Universal coating composition set for forming coating film on exterior and interior panels of automobiles, coating film on exterior and interior panels of automobiles, and method for forming coating film on exterior and interior panels of automobiles

A common paint composition with specific scaly glitter pigments addresses dust streaks and hue differences between outer and inner automobile panels, enhancing design and reducing costs by using a unified coating solution for both.

JP7557364B2Active Publication Date: 2024-09-27NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020219533
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-28
Publication Date
2024-09-27
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

The challenge in automobile painting is the occurrence of dust streaks and hue differences between outer and inner panels due to different coating compositions, leading to inefficiencies and high costs when specialized paints are used for inner panels, and the need for a common paint composition that reduces dust streaks while maintaining design excellence.

Method used

A common paint composition set for both outer and inner panels, comprising a multilayer coating film with specific scaly glitter pigments of 15-25 μm average particle size, including a first base coating film and a second base coating film, reduces dust streaks and enhances design properties.

Benefits of technology

The solution effectively reduces dust streaks on inner panel coatings and maintains excellent design properties, allowing for a unified paint composition that can be used on both outer and inner panels, thereby reducing costs and improving aesthetic consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557364000005
    Figure 0007557364000005
  • Figure 0007557364000004
    Figure 0007557364000004
  • Figure 0007557364000002
    Figure 0007557364000002
Patent Text Reader

Abstract

To provide a shared paint composition set that can be shared with the base coating film of an outer plate and an inner plate of an automobile at the time of forming the coating film of the outer plate and the inner plate, and can reduce dust streaks on the base coating film of the inner plate.SOLUTION: In the shared paint composition set for forming coating films of outer plates and inner plates of an automobile, the coating film of the outer plate of an automobile is a multilayer coating film including a first base coating film (BO1) and a second base coating film, and the coating film of the inner plate of the automobile includes only the first base coating film (BI1) as the base coating film; the shared coating composition set includes a first base paint that forms BO1 and BI1 and a second base paint that forms a second base coating film; the first base paint includes a first scaly luminous pigment of an average particle size in a predetermined range, and the second base paint composition includes a second scaly luminous pigment of an average particle size in a predetermined range; and the PWC of the first scaly luminous pigment is 0.10-2.5 parts by mass, and the PWC of the second scaly luminous pigment is 0.5-5.0 parts by mass.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a universal coating composition set for forming coating films on the exterior and interior panels of an automobile, coating films on the exterior and interior panels of an automobile, and a method for forming coating films on the exterior and interior panels of an automobile. [Background technology]

[0002] A number of coating films are formed on the surface of an automobile. These coating films protect the body of the automobile and at the same time provide the automobile with excellent design.

[0003] Among the surfaces of an automobile, the multiple coating films on the outer panels of the vehicle body include, for example, an undercoat coating film, an intermediate coating film, and a topcoat coating film, in that order from the outer panel side. Of these coating films, the topcoat coating film, which is located on the surface closest to the viewer, has a particularly large influence on the design of the automobile. In addition, the topcoat coating film may be composed of a base coating film and a clear coating film from the vehicle body surface side.

[0004] Furthermore, the base coating may be composed of a first base coating and a second base coating from the vehicle body surface side (see, for example, Patent Documents 1 and 2). In general, the first base coating has a base concealing property that makes the color of the underlying coating (for example, the intermediate coating) less noticeable, and the second base coating has a design property.

[0005] In recent years, consumers have come to prefer cars with a shiny appearance, so flake-like luster pigments that create a shiny appearance are often blended into the base coating of exterior panels, especially the second base coating. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2015-099150 [Patent Document 2] JP 2020-099888 A Summary of the Invention [Problem to be solved by the invention]

[0007] Among the surfaces of an automobile, the interior panels inside the body of the vehicle may have a different paint film composition than the exterior panels. For example, unlike the exterior panels, the interior panels do not require high chipping resistance (resistance to scratches caused by stone chips), so they may not have a middle coat. Also, the interior panels do not require high weather resistance, so they may not have a clear coat.

[0008] Conventionally, when a first base coating and a second base coating are used for the exterior coating, the same paint as that for the first base coating of the exterior panel or a paint specifically for interior panels may be used for the interior coating. This is because the interior coating must be completed within a certain time, and the same coating composition as that for the exterior coating cannot be used. However, (1) when the same paint as that for the first base coating of the exterior panel is used for the interior coating, a hue difference between the interior and exterior panels is likely to occur, and the paint for the exterior base coating attached to the base coating of the interior panel is likely to form streaks (hereinafter referred to as "dust streaks"). On the other hand, (2) when a paint specifically for interior panels is used for the interior coating, new piping for the paint specifically for interior panels is required in the coating line, or the area to be painted using the paint specifically for interior panels is small, and the paint specifically for interior panels is produced in small batches, which often results in high costs.

[0009] In the process of forming a topcoat coating film for an automobile, the window glass and sealing members (for example, weather strips and door outside seals) are not yet attached to the vehicle body to be painted. In the process of forming a topcoat coating film, a base coating paint is usually applied to the interior panel first. Next, the base coating paint is applied to the exterior panel. When painting the exterior panel, if the door of the automobile is completely closed, the edge of the door that opens and closes and the vehicle body part that comes into contact with the edge of the door may rub against each other, or the base coating paint may come off when the door lock is touched and operated to open the door. Therefore, when painting the exterior panel, the base coating paint is applied to the exterior panel when the door is not completely closed but slightly open, i.e., when there are gaps in the center pillar part and the rear pillar part, etc.

[0010] When the paint for the base coating of the exterior panels is applied, the paint for the base coating of the exterior panels may enter the inside of the vehicle body through the windows and gaps and adhere to the base coating of the interior panels. When the coating film configuration of the exterior panels and the coating film configuration of the interior panels are different as described above, dust streaks may occur, causing a difference in hue in the base coating of the interior panels. In addition, when dust streaks occur, a process such as repainting the paint for the base coating of the interior panels is also required to eliminate the dust streaks, which is a problem. Since the glitter pigment has a high glittering effect, the dust streaks are particularly noticeable when the base coating film contains the glitter pigment.

[0011] Therefore, an object of the present invention is to provide a universal paint composition set that can be used for the base coating of the exterior and interior panels of an automobile when forming the coating films on the exterior and interior panels, and that can reduce dust streaks on the base coating film of the interior panel.

[0012] Another object of the present invention is to provide a coating film for the exterior and interior panels of an automobile which reduces dust streaks on the base coating film of the interior panel and has excellent design properties.

[0013] Another object of the present invention is to provide a method for forming coating films for the exterior and interior panels of an automobile which reduce dust streaks on the base coating film of the interior panel and have excellent design properties. [Means for solving the problem]

[0014] The universal coating composition set according to the present invention is a universal coating composition set for forming coating films on exterior and interior panels of an automobile, The coating film of the outer plate is a multi-layer coating film including a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer plate side, The coating film of the inner panel includes only a first base coating film (BI1) as a base coating film, The universal coating composition set includes a first base coating composition that forms the first base coating film (BO1) and the first base coating film (BI1), and a second base coating composition that forms the second base coating film; The first base coating composition includes a resin component, a curing agent, and a first scaly glittering pigment having an average particle size of 15 μm to 25 μm, The second base coating composition includes a resin component, a curing agent, and a second scale-like glittering pigment having an average particle size of 15 μm to 25 μm, The amount of the first scale-like glittering pigment is 0.10 to 2.5 parts by mass relative to 100 parts by mass of the total solid content of the first base coating composition; The amount of the second scale-like bright pigment is 0.5 to 5.0 parts by mass relative to 100 parts by mass of the total solid content of the second base coating composition, and the coating composition set is for forming the coating film of the outer panel and the inner panel of an automobile. This allows the coating film to be used for both the outer panel and the inner panel when forming the coating film of the outer panel and the inner panel of an automobile, and reduces dust streaks on the inner panel base coating film.

[0015] In one embodiment of the universal coating composition set for forming coating films on the exterior and interior panels of an automobile according to the present invention, in the second scaly luster pigment, a glass substrate is coated with a metal oxide.

[0016] In one embodiment of the universal coating composition set for forming coating films on the outer and inner panels of an automobile according to the present invention, the dry film thickness of the first base coating film (BO1) is 8 μm, and the dry film thickness of the second base coating film is 10 μm. In this embodiment, the L * The 110 value is less than 2 and the graininess G value is greater than 3.5.

[0017] The coating film of the outer panel and the inner panel of an automobile according to the present invention includes a multi-layer coating film using any one of the above-mentioned universal coating composition sets for forming the coating film of the outer panel and the inner panel of an automobile, The multi-layer coating film includes a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer panel side, The coating film for the interior panel of an automobile contains only a first base coating film (BI1) using the first base coating composition of the universal coating composition set for forming the coating film for the exterior panel and interior panel of an automobile described above as a base coating film, thereby reducing dust streaks on the base coating film for the interior panel and providing the coating film for the exterior panel and interior panel with excellent design properties.

[0018] The method for forming a coating film on an outer panel and an inner panel of an automobile according to the present invention comprises the steps of: preparing a universal coating composition set for forming a coating film on an outer panel and an inner panel of an automobile according to any one of the above; A step of applying the first base coating composition to a surface side of the exterior panel to form an uncured first base coating film (BO1); A step of applying the second base coating composition onto the uncured first base coating film (BO1) to form an uncured second base coating film; A step of curing the uncured first base coating film (BO1) and the uncured second base coating film to form a multi-layer coating film for the exterior panel; A step of applying the first base coating composition to a surface side of the inner panel to form an uncured first base coating film (BI1); and curing the uncured first base coating film (BI1) to form a first base coating film (BI1), The method for forming coating films for the exterior and interior panels of an automobile includes only the first base coating film (BI1) as a base coating film, thereby reducing dust streaks on the base coating film of the interior panel and forming coating films for the exterior and interior panels with excellent design properties. Effect of the Invention

[0019] According to the present invention, it is possible to provide a coating composition set that can be used for the base coating film of an automobile exterior panel and interior panel when forming the coating film of the exterior panel and interior panel, and can reduce dust streaks on the base coating film of the interior panel. Also, according to the present invention, it is possible to provide a coating film of an automobile exterior panel and interior panel that has excellent design properties, with reduced dust streaks on the base coating film of the interior panel. Also, according to the present invention, it is possible to provide a method for forming a coating film of an automobile exterior panel and interior panel that has excellent design properties, with reduced dust streaks on the base coating film of the interior panel. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic diagram showing an example of the layer structure of a paint film on an outer panel of an automobile according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the layer structure of a coating film on an interior panel of an automobile according to the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing another example of the layer structure of a coating film for an interior panel of an automobile according to the present invention. [Figure 4] FIG. 4 is a schematic diagram showing another example of the layer structure of a coating film for an interior panel of an automobile according to the present invention. [Diagram 5] FIG. 5 is a schematic diagram showing another example of the layer structure of a coating film on an interior panel of an automobile according to the present invention. [Figure 6] FIG. 6 is a perspective view that illustrates a typical method for painting an exterior panel in the embodiment. [Figure 7] FIG. 7 is a photograph of the coating film on the inner panel of Example 18. [Figure 8] FIG. 8 is a photograph of the coating film on the inner panel of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, embodiments of the present invention will be described. These descriptions are intended to be illustrative of the present invention and are not intended to limit the present invention in any way.

[0022] In the present invention, two or more embodiments can be combined in any manner.

[0023] In the present invention, the paint and the paint composition can be used interchangeably.

[0024] Numerical ranges are intended to include the upper and lower limits of the range unless otherwise specified, for example, 0.5 to 5.0 parts by weight means a range of 0.5 parts by weight to 5.0 parts by weight.

[0025] In this specification, the first base coating film (BO1), the second base coating film, and the first base coating film (BI1) may be collectively referred to as "base coating film". Also, the paint for the base coating film may be simply referred to as "base paint".

[0026] In this specification, the amount (parts by mass) of the first scaly glittering pigment relative to 100 parts by mass of the total solids of the first base coating composition may be referred to as the "pigment mass concentration" or "PWC." In this specification, the amount (parts by mass) of the second scaly glittering pigment relative to 100 parts by mass of the total solids of the second base coating composition may be referred to as the "pigment mass concentration" or "PWC."

[0027] In the present invention, the average particle size of the scaly luster pigment refers to the median diameter of the volume-based particle size distribution measured by a laser diffraction scattering method using a Microtrack particle size distribution measuring device (product name "MT3300") manufactured by Nikkiso Co., Ltd.

[0028] In the present invention, a coating composition in which the dispersion medium contained in the largest amount in the coating composition is water is called an aqueous coating composition, whereas a coating composition in which the dispersion medium contained in the largest amount in the coating composition is a solvent is called a solvent-based coating composition.

[0029] In this specification, the non-volatile content may be referred to as the "solid content."

[0030] The accompanying drawings are schematic diagrams given priority in order to facilitate understanding of the present invention, and therefore the scale of each coating film in the drawings is not accurate.

[0031] In the present invention, the average light transmittance of the second base coating film in the wavelength region of 360 to 700 nm is measured by the method described in the examples.

[0032] In the present invention, the lightness L of the coating film at a viewing angle of 110° * The 110 value is measured by the method described in the Examples. The viewing angle refers to the angle from the specular reflection of light incident at an incident angle of 45° (45° from the normal direction of the coating film) toward the incident direction. Therefore, a viewing angle of 110° refers to an angle of 110° toward the incident direction from the specular reflection of light incident at an incident angle of 45°.

[0033] In the present invention, the particle feeling G value of the coating film is measured by the method described in the examples.

[0034] (Universal paint composition set) The universal coating composition set according to the present invention is a universal coating composition set for forming coating films on exterior and interior panels of an automobile, The coating film of the outer plate is a multi-layer coating film including a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer plate side, The coating film of the inner panel includes only a first base coating film (BI1) as a base coating film, The universal coating composition set includes a first base coating composition that forms the first base coating film (BO1) and the first base coating film (BI1), and a second base coating composition that forms the second base coating film; The first base coating composition includes a resin component, a curing agent, and a first scale-like glittering pigment having an average particle size of 15 μm to 25 μm, The second base coating composition includes a resin component, a curing agent, and a second scale-like glittering pigment having an average particle size of 15 μm to 25 μm, The amount of the first scale-like glittering pigment is 0.10 to 2.5 parts by mass relative to 100 parts by mass of the total solid content of the first base coating composition; The amount of the second scaly luster pigment is 0.5 to 5.0 parts by mass per 100 parts by mass of the total solids content of the second base paint composition, and this is a universal paint composition set for forming coating films on the exterior and interior panels of an automobile.

[0035] The first base coating composition and the second base coating composition, which are essential elements of the universal coating composition set according to the present invention, will be described below.

[0036] (First base coating composition) The first base coating composition forms a first base coating film (BO1) for the outer panel and a first base coating film (BI1) for the inner panel. The first base coating composition contains a resin component, a curing agent, and a first scaly glittering pigment having an average particle size of 15 μm to 25 μm, and the amount of the first scaly glittering pigment is 0.10 to 2.5 parts by mass per 100 parts by mass of the total solid content of the first base coating composition.

[0037] The resin component, which is an essential component of the first base coating composition, the curing agent, and the first scaly bright pigment having an average particle size of 15 μm to 25 μm will be described below.

[0038] Resin components The resin component may be a resin component of a conventionally known base paint. Examples of the resin component include acrylic resin, polyester resin, alkyd resin, fluororesin, epoxy resin, polyurethane resin, polyether resin, polyolefin resin, etc. In addition, the resin component may be, for example, a coating film-forming resin such as an acrylic emulsion resin, polyether polyol, or urethane emulsion resin described in Patent Document 1; or a water-dispersible resin described in Patent Document 2.

[0039] The resin components may be used alone or in combination of two or more. The resin components of the first base coating composition may be the same as or different from the resin components of the second base coating composition described below.

[0040] The amount of the resin component in the first base coating composition may be adjusted as appropriate, but for example, it is 40 to 90 parts by mass, and preferably 60 to 80 parts by mass, per 100 parts by mass of the total solids content of the resin component and curing agent in the first base coating composition.

[0041] Hardener The curing agent may be any of those known in the art for use in base coatings, including, for example, amino resins and blocked isocyanates described in Patent Document 1.

[0042] The amount of curing agent in the first base coating composition may be adjusted as appropriate, but for example, it is 10 to 60 parts by mass, and preferably 20 to 40 parts by mass, per 100 parts by mass of the total solids content of the resin component and curing agent in the first base coating composition.

[0043] The curing agent may be used alone or in combination of two or more. The curing agent of the first base coating composition may be the same as or different from the curing agent of the second base coating composition described below.

[0044] ·First scale-like glitter pigment The first scale-like bright pigment can be a conventionally known scale-like bright pigment with an average particle size of 15 μm to 25 μm. Examples of the scale-like bright pigment include metals such as aluminum, copper, zinc, iron, nickel, tin, and aluminum oxide; alloys thereof; bright pigments such as interference mica, white mica, graphite, glass flakes, and alumina flakes; and scale-like bright pigments in which these metals, alloys, interference mica, white mica, graphite, glass flakes, or alumina flakes are coated with metal oxides (e.g., titanium oxide, titanium dioxide, iron oxide) or metals (e.g., gold and silver). Other examples include alumina flake pigments (a) described in JP 2016-221473 A; scaly bright pigments in which a metal substrate or a glass flake substrate is coated with a metal oxide or metal; scaly bright pigments in which a coloring pigment is chemically adsorbed on the surface of a metal substrate or a glass flake substrate; aluminum pigments in which an aluminum oxide layer is formed on the surface of an aluminum substrate; aluminum solid solution plate-like iron oxide pigments; scaly bright pigments in which the surface of interference mica, graphite or silica flakes is coated with titanium dioxide; plate-like iron oxide pigments, etc. Preferred scaly bright pigments are scaly bright pigments in which a glass substrate is coated with a metal oxide, and aluminum flakes.

[0045] In one embodiment, the first flake glitter pigment is aluminum flake.

[0046] The first scale-like glittering pigment may be colorless or colored, or a combination thereof. Examples of colored colors include gray, silver, black, red, yellow, green, and blue. In one embodiment, the first scale-like glittering pigment is one or more selected from the group consisting of gray and silver. In another embodiment, the first scale-like glittering pigment and the second scale-like glittering pigment are one or more selected from the group consisting of gray, silver, and black.

[0047] The average particle size of the first scale-like glittering pigment and the second scale-like glittering pigment described later is 15 μm to 25 μm. If the average particle size of either one of the scale-like glittering pigments is less than 15 μm or more than 25 μm, dust streaks on the base coating film of the inner panel cannot be reduced. In one embodiment, the average particle size of the first scale-like glittering pigment is 15 μm or more, 16 μm or more, 17 μm or more, 18 μm or more, 19 μm or more, 20 μm or more, 21 μm or more, 22 μm or more, 23 μm or more, or 24 μm or more. In another embodiment, the average particle size of the first scale-like glittering pigment is 25 μm or less, 24 μm or less, 23 μm or less, 22 μm or less, 21 μm or less, 20 μm or less, 19 μm or less, 18 μm or less, 17 μm or less, or 16 μm or less.

[0048] The first scale-like bright pigment and the second scale-like bright pigment described later may be commercially available. Examples of commercially available scale-like bright pigments include the Metashine (registered trademark) series, such as the ST1018 series, ST1025 series, and GT1020 series manufactured by Nippon Sheet Glass Co., Ltd.; the Alpaste (registered trademark) series, such as the 76 series, TCR series, and 54 series manufactured by Toyo Aluminum Co., Ltd.; the GX series, such as the product name "Aluminum Paste", manufactured by Asahi Kasei Corporation; and the LUXAN series, such as the product name "B001", manufactured by ECKART Co., Ltd. The commercially available first scale-like bright pigment is particularly preferably the Alpaste (registered trademark) series, such as the 76 series, TCR series, and 54 series manufactured by Toyo Aluminum Co., Ltd.; and the GX series, such as the product name "Aluminum Paste", manufactured by Asahi Kasei Corporation.

[0049] The first scale-like bright pigment may be used alone or in combination of two or more. The first scale-like bright pigment may be the same as or different from the second scale-like bright pigment described below.

[0050] The amount of the first scale-like bright pigment in the first base coating composition is 0.10 to 2.5 parts by mass relative to 100 parts by mass of the total solid content of the first base coating composition, and the amount of the second scale-like bright pigment in the second base coating composition described below is 0.5 to 5.0 parts by mass relative to 100 parts by mass of the total solid content of the second base coating composition. Even if the PWC of the second scale-like bright pigment is 0.5 to 5.0 parts by mass, if the PWC of the first scale-like bright pigment is less than 0.10 parts by mass, dust streaks will be noticeable on the center pillar, and if the PWC of the first scale-like bright pigment is more than 2.5 parts by mass, the color depth will decrease.

[0051] In one embodiment, the PWC of the first scaly luster pigment is 0.10 parts by weight or more, 0.15 parts by weight or more, 0.20 parts by weight or more, 0.25 parts by weight or more, 0.30 parts by weight or more, 0.35 parts by weight or more, 0.40 parts by weight or more, 0.45 parts by weight or more, 0.50 parts by weight or more, 0.60 parts by weight or more, 0.70 parts by weight or more, 0.80 parts by weight or more, 0.90 parts by weight or more, 1.0 parts by weight or more, 1.2 parts by weight or more, 1.4 parts by weight or more, 1.5 parts by weight or more, 1.6 parts by weight or more, 1.8 parts by weight or more, 2.0 parts by weight or more, 2.1 parts by weight or more, 2.2 parts by weight or more, 2.3 parts by weight or more, or 2.4 parts by weight or more. In another embodiment, the PWC of the first flaky glitter pigment is 2.5 parts by weight or less, 2.4 parts by weight or less, 2.3 parts by weight or less, 2.2 parts by weight or less, 2.1 parts by weight or less, 2.0 parts by weight or less, 1.8 parts by weight or less, 1.6 parts by weight or less, 1.5 parts by weight or less, 1.4 parts by weight or less, 1.2 parts by weight or less, 1.0 parts by weight or less. 0.90 parts by mass or less, 0.80 parts by mass or less, 0.70 parts by mass or less, 0.60 parts by mass or less, 0.50 parts by mass or less, 0.45 parts by mass or less, 0.40 parts by mass or less, 0.35 parts by mass or less, 0.30 parts by mass or less, 0.25 parts by mass or less, 0.20 parts by mass or less, or 0.15 parts by mass or less.

[0052] Other Ingredients In addition to the resin component, the curing agent, and the first scaly luster pigment, the first base coating composition may contain known base coating components such as extender pigments, coloring pigments, water, organic solvents, corrosion inhibitors, surface conditioners, thickeners, antioxidants, ultraviolet inhibitors, defoamers, etc. Each of these other components may be used alone or in combination of two or more.

[0053] The first base coating composition may contain a glittering pigment other than the first scaly glittering pigment having an average particle size of 15 μm to 25 μm, without departing from the spirit of the present invention. When the first base coating composition contains the first scaly glittering pigment and the other glittering pigment, the amount of the first scaly glittering pigment relative to a total of 100 parts by mass of the first scaly glittering pigment and the other glittering pigment is 50 parts by mass or more, 70 parts by mass or more, 90 parts by mass or more, 95 parts by mass or more, or 99 parts by mass or more. In one embodiment, the first base coating composition contains only the first scaly glittering pigment as the glittering pigment.

[0054] The first base coating composition may be either a water-based coating composition or a solvent-based coating composition. In one embodiment, the first base coating composition and the second base coating composition are water-based coating compositions.

[0055] The total amount of paint solids in the first base coating composition may be appropriately adjusted and is not particularly limited. For example, the total amount of paint solids is 5 to 50 parts by mass, preferably 10 to 30 parts by mass, relative to 100 parts by mass of the first base coating composition.

[0056] Method for preparing a first base coating composition The method of preparing the first base coating composition is not particularly limited, and can be any conventional method, as long as it contains the above-mentioned resin component, curing agent and first scale-like bright pigment, and the PWC of the first scale-like bright pigment is 0.10 to 2.5 parts by mass.For example, the resin component, curing agent and first scale-like bright pigment are kneaded and dispersed using a kneader or roll to prepare the first base coating composition.

[0057] (Second base coating composition) The second base coating composition forms a second base coating film for the exterior panel. The second base coating composition is not used for the interior panel. The second base coating composition contains a resin component, a curing agent, and a second scaly glittering pigment having an average particle size of 15 μm to 25 μm, and the amount of the second scaly glittering pigment is 0.5 to 5.0 parts by mass per 100 parts by mass of the total solid content of the second base coating composition.

[0058] The resin component, which is an essential component of the second base coating composition, the curing agent, and the second scaly bright pigment having an average particle size of 15 μm to 25 μm will be described below.

[0059] Resin components The resin component may be any of the resin components of conventional base coating compositions. Examples of the resin component are the same as those listed for the first base coating composition.

[0060] The resin components may be used alone or in combination of two or more.

[0061] The amount of the resin component in the second base coating composition may be adjusted as appropriate, but for example, it is 40 to 90 parts by mass, and preferably 60 to 80 parts by mass, per 100 parts by mass of the total solids content of the resin component and curing agent of the second base coating composition.

[0062] Hardener As the curing agent, a conventionally known curing agent for a base coating material can be used. Examples of the curing agent are the same as those listed for the first base coating material composition.

[0063] The amount of curing agent in the second base coating composition may be adjusted as appropriate, but for example, it is 10 to 60 parts by mass, and preferably 20 to 40 parts by mass, per 100 parts by mass of the total solids content of the resin component and curing agent of the second base coating composition.

[0064] The curing agent may be used alone or in combination of two or more kinds.

[0065] · Second scale-like glitter pigment The second scale-like bright pigment can be a conventionally known scale-like bright pigment having an average particle size of 15 μm to 25 μm. The scale-like bright pigment is the same as the first scale-like bright pigment listed in the first base coating composition.

[0066] In one embodiment of the universal coating composition set for forming coating films on the exterior and interior panels of an automobile according to the present invention, in the second scaly luster pigment, a glass substrate is coated with a metal oxide.

[0067] Commercially available products of the second scaly luster pigment are as exemplified for the first scaly luster pigment, but in particular, the Metashine (registered trademark) series, such as the ST1018 series, ST1025 series, and GT1020 series manufactured by Nippon Sheet Glass Co., Ltd.; and the "LUXAN" series, such as the product name "B001" manufactured by ECKART Co., Ltd., are preferred.

[0068] In one embodiment, the average particle size of the second scaly glitter pigment is 15 μm or more, 16 μm or more, 17 μm or more, 18 μm or more, 19 μm or more, 20 μm or more, 21 μm or more, 22 μm or more, 23 μm or more, or 24 μm or more. In another embodiment, the average particle size of the second scaly glitter pigment is 25 μm or less, 24 μm or less, 23 μm or less, 22 μm or less, 21 μm or less, 20 μm or less, 19 μm or less, 18 μm or less, 17 μm or less, or 16 μm or less.

[0069] The second scaly bright pigment may be used alone or in combination of two or more.

[0070] The amount of the second scaly bright pigment in the second base coating composition is 0.5 to 5.0 parts by mass relative to 100 parts by mass of the total solid content of the second base coating composition. Even if the PWC of the first scaly bright pigment is 0.10 to 2.5 parts by mass, if the PWC of the second scaly bright pigment is less than 0.5 parts by mass, excellent brilliance cannot be obtained, and if the PWC of the second scaly bright pigment is more than 5.0 parts by mass, appearance defects such as gloss fade are likely to occur.

[0071] In one embodiment, the PWC of the second scaly luster pigment is 0.5 parts by weight or more, 1.0 parts by weight or more, 1.5 parts by weight or more, 2.0 parts by weight or more, 2.1 parts by weight or more, 2.2 parts by weight or more, 2.3 parts by weight or more, 2.4 parts by weight or more, 2.5 parts by weight or more, 2.6 parts by weight or more, 2.7 parts by weight or more, 2.8 parts by weight or more, 2.9 parts by weight or more, 3.0 parts by weight or more, 3.5 parts by weight or more, 4.0 parts by weight or more, or 4.5 parts by weight or more. In another embodiment, the PWC of the second flaky glitter pigment is 5.0 parts by weight or less, 4.5 parts by weight or less, 4.0 parts by weight or less, 3.5 parts by weight or less, 3.0 parts by weight or less, 2.9 parts by weight or less, 2.8 parts by weight or less, 2.7 parts by weight or less. Parts by weight or less, 2.6 parts by weight or less, 2.5 parts by weight or less, 2.4 parts by weight or less, 2.3 parts by weight or less, 2.2 parts by weight or less, 2.1 parts by weight or less, 2.0 parts by weight or less, 1.5 parts by weight or less, or 1.0 parts by weight or less.

[0072] Other Ingredients In addition to the resin component, the curing agent, and the second scaly luster pigment, the second base coating composition may contain known base coating components such as extender pigments, coloring pigments, water, organic solvents, surface conditioners, thickeners, antioxidants, ultraviolet inhibitors, defoamers, etc. Each of these other components may be used alone or in combination of two or more.

[0073] The second base coating composition may contain a glittering pigment other than the second scaly glittering pigment having an average particle size of 15 μm to 25 μm, without departing from the spirit of the present invention. When the second base coating composition contains the second scaly glittering pigment and the other glittering pigment, the amount of the second scaly glittering pigment relative to a total of 100 parts by mass of the second scaly glittering pigment and the other glittering pigment is 50 parts by mass or more, 70 parts by mass or more, 90 parts by mass or more, 95 parts by mass or more, or 99 parts by mass or more. In one embodiment, the second base coating composition contains only the second scaly glittering pigment as the glittering pigment.

[0074] The second base coating composition may be either a water-based coating composition or a solvent-based coating composition.

[0075] The total amount of paint solids in the second base coating composition may be appropriately adjusted and is not particularly limited. For example, the total amount of paint solids is 5 to 50 parts by mass, preferably 10 to 30 parts by mass, per 100 parts by mass of the second base coating composition.

[0076] Method for preparing the second base coating composition The preparation method of the second base coating composition is not particularly limited, and can be used in the past known method, as long as it contains the above-mentioned resin component, curing agent and second scale-like glittering pigment, and the PWC of the second scale-like glittering pigment is 0.5 to 5.0 parts by mass.For example, can be used the means described in the preparation method of the first base coating composition.

[0077] In one embodiment, the average light transmittance of the second base coating film alone in the wavelength region of 360 to 700 nm when the dry film thickness is 10 μm is 5 to 20%.

[0078] In one embodiment of the universal coating composition set for forming coating films on the outer and inner panels of an automobile according to the present invention, the dry film thickness of the first base coating film (BO1) is 8 μm, and the dry film thickness of the second base coating film is 10 μm. In this embodiment, the L * The 110 value is less than 2 and the graininess G value is greater than 3.5.

[0079] (Painting on exterior and interior panels of automobiles) The coating film of the outer panel and the inner panel of an automobile according to the present invention includes a multi-layer coating film using any one of the above-mentioned universal coating composition sets for forming the coating film of the outer panel and the inner panel of an automobile, The multi-layer coating film includes a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer panel side, The coating film for the interior panel of an automobile includes, as a base coating film, only a first base coating film (BI1) using a first base coating composition of a universal coating composition set for forming coating films for the exterior and interior panels of an automobile described above.

[0080] Fig. 1 is a schematic diagram showing an example of the layer structure of a coating film of an automobile exterior panel according to the present invention. In Fig. 1, a multi-layer coating film is formed on the surface of an exterior panel 1, in adjacent order from the exterior panel side, comprising an undercoat coating film 2, an intermediate coating film 3, a first base coating film (BO1) 4, a second base coating film 5, and a clear coating film 6.

[0081] Fig. 2 is a schematic diagram showing an example of the layer structure of a coating film of an interior panel of an automobile according to the present invention. In Fig. 2, an undercoat coating film 2, an intermediate coating film 3, a first base coating film (BI1) 8, and a clear coating film 6 are formed adjacent to each other on the surface of an interior panel 7 in this order from the interior panel side.

[0082] Fig. 3 is a schematic diagram showing another example of the layer structure of a coating film of an interior panel of an automobile according to the present invention. In Fig. 3, an undercoat coating film, a first base coating film (BI1), and a clear coating film are formed adjacent to each other in this order from the interior panel side on the surface of the interior panel.

[0083] Fig. 4 is a schematic diagram showing another example of the layer structure of a coating film of an interior panel of an automobile according to the present invention. In Fig. 4, an undercoat coating film, an intermediate coating film, and a first base coating film (BI1) are formed adjacent to each other in this order from the interior panel side on the surface of the interior panel.

[0084] Fig. 5 is a schematic diagram showing another example of the layer structure of a coating film of an interior panel of an automobile according to the present invention. In Fig. 5, an undercoat coating film and a first base coating film (BI1) are formed adjacent to each other in this order from the interior panel side on the surface of the interior panel.

[0085] -Multi-layer coating on exterior panels The multi-layer coating film for an automobile exterior panel according to the present invention includes a first base coating film (BO1) and a second base coating film, which are adjacent to each other from the exterior panel side. The first base coating film (BO1) and the second base coating film, which are essential elements of the multi-layer coating film for an automobile exterior panel according to the present invention, will be exemplified below.

[0086] · First base coat (BO1) The first base coating film (BO1) is a base coating film formed using the first base coating composition of the universal coating composition set for forming coating films for the exterior and interior panels of the above-mentioned automobile.

[0087] The dry film thickness of the first base coating film (BO1) may be appropriately adjusted and is, for example, 2 to 20 μm, preferably 6 to 14 μm. The dry film thicknesses of the first base coating film (BO1) and the first base coating film (BI1) may be the same or different.

[0088] Second base coat The second base coating film is a base coating film formed using the second base coating composition of the universal coating composition set for forming coating films on the exterior and interior panels of the above-mentioned automobile, and is located on the observer side of the first base coating film (BO1).

[0089] The dry film thickness of the second base coating film may be appropriately adjusted and is, for example, from 2 to 20 μm, preferably from 6 to 14 μm.

[0090] The transparency of the second base coating film may be appropriately adjusted. For example, when the dry film thickness is 10 μm, the average light transmittance of the second base coating film alone in the wavelength region of 360 to 700 nm is 5 to 20%. When the average light transmittance is 5% or more, the transparency of the second base coating film is high, and the color depth in the shade direction of the first base coating film of the outer panel can be enhanced. When the average light transmittance is 20% or less, the brightness and the base hiding power of the second base coating film can be enhanced. In one embodiment, when the dry film thickness is 10 μm, the average light transmittance of the second base coating film alone in the wavelength region of 360 to 700 nm is 5% or more, 10% or more, or 15% or more. In another embodiment, when the dry film thickness is 10 μm, the average light transmittance of the second base coating film alone in the wavelength region of 360 to 700 nm is 20% or less, 15% or less, or 10% or less.

[0091] From the viewpoint of enhancing the color depth in the shade direction of the multi-layer coating film of the exterior panel, the L of the multi-layer coating film at a viewing angle of 110° when the dry film thickness of the first base coating film (BO1) of the exterior panel is 8 μm and the dry film thickness of the second base coating film is 10 μm is * The L110 value is, for example, 2.6 or less, and preferably less than 2. In one embodiment, the L110 value of the multi-layer coating film when the dry thickness of the first base coating film (BO1) of the exterior panel is 8 μm and the dry thickness of the second base coating film is 10 μm is * The L110 value is 2.6 or less, 2.0 or less, 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, or 1.1 or less. In another embodiment, the L110 value of the multi-layer coating when the dry film thickness of the first base coating (BO1) on the exterior panel is 8 μm and the dry film thickness of the second base coating is 10 μm is 2.6 or less, 2.0 or less, 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, or 1.1 or less. * The 110 value is 1.0 or more, 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 1.6 or more, 1.7 or more, 1.8 or more, or 1.9 or more.

[0092] In the present invention, the brightness of the coating film can be expressed by a particle G value. The higher the G value, the higher the brightness of the coating film. From the viewpoint of increasing the brightness of the multi-layer coating film of the outer panel, when the dry film thickness of the first base coating film (BO1) of the outer panel is 8 μm and the dry film thickness of the second base coating film is 10 μm, the G value of the multi-layer coating film is, for example, 3.5 or more, preferably 4.5 or more. In one embodiment, when the dry film thickness of the first base coating film (BO1) of the outer panel is 8 μm and the dry film thickness of the second base coating film is 10 μm, the G value of the multi-layer coating film is 3.5 or more, 4.0 or more, 4.5 or more, 4.9 or more, 5.0 or more, 5.1 or more, 5.2 or more, 5.3 or more, 5.4 or more, or 5.5 or more. In another embodiment, when the dry film thickness of the first base coating (BO1) on the exterior panel is 8 μm and the dry film thickness of the second base coating is 10 μm, the G value of the multi-layer coating is 6.0 or less, 5.5 or less, 5.4 or less, 5.3 or less, 5.2 or less, 5.1 or less, 5.0 or less, 4.9 or less, 4.5 or less, or 4.0 or less.

[0093] In one embodiment of the coating film for the exterior and interior panels of an automobile according to the present invention, the L of the multi-layer coating film at a viewing angle of 110° is obtained when the dry film thickness of the first base coating film (BO1) is 8 μm and the dry film thickness of the second base coating film is 10 μm. * In another embodiment of the coating for the exterior and interior panels of an automobile, the L value of the multi-layer coating when the dry thickness of the first base coating (BO1) is 8 μm and the dry thickness of the second base coating is 10 μm is 10 μm. * The 110 value is 1.0 to 1.9, and the graininess G value is 4.0 to 5.5.

[0094] Other exterior coatings The coating film of the exterior plate may include, in addition to the first base coating film (BO1) and the second base coating film, an undercoat coating film, an intermediate coating film, and a clear coating film. Furthermore, the coating film of the exterior plate of an automobile may include, between the intermediate coating film and the undercoat coating film, a chipping primer coating film as described in JP2009-102452A. In one embodiment, the coating film of the exterior plate of an automobile includes, adjacently from the exterior plate side, an undercoat coating film, an intermediate coating film, a first base coating film (BO1), a second base coating film, and a clear coating film.

[0095] The materials for the undercoat coating film, the intermediate coating film, and the clear coating film may be the materials for the undercoat coating film, the intermediate coating film, and the clear coating film of the conventionally known automobile exterior panels, respectively. The film thicknesses of the undercoat coating film, the intermediate coating film, and the clear coating film may be the film thicknesses of the undercoat coating film, the intermediate coating film, and the clear coating film of the conventionally known automobile exterior panels, respectively.

[0096] ·Interior panel coating The coating film for the interior panels of an automobile according to the present invention contains only a first base coating film (BI1) using the first base coating composition of the universal coating composition set for forming coating films for the exterior and interior panels of an automobile described above. The first base coating film (BI1), which is an essential element of the coating film for the interior panels of an automobile according to the present invention, will be illustrated below.

[0097] · First base coat (BI1) The first base coating film (BI1) is a base coating film formed using the first base coating composition of the universal coating composition set for forming coating films on the exterior and interior panels of the above-mentioned automobile. The base coating film on the interior panel is only the first base coating film (BI1).

[0098] The dry film thickness of the first base coating film (BI1) may be appropriately adjusted and is, for example, 5 to 20 μm, preferably 7 to 15 μm.

[0099] Other coatings on interior panels The coating film of the interior panel may include, in addition to the above-mentioned first base coating film (BI1), an undercoat coating film, and may further include one or two of an intermediate coating film and a clear coating film, as shown in Figures 2 to 4.

[0100] The materials for the undercoat coating film, the intermediate coating film, and the clear coating film may be the materials for the undercoat coating film, the intermediate coating film, and the clear coating film of the conventionally known interior panels of automobiles, respectively. The film thicknesses of the undercoat coating film, the intermediate coating film, and the clear coating film may be the film thicknesses of the undercoat coating film, the intermediate coating film, and the clear coating film of the conventionally known interior panels of automobiles, respectively.

[0101] (Method of forming coating film on exterior and interior panels of automobiles) The method for forming a coating film on an outer panel and an inner panel of an automobile according to the present invention comprises the steps of: preparing a universal coating composition set for forming a coating film on an outer panel and an inner panel of an automobile according to any one of the above (hereinafter sometimes referred to as "Step A"); A step of applying the first base coating composition to the surface side of the exterior panel to form an uncured first base coating film (BO1) (hereinafter sometimes referred to as "step B"); A step of applying the second base coating composition onto the uncured first base coating film (BO1) to form an uncured second base coating film (hereinafter sometimes referred to as "step C"); A step of curing the uncured first base coating film (BO1) and the uncured second base coating film to form a multi-layer coating film for the exterior panel (hereinafter sometimes referred to as "step D"); A step of applying the first base coating composition to the surface side of the inner panel to form an uncured first base coating film (BI1) (hereinafter sometimes referred to as "step E"); and a step (hereinafter sometimes referred to as "step F") of curing the uncured first base coating film (BI1) to form a first base coating film (BI1), The method for forming coatings for the exterior and interior panels of an automobile includes only the first base coating (BI1) as a base coating.

[0102] Hereinafter, steps A to F of the method for forming coating films on exterior and interior panels of an automobile according to the present invention will be described by way of example.

[0103] ·Process A In step A, a universal coating composition set for forming coating films on the exterior and interior panels of an automobile as described above is prepared.

[0104] ·Process B In step B, a first base paint composition is applied to the surface side of the exterior panel to form an uncured first base paint film (BO1).

[0105] The method of applying the first base coating composition is not particularly limited, and any conventional method for applying a base coating for an outer panel of an automobile can be used. Examples of the method of applying the first base coating composition include spray coating and rotary atomization electrostatic coating.

[0106] The outer panel to which the first base paint composition is applied in step B is usually an intermediate paint film.

[0107] The thickness of the uncured first base coating film (BO1) is not particularly limited, and may be appropriately adjusted according to the desired dry film thickness.

[0108] ·Process C In step C, a second base coating composition is applied onto the uncured first base coating film (BO1) to form an uncured second base coating film.

[0109] The method of applying the second base coating composition is not particularly limited, and can be a conventional method of applying a base coating for an outer panel of an automobile. The method of applying the second base coating composition can be, for example, spray coating, rotary atomization electrostatic coating, etc. The method of applying the first base coating composition in step B and the method of applying the second base coating composition in step C can be the same or different.

[0110] The thickness of the uncured second base coating film is not particularly limited, and may be appropriately adjusted according to the desired dry film thickness.

[0111] ·Process D In step D, the uncured first base coating film (BO1) and the uncured second base coating film are cured to form a multi-layer coating film for the exterior panel. The curing method may be, for example, heat curing. The heat curing conditions may be, for example, a temperature of 120 to 160°C and 10 to 30 minutes.

[0112] Step D simply involves curing the uncured first base coating film (BO1) and the uncured second base coating film to form a multi-layer coating film for the exterior panel; in addition to these two layers, an uncured clear coating film formed on the uncured second base coating film may also be cured together.

[0113] ·Process E In step E, a first base paint composition is applied to the front surface side of the inner plate to form an uncured first base paint film (BI1).

[0114] The method of applying the first base coating composition is not particularly limited, and any conventionally known method for applying base coatings for the interior panels of automobiles can be used. Examples of the method of applying the first base coating composition include spray coating.

[0115] The target of the inner plate to be coated with the first base coating composition in step E can be appropriately selected depending on the configuration of the coating film of the inner plate. The target of the inner plate to be coated with the first base coating composition is, for example, an intermediate coating film or an undercoat coating film as shown in Figures 2 to 5.

[0116] The thickness of the uncured first base coating film (BI1) is not particularly limited, and may be appropriately adjusted according to the desired dry film thickness.

[0117] ·Process F In step F, the uncured first base coating film (BI1) is cured to form the first base coating film (BI1). The curing method may be, for example, heat curing. The heat curing conditions may be, for example, a temperature of 120 to 160° C. and a time of 10 to 30 minutes.

[0118] In the method for forming a coating film for an outer panel and an inner panel of an automobile according to the present invention, the coating film for the inner panel contains only the first base coating film (BI1) as a base coating film, and therefore does not include a step of applying a second base paint composition or another base paint to the surface side of the inner panel.

[0119] In the method for forming coating films on the outer and inner panels of an automobile according to the present invention, the order of the steps is not particularly limited, except that among the steps A to F, step A is the first, step C is after step B, and step F is after step E. As described above, in the painting of an automobile, the inner panel side is usually painted before the outer panel side, and the coating film on the inner panel and the coating film on the outer panel are cured at the same time, that is, step E is before steps B, C, D, and F. However, depending on the vehicle model or manufacturing process, for example, steps B, C, and D may be performed, and then steps E and F may be performed, or steps E and B may be performed simultaneously (for example, step E is performed on the left half of the vehicle body while step B is performed on the right half of the vehicle body). Even when the outer panel side is painted first and then the inner panel side is painted, as described above, the windows and seal members are not attached to the vehicle body at this point, so that, for example, when painting the dash panel part inside the vehicle, the first base coating composition may adhere to the bonnet from the front part. Even in such a case, the universal paint composition set of the present invention reduces dust streaks because the first and second base paint compositions each contain a predetermined amount of a scaly luster pigment having a predetermined average particle size.

[0120] In one embodiment, step E is performed, then step B is performed, then step C is performed, then steps F and D are performed.

[0121] The method of the present invention for forming coating films on the outer and inner panels of an automobile may include a conventionally known step of forming coating films on the outer and inner panels of an automobile in addition to steps A to F. Examples of such steps include a step of forming an undercoat coating film on the outer and inner panels of an automobile, a step of forming an intermediate coating film on the outer or inner panel side, a step of applying a clear paint onto the uncured second base coating film of the outer panel to form an uncured clear coating film, and a step of curing the uncured clear coating film to form a clear coating film. EXAMPLES

[0122] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.

[0123] Details of each component of the coating composition used in the examples are as follows. Resin component 1: Acrylic emulsion resin, average particle size 150 nm, non-volatile content 20%, solid acid value 20 mg KOH / g, hydroxyl value 40 mg KOH / g, prepared by the method of Production Example 6 in paragraph

[0123] of JP2014-147918A. Resin component 2: Water-soluble acrylic resin, non-volatile content 30.0%, solid content acid value 40 mg KOH / g, hydroxyl value 50 mg KOH / g, prepared by the method of Production Example 8 in paragraph

[0125] of JP2014-147918A Resin component 3: Sanyo Chemical Industries, Ltd. product name "Primepol PX-1000", bifunctional polyether polyol, number average molecular weight 400, hydroxyl value 278 mg KOH / g, primary / secondary hydroxyl value ratio = 63 / 37, non-volatile content 100% Resin component 4: Avecia's product name "Neolet's R-9603", polycarbonate-based urethane emulsion resin, non-volatile content 33% Tertiary amine (neutralizer): Dimethylethanolamine 10% by weight aqueous solution Hardener: Mitsui Chemicals' product name "Cymel 204", mixed alkylated melamine resin, 100% non-volatile content First scale-like luster pigment: trade name "Alpaste (registered trademark) 06-0672" manufactured by Toyo Aluminum Co., Ltd., silver color, average particle size 17 μm, indicated as "No. 1" in Table 1 First and second scale-like luster pigments: trade name "Alpaste (registered trademark) 93-0647" manufactured by Toyo Aluminum Co., Ltd., silver color, average particle size 20 μm, indicated as "No. 2" in Table 1 First scale-like luster pigment: Toyo Aluminum's product name "TCR (registered trademark)-2020", silver color, average particle size 23 μm, indicated as "No. 3" in Table 1 Second scale-like glitter pigment: glass flakes coated with metal oxide, product name "Metashine (registered trademark) ST1018RSJ3" manufactured by Nippon Sheet Glass Co., Ltd., colorless, average particle size 18 μm, indicated as "No. 4" in Table 1 Scaly luster pigment: Toyo Aluminum Co., Ltd. product name "Aluminum Paste 01-0651", silver color, average particle size 9 μm, indicated as "No. 5" in Table 1 Scaly luster pigment: Asahi Kasei Aluminum Paste CP-310, silver color, average particle size 12 μm, listed as "No. 6" in Table 1. Scaly glitter pigment: Obtained by crushing and classifying the above No. 4 second glitter pigment, with an average particle size of 12 μm, and referred to as "No. 7" in Table 1 Color pigment 1 (non-luminescent pigment): "EMPEROR-2000 Black" manufactured by CABOT, black color, indicated as "Color No. 1" in Table 1 Color pigment 2 (non-bright pigment): Sanyo Pigment Co., Ltd.'s product name "Cyanine Blue G-314", blue color, indicated as "Color No. 2" in Table 1 Color pigment 3 (non-luminescent pigment): Clariant's product name "Violet RL-NF", violet, indicated as "Color No. 3" in Table 1 Corrosion inhibitor for luster pigments: Lauryl acid phosphate. Clear paint: Nippon Paint Automotive Coatings' product name "Macflow O-1810 Clear", an acid epoxy curing acrylic resin paint

[0124] Details of other materials and equipment used in the examples are as follows: Steel plate: zinc phosphate-treated SPCC-SD steel plate, dimensions 20cm x 30cm x thickness 0.8cm Spectrophotometer: Hitachi product name "U-3310" Multi-angle spectrophotometer: X-rite's product name "MA68 II" Multi-angle colorimeter: BYK's product name "BYK-mac i"

[0125] (Examples 1 to 18 and Comparative Examples 1 to 9) Preparation of the first base coating composition In addition to the scaly luster pigment and coloring pigment in the formulation (PWC) shown in Table 1, the following amounts of resin components, curing agent, tertiary amine and corrosion inhibitor were blended and uniformly dispersed to obtain a first base coating composition. Resin component 1: 200 parts by weight (non-volatile content 40 parts by weight) Resin component 2: 16.7 parts by weight (non-volatile content 5 parts by weight) Resin component 3: 10 parts by weight (non-volatile content 10 parts by weight) Resin component 4:5 parts by weight (non-volatile content 1.65 parts by weight) Hardener: 15.2 parts by weight (non-volatile content 15.2 parts by weight) Tertiary amine: 40 parts by mass (concentration 10% by mass) Corrosion inhibitor: 0.2 parts by weight (non-volatile content 0.1 parts by weight)

[0126] Preparation of the second base coating composition In addition to the scaly luster pigment and coloring pigment in the formulation (PWC) shown in Table 1, the same amounts of resin component, curing agent, tertiary amine and corrosion inhibitor as in the first base paint composition were blended and uniformly dispersed to obtain a second base paint composition.

[0127] -Exterior preparation A zinc phosphate-treated steel plate, intended for use as an automobile exterior panel, was coated in the same manner as in Example 1 of Patent Document 1 with a cationic electrocoat paint and an intermediate coat paint, in that order, to prepare an exterior panel having an undercoat paint film and an intermediate coat paint film formed thereon.

[0128] Preparation of the inner plate A zinc phosphate-treated steel sheet, intended for use as an interior panel of an automobile, was coated with a cationic electrodeposition paint in the same manner as in Example 1 of Patent Document 1 to prepare an interior panel on which an undercoat coating film had been formed.

[0129] Interior panel painting The first base paint composition of Example 1 was applied onto the undercoat film of the inner panel with a spray gun to a dry film thickness of 10 μm to form an uncured first base paint film (BI1).

[0130] -Exterior painting Next, as shown in FIG. 6, an outer panel 9 assuming a front door at a height of 25 mm from the inner panel 7 on which the uncured first base coating film (BI1) was formed, and an outer panel 10 assuming a rear door at a height of 10 mm were placed with a gap of 10 mm. Next, under standard robot painting conditions, the first base paint composition and the second base paint composition were applied to the outer panels from the left end of the outer panel 9 in FIG. 6 to the right end of the outer panel 10 in order to have dry film thicknesses of 8 μm and 10 μm, respectively, to form an uncured first base coating film (BO1) and an uncured second base coating film. Next, the inner panel 7 and the outer panels 9 and 10 were preheated at a temperature of 80° C. for 3 minutes. Next, a clear paint was applied to the preheated uncured first base coating film (BI1) to a dry film thickness of 15 μm, and a clear paint was applied to the uncured second base coating film to a dry film thickness of 30 μm, to form uncured clear coating films on the inner panel and the outer panel. Next, the inner panel 7 and the outer panels 9 and 10 were baked at a temperature of 140°C for 30 minutes to form a first base coating film (BI1) 8 and a clear coating film on the inner panel 7, and a first base coating film (BO1) 4, a second base coating film 5 and a clear coating film on the outer panels 9 and 10.

[0131] · Formation of the second base coat alone Separately from the above-mentioned inner and outer panels, the second base coating composition was applied to a polypropylene substrate so as to give a dry film thickness of 10 μm and baked at a temperature of 140° C. for 30 minutes to form only the second base coating film.

[0132] Dust streak evaluation The resulting painted surfaces of the inner panels of each Example and Comparative Example were visually inspected and evaluated for dust streaks according to the following criteria. The evaluation results are shown in Table 1. Evaluations A and B are acceptable. Photographs of the coatings on the inner panels of Example 18 and Comparative Example 2 are shown in Figures 7 and 8, respectively. A: No discomfort caused by dust streaks B: Dust streaks may appear strange depending on the observation angle, but are within the acceptable range. C: Dust streaks are visible depending on the observation angle, creating a sense of incongruity D: Dust streaks are easily recognized and a strong sense of incongruity is felt

[0133] Design evaluation The color depth and graininess G value of the obtained exterior panels of each Example and Comparative Example were measured as follows to evaluate the design of the multi-layer coating film of the exterior panel. The color depth and graininess G value were measured after the exterior panel was cooled to the standard temperature after baking the coating film.

[0134] -Depth of color in shade direction Using a multi-angle spectrophotometer, the L of the multi-layer coating on the exterior panel was measured. * The evaluation results are shown in Table 1. * The lower the 110 value, the greater the depth of color in the shade direction (jet blackness in the case of a black coating).

[0135] ·brightness Using a multi-angle colorimeter, the particle G value of the multi-layer coating on the exterior panels was measured. The evaluation results are shown in Table 1. The higher the G value, the higher the brightness.

[0136] Measurement of light transmittance The second base coating film formed independently was peeled off from the propylene substrate, and the light transmittance of the peeled second base coating film was measured at wavelengths of 360 to 700 nm every 10 nm using a spectrophotometer, and the average value was calculated. The results are also shown in Table 1.

[0137] [Table 1] In Table 1, the amount of pigment represents the PWC.

[0138] As shown in Table 1, in the examples, the base coating film for the exterior and interior panels of an automobile could be used in common when forming the coating film for the exterior and interior panels, and dust streaks on the base coating film for the interior panel could be reduced. In addition, dust streaks on the base coating film for the interior panel were reduced, and coating films for the exterior and interior panels of an automobile with excellent design properties could be formed.

[0139] In the photograph of the coating film of the inner panel of Example 18 in Fig. 7, the entire coating film has a high jet black color. On the other hand, in the photograph of the coating film of the inner panel of Comparative Example 2 in Fig. 8, a whitish dust streak was observed vertically in the center of the coating film. [Industrial Applicability]

[0140] According to the present invention, it is possible to provide a coating composition set that can be used for the base coating film of an automobile exterior panel and interior panel when forming the coating film of the exterior panel and interior panel, and can reduce dust streaks on the base coating film of the interior panel. Also, according to the present invention, it is possible to provide a coating film of an automobile exterior panel and interior panel that has excellent design properties, with reduced dust streaks on the base coating film of the interior panel. Also, according to the present invention, it is possible to provide a method for forming a coating film of an automobile exterior panel and interior panel that has excellent design properties, with reduced dust streaks on the base coating film of the interior panel. [Explanation of symbols]

[0141] 1: Outer panel 2: Undercoat 3: Undercoat coating 4: First base coat (BO1) 5: Second base coat 6: Clear coating 7: Inner plate 8: First base coat (BI1) 9: Outer panel designed for the front door 10: Exterior panel designed for rear doors

Claims

1. A universal coating composition set for forming coating films on exterior and interior panels of an automobile, comprising: The coating film of the outer plate is a multi-layer coating film including a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer plate side, The coating film of the inner panel includes only a first base coating film (BI1) as a base coating film, The common coating composition set includes a first base coating composition that forms the first base coating film (BO1) and the first base coating film (BI1), and a second base coating composition that forms the second base coating film; The first base coating composition includes a resin component, a curing agent, and a first scale-like glittering pigment having an average particle size of 20 μm to 25 μm, The second base coating composition includes a resin component, a curing agent, and a second scale-like glittering pigment having an average particle size of 17 μm to 19 μm, The amount of the first scale-like glittering pigment is 0.10 to 2.5 parts by mass per 100 parts by mass of the total solid content of the first base coating composition; A universal coating composition set for forming coating films on exterior and interior panels of an automobile, wherein the amount of the second scale-like glittering pigment is 0.5 to 5.0 parts by mass per 100 parts by mass of the total solids content of the second base coating composition.

2. A universal coating composition set for forming coating films on exterior and interior panels of an automobile, comprising: The coating film of the outer plate is a multi-layer coating film including a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer plate side, The coating film of the inner panel includes only a first base coating film (BI1) as a base coating film, The common coating composition set includes a first base coating composition that forms the first base coating film (BO1) and the first base coating film (BI1), and a second base coating composition that forms the second base coating film; The first base coating composition includes a resin component, a curing agent, and a first scale-like glittering pigment having an average particle size of 15 μm to 25 μm, The second base coating composition includes a resin component, a curing agent, and a second scale-like glittering pigment having an average particle size of 15 μm to 25 μm, The first scale-like glittering pigment is one type, The second scale-like bright pigment is two or more kinds, The amount of the first scale-like glittering pigment is 0.10 to 2.5 parts by mass per 100 parts by mass of the total solid content of the first base coating composition; A universal coating composition set for forming coating films on exterior and interior panels of an automobile, wherein the amount of the second scale-like glittering pigment is 0.5 to 5.0 parts by mass per 100 parts by mass of the total solids content of the second base coating composition.

3. A universal coating composition set for forming coating films on exterior and interior panels of an automobile, comprising: The coating film of the outer plate is a multi-layer coating film including a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer plate side, The coating film of the inner panel includes only a first base coating film (BI1) as a base coating film, The common coating composition set includes a first base coating composition that forms the first base coating film (BO1) and the first base coating film (BI1), and a second base coating composition that forms the second base coating film; The first base coating composition includes a resin component, a curing agent, and a first scale-like glittering pigment having an average particle size of 15 μm to 25 μm, The second base coating composition includes a resin component, a curing agent, and a second scale-like glittering pigment having an average particle size of 15 μm to 25 μm, The amount of the first scale-like glittering pigment is 0.10 to 1.8 parts by mass per 100 parts by mass of the total solid content of the first base coating composition; A universal coating composition set for forming coating films on exterior and interior panels of an automobile, wherein the amount of the second scale-like glittering pigment is 2.0 to 5.0 parts by mass per 100 parts by mass of the total solids content of the second base coating composition.

4. The second scale-like bright pigment is a glass substrate coated with a metal oxide, the universal coating composition set for forming a coating film on an outer panel and an inner panel of an automobile according to any one of claims 1 to 3.

5. The L of the multi-layer coating film at a viewing angle of 110° when the dry film thickness of the first base coating film (BO1) is 8 μm and the dry film thickness of the second base coating film is 10 μm. * 5. The universal coating composition set for forming coating films on exterior and interior panels of an automobile according to claim 1, wherein the 110 value is less than 2 and the particle sensitivity G value is greater than 3.

5.

6. A coating for the exterior and interior panels of an automobile, The coating film of the outer panel includes a multi-layer coating film using the universal coating composition set for forming coating films of the outer panel and the inner panel of an automobile according to any one of claims 1 to 5, The multi-layer coating film includes a first base coating film (BO1) and a second base coating film adjacent to each other in order from the outer panel side, The coating film for the interior panel of an automobile includes only a first base coating film (BI1) using a first base coating composition of the universal coating composition set for forming coating films for the exterior and interior panels of an automobile according to any one of claims 1 to 5.

7. A step of preparing a universal coating composition set for forming a coating film on an outer panel and an inner panel of an automobile according to any one of claims 1 to 5; A step of applying the first base coating composition to a surface side of the exterior panel to form an uncured first base coating film (BO1); A step of applying the second base coating composition onto the uncured first base coating film (BO1) to form an uncured second base coating film; A step of curing the uncured first base coating film (BO1) and the uncured second base coating film to form a multi-layer coating film for the exterior panel; A step of applying the first base coating composition to a surface side of the inner panel to form an uncured first base coating film (BI1); and curing the uncured first base coating film (BI1) to form a first base coating film (BI1), The method for forming coating films for exterior and interior panels of an automobile, wherein the coating film for the interior panel contains only the first base coating film (BI1) as a base coating film.

Citation Information

Patent Citations

  • Method of coating outside and inside panel part of automobile

    JP2002205006A

  • Method for forming coating film on vehicle body, and automobile having coating film

    JP2003093966A

  • Method for forming bright metallic coating film

    JP2004358329A

  • Laminated coating film, its forming method and coated product

    JP2005137952A

  • Metallic coating method of car body

    JP2006272249A