Method for producing room temperature curable organopolysiloxane composition, room temperature curable organopolysiloxane composition and article, and sealing material for automobile headlights

A room-temperature-curable organopolysiloxane composition with rapid curing and strong adhesion addresses the limitations of conventional silicone rubber compositions, ensuring effective sealing and antifogging material compatibility in automobile headlights.

JP7557268B2Active Publication Date: 2024-09-27SHIN ETSU CHEMICAL CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2019546622
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-10-06
Filing Date
2018-09-21
Publication Date
2024-09-27
Estimated Expiration
2038-09-21

AI Technical Summary

Technical Problem

Conventional delactate ester type room temperature curable (RTV) silicone rubber compositions have slow curing rates, limiting their applicability beyond sealants, and lack sufficient adhesiveness and workability for applications like automobile headlights, where they are also required to maintain antifogging properties without deteriorating the antifogging materials.

Method used

A room-temperature-curable organopolysiloxane composition is produced using a linear diorganopolysiloxane with silanol groups capped by hydrolyzable silyl groups and combined with amino group-containing hydrolyzable organosilanes, achieving rapid curing and strong adhesion, suitable for automobile headlights.

Benefits of technology

The composition exhibits rapid curing, excellent adhesion, and maintains antifogging material integrity, making it suitable for sealing materials in automobile headlights.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557268000027
    Figure 0007557268000027
  • Figure 0007557268000005
    Figure 0007557268000005
  • Figure 0007557268000030
    Figure 0007557268000030
Patent Text Reader

Abstract

By preliminarily mixing and reacting a linear diorganopolysiloxane having silanol groups at both molecular chain terminals, a hydrolyzable silane having a hydrolyzable group capable of releasing a lactate ester and / or its partial hydrolysis condensate, and an amino group-containing hydrolyzable organosilane and / or its partial hydrolysis condensate, and thereby capping the silanol groups at both molecular chain terminals of the main component (base polymer) with specific hydrolyzable silyl groups, it is possible to produce a delactate ester type room temperature vulcanizable organopolysiloxane composition that has excellent properties in all aspects, including curability, adhesion, and workability, which were not possible with conventional delactate ester type room temperature vulcanizable (RTV) silicone rubber compositions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a room-temperature curable organopolysiloxane composition having excellent adhesive properties, etc., using a linear diorganopolysiloxane having silanol groups at both molecular chain terminals as the starting material for the main component (base polymer), a room-temperature curable organopolysiloxane composition having excellent curability and adhesive properties, etc., and containing a linear diorganopolysiloxane having both molecular chain terminals blocked with hydrolyzable group-containing silyl groups capable of eliminating lactate esters as the main component (base polymer), and an article bonded or coated with a cured product of the composition, etc. In particular, the present invention relates to a room-temperature curable organopolysiloxane composition that can be used for bonding or coating articles suitable for use as a sealing material for vehicle headlights, and a method for producing the same, etc. [Background technology]

[0002] Room temperature vulcanizable (RTV) silicone rubber compositions that crosslink when exposed to moisture are easy to handle and have excellent weather resistance and electrical properties, so they are used in a variety of fields, including as sealing materials for building materials and adhesives in the electrical and electronics fields. These RTV silicone rubber compositions are often designed with organopolysiloxanes that have silanol groups at their ends as the main component (base polymer).

[0003] As the condensation curing type of room temperature vulcanizable (RTV) silicone rubber composition, the dealcohol type, the oxime type, the deacetylated type, etc. are generally known and are used for various applications. For example, the dealcohol type is widely used in adhesives for fixing electrical and electronic components, coating materials, automotive adhesives, etc. The oxime type and the deacetylated type are used mainly in sealing materials for building materials because they cure relatively quickly, but they pose safety problems because the gas generated as a by-product during curing is toxic or has an irritating odor. In addition, the oxime type and the deacetylated type are corrosive to the adherend, so caution is required when using them.

[0004] Now, the progress of the automobile industry in recent years has been tremendous, and hybrid cars, fuel cell cars, and electric cars are becoming mainstream due to the impact on the environment. Silicone rubber is very excellent in heat resistance, weather resistance, processability, etc., so it is used in all kinds of places, such as gasket materials around the engine, heat dissipation materials around the ECU, sealing materials, and potting materials for boost circuits in inverters. Taking advantage of the weather resistance, room temperature curable silicone rubber compositions are considered to be suitable as sealing materials for headlights, but in specifications where anti-fog materials are applied, the phenomenon of corrosion of the anti-fog materials by the outgassing by-product has been confirmed. Since the outgassing by-products of the condensation reaction (alcohol, oxime, acetic acid) all have low boiling points, it is thought that they react with the anti-fog materials, causing changes in their properties and reducing the anti-fog properties. For this reason, hot melt materials such as polyurethane-based materials are used for sealing materials for headlights. However, polyurethane-based materials have overwhelmingly lower heat resistance than silicone rubber, and since they are hot melt materials, the current situation is that they place a great burden on the equipment.

[0005] Therefore, there is a demand for a headlight sealant that is easier to use (good workability) and has curing and adhesive properties. Recently, a room temperature curing (RTV) silicone rubber composition of the de-lactate ester type by condensation reaction has been disclosed as a new curing technology (Patent Document 1: Japanese Patent No. 5399392). This patent shows that a room temperature curing (RTV) silicone rubber composition consisting of polydimethylsiloxane and ethyl lactatosilane, both ends of which have silanol groups at the molecular chain, is superior in terms of human health and the environment compared to conventional deoxime types. It is also described that the odor is weaker and less unpleasant than conventional curing types, and therefore the working environment is also good. However, this patent is configured as an application to sealants, and the curing speed is very slow (the curing time is very long) for the room temperature curing (RTV) silicone rubber composition. If the curing speed is slow, the waiting time until curing is completed is long, making it difficult to apply to applications other than sealants, and it is considered that there is room for improvement. As such, there is no description of adhesion or workability. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 5399392 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the above circumstances, and provides a method for producing a room-temperature-curable organopolysiloxane composition that is excellent in all properties, including curability, adhesion, and workability, which could not be achieved with conventional delactate ester type room-temperature-curable (RTV) silicone rubber compositions; a delactate ester type room-temperature-curable organopolysiloxane composition having such properties and suitable as a sealing material for automobile headlights; and a method for bonding or coating with a cured product of said composition. Things Product , sealing material for automobile headlights The purpose is to provide the following: [Means for solving the problem]

[0008] As a result of intensive research into achieving the above-mentioned object, the present inventors have discovered that it is possible to produce a delactate ester type room temperature curable organopolysiloxane composition that is excellent in all properties, such as curability, adhesion, and workability, which were not achievable with conventional delactate ester type room temperature curable (RTV) silicone rubber compositions, by premixing and reacting a linear diorganopolysiloxane having silanol groups at both molecular chain terminals, a hydrolyzable silane having a hydrolyzable group capable of eliminating a lactate ester and / or a partial hydrolyzed condensate thereof, and an amino group-containing hydrolyzable organosilane and / or a partial hydrolyzed condensate thereof, and going through a process of blocking the silanol groups at both molecular chain terminals of the main component (base polymer) with specific hydrolyzable silyl groups. They also discovered that a delactate ester type room temperature curable organopolysiloxane composition having such properties can be a suitable material for a sealing material for automobile headlights, which led to the completion of the present invention.

[0009] Accordingly, the present invention provides the following method for producing a room-temperature-curable organopolysiloxane composition, said room-temperature-curable organopolysiloxane composition, and articles bonded or coated with a cured product of said composition. [1] A method for producing a room-temperature-curable organopolysiloxane composition, comprising the steps of: (A) 100 parts by mass of an organopolysiloxane represented by the following general formula (1): [ka] (In the formula, R 1 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and m is an integer of 10 or more. (B) a hydrolyzable organosilane compound represented by the following general formula (2) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass, [ka] (In the formula, R 2 , R 3 are each an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a is 3 or 4. (C) A compound represented by the following general formula (3) other than the component (B). and (4 )in at least one amino group-containing hydrolyzable organosilane and / or its partial hydrolyzed condensate selected from the amino group-containing hydrolyzable organosilanes shown below and their partial hydrolyzed condensates: 0.1 to 10 parts by mass, [ka] (In the formula, R 4 is a divalent hydrocarbon group having 7 to 10 carbon atoms containing an alkylene group and an aromatic ring, R 5 is a divalent hydrocarbon group having 1 to 10 carbon atoms, and R 6 , R 7 is an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms; b is 2 or 3; provided that at least one of the primary and secondary amines is R 4It is not directly connected to the aromatic ring in the Y = NZ-SiR3(4 ) ( In the formula, Y is expressed by the following formula (17): [ka] (In the formula, R 8 、R 9 、R 10 、R 11 each independently represents a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, an alkenyl group or an aryl group, and the wavy line portion is a bonding site with a nitrogen atom.) What is indicated by Z is an unsubstituted or substituted divalent hydrocarbon group having 1 to 10 carbon atoms which may contain a heteroatom. R is one or more monovalent groups selected from hydrolyzable groups having 1 to 6 carbon atoms and monovalent hydrocarbon groups having 1 to 6 carbon atoms, and at least two of the three Rs bonded to the silicon atom are hydrolyzable groups. (D) Inorganic filler: 1 to 800 parts by mass, (E) Curing catalyst: 0.001~20 parts by mass, A method for producing a room-temperature-curable organopolysiloxane composition, comprising the steps of premixing and reacting a mixture containing components (A), (B), and (C) to prepare a reaction mixture containing a reaction product of components (A) and (B), and then uniformly mixing the reaction mixture with components (D) and (E). [ 2 ] The conditions for premixing and reacting a mixture containing components (A), (B), and (C) are a temperature range of 0 to 60°C and a mixing time of 10 to 120 minutes. ] A method for producing the room temperature curable organopolysiloxane composition described above. [ 3 ] The room temperature curable organopolysiloxane composition is characterized in that the tack-free time at 23°C is less than 10 minutes. [1] or [ 2] A method for producing the room temperature curable organopolysiloxane composition described above. [ 4 ] (A') Both ends of the molecular chain are -O-CH(CH3)-C(=O)OR 3 (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms.) (B) a hydrolyzable organosilane compound represented by the following general formula (2) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass, [ka] (In the formula, R 2 , R 3 are each an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a is 3 or 4. (C) A compound represented by the following general formula (3) other than the component (B). and (4 )in at least one amino group-containing hydrolyzable organosilane and / or its partial hydrolyzed condensate selected from the amino group-containing hydrolyzable organosilanes shown below and their partial hydrolyzed condensates: 0.1 to 10 parts by mass, [ka] (In the formula, R 4 is a divalent hydrocarbon group having 7 to 10 carbon atoms containing an alkylene group and an aromatic ring, R 5 is a divalent hydrocarbon group having 1 to 10 carbon atoms, and R 6 , R 7 is an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms; b is 2 or 3; provided that at least one of the primary and secondary amines is R 4 It is not directly connected to the aromatic ring in the Y = NZ-SiR3(4 ) ( In the formula, Y is expressed by the following formula (17): [ka] (In the formula, R 8 、R 9、R 10 、R 11 each independently represents a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, an alkenyl group or an aryl group, and the wavy line portion is a bonding site with a nitrogen atom.) What is indicated by Z is an unsubstituted or substituted divalent hydrocarbon group having 1 to 10 carbon atoms which may contain a heteroatom. R is one or more monovalent groups selected from hydrolyzable groups having 1 to 6 carbon atoms and monovalent hydrocarbon groups having 1 to 6 carbon atoms, and at least two of the three Rs bonded to the silicon atom are hydrolyzable groups. (D) Inorganic filler: 1 to 800 parts by mass, (E) Curing catalyst: 0.001~20 parts by mass A room temperature curable organopolysiloxane composition comprising: [ 5 ] The component (A') is a linear diorganopolysiloxane represented by the following general formula (1'): 4 2. The room-temperature-curable organopolysiloxane composition according to claim 1 . [ka] (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, R 2 , R 3 are each an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, m is an integer of 10 or more, and a' is 2 or 3. [ 6 ] The above components (A'), (B) and (C) comprise a reaction mixture of (A) an organopolysiloxane represented by the following general formula (1), the above component (B) and the above component (C): 4 ] or [ 5 2. The room-temperature-curable organopolysiloxane composition according to claim 1 . [ka] (In the formula, R 1 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and m is an integer of 10 or more. [ 7 ] [4 ]~[ 6 13. An article adhered or coated with a cured product of the room-temperature-curable organopolysiloxane composition according to any one of claims 1 to 12. [ 8 ] It is an in-vehicle headlight. 7 ]. [ 9 ] This is an automotive headlight coated with anti-fog material. 7 ]. [ 10 ] [ 4 ]~[ 6 13. A sealing material for automobile headlights comprising the room-temperature-curable organopolysiloxane composition according to any one of claims 1 to 12. Effect of the Invention

[0010] According to the present invention, a linear diorganopolysiloxane having silanol groups at both molecular chain terminals is used as the starting material for the main component (base polymer), a hydrolyzable silane having a hydrolyzable group capable of eliminating a lactate ester is used as the crosslinking agent, and further, an amino group-containing hydrolyzable organosilane and / or a partial hydrolyzed condensate thereof are used in combination. By blocking the silanol groups at both molecular chain terminals of the main component (base polymer) in advance with specific hydrolyzable silyl groups, it is possible to produce a delactate ester type room temperature curable organopolysiloxane composition that is excellent in all properties such as curability, adhesion, and workability, which were not achievable with conventional delactate ester type room temperature curable (RTV) silicone rubber compositions, and this composition can be a suitable material for a sealing material for automobile headlights. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The method for producing the room-temperature-curable organopolysiloxane composition of the present invention involves premixing and reacting a mixture containing components (A), (B), and (C) to prepare a reaction mixture (i.e., a mixture of components (A'), (B), and (C)) containing a reaction product of component (A) and component (B) (i.e., component (A')), and then uniformly mixing this reaction mixture with components (D) and (E).

[0012] [Component (A)] In the method for producing a room-temperature-curable organopolysiloxane composition of the present invention, component (A) used as the starting material for the main component (base polymer) is a linear diorganopolysiloxane, represented by the following general formula (1), in which both molecular chain terminals are blocked with hydroxyl groups (silanol groups) bonded to silicon atoms. [ka]

[0013] In the above formula (1), R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, such as alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, hexyl, 2-ethylhexyl, and octyl; cyclic alkyl groups such as cyclohexyl; alkenyl groups such as vinyl, allyl, and propenyl; aryl groups such as phenyl and tolyl; and groups in which the hydrogen atoms of these groups are partially substituted with halogen atoms, such as 3,3,3-trifluoropropyl. Of these, methyl, phenyl, and 3,3,3-trifluoropropyl groups are particularly preferred. 1 may be the same group or different groups.

[0014] Furthermore, m is an integer of 10 or more (usually 10 to 5,000), preferably 50 to 3,000, and more preferably about 100 to 2,000, and is an integer that gives the diorganopolysiloxane a viscosity at 25°C in the range of 25 to 100,000 mPa s, and preferably 500 to 80,000 mPa s.

[0015] In the present invention, the m value (degree of polymerization) indicating the number of repetitions of diorganosiloxane units or the molecular weight can be determined as the polystyrene-equivalent number average degree of polymerization (or number average molecular weight) in gel permeation chromatography (GPC) analysis using toluene or the like as a developing solvent (hereinafter the same). The viscosity can be measured by a rotational viscometer (e.g., BL type, BH type, BS type, cone-plate type, rheometer, etc.) (hereinafter the same).

[0016] [(B) Component] Component (B) is represented by the following general formula (2), which contains -O-CH(CH3)-C(=O)OR in one molecule. 3 (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms), and has 3 or 4 hydrolyzable groups capable of eliminating a lactic acid ester, and / or a partial hydrolyzed condensate thereof. [ka]

[0017] In the above formula (2), R 2 , R 3 R are unsubstituted or substituted monovalent hydrocarbon groups each having 1 to 10 carbon atoms, such as alkyl groups such as methyl, ethyl, and propyl; cyclic alkyl groups such as cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; and groups in which the hydrogen atoms of these groups are partially substituted with halogen atoms, such as 3,3,3-trifluoropropyl. Of these, methyl, ethyl, and vinyl groups are preferred. 2 , R 3may be the same or different. a is 3 or 4, and is particularly preferably 3. In addition, the methine carbon atom to which the methyl group in formula (2) is bonded can be an asymmetric center, and may be any of the (R) form, the (S) form, and the racemic form.

[0018] Specific examples of the (B) component include compounds such as methyl tris(ethyl lactate) silane, vinyl tris(ethyl lactate) silane, ethyl tris(ethyl lactate) silane, n-propyl tris(ethyl lactate) silane, n-butyl tris(ethyl lactate) silane, methyl tris(methyl lactate) silane, vinyl tris(methyl lactate) silane, ethyl tris(methyl lactate) silane, n-propyl tris(methyl lactate) silane, n-butyl tris(methyl lactate) silane, methyl tris(n-propyl lactate) silane, vinyl tris(n-propyl lactate) silane, ethyl tris(n-propyl lactate) silane, n-propyl tris(n-propyl lactate) silane, and n-butyl tris(n-propyl lactate) silane, as well as partial hydrolysis condensates of these silanes. In the present invention, the partial hydrolysis condensate means an organosiloxane oligomer having at least two, and preferably three or more, residual hydrolyzable groups in the molecule, which is produced by partial hydrolysis condensation of a raw material hydrolyzable organosilane compound (hereinafter the same).

[0019] Among these, methyltris(ethyllactate)silane, vinyltris(ethyllactate)silane, methyltris(methyllactate)silane, and vinyltris(methyllactate)silane are preferred, with methyltris(ethyllactate)silane and vinyltris(ethyllactate)silane being particularly preferred. The component (B) may be used alone or in combination of two or more kinds.

[0020] In the method for producing a room-temperature-curable organopolysiloxane composition of the present invention, a portion of component (B) undergoes a condensation reaction with silanol groups at both molecular terminals of component (A) described above, using component (C) described below as an endblocking catalyst, to convert the terminal silanol groups to -O-CH(CH3)-CH(=O)OR 3 (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms), more specifically, a hydrolyzable silyl group having two or three hydrolyzable groups capable of eliminating a lactic acid ester represented by the formula: 2 ) 3-a’ (O-CH(CH3)-C(=O)OR 3 ) a’ A hydrolyzable silyl group (R 2 , R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a' is 2 or 3.) to form a compound represented by the following general formula (1'): [ka] (In the formula, R 1 , R 2 , R 3 , m, a' are the same as above.) The remaining components of component (B) act as crosslinkers (curing agents) themselves in the room-temperature-curable organopolysiloxane composition obtained by the production method of the present invention.

[0021] Typically, about 5 to 40 mol %, preferably about 10 to 30 mol %, and more preferably about 15 to 25 mol % of component (B) is consumed to cap the silanol groups at both molecular terminals of the raw material component (A) with terminal hydrolyzable silyl groups to modify it to component (A'), and the remaining 60 to 95 mol %, preferably about 70 to 90 mol %, and more preferably about 75 to 85 mol % acts as a crosslinking agent (curing agent) in the composition.

[0022] The amount of component (B) to be blended is within the range of 0.1 to 30 parts by mass, preferably 0.5 to 20 parts by mass, and particularly preferably 1 to 15 parts by mass, per 100 parts by mass of component (A) at a stage prior to preparation of a reaction mixture containing a reaction product of components (A) and (B) (i.e., component (A')) produced by premixing and reacting components (A) to (C). If the amount is less than 0.1 part by mass, the endblocking rate of component (A) is poor, making it difficult to obtain a room-temperature-curable organopolysiloxane composition having the desired rubber elasticity. If the amount exceeds 30 parts by mass, the mechanical properties of the obtained cured product tend to decrease, and the curing rate of the room-temperature-curable organopolysiloxane composition also slows down, which are disadvantages. Furthermore, the amount of component (B) in the room-temperature-curable organopolysiloxane composition of the present invention at a stage after preparation of a reaction mixture containing the reaction product of the above-mentioned components (A) and (B) (i.e., component (A')), is typically 0.1 to 30 parts by mass, preferably 0.1 to 28 parts by mass, more preferably 0.5 to 18 parts by mass, and particularly preferably about 1 to 14 parts by mass, per 100 parts by mass of component (A').

[0023] [(C) component] The amino group-containing hydrolyzable organosilane and / or its partial hydrolysis condensate, component (C), is a compound that exerts an important effect as an endblocking catalyst for the organopolysiloxane having silanol groups at the ends of component (A) and as an adhesion promoter. It contains the -O-CH(CH3)-C(=O)OR 3 (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms. It is essentially different from the above component (B) in that it does not contain a hydrolyzable group capable of eliminating a lactic acid ester represented by the following general formula (3), (4) and (4'), and is preferably at least one selected from amino group-containing hydrolyzable organosilanes represented by the following general formulas (3), (4) and (4') and partial hydrolyzed condensates thereof. [ka] (In the formula, R 4 is a divalent hydrocarbon group having 7 to 10 carbon atoms containing an alkylene group and an aromatic ring, R 5is a divalent hydrocarbon group having 1 to 10 carbon atoms, and R 6 , R 7 is an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms; b is 2 or 3; provided that at least one of the primary and secondary amines is R 4 It is not directly connected to the aromatic ring in the Y=NZ-SiR3(4) Y-NH-Z-SiR3(4') (In the formula, Y is a monovalent or divalent hydrocarbon group having 1 to 15 carbon atoms containing two or more nitrogen atoms in its structure, Z is an unsubstituted or substituted divalent hydrocarbon group having 1 to 10 carbon atoms which may contain a heteroatom, R is one or more monovalent groups selected from hydrolyzable groups having 1 to 6 carbon atoms and monovalent hydrocarbon groups having 1 to 6 carbon atoms, and at least two of the three Rs bonded to the silicon atom are hydrolyzable groups.)

[0024] First, in the amino group-containing hydrolyzable organosilane and / or its partial hydrolysis condensate represented by the general formula (3), this amino group-containing hydrolyzable organosilane contains an aromatic ring between a primary and secondary amine, and further has a structure in which at least one of them is not directly bonded to the aromatic ring, and details thereof are described in JP-A-5-105689.

[0025] In this case, in the general formula (3), R 4 is a divalent hydrocarbon group having 7 to 10 carbon atoms containing an alkylene group and an aromatic ring, and is preferably a group in which a phenylene group (-C6H4-) is bonded to an alkylene group having 1 to 4 carbon atoms, such as a methylene group, an ethylene group, or a trimethylene group, and examples thereof include those represented by the following formulas (5) to (13). -CH2-C6H4- (5) -CH2-C6H4-CH2- (6) -CH2-C6H4-CH2-CH2- (7) -CH2-C6H4-CH2-CH2-CH2- (8) -CH2-CH2-C6H4- (9) -CH2-CH2-C6H4-CH2- (10) -CH2-CH2-C6H4-CH2-CH2- (11) -CH2-CH2-CH2-C6H4- (12) -CH2-CH2-CH2-C6H4-CH2- (13) Among these, (6) is particularly preferred.

[0026] R 5 is a divalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and examples thereof include alkylene groups such as a methylene group, an ethylene group, a propylene group, a tetramethylene group, a hexamethylene group, an octamethylene group, a decamethylene group, and a 2-methylpropylene group, an arylene group such as a phenylene group, and groups in which these alkylene groups are bonded to an arylene group, and is preferably an alkylene group having 1 to 4 carbon atoms.

[0027] Also, R 6 , R 7 are each independently an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, hexyl, 2-ethylhexyl, and octyl groups; cyclic alkyl groups such as cyclohexyl groups; alkenyl groups such as vinyl, allyl, and propenyl groups; and aryl groups such as phenyl and tolyl groups. R 6 is preferably a methyl group, a vinyl group, or a phenyl group, more preferably a methyl group; R 7 As the alkyl group, an alkyl group having 1 to 4 carbon atoms is preferable, and a methyl group or an ethyl group is more preferable.

[0028] Specific examples of the amino group-containing hydrolyzable organosilane represented by general formula (3) include those represented by the following general formulas (14) and (15), in which Me and Et represent a methyl group and an ethyl group, respectively. [ka] [ka]

[0029] Next, the amino group-containing hydrolyzable organosilane and / or its partial hydrolyzed condensate represented by the general formulas (4) and (4') is an amino group-containing hydrolyzable organosilane and / or its partial hydrolyzed condensate which contains 3 or more, preferably 3 to 6, and more preferably 3 to 5 nitrogen atoms in one molecule and has a monovalent or divalent basic site (Y) that exhibits an end-blocking catalytic function.

[0030] In this case, in general formula (4) or general formula (4'), the monovalent or divalent basic moiety Y capable of expressing an end-capping catalytic function is a monovalent or divalent hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, containing 2 or more, preferably 2 to 5, more preferably 2 to 4 nitrogen atoms in its structure, and among the basic moieties Y, examples of the monovalent group include a group consisting of a partial structure of 1,5,7-triazabicyclo[4.4.0]dec-5-ene shown in the following formula (16), and examples of the divalent group include those exhibiting strong basicity, such as an N-substituted or unsubstituted guanidyl group shown in the following formula (17). In the following formulas, the wavy line portion is a bonding site with a nitrogen atom. [ka] [ka]

[0031] R in Equation (17) 8 ~R 11 Each of R represents a hydrogen atom or a linear, branched or cyclic alkyl group, alkenyl group or aryl group having 1 to 10 carbon atoms, examples of which include alkyl groups such as methyl, ethyl and propyl groups; cyclic alkyl groups such as cyclohexyl groups; alkenyl groups such as vinyl and allyl groups; and aryl groups such as phenyl and tolyl groups. Of these, methyl, ethyl and phenyl groups are preferred, with methyl being particularly preferred. Also, R 8 ~R 11 may be the same or different.

[0032] In the above formula (4) or (4'), R is one or more monovalent groups selected from hydrolyzable groups having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, such as alkoxy groups, such as methoxy group, ethoxy group, propoxy group, isopropoxy group, butoxy group, isobutoxy group, and tert-butoxy group; alkenyloxy groups, such as vinyloxy group, allyloxy group, propenoxy group, and isopropenoxy group; ketoxime groups, such as dimethylketoxime group, diethylketoxime group, and methylethylketoxime group; and acyloxy groups, such as acetoxy group; or monovalent hydrocarbon groups having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, such as alkyl groups, such as methyl group and ethyl group; alkenyl groups, such as vinyl group; and aryl groups, such as phenyl group. Of the three Rs bonded to the silicon atom, at least two, preferably three Rs are hydrolyzable groups.

[0033] Examples of the hydrolyzable silyl group (-SiR3) include alkoxysilyl groups such as trimethoxysilyl group, methyldimethoxysilyl group, vinyldimethoxysilyl group, phenyldimethoxysilyl group, and triethoxysilyl group; isopropenoxysilyl groups such as triisopropenoxysilyl group, methyldiisopropenoxysilyl group, ethyldiisopropenoxysilyl group, vinyldiisopropenoxysilyl group, and phenyldiisopropenoxysilyl group; and ketoximesilyl groups such as tris(dimethylketoxime)silyl group, tris(diethylketoxime)silyl group, and tris(ethylmethylketoxime)silyl group.

[0034] In the above formula (4) or (4'), Z is an unsubstituted or substituted divalent hydrocarbon group such as a linear, branched or cyclic alkylene group, alkenylene group, arylene group, etc. having 1 to 10 carbon atoms, particularly 1 to 6 carbon atoms, which may contain a heteroatom such as an oxygen atom or a nitrogen atom, or a group formed by combining these. Examples of the divalent hydrocarbon group include alkylene groups such as methylene group, ethylene group, propylene group, tetramethylene group, hexamethylene group, octamethylene group, decamethylene group, and 2-methylpropylene group; arylene groups such as phenylene group, groups in which these alkylene groups and arylene groups are bonded, and the above alkylene groups interposed by ketones, esters, amides, etc. are preferred, and the like is a methylene group, an ethylene group, a propylene group, a propylene group interposed by an amide bond, etc., and the like is particularly preferred.

[0035] Specific examples of the amino group-containing hydrolyzable organosilane represented by general formula (4) or general formula (4') include those represented by the following general formulae (18) to (25), in which Me, Et, and Ph represent a methyl group, an ethyl group, and a phenyl group, respectively. [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]

[0036] Among these, N-methyl-substituted guanidyl group-containing trialkoxysilanes such as N-methyl-substituted guanidyl group-containing trimethoxysilanes (e.g., γ-(N,N′-dimethylguanidyl)propyltrimethoxysilane) represented by formula (18), formula (19), or formula (20), particularly N-methyl-substituted guanidyl group-containing trialkoxysilanes represented by formula (20), are preferred.

[0037] The amount of component (C) blended is 0.1 to 10 parts by mass, preferably 0.2 to 5 parts by mass, and more preferably 0.5 to 3 parts by mass, per 100 parts by mass of component (A) at a stage prior to preparing a reaction mixture containing a reaction product of components (A) and (B) (i.e., component (A')) produced by premixing and reacting components (A) to (C). If the blending amount is too small, the terminal blocking rate of component (A) decreases and the adhesiveness of the resulting cured product also decreases. If the blending amount is too large, it becomes unaffordable in terms of cost and the storage stability of the resulting composition decreases. Furthermore, the amount of component (C) in the room-temperature-curable organopolysiloxane composition of the present invention at a stage after preparation of the reaction mixture containing the reaction product of components (A) and (B) described above (i.e., component (A')) is in the range of about 0.1 to 10 parts by mass, preferably 0.2 to 5 parts by mass, and more preferably about 0.5 to 3 parts by mass per 100 parts by mass of component (A').

[0038] [(D) component] The inorganic filler of component (D) includes ground silica, fumed silica, wet silica, crystalline silica, aluminum hydroxide, alumina, boehmite, magnesium hydroxide, magnesium oxide, calcium hydroxide, calcium carbonate, zinc carbonate, basic zinc carbonate, zinc oxide, titanium oxide, carbon black, glass beads, glass balloons, resin beads, resin balloons, etc., and may be used alone or in combination of two or more. These inorganic fillers may be untreated or may be surface-treated with a known treatment agent. As a known treatment agent, for example, the hydrolyzable group-containing polysiloxane described in JP-A-2000-256558 is preferable, but is not limited thereto.

[0039] The amount of component (D) blended, prior to the preparation of a reaction mixture containing a reaction product of components (A) and (B) (i.e., component (A')) produced by premixing and reacting components (A) to (C), is 1 to 800 parts by mass, preferably 2 to 600 parts by mass, and particularly preferably 5 to 500 parts by mass, per 100 parts by mass of component (A). If the amount is less than 1 part by mass, the mechanical properties of the resulting cured product will be poor. If the amount exceeds 800 parts by mass, it will be difficult to obtain a room-temperature-curable organopolysiloxane composition having rubber elasticity. Furthermore, the amount of component (D) in the room-temperature-curable organopolysiloxane composition of the present invention at a stage after preparation of the reaction mixture containing the reaction product of components (A) and (B) described above (i.e., component (A')) is in the range of about 1 to 800 parts by mass, preferably 2 to 600 parts by mass, and more preferably about 5 to 500 parts by mass per 100 parts by mass of component (A').

[0040] [(E) component] The curing catalyst of component (E) may be the same or different, and may be used either alone or as a mixture of two or more. Examples of the curing catalyst include organic carboxylates and alkoxides of metals such as tin, titanium, zirconium, iron, antimony, bismuth, and manganese; organic titanate esters and organic titanium chelate compounds; and amine compounds other than component (C) and their salts. More specifically, dibutyltin dilaurate, dibutyltin dioctoate, dioctyltin dilaurate, dibutyltin maleate, dibutyltin terephthal ... to, Tin compounds such as dimethyltin dineodecanoate, dibutyltin dimethoxide, dioctyltin dineodecanoate, and stannous octoate; tetrabutyl titanate, diisopropoxybis(acetylacetonate)titanium, and diisopropoxybis(ethylacetoacetate). titanium Examples include titanium compounds such as dibutylamine, laurylamine, tetramethylguanidine, and other amine compounds and salts thereof other than component (C).The addition of an organotin compound is preferred because it provides the composition of the present invention with excellent curing properties such as rapid curing and deep curing, and among these, dialkyltin dialkoxides and dialkyltin dicarboxylates are preferred.

[0041] The amount of the curing catalyst (E) added is 0.001 to 20 parts by mass, preferably 0.01 to 5 parts by mass, and particularly preferably 0.05 to 3 parts by mass, per 100 parts by mass of component (A) at a stage prior to preparing a reaction mixture containing a reaction product of components (A) and (B) (i.e., component (A')) produced by premixing and reacting components (A) to (C). If the amount is less than 0.001 part by mass, sufficient crosslinking properties cannot be obtained in the resulting composition. If the amount exceeds 20 parts by mass, it becomes uneconomical and there are drawbacks such as a decrease in the curing speed of the resulting composition. Furthermore, the amount of component (E) in the room-temperature-curable organopolysiloxane composition of the present invention at a stage after preparation of the reaction mixture containing the reaction product of components (A) and (B) described above (i.e., component (A')) is in the range of about 0.001 to 20 parts by mass, preferably 0.01 to 5 parts by mass, and more preferably about 0.05 to 3 parts by mass, per 100 parts by mass of component (A').

[0042] [Other ingredients] In the present invention, in addition to the above-mentioned components (A) to (E), other silane coupling agents can be blended.Specific examples include vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-glycidoxypropyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane. This silane coupling agent is preferably blended together with component (D) or component (E) in a step of premixing and reacting a mixture containing components (A), (B), and (C) to prepare a reaction mixture containing a reaction product of components (A) and (B), and then uniformly mixing the reaction mixture with components (D) and (E).

[0043] The amount of other silane coupling agents, when used, is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, per 100 parts by mass of component (A) at a stage prior to preparation of a reaction mixture containing a reaction product of component (A) and component (B) (i.e., component (A')) produced by premixing and reacting components (A) to (C). When other silane coupling agents are added, the amount of the other silane coupling agents in the room-temperature-curable organopolysiloxane composition of the present invention at a stage after preparation of the reaction mixture containing the reaction product of the above-described components (A) and (B) (i.e., component (A')) is preferably within the range of about 0.1 to 10 parts by mass, and more preferably about 0.2 to 5 parts by mass, per 100 parts by mass of component (A').

[0044] In the present invention, additives other than the above components may be added. As the additive, known additives may be added within a range that does not impair the object of the present invention. For example, polyether as a wetter or thixotropy improver, non-reactive dimethyl silicone oil as a plasticizer, isoparaffin, trimethylsiloxy unit [(CH3)3SiO] as a crosslink density improver, 1 / 2 units) and SiO2 units.

[0045] Furthermore, if necessary, colorants such as pigments, dyes, and fluorescent whitening agents, antifungal agents, antibacterial agents, surface modifiers such as non-reactive phenylsilicone oils, fluorosilicone oils, and organic liquids incompatible with silicones as bleed oils, and solvents such as toluene, xylene, volatile oils, cyclohexane, methylcyclohexane, and low-boiling point isoparaffins may also be added.

[0046] [Preparation of the composition] The method for producing the room temperature curable organopolysiloxane composition of the present invention includes first premixing and reacting a mixture containing the above-mentioned components (A), (B), and (C) to obtain a reaction product of components (A) and (B) (i.e., a reaction product in which the silanol groups at both ends of the molecular chain of component (A) are -O-CH(CH3)-C(=O)OR 3 (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms), more specifically, the silanol groups at both ends of the molecular chain of component (A) are each a linear diorganopolysiloxane terminated with a hydrolyzable silyl group having two or three hydrolyzable groups capable of eliminating a lactic acid ester represented by the formula: -Si(R 2 ) 3-a’ (O-CH(CH3)-C(=O)OR 3 ) a’ A hydrolyzable silyl group (R 2 , R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a' is 2 or 3. ) The composition can be produced by preparing a reaction mixture containing the above and then uniformly mixing the reaction mixture with the components (D) and (E).

[0047] The conditions for premixing and reacting the mixture containing the components (A), (B), and (C) are generally in the temperature range of 0 to 60°C, preferably 10 to 40°C, and the mixing time is generally 10 to 120 minutes, preferably 20 to 90 minutes, and the mixture can be mixed uniformly.

[0048] The room-temperature curable organopolysiloxane composition containing components (A'), (B), (C), (D), and (E) produced through these steps can be stored in an atmosphere free from moisture. When left at room temperature (23°C ± 10°C), it will usually cure in 5 minutes to 1 week in the presence of moisture in the air.

[0049] The tack-free time at 23°C of the room-temperature-curable organopolysiloxane composition produced as above, measured in accordance with JIS K 6249, is preferably less than 10 minutes, and more preferably from 2 to 9 minutes. The above tack-free time can be achieved by a production method in which a mixture containing components (A), (B), and (C) is premixed and reacted to prepare a reaction mixture containing a reaction product of components (A) and (B), and then the reaction mixture is uniformly mixed with components (D) and (E).

[0050] The thus obtained delactated ester type room temperature curable organopolysiloxane composition is excellent in all properties such as curability, adhesion, and workability, and is therefore particularly suitable for use as a sealing material for automobile headlights. EXAMPLES

[0051] EXAMPLES Hereinafter, examples and comparative examples will be given to specifically explain the present invention, but the present invention is not limited to the following examples. In the following examples, the viscosity is 25 The values ​​are measured using a rotational viscometer at ℃, and the degree of polymerization is the number average degree of polymerization converted into polystyrene in GPC analysis using toluene as a developing solvent. Room temperature means 23℃±10℃. Me represents a methyl group.

[0052] [Example 1] A reaction mixture containing a polydimethylsiloxane whose molecular chain ends were blocked with a mixture of methylbis(ethyllactato)silyl groups and vinylbis(ethyllactato)silyl groups (molar ratio, approximately 3:1) was prepared by mixing 60 parts by mass (2.0 mmol) of a polydimethylsiloxane whose molecular chain ends were silanol groups and whose viscosity at 25°C was 50,000 mPa s (degree of polymerization, approximately 400), 25 parts by mass of a polydimethylsiloxane whose molecular chain ends were trimethylsilyl groups and whose viscosity at 25°C was 100 mPa s, 6 parts by mass (15.2 mmol) of methyltris(ethyllactato)silane, 2 parts by mass (4.9 mmol) of vinyltris(ethyllactato)silane, and 0.8 parts by mass of an amino-containing hydrolyzable organosilane represented by the following formula (26) as an end-blocking catalyst for component (A) at room temperature and pressure for 60 minutes. Next, 8 parts by mass of fumed silica was mixed with the reaction mixture under reduced pressure (-0.08 MPa or less, the same applies below) for 40 minutes. After mixing under reduced pressure, 0.1 parts by mass of dioctyltin dineodecanoate was added and mixed under reduced pressure for 15 minutes to obtain composition 1. [ka]

[0053] [Example 2] A reaction mixture containing a polydimethylsiloxane whose molecular chain ends were blocked with a mixture of methylbis(ethyllactato)silyl groups and vinylbis(ethyllactato)silyl groups (molar ratio, approximately 3:1) was prepared by mixing 60 parts by mass (2.0 mmol) of a polydimethylsiloxane whose molecular chain ends were silanol groups and whose viscosity at 25°C was 50,000 mPa s (degree of polymerization, approximately 400), 25 parts by mass of a polydimethylsiloxane whose molecular chain ends were trimethylsilyl groups and whose viscosity at 25°C was 100 mPa s, 6 parts by mass (15.2 mmol) of methyltris(ethyllactato)silane, 2 parts by mass (4.9 mmol) of vinyltris(ethyllactato)silane, and 0.8 parts by mass of the amino group-containing hydrolyzable organosilane represented by the above formula (26) as an end-blocking catalyst for component (A) at room temperature and pressure for 60 minutes. Next, 8 parts by mass of fumed silica was mixed into the reaction mixture under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane and 0.1 parts by mass of dioctyltin dineodecanoate were added and mixed under reduced pressure for 15 minutes to obtain composition 2.

[0054] [Example 3] 60 parts by mass (2.0 mmol) of a polydimethylsiloxane having silanol groups at both molecular chain terminals and a viscosity of 50,000 mPa s at 25°C (degree of polymerization approximately 400), 25 parts by mass of a polydimethylsiloxane having trimethylsilyl groups at both molecular chain terminals and a viscosity of 100 mPa s at 25°C, 6.6 parts by mass (16.3 mmol) of vinyltris(ethyllactato)silane, and 0.8 parts by mass of an amino-containing hydrolyzable organosilane represented by the above formula (26) as an end-capping catalyst for component (A) were mixed at room temperature and pressure for 60 minutes to obtain a polymer having both molecular chain terminals of Vinyl A reaction mixture containing polydimethylsiloxane capped with bis(ethyllactato)silyl groups was prepared. Then, 8 parts by mass of fumed silica was mixed with the reaction mixture under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.1 parts by mass of dioctyltin dineodecanoate was added and mixed under reduced pressure for 15 minutes to obtain composition 3.

[0055] [Example 4] A reaction mixture containing a polydimethylsiloxane whose molecular chain ends were blocked with a mixture of methylbis(ethyllactato)silyl groups and vinylbis(ethyllactato)silyl groups (molar ratio, approximately 3:1) was prepared by mixing 60 parts by mass (2.0 mmol) of a polydimethylsiloxane whose molecular chain ends were silanol groups and whose viscosity at 25°C was 50,000 mPa s (degree of polymerization, approximately 400), 25 parts by mass of a polydimethylsiloxane whose molecular chain ends were trimethylsilyl groups and whose viscosity at 25°C was 100 mPa s, 6 parts by mass (15.2 mmol) of methyltris(ethyllactato)silane, 2 parts by mass (4.9 mmol) of vinyltris(ethyllactato)silane, and 0.8 parts by mass of an amino-containing hydrolyzable organosilane represented by the following formula (27) as an end-blocking catalyst for component (A) at room temperature and pressure for 60 minutes. Next, 8 parts by mass of fumed silica was mixed into the reaction mixture under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.1 parts by mass of dioctyltin dilaurate was added and mixed under reduced pressure for 15 minutes to obtain composition 4. [ka]

[0056] [Example 5] A reaction mixture containing a polydimethylsiloxane whose molecular chain ends were blocked with a mixture of methylbis(ethyllactato)silyl groups and vinylbis(ethyllactato)silyl groups (molar ratio, approximately 3:1) was prepared by mixing 60 parts by mass (2.0 mmol) of a polydimethylsiloxane whose molecular chain ends were silanol groups and whose viscosity at 25°C was 50,000 mPa s (degree of polymerization, approximately 400), 25 parts by mass of a polydimethylsiloxane whose molecular chain ends were trimethylsilyl groups and whose viscosity at 25°C was 100 mPa s, 6 parts by mass (15.2 mmol) of methyltris(ethyllactato)silane, 2 parts by mass (4.9 mmol) of vinyltris(ethyllactato)silane, and 0.8 parts by mass of the amino group-containing hydrolyzable organosilane represented by the above formula (27) as an end-blocking catalyst for component (A) at room temperature and pressure for 60 minutes. Next, 8 parts by mass of fumed silica was mixed into the reaction mixture under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane and 0.1 parts by mass of dioctyltin dilaurate were added and mixed under reduced pressure for 15 minutes to obtain composition 5.

[0057] [Comparative Example 1] 60 parts by mass (2.0 mmol) of polydimethylsiloxane having silanol groups at both ends of the molecular chain and a viscosity of 50,000 mPa·s at 25°C (degree of polymerization of about 400), 25 parts by mass of polydimethylsiloxane having trimethylsilyl groups at both ends of the molecular chain and a viscosity of 100 mPa·s at 25°C, 6 parts by mass (15.2 mmol) of methyltris(ethyllactato)silane, and 2 parts by mass (4.9 mmol) of vinyltris(ethyllactato)silane were mixed at room temperature and pressure for 60 minutes. Next, 8 parts by mass of fumed silica were mixed under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.1 parts by mass of dioctyltin dineodecanoate was added and mixed under reduced pressure for 15 minutes to obtain composition 6.

[0058] [Comparative Example 2] 60 parts by mass (2.0 mmol) of polydimethylsiloxane having silanol groups at both ends of the molecular chain and a viscosity of 50,000 mPa·s at 25°C (degree of polymerization approximately 400), 25 parts by mass of polydimethylsiloxane having trimethylsilyl groups at both ends of the molecular chain and a viscosity of 100 mPa·s at 25°C, and 6.6 parts by mass (16.3 mmol) of vinyltris(ethyllactato)silane were mixed at room temperature and pressure for 60 minutes. Next, 8 parts by mass of fumed silica were mixed under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.1 parts by mass of dioctyltin dineodecanoate was added and mixed under reduced pressure for 15 minutes to obtain composition 7.

[0059] [Comparative Example 3] 60 parts by mass (2.0 mmol) of polydimethylsiloxane having silanol groups at both ends of the molecular chain and a viscosity of 50,000 mPa·s at 25°C (degree of polymerization of about 400), 25 parts by mass of polydimethylsiloxane having trimethylsilyl groups at both ends of the molecular chain and a viscosity of 100 mPa·s at 25°C, 6.6 parts by mass (16.3 mmol) of vinyltris(ethyllactato)silane, and 0.1 parts by mass of dioctyltin dilaurate were mixed at room temperature and pressure for 60 minutes. Next, 8 parts by mass of fumed silica were mixed under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane was added and mixed under reduced pressure for 15 minutes to obtain composition 8.

[0060] [Comparative Example 4] 60 parts by mass (2.0 mmol) of polydimethylsiloxane having silanol groups at both molecular chain terminals and a viscosity of 50,000 mPa·s at 25°C (degree of polymerization approximately 400), 25 parts by mass of polydimethylsiloxane having trimethylsilyl groups at both molecular chain terminals and a viscosity of 100 mPa·s at 25°C, 4 parts by mass (13.6 mmol) of methyltris(methylethylketoxime)silane, 1 part by mass (3.3 mmol) of vinyltris(methylethylketoxime)silane, and 0.8 parts by mass of the amino group-containing hydrolyzable organosilane represented by the above formula (26) were mixed at room temperature and normal pressure for 60 minutes. Next, 8 parts by mass of fumed silica were mixed under reduced pressure for 40 minutes. After mixing under reduced pressure, 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane and 0.1 parts by mass of dioctyltin dilaurate were added and mixed under reduced pressure for 15 minutes to obtain composition 9.

[0061] The following properties were confirmed using the prepared compositions 1 to 9. The results are shown in Table 1.

[0062] Tuck free time Measurements were performed in accordance with JIS K 6249.

[0063] ·Initial hardening The prepared compositions 1 to 9 were allowed to stand for 7 days in an environment of 23° C. / 50% RH to harden to a thickness of 3 mm, and their hardness was measured according to JIS K 6249.

[0064] ·Curing speed The prepared compositions 1 to 9 were placed in a glass petri dish with a diameter of 10 mm and a height of 13 mm, and left for one day in a 23°C / 50% RH environment. After one day, the cured rubber was hollowed out from the surface to the depth, and the cured thickness (mm) was measured.

[0065] ·Adhesiveness Automotive headlights are mainly made of polycarbonate. Polycarbonate (PC) and aluminum (Al) with a width of 25 mm and a length of 50 mm were used as adherends, and the prepared compositions 1 to 9 were applied to the adherends with an adhesion area of ​​250 mm 2The specimen was sandwiched between the above-mentioned adherends so that the adhesive thickness was 2.0 mm, and left for 7 days in a 23°C / 50% RH environment to prepare a shear adhesion test specimen. Using this test specimen, the shear adhesive strength (MPa) was measured in accordance with JIS K 6249, and the cohesive failure rate (CF: the ratio (%) of the area of ​​cohesive failure to the total area of ​​the fracture surface) was confirmed.

[0066] ·Dischargeability The prepared compositions 1 to 9 were filled into a polyethylene cartridge and discharged from a nozzle with a diameter of 3 mm at a pressure of 0.2 MPa, and the mass of the composition discharged in 5 seconds was measured.

[0067] -Effectiveness test on anti-fog materials Automotive headlights may be coated with an anti-fogging material to prevent fogging. In order to confirm the effect on the anti-fog material, 10 g of each of the prepared compositions 1 to 9 was placed in a sealable 150 ml glass container. The polycarbonate coated with the anti-fog material was placed in the container so as not to come into contact with the compositions 1 to 9, and the container was completely sealed. The container was left at 70°C for 3 days, and the change in the anti-fog material and the anti-fog properties were evaluated. The evaluation results were judged as follows. Changes in anti-fog materials ○: The anti-fog material is not cloudy or altered. ×: The anti-fog material is cloudy or has deteriorated. Anti-fog ○: Anti-fogging properties are maintained ×: Anti-fogging properties are not maintained, and the anti-fogging material becomes foggy due to human breath, etc.

[0068] [Table 1]

[0069] The results of Examples 1 to 5 above show that in order to achieve good curability, curing speed, and adhesion, the component (C) is necessary, and further, by using the component (B) to form compositions (Compositions 1 to 5), there is almost no effect on the anti-fog materials used in vehicle headlights. In the compositions 6 to 8 of Comparative Examples 1 to 3 in which the component (C) was not added, the curability, adhesion and dischargeability were deteriorated. In addition, in the case of the conventional oxime-free room-temperature curable organopolysiloxane composition (composition 9) not containing the component (B) in Comparative Example 4, although good curing properties were obtained, the anti-fog material deteriorated (became cloudy), and therefore it was unsuitable for use in headlights.

Claims

1. A method for producing a room temperature curable organopolysiloxane composition, comprising the steps of: (A) 100 parts by mass of an organopolysiloxane represented by the following general formula (1): 【Chemistry 1】 (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, and m is an integer of 10 or more. (B) a hydrolyzable organosilane compound represented by the following general formula (2) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass, 【Chemistry 2】 (In the formula, R 2 , R 3 are each an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a is 3 or 4. (C) 0.1 to 10 parts by mass of at least one amino group-containing hydrolyzable organosilane and / or its partial hydrolyzed condensate, which is selected from the amino group-containing hydrolyzable organosilanes represented by the following general formulas (3) and (4) and their partial hydrolyzed condensates, other than the component (B), 【Chemistry 3】 (In the formula, R 4 is a divalent hydrocarbon group having 7 to 10 carbon atoms containing an alkylene group and an aromatic ring, R 5 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 6 , R 7 is an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms; b is 2 or 3; provided that at least one of the primary and secondary amines is R 4 It is not directly connected to the aromatic ring in the Y=N-Z-SiR 3 (4) (wherein Y is the following formula (17) 【Chemistry 4】 (In the formula, R 8 , R 9 , R 10 and R 11 each independently represent a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, an alkenyl group or an aryl group, and the wavy line portion is a bonding site with the nitrogen atom.) where Z is an unsubstituted or substituted divalent hydrocarbon group having 1 to 10 carbon atoms which may contain a heteroatom. R is one or more monovalent groups selected from hydrolyzable groups having 1 to 6 carbon atoms and monovalent hydrocarbon groups having 1 to 6 carbon atoms, and at least two of the three Rs bonded to the silicon atom are hydrolyzable groups. (D) Inorganic filler: 1 to 800 parts by mass, (E) Curing catalyst: 0.001 to 20 parts by mass, A method for producing a room-temperature-curable organopolysiloxane composition, comprising the steps of premixing and reacting a mixture containing components (A), (B), and (C) to prepare a reaction mixture containing a reaction product of components (A) and (B), and then uniformly mixing this reaction mixture with components (D) and (E).

2. 2. The method for producing a room-temperature-curable organopolysiloxane composition according to claim 1, wherein the conditions for premixing and reacting the mixture containing components (A), (B), and (C) are a temperature range of 0 to 60°C and a mixing time of 10 to 120 minutes.

3. 3. The method for producing a room-temperature-curable organopolysiloxane composition according to claim 1, wherein the room-temperature-curable organopolysiloxane composition has a tack-free time at 23° C. of less than 10 minutes.

4. (A') Both ends of the molecular chain are -O-CH(CH 3 )-C(=O)OR 3 (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms.) (B) a hydrolyzable organosilane compound represented by the following general formula (2) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass, 【Chemistry 6】 (In the formula, R 2 , R 3 are each an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a is 3 or 4. (C) 0.1 to 10 parts by mass of at least one amino group-containing hydrolyzable organosilane and / or its partial hydrolyzed condensate, which is selected from the amino group-containing hydrolyzable organosilanes represented by the following general formulas (3) and (4) and their partial hydrolyzed condensates, other than the component (B), 【Chemistry 7】 (In the formula, R 4 is a divalent hydrocarbon group having 7 to 10 carbon atoms containing an alkylene group and an aromatic ring, R 5 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 6 , R 7 is an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms; b is 2 or 3; provided that at least one of the primary and secondary amines is R 4 It is not directly connected to the aromatic ring in the Y=N-Z-SiR 3 (4) (wherein Y is the following formula (17) 【Chemistry 10】 (In the formula, R 8 , R 9 , R 10 and R 11 each independently represent a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, an alkenyl group or an aryl group, and the wavy line portion is a bonding site with the nitrogen atom.) where Z is an unsubstituted or substituted divalent hydrocarbon group having 1 to 10 carbon atoms which may contain a heteroatom. R is one or more monovalent groups selected from hydrolyzable groups having 1 to 6 carbon atoms and monovalent hydrocarbon groups having 1 to 6 carbon atoms, and at least two of the three Rs bonded to the silicon atom are hydrolyzable groups. (D) Inorganic filler: 1 to 800 parts by mass, (E) Curing catalyst: 0.001 to 20 parts by mass A room temperature curable organopolysiloxane composition comprising:

5. 5. The room-temperature-curable organopolysiloxane composition according to claim 4, wherein component (A') is a linear diorganopolysiloxane represented by the following general formula (1'): 【Chemistry 8】 (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms; R 2 , R 3 are each an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, m is an integer of 10 or more, and a' is 2 or 3.

6. 6. The room-temperature-curable organopolysiloxane composition according to claim 4 or 5, wherein the components (A'), (B) and (C) comprise a reaction mixture of (A) an organopolysiloxane represented by the following general formula (1), the component (B) and the component (C): 【Chemistry 9】 (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, and m is an integer of 10 or more.

7. An article adhered or coated with a cured product of the room temperature curable organopolysiloxane composition according to any one of claims 4 to 6.

8. 8. The article of claim 7 which is a vehicle headlight.

9. 8. The article of claim 7 which is a vehicle headlight coated with an anti-fog material.

10. 7. A sealing material for automobile headlights, comprising the room temperature curable organopolysiloxane composition according to any one of claims 4 to 6.

Citation Information

Patent Citations

  • Organic silicon cementing compound and preparation method thereof

    CN105238342A

  • Room-temperature curing ethyl lactate removal type silicone sealant

    CN107523257A

  • Silan and oligomer thereof, manufacture and composition bridged to elastomer therefrom

    JP1983185594A

  • Organopolysiloxane composition coatable after curing at room temperature

    JP1986051056A

  • Curable composition

    JP1991041157A