Coated Pigments

A coated pigment with a translucent base material and a magnetite layer of specific crystal lattice constant addresses the issue of insufficient chroma and limited color tones, enabling high chroma and diverse interference colors.

JP7557294B2Active Publication Date: 2024-09-27TOYO ALUMINIUM KK
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020120328
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-14
Publication Date
2024-09-27
Estimated Expiration
2040-07-14

AI Technical Summary

Technical Problem

Conventional pigments lack sufficient chroma and have limited color tones, particularly in interference colors.

Method used

A coated pigment is developed with a translucent base material coated by a magnetite layer having a specific crystal lattice constant of 8.35 Å or more, which allows for high chroma and expression of various interference colors.

Benefits of technology

The coated pigment achieves high chroma and can express interference colors such as red, blue, yellow, and green with enhanced color development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557294000002
    Figure 0007557294000002
  • Figure 0007557294000004
    Figure 0007557294000004
  • Figure 0007557294000003
    Figure 0007557294000003
Patent Text Reader

Abstract

To provide a pigment having interference colors having various color tones having high chromas.SOLUTION: A coated pigment includes a base material where at least its surface is made of a translucent material, and a magnetite layer coating the base material, in which a crystal lattice constant of the magnetite layer is 8.35Å or more. As the translucent material, at least one selected from the group consisting of silica, alumina, glass, mica and a resin can be used. As the base material, a metal flake coated with the translucent material can be used.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coated pigment coated with a magnetite layer. [Background technology]

[0002] Pigments that have been imparted with interference colors by forming a single or composite coating of silicon oxide, titanium oxide, iron oxide, metal, etc. on the surface of a transparent substrate such as mica, alumina, or glass, or an aluminum pigment, have been conventionally known.

[0003] For example, Patent Document 1 discloses a coated pigment in which a ferrite layer is formed on the surface of a light-transmitting substrate or a metal substrate having a light-transmitting layer formed on the surface thereof. Furthermore, Patent Document 2 discloses an orange pearl pigment in which the surface of a flaky substrate is coated with a metal oxide containing iron oxide. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP2015-178556A [Patent Document 2] Japanese Patent Application Publication No. 10-259318 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the pigment of Patent Document 1 is not sufficient in saturation or color development, and the pigment of Document 2 is limited in the color tone that can be obtained to red or yellow. Therefore, an object of the present invention is to provide a pigment having interference colors of various tones with high chroma. [Means for solving the problem]

[0006] As a result of thorough investigation in light of the above circumstances, the inventors discovered that the above problem can be solved by coating a substrate, at least the surface of which is made of a light-transmitting material, with a magnetite layer and controlling the magnetite layer to a predetermined crystal structure, thereby arriving at the present invention. That is, the gist of the present invention resides in the following [1] to [3]. [1] A coated pigment comprising a substrate having at least a surface made of a light-transmitting material and a magnetite layer coating the substrate, the magnetite layer having a crystal lattice constant of 8.35 Å or more.

[0007] [2] The coated pigment according to [1], wherein the light-transmitting material is at least one selected from the group consisting of silica, alumina, glass, mica, and resin. [3] The coated pigment according to [1] or [2], wherein the substrate is a metal flake coated with the light-transmitting material. [4] The coated pigment according to [3], wherein the metal flakes are at least one selected from the group consisting of aluminum, copper, nickel, tin, titanium, zinc, an alloy containing at least one of these, and stainless steel.

[0008] [5] The coated pigment according to any one of [1] to [4], further comprising a protective layer on the magnetite layer, the protective layer being made of a metal oxide, a metal hydroxide, a metal oxide hydrate, a resin, or a combination thereof. [6] A resin composition comprising the coated pigment according to any one of [1] to [5]. [7] A coated article obtained by coating the resin composition according to [6] on a substrate. [8] A cosmetic preparation comprising the coated pigment according to any one of items [1] to [5]. Effect of the Invention

[0009] The coated pigment according to the present invention has high chroma and color development properties, and can exhibit a wide variety of interference colors, such as reds, blues, yellows, and greens. [Brief description of the drawings]

[0010] [Figure 1]Photographs of the coated pigments obtained in Example 12 and Comparative Example 6 coated on a sheet and formed into a cylindrical shape (color photographs converted to grayscale) [Diagram 2] Photographs of the coated pigments obtained in Example 11 and Comparative Example 5 coated on a sheet and formed into a cylindrical shape (color photographs converted to grayscale) [Diagram 3] Photographs of the coated pigments obtained in Example 4 and Comparative Example 1 when coated onto a sheet and formed into a cylindrical shape (color photographs converted to grayscale) [Figure 4] Photographs of the coated pigments obtained in Example 10 and Comparative Example 4 coated on a sheet and formed into a cylindrical shape (color photographs converted to grayscale) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail. The present invention relates to a coated pigment having an interference color, which comprises a substrate having at least a surface made of a light-transmitting material and a magnetite layer coating the substrate.

[0012] [Base material] The substrate of the present invention is a material that becomes the core of the coated pigment of the present invention, and at least the surface thereof is made of a light-transmitting material. As long as at least the surface thereof is made of a light-transmitting material, the entire substrate may be made of the light-transmitting material, or a core material made of another material may be coated with the light-transmitting material.

[0013] The volume average particle diameter of the substrate (D 50 ) can be selected arbitrarily within the range in which the particle diameter of the coated pigment according to the present invention described below can be achieved, and is more preferably 0.5 μm or more and 200 μm or less. If it is 0.5 μm or more and 200 μm or less, it is preferable because it can be well coated with the magnetite layer. If it is smaller than 0.5 μm, the specific surface area of ​​the substrate becomes large, making it difficult to sufficiently deposit the magnetite layer, while if it is larger than 200 μm, the specific surface area becomes small, decreasing the contact probability between the substrate and the magnetite particles to be coated, making it difficult to achieve good coating with the magnetite layer.

[0014] The shape of the substrate may be in the form of particles or flakes, and is preferably in the form of flakes. When the substrate is a translucent substrate made only of a translucent material, any known translucent substrate can be used without any particular limitation. Among them, translucent substrates made of silica, alumina, glass, mica, resin, and composites thereof are preferably used because of their high translucency. In addition, since the light-transmitting substrate itself serves as an interference layer, it is desirable that the substrate has a uniform thickness if it is in the form of particles or flakes.

[0015] In addition, when the substrate is a core material having a surface coated with a light-transmitting material, and the core material and the light-transmitting material are made of different materials, the material of the core material is not particularly limited and may be a light-transmitting material different from the light-transmitting material constituting the surface, or may be an opaque material. Examples of the opaque material include metals, plate-like iron oxide, and the like. The metal is not particularly limited and any known metal may be used, including aluminum, copper, nickel, tin, titanium, zinc, an alloy containing at least one of these, and stainless steel. As described above, examples of the light-transmitting material include the same materials as those used as the light-transmitting base material consisting only of a light-transmitting material.

[0016] The core material is preferably made of metal flakes, since it is possible to obtain a pigment having particularly high brightness and saturation. In particular, the metal flakes made of aluminum or an aluminum alloy, among the above-mentioned metals, are suitable because they are inexpensive and have high brightness. In addition, the coating layer made of the light-transmitting material that coats the core material is preferably uniform in thickness because it becomes an interference layer that determines the color tone. When the light-transmitting layer is thicker than 100 nm, the interference color becomes stronger, and a coated pigment with high saturation can be obtained. As the thickness increases, the change in color tone depending on the viewing angle (color travel) becomes stronger.

[0017] [Magnetite layer] The magnetite layer of the present invention is a layer made of magnetite that covers the substrate. When a magnetite layer having a specific crystal lattice constant is used as the magnetite layer that covers the substrate, a coated pigment having higher chroma and color development can be obtained, and by changing the conditions of each component that constitutes the coated pigment, it is possible to express various interference colors such as red, blue, yellow to green. Therefore, a coated pigment having various interference colors can be obtained. This is thought to be due to the crystal structure being changed by the loss of oxygen atoms from magnetite, which causes changes in the refraction and transmission of light in the magnetite layer, and tends to increase the depth and intensity of saturation and color development. Also, it becomes possible to produce the various interference colors described above.

[0018] The crystal lattice constant of the magnetite layer must be at least 8.35 Å, and is preferably at least 8.37 Å. If the crystal lattice constant is less than 8.35 Å, the saturation of the interference color may be low, and sufficient color development may not be achieved. In addition, the upper limit of the crystal lattice constant of the magnetite layer is not particularly limited, but is preferably 8.45 Å or less, and more preferably 8.42 Å or less. It may exceed 8.45 Å, but it is difficult to obtain a magnetite layer having a crystal lattice constant exceeding 8.45 Å, and there is an increased risk that the number of oxygen atoms will be too low and the magnetite will no longer be magnetite.

[0019] The average thickness of the magnetite layer is not particularly limited, but is preferably from 10 nm to 200 nm, more preferably from 20 nm to 120 nm, in which case the saturation of the interference color is particularly good.

[0020] [Thickness of the translucent layer and magnetite layer of the substrate] When a core material having a surface coated with a light-transmitting material is used as the substrate, the hue of the interference color also changes depending on the thickness of the magnetite layer. For example, when aluminum flakes (metallic substrate) with a translucent layer of silica of about 140 nm are used as the substrate, a magnetic, highly saturated pink-colored coated pigment (metallic pigment) can be obtained by covering the substrate with a layer of magnetite about 30 nm thick, and a coated pigment (metallic pigment) that changes color from green to purple depending on the observation angle can be obtained by covering the substrate with a layer of magnetite about 100 nm thick. This is presumably because, as the magnetite layer becomes thicker, a difference in the optical path length occurs between the light reflected on the surface of the magnetite layer and the light reflected on the interface between the magnetite layer and the translucent layer.

[0021] [Protective layer] The coated pigment of the present invention may further have a protective layer provided on the surface of the magnetite layer, if necessary. The material of the protective layer is not particularly limited as long as it is transparent and does not impair the color development of the coated pigment. Examples of such a protective layer include metal oxides, metal hydroxides, metal oxide hydrates, resins, and composites thereof, and may be appropriately selected from these depending on the purpose. For example, if the protective layer is made of a metal oxide, the water resistance can be improved, and if the protective layer is made of a resin, the adhesion and chemical resistance of the coating film containing the coated pigment of the present invention are improved.

[0022] The method for forming the protective layer can be any known method that covers a pigment. For example, the protective layer can be formed by radical polymerization in a slurry, or a metal oxide layer can be formed by a sol-gel method. The protective layer can be formed before or after the firing of the magnetite layer.

[0023] [Manufacturing of coated pigments] The coated pigment according to the present invention can be produced by the following method. First, the substrate can be manufactured by the following method. When a light-transmitting substrate made only of a light-transmitting material is used as the substrate, the material can be adjusted to a predetermined size and thickness and used as is as the substrate. In addition, when a core material having a surface coated with a light-transmitting material is used as the substrate, a slurry of the core material is prepared using alcohol or the like, and an alcohol solution of the raw components of the light-transmitting material is dropped onto the slurry to form a coating layer of the light-transmitting material on the surface of the core material. Then, the slurry is separated into solid and liquid and dried to obtain a substrate having a surface coated with the light-transmitting material.

[0024] Next, examples of a method for forming a magnetite layer on the surface of a substrate include the following methods. First, the base material is dispersed in water to obtain a slurry. Next, the slurry is stirred in a deoxidized sealed container and Fe 2+ An aqueous solution containing is gradually added. At this time, since the pH fluctuates, the pH is maintained between 6.5 and 14 by using a pH adjuster, and at the same time, the redox potential of the slurry is maintained between about -160 mV and -750 mV by using an oxidizing agent. This allows the magnetite layer to be coated on the substrate. The pH is preferably maintained in the range of 6.5 to 11.0, and the redox potential of the slurry is preferably maintained between about -300 mV and -500 mV by using an oxidizing agent.

[0025] [Coating pigment] The particle size of the coated pigment of the present invention thus produced is not particularly limited, and although it depends on the application, it is generally a volume average particle size (D 50 ) is preferably 0.5 μm or more. If the particles are finer than 0.5 μm, the amount of reflected light from the particle surface increases, making it difficult to obtain high saturation interference colors.

[0026] For example, when used in paint, if the particle size is between 0.5 μm and 50 μm, the protrusion of coarse particles on the coating surface is eliminated, allowing for smooth coating. Furthermore, when the coated pigment is used in printing, for example in screen printing or gravure printing, the particle size is preferably about 20 μm or less in order to prevent clogging of the printing plate and ensure hiding power. Furthermore, larger sizes can be selected for cosmetics and resin injection moldings, and by using coated pigments of 50 μm or more, it is possible to obtain a grainy design that has the shine of the base material.

[0027] The particle shape of the coated pigment is not particularly limited, but flake-like particles are preferred because they enhance brightness, saturation, and color flop properties due to orientation.

[0028] [Firing process] In the present invention, after the magnetite layer is formed, it is sintered under an inert gas atmosphere, a reducing gas atmosphere, or a reduced pressure (or vacuum) of 50 kPa or less, so that it is transformed into an oxygen-deficient magnetite layer, and the crystal lattice constant falls within a predetermined range. The inert gas is not particularly limited, but may be nitrogen gas, argon gas, etc. The reducing gas is not particularly limited, but may be hydrogen gas, natural gas, city gas, etc. Furthermore, a reducing gas atmosphere also includes a reducing gas atmosphere in which a reducing gas is mixed with an inert gas. If the firing process is carried out under conditions of an atmosphere containing oxygen without using such an inert gas or reducing gas, it is difficult to obtain high saturation, and interference colors tend not to appear easily. Even if interference colors appear, interference colors with sufficient significant differences tend not to appear.

[0029] The firing temperature is preferably 300° C. or higher, and more preferably 300° C. or higher and 800° C. or lower. If the temperature is lower than 300° C., oxygen deficiency does not occur and the desired lattice constant cannot be achieved. For this reason, it is difficult to obtain high chroma, and interference colors tend to be difficult to appear. Even if interference colors are appeared, interference colors with sufficient significant differences tend not to be appeared. On the other hand, if the firing temperature exceeds 800°C, the particle size will increase due to the aggregation of the coated iron oxide fine particles, and the aggregation of the iron oxide fine particles on the surface will cause the coated pigment to aggregate with each other, making it impossible to obtain good color development. Furthermore, the durability will decrease due to the melting of the base material itself and peeling of the coating interface due to thermal expansion.

[0030] The calcination time is preferably 5 minutes to 24 hours from the time when the temperature reaches 300°C or higher, and more preferably 30 minutes to 3 hours. If it is less than 5 minutes, sufficient oxygen deficiency is not generated to obtain the desired lattice constant, and if it exceeds 3 hours, the productivity decreases, which is not preferable. Furthermore, even if it is calcined for 24 hours or more, there is almost no further change in the lattice constant, and it is not preferable because it may cause aggregation or damage to the coated pigment.

[0031] [Application] The coated pigment according to the present invention can be mixed with a resin to produce a resin composition having a vivid interference color, which can be applied to sheets such as paper and resin sheets, and various movable and immovable properties to produce coated objects having an interference color. Furthermore, by mixing the coated pigment according to the present invention with various cosmetics, it is possible to obtain cosmetics containing the coated pigment having an interference color.

[0032] [Appearance of the effects of the invention] In this invention, by setting the above-mentioned conditions, particularly the crystal lattice constant of the magnetite layer within a specific range, and combining it with other conditions as necessary, the effects of the above-mentioned invention, that is, high saturation and color development, and various interference colors such as red, blue, yellow to green, etc. can be produced, thereby making it possible to express interference colors of various colors. The conditions for setting the crystal lattice constant of the magnetite layer within a specific range and the other conditions include the thickness of the magnetite layer, the type of material for the base layer, the thickness of the light-transmitting material for the base layer, and firing conditions (firing temperature, firing time, firing environment), etc. EXAMPLES

[0033] The present invention will be described below with reference to examples. First, the test methods and raw materials used in the examples are shown below.

[0034] (Test Method) [Crystal lattice constant] The coated pigment was uniformly filled into a measurement cell, and the magnetite layer of the coated pigment was identified using an X-ray diffractometer (product name: "Smart Lab" (Rigaku Corporation)). The measurement was performed under the following conditions: CuKα radiation was used as the X-ray source, tube voltage was 40 kV, tube current was 30 mA, sampling width was 0.01°, and scan speed was 0.2° / min. Using these results, the "lattice constant refinement" of the integrated powder X-ray analysis software PDXL2 was performed to calculate the lattice constant of magnetite.

[0035] [Color tone] To 4.0 g of the coated pigment, 16.0 g of acrylic resin binder (Nippe Acrylic Autoclear, Nippon Paint Co., Ltd.) was added and mixed uniformly using a planetary mixer deaerator (Mazerustar KK-400W, Kurashiki Boseki Co., Ltd.) to prepare a paint. This was applied onto art paper using an applicator with a 100 μm gap and allowed to dry naturally at room temperature to prepare a coating film for evaluation. The color tone was evaluated using an X-Rite MA68II multi-angle spectrophotometer. The color values ​​were expressed in the L*a*b* color system (CIE1976), and the color was measured by detecting light that was 15° off the regular reflection angle with respect to the incident light. Here, L* represents lightness, color a* represents chromaticity indicating hue and saturation on the red-green axis, b* represents chromaticity indicating hue and saturation on the yellow-blue axis, and ΔE represents the color difference (the distance between two points on the L*a*b* color space) between the embodiment in which a baking process was performed and the comparison example in which the baking process was not performed and which was otherwise under the same conditions.

[0036] [Magnetism] 1.0 g of the coated pigment was placed in a 50 cc glass beaker and 10 g of ion-exchanged water was added to prepare a slurry. Next, a ferrite magnet (φ20 mm, thickness 5 mm, surface magnetic flux density 100 mT) was placed on the outside of the bottom of the beaker and the presence or absence of magnetism was confirmed visually. If the coated pigment is not magnetic, no change occurs in the slurry. However, if the coated pigment is magnetic, the coated pigment will be oriented by magnetism or will gather around the magnet itself, making it possible to visually confirm that the pigment is magnetic.

[0037] (raw materials) [Base material] Flake aluminum pigment...Manufactured by Toyo Aluminum Co., Ltd. Product name: 5422NS IPA: Isopropyl alcohol (Godo Co., Ltd.) 30% hydrogen peroxide solution (Fujifilm Wako Pure Chemical Industries, Ltd.) Ammonia water: Fujifilm Wako Pure Chemical Industries, Ltd.: 25% by mass Tetraethoxysilane: Fujifilm Wako Pure Chemical Industries, Ltd.

[0038] [Magnetite layer] Polyacrylic acid (manufactured by Toa Gosei Co., Ltd., product name: Aron T-50) Sodium acetate…manufactured by Niwagosei Co., Ltd. Ferrous sulfate heptahydrate…Manufactured by Ensho Sangyo Co., Ltd. Sodium hydroxide… Fujifilm Wako Pure Chemical Industries, Ltd.

[0039] <Example 1> (Base material manufacturing process) The substrate used was a commercially available flaky aluminum pigment with a translucent layer made of silica on its surface. First, 150g of flaky aluminum pigment in solid content was added to 1000g of IPA, and the mixture was stirred and mixed at 75°C to obtain a slurry. After stirring 30% hydrogen peroxide for 30 minutes, 100g of ammonia water and ion-exchanged water were added to adjust the pH value of the slurry to 10.0. A solution of 300g of tetraethoxysilane dissolved in 300g of IPA was gradually added dropwise to the mixture, and the mixture was further stirred and mixed at 75°C for 4 hours. The slurry was then subjected to solid-liquid separation and dried in an oven at 150°C for 24 hours to obtain a flaky aluminum substrate with a translucent layer made of silica on its surface.

[0040] (Magnetite layer manufacturing process) 120 g of the base material obtained above and 1,000 g of ion-exchanged water that had been thoroughly degassed with nitrogen were added to a sealed reactor equipped with a stirrer, a pH measuring electrode, and a gas inlet tube to obtain a slurry in which the base material was dispersed in the ion-exchanged water. Next, 1.0 g of polyacrylic acid and 7 g of sodium acetate were added to the above slurry, and the slurry was heated with stirring until it reached 40°C. Next, 110 g of ferrous sulfate heptahydrate was dissolved in 300 g of ion-exchanged water that had been thoroughly deaerated with nitrogen to prepare an aqueous solution, and this aqueous solution of ferrous sulfate was gradually added to the above slurry over a period of 1 hour while stirring. At this time, a 5 wt% aqueous solution of sodium hydroxide was added to adjust the pH to 9. Air was also introduced into the reactor so that the redox potential was -400 mV. After that, the mixture was filtered and washed with water, then washed with IPA, and dried in an oven at 160°C for 6 hours to obtain a magnetite-coated pigment.

[0041] (Firing process) 200 g of the magnetite-coated pigment obtained above was calcined under argon gas at 300°C for 2 hours, resulting in an interference pigment with magnetite lattice constant within the specified range, showing a vivid pink color in the center and red toward the edges. The measurement results of the color tone, magnetism, and crystal lattice constant of the obtained interference pigment are shown in Table 1.

[0042] <Examples 2 to 12 and Comparative Examples 2 to 3> An interference color pigment was obtained according to the method described in Example 1, except for the conditions of each step shown in Table 1. Table 1 shows the measurement results of the color tone, magnetic property, and crystal lattice constant of the obtained interference color pigment.

[0043] <Comparative Examples 1, 4 to 6> A coated pigment was produced in the same manner as in Example 1, except that the conditions for the base material production process and magnetite production process shown in Table 1 were carried out and the firing process was not carried out. The measurement results of the color tone, magnetic property, and crystal lattice constant of the obtained interference color pigment are shown in Table 1.

[0044] [Table 1]

[0045] From the above results, in Examples 1 to 12, which satisfy the requirements of the present invention, dark interference colors with higher saturation were obtained, whereas in Comparative Examples 1 to 6, which do not satisfy the requirements of the present invention, only pale colors with low saturation were obtained, and in some cases no interference colors were produced. Moreover, since each of the examples and comparative examples had magnetism, it became clear that the magnetite layer maintained the magnetite structure. This is also clear from Figures 1 to 4. Figures 1 to 4 show sheets coated with the interference color pigments obtained in each Example and Comparative Example rolled into a cylindrical shape and placed so that the circumferential surface is in contact with a stand (arranged so that the circumferential direction is the up-down direction in each figure). Arranged in this way, the color tone when viewed at an angle nearly perpendicular to the cylindrical surface can be observed in the center, and the color tone when viewed at angles that become smaller from the cylindrical surface can be observed as one moves up and down, so the presence or absence of interference color can be confirmed.

[0046] Example 12 (right) and Comparative Example 6 (left) in Fig. 1 differ in the presence or absence of a firing process, and in whether the crystal lattice constant satisfies a predetermined range. Example 12 had a high saturation of vivid yellow (center) to vivid green (upper and lower parts), and a clear interference color was obtained with respect to the change in color tone, whereas Comparative Example 6 had a light yellow color with a low saturation, making it difficult to see the change in color tone between the center and the upper and lower parts, and no clear interference color was obtained.

[0047] Example 11 (right) and Comparative Example 5 (left) in Fig. 2 differ in the presence or absence of a firing process, and in whether the crystal lattice constant satisfies a predetermined range. In Example 11, the center is bright orange, and the color changes from bright yellow to bright green toward the top and bottom, with high saturation and clear interference colors in terms of the change in color tone, whereas in Comparative Example 5, the color is light beige (center) to light yellow (top and bottom), and the saturation is not very high, and although there is a change in color tone between the center and the top and bottom, it is difficult to say that a clear interference color was obtained.

[0048] Example 4 (right) and Comparative Example 1 (left) in Fig. 3 differ in the presence or absence of a firing process, and in whether the crystal lattice constant satisfies a predetermined range. In Example 4, the center is bright red, and the color changes from bright orange to bright green toward the top and bottom, with high saturation and a clear interference color with respect to the change in color tone, whereas in Comparative Example 1, the center is light pink, and the color changes to light yellow toward the top and bottom, but the saturation is not very high, and although there is a change in color tone between the center and the top and bottom, it is difficult to say that a clear interference color was obtained.

[0049] Example 10 (right) and Comparative Example 4 (left) in Figure 4 differ in the conditions of the firing process, and in whether the crystal lattice constant satisfies a predetermined range. In Example 10, the center is bright blue, and changes to bright reddish purple toward the top and bottom, with high saturation and clear interference colors in the change in color tone, whereas in Comparative Example 4, the color is silver overall, and no interference colors can be confirmed.

Claims

1. The magnetite layer is provided on a substrate having at least a surface made of a light-transmitting material, and the magnetite layer covers the substrate. The magnetite layer has a crystal lattice constant of 8.35 Å or more; A coated pigment, wherein the substrate is a metal flake coated with the light-transmitting material.

2. 2. The coated pigment according to claim 1, wherein the light-transmitting material is at least one selected from the group consisting of silica, alumina, glass, mica, and resin.

3. 3. The coated pigment according to claim 1, wherein the metal flakes are at least one selected from the group consisting of aluminum, copper, nickel, tin, titanium, zinc, an alloy containing at least one of these, and stainless steel.

4. 4. The coated pigment according to claim 1, further comprising a protective layer on the magnetite layer, the protective layer being made of a metal oxide, a metal hydroxide, a metal oxide hydrate, a resin, or a combination thereof.

5. A resin composition comprising the coated pigment according to any one of claims 1 to 4.

6. A coated article comprising the resin composition according to claim 5 coated on a substrate.

7. A cosmetic preparation comprising the coated pigment according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Magnetic pearlescent pigment and preparation method thereof

    CN101445674A

  • Inorganic pigment consisting of solid solution of different spinels

    JP1978026299A

  • Production of colored pearlescent pigment

    JP1986019666A

  • High-chroma orange-colored pearl pigment

    JP1998259318A

  • Colored metallic powdery pigment and coating material composition

    JP1999080587A