Method for pre-treating gold ore and method for gold recovery
The pretreatment of gold ores with phenol oxidase and an electron transfer substance modifies carbonaceous components, enhancing gold recovery rates by reducing adsorption in the gold recovery process.
Patent Information
- Application Number
- JP2020175079
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-25
- Filing Date
- 2020-10-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-19
AI Technical Summary
Gold ores containing carbonaceous components adsorb a portion of leached gold, leading to reduced gold recovery rates due to increased gold remaining in the ore.
A pretreatment method involving the use of phenol oxidase, such as laccase, to modify the surface of carbonaceous components in gold ore, combined with an electron transfer substance, followed by a cleaning step to reduce gold adsorption ability, and subsequent gold recovery through leaching, adsorption, and elution steps.
The method effectively reduces the gold adsorption ability of carbonaceous components, increasing the gold recovery rate by minimizing gold adsorption during the recovery process.
Smart Images

Figure 0007558512000003 
Figure 0007558512000004 
Figure 0007558512000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for pretreating gold ore and a method for recovering gold, more particularly to a method for pretreating gold ore containing carbonaceous components and a method for recovering gold using the pretreated gold ore. [Background technology]
[0002] Patent Document 1 discloses the Carbon In Pulp (CIP) method as a method for recovering gold from gold ore. Gold recovery by the CIP method is carried out in the following procedure. First, a dilute cyanide solution of an alkali metal or alkaline earth metal and an alkali are added to finely pulverized gold ore to convert the gold in the gold ore into a gold cyanide ion complex (Au(CN)2 - The gold complex is then eluted as a slag. The slurry containing the ore and the gold complex is then brought into countercurrent contact with activated carbon, causing the gold complex to be adsorbed onto the activated carbon. A hot cyanide solution is then applied to the activated carbon separated from the slurry, causing the gold complex to be desorbed from the activated carbon. The cyanide solution in which the gold complex has been concentrated is then subjected to electrowinning to recover the gold. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 03-030834 Summary of the Invention [Problem to be solved by the invention]
[0004] When gold ore contains carbonaceous matter, some of the gold leached from the gold ore is adsorbed by the carbonaceous matter in the ore, resulting in an increase in the amount of gold remaining in the ore and a decrease in the gold recovery rate.
[0005] In view of the above circumstances, an object of the present invention is to provide a method for pretreating gold ore that can reduce the gold adsorption capacity of carbonaceous components contained in gold ore. Another object of the present invention is to provide a gold recovery method that has a high gold recovery rate even if gold ore contains carbonaceous components. [Means for solving the problem]
[0006] The gold ore pretreatment method of the first invention is a pretreatment method carried out before leaching gold from gold ore containing carbonaceous components, and is characterized by comprising an enzyme treatment step in which the gold ore is contacted with phenol oxidase and maintained for a predetermined period of time. The gold ore pretreatment method of the second invention is characterized in that, in the first invention, laccase is used as the phenol oxidase. The gold ore pretreatment method of the third invention is characterized in that, in the second invention, the amount of the laccase to be contacted with the gold ore is an amount such that the enzyme activity relative to the weight of the carbonaceous component is 39 to 198 U / g. A fourth aspect of the present invention is a method for pretreating gold ore according to any one of the first to third aspects of the present invention, characterized in that in the enzyme treatment step, the gold ore is brought into contact with an electron mediator. The gold ore pretreatment method of the fifth invention is characterized in that, in the fourth invention, ABTS (2,2'-azino-bis(3-ethylbenzothiazoline-6-sulfonic acid)) or HOBT (1-hydroxybenzotriazole) is used as the electron transfer substance. A gold ore pretreatment method according to a sixth aspect of the present invention is any one of the first to fifth aspects of the present invention, characterized in that it further comprises a washing step of washing the surface of the gold ore after the enzyme treatment step. The gold recovery method of the seventh invention is characterized by comprising: a pretreatment step of pretreating gold ore containing a carbonaceous component by any of the methods of the first to sixth inventions; a leaching step of leaching gold from the gold ore after the pretreatment step to obtain a leachate; an adsorption step of adsorbing the gold in the leachate onto activated carbon; and an elution step of eluting the gold from the activated carbon to obtain a gold solution. Effect of the Invention
[0007] According to the gold ore pretreatment method of the present invention, the surface of the carbonaceous component is modified by the action of phenol oxidase, and the gold adsorption ability of the carbonaceous component is reduced. Furthermore, according to the gold recovery method of the present invention, since the gold adsorption capacity of the carbonaceous components contained in the gold ore is reduced, the amount of gold contained in the leachate that is adsorbed onto the carbonaceous components can be reduced, thereby increasing the gold recovery rate. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a process diagram of a gold recovery method according to one embodiment. [Diagram 2] 1 shows SEM images in Examples 1 to 3 and Comparative Example 1. [Diagram 3] 1 shows Raman spectra in Examples 1 to 3 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Next, an embodiment of the present invention will be described with reference to FIG. [Pretreatment method] The gold ore pretreatment method according to one embodiment of the present invention is carried out as a pretreatment for a process for recovering gold from gold ore. As described above, when gold is leached from gold ore containing carbonaceous components, a part of the leached gold is adsorbed by the carbonaceous components in the ore. As a result, the amount of gold remaining in the ore increases, and the gold recovery rate decreases. Therefore, a pretreatment is carried out before leaching gold from the gold ore to reduce the gold adsorption capacity of the carbonaceous components contained in the gold ore.
[0010] Gold ore is an aggregate of minerals that contain gold. Gold is often contained as a single element in metallic sulfide ores such as chalcocite, bornite, covellite, chalcopyrite, pyrite, arsenopyrite, and arsenopyrite. These types of ores are referred to as gold ores. In general, gold concentrates are obtained by increasing the gold content through processes such as flotation, and then the gold is recovered. Gold ores include such gold concentrates.
[0011] The gold ore to be pretreated is not particularly limited as long as it contains carbonaceous components. Among carbonaceous components, activated carbon is known to have a high adsorption capacity for cyanide ions. Therefore, pretreatment is particularly effective for gold ores that contain activated carbon or carbonaceous components with properties similar to those of activated carbon.
[0012] (Enzyme treatment process) The pretreatment includes an enzyme treatment step. The enzyme treatment step is carried out by contacting gold ore with phenol oxidase and holding the mixture for a predetermined time. Here, it is preferable to crush the gold ore in advance. The contact between the gold ore and phenol oxidase can be achieved by various methods. For example, the gold ore may be immersed in an enzyme solution containing phenol oxidase, or the enzyme solution may be sprayed on the gold ore. Specifically, the gold ore may be put into the enzyme solution containing phenol oxidase. The gold ore may be crushed in advance and water may be added to produce a gold ore slurry, and phenol oxidase or the enzyme solution containing phenol oxidase may be added to the gold ore slurry. Alternatively, the enzyme solution containing phenol oxidase may be sprayed on the gold ore in bulk.
[0013] Phenol oxidase is an enzyme that has the ability to oxidize phenol. Examples of phenol oxidase include laccase, tyrosinase, and enzymes secreted by white rot fungi. Among these, it is preferable to use laccase. This is because laccase is relatively inexpensive and has high enzymatic activity, allowing the amount of laccase to be reduced.
[0014] The amount of phenol oxidase added, the pH and temperature of the enzyme solution containing phenol oxidase, and the contact time between the gold ore and phenol oxidase may be appropriately adjusted depending on the type of phenol oxidase used, etc.
[0015] When laccase is used, the amount of laccase to be contacted with the gold ore is preferably an amount such that the enzyme activity relative to the weight of the carbonaceous component contained in the gold ore is 39 to 198 U / g. The enzyme activity per unit volume of the enzyme solution containing laccase may be 19.5 to 100 U / L. The pH of the enzyme solution containing laccase is preferably 4 to 5, and the temperature is preferably 25 to 40°C. The retention time for contacting the gold ore with the laccase is preferably 1 to 7 days. However, from an industrial perspective, the shorter the retention time, the more efficient it is. Therefore, a retention time of 1 to 2 days is more preferable.
[0016] As described above, when gold ore is brought into contact with phenol oxidase, the surface of the carbonaceous component is modified by the action of phenol oxidase, and the gold adsorption ability of the carbonaceous component is reduced. As a result, when gold is leached from the gold ore in the subsequent gold recovery process, the leached gold can be prevented from being adsorbed by the carbonaceous component in the ore.
[0017] In the enzyme treatment step, the gold ore may be contacted with the phenol oxidase and the electron transfer substance at the same time. The gold ore may be contacted with the electron transfer substance by various methods. For example, the gold ore may be immersed in an enzyme solution containing phenol oxidase and an electron transfer substance, or the enzyme solution may be sprayed on the gold ore. Specifically, the gold ore may be put into the enzyme solution containing phenol oxidase and an electron transfer substance. The gold ore may be crushed in advance and water may be added to produce a gold ore slurry, and the phenol oxidase and the electron transfer substance may be added to the gold ore slurry, or the enzyme solution containing phenol oxidase and the electron transfer substance may be added to the gold ore slurry. Alternatively, the enzyme solution containing phenol oxidase and the electron transfer substance may be sprayed on the gold ore in bulk.
[0018] An electron mediator is a substance that mediates electrons when an enzyme works. In the present invention, the electron mediator plays a role of mediating electron transfer between the gold ore carbonaceous material and phenol oxidase. ABTS, HOBT, etc. can be used as the electron mediator. Since the electron mediator mediates electrons in the enzyme reaction, the enzyme reaction can be efficiently promoted. In detail, it is considered that the enzyme reaction is promoted and the activated carbon can be effectively modified, or the electron mediator occupies the adsorption site of the activated carbon and prevents gold adsorption, or both occur simultaneously.
[0019] After the enzyme treatment step, solid-liquid separation is performed as necessary. By removing the liquid, the enzyme-treated gold ore (solid fraction) can be obtained.
[0020] (Cleaning process) After the enzyme treatment step, it is preferable to wash the gold ore. The surface of the carbonaceous components contained in the gold ore is modified by the enzyme reaction, and the gold adsorption capacity is reduced. At the same time, intermediate decomposition products of the carbonaceous components may be generated and remain in the solid phase. The intermediate decomposition products may adsorb gold in the subsequent gold recovery process. If the gold ore is washed to remove the intermediate decomposition products, it is possible to prevent the leached gold from being adsorbed by the intermediate decomposition products in the gold recovery process.
[0021] Furthermore, washing the gold ore can remove phenol oxidase and electron mediators attached to the surface of the gold ore, which prevents the gold adsorption capacity of activated carbon added in the subsequent gold recovery process from being reduced by the enzyme reaction.
[0022] The washing method is not particularly limited. For example, a washing liquid may be added to the gold ore after the enzyme treatment, and the gold ore may be extracted by solid-liquid separation after stirring. The addition of the washing liquid and the solid-liquid separation may be performed multiple times. As the washing liquid, an organic solvent may be used in addition to water. The decomposition products of the carbonaceous components may be insoluble in water. In this case, it is preferable to use an organic solvent as the washing liquid.
[0023] [Gold recovery method] Following the pretreatment step described above, gold can be recovered from the gold ore by carrying out the steps described below.
[0024] (Leaching process) In the leaching process, gold is leached from the gold ore to obtain a leachate. For example, a cyanide compound is added to a slurry containing crushed gold ore, and leaching is performed while blowing air into the slurry. Examples of the cyanide compound include sodium cyanide, potassium cyanide, and calcium cyanide. Other gold leaching agents such as thiourea, thiosulfate, and halogen gas may be used instead of the cyanide compound.
[0025] Here, because the gold ore has been pretreated, the gold adsorption capacity of the carbonaceous components in the gold ore is reduced, so the amount of gold in the leachate that is adsorbed by the carbonaceous components can be reduced, and the gold recovery rate can be increased.
[0026] (Adsorption process) In the adsorption step, the leachate is brought into contact with activated carbon to adsorb the gold in the leachate onto the activated carbon. It is preferable to adjust the retention time so that most of the gold in the leachate is adsorbed onto the activated carbon. The activated carbon with the gold adsorbed thereon is separated from the leachate.
[0027] The type of activated carbon used is not particularly limited, but one with a high gold adsorption capacity is preferred. In the adsorption process, activated carbon is generally added to the leachate and stirred. Because the activated carbon particles collide with each other during stirring, activated carbon that is less likely to crumble or become powdery is preferred. An example of such activated carbon is coconut shell activated carbon.
[0028] It is preferable to wash the activated carbon with hydrochloric acid or the like before supplying it to the next step. The activated carbon may have copper, calcium, etc., derived from gold ore, adhering thereto. By removing these in advance, the impurity concentration of the gold solution obtained in the next step can be reduced.
[0029] (Elution step) In the elution step, gold is eluted from the activated carbon after the adsorption step to obtain a gold solution. For example, the activated carbon is contacted with a heated alkaline cyanide solution to elute the gold from the activated carbon. Note that gold may be eluted using an alkaline solution such as sodium hydroxide instead of the cyanide solution.
[0030] The gold can then be recovered by electrowinning using a gold solution. It is preferable to reactivate the activated carbon after gold has been eluted so that it can be reused. EXAMPLES
[0031] Next, an embodiment will be described. [Examples 1 to 3, Comparative Example 1] Laccase, a type of phenol oxidase (Sigma-Andrich, Lacasse from Trametes versicolor, hereinafter referred to as "laccase A") was prepared. Details of laccase A are as follows. <Laccase A> Form: Powder Color: Light brown Lot. Activity: 0.99 U / mg Bottle weight: 1 g Storage Temp.: 2 - 9℃ Code: 38429
[0032] An enzyme solution was prepared by adding laccase A to water. The amount of laccase A added was adjusted based on the lot activity of laccase A (0.99 U / mg), and three types of enzyme solutions with enzyme activities per unit volume of 19.5, 49.5, and 99.0 U / L were prepared. The pH of each enzyme solution was adjusted to 4 using succinic acid and sodium hydroxide.
[0033] Next, 100 mg of activated carbon (Fujifilm Wako Pure Chemical Industries, activated carbon, powder, Wako special grade, the same applies below) was added to 200 mL of each enzyme solution. Each enzyme solution was kept at 30° C. and stirred at 128 rpm for 3 days.
[0034] The treated enzyme solution was subjected to solid-liquid separation to extract the activated carbon. The surface of the activated carbon was observed with a SEM (Keyence Corporation, VE-9800). For comparison, the surface of untreated activated carbon was also observed with the SEM. The SEM images of each activated carbon are shown in Figure 2.
[0035] As can be seen from Figure 2, the surface of the activated carbon treated with laccase shows irregularities due to erosion. Furthermore, the higher the enzyme activity, the more advanced the erosion. This confirmed that some modification of the surface of activated carbon occurs when laccase is brought into contact with activated carbon.
[0036] Next, Raman spectroscopy (XDR Smart Raman, manufactured by Thermo Fisher Scientific) was performed on the treated activated carbon. For comparison, Raman spectroscopy was also performed on untreated activated carbon. The Raman spectrum of each activated carbon is shown in Figure 3.
[0037] After fitting each Raman spectrum, the peak intensities (maximum values) of the peak (G band) derived from the graphene structure and the peak (D band) derived from the defect structure were calculated. The ratio of the peak intensity of the D band to the peak intensity of the G band (I D / I G ) was sought.
[0038] As a result, untreated activated carbon is I D / I G = 2.05. Activated carbon treated with 19.5 U / L enzyme solution was I D / I G = 2.29. Activated carbon treated with 49.5 U / L enzyme solution was I D / I G = 2.32. Activated carbon treated with 99.0 U / L enzyme solution had an I D / I G =2.53.
[0039] I D / I Gis the ratio of defect structures to graphene structures. I D / I G The higher the value of , the more the graphene structure is destroyed. In other words, when treated with laccase, the graphene structure of the activated carbon is destroyed. Also, the higher the enzyme activity, the more the graphene structure is destroyed.
[0040] Activated carbon with many graphene structures has a high density of π electrons and is easy to adsorb cations. - One of the reasons why ) is adsorbed to activated carbon is thought to be electrostatic adsorption via cations adsorbed to activated carbon. If the graphene structure of activated carbon is destroyed by treatment with laccase, the sp 2 It is believed that orbital collapse occurs, the frequency of cation adsorption decreases, and the adsorption of cyanogen gold is suppressed.
[0041] Next, a cyanide gold adsorption test was carried out. A cyanide gold solution was prepared by dissolving 36.6 mg of potassium cyanide gold (KAu(CN)2) in 500 mL of an alkaline solution of pH 11.5. The pH of the alkaline solution was adjusted using 1 M potassium hydroxide solution. 10 mg of the treated activated carbon was added to 4.0 mL of the cyanide gold solution, and the solution was shaken at 120 rpm for 24 hours while maintaining the temperature at 25°C. The solution was then subjected to solid-liquid separation, and the Au(CN)2 in the solution was separated. - The concentration was measured. From the measurement results, the amount of gold adsorbed to the activated carbon and the gold adsorption rate were calculated. In addition, a cyanide gold adsorption test was also performed on untreated activated carbon using the same procedure.
[0042] The results are summarized in Table 1. [Table 1] The case where activated carbon was not treated with the enzyme solution was designated Comparative Example 1. The cases where activated carbon was treated with enzyme solutions having enzyme activities of 19.5, 49.5, and 99.0 U / L were designated Examples 1, 2, and 3, respectively.
[0043] As can be seen from Table 1, the activated carbon treated with laccase (Examples 1 to 3) had a smaller amount of gold adsorption and a lower gold adsorption rate than the untreated activated carbon (Comparative Example 1). This confirmed that treatment with laccase reduces the gold adsorption capacity of activated carbon.
[0044] Moreover, the higher the enzyme activity of laccase, the smaller the amount of gold adsorbed and the lower the gold adsorption rate. From the results of Examples 1 to 3, it was confirmed that the gold adsorption capacity of activated carbon decreases at least when the enzyme activity per unit volume of the enzyme solution is in the range of 19.5 to 99.0 U / L. Furthermore, when comparing the case of an enzyme activity of 49.5 U / L with the case of 99.0 U / L, there is not much difference in the amount of gold adsorbed. From the viewpoint of reducing the amount of laccase used, it is preferable to set the enzyme activity to 50 U / L or less.
[0045] The enzyme activity per unit volume of the enzyme solution "U / L" can be converted into the enzyme activity relative to the weight of activated carbon [U / g] as shown in Table 1. Therefore, the enzyme activity relative to the weight of activated carbon is preferably 39 to 198 U / g, and more preferably 39 to 100 U / g.
[0046] Among the carbonaceous components in gold ore, the main component that adsorbs gold is thought to be activated carbon or a carbonaceous component with properties similar to activated carbon. Therefore, it is thought that if gold ore containing carbonaceous components is contacted with laccase, the gold adsorption ability of the carbonaceous components in the gold ore will decrease.
[0047] In addition, not only laccase but also other phenol oxidases have similar properties and are therefore thought to be able to reduce the gold adsorption ability of carbonaceous components.
[0048] [Examples 4 to 12] A laccase (Laccase Y-120, manufactured by Amano Enzyme Inc., hereinafter referred to as "Laccase B") made by a different manufacturer from the Laccase A used in Examples 1 to 3 was prepared. Details of Laccase B are as follows. The lot activities are test values from each manufacturer and cannot be simply compared, but as far as the lot activities are compared, it can be said that Laccase B has a higher enzyme activity than Laccase A. <Laccase B> Form: powder Color: White to greenish white Lot activity: 108U / mg Optimum temperature: 60℃ Optimal pH: 4.0~4.5
[0049] An enzyme solution was prepared by adding laccase B to water. The amount of laccase B added was adjusted based on the lot activity of laccase B (108 U / mg) to give an enzyme activity per unit volume of the enzyme solution of 4,000 U / L. The pH of the enzyme solution was adjusted to 4.5 using sodium acetate (0.1 M solution).
[0050] Example 4 2.5 mL of the enzyme solution and 97.5 mL of 0.1 M sodium acetate buffer were mixed to prepare 100 mL of reagent solution A. The enzyme activity per unit volume of reagent solution A was 100 U / L.
[0051] 100 mg of activated carbon was added to 100 mL of test solution A. Using a stirring device (TAITEC Bioshaker, model number BR-40LF, the same applies below), the solution was stirred at 128 rpm for one day while maintaining the liquid temperature at 37°C. The treated liquid was subjected to solid-liquid separation to extract the activated carbon.
[0052] The activated carbon pretreated as described above was used to carry out an adsorption test for cyanide gold. A cyanide gold solution was prepared by dissolving 32.3 mg of potassium cyanide gold (KAu(CN)2) in 500 mL of an alkaline solution of pH 11.5. The pH of the alkaline solution was adjusted using 1 M potassium hydroxide solution. 10 mg of the treated activated carbon was added to 4.0 mL of the cyanide gold solution, and the solution was shaken at 125 rpm for 24 hours while maintaining the temperature at 25°C. The solution was then subjected to solid-liquid separation, and the Au(CN)2 in the solution was separated. - The concentration was measured, and the amount of gold adsorbed onto the activated carbon was calculated from the measurement results.
[0053] Example 5 After treating the activated carbon with the test solution A in the same manner as in Example 4, the activated carbon was washed with pure water. The washing was performed in the following manner. A conical tube for centrifugation containing 50 mg of activated carbon and 10 mL of pure water was set in a shaking device (Shaker, model SRR-2, manufactured by AS ONE Corporation, the same applies below), and the liquid temperature was maintained at 25°C while shaking at 120 rpm for 5 minutes. Next, the conical tube for centrifugation was set in a centrifugal separator (Centrifugal separator, model 5430 R, manufactured by Eppendorf Corporation, the same applies below), and the liquid temperature was maintained at 4°C while performing solid-liquid separation at 7,600 rpm for 10 minutes to obtain a solid fraction. The obtained solid fraction (activated carbon) was washed again in the same manner.
[0054] Using the washed activated carbon, a cyanide gold adsorption test was carried out in the same manner as in Example 4 to determine the amount of gold adsorbed onto the activated carbon.
[0055] Example 6 After treating the activated carbon with the test solution A in the same manner as in Example 4, the activated carbon was washed with an organic solvent. The washing was performed in the following manner. A conical tube for centrifugation containing 100 mg of activated carbon and 2 mL of organic solvent was set in a shaker and shaken at 150 rpm for 1 hour while maintaining the liquid temperature at 25°C. Next, the conical tube for centrifugation was set in a centrifuge and solid-liquid separation was performed at 7,600 rpm for 10 minutes while maintaining the liquid temperature at 4°C to obtain a solid fraction. The same procedure was repeated a total of four times. As the organic solvent, ethylene glycol was used in the first washing, methanol in the second washing, ethyl acetate in the third washing, and hexane in the fourth washing.
[0056] Using the washed activated carbon, a cyanide gold adsorption test was carried out in the same manner as in Example 4 to determine the amount of gold adsorbed onto the activated carbon.
[0057] Example 7 HOBT was prepared as an electron transfer substance. The details of HOBT are as follows. <hobt> Chemical Name:1-Hydroxybenzotriazole hydrate Chemical formula: C6H5N3O xH2O Manufacturer: Sigma Andrich
[0058] HOBT was added to 99% ethanol to prepare a 100 mM HOBT solution. Next, 2.5 mL of the enzyme solution, 0.8 mL of the HOBT solution, and 96.7 mL of 0.1 M sodium acetate buffer were mixed to prepare 100 mL of test solution B. The enzyme activity per unit volume of test solution B was 100 U / L. The HOBT concentration in test solution B was 0.8 mM.
[0059] 100 mg of activated carbon was added to 100 mL of test solution B. The solution was stirred at 128 rpm for 7 days using a stirring device while maintaining the liquid temperature at 37°C. The activated carbon was removed on the 1st, 2nd, 5th, and 7th days after the start of stirring.
[0060] Using the same procedure as in Example 4, a cyanide gold adsorption test was carried out using each activated carbon, and the amount of gold adsorbed onto the activated carbon was determined.
[0061] Example 8 The activated carbon was treated with the test solution B in the same manner as in Example 7, and then washed with pure water. The washing method was the same as in Example 5. Next, a cyanide gold adsorption test was carried out using each activated carbon in the same manner as in Example 4, and the amount of gold adsorbed onto the activated carbon was determined.
[0062] Example 9 The activated carbon was treated with the reagent B in the same manner as in Example 7, and then washed with an organic solvent. The washing method was the same as in Example 6. Next, a cyanide gold adsorption test was carried out using each activated carbon in the same manner as in Example 4, and the amount of gold adsorbed onto the activated carbon was determined.
[0063] Example 10 ABTS was used as an electron transfer substance. The details of ABTS are as follows. <abts> Chemical name: (2,2'-azino-bis(3-ethylbenzothiazoline-6-sulfonic acid)) diammonium salt Chemical formula:C 18 H 16 N4O6S4·(NH4)2 Manufacturer: Fujifilm Wako Pure Chemical
[0064] ABTS was added to 50% ethanol to prepare a 50 mM ABTS solution. Next, 2.5 mL of the enzyme solution, 1.6 mL of the ABTS solution, and 95.9 mL of 0.1 M sodium acetate buffer were mixed to prepare 100 mL of test solution C. The enzyme activity per unit volume of test solution C was 100 U / L. The ABTS concentration of test solution C was 0.8 mM.
[0065] 100 mg of activated carbon was added to 100 mL of test solution C. Using a stirrer, the solution was stirred at 128 rpm for 7 days while maintaining the liquid temperature at 37°C. The activated carbon was removed on the 1st, 2nd, 5th, and 7th days after the start of stirring.
[0066] Using the same procedure as in Example 4, a cyanide gold adsorption test was carried out using each activated carbon, and the amount of gold adsorbed onto the activated carbon was determined.
[0067] Example 11 The activated carbon was treated with the reagent C in the same manner as in Example 10, and then washed with pure water. The washing method was the same as in Example 5. Next, a cyanide gold adsorption test was carried out using each activated carbon in the same manner as in Example 4, and the amount of gold adsorbed onto the activated carbon was determined.
[0068] Example 12 The activated carbon was treated with the reagent C in the same manner as in Example 10, and then washed with an organic solvent. The washing method was the same as in Example 6. Next, a cyanide gold adsorption test was carried out using each activated carbon in the same manner as in Example 4, and the amount of gold adsorbed onto the activated carbon was determined.
[0069] The results of Examples 4 to 12 are summarized in Table 2. [Table 2]
[0070] As can be seen from Table 2, the amount of gold adsorbed was less when an electron mediator was added (Examples 7 to 12) than when no electron mediator was added (Examples 4 to 6). This confirmed that the addition of an electron mediator promoted the enzyme reaction and effectively modified the activated carbon.
[0071] Furthermore, the amount of gold adsorbed was generally less when ABTS was used as the electron transfer substance (Examples 10 to 12) than when HOBT was used as the electron transfer substance (Examples 7 to 9). This suggests that it is preferable to use ABTS as the electron transfer substance or adsorbent.
[0072] The amount of gold adsorbed tends to be less when the activated carbon is washed than when it is not washed. Also, the amount of gold adsorbed tends to be less when an organic solvent is used as the washing solution than when pure water is used. Therefore, it is preferable to wash the gold ore after the enzyme treatment, and washing with an organic solvent is more preferable.
[0073] In some cases, the longer the retention time of the enzyme treatment, the lower the amount of gold adsorption (Examples 7, 8, and 11), but in other cases, the amount of gold adsorption decreases with the retention time and then increases (Examples 9, 10, and 12). From an industrial perspective, a shorter retention time allows for more efficient operation, so it is preferable to be able to suppress the amount of gold adsorption with a short retention time.
[0074] Among Examples 4 to 12, in Example 12 in which ABTS was used as the electron transfer substance and washing was performed with an organic solvent, the effect of suppressing the amount of gold adsorption was the highest when the retention time was set to one day.< / abts> < / hobt>
Claims
1. A method for pre-treating gold ore containing carbonaceous components prior to leaching of gold, comprising the steps of: An enzyme treatment step of contacting the gold ore with phenol oxidase and maintaining the same for a predetermined period of time is provided. In the enzyme treatment step, the gold ore is contacted with an electron mediator, The electron transfer substance used is ABTS (2,2'-azino-bis(3-ethylbenzothiazoline-6-sulfonic acid)) or HOBT (1-hydroxybenzotriazole). A method for pre-treating gold ore.
2. Laccase is used as the phenol oxidase.
2. The method for pre-treating gold ore according to claim 1.
3. The amount of the laccase to be contacted with the gold ore is set to an amount such that the enzyme activity relative to the weight of the carbonaceous component is 39 to 198 U / g.
3. The method for pre-treating gold ore according to claim 2.
4. After the enzyme treatment step, a washing step is provided for washing the surface of the gold ore. The method for pretreatment of gold ore according to any one of claims 1 to 3.
5. A pretreatment step of pretreating gold ore containing carbonaceous components by the method according to any one of claims 1 to 4; a leaching step of leaching gold from the gold ore after the pretreatment step to obtain a leachate; an adsorption step of adsorbing gold in the leachate onto activated carbon; and an elution step of eluting gold from the activated carbon to obtain a gold solution. A method for recovering gold.
Citation Information
Patent Citations
Spherical activated carbon for gold recovery and recovery method
JP1991030834A
Lignin decomposition using laccase and lignin decomposing agent
JP2000064185A
New cyclosporin
JP2006524232A
Microbial fuel cell, fuel and microbe for the fuel cell, and bioreactor and biosensor
JP2012190787A
Platinum group metal separation agent and platinum group metal ion separation method
JP2016011456A