Method for producing zirconia sintered body
The method addresses the challenge of rapid zirconia sintering without deformation by controlling heating rates and temperatures, enabling efficient production of large dental prostheses with minimal deformation and composition limitations.
Patent Information
- Application Number
- JP2021565697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-12-18
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Conventional methods for manufacturing zirconia dental prostheses face challenges in achieving short firing times without causing deformation, especially for large-shaped prostheses, and are limited in composition flexibility.
A method involving a controlled heating process with specific temperature adjustments and heating rates to ensure consistent shrinkage rates across temperature sections, allowing for rapid sintering of zirconia bodies while minimizing deformation.
Enables the production of zirconia sintered bodies in under 2 hours, suppressing deformation and maintaining composition flexibility, suitable for large dental prostheses with improved model compatibility.
Smart Images

Figure 0007556889000012 
Figure 0007556889000011 
Figure 0007556889000013
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a zirconia sintered body. [Background technology]
[0002] Traditionally, metals have been widely used as dental products (for example, typical prosthetics such as veneers, dental crowns, crowns, and dental implants, as well as orthodontic products and dental implant products). However, metals have the drawback of being clearly different in color from natural teeth and lacking in aesthetics, and metal elution can cause allergies. Therefore, in order to solve the problems associated with the use of metals, ceramic materials such as aluminum oxide (alumina) and zirconium oxide (zirconia) have been used in dental products as alternative materials to metals. In particular, zirconia is strong and relatively aesthetically pleasing, and demand for it has been increasing, especially in recent years as prices have fallen.
[0003] On the other hand, in order to manufacture a dental prosthesis using zirconia, a block or disk-shaped workpiece for cutting (a workpiece to be cut) is pre-sintered at a temperature 400°C to 700°C lower than the temperature at which an ideal sintered body is obtained, and then the shape of the dental prosthesis is cut out using CAD / CAM equipment. The cut-out unsintered zirconia workpiece is then held at a maximum temperature of 1400°C to 1650°C and sintered. This usually requires a total time of 6 to 12 hours for heating, holding, and cooling. In recent years, there has been an increasing demand for short-time firing at dental clinics, and firing furnaces that enable short-time firing as described in Patent Document 1 have also been manufactured. However, there is a problem in that deformation and distortion are observed when a large-shaped prosthesis is manufactured during short-time firing.
[0004] Patent Document 2 is a document relating to a multilayer oxide ceramic body, in particular a pre-sintered multilayer oxide ceramic blank and an oxide ceramic green body suitable for dental applications, and relates to a coefficient of distortion (d=(HV max -HV MIN ) / HV AVEA pre-sintered multilayer oxide ceramic blank with a porosity of less than 0.4 has been described. This makes it possible to suppress deformation of the prosthesis, but the composition is limited, and even with this composition, there is a problem that deformation occurs in large prostheses (approximately twice the length of the 3 to 4 cm described in the examples). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2015-531048 [Patent Document 2] Special Publication No. 2016-527017 Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, an object of the present invention is to provide a method for producing a zirconia sintered body that can be fired in a short period of time, has no composition restrictions, and can suppress deformation even in the case of a large-sized prosthesis. [Means for solving the problem]
[0007] As a result of intensive research into solving the above problems, the inventors have found that the above problems can be solved by creating a short firing schedule by adjusting the heating rate to a specific rate. Based on this finding, the inventors have conducted further research and have completed the present invention.
[0008] That is, the present invention includes the following inventions. [1] A heating step of heating a zirconia compact or a zirconia calcined body, The heating step includes a temperature increasing step, In the heating step, the heating rate is adjusted in a temperature range from the temperature at which the shrinkage of zirconia starts to the temperature at which the shrinkage ends, A method for producing a zirconia sintered body, in which, when the temperature region is equally divided into a plurality of sections having specific temperature widths, the rate of shrinkage of a zirconia molded body or a zirconia calcined body during heating in each section is substantially constant. [2] The method for producing a zirconia sintered body according to [1], wherein the temperature range of each of the sections is 50°C. [3] The method for producing a zirconia sintered body according to [1] or [2], wherein the heating rate in each section is set within a range of 0.1 to 1.0 times the allowable heating rate in each section, calculated by the following formula (1), and the heating rate in each section is substantially the same magnification as the allowable heating rate in each section. (Allowable heating rate in each section) = (Maximum heating rate of the kiln) / (Shrinkage coefficient in each section) ... (1) (In formula (1), the contraction coefficient for each section is expressed by the following formula (2).) (Shrinkage coefficient in each section) = (Shrinkage difference in each section) / (Temperature range / 100) ... (2) (However, if the contraction coefficient for each section calculated based on formula (2) is less than 1, the contraction coefficient for each section shall be set to 1 and formula (1) shall be calculated.) [4] The method for producing a zirconia sintered body according to any one of [1] to [3], wherein the temperature range is in the range of 1050 to 1400°C. [5] The method for producing a zirconia sintered body according to any one of [1] to [4], wherein a total firing time from the start of heating in the heating step to the end of the retention time at the maximum firing temperature in the heating step is 120 minutes or less. [6] The method for producing a zirconia sintered body according to any one of [1] to [5], wherein the heating step further includes, following the temperature-raising step, a retention step of maintaining the maximum firing temperature in the temperature-raising step. [7] The method for producing a zirconia sintered body according to any one of [1] to [6], wherein the zirconia sintered body is for dental use. Effect of the Invention
[0009] According to the present invention, a method for producing a zirconia sintered body can be provided that can be fired in a short time, has no composition restrictions, and can suppress deformation even in the case of a prosthesis with a large shape. Therefore, it is possible to reduce the time required for correction due to deformation that has conventionally occurred at the user (dental laboratory or dental clinic), and it is possible to shorten the total time required for the user to manufacture a prosthesis. In addition, according to the method for producing a zirconia sintered body of the present invention, a zirconia sintered body with high model compatibility can be produced. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram showing the shapes of the prostheses produced in Examples 1 to 3 and Comparative Examples 1 to 3. [Diagram 2] FIG. 2 is a diagram showing a model used for evaluating the model compatibility of the prostheses produced in Examples 1 to 3 and Comparative Examples 1 to 3. [Diagram 3] FIG. 2 is a diagram showing the firing schedules and evaluation results of the prostheses produced in Examples 1 to 3 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The method for producing a zirconia sintered body of the present invention includes a heating step of heating a zirconia molded body or a zirconia calcined body, the heating step includes a temperature increasing step, and when the temperature range in the temperature increasing step from the temperature at which the contraction of zirconia starts to the temperature at which the contraction ends is equally divided into a plurality of sections having specific temperature widths by adjusting the heating rate, it is important that the rate of contraction of the zirconia molded body or the zirconia calcined body during heating in each section is substantially constant. Hereinafter, the present invention will be described in detail.
[0012] In the temperature-raising step of the present invention, for example, the zirconia molded body or the zirconia calcined body is heated in a firing furnace that has been preheated to room temperature or higher or to a temperature higher than room temperature and not higher than 500° C. The zirconia molded body or the zirconia calcined body before firing is preferably one having a predetermined shape of a dental product. Examples of dental products include typical dental prostheses such as veneers, dental crowns, crowns, and dental implants; orthodontic products; and dental implant products. The zirconia molded body or the zirconia calcined body before heating may be processed using a dental CAD / CAM device, or may be prepared by a dental technician through cutting or the like.
[0013] The zirconia molded body or the zirconia calcined body before heating may be placed directly on a muffle member of a firing furnace during firing, or may be placed in the furnace using a tray, base, or pin made of ceramic or a high-melting point metal, or may be placed using ceramic beads.
[0014] The starting temperature of the temperature-raising step is from room temperature to 500° C., preferably from room temperature to 400° C., more preferably from room temperature to 300° C., and further preferably from room temperature to 200° C. The rate of temperature rise before the start of the temperature-raising step is not particularly limited as long as the starting temperature of the temperature-raising step can be raised to the above-mentioned temperature range.
[0015] The firing furnace used in the firing of the present invention is an atmospheric furnace, and may be a box furnace, a crucible furnace, a tubular furnace, a hearth lifting furnace, a continuous furnace, or a rotary kiln, or may be a resistance heating furnace, an induction heating furnace, a direct current type electric furnace, an IH furnace, a high frequency furnace, or a microwave furnace, and may be a metal heating element, silicon carbide, molybdenum disilicide, lanthanum chromium yarn, molybdenum, carbon, tungsten, or the like, and may be used as a heating element susceptor using SiC. A firing furnace that combines any two or more of these may also be used. In addition, the smaller the volume of the firing chamber having a pedestal on which a zirconia molded body or zirconia calcined body having a predetermined shape such as a dental crown is placed, the better the thermal efficiency and the easier it is to maintain the heat amount in the furnace during firing.
[0016] In the present invention, the temperature range from the temperature at which the shrinkage of zirconia starts (hereinafter also referred to as the "shrinkage start temperature") to the temperature at which the shrinkage ends (hereinafter also referred to as the "shrinkage end temperature") (hereinafter also referred to as the "shrinkage temperature range") can be determined by the following method. The shrinkage start temperature refers to the lowest firing temperature at which the shrinkage rate exceeds 0% when a rectangular sample block of unsintered zirconia measuring 1 cm x 2 cm x 1 cm is prepared and the sample block is fired in the firing furnace at a firing temperature higher than the starting temperature of the temperature rise step for a specific time (for example, 10 minutes). The method for measuring the shrinkage rate will be described later. The shrinkage end temperature refers to the lowest temperature at which the difference between the shrinkage rate (%) at firing temperature T°C and the shrinkage rate (%) at firing temperature T+50°C is 0% when the temperature width of each section of the shrinkage temperature range is 50°C. The temperature range varies depending on the content of the stabilizer described below, and may be, for example, 1000 to 1600°C, 1000 to 1500°C, or 1050 to 1400°C.
[0017] In the present invention, the shrinkage rate at a specific firing temperature can be determined by the following method: A rectangular parallelepiped sample block of unsintered zirconia measuring 1 cm x 2 cm x 1 cm is prepared, the length of the sample block in the x-axis direction after firing at a specific firing temperature is measured (n=3), the shrinkage rate in the x-axis direction is calculated using the following formula (%), and the average of the calculation results is regarded as the shrinkage rate in the x-axis direction. (x-axis shrinkage rate (%)) = [(x-axis length before firing) - (x-axis length after firing)] x 100 / (x-axis length before firing) Similarly, the shrinkage rates in the y-axis and z-axis directions are calculated, and the average of the three shrinkage rates is taken as the "shrinkage rate (%)" at that firing temperature.
[0018] The method for adjusting the heating rate in the present invention is not particularly limited as long as the rate of shrinkage of the zirconia molded body or the zirconia calcined body during heating in each of the above-mentioned sections is substantially constant. As a specific example of a preferred embodiment, the heating rate in each section may be determined by a method consisting of the following Steps 1 to 5.
[0019] Step 1: Divide the temperature range from the start of shrinkage to the end of shrinkage into multiple sections with a specific temperature range, and measure the shrinkage rate when firing at the firing temperature at the boundary of each section (temperature range). However, the retention time at each temperature is constant. Step 2: From the shrinkage rate at the firing temperature at the boundary of each section obtained in Step 1, calculate the difference in shrinkage rate between the start temperature and the end temperature of each section, and use this as the "shrinkage rate difference in each section." Step 3: Calculate the contraction coefficient for each section using the following formula. (Shrinkage coefficient in each section) = (Shrinkage difference in each section) / (Temperature range / 100) ... (2) (However, if the contraction coefficient for each section calculated based on formula (2) is less than 1, the contraction coefficient for each section shall be set to 1.) Step 4: Calculate the allowable temperature rise rate for each section using the following formula. (Allowable heating rate in each section) = (Maximum heating rate of the kiln) / (Shrinkage coefficient in each section) ... (1) Step 5: The heating rate in each section is set within a range of 0.1 to 1.0 times the allowable heating rate in each section. The heating rate in each section is set at substantially the same rate as the allowable heating rate in each section.
[0020] It is preferable to include a step of determining a temperature range from a shrinkage start temperature to a shrinkage end temperature prior to the step 1. The temperature range can be determined by firing a sample block of unsintered zirconia using a firing furnace and measuring the shrinkage rate, thereby measuring the shrinkage start temperature and the shrinkage end temperature, as described above.
[0021] In Step 1, the specific intervals (temperature widths) into which the temperature is evenly divided can be set appropriately depending on the accuracy of the desired deformation suppression, and may be, for example, a temperature width of 100° C., preferably a temperature width of 50° C., and more preferably a temperature width of 20° C. The number of evenly divided intervals can be set appropriately depending on the accuracy of the desired deformation suppression, and may be, for example, 4 or more, or 5 or more.
[0022] In Step 3, when the contraction coefficient in each section calculated based on formula (2) is less than 1, it is necessary to set the contraction coefficient in each section to 1 in order to make the rate of contraction of the zirconia molded body or the zirconia calcined body during heating in each section of the contraction temperature range in the heating step substantially constant and to determine an appropriate allowable heating rate for suppressing deformation due to shrinkage. Also, in formula (2), for example, when the temperature range is 50°C, "50" is substituted for "temperature range," and when the difference in contraction rate in a certain section is 1.5%, "1.5" is substituted for "difference in contraction rate in each section."
[0023] The allowable heating rate in each section calculated in Step 4 is a value represented by formula (1), and serves as a standard for an allowable heating rate in order to keep the rate of shrinkage of the zirconia molded body or the zirconia calcined body during heating in each section of the shrinkage temperature range in the heating step substantially constant and to suppress deformation due to shrinkage. The maximum heating rate of the sintering furnace is not particularly limited as long as it is within a range that can be set based on the performance of the sintering furnace, and may be set appropriately to any value within a range of about 30°C / min to 200°C / min, for example, or may be set appropriately to any value within a range of about 50°C / min to 120°C / min.
[0024] In the above Step 5, if the heating rate in each section exceeds 1.0 times the allowable heating rate in each section, deformation may not be sufficiently suppressed. In the above Step 5, if the heating rate in each section is less than 0.1 times the allowable heating rate in each section, firing may not be possible in a short time. In the above Step 5, from the viewpoint of suppressing deformation and firing in a shorter time, it is preferable to set the heating rate in each section within a range of 0.2 to 1.0 times the allowable heating rate, more preferably within a range of 0.5 to 1.0 times, and even more preferably within a range of 0.8 to 1.0 times. In addition, in order to make the rate of contraction of the zirconia molded body or the zirconia calcined body during heating in each section substantially constant, it is preferable to set the heating rate to a uniform predetermined ratio of the allowable heating rate in all sections (for example, set the heating rate in all sections to 1.0 times the allowable heating rate in each section). In other words, it is preferable to set the heating rate in each section to a substantially identical ratio to the allowable heating rate in each section. By "substantially identical," it is preferable that the difference between the heating rate ratio to the allowable heating rate in one section and the heating rate ratio to the allowable heating rate in another section is less than 10%, more preferably 6% or less, and even more preferably 5% or less. From the viewpoint of controlling the rate of contraction of the zirconia molded body or the zirconia calcined body during heating in each section, it is more preferable to set the heating rate in each section to a substantially identical ratio to the allowable heating rate.
[0025] By determining the heating rate for each section using the method consisting of Steps 1 to 5 and adjusting the heating rate, the heating rate can be made slower in the temperature section where shrinkage is large and faster in the temperature section where shrinkage is small. As a result, in the temperature range from the shrinkage start temperature to the shrinkage end temperature, the rate of shrinkage of the zirconia molded body or the zirconia calcined body during heating in each section becomes substantially constant. This eliminates the uneven heating state that occurs when firing a prosthesis with a large shape (a large dental prosthesis with three or more bridges such as a long span bridge), and the firing shrinkage of the prosthesis progresses uniformly in every part. In the present invention, the "rate of shrinkage during heating in each section" can be calculated using the following formula. (Percentage of shrinkage during heating in each section) = {(dimension at start temperature of section) - (dimension at end temperature of section)} / (dimension at start temperature of section) In the above formula, the percentage of shrinkage during heating is calculated for each of the dimensional changes in the x-axis, y-axis, and z-axis, and the average of the obtained percentages in the three directions is the percentage of shrinkage during heating in that section. Furthermore, "the percentage of shrinkage of the zirconia molded body or the zirconia calcined body during heating in each section is substantially constant" means that the percentage of shrinkage during heating calculated in each section falls within the range of 0.8 to 1.2 times the average value.
[0026] In the present invention, the heating rate in the heating step to the shrinkage start temperature is, for example, 50° C. / min or more, and from the viewpoint of further shortening the working time, is preferably 60° C. / min or more, more preferably 70° C. / min or more, and even more preferably 80° C. / min or more. The heating rate is 500° C. / min or less, preferably 450° C. / min or less, more preferably 400° C. / min or more, and even more preferably 350° C. / min or less. If the heating rate exceeds 500° C. / min, there is a risk of inducing the occurrence of fractures or cracks during firing. If the zirconia molded body or the zirconia calcined body contains moisture or color liquid used during processing, the heating step may be started after a drying step at 300° C. or less for 1 minute to 20 minutes, preferably 5 minutes to 15 minutes.
[0027] The zirconia molded body or zirconia calcined body used in the method for producing a zirconia sintered body of the present invention preferably contains, in addition to zirconia, a stabilizer capable of suppressing the phase transition of zirconia. As the zirconia molded body or zirconia calcined body, a zirconia molded body or zirconia calcined body in which at least a part of the stabilizer is not solid-dissolved in zirconia is preferable. The stabilizer is preferably capable of forming partially stabilized zirconia.
[0028] Examples of the stabilizer include calcium oxide (CaO), magnesium oxide (MgO), yttria, cerium oxide (CeO2), scandium oxide (Sc2O3), niobium oxide (Nb2O5), lanthanum oxide (La2O3), erbium oxide (Er2O3), and praseodymium oxide (Pr6O 11Examples of the stabilizer include oxides such as samarium oxide (Sm2O3), europium oxide (Eu2O3) and thulium oxide (Tm2O3). The stabilizer may be used alone or in combination of two or more. The content of the stabilizer in the zirconia calcined body and sintered body thereof of the present invention can be measured, for example, by inductively coupled plasma (ICP) emission spectrometry, fluorescent X-ray analysis, etc. In the zirconia calcined body and sintered body thereof of the present invention, the content of the stabilizer is preferably 0.1 to 18 mol%, more preferably 1 to 15 mol%, and even more preferably 2 to 8 mol%, based on the total molar number of zirconia and the stabilizer. From the viewpoint of the strength and translucency of the obtained zirconia sintered body, the zirconia molded body or the zirconia calcined body preferably contains yttria as a stabilizer. The content of yttria is preferably 3.0 mol% or more, more preferably 3.5 mol% or more, even more preferably 3.8 mol% or more, and particularly preferably 4.0 mol% or more, based on the total mole number of zirconia and yttria. When the content of yttria is 3.0 mol% or more, the translucency of the zirconia sintered body can be increased. In addition, the content of yttria is preferably 7.5 mol% or less, more preferably 7.0 mol% or less, even more preferably 6.5 mol% or less, and particularly preferably 6.0 mol% or less, based on the total mole number of zirconia and yttria. When the content of yttria is 7.5 mol% or less, the strength reduction of the obtained zirconia sintered body can be suppressed.
[0029] In the zirconia compact or zirconia calcined body of the present invention, it is preferable that at least a part of the stabilizer is not dissolved in zirconia. The fact that a part of the stabilizer is not dissolved in zirconia can be confirmed, for example, by an XRD pattern. When a peak derived from the stabilizer is confirmed in the XRD pattern of the zirconia calcined body, the stabilizer that is not dissolved in zirconia is present in the zirconia compact or zirconia calcined body. When the entire amount of the stabilizer is dissolved in solid solution, basically, no peak derived from the stabilizer is confirmed in the XRD pattern. However, depending on conditions such as the crystal state of the stabilizer, even if there is no stabilizer peak in the XRD pattern, the stabilizer may not be dissolved in zirconia. When the main crystal system of zirconia is a tetragonal and / or cubic system and there is no stabilizer peak in the XRD pattern, it is considered that most of the stabilizer, basically all of it, is dissolved in zirconia. In the zirconia molded body or zirconia calcined body of the present invention, the stabilizer does not have to be entirely dissolved in zirconia. In the present invention, the stabilizer being dissolved in solid solution means, for example, that an element (atom) contained in the stabilizer is dissolved in solid solution in zirconia.
[0030] In the zirconia molded body or zirconia calcined body of the present invention, the abundance rate f of yttria that is not dissolved in zirconia (hereinafter sometimes referred to as "undissolved yttria") is y The fraction of undissolved yttria f can be calculated based on the formula (3) described below. y is preferably greater than 0%, more preferably 1% or more, even more preferably 2% or more, and particularly preferably 3% or more. y The upper limit of may be, for example, 15% or less, but preferably depends on the yttria content in the zirconia compact or the zirconia calcined body. When the yttria content is 3 mol% or more and less than 4.5 mol%, f y When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f yWhen the yttria content is 5.8 mol% or more and 7.5 mol% or less, f y may be 15% or less.
[0031] In the zirconia molded body or zirconia calcined body of the present invention, when the yttria content is 3 mol% or more and less than 4.5 mol%, y is preferably 0.5% or more, more preferably 1.0% or more, and even more preferably 2.0% or more. When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f y is preferably 1% or more, more preferably 2% or more, and even more preferably 3% or more. When the yttria content is 5.8 mol% or more and 7.5 mol% or less, f y is preferably 2% or more, more preferably 3% or more, and even more preferably 4% or more.
[0032]
number
[0033] In formula (3), I y (111) indicates the peak intensity of the (111) plane of yttria at around 2θ=29° in the XRD pattern using CuKα radiation. m (111) and I m (11-1) indicates the peak intensity of the (111) and (11-1) planes of the monoclinic crystal system of zirconia. t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal crystal system. I c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia.
[0034] The above formula (3) is I y By substituting other peaks in place of (111), this method can also be applied to calculate the undissolved fraction of stabilizers other than yttria.
[0035] The main crystal system of the zirconia in the zirconia molded body or zirconia calcined body of the present invention is preferably a monoclinic system. In the present invention, the term "main crystal system is a monoclinic system" means that the ratio f of the monoclinic system in the zirconia calculated by the formula (4) described later to the total amount of all crystal systems (monoclinic system, tetragonal system, and cubic system) in the zirconia is 1.0 to 1.0 times the ratio f m In the zirconia formed body or zirconia calcined body of the present invention, the monoclinic ratio f m is preferably 55% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 75% or more, particularly preferably 80% or more, even more particularly preferably 85% or more, and most preferably 90% or more, based on the total amount of monoclinic, tetragonal and cubic crystals. m can be calculated from the peak of the X-ray diffraction (XRD) pattern by CuKα radiation using the formula (4) described below. The main crystal system in the zirconia compact or calcined zirconia body may contribute to the increase in the shrinkage temperature and the shortening of the firing time.
[0036] In the zirconia formed body or zirconia calcined body of the present invention, the peaks of the tetragonal and cubic crystal systems may not be substantially detected. m can be set to 100%.
[0037]
number
[0038] In formula (4), I m (111) and I m (11-1) indicates the peak intensity of the (111) and (11-1) planes of the monoclinic crystal system of zirconia, respectively. t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal crystal system. I c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia.
[0039] In the zirconia molded body or zirconia calcined body of the present invention, when the yttria content is 3 mol% or more and less than 4.5 mol%, m / f y is preferably 20 to 200, more preferably 25 to 100, and further preferably 30 to 60. When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f m / f y is preferably 5 to 45, more preferably 10 to 40, and further preferably 15 to 35. When the content of yttria is 5.8 mol % or more and 7.5 mol % or less, f m / f y is preferably 2-40, more preferably 5-35, and further preferably 10-30.
[0040] The zirconia molded body or zirconia calcined body of the present invention may contain additives as necessary. Examples of additives include binders, colorants (including pigments and composite pigments), fluorescent agents, alumina (Al2O3), titanium oxide (TiO2), silica (SiO2), etc. The additives may be used alone or in combination of two or more.
[0041] Examples of the binder include polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, acrylic binders, wax-based binders (paraffin wax, etc.), polyvinyl butyral, polymethyl methacrylate, ethyl cellulose, polyethylene, polypropylene, ethylene-vinyl acetate copolymer, polystyrene, atactic polypropylene, methacrylic resin, and stearic acid.
[0042] Examples of the pigment include oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb and Er (specifically, NiO, Cr2O3, etc.), and oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd and Tb are preferred, and oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Sm, Eu, Gd and Tb are more preferred. In addition, the zirconia molded body or zirconia calcined body of the present invention may not contain erbium oxide (Er2O3). Examples of the composite pigment include composite oxides such as (Zr,V)O2, Fe(Fe,Cr)2O4, (Ni,Co,Fe)(Fe,Cr)2O4·ZrSiO4, (Co,Zn)Al2O4, etc. Examples of the fluorescent agent include Y2SiO5:Ce, Y2SiO5:Tb, (Y,Gd,Eu)BO3, Y2O3:Eu, YAG:Ce, ZnGa2O4:Zn, BaMgAl 10 O 17 :Eu, etc.
[0043] The method for producing the zirconia molded body used in the present invention is not particularly limited, but may be, for example, a method including a step of press-molding a mixed powder consisting of zirconia and the stabilizer at a pressure of 175 MPa or more to obtain a zirconia molded body. By press-molding at the pressure, the bulk density of the zirconia molded body (and thus the obtained zirconia sintered body) can be increased regardless of the thickness. In this specification, the pressure of 175 MPa or more means the maximum pressure during press molding.
[0044] The method for producing the zirconia calcined body used in the present invention is not particularly limited, and examples thereof include a method for firing (i.e., calcining) a zirconia molded body formed from a raw material powder containing zirconia particles and a stabilizer at a temperature at which the zirconia particles do not sinter. The zirconia molded body is as described above. An example of a method for producing the zirconia calcined body of the present invention will be described. First, a raw material powder for the zirconia molded body is produced. A mixture is prepared using monoclinic zirconia powder and a stabilizer powder (e.g., yttria powder) so as to have a desired stabilizer (e.g., yttria) content. Next, this mixture is added to water to prepare a slurry, which is wet-pulverized and mixed in a ball mill until the desired particle size is reached. The pulverized slurry is dried and granulated with a spray dryer. The obtained powder is fired at a temperature at which the zirconia particles do not sinter (e.g., 800 to 1200°C) to prepare a powder (primary powder). A pigment may be added to the primary powder. The primary powder is then added to water to prepare a slurry, which is then wet-pulverized and mixed in a ball mill until the desired particle size is reached. Additives such as binders are added to the pulverized slurry as necessary, and the slurry is then dried in a spray dryer to prepare a mixed powder (secondary powder). The secondary powder is filled into a specified mold, the upper surface is leveled off to make it flat, an upper mold is set, and the secondary powder is press-molded by a uniaxial press molding machine to obtain a zirconia molded body. As described above, the pressure for press-molding the mixed powder is preferably 175 MPa or more. The obtained zirconia molded body may or may not be further molded by CIP (Cold Isostatic Press).
[0045] The zirconia calcined body may have a multi-layer structure. When producing a zirconia calcined body having a multi-layer structure, the primary powder may be divided into at least two (preferably four) in the above-mentioned production method in order to give the zirconia molded body a multi-layer structure.
[0046] Next, the zirconia molded body obtained as described above is calcined to obtain a calcined zirconia body. The calcination temperature is, for example, preferably 800°C or higher, more preferably 900°C or higher, and even more preferably 950°C or higher. In order to improve dimensional accuracy, the calcination temperature is, for example, preferably 1200°C or lower, more preferably 1150°C or lower, and even more preferably 1100°C or lower. This is because it is believed that the dissolution of the stabilizer does not proceed at such a calcination temperature.
[0047] The zirconia calcined body used in the present invention may be a commercially available product. Examples of commercially available products include "Noritake Katana (registered trademark) Zirconia" (model numbers: Disk UTML, Disk STML, Disk ML, Disk HT, Disk LT) (all manufactured by Kuraray Noritake Dental Co., Ltd.). In the method for producing the zirconia sintered body of the present invention, it is preferable to use the commercially available zirconia calcined body by cutting it into a predetermined shape for a dental product.
[0048] In the method for producing a zirconia sintered body of the present invention, the heating rate in the heating step up to the shrinkage starting temperature may be a constant rate or may be changed midway to multiple stages, as long as the effects of the present invention are not impaired.
[0049] In the method for producing a zirconia sintered body of the present invention, after the shrinkage end temperature is reached, a step of further increasing the temperature (second heating step) may be included in order to obtain a zirconia sintered body having superior brightness, translucency and chroma, and to obtain a zirconia molded body or a zirconia calcined body having superior color development. The second heating step is distinguished from the heating step (first heating step) in that it is a heating step after the shrinkage of zirconia is completed. The heating rate is, for example, 10° C. / min or more, and from the viewpoint of further shortening the working time, it is preferably 11° C. / min or more, more preferably 12° C. / min or more, and even more preferably 13° C. / min or more. In addition, from the viewpoint of obtaining a zirconia sintered body having superior chroma and to obtain a zirconia molded body or a zirconia calcined body having superior color development, it is, for example, 299° C. / min or less, preferably 270° C. / min or less, more preferably 250° C. / min or less, and even more preferably 200° C. / min or less.
[0050] [Mooring process] In the method for producing a zirconia sintered body of the present invention, the heating step preferably includes a retention step of holding the maximum firing temperature in the temperature rise step following the temperature rise step, from the viewpoint of promoting the development of translucency due to grain growth. The retention time at the maximum firing temperature is preferably within 30 minutes, and is more preferably 1 to 30 minutes, and even more preferably 10 to 20 minutes, from the viewpoint of further shortening the working time and excellent strength of the obtained zirconia sintered body. In addition, the maximum firing temperature is preferably 1400 to 1650°C, and is more preferably 1450°C or higher, even more preferably 1500°C or higher, and particularly preferably 1520°C or higher, from the viewpoint of excellent brightness, translucency and chroma of the obtained zirconia sintered body and excellent color development of the composite oxide contained in the zirconia molded body or the zirconia calcined body. Furthermore, the maximum firing temperature is more preferably 1630°C or less, even more preferably 1620°C or less, and particularly preferably 1610°C or less, from the viewpoints of being able to further shorten the working time, of the resulting zirconia sintered body being superior in brightness, translucency and chroma, and of the color development property of the composite oxide contained in the zirconia molded body or the zirconia calcined body being superior.
[0051] In the method for producing a zirconia sintered body of the present invention, the total firing time from the start of the temperature increase in the temperature increase step to the end of the retention time at the maximum firing temperature is preferably within 100 minutes, more preferably within 80 minutes, and even more preferably within 50 minutes, in order to further shorten the working time. The lower limit of the firing time is not limited as long as it does not impair the effects of the present invention, but is usually 10 minutes or more.
[0052] [Cooling process] In the method for producing a zirconia sintered body of the present invention, it is preferable to include a step of cooling the zirconia sintered body after holding it at the maximum firing temperature for a predetermined time. In the cooling step, the temperature drop rate is preferably 40°C / min or more, more preferably 45°C / min or more, and even more preferably 50°C / min or more. The temperature drop method can be any one or a combination of cooling by introducing outside air, water cooling, air cooling, slow cooling, and natural cooling. The temperature reached in the cooling step varies depending on the type and performance of the firing furnace, and may be 1000°C, 900°C, or 800°C.
[0053] The color difference ΔE*ab of the zirconia sintered body obtained by the manufacturing method of the present invention is preferably 2.7 or less, more preferably 2.0 or less, even more preferably 1.6 or less, and particularly preferably 0.8 or less, since it is suitable as a dental product. The object of comparison and measurement of the color difference ΔE*ab is the chromaticity of the zirconia sintered body in the case of normal firing (total firing time: 6 to 12 hours). A known method can be used to evaluate the chromaticity. The color difference ΔE*ab is, for example, a color difference ΔE* (ΔE*ab) calculated by the following formula (5) for two samples of the zirconia sintered body (L1*, a1*, b1*) when normally fired and the zirconia sintered body (L2*, a2*, b2*) when fired for a short time (total firing time: 15 to 30 minutes) using the lightness index L* and color coordinates a* and b* in the CIE 1976 L*a*b* color space, measured using a dental color measuring device (Olympus Corporation, 7 band LED light source, "Crystal Eye"). ΔE*={(L1*-L2*) 2 +(a1*-a2*) 2 +(b1*-b2*) 2} 1 / 2 …(5)
[0054] The difference between the lightness index L* of the zirconia sintered body obtained by the manufacturing method of the present invention and the lightness index L* of the zirconia sintered body obtained by normal firing (total firing time: 6 to 12 hours) is preferably 2.0 or less, more preferably 1.5 or less, and even more preferably 1.0 or less, since it is suitable for a dental product. The L*, a*, and b* of the zirconia sintered body obtained by the manufacturing method of the present invention can be selected and set depending on the target site such as the cervical (tooth neck) or incisal (incisal edge).
[0055] The present invention includes embodiments in which the above configurations are combined in various ways within the scope of the technical concept of the present invention, as long as the effects of the present invention are achieved. In this specification, the upper and lower limits of the numerical ranges (heating rate, temperature decreasing rate, firing time, temperature, rate ratio, content of each component (e.g., stabilizer), etc.) can be appropriately combined. EXAMPLES
[0056] Next, the present invention will be described in more detail with reference to examples. However, the present invention is not limited to these examples, and many modifications within the scope of the technical concept of the present invention are possible by those having ordinary skill in the art.
[0057] [How to determine the shrinkage start temperature and shrinkage end temperature] In each of the examples and comparative examples described later, the shrinkage start temperature was determined by preparing a rectangular parallelepiped sample block of unsintered zirconia measuring 1 cm x 2 cm x 1 cm, and measuring the lowest firing temperature at which the shrinkage rate exceeded 0% when the sample block was fired for 10 minutes in a firing furnace at a firing temperature higher than the starting temperature of the temperature rise step. The shrinkage end temperature was determined by measuring the lowest temperature at which the difference between the shrinkage rate (%) at firing temperature T°C and the shrinkage rate (%) at firing temperature T+50°C was 0%, with the temperature width of each section of the shrinkage temperature range being 50°C.
[0058] [Example 1] A sample of a calcined zirconia body was prepared by cutting out a zirconia disk workpiece (Kuraray Noritake Dental Co., Ltd.) of "Noritake Katana (registered trademark) Zirconia" HTML using a DWX52DC (Roland DG Co., Ltd.) to have the shape shown in Fig. 1 ((a) plan view, (b) front view). The sample was fired using an F-2N (SK Medical Electronics Co., Ltd.) firing furnace under the firing schedule conditions shown in Table 1 to produce a zirconia sintered body (prosthesis).
[0059] [Table 1]
[0060] In Example 1, the shrinkage start temperature and shrinkage end temperature determined by the above method were 1000°C and 1400°C, respectively, and the heating rate in each section in the temperature range from the shrinkage start temperature to the shrinkage end temperature was set according to the method consisting of Steps 1 to 5 described above. In Step 1, the temperature was divided into 50°C temperature ranges, and the shrinkage rate was measured when firing was performed at the boundary temperature of each section. The shrinkage rate difference in each section calculated in Step 2 and the shrinkage coefficient in each section calculated in Step 3 are shown in Table 2. In Step 4, the maximum heating rate of the firing furnace was set to 50°C / min, and the allowable heating rate in each section was calculated. In Step 5, the heating rate in each section was set to 1.0 times the allowable heating rate.
[0061] [Table 2]
[0062] [Example 2] A zirconia sintered body (prosthesis) was manufactured in the same manner as in Example 1, except that the zirconia disk workpiece was changed to "Noritake Katana (registered trademark) Zirconia" HT (Kuraray Noritake Dental Co., Ltd., zirconia calcined body) and the firing schedule was changed as shown in Table 3. The shrinkage rate difference in each section calculated in Step 2 and the shrinkage coefficient in each section calculated in Step 3 are shown in Table 4. In Step 5, the heating rate in each section was set to 1.0 times the allowable heating rate.
[0063] [Table 3]
[0064] [Table 4]
[0065] [Example 3] A zirconia sintered body (prosthesis) was manufactured in the same manner as in Example 1, except that the zirconia disk workpiece was changed to "Noritake Katana (registered trademark) Zirconia" STML (Kuraray Noritake Dental Co., Ltd., zirconia calcined body) and the firing schedule was changed as shown in Table 5. The shrinkage rate in each section calculated in Step 2 and the shrinkage coefficient in each section calculated in Step 3 are shown in Table 6. In Step 5, the heating rate in each section was set to 1.0 times the allowable heating rate.
[0066] [Table 5]
[0067] [Table 6]
[0068] [Comparative Example 1] A zirconia sintered body (prosthesis) was manufactured in the same manner as in Example 1, except that the firing schedule was changed as shown in Table 7.
[0069] [Table 7]
[0070] [Comparative Example 2] A zirconia sintered body (prosthesis) was manufactured in the same manner as in Example 2, except that the firing schedule was changed as shown in Table 7.
[0071] [Comparative Example 3] A zirconia sintered body (prosthesis) was manufactured in the same manner as in Example 3, except that the firing schedule was changed as shown in Table 8.
[0072] [Table 8]
[0073] [Model compatibility] A model shown in FIG. 2 ((a) plan view, (b) front view) was made assuming a long span bridge, and the prosthesis (n=1) of the shape of FIG. 1 made in each of the above-mentioned examples and comparative examples was checked for compatibility with the model. When the prosthesis of the shape of FIG. 1 was attached to the model of FIG. 2, the case where there was no distance (gap) between the margins was evaluated as "◯", and the case where it was confirmed that there was a distance between the margins was evaluated as "×". Furthermore, the distance between the prosthesis margin 1 and the model margin 2 (the distance between the margins when the prosthesis of the shape of FIG. 1 was attached to the model of FIG. 2) was measured, and the average value of six points was calculated. The evaluation results are shown in FIG. 3.
[0074] Furthermore, all of the zirconia sintered bodies of Examples 1 to 3 were compatible with the model as shown in the image of FIG. 3, and the distance between the margins was also very small at 0.01 to 0.16 mm, and it was confirmed that deformation during firing was suppressed. All of the zirconia sintered bodies of Comparative Examples 1 to 3 had a gap of 0.94 to 1.65 mm between the prosthesis margin 1 and the model margin 2, and did not match the model, and it was confirmed that deformation during firing was not suppressed. From the above results, it was confirmed that the zirconia sintered body obtained by the manufacturing method of the present invention can be fired in a short time, and deformation can be suppressed even for prostheses with large shapes without limiting the composition, and is suitable as a dental product (e.g., a dental prosthesis). [Industrial Applicability]
[0075] The method for producing a zirconia sintered body of the present invention sinters a zirconia molded body or a zirconia calcined body in a short time, and the obtained zirconia sintered body can be fired in a short time, and the composition is not limited, and deformation can be suppressed even in a prosthesis having a large shape, so that it is useful for producing a dental product (e.g., a dental prosthesis). In particular, it is useful for producing a dental prosthesis having a large shape such as a bridge having three or more bridges such as a long span bridge. [Explanation of symbols]
[0076] 1 Prosthetic margin 2 Model margin
Claims
1. The method includes a heating step of heating a zirconia molded body or a zirconia calcined body, The heating step includes a temperature increasing step, In the heating step, the heating rate is adjusted in a temperature range from the temperature at which the shrinkage of zirconia starts to the temperature at which the shrinkage ends, when the temperature range is equally divided into a plurality of sections each having a specific temperature range, the rate of contraction of the zirconia molded body or the zirconia calcined body during heating in each section is substantially constant; The heating rate in each section is set within a range of 0.1 to 1.0 times the allowable heating rate in each section, calculated by the following formula (1), and the heating rate in each section is substantially the same magnification as the allowable heating rate in each section. A method for producing a zirconia sintered body. (Allowable heating rate in each section) = (Maximum heating rate of the firing furnace) / (Shrinkage coefficient in each section) ... (1) (In formula (1), the contraction coefficient in each section is expressed by the following formula (2).) (Shrinkage coefficient in each section)=(Shrinkage difference in each section) / (Temperature range / 100) (2) (However, if the contraction coefficient for each section calculated based on formula (2) is less than 1, the contraction coefficient for each section is set to 1 and formula (1) is calculated.)
2. The method for producing a zirconia sintered body according to claim 1, wherein the temperature range of each of the sections is 50°C.
3. The temperature range is 1050 to 1400 ° C., the temperature at which zirconia contraction begins is 1050 ° C., and the temperature at which zirconia contraction ends is 1400 ° C. The method for producing a zirconia sintered body according to claim 1 or 2.
4. The method for producing a zirconia sintered body according to any one of claims 1 to 3, wherein the total firing time from the start of the temperature rise in the temperature rise step to the end of the retention time at the maximum firing temperature in the temperature rise step is 120 minutes or less.
5. The method for producing a zirconia sintered body according to any one of claims 1 to 4, wherein the heating step further includes a mooring step of maintaining the maximum firing temperature in the heating step following the heating step.
6. The method for producing a zirconia sintered body according to any one of claims 1 to 5, wherein the zirconia sintered body is for dental use.
Citation Information
Patent Citations
Production of high-toughness silicon nitride sintered body
JP1990255573A
Preparation of aln sintered product
JP1992050171A
Method for controlling sintering of material
JP1992143646A
Sintering control method of material and device therefore
JP1998078400A
Calcined ceramic body for dental use
JP2010220779A