CURABLE RESIN COMPOSITION, CURED PRODUCT, AND ELECTRONIC COMPONENT

The curable resin composition addresses the issues of adhesive strength and impact resistance in bonding small electronic components by achieving a storage modulus of 10 MPa and elongation at break of 700% or more, effectively preventing peeling and shock propagation.

JP7557461B2Active Publication Date: 2024-09-27SEKISUI CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021522888
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-30
Filing Date
2020-05-28
Publication Date
2024-09-27
Estimated Expiration
2040-05-28

AI Technical Summary

Technical Problem

Existing moisture-curable resin compositions used for bonding small electronic components and designing narrow frames lack sufficient adhesive strength and impact resistance, leading to potential peeling and propagation of shocks to the components.

Method used

A curable resin composition is formulated with a moisture-curable resin having a storage modulus of 10 MPa or more and elongation at break of 700% or more, incorporating a crosslinking agent, photopolymerizable compound, and photopolymerization initiator to enhance adhesive strength and impact resistance.

Benefits of technology

The composition provides high adhesive strength and impact resistance, preventing peeling and shock propagation in electronic components, even with small bonding areas, by ensuring a balanced storage modulus and elongation at break.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557461000004
    Figure 0007557461000004
  • Figure 0007557461000005
    Figure 0007557461000005
  • Figure 0007557461000003
    Figure 0007557461000003
Patent Text Reader

Abstract

The curable resin composition of the present invention includes a moisture-curable resin (A) and gives cured objects having a 25°C storage modulus of 10 MPa or greater and a 25°C elongation at break of 700% or greater.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition, a cured product of the curable resin composition, and an electronic component including the cured product of the curable resin composition. [Background technology]

[0002] In recent years, there has been a demand for higher integration and miniaturization of electronic components such as semiconductor chips. For example, a stack of semiconductor chips may be formed by bonding multiple thin semiconductor chips via an adhesive layer. In addition, in today's world where mobile devices with various display elements are widespread, a method of miniaturizing display elements is to narrow the frame of the image display section (hereinafter, also referred to as "narrow frame design"). In narrow frame design, a technology is required for bonding with an adhesive with a narrow line width using a dispenser or the like.

[0003] In general, high adhesive strength is required for the adhesion of these small electronic components and in narrow frame designs, and therefore the use of moisture-curing adhesives has been considered. For example, Patent Document 1 discloses a moisture-curing polyurethane hot melt resin composition containing a urethane prepolymer having an isocyanate group, an acrylic polymer, a thermoplastic resin having a softening point in the range of 50 to 80°C, and a curing catalyst, as a moisture-curing adhesive with improved adhesive strength. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-113552 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the bonding of small electronic components and in narrow frame designs, in addition to high adhesive strength, high impact absorption is also required to prevent impact from being transmitted to the electronic components. However, the moisture-curable resin composition disclosed in Patent Document 1 does not have sufficient adhesive strength or impact resistance, and further improvement is desired. Therefore, an object of the present invention is to provide a curable resin composition having good adhesive strength and impact resistance. [Means for solving the problem]

[0006] As a result of intensive research, the present inventors have found that the above problems can be solved by setting both the storage modulus at 25°C and the breaking elongation of the cured product at or above a predetermined value in a curable resin composition containing a moisture-curable resin, and have completed the present invention as described below. That is, the present invention provides the following (1) to (13). (1) A curable resin composition comprising a moisture-curable resin (A), A curable resin composition, wherein a cured product of the curable resin composition has a storage modulus at 25°C of 10 MPa or more and a breaking elongation at 25°C of 700% or more. (2) The curable resin composition according to (1) above, further comprising a crosslinking agent (X), the content of the crosslinking agent (X) being 0.4 mass% or more and 10 mass% or less based on the total amount of the curable resin composition. (3) The curable resin composition according to the above (2), wherein the crosslinking agent (X) is a compound having an isocyanate group. (4) The curable resin composition according to any one of the above (1) to (3), further comprising a photopolymerizable compound (B) and a photopolymerization initiator (Y). (5) The curable resin composition according to (4) above, wherein the photopolymerizable compound (B) contains a compound (B1) having a glass transition temperature (Tg) of 70° C. or higher when made into a homopolymer. (6) The curable resin composition according to the above (5), wherein the content of the compound (B1) is 10% by mass or more and 50% by mass or less based on the total amount of the photopolymerizable compound (B). (7) The curable resin composition according to (5) or (6) above, wherein the content of the compound (B1) is 2.5 mass % or more and 15 mass % or less based on the total amount of the curable resin composition. (8) The curable resin composition according to any one of the above (4) to (7), wherein the photopolymerizable compound (B) contains an alicyclic structure-containing (meth)acrylic compound. (9) The curable resin composition according to any one of the above (4) to (8), wherein the photopolymerizable compound (B) contains a compound (B2) having a glass transition temperature (Tg) of less than 70° C. when made into a homopolymer. (10) The curable resin composition according to any one of the above (1) to (9), wherein the moisture-curable resin (A) is a moisture-curable urethane resin. (11) The curable resin composition according to any one of (1) to (10), wherein the content of the moisture-curable resin (A) is 50 mass % or more and 80 mass % or less based on the total amount of the curable resin composition. (12) A cured product of the curable resin composition according to any one of (1) to (11) above. (13) An electronic component comprising the cured body according to (12) above. Effect of the Invention

[0007] According to the present invention, it is possible to provide a curable resin composition having good adhesive strength and impact resistance. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic diagram for explaining a method for measuring a PUSH adhesive force. [Diagram 2] FIG. 2 is a schematic diagram for explaining a method for evaluating impact resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below. [Curable resin composition] The curable resin composition of the present invention is a curable resin composition containing a moisture-curable resin, and a cured product of the curable resin composition has a storage modulus of 10 MPa or more at 25°C and a breaking elongation of 700% or more at 25°C. The curable resin composition of the present invention has high adhesive strength, particularly high PUSH adhesive strength, and excellent impact resistance, because the cured product has high storage modulus and high breaking elongation as described above. Therefore, when an adherend is bonded with the curable resin composition of the present invention, even if the adhesion area is small or the application width is small, the adherend can be prevented from peeling off when a strong impact is applied, and the impact can also be prevented from being transmitted to electronic components.

[0010] On the other hand, if the storage modulus of the curable resin composition at 25°C of the cured product is less than 10 MPa or the breaking elongation at 25°C is less than 700%, it becomes difficult to achieve excellent adhesion performance and impact resistance, and the application of impact may cause the adherend to peel off or the impact to be transmitted to the electronic component. From the viewpoint of stably achieving both excellent adhesive performance and impact resistance, the storage modulus of the cured product at 25° C. is preferably 16 MPa or more, more preferably 20 MPa or more. In addition, from the viewpoint of easily ensuring high breaking elongation, the storage modulus at 25° C. is, for example, 75 MPa or less, preferably 45 MPa or less, and from the viewpoint of further increasing adhesive strength, more preferably 32 MPa or less. From the viewpoint of stably achieving both excellent adhesion and impact resistance, the breaking elongation is preferably 750% or more, more preferably 800% or more, and even more preferably 850% or more. From the viewpoint of easily ensuring a high storage modulus of the cured body, the breaking elongation is, for example, 1500% or less, and preferably 1000% or less.

[0011] In the present invention, the storage modulus of the cured product is measured by the following method. The curable resin composition is poured into a Teflon (registered trademark) mold with a width of 3 mm, a length of 30 mm, and a thickness of 1 mm, and cured to obtain a cured sample. The obtained cured sample is used to measure the dynamic viscoelasticity in the range of 40 to 150°C using a dynamic viscoelasticity measuring device, and the storage modulus at 25°C is obtained. The measurement conditions are a tensile deformation mode, a set strain of 1%, a measurement frequency of 1 Hz, and a heating rate of 5°C / min.

[0012] The breaking elongation of the cured product is measured by the following method. The curable resin composition is poured into a silicone rubber mold with a dumbbell-shaped hole (type 6 specified in "JIS K6251") and cured to obtain a dumbbell-shaped test piece of type 6. The breaking elongation of the obtained test piece is measured at 25°C by pulling at a pulling speed of 50 mm / min using a tensile tester.

[0013] The curing of the curable resin composition to obtain a cured sample may be performed as long as the curable resin composition is completely cured, and may be performed according to the curing mechanism as follows. For example, in the case of photo-moisture curing, a UV-LED (wavelength 365 nm) is used to irradiate ultraviolet light at 1000 mJ / cm. 2 The resin is then exposed to light to cause photocuring, and then left for 24 hours in an environment of 23°C and 50% RH to cause moisture curing. In the case of moisture curing, the same procedure as above is followed except that the photocuring step is omitted. In the case of a heat-curable and moisture-curable resin composition, the composition is heated at 90°C for 2 hours, and then left in an environment of 23°C and 50% RH for 24 hours to be moisture-cured. In the case of a light-, heat-, and moisture-curable resin composition, the composition is irradiated with ultraviolet light at 1000 mJ / cm using a UV-LED (wavelength 365 nm). 2 It is preferable to carry out the process by irradiating the resin to cause it to be photo-cured, then heating at 90° C. for 2 hours to cause it to be thermally cured, and then leaving it in an environment of 23° C. and 50% RH for 24 hours to cause it to be moisture-cured.

[0014] As described above, the curable resin composition of the present invention has at least the moisture-curable resin (A) and is a moisture-curable resin composition. When the curable resin composition is moisture-curable, it is easy to increase the adhesive strength. In addition to the moisture-curable resin (A), the curable resin composition of the present invention preferably contains at least one of a photopolymerizable compound (B) (photocurable resin) that is cured by irradiation with light and a thermosetting resin (C) that is cured by heating.

[0015] Here, when the curable resin composition further contains a photopolymerizable compound (B) in addition to the moisture-curable resin (A), it becomes a photo-moisture-curable resin composition that is cured by light irradiation and moisture. When the curable resin composition further contains a thermosetting resin (C) in addition to the moisture-curable resin (A), it becomes a heat-moisture-curable resin composition that is cured by heating and moisture. Furthermore, when the curable resin composition contains a photopolymerizable compound (B) and a thermosetting resin (C) in addition to the moisture-curable resin (A), it becomes a light-, heat-, and moisture-curable resin composition that is cured by light irradiation, heating, and moisture.

[0016] The curable resin composition preferably contains a moisture-curable resin (A) and a photopolymerizable compound (B). That is, the curable resin composition is preferably a photo-moisture-curable resin composition. The photo-moisture-curable resin composition has excellent adhesive performance even when cured without heating, so that when the curable resin composition is cured, the adhesive portion or electronic components around the adhesive portion can be prevented from being damaged by heating, and the adhesive performance can be excellent. For example, a photo-curable resin composition can be first photo-cured to give it a B-stage state with relatively low adhesive strength (tackiness), and then left in the air or the like to cure with moisture, making it possible to produce a cured product with sufficiently high adhesive strength. Hereinafter, when the curable resin composition of the present invention is a photo-moisture-curable resin composition containing a moisture-curable resin (A) and a photopolymerizable compound (B), each component will be described in detail.

[0017] (Moisture curing resin (A)) Examples of the moisture-curable resin (A) used in the present invention include moisture-curable urethane resin, hydrolyzable silyl group-containing resin, and moisture-curable cyanoacrylate resin. Among these, moisture-curable urethane resin and hydrolyzable silyl group-containing resin are preferred, and moisture-curable urethane resin is more preferred. By using a moisture-curable urethane resin, the breaking elongation of the cured body is improved, and the adhesive strength is easily increased. In addition, when used in combination with a high Tg compound (B1) or a crosslinking agent (X) described later, the adhesive performance is further improved.

[0018] The moisture-curing urethane resin has an isocyanate group. The moisture-curing urethane resin cures when the isocyanate group in the molecule reacts with moisture in the air or the adherend. The moisture-curing urethane resin may have only one isocyanate group in one molecule, or may have two or more isocyanate groups. In particular, it is preferable that the molecule has an isocyanate group at both ends of the main chain.

[0019] The moisture-curable urethane resin can be obtained by reacting a polyol compound having two or more hydroxyl groups in one molecule with a polyisocyanate compound having two or more isocyanate groups in one molecule. The reaction between the polyol compound and the polyisocyanate compound is usually carried out in a molar ratio of hydroxyl groups (OH) in the polyol compound to isocyanate groups (NCO) in the polyisocyanate compound, [NCO] / [OH], within the range of 2.0 to 2.5.

[0020] As the polyol compound serving as the raw material of the moisture-curable urethane resin, a known polyol compound usually used in the production of polyurethane can be used, such as polyester polyol, polyether polyol, polyalkylene polyol, polycarbonate polyol, etc. These polyol compounds may be used alone or in combination of two or more. Examples of the polyester polyol include polyester polyol obtained by reacting a polyvalent carboxylic acid with a polyol, and poly-ε-caprolactone polyol obtained by ring-opening polymerization of ε-caprolactone. Examples of the polyvalent carboxylic acid that is used as a raw material for the polyester polyol include terephthalic acid, isophthalic acid, 1,5-naphthalic acid, 2,6-naphthalic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decamethylene dicarboxylic acid, and dodecamethylene dicarboxylic acid. Examples of polyols that can be used as raw materials for polyester polyols include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, and cyclohexanediol.

[0021] Examples of polyether polyols include ethylene glycol, propylene glycol, ring-opening polymers of tetrahydrofuran, ring-opening polymers of 3-methyltetrahydrofuran, and random or block copolymers of these or their derivatives, and bisphenol-type polyoxyalkylene modified products. Here, the bisphenol-type polyoxyalkylene modified product is a polyether polyol obtained by addition reaction of an alkylene oxide (e.g., ethylene oxide, propylene oxide, butylene oxide, isobutylene oxide, etc.) with the active hydrogen portion of a bisphenol-type molecular skeleton. The polyether polyol may be a random copolymer or a block copolymer. The bisphenol-type polyoxyalkylene modified product preferably has one or more alkylene oxides added to both ends of the bisphenol-type molecular skeleton. The bisphenol type is not particularly limited, and examples thereof include A-type, F-type, S-type, etc., with bisphenol A-type being preferred.

[0022] Examples of polyalkylene polyols include polybutadiene polyols, hydrogenated polybutadiene polyols, and hydrogenated polyisoprene polyols. Examples of the polycarbonate polyol include polyhexamethylene carbonate polyol and polycyclohexane dimethylene carbonate polyol.

[0023] As the polyisocyanate compound serving as the raw material of the moisture-curable urethane resin, an aromatic polyisocyanate compound or an aliphatic polyisocyanate compound is preferably used. Examples of aromatic polyisocyanate compounds include diphenylmethane diisocyanate, liquid modified products of diphenylmethane diisocyanate, polymeric MDI, tolylene diisocyanate, and naphthalene-1,5-diisocyanate. Examples of the aliphatic polyisocyanate compound include hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, norbornane diisocyanate, transcyclohexane-1,4-diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated diphenylmethane diisocyanate, cyclohexane diisocyanate, bis(isocyanatemethyl)cyclohexane, and dicyclohexylmethane diisocyanate. Of these, the polyisocyanate compound is preferably diphenylmethane diisocyanate or a modified product thereof, from the viewpoint of increasing the adhesive strength after full curing. The polyisocyanate compounds may be used alone or in combination of two or more kinds.

[0024] The moisture-curable urethane resin is preferably obtained by using a polyol compound having a structure represented by the following formula (1). By using a polyol compound having a structure represented by the following formula (1), a curable resin composition having excellent adhesiveness and a cured product having flexibility, good elongation, and high elongation at break can be obtained, and the compatibility with the photopolymerizable compound (B) is excellent. In addition, the storage modulus can be easily adjusted to within the desired range. Among them, polyether polyols made of propylene glycol, ring-opening polymerized compounds of tetrahydrofuran (THF) compounds, or ring-opening polymerized compounds of tetrahydrofuran compounds having a substituent such as a methyl group are preferred. Ring-opening polymerized compounds of tetrahydrofuran compounds are more preferred, and polytetramethylene ether glycol is particularly preferred.

[0025] [ka] In formula (1), R represents a hydrogen atom, a methyl group, or an ethyl group, l is an integer of 0 to 5, m is an integer of 1 to 500, and n is an integer of 1 to 10. l is preferably 0 to 4, m is preferably 50 to 200, and n is preferably 1 to 5. When l is 0, it means that the carbon bonded to R is directly bonded to oxygen. Among the above, the sum of n and l is more preferably 1 or more, and further preferably 3 to 6. Furthermore, R is more preferably a hydrogen atom or a methyl group, and particularly preferably a hydrogen atom.

[0026] The hydrolyzable silyl group-containing resin used in the present invention is cured when the hydrolyzable silyl group in the molecule reacts with moisture in the air or on the adherend. The hydrolyzable silyl group-containing resin may have only one hydrolyzable silyl group in one molecule, or may have two or more hydrolyzable silyl groups in one molecule. In particular, it is preferable that the resin has hydrolyzable silyl groups at both ends of the main chain of the molecule. The hydrolyzable silyl group-containing resin does not include those having an isocyanate group.

[0027] The hydrolyzable silyl group is represented by the following formula (2). [ka] In formula (2), R 1 each independently represents an optionally substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, or -OSiR 2 3(R 2 are each independently a hydrocarbon group having 1 to 20 carbon atoms. In formula (2), X is each independently a hydroxyl group or a hydrolyzable group. In formula (2), a is an integer of 1 to 3.

[0028] The hydrolyzable group is not particularly limited, and examples thereof include halogen atoms, alkoxy groups, alkenyloxy groups, aryloxy groups, acyloxy groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, and mercapto groups. Among these, halogen atoms, alkoxy groups, alkenyloxy groups, and acyloxy groups are preferred because of their high activity. In addition, alkoxy groups such as methoxy groups and ethoxy groups are more preferred because of their mild hydrolysis and ease of handling, and methoxy groups and ethoxy groups are even more preferred. In addition, from the viewpoint of safety, ethoxy groups and isopropenoxy groups are preferred because the compounds that are eliminated by the reaction are ethanol and acetone, respectively.

[0029] The number of the hydroxyl groups or hydrolyzable groups bonded to one silicon atom may be in the range of 1 to 3. When two or more hydroxyl groups or hydrolyzable groups are bonded to one silicon atom, those groups may be the same or different.

[0030] In the above formula (2), from the viewpoint of curability, a is preferably 2 or 3, and particularly preferably 3. Furthermore, from the viewpoint of storage stability, a is preferably 2. In addition, R in the above formula (2) 1 Examples of the alkyl group include alkyl groups such as a methyl group and an ethyl group, cycloalkyl groups such as a cyclohexyl group, aryl groups such as a phenyl group, aralkyl groups such as a benzyl group, a trimethylsiloxy group, a chloromethyl group, a methoxymethyl group, etc. Of these, a methyl group is preferred.

[0031] Examples of the hydrolyzable silyl group include a methyldimethoxysilyl group, a trimethoxysilyl group, a triethoxysilyl group, a tris(2-propenyloxy)silyl group, a triacetoxysilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl)diethoxysilyl group, a (dichloromethyl)dimethoxysilyl group, a (1-chloroethyl)dimethoxysilyl group, a (1-chloropropyl)dimethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)diethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (chloro ...chloromethyl)dimethoxysilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl) Examples of such silyl groups include an (ethoxymethyl)dimethoxysilyl group, a (1-methoxyethyl)dimethoxysilyl group, an (aminomethyl)dimethoxysilyl group, an (N,N-dimethylaminomethyl)dimethoxysilyl group, an (N,N-diethylaminomethyl)dimethoxysilyl group, an (N,N-diethylaminomethyl)diethoxysilyl group, an (N-(2-aminoethyl)aminomethyl)dimethoxysilyl group, an (acetoxymethyl)dimethoxysilyl group, and an (acetoxymethyl)diethoxysilyl group.

[0032] Examples of the hydrolyzable silyl group-containing resin include hydrolyzable silyl group-containing (meth)acrylic resins, organic polymers having a hydrolyzable silyl group at the molecular chain terminal or at the molecular chain terminal site, and hydrolyzable silyl group-containing polyurethane resins. The hydrolyzable silyl group-containing (meth)acrylic resin preferably has repeating units derived from a hydrolyzable silyl group-containing (meth)acrylic acid ester and / or a (meth)acrylic acid alkyl ester in the main chain.

[0033] Examples of hydrolyzable silyl group-containing (meth)acrylic acid esters include 3-(trimethoxysilyl)propyl (meth)acrylate, 3-(triethoxysilyl)propyl (meth)acrylate, 3-(methyldimethoxysilyl)propyl (meth)acrylate, 2-(trimethoxysilyl)ethyl (meth)acrylate, 2-(triethoxysilyl)ethyl (meth)acrylate, 2-(methyldimethoxysilyl)ethyl (meth)acrylate, trimethoxysilylmethyl (meth)acrylate, triethoxysilylmethyl (meth)acrylate, and (methyldimethoxysilyl)methyl (meth)acrylate. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, and stearyl (meth)acrylate.

[0034] Specific examples of methods for producing hydrolyzable silyl group-containing (meth)acrylic resins include the method for synthesizing hydrolyzable silicon group-containing (meth)acrylic acid ester polymers described in WO 2016 / 035718. The organic polymer having a hydrolyzable silyl group at or in a molecular chain terminal portion has a hydrolyzable silyl group at or in at least one of the main chain terminal and the side chain terminal. The skeleton structure of the main chain is not particularly limited, and examples thereof include saturated hydrocarbon polymers, polyoxyalkylene polymers, and (meth)acrylic acid ester polymers.

[0035] Examples of the polyoxyalkylene polymer include polymers having a polyoxyethylene structure, a polyoxypropylene structure, a polyoxybutylene structure, a polyoxytetramethylene structure, a polyoxyethylene-polyoxypropylene copolymer structure, and a polyoxypropylene-polyoxybutylene copolymer structure. Specific examples of the method for producing an organic polymer having a hydrolyzable silyl group at the molecular chain end or at a molecular chain end include a method for synthesizing an organic polymer having a crosslinkable silyl group only at the molecular chain end or at a molecular chain end, as described in WO 2016 / 035718. Other examples of the method for producing an organic polymer having a hydrolyzable silyl group at the molecular chain end or at a molecular chain end include a method for synthesizing a reactive silicon group-containing polyoxyalkylene polymer, as described in WO 2012 / 117902.

[0036] Examples of the method for producing the hydrolyzable silyl group-containing polyurethane resin include a method in which a polyol compound and a polyisocyanate compound are reacted with each other to produce a polyurethane resin, and then a silyl group-containing compound such as a silane coupling agent is reacted with the polyurethane resin.Specific examples of the method include the method for synthesizing a urethane oligomer having a hydrolyzable silyl group described in JP 2017-48345 A.

[0037] Examples of the silane coupling agent include vinyltrichlorosilane, vinyltriethoxysilane, vinyltris(β-methoxy-ethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, 3-isocyanatepropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane. Among these, γ-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane are preferred. These silane coupling agents may be used alone or in combination of two or more.

[0038] The moisture-curable urethane resin may have both an isocyanate group and a hydrolyzable silyl group. The moisture-curable urethane resin having both an isocyanate group and a hydrolyzable silyl group is preferably produced by first obtaining a moisture-curable urethane resin having an isocyanate group by the above-mentioned method, and then reacting the moisture-curable urethane resin with a silane coupling agent. The details of the moisture-curable urethane resin having an isocyanate group are as described above. The silane coupling agent to be reacted with moisture curing may be appropriately selected from those listed above, but it is preferable to use a silane coupling agent having an amino group or a mercapto group from the viewpoint of reactivity with the isocyanate group. Preferred specific examples include N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, and 3-isocyanatepropyltrimethoxysilane.

[0039] Furthermore, the moisture-curable resin (A) may have a radically polymerizable functional group. As the radically polymerizable functional group that the moisture-curable resin (A) may have, a group having an unsaturated double bond is preferable, and in particular, from the viewpoint of reactivity, a (meth)acryloyl group is more preferable. Note that the moisture-curable resin having a radically polymerizable functional group is not included in the photopolymerizable compound (B) described later, and is treated as a moisture-curable resin. The moisture-curable resin (A) may be appropriately selected from the various resins described above and used alone or in combination of two or more kinds.

[0040] The weight average molecular weight of the moisture-curable resin (A) is not particularly limited, but the preferred lower limit is 800, and the preferred upper limit is 10000. When the weight average molecular weight is within this range, the storage modulus of the cured product can be easily adjusted within the above range. In addition, when the obtained curable resin composition is fully cured, the crosslink density is not too high and the flexibility is excellent, and the breaking strength can be easily adjusted within the above range. The weight average molecular weight of the moisture-curable resin (A) is more preferably 2000 in lower limit, 8000 in upper limit, 2500 in lower limit, and 6000 in upper limit. In this specification, the weight average molecular weight is a value obtained by measuring by gel permeation chromatography (GPC) and converting into polystyrene. Shodex LF-804 (Showa Denko KK) is an example of a column used for measuring the weight average molecular weight converted into polystyrene by GPC. Tetrahydrofuran is an example of a solvent used in GPC.

[0041] The content of the moisture-curable resin (A) in the curable resin composition is preferably 50% by mass or more based on the total amount of the curable resin composition. When the content of the moisture-curable resin (A) is as high as 50% by mass or more, the breaking elongation is increased, and the adhesive performance, particularly the PUSH adhesive strength, is easily improved. From the viewpoint of improving adhesive performance, the content of the moisture-curable resin (A) is preferably 54% by mass or more, more preferably 56% by mass or more, based on the total amount of the curable resin composition. The content of the moisture-curable resin (A) is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less, in order to contain a certain amount of the photopolymerizable compound (B) and the crosslinking agent (X) described later. The total amount of the curable resin composition is based on the total amount of solids contained in the curable resin composition. For example, when the curable resin composition contains a solvent to dilute the composition, the total amount of the curable resin composition is the amount of the components excluding the solvent.

[0042] (Photopolymerizable compound (B)) The photopolymerizable compound (B) is not particularly limited as long as it is a radically polymerizable compound having a radically polymerizable functional group in the molecule. The photopolymerizable compound (B) is preferably a compound having an unsaturated double bond as a radically polymerizable functional group, and is particularly preferably a compound having a (meth)acryloyl group (hereinafter also referred to as "(meth)acrylic compound"). In the present invention, by using a (meth)acrylic compound, the storage modulus and breaking elongation described above can be easily adjusted to a predetermined range.

[0043] Examples of the (meth)acrylic compound include (meth)acrylic acid ester compounds, epoxy (meth)acrylates, and urethane (meth)acrylates. Among these, (meth)acrylic acid ester compounds are preferred. The urethane (meth)acrylates do not have residual isocyanate groups. In this specification, the term "(meth)acryloyl group" means an acryloyl group or a (meth)acryloyl group, and the term "(meth)acrylate" means an acrylate or a methacrylate, and similar terms are used herein.

[0044] The (meth)acrylic acid ester compound may be monofunctional, bifunctional, or trifunctional or higher, but is preferably monofunctional. Examples of monofunctional (meth)acrylic acid ester compounds include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2- Alkyl (meth)acrylates such as ethylhexyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, myristyl (meth)acrylate, isomyristyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, 3,3,Alicyclic (meth)acrylates such as 5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and 1-adamantyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, and 2-butoxyethyl (meth)acrylate; Examples of the alkoxyethylene glycol (meth)acrylates include alkoxyethylene glycol (meth)acrylates such as alkoxyethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, ethyl carbitol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, ethoxytriethylene glycol (meth)acrylate, and ethoxypolyethylene glycol (meth)acrylate.

[0045] The (meth)acrylic acid ester compound may have an aromatic ring, and examples thereof include phenylalkyl (meth)acrylates such as benzyl (meth)acrylate and 2-phenylethyl (meth)acrylate, and phenoxyalkyl (meth)acrylates such as phenoxyethyl (meth)acrylate, etc. Furthermore, the compound may be a (meth)acrylate having a plurality of benzene rings such as a fluorene skeleton or a biphenyl skeleton, and specific examples thereof include fluorene type (meth)acrylate, ethoxylated o-phenylphenol acrylate, etc. Further examples include phenoxypolyoxyethylene (meth)acrylates such as phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, nonylphenoxydiethylene glycol (meth)acrylate, and nonylphenoxypolyethylene glycol (meth)acrylate.

[0046] Further, examples of the monofunctional (meth)acrylic acid ester compound include (meth)acrylates having a heterocyclic structure such as tetrahydrofurfuryl (meth)acrylate, alkoxylated tetrahydrofurfuryl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, 3-ethyl-3-oxetanylmethyl (meth)acrylate, and the like, phthalimide acrylates such as N-acryloyloxyethylhexahydrophthalimide, various imide (meth)acrylates, 2,2,2-trifluoroethyl (meth)acrylate, and the like. acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H,1H,5H-octafluoropentyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, glycidyl (meth)acrylate, 2-(meth)acryloyloxyethyl phosphate, and the like.

[0047] Examples of the bifunctional (meth)acrylic acid ester compounds include 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and the like. meth)acrylate, ethylene oxide-added bisphenol A di(meth)acrylate, propylene oxide-added bisphenol A di(meth)acrylate, ethylene oxide-added bisphenol F di(meth)acrylate, dimethylol dicyclopentadienyl di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide-modified isocyanuric acid di(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, carbonate diol di(meth)acrylate, polyether diol di(meth)acrylate, polyester diol di(meth)acrylate, polycaprolactone diol di(meth)acrylate, polybutadiene diol di(meth)acrylate, and the like.

[0048] Examples of the (meth)acrylic acid ester compounds having three or more functional groups include trimethylolpropane tri(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, propylene oxide-added trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ethylene oxide-added isocyanuric acid tri(meth)acrylate, glycerin tri(meth)acrylate, propylene oxide-added glycerin tri(meth)acrylate, tris(meth)acryloyloxyethyl phosphate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0049] The epoxy (meth)acrylate may be, for example, a product of reaction between an epoxy compound and (meth)acrylic acid. The reaction between the epoxy compound and (meth)acrylic acid may be carried out in the presence of a basic catalyst according to a conventional method. The epoxy (meth)acrylate may be monofunctional or multifunctional such as bifunctional. Examples of epoxy compounds that serve as raw materials for synthesizing the above-mentioned epoxy (meth)acrylates include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, 2,2'-diallyl bisphenol A type epoxy resins, hydrogenated bisphenol type epoxy resins, propylene oxide-added bisphenol A type epoxy resins, resorcinol type epoxy resins, biphenyl type epoxy resins, sulfide type epoxy resins, diphenyl ether type epoxy resins, dicyclopentadiene type epoxy resins, naphthalene type epoxy resins, phenol novolac type epoxy resins, ortho-cresol novolac type epoxy resins, dicyclopentadiene novolac type epoxy resins, biphenyl novolac type epoxy resins, naphthalene phenol novolac type epoxy resins, glycidyl amine type epoxy resins, alkyl polyol type epoxy resins, rubber-modified type epoxy resins, glycidyl ester compounds, bisphenol A type episulfide resins, and the like.

[0050] Among the above epoxy (meth)acrylates, commercially available ones include, for example, EBECRYL860, EBECRYL3200, EBECRYL3201, EBECRYL3412, EBECRYL3600, EBECRYL3700, EBECRYL3701, EBECRYL3702, EBECRYL3703, EBECRYL3800, EBECRYL6040, EBECRYL Examples of the epoxy ester include RDX63182 (all manufactured by Daicel-Allnex Corporation), EA-1010, EA-1020, EA-5323, EA-5520, EACHD, and EMA-1020 (all manufactured by Shin-Nakamura Chemical Co., Ltd.), epoxy ester M-600A, epoxy ester 40EM, epoxy ester 70PA, epoxy ester 200PA, epoxy ester 80MFA, epoxy ester 3002M, epoxy ester 3002A, epoxy ester 1600A, epoxy ester 3000M, epoxy ester 3000A, epoxy ester 200EA, and epoxy ester 400EA (all manufactured by Kyoeisha Chemical Co., Ltd.), Denacol Acrylate DA-141, Denacol Acrylate DA-314, and Denacol Acrylate DA-911 (all manufactured by Nagase ChemteX Corporation).

[0051] The urethane (meth)acrylate can be, for example, a product obtained by reacting an isocyanate compound with a (meth)acrylic acid derivative having a hydroxyl group. Here, a catalytic amount of a tin-based compound or the like can be used as a catalyst for the reaction between the isocyanate compound and the (meth)acrylic acid derivative. The urethane (meth)acrylate can be monofunctional or multifunctional, such as bifunctional. Examples of the isocyanate compound used to obtain the urethane (meth)acrylate include polyisocyanate compounds such as isophorone diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, diphenylmethane-4,4'-diisocyanate (MDI), hydrogenated MDI, polymeric MDI, 1,5-naphthalene diisocyanate, norbornane diisocyanate, tolidine diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, lysine diisocyanate, triphenylmethane triisocyanate, tris(isocyanatephenyl)thiophosphate, tetramethylxylylene diisocyanate, and 1,6,11-undecane triisocyanate. Also usable as the isocyanate compound are chain-extended polyisocyanate compounds obtained by reacting a polyol with an excess of an isocyanate compound. Examples of the polyol include ethylene glycol, propylene glycol, glycerin, sorbitol, trimethylolpropane, carbonate diol, polyether diol, polyester diol, polycaprolactone diol, etc.

[0052] Examples of the (meth)acrylic acid derivative having a hydroxyl group include mono(meth)acrylates of dihydric alcohols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and polyethylene glycol; mono(meth)acrylates or di(meth)acrylates of trihydric alcohols such as trimethylolethane, trimethylolpropane, and glycerin; and epoxy(meth)acrylates such as bisphenol A-type epoxy(meth)acrylate.

[0053] Among the above urethane (meth)acrylates, commercially available ones include, for example, M-1100, M-1200, M-1210, M-1600 (all manufactured by Toagosei Co., Ltd.), EBECRYL230, EBECRYL270, EBECRYL8402, EBECRYL8411, EBECRYL8412, EBECRYL8413, EBECRYL8804, EBECRYL8803, EBECRYL8807, EB ECRYL9270, EBECRYL210, EBECRYL4827, EBECRYL6700, EBECRYL220, EBECRYL2220 (all manufactured by Daicel-Allnex), Art Resin UN-9000H, Art Resin UN-9000A, Art Resin UN-7100, Art Resin UN-1255, Art Resin UN-330, Art Resin UN-3320HB, Art Resin UN-1200 TPK, Art Resin SH-500B (all manufactured by Negami Chemical Industries), U-2HA, U-2PHA, U-3HA, U-4HA, U-6H, U-6LPA, U-6HA, U-10H, U-15HA, U-122A, U-122P, U-108, U-108A, U-324A, U-340A, U-340P, U-1084A, U-2061BA, UA-340P, UA-4100, UA-4000, UA-4200, UA- 4400, UA-5201P, UA-7100, UA-7200, UA-W2A (all manufactured by Shin-Nakamura Chemical Co., Ltd.), AI-600, AH-600, AT-600, UA-101I, UA-101T, UA-306H, UA-306I, UA-306T (all manufactured by Kyoeisha Chemical Co., Ltd.), CN-902, CN-973, CN-9021, CN-9782, CN-9833 (all manufactured by Arkema), etc. The above-mentioned (meth)acrylic compounds may be used alone or in combination of two or more kinds.

[0054] In addition, it is also preferable to use the above-mentioned (meth)acrylic acid ester compound in combination with a monofunctional (meth)acrylic compound or vinyl compound other than the (meth)acrylic acid ester compound as the photopolymerizable compound (B). As such compounds, (meth)acrylic compounds having a cyclic structure such as (meth)acryloylmorpholine, and vinyl compounds having a cyclic structure such as N-vinyl-2-pyrrolidone and N-vinyl-ε-caprolactam can also be used. In addition, (meth)acrylamide compounds such as N,N-dimethyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and N,N-dimethylaminopropyl(meth)acrylamide can also be used.

[0055] In the present invention, the storage modulus and breaking elongation of the cured product can be adjusted by appropriately selecting the photopolymerizable compound (B). For example, the photopolymerizable compound (B) preferably contains a compound (B1) (high Tg compound (B1)) that has a glass transition temperature (Tg) of 70° C. or higher when made into a homopolymer. The use of such a high Tg compound (B1) makes it easier to increase the storage modulus. The glass transition temperature (Tg) may be measured by synthesizing a homopolymer of each compound. Specifically, the glass transition temperature (Tg) refers to the temperature at which a maximum due to micro-Brownian motion appears among the maximum loss tangents (tan δ) obtained by dynamic viscoelasticity measurement of the synthesized homopolymer, and can be measured by a conventionally known method using a dynamic viscoelasticity measuring device. For example, the synthesis of the homopolymer may be carried out by pouring the monomer components constituting the homopolymer into a Teflon (registered trademark) mold having a width of 3 mm, a length of 30 mm, and a thickness of 1 mm, and irradiating ultraviolet rays at 1000 mJ / cm using a UV-LED (wavelength 365 nm). 2The cured product may be photocured by irradiating the resin with light to obtain a cured product sample. The dynamic viscoelasticity may be measured by using the obtained cured product sample with a dynamic viscoelasticity measuring device at a temperature range of, for example, -50 to 160°C. The measurement conditions are a tensile deformation mode, a set strain of 1%, a measurement frequency of 1 Hz, and a heating rate of 5°C / min. Literature values ​​described in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989) and the like may also be used.

[0056] The content of the compound (B1) is preferably 10% by mass or more and 50% by mass or less based on the total amount of the photopolymerizable compound (B). By setting the content of the compound (B1) within the above range, it is easy to increase the storage modulus and the elongation at break, and it is easy to obtain excellent adhesive performance and impact resistance. From these viewpoints, the content of the compound (B1) is more preferably 10% by mass or more and 40% by mass or less based on the total amount of the photopolymerizable compound (B), and further preferably 14% by mass or more and 35% by mass or less. From the same viewpoint, the content of the compound (B1) is preferably 2.5 mass% or more and 15 mass% or less, more preferably 3.2 mass% or more and 13 mass% or less, and even more preferably 5.0 mass% or more and 11 mass% or less, based on the total amount of the curable resin composition.

[0057] In addition to the above-mentioned compound (B1), the photopolymerizable compound (B) preferably contains a compound (B2) (low Tg compound (B2)) having a glass transition temperature (Tg) of less than 70° C. when made into a homopolymer. By containing the low Tg compound (B2) in addition to the high Tg compound (B1), the above-mentioned storage modulus and breaking elongation are improved in a well-balanced manner, and it becomes easier to improve the adhesive performance and impact resistance. From such a viewpoint, the content of the low Tg compound (B2) is preferably 50% by mass or more based on the total amount of the photopolymerizable compound (B), but is preferably 50% by mass or more and 90% by mass or less, more preferably 60% by mass or more and 90% by mass or less, and even more preferably 65% ​​by mass or more and 86% by mass or less. From the same viewpoint, the content of the low Tg compound (B2) is preferably 12 mass% or more and 35 mass% or less, more preferably 16 mass% or more and 29 mass% or less, and even more preferably 20 mass% or more and 27 mass% or less, based on the total amount of the curable resin composition.

[0058] From the viewpoint of achieving a good balance between adhesion and impact resistance, the high Tg compound (B1) used is a compound having, when made into a homopolymer, a glass transition temperature of preferably 200° C. or lower, more preferably 160° C. or lower, and preferably 80° C. or higher, more preferably 90° C. or higher. On the other hand, as the low Tg compound (B2), a compound is used which, when made into a homopolymer, has a glass transition temperature of preferably 60°C or lower, more preferably 45°C or lower, and is preferably -20°C or higher, more preferably -10°C or higher.

[0059] The photopolymerizable compound (B) preferably contains an alicyclic structure-containing (meth)acrylic compound. Here, the alicyclic structure may be formed of only carbon atoms, but may contain heteroatoms such as nitrogen, oxygen, and sulfur. The heteroatom is preferably a nitrogen atom. The alicyclic structure-containing (meth)acrylic compound is preferably monofunctional. By making it monofunctional, it becomes easier to increase the breaking elongation. By containing an alicyclic structure-containing (meth)acrylic compound in the photopolymerizable compound (B), it becomes easier to increase the breaking elongation of the cured product. Furthermore, by containing an alicyclic structure-containing (meth)acrylic compound in the photopolymerizable compound (B), when the moisture-curable resin (A) is a moisture-curable urethane resin, the compatibility with the moisture-curable resin (A) becomes good, and various performances become easier to improve. The alicyclic structure-containing (meth)acrylic compound is preferably a high Tg compound (B1) (i.e., a Tg of 70° C. or higher when made into a homopolymer). When the alicyclic structure-containing (meth)acrylic compound, which is the high Tg compound (B1), is used, it becomes easier to improve both the storage modulus and the breaking elongation of the cured product.

[0060] Examples of the alicyclic structure-containing (meth)acrylic compound that can be used as the high Tg compound (B1) include alicyclic (meth)acrylates such as dicyclopentenyl acrylate (Tg: 120°C), dicyclopentanyl methacrylate (Tg: 175°C), dicyclopentanyl acrylate (Tg: 120°C), isobornyl methacrylate (Tg: 173°C), isobornyl acrylate (Tg: 94°C), 1-adamantyl methacrylate (Tg: 250°C), 1-adamantyl acrylate (Tg: 153°C), and 4-tert-butylcyclohexyl acrylate (Tg: 80°C), as well as (meth)acrylic compounds in which the alicyclic structure has a heteroatom, such as acryloylmorpholine (Tg: 145°C). Among these, isobornyl acrylate, acryloyl morpholine, and 4-tert-butylcyclohexyl acrylate are preferred, and isobornyl acrylate and acryloyl morpholine are more preferred. These alicyclic structure-containing (meth)acrylic compounds may be used alone or in combination of two or more. The content of the alicyclic structure-containing (meth)acrylic compound, which is the high Tg compound (B1), is preferably 5 mass% or more and 50 mass% or less, more preferably 10 mass% or more and 40 mass% or less, and even more preferably 14 mass% or more and 35 mass% or less, based on the total amount of the photopolymerizable compound (B).

[0061] However, the high Tg compound (B1) does not necessarily have to be an alicyclic structure-containing (meth)acrylic compound, and a photopolymerizable compound other than an alicyclic structure-containing (meth)acrylic compound may be used. Examples of such compounds include alkyl (meth)acrylates such as methyl methacrylate (Tg: 105°C) and t-butyl methacrylate (Tg: 118°C), amide group-containing vinyl monomers such as dimethylacrylamide (Tg: 119°C), diethylacrylamide (Tg: 81°C), dimethylaminopropylacrylamide (Tg: 134°C), isopropylacrylamide (Tg: 134°C), and hydroxyethylacrylamide (Tg: 98°C). These may be used alone or in combination with the above-mentioned alicyclic structure-containing (meth)acrylic compound as the high Tg compound (B1).

[0062] The low Tg compound (B2) is not particularly limited, but from the viewpoint of reactivity, an alkyl(meth)acrylate is preferably used. The alkyl(meth)acrylate may have an alkyl group with 1 to 18 carbon atoms, and preferably has an alkyl(meth)acrylate with an alkyl group with 12 to 18 carbon atoms. The alkyl group may be linear or branched. The alkyl(meth)acrylate as the low Tg compound (B2) may be used alone or in combination of two or more. Preferable examples of such alkyl(meth)acrylate include lauryl acrylate (Tg=-3°C) and stearyl acrylate (Tg=35°C). The content of the alkyl (meth)acrylate, which is the low Tg compound (B2), is, for example, 40 mass% or more, preferably 45 mass% or more and 90 mass% or less, more preferably 50 mass% or more and 89 mass% or less, and even more preferably 60 mass% or more and 86 mass% or less, based on the total amount of the photopolymerizable compound (B).

[0063] In the curable resin composition, the content of the photopolymerizable compound (B) is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, based on the total amount of the curable resin composition. The content of the photopolymerizable compound (B) is preferably 45% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less, and even more preferably 31.5% by mass or less, based on the total amount of the curable resin composition. By setting the content of the photopolymerizable compound (B) within the above range, the breaking elongation and storage modulus are set within a predetermined range, and it is easy to improve the adhesive performance, impact resistance, etc. Furthermore, by reducing the amount of the photopolymerizable compound (B), it is easy to increase the storage modulus and breaking elongation of the cured product, for example, without using the compound (B1).

[0064] In the curable resin composition, the ratio (B / A) of the content of the photopolymerizable compound (B) to the moisture-curable resin (A) is preferably 0.30 to 0.80, more preferably 0.35 to 0.65, and even more preferably 0.40 to 0.55, based on the total amount of the curable resin composition. By making the content ratio (B / A) within the above range, the breaking elongation and storage modulus are within a predetermined range, and it is easy to improve the adhesive performance, impact resistance, etc. In addition, by making it 0.55 or less, the storage modulus and breaking elongation of the cured product can be increased without using the compound (B1).

[0065] (Crosslinking agent (X)) The curable resin composition of the present invention preferably contains a crosslinking agent (X). By containing the crosslinking agent (X), the breaking elongation and storage modulus are increased, and the adhesive performance and impact resistance are easily improved. The crosslinking agent (X) is preferably a compound having a functional group capable of reacting with at least one of the moisture-curable resin (A) and the photopolymerizable compound (B) when the curable resin composition is cured. Specifically, a compound having an isocyanate group can be mentioned. Such a compound can be a polyisocyanate compound having two or more isocyanate groups in one molecule.

[0066] Examples of the polyisocyanate compound used as the crosslinking agent (X) include aromatic polyisocyanate compounds and aliphatic polyisocyanate compounds. Examples of the aromatic polyisocyanate compound include diphenylmethane diisocyanate, liquid modified diphenylmethane diisocyanate, polymeric MDI, tolylene diisocyanate, and naphthalene-1,5-diisocyanate. Examples of the aliphatic polyisocyanate compound include hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, norbornane diisocyanate, transcyclohexane-1,4-diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated diphenylmethane diisocyanate, cyclohexane diisocyanate, bis(isocyanatemethyl)cyclohexane, and dicyclohexylmethane diisocyanate. As the polyisocyanate compound, from the viewpoint of increasing the storage modulus and improving the adhesive performance, an aromatic polyisocyanate compound is preferable, diphenylmethane diisocyanate and modified products thereof, and polymeric MDI are more preferable, and diphenylmethane diisocyanate is even more preferable. The polyisocyanate compounds may be used alone or in combination of two or more kinds.

[0067] The content of the crosslinking agent (X) in the curable resin composition is preferably 0.4% by mass or more and 10% by mass or less based on the total amount of the curable resin composition. By making the content of the crosslinking agent (X) 0.4% by mass or more, it becomes easier to make the storage modulus and elongation at break greater than or equal to a predetermined value, and it becomes easier to improve the adhesive strength and the like. In addition, by making the content of the crosslinking agent 0.4% by mass or more, it becomes easier to make the storage modulus and elongation at break greater than or equal to a predetermined value, for example, without using the above-mentioned high Tg compound (B1). On the other hand, by making it 10% by mass or less, it is possible to ensure the content of the moisture-curable resin (A) and the photopolymerizable compound (B) at a certain amount or more, so that it becomes easier to increase the elongation at break, and it becomes easier to improve the adhesive strength and impact resistance. The content of the crosslinking agent is more preferably 0.8% by mass or more, and even more preferably 1.0% by mass or more, from the viewpoint of easily increasing the storage modulus, etc. Also, the content of the crosslinking agent is more preferably 6% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, from the viewpoint of easily maintaining the breaking elongation at a high value, etc.

[0068] (Photopolymerization initiator (Y)) When the curable resin composition of the present invention uses the above-mentioned photopolymerizable compound (B), it preferably contains a photopolymerization initiator (Y) in order to ensure photocurability. The photopolymerization initiator (Y) may be a photoradical polymerization initiator.Specific examples include benzophenone-based compounds, acetophenone-based compounds such as α-aminoalkylphenone and α-hydroxyalkylphenone, acylphosphine oxide-based compounds, titanocene-based compounds, oxime ester-based compounds, benzoin ether-based compounds, and thioxanthone.Among these, acetophenone-based compounds are preferred, and α-aminoalkylphenone is more preferred, from the viewpoint of easily adjusting the breaking elongation and storage modulus within a predetermined range. Among the above photopolymerization initiators, commercially available ones include, for example, IRGACURE184, IRGACURE369, IRGACURE379, IRGACURE379EG, IRGACURE651, IRGACURE784, IRGACURE819, IRGACURE907, IRGACURE2959, IRGACURE OXE01, Lucirin TPO (all manufactured by BASF), benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether (all manufactured by Tokyo Chemical Industry Co., Ltd.).

[0069] The content of the photopolymerization initiator (Y) in the curable resin composition is preferably 0.01 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the photopolymerizable compound. By having the content of the photopolymerization initiator (Y) within this range, the obtained curable resin composition has excellent photocurability and storage stability. In addition, by setting the content within the above range, the photopolymerizable compound (B) is appropriately cured, and the storage modulus and breaking elongation described above can be easily adjusted within a predetermined range.

[0070] (Filler) The curable resin composition of the present invention may contain a filler. By containing a filler, the curable resin composition of the present invention has a suitable thixotropy and can sufficiently retain its shape after application. As the filler, a particulate filler may be used. As the filler, inorganic fillers are preferred, such as silica, talc, titanium oxide, zinc oxide, calcium carbonate, etc. Among them, silica is preferred because the resulting curable resin composition has excellent ultraviolet transmittance. In addition, the filler may be subjected to hydrophobic surface treatment such as silylation treatment, alkylation treatment, and epoxidation treatment. The fillers may be used alone or in combination of two or more. The content of the filler is preferably from 1 mass % to 20 mass %, more preferably from 2 mass % to 15 mass %, and further preferably from 5 mass % to 12 mass %, based on the total amount of the curable resin composition.

[0071] (Coupling Agent) The curable resin composition may contain a coupling agent. By containing a coupling agent, the adhesive strength is easily improved. Examples of the coupling agent include a silane coupling agent, a titanate coupling agent, and a zirconate coupling agent. Among them, the silane coupling agent is preferable because it has an excellent effect of improving adhesiveness. The above coupling agents may be used alone or in combination of two or more. The content of the coupling agent is preferably 0.05% by mass or more and 5% by mass or less, more preferably 0.2% by mass or more and 2% by mass or less, and even more preferably 0.5% by mass or more and 1.5% by mass or less, based on the total amount of the curable resin composition. By setting the content of the coupling agent within these ranges, the adhesive strength can be improved without affecting the storage modulus, etc.

[0072] The curable resin composition of the present invention may be diluted with a solvent as necessary. When the curable resin composition is diluted with a solvent, the mass parts of the curable resin composition are based on the solid content, that is, the mass parts excluding the solvent. In addition to the components described above, the curable resin composition may contain additives such as wax particles, metal-containing particles, light-shielding agents, colorants, reactive diluents, and moisture-cure accelerating catalysts.

[0073] The method for producing the curable resin composition may be to mix the components constituting the curable resin composition using a mixer. For example, a method of mixing a moisture-curable resin (A), a photopolymerizable compound (B), and a crosslinking agent (X), a photopolymerization initiator (Y), a filler, a coupling agent, and other additives, which are blended as necessary, may be mentioned. Examples of the mixer include a homodisper, a homomixer, a universal mixer, a planetary mixer (planetary stirring device), a kneader, and a three-roll mill.

[0074] [Method of using the curable resin composition] The curable resin composition of the present invention is cured and used as a cured product. When the curable resin composition of the present invention has photocurability, thermosetting or both of these curability, it is preferable to first cure the composition by photocuring, thermosetting or both of these by light irradiation or heating to, for example, a B-stage state (semi-cured state), and then cure it by moisture to fully cure it. The curable resin composition of the present invention is preferably photo-moisture curable. Therefore, it is preferable to photocur the composition by light irradiation to a B-stage state (semi-cured state), and then cure it by moisture to fully cure it.

[0075] Here, when the curable resin composition is placed between the adherends and the adherends are bonded together, it is preferable to apply the composition to one of the adherends, and then photo-curing the composition by light irradiation to bring it to, for example, a B-stage state, and then superimposing the other adherend on the curable resin composition cured to the B-stage state, and temporarily bonding the adherends with an appropriate adhesive strength (initial adhesive strength). The curable resin composition in the B-stage state is then fully cured by curing with moisture, and the superimposed adherends are bonded together with sufficient adhesive strength via the curable resin composition.

[0076] Here, the light irradiated during photocuring is not particularly limited as long as it is light that cures the photopolymerizable compound (B), but ultraviolet light is preferred. When heat curing, it is not particularly limited as long as it is a temperature at which the thermosetting resin cures, but for example, it is preferable to heat to a temperature of 60°C or higher and lower than 120°C, more preferably a temperature lower than 100°C. When the curable resin composition is cured by moisture, it is sufficient to leave it in the air for a predetermined time.

[0077] The curable resin composition of the present invention is preferably used as an adhesive for electronic devices. The curable resin composition of the present invention is more preferably used as an adhesive for portable electronic devices. More specifically, examples of portable electronic devices include mobile phones such as smartphones and tablet terminals. When these portable electronic devices are accidentally dropped during use, parts may come off. However, when the curable resin composition of the present invention is used as an adhesive for portable electronic devices, the cured product of the curable resin composition of the present invention has excellent PUSH adhesive strength and impact resistance, so that the parts are less likely to come off. In electronic devices, the adherend is not particularly limited, but may be, for example, various components constituting the electronic device. Examples of various components constituting the electronic device include electronic components or substrates on which electronic components are attached, and more specifically, various electronic components provided in display elements, substrates on which electronic components are attached, and semiconductor chips. That is, the present invention also provides an electronic component having a cured product of the curable resin composition. The material of the adherend may be any of metal, glass, plastic, etc. The shape of the adherend is not particularly limited, and examples thereof include a film, sheet, plate, panel, tray, rod (rod-shaped body), box, housing, etc.

[0078] The curable resin composition of the present invention has a specific storage modulus and breaking elongation, and thus the cured product of the curable resin composition has high adhesive strength, particularly PUSH adhesive strength, and excellent impact resistance. Therefore, even when the application width or adhesion area of ​​the curable resin composition of the present invention is small, when a large impact is applied to an adherend, the impact is prevented from being transmitted to electronic components or the adherend is prevented from peeling off. Therefore, it is suitable for use as an adhesive for bonding semiconductor chips which have a small bonding area, and as an adhesive for use in display devices, such as display devices for portable electronic devices, which tend to have a small application width, particularly display devices for mobile phones such as smartphones. EXAMPLES

[0079] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0080] In the present examples, various physical property measurements and performance evaluations were carried out as follows. (Storage modulus) According to the method described in the specification, a cured sample was prepared from the curable resin composition, and the storage modulus of the cured sample at 25° C. was measured using a dynamic viscoelasticity measuring device (manufactured by IT Measurement & Control Co., Ltd., product name "DVA-200"). (Elongation at break) According to the method described in the specification, test pieces were prepared from the curable resin composition and pulled to break at a speed of 50 mm / min using a tensile tester (manufactured by A&D Corporation, product name "TENSILON"), and the breaking elongation at 25°C was measured.

[0081] (PUSH adhesion test) An overview of the PUSH adhesion test is shown in Figure 1. As shown in Figure 1(a), a polycarbonate plate 3 of 2 mm thickness with a rectangular hole 2 of 38 mm x 50 mm in the center was prepared. The curable resin composition 1 was applied to the polycarbonate plate 3 in a square frame shape with an outer diameter of 46 mm x 61 mm, an inner diameter of 44 mm x 59 mm, and an application width of 1 mm so as to surround the rectangular hole 2. Ultraviolet light of 1000 mJ / cm was applied using a UV-LED (wavelength 365 nm). 2 The curable resin composition 1 was photocured by irradiating the glass plate 4. Thereafter, a glass plate 4 measuring 50 mm×75 mm and having a thickness of 4 mm was attached to a polycarbonate plate 3 via the semi-cured curable resin composition 1, to fabricate a test specimen. The glass plate 4 and the square frame-shaped curable resin composition 1 were positioned so that their centers coincided with each other. Thereafter, the product was inverted from the state shown in FIG. 1(a) and placed so that the polycarbonate plate 3 was placed on top of the glass plate 4. A pressure of 5 kgf was applied from the polycarbonate plate 3 side, and the product was left for 24 hours at room temperature (23°C) and 50% RH to moisture-cure the curable resin composition 1, and the glass plate 4 and the polycarbonate plate 3 were bonded together by the fully cured curable resin composition 1. Next, as shown in FIG. 1(b), the test specimen was fixed to a support 5 with the glass plate 4 facing downward. A load was applied to the glass plate 4 through the rectangular hole 2 at a speed of 10 mm / min, and the load value was measured when the glass plate 4 peeled off.

[0082] (Impact resistance test) An overview of the impact resistance test is shown in Figure 2. First, a test specimen was prepared in the same manner as in the PUSH adhesion test. Next, as shown in Figure 2(b), the prepared test specimen was fixed to a support stand 5, and an iron ball 6 weighing 200 g, which is large enough to pass through the rectangular hole 2, was dropped from a height of 20 mm so that it would pass through the rectangular hole 2. The iron ball was dropped repeatedly under the same conditions, and the impact resistance was evaluated according to the following evaluation criteria. A: The glass plate peeled off after the iron ball was dropped on it more than 40 times. B: The glass plate peeled off after the iron ball was dropped less than 40 times.

[0083] (Moisture curing resin (A)) Moisture-curable urethane resin A was prepared according to Synthesis Example 1 below. [Synthesis Example 1] 100 parts by mass of polytetramethylene ether glycol (manufactured by Mitsubishi Chemical Corporation, product name "PTMG-2000") as a polyol compound and 0.01 parts by mass of dibutyltin dilaurate were placed in a 500 mL separable flask and mixed by stirring under vacuum (20 mmHg or less) at 100°C for 30 minutes. The pressure was then returned to normal pressure, and 26.5 parts by mass of diphenylmethane diisocyanate (manufactured by Nisso Shoji Co., Ltd., product name "Pure MDI") as a polyisocyanate compound was added, and the mixture was stirred at 80°C for 3 hours to react, obtaining a moisture-curable urethane resin A (weight average molecular weight 2700).

[0084] Moisture-curable urethane resin B was prepared according to Synthesis Example 2 below. [Synthesis Example 2] 9.8 parts by mass of 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM-803") was added to a reaction vessel containing 100 parts by mass of moisture-curing urethane resin A obtained in the same manner as in Synthesis Example 1. The mixture was then stirred and mixed at 80°C for 1 hour to obtain moisture-curing urethane resin B (weight average molecular weight 3100) having an isocyanate group and a trimethoxysilyl group at the molecular end as an organic silyl group-containing urethane resin.

[0085] The components other than the moisture-curable urethane resin used in the examples and comparative examples were as follows: (Photopolymerizable compound (B)) Isobornyl acrylate: Kyoeisha Chemical Co., Ltd., product name "IB-XA", monofunctional, Tg 94℃ Acryloylmorpholine: KJ Chemicals, product name "ACMO", monofunctional, Tg 145℃ Lauryl acrylate: Kyoeisha Chemical Company, product name "Light Acrylate LA", monofunctional, Tg-3℃ Stearyl acrylate: Sartomer Corporation, product name "SR257", monofunctional, Tg: 35°C (Crosslinking agent (X)) Diphenylmethane Diisocyanate (Photopolymerization initiator (Y)) Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide: BASF, trade name "IRGACURE 819" (Filler) Silicone-treated silica: Nippon Aerosil Co., Ltd., product name "RY300" (Coupling Agent) 3-Acryloxypropyltrimethoxysilane: Shin-Etsu Chemical Co., Ltd., product name "KBM-5103"

[0086] [Examples 1 to 8, Comparative Examples 1 to 5] According to the formulation shown in Table 1, each material was stirred at a temperature of 50°C using a planetary stirrer (Thinky Corporation, "Awatori Rentaro"), and then uniformly mixed at a temperature of 50°C using a ceramic triple roll to obtain the curable resin compositions of Examples 1 to 8 and Comparative Examples 1 to 5.

[0087] [Table 1]

[0088] As shown in the above examples, both the PUSH adhesive strength and impact resistance were excellent by increasing both the storage modulus and breaking elongation of the cured product at 25° C. In contrast, as shown in the comparative examples, when either the storage modulus or breaking elongation was below the specified value, it was not possible to obtain both excellent PUSH adhesive strength and impact resistance. [Explanation of symbols]

[0089] 1 Curable resin composition 2 rectangular hole 3 Polycarbonate plate 4 Glass Plate 5 Support stand 6. Iron Ball

Claims

1. A curable resin composition comprising a moisture-curable resin (A), a cured product of the curable resin composition has a storage modulus of 10 MPa or more at 25° C. and a breaking elongation of 700% or more at 25° C.; Further comprising a photopolymerizable compound (B) and a photopolymerization initiator (Y), The curable resin composition, wherein the photopolymerizable compound (B) contains a compound (B1) that, when made into a homopolymer, has a glass transition temperature (Tg) of 70° C. or higher.

2. A curable resin composition comprising a moisture-curable resin (A), wherein a cured product of the curable resin composition has a storage modulus of 10 MPa or more at 25°C and a breaking elongation of 700% or more at 25°C; Further comprising a photopolymerizable compound (B) and a photopolymerization initiator (Y), The curable resin composition, wherein the photopolymerizable compound (B) contains an alicyclic structure-containing (meth)acrylic compound.

3. The curable resin composition according to claim 1 or 2, further comprising a crosslinking agent (X), and the content of the crosslinking agent (X) is 0.4 mass% or more and 10 mass% or less based on the total amount of the curable resin composition.

4. The curable resin composition according to claim 3 , wherein the crosslinking agent (X) is a compound having an isocyanate group.

5. The curable resin composition according to claim 1 , wherein the content of the compound (B1) is 10% by mass or more and 50% by mass or less based on the total amount of the photopolymerizable compound (B).

6. The curable resin composition according to claim 1 or 5, wherein the content of the compound (B1) is 2.5 mass % or more and 15 mass % or less based on the total amount of the curable resin composition.

7. The photopolymerizable compound (B) includes a compound (B2) having a glass transition temperature (Tg) of less than 70° C. when made into a homopolymer. The curable resin composition according to any one of claims 1 to 6.

8. The curable resin composition according to any one of claims 1 to 7, wherein the moisture-curable resin (A) is a moisture-curable urethane resin.

9. The content of the moisture-curable resin (A) is 50 mass% or more and 80 mass% or less based on the total amount of the curable resin composition. The curable resin composition according to any one of claims 1 to 8.

10. A cured product of the curable resin composition according to any one of claims 1 to 9.

11. An electronic component comprising the cured body according to claim 10.

Citation Information

Patent Citations

  • Method for producing urethane resin for vibration damping material and urethane prepolymer for vibration damping material

    JP2008133460A

  • Polyurethane-based curable composition

    JP2008208191A

  • Moisture-curable hot-melt urethane composition and adhesive

    JP2016113552A

  • Resin composition, cured product, civil engineering and construction structure, and coating method

    JP2019199544A

  • Cured body, electronic component, display element, and light- / moisture-curable resin composition