Method for producing alloy powder, and alloy powder, paste, and capacitor produced by the method
The method of thermal radiation solidification, quench cooling, and surface passivation addresses the stability and uniformity issues in conductive powders, resulting in improved multilayer ceramic capacitors with enhanced manufacturing efficiency.
Patent Information
- Application Number
- JP2023528289
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-11
- Filing Date
- 2022-02-25
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2042-02-25
AI Technical Summary
Existing methods for producing conductive powders for multilayer ceramic capacitors face challenges in achieving high stability, uniform thermal expansion, and effective chemical passivation, leading to issues like expansion cracks and chemical instability during the manufacturing process.
A method combining thermal radiation solidification, quench cooling, and surface chemical and physical passivation processes to produce alloy powder, involving steps like cooling metal droplets in a carrier gas, rapid quenching, and applying an oxygen or sulfur-containing compound to form a dense chemical passivation layer.
The resulting alloy powder exhibits high stability, uniform thermal expansion, and improved co-firing properties, enhancing the manufacturing efficiency and yield of multilayer ceramic capacitors.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing metal alloy powder suitable for electronic applications, more specifically to a method for producing a highly stable alloy powder as a conductive powder for use in a conductive paste, and further to an alloy powder produced by this method, a conductive paste produced from this alloy powder, and a multilayer ceramic capacitor produced from this conductive paste. [Background technology]
[0002] The alloy powder, which is the main component of the conductive paste used in the electrode manufacturing process of the multilayer ceramic capacitor, needs to have as few unnecessary impurities as possible so as not to affect the conductivity. However, the number of layers in the multilayer ceramic capacitor is increasing, and the conductive powder is required to have good conductivity. In addition, the conductive powder is required to have good bonding properties during the co-firing process of the ceramic insulating layer and the glass powder, and to have similar thermal expansion properties to prevent expansion cracks between layers and bending or breaking of the ceramic body due to differences in thermal expansion properties between each layer.
[0003] Therefore, the conductive powder must have a high sintering start temperature and good co-firing with the oxide ceramic powder or glass powder. In the international division of labor environment, the time required to manufacture multilayer ceramic capacitors from powder is long (sometimes more than 30 days), so the metal powder is also required to have relatively high stability. In order to maintain the stability of the powder, the powder can be vacuum or inert atmosphere packaged or the powder surface can be coated. In order to improve the co-firing of the metal powder and ceramic powder, the powder can be treated with an oxygen or sulfur addition process. However, micro-materials, especially nano-materials, have a very large specific surface area and very strong chemical activity, so that chemical reactions are likely to occur inside the powder particles during the oxygen or sulfur addition process, and the chemical passivation layer or coating layer on the powder surface is also likely to be uneven and unstable. In addition, if the chemical passivation layer on the surface of the powder particles is not effectively controlled, the reaction will continue to the inside of the particles, which will also affect the stability of the metal powder. Summary of the Invention [Problem to be solved by the invention]
[0004] In view of the problems in the background art, the present invention provides a method for producing high stability alloy powder, which produces high stability alloy powder by a combination of a thermal radiation solidification process, a rapid cooling process, a surface chemical passivation process and a surface physical passivation process. [Means for solving the problem]
[0005] In order to achieve the above objectives, the present invention has been achieved by the following technical solutions:
[0006] The method for producing the high stability alloy powder is specifically described as follows: 1. A step of carrying molten metal droplets by a carrier gas having a temperature higher than the melting point of the metal, sending the metal droplets into a heat radiation area, and cooling them until they are solidified to obtain particles, in which the metal content in the metal droplets exceeds 99.9 wt%; 2. The solidified high-temperature solid particles are mixed with a room temperature fluid and rapidly quenched to obtain a dense and stable alloy powder particle structure, and the average temperature of the particles and carrier gas before quenching is higher than 500°C, and the average temperature of the particles and carrier gas after quenching is lower than 300°C; 3. During the formation of the metal droplets, or after hardening, or after quenching, contacting the surface of the metal droplets or particles with an oxygen group element, and forming a chemical passivation layer on the surface of the particles through a reaction with the oxygen group element to form an oxygen group element-containing nickel compound, in which the amount of the oxygen group element is controlled so that the mass of the oxygen group element is 0.10-15.00 wt% relative to the mass of the alloy powder; 4. Dispersing an alloy powder having a chemical passivation layer containing an oxygen group element in a fluid in a container of a housing having a hard inner wall at room temperature, rotating the alloy powder in the container while the fluid is supported by pressure, and causing the rotated particles to collide with each other or with the hard inner wall of the container housing, thereby making the chemical passivation layer on the surface of the particles denser.
[0007] Furthermore, the metal source in the metal droplets is at least one of nickel and copper.
[0008] Furthermore, the carrier gas is at least one of nitrogen gas and argon gas.
[0009] Furthermore, the fluid in step 2 is at least one of an inert gas or a liquid.
[0010] Furthermore, the oxygen group element is at least one of oxygen and sulfur.
[0011] Furthermore, the alloy powder has an average particle size of 20-1000 nm, each particle is roughly circular to spherical, the metal content in the particles is 84.00-99.80 wt%, the non-metallic and non-oxygen group element content is 0.01-1.00 wt%, the oxygen group element content is 0.10-15.00 wt%, and the oxygen group element content is greater than 90 wt% is concentrated within an outer surface layer of the particles having a thickness of 5 nm.
[0012] The present invention further provides a conductive paste using the above-mentioned highly stable alloy powder.
[0013] The present invention further provides a multilayer ceramic capacitor using electrodes made of the above-mentioned conductive paste. Effect of the Invention
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: The high-stability alloy powder produced by this method has particles undergoing thermal radiation cooling and solidification processes, and the thermal radiation cooling method has a stable temperature field, which contributes to obtaining particles with a shape closer to a round sphere. The solidified and molded particles are quenched by fluid cooling under high temperature conditions, and the surface of the particles rapidly shrinks to form a denser surface layer. A chemical passivation reaction occurs in the surface layer of the particles, and when the surface layer where the chemical passivation reaction occurs is compressed by impact of physical means, the oxide layer or vulcanization layer in the surface layer changes from fluffy to a dense protective layer. The high-stability alloy powder particles formed by thermal radiation solidification, fluid quenching, chemical passivation and physical impact passivation have more stable chemical properties and good dispersibility, and the yield of multilayer ceramic capacitors produced from the conductive paste made of alloy powder particles is high. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be further described with reference to the examples. Although the present invention is described clearly and completely, it is clear that the described examples are only a part of the embodiments of the present invention, and are not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by a person skilled in the art without performing any labor worthy of inventive step, all belong to the protection scope of the present invention.
[0016] Example 1 Molten droplet microparticles (nickel content exceeding 99.9 wt%) were carried by a carrier gas (nitrogen gas) at a temperature higher than the melting point of nickel, 1453°C, and sent to a heat radiation area where they were cooled until solidified, obtaining particles. The solidified high-temperature solid particles are mixed with a room temperature fluid and rapidly quenched to obtain dense and stable nickel alloy powder particles. The average temperature of the particles and carrier gas before quenching is higher than 800°C, and the average temperature of the particles and carrier gas after quenching is lower than 200°C, and the average particle size of the particles is 275nm. After the metal droplet particles were rapidly cooled, the surfaces of the particles were exposed to oxygen gas to form oxygen-containing nickel compounds on the surfaces of the highly active ultrafine particles, and the oxygen content in the particles was 0.70 wt%. High-pressure (0.6 MPa) gas is introduced into the cavity of the ceramic cyclone to form a cyclone, and the nickel alloy powder having a chemical passivation layer is dispersed in the airflow and rotated at high speed. The rotating nickel alloy powder particles collide with each other or with the ceramic inner wall of the container housing and are compressed, making the chemical passivation layer on the surface of the particles denser.
[0017] Example 2 Molten droplet microparticles (nickel content exceeding 99.9 wt%) were carried by a carrier gas (nitrogen gas) at a temperature higher than the melting point of nickel, 1453°C, and sent to a heat radiation area where they were cooled until solidified, obtaining particles. The solidified high-temperature solid particles are mixed with a room temperature fluid and rapidly quenched to obtain dense and stable nickel alloy powder particles. The average temperature of the particles and carrier gas before quenching is higher than 750°C, and the average temperature of the particles and carrier gas after quenching is lower than 250°C, and the average particle size of the particles is 72 nm. After the metal droplet particles were quenched, the particle surfaces were exposed to oxygen gas to form oxygen-containing nickel compounds on the surfaces of the highly active ultrafine particles, and the oxygen content in the particles was 4.50 wt%. A negative pressure fan draws in normal pressure airflow into the cavity of the stainless steel cyclone to form a negative pressure (-0.03 MPa) cyclone, and the nickel alloy powder with the chemical passivation layer is dispersed into the airflow and rotated at high speed. The rotating nickel alloy powder particles collide with each other or with the inner wall of the container housing and are compressed, making the chemical passivation layer on the surface of the particles denser.
[0018] Example 3 Molten droplet microparticles (nickel content exceeding 99.9 wt%) were carried by a carrier gas (nitrogen gas) at a temperature higher than the melting point of nickel, 1453°C, and sent to a heat radiation area where they were cooled until solidified, obtaining particles. The solidified high-temperature solid particles are mixed with a room temperature fluid and rapidly quenched to obtain dense and stable nickel alloy powder particles, in which the average temperature of the particles and carrier gas before quenching is higher than 750°C, and the average temperature of the particles and carrier gas after quenching is lower than 200°C, and the average particle size of the particles is 150nm. Sulfur was added before the molten droplets solidified, and the metal droplet particles were rapidly cooled. The surfaces of the particles were then exposed to oxygen gas, forming nickel compounds containing sulfur and oxygen on the surface of the highly active ultrafine particles. The oxygen content in the particles was 1.30 wt%, and the sulfur content was 0.11 wt%. A high-pressure (0.8 MPa) liquid is introduced into the cavity of the ceramic swirling flow tube to form a liquid swirling flow, and the nickel alloy powder having a chemical passivation layer is dispersed in the liquid flow and rotated at high speed. The rotating nickel alloy powder particles collide with each other or with the ceramic inner wall of the container housing and are compressed, making the chemical passivation layer on the surface of the particles denser.
Claims
1. A method for producing an alloy powder, comprising the steps of: (1) carrying molten metal droplets by a carrier gas having a temperature higher than the melting point of the metal, sending the metal droplets to a heat radiation area, and cooling the metal droplets until they are solidified to obtain particles, in which the content of the metal in the metal droplets exceeds 99.9 wt %; (2) mixing the solidified high-temperature solid particles with a room temperature fluid and rapidly quenching them to obtain a dense and stable alloy powder particle structure, in which the average temperature of the particles and carrier gas before quenching is higher than 500°C, and the average temperature of the particles and carrier gas after quenching is lower than 300°C; (3) contacting the surface of the metal droplets or particles with an oxygen group element during the formation of the metal droplets, or after hardening, or after quenching, to produce a chemical passivation layer on the surface of the particles by reaction with the oxygen group element, thereby producing an oxygen group element-containing nickel compound, in which the amount of the oxygen group element is controlled so that the mass of the oxygen group element is 0.10-15.00 wt % based on the mass of the alloy powder; (4) A method for producing an alloy powder, comprising the steps of dispersing an alloy powder having a chemical passivation layer containing an oxygen group element in a fluid in a container of a housing having a hard inner wall at room temperature, rotating the alloy powder in the container while the fluid is supported by pressure, and causing the rotated particles to collide with each other or with the hard inner wall of the housing of the container, thereby making the chemical passivation layer on the surface of the particles denser.
2. 2. The method for producing an alloy powder according to claim 1, wherein the metal raw material in the metal droplets is at least one of nickel and copper.
3. 3. The method for producing an alloy powder according to claim 1, wherein the carrier gas is at least one of nitrogen gas and argon gas.
4. The method for producing an alloy powder according to any one of claims 1 to 3, characterized in that the fluid in step (2) is at least one of an inert gas or a liquid.
5. 5. The method for producing an alloy powder according to claim 1, wherein the oxygen group element is at least one of oxygen and sulfur.
6. 6. The method for producing an alloy powder according to claim 1, wherein the alloy powder has an average particle size of 20-1000 nm, each particle is quasi-circular and spherical, the metal content in the particles is 84.00-99.80 wt %, the non-metallic and non-oxygen group element content is 0.01-1.00 wt %, the oxygen group element content is 0.10-15.00 wt %, and the oxygen group element content of more than 90 wt % is concentrated in an outer surface layer of the particles having a thickness of 5 nm.
7. An alloy powder in which a chemical passivation layer is formed on a surface of the alloy powder by a reaction with an oxygen group element by the manufacturing method according to any one of claims 1 to 6, and the chemical passivation layer is densified by causing the rotated particles to collide with each other or the rotated particles to collide with a hard inner wall of a housing of a container, The alloy powder has an average particle size of 20 to 1000 nm, and each particle is roughly circular and spherical; The content of metal in the particles is 84.00 to 99.80 wt %, the content of non-metallic and non-oxygen group elements is 0.01 to 1.00 wt %, and the content of oxygen group elements is 0.10 to 15.00 wt %, and wherein the oxygen group element content is greater than 90 wt % and is concentrated in an outer surface layer of the particles having a thickness of 5 nm.
8. A conductive paste comprising the alloy powder according to claim 7.
9. A multilayer ceramic capacitor comprising an electrode manufactured using the conductive paste according to claim 8.
Citation Information
Patent Citations
Fine copper powder and its manufacturing method
JP2008013837A
Nickel powder and its manufacturing method, and conductive paste and multilayer ceramic electronic component using it
JP2008223068A