Separator for non-aqueous secondary battery and non-aqueous secondary battery

The separator design with controlled polyvinylidene fluoride resins and fillers addresses electrolyte decomposition and high-temperature issues, ensuring strong adhesion and preventing short circuits, thus maintaining battery performance and capacity.

JP7557552B2Active Publication Date: 2024-09-27TEIJIN LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022575294
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-16
Filing Date
2022-07-15
Publication Date
2024-09-27
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

Batteries using separators with polyvinylidene fluoride resin adhesive porous layers face issues such as electrolyte decomposition and gas generation during high-temperature wet heat pressing, leading to decreased cycle characteristics and dimensional stability, and high-temperature exposure causes changes in the porous structure, weakening the separator and increasing the risk of short circuits.

Method used

A separator design with a porous base material and an adhesive porous layer containing specific polyvinylidene fluoride resins and fillers, characterized by controlled Gurley values and differential scanning calorimetry peaks, ensures strong adhesion to electrodes through dry and wet heat pressing, maintaining structural integrity and preventing short circuits even at high temperatures.

Benefits of technology

The separator maintains excellent adhesion to electrodes, reduces the risk of short circuits, and preserves battery capacity retention rate under high temperatures, enhancing the performance and stability of non-aqueous secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557552000005
    Figure 0007557552000005
  • Figure 0007557552000006
    Figure 0007557552000006
  • Figure 0007557552000004
    Figure 0007557552000004
Patent Text Reader

Abstract

This separator for nonaqueous secondary batteries is provided with a porous base material and an adhesive porous layer that contains a polyvinylidene fluoride resin and a filler; this separator for nonaqueous secondary batteries has a Gurley value of 50 seconds / 100 mL to 200 seconds / 100 mL; and if the entirety of the polyvinylidene fluoride resin contained in the adhesive porous layer is subjected, as a sample, to differential scanning calorimetry, two or more endothermic peaks and / or two or more exothermic peaks are found.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a separator for a nonaqueous secondary battery and a nonaqueous secondary battery. [Background technology]

[0002] Each of WO 2013 / 058367, WO 2013 / 058368, WO 2013 / 058369, and WO 2013 / 058370 discloses a separator for a nonaqueous secondary battery comprising a porous substrate and an adhesive porous layer containing a polyvinylidene fluoride-based resin, the polyvinylidene fluoride-based resin containing at least two types of polyvinylidene fluoride-based resin. Japanese Patent No. 6487130 discloses a separator for a non-aqueous secondary battery, which comprises a porous substrate and an adhesive porous layer containing a polyvinylidene fluoride resin, the polyvinylidene fluoride resin containing a copolymer of vinylidene fluoride, hexafluoropropylene, and a monomer having an acidic group or an ester group. Summary of the Invention [Problem to be solved by the invention]

[0003] A battery using a separator having an adhesive porous layer containing a polyvinylidene fluoride resin is generally manufactured by producing a laminate of an electrode and a separator, housing the laminate in an exterior material, injecting an electrolyte solution, and performing a heat press treatment (referred to as "wet heat press" in this disclosure). According to the wet heat press, the polyvinylidene fluoride resin is heat pressed in a state where it is swollen with the electrolyte solution, so that the adhesion between the electrode and the separator is good and good battery characteristics are easily obtained. However, when the wet heat press is performed at a relatively high temperature, the electrolyte solution or electrolyte may decompose and generate gas in the battery, which may cause, for example, a decrease in the cycle characteristics and dimensional stability of the battery.

[0004] On the other hand, there is a technique in which a laminate of an electrode and a separator is subjected to a heat press treatment (referred to as "dry heat press" in this disclosure) without impregnating the laminate with an electrolytic solution to bond the electrode and the separator. If the electrode and the separator are sufficiently bonded by the dry heat press, a wet heat press is not required, and therefore decomposition of the electrolytic solution and electrolyte does not occur. Even when wet heat pressing is performed, if the laminate is dry heat pressed prior to the wet heat pressing to bond the electrodes and separator, the temperature of the wet heat pressing can be set to a relatively low temperature, thereby suppressing decomposition of the electrolyte and electrolyte. In addition, if the separator is bonded to the electrodes by dry heat pressing before the laminate is housed in an exterior packaging, deformation of the laminate that may occur during transportation for housing in an exterior packaging is suppressed. Therefore, if the separator can be bonded well to the electrodes by dry heat pressing, it is expected that the performance of larger batteries can be maintained.

[0005] Incidentally, when a non-aqueous secondary battery is charged and discharged at high speed, the inside of the battery can become hot. It is known that when a non-aqueous secondary battery is exposed to high temperatures, the porous structure of the separator changes, causing a decrease in battery performance (e.g., capacity retention rate). Furthermore, when the temperature inside the battery becomes high and the pores in the porous substrate are relatively large, the strength of the separator is significantly weakened at high temperatures, making the battery more susceptible to short circuits.

[0006] It is against the above background that the present disclosure has been made. An object of the present disclosure is to provide a separator for a nonaqueous secondary battery that has excellent adhesion to an electrode by dry heat press and excellent adhesion to an electrode by wet heat press, is less likely to cause a short circuit in the battery at high temperatures, and has a high capacity retention rate of the battery even after exposure to high temperatures. [Means for solving the problem]

[0007] Specific means for solving the above problems include the following aspects. <1> A porous substrate; An adhesive porous layer provided on one or both sides of the porous substrate, the adhesive porous layer containing a polyvinylidene fluoride resin and a filler; The Gurley value is 50 seconds / 100 mL to 200 seconds / 100 mL. When the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, two or more endothermic peaks and / or two or more exothermic peaks are observed. Separator for non-aqueous secondary batteries. <2> When the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, at least one endothermic peak is observed in a region of 125° C. or higher and lower than 140° C. and at least one endothermic peak is observed in a region of 140° C. or higher and lower than 190° C. <1> The non-aqueous secondary battery separator according to claim 1 . <3> when the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, two or more endothermic peaks are observed, and the temperature difference between adjacent endothermic peaks is 10° C. or more and 60° C. or less. <1> or <2> The non-aqueous secondary battery separator according to claim 1 . <4> When the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, at least one exothermic peak is observed in a region of 80° C. or higher and lower than 125° C. and at least one exothermic peak is observed in a region of 125° C. or higher and lower than 190° C. <1> ~ <3> 13. The separator for a non-aqueous secondary battery according to claim 12. <5> when the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, two or more exothermic peaks are observed, and the temperature difference between adjacent exothermic peaks is 10° C. or more and 90° C. or less. <1> ~ <4> 13. The separator for a non-aqueous secondary battery according to claim 12. <6> A porous substrate; An adhesive porous layer provided on one or both sides of the porous substrate, the adhesive porous layer containing a polyvinylidene fluoride resin and a filler; The Gurley value is 50 seconds / 100 mL to 200 seconds / 100 mL. The polyvinylidene fluoride resin includes the following polyvinylidene fluoride resin X and polyvinylidene fluoride resin Y, Separator for non-aqueous secondary batteries. Polyvinylidene fluoride resin X: Contains constituent units derived from vinylidene fluoride and constituent units derived from hexafluoropropylene, in which the proportion of constituent units derived from hexafluoropropylene in all constituent units is more than 3.5 mol% and not more than 15 mol%, has a weight average molecular weight of 100,000 or more and less than 1,000,000, and has a melting point of 125°C or more and less than 150°C. Polyvinylidene fluoride resin Y: Contains structural units derived from vinylidene fluoride and may contain structural units derived from hexafluoropropylene, the proportion of structural units derived from hexafluoropropylene in all structural units is 0 mol% or more and 3.5 mol% or less, the weight average molecular weight is 1 million or more and less than 3 million, and the melting point is 150°C or more and less than 180°C. <7> When the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, two or more endothermic peaks and / or two or more exothermic peaks are observed. <6> The non-aqueous secondary battery separator according to claim 1 . <8> The difference between the melting point of the polyvinylidene fluoride resin X and the melting point of the polyvinylidene fluoride resin Y is 25°C or more and less than 55°C. <6> or <7> The non-aqueous secondary battery separator according to claim 1 . <9> a mass ratio of the polyvinylidene fluoride resin X to the polyvinylidene fluoride resin Y contained in the adhesive porous layer is 20:80 to 80:20; <6> ~ <8> 13. The separator for a non-aqueous secondary battery according to claim 12. <10> the polyvinylidene fluoride resin X contains constituent units derived from vinylidene fluoride and constituent units derived from hexafluoropropylene, the proportion of the constituent units derived from hexafluoropropylene in all constituent units is more than 5.0 mol% and not more than 15 mol%, the weight average molecular weight is 300,000 or more and less than 1,000,000, and the melting point is 125°C or more and less than 140°C; <6> ~ <9> 13. The separator for a non-aqueous secondary battery according to claim 12. <11> The polyvinylidene fluoride resin Y contains a constituent unit derived from vinylidene fluoride and may contain a constituent unit derived from hexafluoropropylene, the proportion of the constituent units derived from hexafluoropropylene in all constituent units is 0 mol% or more and 2.0 mol% or less, the weight average molecular weight is 1.5 million or more and less than 2 million, and the melting point is 150°C or more and less than 170°C. <6> ~ <10> 13. The separator for a non-aqueous secondary battery according to claim 12. <12> The adhesive porous layer contains a polyvinylidene fluoride resin having a monomer-derived structural unit represented by the following formula (1): <1> ~ <11> 13. The separator for a non-aqueous secondary battery according to claim 12.

[0008] [ka] In formula (1), R 1 , R 2 and R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms, a carboxy group, or a derivative of a carboxy group; X represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene group having 1 to 5 carbon atoms and having a substituent; Y represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms substituted with at least one hydroxy group, an alkyl group having 1 to 5 carbon atoms substituted with at least one carboxy group, or -ROC(=O)-(CH2) n It represents -C(=O)-OH (R represents an alkylene group having 1 to 5 carbon atoms, and n represents an integer of 0 or more).

[0009] <13> the acid value of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is less than 3.0 mgKOH / g; <1> ~ <12> 13. The separator for a non-aqueous secondary battery according to claim 12. <14> The weight average molecular weight of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is 300,000 or more and less than 3,000,000. <1> ~ <13> 13. The separator for a non-aqueous secondary battery according to claim 12. <15> In the entire polyvinylidene fluoride resin contained in the adhesive porous layer, the proportion of structural units derived from hexafluoropropylene to all structural units is more than 3.5 mol % and not more than 7.0 mol %. <1> ~ <14> 13. The separator for a non-aqueous secondary battery according to claim 12. <16> The volume ratio of the filler to the volume of the adhesive porous layer excluding pores is 30 volume % to 90 volume %. <1> ~ <15> 13. The separator for a non-aqueous secondary battery according to claim 12. <17> The filler contains at least one selected from the group consisting of metal hydroxide particles, metal sulfate particles, and barium titanate particles. <1> ~ <16> 13. The separator for a non-aqueous secondary battery according to claim 12. <18> The average primary particle size of the entire filler contained in the adhesive porous layer is 0.01 μm to 1.5 μm. <1> ~ <17> 13. The separator for a non-aqueous secondary battery according to claim 12. <19> A positive electrode, a negative electrode, and a conductive material disposed between the positive electrode and the negative electrode. <1> ~ <18> 13. A nonaqueous secondary battery comprising: the separator for a nonaqueous secondary battery according to claim 12, and generating an electromotive force by doping and undoping lithium ions. Effect of the Invention

[0010] According to the present disclosure, there is provided a separator for a nonaqueous secondary battery that has excellent adhesion to an electrode by dry heat press and excellent adhesion to an electrode by wet heat press, is less likely to cause a short circuit in the battery at high temperatures, and has a high capacity retention rate of the battery even after exposure to high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0012] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0013] In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved.

[0014] In the present disclosure, when referring to the amount of each component in a composition, in cases where multiple substances corresponding to each component are present in the composition, unless otherwise specified, it means the total amount of those multiple substances present in the composition. In the present disclosure, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.

[0015] In the present disclosure, MD (Machine Direction) means the longitudinal direction of the porous substrate and separator produced in a longitudinal shape, and TD (Transverse Direction) means the direction perpendicular to MD in the planar direction of the porous substrate and separator. In the present disclosure, TD is also referred to as "width direction".

[0016] In the present disclosure, when the stacking relationship of each layer constituting a separator is expressed as "upper" and "lower", the layer closer to the porous substrate is referred to as "lower" and the layer farther from the porous substrate is referred to as "upper".

[0017] In the present disclosure, performing a heat press treatment after impregnating a separator with an electrolyte is referred to as "wet heat press", and performing a heat press treatment without impregnating a separator with an electrolyte is referred to as "dry heat press".

[0018] In the present disclosure, the term "structural unit" of a copolymer or resin is synonymous with a monomer unit.

[0019] In the present disclosure, the volume of the adhesive porous layer excluding pores is referred to as the "solids volume."

[0020] <Separator for non-aqueous secondary batteries> The separator for a non-aqueous secondary battery according to the present disclosure (also simply referred to as a "separator" in the present disclosure) comprises a porous substrate and an adhesive porous layer provided on one or both sides of the porous substrate. The adhesive porous layer of the separator according to the present disclosure contains a polyvinylidene fluoride resin and a filler.

[0021] The description of the adhesive porous layer in the present disclosure is for the adhesive porous layer on each side of the porous substrate. The separator of the present disclosure may have the adhesive porous layer of the present disclosure on at least one side of the porous substrate. The following embodiment examples (1) to (3) are examples of the separator of the present disclosure. (1) A separator having an adhesive porous layer of the present disclosure on both sides of a porous substrate, in which the adhesive porous layer on one side of the separator and the adhesive porous layer on the other side of the separator may be the same or different in components, composition, thermal properties, etc. (2) A separator having an adhesive porous layer of the present disclosure on one side of a porous substrate and another layer on the other side of the porous substrate. (3) A separator having an adhesive porous layer of the present disclosure on one side of a porous substrate and no layer on the other side of the porous substrate (i.e., the surface of the porous substrate is exposed).

[0022] The separator of the present disclosure has a Gurley value of 50 sec / 100 mL to 200 sec / 100 mL.

[0023] If the Gurley value of the separator is less than 50 seconds / 100 mL, the battery may short-circuit under high temperatures. From the viewpoint of suppressing a short circuit under high temperatures, the Gurley value of the separator is 50 seconds / 100 mL or more, preferably 60 seconds / 100 mL or more, more preferably 70 seconds / 100 mL or more, and even more preferably 80 seconds / 100 mL or more. If the Gurley value of the separator exceeds 200 sec / 100 mL, the ion permeability is low, and the porous structure may be blocked when exposed to high temperatures, resulting in a decrease in battery capacity. From the viewpoint of ensuring ion permeability and maintaining the porous structure even when exposed to high temperatures, the Gurley value of the separator is 200 sec / 100 mL or less, preferably 180 sec / 100 mL or less, more preferably 150 sec / 100 mL or less, and even more preferably 130 sec / 100 mL or less.

[0024] The Gurley value for the separator of the present disclosure is measured in accordance with the JIS P8117:2009 standard.

[0025] The method for controlling the Gurley value of the separator of the present disclosure is not particularly limited, but it is preferable to control it by the Gurley value of the porous substrate. The Gurley value of the porous substrate can be controlled by the porosity of the porous substrate, and the porosity of the porous substrate can be controlled by, for example, the stretching ratio when producing the porous substrate (particularly the polyolefin microporous membrane).

[0026] In the separator of the present disclosure, when the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry (DSC) as a sample, two or more endothermic peaks and / or two or more exothermic peaks are observed. At least two or more endothermic peaks and two or more exothermic peaks may be observed, and two or more of both may be observed. When two or more endothermic peaks are observed, the number of endothermic peaks may be two or three or more. When two or more exothermic peaks are observed, the number of exothermic peaks may be two or three or more.

[0027] When DSC is performed on the entire polyvinylidene fluoride resin contained in the adhesive porous layer as a sample, the observation of two or more endothermic peaks or two or more exothermic peaks in a DSC curve with heat flow on the vertical axis and time or temperature on the horizontal axis means that the adhesive porous layer contains a polyvinylidene fluoride resin whose polymer chains move when heated at a relatively low temperature (in other words, a polyvinylidene fluoride resin whose polymer chains move easily) and a polyvinylidene fluoride resin whose polymer chains move when heated at a relatively high temperature (in other words, a polyvinylidene fluoride resin whose polymer chains do not move easily). It is presumed that the adhesive porous layer contains a polyvinylidene fluoride resin in which the polymer chains are easily mobile, so that the adhesive porous layer exhibits adhesiveness even when heat pressing is performed in a state in which the polyvinylidene fluoride resin is not swollen in the electrolyte or at a relatively low temperature, and that the adhesive porous layer contains a polyvinylidene fluoride resin in which the polymer chains are not easily mobile, so that clogging of the adhesive porous layer is suppressed even when heat pressing is performed in a state in which the polyvinylidene fluoride resin is swollen in the electrolyte or at a relatively high temperature, so that the performance of the separator is maintained. It is also believed that the inclusion of a polyvinylidene fluoride resin in which polymer chains are less mobile in the adhesive porous layer prevents the adhesive porous layer from becoming clogged even when the temperature inside the battery becomes high. Therefore, it is presumed that the separator of the present disclosure maintains the performance of the separator while providing excellent adhesion to the electrode through both dry heat press and wet heat press, and also provides a high capacity retention rate for the battery even after exposure to high temperatures.

[0028] From the viewpoint of achieving both adhesion to the electrodes by hot pressing and maintaining the performance of the separator after hot pressing, the separator of the present disclosure preferably exhibits at least one of the following (a) to (d).

[0029] (a) When DSC is performed on the entire polyvinylidene fluoride resin contained in the adhesive porous layer, two or more endothermic peaks are observed, including at least one endothermic peak in the range of 125°C or higher and lower than 140°C and at least one endothermic peak in the range of 140°C or higher and lower than 190°C. In this case, an endothermic peak may be observed in a region other than the above two regions.

[0030] (b) When the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to DSC as a sample, two or more endothermic peaks are observed, and the temperature difference between adjacent endothermic peaks is 10°C or more and 60°C or less. The temperature difference is preferably 15° C. or more, and more preferably 20° C. or more. The temperature difference is preferably 50° C. or less, and more preferably 40° C. or less.

[0031] (c) When DSC is performed on the entire polyvinylidene fluoride resin contained in the adhesive porous layer as a sample, two or more exothermic peaks are observed, including at least one exothermic peak in the range of 80°C or higher and lower than 125°C and at least one exothermic peak in the range of 125°C or higher and lower than 190°C. In this case, an exothermic peak may be observed in a region other than the above two regions.

[0032] (d) When the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to DSC as a sample, two or more exothermic peaks are observed, and the temperature difference between adjacent exothermic peaks is 10°C or more and 90°C or less. The temperature difference is preferably 15° C. or more, more preferably 18° C. or more, and even more preferably 20° C. or more. The temperature difference is preferably 80° C. or less, more preferably 50° C. or less, and even more preferably 40° C. or less.

[0033] Methods for controlling the endothermic peak and exothermic peak of the DSC for the polyvinylidene fluoride resin contained in the adhesive porous layer include, for example, the following (I) and (II). (I) In forming the polyvinylidene fluoride resin, two or more kinds of polyvinylidene fluoride resins differing in the type or amount of polymerization components, molecular weight, or melting point are used, and the mixing ratio thereof is adjusted. (II) The crystallinity of the polyvinylidene fluoride resin contained in the adhesive porous layer is controlled by the thermal conditions when forming the adhesive porous layer, the type or amount of the filler, or the incorporation of a crystallinity regulator.

[0034] A method for performing DSC and observing endothermic and exothermic peaks using the entire polyvinylidene fluoride resin contained in the adhesive porous layer as a sample will be described.

[0035] -sample- The adhesive porous layer is peeled off from the separator, immersed in dimethylacetamide, and heated to about 50°C to obtain a resin solution in which the polyvinylidene fluoride resin is dissolved. The resin solution is centrifuged in a centrifuge to precipitate insoluble matter. The rotation speed of the centrifuge is set to an effective speed for precipitating the insoluble matter according to the radius of the rotor. The supernatant of the resin solution from which the insoluble matter has been precipitated is taken out, and the centrifugation is repeated to remove the insoluble matter. The resin solution from which the insoluble matter has been removed is dropped into water to coagulate the polyvinylidene fluoride resin. The coagulated matter is removed from the water and dried, and the solid after drying is used as the sample. If the separator has an adhesive porous layer (or a similar layer) on both sides, peel off the adhesive porous layer (or a similar layer) from each side, and use each side as a separate sample.

[0036] -Differential Scanning Calorimetry (DSC)- A sample weighing 5.0 mg ± 0.3 mg is placed in an aluminum sample pan and set in the measuring device. The following three steps are carried out in succession under a nitrogen atmosphere to perform thermal analysis of the sample. Step 1: Heat from 30°C to 200°C at a rate of 5°C / min. Step 2: Decrease the temperature from 200°C to 30°C at a rate of 5°C / min. Step 3: Increase the temperature from 30°C to 200°C at a rate of 5°C / min.

[0037] -Observation of endothermic and exothermic peaks- Based on the results of the DSC thermal analysis, a DSC curve is drawn with the horizontal axis representing temperature (℃) and the vertical axis representing heat flow (W / g). In step 2, the upwardly convex portion in the temperature range from 180°C to 60°C is taken as the exothermic peak. The temperature of the maximum point of the exothermic peak, i.e., the temperature at which the slope of the tangent line changes from negative to positive from high to low temperatures in the DSC curve in step 2, is taken as the exothermic peak temperature. In step 3, the downward convex part in the temperature range from 60°C to 180°C is taken as the endothermic peak. The temperature of the minimum point of the endothermic peak, i.e., the temperature at which the slope of the tangent line changes from negative to positive from low to high temperatures in the DSC curve in step 3, is taken as the endothermic peak temperature.

[0038] The porous substrate and adhesive porous layer of the separator of the present disclosure will be described in detail below.

[0039] [Porous base material] In the present disclosure, the porous substrate means a substrate having pores or gaps therein. Examples of such substrates include microporous membranes; porous sheets such as nonwoven fabrics and paper made of fibrous materials; composite porous sheets obtained by laminating one or more other porous layers on these microporous membranes or porous sheets; and the like. In the present disclosure, from the viewpoint of thinning and strength of the separator, microporous membranes are preferred. The microporous membrane means a membrane having a large number of micropores therein, a structure in which the micropores are connected, and which allows gas or liquid to pass from one surface to the other surface.

[0040] The material of the porous substrate is preferably an electrically insulating material, and may be either an organic material or an inorganic material.

[0041] The porous substrate preferably contains a thermoplastic resin in order to provide the porous substrate with a shutdown function. The shutdown function refers to a function in which, when the battery temperature rises, the constituent material dissolves and blocks the pores of the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery. The thermoplastic resin is preferably a thermoplastic resin having a melting point of less than 200°C. Examples of the thermoplastic resin include polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; and the like, and among these, polyolefins are preferred.

[0042] The porous substrate is preferably a microporous membrane containing polyolefin (referred to as a "polyolefin microporous membrane" in the present disclosure). Examples of the polyolefin microporous membrane include polyolefin microporous membranes used in conventional battery separators, and it is preferable to select one having sufficient mechanical properties and ion permeability from these.

[0043] From the viewpoint of exhibiting a shutdown function, the polyolefin microporous membrane is preferably a microporous membrane containing polyethylene, and the polyethylene content is preferably 95% by mass or more based on the total mass of the polyolefin microporous membrane.

[0044] The polyolefin microporous film is preferably a microporous film containing polypropylene, from the viewpoint of having heat resistance such that the film does not easily break when exposed to high temperatures.

[0045] From the viewpoint of having a shutdown function and heat resistance that does not easily break when exposed to high temperatures, the polyolefin microporous film is preferably a polyolefin microporous film containing polyethylene and polypropylene. An example of a polyolefin microporous film containing polyethylene and polypropylene is a microporous film in which polyethylene and polypropylene are mixed in one layer. From the viewpoint of achieving both the shutdown function and heat resistance, the microporous film preferably contains 95% by mass or more of polyethylene and 5% by mass or less of polypropylene. Also, from the viewpoint of achieving both the shutdown function and heat resistance, a polyolefin microporous film having a laminated structure of two or more layers, at least one layer containing polyethylene and at least one layer containing polypropylene, is also preferred.

[0046] The polyolefin contained in the polyolefin microporous membrane is preferably a polyolefin having a weight average molecular weight (Mw) of 100,000 to 5,000,000. When the Mw of the polyolefin is 100,000 or more, the microporous membrane can be imparted with sufficient mechanical properties. On the other hand, when the Mw of the polyolefin is 5,000,000 or less, the microporous membrane has good shutdown properties and is easy to mold.

[0047] Examples of methods for producing a polyolefin microporous membrane include a method in which a molten polyolefin resin is extruded through a T-die to form a sheet, which is crystallized, stretched, and then heat-treated to form a microporous membrane; a method in which a molten polyolefin resin together with a plasticizer such as liquid paraffin is extruded through a T-die, cooled to form a sheet, stretched, the plasticizer is extracted, and then heat-treated to form a microporous membrane; and the like.

[0048] Examples of the porous sheet made of a fibrous material include porous sheets such as nonwoven fabrics and papers made of fibrous materials such as polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; heat-resistant resins such as wholly aromatic polyamide, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, and polyetherimide; and cellulose.

[0049] In the present disclosure, a heat-resistant resin refers to a resin having a melting point of 200° C. or higher, or a resin having no melting point and a decomposition temperature of 200° C. or higher. In other words, a heat-resistant resin in the present disclosure refers to a resin that does not melt or decompose in a temperature range below 200° C.

[0050] The composite porous sheet may be a sheet in which a functional layer is laminated on a porous sheet made of a microporous membrane or a fibrous material. Such a composite porous sheet is preferable from the viewpoint of enabling the functional layer to add further functions. From the viewpoint of imparting heat resistance, for example, the functional layer may be a porous layer made of a heat-resistant resin, or a porous layer made of a heat-resistant resin and an inorganic filler. The heat-resistant resin may be one or more heat-resistant resins selected from wholly aromatic polyamide, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, and polyetherimide. The inorganic filler may be a metal oxide such as alumina; a metal hydroxide such as magnesium hydroxide; or the like. Examples of the composite method include a method of coating a functional layer on a microporous membrane or a porous sheet, a method of bonding a microporous membrane or a porous sheet to a functional layer with an adhesive, and a method of thermocompression bonding a microporous membrane or a porous sheet to a functional layer.

[0051] The surface of the porous substrate may be subjected to various surface treatments in order to improve wettability with the coating liquid for forming the adhesive porous layer, as long as the properties of the porous substrate are not impaired. Examples of the surface treatments include corona treatment, plasma treatment, flame treatment, and ultraviolet irradiation treatment.

[0052] [Characteristics of porous substrate] From the viewpoint of increasing the energy density of the battery, the thickness of the porous substrate is preferably 25 μm or less, more preferably 20 μm or less, and even more preferably 15 μm or less, and from the viewpoint of the production yield of the separator and the production yield of the battery, the thickness is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 8 μm or more.

[0053] From the viewpoint of suppressing short circuits in the battery, the Gurley value (JIS P8117:2009) of the porous substrate is preferably 20 seconds / 100 mL or more, more preferably 25 seconds / 100 mL or more, even more preferably 60 seconds / 100 mL or more, and even more preferably 65 seconds / 100 mL or more. The Gurley value (JIS P8117:2009) of the porous substrate is preferably 220 sec / 100 mL or less, more preferably 200 sec / 100 mL or less, even more preferably 190 sec / 100 mL or less, and even more preferably 150 sec / 100 mL or less, from the viewpoint of ion permeability and of preventing the porous structure from being blocked at the boundary between the porous substrate and the adhesive porous layer when exposed to high temperatures.

[0054] The porosity of the porous substrate is preferably 20% to 60% from the viewpoint of obtaining an appropriate membrane resistance and shutdown function. The porosity ε (%) of the porous substrate is calculated by the following formula. ε={1-Ws / (ds·t)}×100 Here, Ws is the basis weight of the porous substrate (g / m 2 ), ds is the true density of the porous substrate (g / cm 3 ), t is the thickness (μm) of the porous substrate. Basis weight is the mass per unit area.

[0055] The average pore size of the porous substrate is preferably 15 nm to 100 nm from the viewpoint of ion permeability or suppression of short circuit in the battery. The average pore size of the porous substrate is measured using a perm porometer (CFP-1500-A manufactured by PMI) in accordance with ASTM E1294-89.

[0056] [Adhesive porous layer] The adhesive porous layer has a structure in which a large number of micropores are internally connected, and is a layer through which gas or liquid can pass from one surface to the other.

[0057] The adhesive porous layer may be present on only one side of the porous substrate, or on both sides of the porous substrate. When the adhesive porous layer is present on both sides of the porous substrate, the separator is less likely to curl, and handling during battery production is excellent. When the adhesive porous layer is present on only one side of the porous substrate, the ion permeability of the separator is more excellent. In addition, the thickness of the entire separator can be reduced, and a battery with a higher energy density can be produced.

[0058] The adhesive porous layer contains at least a polyvinylidene fluoride resin and a filler. The adhesive porous layer may contain a resin other than the polyvinylidene fluoride resin. The filler contained in the adhesive porous layer may be either an inorganic filler or an organic filler.

[0059] -Polyvinylidene fluoride resin- The content of the polyvinylidene fluoride resin in the adhesive porous layer is preferably 85% by mass to 100% by mass, more preferably 90% by mass to 100% by mass, and even more preferably 95% by mass to 100% by mass, based on the total amount of all resins in the adhesive porous layer.

[0060] When adhesive porous layers are present on both sides of a porous substrate, the type or amount of polyvinylidene fluoride resin contained in one adhesive porous layer may be the same as or different from the type or amount of polyvinylidene fluoride resin contained in the other adhesive porous layer.

[0061] Examples of polyvinylidene fluoride resins include homopolymers of vinylidene fluoride (i.e., polyvinylidene fluoride); copolymers of vinylidene fluoride and halogen-containing monomers such as hexafluoropropylene, tetrafluoroethylene, trifluoroethylene, chlorotrifluoroethylene, vinyl fluoride, and trichloroethylene; copolymers of vinylidene fluoride and other monomers other than halogen-containing monomers; copolymers of vinylidene fluoride, halogen-containing monomers, and other monomers other than halogen-containing monomers; and mixtures thereof. Polyvinylidene fluoride resins may be used alone or in combination of two or more.

[0062] As the polyvinylidene fluoride resin, a copolymer of vinylidene fluoride (VDF) and hexafluoropropylene (HFP) (VDF-HFP copolymer) is preferable from the viewpoint of adhesion to the electrode. In the present disclosure, the VDF-HFP copolymer includes both a copolymer obtained by polymerizing only VDF and HFP, and a copolymer obtained by polymerizing VDF, HFP, and other monomers. By increasing or decreasing the content of HFP units, the crystallinity, heat resistance, and resistance to dissolution in an electrolyte of the VDF-HFP copolymer can be controlled within an appropriate range.

[0063] In the entire polyvinylidene fluoride resin contained in the adhesive porous layer, the proportion of structural units derived from HFP to all structural units is preferably more than 3.5 mol % and 7.0 mol % or less. When the proportion of the HFP-derived structural units in the total structural units of the entire polyvinylidene fluoride resin exceeds 3.5 mol%, the polymer chains of the polyvinylidene fluoride resin are easily mobile, and the polyvinylidene fluoride resin has excellent adhesion to the electrode even when heat-pressed in a state where the polyvinylidene fluoride resin does not swell in the electrolyte or at a relatively low temperature. From this viewpoint, the proportion of the HFP-derived structural units is more preferably more than 4.0 mol%, and even more preferably more than 4.5 mol%. When the proportion of the HFP-derived structural units in the total structural units of the polyvinylidene fluoride resin is 7.0 mol % or less, the resin has excellent resistance to dissolution in an electrolyte. From this viewpoint, the proportion of the HFP-derived structural units is more preferably 6.8 mol % or less, and even more preferably 6.5 mol % or less.

[0064] The polyvinylidene fluoride resin preferably contains a polyvinylidene fluoride resin having a constituent unit derived from a monomer represented by the following formula (1) (referred to as "polyvinylidene fluoride resin (1)" in the present disclosure).

[0065] [ka]

[0066] In formula (1), R 1 , R 2 and R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms, a carboxy group, or a derivative of a carboxy group; X represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene group having 1 to 5 carbon atoms and having a substituent; Y represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms substituted with at least one hydroxy group, an alkyl group having 1 to 5 carbon atoms substituted with at least one carboxy group, or -ROC(=O)-(CH2) n It represents -C(=O)-OH (R represents an alkylene group having 1 to 5 carbon atoms, and n represents an integer of 0 or more).

[0067] In formula (1), R 1 , R 2 and R 3 The halogen atom represented by may be any one of a fluorine atom, a chlorine atom, a bromine atom and an iodine atom, and is preferably a fluorine atom.

[0068] In formula (1), R 1 , R 2 and R 3 Examples of the alkyl group having 1 to 5 carbon atoms represented by R include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, and n-pentyl groups; and branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, and tert-pentyl groups. 1 , R 2 and R 3 As the alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 4 carbon atoms is preferable, and an alkyl group having 1 to 3 carbon atoms is more preferable.

[0069] In formula (1), R 1 , R 2 and R 3 Examples of the derivative of the carboxy group represented by the formula: 4 (R 4 represents an alkyl group. 4Examples of R include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, and n-pentyl groups; and branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, and tert-pentyl groups. 4 As the alkyl group, an alkyl group having 1 to 5 carbon atoms is preferable, an alkyl group having 1 to 4 carbon atoms is more preferable, and an alkyl group having 1 to 3 carbon atoms is further preferable.

[0070] In formula (1), examples of the alkylene group having 1 to 5 carbon atoms represented by X include linear alkylene groups such as methylene, ethylene, n-propylene, n-butylene, and n-pentylene, and branched alkylene groups such as isopropylene, isobutylene, sec-butylene, tert-butylene, isopentylene, neopentylene, and tert-pentylene. The alkylene group having 1 to 5 carbon atoms represented by X is preferably an alkylene group having 1 to 4 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms.

[0071] In formula (1), the substituent in the alkylene group having 1 to 5 carbon atoms represented by X includes, for example, a halogen atom, which may be any of a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the alkylene group having 1 to 5 carbon atoms substituted in X include linear alkylene groups such as a methylene group, an ethylene group, an n-propylene group, an n-butylene group, and an n-pentylene group; and branched alkylene groups such as an isopropylene group, an isobutylene group, a sec-butylene group, a tert-butylene group, an isopentylene group, a neopentylene group, and a tert-pentylene group. The alkylene group having 1 to 5 carbon atoms substituted in X is preferably an alkylene group having 1 to 4 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms.

[0072] In formula (1), examples of the alkyl group having 1 to 5 carbon atoms represented by Y include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, and n-pentyl groups, and branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, and tert-pentyl groups. The alkyl group having 1 to 5 carbon atoms represented by Y is preferably an alkyl group having 1 to 4 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.

[0073] In the formula (1), in the alkyl group having 1 to 5 carbon atoms substituted with at least one hydroxy group represented by Y, examples of the substituted alkyl group having 1 to 5 carbon atoms include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, and n-pentyl; and branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, and tert-pentyl. The substituted alkyl group having 1 to 5 carbon atoms in Y is preferably an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms. The number of hydroxy groups substituted is preferably one or two, more preferably one.

[0074] In the formula (1), examples of the alkyl group having 1 to 5 carbon atoms and substituted with at least one hydroxy group represented by Y include a 2-hydroxyethyl group, a 2-hydroxypropyl group, and a 4-hydroxybutyl group.

[0075] In the formula (1), in the alkyl group having 1 to 5 carbon atoms substituted with at least one carboxy group represented by Y, examples of the substituted alkyl group having 1 to 5 carbon atoms include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, and n-pentyl groups; and branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, and tert-pentyl groups. The substituted alkyl group having 1 to 5 carbon atoms in Y is preferably an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms. The number of substituted carboxy groups is preferably one or two, more preferably one.

[0076] In the formula (1), examples of the alkyl group having 1 to 5 carbon atoms and substituted with at least one carboxy group represented by Y include a 2-carboxyethyl group, a 2-carboxypropyl group, and a 4-carboxybutyl group.

[0077] In formula (1), Y represents -ROC(=O)-(CH2) n In the -C(=O)-OH, R represents an alkylene group having 1 to 5 carbon atoms, and n represents an integer of 0 or more. Examples of R include linear alkylene groups such as methylene, ethylene, n-propylene, n-butylene, and n-pentylene, and branched alkylene groups such as isopropylene, isobutylene, sec-butylene, tert-butylene, isopentylene, neopentylene, and tert-pentylene. R is preferably an alkylene group having 1 to 4 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms. As n, an integer of 0 to 5 is preferable, an integer of 1 to 4 is more preferable, and 2 or 3 is even more preferable. Specific examples of such groups include -(CH2)2-OC(=O)-(CH2)2-C(=O)-OH.

[0078] The monomer represented by formula (1) is, for example, R 1 , R 2 and R 3are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, X is a single bond, and Y is an alkyl group having 1 to 4 carbon atoms or an alkyl group having 1 to 3 carbon atoms substituted with at least one hydroxy group.

[0079] Examples of the monomer represented by formula (1) include acrylic monomers, unsaturated dibasic acids, and monoesters of unsaturated dibasic acids.

[0080] Examples of acrylic monomers include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-carboxyethyl (meth)acrylate, 2-carboxypropyl (meth)acrylate, 4-carboxybutyl (meth)acrylate, butenoic acid, pentenoic acid, hexenoic acid, and (meth)acryloyloxyethyl succinic acid. The term "(meth)acrylic" means that it can mean either "acrylic" or "methacrylic".

[0081] Examples of the unsaturated dibasic acid include unsaturated dicarboxylic acids, more specifically, maleic acid, maleic anhydride, citraconic acid, itaconic acid, and the like.

[0082] Examples of monoesters of unsaturated dibasic acids include monomethyl maleate, monoethyl maleate, monomethyl citraconic acid, monoethyl citraconic acid, monomethyl itaconic acid, and monoethyl itaconic acid. Of these, monomethyl maleate and monomethyl citraconic acid are preferred.

[0083] In the polyvinylidene fluoride resin (1), the proportion of the constituent units derived from the monomer represented by formula (1) in all constituent units is preferably 0.005 mol % or more, more preferably 0.01 mol % or more, and even more preferably 0.02 mol % or more, from the viewpoint of adhesion to electrodes. In the polyvinylidene fluoride resin (1), the proportion of the constituent units derived from the monomer represented by formula (1) in all constituent units is preferably 3.0 mol % or less, more preferably 2.0 mol % or less, and even more preferably 1.0 mol % or less, from the viewpoint of low influence on the active material contained in the electrode.

[0084] The polyvinylidene fluoride resin (1) may contain a constituent unit derived from a monomer other than vinylidene fluoride (VDF) and the monomer represented by formula (1). Examples of the other monomer include halogen-containing monomers such as hexafluoropropylene, tetrafluoroethylene, trifluoroethylene, chlorotrifluoroethylene, vinyl fluoride, and trichloroethylene.

[0085] The polyvinylidene fluoride resin (1) preferably contains a structural unit derived from hexafluoropropylene (HFP). By increasing or decreasing the proportion of HFP in the total polymerization components, the crystallinity, adhesion to electrodes, and resistance to dissolution in an electrolyte can be controlled within appropriate ranges.

[0086] The polyvinylidene fluoride resin (1) is preferably a terpolymer consisting of VDF, HFP, and a monomer represented by formula (1). As the terpolymer, a VDF-HFP-acrylic acid terpolymer is preferable.

[0087] The proportion of the polyvinylidene fluoride resin (1) in the entire polyvinylidene fluoride resin contained in the adhesive porous layer is preferably 20% by mass to 80% by mass, more preferably 30% by mass to 70% by mass, and even more preferably 40% by mass to 60% by mass, from the viewpoint of setting the acid value of the entire polyvinylidene fluoride resin in an appropriate range.

[0088] The acid value (mgKOH / g) of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is preferably less than 3.0, more preferably 2.9 or less, and even more preferably 2.8 or less, from the viewpoint of low influence on the active material contained in the electrode. The acid value (mgKOH / g) of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is preferably 0.5 or more, more preferably 0.8 or more, and even more preferably 1.0 or more, from the viewpoint of adhesion to the electrode.

[0089] The acid value (mgKOH / g) of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is determined by extracting the polyvinylidene fluoride resin contained in the adhesive porous layer and measuring its acid value by potentiometric titration (JIS K1557-5:2007). Alternatively, the acid value (mgKOH / g) of the polyvinylidene fluoride resin used to form the adhesive porous layer is determined by potentiometric titration (JIS K1557-5:2007).

[0090] The weight average molecular weight (Mw) of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is preferably 300,000 or more, more preferably 500,000 or more, even more preferably 650,000 or more, and even more preferably 850,000 or more, from the viewpoint of preventing blockage of the pores in the adhesive porous layer when heat is applied to the adhesive porous layer during battery production. The Mw of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is preferably less than 3 million, more preferably less than 2.5 million, even more preferably less than 2.3 million, and even more preferably less than 2 million, from the viewpoint of adequately softening the polyvinylidene fluoride resin when heat is applied to the adhesive porous layer during battery production, and achieving good adhesion between the adhesive porous layer and the electrode.

[0091] The Mw of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is a polystyrene-equivalent molecular weight measured by gel permeation chromatography (GPC). The polyvinylidene fluoride resin extracted from the adhesive porous layer or the polyvinylidene fluoride resin used to form the adhesive porous layer is used as a sample.

[0092] From the viewpoint of controlling the endothermic peak temperature and exothermic peak temperature in the DSC curve of the polyvinylidene fluoride resin contained in the adhesive porous layer within the desired range, it is preferable that the adhesive porous layer contains polyvinylidene fluoride resin X and polyvinylidene fluoride resin Y described below.

[0093] The total amount of polyvinylidene fluoride resin X and polyvinylidene fluoride resin Y contained in the adhesive porous layer is preferably 85% by mass to 100% by mass, more preferably 90% by mass to 100% by mass, and even more preferably 95% by mass to 100% by mass, based on the entire polyvinylidene fluoride resin contained in the adhesive porous layer.

[0094] -Polyvinylidene fluoride resin X- Polyvinylidene fluoride resin X contains constituent units derived from vinylidene fluoride (VDF) and constituent units derived from hexafluoropropylene (HFP), in which the proportion of constituent units derived from HFP in all constituent units is more than 3.5 mol% and not more than 15 mol%, has a weight average molecular weight (Mw) of 100,000 or more and less than 1,000,000, and has a melting point of 125°C or more and less than 150°C.

[0095] In the polyvinylidene fluoride resin X, the proportion of the HFP-derived structural units in all structural units is more than 3.5 mol%, preferably more than 4.0 mol%, more preferably more than 4.5 mol%, and even more preferably more than 5.0 mol%, from the viewpoint of facilitating movement of the polymer chains of the resin by heat pressing and providing excellent adhesion to electrodes. In the polyvinylidene fluoride resin X, the proportion of the structural units derived from HFP in all structural units is 15 mol % or less, preferably 12 mol % or less, more preferably 10 mol % or less, and even more preferably 8.0 mol % or less, since this has excellent resistance to dissolution in an electrolytic solution.

[0096] The Mw of the polyvinylidene fluoride resin X is 100,000 or more, preferably 150,000 or more, more preferably 200,000 or more, and even more preferably 250,000 or more, from the viewpoint of preventing blockage of the pores of the adhesive porous layer when heat is applied to the adhesive porous layer during the production of the battery. The Mw of the polyvinylidene fluoride resin X is less than 1,000,000, preferably less than 900,000, more preferably less than 600,000, and even more preferably less than 400,000, from the viewpoint that the resin softens when heat is applied to the adhesive porous layer during battery production, and the adhesive porous layer and the electrode are well bonded to each other.

[0097] The Mw of the polyvinylidene fluoride resin X is a molecular weight measured by GPC and converted into polystyrene. The polyvinylidene fluoride resin X used for forming the adhesive porous layer is used as a sample.

[0098] The melting point of the polyvinylidene fluoride resin X is 125°C or higher, preferably 128°C or higher, and more preferably 130°C or higher, from the viewpoint of preventing blockage of the pores in the adhesive porous layer when heat is applied to the adhesive porous layer during battery production. The melting point of the polyvinylidene fluoride resin X is less than 150°C, preferably less than 145°C, and more preferably less than 140°C, from the viewpoint of softening the resin when heat is applied to the adhesive porous layer during battery production, and thereby achieving good adhesion between the adhesive porous layer and the electrodes.

[0099] The melting point of polyvinylidene fluoride resin X is determined from a DSC curve obtained by performing differential scanning calorimetry (DSC). The polyvinylidene fluoride resin X used to form the adhesive porous layer is used as a sample. The sample is placed in an aluminum sample pan and set in a measuring device, and the following three steps are carried out consecutively in a nitrogen atmosphere to perform a thermal analysis of the sample. Step 1: Heat from 30°C to 200°C at a rate of 5°C / min. Step 2: Decrease the temperature from 200°C to 30°C at a rate of 5°C / min. Step 3: Increase the temperature from 30°C to 200°C at a rate of 5°C / min. The temperature of the endothermic peak that appears on the DSC curve in step 3 above is taken as the melting point of polyvinylidene fluoride resin X. When there are multiple endothermic peaks, the temperature of the endothermic peak on the lowest temperature side is taken as the melting point.

[0100] A preferred embodiment of the polyvinylidene fluoride resin X is one in which the proportion of HFP-derived structural units in all structural units is more than 5.0 mol % and 15 mol % or less, the Mw is 300,000 or more and less than 1,000,000, and the melting point is 125°C or more and less than 140°C.

[0101] -Polyvinylidene fluoride resin Y- The polyvinylidene fluoride resin Y contains structural units derived from vinylidene fluoride (VDF) and may contain structural units derived from hexafluoropropylene (HFP), in which the proportion of structural units derived from HFP to all structural units is 0 mol% or more and 3.5 mol% or less, the weight average molecular weight (Mw) is 1 million or more and less than 3 million, and the melting point is 150°C or more and less than 180°C.

[0102] In the polyvinylidene fluoride resin Y, the proportion of HFP-derived structural units in all structural units is 3.5 mol % or less, preferably 3.0 mol % or less, more preferably 2.5 mol % or less, and even more preferably 2.0 mol % or less, since the polyvinylidene fluoride resin Y has excellent resistance to dissolution in an electrolyte solution. In the polyvinylidene fluoride resin Y, the proportion of HFP-derived structural units in all structural units is preferably more than 0 mol%, more preferably 0.2 mol% or more, even more preferably 0.5 mol% or more, and even more preferably 0.7 mol% or more, from the viewpoint of facilitating movement of the polymer chains of the resin by heat pressing and providing excellent adhesion to electrodes.

[0103] The Mw of the polyvinylidene fluoride resin Y is 1,000,000 or more, preferably 1,200,000 or more, more preferably 1,500,000 or more, and even more preferably 1,600,000 or more, from the viewpoint of preventing blockage of the pores in the adhesive porous layer when heat is applied to the adhesive porous layer during battery production. The Mw of the polyvinylidene fluoride resin Y is less than 3 million, preferably less than 2.5 million, more preferably less than 2.3 million, and even more preferably less than 2 million, from the viewpoint of adequately softening the resin when heat is applied to the adhesive porous layer during battery production, and of providing good adhesion between the adhesive porous layer and the electrode.

[0104] The Mw of the polyvinylidene fluoride resin Y is a molecular weight measured by GPC and converted into polystyrene. The polyvinylidene fluoride resin Y used for forming the adhesive porous layer is used as a sample.

[0105] The melting point of the polyvinylidene fluoride resin Y is 150°C or higher, preferably 155°C or higher, and more preferably 160°C or higher, from the viewpoint of preventing blockage of the pores in the adhesive porous layer when heat is applied to the adhesive porous layer during battery production. The melting point of the polyvinylidene fluoride resin Y is less than 180°C, preferably less than 175°C, and more preferably less than 170°C, from the viewpoint of appropriately softening the resin when heat is applied to the adhesive porous layer during battery production, and achieving good adhesion between the adhesive porous layer and the electrodes.

[0106] The melting point of polyvinylidene fluoride resin Y is determined from a DSC curve obtained by performing differential scanning calorimetry (DSC). The polyvinylidene fluoride resin Y used to form the adhesive porous layer is used as a sample. The sample is placed in an aluminum sample pan and set in a measuring device, and the following three steps are carried out consecutively in a nitrogen atmosphere to perform thermal analysis of the sample. Step 1: Heat from 30°C to 200°C at a rate of 5°C / min. Step 2: Decrease the temperature from 200°C to 30°C at a rate of 5°C / min. Step 3: Increase the temperature from 30°C to 200°C at a rate of 5°C / min. The temperature of the endothermic peak that appears on the DSC curve in step 3 above is taken as the melting point of polyvinylidene fluoride resin Y. When there are multiple endothermic peaks, the temperature of the endothermic peak on the lowest temperature side is taken as the melting point.

[0107] A preferred embodiment of the polyvinylidene fluoride resin Y is one in which the proportion of HFP-derived structural units in all structural units is 0 mol% or more (preferably more than 0 mol%, more preferably 0.2 mol% or more) and 2.0 mol% or less, the Mw is 1.5 million or more and less than 2 million, and the melting point is 150°C or more and less than 170°C.

[0108] The polyvinylidene fluoride resin Y is preferably a polyvinylidene fluoride resin having a constituent unit derived from the monomer represented by the formula (1). That is, the polyvinylidene fluoride resin Y is preferably a polyvinylidene fluoride resin (1). That is, the polyvinylidene fluoride resin Y is preferably a terpolymer consisting of VDF, HFP, and the monomer represented by the formula (1). As the terpolymer, a VDF-HFP-acrylic acid terpolymer is preferable.

[0109] In the polyvinylidene fluoride resin Y, the proportion of the constituent units derived from the monomer represented by formula (1) in all constituent units is preferably 0.05 mol % or more, more preferably 0.08 mol % or more, and even more preferably 0.1 mol % or more, from the viewpoint of adhesion to electrodes. In the polyvinylidene fluoride resin Y, the proportion of the constituent units derived from the monomer represented by formula (1) in all constituent units is preferably 5.0 mol % or less, more preferably 4.0 mol % or less, and even more preferably 3.0 mol % or less, from the viewpoint of low influence on the active material contained in the electrode.

[0110] From the viewpoint of controlling the endothermic peak temperature and exothermic peak temperature in a DSC curve of the polyvinylidene fluoride resin contained in the adhesive porous layer within a desired range, the mass ratio of polyvinylidene fluoride resin X:polyvinylidene fluoride resin Y contained in the adhesive porous layer is preferably polyvinylidene fluoride resin X:polyvinylidene fluoride resin Y=20:80 to 80:20, more preferably 30:70 to 70:30, even more preferably 35:65 to 65:35, and even more preferably 40:60 to 60:40.

[0111] The difference between the melting point of the polyvinylidene fluoride resin X and the melting point of the polyvinylidene fluoride resin Y contained in the adhesive porous layer is preferably 25° C. or more, more preferably 27° C. or more, even more preferably 28° C. or more, and even more preferably 29° C. or more, from the viewpoint of achieving both adhesion to the electrode by dry heat press and wet heat press and a high capacity retention rate of the battery even after exposure to high temperatures. From the viewpoint of forming a highly uniform porous structure in the adhesive porous layer, the difference between the melting point of the polyvinylidene fluoride resin X and the melting point of the polyvinylidene fluoride resin Y contained in the adhesive porous layer is preferably less than 55°C, more preferably less than 50°C, even more preferably less than 45°C, and even more preferably less than 40°C.

[0112] -Other resins- The adhesive porous layer may contain other resins besides polyvinylidene fluoride resins. Examples of other resins include acrylic resins, fluorine-based rubbers, styrene-butadiene copolymers, homopolymers or copolymers of vinyl nitrile compounds (such as acrylonitrile and methacrylonitrile), carboxymethyl cellulose, hydroxyalkyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, polyethers (such as polyethylene oxide and polypropylene oxide), polyamides, wholly aromatic polyamides, polyimides, polyamideimides, polysulfones, polyketones, polyether ketones, polyether sulfones, polyetherimides, and mixtures thereof.

[0113] The content of resins other than polyvinylidene fluoride resins in the adhesive porous layer is preferably 0% by mass to 15% by mass, more preferably 0% by mass to 10% by mass, and even more preferably 0% by mass to 5% by mass, relative to the total amount of all resins in the adhesive porous layer.

[0114] -Inorganic filler- Examples of inorganic fillers include metal hydroxide particles, metal sulfate particles, metal oxide particles, metal carbonate particles, metal nitride particles, metal fluoride particles, and clay mineral particles. The inorganic fillers may be used alone or in combination of two or more.

[0115] Examples of metal hydroxides constituting the metal hydroxide particles include magnesium hydroxide, aluminum hydroxide, calcium hydroxide, chromium hydroxide, zirconium hydroxide, cerium hydroxide, and nickel hydroxide.

[0116] Examples of metal sulfates constituting the metal sulfate particles include barium sulfate, strontium sulfate, calcium sulfate, calcium sulfate dihydrate, alum, and jarosite.

[0117] Examples of metal oxides that constitute the metal oxide particles include barium titanate (BaTiO3), magnesium oxide, alumina (Al2O3), boehmite (alumina monohydrate), titania (TiO2), silica (SiO2), zirconia (ZrO2), and zinc oxide.

[0118] Examples of metal carbonates constituting the metal carbonate particles include calcium carbonate and magnesium carbonate.

[0119] Examples of metal nitrides constituting the metal nitride particles include magnesium nitride, aluminum nitride, calcium nitride, and titanium nitride.

[0120] Examples of metal fluorides constituting the metal fluoride particles include magnesium fluoride and calcium fluoride.

[0121] Examples of clay minerals constituting the clay mineral particles include calcium silicate, calcium phosphate, apatite, and talc.

[0122] The inorganic filler may be an inorganic filler whose surface has been modified with a silane coupling agent or the like.

[0123] The inorganic filler is preferably at least one type selected from the group consisting of metal hydroxide particles, metal sulfate particles, and barium titanate particles, from the viewpoint of being less likely to decompose the electrolytic solution or electrolyte and therefore less likely to cause gas generation.

[0124] From the viewpoint of suppressing gas generation, the total amount of metal hydroxide particles, metal sulfate particles, and barium titanate particles in the entire inorganic filler contained in the adhesive porous layer is preferably 80 mass% or more, more preferably 85 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and most preferably 100 mass%.

[0125] When adhesive porous layers are present on both sides of the porous substrate, the type of inorganic filler contained in one adhesive porous layer may be the same as or different from the type of inorganic filler contained in the other adhesive porous layer.

[0126] The particle shape of the inorganic filler is not limited, and may be any of spherical, plate-like, needle-like, and irregular shapes. From the viewpoint of suppressing short circuits in the battery or forming a highly uniform adhesive porous layer, the inorganic filler is preferably a spherical or plate-like particle.

[0127] The average primary particle size of the entire inorganic filler contained in the adhesive porous layer is preferably 1.5 μm or less, more preferably 1.2 μm or less, and even more preferably 1.0 μm or less, from the viewpoint of improving the heat resistance of the adhesive porous layer. The average primary particle size of all the inorganic fillers contained in the adhesive porous layer is preferably 0.01 μm or more, more preferably 0.1 μm or more, and even more preferably 0.5 μm or more, from the viewpoint of suppressing aggregation between the inorganic fillers and forming a highly uniform adhesive porous layer.

[0128] The average primary particle size of all inorganic fillers contained in the adhesive porous layer is obtained by measuring the long diameter of 100 inorganic fillers randomly selected in observation with a scanning electron microscope (SEM) and averaging the long diameters of the 100. The sample provided for SEM observation is an inorganic filler that is a material forming the adhesive porous layer, or an inorganic filler taken out from the adhesive porous layer of a separator. There is no limitation on the method for taking out the inorganic filler from the adhesive porous layer of a separator. The method includes, for example, a method in which the adhesive porous layer peeled off from the separator is immersed in an organic solvent that dissolves the resin to take out the inorganic filler with the organic solvent; a method in which the adhesive porous layer peeled off from the separator is heated to about 800°C to eliminate the resin and take out the inorganic filler; and the like.

[0129] When adhesive porous layers are present on both sides of the porous substrate, the average primary particle size of the inorganic filler in one adhesive porous layer may be the same as or different from the average primary particle size of the inorganic filler in the other adhesive porous layer.

[0130] From the viewpoint of the heat resistance of the separator, the proportion of the inorganic filler in the solid volume of the adhesive porous layer is preferably 30% by volume or more, more preferably 35% by volume or more, even more preferably 40% by volume or more, and even more preferably 45% by volume or more. The proportion of inorganic filler in the solid volume of the adhesive porous layer is preferably 67% by volume or less, more preferably 66% by volume or less, even more preferably 65% ​​by volume or less, and even more preferably 63% by volume or less, from the viewpoint of preventing the adhesive porous layer from peeling off from the porous substrate.

[0131] The proportion V (vol %) of the inorganic filler in the solid volume of the adhesive porous layer is calculated by the following formula. V={(Xa / Da) / (Xa / Da+Xb / Db+Xc / Dc+…+Xn / Dn)}×100 Here, among the constituent materials of the adhesive porous layer, the inorganic filler is a, the other constituent materials are b, c, ..., n, the masses of the constituent materials contained in a predetermined area of ​​the adhesive porous layer are Xa, Xb, Xc, ..., Xn (g), and the true densities of the constituent materials are Da, Db, Dc, ..., Dn (g / cm 3 ). Xa etc. substituted into the above formula is the mass (g) of the constituent material used to form an adhesive porous layer of a specified area, or the mass (g) of the constituent material removed from an adhesive porous layer of a specified area. The Da and other values ​​substituted in the above formula are the true densities (g / cm) of the constituent materials used to form the adhesive porous layer. 3 ), or the true density (g / cm 3 ).

[0132] When adhesive porous layers are present on both sides of a porous substrate, the volume proportion of inorganic filler in the solid volume of one adhesive porous layer may be the same as or different from the volume proportion of inorganic filler in the solid volume of the other adhesive porous layer.

[0133] From the viewpoint of the heat resistance of the separator, the proportion of the inorganic filler in the total amount of filler contained in the adhesive porous layer (i.e., the total amount of inorganic filler and organic filler) is preferably 90 mass % or more, more preferably 95 mass % or more, and even more preferably 100 mass %.

[0134] -Organic filler- Examples of organic fillers include particles made of crosslinked polymers such as crosslinked poly(meth)acrylic acid, crosslinked poly(meth)acrylic acid ester, crosslinked polysilicone, crosslinked polystyrene, crosslinked polydivinylbenzene, styrene-divinylbenzene copolymer crosslinked product, polyimide, melamine resin, phenol resin, and benzoguanamine-formaldehyde condensate; particles made of heat-resistant polymers such as polysulfone, polyacrylonitrile, aramid, polyacetal, and thermoplastic polyimide; etc. The term "(meth)acrylic" means that it can mean either "acrylic" or "methacrylic". The resin constituting the organic filler may be a mixture, modified product, derivative, copolymer (random copolymer, alternating copolymer, block copolymer, graft copolymer) or crosslinked product of the above-exemplified materials.

[0135] The organic fillers may be used alone or in combination of two or more.

[0136] From the viewpoint of the heat resistance of the separator, the proportion of the total filler in the solid volume of the adhesive porous layer (i.e., the combined proportion of inorganic filler and organic filler) is preferably 30 volume % or more, more preferably 35 volume % or more, even more preferably 40 volume % or more, and even more preferably 45 volume % or more. The proportion of the total filler in the solid volume of the adhesive porous layer is preferably 90% by volume or less, more preferably 85% by volume or less, even more preferably 80% by volume or less, and even more preferably 75% by volume or less, from the viewpoint of preventing the adhesive porous layer from peeling off from the porous substrate.

[0137] The proportion V (vol %) of the entire filler in the solid volume of the adhesive porous layer is calculated by the following formula. V={(Xa / Da) / (Xa / Da+Xb / Db+Xc / Dc+…+Xn / Dn)}×100 Here, among the constituent materials of the adhesive porous layer, a is the filler, b, c, ..., n are the other constituent materials, the masses of the constituent materials contained in a given area of ​​the adhesive porous layer are Xa, Xb, Xc, ..., Xn (g), and the true densities of the constituent materials are Da, Db, Dc, ..., Dn (g / cm 3 ). Xa etc. substituted into the above formula is the mass (g) of the constituent material used to form an adhesive porous layer of a specified area, or the mass (g) of the constituent material removed from an adhesive porous layer of a specified area. The Da and other values ​​substituted in the above formula are the true densities (g / cm) of the constituent materials used to form the adhesive porous layer. 3 ), or the true density (g / cm 3 ).

[0138] -Other ingredients- The adhesive porous layer may contain additives such as a dispersant such as a surfactant, a wetting agent, an antifoaming agent, and a pH adjuster. The dispersant is added to the coating liquid for forming the adhesive porous layer for the purpose of improving dispersibility, coatability, or storage stability. The wetting agent, antifoaming agent, and pH adjuster are added to the coating liquid for forming the adhesive porous layer for the purpose of improving compatibility with the porous substrate, suppressing air entrapment in the coating liquid, or adjusting the pH, for example.

[0139] [Characteristics of adhesive porous layer] From the viewpoint of adhesion to the electrode or handling properties, the thickness of the adhesive porous layer is preferably 0.5 μm or more on one side, more preferably 1.0 μm or more on one side, and even more preferably 1.5 μm or more on one side; from the viewpoint of ion permeability and battery energy density, the thickness is preferably 10.0 μm or less on one side, more preferably 8.0 μm or less on one side, and even more preferably 6.0 μm or less on one side.

[0140] When the adhesive porous layer is present on both sides of the porous substrate, the thickness of the adhesive porous layer, calculated as the total thickness of both sides, is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 3.0 μm or more, and is preferably 20.0 μm or less, more preferably 16.0 μm or less, and even more preferably 12.0 μm or less.

[0141] When adhesive porous layers are present on both sides of a porous substrate, the smaller the difference (μm) between the thickness of one adhesive porous layer and the thickness of the other adhesive porous layer, the better, and it is preferable that the difference is 20% or less of the total thickness (μm) of both sides.

[0142] The mass per unit area of ​​the adhesive porous layer is set to 1.0 g / m in total for both sides from the viewpoint of adhesion to the electrode or handling, whether the adhesive porous layer is on one side or both sides of the porous substrate. 2 More than 2.0 g / m is preferable. 2 More preferably, 3.0 g / m or more 2 More preferably, the total of both surfaces is 30.0 g / m from the viewpoint of ion permeability and the energy density of the battery. 2 Less than 20.0 g / m is preferred. 2 Less than 10.0 g / m is more preferable. 2 The following is even more preferred:

[0143] When the adhesive porous layer is present on both sides of the porous substrate, the difference between the mass per unit area of ​​one adhesive porous layer and the mass per unit area of ​​the other adhesive porous layer (g / m 2 ) is preferably as small as possible from the viewpoint of suppressing curling of the separator or improving the cycle characteristics of the battery, and the total amount (g / m 2 ) is preferably 20% or less.

[0144] The porosity of the adhesive porous layer is preferably 30% or more, more preferably 35% or more, and even more preferably 40% or more from the viewpoint of ion permeability, and is preferably 70% or less, more preferably 65% ​​or less, and even more preferably 60% or less from the viewpoint of the mechanical strength of the adhesive porous layer and adhesion to the electrode. The porosity ε (%) of the adhesive porous layer is calculated by the following formula.

[0145]

number

[0146] The average pore size of the adhesive porous layer is preferably 10 nm to 200 nm. When the average pore size is 10 nm or more, when the adhesive porous layer is impregnated with an electrolyte solution, the pores are less likely to be blocked even if the resin contained in the adhesive porous layer swells. When the average pore size is 200 nm or less, the uniformity of ion migration in the adhesive porous layer is high, and the cycle characteristics and load characteristics of the battery are excellent.

[0147] The average pore size (nm) of the adhesive porous layer is calculated by the following formula, assuming that all pores are cylindrical. d=4V / S In the formula, d is the average pore size (diameter) of the adhesive porous layer, and V is the average pore size (diameter) of the adhesive porous layer per 1 m 2 S is the pore volume per m of adhesive porous layer. 2 It represents the pore surface area per unit area. Adhesive porous layer 1m 2 The pore volume V per unit area is calculated from the porosity of the adhesive porous layer. Adhesive porous layer 1m 2 The surface area S of each pore is calculated by the following method. First, the specific surface area (m 2 / g) and the specific surface area of ​​the separator (m 2 / g) is calculated from the amount of nitrogen gas adsorption by applying the BET equation to the nitrogen gas adsorption method. 2 / g) for each basis weight (g / m 2 ) and multiply each 1m 2 The pore surface area per square meter of the porous substrate is then calculated. 2 The pore surface area per 1 m of separator 2 The area of ​​the adhesive porous layer per square meter is calculated by subtracting the area of ​​the pores per square meter. 2 The pore surface area S per unit area is calculated. The basis weight is the mass per unit area.

[0148] [Separator characteristics] From the viewpoint of the mechanical strength of the separator, the thickness of the separator is preferably 8 μm or more, more preferably 10 μm or more, and even more preferably 12 μm or more, and from the viewpoint of the energy density of the battery, the thickness is preferably 25 μm or less, more preferably 22 μm or less, and even more preferably 20 μm or less.

[0149] From the viewpoint of the load characteristics of the battery, the membrane resistance of the separator is set to 1 Ω cm 2 ~10Ω cm 2 The membrane resistance of the separator is the resistance value when the separator is impregnated with an electrolytic solution, and is a value measured by an AC method at a temperature of 20°C using 1 mol / L LiBF4-propylene carbonate:ethylene carbonate (mass ratio 1:1) as the electrolytic solution. The lower the membrane resistance of the separator, the better the ion permeability of the separator.

[0150] [Separator manufacturing method] The separator of the present disclosure can be manufactured, for example, by forming an adhesive porous layer on a porous substrate by a wet coating method or a dry coating method. In the present disclosure, the wet coating method is a method in which a coating layer is solidified in a coagulating liquid, and the dry coating method is a method in which a coating layer is dried and solidified. An embodiment example of the wet coating method will be described below.

[0151] The wet coating method is a method in which a coating liquid containing a polyvinylidene fluoride resin and a filler is applied onto a porous substrate, the substrate is immersed in a coagulating liquid to solidify the coating layer, and the substrate is then removed from the coagulating liquid, washed with water, and dried.

[0152] The coating liquid for forming the adhesive porous layer is prepared by dissolving or dispersing the polyvinylidene fluoride resin and the filler in a solvent. If necessary, other components than the polyvinylidene fluoride resin and the filler are dissolved or dispersed in the coating liquid.

[0153] The solvent used in preparing the coating liquid includes a solvent that dissolves polyvinylidene fluoride resin (hereinafter, also referred to as a "good solvent.") Examples of the good solvent include polar amide solvents such as N-methylpyrrolidone, dimethylacetamide, and dimethylformamide.

[0154] The solvent used in preparing the coating liquid may contain a phase separation agent that induces phase separation from the viewpoint of forming a porous layer having a good porous structure. Therefore, the solvent used in preparing the coating liquid may be a mixed solvent of a good solvent and a phase separation agent. It is preferable that the phase separation agent is mixed with the good solvent in an amount within a range that ensures a viscosity suitable for coating. Examples of the phase separation agent include water, methanol, ethanol, propyl alcohol, butyl alcohol, butanediol, ethylene glycol, propylene glycol, and tripropylene glycol.

[0155] When the solvent used to prepare the coating liquid is a mixed solvent of a good solvent and a phase separation agent, from the viewpoint of forming a good porous structure, the mixed solvent preferably contains 60 mass % or more of the good solvent and 5 mass % to 40 mass % of the phase separation agent.

[0156] The resin concentration in the coating liquid is preferably 1% by mass to 20% by mass from the viewpoint of forming a good porous structure, and the filler concentration in the coating liquid is preferably 0.5% by mass to 50% by mass from the viewpoint of forming a good porous structure.

[0157] The coating liquid may contain a dispersant such as a surfactant, a wetting agent, an antifoaming agent, a pH adjuster, etc. These additives may remain in the adhesive porous layer as long as they are electrochemically stable within the range of use of the nonaqueous secondary battery and do not inhibit the reaction within the battery.

[0158] Examples of a means for applying the coating liquid to the porous substrate include a Mayer bar, a die coater, a reverse roll coater, a roll coater, a gravure coater, etc. When forming an adhesive porous layer on both sides of the porous substrate, it is preferable from the viewpoint of productivity to apply the coating liquid to both sides of the porous substrate simultaneously.

[0159] The coating layer is solidified by immersing the porous substrate on which the coating layer is formed in a coagulation liquid to induce phase separation in the coating layer while solidifying the polyvinylidene fluoride resin, thereby obtaining a laminate consisting of the porous substrate and the adhesive porous layer.

[0160] The solidification liquid generally contains the good solvent and phase separation agent used in preparing the coating liquid, and water. The mixing ratio of the good solvent and the phase separation agent is preferably the same as the mixing ratio of the mixed solvent used in preparing the coating liquid from the viewpoint of productivity. The content of water in the solidification liquid is preferably 40% by mass to 90% by mass from the viewpoint of forming a porous structure and productivity. The temperature of the solidification liquid is, for example, 20°C to 50°C.

[0161] After the coating layer is solidified in the coagulating liquid, the laminate is lifted out of the coagulating liquid and washed with water. The coagulating liquid is removed from the laminate by washing with water. Furthermore, water is removed from the laminate by drying. The washing with water is performed, for example, by conveying the laminate in a water bath. The drying is performed, for example, by conveying the laminate in a high-temperature environment, by blowing air on the laminate, or by bringing the laminate into contact with a heat roll. The drying temperature is preferably 40°C to 80°C.

[0162] The separator of the present disclosure may also be manufactured by a dry coating method, which is a method in which a coating liquid is applied to a porous substrate, and the coating layer is dried to volatilize and remove the solvent, thereby forming an adhesive porous layer on the porous substrate.

[0163] The separator of the present disclosure can also be manufactured by a method in which the adhesive porous layer is prepared as an independent sheet, the adhesive porous layer is laminated on a porous substrate, and the layers are combined by thermocompression bonding or an adhesive. Examples of a method for preparing the adhesive porous layer as an independent sheet include a method in which the adhesive porous layer is formed on a release sheet by applying the above-mentioned wet coating method or dry coating method.

[0164] <Non-aqueous secondary battery> The nonaqueous secondary battery of the present disclosure is a nonaqueous secondary battery that obtains electromotive force by doping and dedoping lithium ions, and includes a positive electrode, a negative electrode, and the separator for a nonaqueous secondary battery of the present disclosure. Doping means occlusion, support, adsorption, or insertion, and refers to the phenomenon in which lithium ions enter the active material of an electrode such as a positive electrode.

[0165] The nonaqueous secondary battery of the present disclosure has a structure in which, for example, a battery element in which a negative electrode and a positive electrode face each other with a separator interposed therebetween is enclosed in an exterior material together with an electrolyte solution. The nonaqueous secondary battery of the present disclosure is suitable for nonaqueous electrolyte secondary batteries, particularly lithium ion secondary batteries.

[0166] Hereinafter, examples of the positive electrode, negative electrode, electrolyte, and exterior material included in the nonaqueous secondary battery of the present disclosure will be described.

[0167] An example of the positive electrode is a structure in which an active material layer containing a positive electrode active material and a binder resin is formed on a current collector. The active material layer may further contain a conductive additive. Examples of the positive electrode active material include lithium-containing transition metal oxides, specifically LiCoO2, LiNiO2, LiMn 1 / 2 Ni 1 / 2 O2, LiCo 1 / 3 Mn 1 / 3 Ni 1 / 3 O2, LiMn2O4, LiFePO4, LiCo 1 / 2 Ni 1 / 2 O2, LiAl 1 / 4 Ni 3 / 4Examples of the binder resin include polyvinylidene fluoride resin, styrene-butadiene copolymer, etc. Examples of the conductive assistant include carbon materials such as acetylene black, ketjen black, graphite powder, etc. Examples of the current collector include aluminum foil, titanium foil, stainless steel foil, etc., having a thickness of 5 μm to 20 μm.

[0168] An example of the negative electrode is a structure in which an active material layer containing a negative electrode active material and a binder resin is formed on a current collector. The active material layer may further contain a conductive assistant. The negative electrode active material may be a material capable of electrochemically absorbing lithium ions, specifically, for example, a carbon material; an alloy of lithium with silicon, tin, aluminum, or the like; Wood's alloy; and the like. The binder resin may be, for example, a polyvinylidene fluoride resin, a styrene-butadiene copolymer, and the like. The conductive assistant may be, for example, a carbon material such as acetylene black, ketjen black, graphite powder, or ultrafine carbon fiber. The current collector may be, for example, a copper foil, a nickel foil, a stainless steel foil, or the like having a thickness of 5 μm to 20 μm. In addition, instead of the above-mentioned negative electrode, a metallic lithium foil may be used as the negative electrode.

[0169] The electrolyte is a solution in which a lithium salt is dissolved in a non-aqueous solvent. Examples of the lithium salt include LiPF6, LiBF4, and LiClO4. Examples of the non-aqueous solvent include cyclic carbonates such as ethylene carbonate, propylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and fluorine-substituted derivatives thereof; and cyclic esters such as γ-butyrolactone and γ-valerolactone; which may be used alone or in combination. The electrolyte is preferably a solution in which a cyclic carbonate and a chain carbonate are mixed in a mass ratio (cyclic carbonate:chain carbonate) of 20:80 to 40:60, and a lithium salt is dissolved in the range of 0.5 mol / L to 1.5 mol / L.

[0170] Examples of the exterior material include a metal can, an aluminum laminate film pack, etc. The shape of the battery may be rectangular, cylindrical, coin-shaped, etc., and the separator of the present disclosure is suitable for any shape.

[0171] The nonaqueous secondary battery of the present disclosure can be produced by producing a laminate in which the separator of the present disclosure is disposed between a positive electrode and a negative electrode, and then using this laminate by, for example, any of the following methods (1) to (3).

[0172] (1) The laminate is dry heat pressed to bond the electrodes and separator, and then housed in an exterior material (e.g., an aluminum laminate film pack; the same applies below). The electrolyte is injected into the exterior material, and a vacuum is created inside the exterior material. Then, the laminate is further wet heat pressed on top of the exterior material to bond the electrodes and separator and seal the exterior material.

[0173] (2) The laminate is placed in an exterior packaging material, an electrolyte is injected therein, and a vacuum is created inside the exterior packaging material. The laminate is then wet heat pressed onto the exterior packaging material to bond the electrodes and separator together and seal the exterior packaging material.

[0174] (3) The laminate is dry heat pressed to bond the electrodes and separator, and then housed in an exterior packaging. An electrolyte is injected into the exterior packaging, and a vacuum is created inside the exterior packaging, after which the exterior packaging is sealed.

[0175] The conditions for the wet heat press in the above manufacturing method are preferably a press temperature of 70°C to 110°C and a press pressure of 0.5 MPa to 2 MPa. The conditions for the dry heat press in the above manufacturing method are preferably a press temperature of 20°C to 100°C and a press pressure of 0.5 MPa to 9 MPa. The press time is preferably adjusted according to the press temperature and press pressure, for example, within the range of 0.5 minutes to 60 minutes.

[0176] When manufacturing a laminate in which a separator is disposed between a positive electrode and a negative electrode, the method of disposing the separator between the positive electrode and the negative electrode may be a method of stacking at least one layer of a positive electrode, a separator, and a negative electrode in this order (a so-called stack method), or a method of stacking a positive electrode, a separator, a negative electrode, and a separator in this order and winding them in the length direction. EXAMPLES

[0177] The separator and nonaqueous secondary battery of the present disclosure will be described in more detail below with reference to examples. The materials, amounts, ratios, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the separator and nonaqueous secondary battery of the present disclosure should not be interpreted as being limited by the specific examples shown below.

[0178] In the following description, syntheses, treatments, manufactures, etc. were carried out at room temperature (25° C.±3° C.) unless otherwise specified.

[0179] <Measurement and evaluation methods> The measurement and evaluation methods applied in the examples and comparative examples are as follows.

[0180] [Thickness of polyethylene microporous membrane] The thickness (μm) of the polyethylene microporous membrane was measured at 20 points within a 10 cm square using a contact thickness meter (Mitutoyo Corporation, LITEMATIC VL-50S) and the average was calculated. A cylindrical terminal with a diameter of 5 mm was used as the measurement terminal, and it was adjusted so that a load of 7 g was applied during the measurement.

[0181] [Porosity of polyethylene microporous membrane] The porosity ε (%) of the polyethylene microporous membrane was calculated by the following formula. ε={1-Ws / (ds·t)}×100 Here, Ws is the basis weight of the polyethylene microporous membrane (g / m 2 ), ds is the true density of the polyethylene microporous membrane (g / cm 3 ), and t is the thickness of the polyethylene microporous membrane (μm).

[0182] [Gurley value of polyethylene microporous membrane and separator] The Gurley values ​​(sec / 100 mL) of the polyethylene microporous membrane and the separator were measured using a Gurley densometer (Toyo Seiki Co., Ltd., G-B2C) in accordance with JIS P8117:2009.

[0183] [Analysis of structural units of polyvinylidene fluoride resin] The polyvinylidene fluoride resin used for forming the adhesive porous layer was used as a sample. 20 mg of polyvinylidene fluoride resin was dissolved in 0.6 mL of deuterated dimethyl sulfoxide at 100°C. 19 The F-NMR spectrum was measured. From the obtained NMR spectrum, the proportion (mol %) of the constitutional unit derived from HFP and the proportion (mol %) of the constitutional unit derived from the monomer represented by formula (1) were determined.

[0184] [Weight average molecular weight (Mw) of polyvinylidene fluoride resin] The polyvinylidene fluoride resin used to form the adhesive porous layer was used as a sample to measure the molecular weight by GPC. The molecular weight measurement by GPC was performed using a GPC device GPC-900 manufactured by JASCO Corporation, two TSKgel SUPER AWM-H columns manufactured by Tosoh Corporation, and N,N-dimethylformamide as the solvent at a temperature of 40°C and a flow rate of 0.6 mL / min to obtain the molecular weight in terms of polystyrene.

[0185] [Melting point of polyvinylidene fluoride resin] The polyvinylidene fluoride resin used for forming the adhesive porous layer was used as a sample, and subjected to differential scanning calorimetry to determine the melting point. The measuring device used was a product name: DSC Q20 (TA Instruments).

[0186] [Acid value of polyvinylidene fluoride resin] The polyvinylidene fluoride resin used in forming the adhesive porous layer was used as a sample, and the acid value (mgKOH / g) was measured by potentiometric titration (JIS K1557-5:2007).

[0187] [Average primary particle size of inorganic filler] The inorganic filler used in forming the adhesive porous layer was used as a sample and observed with an SEM to determine the average primary particle size.

[0188] [Volume ratio of inorganic filler] The proportion V (vol %) of the inorganic filler in the solid volume of the adhesive porous layer was calculated by the following formula. V={(Xa / Da) / (Xa / Da+Xb / Db+Xc / Dc+…+Xn / Dn)}×100 Here, among the constituent materials of the adhesive porous layer, the inorganic filler is a, the other constituent materials are b, c, ..., n, the masses of the constituent materials contained in a predetermined area of ​​the adhesive porous layer are Xa, Xb, Xc, ..., Xn (g), and the true densities of the constituent materials are Da, Db, Dc, ..., Dn (g / cm 3 ) Xa, etc. substituted in the above formula are the mass (g) of the constituent material used to form the adhesive porous layer of a given area. Da, etc. substituted in the above formula are the true density (g / cm 3 ).

[0189] [Differential scanning calorimetry of polyvinylidene fluoride resin contained in adhesive porous layer] In each of the examples and comparative examples, the adhesive porous layers were formed by applying equal amounts of the same coating liquid to both sides of the porous substrate, and it was assumed that the adhesive porous layers on both sides had the same thermal properties. One of the adhesive porous layers was peeled off from the separator, and the adhesive porous layer was immersed in dimethylacetamide and heated to about 50°C to obtain a resin solution in which the polyvinylidene fluoride resin was dissolved. The resin solution was centrifuged in a centrifuge to precipitate the insoluble matter. The supernatant of the resin solution from which the insoluble matter had been precipitated was taken out and centrifuged repeatedly to remove the insoluble matter. The resin solution from which the insoluble matter had been removed was dropped into water to coagulate the polyvinylidene fluoride resin. The coagulated matter was removed from the water and dried, and the solid after drying was used as the sample. 5 mg of the sample was placed in an aluminum sample pan (manufactured by TA Instruments, part number 900786.901), covered with a lid (manufactured by TA Instruments, part number 900779.901), and set in the measuring device. The measuring device used was a product name: DSC Q20 (manufactured by TA Instruments). Thermal analysis was performed by changing the sample temperature in the three steps described above while flowing nitrogen gas at a flow rate of 50 ml / min.

[0190] [Dry adhesion] A negative electrode slurry was prepared by mixing 300 parts by mass of artificial graphite as a negative electrode active material, 7.5 parts by mass of a water-soluble dispersion containing 40% by mass of a modified styrene-butadiene copolymer as a binder resin, 3 parts by mass of carboxymethylcellulose as a thickener, and an appropriate amount of water with a twin-arm mixer. The negative electrode slurry was applied to one side of a copper foil with a thickness of 10 μm, dried, and pressed to obtain a negative electrode having a negative electrode active material layer.

[0191] The negative electrode was cut into a rectangle of 15 mm x 70 mm. The separator was cut into a rectangle measuring TD 20 mm x MD 75 mm. A rectangular release paper measuring 15 mm x 70 mm was prepared. The laminate, in which the negative electrode, separator, and release paper were stacked in this order, was inserted into a pack made of aluminum laminate film, and the pack was heat-pressed in the stacking direction using a heat press (dry heat press), thereby bonding the negative electrode and separator. The heat press conditions were a temperature of 90°C, 1 cm of electrode 2 The load was 30 kg per unit area and the pressing time was 30 seconds. After that, the laminate was taken out of the pack, and the release paper was peeled off to obtain a test piece.

[0192] The uncoated surface of the negative electrode of the test piece was fixed to a metal plate with double-sided tape, and the metal plate was fixed to the lower chuck of a Tensilon (A&D, STB-1225S). At this time, the metal plate was fixed to the Tensilon so that the length direction of the test piece (i.e., the MD of the separator) was the direction of gravity. The separator was peeled off from the negative electrode by about 2 cm from the bottom end, and the end was fixed to the upper chuck, and a 180° peel test was performed. The tensile speed of the 180° peel test was 300 mm / min, and the load (N) from 10 mm to 40 mm after the start of the measurement was collected at 0.4 mm intervals, and the average was calculated. The load of 10 test pieces was then averaged.

[0193] [Wet adhesion] 89.5 parts by mass of lithium cobalt oxide powder as a positive electrode active material, 4.5 parts by mass of acetylene black as a conductive additive, 6 parts by mass of polyvinylidene fluoride as a binder resin, and an appropriate amount of N-methyl-2-pyrrolidone were mixed by stirring with a twin-arm mixer to prepare a positive electrode slurry. The positive electrode slurry was applied to both sides of an aluminum foil with a thickness of 20 μm, dried, and pressed to obtain a double-sided positive electrode having a positive electrode active material layer on both sides. A negative electrode slurry was prepared by mixing 300 parts by mass of artificial graphite as a negative electrode active material, 7.5 parts by mass of an aqueous dispersion containing 40% by mass of a modified styrene-butadiene copolymer as a binder resin, 3 parts by mass of carboxymethylcellulose as a thickener, and an appropriate amount of water with a twin-arm mixer. The negative electrode slurry was applied to both sides of a copper foil with a thickness of 10 μm, dried, and pressed to obtain a double-sided negative electrode having a negative electrode active material layer on both sides.

[0194] The positive electrode and negative electrode were each cut into a rectangle of 30 mm×70 mm. The separator was cut into a rectangle measuring TD 35 mm x MD 75 mm. These were stacked so that the positive and negative electrodes were alternated and a separator was sandwiched between the positive and negative electrodes to produce a laminate consisting of three positive electrodes, three negative electrodes, and five separators. The laminate was inserted into a pack made of aluminum laminate film, and electrolyte (1 mol / L LiPF6-ethylene carbonate:ethyl methyl carbonate [mass ratio 3:7]) was injected into the pack to allow the electrolyte to soak into the laminate. Next, the laminate including the pack was heat-pressed in the stacking direction using a heat press machine (wet heat press) to bond the electrodes and separators. The heat press conditions were a temperature of 90°C, 1 cm of electrode, and 100 cm of electrode. 2 The load was 10 kg per unit area and the pressing time was 2 minutes. This was used as a cell for measuring wet adhesion.

[0195] A compression type bending test (three-point bending measurement) was performed on the above cell. The measurement was performed by attaching a compression type bending test jig to a Tensilon (A&D Co., Ltd., STB-1225S). The distance between the supports was 4 cm, and the cell was placed on the support so that the short side of the cell was parallel to the long direction of the indenter and the compression position during measurement was the center of the long direction of the electrode in the cell. The measurement was started by setting the displacement at 0 when the indenter was lowered until a load of 0.1 N was applied. The compression speed during measurement was 2 mm / min, and the measurement was performed up to a displacement of 2 mm. The yield point load in the load-displacement curve obtained from this result was taken as the wet adhesive strength. If the yield point load could not be observed, the maximum load was taken as the wet adhesive strength.

[0196] [Battery short circuit] 89.5 parts by mass of lithium cobalt oxide powder as a positive electrode active material, 4.5 parts by mass of acetylene black as a conductive additive, 6 parts by mass of polyvinylidene fluoride as a binder resin, and an appropriate amount of N-methyl-2-pyrrolidone were mixed by stirring with a twin-arm mixer to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum foil with a thickness of 20 μm, dried, and pressed to obtain a positive electrode having a positive electrode active material layer. A negative electrode slurry was prepared by mixing 300 parts by mass of artificial graphite as a negative electrode active material, 7.5 parts by mass of a water-soluble dispersion containing 40% by mass of a modified styrene-butadiene copolymer as a binder resin, 3 parts by mass of carboxymethylcellulose as a thickener, and an appropriate amount of water with a twin-arm mixer. The negative electrode slurry was applied to one side of a copper foil with a thickness of 10 μm, dried, and pressed to obtain a negative electrode having a negative electrode active material layer.

[0197] The positive electrode was cut into a 3 cm x 5 cm rectangle, the negative electrode was cut into a 3.2 cm x 5.2 cm rectangle, and a lead tab was welded to each. The separator was cut into a 3.5 cm x 5.5 cm rectangle. The positive electrode, separator, and negative electrode were stacked in this order, and the stack was inserted into a pack made of an aluminum laminate film, and an electrolyte (1 mol / L LiPF6-ethylene carbonate:propylene carbonate [mass ratio 1:1]) was poured into the pack to allow the electrolyte to soak into the stack. Next, the pack was evacuated and sealed using a vacuum sealer to obtain a battery for short circuit testing.

[0198] At a temperature of 25°C, 100 test batteries were charged at a constant current and constant voltage of 0.2C and 4.2V. Then, all test batteries were placed in an oven at a temperature of 150°C for 60 minutes. At this time, a weight of about 500g was placed on each test battery. After the heat treatment, the test batteries were removed from the oven and the weight was removed. After the test batteries were cooled to room temperature of 25°C, the voltage was measured. Test batteries with a voltage of 3.5V or less were determined to be short-circuited, and the number of short-circuited test batteries out of the 100 was counted.

[0199] [Discharge capacity maintenance rate] Twenty test batteries were prepared. Ten of them were not heat-treated and were used as standard batteries. The remaining ten were left at a temperature of 100°C for 30 minutes and were used as heat-treated batteries. The following charge and discharge were performed on 10 standard batteries and 10 heat-treated batteries. Five cycles of charge and discharge were performed, with charging at a constant current and constant voltage of 0.2C and 4.2V, and discharging at a constant current of 0.2C and 2.5V cutoff. Next, charging at a constant current and constant voltage of 0.2C and 4.2V, and discharging at a constant current of 10C and 2.5V cutoff. The discharge capacity at this time was recorded, and the average value of the discharge capacity of each of the 10 standard batteries and the 10 heat-treated batteries was calculated. The ratio of the discharge capacity of the heat-treated battery to the discharge capacity of the standard battery was taken as the discharge capacity retention rate (%) of the battery exposed to high temperature, and was calculated from the following formula. Discharge capacity retention rate = Discharge capacity of heat-treated battery ÷ Discharge capacity of standard battery × 100

[0200] <Preparation of separator and battery> [Example 1] -Making the separator- As materials for the adhesive porous layer, two types of polyvinylidene fluoride resins and magnesium hydroxide particles were prepared. The physical properties of these are shown in Table 1. Two types of polyvinylidene fluoride resins were mixed in a mass ratio of 60:40 and dissolved in dimethylacetamide (DMAc) so that the resin concentration became 5.0 mass %, and magnesium hydroxide particles were further dispersed therein by stirring to obtain a coating solution (1).

[0201] An appropriate amount of coating liquid (1) was placed on a Mayer bar, and coating liquid (1) was applied to both sides of a polyethylene microporous membrane (physical properties are as shown in Table 1). At this time, coating was performed so that the coating amount on the front and back of the polyethylene microporous membrane was equal. This was immersed in a coagulation liquid (DMAc:water = 50:50 [mass ratio], liquid temperature 40°C) to solidify the coating layer, and then washed in a water washing tank with water temperature of 40°C and dried. In this way, a separator in which an adhesive porous layer was formed on both sides of the polyethylene microporous membrane was obtained. The thickness of the adhesive porous layer was approximately 3 μm per side.

[0202] - Preparation of negative electrode - A negative electrode slurry was prepared by mixing 300 parts by mass of artificial graphite as a negative electrode active material, 7.5 parts by mass of a water-soluble dispersion containing 40% by mass of a modified styrene-butadiene copolymer as a binder resin, 3 parts by mass of carboxymethylcellulose as a thickener, and an appropriate amount of water with a twin-arm mixer. The negative electrode slurry was applied to one side of a copper foil with a thickness of 10 μm, dried, and pressed to obtain a negative electrode having a negative electrode active material layer.

[0203] - Preparation of positive electrode - 89.5 parts by mass of lithium cobalt oxide powder as a positive electrode active material, 4.5 parts by mass of acetylene black as a conductive additive, 6 parts by mass of polyvinylidene fluoride as a binder resin, and an appropriate amount of N-methyl-2-pyrrolidone were mixed by stirring with a twin-arm mixer to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum foil with a thickness of 20 μm, dried, and pressed to obtain a positive electrode having a positive electrode active material layer.

[0204] -Battery construction- The positive electrode was cut into a 3 cm x 5 cm rectangle, the negative electrode was cut into a 3.2 cm x 5.2 cm rectangle, and a lead tab was welded to each. The separator was cut into a 3.4 cm x 5.4 cm rectangle. The positive electrode, separator, and negative electrode were stacked in this order. The stack was heat-pressed in the stacking direction using a heat press (dry heat press) to temporarily bond the electrodes and separators. The heat press conditions were: temperature 90°C, 1 cm 2 The load was 30 kg and the pressing time was 30 seconds. The temporarily bonded laminate was inserted into a pack made of aluminum laminate film, and electrolyte (1 mol / L LiPF6-ethylene carbonate:ethyl methyl carbonate [mass ratio 3:7]) was injected into the pack to allow the electrolyte to soak into the laminate. Next, the laminate including the pack was heat-pressed in the stacking direction using a heat press machine (wet heat press) to bond the electrodes and separators. The heat press conditions were a temperature of 90°C, 1 cm of electrode 2 The load was 10 kg and the pressing time was 2 minutes. The pack was then sealed using a vacuum sealer to create a vacuum inside, yielding a test battery.

[0205] [Examples 2 to 6, Comparative Examples 1 to 7] Each separator was produced in the same manner as in Example 1, except that the polyethylene microporous membrane and the type and amount of the polyvinylidene fluoride resin and filler, which are materials for the adhesive porous layer, were changed to the specifications shown in Table 1. The thickness of the adhesive porous layer was approximately 3 μm per side. The thickness of the adhesive porous layer was 0.3 μm per side in Comparative Example 6 and 2.0 μm per side in Comparative Example 7. Then, test batteries were fabricated in the same manner as in Example 1 using each separator.

[0206] "PVDF resin X" in Table 1 is a resin corresponding to polyvinylidene fluoride resin X or a comparative polyvinylidene fluoride resin. PVDF resin X is a binary copolymer made of VDF and HFP. The comparative polyvinylidene fluoride resin used in Comparative Example 6 is a ternary copolymer (VDF / HFP / AA=87.2 / 12.0 / 0.8 [mol %]) made of VDF, HFP, and acrylic acid (AA: monomer represented by formula (1)). The comparative polyvinylidene fluoride resin used in Comparative Example 7 is a ternary copolymer (VDF / HFP / AA=94.6 / 5.2 / 0.2 [mol %]) made of VDF, HFP, and acrylic acid (AA: monomer represented by formula (1)). "PVDF resin Y" in Table 1 is a resin corresponding to polyvinylidene fluoride resin Y or a comparative polyvinylidene fluoride resin. PVDF resin Y is a ternary copolymer consisting of VDF, HFP, and a monomer represented by formula (1). In PVDF resin Y, the monomer represented by formula (1) is acrylic acid in all cases.

[0207] The composition, physical properties and evaluation results of each of the separators of Examples 1 to 6 and Comparative Examples 1 to 7 are shown in Tables 1 and 2.

[0208] [Table 1]

[0209] [Table 2]

[0210] [Reference example 1] The two types of polyvinylidene fluoride resins used in Examples 1 to 4 were mixed in a mass ratio of 50:50. The mixed resin was used as a sample to perform DSC to analyze the thermal properties. The analysis results are shown in Table 3.

[0211] [Reference example 2] The two types of polyvinylidene fluoride resins used in Example 5 were mixed in a mass ratio of 50:50. The mixed resin was used as a sample to perform DSC to analyze the thermal properties. The analysis results are shown in Table 3.

[0212] [Table 3]

[0213] Reference Examples 1 and 2 have the same mixing ratio of two types of polyvinylidene fluoride resins, but the low-melting point polyvinylidene fluoride resin (corresponding to polyvinylidene fluoride resin X) is a different type from the other, and the high-melting point polyvinylidene fluoride resin (corresponding to polyvinylidene fluoride resin Y) is the same type. Comparing Reference Example 1 with Reference Example 2, it is clear that by changing the type of low-melting point polyvinylidene fluoride resin, the endothermic peak temperature and exothermic peak temperature on the low temperature side change.

[0214] The two types of polyvinylidene fluoride resins used in Reference Example 1 and Example 1 are the same in their mixing ratios, but the sample subjected to DSC in Example 1 is a polyvinylidene fluoride resin extracted from an adhesive porous layer, and is therefore a polyvinylidene fluoride resin that has been subjected to a step of forming an adhesive porous layer. Comparing Reference Example 1 with Example 1, it is found that the mixture of two types of polyvinylidene fluoride resins has a smaller temperature difference between the endothermic peak and the exothermic peak by undergoing the step of forming an adhesive porous layer. That is, by undergoing the step of forming an adhesive porous layer, the endothermic peak and the exothermic peak on the low temperature side are shifted to the high temperature side, and the endothermic peak and the exothermic peak on the high temperature side are shifted to the low temperature side. From this, it is presumed that in the process of forming the adhesive porous layer, the two types of polyvinylidene fluoride resins are partially compatible with each other, and there are regions where the high-melting-point polyvinylidene fluoride resin is slightly dissolved in the low-melting-point polyvinylidene fluoride resin and regions where the low-melting-point polyvinylidene fluoride resin is slightly dissolved in the high-melting-point polyvinylidene fluoride resin. As a result, it is presumed that the endothermic peak and exothermic peak on the low-temperature side are shifted to the high-temperature side, and the endothermic peak and exothermic peak on the high-temperature side are shifted to the low-temperature side.

[0215] In Comparative Example 1, the difference in melting points between the two types of polyvinylidene fluoride resins was 22°C, but the DSC curve of the polyvinylidene fluoride resin extracted from the adhesive porous layer showed one endothermic peak and one exothermic peak, not two each. As described above, it is presumed that the two types of polyvinylidene fluoride resins are at least partially compatible in the process of forming the adhesive porous layer. At this time, if the characteristics of the two types of polyvinylidene fluoride resins (characterized by the HFP ratio, molecular weight, and melting point) are similar, it is presumed that the two types of polyvinylidene fluoride resins are completely compatible, and one endothermic peak and one exothermic peak are observed in the DSC curve.

[0216] The disclosure of Japanese Patent Application No. 2021-118148, filed on July 16, 2021, is incorporated herein by reference in its entirety. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A porous substrate; An adhesive porous layer provided on one or both sides of the porous substrate, the adhesive porous layer containing a polyvinylidene fluoride resin and a filler; The Gurley value is 50 seconds / 100 mL to 200 seconds / 100 mL; when the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, two or more endothermic peaks and two or more exothermic peaks are observed; The temperature difference between adjacent endothermic peaks among two or more observed endothermic peaks is 27° C. or more and 60° C. or less. Separator for non-aqueous secondary batteries.

2. 2. The separator for a nonaqueous secondary battery according to claim 1, wherein, when differential scanning calorimetry is performed on the entire polyvinylidene fluoride resin contained in the adhesive porous layer, at least one endothermic peak is observed in a region of 125° C. or higher and lower than 140° C. and at least one endothermic peak is observed in a region of 140° C. or higher and lower than 190° C.

3. 2. The separator for a nonaqueous secondary battery according to claim 1, wherein, when a differential scanning calorimetry is performed on the entire polyvinylidene fluoride resin contained in the adhesive porous layer, at least one exothermic peak is observed in a region of 80° C. or more and less than 125° C. and at least one exothermic peak is observed in a region of 125° C. or more and less than 190° C.

4. 2. The separator for a nonaqueous secondary battery according to claim 1, wherein when differential scanning calorimetry is performed on the entire polyvinylidene fluoride resin contained in the adhesive porous layer as a sample, two or more exothermic peaks are observed, and the temperature difference between adjacent exothermic peaks is 10° C. or more and 90° C. or less.

5. A porous substrate; An adhesive porous layer provided on one or both sides of the porous substrate, the adhesive porous layer containing a polyvinylidene fluoride resin and a filler; The Gurley value is 50 seconds / 100 mL to 200 seconds / 100 mL; The polyvinylidene fluoride resin includes the following polyvinylidene fluoride resin X and polyvinylidene fluoride resin Y, The difference between the melting point of the polyvinylidene fluoride resin X and the melting point of the polyvinylidene fluoride resin Y is 25° C. or more and less than 55° C. Separator for non-aqueous secondary batteries. Polyvinylidene fluoride resin X: Contains constituent units derived from vinylidene fluoride and constituent units derived from hexafluoropropylene, in which the proportion of constituent units derived from hexafluoropropylene in all constituent units is more than 3.5 mol% and not more than 15 mol%, has a weight average molecular weight of 100,000 or more and less than 1,000,000, and has a melting point of 125°C or more and less than 150°C. Polyvinylidene fluoride resin Y: Contains structural units derived from vinylidene fluoride and may contain structural units derived from hexafluoropropylene, in which the proportion of structural units derived from hexafluoropropylene in all structural units is 0 mol% or more and 3.5 mol% or less, the weight average molecular weight is 1 million or more and less than 3 million, and the melting point is 150°C or more and less than 180°C.

6. 6. The separator for a non-aqueous secondary battery according to claim 5, wherein when the entire polyvinylidene fluoride resin contained in the adhesive porous layer is subjected to differential scanning calorimetry, two or more endothermic peaks and / or two or more exothermic peaks are observed.

7. 6. The separator for a non-aqueous secondary battery according to claim 5, wherein a mass ratio of the polyvinylidene fluoride resin X to the polyvinylidene fluoride resin Y contained in the adhesive porous layer is 20:80 to 80:

20.

8. 6. The separator for a nonaqueous secondary battery according to claim 5, wherein the polyvinylidene fluoride resin X contains constituent units derived from vinylidene fluoride and constituent units derived from hexafluoropropylene, the proportion of the constituent units derived from hexafluoropropylene in all constituent units is more than 5.0 mol % and not more than 15 mol %, the weight average molecular weight is 300,000 or more and less than 1,000,000, and the melting point is 125° C. or more and less than 140° C.

9. 6. The separator for a nonaqueous secondary battery according to claim 5, wherein the polyvinylidene fluoride resin Y contains a constituent unit derived from vinylidene fluoride and may contain a constituent unit derived from hexafluoropropylene, the proportion of the constituent units derived from hexafluoropropylene in all constituent units is 0 mol% or more and 2.0 mol% or less, the weight average molecular weight is 1.5 million or more and less than 2 million, and the melting point is 150°C or more and less than 170°C.

10. 6. The separator for a non-aqueous secondary battery according to claim 1, wherein the adhesive porous layer contains a polyvinylidene fluoride resin having a constituent unit derived from a monomer represented by the following formula (1): [Formula 1] In formula (1), R 1 , R 2 and R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms, a carboxy group, or a derivative of a carboxy group; X represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene group having 1 to 5 carbon atoms and having a substituent; Y represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms substituted with at least one hydroxy group, an alkyl group having 1 to 5 carbon atoms substituted with at least one carboxy group, or -R-O-C(=O)-(CH 2 ) n It represents —C(═O)—OH (R represents an alkylene group having 1 to 5 carbon atoms, and n represents an integer of 0 or more).

11. 6. The separator for a non-aqueous secondary battery according to claim 1, wherein the polyvinylidene fluoride resin contained in the adhesive porous layer has an acid value of less than 3.0 mgKOH / g.

12. 6. The separator for a non-aqueous secondary battery according to claim 1, wherein the weight average molecular weight of the entire polyvinylidene fluoride resin contained in the adhesive porous layer is 300,000 or more and less than 3,000,000.

13. 6. The separator for a non-aqueous secondary battery according to claim 1, wherein the proportion of structural units derived from hexafluoropropylene in all structural units in the entire polyvinylidene fluoride resin contained in the adhesive porous layer is more than 3.5 mol% and not more than 7.0 mol%.

14. 6. The separator for a non-aqueous secondary battery according to claim 1, wherein a volume ratio of said filler to a volume excluding pores of said adhesive porous layer is 30 volume % to 90 volume %.

15. 6. The separator for a non-aqueous secondary battery according to claim 1, wherein the filler comprises at least one selected from the group consisting of metal hydroxide particles, metal sulfate particles, and barium titanate particles.

16. 6. The separator for a non-aqueous secondary battery according to claim 1, wherein the average primary particle size of the entire filler contained in said adhesive porous layer is 0.01 μm to 1.5 μm.

17. 13. A nonaqueous secondary battery comprising: a positive electrode; a negative electrode; and the separator for a nonaqueous secondary battery according to claim 1 or 5, the separator being disposed between the positive electrode and the negative electrode, the nonaqueous secondary battery generating an electromotive force by doping and dedoping lithium ions.

Citation Information

Patent Citations

  • Separation film for secondary battery, and lithium secondary battery including the same

    JP2017208338A

  • Binder composition for non-aqueous secondary cell function layer, slurry composition for non-aqueous secondary cell function layer, function layer for non-aqueous secondary cell, separator provided with function layer for non-aqueous secondary cell, non-aqueous secondary cell, and method for producing same

    WO2018163969A1

  • Separator for non-aqueous secondary batteries, non-aqueous secondary battery, and method for producing non-aqueous secondary battery

    WO2018212252A1