Laminated films, lids and containers

A three-layer laminated film with specific resin compositions and organic sulfonate in the intermediate layer addresses the issue of water droplet adhesion in transparent lids, ensuring clear visibility and easy opening.

JP7557384B2Active Publication Date: 2024-09-27SUMIKA PLASTECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021008286
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-31
Filing Date
2021-01-21
Publication Date
2024-09-27
Estimated Expiration
2041-01-21

AI Technical Summary

Technical Problem

Conventional easy-peel films used in transparent lids for food containers suffer from water droplet adhesion, leading to clouding and reduced visibility of contents, necessitating improvements in transparency and antifogging properties.

Method used

A three-layer laminated film comprising a sealing layer made of polyester resin and nonionic surfactant, an intermediate layer with ethylene-unsaturated carboxylic acid ester copolymer and nonionic surfactant, and a base layer of olefin resin, with at least one intermediate layer containing an organic sulfonate, to enhance easy peelability, transparency, and antifogging properties.

Benefits of technology

The laminated film achieves excellent transparency and antifogging properties, allowing clear visibility of contents even when water droplets form, while maintaining easy peelability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557384000001
    Figure 0007557384000001
Patent Text Reader

Abstract

To provide a laminated film having easy peelability, transparency, and antifogging properties.SOLUTION: The laminated film is formed by laminating a seal layer containing a polyester resin and a nonionic surfactant, an intermediate layer containing an ethylene-unsaturated carboxylic acid ester copolymer and a nonionic surfactant, and a substrate layer containing an olefin resin in this order. At least one of the seal layer and the intermediate layer contains an organic sulfonate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film, a covering material, and a container. [Background technology]

[0002] In food packaging, a packaging form in which the contents are placed in a cup-shaped container body and the opening of the container body is covered with a lid is often used. One such packaging form is a so-called top seal, in which an easy-peel film equipped with a support material and a sealant is heat-sealed to the container as a lid material on the flange portion around the opening of the container body.

[0003] For example, Patent Document 1 discloses a four-layer laminate film that includes a laminate layer, an intermediate layer, an adhesive layer, and a heat seal layer and can be used as an easy-peel film in food packaging and the like. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2015 / 046132 Summary of the Invention [Problem to be solved by the invention]

[0005] Top-sealed packaging containers have excellent sealing properties, which contribute to extending the shelf life of foods. In addition, compared to snap-on lids, which require a certain thickness to achieve a certain level of strength, the lid material of top-sealed packaging containers can be made thin and can be formed with a small amount of resin, which has the advantage of reducing the burden on the environment. For this reason, top-sealed packaging containers have been used in recent years to package a variety of foods, such as salads, cut fruits, side dishes, pickles, yogurt, and jellies.

[0006] In top-sealed food packaging containers, at least a part of the lid is made transparent so that the state of the contents can be visually confirmed. However, when a conventional easy-peel film is used as a sealant for such a transparent lid, if the contents contain moisture, a problem occurs in that water droplets adhere to the inside of the lid, causing it to become cloudy. In such products, the contents cannot be clearly seen, and the commercial value may decrease.

[0007] In response to this, the laminate film described in Patent Document 1 attempts to prevent adhesion of water droplets by adding a nonionic surfactant as an anti-fogging agent. However, there is a demand for further improvements in transparency and anti-fogging properties, as well as a demand for these properties to be compatible with easy peelability.

[0008] The present invention has been made in consideration of the above problems, and has an object to provide a laminated film that combines easy peelability with transparency and anti-fogging properties, and related techniques thereof. [Means for solving the problem]

[0009] As a result of intensive research into the above-mentioned problems, the inventors have discovered that a laminate film having a three-layer structure made of a specific resin, in which at least one of the sealing layer and the intermediate layer contains an organic sulfonate, exhibits excellent peelability as well as excellent transparency and anti-fogging properties, and have completed the present invention.

[0010] A laminated film according to one embodiment of the present invention is a laminated film comprising a sealing layer, an intermediate layer, and a base layer laminated in this order, wherein the sealing layer contains a polyester-based resin and a nonionic surfactant, the intermediate layer contains an ethylene-unsaturated carboxylic acid ester copolymer and a nonionic surfactant, the base layer contains an olefin-based resin, and at least one of the sealing layer and the intermediate layer further contains an organic sulfonate. Effect of the Invention

[0011] According to one aspect of the present invention, it is possible to provide a laminate film that has easy peelability as well as transparency and anti-fogging properties, and related techniques thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each of the configurations described below, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples. In addition, in this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more, B or less."

[0013] Each aspect included in the present invention will be described in detail below.

[0014] <Laminated film> The laminated film according to one embodiment of the present invention is an easily peelable film that can be easily peeled off from a container after sealing the container. The laminated film has at least three layers, a seal layer, an intermediate layer, and a base layer. The easily peelable film is also called an easy peel film.

[0015] The seal layer is a layer that heat-seals the laminated film to the adherend by heating the laminated film. The intermediate layer is a layer located between the base layer and the seal layer, and the base layer is a layer that supports the seal layer and the intermediate layer. In addition, any layer such as a resin film, a metal foil, or paper can be laminated on the surface of the base layer side of the laminated film depending on the packaging purpose, etc.

[0016] The laminated film covers, for example, the opening of a container with its surface on the sealing layer side, and the container is sealed by abutting the sealing layer against a flange portion around the opening and heat-sealing the sealing layer.

[0017] When the laminated film is peeled off to open the container, the seal layer heat-sealed to the container is sheared so that the portion heat-sealed to the flange of the container remains on the container side, and the remaining seal layer remains on the intermediate layer and base layer side. At this time, the laminated film causes interlayer delamination between the intermediate layer and the seal layer at the portion where the seal layer heat-sealed to the flange of the container. This interlayer delamination contributes to the easy peelability of the laminated film.

[0018] The laminated film is formed from a resin composition for the seal layer, a resin composition for the intermediate layer, and a resin composition for the base layer. The resin composition for the seal layer and the resin composition for the intermediate layer each contain a nonionic surfactant. In addition, at least one of the resin compositions for the seal layer and the resin composition for the intermediate layer contains an organic sulfonate, and at least one of the resin compositions for the seal layer and the resin composition for the intermediate layer contains an inorganic salt. This allows the laminated film to have both transparency and anti-fogging properties as well as easy peelability.

[0019] [Nonionic Surfactant] Both the resin composition for the seal layer and the resin composition for the intermediate layer contain a nonionic surfactant.

[0020] In the resin composition for the seal layer, the content of the nonionic surfactant is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, based on 100% by mass of the resin composition for the seal layer. The nonionic surfactant contributes to the migration (also called bleeding) of the organic sulfonate blended in the seal layer and / or intermediate layer to the outside of the layer, and stably exerts the antifogging effect of the organic sulfonate. By the content of the nonionic surfactant in the resin composition for the seal layer being 0.05% by mass or more, the migration of the organic sulfonate between the seal layer / intermediate layer and to the surface of the seal layer immediately after film formation (initial stage) and over time occurs favorably, and the laminated film can be given high antifogging properties. In addition, from the viewpoint of ensuring an appropriate seal strength with the container body, the content of the nonionic surfactant in the resin composition for the seal layer is preferably 5.0% by mass or less, more preferably 4% by mass or less.

[0021] The content of the nonionic surfactant in the resin composition for the intermediate layer is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, based on 100% by mass of the resin composition for the intermediate layer. By having the content of the nonionic surfactant in the resin composition for the intermediate layer be 0.05% by mass or more, the migration of the organic sulfonate between the seal layer / intermediate layer immediately after film formation (initial stage) and over time occurs favorably, and the laminated film can be given high anti-fogging properties. In addition, from the viewpoint of ensuring the interlayer adhesive strength with the seal layer, the content of the nonionic surfactant in the resin composition for the intermediate layer is preferably 5.0% by mass or less, more preferably 4% by mass or less.

[0022] The nonionic surfactant contained in the sealing layer and the intermediate layer includes a compound having a hydrophobic group derived from a fatty acid having 6 to 22 carbon atoms, an aliphatic alcohol having 6 to 22 carbon atoms, an aliphatic amide having 6 to 22 carbon atoms, etc., and a hydrophilic group derived from a polyol, etc. In the nonionic surfactant, a compound having a hydrophobic group and a compound having a hydrophilic group are bonded to each other by a bond such as an ether bond or an ester bond.

[0023] Examples of aliphatic carboxylic acids having 6 to 22 carbon atoms, which are compounds having a hydrophobic group, include caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, palmitic acid, margaric acid, stearic acid, oleic acid, linoleic acid, linolenic acid, arachidonic acid, sorbic acid, erucic acid, undecylic acid, undecylenic acid, tridecylic acid, and pentadecylic acid.

[0024] Examples of aliphatic alcohols having 6 to 22 carbon atoms, which are compounds having a hydrophobic group, include caproic alcohol, heptyl alcohol, capryl alcohol, pelargonic alcohol, capric alcohol, lauryl alcohol, myristyl alcohol, palmitoleic alcohol, oleyl alcohol, linoleyl alcohol, linolenyl alcohol, erucyl alcohol, undecyl alcohol, tridecyl alcohol, pentadecyl alcohol, cetyl alcohol, isocetyl alcohol, heptadecyl alcohol, stearyl alcohol, and isostearyl alcohol.

[0025] Examples of aliphatic amides having 6 to 22 carbon atoms, which are compounds having a hydrophobic group, include caproic acid amide, enanthic acid amide, caprylic acid amide, pelargonic acid amide, capric acid amide, lauric acid amide, myristic acid amide, palmitic acid amide, margaric acid amide, stearic acid amide, oleic acid amide, linoleic acid amide, linolenic acid amide, arachidonic acid amide, and sorbic acid amide.

[0026] As the compound having a hydrophilic group, for example, a trivalent to hexavalent polyol can be preferably used. Examples of such polyols include glycerin, sorbitol, glucose, pentaerythritol, sorbitan, sorbide, diglycerin, ethylene glycol diglyceryl ether, triglycerin, tetraglycerin, and dipentaerythritol, and the polyol may be ethylene glycol, polyethylene glycol, etc.

[0027] When the nonionic surfactant has a hydrophobic group derived from an aliphatic amide having 6 to 22 carbon atoms, examples of the nonionic surfactant include alkyl diethanolamides, such as octyl diethanolamide, nonyl diethanolamide, decyl diethanolamide, undecyl diethanolamide, dodecyl diethanolamide, tridecyl diethanolamide, tetradecyl diethanolamide, cetyl diethanolamide, heptadecyl diethanolamide, octadecyl diethanolamide, and oleyl diethanolamide.

[0028] Among nonionic surfactants, a partial ester compound of a polyol and an aliphatic carboxylic acid, or an ether compound of a polyol and an aliphatic alcohol is preferably used, and a partial ester compound of a trihydric to hexahydric polyol and a fatty acid is more preferably used.

[0029] (Organic Sulfonates) At least one of the resin composition for the seal layer and the resin composition for the intermediate layer contains an organic sulfonate.

[0030] It is preferable that the content of organic sulfonate in one of the resin compositions for the seal layer and the resin composition for the intermediate layer is 0.05% by mass or more, and the content of organic sulfonate in the other resin composition is less than 0.05% by mass. As a result, when a seal layer is formed from the resin composition for the seal layer and an intermediate layer is formed from the resin composition for the intermediate layer and laminated together, a gradient in the concentration of organic sulfonate occurs in the seal layer and the intermediate layer. The present inventors have found that creating a gradient in the concentration of organic sulfonate in the seal layer and the intermediate layer contributes to further improving the anti-fogging properties of the laminated film, and have completed the present invention. From this perspective, it is more preferable that the composition is blended so that the content of organic sulfonate in one of the resin compositions for the seal layer and the resin composition for the intermediate layer is 0.05% by mass or more, and no organic sulfonate is blended in the other resin composition. This allows the organic sulfonate to migrate more suitably from the intermediate layer to the seal layer, or from the seal layer to the intermediate layer, in a laminate film formed from these compositions, thereby imparting higher anti-fogging properties to the laminate film. The laminate film formed from these resin compositions may have an organic sulfonate content of 0.05% by mass or more in one of the seal layer and the intermediate layer.

[0031] A more preferred embodiment of the present invention is a laminate film having an intermediate layer and a seal layer formed from a resin composition for the intermediate layer, the resin composition for the seal layer being blended with an organic sulfonate, and the resin composition for the seal layer being not blended.

[0032] In addition, the content of the organic sulfonate in one of the resin compositions for the seal layer and the resin composition for the intermediate layer is preferably 3% by mass or less. By having the content of the organic sulfonate in the resin composition be 3% by mass or less, high transparency can be imparted to the laminated film.

[0033] As the organic sulfonate, an alkali metal salt of an organic sulfonic acid, for example, an alkali metal salt of an alkyl sulfonate, an alkali metal salt of an alkylaryl sulfonate, an alkali metal salt of an aliphatic sulfonate, etc., is preferably used. In particular, an organic sulfonate having an alkyl group with a carbon number of 6 to 22 is preferable. These may be used alone or in combination of two or more kinds.

[0034] Examples of the alkali metal salt include lithium salts, sodium salts, and potassium salts.

[0035] Examples of alkylsulfonic acids constituting the organic sulfonate include hexylsulfonic acid, octylsulfonic acid, nonylsulfonic acid, decylsulfonic acid, undecylsulfonic acid, dodecylsulfonic acid, tridecylsulfonic acid, tetradecylsulfonic acid, pentadecylsulfonic acid, hexadecylsulfonic acid, heptadecylsulfonic acid, octadecylsulfonic acid, and behenylsulfonic acid.

[0036] Examples of the alkylarylsulfonic acid constituting the organic sulfonate include alkylbenzenesulfonic acid, alkylnaphthalenesulfonic acid, etc. More specifically, examples of the alkylarylsulfonic acid include hexylbenzenesulfonic acid, behenylbenzenesulfonic acid, and dibutylnaphthalenesulfonic acid.

[0037] Examples of the aliphatic sulfonate constituting the organic sulfonate include diethyl sulfosuccinate, dipropyl sulfosuccinate, dodecyl sulfoacetate, and nonylphenoxy polyethylene glycol sulfoacetate.

[0038] Among the organic sulfonates, alkali metal alkylsulfonates and alkali metal alkylarylsulfonates are preferably used.

[0039] [Inorganic salts] At least one of the resin compositions for the seal layer and the resin composition for the intermediate layer preferably contains an inorganic salt. The organic sulfonate and the inorganic salt may be contained in the same layer or in different layers. Since the antifogging property is synergistically increased, it is preferable that the organic sulfonate and the inorganic salt are contained in the same layer.

[0040] When the resin composition for the seal layer or the resin composition for the intermediate layer contains an inorganic salt, the content of the inorganic salt in each layer is preferably 0.01% by mass or more, more preferably 0.02% by mass or more. In addition, from the viewpoint of obtaining a film with good appearance, the content of the inorganic salt in each layer is preferably 1% by mass or less, more preferably 0.5% by mass or less. By having the content of the inorganic salt in each layer within the above range, the anti-fogging property is further improved by the synergistic effect with the nonionic surfactant present in the layer.

[0041] Examples of inorganic salts include sodium sulfate, potassium sulfate, calcium sulfate, lithium sulfate, sodium chloride, potassium chloride, lithium chloride, magnesium chloride, and calcium chloride. These may be used alone or in combination of two or more. Among inorganic salts, sodium chloride and sodium sulfate are preferably used.

[0042] [Resin composition for sealing layer] The resin composition for the sealing layer contains a polyester resin and a nonionic surfactant. More preferably, the resin composition for the sealing layer contains an olefin resin.

[0043] As described above, the resin composition for the seal layer contains 0.05% by mass or more and 5% by mass or less of a nonionic surfactant. Also, as described above, the resin composition for the seal may contain 3% by mass or less of an organic sulfonate and 1% by mass or less of an inorganic salt.

[0044] In addition, the resin composition for the sealing layer preferably contains an antiblocking agent and an antioxidant, and may contain other components.

[0045] (Polyester resin) The content of the polyester-based resin in the resin composition for the seal layer is preferably 60% by mass or more, more preferably 65% ​​by mass or more, based on 100% by mass of the resin composition for the seal layer. By having the content of the polyester-based resin in the resin composition for the seal layer be 60% by mass or more, sufficient seal strength is obtained when heat-sealed to the flange of the container body made of polyester-based resin, and good sealing properties are obtained, and suitable interlayer adhesive strength with the intermediate layer is shown, and easy peeling is obtained. In addition, from the viewpoint of easy peeling and anti-fogging properties, the content of the polyester-based resin in the polyester-based resin composition is preferably 95% by mass or less, more preferably 93% by mass or less.

[0046] The polyester resin contained in the resin composition for the seal layer includes crystalline polyester and amorphous polyester, and crystalline polyester is more preferable. The polyester resin exemplified by crystalline polyester and amorphous polyester is produced by polycondensation of dibasic acid and polyhydric alcohol. Examples of dibasic acid include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid, and aliphatic dicarboxylic acids such as adipic acid. Examples of polyhydric alcohol include diols such as ethylene glycol, butanediol, 1,4-cyclohexanedimethanol, pentaethylene glycol, 2,2-dimethyltrimethylene glycol, hexamethylene glycol, and neopentyl glycol. The above dibasic acid and polyhydric alcohol are used in any combination. Specifically, examples include terephthalic acid / ethylene glycol copolymer, terephthalic acid / ethylene glycol / 1,4-cyclohexanedimethanol terpolymer, 2,6-naphthalenedicarboxylic acid / ethylene glycol copolymer, and terphthalic acid / isophthalic acid / butanediol terpolymer.

[0047] The crystalline polyester in the present invention is a resin in which a crystallization peak and / or a melting peak can be observed by the following method. The melting behavior of the resin is measured under the following conditions using a differential scanning calorimeter (DSC220C manufactured by Seiko Electronics Industries Co., Ltd.) The melting curve is obtained by plotting the time on the horizontal axis and the heat of fusion on the vertical axis in each process, and the peak observed in process (ii) is the crystallization peak, and the peak observed in process (iii) is the melting peak. (i) Approximately 5 mg of a sample is heated from room temperature to 200°C at a rate of 30°C / min, and after the temperature increase is complete, the sample is held at this temperature for 5 minutes. (ii) Next, the temperature is lowered from 200° C. to −100° C. at a rate of 10° C. / min, and after the temperature drop is complete, the temperature is held at this temperature for 5 minutes. (iii) The temperature is then increased from -100°C to 200°C at a rate of 10°C / min.

[0048] From the viewpoint of inflation moldability, the crystalline polyester preferably has a melting point of 100 to 180° C. and a glass transition temperature of 10° C. or lower. An example of such a crystalline polyester is a resin commercially available under the trade name "Vylon" (manufactured by Toyobo Co., Ltd.).

[0049] (Olefin resin) The resin composition for the seal layer preferably contains an olefin resin. The content of the olefin resin in the resin composition for the seal layer is preferably 3% by mass or more and 39% by mass or less, based on 100% by mass of the resin composition.

[0050] Examples of olefin-based resins include ethylene-based resins and propylene-based resins. Examples of ethylene-based resins include polyethylenes such as low-density polyethylene and high-density polyethylene, ethylene-α-olefin copolymers such as ethylene / butene-1 copolymers and ethylene / hexene-1 copolymers, and ethylene copolymers consisting of one or more vinyl monomer-derived structural units and ethylene-derived structural units, such as ethylene-unsaturated carboxylic acid ester copolymers and ethylene-vinyl acetate copolymers. However, when using an ethylene copolymer consisting of one or more vinyl monomer-derived structural units and ethylene-derived structural units, such as ethylene-unsaturated carboxylic acid ester copolymers and ethylene-vinyl acetate copolymers, as the olefin-based resin, the content of ethylene-derived structural components in the ethylene copolymer is preferably 80% by mass or more and 95% by mass or less. A laminated film having a seal layer consisting of an ethylene copolymer consisting of one or more vinyl monomer-derived structural units and ethylene-derived structural units has excellent adhesive strength between the seal layer and the intermediate layer, and therefore can improve the appearance after peeling the laminated film from a container.

[0051] Examples of the vinyl monomer include unsaturated carboxylic acids such as acrylic acid and methacrylic acid, unsaturated carboxylic acid esters such as ethyl acrylate, methyl acrylate and ethyl methacrylate, and unsaturated carboxylic acid anhydrides such as maleic anhydride.

[0052] Other examples of the olefin-based resin include propylene-based resins such as propylene homopolymers, propylene-α-olefin block copolymers, propylene-α-olefin random copolymers, etc. The olefin-based resin may also be an ethylene-propylene copolymer.

[0053] (Anti-blocking agent) It is more preferable that the resin composition for the seal layer contains an antiblocking agent. The content of the antiblocking agent in the resin composition for the seal layer is preferably 3% by mass or less, more preferably 1% by mass or less, based on 100% by mass of the resin composition, from the viewpoint of ensuring an appropriate seal strength with the container body. The lower limit is not particularly limited, but may be, for example, 0.01% by mass or more, as an amount contributing to the antiblocking effect.

[0054] Examples of the antiblocking agent contained in the sealing layer and the intermediate layer described below include aluminosilicate, talc, diatomaceous earth, zeolite, mica, clay, crosslinked silicone particles, crosslinked polyamide particles, crosslinked polyacrylic particles, crosslinked polystyrene particles, etc. These may be used alone or in combination of two or more kinds.

[0055] (Antioxidants) The resin composition for the sealing layer preferably contains an antioxidant. The content of the antioxidant in the resin composition for the sealing layer is preferably 1% by mass or less, more preferably 0.5% by mass or less, based on 100% by mass of the resin composition, from the viewpoint of ensuring an appropriate seal strength with the container body. The lower limit is not particularly limited, but may be, for example, 0.01% by mass or more, as an amount contributing to the antioxidant effect.

[0056] Examples of the antioxidant include phenols such as 2,6-di-t-butyl-p-cresol (BHT), tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (manufactured by Ciba Specialty Chemicals, trade name: IRGANOX (registered trademark) 1010) and n-octadecyl-3-(4'-hydroxy-3,5'-di-t-butylphenyl)propionate (manufactured by Ciba Specialty Chemicals, trade name: IRGANOX (registered trademark) 1076). phosphite stabilizers such as bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite and tris(2,4-di-t-butylphenyl)phosphite; and phenol-phosphite bifunctional stabilizers such as 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine (manufactured by Sumitomo Chemical Co., Ltd., trade name: Sumilizer (registered trademark) GP). These antioxidants may be used alone or in combination of two or more kinds.

[0057] (Other Ingredients) The polyester-based resin composition may contain additives such as resins other than the above-mentioned polyester-based resins and olefin-based resins, compatibilizers, lubricants, heat stabilizers, UV absorbers, antistatic agents, antifungal agents, and antibacterial agents, as long as the effects of the present invention are not impaired.

[0058] [Resin composition for intermediate layer] The resin composition for the intermediate layer contains an ethylene-unsaturated carboxylic acid ester copolymer and a nonionic surfactant, and the resin composition for the seal layer preferably contains an olefin resin.

[0059] As described above, the resin composition for the intermediate layer contains 0.05% by mass or more and 5% by mass or less of a nonionic surfactant. Also, as described above, the resin composition for the intermediate layer may contain 3% by mass or less of an organic sulfonate and 1% by mass or less of an inorganic salt.

[0060] In addition, the resin composition for the intermediate layer preferably contains an antiblocking agent and an antioxidant, similar to the resin composition for the seal layer, and may contain other components. Note that the antiblocking agent, antioxidant, and other components are the same as those in the resin composition for the seal layer, and therefore the description thereof will be omitted.

[0061] [Ethylene-unsaturated carboxylic acid ester copolymer] The content of the ethylene-unsaturated carboxylic acid ester copolymer in the resin composition for the intermediate layer is preferably 60% by mass or more, more preferably 65% ​​by mass or more, based on 100% by mass of the resin composition for the seal layer. By having the content of the ethylene-unsaturated carboxylic acid ester copolymer in the resin composition for the intermediate layer be 60% by mass or more, it is possible to exhibit suitable interlayer adhesive strength with the adjacent seal layer and base layer, ensure sealing properties, and exhibit easy peeling properties. In addition, from the viewpoint of easy peeling properties and anti-fogging properties, the content of the ethylene-unsaturated carboxylic acid ester copolymer in the ethylene-based resin composition is preferably 95% by mass or less, more preferably 93% by mass or less.

[0062] The content of the monomer unit derived from ethylene in the ethylene-unsaturated carboxylic acid ester copolymer is preferably 60% by mass or more, more preferably 65% ​​by mass or more, and preferably 80% by mass or less, and more preferably 75% by mass or less. The content of the monomer unit derived from the unsaturated carboxylic acid ester in the ethylene-unsaturated carboxylic acid ester copolymer is preferably 20% by mass or more, more preferably 25% by mass or more, and preferably 40% by mass or less, and more preferably 35% by mass or less. When the content of each monomer unit is within the above range, the compatibility with nonionic surfactants, inorganic salts, and organic sulfonates is increased, and good antifogging properties are obtained.

[0063] (Olefin resin) The olefin resin contained in the resin composition for the intermediate layer may be the olefin resin exemplified in the resin composition for the seal layer, and is preferably an ethylene resin. However, when an ethylene copolymer consisting of one or more vinyl monomer-derived structural units and ethylene-derived structural units is used as the resin composition for the intermediate layer, the content of the ethylene-derived structural components in the ethylene copolymer is preferably 80 to 95% by mass. The laminated film having an intermediate layer has excellent adhesive strength with the adjacent seal layer and base layer, and therefore can improve the appearance after peeling the laminated film from the container.

[0064] The content of the olefin resin in the resin composition for the intermediate layer is preferably 3% by mass or more and 39% by mass or less, with the resin composition being 100% by mass.

[0065] [Resin composition for base layer] The resin composition for the base layer contains an olefin resin. In addition, the resin composition for the base layer preferably contains an antiblocking agent and an antioxidant, similar to the resin composition for the seal layer and the resin composition for the intermediate layer, and may contain other components. Note that the antiblocking agent, the antioxidant, and other components are the same as those in the resin composition for the seal layer and the resin composition for the intermediate layer, and therefore the description thereof will be omitted.

[0066] The olefin resin contained in the resin composition for the base layer may be the olefin resin exemplified in the resin composition for the seal layer described above, and is preferably an ethylene resin. However, when an ethylene copolymer consisting of one or more vinyl monomer-derived structural units and ethylene-derived structural units is used as the resin composition for the base layer, the content of the ethylene-derived structural components in the ethylene copolymer is preferably 80 to 95% by mass. A laminated film having a base layer consisting of such an ethylene copolymer consisting of one or more vinyl monomer-derived structural units and ethylene-derived structural units has excellent adhesive strength between the base layer and the adjacent layer, so that the appearance of the laminated film after peeling it from the container can be improved. In addition, the resin composition for the base layer may contain a polyester resin, a polyamide resin, or the like.

[0067] [Method for producing laminated film] The method for producing the resin composition for the seal layer, the resin composition for the intermediate layer, and the resin composition for the base layer is not particularly limited, and each may be melt-blended (melted and kneaded) separately in advance, or may be dry-blended individually, or may be dry-blended as one or more masterbatches. In dry blending, various blenders such as a Henschel mixer or a tumbler mixer are used, and in melt blending, various mixers such as a single-screw extruder, a twin-screw extruder, a Banbury mixer, or a heat roll are used.

[0068] The method for producing the laminated film is not particularly limited, and any known film production method can be used. The seal layer, intermediate layer, and base layer can be produced by coextrusion inflation molding, coextrusion T-die casting, coextrusion lamination, etc.

[0069] Alternatively, the two layers of the seal layer and the intermediate layer may be laminated by co-extrusion inflation molding, co-extrusion T-die casting, co-extrusion lamination molding, etc., and then the base layer may be laminated on the intermediate layer by extrusion lamination molding or dry lamination molding. When the two layers of the seal layer and the intermediate layer are laminated, the organic sulfonate bleeds from the seal layer to the intermediate layer or from the intermediate layer to the seal layer. It is presumed that this is how the effect of the present invention is achieved.

[0070] The thickness of the laminated film is not particularly limited, but is usually 10 to 100 μm. The thickness of the seal layer is preferably 3 to 70%, more preferably 5 to 50%, of the total thickness of the laminated film. If the thickness of the seal layer is too thin, the seal strength with the container tends to be insufficient when the laminated film is used as a lid material for a container, and if the thickness is too thick, the resin composition constituting the seal layer may stretch when the lid material is peeled off, resulting in a loss of appearance after peeling. The thicknesses of the intermediate layer and the base layer can be appropriately set depending on the application of the lid material to which the laminated film is applied.

[0071] [Lid material] The laminated film according to one embodiment of the present invention can be suitably used as a container lid by laminating a support material on the surface of the substrate layer. The support material may be a preformed film laminated on the substrate layer by dry lamination or the like, or may be laminated on the substrate layer by extrusion lamination. Before laminating the support material, the substrate layer side surface of the laminated film may be subjected to surface treatment such as corona discharge treatment. Furthermore, if necessary, further layers such as a printed layer, a coating layer, a vapor deposition layer, and a transparent protective layer may be laminated on the support material.

[0072] Examples of preformed films used as the support material include resin films such as polyester film, polyamide film, polypropylene film, and ethylene-vinyl alcohol copolymer film, metal foil such as aluminum, and paper. When the support material is an opaque material such as metal foil or paper, it is preferable to form a window portion in at least a part of the support material so that the state of the contents can be visually confirmed from the outside. The window portion can be formed, for example, by cutting out a part of the support material.

[0073] The laminated film according to one embodiment of the present invention has both easy peelability, transparency and anti-fogging properties. Therefore, a lid material including the laminated film can be suitably used as a lid material for a top-sealed packaging container in which it is preferable to visually check the state of the contents from the outside.

[0074] 〔container〕 A top-sealed container comprising the lid material and the container body can be formed by heat-sealing the lid material containing the laminated film according to one embodiment of the present invention to a flange portion of the container body such that the sealing layer of the laminated film abuts against the container body. The container body is preferably made of a polyester resin.

[0075] A container comprising the above-mentioned lid material and container body can be suitably used as a packaging container for storing various products for which it is preferable to visually check the state of the contents, such as foods that contain moisture, such as salads, cut fruit, side dishes, pickles, yogurt, and jelly. EXAMPLES

[0076] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0077] <Masterbatch production> The mixture contained 7% by mass of glycerol monooleate (Rikemal OL-100E, manufactured by Riken Vitamin Co., Ltd.) as a nonionic surfactant, 2.5% by mass of sodium alkylbenzene sulfonate (Elecut S-412-2, manufactured by Takemoto Oil & Fat Co., Ltd., alkyl group having 6 to 22 carbon atoms) as an organic sulfonate, 0.5% by mass of sodium chloride as an inorganic salt, 3% by mass of aluminosilicate (Shilton JC-50, manufactured by Mizusawa Industrial Chemicals Co., Ltd.) as an antiblocking agent, 3% by mass of antioxidant master batch (Sumikathen-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.), and linear low-density polyethylene (Sumikathen-E FV402, manufactured by Sumitomo Chemical Co., Ltd., density 913 kg / m 3 84% by mass of a copolymer of 1,2-difluorophenyl ether (MFR=3.8 g / 10 min) was fed to a Banbury mixer and mixed at 140° C. for 5 minutes, and the resulting mixture was fed to a 65 mmΦ single-screw extruder and pelletized to obtain master batch A.

[0078] The mixture contained 10% by mass of diglycerol stearate (Rikemal S-71-D, manufactured by Riken Vitamin Co., Ltd.) as a nonionic surfactant, 3% by mass of aluminosilicate (Shilton JC-50, manufactured by Mizusawa Industrial Chemicals Co., Ltd.) as an antiblocking agent, 3% by mass of antioxidant masterbatch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.), and linear low-density polyethylene (Sumikathene-E FV402, manufactured by Sumitomo Chemical Co., Ltd. (density 913 kg / m 3 84% by mass of the polymer (MFR=3.8 g / 10 min) was fed to a Banbury mixer and pelletized in the same manner as in the case of Masterbatch A, to obtain Masterbatch B.

[0079] The mixture contained 7.5% by mass of glycerol monooleate (Rikemal OL-100E, manufactured by Riken Vitamin Co., Ltd.) as a nonionic surfactant, 2.5% by mass of sodium alkylbenzene sulfonate (Elecut S-412-2, manufactured by Takemoto Oil & Fat Co., Ltd., alkyl group having 6 to 22 carbon atoms) as an organic sulfonate, 3% by mass of aluminosilicate (Shilton JC-50, manufactured by Mizusawa Industrial Chemicals Co., Ltd.) as an antiblocking agent, 3% by mass of antioxidant master batch (Sumikathen-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.), and linear low-density polyethylene (Sumikathen-E FV402, manufactured by Sumitomo Chemical Co., Ltd., density 913 kg / m 3 The mixture was fed to a 65 mmΦ single-screw extruder and pelletized to obtain Masterbatch C.

[0080] Example 1 A polyester resin composition for the sealing layer was obtained by dry blending 92% by mass of a crystalline polyester (Vylon GM915 (melting point 139°C, glass transition point -70°C) manufactured by Toyobo Co., Ltd.), 5% by mass of Masterbatch A, and 3% by mass of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.).

[0081] Furthermore, 92 mass% of an ethylene-methyl acrylate copolymer (Acryft CG4002 manufactured by Sumitomo Chemical Co., Ltd. (content of monomer units derived from ethylene: 69 mass%, content of monomer units derived from methyl acrylate: 31 mass%, MFR (190°C, 2.16 kgf) = 5 g / 10 min)), 5 mass% of masterbatch B, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.) were dry blended to obtain an ethylene-based resin composition for an intermediate layer.

[0082] In addition, linear low-density polyethylene (Evolue SP4020, manufactured by Prime Polymer Co., Ltd., density 937 kg / m 3An olefin resin composition for the base layer was obtained by dry blending 97% by mass of an olefin copolymer having a molecular weight of 1.2 or more and MFR (190° C., 2.16 kgf)=1.8 g / 10 min) and 3% by mass of an antioxidant masterbatch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.).

[0083] A three-kind three-layer co-extrusion inflation processing machine (extruder A: 50 mmΦ, extruder B: 50 mmΦ, extruder C: 50 mmΦ, layer structure: tubular film outer surface / middle surface / inner surface=extruder A / extruder B / extruder C) was prepared, and a polyester-based resin composition for the seal layer was put into extruder A, an ethylene-based resin composition for the intermediate layer was put into extruder B, and an olefin-based resin composition for the base layer was put into extruder C. Next, molding was performed at extruder A / extruder B / extruder C / die = 170 ° C. / 160 ° C. / 180 ° C. / 180 ° C. to produce a tubular laminated film in which the seal layer / intermediate layer / base layer were laminated in order. The thickness of the seal layer of the obtained laminated film was 4 μm, the thickness of the intermediate layer was 8 μm, the thickness of the base layer was 18 μm, and the total thickness was 30 μm.

[0084] Example 2 A polyester resin composition for the sealing layer was obtained by dry blending 72 mass% of a crystalline polyester (Vylon GM915 manufactured by Toyobo Co., Ltd.), 25 mass% of Masterbatch B, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.).

[0085] In addition, 72% by mass of ethylene-methyl acrylate copolymer (Acryft CG4002, manufactured by Sumitomo Chemical Co., Ltd.), 25% by mass of masterbatch A, and 3% by mass of antioxidant masterbatch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.) were dry blended to obtain an ethylene-based resin composition for the intermediate layer.

[0086] A tubular laminate film having a seal layer / intermediate layer / base material layer laminated in that order was produced in the same manner as in Example 1, except that the polyester-based resin composition for the seal layer obtained above was used as the resin composition constituting the seal layer, and the ethylene-based resin composition for the intermediate layer obtained above was used as the resin composition constituting the intermediate layer.

[0087] Example 3 A polyester resin composition for the sealing layer was obtained by dry blending 72 mass% of a crystalline polyester (Vylon GM915 manufactured by Toyobo Co., Ltd.), 25 mass% of Masterbatch A, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.).

[0088] In addition, 72 mass% of an ethylene-methyl acrylate copolymer (Acryft CG4002, manufactured by Sumitomo Chemical Co., Ltd.), 25 mass% of masterbatch B, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.) were dry-blended to obtain an ethylene-based resin composition for an intermediate layer.

[0089] A tubular laminate film having a seal layer / intermediate layer / base material layer laminated in that order was produced in the same manner as in Example 1, except that the polyester-based resin composition for the seal layer obtained above was used as the resin composition constituting the seal layer, and the ethylene-based resin composition for the intermediate layer obtained above was used as the resin composition constituting the intermediate layer.

[0090] Comparative Example 1 A polyester resin composition for the sealing layer was obtained by dry blending 72 mass% of a crystalline polyester (Vylon GM915 manufactured by Toyobo Co., Ltd.), 25 mass% of Masterbatch B, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.).

[0091] In addition, 72 mass% of an ethylene-methyl acrylate copolymer (Acryft CG4002, manufactured by Sumitomo Chemical Co., Ltd.), 25 mass% of masterbatch B, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.) were dry-blended to obtain an ethylene-based resin composition for an intermediate layer.

[0092] A tubular laminate film having a seal layer / intermediate layer / base material layer laminated in that order was produced in the same manner as in Example 1, except that the polyester-based resin composition for the seal layer obtained above was used as the resin composition constituting the seal layer, and the ethylene-based resin composition for the intermediate layer obtained above was used as the resin composition constituting the intermediate layer.

[0093] Example 4 A polyester resin composition for a sealing layer was obtained by dry blending 67 mass% of a crystalline polyester (Vylon GM915 (melting point 139°C, glass transition point -70°C) manufactured by Toyobo Co., Ltd.), 15 mass% of Masterbatch C, 15 mass% of an antiblocking agent masterbatch (Sumikathene-E EMB-21 manufactured by Sumitomo Chemical Co., Ltd.), and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.).

[0094] Furthermore, 72 mass% of an ethylene-methyl acrylate copolymer (Acryft CG4002 manufactured by Sumitomo Chemical Co., Ltd. (content of monomer units derived from ethylene: 69 mass%, content of monomer units derived from methyl acrylate: 31 mass%, MFR (190°C, 2.16 kgf) = 5 g / 10 min)), 25 mass% of masterbatch B, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.) were dry blended to obtain an ethylene-based resin composition for an intermediate layer.

[0095] Furthermore, linear low-density polyethylene (Sumitomo Chemical Co., Ltd., Sumikasen-E FV202 (density 925 kg / m 397% by mass of an olefin resin composition for use in a substrate layer (MFR (190° C., 2.16 kgf)=1.9 g / 10 min)) and 3% by mass of an antioxidant master batch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.) were dry-blended to obtain an olefin resin composition for use in a substrate layer.

[0096] A three-kind three-layer co-extrusion inflation processing machine (extruder A: 50 mmΦ, extruder B: 50 mmΦ, extruder C: 50 mmΦ, layer structure: tubular film outer surface / middle surface / inner surface=extruder A / extruder B / extruder C) was prepared, and an olefin-based resin composition for the base layer was put into extruder A, an ethylene-based resin composition for the intermediate layer was put into extruder B, and a polyester-based resin composition for the seal layer was put into extruder C. Then, molding was performed at extruder A / extruder B / extruder C / die=180°C / 160°C / 170°C / 180°C to produce a tubular laminated film in which the seal layer / intermediate layer / base layer were laminated in order. The thickness of the seal layer of the obtained laminated film was 4 μm, the thickness of the intermediate layer was 8 μm, the thickness of the base layer was 18 μm, and the total thickness was 30 μm. A 28 W·min / m 2 The corona treatment was carried out under the following conditions.

[0097] Example 5 A polyester resin composition for a sealing layer was obtained by dry blending 67 mass% of a crystalline polyester (Vylon GM915 (melting point 139°C, glass transition point -70°C) manufactured by Toyobo Co., Ltd.), 15 mass% of masterbatch B, 15 mass% of an antiblocking agent masterbatch (Sumikathene-E EMB-21 manufactured by Sumitomo Chemical Co., Ltd.), and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.).

[0098] In addition, 72 mass% of an ethylene-methyl acrylate copolymer (Acryft CG4002, manufactured by Sumitomo Chemical Co., Ltd.), 25 mass% of masterbatch C, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.) were dry-blended to obtain an ethylene-based resin composition for an intermediate layer.

[0099] A tubular laminate film having a sealing layer / intermediate layer / base material layer laminated in that order was produced in the same manner as in Example 4, except that the polyester-based resin composition for the sealing layer obtained above was used as the resin composition constituting the sealing layer, and the ethylene-based resin composition for the intermediate layer obtained above was used as the resin composition constituting the intermediate layer, and corona treatment was performed.

[0100] Comparative Example 2 A polyester resin composition for a sealing layer was obtained by dry blending 67 mass% of a crystalline polyester (Vylon GM915 (melting point 139°C, glass transition point -70°C) manufactured by Toyobo Co., Ltd.), 15 mass% of masterbatch B, 15 mass% of an antiblocking agent masterbatch (Sumikathene-E EMB-21 manufactured by Sumitomo Chemical Co., Ltd.), and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735 manufactured by Sumitomo Chemical Co., Ltd.).

[0101] In addition, 72 mass% of an ethylene-methyl acrylate copolymer (Acryft CG4002, manufactured by Sumitomo Chemical Co., Ltd.), 25 mass% of masterbatch B, and 3 mass% of an antioxidant masterbatch (Sumikathene-E CMB-735, manufactured by Sumitomo Chemical Co., Ltd.) were dry-blended to obtain an ethylene-based resin composition for an intermediate layer.

[0102] A tubular laminate film having a sealing layer / intermediate layer / base material layer laminated in that order was produced in the same manner as in Example 4, except that the polyester-based resin composition for the sealing layer obtained above was used as the resin composition constituting the sealing layer, and the ethylene-based resin composition for the intermediate layer obtained above was used as the resin composition constituting the intermediate layer, and corona treatment was performed.

[0103] <Preparation of Laminate Film for Evaluation 1> Both ends of the tubular laminated film obtained in Examples 1 to 3 and Comparative Example 1 were slit, the tubular laminated film was opened into two pieces, and one of them was wound into a roll so that the seal layer and the base layer were in contact with each other. The obtained rolled sample was conditioned at 35°C for 7 days, and then the surface on the base layer side was subjected to a 93 W·min / m2 After the corona treatment, the condition was further adjusted at 35°C for 7 days. Using a coater manufactured by Yasui Seiki Co., Ltd., an aliphatic ester-based coating agent (main agent: Mitsui Chemicals Co., Ltd.'s "Takelac A-525", hardener: Mitsui Chemicals Co., Ltd.'s "Takenate A-52", and ethyl acetate were mixed thoroughly in a mass ratio of 10:1:15) was applied to a polyester film (manufactured by Unitika Co., Ltd., product name "PTMX", thickness 25 μm, width 330 mm), and pressure-bonded to the corona-treated surface of the laminated film obtained above and conditioned at 35°C for 7 days after the corona treatment, and then heated in an oven at 40°C for 17 hours to obtain a laminate film for evaluation.

[0104] <Preparation of Laminate Film for Evaluation 2> Both ends of the tubular laminated film obtained in Examples 4 and 5 and Comparative Example 2 were slit, the tubular laminated film was opened into two pieces, and one of them was wound into a roll so that the seal layer and the base material layer were in contact with each other. The obtained rolled sample was conditioned for 7 days at 35°C. Using a coater manufactured by Yasui Seiki Co., Ltd., an aliphatic ester-based coating agent (main agent: Mitsui Chemicals Co., Ltd. "Takelac A-525", hardener: Mitsui Chemicals Co., Ltd. "Takenate A-52", and ethyl acetate were mixed thoroughly in a mass ratio of 10:1:15) was applied to a polyester film (manufactured by Unitika Co., Ltd., product name "PTMX", thickness 25 μm, width 330 mm), and pressure-bonded to the corona-treated surface of the laminated film obtained above that had been conditioned for 7 days at 35°C, and then heated in an oven at 40°C for 17 hours to obtain a laminated film for evaluation.

[0105] <Anti-fogging evaluation> A label with two different font sizes, large and small, printed on it was attached to the inside bottom of a cup-shaped polyester resin container body (volume 280 mL, depth 3 cm), and 40 mL of water was filled inside. Double-sided tape was attached to the flange of the upper edge of the cup, and the laminate film for evaluation obtained above was attached so that the surface of the seal layer abutted against the double-sided tape of the flange, and the container was sealed. This container was left in a refrigerator at 5°C for 30 minutes, and then taken out to an environment at 23°C and a relative humidity of 50%, and the adhesion state of water droplets on the inside of the laminate film was observed. The adhesion state of water droplets was evaluated from 5 to 1, with 3 or more being ``passable'' and less than that being ``bad.'' The character strings used for the evaluation were katakana with 2 to 3 strokes, 4 katakana characters in a large font and 10 katakana characters in a small font. The font size of the large font was approximately 15 mm wide by approximately 10 mm high, and the font size of the small font was approximately 5 mm wide by approximately 5 mm high. 5. When water was spread over the film surface, the film had good transparency and all of the katakana characters in both large and small font sizes were clearly readable. 4. All characters in both large and small font sizes were legible, but some of the katakana characters in the small font size were blurred by water droplets. 3. All of the katakana characters in larger font sizes were readable, but some of the katakana characters in smaller font sizes were unreadable due to water droplets. 2. Some of the katakana characters in both large and small font sizes were unreadable due to water droplets. 1. The surface of the film was covered with tiny water droplets, and all of the katakana characters in both large and small font sizes were unreadable due to the water droplets.

[0106] <Transparency> According to JIS K7105:1981, the total light transmittance and diffuse light transmittance of the laminate film for evaluation obtained above were measured, and the haze value ((diffuse light transmittance / total light transmittance)×100) was calculated. A haze value of 20 or less was rated as "passable," and a haze value of more than 20 was rated as "unacceptable."

[0107] <Easy peelability> An amorphous polyester sheet (thickness 200 μm) cut into a size of 90 mm length × 100 mm width was prepared as an adherend. The adherend and the seal layer of the laminate film for evaluation obtained above were brought into contact with each other, and a pressure of 3 kg / cm was applied. 2 The composite sheet was obtained by heat sealing the adhesive at 200°C for 1 second into a 10 mm wide strip parallel to the length of the adherend. The composite sheet obtained was cut into 15 mm wide intervals perpendicular to the strip-shaped sealed portion so as to include the sealed portion, to prepare a 15 mm x 100 mm test piece. The peel strength was measured using a Shimadzu Corporation autograph AGS-X tensile tester when peeled at 180 degrees at a tensile speed of 300 mm / min in an atmosphere of 23°C. If the peel strength is 5 to 15 N / 15 mm width, it can be said that the balance between the ease of peeling and the seal strength with the container body is excellent. Therefore, peel strengths within the range of 5 to 15 N / 15 mm width were evaluated as "passable", and those outside the range of 5 to 15 N / 15 mm width were evaluated as "unacceptable".

[0108] [Table 1]

[0109] The laminate films including the laminate films of Examples 1 to 5 had excellent anti-fogging properties in addition to good peelability and transparency. In contrast, the laminate films including the laminate films of Comparative Examples 1 and 2 had poor anti-fogging properties, and the inside of the container could not be clearly seen due to the adhesion of water droplets. [Industrial Applicability]

[0110] The laminate film according to one embodiment of the present invention has easy peelability, transparency and anti-fogging properties, and is suitably used as a sealant for lids of packaging containers for storing various foods and the like.

Claims

1. A laminated film comprising a seal layer, an intermediate layer, and a base layer laminated in this order, The sealing layer contains a polyester resin and a nonionic surfactant, the intermediate layer contains an ethylene-unsaturated carboxylic acid ester copolymer and a nonionic surfactant; The substrate layer contains an olefin-based resin, At least one of the sealing layer and the intermediate layer further comprises an organic sulfonate.

2. 10. The laminate film of claim 1, wherein at least one of the sealing layer and the intermediate layer further comprises an inorganic salt.

3. 3. The laminate film according to claim 1, wherein one of the seal layer and the intermediate layer has a content of the organic sulfonate of 0.05% by mass or more, and the other layer has a content of the organic sulfonate of less than 0.05% by mass.

4. 3. The laminate film according to claim 2, wherein one of the seal layer and the intermediate layer has a content of the organic sulfonate of 0.05% by mass or more and a content of the inorganic salt of 0.01% by mass or more, and the other layer has a content of the organic sulfonate of less than 0.05% by mass and a content of the inorganic salt of less than 0.01% by mass.

5. The laminate film according to any one of claims 1 to 4, wherein the intermediate layer contains the organic sulfonate.

6. The organic sulfonate is at least one selected from the group consisting of an alkylsulfonic acid alkali metal salt, an alkylarylsulfonic acid alkali metal salt, and an aliphatic sulfonic acid ester alkali metal salt. The laminate film according to any one of claims 1 to 5.

7. 5. The laminated film according to claim 2, wherein the inorganic salt is at least one selected from the group consisting of sodium sulfate, potassium sulfate, calcium sulfate, lithium sulfate, sodium chloride, potassium chloride, lithium chloride, magnesium chloride and calcium chloride.

8. 8. The laminate film according to claim 1, wherein the nonionic surfactant is a partial ester of a trihydric to hexahydric polyol and an aliphatic carboxylic acid.

9. The sealing layer has a polyester resin content of 60 to 95% by mass and a nonionic surfactant content of 0.05 to 5.0% by mass. The laminate film according to any one of claims 1 to 8.

10. The intermediate layer has a content of the ethylene-unsaturated carboxylic acid ester copolymer of 60 to 95% by mass and a content of the nonionic surfactant of 0.05 to 5.0% by mass. The laminate film according to any one of claims 1 to 9.

11. The ethylene-unsaturated carboxylic acid ester copolymer contains 60 to 80 mass% of a monomer unit derived from ethylene and 20 to 40 mass% of a monomer unit derived from an unsaturated carboxylic acid ester. The laminate film according to any one of claims 1 to 10.

12. The laminate film according to any one of claims 1 to 11, wherein the polyester resin is a crystalline polyester.

13. The laminate film according to any one of claims 1 to 12, wherein the sealing layer and the intermediate layer further contain an olefin-based resin.

14. The laminate film according to any one of claims 1 to 13, wherein the sealing layer and the intermediate layer further contain an antiblocking agent.

15. The laminate film according to any one of claims 1 to 14, wherein the sealing layer, the intermediate layer and the base layer further contain an antioxidant.

16. A covering material comprising the laminate film according to any one of claims 1 to 15.

17. A container comprising a lid material comprising the laminate film according to any one of claims 1 to 15.

Citation Information

Patent Citations

  • Multilayred film for agriculture

    JP1997183193A

  • Anti-clouding multilayer sealable polyester film and gas-pack package including the same

    JP2004025825A

  • Manufacturing method of thermoplastic resin laminated film and thermoplastic resin laminated film

    JP2005186320A

  • Aqueous surface treatment agent, coating sheet and coating property improvement method

    JP2016094553A

  • Sealant film and packaging material

    JP2019171792A