Design method for hot rolling of triple-layer clad plate and manufacturing method of triple-layer clad plate

The method addresses low productivity and warping issues in three-layer clad plates by optimizing material properties and thickness ratios, resulting in improved manufacturing efficiency and reduced warping.

JP7557324B2Active Publication Date: 2024-09-27MA ALUMINUM CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2020163610
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-09-27
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Existing methods for manufacturing three-layer clad plates face challenges such as low productivity and warping due to limitations in thickness, material properties, and unstable lubrication control during hot rolling.

Method used

A method for designing and manufacturing three-layer clad plates using aluminum-based alloys with specific thickness ratios, deformation resistances, and strain rate sensitivity coefficients to minimize warping, involving a core material and two skin materials with optimized parameters.

Benefits of technology

The method enhances productivity and reduces warping in three-layer clad plates by selecting materials with controlled thickness ratios and strain rate sensitivity coefficients, ensuring high manufacturing efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557324000007
    Figure 0007557324000007
  • Figure 0007557324000010
    Figure 0007557324000010
  • Figure 0007557324000009
    Figure 0007557324000009
Patent Text Reader

Abstract

To provide a design method for hot rolling of a three-layer clad plate that improves productivity and can reduce warpage.SOLUTION: A design method for three-layer clad plate is a design method for hot rolling when manufacturing a three-layer clad plate by locating a first skin material on one surface side of a core material and locating a second skin material on the other surface side of the core material, and performing hot-rolling. In the method, when a difference of plate thickness ratio between the first skin material and the second skin material before hot-rolling is represented by ΔCL and deformation resistances of the core material, the first skin material and the second skin material before hot-rolling are represented by sc, s1, s2, Δs and S are respectively defined with a prescribed formula, when strain rate sensitivity coefficients of the core material, the first skin material and the second skin material before hot-rolling are represented by mc, m1, m2, Δm and M are respectively defined with a prescribed formula, and when S>0.65 and |ΔCL|>0.1 or when S≤0.65, the core material, the first skin material and the second skin material are selected to as to become a condition that satisfies the prescribed formula.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for designing hot rolling of a triple-layer clad plate and a method for manufacturing a triple-layer clad plate. [Background technology]

[0002] Conventionally, clad metal plates in which a plurality of metal plates are joined together are known. As a method for manufacturing such clad plates, Patent Document 1 describes a method in which a base material, a cladding material, and a covering material are stacked together to form a layered assembly material, which is hot-rolled, and then the covering material is removed. However, this method requires additional work to separate the covering material after hot rolling. In addition, since there is a limit to the thickness that can be hot-rolled, there is a limit to the plate thickness of the base material, the cladding material, and the covering material, and ultimately the productivity is low.

[0003] In Patent Document 2, when manufacturing a two-layer clad material by hot rolling, the diameters of the upper and lower work rolls are made unequal, and further, the lubrication state between the work rolls and the rolled material is adjusted to prevent warping. However, this method requires changing the work rolls for each material characteristic, which results in low productivity. In addition, it is difficult to control the lubrication state stably, which ultimately results in low productivity.

[0004] In Patent Document 3, in a manufacturing method of a clad steel plate made of carbon steel as a base material and stainless steel as a clad material, warping is prevented by controlling the cooling conditions after the start of rolling. However, in this method, cooling water is sprayed from above the conveying table onto the material to be rolled, which is placed on the conveying table, so that the material to be rolled is pressed against the conveying table, which may cause scratches on the surface, thereby degrading the quality of the clad steel plate.

[0005] In Patent Document 4, in a hot rolling method for clad steel made of an iron alloy as a base material and copper or a copper alloy as a clad material, warping is prevented by rolling so that the rolling temperature and the transformation temperature of the iron alloy satisfy a predetermined formula. However, this method cannot be applied to clad materials with three or more layers. In addition, since it does not consider the strain rate sensitivity coefficient, it is not a concept that can accurately reduce warping.

[0006] In Patent Document 5, a laminated material is sealed with a cover steel plate to form a cover steel plate assembly, which is sandwiched between a steel base material and a warp prevention material, and the steel base material and the warp prevention material are welded together before hot rolling, and then the cover steel plate is removed to prevent warping. However, this method requires a lot of work for preparation before rolling and for removing the cover steel plate after rolling.

[0007] In Patent Document 6, a hot rolling control device for clad steel plate prevents warping by controlling the upper and lower rolls with different systems and rolling at different speeds. However, this device has a problem in that it cannot fully control the configuration of clad material that causes large warping.

[0008] Patent Document 7 describes a method for manufacturing a three-layer clad aluminum alloy plate by specifying a small reduction ratio in the early stage of rolling to eliminate poor bonding and to suppress warpage to a minimum, thereby avoiding impossibility of manufacturing. However, this method has the problem that productivity decreases when the reduction ratio is reduced. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Publication No. 61-232075 [Patent Document 2] Japanese Patent Application Publication No. 62-259607 [Patent Document 3] Japanese Patent Application Publication No. 5-23702 [Patent Document 4] Japanese Patent Application Publication No. 59-56903 [Patent Document 5] Japanese Patent Publication No. 158583 / 1983 [Patent Document 6] Japanese Utility Model Application Publication No. 60-131213 [Patent Document 7] Japanese Patent Application Publication No. 9-184038 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a design method for hot rolling of a three-layer clad plate and a manufacturing method for a three-layer clad plate, which have high productivity and can reduce warping. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention employs the following configuration. [1] A method for designing the hot rolling when manufacturing a three-layer clad plate by hot rolling, the method comprising: arranging a first skin material made of a metal plate different from the core material on one side of the core material; arranging a second skin material made of a metal plate different from the core material on the other side of the core material; and hot rolling the resulting three-layer clad plate, the core material, the first skin material, and the second skin material are each made of pure aluminum or an aluminum-based alloy, A total thickness CL of the core material, the first skin material, and the second skin material before the hot rolling T The plate thickness ratio CL1, which is the ratio of the thickness of the first skin material to the total thickness CL T The difference between the thickness ratio CL1 and the thickness ratio CL2, which is the ratio of the thickness of the second skin material to the thickness ratio CL2, is defined as ΔCL (CL1-CL2), The strain rate of the core material, the first skin material, and the second skin material before the hot rolling is 0.1 sec -1 The deformation resistance at the hot rolling temperature in c , s1, and s2, Δs and S are defined as the following formulas (1) and (2), respectively: The strain rate sensitivity coefficients of the deformation resistance at the hot rolling temperature of the core material, the first skin material, and the second skin material before the hot rolling are respectively defined as m c , m1, m2, and Δm and M are defined as in the following formula (3) and the following formula (4), respectively: A design method for hot rolling of a three-layer clad plate, characterized in that when S>0.65 and |ΔCL|>0.1, or when S≦0.65, the core material, the first skin material, and the second skin material are selected so as to satisfy the condition of the following formula (5). Δs=(s1-s2) / s c …(1) S = 0.5(s1 + s2) / s c …(2) Δm = m1 - m2 … (3) M = 0.5(m1+m2) / m c …(4) |k1Δs+k2Δm+k3ΔCL|≦0.3 …(5) However, when S>0.65 and |ΔCL|>0.1, in the above formula (5), k1=1.0, k2=2.6, and k3=-9.9+7.7S+1.5M. When S≦0.65, k1=-1.0, k2=-0.7, and k3=1.2-3.2S-4.3M in the above formula (5). However, the case where ΔCL=Δs=Δm=0 is excluded. do. [2] The core material is formed from an Al-Mn based aluminum-based alloy. [1] A method for designing hot rolling of a three-layer clad plate according to the present invention. [3] The first skin material is formed from an Al-Si aluminum-based alloy. [1] or [2] A method for designing hot rolling of a three-layer clad plate according to claim 1. [4] The second skin material is made of an Al-Zn aluminum-based alloy. [1] ~[3] A method for designing hot rolling of a three-layer clad plate according to claim 1. [5] A method for manufacturing a three-layer clad plate, comprising the steps of: using the core material, the first skin material, and the second skin material selected in the design method for hot rolling of a three-layer clad plate described in any one of [1] to [4]; arranging the first skin material and the second skin material on one side and the other side of the core material, respectively; and hot rolling the core material.

[0012] In this specification, “k1Δs+k2Δm+k3ΔCL” on the left side of the above equation (5) may be referred to as a parameter P. Effect of the Invention

[0013] According to the present invention, it is possible to provide a design method for hot rolling of a triple-layer clad plate and a manufacturing method for a triple-layer clad plate, which are highly productive and capable of reducing warpage. [Brief description of the drawings]

[0014] [Figure 1]FIG. 1 is a model diagram showing a rolling analysis model using the finite element method when a core material, a first skin material, and a second skin material are hot-rolled to produce a three-layer clad plate. [Diagram 2] FIG. 2 is a graph showing the relationship between the Δs value and the curvature for Nos. 1 to 5, 6 to 9, 10 to 15, and 16 to 21 in Table 1. [Diagram 3] FIG. 3 is a graph showing the relationship between Δm value and curvature for Nos. 22 to 38 in Table 1. [Figure 4] FIG. 4 is a graph showing the relationship between ΔCL value and curvature for Nos. 39 to 56 in Table 1. [Diagram 5] FIG. 5 is a graph showing the relationship between the parameter P and the predicted value of the curvature of the three-layer clad plate for Nos. 1 to 56 in Table 1, Nos. 57 to 60 in Table 4, and Nos. 61 to 82 in Table 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] When a triple-layer clad plate is manufactured by placing a first skin on one side of a core material and a second skin on the other side of the core material and then hot rolling the plate, warping may occur. For example, if the first skin and the second skin are the same thickness and the deformation resistance of the first skin is smaller than the deformation resistance of the second skin, i.e., if the first skin is easily stretched, the first skin will elongate more than the second skin during hot rolling, and the triple-layer clad plate will warp toward the second skin after hot rolling.

[0016] Furthermore, for example, if the deformation resistance of the first skin material and the deformation resistance of the second skin material are the same and the thickness of the second skin material is greater than the thickness of the first skin material, assuming that the rolling reduction amounts for the first skin material and the second skin material are approximately the same, the elongation of the first skin material increases during hot rolling, and the three-layer clad plate after hot rolling warps towards the second skin material.

[0017] Therefore, in the past, when rolling a triple-layer clad plate, the thicknesses and deformation resistances of the first and second skin materials placed on either side of the core material were made close to each other by ensuring symmetry of shape and material, thereby preventing warping of the triple-layer clad plate after hot rolling.

[0018] However, after extensive research, the inventors have found that the elongation of the skin material during hot rolling is affected not only by the deformation resistance and thickness, but also by the strain rate sensitivity coefficient of the deformation resistance at the hot rolling temperature. That is, by focusing on the strain rate sensitivity coefficients of the first skin material and the second skin material and selecting the first skin material and the second skin material so as to optimize the combination of the respective strain rate sensitivity coefficients of the first skin material and the second skin material, it has been found that even when the symmetry of the thickness and deformation resistance of the first skin material and the second skin material arranged on both sides of the core material cannot be ensured, the warpage of the triple-layer clad plate after hot rolling can be reduced.

[0019] Furthermore, as a result of the analysis by the inventors using the finite element method, the total thickness CL of the core material, the first skin material, and the second skin material before hot rolling T The thickness ratios CL1 and CL2 of the first and second skin materials, ΔCL (=CL1-CL2), and the deformation resistances s c , s1, s2, and the strain rate sensitivity coefficient m c It has been found that when the absolute value of the parameter P calculated from the relational expression among m1, m2, m2 is 0.3 or less, more preferably 0.24 or less, the warpage of the three-layer clad plate after hot rolling can be reduced.

[0020] First, the inventors predicted the amount of warpage of a triple-layer clad plate after hot rolling by the finite element method. Since it is empirically known that simulations reproduce reality well in plastic processing such as clad rolling, the inventors investigated many conditions using a model material and found conditions that would reduce warpage, as described below.

[0021] Figure 1 shows a rolling analysis model using the finite element method. The rolling analysis model was constructed in two dimensions, assuming plane strain with constant sheet width. The shape of the finite element model was determined based on the thickness of each layer of the triple-layer clad plate and the diameter of the rolling roll. The rolling roll was also defined as a rigid body, a two-dimensional circle. In other words, the total thickness of the triple-layer clad plate before hot rolling (the total thickness of the core, first skin and second skin before hot rolling, CL TThe rolling direction length of the finite element model is the same for the core, first skin, and second skin, and the total thickness (CL T ) was set to 2.3 times or more. Regarding element division in the longitudinal direction, the length of each element in the longitudinal direction was set to be the same for the core material, the first skin material, and the second skin material, and was set to 1 / 20 or less of the roll radius. Furthermore, the friction coefficient between the workpiece (core material, the first skin material, and the second skin material) and the rolling rolls was set to 0.3 according to the Coulomb model.

[0022] In addition, the reduction ratio in the rolling analysis model was set to 6%. This is because it is empirically predicted that if the warpage is small under the condition of a reduction ratio of 6%, the rolling can be continued at a relatively large reduction ratio, and efficient manufacturing can be achieved. Since the tendency of warpage does not change if the reduction ratio is 2 to 10%, when manufacturing the three-layer clad plate according to the present invention by hot rolling, as described later, it is preferable to set the rolling ratio to 2 to 10%.

[0023] Regarding element division in the thickness direction, the length of each element in the thickness direction was set to 1 / 10 or less of the core thickness for the core, and 1 / 4 or less of the thickness of each skin for the first and second skins. In this case, if the aspect ratio in the longitudinal direction / thickness direction was less than 1 / 2 or more than 2, the elements were further divided so that the aspect ratio was between 1 / 2 and 2.

[0024] The interface between the core and the first skin, and the interface between the core and the second skin, were bonded by sharing nodes of the finite elements.

[0025] As the physical property value of plastic deformation, the stress σ of the core material, the first skin material, and the second skin material was input using the following strain rate dependent formula (A). In formula (A), s is the strain rate ε v where s is the deformation resistance at strain ε = 0.1, and m is the strain rate sensitivity coefficient. The deformation resistance s and the strain rate sensitivity coefficient m were measured based on the deformation resistance at strain ε = 0.1 by performing uniaxial tensile tests or uniaxial compression tests with varying strain rates.

[0026] σ = s(ε v / 0.1) m …(A)

[0027] As physical values ​​of elastic deformation, for aluminum and aluminum-based alloys, Young's modulus was 40 GPa and Poisson's ratio was 0.3. Since Young's modulus and Poisson's ratio of aluminum alloys are less dependent on alloy components, the above values ​​were used as they are considered to be representative values ​​around 400 to 500°C. It should be noted that it has been confirmed that the warping of clad metal plates is largely due to plastic deformation characteristics and is not significantly affected by elastic properties.

[0028] Similarly, for copper and copper-based alloys, a Young's modulus of 50 GPa and a Poisson's ratio of 0.35 were used, and for titanium, a Young's modulus of 60 GPa and a Poisson's ratio of 0.35 were used.

[0029] Furthermore, after the rolling analysis, the warpage of the three-layer clad plate was calculated by selecting 8 to 12 nodes in the center of the thickness from the steady part of the rolling, and calculating the curvature (mm -1 ) and calculate this curvature (mm -1 ) was used for evaluation.

[0030] The results of rolling analysis using the finite element method under the above conditions are shown in Table 1. Table 1 shows the curvature (mm ) of the clad plate after hot rolling under each condition (No. 1 to No. 56) when the characteristic values ​​of the core material, first skin material, and second skin material are changed when manufacturing a triple-layer clad plate by stacking the core material, first skin material, and second skin material together and hot rolling them. -1 The characteristic values ​​of the core, first skin and second skin were changed as follows: c , s1, s2, strain rate sensitivity coefficient m c , m1, m2, the sheet thickness ratios CL1, CL2 of the first skin material and the second skin material, and the difference therebetween ΔCL (CL1-CL2).

[0031] Δs, Δm, S, and parameter P in Table 1 were calculated from the following formulas (B) to (E). Parameter P in the table is the calculated value of "k1Δs+k2Δm+k3ΔCL" in the left side of the following formula (C). The present inventors found that the term on the right side of formula (C) (the absolute value of parameter P) correlates well with the amount of warpage after hot rolling.

[0032] From the results shown in Table 1, it was estimated that warpage of a triple-layer clad plate would be reduced under the conditions that S calculated by the following formula (B) exceeds 0.65 (S>0.65), the absolute value of ΔCL exceeds 0.1 (|ΔCL|>0.1), and the absolute value of parameter P is 0.3 or less (satisfying the following formula (C)). It was also estimated that warpage of a triple-layer clad plate would be further reduced under the conditions that the absolute value of parameter P is 0.24 or less.

[0033] From the results shown in Table 1, it was also estimated that warpage of the triple-layer clad plate would be reduced under the condition that S calculated by the following formula (B) is 0.65 or less (S≦0.65) and the absolute value of the parameter P is 0.3 or less (satisfying the following formula (C)). It was also estimated that warpage of the triple-layer clad plate would be further reduced under the condition that the absolute value of the parameter P is 0.24 or less.

[0034] More specifically, in Table 1, the condition of the example is that the parameter P is not less than -0.30 and not more than 0.30, and the condition of the comparative example is that the parameter P is less than -0.30 or more than 0.30. -5 (mm -1 )~8.0×10 -5 (mm -1 ) range. On the other hand, in the comparative example, the curvature is in the range of -8.0×10 -5 (mm -1 ) or less than 8.0 × 10 -5 (mm -1 In this way, the deformation resistance s of the core, first skin and second skin is set to a range of 0.30 or less so that the absolute value of the parameter P is 0.30 or less. c , s1, s2, strain rate sensitivity coefficient m cIt was revealed that it is possible to predict that the warpage of the three-layer clad plate after hot rolling can be reduced by adjusting the thickness ratios CL1, CL2 of the first skin material and the second skin material, and the difference ΔCL (CL1-CL2) between them.

[0035] [Table 1]

[0036] S = 0.5(s1 + s2) / s c …(B)

[0037] |k1Δs+k2Δm+k3ΔCL|≦0.3 …(C)

[0038] Δs=(s1-s2) / s c …(D)

[0039] Δm = m1 - m2 … (E)

[0040] M = 0.5(m1+m2) / m c …(F)

[0041] Here, s in the above formulas (B) and (D) c , s1, s2 are the strain rates of the core, first skin and second skin, respectively, 0.1 sec -1 is the deformation resistance at the hot rolling temperature.

[0042] In addition, Δs in the above formula (C) is calculated by the above formula (D), and Δm is calculated by the above formula (E). In addition, ΔCL in the above formula (C) is the difference between the sheet thickness ratios CL1 and CL2 of the first and second skin materials (ΔCL=CL1-CL2). The sheet thickness ratio CL1 of the first skin material is the total thickness CL of the core material, the first skin material, and the second skin material. T The thickness ratio CL2 of the second skin is the ratio of the thickness of the first skin to the total thickness CL T is the ratio of the thickness of the second skin material to the thickness of the first skin material.

[0043] In addition, the coefficients k1, k2, and k3 in the above formula (C) are coefficients determined according to S and ΔCL. That is, when S>0.65 and |ΔCL|>0.1, k1=1.0, k2=2.6, and k3=-9.9+7.7S+1.5M. In addition, when S≦0.65, k1=-1.0, k2=-0.7, and k3=1.2-3.2S-4.3M. Here, M in the formula for determining the coefficient k3 is calculated by the above formula (F). These coefficients k1, k2, and k3 are empirically calculated.

[0044] In the above formulas (E) and (F), m1 and m2 are strain rate sensitivity coefficients of the deformation resistance at the hot rolling temperature of the first skin material and the second skin material, respectively, and are calculated from the above formula (A). c is the strain rate sensitivity coefficient of the deformation resistance at the hot rolling temperature of the core material, and is calculated from the above formula (A).

[0045] The above formulas (B) to (F) and the method for determining the coefficients k1, k2, and k3 will be described later.

[0046] Hereinafter, a design method for hot rolling of a triple-layer clad plate (hereinafter sometimes referred to as a "design method"), a manufacturing method for a triple-layer clad plate, and a triple-layer clad plate according to embodiments of the present invention will be described.

[0047] The design method of this embodiment is based on the above findings, and the thicknesses of the core material, the first skin material, and the second skin material before hot rolling, the thickness ratios CL1, CL2, ΔCL, the deformation resistance s c , s1, s2 and strain rate sensitivity coefficient m c The core material, the first skin material, and the second skin material are selected so that m1, m2, and m3 satisfy the condition of formula (C) above. In other words, the hot rolling design method of this embodiment selects the thicknesses, thickness ratios CL1, CL2, ΔCL, deformation resistance s c , s1, s2 and strain rate sensitivity coefficient m cWhen the absolute value of parameter P, which is the term on the left side of the above formula (C), is 0.3 or less, it is predicted that the amount of warpage of the triple-layer clad plate after hot rolling will be small, and hot rolling is judged to be possible. More preferably, the absolute value of parameter P is 0.24 or less. When the absolute value of parameter P is 0.24 or less, it is predicted that the amount of warpage of the triple-layer clad plate after hot rolling will be even smaller, and therefore it is more preferable.

[0048] The core material, the first skin material, and the second skin material may each be pure aluminum or an aluminum-based alloy. The core material, the first skin material, and the second skin material may each be pure copper or a copper-based alloy. The core material, the first skin material, and the second skin material may each be pure aluminum, an aluminum-based alloy, pure copper, a copper-based alloy, titanium, a titanium-based alloy, magnesium, or a magnesium-based alloy.

[0049] Next, characteristic values ​​used in the design method of this embodiment will be described. There is no particular restriction on the thickness of the core material, the first skin material, and the second skin material, but due to restrictions on hot rolling equipment, the total thickness of the core material, the first skin material, and the second skin material before hot rolling, CL T It is preferable that the distance be, for example, 600 mm or less.

[0050] The total thickness of the core, first skin and second skin is CL T The plate thickness ratio CL1, which is the ratio of the thickness of the first skin material to the total thickness CL T A plate thickness ratio CL2, which is the ratio of the thickness of the second skin material to the plate thickness ratio CL1, is calculated. Furthermore, a plate thickness ratio ΔCL, which is the difference between the plate thickness ratio CL1 and the plate thickness ratio CL2 (CL1-CL2), is calculated.

[0051] In addition, the strain rate of the core, first skin and second skin is 0.1 sec -1 Deformation resistance at hot rolling temperature s c , s1, and s2 are calculated. c How to calculate s1 and s2 will be described later.

[0052] Furthermore, S is calculated from the above formula (B), and Δs is calculated from the above formula (D).

[0053] In addition, the strain rate sensitivity coefficient m of the deformation resistance at the hot rolling temperature of the core material, the first skin material, and the second skin material c , m1, and m2 are calculated from the above formula (A). The strain rate sensitivity coefficient m c Specific methods for measuring m1, m2 will be described later.

[0054] Furthermore, Δm is calculated from the above formula (E), and M is calculated from the above formula (F).

[0055] Then, a parameter P is calculated as the calculated value of "k1Δs+k2Δm+k3ΔCL" on the left side of the above formula (C) and determined. If the parameter P is within the range of -0.3 to 0.3 (if the above formula (C) is satisfied), it is estimated that warpage will be small when hot rolling is performed with the selected combination of core material, first skin material, and second skin material, and it is determined that rolling is possible, whereas if the parameter P is less than -0.3 or more than 0.3, it is estimated that warpage will be large when hot rolling is performed, and it is determined that rolling is impossible.

[0056] In the design method of this embodiment, the case of S>0.65 and |ΔCL|>0.1 or the case of S≦0.65 is the prediction target, and the case of S>0.65 and |ΔCL|≦0.1 is not the prediction target of this embodiment.

[0057] In the range of S>0.65 and |ΔCL|≦0.1, which is outside the scope of prediction in this embodiment, the asymmetry of the shape of the material before hot rolling is small to begin with, and hot rolling can be easily performed within this range, so there is little need to limit the absolute value of the parameter P. Therefore, the range of S>0.65 and |ΔCL|≦0.1 is outside the scope of this embodiment.

[0058] On the other hand, in the range of S>0.65 and |ΔCL|>0.1, the difference in the sheet thickness ratio between the first skin material and the second skin material becomes excessive, and the asymmetry of the shape of the material before hot rolling increases, and it is expected that the amount of warpage will increase. Therefore, in the range of S>0.65 and |ΔCL|>0.1, the parameter P including Δs, Δm, and ΔCL needs to be in the range of -0.3 to 0.3. If the parameter P is in the range of -0.3 to 0.3, the amount of warpage can be reduced even when the asymmetry of the shape of the material is large.

[0059] Furthermore, when S≦0.65, the deformation of the core material is small, and the deformation of the first skin material and the second skin material is likely to be concentrated, the asymmetry of the material before hot rolling becomes prominent, the amount of warpage is likely to be large, and rolling becomes difficult. Therefore, even when S≦0.65, the parameter P including Δs, Δm, and ΔCL needs to be in the range of -0.3 to 0.3. If the parameter P is in the range of -0.3 to 0.3, the amount of warpage can be reduced even when the material shape is highly asymmetric.

[0060] Next, the core, first skin and second skin are strained at a rate of 0.1 sec -1 Deformation resistance at hot rolling temperature s c The measurement methods for s1, s2 and s3 are described below. The strain rate sensitivity coefficients m c We also describe how to measure m1 and m2.

[0061] The test pieces are cylindrically cut from the center of the thickness and width of the core, first skin, and second skin. The axial direction of the cylinder is cut to match the thickness direction of the material to be rolled. The dimensions of the test piece are 8 mm in diameter and 12 mm in height.

[0062] The test piece is heated to the test temperature at a rate of 60°C / min or more, and is held at that temperature for 2 to 6 minutes after reaching the test temperature, and then compressed. The test temperature can be selected from the temperature at which the material being examined will be hot-rolled. For example, for aluminum, the range is 300 to 600°C. Just before compression, the test piece is allowed to run 0.5 mm free (run-up), and strain is applied to the test piece at a constant strain rate during compression. At this time, the strain is logarithmic strain (true strain).

[0063] From the change in the height of the test piece before and after compression, the amount of compression L sample,end Measure.

[0064] On the other hand, during compression, the load F and the displacement L measure The point where the load rises from the free run (approach) is regarded as the zero point of displacement.

[0065] Displacement L measured during compression measure Since it includes the effect of deformation of each part of the device due to the load, the displacement L at the moment when compression is completed measure,end and the compression amount L sample,end does not match perfectly. Displacement L measure This means that correction is necessary. Therefore, the displacement L measure L correct =(L sample,end / L measure,end )×L measure Linear correction is performed using

[0066] Corrected displacement L correct and the original height H of the specimen initial Strain ε = |ln((H initial -L correct ) / H initial )| is required.

[0067] The stress is calculated by dividing the test load by the cross-sectional area during compression. Assuming a constant volume, the cross-sectional area during compression is A = (H initial / (H initial -L correct ))×A initial In addition, A initial is the cross-sectional area of ​​the cylindrical specimen before compression.

[0068] The deformation resistance σ is obtained when the strain ε=0.1.

[0069] Such an evaluation is called the strain rate ε v 0.01sec -1 , 0.1sec -1 , 1sec -1 Each test was performed at a strain rate of 0.1 sec -1 The average value of the results at s(s c , s1, s2).

[0070] In addition, the above results are expressed as σ=s(ε v / 0.1) m The strain rate sensitivity coefficient m(m c , m1, m2).

[0071] Next, a method for manufacturing the three-layer clad plate of this embodiment will be described. In the manufacturing method of a three-layer clad plate of this embodiment, the core material, first skin material, and second skin material selected by the above design method are used, the first skin material and the second skin material are placed on one side and the other side of the core material, respectively, and the three-layer clad plate is manufactured by hot rolling.

[0072] The heating temperature before hot rolling is, for example, in the range of 300 to 600°C when the core material, first skin material, and second skin material are each pure aluminum or an aluminum-based alloy, in the range of 400 to 1000°C when the core material, first skin material, and second skin material are each pure copper or a copper-based alloy, in the range of 600 to 1000°C when the core material, first skin material, and second skin material are titanium or a titanium-based alloy, and in the range of 300 to 500°C when the core material, first skin material, and second skin material are magnesium or a magnesium-based alloy.

[0073] Furthermore, when the core material, the first skin material, and the second skin material are made of different materials, for example, when aluminum and copper are combined, it is preferable to take into consideration the recrystallization temperature and melting point of each metal and adjust the heating temperature for the hot rolling to be within a range of not less than the recrystallization temperature and not more than the melting point of each metal.

[0074] The reduction rate of the hot rolling may be 2% or more, or may be 4% or more. If the reduction rate is 2% or more, the bonding strength between the core material, the first skin material, and the second skin material can be made sufficient, and if it is 4% or more, the manufacturing efficiency can be further improved. There is no need to limit the upper limit of the reduction rate. In addition, if the reduction rate is within a certain range, there is a tendency for the increase in the amount of warping to be suppressed, so it may be, for example, 30% or less, 20% or less, or 10% or less.

[0075] The three-layer clad plate manufactured by hot rolling is made of the core material, the first skin material, and the second skin material selected by the above design method. This three-layer clad metal plate has a curvature of -8.00×10 -5 mm -1 ~8.00×10 -5 mm -1 The range is as follows:

[0076] Next, the reason for deriving the above formula (C) used in the determination method of this embodiment will be explained. In the rolling analysis by the finite element method described above, as shown in Nos. 1 to 56 in Table 1, model materials assuming predetermined material properties were used to evaluate the effects of the properties and the cladding ratio.

[0077] FIG. 2 is a graph showing the relationship between the Δs value and the curvature for Nos. 1 to 5, 6 to 9, 10 to 15, and 16 to 21. The effect of the Δs value in formula (D) can be confirmed in conditions No. 1 to 21. In Table 1 and Figure 2, conditions No. 1 to 21 are divided into ranges of S value, with No. 1 to 9 being conditions where S>0.65, and No. 10 to 21 being conditions where S≦0.65. In addition, when No. 1 to 5, No. 6 to 9, No. 10 to 15, and No. 16 to 21 are each grouped, only Δs is varied within each group. Note that s1, s2, and s c Since s is a physical quantity with units (MPa), cThe S value is an average evaluation value that determines whether the bark is softer than the heartwood (formula (B)).

[0078] As shown in Figure 2, it can be seen that there is a nearly linear correlation between the Δs value and warpage. For Nos. 1 to 9 (S > 0.65), there is a positive correlation and the slope is roughly constant. This can be interpreted as meaning that the harder material does not stretch during rolling, but is pulled and warps instead. Additionally, for Nos. 10 to 21 (S ≦ 0.65), there is a negative correlation and the slope is roughly constant. This is thought to be due to the influence of strain being concentrated only on the surface due to the soft skin material, which is the opposite of the trend for Nos. 1 to 9.

[0079] Next, FIG. 3 shows a graph of the relationship between Δm value and curvature for Nos. 22 to 38. As shown in Fig. 3, the effect of Δm can be confirmed in No. 22 to 38. In Table 1 and Fig. 3, No. 22 to 38 are classified by S value, No. 22 to 30 have S>0.65, and No. 31 to 38 have S≦0.65. In addition, when No. 22 to 25, No. 26 to 30, No. 31 to 34, and No. 35 to 38 are each grouped, only Δm is varied within each group. Note that m1, m2, and m c Since is a dimensionless number with no unit, m c No division by is performed.

[0080] As shown in Figure 3, Δm and warpage show a nearly linear correlation. For Nos. 22-30 (S>0.65), there is a positive correlation between Δm and warpage, and the slope is roughly constant. It can be interpreted that the larger m1 and m2 are, the harder they are due to strain, making them less likely to stretch when rolled, and the tension that causes them to warp. For Nos. 31-38 (S≦0.65), there is a small negative slope. This is thought to be due to the fact that the skin material is soft, so strain is concentrated only on the surface, and is the opposite of the trend for Nos. 22-30.

[0081] Next, FIG. 4 shows a graph of the relationship between ΔCL value and curvature for Nos. 39 to 56. As shown in Figure 4, the effect of ΔCL can be confirmed in Nos. 39 to 56. In Table 1 and Figure 4, Nos. 39 to 56 are classified by S value, with Nos. 39 to 48 having S>0.65 and Nos. 49 to 56 having S≦0.65. Additionally, when Nos. 39 to 43, Nos. 44 to 48, Nos. 49 to 52, and Nos. 53 to 56 are each grouped, only ΔCL is varied within each group.

[0082] As shown in Figure 4, there is a nearly linear correlation between ΔCL and warpage. It is suggested that the slope changes depending on the physical properties of the core and skin materials. When the S value is large, the skin material with the larger sheet thickness, either the first or second skin material, does not receive all the strain, while the skin material with the smaller sheet thickness tends to receive the rolling strain evenly, resulting in warpage on the side where the strain is not fully received. The degree of this phenomenon varies depending on the strength of the material. Note that ΔCL is only considered in the negative range because this is sufficient from the standpoint of symmetry, and ΔCL is not limited to being negative.

[0083] Based on the above trends, we came up with the idea of ​​expressing warpage using the following parameter P.

[0084] P = k1Δs + k2Δm + k3ΔCL

[0085] The coefficient k1 of Δs and the coefficient k2 of Δm in the above formula correspond to the slope of the straight lines shown in Figures 2 and 3. From the above considerations, it was thought that k1 and k2 could be constants. On the other hand, the coefficient k3 of ΔCL depends on the physical properties as shown in Figure 4. Since Δs and Δm have already been used, it was considered to express the coefficient k3 with S and M. After careful consideration based on the results of No. 1 to No. 56, it was found that there is a good correlation between the parameter P and the warpage (curvature) in the simulation by setting the coefficients as shown below.

[0086] When S>0.65, k1=1.0, k2=2.6, k3=-9.9+7.7S+1.5M

[0087] When S≦0.65, k1=-1.0, k2=-0.7, and k3=1.2-3.2S-4.3M

[0088] Figure 5 shows the relationship between the parameter P and the warpage (curvature). When the parameter P is in the range of -0.3 to 0.3, the curvature is -8.00×10 -5 mm -1 ~8.00×10 -5 mm -1 It was found that it was possible to estimate that the range

[0089] In addition, when the parameter P is in the range of -0.24 to 0.24, the curvature is -5.50×10 -5 mm -1 ~5.50×10 -5 mm -1 It was found that it was possible to estimate that the range Details of FIG. 5 will be described later.

[0090] As described above, according to the design method of this embodiment, by focusing on the strain rate sensitivity coefficients of the first and second skin materials and selecting the first and second skin materials so as to optimize the combination of the strain rate sensitivity coefficients of the first and second skin materials, it can be inferred that the warpage of the triple-layer clad plate after hot rolling can be reduced even when the symmetry of the thickness and deformation resistance of the first and second skin materials arranged on both sides of the core material cannot be ensured. This makes it possible to easily design the combination of the core material, the first skin material, and the second skin material that constitute the triple-layer clad metal plate, and to increase the productivity of the triple-layer clad metal plate. Furthermore, according to the method for manufacturing a three-layer clad metal plate of this embodiment, a three-layer clad metal plate with a small amount of warping can be manufactured. EXAMPLES

[0091] The present invention will now be described in more detail with reference to examples. The materials were prepared as shown in Tables 2 and 3 below. Tables 2 and 3 show the material type of each material, the deformation resistance s (MPa) at 440°C, 480°C, and 520°C, and the measured values ​​of the strain rate sensitivity coefficient m.

[0092] [Table 2]

[0093] [Table 3]

[0094] The materials shown in Table 2 were hot-rolled to adjust the plate thickness to obtain the core, first skin, and second skin for clad rolling. The first skin and second skin were placed on one side and the other side of the core, respectively, and this laminate was hot-rolled. The heating temperature of the laminate before hot rolling was 480°C. The roll diameter of the rolling roll during hot rolling was 860 mm. The reduction ratio of the hot rolling was in the range of 4 to 10%. In this manner, three-layer clad plates No. 57 to 60 shown in Table 4 were manufactured. The obtained three-layer clad plates were evaluated for warpage and manufacturability. The results are shown in the lower part of Table 4.

[0095] The material type, casting method, and homogenization temperature are shown below for the materials shown in Table 2. "%" for chemical components is mass%. Also, "hot rolled" in AA1 to AA3 and AC1 to AC5 means that blooming and hot rolling were performed to obtain the specified plate thickness.

[0096] "AA1" Al-Si brazing filler metal AA1. Melted and cast. Homogenized heat treatment at 550°C. Hot rolled. "AA2" Al-Si brazing filler metal AA2. Melted and cast. Homogenized heat treatment at 450°C. Hot rolled. "AA3" Al-Si brazing filler metal AA3. Melted and cast. Homogenized heat treatment at 500°C. Hot rolled. "AB1" Al-Mn core material AB1. Melting and casting. Homogenization heat treatment at 500℃. "AB2" Al-Mn core material AB2. Melting and casting. Homogenization heat treatment at 600℃. "AC1" Al-Zn sacrificial material AC1. Melted and cast. Homogenized heat treatment 550℃. Hot rolled. "AC2" Al-Zn sacrificial material AC2. Melted and cast. Homogenized heat treatment at 450°C. Hot rolled. "AC3" Al-Zn sacrificial material AC3. Melted and cast. Homogenized heat treatment 550℃. Hot rolled. "AC4" Al-Zn sacrificial material AC4. Melted and cast. Homogenized heat treatment at 450°C. Hot rolled. "AC5" Al-Zn sacrificial material AC5. Melted and cast. Homogenized heat treatment at 500°C. Hot rolled.

[0097] The rolling conditions for Nos. 57 to 60 are as follows: "Rolling of No. 57" Total thickness of laminate before rolling CL T : 510mm. After crimping, the reduction is 4-10% for thicknesses of 400mm or more, and over 10% for thicknesses of less than 400mm. Almost no warping, good manufacturability. "Rolling of No. 58" Total thickness of laminate before rolling CL T : 510mm. After crimping, the reduction is 4-10% for thicknesses of 350mm or more, and over 10% for thicknesses of less than 350mm. Large upward warping and poor manufacturability. "Rolling of No. 59" Total thickness of laminate before rolling CL T : 590mm. After crimping, the reduction is 4-10% for thicknesses of 400mm or more, and over 10% for thicknesses of less than 400mm. Good manufacturability with slight upward warping. "Rolling of No. 60" Total thickness of laminate before rolling CL T : 510mm. After crimping, the reduction is 4-10% for thicknesses of 350mm or more, and over 10% for thicknesses of less than 350mm. It has a large upward warp and is difficult to manufacture. In addition, the rolls are often stopped and returned during rolling.

[0098] As a determination method according to the present invention, CL1, CL2, Δs, Δm, ΔCL, S, and parameter P were determined from the deformation resistance (MPa) at 480°C, strain rate sensitivity coefficient, and sheet thickness of the materials shown in Table 2. These are also shown in Table 4. Δs, Δm, ΔCL, S, and parameter P were determined by the above formulas (B) to (F). The results are shown in the upper part of Table 4. Furthermore, the curvatures shown in the upper part of Table 4 are predicted values ​​determined by the finite element method.

[0099] As shown in Table 4, the results of the determination method according to the present invention and the warpage of the three-layer clad metal sheet actually manufactured show a good tendency to coincide.

[0100] That is, for No. 57, the parameter P is -0.079, which is within the range of -0.3 to 0.3, and the predicted value of the curvature obtained by the finite element method is -1.66 × 10 -5 ( / mm), -8.00×10 -5 mm -1 ~8.00×10 -5 mm -1 The actual manufacturing results show that there is almost no warping. The same is true for No. 59.

[0101] On the other hand, the parameter P of No. 58 is 0.387, which is outside the range of -0.3 to 0.3, and the predicted value of the curvature obtained by the finite element method is 8.77 × 10 -5 ( / mm), -8.00×10 -5 mm -1 ~8.00×10 -5 mm -1 The actual results of the manufacturing process were evaluated as being significantly higher than expected. The same was true for No. 60.

[0102] From these results, it is clear that the results of the determination method according to the present invention are in good agreement with the warpage of the three-layer clad metal plate actually manufactured, and therefore it is understood that the determination method according to the present invention has very high prediction accuracy.

[0103] [Table 4]

[0104] In addition, CL1, CL2, Δs, Δm, ΔCL, S, and parameter P were calculated from the deformation resistance (MPa), strain rate sensitivity coefficient, and plate thickness of the materials shown in Tables 2 and 3. These are shown in Table 5. Δs, Δm, ΔCL, S, and parameter P were calculated using the above formulas (B) to (F). In addition, the curvatures shown in Table 5 are predicted values ​​of curvature calculated using the finite element method.

[0105] As shown in Table 5, it is understood that the amount of warpage of a three-layer clad plate after hot rolling can be predicted with high accuracy even when the material is an aluminum alloy, a Cu alloy, or a Ti alloy.

[0106] Moreover, Fig. 5 shows the relationship between the parameter P and the curvature in Tables 1, 4 and 5. The curvatures shown in Fig. 5 are predicted values ​​of the curvatures obtained by the finite element method. As shown in Fig. 5, even if the core material, the first skin material and the second skin material are an aluminum-based alloy, pure copper, a copper-based alloy and titanium, respectively, it can be seen that there is a correlation between the parameter P and the curvature. This demonstrates that the determination method of the present invention can accurately predict the curvature of a triple-layer clad plate after hot rolling using the parameter P.

[0107] [Table 5]

Claims

1. A method for designing the hot rolling in a case where a three-layer clad plate is manufactured by hot rolling a core material made of a metal plate, a first skin material made of a metal plate different from the core material is arranged on one side of the core material, a second skin material made of a metal plate different from the core material is arranged on the other side of the core material, and the three-layer clad plate is manufactured by hot rolling, the core material, the first skin material, and the second skin material are each made of pure aluminum or an aluminum-based alloy, The total thickness CL of the core material, the first skin material, and the second skin material before the hot rolling T The plate thickness ratio CL is the ratio of the thickness of the first skin material to the 1 and the total thickness CL T The plate thickness ratio CL is the ratio of the thickness of the second skin material to 2 Difference with (CL 1 -CL 2 ) is ΔCL, The strain rate of the core material, the first skin material, and the second skin material before the hot rolling is 0.1 sec -1 The deformation resistance at the hot rolling temperature in c , s 1 , s 2 In this case, Δs and S are defined as shown in the following formula (1) and formula (2), respectively: The strain rate sensitivity coefficients of the deformation resistance at the hot rolling temperature of the core material, the first skin material, and the second skin material before the hot rolling are respectively defined as m c , m 1 , m 2 In this case, when Δm and M are defined as in the following formula (3) and the following formula (4), A design method for hot rolling of a three-layer clad plate, characterized in that, when S>0.65 and |ΔCL|>0.1, or when S≦0.65, the core material, the first skin material, and the second skin material are selected so as to satisfy the following formula (5). Δs = (s 1 -s 2 ) / s c …(1) S = 0.5 (s 1 +s 2 ) / s c …(2) Δm = m 1 -m 2 …(3) M = 0.5 (m 1 +m 2 ) / m c …(4) |k 1 Δs + k 2 Δm+k 3 ΔCL|≦0.3…(5) However, when S>0.65 and |ΔCL|>0.1, k 1 = 1.0, k 2 = 2.6 and k 3 = -9.9 + 7.7S + 1.5M, When S≦0.65, k in the above formula (5) 1 =-1.0, k 2 = -0.7 and k 3 = 1.2 - 3.2S - 4.3M, and the case where ΔCL = Δs = Δm = 0 is excluded.

2. A design method for hot rolling of a three-layer clad plate as described in claim 1, characterized in that the core material is formed from an Al-Mn aluminum-based alloy.

3. A design method for hot rolling of a three-layer clad plate as described in claim 1 or claim 2, characterized in that the first skin material is formed from an Al-Si type aluminum-based alloy.

4. A design method for hot rolling of a three-layer clad plate described in any one of claims 1 to 3, characterized in that the second skin material is formed from an Al-Zn aluminum-based alloy.

5. 5. A method for manufacturing a three-layer clad plate, comprising the steps of: using the core material, the first skin material, and the second skin material selected in the design method for hot rolling of a three-layer clad plate according to any one of claims 1 to 4; arranging the first skin material and the second skin material on one side and the other side of the core material, respectively; and hot rolling the core material.

Citation Information

Patent Citations

  • Rolling method of copper or copper alloy clad steel

    JP1984056903A

  • Clad steel hot rolling device

    JP1985131213U

  • Production of rolling clad material

    JP1986232075A

  • Production of rolled clad steel sheet

    JP1987158583A

  • Rolling method for clad metallic material

    JP1987259607A