Positive electrode additive, its manufacturing method, positive electrode and lithium secondary battery including the same
The use of a positive electrode additive with compounds like Li2Ni1-bO2+c, Ni2-eM1-eP4O12, and Li3PO4 in lithium secondary batteries addresses irreversible capacity loss by stabilizing the negative electrode and maintaining battery performance.
Patent Information
- Application Number
- JP2021523290
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-27
- Filing Date
- 2020-03-03
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-03-03
AI Technical Summary
Lithium secondary batteries experience irreversible capacity loss due to lithium ions not being collected back at the positive electrode during charging and discharging, leading to reduced energy density and battery life.
A positive electrode additive composed of specific compounds like Li2Ni1-bO2+c, Ni2-eM1-eP4O12, and Li3PO4 is used, which offsets the initial irreversible capacity by releasing excess lithium and forming a nickel layer on the negative electrode surface, stabilizing it.
This additive stabilizes the negative electrode surface, suppresses gas generation, and maintains battery performance by effectively offsetting initial irreversible capacities, ensuring stable operation.
Smart Images

Figure 0007556555000007 
Figure 0007556555000003 
Figure 0007556555000005
Abstract
Description
[Technical field]
[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0062076 filed on May 27, 2019, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a positive electrode additive, a method for producing the same, and a positive electrode and a lithium secondary battery containing the same. [Background technology]
[0003] A lithium secondary battery applies an electrode active material capable of reversibly inserting and extracting lithium ions to a negative electrode and a positive electrode, respectively, realizes the movement of lithium ions through an electrolyte, and generates electrical energy through oxidation and reduction reactions at each electrode.
[0004] However, during the initial charge and discharge of a lithium secondary battery (1 ST In the battery, there are inevitably lithium ions that are inserted into the negative electrode (battery charging) and then removed (battery discharging), and lithium ions that are removed from the positive electrode (battery charging) and then not re-recovered (battery discharging). This is related to the irreversible capacity of the two electrodes.
[0005] As the difference in irreversible capacity between the two electrodes increases, the initial efficiency of the positive electrode decreases, which in turn reduces the energy density during battery operation, and may shorten the battery life. Summary of the Invention [Problem to be solved by the invention]
[0006] In one embodiment of the present invention, a substance is provided as a positive electrode additive that can effectively offset the initial irreversible capacity of the positive and negative electrodes in a lithium ion battery without causing a side reaction with the electrolyte and thus contributes to stabilizing the surface of the negative electrode.
[0007] In another embodiment of the present invention, there is provided a method for producing the positive electrode additive of the above embodiment under specific conditions. [Means for solving the problem]
[0008] The advantages and features of the embodiments of the present invention, and the methods for achieving them, will become clear from the detailed examples described below. However, the present invention is not limited to the examples disclosed below, and can be realized in various different forms. The examples are provided merely to complete the disclosure of the present invention, and to fully inform those skilled in the art of the invention of the scope of the invention, and the present invention is defined only by the scope of the claims.
[0009] In the following, unless otherwise defined, technical and scientific terms used in the present invention have the meanings that are commonly understood by those having ordinary knowledge in the technical field to which the invention belongs. In addition, redundant explanations of the same technical configurations and functions as those in the past will be omitted.
[0010] Throughout this specification, when a part is said to be "connected" to another part, this includes not only "directly connected" but also "electrically connected" with another element therebetween.
[0011] Throughout this specification, when an element is said to be "on" another element, this includes not only when the element is in contact with the other element, but also when there is another element between the two elements.
[0012] Throughout this specification, when a part is said to "comprise" a certain element, this means that it can further include other elements, not excluding other elements, unless specifically stated to the contrary.
[0013] As used throughout this specification, the terms "about," "substantially," and the like, when given the manufacturing and material tolerances inherent in the recited meaning, are used in a numerical or approximate sense to that numerical value, and are used to prevent unscrupulous infringers from unfairly taking advantage of disclosures in which precise or absolute numerical values are recited to aid in the understanding of this application.
[0014] As used throughout this specification, the terms "step of" or "step of" do not mean "step for."
[0015] Throughout this specification, the term "combinations thereof" included in a Markush form expression means a mixture or combination of one or more selected from the group of elements set forth in the Markush form expression, and is meant to include one or more selected from the group of elements.
[0016] Throughout this specification, the phrase "A and / or B" means "A or B, or A and B."
[0017] Positive Electrode Additives In one embodiment of the present invention, a compound represented by the following formula 1; a compound represented by the following formula 2; lithium phosphate (Li 3 PO 4 );
[0018] [Chemical formula 1] Li 2+a Ni b M 1-b O 2+c In the formula 1, M is a metal element that forms a divalent cation, and -0.2≦a≦0.2, 0.5≦b≦1.0, and -0.2≦c≦0.2; [Chemical formula 2]Ni 2-e M 1-e P 4 O 12 In Formula 2, 0.5≦e≦1.0, and M is defined as in Formula 1.
[0019] The compound represented by Chemical Formula 1 contains an excess amount of lithium compared to a typical positive electrode active material having a lithium 1 mol level, and therefore can be a positive electrode additive that releases lithium prior to the positive electrode active material during initial charging of a lithium secondary battery, thereby offsetting the irreversible capacity of the positive and negative electrodes and increasing the initial charging capacity.
[0020] The compound represented by Formula 1 can be used as a lithium source material (e.g., Li 2 O) and nickel source material (e.g., (Ni d M 1-d O)) in the stoichiometric molar ratio of Formula 1, followed by heat treatment.
[0021] A large amount of unreacted raw materials may be present on the surface of the compound represented by Formula 1 prepared using only the lithium raw material and the nickel raw material. If the lithium raw material comes into contact with air or moisture, LiOH, Li 2 CO 3 If these lithium by-products come into contact with the electrolyte inside the battery, they can produce HF gas and other substances, which can cause battery deterioration.
[0022] However, the lithium by-products not only cannot participate in electrochemical reactions in the battery, but also generate gas in the battery, thereby reducing the initial capacity and initial charge / discharge efficiency of the battery.
[0023] In this regard, one method is to perform a washing process to remove the unreacted raw materials. However, lithium and the like may be eluted from the compound represented by Chemical Formula 1 during the washing process, and by-products may increase again during the drying process after washing. In addition, there is a limit to how much the lithium by-products can be removed due to re-contamination after washing.
[0024] Therefore, in one embodiment, the unreacted raw material is not washed with water, but is reacted with a phosphorus raw material to obtain the compound represented by Chemical Formula 2; and the lithium phosphate (Li 3 PO 4 ) was converted to
[0025] The compound represented by Chemical Formula 2 is a reaction product of the unreacted nickel source material and the phosphorus source material, and a reaction product of the unreacted lithium source material and the phosphorus source material, all of which may not generate lithium by-products.
[0026] Meanwhile, the compound represented by Formula 2 can be dissolved in an electrolyte in a battery and can be reduced on the surface of the negative electrode during the formation charging process of the battery to form a Ni layer, which does not deteriorate the electrochemical performance of the battery but rather contributes to improving the stability.
[0027] However, the conditions for producing the cathode additive of the one embodiment need to be specifically controlled.
[0028] According to the experimental examples described below, it has been confirmed that the positive electrode additive can be produced only by mixing the lithium raw material, the nickel raw material, and the phosphorus raw material together, and then heat-treating the mixture at a temperature in the range of 600 to 900°C, and supplying an inert gas during this process.
[0029] Here, the raw materials must be mixed together (the number of heat treatments), the heat treatment temperature, whether or not an inert gas is supplied during the heat treatment, and the supply flow rate thereof must all satisfy the conditions set forth above.
[0030] If any one of the factors is not controlled, the compound represented by the formula 2 may not be produced. In other words, if any one of the factors is not controlled, the compound represented by the formula 1; and the lithium phosphate (Li 3 PO 4The compound represented by the formula 1; the compound represented by the formula 2; and lithium phosphate (Li 3 PO 4 ); the positive electrode additive of the embodiment containing all of the above is not produced.
[0031] The manufacturing conditions will be described in detail later, and the configuration of the positive electrode additive according to the embodiment manufactured by controlling the manufacturing conditions will be described in detail below.
[0032] structure The cathode additive of the embodiment may have a structure of a first phase secondary particle and a second phase particle located on the surface of the first phase secondary particle. Here, the "particle" of the second phase particle may be a primary particle or a secondary particle formed by agglomeration of the primary particles.
[0033] Specifically, the compound represented by Chemical Formula 1 may form secondary particles of the first phase, and the lithium phosphate may form particles of the second phase and be attached to the surfaces of the secondary particles.
[0034] The compound represented by Formula 2 may be distributed on the surface of the secondary particles, inside the secondary particles, or on both surfaces.
[0035] Ingredients and content of each ingredient Meanwhile, the positive electrode additive of the embodiment includes a compound represented by the formula 1; a compound represented by the formula 2; and lithium phosphate (Li 3 PO 4 ); as well as Li 2 The form of these may be any form. For example, the NiO particles and Li 2 The NiO particles are attached to the surface of the particles represented by Chemical Formula 1, or the NiO particles and the Li 2 The O particles may be in a mixed form separately from the compound particles represented by Chemical Formula 1.
[0036] These are the compound represented by the formula 2; and the lithium phosphate (Li 3 PO 4 ); may refer to unreacted raw material that has not yet been converted to
[0037] Among them, Li 2 Although O may cause the generation of lithium by-products as described above, it is not necessary to remove O since O can provide extra Li to the positive electrode together with the compound represented by Chemical Formula 1, thereby further increasing the initial charge capacity of the positive electrode.
[0038] The compound represented by the formula 1 is contained in an amount of 80 to 90% by weight of the total amount (100% by weight) of the positive electrode additive, and the Li 3 PO 4 is contained in an amount of 2 to 5% by weight, the NiO is contained in an amount of 5 to 15% by weight, and the Li 2 O and the compound represented by Chemical Formula 2 may correspond to the remainder.
[0039] Specifically, the compound represented by the formula 1 is the lithium phosphate (Li 3 PO 4 ); Li 2 O and the NiO are each crystalline and can be detected by X-ray diffraction analysis (XRD: X-ray diffraction) using CuKα X-rays (X-rα).
[0040] In other words, the core can be qualitatively and quantitatively analyzed using X-ray diffraction (XRD) with CuKα X-ray (X-rα) to determine that the lithium phosphate (Li 3 PO 4 ); Li 2 The presence or absence of each of O and NiO, as well as the amount of each, can be confirmed.
[0041] In the experimental examples described below, the X-ray diffraction analysis results of each of the positive electrode additives were qualitatively analyzed using Bruker's evaluation program to determine Li 2 NiO 2, Li 3 PO 4 , Li 2 The corresponding peaks for O and NiO were identified. For these corresponding peaks, quantitative analysis between the two phases was performed by Rietveld refinement using the TOPAS program (Bruker-AXS, TOPAS4, Karlsruhe, Germany). The Rietveld refinement was carried out by comparing the measured X-ray diffraction patterns with Li 2 NiO 2 , Li 3 PO 4 , Li 2 This is a feedback process in which available variables are iteratively adjusted until the patterns calculated from the O and NiO structural models match best, and in this process, not only the positions of the diffraction peaks but also the peak intensities and intensity ratios are analyzed to quantitatively analyze the content of the two phases (see Rietveld, HML "Line Profiles of Neutron Powder-diffraction Peaks for Structure Refinement" Axta. Cryst., 22, 151-2, 1967, and Bish DL and Howard CJ, "Quantitative phase analysis using the Rietveld method" J. Appl. Cryst., 21, 86-81, 1988).
[0042] Meanwhile, the compound represented by Chemical Formula 2 is also crystalline, but since it is present in a small amount compared to other components, it may be difficult to detect during XRD analysis of the positive electrode additive itself. However, in an experimental example described below, when only nickel raw material and phosphorus raw material are mixed and heat-treated, and then analyzed by XRD, the compound represented by Chemical Formula 2 is detected, and it can be inferred that the positive electrode additive also contains a small amount of the compound represented by Chemical Formula 2.
[0043] Furthermore, since a nickel metal layer was detected on the surface of the negative electrode separated after the formation charging of a lithium secondary battery using the positive electrode active material, it can be inferred that the positive electrode active material contains the compound represented by Chemical Formula 2, and that this material is dissolved in the electrolyte and then reduced to nickel metal on the surface of the negative electrode during the formation charging of the battery.
[0044] Method for producing positive electrode additive In another embodiment of the present invention, there is provided a method for producing a positive electrode additive for a lithium secondary battery, the method including: preparing a raw material mixture containing a lithium raw material, a nickel raw material, and a phosphorus raw material; and heat-treating the raw material mixture at a temperature in the range of 600 to 900° C. in a reactor to which an inert gas is supplied.
[0045] Here, the cathode additive of the embodiment described above can be finally obtained only when the raw materials are mixed together (the number of heat treatments), the heat treatment temperature, the supply of an inert gas during the heat treatment, and the supply flow rate thereof all satisfy the above-mentioned conditions.
[0046] In the case where the raw materials are not mixed at once, a process may be considered in which only the lithium raw material and the nickel raw material are mixed and heat-treated to produce the compound represented by Chemical Formula 1, and then the phosphorus raw material is mixed and heat-treated. However, in the process of performing the heat treatment twice in this manner, the compound represented by Chemical Formula 1 may be decomposed and then resynthesized, so that the compound represented by Chemical Formula 2 may not be produced or may be produced in only a small amount, and the amount of the compound represented by Chemical Formula 1 may also be reduced.
[0047] In addition, when the heat treatment is performed at a temperature exceeding 900° C., when the inert gas is not supplied or when the inert gas is supplied at a flow rate of less than 1.5 L / min, the structurally unstable compound represented by Chemical Formula 1 may be decomposed and then resynthesized, and thus the compound represented by Chemical Formula 2 may not be produced or may be produced only in trace amounts, and the amount of the compound represented by Chemical Formula 1 may also be reduced.
[0048] Hereinafter, the manufacturing method according to the embodiment will be described in detail, omitting the content that overlaps with the above content.
[0049] raw material In the raw material mixture, the phosphorus raw material may be present in an amount of 1 to 10% by weight, specifically 2 to 8% by weight, for example 3 to 7% by weight, based on the total amount (100% by weight) of the raw material mixture. In addition, in the case of the lithium raw material and the nickel raw material, the molar ratio of lithium (Li):nickel (Ni) may be 3:1 to 3:2, and although the molar ratio of Li:Ni in the formula 1 is theoretically 2:1, this is a range that can be adjusted in consideration of the fact that there are many cases in which the raw materials do not react or are lost in the actual manufacturing process. Therefore, the above range is merely an example, and can be appropriately adjusted in consideration of theory and practice.
[0050] The phosphorus source material is diammonium phosphate ((NH 4 ) 2 HPO 4 ), ammonium phosphate dibasic (NH 4 H 2 PO 4 ), or a mixture thereof, wherein the lithium source material comprises Li 2 O, LiOH, or a mixture thereof, and the nickel source material may include a compound represented by the following Formula 3:
[0051] [Chemical formula 3](Ni d M 1-d )O In the above formula 3, M is a metal element that forms a divalent cation, and 0≦d≦0.5.
[0052] Heat Treatment Process In the heat treatment step, the inert gas is nitrogen (N 2 ) gas, which may be fed to the reactor at a flow rate of 1.5 to 2.5 L / min.
[0053] Specifically, the step of heat-treating the raw material mixture at a temperature in the range of 600 to 900° C. in the reactor to which the inert gas is supplied may be carried out as follows.
[0054] a) reacting the lithium source material and the nickel source material to produce a compound represented by the following Chemical Formula 1: b) reacting the nickel source material that has not reacted in step a) and the phosphorus source material to produce a compound represented by the following Chemical Formula 2: c) The lithium source material that did not react in step a) and the phosphorus source material that did not react in step b) react to form lithium phosphate (Li 3 PO 4 ) ) ) ) ); and d) The compound represented by Chemical Formula 1 produced in step a), the compound represented by Chemical Formula 2 produced in step b), and lithium phosphate (Li 3 PO 4 ) to obtain a positive electrode additive comprising: [Chemical formula 1] Li 2+a Ni b M 1-b O 2+c In the formula 1, M is a metal element that forms a divalent cation, and -0.2≦a≦0.2, 0.5≦b≦1.0, and -0.2≦c≦0.2; [Chemical formula 2]Ni 2-e M 1-e P 4 O 12 In Formula 2, 0.5≦e≦1.0, and M is defined as in Formula 1.
[0055] The positive electrode additive obtained in step d) may also contain the lithium source material, the nickel source material, or a mixture thereof that did not react in steps a) to c), as described above.
[0056] Meanwhile, in step b), the compound represented by the formula 2 is produced, and Ni 3 P2 O 8 is also produced, and this may also be included in the positive electrode additive obtained in step d), but the embodiment is not limited thereto.
[0057] At this time, the heat treatment is preferably carried out within the above temperature range for 5 to 11 hours, and more specifically, for 8 to 10 hours.
[0058] If the reaction time is too short, i.e., outside the above range, the reaction may not proceed sufficiently, whereas if the reaction time is too long, the structurally unstable compound represented by Chemical Formula 1 may be decomposed and then resynthesized, and in the process, the compound represented by Chemical Formula 2 may not be produced.
[0059] Positive electrode mixture, positive electrode, and lithium secondary battery In still another embodiment of the present invention, there is provided a positive electrode mixture, a positive electrode, and a lithium secondary battery, each including the above-described positive electrode additive.
[0060] The above-mentioned positive electrode additives can be applied to a common positive electrode mixture in the industry. When a positive electrode made from such a positive electrode mixture is combined with components such as a negative electrode and an electrolyte to implement a lithium secondary battery, the initial irreversible capacity of the positive electrode and negative electrode can be effectively offset, gas generation can be suppressed, and the negative electrode surface can be stabilized by the Ni layer.
[0061] In the experimental examples described below, in order to confirm the effect of forming a Ni layer on the negative electrode surface by the positive electrode additive of the embodiment, a positive electrode mixture containing no positive electrode active material, a positive electrode additive, a conductive agent, and a binder was also produced (Examples 1 to 3).
[0062] When the positive electrode additive of the embodiment is applied to any positive electrode active material and negative electrode active material, the compound represented by Formula 2 can be dissolved in an electrolyte containing a lithium salt and an organic solvent during formation charging of a battery and reduced to Ni metal on the surface of the negative electrode.
[0063] The conditions for forming and charging the lithium secondary battery using the positive electrode additive, and the positive and negative electrode active materials used together with the positive electrode additive are not particularly limited. In the experimental examples described below, no positive electrode active material was used, or if a positive electrode active material was used, a so-called NCM-based positive electrode active material was used, and graphite was used as the negative electrode active material, and the battery was formed and charged up to 4.2 V.
[0064] As a result, it was confirmed that 200 to 4000 ppm of Ni metal was detected on the surface of the separated negative electrode. This is 2 to 2000 times higher than the amount of Ni metal detected under the same conditions, which is less than 100 ppm, when any one of the factors that must be limited in producing the positive electrode additive of the embodiment, i.e., whether or not the raw materials are mixed together (number of times of heat treatment), the heat treatment temperature, whether or not an inert gas is supplied during the heat treatment and the supply flow rate, etc., is not satisfied.
[0065] It was also confirmed in the experimental examples described below that the Ni metal reduced on the surface of the negative electrode in this manner does not reduce the electrochemical performance of the battery, but rather stabilizes the surface of the negative electrode, thereby enabling stable operation of the battery.
[0066] Meanwhile, the positive electrode additive of the embodiment can be prepared as a positive electrode mixture together with a positive electrode active material (Example 4). In this case, the weight ratio of the positive electrode additive of the embodiment and the positive electrode active material can be 1:99 to 35:65, and the content of the Ni layer formed on the negative electrode surface can be reduced in proportion to the mixing ratio.
[0067] Specifically, when the positive electrode mixture does not contain any positive electrode active material, the amount of Ni detected is 3000 to 4000 ppm, but when the positive electrode active material is contained in a weight ratio of positive electrode additive:positive electrode active material = 10:90, Ni at the level of 200 to 3000 ppm can be detected. This is also within the range that can be predicted by the formula (3000 to 4000 ppm) * (positive electrode additive) / (positive electrode additive + positive electrode active material).
[0068] In the lithium secondary battery according to the embodiment, apart from the positive electrode additive and the positive electrode mixture, any material commonly known in the art may be used.
[0069] Hereinafter, matters generally known in the art will be briefly presented, but these are merely examples and are not intended to limit the positive electrode mixture of the embodiment.
[0070] The positive electrode active material is not particularly limited as long as it is a material capable of reversibly inserting and extracting lithium ions, and may, for example, include one or more of composite oxides of metals such as cobalt, manganese, nickel, or a combination thereof; and lithium.
[0071] More specifically, the positive electrode active material may be a compound represented by any one of the following chemical formulas: a A 1-b R b D 2 (wherein 0.90≦a≦1.8 and 0≦b≦0.5); Li a E 1-b R b O 2-c D c (wherein 0.90≦a≦1.8, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b R b O 4-c D c (wherein 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b R c D α (wherein 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b R c O 2-α Z α (wherein 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Cob R c O 2-α Z 2 (wherein 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b R c D α (wherein 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b R c O 2-α Z α (wherein 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b R c O 2-α Z 2 (wherein 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O 2 (wherein 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G e O 2 (wherein 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O 2 (wherein 0.90≦a≦1.8 and 0.001≦b≦0.1); Li a CoG b O 2 (wherein 0.90≦a≦1.8 and 0.001≦b≦0.1); Li a MnG b O 2(wherein 0.90≦a≦1.8 and 0.001≦b≦0.1); Li a Mn 2 G b O 4 (wherein 0.90≦a≦1.8 and 0.001≦b≦0.1);QO 2 ;QS 2 ;LiQS 2 ;V 2 O 5 ;LiV 2 O 5 ;LiTO 2 ;LiNiVO 4 Li (3-f) J 2 (PO 4 ) 3 (0≦f≦2);Li (3-f) Fe 2 (PO 4 ) 3 (0 ≤ f ≤ 2); and LiFePO 4 .
[0072] In the above chemical formula, A is Ni, Co, Mn or a combination thereof; R is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; Z is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; T is Cr, V, Fe, Sc, Y or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.
[0073] Of course, the compound may have a coating layer on its surface, or the compound may be mixed with a compound having a coating layer. The coating layer may include oxides, hydroxides, oxyhydroxides, oxycarbonates, or hydroxycarbonates of coating elements as coating element compounds. The compounds forming the coating layer may be amorphous or crystalline. The coating elements included in the coating layer may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating layer forming process may use any coating method that does not adversely affect the physical properties of the positive electrode active material by using such elements in the compound (e.g., spray coating, immersion method), and the detailed description thereof will be omitted since it is well understood by those skilled in the art.
[0074] The positive electrode mixture of the embodiment may further include a conductive agent, a binder, or a mixture thereof. The conductive agent is used to impart electrical conductivity to the electrode, and any electronically conductive material that does not undergo chemical change in the battery that is constructed may be used. Examples of the conductive agent include natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, metal powders such as copper, nickel, aluminum, and silver, metal fibers, and the like. Also, one or more conductive materials such as polyphenylene derivatives may be used in combination.
[0075] The binder serves to favorably adhere the positive electrode active material particles to each other and to favorably adhere the positive electrode active material to a current collector. Representative examples of the binder include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, and the like.
[0076] The positive electrode can include a positive electrode current collector; and a positive electrode mixture layer located on the positive electrode current collector and including the positive electrode mixture described above.
[0077] Specifically, the positive electrode may be prepared by applying an electrode mixture, which is a mixture of a positive electrode active material, a conductive agent, and / or a binder, onto a positive electrode current collector and then drying the applied mixture. If necessary, a filler may be further added to the mixture.
[0078] The positive electrode current collector can be generally made to a thickness of 3 to 500 μm. Such a positive electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and can be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The current collector can be formed with fine irregularities on its surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0079] The conductive agent is usually added in an amount of 1 to 50% by weight based on the total weight of the mixture including the positive electrode active material. Such a conductive agent is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and examples of such conductive agents include graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and summer black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0080] Meanwhile, the elastic graphite-based material may be used as a conductive agent, or may be used together with the above material.
[0081] The binder is a component that aids in binding the active material and conductive agent and binding to the current collector, and is usually added in an amount of 1 to 50% by weight based on the total weight of the mixture including the positive electrode active material. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers.
[0082] The filler is selectively used as a component that suppresses the expansion of the positive electrode, and is not particularly limited as long as it is a fibrous material that does not induce chemical changes in the battery. For example, fibrous materials such as olefin polymers such as polyethylene and polypropylene; glass fibers, and carbon fibers are used.
[0083] The negative electrode may include a current collector and a negative electrode active material layer formed on the current collector, and the negative electrode active material layer may include a negative electrode active material.
[0084] As the negative electrode active material, a carbon-based negative electrode active material, lithium metal, an alloy of lithium metal, Si, SiO x (0 < x < 2), Si-C composite, Si-Q alloy (wherein Q is an alkali metal, alkaline earth metal, Group 13 to Group 16 element, transition metal, rare earth element or a combination thereof, but not Si), Sn, SnO 2 , Sn-C composite, and at least one negative electrode active material selected from the group consisting of Sn-R (wherein R is an alkali metal, alkaline earth metal, Group 13 to Group 16 element, transition metal, rare earth element or a combination thereof, but not Sn) can be used.
[0085] The negative electrode current collector can generally be made to have a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it has conductivity without inducing a chemical change in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, those surface-treated with carbon, nickel, titanium, silver, etc. on the surface of copper or stainless steel, aluminum-cadmium alloy, etc. can be used. Also, similar to the positive electrode current collector, fine irregularities can be formed on the surface to strengthen the binding force of the negative electrode active material, and it can be used in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric body, etc.
[0086] The lithium secondary battery of the above-described embodiment can be a lithium ion battery, a lithium ion polymer battery, or a lithium polymer battery depending on the type of electrolyte and / or the type of separator.
[0087] When the lithium secondary battery of the embodiment is a lithium ion battery using a liquid electrolyte, the liquid electrolyte can be impregnated into a separator. The separator is an insulating thin film that is interposed between a positive electrode and a negative electrode and has high ion permeability and mechanical strength. The pore diameter of the separator is generally 0.01 to 10 μm, and the thickness is generally 5 to 300 μm. As such a separator, for example, a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, which is chemically resistant and hydrophobic; glass fiber, polyethylene, or the like is used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separator.
[0088] The liquid electrolyte may be a lithium salt-containing nonaqueous electrolyte. The lithium salt-containing nonaqueous electrolyte is composed of a nonaqueous electrolyte and lithium. The nonaqueous electrolyte may be, but is not limited to, a nonaqueous organic solvent, an organic solid electrolyte, an inorganic solid electrolyte, or the like.
[0089] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0090] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymerizing agents containing ionic dissociation groups.
[0091] The inorganic solid electrolyte may be, for example, Li 3 N, LiI, Li 5 NI 2 , Li 3 N-LiI-LiOH, LiSiO 4 , LiSiO 4 -LiI-LiOH, Li 2 SiS 3 , Li 4 SiO 4 , Li 4 SiO 4 -LiI-LiOH, Li 3 PO 4 -Li 2 S-SiS 2 Nitrides, halides, sulfates, etc. of Li such as Li may be used.
[0092] The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, and is, for example, LiCl, LiBr, LiI, LiClO 4 , LiBF 4 , LiB 10 Cl 10 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiAlCl 4 , C.H. 3 SO 3 Li, (CF 3 SO 2 ) 2 NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylborate, imides, etc. can be used.
[0093] In addition, the lithium salt-containing non-aqueous electrolyte may contain, for example, pyridine, triethyl phosphate, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, etc., in order to improve charge / discharge characteristics, flame retardancy, etc. In some cases, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further added to impart flame retardancy, carbon dioxide may be further added to improve high-temperature storage characteristics, or fluoroethylene carbonate (FEC), propene sultone (PRS), etc. may be further added.
[0094] In one specific example, LiPF 6 , LiClO 4 , LiBF 4 , LiN(SO 2 CF 3 ) 2 A lithium salt-containing non-aqueous electrolyte can be produced by adding a lithium salt such as the above to a mixed solvent of a cyclic carbonate of EC or PC, which is a high dielectric solvent, and a linear carbonate of DEC, DMC, or EMC, which is a low viscosity solvent.
[0095] The lithium secondary battery of the embodiment may be embodied as a battery module including the lithium secondary battery as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source.
[0096] In this case, specific examples of the device may be, but are not limited to, an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, or a power storage system. [Brief description of the drawings]
[0097] [Figure 1] 1 shows XRD of Ni2P4O12 separately synthesized in Experimental Example 1. [Figure 2a] 1 is a FE-SEM image of the positive electrode active material of Example 1. [Figure 2b] Figure 2a shows an EDS image of a specific area. [Figure 3a] 1 is a SEM image of a negative electrode separated from the lithium secondary battery of Example 1 after one charge. [Figure 3b] Figure 3a shows an EDS image of a specific area. [Figure 3c] Figure 3a shows an EDS image of a specific area. [Figure 4] 1 shows the results of evaluating the capacity (life) retention rate through charging and discharging of each of the lithium secondary batteries of Examples 1 and 3 and Comparative Examples 1 and 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0098] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these are presented as examples of the present invention and do not limit the scope of the invention in any way.
[0099] Example 1 (1) Manufacturing of positive electrode additives Li 2 O, NiO, and (NH 4 ) 2 HPO 4 were mixed to produce a raw material mixture.
[0100] However, the Li:Ni molar ratio in the raw material mixture is 2:1. 2 O and the NiO were mixed in a molar ratio of 1:1, and the (NH 4 ) 2 HPO 4 was adjusted to 5% by weight based on 100% by weight of the total amount of the raw material mixture.
[0101] The raw material mixture was heat-treated at 680° C. for 10 hours under the condition that nitrogen gas, which is a kind of inert gas, was flowed in at 2 L / min, to obtain the positive electrode additive of Example 1.
[0102] (2) Manufacturing of cathodes and lithium secondary batteries (coin full cells) The positive electrode additive of Example 1, conductive agent (Super-P, Denka Black), and binder (PVdF) were mixed in an organic solvent (NMP) at a weight ratio of 97:2:1 (positive electrode additive:conductive agent:binder) to prepare a positive electrode mixture in a slurry form. The positive electrode mixture was then applied onto an aluminum current collector and dried in a vacuum oven at 120°C for 30 minutes to prepare a positive electrode.
[0103] For the counter electrode, graphite:conductive agent (super P):binder (CMC) were mixed in a weight ratio of 95:1:4, and water was used as a solvent to prepare a negative electrode mixture slurry. The negative electrode mixture slurry was applied onto a copper current collector and dried in a vacuum oven at 50°C for 20 minutes to prepare a negative electrode.
[0104] Using the above components, a 2032 coin full-cell was fabricated by a conventional manufacturing method.
[0105] Example 2 (1) Manufacturing of positive electrode additives The positive electrode additive of Example 2 was obtained using the same method as in Example 1, except that the heat treatment temperature was changed from 680° C. to 730° C.
[0106] (2) Manufacturing of cathodes and lithium secondary batteries (coin full cells) The positive electrode and lithium secondary battery of Example 2 were manufactured in the same manner as in Example 1, except that the positive electrode additive of Example 2 was used instead of the positive electrode additive of Example 1.
[0107] Example 3 (1) Manufacturing of positive electrode additives The positive electrode additive of Example 3 was obtained using the same method as in Example 1, except that the heat treatment temperature was changed from 680° C. to 850° C.
[0108] (2) Manufacturing of cathodes and lithium secondary batteries (coin full cells) The positive electrode and lithium secondary battery of Example 3 were manufactured in the same manner as in Example 1, except that the positive electrode additive of Example 3 was used instead of the positive electrode additive of Example 1.
[0109] Example 4 (1) Manufacturing of positive electrode additives A positive electrode additive was produced in the same manner as in Example 1.
[0110] (2) Manufacturing of cathodes and lithium secondary batteries (coin full cells) Cathode active material (LiNi 0.8 Co 0.1 Mn 0.1 O 2 ), the positive electrode additive, conductive agent (Super-P, Denka Black) and binder (PVdF) were mixed in an organic solvent (NMP) in a weight ratio of 88:9:2:1 (positive electrode active material: positive electrode additive: conductive agent: binder) to prepare a positive electrode mixture in a slurry form, and the positive electrode mixture was then applied onto an aluminum current collector and dried in a vacuum oven at 120° C. for 30 minutes to prepare a positive electrode.
[0111] For the counter electrode, graphite:conductive agent (super P):binder (CMC) were mixed in a weight ratio of 95:1:4 and water was used as a solvent to prepare a negative electrode mixture slurry. The negative electrode mixture slurry was applied onto a copper current collector and dried in a vacuum oven at 50°C for 20 minutes to prepare a negative electrode.
[0112] Comparative Example 1 (1) Manufacturing of positive electrode additives N 2 A positive electrode additive of Comparative Example 1 was obtained using the same method as in Example 1, except that the flow rate was changed from 2 L / min to 0.5 L / min.
[0113] (2) Manufacturing of cathodes and lithium secondary batteries (coin full cells) The positive electrode and lithium secondary battery of Comparative Example 1 were manufactured in the same manner as in Example 1, except that the positive electrode additive of Comparative Example 1 was used instead of the positive electrode additive of Example 1.
[0114] Comparative Example 2 (1) Manufacturing of positive electrode additives A positive electrode additive of Comparative Example 2 was obtained using the same method as in Example 1, except that the heat treatment temperature was changed from 680°C to 920°C.
[0115] (2) Manufacturing of cathodes and lithium secondary batteries (coin full cells) A positive electrode and a lithium secondary battery of Comparative Example 2 were manufactured in the same manner as in Example 1, except that the positive electrode additive of Comparative Example 2 was used instead of the positive electrode additive of Example 1.
[0116] Comparative Example 3 (1) Manufacturing of positive electrode additives Li 2 O and NiO were mixed in a molar ratio of 1:1, and then heat-treated at 680° C. for 10 hours under the condition that nitrogen gas, which is a type of inert gas, was flowed in at 2 L / min, as in Example 1, to obtain lithium nickel oxide.
[0117] After the lithium nickel oxide is recovered, NH 4 H 2 PO 4 In this case, the lithium nickel oxide and NH 4 H 2 PO 4 Of the total mixture of 100% by weight, NH 4 H 2 PO 4 The amount of Li was 5% by weight. 2 The same as that used when mixing O and NiO.
[0118] The lithium nickel oxide and NH 4 H 2 PO 4The mixture was heat-treated at 730° C. for 10 hours under the condition that an inert gas, nitrogen gas, was flowed in at 2 L / min, and as a result, a positive electrode additive of Comparative Example 3 was obtained.
[0119] (2) Manufacturing of cathodes and lithium secondary batteries (coin full cells) A positive electrode and a lithium secondary battery of Comparative Example 3 were manufactured in the same manner as in Example 1, except that the positive electrode additive of Comparative Example 3 was used instead of the positive electrode additive of Example 1.
[0120] Experimental example 1: Qualitative and quantitative analysis of positive electrode additives using X-ray diffraction (XRD) analysis XRD analysis of each of the positive electrode additives of Examples 1 to 3 and Comparative Examples 1 to 3 was carried out using an X-ray diffraction analyzer (Bruker AXS D4-Endeavor XRD) using CuKα X-rays (X-rα).
[0121] The X-ray diffraction analysis results of each of the positive electrode additives were qualitatively analyzed using Bruker's evaluation program to determine the Li 2 NiO 2 , Li 3 PO 4 , Li 2 The corresponding peaks for O and NiO were identified. For these corresponding peaks, quantitative analysis between the two phases was performed by Rietveld refinement using the TOPAS program (Bruker-AXS, TOPAS4, Karlsruhe, Germany). The Rietveld refinement was carried out by comparing the measured X-ray diffraction patterns with Li 2 NiO 2 , Li 3 PO 4 , Li 2This is a feedback process in which available variables are iteratively adjusted until the patterns calculated from the O and NiO structural models match best, and in this process, not only the positions of the diffraction peaks but also the peak intensities and intensity ratios are analyzed to quantitatively analyze the content of the two phases (see Rietveld, HML "Line Profiles of Neutron Powder-diffraction Peaks for Structure Refinement" Axta. Cryst., 22, 151-2, 1967, and Bish DL and Howard CJ, "Quantitative phase analysis using the Rietveld method" J. Appl. Cryst., 21, 86-81, 1988).
[0122] The results of such XRD analysis are shown in Table 1 below. As a result, in Examples 1 to 3 and Comparative Examples 1 to 3, Li 2 NiO 2 , Li 3 PO 4 , Li 2 It was found to contain O and NiO.
[0123] However, referring to Table 1 below, it can be seen that the mixing ratio of each component is affected by whether or not the raw materials are mixed together (number of heat treatments), the heat treatment temperature, whether or not an inert gas is supplied during the heat treatment, and the supply flow rate thereof.
[0124] [Table 1]
[0125] According to Table 1, when the flow rate of the nitrogen gas supplied in the heat treatment process was less than 1.5 L / min (Comparative Example 1), Li 2 No O was detected.
[0126] In addition, when the heat treatment temperature exceeded 900° C. (Comparative Example 2), Li 2 A mixture of O and NiO was heat treated to form Li2 NiO 2 After producing (NH 4 ) 2 HPO 4 When mixed separately and heat treated (Comparative Example 3), Li 2 NiO 2 The amount of detection was significantly reduced compared to the examples.
[0127] In this way, when the heat treatment temperature exceeds 900°C or the heat treatment is carried out twice, Li 2 NiO 2 can be decomposed and then resynthesized, and Li 2 The rate of return to O can be increased.
[0128] On the other hand, the Ni synthesized in Examples 1 to 3 2 P 4 O 12 Since the amount is very small, it is recommended to measure NiO and (NH 4 ) 2 HPO 4 By mixing only Ni and P in a molar ratio of 1:2 and heat treating the mixture, 2 P 4 O 12 It was decided to confirm that the above was synthesized.
[0129] The resulting material was subjected to XRD analysis in the same manner as above, and the results are shown in FIG.
[0130] According to Figure 1, Ni 2 P 4 O 12 At the same positions as those of the NiO and (NH 4 ) 2 HPO 4 The XRD peaks of the material produced from the raw material are observed. 2 O, NiO, and (NH 4 ) 2 HPO 4 The process of heat treating the raw material mixture containing Li 2 NiO 2The NiO that does not participate in the generation of (NH 4 ) 2 HPO 4 can react with Ni 2 P 4 O 12 can be generated.
[0131] Also, Ni 2 P 4 O 12 Since is a highly reactive compound due to its unstable structure, it was predicted that the entire amount would be dissolved in the electrolyte and reduced to Ni on the surface of the negative electrode.
[0132] Experimental Example 2: Scanning Electron Microscope (SEM) and Energy Dispersive X-ray Spectroscopy (EDS) to Determine Li in the Positive Electrode Additive 3 PO 4 Confirmation of the form of existence The surface of the positive electrode additive of Example 1 was photographed using a scanning electron microscope (FE-SEM) (JSM-7610F Schottky Field Emission Scanning Election Microscope), and the photographed image is shown in FIG. 2a.
[0133] In Figure 2a, secondary particles of the first phase and particles of the second phase (indicated by a circle in Figure 2a) attached to their surfaces can be observed.
[0134] The most abundant component of the positive electrode additive analyzed in Table 1 was Li. 2 NiO 2 Therefore, the secondary particles of the first phase are Li 2 NiO 2 It is judged that:
[0135] In order to identify the particle composition of the second phase, energy spectroscopy (EDS) (JSM-7610F Schottky Field Emission Scanning Election Microscope) was performed, and the element P was recognized at a position corresponding to the part shown in Figure 2a. Therefore, it was found that the coating layer contains P.
[0136] The P-containing compounds among the components of the positive electrode additive analyzed in Table 1 were Li 3 PO 4 Since there is only one, the second phase particles are Li 3 PO 4 It can be seen that.
[0137] Of course, in the embodiment, Ni 2 P 4 O 12 is also synthesized, but this is in very small quantities, so Ni 2 P 4 O 12 I believe so.
[0138] Experimental Example 3: Evaluation of negative electrode surface characteristics after charging and discharging of lithium secondary batteries The lithium secondary battery of Example 1 was charged once at 25° C. under the following conditions, and then the negative electrode was separated and the surface of the negative electrode was analyzed by a scanning electron microscope (SEM) and an energy dispersive X-ray spectroscopy (EDS).
[0139] Charge: 0.2C, CC / CV, 4.2V, 0.05C cut-off According to the SEM image of FIG. 3a, a film is observed on the surface of the negative electrode separated from the lithium secondary battery of Example 1 after one charge. The EDS analysis of the film confirmed that the main component of the film was Ni (FIG. 3c). This is due to the Ni contained in the positive electrode additive of Example 1. 2 P 4 O 12It is presumed that this is the result of being dissolved in the electrolyte and then reduced on the surface of the negative electrode to form a Ni metal layer.
[0140] Moreover, an inductively coupled plasma (ICP) analysis was carried out on Examples 1 to 4 and Comparative Examples 1 to 3, and the results are shown in Table 2 below.
[0141] [Table 2]
[0142] It can be seen from Table 2 above that the amount of Ni reduced in Examples 1 to 3 is significantly excessive compared to Comparative Examples 1 to 3.
[0143] In the cases of Examples 1 to 3, Li 2 NiO 2 NiO that does not participate in the production reaction (unreacted) is 4 ) 2 HPO 4 can react with Ni 2 P 4 O 12 It is inferred that Ni can be generated. 2 P 4 O 12 Since is a highly reactive compound due to its unstable structure, it is hypothesized that the entire amount of it may be dissolved in the electrolyte and reduced to Ni on the surface of the negative electrode.
[0144] On the other hand, the reaction temperature in Comparative Example 1 itself is within the range of Examples 1 to 3, but by lowering the supply flow rate of the inert gas to less than 1.5 L / min, Ni 2 P 4 O 12 Thus, Ni 2 P 4 O 12 The additive without the Ni would not have been able to form a Ni metal layer on the negative electrode surface.
[0145] In addition, when the heat treatment temperature exceeded 900° C. (Comparative Example 2), Li 2A mixture of O and NiO was heat treated to form Li 2 NiO 2 After producing (NH 4 ) 2 HPO 4 When the materials are mixed separately and heat treated (Comparative Example 3), the structurally unstable Li 2 NiO 2 was decomposed under these heat treatment conditions and then resynthesized, and Ni 2 P 4 O 12 would not have been generated.
[0146] However, it is presumed that the Ni detected in Comparative Examples 1 to 3 was the result of a trace amount of NiO being eluted from the positive electrode additive.
[0147] Experimental Example 4: Capacity retention evaluation by charging and discharging a lithium secondary battery At 25° C., 50 cycles of charge and discharge were carried out for each of the lithium secondary batteries of Examples 1 and 3 and Comparative Examples 1 and 3 under the following conditions. st The discharge capacity after the 50th cycle was evaluated against the discharge capacity after the 50th cycle, and the results are shown in FIG.
[0148] Charge: 0.2C, CC / CV, 4.25V, 0.05C cut-off Discharge: 0.2C, CC, 2.5V, cut-off
[0149] From FIG. 4, it can be seen that the Ni metal layer formed on the surface of the negative electrode in Examples 1 and 3 does not impair the electrochemical properties of the battery, and allows the capacity to be maintained at the same level as in Comparative Examples 1 and 3 at the same cycle. [Industrial Applicability]
[0150] In the lithium ion battery using the positive electrode additive according to the embodiment, the initial irreversible capacity of the positive electrode and the negative electrode is effectively offset, while gas generation is suppressed, and stable operation can be achieved.
Claims
1. A compound represented by the following chemical formula 1: A compound represented by the following chemical formula 2: Lithium phosphate (Li 3 P.O. 4 ); Positive electrode additives for lithium secondary batteries: [Chemical formula 1] Li 2+a Ni b M 1-b O 2+c In the formula 1, M is a metal element that forms a divalent cation, and −0.2≦a≦0.2, 0.5≦b≦1.0, and −0.2≦c≦0.2; [Chemical formula 2] Yes 2-e M 1-e P 4 Oh 12 In Formula 2, 0.5≦e≦1.0, and M is defined as in Formula 1.
2. The compound represented by the formula 2 is Dissolved in an electrolyte solution comprising a lithium salt and an organic solvent; The positive electrode additive for a lithium secondary battery according to claim 1 .
3. In the positive electrode additive, The compound represented by Chemical Formula 1 forms secondary particles, The lithium phosphate particles are attached to the surfaces of the secondary particles. The positive electrode additive for a lithium secondary battery according to claim 1 or 2.
4. The positive electrode additive is Li 2 Further comprising O and NiO; The positive electrode additive for a lithium secondary battery according to any one of claims 1 to 3.
5. providing a source mixture including a lithium source material, a nickel source material, and a phosphorus source material; and heat-treating the raw material mixture at a temperature in the range of 600 to 900° C. in a reactor to which an inert gas is supplied at a flow rate of 1.5 to 2.5 L / min; The method for producing the positive electrode additive for lithium secondary batteries according to any one of claims 1 to 4.
6. The inert gas is nitrogen (N 2 ) gas, The method for producing the positive electrode additive for lithium secondary batteries according to claim 5.
7. In the raw material mixture, the molar ratio of lithium (Li):nickel (Ni) based on the lithium raw material and the nickel raw material is 3:1 to 3:2; The method for producing the positive electrode additive for lithium secondary batteries according to claim 5 or 6.
8. The phosphorus raw material is contained in an amount of 1 to 10% by weight in the total amount (100% by weight) of the raw material mixture. A method for producing the positive electrode additive for a lithium secondary battery according to any one of claims 5 to 7.
9. The phosphorus source material is Ammonium phosphate dibasic (NH 4 ) 2 H.P.O. 4 ), ammonium phosphate monobasic (NH 4 H 2 P.O. 4 ), or mixtures thereof, A method for producing the positive electrode additive for a lithium secondary battery according to any one of claims 5 to 8.
10. heat-treating the raw material mixture at a temperature in the range of 600 to 900° C. in the reactor to which the inert gas is supplied; a) reacting the lithium source material and the nickel source material to produce a compound represented by the following Formula 1: b) reacting the nickel source material and the phosphorus source material that did not react in step a) to produce a compound represented by the following Formula 2: c) The lithium source material that did not react in step a) and the phosphorus source material that did not react in step b) react to form lithium phosphate (Li 3 P.O. 4 ) ) ) ) ); and d) The compound represented by Formula 1 produced in step a), the compound represented by Formula 2 produced in step b), and lithium phosphate (Li 3 P.O. 4 obtaining a positive electrode additive comprising: A method for producing the positive electrode additive for a lithium secondary battery according to any one of claims 5 to 9: [Chemical formula 1] Li 2+a Ni b M 1-b O 2+c In the formula 1, M is a metal element that forms a divalent cation, and −0.2≦a≦0.2, 0.5≦b≦1.0, and −0.2≦c≦0.2; [Chemical formula 2] Yes 2-e M 1-e P 4 Oh 12 In Formula 2, 0.5≦e≦1.0, and M is defined as in Formula 1.
11. The positive electrode additive obtained in step d) includes Also included are lithium source materials, nickel source materials, or mixtures thereof that have not reacted in steps a) to c). The method for producing the positive electrode additive for a lithium secondary battery according to claim 10.
12. A positive electrode comprising the positive electrode additive according to any one of claims 1 to 4; an electrolyte solution comprising a lithium salt and an organic solvent; and a negative electrode; Lithium secondary battery.
13. During formation charging of the lithium secondary battery, The compound represented by Chemical Formula 2 is dissolved from the positive electrode additive and dissolved in the electrolyte, and then reduced to Ni metal on the surface of the negative electrode. The lithium secondary battery according to claim 12.
14. After the lithium secondary battery is charged to 4.2 V, 200 to 4000 ppm of Ni metal is detected on the surface of the separated negative electrode.
14. The lithium secondary battery according to claim 12 or 13.
Citation Information
Patent Citations
Cathode additives for lithium secondary battery with high capacity
CN104781961A
Lithium titanate composite negative electrode material, preparation method thereof and lithium-ion battery
CN110416537A
Lithium nickel multiple oxide, its production and it use
JP1997241026A
Electrode materials for lithium interlayer electrochemical cells
JP2000502831A
Method for adjusting end voltage of positive electrode during overdischarge and positive electrode active material for lithium secondary battery
JP2006514776A