Coating laminate and method for forming same

The film laminate with controlled extender pigment and transparent coating layers addresses the issue of scratch resistance without compromising the aesthetic finish of interior materials, offering a low gloss and calm appearance.

JP7556805B2Active Publication Date: 2024-09-26BEKKU KK
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021030818
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-26
Publication Date
2024-09-26
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Existing interior materials for building surfaces, when covered with a transparent film for scratch resistance, risk impairing their unique finish and aesthetic appeal.

Method used

A film laminate comprising an interior material layer with specific ratios of extender pigment and aggregate, and a transparent coating material layer, applied in controlled amounts to maintain a low gloss and calm finish while providing scratch resistance.

Benefits of technology

The laminate achieves a low gloss, calm finish with enhanced scratch resistance, preserving the aesthetic qualities of the interior material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a coating that offers a low-gloss and unobtrusive finish feeling and also has scratch resistance or the like.SOLUTION: A coating laminate has an interior material layer and a transparent coating material layer. The interior material layer contains an extender pigment 200-2000 pts.wt. relative to 100 pts.wt. of the resin component. The transparent coating material layer has its coating amount of 0.1-30 g / m2 in terms of solid content.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating laminate that can be applied to the decorative surfaces of building interiors. [Background technology]

[0002] Conventionally, interior walls of buildings have been painted with interior materials to impart beauty to them. One example of such an interior material is one that contains powder as a main component. Such an interior material can provide a low gloss and a calm finish.

[0003] Patent Document 1 describes a coating material containing granular aggregate, powdered filler, fibrous substance, water-soluble adhesive, synthetic resin binder, etc., as an interior material for renovating interior wallpaper. Although such an interior material can provide a finish such as a Juraku style, the coating surface may be easily scratched.

[0004] Patent Document 2 describes the formation of a transparent coating on interior materials using a clear paint. By providing such a transparent coating, it is expected that the scratch resistance of the interior materials will be improved. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-141090 [Patent Document 2] Japanese Patent Application Publication No. 8-89887 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when the interior material is covered with a transparent film as in Patent Document 2, there is a risk that the inherent finish feel of the interior material may be impaired.

[0007] The present invention has been made in consideration of such problems, and has an object to form a coating that can present a low gloss and calm finish and also has scratch resistance and the like. [Means for solving the problem]

[0008] As a result of extensive research aimed at solving the above problems, the present inventors came up with the idea of ​​a coating laminate having a specific interior material layer and a transparent coating material layer, and completed the present invention.

[0009] That is, the present invention has the following features. 1. A coating laminate having an interior material layer and a transparent coating material layer, The interior material layer is made of 100 parts by weight of a resin component and 200 to 2000 parts by weight of a body pigment. , 20~2000 parts by weight of aggregate and The average particle size of the extender pigment is less than 50 μm, and the average particle size of the aggregate is 0.05 to 3 mm. The transparent coating layer has a coating amount of 0.1 to 30 g / m2 in terms of solid content. 2 A coating laminate comprising: 2. A method for forming a coating laminate having an interior material layer and a transparent coating material layer, comprising the steps of: The interior material layer is made of 100 parts by weight of a resin component and 200 to 2000 parts by weight of a body pigment. , 20~2000 parts by weight of aggregate and The average particle size of the extender pigment is less than 50 μm, and the average particle size of the aggregate is 0.05 to 3 mm. A transparent coating material is applied to the interior material layer in an amount of 0.1 to 30 g / m2 in terms of solid content. 2 A transparent coating layer is formed by applying the A method for forming a coating laminate comprising the steps of: 3. The coating amount of the interior material layer is 80 to 3,000 g / m2 in terms of solid content. 2 1. The coating laminate according to claim 1, 4. The interior material layer is formed by an interior material, and the coating amount of the interior material (converted into solid content) is 80 to 3000 g / m 2 2. The method for forming a coating laminate according to 2., Effect of the Invention

[0010] According to the present invention, a coating film can be obtained that has a low gloss and a calm finish and also has scratch resistance and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail.

[0012] The present invention relates to a coating laminate having an interior material layer and a transparent coating material layer, which is obtained by laminating a coating formed by an interior material and a coating formed by a transparent coating material. The coating laminate of the present invention is applicable to the surface decoration of the interior of a building (such as an inner wall surface).

[0013] [Interior material layer] The interior material layer in the present invention contains 200 to 2000 parts by weight of a body pigment per 100 parts by weight of a resin component. Such an interior material layer can present a low gloss and calm finish, and can be formed by applying (painting) an interior material containing the resin component and the body pigment. In the present invention, "α to β" is synonymous with "α or more and β or less."

[0014] The resin component in the interior material is a component that plays a role in fixing powder particles such as extender pigments. Examples of the resin component include cellulose, polyvinyl alcohol, ethylene resin, vinyl acetate resin, polyester resin, alkyd resin, vinyl chloride resin, epoxy resin, acrylic resin, urethane resin, acrylic silicone resin, fluororesin, and the like, or composites thereof. These can be used alone or in combination of two or more. Examples of the form of the resin component include water-soluble resin, water-dispersible resin (resin emulsion), solvent-soluble resin, solventless resin, non-water-dispersible resin, powdered resin, and the like. Among these, water-soluble resin and / or water-dispersible resin are preferred, and particularly, an embodiment containing water-dispersible resin is preferred. By using water-soluble resin and / or water-dispersible resin, a water-based interior material can be obtained. In addition, these resin components may be either those having crosslinking reactivity or those not having crosslinking reactivity.

[0015] The extender pigment in the interior material is a component that contributes to lowering the gloss, and furthermore, contributes to imparting a natural texture and improving the ease of painting. Examples of the extender pigment include heavy calcium carbonate, light calcium carbonate, kaolin, clay, china clay, diatomaceous earth, hydrous fine powder of silicic acid, talc, baryte powder, barium sulfate, precipitated barium sulfate, barium carbonate, magnesium carbonate, silica powder, resin powder, resin beads, and aluminum hydroxide, and one or more of these can be used. The average particle size of the extender pigment is preferably less than 50 μm, more preferably 0.5 to 45 μm, and even more preferably 1 to 40 μm. The average particle size of the extender pigment is a value measured by a laser diffraction type particle size distribution measuring device.

[0016] The constituent ratio of the extender pigment is 200 to 2000 parts by weight, preferably 300 to 1800 parts by weight, more preferably 400 to 1600 parts by weight, and further preferably 500 to 1500 parts by weight, per 100 parts by weight of the solid content of the resin component. The constituent ratio of the extender pigment is equal to or more than the lower limit, which is suitable for reducing gloss, imparting a natural texture, improving coating workability, etc., and is also advantageous in forming a relatively thin and flat coating. The constituent ratio of the extender pigment is equal to or less than the upper limit, which is suitable for preventing coating cracking, etc.

[0017] In addition to the above components, the interior material may further contain aggregate. Aggregate is a component that contributes to imparting a natural texture and improving paint workability. Examples of aggregate include crushed materials such as marble, granite, serpentine, granite, fluorite, kansui stone, feldspar, silica stone, and silica sand, crushed ceramics, crushed ceramics, crushed glass, glass beads, crushed resin, resin beads, metal particles, and the like, or materials having a colored coating on the surface thereof. These materials may be used alone or in combination of two or more.

[0018] In the present invention, the aggregate may contain colored aggregate. As the colored aggregate, aggregate that has a visible color may be used. The color of the colored aggregate may be, for example, naturally occurring or artificially applied. By using the colored aggregate, the coloring property of the interior material layer can be enhanced, and it becomes possible to impart a desired color.

[0019] The aggregate has a larger average particle size than the extender pigment described above and the color pigment described below, and the average particle size is preferably 0.05 to 3 mm, more preferably 0.06 to 1 mm, even more preferably 0.07 to 0.5 mm, and particularly preferably 0.075 to 0.2 mm. When the aggregate has such an average particle size, an interior material layer with high aesthetic appearance can be formed with a relatively small amount of application, and it is also advantageous in terms of thinning and weight reduction of the interior material layer. The average particle size of the aggregate is a value obtained by sieving using a metal mesh sieve specified in JIS Z8801-1:2000 and calculating the average weight distribution.

[0020] The composition ratio of the aggregate is preferably 20 to 2000 parts by weight, more preferably 50 to 1600 parts by weight, further preferably 100 to 1400 parts by weight, and particularly preferably 200 to 1200 parts by weight, relative to 100 parts by weight of the solid content of the resin component. When the composition ratio of the aggregate is equal to or more than the above lower limit, it is preferable in terms of imparting a natural texture and improving the ease of painting. When the composition ratio of the aggregate is equal to or less than the above upper limit, it is preferable in terms of suppressing film cracking, and is also advantageous in forming a relatively thin and flat film. From this viewpoint, the weight ratio of the body pigment to the aggregate (body pigment:aggregate) is preferably 95:5 to 20:80, more preferably 90:10 to 40:60, and further preferably 85:15 to 50:50.

[0021] In addition to the above components, the interior material may further contain a coloring pigment. The coloring pigment is a component that contributes to the coloring property, hiding property, etc. of the interior material layer. By using the coloring pigment, it is possible to impart a desired color to the interior material layer.

[0022] Examples of color pigments include titanium oxide, zinc oxide, carbon black, graphite, black iron oxide, iron-manganese composite oxide, iron-copper-manganese composite oxide, iron-chromium composite oxide, iron-chromium-cobalt composite oxide, copper-chromium composite oxide, copper-manganese-chromium composite oxide, copper-magnesium composite oxide, bismuth-manganese composite oxide, red iron oxide, molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, chrome green, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, aluminum pigments, and pearl pigments. These can be used alone or in combination of two or more. The average particle size of the color pigment is preferably 2 μm or less, more preferably 0.01 to 1 μm. The average particle size of the color pigment is a value measured by a laser diffraction particle size distribution measuring device.

[0023] The composition ratio of the color pigment is preferably 1 to 200 parts by weight, more preferably 5 to 180 parts by weight, further preferably 10 to 160 parts by weight, and particularly preferably 20 to 150 parts by weight, relative to 100 parts by weight of the solid content of the resin component. When the composition ratio of the color pigment is equal to or more than the above lower limit, it is preferable in terms of color development, hiding power, etc. When the composition ratio of the color pigment is equal to or less than the above upper limit, it is preferable in terms of suppressing film cracking, imparting a natural texture, etc. When the color pigment and the color aggregate are used in combination, it is possible to develop a composite color of these, and it is also possible to improve the texture, naturalness, fineness, etc.

[0024] The interior material may contain other components than those described above, so long as they do not significantly impair the effects of the present invention. Examples of such components include thickeners, film-forming assistants, leveling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, defoamers, adsorbents, fibers, water repellents, hydrophilizing agents, crosslinking agents, coupling agents, UV absorbers, light stabilizers, antioxidants, catalysts, solvents, water, etc. The interior material can be produced by uniformly mixing the above-mentioned resin components, extender pigments, and, if necessary, each of the above-mentioned components, etc., by a conventional method.

[0025] The interior material layer in the present invention can be formed by applying and drying the above-mentioned interior material to a surface to be coated, such as the inner wall surface of a building. The interior material layer can be formed as a new coating by painting at the same time as the transparent coating material. The interior material layer may also be one that already exists as an old coating film before the transparent coating material is painted.

[0026] Examples of the substrate that constitutes the surface to be coated include concrete, mortar, porcelain tile, fiber-mixed cement board, cement calcium silicate board, slag cement perlite board, cement board, ALC board, siding board, gypsum board, plywood, extrusion molding board, steel board, plastic board, etc. The surface of these substrates may be subjected to some surface treatment (for example, treatment with putty, sealer, surfacer, filler, etc.), may already have a coating film formed thereon, or may have wallpaper, etc. attached thereto. When using an undercoat material such as a sealer, surfacer, or filler, the color tone of the undercoat material may be set to an approximate color (common color) of the interior material.

[0027] In painting the interior material, for example, tools such as a spray, roller, brush, trowel, spatula, etc. can be used. Specifically, when applying the interior material to the surface to be coated, for example, tools such as a spray, roller, trowel, spatula, etc. can be used. The shape and amount of the interior material applied to the surface to be coated can be appropriately set according to the desired finish state, aesthetics, etc. Next, when spreading the applied interior material, for example, tools such as a trowel, spatula, roller, etc. can be used. Among these, when a trowel, spatula, etc. is used when spreading the interior material, a flat interior material layer is easily obtained by leveling the coating surface. In the present invention, it is preferable to use a trowel at least when spreading the interior material, and it is more preferable to use a trowel when applying the interior material to the surface to be coated and when spreading the interior material. When spreading the interior material, the coating surface can be leveled while supplying water or solvent to the coating surface with a sprayer, etc.

[0028] The coating amount of the interior material (solid content equivalent) is preferably 80 to 3000 g / m 2 , more preferably 150 to 1000 g / m 2 , and more preferably 200 to 750 g / m 2 , particularly preferably 300 to 700 g / m 2 In the present invention, a highly aesthetic interior material layer can be formed with a relatively small amount of coating, and the coating can be made thinner and lighter.

[0029] Drying after painting the interior material may be carried out at room temperature (preferably 0 to 50° C., more preferably 5 to 45° C.), and can also be heated if necessary.

[0030] The interior material layer formed by such an interior material can present a low gloss and a calm finish. The specular gloss of the interior material layer (measurement angle 60 degrees) is preferably 40 or less, more preferably 20 or less, and even more preferably 10 or less.

[0031] The interior material layer can be formed using one type or two or more types of interior materials. When two or more types of interior materials of different colors are used, a colorful interior material layer with a mixture of multiple colors can be formed.

[0032] In the present invention, after the interior material is painted, the surface of the interior material layer can be subjected to a polishing treatment. The polishing treatment can be performed, for example, for the purpose of improving the smoothness of the coating. The polishing treatment can be performed by a known method using an abrasive cloth or the like. The grain size of the abrasive cloth or the like can be appropriately selected according to the desired degree of smoothness. The treatment can also be performed using two or more types of abrasive cloth or the like. In the polishing treatment, the coating surface can be wetted with water or the like as necessary while polishing. Powder generated by polishing can be removed by air blowing or with a rag or the like.

[0033] [Transparent coating layer] In the present invention, a transparent coating material layer is laminated on the surface of the interior material layer. The coating amount of the transparent coating material layer is 0.1 to 30 g / m2 in terms of solid content. 2 In the present invention, by laminating such an interior material layer and a transparent covering material layer, it is possible to obtain a coating film that has a low gloss and a calm finish and also has scratch resistance.

[0034] The transparent coating layer can be obtained by applying (painting) a transparent coating material containing a resin component. Examples of the resin component in the transparent coating material include cellulose, polyvinyl alcohol, ethylene resin, vinyl acetate resin, polyester resin, alkyd resin, vinyl chloride resin, epoxy resin, acrylic resin, urethane resin, acrylic silicone resin, fluororesin, and the like, or composites thereof. These can be used alone or in combination of two or more. Examples of the form of the resin component include water-soluble resin, water-dispersible resin (resin emulsion), solvent-soluble resin, solventless resin, non-water-dispersible resin, powdered resin, and the like, among which water-soluble resin and / or water-dispersible resin are preferred, and particularly preferred are embodiments containing water-dispersible resin. By using water-soluble resin and / or water-dispersible resin, an aqueous transparent coating material can be obtained. In addition, these resin components may be either those having crosslinking reactivity or those not having crosslinking reactivity.

[0035] The glass transition temperature of the resin component in the transparent coating material is preferably 20° C. or higher, more preferably 25 to 80° C., and even more preferably 30 to 60° C. When the transparent coating material contains such a resin component, it is possible to further improve scratch resistance, etc. This glass transition temperature can be calculated by the Fox formula.

[0036] As the resin component in the transparent coating material, an acrylic resin emulsion is suitable. The acrylic resin emulsion is an aqueous dispersion of polymer particles mainly composed of (meth)acrylic acid alkyl ester. Such an acrylic resin emulsion can be obtained, for example, by emulsion polymerization of a monomer group including (meth)acrylic acid alkyl ester and other monomers as required, by a known method.

[0037] Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate. These can be used alone or in combination. The composition ratio of such (meth)acrylic acid alkyl esters is preferably 30% by weight or more, more preferably 40 to 99.9% by weight, and even more preferably 50 to 99.5% by weight, based on the total monomers constituting the acrylic resin emulsion. In the present invention, alkyl acrylates and alkyl methacrylates are collectively referred to as alkyl (meth)acrylates.

[0038] Examples of the other monomers include carboxyl group-containing monomers, amino group-containing monomers, pyridine-based monomers, hydroxyl group-containing monomers, nitrile group-containing monomers, amide group-containing monomers, epoxy group-containing monomers, carbonyl group-containing monomers, alkoxysilyl group-containing monomers, aromatic monomers, sulfonic acid group-containing monomers, fluorine-containing monomers, polyoxyalkylene chain-containing monomers, divinyl-based monomers, trivinyl-based monomers, ultraviolet absorbing group-containing monomers, and light stable group-containing monomers. These can be used alone or in combination of two or more. The composition ratio of these other monomers is preferably 0.1 to 60% by weight, more preferably 0.5 to 50% by weight, based on the total monomers constituting the acrylic resin emulsion.

[0039] The acrylic resin emulsion may be one that satisfies the above conditions, and may be, for example, an acrylic-styrene resin emulsion, an epoxy-modified acrylic resin emulsion, a urethane-modified acrylic resin emulsion, a silicon-modified acrylic resin emulsion, a fluorine-modified acrylic resin emulsion, etc. The form of the acrylic resin emulsion may be, for example, a multilayer structure type emulsion (core-shell type emulsion) obtained by multistage polymerization, or a crosslinking reaction type emulsion that generates a crosslinking reaction.

[0040] The average particle size of the acrylic resin emulsion is preferably 30 to 200 nm, more preferably 50 to 160 nm. This average particle size is a value measured by dynamic light scattering (measurement temperature: 25° C.).

[0041] The ratio of the resin component (solid content) in the transparent coating material is preferably 1 to 50% by weight, more preferably 2 to 30% by weight, and further preferably 3 to 15% by weight.

[0042] The transparent coating material may contain other components than those described above, so long as they do not significantly impair the effects of the present invention. Examples of such components include color pigments, extender pigments, matting agents, thickeners, film-forming assistants, leveling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, defoamers, adsorbents, fibers, water repellents, hydrophilizing agents, crosslinking agents, coupling agents, ultraviolet absorbers, light stabilizers, antioxidants, catalysts, solvents, water, etc. The transparent coating material can be produced by uniformly mixing the above-mentioned resin components and, if necessary, each of the above-mentioned components, etc., by a conventional method.

[0043] The heating residue of the transparent coating material is preferably 1 to 50% by weight, more preferably 2 to 30% by weight, and even more preferably 3 to 15% by weight. This makes it possible to sufficiently suppress unevenness caused by the coating of the transparent coating material, and makes it easier to obtain a uniform transparent coating material layer. The heating residue referred to here is the heating residue of the transparent coating material at the time of coating, and in the case of diluting the transparent coating material and coating it, the heating residue refers to the transparent coating material after dilution. The heating residue is a value measured according to the method of JIS K5601-1-2 "heating residue" under conditions of a heating temperature of 135°C and a heating time of 60 minutes.

[0044] In applying the transparent coating material, for example, tools such as a spray, roller, brush, etc. After application of the transparent coating material, drying may be performed at room temperature (preferably 0 to 50°C, more preferably 5 to 45°C), and can also be performed with heating if necessary.

[0045] The amount of transparent coating material applied is 0.1 to 30 g / m2 in solid content. 2 and preferably 0.5 to 20 g / m 2 , more preferably 1 to 10 g / m 2This provides a low gloss and a calm finish and improves scratch resistance. For interior material layers that have been polished, whitening due to polishing can be suppressed. Furthermore, scratches caused by polishing can be repaired. If the amount of transparent coating material applied is below the lower limit, it is difficult to obtain sufficient scratch resistance. If the amount of transparent coating material applied is above the upper limit, it is difficult to obtain a low gloss and a calm finish. EXAMPLES

[0046] The following examples will be given to clarify the features of the present invention, but the present invention is not limited to these examples.

[0047] The following raw materials were used to manufacture the interior materials and transparent coating materials. Resin A: Acrylic resin emulsion (solid content 50% by weight, glass transition temperature 30°C, average particle size 120 nm) Resin B: Acrylic resin emulsion (solid content 50% by weight, glass transition temperature 40°C, average particle size 110 nm) · Extender pigment A: Heavy calcium carbonate (average particle size 15 μm) · Extender pigment B: Resin beads (average particle size 8 μm) Aggregate A: White silica sand (average particle size 150 μm) Color pigment A: Black pigment dispersion (20% by weight dispersion of carbon black (average particle size 0.05 μm)) Color pigment B: Yellow pigment dispersion (50% by weight dispersion of yellow iron oxide (average particle size 0.5 μm)) Color pigment C: Red pigment dispersion (50% by weight dispersion of red iron oxide (average particle size 0.2 μm)) Color pigment D: White pigment dispersion (60% by weight dispersion of titanium oxide (average particle size 0.3 μm)) Fiber: Inorganic fiber (average fiber length 0.1 mm) Dispersant: Polycarboxylic acid dispersant Coalescence agent: Ether-based coalescence agent Thickener: Hydroxyethylcellulose 3% by weight aqueous solution · Defoamer: Silicone-based defoamer

[0048] · Manufacturing of interior materials 1 Interior material 1 (light gray) was produced by mixing and stirring 200 parts by weight of resin A (100 parts by weight converted to solids) in a conventional manner with 830 parts by weight of extender pigment A, 670 parts by weight of aggregate, 0.2 parts by weight of coloring pigment A, 0.2 parts by weight of coloring pigment B, 0.05 parts by weight of coloring pigment C, 65 parts by weight of coloring pigment D, 15 parts by weight of fiber, 5 parts by weight of dispersant, 12 parts by weight of film-forming aid, 160 parts by weight of thickener, 60 parts by weight of water, and 5 parts by weight of defoamer.

[0049] · Manufacturing of interior materials 2 Interior material 2 (dark gray) was produced by mixing and stirring 200 parts by weight of resin A (100 parts by weight converted to solids) in a conventional manner with 980 parts by weight of extender pigment A, 520 parts by weight of aggregate, 18 parts by weight of coloring pigment A, 18 parts by weight of coloring pigment B, 6 parts by weight of coloring pigment C, 35 parts by weight of coloring pigment D, 15 parts by weight of fiber, 5 parts by weight of dispersant, 12 parts by weight of film-forming aid, 160 parts by weight of thickener, 60 parts by weight of water, and 5 parts by weight of defoamer.

[0050] -Manufacture of transparent coating material 1 200 parts by weight of resin B (100 parts by weight in terms of solid content) was mixed with 18 parts by weight of film-forming agent and 2 parts by weight of antifoaming agent, and water was added to this to produce transparent coating material 1 with a heating residue of 5% by weight.

[0051] · Transparent coating material 2 production 200 parts by weight of resin B (100 parts by weight in terms of solid content) was mixed with 20 parts by weight of extender pigment B, 18 parts by weight of film-forming aid, and 2 parts by weight of defoamer, and water was added to this to produce transparent coating material 2 with a heating residue of 5% by weight.

[0052] Example 1 A slate board with a grey sealer coating was prepared as the coating surface. Interior material 1 was applied to this coating surface with a trowel, and then immediately spread and smoothed with the trowel to form a coating surface. The coating amount of interior material 1 (calculated as solid content) was 450 g / m 2 After drying for 24 hours, the right half of the interior material coating was coated with transparent coating material 1 at a coating amount (solid content equivalent) of 6 g / m 2After applying the paint by roller at 100°C, the paint was dried and cured for 7 days. When the appearance of the coating obtained by the above method was checked, the right half (with the transparent coating layer) had the same low gloss as the left half (without the transparent coating layer), and was a light gray coating with a flat and calm finish. When the coating surface on the right half was rubbed with a cloth, no particular abnormalities were found, and the scratch resistance was good.

[0053] Example 2 The interior material 1 was applied with a trowel to the same surface as in Example 1, and then immediately spread and smoothed with the trowel to form a coated surface. The amount of the interior material 1 applied (in terms of solid content) was 450 g / m 2 After drying for 24 hours, the surface of the interior material coating was lightly polished with an abrasive cloth. Next, transparent coating material 1 was applied to the right half of the interior material coating in an amount of 3 g / m (solid content equivalent). 2 After roller painting with a temperature of 100° C., the coating was dried and cured for 7 days. When the appearance of the coating obtained by the above method was checked, the right half (with a transparent coating layer) had a low gloss similar to that of the left half (without a transparent coating layer), and was a light gray coating with a flat and calm finish. In addition, the left half had become slightly white due to polishing, but the whitening had disappeared on the right half. When the scratch resistance of the coating surface on the right half was checked by the same method as in Example 1, no particular abnormalities were found and it was good.

[0054] Example 3 On the same substrate as in Example 1, interior material 1 and interior material 2 were applied with a trowel so that they were adjacent to each other and partially overlapping, and then immediately spread and smoothed with the trowel to form a coated surface. The amount of interior material 1 applied (in terms of solids) was 250 g / m 2 The coating amount of interior material 2 (solid content equivalent) is 200 g / m 2 After drying for 24 hours, the surface of the interior material coating was lightly polished with an abrasive cloth. Next, transparent coating material 1 was applied to the right half of the interior material coating in an amount of 2 g / m (solid content equivalent). 2After roller painting, the coating was dried and cured for 7 days. When the appearance of the coating obtained by the above method was confirmed, the right half (with a transparent coating layer) had a low gloss similar to that of the left half (without a transparent coating layer), and the coating had a flat and calm finish. The obtained coating had a mortar-like aesthetic appearance in which light gray and dark gray areas were mixed and further the shade changes due to the intermediate color tones were visible. In addition, the left half was slightly whitened by polishing, but the whitening was eliminated on the right half. When the scratch resistance of the coating surface on the right half was confirmed by the same method as in Example 1, no particular abnormalities were observed and it was good.

[0055] Example 4 The interior material 1 was applied with a trowel to the same surface as in Example 1, and then immediately spread and smoothed with the trowel to form a coated surface. The amount of the interior material 1 applied (in terms of solid content) was 450 g / m 2 After drying for 24 hours, the surface of the interior material coating was lightly polished with an abrasive cloth. Next, the transparent coating material 2 was applied to the right half of the interior material coating in an amount of 3 g / m (solid content equivalent). 2 After roller painting with a temperature of 100° C., the coating was dried and cured for 7 days. When the appearance of the coating obtained by the above method was checked, the right half (with a transparent coating layer) had a low gloss similar to that of the left half (without a transparent coating layer), and was a light gray coating with a flat and calm finish. In addition, the left half had become slightly white due to polishing, but the whitening had disappeared on the right half. When the scratch resistance of the coating surface on the right half was checked by the same method as in Example 1, no particular abnormalities were found and it was good.

[0056] Comparative Example 1 The interior material 1 was applied with a trowel to the same surface as in Example 1, and then immediately spread and smoothed with the trowel to form a coated surface. The amount of the interior material 1 applied (in terms of solid content) was 450 g / m 2 After drying for 24 hours, the right half of the interior material coating was coated with transparent coating material 1 at a coating amount (solid content equivalent) of 0.05 g / m 2After roller painting with a paint, the coating was dried and cured for 7 days. When the appearance of the coating obtained by the above method was checked, the right half (with a transparent coating layer) had a low gloss similar to that of the left half (without a transparent coating layer), and a light gray coating with a flat and calm finish was obtained. However, when the scratch resistance of the coating surface of the right half was checked by the same method as in Example 1, some scratches were found.

[0057] Comparative Example 2 The interior material 1 was applied with a trowel to the same surface as in Example 1, and then immediately spread and smoothed with the trowel to form a coated surface. The amount of the interior material 1 applied (in terms of solid content) was 450 g / m 2 After drying for 24 hours, the right half of the interior material coating was coated with transparent coating material 1 at a coating amount (solid content equivalent) of 50 g / m 2 After applying the paint by roller, the paint was dried and cured for 7 days. When the appearance of the coating obtained by the above method was checked, the right half (with the transparent coating layer) had a glossier appearance than the left half (without the transparent coating layer), and the finish was different from that of the coating of interior material 1.

Claims

1. A coating laminate having an interior material layer and a transparent coating material layer, The interior material layer contains 200 to 2,000 parts by weight of a body pigment and 20 to 2,000 parts by weight of an aggregate, relative to 100 parts by weight of a resin component, The average particle size of the extender pigment is less than 50 μm, and the average particle size of the aggregate is 0.05 to 3 mm. The transparent coating layer has a coating amount of 0.1 to 30 g / m2 in terms of solid content. 2 A coating laminate comprising:

2. A method for forming a coating laminate having an interior material layer and a transparent coating material layer, comprising the steps of: The interior material layer contains 200 to 2,000 parts by weight of a body pigment and 20 to 2,000 parts by weight of an aggregate, relative to 100 parts by weight of a resin component, The average particle size of the extender pigment is less than 50 μm, and the average particle size of the aggregate is 0.05 to 3 mm. A transparent coating material is applied to the interior material layer in an amount of 0.1 to 30 g / m2 in terms of solid content. 2 A transparent coating layer is formed by applying the A method for forming a coating laminate comprising the steps of:

3. The coating laminate according to claim 1, wherein the interior material layer has a coating amount of 80 to 3,000 g / m 2 calculated as solid content.

4. The method for forming a coating laminate according to claim 2, wherein the interior material layer is formed by an interior material, and the amount of the interior material applied (converted into solid content) is 80 to 3000 g / m 2 .

Citation Information

Patent Citations

  • Method for forming antibacterial coating film and infection preventive method by the same

    JP1996089887A

  • Multicoating-type plaster-like finish coating material

    JP1998259322A

  • Trowelling material composition for renovation of cross wall

    JP1999141090A

  • Coating composition having neptunian stone-like multicolored pattern, and coating finish by using the same

    JP2000086942A

  • Method for forming patterned surface

    JP2005013888A