Core / shell type particles and their manufacturing method, and method for manufacturing hollow particles
By using magnesium-based core materials to directly form a magnesium fluoride shell on particles and remove cores with acid, the method simplifies and cost-reduces the production of core/shell and hollow particles, achieving efficient and high-strength results.
Patent Information
- Application Number
- JP2022192644
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-01
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2042-12-01
AI Technical Summary
Conventional methods for producing core/shell type particles and hollow particles require complex processes involving core particle synthesis, surface modification, and high-temperature core removal, making them inefficient and costly.
A method for producing core/shell type particles using magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide, or magnesium carbonate as core materials, which allows direct formation of a magnesium fluoride shell without core synthesis or surface modification, and core removal through acid treatment at ambient temperatures.
This method simplifies the manufacturing process, reduces costs, and enables the production of core/shell particles with uniform shell thickness and high strength, as well as hollow particles without thermal energy, enhancing industrial efficiency and cost-effectiveness.
Smart Images

Figure 0007557214000005 
Figure 0007557214000004 
Figure 0007557214000006
Abstract
Description
[Technical field]
[0001] The present invention relates to Particles made of at least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide, and magnesium carbonate. The present invention relates to a core / shell particle having a core particle formed of magnesium fluoride on the surface of the core particle, and a method for producing the same. The present invention also relates to a method for producing hollow particles, comprising a step of removing the core particle of the above-mentioned core / shell particle with an acid. [Background technology]
[0002] Anti-reflective films are used on the surfaces of displays of personal computers, smartphones, etc. Anti-reflective films are also used to coat the surfaces of optical elements such as camera lenses. The materials used for the outermost layer of these anti-reflective films must have a low refractive index and be transparent, so silica, magnesium fluoride, silicone resin, etc. are known to be used.
[0003] Furthermore, to keep reflectance low, anti-reflective coatings are known that utilize the refractive index of air, which is 1.0, and there are also known methods for producing materials with even lower refractive indexes by forming voids in layers of silica or magnesium fluoride.
[0004] As prior art relating to the above, there are known core / shell particles having high shell strength obtained by using a polyvinyl polymer as a core particle and forming a continuous shell made of magnesium fluoride on the surface thereof, and a method for producing hollow particles obtained from the core / shell particles (see Patent Document 1).
[0005] Also, there is known a method for producing core / shell type particles and hollow particles in which a polystyrene polymer is used as a core particle and a shell made of magnesium fluoride is formed on the surface thereof, in which the particle size and surface shape of the obtained particles can be controlled by controlling the concentration of the styrene monomer and the reaction temperature when synthesizing the core particle (see Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-19626 A [Patent Document 2] JP 2015-145325 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the manufacturing methods of Patent Documents 1 and 2, since the core particles are made of polyvinyl polymers, polystyrene polymers, etc., it is necessary to synthesize the core particles from scratch, and therefore organic solvents, monomers, polymerization initiators, etc. are required in the process of synthesizing the core particles.
[0008] Furthermore, in order to form a shell made of magnesium fluoride on the surface of a core particle made of the above-mentioned synthetic resin, it is necessary to appropriately adjust the zeta potential of the core particle surface by a method of modifying the core particle surface with a functional group, etc. Furthermore, in order to obtain a core / shell type particle by forming a strong continuous shell layer made of magnesium fluoride on the surface of the core particle, a process is required in which a crystal nucleus made of fluorine and magnesium is attached to the surface of the core particle under limited temperature conditions, and then a process is required in which a shell layer made of magnesium fluoride is formed by changing reaction conditions such as temperature to promote the growth of the crystal nucleus on the surface of the core particle.
[0009] Moreover, in order to obtain hollow particles from the core / shell particles obtained by the above-mentioned method, a step of heating the core / shell particles at a high temperature of 200° C. or more to remove the core particles is required.
[0010] As described above, the manufacturing methods described in Patent Documents 1 and 2 involve a wide variety of steps and reaction conditions for manufacturing core / shell particles and hollow particles, which makes the manufacturing process complicated, and therefore is not preferable from the viewpoint of industrial application in terms of securing manufacturing facilities, manufacturing efficiency, and economic efficiency.
[0011] An object of the present invention is to provide core / shell particles which can be obtained with fewer steps than conventional methods without requiring a core particle synthesis step, charge adjustment by surface modification of the core particles, or thermal energy in a hollowing step for obtaining fluoride hollow particles from core / shell particles, and to provide a method for producing the same and a method for producing fluoride hollow particles. [Means for solving the problem]
[0012] The method for producing core / shell type particles according to a first aspect of the present invention includes a shell formation step. At least one member selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide, and magnesium carbonate A shell made of magnesium fluoride is formed on the surface of the core particle made of magnesium fluoride.
[0013] According to the method for producing core / shell particles of this aspect, it is not necessary to synthesize core particles from scratch as in the conventional methods, and it is possible to produce core / shell particles without using a synthesis process and the associated equipment, chemicals, solvents, etc. Also, unlike the conventional methods in which a polyvinyl polymer or a polystyrene polymer is used as the core particle, in the production method of this aspect, At least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate Core Grain Child A shell layer made of magnesium fluoride can be formed by directly reacting the surface layer with a fluorinating agent. This makes it possible to manufacture core / shell type particles without the need to manage functional group modification of the core particle surface or the zeta potential of the core particle surface. This makes it possible to simplify process management, reduce manufacturing costs, and improve manufacturing efficiency compared to conventional methods. Furthermore, unlike conventional methods in which fluorine and magnesium are attached to the surface layer of a core particle and the resulting crystal nuclei are grown to form a shell layer of magnesium fluoride, the manufacturing method according to this aspect: At least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate Core Grain Child The surface layer can be directly fluorinated to form a shell, which allows the production of core / shell particles with high shell strength. In the method for producing core / shell particles according to this aspect, magnesium oxide, magnesium hydroxide, and magnesium carbonate are more suitable for fluorinating the surface layer, and are preferably used as core particles. The particle size and shape of the core / shell particles or hollow fluoride particles obtained by the production process according to the present invention are in accordance with the particle size and shape of the core particles. Therefore, by controlling the particle size and shape of the core particles, the particle size and shape of the core / shell particles or hollow fluoride particles obtained therefrom can be controlled.
[0014] A method for producing core / shell type particles according to a second aspect of the present invention is the method for producing core / shell type particles according to the first aspect, wherein the shell forming step comprises a solution of a fluorinating agent and Core particles made of at least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate. reacts to form a shell.
[0015] As a result of intensive research by the present inventors, it has become clear that the method for producing core / shell particles according to this aspect can produce core / shell particles having a shell layer with a more uniform thickness. In addition, the method for producing core / shell particles according to this aspect under wet conditions can produce core / shell particles having a shell made of granular magnesium fluoride on the surface layer of the core particles, and thus produce core / shell particles having a different shape from the particles obtained by the method for producing core / shell particles under dry conditions described below. Therefore, by changing the conditions of the fluorination step, it is possible to selectively produce core / shell particles having different shapes.
[0016] A method for producing core / shell type particles according to a third aspect of the present invention is the method for producing core / shell type particles according to the first aspect, wherein the shell forming step comprises fluorinating a gaseous agent and Core particles made of at least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate. reacts to form a shell.
[0017] As a result of intensive research by the present inventors, according to the method for producing core / shell particles of this aspect, a shell layer made of magnesium fluoride can be formed even on the surface layer of small core particles having a particle size of 1 μm or less to obtain core / shell particles. As a result, core / shell particles having a small particle size can be obtained. Furthermore, according to the method for producing core / shell particles of this aspect under dry conditions, core / shell particles having a shell made of extremely fine needle-like magnesium fluoride on the surface layer of the core particles can be obtained. Therefore, it is possible to selectively obtain core / shell particles having a shape different from that of particles obtained by the above-mentioned method for producing core / shell particles under wet conditions.
[0018] A method for producing core / shell type particles according to a fourth aspect of the present invention is the method for producing core / shell type particles according to the first aspect, wherein the shell formation step comprises: Core particles made of at least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate.The shell is formed by reacting the solid fluorinating agent with hydrogen fluoride generated by heating the solid fluorinating agent to its decomposition temperature.
[0019] As a result of intensive research by the present inventors, it has been found that, according to the method for producing core / shell type particles according to this aspect, the decomposition reactivity of the fluorinating agent is increased, Core particles made of at least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate. The efficiency of surface fluorination is improved. By using solid particles with small particle diameters as the fluorinating agent, The above core particles The efficiency of fluorination of the surface layer is further improved. Therefore, the method is an industrially practical method that combines high cost performance, in which a shell layer made of magnesium fluoride can be formed on the surface layer of the core particles with a smaller amount of fluorinating agent than in the liquid phase process or gas phase process, with high handleability, such as not requiring a separation process from the liquid phase and not directly handling anhydrous hydrogen fluoride gas.
[0020] A method for producing core / shell particles according to a fifth aspect of the present invention is a method for producing core / shell particles according to any one of the second to fourth aspects, in which the fluorinating agent is at least one fluorinating agent selected from the group consisting of hydrogen fluoride, hydrofluoric acid, ammonium fluoride, and ammonium acid fluoride.
[0021] Using the above fluorinating agent Core particles made of at least one selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate. By directly fluorinating the surface layer of the core / shell type particles, it is possible to obtain core / shell type particles having a shell layer with high strength. Specifically, as the fluorinating agent according to the second aspect of the present invention, hydrofluoric acid, an aqueous solution of ammonium fluoride, a mixed solution of hydrogen fluoride dissolved in ethanol, etc. are used, and it is particularly preferable to use hydrofluoric acid. As the fluorinating agent according to the third aspect of the present invention, hydrogen fluoride, ammonium fluoride, acidic ammonium fluoride, etc. are used, and it is particularly preferable to use hydrogen fluoride. Finally, as the fluorinating agent according to the fourth aspect of the present invention, sodium hydrogen fluoride, potassium hydrogen fluoride, ammonium fluoride, acidic ammonium fluoride, etc. are used, and it is particularly preferable to use ammonium fluoride or acidic ammonium fluoride.
[0022] The present invention 6 A core / shell particle according to an aspect comprises a core particle and a shell. The core particle comprises: At least one member selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide, and magnesium carbonate The shell is formed on the surface of the core particle. The shell is made of magnesium fluoride. The core / shell type particle has a first phase to a second phase. 5 The core / shell type particle can be obtained by a method for producing core / shell type particles according to any one of the aspects.
[0023] Therefore, the hollow particles of fluoride obtained from the core / shell type particles according to this aspect have a shell layer with high strength. The core / shell type particles according to this aspect have high heat resistance and can contribute to the invention of new materials that are less susceptible to high-temperature creep.
[0024] The present invention 7 A method for producing hollow particles of a fluoride according to an aspect includes a removing step. At least one member selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide, and magnesium carbonate From a core / shell type particle having a core particle made of magnesium fluoride and a shell made of magnesium fluoride formed on the surface layer of the core particle, the core particle is removed with an acid.
[0025] Therefore, in the hollowing step of removing only the core particles from the core / shell particles, hollow fluoride particles can be obtained without requiring thermal energy.
[0026] The present invention 8 A method for producing hollow particles of a fluoride according to an aspect of the present invention includes the steps of: 7 In a method for producing hollow fluoride particles according to an aspect, the acid is at least one acid selected from the group consisting of hydrochloric acid, nitric acid, and sulfuric acid.
[0027] Therefore, the elution time of the core particles can be controlled by adjusting the concentrations of hydrochloric acid, nitric acid, and sulfuric acid used to remove the core particles. Effect of the Invention
[0028] According to the present invention, it is possible to produce core / shell particles having a strong shell layer made of magnesium fluoride and a desired particle size or shape, and hollow fluoride particles, without requiring the steps that were essential in conventional methods: a step of synthesizing particles that will become the core of the core / shell particles; a step of adjusting the surface charge to form a shell layer made of magnesium fluoride on the surface of the core particles; and a step of removing the core particles of the core / shell particles using thermal energy. [Brief description of the drawings]
[0029] [Figure 1] 1 is a scanning electron microscope photograph of the core / shell particles produced in Example 1. [Diagram 2] 1 is a scanning electron microscope photograph of the core / shell particles produced in Example 2. [Diagram 3] 1 is a scanning electron microscope photograph of the core / shell particles produced in Example 3. [Figure 4] 1 is a transmission electron microscope photograph of the hollow particles produced in Example 1. [Diagram 5] 1 is a transmission electron microscope photograph of hollow particles produced in Example 2. [Figure 6] 1 is a transmission electron microscope photograph of hollow particles produced in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The method for producing hollow particles according to an embodiment of the present invention includes (1) a step of forming a shell on the surface of a core particle by a liquid phase method (wet method) or a gas phase method / solid phase method (dry method), and (2) a step of removing the core particle by an acid. These steps will be described in detail below.
[0031] <Shell formation process> In this process, the core grains To the child On the other hand, by reacting a fluorinating agent to form a shell layer on the surface of the core particle, the core becomes magnesium. Salt, core / shell particles can be made in which the shell is magnesium fluoride.
[0032] Magnesium Mu salt The magnesium salt is at least one kind of magnesium selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate. Mu salt Among them, magnesium oxide, magnesium hydroxide and magnesium carbonate are more suitable for fluorinating the surface layer, and are preferably used as the material for the core particle.
[0033] In addition, magnesium used as a core particle Mu salt The particle size is preferably in the range of 50 nm or more and 5 μm or less, and when the purpose is to form an anti-reflection film, it is particularly preferable to use particles with a particle size in the range of 50 nm or more and 100 nm or less from the viewpoint of achieving a low refractive index.
[0034] The fluorinating agent may be at least one selected from the group consisting of hydrogen fluoride, hydrofluoric acid, ammonium fluoride, and acidic ammonium fluoride.
[0035] The method of reacting the fluorinating agent with the core particles may be, for example, (a) adding magnesium to a solution of the fluorinating agent dissolved in a solvent. Mu salt (b) A method in which the vaporized fluorinating agent is added directly or in a mixed gas diluted with an inert gas such as nitrogen gas, and then the mixture is reacted with magnesium. Mu salt Ventilate the space in which the magnesium Mu salt (c) a method of contacting a fluorinating agent with magnesium (vapor phase method) Mu salt In the embodiment of the present invention, the method of reacting the fluorinating agent with the core particles includes mixing the fluorinating agent and the like in a solid state and heating the mixture to the decomposition temperature of the fluorinating agent (solid phase method). Mu salt The method is not limited to the above-mentioned methods as long as the method can fluorinate the surface layer.
[0036] The fluorinating agent used in the liquid phase method includes hydrofluoric acid, an aqueous solution of ammonium fluoride, or a solution in which hydrogen fluoride is dissolved in ethanol or the like. In particular, it is preferable to use hydrofluoric acid. The concentration of hydrofluoric acid is preferably adjusted to 1 to 10 mass %. The temperature during the reaction is preferably within a range of 25°C to 50°C in order to suppress the particle growth of the fluoride produced.
[0037] The fluorinating agent used in the above-mentioned gas phase method may be at least one selected from the group consisting of hydrogen fluoride, ammonium fluoride, and acidic ammonium fluoride. In particular, it is preferable to use anhydrous hydrogen fluoride gas. Mu salt When the vaporized fluorinating agent is passed through the reaction vessel from which the fluorinating agent is collected to react, the gas obtained by vaporizing the fluorinating agent may be diluted with an inert gas such as nitrogen gas and passed through the reaction vessel. From the viewpoint of suppressing condensation of hydrogen fluoride gas, the temperature during the reaction is preferably within a range of the condensation point of hydrogen fluoride to 300°C. In addition, the temperature during the reaction of ammonium fluoride and acidic ammonium fluoride may be any temperature that is equal to or higher than the boiling point of these fluorinating agents, and specifically, is preferably 240°C or higher under normal pressure.
[0038] The fluorinating agent used in the above-mentioned solid phase method may be at least one selected from the group consisting of ammonium fluoride and ammonium acid fluoride. The reaction temperature is preferably at or above the decomposition temperature of ammonium fluoride and ammonium acid fluoride. Specifically, the reaction temperature is preferably 100°C or higher for ammonium fluoride and 240°C or higher for ammonium acid fluoride under normal pressure.
[0039] The surfaces of the core / shell particles having irregularities obtained by fluorination in the shell formation step of each of the above-mentioned liquid phase method, gas phase method, and solid phase method can be smoothed by heat treatment at a temperature in the range of 600° C. to 800° C. In particular, in order to smooth the surfaces of the core / shell particles having irregularities, it is preferable to perform heat treatment at about 800° C.
[0040] <Process for removing core particles using acid> In this step, magnesium, which is the core part, is extracted from the core / shell type particles obtained in the above shell formation step. Mu salt The hollow particles can be produced by dissolving the above in an acid.
[0041] The core part is magnesium Mu salt The acid for dissolving the above may be at least one acid selected from the group consisting of hydrochloric acid, nitric acid, and sulfuric acid. In particular, it is preferable to use hydrochloric acid.
[0042] The concentration of the acid used to remove the core is preferably 0.5 to 2 M. By using an acid in this concentration range, only the core portion can be selectively dissolved. In addition, the amount of liquid to be treated during solid-liquid separation after dissolving the core portion is reduced, which is economical.
[0043] The temperature during dissolution is preferably room temperature. Furthermore, the concentration of the suspension during dissolution of the core portion is preferably 1 to 4% by mass. (Example)
[0044] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the examples shown below. EXAMPLES
[0045] 1. Preparation of core / shell particles by fluorinating the surface of magnesium oxide core particles using a liquid phase method (wet method) 50% by mass of hydrofluoric acid was collected in a 500 mL fluororesin container, and water was added thereto to dilute the concentration of hydrofluoric acid to 5% by mass, to prepare 250.8 g of 5% by mass of hydrofluoric acid. Next, 8.1 g of magnesium oxide (SMO-5 manufactured by Sakai Chemical Industry Co., Ltd., particle size approximately 5 μm) was added to the prepared 5% by mass of hydrofluoric acid, and the mixture was stirred at room temperature for 2 hours. The obtained suspension was subjected to sedimentation separation by centrifugation (2500 rpm, 10 minutes), and the supernatant liquid was removed. Next, 40 mL of water was added to the precipitate from which the supernatant liquid had been removed, and the precipitate was separated again by centrifugation (2500 rpm, 10 minutes), and the supernatant liquid was removed. After that, the precipitate was dried at 120 ° C. for 3 hours to obtain 9.9 g of white powder.
[0046] When the white powder obtained above was observed with a scanning electron microscope (JSM-IT200, manufactured by JEOL Ltd.), it was confirmed that fine granular particles were attached to the surface of particles with a diameter of about 5 μm (Figure 1). Furthermore, elemental analysis of the observed white powder revealed that the powder contained oxygen, magnesium, and fluorine. This confirmed that core / shell particles had been produced, with magnesium oxide as the core particle and a magnesium fluoride shell on the surface.
[0047] 2. Removal of core particles to create hollow particles 10 mL of 2M hydrochloric acid solution was added to 0.1 g of the core / shell particles obtained above and allowed to stand for 2 hours. After that, the supernatant was removed and 1 mL of methanol was added to the residue to obtain a dispersion. After immersing a TEM grid for observation in the dispersion obtained above, the grid was dried overnight at room temperature under reduced pressure in a desiccator to obtain a sample for observation. When the observation sample obtained above was observed with a transmission electron microscope (JEOL Ltd., JEM-2010-K), hollow particles with a particle size of about 5 μm and a shell thickness of about 500 nm were observed (Figure 4). In addition, elemental analysis by energy dispersive X-ray spectroscopy (EDS) of a scanning electron microscope (JEOL Ltd., JSM-IT200) showed that the composition of the hollow particles mentioned above contained magnesium and fluorine, and no oxygen was detected. This confirmed that the magnesium oxide core particles had been removed. EXAMPLES
[0048] 1. Preparation of core / shell particles by fluorinating the surface of magnesium oxide core particles using a gas phase method (dry method) 40.1 g of magnesium oxide (SMO-1, manufactured by Sakai Chemical Industry Co., Ltd., particle size approximately 1 μm) was collected in a 1 L fluororesin reaction vessel, and the reaction vessel was rotated at a speed of 20 rpm to stir the magnesium oxide in the reaction vessel. Next, a 1 L fluororesin vessel was prepared as a hydrogen fluoride gas generation vessel, and 60.1 g of liquid hydrogen fluoride (2.9 times the equivalent amount of magnesium oxide) was collected therein. Next, the hydrogen fluoride gas generation vessel was heated to 24°C in a water bath to generate hydrogen fluoride gas. A mixed gas obtained by diluting the hydrogen fluoride gas generated above with nitrogen gas at a flow rate of 1 L / min was passed through the reaction vessel, and the magnesium oxide and hydrogen fluoride gas were reacted at room temperature for 3 hours. Thereafter, the reaction product obtained above was dried at 120°C for 5 hours to obtain 45.3 g of white powder.
[0049] When the white powder obtained above was observed with a scanning electron microscope (JSM-IT200, manufactured by JEOL Ltd.), it was confirmed that fine needle-like particles were attached to the surface of particles with a diameter of about 1 μm (Figure 2). Furthermore, elemental analysis of the observed white powder revealed that the powder contained oxygen, magnesium, and fluorine. This confirmed that core / shell particles had been produced, with magnesium oxide as the core particle and a magnesium fluoride shell on the surface.
[0050] 2. Removal of core particles to create hollow particles 48 mL of 2M hydrochloric acid solution was added to 1 g of the core / shell particles obtained above and left to stand for 24 hours. Then, the precipitate obtained above was separated by centrifugation (2500 rpm, 10 minutes) and the supernatant was removed. Then, 40 mL of water was added to the residue obtained by removing the supernatant, and it was separated again by centrifugation (2500 rpm, 10 minutes) and the supernatant was removed. This operation was repeated twice, and then dried at 120 ° C for 3 hours to obtain 0.19 g of white powder. 0.1 g of this white powder was collected and 1 mL of methanol was added thereto to obtain a dispersion. After immersing a TEM grid for observation in the dispersion obtained above, the grid was dried under reduced pressure at room temperature overnight in a desiccator to obtain a sample for observation. When the observation sample obtained above was observed with a transmission electron microscope (JEOL Ltd., JEM-2010-K), hollow particles with a particle size of approximately 1 μm and a shell thickness of 200 nm were observed (Figure 5). Furthermore, elemental analysis using a scanning electron microscope energy dispersive X-ray spectroscopy (EDS) (JEOL Ltd., JSM-IT200) revealed that the composition of the hollow particles mentioned above contained magnesium and fluorine, but no oxygen was detected. This confirmed that the magnesium oxide core particles had been removed. EXAMPLES
[0051] 1. Preparation of core / shell particles by fluorinating the surface of magnesium hydroxide core particles using a gas phase method (dry method) 11.4 g of magnesium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, particle size approximately 0.07 μm) was collected in a 1 L fluororesin reaction vessel, and the reaction vessel was rotated at a speed of 20 rpm to stir the magnesium hydroxide in the reaction vessel. Next, a 1 L fluororesin vessel was prepared as a hydrogen fluoride gas generation vessel, and 8.7 g of liquid hydrogen fluoride (2.2 times the equivalent amount of magnesium hydroxide) was collected therein. Next, the hydrogen fluoride gas generation vessel was heated to 24 ° C. in a water bath to generate hydrogen fluoride gas. A mixed gas obtained by diluting the hydrogen fluoride gas generated above with nitrogen gas at a flow rate of 2 L / min was passed through the reaction vessel, and the reaction vessel was heated in an oil bath set at 110 ° C. for 1.5 hours to react the magnesium hydroxide with the hydrogen fluoride gas. Thereafter, the reaction product obtained above was dried at 120 ° C. for 5 hours to obtain 10.3 g of white powder.
[0052] The white powder obtained above was observed with a scanning electron microscope (JSM-IT200, manufactured by JEOL Ltd.), and particles with a diameter of approximately 100 nm were confirmed (Figure 3). Furthermore, elemental analysis of the observed white powder revealed that the powder contained oxygen, magnesium, and fluorine. This confirmed that core / shell particles had been produced, with magnesium oxide as the core particle and a magnesium fluoride shell on the surface.
[0053] 2. Removal of core particles to create hollow particles 200 mL of 0.5 M hydrochloric acid solution was added to 5.0 g of the core / shell particles obtained above and left to stand for 24 hours. The precipitate obtained above was then separated by centrifugation (2500 rpm, 10 min) and the supernatant liquid was removed. This operation was repeated twice, and then dried at 120 °C for 3 hours to obtain 1.58 g of white powder. 0.1 g of this white powder was taken and 1 mL of methanol was added thereto to obtain a dispersion liquid. After immersing a TEM grid for observation in the dispersion liquid obtained above, the grid was dried overnight at room temperature under reduced pressure in a desiccator to obtain a sample for observation. When the sample for observation obtained above was observed with a transmission electron microscope (JEM-2010-K, manufactured by JEOL Ltd.), hollow particles with a particle size of about 100 nm and a shell thickness of about 20 nm were observed (Figure 6). In addition, elemental analysis using a scanning electron microscope with energy dispersive X-ray spectroscopy (EDS) (JSM-IT200, manufactured by JEOL Ltd.) showed that the composition of the above-mentioned white powder contained magnesium and fluorine, but no oxygen was detected. This confirmed that the magnesium oxide core particle had been removed.
Claims
1. A method for producing core / shell particles, comprising heating a mixture containing core particles consisting of at least one type selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate and a fluorinating agent to a decomposition temperature of the fluorinating agent to form a shell consisting of magnesium fluoride on the surface of the core particles.
2. A method for producing hollow particles, comprising a removal step of removing, with an acid, from core / shell particles having a core particle made of at least one type selected from the group consisting of magnesium acetate, magnesium chloride, magnesium oxide, magnesium hydroxide and magnesium carbonate, and a shell made of magnesium fluoride and formed on the surface of the core particle.
3. The method for producing hollow particles according to claim 2 , wherein the acid is at least one acid selected from the group consisting of hydrochloric acid, nitric acid, and sulfuric acid.
Citation Information
Patent Citations
Electrode sheet for nonaqueous secondary battery, and nonaqueous secondary battery employing the same
JP2011108516A
Method for producing hollow particle, hollow particle, antireflection film, and optical element
JP2014019626A
Method for producing hollow magnesium fluoride particle
JP2015145325A