Extractant for scandium and method for separating and extracting it

A deep eutectic solvent and polymer membrane combination effectively separates scandium from solutions with rare earth metals and iron, addressing inefficiencies in existing methods by enhancing selectivity and reducing costs.

JP7558513B2Active Publication Date: 2024-10-01UNIVERSITY OF MIYAZAKI +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020184559
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-04
Publication Date
2024-10-01
Estimated Expiration
2040-11-04

AI Technical Summary

Technical Problem

Existing methods for separating scandium from solutions containing rare earth metals or iron are inefficient, costly, and prone to impurity extraction, with challenges such as inclusion formation and chemical similarity leading to co-precipitation and loss of valuable elements.

Method used

A deep eutectic solvent prepared by mixing a compound with a hydroxyl group and a trialkylphosphine oxide compound, incorporated into a polymer membrane, is used to selectively extract scandium at low pH, leveraging cooperative and antagonistic effects to separate scandium from iron and other rare earth metals.

Benefits of technology

The method enables efficient, low-cost separation of scandium without impurities, achieving high selectivity and adsorption efficiency, even in the presence of chemically similar metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558513000013
    Figure 0007558513000013
  • Figure 0007558513000014
    Figure 0007558513000014
  • Figure 0007558513000015
    Figure 0007558513000015
Patent Text Reader

Abstract

To provide an extractant capable of separating and extracting scandium efficiently and at low cost by a simple treatment step without generation of an inclusion called a clad or extraction of impurities, from a solution containing rare earth metals or iron and a separation extraction method.SOLUTION: An extractant that selectively separates and extracts scandium from a solution containing rare earth metals or iron, in which the extractant is a deep eutectic solvent prepared by mixing a compound having at least hydroxyl groups and a trialkylphosphine oxide compound.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an extractant and a method for separating and extracting scandium using a deep eutectic solvent prepared by mixing a plurality of extractants. [Background technology]

[0002] Rare earth elements are made up of 17 elements, including 15 lanthanides, scandium (Sc) and yttrium (Y), and their applications are attracting great interest in many fields. Among them, scandium is used in structural materials, electronic materials, magnetic materials, functional materials, etc., as adding small amounts of it can dramatically improve the functions and physical properties of metal materials and semiconductor materials, and plays a very important role in various industrial products. Furthermore, demand is expected to increase in new fields, such as fuel cells, the aerospace industry, and special alloys.

[0003] On the other hand, scandium does not exist as a concentrated mineral, but is produced as a by-product of other metal ores. In addition, the supply of scandium is unstable because the country of production is limited. In addition, since scandium's chemical properties are very similar to other rare earth elements such as yttrium, it is extremely difficult to separate scandium from these compounds.

[0004] Methods for separating and recovering scandium include a solvent extraction method using an acidic alkyl phosphate ester, such as PC-88A (main component: 2-ethylhexyl 2-ethylhexyl phosphonate), as an extractant (see Patent Document 1). There is also a solvent extraction method using an acidic phosphate ester with an alkylcyclohexyl group as the alkyl chain instead of the usual 2-ethylhexyl group as an extractant (see Patent Document 2). However, with the above methods, not only scandium but also impurities are extracted to a non-negligible extent into the organic solvent.

[0005] There is also a method in which acidic alkyl phosphate esters are used as adsorbents in a resin-supported form rather than as a solvent extraction method (see Patent Documents 3 and 4). However, this method using acidic alkyl phosphate esters has problems in that it is difficult to elute scandium from the resin, and that adsorption is inhibited due to the formation of a polymer between scandium and the extractant on the resin surface. Furthermore, there is a concern that the extractant supported on the resin may leak into the aqueous solution during the extraction process, even if only in small amounts.

[0006] In addition, when a currently practical method is to selectively extract scandium from a solution containing iron ions as an impurity, such as a solution obtained by acid leaching of nickel oxide ore, it is necessary to raise the pH of the solution to about 4 to 5, but this not only requires a large amount of neutralizing agent, but also promotes the formation of iron hydroxide, which causes scandium and other valuable elements to co-precipitate, resulting in losses. In particular, even if scandium is separated from such a solution containing iron ions by ion exchange or solvent extraction, there is a problem that inclusions called crud are easily formed during the extraction process. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 9-291320 [Patent Document 2] Japanese Patent Application Publication No. 4-36373 [Patent Document 3] Japanese Unexamined Patent Publication No. 1-108119 [Patent Document 4] Japanese Patent Application Publication No. 1-246328 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in light of these problems, and aims to provide an extractant and a method for separating and extracting scandium efficiently and at low cost through a simple processing step from a solution containing rare earth metals or iron, without generating inclusions called crud or extracting impurities. [Means for solving the problem]

[0009] In order to solve the above problems, the extractant for scandium of the present invention has the following characteristics. (1) An extractant for selectively separating and extracting scandium from a solution containing rare earth metals or iron, comprising: The extractant is characterized in that it is a deep eutectic solvent prepared by mixing at least a compound having a hydroxyl group and a trialkylphosphine oxide compound (formula I). (Formula I) [ka] (In the formula, R 1 ,R 2 ,R 3 represents an alkyl group of C1 to C20. (2) The extractant is incorporated in a polymer membrane. (3) The trialkylphosphine oxide compound is characterized in that it is tri-n-octylphosphine oxide (formula II). (Formula II) [ka] (4) The compound having a hydroxyl group is N-lauroyl sarcosine (formula III). (Formula III) [ka] (5) The rare earth metal is yttrium. (6) The method for separating and extracting scandium according to the present invention comprises the steps of: A method for selectively separating and extracting scandium from a solution containing rare earth metals or iron, comprising the steps of: The method is characterized by using a deep eutectic solvent prepared by mixing at least a compound having a hydroxyl group and a trialkylphosphine oxide compound. (7) The method is characterized in that the deep eutectic solvent or an extractant-encapsulating polymer membrane in which the deep eutectic solvent is encapsulated in a polymer membrane is used, and the pH of the solution is set to 1.5 or less. Effect of the Invention

[0010] According to the extractant and separation / extraction method of the present invention, scandium alone can be efficiently separated and extracted at low cost from a solution containing rare earth metals or iron using a simple processing step, without producing inclusions called crud or extracting impurities. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 shows the extraction results (pH dependence) by the solvent extraction method using a deep eutectic solvent. [Diagram 2] FIG. 1 shows the results of adsorption (pH dependence) by an adsorption method using an extractant-encapsulating polymer membrane. [Diagram 3] FIG. 1 shows the results of adsorption by an adsorption method using an extractant-encapsulating polymer membrane (the effect of shaking time). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the present invention will be described, but the present invention is not limited to the following embodiments, and can be practiced with appropriate modifications within the scope of the object of the present invention. Note that the "extractant" in the present invention includes the case where the extractant is incorporated into a polymer membrane and used as an adsorbent, and also includes the case where the extractant is used not only in liquid-liquid extraction but also in solid-phase extraction.

[0013] 1. Extractant The extractant in the present invention selectively separates and extracts scandium (Sc) from a solution containing rare earth metals or iron (Fe), and more specifically, selectively separates and extracts only scandium (Sc) from a solution containing scandium (Sc) and at least one metal selected from 15 lanthanoids, yttrium (Y) or iron (Fe).

[0014] Scandium (Sc) is an element with atomic number 21 and atomic weight 44.9, and is classified as a rare earth element together with yttrium (Y) and lanthanoids. Therefore, these elements have very similar chemical properties, and it is considered difficult to separate them from each other. In addition, since lanthanoids and iron (Fe) also have very similar chemical properties, the extraction process becomes complicated and expensive when separating only the target scandium (Sc) from metals containing these rare earth elements and iron (Fe). However, according to the present invention, only scandium (Sc) can be extracted easily and at low cost from a solution in which these metals coexist.

[0015] The extractant of the present invention is a deep eutectic solvent (DES) prepared by mixing a compound having a hydroxyl group and a trialkylphosphine oxide compound. A deep eutectic solvent is a compound that is liquid at room temperature and is created by combining a hydrogen bond donor compound (hereinafter referred to as "hydrogen bond donor") and a hydrogen bond acceptor compound (hereinafter referred to as "hydrogen bond acceptor"). Room temperature refers to 20°C ± 15°C, that is, the range of 5°C to 35°C, and room temperature is included in this temperature range.

[0016] When the hydrogen bond donor and the hydrogen bond acceptor are solid at room temperature, or when either one is solid, mixing them causes a eutectic melting point depression, and a liquid state can be created at room temperature. Deep eutectic solvents have physical properties similar to ionic liquids, and are characterized by low vapor pressure, flame retardancy, high thermal stability and electrochemical stability, and the ease of dissolving any substance. Deep eutectic solvents have higher environmental compatibility than ionic liquids, are less toxic, and are therefore environmentally friendly. They have the advantage that they can be easily prepared by simply mixing, making the processing process simple and allowing processing at low cost.

[0017] The mixing ratio of the hydrogen bond donor and the hydrogen bond acceptor is appropriately selected depending on the type of hydrogen bond donor and hydrogen bond acceptor used and the type of coexisting metal, but each compound is mixed so that it accounts for at least 1% by weight of the total. In order to efficiently exert the extraction effect of each compound, for example, when one type of hydrogen bond donor and one type of hydrogen bond acceptor are used, the volume ratio of these is preferably in the range of 1:10 to 10:1, more preferably in the range of 1:5 to 5:1, and even more preferably in the range of 1:3 to 3:1.

[0018] Hydrogen bond donors and hydrogen bond acceptors have the role of facilitating the separation of metals that are difficult to separate, such as rare earth elements and iron. For example, even if scandium and iron draw the same extraction curves in each pH region when a single extractant is used, by combining an extractant that exerts a synergistic effect on scandium (hydrogen bond acceptor) and an extractant that exerts an antagonistic effect on iron (hydrogen bond donor), the extraction curve is drawn with scandium shifting to the low pH region and iron shifting to the high pH region, and as a result, only scandium can be extracted in the low pH region and only iron can be extracted in the high pH region.

[0019] The fewer the number of target metals, the easier it is to design, but for example, when separating from waste leachate that is composed of several dozen types of metal ions, the number of extractants can be increased or the combination of extractants can be appropriately changed. In this way, even in cases where a single extractant cannot fully exert its power for separation and recovery, by using at least two or more extractants as in the present invention, the extraction characteristics of each extractant can be exerted, and scandium alone can be selectively separated and extracted reliably from a solution in which metals with very similar chemical properties coexist.

[0020] The compound that becomes the hydrogen bond donor is a compound having a hydroxyl group, for example, alkylated sarcosine, acylated sarcosine, alkyl carboxylic acid, dialkyl phosphoric acid, alkyl phenol or alkyl thiol. Suitable alkyls include, but are not limited to, n-hexyl, n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, 3,5,5-trimethylhexyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl and octadecyl. To be more specific, when the compound having a hydroxyl group is, for example, acylated sarcosine, N-lauroyl sarcosine (hereinafter also referred to as "NLS") represented by the above formula II, in which the acyl group is a lauroyl group, can be used.

[0021] The hydrogen bond acceptor compound is a trialkylphosphine oxide compound (formula I) shown below, where R 1 ,R 2 ,R 3 represents an alkyl group of C1 to C20. (Formula I) [ka] The term "alkyl group" refers to a linear or branched saturated aliphatic hydrocarbon group containing a specific number of carbon atoms. For example, a "C1-C20 alkyl group" refers to a linear or branched saturated hydrocarbon chain containing at least 1 to 20 carbon atoms. Suitable alkyl groups include, but are not limited to, n-hexyl, n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, 3,5,5-trimethylhexyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, and octadecyl. From the viewpoint of molecular structure, the alkyl group is preferably a C3-C20 alkyl group, and more preferably a C5-C10 alkyl group. To be more specific, R 1 ,R 2 ,R 3 In the present invention, tri-n-octylphosphine oxide (hereinafter, also referred to as "TOPO"), in which all of the alkyl groups are C8 linear alkyl groups, can be used.

[0022] The method of mixing these extractants to make a deep eutectic solvent involves, for example, placing at least one hydrogen bond donor and one hydrogen bond acceptor extractant in a container in any ratio, and applying heat or ultrasound to turn them into a liquid at room temperature. The liquid is an even mixture of multiple extractants, and can be used as is without the use of a diluent. In addition, when melting from a solid to a liquid, the functional groups of each extractant can be densely aggregated, making it possible to maximize the cooperative and antagonistic effects on the target metal. In addition, since it is in the form of a liquid at room temperature, it is easy to handle.

[0023] 2. Extractant-containing polymer membrane A method for incorporating the aforementioned extractant into a polymer membrane will be described. The polymer material used can be, for example, cellulose triacetate (CTA), polyvinyl chloride (PVC), or polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP), and can be produced by a casting method. Specifically, the polymer material, the aforementioned deep eutectic solvent, and the plasticizer are dissolved in tetrahydrofuran (THF) and thoroughly stirred. The resulting solution is poured into a petri dish or the like, cast for several days, and the THF is evaporated to produce a thin-film extractant-encapsulated polymer membrane containing the extractant.

[0024] By forming an extractant-containing polymer membrane, it is possible to more efficiently separate and extract metals by utilizing not only the characteristics of the extractant but also the characteristics of the difference in the speed of metal ions passing through the membrane. In addition, since forward extraction (adsorption) and back extraction (desorption) can be repeated by contacting both sides of the membrane with solutions of different pH ranges, forward extraction and back extraction can be performed in one step, making it a simple separation and extraction process.

[0025] 3. How scandium is extracted The metals in the aqueous phase in the present invention are solutions containing at least one rare earth metal or iron, and scandium is selectively separated and extracted from the solutions. The rare earth metals are 17 elements: scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

[0026] In the method for recovering scandium according to the present invention, the pH of an acidic aqueous solution containing metal ions is appropriately adjusted, and scandium alone can be selectively separated and extracted by contacting the solution with a deep eutectic solvent or a polymeric membrane containing a deep eutectic solvent. The concentrations of the metals in the aqueous phase are each independently 1×10 -4 Preferably, the concentration is 1M or less, and more preferably, 1×10 -3 ~0.1M.

[0027] Examples of the acid contained in the aqueous phase include mineral acids such as hydrochloric acid, nitric acid, and sulfuric acid, and organic acids such as formic acid, acetic acid, and oxalic acid, and preferably hydrochloric acid or nitric acid is used. The acid may be only one type, or may be a mixture of two or more types of acids. The pH of the aqueous solution is preferably 1.5 or less. The acid used to adjust the pH is the same as the above-mentioned acid. The base used to adjust the pH is, for example, NaOH, KOH, LiOH, and NH 3 Examples include:

[0028] The concentration of the deep eutectic solvent of the present invention is preferably 0.05 to 1 M, and when this is contained in a polymer membrane by impregnation, it is preferably contained in the polymer in the range of 1 to 5 mmol / g.

[0029] The aqueous phase used in this step is not particularly limited in terms of other components as long as it satisfies the above-mentioned requirements. For example, even if the aqueous phase contains metals other than rare earth metals and iron, scandium can be selectively extracted by the method of the present invention. EXAMPLES

[0030] The present invention will be described in more detail below with reference to examples, although the technical scope of the present invention is not limited to these examples.

[0031] First, for comparison, a solvent extraction method using a deep eutectic solvent was used to conduct an experiment on pH dependency. The experimental conditions are as shown in the table below. [Table 1]

[0032] 30cm 3In a sample tube, 3 mL of the aqueous phase (1M ammonium nitrate aqueous solution having a metal ion concentration of 1 mM) and 3 mL of the deep eutectic solvent as the organic phase were placed, and the mixture was shaken at 30 ° C. for 24 hours using a thermostatic bath. The deep eutectic solvent was prepared by taking 20 g of N-lauroyl sarcosine (manufactured by Tokyo Kasei Co., Ltd.) and 10 g of tri-n-octylphosphine oxide (manufactured by Tokyo Kasei Co., Ltd.) into an Erlenmeyer flask, dissolving at a high temperature of about 40 ° C., and using the liquid at room temperature without diluent. Next, the aqueous phase was collected, and the pH was measured using a pH meter, and the initial metal ion concentration and the metal ion concentration of the aqueous phase after equilibrium were measured using an ICP emission spectrometer and an atomic absorption spectrometer, and the extraction rate was calculated using the following formula. Extraction rate (%) = (initial metal ion concentration [mmol dm -3 ]-Metal ion concentration in the aqueous phase after equilibrium [mmol dm -3 ]) / initial metal ion concentration [mmol dm -3 ] x 100

[0033] Figure 1 shows the extraction results (pH dependence) from a mixed solution of various metal ions using a solvent extraction method that uses a deep eutectic solvent. Figure 1 makes clear that the extractant used this time (a deep eutectic solvent using NLS and TOPO) has higher extraction selectivity for scandium than for iron at low pH levels below 0.5. However, since about 60% of yttrium is extracted even at a pH of around 0.5, it is believed that mutual separation of these three elements will be difficult. However, it is highly promising as a separation material for iron and scandium.

[0034] Next, the above-mentioned deep eutectic solvent was incorporated into the extractant-containing polymer membrane, and an experiment was conducted to examine the pH dependence of the metal ions by adsorption using the adsorption method. The experimental conditions are as shown in the table below. [Table 2]

[0035] 0.15 g of the extractant-containing polymer membrane, which serves as the adsorbent, was placed in 5 mL of the aqueous phase (1 M ammonium nitrate aqueous solution with a metal ion concentration of 1 mM), and the mixture was shaken for 24 hours at 30° C. using a thermostatic bath. The extractant-containing polymer membrane was prepared by using polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP) as the polymer material, and the adsorbent was prepared by incorporating 60 wt % of the deep eutectic solvent (NLS / TOPO=2 / 1) prepared by the above-mentioned method in 40 wt % of the polymer material.

[0036] Figure 2 shows the results of adsorption (pH dependence) from a mixed solution of various metal ions using an adsorption method using an extractant-containing polymer membrane. From Figure 2, it was revealed that even though the same deep eutectic solvent was used, the selectivity of yttrium was significantly reduced by including it in the polymer membrane compared to the solvent extraction method, and only scandium was selectively adsorbed at low pH levels below pH 1.5. Furthermore, in the case of the adsorption method, the amount of deep eutectic solvent used was about 1 / 30 compared to the solvent extraction method in Figure 1, and the adsorption efficiency was very good. In this way, by using a deep eutectic solvent consisting of multiple extractants and including it in the polymer membrane, the amount of extractant used can be reduced, and only scandium can be selectively extracted efficiently and at low cost. The amount of deep eutectic solvent used varies depending on the type of polymer and the ratio of inclusion, but since it is possible to include about 20 to 80%, it is only necessary to use a very small amount of 0.8 g per 1 g of membrane.

[0037] Next, an experiment was carried out to examine the effect of shaking time on the adsorption of various metal ions from a mixed solution by the extractant-encapsulated polymer membrane. The experimental conditions are as shown in the table below. [Table 3]

[0038] 0.15 g of the extractant-encapsulating polymer membrane, which serves as the adsorbent, was placed in 30 mL of the aqueous phase (1 M ammonium nitrate aqueous solution with a metal ion concentration of 0.5 mM), and the mixture was shaken for 24 hours at 30° C. using a thermostatic bath. The extractant-encapsulating polymer membrane was prepared by encapsulating 80 wt% of the deep eutectic solvent (NLS / TOPO=2 / 1) prepared by the above-mentioned method in 20 wt% of the polymer material.

[0039] The results of adsorption from a mixed solution of various metal ions using an extractant-encapsulated polymer membrane (the effect of shaking time) are shown in Figure 3. As shown in Figure 3, it was clear that the adsorption equilibrium was reached in about 2 hours, and that the adsorption speed was comparable to that of solvent extraction. [Industrial Applicability]

[0040] The extractant of the present invention is capable of selectively separating and recovering scandium from a solution containing rare earth metals or iron, thereby enabling trace amounts of scandium contained in ores and waste materials discharged from the electronics industry to be efficiently separated and extracted at low cost.

Claims

1. An extractant for selectively separating and extracting scandium from a solution containing rare earth metals or iron, comprising: The extractant is a deep eutectic solvent prepared by mixing N-lauroyl sarcosine (formula III) and a trialkylphosphine oxide compound (formula I). (Formula I) 【Chemistry 1】 (In the formula, R1, R2, and R3 each represent an alkyl group having 1 to 20 carbon atoms.) (Formula III) 【Chemistry 3】

2. 2. The extractant according to claim 1, characterized in that the trialkylphosphine oxide compound is tri-n-octylphosphine oxide (formula II). (Formula II) 【Chemistry 2】

3. 3. The extractant according to claim 1 or 2, characterized in that the rare earth metal is yttrium.

4. An adsorbent comprising an extractant according to any one of claims 1 to 3, a polymeric material and a plasticizer, and formed into a thin film.

5. A method for selectively separating and extracting scandium from a solution containing rare earth metals or iron, comprising the steps of: An extraction method using a deep eutectic solvent prepared by mixing N-lauroyl sarcosine (formula III) and a trialkylphosphine oxide compound (formula I). (Formula I) 【Chemistry 1】 (In the formula, R1, R2, and R3 each represent an alkyl group having 1 to 20 carbon atoms.) (Formula III) 【Chemistry 3】

6. The extraction method according to claim 5, characterized in that the separation and extraction method uses an adsorbent formed into a thin film containing the deep eutectic solvent, a polymer material and a plasticizer, and the pH of the solution is 1.5 or less.

Citation Information

Patent Citations

  • Purification of rare-earth element

    JP1989108119A

  • Method for capturing scandium

    JP1989246328A

  • Extracting agent for rare earth metal and method of extracting it

    JP1992036373A

  • Recovering method of rare earth metal

    JP1997291320A

  • Method for recovering tantalum compound and / or niobium compound from composite containing various metallic compounds

    JP1998212532A