Graphene laminate and method for producing same

The graphene laminate with an intermediate layer of nanographene and impurities addresses substrate-induced conductivity shifts, ensuring stable electrical properties for graphene films, suitable for large-area applications.

JP7558569B2Active Publication Date: 2024-10-01NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021069176
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-15
Publication Date
2024-10-01
Estimated Expiration
2041-04-15

AI Technical Summary

Technical Problem

Existing methods for producing graphene laminates struggle to control electrical characteristics due to the influence of charged impurities from substrates, leading to unpredictable carrier conductivity and device performance issues.

Method used

A graphene laminate structure is developed with an intermediate layer containing nanographene and impurities that act as hole killers, sandwiched between the substrate and graphene film, using methods like CVD and ultraviolet irradiation to form the laminate.

Benefits of technology

The intermediate layer effectively blocks the influence of charged impurities, maintaining the original characteristics of graphene, enabling ambipolar conductivity and controlled carrier density, suitable for large-area substrates at low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558569000001
    Figure 0007558569000001
  • Figure 0007558569000002
    Figure 0007558569000002
  • Figure 0007558569000003
    Figure 0007558569000003
Patent Text Reader

Abstract

To provide a graphene laminate with controlled electrical properties and a fabrication method of the same.SOLUTION: A graphene laminate includes a substrate 102 with an insulating surface, an intermediate layer 104 located on and in contact with the substrate, and a graphene film 106 located on and in contact with the intermediate layer. The intermediate layer comprises nanographene containing impurities that act as hole killers. The graphene film has a structure in which one, two or three layers of single-layer graphene are stacked. The conductivity of the intermediate layer is lower than that of the graphene film. A thickness of the intermediate layer is 0.3 nm or more and 300 nm or less, and a thickness of the graphene film is 0.3 nm or more and 1.0 nm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One embodiment of the present invention relates to a graphene stack and a method for producing the same. [Background technology]

[0002] Various two-dimensional materials have been attracting attention as semiconductor materials to replace silicon. Examples of two-dimensional materials include graphene and molybdenum disulfide (MoS 2 ) and other transition metal dichalcogenides are known. Graphene, one of the two-dimensional materials, is sp 2 Graphene is a carbon nanomaterial composed of carbon atoms, and due to its unique two-dimensional structure, it has distinctive electrical properties such as high electron mobility. For this reason, graphene and its laminated films are expected to be used not only as materials for forming transparent conductive films and wiring, but also as key materials for electronic devices such as high-frequency devices and sensors.

[0003] Graphene can be synthesized by various methods, and for example, a method is known in which a film containing graphene is deposited on the surface of a thin copper film by chemical vapor deposition (CVD) (see Patent Document 1 and Non-Patent Document 1). In addition, when a film containing graphene is transferred onto a substrate such as a glass substrate, it is known that the substrate is chemically modified or an insulating film such as boron nitride is formed on the substrate in order to suppress the influence of the substrate on the electrical characteristics (see Non-Patent Documents 2 to 5). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-162442 A [Non-patent literature]

[0005] [Non-Patent Document 1] Takatoshi Yamada and 2 others, "Potassium-doped n-type stacked graphene layers", Material Research Express, (USA), 2019, Vol. 6, p.055009 [Non-Patent Document 2] Nagashio, K. and 4 others, "Electrical transport properties of graphene on SiO2 with specific surface structures," Journal of Applied Physics, (USA), 2011, Vol. 110, p.024513-1-024513-6 [Non-Patent Document 3] Lafkioti, Mirsini, et al., "Graphene on a Hydrophobic Substrate: Doping Reduction and Hysteresis Suppression under Ambient Conditions," NANO Letters, (USA), 2010, Vol. 10, pp. 1149-1153 [Non-Patent Document 4] Watanabe, Kenji, et al., "Direct-bandgap properties and evidence for ultraviolet lasing of hexagonal boron nitride single crystal," Nature Materials, (UK), 2004, Vol. 3, p. 404-409 [Non-Patent Document 5] Dean, CR, et al., "Boron nitride substrates for high quality graphene electronics," Nature Nanotechnology, (UK), 2010, Vol. 5, pp. 772-726 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of one embodiment of the present invention is to provide a stack of two-dimensional materials having a novel structure and a method for manufacturing the same. For example, an object of one embodiment of the present invention is to provide a graphene stack having a novel structure and a method for manufacturing the same. Alternatively, an object of one embodiment of the present invention is to provide a graphene stack having controlled electrical properties and a method for manufacturing the same. [Means for solving the problem]

[0007] One embodiment of the present invention is a graphene laminate comprising a substrate having an insulating surface, an intermediate layer located on the substrate and in contact with the substrate, and a graphene film located on the intermediate layer and in contact with the intermediate layer. The intermediate layer includes nanographene containing impurities that function as a hole killer.

[0008] One embodiment of the present invention is a method for producing a graphene laminate. The method includes forming a graphene film on a first support substrate, forming a resin film on the graphene film, removing the first support substrate, forming an intermediate layer on a second support substrate, bonding the graphene film and the intermediate layer, removing the second support substrate, bonding a substrate having an insulating surface to the intermediate layer such that the insulating surface is in contact with the intermediate layer, and removing the resin film. The intermediate layer includes nanographene containing impurities that function as hole killers.

[0009] One embodiment of the present invention is a method for producing a graphene laminate, which includes forming a first graphene film on a first support substrate, irradiating the first graphene film with ultraviolet light, forming a first resin layer on the first graphene film irradiated with ultraviolet light, removing the first support substrate, treating the first graphene film irradiated with ultraviolet light with an aqueous solution of potassium hydroxide to convert the first graphene film irradiated with ultraviolet light into an intermediate layer containing nanographene containing impurities that function as a hole killer, bonding the intermediate layer to a substrate having an insulating surface, removing the first resin layer, forming a second graphene film on a second support substrate, forming a second resin layer on the second graphene film, removing the second support substrate, bonding the second graphene film to the intermediate layer, and removing the second resin layer. Effect of the Invention

[0010] According to one embodiment of the present invention, it is possible to provide a graphene stack having controlled electrical properties and a method for producing the same. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic end view of a graphene stack according to one embodiment of the present invention. [Diagram 2] 1A to 1C are schematic end views illustrating a method for producing a graphene laminate according to one embodiment of the present invention. [Diagram 3] 1A to 1C are schematic end views illustrating a method for producing a graphene laminate according to one embodiment of the present invention. [Figure 4] 1A to 1C are schematic end views illustrating a method for producing a graphene laminate according to one embodiment of the present invention. [Diagram 5] 1 is an X-ray photoelectron spectroscopy (XPS) spectrum of the intermediate layer of Example 1. [Figure 6] 4 is an XPS spectrum of the intermediate layer of Example 2. [Figure 7] 3 is a transmission electron microscope (TEM) image of a cross section of the intermediate layer of Example 1. [Figure 8] TEM image of a cross section of the intermediate layer of Example 2. [Figure 9] 4 shows Raman spectra of the graphene laminates of Examples 1 and 2 and the laminates of Comparative Examples 1 and 2. [Figure 10] A plot of the ratio (ID / IG) of the D band peak intensity (ID) to the G band peak intensity (IG) for the graphene laminates of Examples 1 and 2 and the laminates of Comparative Examples 1 and 2, with the horizontal axis representing the ratio (I2D) of the 2D band peak intensity (I2D) to IG with the vertical axis representing the ratio (I2D / IG). [Figure 11] 1 is a plot of the half-width of the 2D band (Γ2D) versus the half-width of the G band (ΓG) for the graphenes of Examples 1 and 2 and the stacks of Comparative Examples 1 and 2. [Figure 12] 1A and 1B are schematic top and end views of a transistor for evaluating the electrical properties of a graphene stack according to one embodiment of the present invention. [Figure 13] 1 is a plot of resistance versus gate-source voltage (VGS) for transistors of Examples 3 and 4 and Comparative Example 3. [Figure 14] 13 is a plot of resistance versus VGS for transistors of Example 4 and Comparative Example 4. [Figure 15] Schematic diagram showing the resistance vs. gate-source voltage (VGS) characteristics of a field-effect transistor with a graphene channel layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the invention disclosed in this application will be described. The present invention can be implemented in various forms without departing from the gist of the invention, and should not be construed as being limited to the description of the embodiments exemplified below. Even if the effects and advantages brought about by the following embodiments are different from those brought about by the following embodiments, those that are clear from the description in this specification or that can be easily predicted by a person skilled in the art are naturally understood to be brought about by the present invention.

[0013] In order to clarify the description, the drawings may show the width, thickness, shape, etc. of each part in a schematic manner compared to the actual embodiment, but these are merely examples and do not limit the interpretation of the present invention. In this specification and each drawing, elements having the same functions as those described in the previous drawings may be given the same reference numerals, and duplicated descriptions may be omitted.

[0014] In this specification and the claims, when describing an aspect in which a structure is placed on top of another structure, the term "on top" is used, unless otherwise specified, to include both a case in which another structure is placed directly on top of a structure so as to be in contact with the structure, and a case in which another structure is placed above a structure via yet another structure.

[0015] As used herein, single-layer graphene refers to sp 2 It refers to a material in which carbon atoms are arranged in a two-dimensional honeycomb lattice and have a thickness of one atomic layer. Monolayer graphene is one of the layers that make up the layered structure of graphite, and is also simply called graphene. Nanographene is a continuous or laminated body of graphene with domains of 200 nm or less. Nanographene is a continuous or laminated body of graphene with domains of preferably 5 nm to 20 nm. The thickness of nanographene varies depending on the synthesis conditions, but can be 0.3 nm or more and 300 nm or less. Graphene film refers to a laminate of one, two, or three monolayer graphene layers.

[0016] 1. Graphene laminate structure 1A and 1B are schematic end views of a graphene laminate 100 according to one embodiment of the present invention. As shown in FIG. 1A, the graphene laminate 100 includes a substrate 102, an intermediate layer 104, and a graphene film 106.

[0017] 1-1. Circuit board The substrate 102 has an insulating surface on which the intermediate layer 104 is provided. The substrate 102 may include an inorganic insulator such as glass, quartz, sapphire, alumina, etc., or may include a polymer such as a polyester, exemplified by polyimide, polycarbonate, and polyethylene terephthalate. When the substrate 102 includes an inorganic insulator or a polymer, the surface of the substrate 102 functions as the insulating surface.

[0018] Alternatively, the substrate 102 may include a base material 108 containing a semiconductor or a metal (a zero-valent metal) and an insulating layer 110 located on the base material 108 (FIG. 1(B)). In this case, the surface of the insulating layer 110 functions as the insulating surface of the substrate 102, and the intermediate layer 104 is provided thereon. The semiconductor contained in the base material 108 may be not only a Group 14 element such as silicon or germanium, but also a compound semiconductor such as gallium arsenide, gallium phosphide, indium phosphide, or silicon carbide. A typical example of a semiconductor is single crystal silicon. Examples of metals contained in the base material 108 include alloys such as copper, aluminum, iron, molybdenum, titanium, tantalum, and stainless steel.

[0019] The insulating layer 110 may be a silicon-containing inorganic compound such as silicon oxide or silicon nitride, an insulating metal nitride such as titanium nitride, or a high-dielectric inorganic oxide or inorganic oxynitride such as hafnium oxide or yttrium oxide. The insulating layer 110 may be formed by applying a CVD method or a sputtering method, or by oxidizing the surface of the substrate 108 or by implanting oxygen ions into the substrate 108. For example, the insulating layer 110 may be formed by using single crystal silicon as the substrate 108 and thermally oxidizing the surface in the presence of oxygen gas.

[0020] 1-2. Middle class The intermediate layer 104 is provided so as to contact the insulating surface of the substrate 102. The intermediate layer 104 includes nanographene and further includes impurities that act as hole killers for holes injected into the nanographene. The intermediate layer 104 has lower electrical conductivity than the graphene film 106. The following two examples of the intermediate layer 104 can be given.

[0021] (1) Intermediate layer containing damage-free nanographene An example of the intermediate layer 104 is nanographene containing a group 15 element such as nitrogen or phosphorus, preferably nitrogen, as an impurity. The content of the group 15 element in the intermediate layer 104 is, for example, 0.01% by mass or more and 5.0% by mass or less. In this intermediate layer 104, the layer structure of the graphene is relatively clear, and as shown in the examples, the layered structure of each graphene corresponding to the domain size can be clearly observed in a TEM image of the cross section. For this reason, in order to distinguish from the intermediate layer 104 containing damaged nanographene described later, this intermediate layer 104 is also called an "intermediate layer containing damageless nanographene" for convenience. The domain size of the nanographene contained in the intermediate layer 104 is 300 nm or less, for example, 5 nm to 20 nm. The thickness of the intermediate layer 104 is, for example, 0.3 nm to 300 nm, 1 nm to 50 nm, 3 nm to 10 nm, or 3 nm to 7.5 nm. When nitrogen is contained as an impurity, the XPS spectrum of the intermediate layer 104 shows a peak at about 398 eV originating from the 1s orbital of nitrogen. As will be described later, one method of producing the intermediate layer 104 is a CVD method in the presence of plasma (plasma CVD, PCVD), in which case nitrogen can be introduced into the intermediate layer 104 by using nitrogen gas contained in the residual gas in the chamber or nitrogen gas introduced into the chamber.

[0022] (2) Intermediate layer containing damaged nanographene Another example of the intermediate layer 104 is an intermediate layer containing damaged nanographene. This intermediate layer 104 contains Group 1 metal elements such as sodium, potassium, and lithium as impurities, and a typical impurity is potassium. These impurities are present in the intermediate layer 104 as ions. The content of the Group 1 metal elements in the intermediate layer 104 is, for example, 0.01 mass% to 5 mass%. As described later, this type of intermediate layer 104 can be obtained by irradiating a graphene film with ultraviolet light to damage it, and then treating it with a solution or suspension of a compound containing an impurity such as potassium hydroxide. For this reason, peaks due to impurities are observed in the XPS spectrum. For example, when potassium is contained as an impurity, peaks due to potassium are observed around 291 eV and 294 eV. In addition, the ultraviolet light irradiation breaks the bonds between carbons and damages the structure, so that the domain size of the graphene film decreases and some of it is stacked. In other words, the impurity doping and ultraviolet light irradiation cause the graphene film to transition to a structure in which graphene with reduced domain size is stacked, that is, nanographene. Therefore, like the intermediate layer 104 including damageless nanographene, the thickness of the intermediate layer 104 including damageless nanographene is, for example, 0.3 nm to 300 nm, 1 nm to 50 nm, 3 nm to 10 nm, or 3 nm to 7.5 nm. However, the layered structure is not clear compared to the intermediate layer 104 including damageless nanographene. For example, although the layered structure of graphene is confirmed in a TEM image of a cross section, the regularity of the structure is lower compared to the intermediate layer 104 including damageless nanographene.

[0023] Graphene The graphene film 106 is provided so as to be in contact with the intermediate layer 104. As described above, the graphene film has a structure in which one, two, or three single-layer graphene layers are laminated, and since the thickness of the single-layer graphene is about 0.34 nm, the thickness of the graphene film 106 is 0.3 nm or more and 1 nm or less.

[0024] 2.Characteristics of graphene laminates 2-1.Raman spectrum When the graphene film 106 is a single-layer graphene, the graphene laminate 100 includes an intermediate layer 104 including nanographene and a graphene film 106 including single-layer graphene. For this reason, in the resonant Raman spectrum of the graphene laminate 100, the G band and 2D band, which are bands derived from graphene, and the D band due to defects are located at 1585 cm -1 , 2700cm -1 , 1350cm -1 Observed nearby.

[0025] However, the intensity ratio and half-width of these Raman bands do not simply depend on the abundance ratio of monolayer graphene and nanographene, but have characteristic values. Specifically, the peak intensity (I G ) versus the 2D band peak intensity (I 2D ) ratio (I 2D / I G ) are about 2.65 and 0.25, respectively. In contrast, the I 2D / I G The I of monolayer graphene and nanographene is distributed in the range of 0.30 to 2.51 or 0.60 to 2.50. G D band peak intensity (I D ) ratio (I D / I G ) are about 0.20 and 2.25, respectively. In contrast, the I D / I G is distributed in the range of 0.16 to 2.10 or 0.16 to 1.5.

[0026] Similarly, the half-width (Γ G ) are approximately 20.0 cm -1 , 46.0cm -1 In contrast, Γ of the graphene laminate 100 G is 24.4cm -1 More than 60.1cm -1 The range is as follows: GThe half-width (Γ) of the 2D band of single-layer graphene and nanographene is shown. 2D ) are approximately 35.0 cm -1 , 150.0cm -1 whereas the Γ of the graphene stack 100 2D is 20.6 cm -1 155.0cm or more -1 Less than or equal to 35.0cm -1 More than 90.0cm -1 It is distributed in the following range:

[0027] By utilizing such a distribution of spectral characteristics, a graphene laminate 100 containing nanographene can be distinguished from nanographene or single layer graphene.

[0028] 2-2.Electrical characteristics In the application of graphene-containing films to electronic devices, graphene may be formed on a substrate having an insulating surface. In this case, the graphene-containing film may be affected by charged impurities contained on the substrate. In particular, graphene is a material having a thickness of substantially one atomic layer, so it is easily affected by charged impurities. For example, when a glass substrate or a quartz substrate, which is one of typical substrates, is used, the hole density increases due to the influence of the charged impurities contained in the substrate. As a result, the Dirac point shifts in the positive direction, that is, the carrier conduction of graphene becomes p-type. Such a change in carrier conductivity significantly changes the electrical properties of the graphene-containing film, such as a decrease in mobility, making it difficult to control the device properties.

[0029] For example, the resistance vs. gate-source voltage (V GS) characteristics, as shown by the solid line in Figure 15, the voltage at which the resistance is maximum (Dirac point) is located on the positive side, and it is known that the inherent graphene characteristic of maximum resistance being 0 V (see the dotted line in Figure 15) cannot be obtained. This is explained by the injection of holes from the substrate into graphene. It has been reported that this phenomenon can be solved by using hexagonal boron nitride (h-BN) synthesized at high temperature and high pressure, but high temperature and high pressure synthesized h-BN is in the form of flakes of about several hundred micrometers, so it is not suitable as a substrate material from the viewpoint of industrial application. Research and development has also been conducted on the synthesis of h-BN thin films using the CVD method, but ideal device characteristics have not yet been realized, and the current situation is that the only way to realize graphene devices is to wait for the synthesis of high-quality, large-area h-BN.

[0030] However, as shown in the examples, the inventors have found that the inherent properties of graphene can be brought out by forming an intermediate layer 104 between the substrate 102 and the graphene film 106, which functions as a layer that compensates for hole injection. Specifically, by providing the graphene film 106 on the substrate 102 via the intermediate layer 104, the intermediate layer 104 can block the influence of charged impurities, and can effectively prevent carrier conduction shift of the graphene film 106. That is, it is possible to fabricate on the substrate 102 a graphene film 106 with ambipolar conduction that is prevented from becoming p-type, has a low carrier density, and exhibits a Dirac point in the substantial absence of an external electric field. Furthermore, the distance from the graphene film 106, which forms the channel layer of the electronic device, to the substrate 102 can be increased by the intermediate layer 104, so that the influence of Coulomb scattering due to charged impurities on the surface of the substrate 102 can also be reduced.

[0031] Due to such an effect, the intrinsic carrier density of the graphene film 106 in the graphene laminate 100 is, for example, 1.0×10 10 cm -2 Above 1.0×10 12 cm -2 Below, 1.0 x 10 10 cm -2 Above 5.0×10 11 cm -2or less, or 8.6 x 10 10 cm -2 More than 1.7 x 10 11 The Dirac point of the graphene film 106 in the graphene laminate 100 is the V GS The Dirac point appears when V is between -2.0 V and 2 V, between -1.5 V and 1.0 V, or between -1.5 V and 0.0 V. GS The above-mentioned electrical characteristics were measured by fabricating a transistor including the graphene film 106 containing single-layer graphene as a channel layer, and measuring the electrical conductivity at room temperature and a resistance of 1.0×10 -2 Pa or more 1.0×10 -1 The source-drain resistance V GS The measurement method may be any method, such as a four-terminal measurement method, a three-terminal measurement method, or a two-terminal measurement method.

[0032] As described later, the intermediate layer 104 can be formed under relatively mild conditions (e.g., 400° C. to 600° C.) by applying a general PCVD method, and therefore can be formed even on a large-area substrate 102. Furthermore, since surface modification of the substrate 102 is not required, the application of the embodiment of the present invention makes it possible to provide the graphene laminate 100 at low cost.

[0033] 3. Method for producing graphene laminates The following describes a method for producing the graphene laminate 100. The production method described below is an example that uses a transfer method, and the graphene laminate 100 may be formed by applying other methods.

[0034] 3-1. Graphene laminate including damage-free nanographene FIG. 2 shows a method for producing a graphene laminate 100 having an intermediate layer 104 containing damage-less nanographene.

[0035] First, a graphene film 106 is formed (step S01). The graphene film 106 is formed by placing a support substrate (hereinafter, first support substrate) 120 in a chamber and growing graphene on the first support substrate 120 by applying a thermal CVD method. The temperature at which graphene is grown is, for example, 600° C. or higher and 1200° C. or lower, and under these conditions, a graphene film 106 having one atomic layer is obtained. As reactive gases in the thermal CVD method, raw material gases such as methane, ethane, acetylene, ethanol, and benzene, and reducing gases such as hydrogen are used.

[0036] The first support substrate 120 has at least a metal having catalytic activity for growing graphene on the surface. Therefore, the first support substrate 120 may be a metal plate or metal foil containing a metal having catalytic activity, such as gold, silver, copper, nickel, molybdenum, chromium, iridium, or platinum, or an alloy such as stainless steel or nickel-chromium. Alternatively, the first support substrate 120 may be an insulating substrate or a semiconductor substrate on which a metal layer containing the above-mentioned metal or alloy is formed. Examples of the insulating substrate include a glass substrate, a quartz substrate, and a sapphire substrate, and examples of the semiconductor substrate include a single crystal silicon substrate. Typically, a glass substrate, a quartz substrate, a sapphire substrate, or a silicon substrate, and a copper thin film, a copper foil, or a copper plate provided thereon are provided as the first support substrate 120.

[0037] The intermediate layer 104 is formed on a support substrate (hereinafter, second support substrate) 124 different from the first support substrate 120 (step S02). The second support substrate 124 may be a substrate similar to the first support substrate 120. The intermediate layer 104 may be formed by applying a PCVD method at a temperature of, for example, 400° C. to 600° C. In this case, microwaves may be irradiated. The reactive gas may be any gas that can be used in step S01. When the intermediate layer 104 is formed by the PCVD method, a small amount of nitrogen contained in the chamber or reactive gas is taken into the intermediate layer 104, so that the intermediate layer 104 containing nitrogen as an impurity can be formed. A small amount of nitrogen or phosphorus may be separately introduced into the reactive gas or chamber as an impurity source.

[0038] Subsequently, the graphene film 106 and the intermediate layer 104 are transferred. Specifically, a resin layer 122 is formed on the graphene film 106 (step S03). Examples of the resin layer 122 include, but are not limited to, acrylic resins such as polymethyl methacrylate, aliphatic polyimides such as poly(methyl glutarimide), epoxy resins, and water-soluble polymers such as polyvinyl alcohol. A material that is soluble in an organic solvent or water, which will be described later, and that can be removed from the graphene film 106 can be used as the resin layer 122. Examples of methods for forming the resin layer 122 include a spin coating method, an inkjet method, a dip coating method, and a printing method.

[0039] Next, the first support substrate 120 is removed (step S04). Specifically, the first support substrate 120 is removed by using an etchant that dissolves a metal that functions as a catalyst. As the etchant, for example, an aqueous solution of ferric chloride, an aqueous solution of ammonium persulfate, an inorganic acid such as nitric acid, or an aqueous solution of an organic acid such as methanesulfonic acid is used.

[0040] Thereafter, the intermediate layer 104 and the graphene film 106 on the second support substrate 124 are bonded (step S05). Specifically, the resin layer 122 and the second support substrate 124 are placed opposite each other so as to sandwich the intermediate layer 104 and the graphene film 106, and are brought into close contact with each other, thereby performing bonding. After bonding, the second support substrate 124 is removed (step S06) in the same manner as the first support substrate 120 is removed (step S04). This results in a structure in which the graphene film 106 and the intermediate layer 104 are laminated in this order on the resin layer 122.

[0041] Subsequently, the substrate 102 is bonded to the intermediate layer 104 (step S07). Specifically, the resin layer 122 and the substrate 102 are placed opposite each other so as to sandwich the intermediate layer 104 and the graphene film 106 therebetween, and are then brought into close contact with each other, thereby performing bonding.

[0042] Finally, the resin layer 122 is removed (step S08). Specifically, the resin layer 122 is removed by immersing in a solvent that dissolves the resin layer 122. In addition to water, the solvent may be ketones such as acetone and methyl ethyl ketone, aromatic solvents such as toluene and xylene, halogenated solvents such as methylene chloride and chloroform, or ether solvents such as tetrahydrofuran and dioxane. As an optional step, after removing the resin layer 122 with the solvent, a trace amount of the remaining resin layer 122 may be removed by heat treatment. For example, the remaining resin layer 122 is removed by heat treatment at a temperature of 300° C. to 500° C. in a mixed gas of an inert gas such as argon or nitrogen and hydrogen gas, or in a vacuum atmosphere.

[0043] Through the above steps, the graphene laminate 100 can be produced. In this method, both the intermediate layer 104 and the graphene film 106 can be formed by a CVD method, and chemical surface modification of the substrate 102 is not required. Therefore, it is possible to provide the graphene laminate 100 at low cost by using a large substrate 102.

[0044] 3-2. Graphene laminate including damaged nanographene A method for producing a graphene laminate 100 having an intermediate layer 104 containing damaged nanographene is shown in FIG. 3 and FIG.

[0045] First, a graphene film (hereinafter, precursor) 126, which is a precursor of the intermediate layer 104, is formed on a first support substrate 120 (step S10). The same substrate as the first support substrate 120 in step S01 can be used as the first support substrate 120. The formation of the precursor 126 may be performed in the same manner as the graphene growth described in step S01. Subsequently, the precursor 126 is irradiated with ultraviolet light (step S11). The wavelength of the irradiated ultraviolet light is, for example, 100 nm to 400 nm, 280 nm to 400 nm, or 315 nm to 400 nm, and a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, or a deuterium lamp may be used as a light source. By this step, the precursor 126 is damaged, at least a part of it causes carbon loss, and the precursor 126 containing damaged graphene is formed. A resin layer 122 is formed on the precursor 126 (step S12), and the first support substrate 120 is removed (step S13). The formation of the resin layer 122 and the removal of the first support substrate 120 may be performed in the same manner as in steps S03 and S04, respectively.

[0046] Then, impurities are added (doped) (step S14). Specifically, a laminate of the resin layer 122 and the precursor 126 including damaged graphene provided thereon is immersed in a solution or suspension containing impurities. Examples of the solution containing impurities include an aqueous solution of potassium hydroxide, an aqueous solution of sodium hydroxide, and an aqueous solution of lithium hydroxide. Examples of the compound containing impurities are not limited to the above-mentioned Group 1 metal hydroxides, and may be, for example, carbonates or hydrogen carbonates of Group 1 metals. By this step, ions of the Group 1 metal are doped into the precursor 126, and the precursor 126 is converted into the intermediate layer 104.

[0047] Thereafter, the precursor 126 is transferred onto the substrate 102. That is, the intermediate layer 104 is bonded to the substrate 102 (step S15) in the same manner as in step S07, and then the resin layer 122 is removed (step S16) in the same manner as in step S07. Through these steps, the intermediate layer 104 is formed on the substrate 102.

[0048] Meanwhile, the graphene film 106 is provided on a second support substrate 124 different from the first support substrate 120 (step S17). After that, a resin layer 122 is formed on the graphene film 106, and the second support substrate 124 is removed (steps S18 and S19). These steps are similar to the above-mentioned steps S01, S03, and S04, and therefore the description thereof will be omitted.

[0049] Next, the intermediate layer 104 and the graphene film 106 are bonded (FIG. 4, step S20). Specifically, the resin layer 122 and the substrate 102 are placed opposite each other so that the intermediate layer 104 and the graphene film 106 are sandwiched between them, and the bonding is performed by bringing them into close contact with each other. Finally, the resin layer 122 is removed in the same manner as in step S08, and the graphene laminate 100 can be obtained (step S21).

[0050] In this method, both the intermediate layer 104 and the graphene film 106 can be formed by the CVD method, and there is no need to chemically modify the surface of the substrate 102. Therefore, it is possible to provide the graphene laminate 100 at low cost using a large substrate 102. EXAMPLES

[0051] 1. Preparation of Graphene Stacks 1-1. Example 1: Preparation of a graphene laminate containing damage-free nanographene as an intermediate layer The graphene laminate 100 was produced by the above-mentioned steps S01 to S08. Specifically, a substrate (manufactured by Graphenea) having a graphene film 106 formed on a copper foil was used, and a 2 wt % anisole solution of polymethyl methacrylate was applied onto the graphene film 106 to form a resin layer 122. Furthermore, the obtained laminate was treated with an aqueous ammonium persulfate solution (0.5 mol / L) for 210 minutes to dissolve the first support substrate 120, and a laminate of the resin layer 122 and the graphene film 106 was obtained.

[0052] On the other hand, the intermediate layer 104 was formed by using a tough pitch copper foil (10 cm x 10 cm) with a purity of 99.9% as the second support substrate 124, introducing methane and hydrogen (flow rates of 3.27 sccm and 3.27 sccm, respectively) as reactive gases into the chamber, and treating the second support substrate 124 for 3 seconds while irradiating it with 4 kW microwaves under conditions of a pressure of 5 Pa and a temperature of 600°C.

[0053] Next, the laminate of the resin layer 122 containing polymethylmethacrylate and the graphene film 106 was bonded to the intermediate layer 104 formed on the second support substrate 124, and then the second support substrate 124 was removed by treating with an aqueous ammonium persulfate solution (0.5 mol / L) for 210 minutes. Furthermore, a p-type silicon substrate (1.6 cm×1.6 cm, thickness 0.5 mm) with a thermal oxide film formed on the surface was used as the substrate 102, and the substrate 102 was bonded to the graphene film 106. Thereafter, the resin layer 122 was removed using toluene and acetone, and the graphene laminate 100 was obtained.

[0054] 1-2. Example 2: Preparation of a graphene laminate including an intermediate layer containing damaged nanographene The graphene laminate 100 was produced by the above-mentioned steps S10 to S21. As in Example 1, a substrate (manufactured by Graphenea) having a graphene film formed on a copper foil by a thermal CVD method was used. Here, the graphene film corresponds to the precursor 126. The precursor 126 was irradiated with ultraviolet light at room temperature for 120 seconds using a UV cleaner (manufactured by Filgen, model number UV253V12) equipped with five 6 W high-pressure mercury lamps, to obtain a precursor 126 containing damaged nanographene.

[0055] Thereafter, a 2 wt % anisole solution of polymethylmethacrylate was applied onto the precursor 126 to form a resin layer 122. Furthermore, the obtained laminate was treated with ferric chloride (10 mol / L) for 60 minutes to dissolve the first support substrate 120, and a laminate of the resin layer 122 and the precursor 126 was obtained. Next, the laminate of the resin layer 122 and the precursor 126 was treated with a 0.5 mol / L potassium hydroxide aqueous solution at room temperature for 30 minutes to perform doping with potassium ions. After the treatment, the laminate was washed with pure water and dried. Through this process, the precursor 126 is converted into the intermediate layer 104.

[0056] Next, p-type silicon (1.6 cm x 1.6 cm, 0.5 mm thick) with a thermal oxide film formed on its surface was bonded to the intermediate layer 104 as the substrate 102, and the resin layer 122 was then removed using acetone to transfer the intermediate layer 104 onto the substrate 102.

[0057] Subsequently, a laminate of the resin layer 122 containing polymethyl methacrylate and the graphene film 106 was formed by the same method as described above, and the graphene film 106 was bonded to the intermediate layer 104. Thereafter, the resin layer 122 was removed with acetone, thereby obtaining the graphene laminate 100.

[0058] 2. Evaluation 2-1. Identification of impurities FIG. 5 shows an XPS spectrum of the intermediate layer 104 including damage-less nanographene formed on the second support substrate 124. The XPS spectrum was obtained using an X-ray photoelectron spectrometer manufactured by PHI and an AlKα radiation source. The measurement range was 400 μm (hereinafter the same). As shown in FIG. 5, it can be seen that the intermediate layer 104 including damage-less nanographene gives a peak at 397.9 eV corresponding to the 1s orbital of nitrogen. This result indicates that the intermediate layer 104 including damage-less nanographene contains nitrogen as an impurity. It is believed that the nitrogen is due to nitrogen gas remaining in the chamber.

[0059] Regarding the intermediate layer 104 containing damaged nanographene, the XPS measurement result of potassium-added damaged nanographene formed on silicon oxide is shown in Figure 6. As shown in Figure 6, it can be seen that the intermediate layer 104 gives peaks derived from potassium at around 294 eV and 297 eV (see the arrows in the figure). This result clearly indicates that the intermediate layer 104 containing damaged nanographene contains potassium as an impurity.

[0060] 2-2. Cross-sectional structure FIG. 7 shows a TEM image of a cross section of the intermediate layer 104 of Example 1 formed on the second support substrate 124. The TEM image was obtained using a transmission electron microscope manufactured by JEOL (hereinafter the same). From this TEM image, it can be seen that the intermediate layer 104 contains nanographene composed of multiple graphene layers. In addition, this layered structure is clear, and the graphene layers are relatively regularly layered over a domain size of about 2 nm to 10 nm. From this cross-sectional TEM image, it was confirmed that the thickness of the intermediate layer 104 of Example 1 was about 5 nm.

[0061] 8 shows a TEM image of a cross section of the intermediate layer 104 of Example 2 formed on the substrate 102. From this TEM image, it can be seen that the intermediate layer 104 of Example 2 is composed of graphene layers having a single-layer to three-layer laminated structure. It can also be seen that, compared to the intermediate layer 104 of Example 1, the laminated structure of the intermediate layer 104 containing damaged nanographene is not clear, and the domain size is also limited to about 1 nm to 5 nm. From this cross-sectional TEM image, it was confirmed that the thickness of the intermediate layer 104 was about 1 nm.

[0062] 2-3.Raman spectrum FIG. 9 shows Raman spectra of the graphene laminates 100 obtained in Examples 1 and 2. The Raman spectra were measured with an excitation laser wavelength of 532 nm and a spot diameter of 1 μm. For comparison, the Raman spectra are shown of a laminate in which nanographene is formed directly on a p-type silicon substrate having a thermal oxide film formed on its surface (Comparative Example 1), and a laminate in which a single-layer graphene film is formed directly on a p-type silicon substrate having a thermal oxide film formed on its surface (Comparative Example 2). As can be seen from these spectra, in Examples 1 and 2, which are the graphene laminates 100 according to the embodiments of the present invention, the D band, G band, and 2D band derived from the nanographene and the graphene film are respectively at 1350 cm. -1 , 1585cm -1 , 2700cm -1 Observed nearby.

[0063] The Raman spectrum was measured at multiple points for the graphene laminate 100 of the example and the laminate of the comparative example. The G band peak intensity (I G ) versus D band peak intensity (I D ) ratio (I D / I G ) on the horizontal axis, I G The peak intensity of the 2D band (I 2D ) ratio (I 2D / I G 10 shows a plot diagram with the ratio (I D / I G ) ranges from 0.16 to 1.5, while the ratio (I 2D / I G ) was found to be distributed in the range of 0.60 to 2.50.

[0064] FIG. 11 shows the half-width (Γ) of the G band for the graphene laminate 100 of the example and the laminate of the comparative example. G ) vs. half-width of the 2D band (Γ 2D 11 shows plots of Γ. As shown in FIG. 11, the laminates of Comparative Examples 1 and 2 are each plotted at a single point. In contrast, in the graphene laminate 100 of the example, this plot is distributed in a rectangular region with Comparative Examples 1 and 2 as diagonals and also outside the region. In addition, the plot of the example deviates significantly from the straight line passing through the plots of Comparative Examples 1 and 2. In the graphene laminate 100 of the example, Γ G is 24.4cm -1 More than 60.1cm -1 Distributed in the following range, Γ 2D is 35.0cm -1 More than 90.0cm -1 It was found to be distributed in the following range:

[0065] 2-4.Electrical characteristics In order to evaluate the electrical characteristics of the graphene laminates 100 of Examples 1 and 2, a bottom-gate transistor 130 having a graphene film 106 as a channel layer was fabricated. A schematic top view of the fabricated transistor 130 is shown in FIG. 12(A), and schematic views of the end faces along the dashed lines AA′ and BB′ in FIG. 12(A) are shown in FIG. 12(B) and FIG. 12(C), respectively. The transistor 130 was fabricated by the following procedure. That is, after the graphene laminate 100 was bonded onto a p-type silicon semiconductor functioning as a gate electrode 132, a resist was formed on the graphene laminate 100, and the graphene film 106 and the intermediate layer 104 were etched using oxygen plasma. Thereafter, the source electrode 134, the drain electrode 136, and the measurement terminal 138 were formed by EB deposition. The source electrode 134, the drain electrode 136, and the measurement terminal 138 were stacked layers of nickel (10 nm) and gold (90 nm). The channel length and the channel width were 50 μm and 40 μm, respectively, in the transistor 130. Hereinafter, the transistors 130 including the graphene laminates 100 of Examples 1 and 2 will be referred to as Examples 3 and 4, respectively.

[0066] For comparison, transistors of Comparative Examples 3 and 4 were fabricated. The transistor of Comparative Example 3 does not include intermediate layer 104, and includes a graphene film formed directly on substrate 102 as a channel layer. On the other hand, the transistor of Comparative Example 4 includes an intermediate layer that is a layer fabricated by doping a graphene film formed directly on substrate 102 with potassium but without irradiating it with light, and graphene is laminated thereon.

[0067] The transistors of Examples 3 and 4 and Comparative Example 3 were subjected to heating at room temperature and a pressure of 1×10 -2 A four-terminal measurement was performed in the order of Pa, and the electrical resistance V GS The voltage dependence was evaluated. The results are shown in FIG. 13. As shown in FIG. 13, in Comparative Example 3, the Dirac point was GS (about 9 V), which indicates that the graphene is p-type. In addition, the plotted curve confirms that the graphene film exhibits ambipolar conduction. The graphene film is considered to have become p-type due to the influence of charged impurities contained in the substrate 102. The intrinsic carrier density of Comparative Example 3 was 1.9×10 12 cm -2 It was estimated that:

[0068] In contrast, in the transistor 130 of Example 3, the Dirac point is V GS It was also confirmed that the graphene film 106 exhibited ambipolar conduction. Similarly, in the transistor 130 of Example 4, the Dirac point appeared at a V GS It was confirmed that the graphene film 106 also exhibited ambipolar conduction in this case. GS The appearance of the Dirac point at 1000 nm suggests that the intermediate layer 104 effectively suppresses the influence of charged impurities contained in the substrate 102. The intrinsic carrier densities of the graphene films 106 in Examples 3 and 4 were 8.6×10 10 cm -2 , 1.7×10 11 This is approximately one to two orders of magnitude smaller than that of Comparative Example 3.

[0069] The measurement results of the transistor 130 of Example 4 and the transistor of Comparative Example 4 are also shown in FIG. 14. As can be seen from FIG. 14, compared to the transistor of Comparative Example 4, the transistor 130 of Example 4 having the intermediate layer 104 formed by ultraviolet irradiation has a peak position located on the positive side, and V GS It was confirmed that the Dirac point appears when the potential V s is approximately 0 V. This suggests that defects are generated in the intermediate layer 104 by irradiation with ultraviolet light, and that these defects more effectively suppress the effects of charged impurities.

[0070] As described above, by providing the intermediate layer 104 having nanographene containing impurities acting as hole killers between the graphene film 106 and the substrate 102, the influence of charged impurities can be effectively suppressed, and the graphene film 106 with controlled electrical properties can be obtained. In addition, since the intermediate layer 104 can be formed by applying a CVD method, the graphene film 106 with controlled electrical properties can be easily formed even on a large substrate 102. This suggests that the embodiment of the present invention will greatly contribute to the application of the graphene film 106 to electronic devices. [Explanation of symbols]

[0071] 100: graphene laminate, 102: substrate, 104: intermediate layer, 106: graphene film, 108: base material, 110: insulating layer, 120: first support substrate, 122: resin layer, 124: second support substrate, 126: precursor, 130: transistor, 132: gate electrode, 134: source electrode, 136: drain electrode, 138: measurement terminal

Claims

1. A substrate having an insulating surface; an intermediate layer located on and in contact with the substrate; and a graphene film located on the intermediate layer and in contact with the intermediate layer; The intermediate layer is a graphene laminate including nanographene containing impurities that function as a hole killer.

2. The graphene laminate according to claim 1 , wherein the graphene film has a structure in which one, two or three monolayer graphene layers are stacked.

3. The graphene laminate according to claim 1 , wherein the intermediate layer has a lower electrical conductivity than the graphene film.

4. The graphene laminate according to claim 1 , wherein the intermediate layer has a thickness of 0.3 nm or more and 300 nm or less.

5. The graphene laminate according to claim 1 , wherein the graphene film has a thickness of 0.3 nm or more and 1.0 nm or less.

6. The graphene stack according to claim 1 , wherein the impurity is nitrogen.

7. The graphene stack according to claim 1 , wherein the impurity is potassium.

8. The graphene laminate according to claim 1, wherein a ratio of a peak intensity of a D band to a peak intensity of a G band in a Raman spectrum is 0.16 or more and 2.10 or less.

9. The graphene laminate according to claim 1, wherein a ratio of a 2D band peak intensity to a G band peak intensity in a Raman spectrum is 0.30 or more and 2.51 or less.

10. The half-width of the G band in the Raman spectrum is 24.4 cm -1 60.1cm or more -1 is as follows: The half-width of the 2D band in the Raman spectrum is 20.6 cm -1 155.0cm or more -1 The graphene stack according to claim 1, wherein:

11. forming a graphene film on a first support substrate; forming a resin film on the graphene film; removing the first support substrate; forming an intermediate layer on a second supporting substrate; bonding the graphene film and the intermediate layer; removing the second support substrate; bonding a substrate having an insulating surface to the intermediate layer such that the insulating surface contacts the intermediate layer; and removing the resin film; The method for producing a graphene laminate, wherein the intermediate layer includes nanographene containing an impurity that functions as a hole killer.

12. The method according to claim 11 , wherein the graphene film has a structure in which one, two, or three monolayer graphene layers are stacked.

13. The method of claim 11 , wherein the impurity is nitrogen.

14. The method according to claim 11 , wherein the intermediate layer has a thickness of 0.3 nm or more and 300 nm or less.

15. The method according to claim 11 , wherein the graphene film has a thickness of 0.3 nm or more and 1.0 nm or less.

16. forming a first graphene film on a first support substrate; irradiating the first graphene film with ultraviolet light; forming a first resin layer on the first graphene film irradiated with the ultraviolet light; removing the first support substrate; treating the first graphene film irradiated with ultraviolet light with an aqueous solution of potassium hydroxide to convert the first graphene film into an intermediate layer including nanographene containing impurities that function as a hole killer; bonding the intermediate layer onto a substrate having an insulating surface; removing the first resin layer; forming a second graphene film on a second support substrate; forming a second resin layer on the second graphene film; removing the second support substrate; bonding the second graphene film to the intermediate layer; and removing the second resin layer.

17. The method according to claim 16 , wherein the second graphene film has a structure in which one, two or three layers of single-layer graphene are stacked.

18. 17. The method of claim 16, wherein the impurity is potassium.

19. The method according to claim 16 , wherein the intermediate layer has a thickness of 0.3 nm or more and 300 nm or less.

20. The method according to claim 16 , wherein the first graphene film and the second graphene film each have a thickness of 0.3 nm or more and 1.0 nm or less.

Citation Information

Patent Citations

  • GB2004、3

  • Semiconductor device

    JP1999312807A

  • Method for producing transparent conductive carbon film, and the transparent conductive carbon film

    JP2012162442A

  • Method of producing graphene film and method of producing semiconductor device

    JP2015160794A

  • Semiconductor element including metal-two dimensional material-semiconductor contact

    JP2016219788A