (1) Evaluation of film-forming properties (resin compatibility) The negative photosensitive resin composition was applied to a silicon wafer having a diameter of 5 inches using a spin coater to a thickness of about 5 μm, and then prebaked at 120° C. for 180 seconds to obtain a wafer with a photosensitive film formed thereon. The photosensitive film formed on the wafer surface was observed using an optical microscope to evaluate repellency and unevenness during film formation. The photosensitive film was evaluated as having good compatibility (◯) when there was no repellency or unevenness, and as having insufficient compatibility (×) when there was repellency or unevenness. The evaluation results are shown in Table 1. (2) Alkaline solubility before exposure The negative photosensitive resin composition was applied to a silicon wafer having a diameter of 5 inches to a thickness of about 5 μm using a spin coater, and then prebaked at 120° C. for 180 seconds to obtain a wafer on which a photosensitive film (resist film) was formed. The wafer was immersed in a vat filled with 250 mL of a developer (2.38 wt % aqueous tetramethylammonium hydroxide solution (TMAH)) for 10 seconds. The wafer removed from the vat was rinsed with pure water for 10 seconds, and the residue of the photosensitive film on the wafer was observed to evaluate the alkali solubility. The absence of any residue was evaluated as extremely good (◎), the absence of almost no residue was evaluated as good (◯), and the presence of residue was evaluated as insufficient (×). The evaluation results are shown in Table 1.
[0097] (3) Chemical resistance of the cured film The negative photosensitive resin composition was applied to a silicon wafer having a diameter of 5 inches using a spin coater to a thickness of about 10 μm, and then prebaked at 120° C. for 180 seconds to obtain a wafer having a photosensitive film formed thereon. Next, the photosensitive film was irradiated with 200 mJ of ghi rays using a Ushio Multilight. After irradiation, the film was heated on a hot plate at 130° C. for 120 seconds, and further heated at 200° C. for 1 hour in a nitrogen atmosphere to obtain a cured film. After the heating was completed, when the temperature inside the heating device became 50° C. or lower, the wafer was taken out and the film thickness was measured. The wafer was then divided into three equal parts, which were then immersed in acetone, N-methylpyrrolidone (NMP), and 2.38 wt% TMAH for 15 minutes, respectively. After removing the wafer from each solvent, the wafer was washed with pure water, and the film thickness was measured again. Chemical resistance was evaluated based on the rate of change in film thickness before and after immersion in a solvent. A rate of change of less than 2% was rated as good (◯), and a rate of change of 2% or more was rated as insufficient (×). The evaluation results are shown in Table 1.
[0098] (4) Hardness of the cured film After obtaining a cured film in the same manner as in (2) above, the wafer was removed when the temperature of the heating device became 50°C or less, and the film thickness was measured. The film hardness was measured by a nanoindentation method (ENT-2100: manufactured by Elionix Co., Ltd.). A film with an indentation modulus of 8 GPa or more was rated as good (◯), and a film with an indentation modulus of less than 8 GPa was rated as insufficient (×). The evaluation results are shown in Table 1.
[0099] [Table 1]
[0100] In Table 1, the molar ratio of the structural units of component (A), "(a1) / (a2) / (a3)," is the molar ratio of the structural unit (a1) derived from m-cresol, the structural unit (a2) derived from benzaldehyde, and the structural unit (a3) derived from salicylaldehyde.
[0101] From the results in Table 1, it can be confirmed that the negative type photosensitive resin composition of the present invention has excellent compatibility without occurrence of film formation defects. It can also be confirmed that the resist film obtained from the negative type photosensitive resin composition of the present invention has alkali solubility. Furthermore, it can be confirmed that the cured film has excellent chemical resistance and high hardness, even though it is cured at a low temperature of 200°C.
[0102] Preparation Example 1 (Preparation of Novolac Phenolic Resin (a-1)) The content of low molecular weight components having a weight average molecular weight of less than 500 in the novolak phenolic resin (A-1) obtained in Synthesis Example 1 was evaluated by GPC. As a result, the GPC area ratio was 3.9. % It was. 200 g of this novolac-type phenolic resin (A-1) was thoroughly dissolved in 300 g of methyl isobutyl ketone in a 2000 ml beaker, and then 300 g of heptane was added to precipitate the resin components. The supernatant was removed to remove the low molecular weight components. This process was repeated three times, and the resin components were again recovered by dissolving the precipitated resin components in 300 g of methyl isobutyl ketone, and the solvent was distilled off under reduced pressure, followed by vacuum drying to obtain 153 g of a pale red powder of low molecular weight component-removed phenolic novolac resin powder (a-1).
[0103] The weight average molecular weight (Mw) of the phenol novolac resin (a-1) was 2,750, and the content of low molecular weight components having a weight average molecular weight of less than 500 was 0.7% in terms of GPC area ratio. The GPC chart of the phenol novolac resin (a-1) is shown in FIG.
[0104] Preparation Example 2 (Preparation of Novolac Phenolic Resin (a-2)) The content of low molecular weight components having a weight average molecular weight of less than 500 in the novolak phenolic resin (A-2) obtained in Synthesis Example 2 was evaluated by GPC. As a result, the GPC area ratio was 3.7. % It was. This novolak type phenolic resin (A-2) was subjected to removal of low molecular weight components in the same manner as in Preparation Example 1, to obtain 156 g of a phenolic novolak resin powder (a-2). The weight average molecular weight (Mw) of the phenol novolak resin (a-2) was 2,840, and the content of low molecular weight components having a weight average molecular weight of less than 500 was 0.6% in terms of GPC area ratio.
[0105] Preparation Example 3 (Preparation of Novolac Phenolic Resin (a-3)) The content of low molecular weight components having a weight average molecular weight of less than 500 in the novolak phenolic resin (A-3) obtained in Synthesis Example 3 was evaluated by GPC. As a result, the GPC area ratio was 3.2 % It was. This novolac type phenolic resin (A-3) was subjected to removal of low molecular weight components in the same manner as in Preparation Example 1, to obtain 151 g of a phenolic novolac resin powder (a-3). The weight average molecular weight (Mw) of the phenol novolak resin (a-3) was 3,130, and the content of low molecular weight components having a weight average molecular weight of less than 500 was 0.7% in terms of GPC area ratio.
[0106] Preparation Example 4 (Preparation of Novolac Phenolic Resin (a-4)) The content of low molecular weight components having a weight average molecular weight of less than 500 in the novolak phenolic resin (A-4) obtained in Synthesis Example 4 was evaluated by GPC. As a result, the GPC area ratio was 4.1 % It was. This novolac type phenolic resin (A-4) was subjected to removal of low molecular weight components in the same manner as in Preparation Example 1, to obtain 152 g of a phenolic novolac resin powder (a-4). The weight average molecular weight (Mw) of the phenol novolak resin (a-4) was 2,780, and the content of low molecular weight components having a weight average molecular weight of less than 500 was 0.8% in terms of GPC area ratio.
[0107] [Negative-type photosensitive resin composition] Example 5 A negative photosensitive resin composition (f-1) was obtained by dissolving 4.2 g of the phenol novolak resin (a-1) powder obtained in Preparation Example 1 as component (A), 1.8 g of the ethylenically unsaturated group-containing polyimide precursor polymer (B-1) powder obtained in Synthesis Example 5 as component (B), and 4.0 g of a radical polymerizable compound solution (dipentaerythritol hexaacrylate: manufactured by Nippon Kayaku Co., Ltd.) and 0.9 g of a photopolymerization initiator solution (NCI-831: manufactured by ADEKA Corporation) as component (C) in 98 g of γ-butyrolactone as component (D).
[0108] Examples 6 to 8, Reference Examples 1 to 2 In Examples 6 to 8 and Reference Examples 1 and 2, negative photosensitive resin compositions (f-2) to (f-6) were obtained in the same manner as in Example 1, except that the phenol novolak resin (a-2) to (a-4), (A-1) and (A-6) powders shown in Table 2 were used as component (A).
[0109] The obtained negative type photosensitive resin composition was evaluated in the same manner as in Examples 1 to 4 and Comparative Examples 1 to 3. The results are shown in Table 2.
[0110] [Table 2]
Claims
1. A negative photosensitive resin composition comprising the following components (A) to (D): (A) A novolak-type phenolic resin in which the molar ratio [(a1):(a2):(a3)] of the structural unit (a1) derived from m-cresol, the structural unit (a2) derived from benzaldehyde, and the structural unit (a3) derived from salicylaldehyde is 1.0:0.55-0.65:0.35-0.
45. (B) one or more resins selected from the group consisting of ethylenically unsaturated group-containing polyimides, ethylenically unsaturated group-containing polyimide precursors, ethylenically unsaturated group-containing polybenzoxazoles, and ethylenically unsaturated group-containing polybenzoxazole precursors; (C) A photopolymerization initiator and a photosensitizer which is a radical polymerizable compound (D) Solvent
2. 2. The negative type photosensitive resin composition according to claim 1, wherein the total content of the structural unit (a1) derived from m-cresol, the structural unit (a2) derived from benzaldehyde, and the structural unit (a3) derived from salicylaldehyde in the component (A) is 30 mass% or more.
3. 3. The negative type photosensitive resin composition according to claim 1, wherein the weight average molecular weight of the component (A) is 1,000 or more and 7,000 or less.
4. 3. The negative type photosensitive resin composition according to claim 1, wherein the component (A) having a molecular weight of less than 500 accounts for less than 3.0% by area as measured by gel permeation chromatography.
5. A cured film obtained from the negative photosensitive resin composition according to claim 1 or 2.
6. A resist film obtained from the negative photosensitive resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Method for producing novolac type phenol resin and novolac type phenol resin for photoresist
JP2005306987A
Novolak type phenolic resin for photoresist and its manufacturing method
JP2008138128A
Method for producing novolak-type phenol resin and photoresist composition
JP2014227464A