SCR catalysts containing iron vanadate
The formulation of a selective catalytic reduction catalyst with iron and vanadium (Fe x M y V O 4) on titania support, combined with tungsten and antimony, addresses the deactivation issues of vanadium catalysts at high temperatures, enhancing NOx conversion and thermal stability in automotive applications.
Patent Information
- Application Number
- JP2021552674
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-31
- Filing Date
- 2020-03-06
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-03-06
AI Technical Summary
Vanadium catalysts used in selective catalytic reduction (SCR) systems experience deactivation at higher temperatures and have a limited activation temperature window, which is problematic in automotive applications where exhaust temperatures vary.
A selective catalytic reduction catalyst comprising iron and vanadium, formulated as Fe x M y V O 4, where x=0.2~1 and y=1-x, with M including non-Fe metals, is prepared using a vanadium oxide precursor and a metal vanadate, supported on titania, and optionally includes tungsten and antimony, to enhance thermal stability and NOx conversion.
The catalyst exhibits improved thermal stability and increased NOx conversion performance, maintaining high activity even after aging at elevated temperatures, with minimal deactivation, thus simplifying OEM calibration and reducing fresh-to-aged delta.
Smart Images

Figure 0007556875000013 
Figure 0007556875000011 
Figure 0007556875000008
Abstract
Description
[Background technology]
[0001] Nitrogen oxides (NO x Nitrogen compounds (NOx) are typically produced when fuels are burned and are emitted from mobile sources such as automobiles and stationary sources such as power plants or incinerators. These nitrogen compounds are identified as the main cause of acid rain and smog formation. In light of stricter environmental protection regulations and the increasing importance of environmental protection, more research is being conducted focusing on the reduction of nitrogen compounds through catalysts.
[0002] Selective catalytic reduction (SCR) devices using active materials such as vanadium have been commonly used to remove nitrogen compounds from stationary and mobile sources. Ammonia is known to be a suitable reducing agent for such systems. Summary of the Invention [Problem to be solved by the invention]
[0003] However, vanadium catalysts often suffer from deactivation issues at higher temperatures and are often limited to a smaller activation temperature window, which can be problematic especially in on-board applications where exhaust temperatures vary. Therefore, a catalyst with higher performance in NOx conversion and improved thermal stability would offer an immediate advantage.
[0004] According to some embodiments of the present invention, the selective catalytic reduction catalyst comprises iron and vanadium, the vanadium being selected from the group consisting of (1) one or more vanadium oxides and (2) Fe x M y It exists as a metal vanadate in the form of VO4, where x=0.2-1, y=1-x, and if y>0, then M includes one or more non-Fe metals.
[0005] According to some aspects of the present invention, the selective catalytic reduction catalyst comprises iron and vanadium, the catalyst comprising a vanadium oxide precursor and Fe x M yIt is prepared using metal vanadates in the form of VO4, where x=0.2-1, y=1-x, and if y>0, then M includes one or more non-Fe metals.
[0006] According to some aspects of the invention, the selective catalytic reduction catalyst comprises vanadium, iron and titania, the catalyst being Fe x M y The selective catalytic reduction catalyst comprises a metal vanadate in the form of VO4, where x=0.2-1, y=1-x, and if y>0, then M comprises one or more non-Fe metals, in an amount up to about 7 wt% vanadium, expressed as V2O5 wt% of V2O5+TiO2, the metal vanadate being present in an amount between 20% and 75% of the total amount of vanadium in the selective catalytic reduction catalyst.
[0007] In some embodiments, the vanadium precursor comprises vanadyl oxalate, ammonium metavanadate, vanadyl oxysulfate, vanadium pentoxide, vanadyl acetylacetonate, vanadium(III) acetylacetonate, or combinations thereof. In some embodiments, the vanadium precursor comprises vanadyl oxalate, ammonium metavanadate, or combinations thereof.
[0008] In some embodiments, for metal vanadates, when y>0, M can include Er, Al, Ce, or a combination thereof. For example, metal vanadates include FeVO4, Fe 0.5 Ce 0.5 VO4, Fe 0.33 Al 0.33 Er 0.33 VO4, or combinations thereof. In some embodiments, the metal vanadate may include FeVO4.
[0009] In some embodiments, the vanadium is present on a support comprising titania, hi certain embodiments, the titania is doped with, for example, W, Si, Mo, Nb, Sb, or combinations thereof.
[0010] In some embodiments, vanadium is present in an amount of about 2 wt% to about 7 wt%, expressed as V2O5 wt% of V2O5 + TiO2, in an amount of 3.5 wt% to about 7 wt%, expressed as V2O5 wt% of V2O5 + TiO2, or in an amount of about 3.5 wt% to about 6.05 wt%, expressed as V2O5 wt% of V2O5 + TiO2.
[0011] In some embodiments, the vanadium oxide precursor and the metal vanadate are present in a weight ratio expressed as a ratio of elemental vanadium of about 4:1 to about 1:2. In some embodiments, the catalyst is prepared using the vanadium oxide precursor and the metal vanadate, and the vanadium oxide precursor and the metal vanadate are present in a weight ratio expressed as a ratio of elemental vanadium of about 4:1 to about 1:2.
[0012] In some embodiments, the catalyst comprises titania in an amount of about 60 wt% to about 93 wt% of the selective catalytic reduction catalyst. In some embodiments, the titania comprises a blend of colloidal titania and standard micro-sized titania. The colloidal titania and standard micro-sized titania may be present in a weight ratio of about 0.08 to about 0.4.
[0013] In some embodiments, the catalyst further comprises tungsten. In some embodiments, the catalyst further comprises antimony. In some embodiments, the catalyst further comprises tungsten and antimony. In some embodiments, tungsten may be included in addition to any tungsten doped in the titania. In some embodiments, antimony may be included in addition to any antimony doped in the titania. In some embodiments, the weight ratio of W:Ti in the catalyst is about 0.025 to about 0.2. In some embodiments, the weight ratio of Sb:Ti in the catalyst is about 0.025 to about 0.2.
[0014] According to some aspects of the present invention, a washcoat for preparing a selective catalytic reduction catalyst comprises: (1) a vanadium oxide precursor; and (2) Fe x M yThe washcoat includes a metal vanadate in the form of VO4, where x=0.2-1, y=1-x, and if y>0, M includes one or more non-Fe metals. The washcoat may further include titania, tungsten, and / or antimony. In some embodiments, tungsten and antimony may be included in addition to any tungsten and / or antimony doped into the titania.
[0015] According to some aspects of the present invention, a method for preparing a selective catalytic reduction catalyst containing iron and vanadium includes: (1) reacting a vanadium oxide precursor with an Fe x M y The method includes preparing a washcoat comprising a metal vanadate in the form of VO4, where x=0.2-1, y=1-x, and where y>0, M comprises one or more non-Fe metals. The washcoat may further comprise titania, tungsten, and / or titania. In some embodiments, tungsten and antimony may be included in addition to any tungsten and / or antimony doped into the titania. The method may include applying the washcoat to a substrate and calcining, where the vanadium oxide precursor decomposes to one or more vanadium oxides. The method may include applying the washcoat to a substrate and calcining, where the calcined catalyst comprises one or more vanadium oxides and a metal vanadate. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 contains data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Diagram 2] FIG. 2 contains data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Diagram 3] FIG. 3 includes data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Figure 4] FIG. 4 includes data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Diagram 5] FIG. 5 includes data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Figure 6] FIG. 6 includes data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Figure 7] FIG. 7 includes data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Figure 8] FIG. 8 includes data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. [Figure 9] FIG. 9 includes data and images relating to the catalysts of the present invention and comparative formulations, as described in more detail herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The compositions and methods of the present invention relate to the purification of exhaust gases from internal combustion engines, and in particular to the cleaning of exhaust gases from diesel engines, especially vehicle engines.
[0018] It has been discovered that vanadium selective catalytic reduction ("SCR") catalysts prepared according to the formulations and methods of the present invention can provide surprising and unexpected advantages, including increased NOx conversion and greater thermal stability. Embodiments of the present invention are described in further detail herein.
[0019] SCR / V-SCR Selective catalytic reduction ("SCR") catalysts are catalysts that reduce NOx to N2 by reaction with nitrogen compounds (such as ammonia or urea) or hydrocarbons (lean NOx reduction). SCR catalysts can generally be composed of vanadium-titania catalysts, vanadium-tungsta-titania catalysts, or transition metal / molecular sieve catalysts.
[0020] Vanadium-containing SCR catalysts (vanadium SCR catalysts) may generally include vanadium on a support such as TiO2, or may include hybrid catalysts including vanadium on a support such as TiO2 blended with metal-zeolite or neat zeolite components in the formulation.
[0021] Vanadium SCR catalysts may contain vanadium as free vanadium, vanadium ions, or vanadium oxides or derivatives thereof. In addition to vanadium, the catalyst may contain other metal oxides, such as oxides of tungsten, oxides of niobium, oxides of antimony, and / or oxides of molybdenum. As used herein, a "catalytically active" metal oxide is one that is capable of reducing NO x and / or the oxidation of NH3 or other nitrogen-based SCR reductants. By inference, the "catalytically inactive" metal oxides are those that directly participate as molecular components in the catalytic reduction of NO x and / or the oxidation of NH3 or other nitrogen-based SCR reductants. In certain embodiments, the oxides of vanadium are present in major amounts (i.e., greater than 50 wt%) relative to other catalytically active metal oxides, such as tungsten oxide. In certain embodiments, the oxides of vanadium are present in minor amounts (i.e., less than 50 wt%) relative to other catalytic metal oxides, such as tungsten oxide.
[0022] In certain embodiments, the support material for the vanadium component is titania or titania in combination with another component such as tungsten (VI) oxide, molybdenum oxide, niobium oxide, antimony oxide, or silica as a mixture or mixed oxide. The support material may be an aluminosilicate, alumina, silica, and / or silica-doped titania. In some embodiments, the support may be titania doped with W, Si, Mo, Nb, Sb, or combinations thereof. In some embodiments, the support may be titania doped with W and Si. While both vanadium and the support may be metal oxides, the two components are structurally distinct from each other in that the support exists as individual particles and the vanadium exists in a relatively thin layer or coating attached to the particles. Thus, vanadium and titania do not exist as mixed oxides.
[0023] The support material preferably has an average particle size based on particle count of about 0.01-10 μm, e.g., about 0.5-5 μm, about 0.1-1 μm, or about 5-10 μm, preferably with a majority of the particle count within one of these ranges. In some embodiments, the support is a high surface area support.
[0024] In some embodiments, the support is a molecular sieve. The molecular sieve may have an aluminosilicate framework (e.g., zeolite) or a silicoaluminophosphate framework (e.g., SAPO).
[0025] When the molecular sieve has an aluminosilicate framework (e.g., the molecular sieve is a zeolite), typically the molecular sieve has a silica-to-alumina molar ratio (SAR) of 5-200 (e.g., 10-200), 10-100 (e.g., 10-30 or 20-80), 10-50, 10-30, 12-40, 15-30, 5-20, 5-15, 8-15, 8-13, 10-15, 10-20, 10-40, 10-60, 10-80, 10-100, 10-150, <30, <20, <15, or <13. In some embodiments, suitable molecular sieves have a SAR of >200, >600, or >1200. In some embodiments, the molecular sieve has a SAR of about 1500 to about 2100.
[0026] Typically, the molecular sieve is microporous. Microporous molecular sieves have pores with diameters of less than 2 nm (see, for example, the IUPAC definition of "microporous" [Pure & Appl. Chem., 66(8), (1994), 1739-1758]).
[0027] The molecular sieve may be a small pore molecular sieve (e.g., a molecular sieve having a maximum ring size of 8 tetrahedral atoms), a medium pore molecular sieve (e.g., a molecular sieve having a maximum ring size of 10 tetrahedral atoms) or a large pore molecular sieve (e.g., a molecular sieve having a maximum ring size of 12 tetrahedral atoms), or a combination of two or more thereof.
[0028] In some embodiments, the molecular sieve may be mesoporous. Mesoporous molecular sieves have pores with diameters between 2 and 50 nm (e.g., according to the IUPAC definition of "microporous").
[0029] When the molecular sieve is a small pore molecular sieve, the small pore molecular sieve can have a framework structure represented by a framework type code (FTC) selected from the group consisting of ACO, AEI, AEN, AFN, AFT, AFX, ANA, APC, APD, ATT, CDO, CHA, DDR, DFT, EAB, EDI, EPI, ERI, GIS, GOO, IHW, ITE, ITW, LEV, LTA, KFI, MER, MON, NSI, OWE, PAU, PHI, RHO, RTH, SAT, SAV, SFW, SIV, THO, TSC, UEI, UFI, VNI, YUG, and ZON, or mixtures and / or combinations of two or more thereof and / or intergrowth. In some embodiments, the small pore molecular sieve has a framework structure selected from the group consisting of CHA, LEV, AEI, AFX, ERI, LTA, SFW, KFI, DDR, and ITE. In some embodiments, the small pore molecular sieve has a framework structure selected from the group consisting of CHA, AEI and AFX. In some embodiments, the small pore molecular sieve has a framework structure selected from the group consisting of CHA and AEI. The small pore molecular sieve may have a CHA framework structure. The small pore molecular sieve may have an AEI framework structure.
[0030] When the molecular sieve is a medium pore molecular sieve, the medium pore molecular sieve can have a framework structure represented by a framework type code (FTC) selected from the group consisting of AEL, AFO, AHT, BOF, BOZ, CGF, CGS, CHI, DAC, EUO, FER, HEU, IMF, ITH, ITR, JRY, JSR, JST, LAU, LOV, MEL, MFI, MFS, MRE, MTT, MVY, MWW, NAB, NAT, NES, OBW, PAR, PCR, PON, PUN, RRO, RSN, SFF, SFG, STF, STI, STT, STW, SVR, SZR, TER, TON, TUN, UOS, VSV, WEI and WEN, or mixtures of two or more thereof and / or intergrowth. In some embodiments, the medium pore molecular sieve has a framework structure selected from the group consisting of FER, MEL, MFI and STT. In some embodiments, the medium pore molecular sieve has a framework structure selected from the group consisting of FER and MFI, particularly MFI. When the medium pore molecular sieve is a zeolite and has a FER or MFI framework, the zeolite can be ferrierite, silicalite or ZSM-5.
[0031] When the molecular sieve is a large pore molecular sieve, the large pore molecular sieve may have a framework structure represented by a framework type code (FTC) selected from the group consisting of AFI, AFR, AFS, AFY, ASV, ATO, ATS, BEA, BEC, BOG, BPH, BSV, CAN, CON, CZP, DFO, EMT, EON, EZT, FAU, GME, GON, IFR, ISV, ITG, IWR, IWS, IWV, IWW, JSR, LTF, LTL, MAZ, MEI, MOR, MOZ, MSE, MTW, NPO, OFF, OKO, OSI, RON, RWY, SAF, SAO, SBE, SBS, SBT, SEW, SFE, SFO, SFS, SFV, SOF, SOS, STO, SSF, SSY, USI, UWY, and VET, or mixtures of two or more thereof and / or intergrowth. In some embodiments, the large pore molecular sieve has a framework structure selected from the group consisting of AFI, BEA, MAZ, MOR and OFF. In some embodiments, the large pore molecular sieve has a framework structure selected from the group consisting of BEA, MOR and FAU. When the large pore molecular sieve is a zeolite and has a BEA, FAU or MOR framework, the zeolite can be beta zeolite, faujasite, zeolite Y, zeolite X or mordenite.
[0032] In some embodiments, suitable molecular sieves include a combination of small and large pore frameworks, hi some embodiments, suitable molecular sieves include ZSM-34(ERI+OFF).
[0033] The transition metal / molecular sieve catalyst comprises a transition metal and a molecular sieve, such as an aluminosilicate zeolite or a silicoaluminophosphate. The transition metal can be selected from chromium, cerium, manganese, iron, cobalt, nickel, and copper, and mixtures thereof. Iron and copper may be particularly preferred. The SCR catalyst may comprise a metal / zeolite catalyst, such as iron / beta zeolite, copper / beta zeolite, copper / SSZ-13, copper / SAPO-34, Fe / ZSM-5, or copper / ZSM-5. In some embodiments, the molecular sieve may comprise a beta zeolite, ferrierite, or chabazite. Preferred SCR catalysts include Fe-CHA, Fe-AEI, Mn-CHA, Mn-BEA, Mn-FER, Mn-MFI, Cu-CHA, such as Cu-SSZ-13, and Fe-beta zeolite.
[0034] Selective catalytic reduction catalysts can be used with filters called SCRFs. Selective catalytic reduction filters (SCRFs) are single substrate devices that combine the functionality of SCR with a particulate filter. They are used to remove NO x and reducing particulate matter emissions from an internal combustion engine. In addition to the SCR catalyst coating, the particulate filter may also include other metal and metal oxide components (such as Pt, Pd, Fe, Mn, Cu, and ceria) to oxidize hydrocarbons and carbon monoxide in addition to breaking down soot trapped by the filter. The systems of the present invention may include SCRF catalysts, including vanadium catalysts, referred to herein as vanadium SCRF catalysts. References throughout this application to the use of vanadium SCR catalysts, where applicable, are understood to include the use of vanadium SCRF catalysts as well.
[0035] Any suitable washcoat preparation method may be used for the catalyst of the present invention, such as, for example, a one-pot preparation. The catalyst may typically be prepared as an aqueous slurry of components, which may include a mixture of soluble and insoluble components, and in some embodiments, may have a final slurry pH of 5 to 8. The slurry may be deposited on the catalyst monolith by a washcoating process, such as a dip or vacuum process from one or both ends of the monolith, typically followed by drying and calcination. Unless otherwise noted, the examples described below were dried at 100° C. for about 15 minutes, and then calcined at 500° C. for about 10 minutes.
[0036] Vanadium oxide precursor / Fe x M y VO4 Vanadium SCR catalysts are typically prepared using vanadium oxide precursors such as a single vanadium salt like vanadyl oxalate (COV). Vanadium oxide precursors such as vanadyl oxalate offer advantages such as strong fresh NOx conversion at low temperatures, but have been found to deactivate upon aging due to vanadium sintering. Higher vanadium loadings result in stronger fresh activity at low temperatures, but also a greater degree of deactivation.
[0037] Fe x M y Metal vanadates of the VO4 family (where Fe x M y Vanadium oxide (also called vanadium oxide) is a family of iron vanadium materials, where x=0.2-1, y=1-x, and M is Er, Al, Ce, e.g., FeVO4, Fe 0.5 Ce 0.5 VO4 and Fe 0.33 Al 0.33 Er 0.33 It may be composed of one or more non-Fe metals, including but not limited to VO4. x M yIt was discovered that the fresh NOx conversion activity of VO4 is very low, but is significantly activated by aging or exposure to high temperatures of about 650 °C for 2 hours. Within a specific range of ratios, (1) one or more vanadium oxide precursors that decompose to one or more vanadium oxides upon calcination, and (2) Fe x M y By preparing catalysts with a blend of VO4, such catalysts can achieve unexpected levels of catalytic stability with aging while minimizing the fresh-to-aged delta in low temperature (e.g., about 175°C to about 300°C) NO-SCR activity.
[0038] Surprisingly, vanadium oxide precursors and Fe x M y Catalysts prepared with both VO4 allow for higher total vanadium loadings, resulting in higher performance and more thermally durable catalysts. Higher vanadium loadings also increase the total number of vanadium sites in the catalyst, thereby increasing resistance to site-specific poisons that can build up in SCR catalysts during operation.
[0039] As used herein, vanadium oxide precursors are understood to refer to vanadium compositions that can decompose into one or more vanadium oxides upon calcination. Examples of suitable vanadium oxide precursors may include vanadyl oxalate, ammonium metavanadate, vanadyl oxysulfate, vanadium pentoxide, vanadyl acetylacetonate, vanadium(III) acetylacetonate, or combinations thereof. In some embodiments, suitable vanadium oxide precursors include vanadyl oxalate and ammonium metavanadate.
[0040] The selective catalytic reduction catalyst described herein comprises a vanadium oxide precursor and Fe x M y Upon calcination, the vanadium oxide precursor may decompose into one or more vanadium oxides. Thus, the selective catalytic reduction catalysts described herein may include iron and vanadium, where the vanadium is either (1) one or more vanadium oxides, or (2) Fe x My It exists as VO4. In some embodiments, the selective catalytic reduction catalyst described herein can include (1) vanadium on a support comprising titania, and (2) iron.
[0041] ratio Vanadium oxide precursors such as vanadium oxalate and Fe oxide such as FeVO4 x M y Metal vanadates of the VO4 family can be combined to provide a highly stable catalyst with minimal deactivation after typical vanadium SCR aging, e.g., aging at about 580°C for about 100 hours, compared to catalysts made using vanadyl oxalate alone. The catalyst is prepared by combining a vanadium oxide precursor, such as vanadyl oxalate, and an Fe oxide precursor, such as FeVO4. x M y The metal vanadates of the VO4 family may be included in a weight ratio, expressed as a ratio of elemental vanadium, of about 6:1 to about 1:2, about 5:1 to about 1:2, about 4:1 to about 1:2, about 3:1 to about 1:2, about 3:1 to about 1:1, about 6:1, about 5:1, about 4:1, about 3:1, about 2:1, about 1:1, about 1:2, or about 1:3.
[0042] Vanadium loading Vanadium oxide precursor and Fe x M y It has been discovered that the combination of VO4 may provide a more stable catalyst, and as a result, the total vanadium loading on the catalyst can be increased without compromising aging performance. Vanadium on titania support is an active catalyst, but vanadium oxide on the surface is known to promote sintering of the titania support and loss of surface area, which may reduce aging activity. Typically, when using a vanadium oxide precursor-only source and a typical 500°C calcination, there can be a significant fresh-to-aged delta at any vanadium loading. In particular, vanadium loadings above about 4 wt% (expressed as V2O5 wt% of V2O5+TiO2) can lose light-off performance with aging, such as 580°C / 100 hour aging. The vanadium precursor and Fe x M yIn combination with VO4, vanadium loadings in the range of about 2 wt% to about 6.5 wt% (expressed as V2O5 wt% of V2O5+TiO2) can be achieved with minimal deactivation of light-off performance on aging. While not wishing to be bound by this theory, it is believed that Fe x M y The VO4 vanadium source has less damage to the titania support and reduces the amount of Fe due to aging. x M y It is believed that the activation of VO4 compensates for the deactivation of vanadium oxide. The catalyst may be expressed as V2O5wt% of V2O5+TiO2, up to about 2wt%, up to about 3wt%, up to about 3.5wt%, up to about 4wt%, up to about 4.5wt%, up to about 5wt%, up to about 5.5wt%, up to about 6wt%, up to about 6.5wt%, up to about 7wt%, up to about 7.5wt%, up to about 8wt%, about 1wt% to about 8wt%, about 1wt% to about 7.5wt%, about 1wt% to about 7wt%, about 1wt% to about 6.5wt%, about 1wt% to about 6wt%, about 1wt% to about 6wt%, about 1wt% to about 1 ... % to about 5.5 wt%, about 2 wt% to about 7.5 wt%, about 2 wt% to about 7 wt%, about 3 wt% to about 7.5 wt%, about 3.5 wt% to about 7.5 wt%, about 3.5 wt% to about 7 wt%, about 3.7 wt% to about 6.5 wt%, about 3.7 wt% to about 6.05 wt%, about 1 wt% to about 5 wt%, about 2 wt% to about 4.5 wt%, about 1 wt% to about 4 wt%, about 2.5 wt% to about 4.5 wt%, about 2 wt% to about 4 wt%, or about 3 wt% to about 4 wt% vanadium. As used throughout this specification, in calculating total vanadium loading expressed as "V2O5 + V2O5 wt% of TiO2," it is understood that TiO2 refers to the TiO2 content and not the loading of doped TiO2 in the formulation. For example, a washcoat containing 10% doped titania at 80 wt% of the total washcoat and no other titania components would be 72% TiO2, and if the washcoat contains 3 wt% vanadium (as V2O5) of the total washcoat, it would be expressed as having 4 wt% V2O5 of (3 / [72+3])=V2O5+TiO2.
[0043] In some embodiments, the catalyst comprises Fe in an amount of about 20% to about 75%, about 20% to about 67%, about 25% to about 67%, about 33% to about 50%, about 20%, about 25%, about 33%, about 50%, about 67%, or about 75% of the total amount of vanadium in the catalyst (expressed as a % of the total amount of vanadium in the catalyst). x M y May contain VO4.
[0044] thermal durability For automotive SCR applications, OEMs must adjust reductant dosing strategies to ensure relevant NOx legislation is met both at the catalyst's fresh state and at the end of its life. If the application knows that the catalyst's performance will degrade over time, a degradation factor (DF) for SCR performance typically must be established and incorporated into the engine calibration, and accurately establishing this DF can be a challenge for OEMs. Therefore, catalysts with low fresh-to-aged deltas for thermal aging are desirable to simplify OEM calibration. For example, NO-only SCR performance at low temperatures with less than a 10% decrease between fresh and aged, or less than a 15% increase between fresh and aged, is desired.
[0045] In certain circumstances, higher firing temperatures can be used to reduce the fresh performance and therefore the fresh to aged delta, however from a cost and sustainability standpoint, using higher temperatures is undesirable and compositional approaches that reduce the fresh to aged delta are preferred.
[0046] The catalysts described herein can exhibit high thermal stability as evidenced by minimal deactivation after aging of typical vanadium SCR catalysts. For example, vanadium oxide precursors and Fe x M y Catalysts prepared with VO4 may exhibit thermal durability after aging at about 550°C to about 650°C for about 50 to about 200 hours, such as at about 580°C for 100 hours and / or at about 600°C for about 50 hours.
[0047] The vanadium precursor and Fe x M y Catalysts prepared with VO4 may advantageously provide a high level of catalytic stability with aging, as indicated by the smallest fresh-to-aged delta at low temperatures (150°C-300°C). In a specific example, after thermal aging at 580°C for 100 hours, the vanadium precursor and Fe x M y The catalyst prepared with VO4 can provide NOx conversion performance at 225°C under the conditions of 60K SV, ANR 1.05, and 500 ppm NOx with 73% fresh and 75% aged (2% increase). The reference catalyst prepared with vanadium precursor only can provide NOx conversion under the same conditions with 79% fresh and 64% aged (15% decrease). x M y Catalysts prepared with VO4 may exhibit a fresh to aged delta (expressed as a percentage increase or decrease) in NOx conversion at low temperatures (150°C-300°C) of less than 13%, less than 12%, less than 10%, less than 8%, less than 6%, less than 4%, less than 2%, less than 1%, 0%-13%, 0%-10%, 0%-8%, 0%-6%, 0%-4%, 0%-2% reduction, less than 0%, less than 1%, less than 2%, less than 4%, less than 5%, less than 6%, less than 8%, less than 10%, less than 15%, 0%-1%, 0%-2%, 0%-4%, 0%-6%, 0%-8%, 0%-10%, or 0%-15% increase.
[0048] Titania Binder Vanadium SCR catalysts may be conventionally prepared using a certain amount of vanadium, tungsten as a promoter or dopant, and a titania support. These components may be coated onto a monolith and adhered using a binder, which may be any one or more of several colloidal oxides. The binder is considered to be largely inert, since it does not participate in the catalytic action, but serves only to secure the catalyst to the monolith.
[0049] However, it has been discovered that the use of colloidal anatase titania as a binder can provide additional catalytic performance advantages. These advantages are believed to arise because the action of calcining the catalyst sinters the colloidal anatase particles, forming an active support material where the vanadium can participate in the SCR reaction. It has further been discovered that by incorporating enough vanadium to optimally coat this newly formed surface, and enough tungsten to support the titania and promote the SCR reaction, the binder can be used not only to adhere the catalytic materials together, but also to function as an active catalyst.
[0050] Colloidal / Standard Titania Blend Supports It has also been discovered that catalysts prepared using blends of colloidal titania and standard micro-sized titania may result in catalysts with increased active SCR temperatures compared to catalysts prepared with colloidal silica and standard micro-sized titania. It is believed that the small particle size of the colloidal titania particles, when incorporated into a washcoat as a blend with standard micro-sized titania, allows the larger support particles to be sintered and bonded together, and the standard micro-sized titania to adhere together to the support, creating a larger support surface. By including a carefully optimized amount of tungsten in the formulation, the tungsten can be incorporated into the colloidal titania binder during sintering, creating an active and promoted support. It has been discovered that a mixture of colloidal titania and calcined anatase titania can provide high titania surface area with sufficient stability to prevent high aging effects. Furthermore, the binding function of colloidal titania allows for the use of less inert binder (such as SiO2) without compromising washcoat adhesion, thereby increasing the weight percent of titania in the overall washcoat compared to catalysts prepared with a blend of colloidal silica and standard microsized titania. Such an arrangement allows for a higher total washcoat vanadium content to be stabilized without increasing the V2O5 wt% of V2O5+TiO2, resulting in a catalyst with an increased active SCR temperature window.
[0051] Catalysts containing blends of colloidal titania and standard microsized titania have been shown to be effective in reducing the amount of titania by weight percent of the catalyst, from about 60% to about 93%, from about 60% to about 90% by weight, from about 65% to about 90% by weight, from about 70% to about 90% by weight, from about 75% to about 85% by weight, from about 77% to about 82% by weight, from about 79% to about 81% by weight, from about 60% to about 62% by weight, from about 65% to about 67% by weight, from about 78% to about 81% by weight, from about 79% to about 82% by weight, from about 79% to about 81% by weight, from about 60% to about 62% by weight, from about 65% to about 67% by weight, from about 78% to about 82% by weight, from about 79% to about 81 ... %, about 70 wt%, about 72 wt%, about 75 wt%, about 77 wt%, about 80 wt%, about 82 wt%, about 85 wt%, about 87 wt%, about 90 wt%, about 93%, greater than 60 wt%, greater than 62 wt%, greater than 65 wt%, greater than 67 wt%, greater than 70 wt%, greater than 72 wt%, greater than 75 wt%, greater than 77 wt%, greater than 80 wt%, greater than 82 wt%, greater than 85 wt%, greater than 87 wt%, or greater than 90% titania.
[0052] Catalysts comprising blends of colloidal titania and standard microsized titania may contain an increased weight percent of titania, which may correspond to a higher total vanadium loading, as compared to catalysts prepared with blends of colloidal silica and standard microsized titania. Catalysts comprising blends of colloidal titania and standard microsized titania may contain an increased weight percent of titania, which may correspond to a higher total vanadium loading, as compared to catalysts prepared with blends of colloidal titania and standard microsized titania. Catalysts comprising blends of colloidal titania and standard microsized titania may contain an increased weight percent of titania, which may correspond to a higher total vanadium loading, as compared to catalysts prepared with blends of colloidal titania and standard microsized titania, from about 7% to about 30%, from about 10% to about 30%, from about 5% to about 25%, from about 7% to about 23%, from about 10% to about 20%, from about 10% to about 15%, from about 10% to about 20%, from about 10% to about 25 ... The composition may include a weight percent of titania that is an increment of 5% to about 20%, about 12% to about 18%, about 15% to about 30%, about 20% to about 30%, about 25% to about 30%, about 7% to about 10%, about 7% to about 15%, about 7% to about 20%, about 7% to about 25%, about 10% to about 25%, about 15% to about 20%, about 7%, about 10%, about 15%, about 20%, about 25%, or about 30%. Similarly, catalysts comprising blends of colloidal titania and standard microsized titania have a vanadium weight percentage of about 7% to about 30%, about 10% to about 30%, about 5% to about 25%, about 7% to about 23%, about 10% to about 20%, about 10% to about 15%, about 10% to about 20 ... The vanadium may include a weight percentage that is an increment of about 15% to about 20%, about 12% to about 18%, about 15% to about 30%, about 20% to about 30%, about 25% to about 30%, about 7% to about 10%, about 7% to about 15%, about 7% to about 20%, about 7% to about 25%, about 10% to about 25%, about 15% to about 20%, about 7%, about 10%, about 15%, about 20%, about 25%, or about 30%.
[0053] The catalyst can be formulated with a blend of colloidal titania and standard microsized titania in a range of weight ratios to provide a thermally stable catalyst. For example, the catalyst can be formulated with a range of weight ratios of titania to colloidal to standard microsized titania (excluding dopants) from about 0.025 to about 0.4, about 0.05 to about 0.4, about 0.06 to about 0.4, about 0.07 to about 0.4, about 0.08 to about 0.35, about 0.09 to about 0.3, about 0.1 to about 0.25, about 0.11 to about 0.25, about 0.12 to about 0.24, about 0.1 to about 0.4, about 0.12 to about 0.4, about 0.15 to about 0.4, about 0.17 to about 0.37, about 0. The weight ratios may include colloidal titania and standard microsized titania, with the weight ratio being about 0.18 to about 0.35, about 0.18 to about 0.33, about 0.18 to about 0.3, about 0.18 to about 0.28, about 0.2 to about 0.26, about 0.22 to about 0.24, about 0.1, about 0.12, about 0.15, about 0.17, about 0.18, about 0.2, about 0.22, about 0.23, about 0.24, about 0.25, about 0.26, about 0.28, about 0.3, about 0.33, about 0.35, about 0.37, or about 0.4. Such weight ratios refer to microsized titania including any dopants.
[0054] Catalysts formulated with a blend of colloidal titania and standard microsized titania can provide a low delta in SCR performance between fresh and aged states, thereby providing a stable catalyst. This low delta is understood to represent high thermal stability as indicated by minimal deactivation after aging of a typical vanadium SCR catalyst. In some embodiments, low delta is understood to mean less than a 10% difference in absolute NOx conversion between a fresh catalyst and an aged catalyst at 580° C. for 100 hours.
[0055] tungsten Tungsten may be included in the catalyst formulation to activate colloidal titania as an effective support material. A typical titania support material may contain about 3 wt% to about 10 wt% WO3 and up to about 10 wt% SiO2 with a W:Ti weight ratio of about 0.015 to about 0.06, or more optimally, about 3 wt% to about 7 wt% WO3 and up to about 5 wt% SiO2 with a W:Ti weight ratio of about 0.015 to about 0.056. A typical titania support material may be doped with tungsten in the range of about 1 to about 15%. However, adding extra tungsten to the washcoat to maintain the total W:Ti weight ratio of the catalyst in the range of about 0.025 to about 0.2, about 0.025 to about 0.09, about 0.035 to about 0.09, or about 0.035 to about 0.06 may provide a more active and stable catalyst. Tungsten may be added as a component to the washcoat, separate from the tungsten doped in the titania. In some embodiments, the selective catalytic reduction catalyst of the present invention may include additional tungsten in an amount of up to about 5 wt% WO3 in the catalyst. In some embodiments, the selective catalytic reduction catalyst of the present invention may include about 1 to about 15 wt% WO3 in the catalyst.
[0056] Antimony In some embodiments, the catalyst further comprises antimony. In some embodiments, the catalyst further comprises tungsten and antimony. In some embodiments, antimony may be included in addition to any antimony doped into the titania. In some embodiments, the weight ratio of Sb:Ti in the catalyst is about 0.025 to about 0.2, about 0.025 to about 0.09, about 0.035 to about 0.09, or about 0.035 to about 0.06.
[0057] Antimony may be added to the washcoat apart from the antimony doped in the titania. The washcoat may include titania, tungsten and / or antimony.
[0058] Other components Base material The catalytic article of the present invention may include a substrate and a vanadium SCR catalyst. The substrate may be a flow-through substrate or a filter substrate. The substrate may include a vanadium SCR catalyst (i.e., the catalytic article is obtained by extrusion), or the vanadium SCR catalyst may be disposed or supported on a substrate (i.e., the vanadium SCR catalyst is applied onto the substrate by a washcoating method). The vanadium SCR catalyst may fully or partially coat the substrate, as desired. In some embodiments, the catalytic article includes a vanadium SCR catalyst extrusion article coated with one or more additional catalysts. In some embodiments, the extruded catalyst is coated with one or more additional SCR catalysts, which may include, for example, a vanadium SCR catalyst.
[0059] In some embodiments, the catalyst article has a mass of about 1 to about 8.5 g in -3 , about 2 to about 7.5g in -3 , about 3 to about 6.5g in -3 , about 4 to about 5.5g in -3 , about 0.5 to about 4.0g in -3 , about 1.0 to about 3.0g in -3 or about 1.2 to about 2.5 g / in 3 The vanadium SCR catalyst may include a total concentration of
[0060] When a catalyst article has a filter substrate, such catalyst article is a selective catalytic reduction filter catalyst. A selective catalytic reduction filter includes a filter substrate and a vanadium SCR catalyst. Throughout this application, references to the use of an SCR catalyst are understood to also include the use of a selective catalytic reduction filter catalyst, where applicable.
[0061] The flow-through or filter substrate is a substrate that can contain catalyst / sorbent components. The substrate is preferably a ceramic substrate or a metal substrate. The ceramic substrate may comprise any suitable refractory material, such as alumina, silica, titania, ceria, zirconia, magnesia, zeolite, silicon nitride, silicon carbide, zirconium silicate, magnesium silicate, aluminosilicate, metalloaluminosilicate (such as cordierite and spodumene), or any two or more mixtures or mixed oxides thereof. Cordierite, magnesium aluminosilicate, and silicon carbide are particularly preferred.
[0062] The metal substrate may be made of any suitable metal, particularly heat-resistant metals and metal alloys such as titanium and stainless steel, and ferritic alloys containing iron, nickel, chromium, and / or aluminum in addition to other trace metals.
[0063] The flow-through substrate is preferably a flow-through monolith having a honeycomb structure with many small parallel thin-walled channels that are axially continuous through the substrate and extend entirely from the inlet or outlet of the substrate. The channel cross-section of the substrate may be any shape, but is preferably square, sinusoidal, triangular, rectangular, hexagonal, trapezoidal, circular, or elliptical. The flow-through substrate may also be highly porous, allowing the catalyst to penetrate the substrate wall.
[0064] The filter substrate is preferably a wall-flow monolith filter. The channels of the wall-flow filter are alternately blocked. This allows the exhaust gas flow to enter the channels through an inlet, then flow through the channel walls and exit the filter through a different channel that leads to an outlet. Thus, particulate matter in the exhaust gas flow is trapped within the filter.
[0065] The catalyst composition may be applied to the flow-through or filter substrate by any known means, such as a washcoat procedure.
[0066] When the catalyst article is a selective catalytic reduction filter, the filter substrate may preferably be a wall-flow filter substrate monolith. Wall-flow filter substrate monoliths (e.g., SCR-DPFs) typically have a cell density of 60 to 400 cells per square inch (cpsi). Wall-flow filter substrate monoliths preferably have a cell density of 100 to 350 cpsi, more preferably 200 to 300 cpsi.
[0067] The wall-flow filter substrate monolith can have a wall thickness (eg, average internal wall thickness) of 0.20 to 0.50 mm, preferably 0.25 to 0.35 mm (eg, about 0.30 mm).
[0068] Generally, uncoated wall-flow filter substrate monoliths have a porosity of 50-80%, preferably 55-75%, more preferably 60-70%.
[0069] Uncoated wall-flow filter substrate monoliths typically have an average pore size of at least 5 μm, preferably between 10 and 40 μm, for example between 15 and 35 μm, more preferably between 20 and 30 μm.
[0070] The wall-flow filter substrate may have a symmetric or asymmetric cell design.
[0071] In the case of selective catalytic reduction filters, the catalyst composition is generally disposed within the walls of the monolith of the wall-flow filter substrate. In addition, the catalyst composition may be disposed on the walls of the inlet channels and / or on the walls of the outlet channels.
[0072] The catalyst composition of the present embodiment can be coated onto a suitable monolith substrate. Washcoat compositions containing the catalyst composition of the present invention for coating onto monolith substrates or for producing extruded substrate monoliths may include a binder selected from the group consisting of alumina, silica, (non-zeolitic) silica-alumina, natural clay, TiO2, ZrO2, and SnO2. Generally, catalyst articles containing the catalyst composition at a desired loading level can be prepared by washcoating, extrusion, or other methods known in the art.
[0073] Methods and systems The method of the present invention involves treating an exhaust gas containing nitrogen oxides by contacting it with a reducing agent, such as a nitrogenous reducing agent or a hydrocarbon reducing agent, in the presence of the catalyst composition described herein. Thus, the vanadium SCR catalyst of the present invention can function as a selective catalytic reduction catalyst.
[0074] In some embodiments, the nitrogen oxides are reduced with a reducing agent at a temperature of at least 100° C. In another embodiment, the catalysts described herein are effective at reducing nitrogen oxides reduced with a reducing agent over a wide temperature range (e.g., from about 150° C. to 750° C.) in addition to being hydrothermally stable at temperatures above 900° C. The latter embodiment may be particularly useful for treating exhaust gases from heavy and light-duty diesel engines, particularly engines that include exhaust systems that include actively regenerated (optionally catalyzed) particulate filters, by injecting hydrocarbons into the exhaust system upstream of the filter. The zeolite catalyst for use in the present invention is located downstream of the filter.
[0075] In certain aspects, the temperature range is 175-550° C. In other embodiments, the temperature range is 175-400° C. In some aspects, the temperature range is 275-500° C., or 250-550° C. If NO is present in the gas stream, the temperature range can be broader, for example, 150-650° C., 175-625° C., 200-600° C., or 225-575° C.
[0076] In some embodiments, the reduction of nitrogen oxides is carried out in the presence of oxygen. In some embodiments, the reduction of nitrogen oxides is carried out in the absence of oxygen.
[0077] The nitrogenous reductant may itself be ammonia, or the source of the nitrogenous reductant may be hydrazine, or any suitable ammonia precursor such as urea ((NH2)2CO), ammonium carbonate, ammonium carbamate, ammonium bicarbonate, or ammonium formate. The reductant may be injected into the exhaust gas stream from an external source such as a reservoir or tank, supplied in situ by the nitrogen storage catalyst or NOx adsorber catalyst, or a combination of both. The reductant must be introduced into the exhaust gas upstream of the vanadium SCR catalyst.
[0078] The method can be performed on gases originating from combustion processes, such as internal combustion engines (either mobile or stationary), gas turbines, and coal or oil fired power plants. The method can also be used to treat gases from industrial processes such as refining, refinery heaters and boilers, furnaces, chemical processing industries, coke ovens, municipal waste plants and incinerators, coffee roasting plants, etc.
[0079] In certain embodiments, the method is used to treat exhaust gas from a lean-burn internal combustion engine of a vehicle, such as a diesel engine, a lean-burn gasoline engine, or an engine powered by liquid petroleum gas or natural gas.
[0080] In some aspects, the present invention provides an exhaust system for a lean-burn internal combustion engine of a vehicle, the system including a conduit for carrying a flowing exhaust gas, a source of nitrogenous reductant, a vanadium SCR catalyst disposed in a flow path of the exhaust gas, and means for metering the nitrogenous reductant into the flowing exhaust gas upstream of the vanadium SCR catalyst.
[0081] The system may be configured to, in use, for example, at 100° C. or more, 150° C. or more, or 175° C. or more, such that the catalyst composition produces NO at or above a desired efficiency. x and means for controlling the metering means such that the nitrogenous reductant is metered into the flowing exhaust gas only if it is determined that the reduction can be catalyzed. The determination by the control means may be assisted by one or more suitable sensor inputs indicative of engine conditions selected from the group consisting of exhaust gas temperature, catalyst bed temperature, promoter position, exhaust gas mass flow rate in the system, manifold vacuum, ignition timing, engine speed, exhaust gas lambda value, the amount of fuel injected into the engine, exhaust gas recirculation (EGR) valve position, and thus the magnitude of EGR and boost pressures.
[0082] In some embodiments, the metering may be performed using, for example, a pre-correlated look-up table or map stored in the control means, or by using any one or more of the above inputs indicative of the engine condition to calculate a predicted NO of the exhaust gas. x By correlating with the content, the appropriate NO x The control is dependent on the amount of nitrogen oxides in the exhaust gas, which is determined either indirectly or via a sensor.
[0083] The control means may include a pre-programmed processor, such as an electronic control unit (ECU).
[0084] The metering of nitrogenous reductant can be adjusted so that 60% to 200% of the theoretical ammonia is present in the exhaust gas entering the SCR catalyst, calculated at 1:1 NH3 / NO and 4:3 NH3 / NO2.
[0085] In some aspects, an oxidation catalyst for oxidizing nitric oxide in the exhaust gas to nitrogen dioxide can be located upstream of where the nitrogenous reductant is metered into the exhaust gas. In some embodiments, the oxidation catalyst is adapted to produce a gas stream entering the SCR catalyst composition having a ratio of NO to NO2 of about 4:1 to about 1:3 by volume at an exhaust gas temperature at the oxidation catalyst inlet of, for example, 200°C to 450°C or 250°C to 450°C. This concept is disclosed in S. Kasaoka et al., "Effect of Inlet NO / NO2 Molar Ratio and Role of Oxygen in Catalytic Reduction of Nitrogen Oxides by Ammonia," Journal of the Chemical Society of Japan, 1978, No. 6, pp. 874-881, and WO 99 / 39809.
[0086] The oxidation catalyst may include at least one platinum group metal (or some combination thereof), such as platinum, palladium, or rhodium, coated on a flow-through monolith substrate. In one embodiment, the at least one platinum group metal is platinum, palladium, or a combination of both platinum and palladium. The platinum group metal may be supported on a high surface area washcoat component, such as alumina, a zeolite, such as an aluminosilicate zeolite, silica, a non-zeolitic silica alumina, ceria, zirconia, titania, or a mixed or composite oxide containing both ceria and zirconia.
[0087] In some embodiments, a suitable filter substrate is located between the oxidation catalyst and the SCR catalyst. The filter substrate may be selected from any of those described above, for example a wall-flow filter. Where the filter is catalyzed, for example with an oxidation catalyst of the type discussed above, preferably the location where the nitrogenous reductant is metered is located between the filter and the SCR catalyst. Alternatively, if the filter is not catalyzed, the means for metering the nitrogenous reductant can be located between the oxidation catalyst and the filter. It will be appreciated that this arrangement is disclosed in WO 99 / 39809.
[0088] In some embodiments, the catalyst composition for use in the present invention is coated on a filter located downstream of the oxidation catalyst. If the filter contains the catalyst composition for use in the present invention, the metering point for the nitrogenous reductant is preferably located between the oxidation catalyst and the filter.
[0089] In some embodiments, the system configuration may include a selective catalytic reduction filter followed by a NOx adsorption catalyst, e.g., a vanadium SCR catalyst. In some embodiments, the system configuration includes a first SCR followed by a second SCR. In some embodiments, the system configuration includes a selective catalytic reduction filter followed by an SCR. In some embodiments, the catalyst configuration includes an SCR followed by an ammonia oxidation catalyst. Where suitable, such catalysts may be included as different coatings on the same substrate. In some embodiments, the SCR catalyst may include a vanadium SCR catalyst.
[0090] In some aspects, a lean-burn engine for a vehicle is provided that includes an exhaust system according to the present invention.
[0091] In some aspects, the vehicle lean-burn internal combustion engine may be a diesel engine, a lean-burn gasoline engine, or an engine powered by liquid petroleum gas or natural gas.
[0092] Zoning and Configuration In some embodiments, the vanadium SCR catalyst may be combined with one or more additional catalyst compositions, which may involve zoned and / or layered configurations on one or more substrates.
[0093] In some aspects, the vanadium SCR catalyst can be combined with additional catalyst compositions formulated as SCR catalysts and / or oxidation catalysts, such as ammonia oxidation catalysts. In some embodiments, the vanadium SCR catalyst can be combined with one or more additional SCR catalysts. In some embodiments, the vanadium SCR catalyst and the additional SCR catalyst can be located on the same substrate. In some embodiments, the vanadium SCR catalyst and the additional SCR catalyst can be located on different substrates. In some embodiments, the catalyst configuration can include a vanadium SCR catalyst with one or more additional SCR catalysts on the same substrate and one or more additional SCR catalysts on a separate substrate.
[0094] In some embodiments, the vanadium SCR catalyst can be zoned before another SCR catalyst, such as a Cu-zeolite or Fe-zeolite SCR catalyst. In some embodiments, the vanadium SCR catalyst can be zoned before an ammonia slip catalyst (ASC), which can be one or two layers. In some embodiments, the ASC can be a single layer catalyst and can include only oxidation functionality, or mixed oxidation and SCR functionality (e.g., Pt on an oxide support, and Cu-zeolite). In some embodiments, the ASC can be a two-layer catalyst and can include oxidation functionality in only the bottom layer or both layers, and SCR functionality in only the top layer or both layers. In some embodiments, the vanadium SCR catalyst can overlap the rear zone in each of the previous configurations. In some embodiments, the vanadium SCR catalyst can be zoned before the ASC / DOC hybrid brick, i.e., the ASC with higher DOC functionality (e.g., no oxidation), such as by higher PGM loading.
[0095] term In this disclosure, the singular forms "a," "an," and "the" include plural references unless expressly stated otherwise, and a reference to a particular numerical value includes at least that particular value. Thus, for example, a reference to a "material" is a reference to at least one of such materials and equivalents thereof known to those skilled in the art.
[0096] When values are expressed as approximations by using the descriptor "about", it will be understood that the particular value forms another embodiment. In general, the use of the term "about" indicates an approximation that may vary depending on the desired properties sought to be obtained by the disclosed subject matter and should be interpreted in the particular context in which it is used based on its function. Those skilled in the art will be able to interpret this as they do routinely. In some cases, the number of significant figures used for a particular value may be one non-limiting way of determining the scope of the word "about". In other cases, the gradations used in a series of values can be used to determine the intended range available to the term "about" for each value. When present, all ranges are inclusive and combinable. That is, reference to values stated in a range includes every value within that range.
[0097] For clarity, it should be understood that certain features of the invention described herein in the context of separate embodiments may also be provided in combination in a single embodiment. That is, unless expressly incompatible or specifically excluded, each individual embodiment is considered to be combinable with any other embodiment, and such combination is considered to be another embodiment. Conversely, for brevity, various features of the invention that are described in the context of a single embodiment may also be provided individually or in any subcombination. Finally, while an embodiment may be described as part of a series of steps or as part of a more general structure, each step may also be considered to be an independent embodiment in itself and combinable with other steps.
[0098] The transitional terms "comprising," "consisting essentially of," and "consisting" are intended to include their generally accepted meanings in patent terminology, i.e., (i) "comprising" is synonymous with "including," "containing," or "characterized by," and is inclusive or open-ended and does not exclude additional, unrecited elements or method steps; (ii) "consisting of" excludes any element, step, or ingredient not specified in the claim; and (iii) "consisting essentially of" limits the scope of the claim to those materials or steps specified and which do not "materially affect the basic and novel characteristics" of the claimed invention. Embodiments described with the term "comprising" (or its equivalent) also provide, as embodiments, embodiments described independently with the terms "consisting of" and "consisting essentially of." In those embodiments provided with the term "consisting essentially of," the fundamental and novel property is the ability of the system to efficiently combust fuel without the need for a separate ignition device or the need to heat the fuel mixture above ignition temperatures prior to introduction to the catalyst. Any materials or processes that do not impair such operability are considered within the scope of such embodiments.
[0099] When lists are presented, unless otherwise stated, it is to be understood that each individual member of that list, and every combination of that list, is a separate embodiment. For example, a list of embodiments presented as "A, B, or C" should be interpreted as including the embodiments "A," "B," "C," "A or B," "A or C," "B or C," or "A, B, or C."
[0100] Throughout this specification, words should be given their ordinary meaning as understood by those of ordinary skill in the relevant art. However, to avoid any doubt, the meaning of certain terms will be specifically defined or clarified.
[0101] "Optional" or "optionally" means that the subsequently described circumstance may or may not occur. Thus, the description includes instances where the circumstance occurs and instances where it does not occur. Similarly, embodiments that refer to an ingredient or step as "optionally present" include separate and independent embodiments in which the step or ingredient is or is not present. The term "optional" allows for the optional condition to occur, but does not require it. EXAMPLES
[0102] Example 1: Catalysts prepared with vanadyl oxalate and iron vanadate Catalysts were prepared having the following formulations, including a weight ratio of V from vanadyl oxalate and V from FeVO4 of 50:50: 55g / ft of element V 3 Vanadyl oxalate 55g / ft of element V 3 FeVO4 3.21g / in 3 5wt% WO3 / 5wt% SiO2 / TiO2 0.8g / in 3 Colloidal silica sol at Xanthan gum at 0.2-0.3 wt% of the wet washcoat mass 150g / ft of element W 3 Ammonium metatungstate at Ammonium hydroxide (to adjust pH to 8-9) Total loading of calcined washcoat = 4.28 g / in 3 Total vanadium loading (expressed as V2O5wt% of V2O5+TiO2) = 3.78wt%
[0103] It should be noted again that throughout this specification, TiO2 in this calculation refers to the TiO2 content, not the loading of doped TiO2 in the formulation.
[0104] Catalysts with weight ratios of V from vanadium oxalate and V from FeVO4 of 100:0 and 0:100 were also prepared.
[0105] 100:0 formulation 110g / ft of element V 3 Vanadium oxalate 3.21g / in 3 5wt% WO3 / 5wt% SiO2 / TiO2 0.8g / in 3 Colloidal silica sol at Xanthan gum at 0.2-0.3 wt% of the wet washcoat mass 150g / ft of element W 3 Ammonium metatungstate at Ammonium hydroxide (to adjust pH to 8-9) Total loading of calcined washcoat = 4.23 g / in 3
[0106] 0:100 Mixture 110g / ft of element V 3 FeVO4 3.21g / in 3 5wt% WO3 / 5wt% SiO2 / TiO2 0.8g / in 3 Colloidal silica sol at Xanthan gum at 0.2-0.3 wt% of the wet washcoat mass 150g / ft of element W 3 Ammonium metatungstate at Ammonium hydroxide (to adjust pH to 8-9) Total loading of calcined washcoat = 4.33 g / in 3
[0107] Example 2: Stability against aging Next, 110g / ft 3 The catalyst of Example 1 having an elemental V loading of 1.05 was tested for NOx conversion at 60k SV, 500 ppm NO, ANR 1.05, 225° C. and 500° C. The catalyst was tested fresh and after aging at 580° C. for 100 hours. The results are shown in FIG.
[0108] The results show that catalysts prepared with a blend of vanadyl oxalate and iron vanadate have improved stability against aging at low temperatures.
[0109] Example 3: V loading 110 g / ft with 3.78 wt% V2O5 of total V2O5+TiO2 3 A 50:50 catalyst from Example 1 was prepared with a vanadium loading of 10 ...
[0110] The results are shown in Figure 2. Using a blend of iron vanadate and vanadium oxalate (nominal 3.78 wt% V2O5 as a % of V2O5+TiO2) as in Example 1, both fresh and aged performance can be improved through increased vanadium loading, which results in better performance and improved stability.
[0111] Example 4: Vox:FeVO4 The samples were prepared as follows. 0.85g / in 3 Colloidal titania sol at 3.65g / in 3 5wt% WO3 / 5wt% SiO2 / TiO2 Vanadium oxalate + FeVO4 with total V loading and ratio as listed in Table 1 300g / ft of element W 3 Ammonium metatungstate at 0.3g / in 3 Colloidal silica sol at 5wt% urea in wet washcoat mass 0.25 wt% xanthan gum of the wet washcoat mass
[0112] [Table 1]
[0113] The formulations were coated onto cordierite substrates and tested fresh and after aging at 580°C / 100 hours. Total loading of fired washcoat = 5.3 g / in 3 Each was tested under the following conditions: 60KSV NO500ppm NH3 525ppm CO28% O2 10% CO 0.035% 5% H2O N2 Balance
[0114] The catalysts were then tested for NOx conversion at 60k SV, 500 ppm NO, ANR 1.05, 225° C. and 500° C. The catalysts were tested fresh and after aging at 580° C. for 100 hours.
[0115] The results are shown in Figures 3 and 4. The 2:1 ratio catalyst (Formulation 2) had a higher total V loading and showed higher NOx conversion at low temperatures, indicating that the blend of vanadyl oxalate and iron vanadate allows for a higher total vanadium loading to be achieved.
[0116] Example 5 - FeVO4 Inclusion The catalysts were prepared according to the following formulation: 0.85g / in 3 Colloidal titania sol at 3.65g / in 3 5wt% WO3 / 5wt% SiO2 / TiO2 Vanadium oxalate + FeVO4 with total V loading and ratio as listed in Table 2 300g / ft of element W 3 Ammonium metatungstate at 0.3g / in 3 Colloidal silica sol at 5wt% urea in wet washcoat mass 0.25 wt% xanthan gum of the wet washcoat mass
[0117] [Table 2] * Same formulation as formulation 2 in Example 4
[0118] The catalysts were then tested for NOx conversion at 60k SV, 500 ppm NO, ANR 1.05, 225° C. and 500° C. The catalysts were tested fresh and after aging at 580° C. for 100 hours.
[0119] The results are shown in Figure 5 and indicate that catalysts prepared with a blend of vanadyl oxalate and iron vanadate have improved stability against aging at low temperatures. The catalyst containing only vanadium oxalate (formulation 3) shows severe deactivation.
[0120] The washcoat-monolith interface of the catalyst according to Example 5 was analyzed by FIB / STEM / EELS techniques, as shown in FIG. 6. Region A identifies TiO2 from standard micro-sized titania, region B identifies TiO2 from colloidal titania, and region C identifies the substrate. TiO2 from standard micro-sized titania in region (A) and TiO2 from colloidal titania in region (B) can be clearly distinguished by Ti EDX, indicating that TiO2 from colloidal titania behaves as a binder binding standard micro-sized titania to the substrate. Vanadium and tungsten are found in both regions A and B, indicating that TiO2 from colloidal titania acts as a support for the active components. FIG. 6A is a TEM image, and FIG. 6B, 6C, and 6D are EDX mappings.
[0121] Example 6 - FeVO4 only, Vox only and blend Catalysts were prepared with vanadium from vanadyl oxalate only, vanadium from FeVO4 only, and vanadium from a blend of vanadyl oxalate and FeVO4. Such catalysts were prepared using colloidal silica sol only. Multiple catalysts of each type were prepared with various total vanadium loadings (expressed as V2O5 wt% of total V2O5 + TiO2).
[0122] The catalyst includes the following: 3.21g / in 3 5wt% WO3 / 5wt% SiO2 / TiO2 0.8g / in 3 Colloidal silica sol at Xanthan gum at 0.2-0.3 wt% of the wet washcoat mass 150g / ft of element W 3 Ammonium metatungstate at Ammonium hydroxide (to adjust pH to 8-9)
[0123] Various V sources and loadings, i.e. total WCL, are used.
[0124] The catalysts were then tested for NOx conversion at 60k SV, 500ppm NO, ANR 1.05, 225°C and 500°C. The catalysts were tested in the fresh state and after aging at 580°C for 100 hours. The results are shown in Figure 7. The results show that for vanadyl oxalate only formulations, the fresh to aged delta drops by at least about 10% for all loadings evaluated, from 1.93 to 4.77% V2O5 as % of V2O5+TiO2, and further increases significantly at loadings above 4.11%. The FeVO4 only formulations show high activation and fresh to aged delta. By blending vanadyl oxalate with FeVO4, a low fresh to aged delta is achieved by optimizing the combined deactivation and activation behavior of vanadyl oxalate and FeVO4. The fresh to aged delta for this vanadium source blend is lower than that of the single vanadium source at all data points (3.78-6.05% V2O5 as % of V2O5+TiO2) and remains within + / - 10%. Furthermore, when further extrapolated down to about 2% V2O5 and lower loadings as % of V2O5+TiO2, it is clear from the trends that the blend provides the same advantage in reducing the fresh to aged delta and constitutes an embodiment of the present invention.
[0125] Example 7: Titania ratio The catalyst samples were prepared as follows. Colloidal titania sol loading according to table - 5wt% WO3 / 5wt% SiO2 / TiO2 loading according to table 125g / ft of element V 3 Vanadium oxalate in 62g / ft of element V 3 FeVO4 in 300g / ft of element W 3 Ammonium metatungstate at 0.3g / in 3 Colloidal silica sol at 5% urea by weight of wet washcoat 0.25 wt% xanthan gum based on wet washcoat weight
[0126] [Table 3]
[0127] The catalyst was then tested for NOx conversion at 60k SV, 500 ppm NO, ANR 1.05, and 225°C. The catalyst was tested in the fresh state and after aging at 580°C for 100 hours. The results are shown in Figure 8. The results show that using colloidal titania blends provides benefits in the range of titania weight ratios from about 0.11 to about 0.25. The linear trend from 0.05 to 0.18 supports reaching a fresh to aged delta of 10% at a titania weight ratio of 0.08.
[0128] Example 8: FeVO4 inclusion in antimony promoted catalyst The catalyst samples were prepared as follows. 3.8g / in3 undoped TiO2 Vanadium oxalate loading according to the table below FeVO4 loading according to the table below 460g / ft of elemental Sb 3 Antimony pentoxide in 1.0g / in 3 Colloidal silica sol at 5% urea by weight of wet washcoat 0.25 wt% xanthan gum based on wet washcoat weight
[0129] [Table 4]
[0130] The catalyst was then tested for NOx conversion at 60k SV, 500 ppm NO, ANR 1.05, 225°C and 500°C. The catalyst was tested in the fresh state and after aging at 580°C for 100 hours. The results are shown in Figure 9. The results show that replacing some of the vanadium oxalate with iron vanadate has a clear advantage in aging durability and fresh to aged delta, even in an antimony promoted system.
Claims
1. A selective catalytic reduction catalyst comprising vanadium, iron and titania, 2 O 5 + TiO 2 V 2 O 5 Vanadium in an amount of up to 7 wt. % by weight, Fe x M y V.O. 4 wherein x=0.2 to 1, y=1-x, and if y>0, M comprises one or more non-Fe metals, said metal vanadate being present in an amount of 20% to 75% of the total amount of vanadium in said selective catalytic reduction catalyst; The selective catalytic reduction catalyst comprises titania in an amount of 60 wt % to 93 wt %; The titania comprises a blend of colloidal titania and standard microsized titania. Selective catalytic reduction catalyst.
2. 2. The selective catalytic reduction catalyst of claim 1, wherein, when y>0, M comprises Er, Al, Ce, or a combination thereof.
3. The metal vanadate is FeVO 4 , Fe 0.5 C.E. 0.5 V.O. 4 , Fe 0.33 A 0.33 Er 0.33 V.O. 4 3. The selective catalytic reduction catalyst according to claim 1 or 2, comprising:
4. The selective catalytic reduction catalyst according to any one of claims 1 to 3, wherein the vanadium is present on a support comprising titania.
5. The vanadium is V 2 O 5 + TiO 2 V 2 O 5 The selective catalytic reduction catalyst according to any one of claims 1 to 4, which is present in an amount, as wt%, from 2 wt% to 7 wt%.
6. 2. The selective catalytic reduction catalyst of claim 1, wherein the catalyst is prepared using a vanadium oxide precursor and a metal vanadate, the vanadium oxide precursor and the metal vanadate being included in a weight ratio expressed as a ratio of elemental vanadium of 6:1 to 1:
2.
7. 2. The selective catalytic reduction catalyst of claim 1, wherein said colloidal titania and said standard micro-sized titania are present in a weight ratio of 0.08 to 0.
4.
8. The selective catalytic reduction catalyst according to any one of claims 1 to 7, wherein the catalyst further comprises tungsten.
9. 9. The selective catalytic reduction catalyst of claim 8, comprising tungsten in addition to the tungsten doped in the titania.
10. The selective catalytic reduction catalyst according to claim 8, wherein the weight ratio of W:Ti in the catalyst is 0.025 to 0.
2.
11. The selective catalytic reduction catalyst according to any one of claims 1 to 10, wherein the catalyst further comprises antimony.
12. 12. The selective catalytic reduction catalyst of claim 11, comprising antimony in addition to the antimony doped in the titania.
13. The selective catalytic reduction catalyst according to claim 11, wherein the weight ratio of Sb:Ti in the catalyst is 0.025 to 0.2.
Citation Information
Patent Citations
Preparation method for titanium dioxide group catalyst carrier
CN101513620A
Catalyst composition for selective catalytic reduction of exhaust gases
JP2012524646A
Catalyst composition for selective catalytic reduction of exhaust gases
JP2013523445A
V / TiW catalyst activated by zeolite