Low-loss inductor and its manufacturing method
Patent Information
- Application Number
- JP2023133004
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-22
- Filing Date
- 2023-08-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-08-17
AI Technical Summary
【0009】 以上の説明から分かるように、非晶質鉄基材料粉末及び非晶質ニッケル基材料粉末は損失が低いため、これらの非晶質材料を用いて低損失の主磁心を製造することができ、また、主磁心粉末の組成を調整することで、主磁心の透磁率を高く維持することができる。更に、コイルが環装された主磁心と、軟磁性粉末及び磁性体粉末を含む残留磁性体複合材料粉末とを第1の金型内に配置することで、主磁心と同等の透磁率を有し且つ主磁心を一体的に覆う残留磁性体を形成することができ、この構成により、磁気漏れを回避することができる。したがって、本発明に係る製造方法によれば、品質係数(Q)が高く、損失が更に低減して変換效率が向上したインダクタを得ることができる。
Smart Images

Figure 0007558590000003 
Figure 0007558590000004 
Figure 0007558590000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an inductor and a manufacturing method thereof, and more particularly to a low-loss inductor and a manufacturing method thereof. [Background technology]
[0002] With ever-changing technical requirements, inductors, which are mainly arranged in a circuit as an on-off switch, are required to have lower losses and higher conversion efficiency. Conventional inductors are known to be made of a magnet alloy composite material, placed in a mold, and pressed and molded at high pressure. However, in the conventional inductor, the coil covered by the external magnet is also pressurized at high pressure during the pressure molding process for forming the external magnet, so that the coil may be deformed or damaged, which may cause a short circuit. Therefore, in the conventional inductor, it is necessary to increase the number of turns of the coil in order to improve the strength and prevent deformation or damage. However, when the number of turns of the coil is increased, there is a problem that the DC resistance increases accordingly, and the overall loss increases.
[0003] In addition, some conventional inductors are manufactured by using two types of magnet alloy composite materials and secondary molding them in two different dies. In the case of such an inductor, although it is possible to improve the local magnet density, the magnetic permeability of the two types of magnet alloy composite materials is significantly different, and magnetic leakage may occur, so that the AC resistance is further increased and the overall loss is still excessive.
[0004] As described above, conventional inductors need to be improved to reduce magnetic leakage and loss. Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above-mentioned problem with conventional inductors, in which loss increases due to the unequal magnetic permeability of the materials, and has an object to provide an improved low-loss inductor that reduces loss and improves conversion efficiency, and a manufacturing method thereof. [Means for solving the problem]
[0006] In order to achieve the above object of the present invention, a low-loss inductor according to the present invention is provided, A main core; A coil attached to the main magnetic core; a residual magnetic body integrally covering the main core and partially covering the coil, The main core includes a main core powder, the main core powder comprising: An amorphous iron-based material powder containing, by mass percentage, 89.7 to 92.35% iron (Fe), 4 to 5% silicon (Si), 3.5 to 4% boron (B), 0.05 to 0.5% phosphorus (P), and 0.1 to 0.8% carbon (C); and an amorphous nickel-based material powder containing, by mass percentage, 60.5 to 67.7% nickel (Ni), 25 to 28% iron (Fe), 3.5 to 5% boron (B), 3.5 to 5% silicon (Si), and 0.3 to 1.5% phosphorus (P); The residual magnetic material includes a residual magnetic powder, and the residual magnetic powder includes A magnetic powder containing, by mass percentage, 72.7 to 83.7% iron (Fe), 8 to 11% nickel (Ni), 3 to 5% cobalt (Co), 3 to 6% silicon (Si), 2 to 4% boron (B), 0.2 to 0.8% phosphorus (P), and 0.1 to 0.5% niobium (Nb); a soft magnetic powder including an iron-silicon-chromium alloy powder and a carbonyl iron powder; The iron-silicon-chromium alloy powder is characterized in that it contains, by mass percentage, 90.5 to 93.5% iron (Fe), 4.5 to 6.5% silicon (Si), and 2 to 3% chromium (Cr).
[0007] A main core manufactured using a main core powder containing an amorphous iron-based material powder and an amorphous nickel-based material powder can reduce loss while maintaining high magnetic permeability because the loss of the amorphous material is relatively low. In addition, by manufacturing the residual magnetic body that covers the main core and partially covers the coil using a residual magnetic body powder containing a soft magnetic powder and a magnetic body powder, the magnetic permeability of the main core and the magnetic permeability of the residual magnetic body can be made equal, thereby preventing magnetic leakage and reducing the AC resistance of the inductor. Therefore, the low-loss inductor according to the present invention has a high quality factor (Q), reliably reduces loss during operation, and improves conversion efficiency.
[0008] In order to achieve the above object of the present invention, a method for manufacturing a low-loss inductor according to the present invention is provided, (a) providing a main core and preparing a remanent magnetic composite powder; (b) wrapping a coil around the main magnetic core; (c) placing the main core with the coil wrapped around it and the residual magnetic composite powder in a first mold such that the main core is covered and the coil is partially covered by the residual magnetic composite powder; (d) hot pressing the remnant magnetic composite powder in the first mold to integrally form a remnant magnetic material; and (e) removing the residual magnetic body from the first die to obtain an inductor; In the step (a), The main core includes a main core powder, the main core powder comprising: An amorphous iron-based material powder containing, by mass percentage, 89.7 to 92.35% iron (Fe), 4 to 5% silicon (Si), 3.5 to 4% boron (B), 0.05 to 0.5% phosphorus (P), and 0.1 to 0.8% carbon (C); and an amorphous nickel-based material powder containing, by mass percentage, 60.5 to 67.7% nickel (Ni), 25 to 28% iron (Fe), 3.5 to 5% boron (B), 3.5 to 5% silicon (Si), and 0.3 to 1.5% phosphorus (P); The remnant magnetic composite powder comprises a remnant magnetic powder, the remnant magnetic powder comprising: A magnetic powder containing, by mass percentage, 72.7 to 83.7% iron (Fe), 8 to 11% nickel (Ni), 3 to 5% cobalt (Co), 3 to 6% silicon (Si), 2 to 4% boron (B), 0.2 to 0.8% phosphorus (P), and 0.1 to 0.5% niobium (Nb); a soft magnetic powder including an iron-silicon-chromium alloy powder and a carbonyl iron powder; The iron-silicon-chromium alloy powder is characterized in that it contains, by mass percentage, 90.5 to 93.5% iron (Fe), 4.5 to 6.5% silicon (Si), and 2 to 3% chromium (Cr).
[0009] As can be seen from the above explanation, since the amorphous iron-based material powder and the amorphous nickel-based material powder have low loss, it is possible to manufacture a low-loss main core using these amorphous materials, and by adjusting the composition of the main core powder, it is possible to maintain a high magnetic permeability of the main core. Furthermore, by arranging the main core with the coil wrapped around it and the residual magnetic composite material powder containing soft magnetic powder and magnetic powder in the first mold, it is possible to form a residual magnetic body that has the same magnetic permeability as the main core and integrally covers the main core, and this configuration makes it possible to prevent magnetic leakage. Therefore, according to the manufacturing method of the present invention, it is possible to obtain an inductor with a high quality factor (Q) and further reduced loss, thereby improving conversion efficiency. [Brief description of the drawings]
[0010] [Figure 1] 1 is a perspective view showing a low-loss inductor according to the present invention; [Diagram 2] 1 is an exploded perspective view showing a low-loss inductor according to the present invention; [Diagram 3] 2 is a cross-sectional view of the low-loss inductor shown in FIG. [Figure 4] 4 is a flow chart illustrating the steps involved in a method for manufacturing a low-loss inductor according to the present invention. [Diagram 5]4 is a flow chart illustrating the steps involved in a method for manufacturing a low-loss inductor according to the present invention. [Figure 6] 4 is a flow chart illustrating the steps involved in a method for manufacturing a low-loss inductor according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A low-loss inductor and a manufacturing method thereof according to the present invention will be described below using embodiments with reference to the drawings.
[0012] As shown in FIGS. 1 and 2, in one embodiment, a low-loss inductor according to the present invention includes a main core 10, a coil 20, and a residual magnet 30.
[0013] The main core 10 has a pillar portion 11. In this embodiment, a pedestal 111 extends integrally from one end of the pillar portion 11. The pedestal 111 is substantially rectangular, and protrusions 112 protrude from two opposing edges of the pedestal 111. In one embodiment, the main core 10 further has a central pillar 12 that is integrally covered by the pillar portion 11 so as to be located at an upper part within the pillar portion 11.
[0014] The main core 10 mainly contains a main core powder obtained by mixing an amorphous iron-based material powder and an amorphous nickel-based material powder. The mass percentage of the amorphous iron-based material powder in the main core powder is 70-90%, and the amorphous iron-based material powder contains, by mass percentage, 89.7-92.35% iron (Fe), 4-5% silicon (Si), 3.5-4% boron (B), 0.05-0.5% phosphorus (P), and 0.1-0.8% carbon (C). The mass percentage of the amorphous nickel-based material powder in the main core powder is 10-30%, and the amorphous nickel-based material powder contains, by mass percentage, 60.5-67.7% nickel (Ni), 25-28% iron (Fe), 3.5-5% boron (B), 3.5-5% silicon (Si), and 0.3-1.5% phosphorus (P). In this embodiment, the main core 10 is manufactured by mixing the main core powder with a thermosetting resin. In this embodiment, the thermosetting resin may be manufactured by an unsaturated polyester resin thermally crosslinked with bisphenol A diglycidyl ether and 4,4'-dihydroxydiphenylmethane, but the composition of the thermosetting resin is not limited thereto.
[0015] The coil 20 is formed by winding a bare metal wire, and is attached to the main core 10. In this embodiment, the coil 20 has a winding section 21 attached to the column section 11 of the main core 10, and two electrodes 22. In this embodiment, the bare metal wire has a flat shape, and the number of turns of the winding section 21 of the coil 20 is 9, but is not limited to this. The two end portions of the coil 20 are bent and fixed to the base 111 of the main core 10 so as to integrally form the two electrodes 22. In an embodiment, the low-loss inductor may be, but is not limited to, a surface mount device in which a solder layer 221 having a thickness of 15 to 25 μm is formed on the bottom of each of the two electrodes 22.
[0016] The residual magnetic body 30 covers the main core 10 as a whole and partially covers the coil 20. Specifically, as shown in FIG. 3, the residual magnetic body 30 covers the main core 10 and the winding portion 21 of the coil 20 as a whole, and partially covers two end portions of the winding portion 21 so that the two electrodes 22 of the coil 20 and their solder layers 221 are both exposed from the residual magnetic body 30. In this embodiment, the residual magnetic body 30 further has an insulating rust-preventive layer 31 formed on its outer surface. In this embodiment, the insulating rust-preventive layer 31 contains epoxy resin and nanometer silicon powder. The mass percentage of the epoxy resin in the insulating rust-preventive layer 31 is 80%. The mass percentage of the nanometer silicon powder in the insulating rust-preventive layer 31 is 20%. In this embodiment, the thickness T1 of the insulating rust-preventive layer 31 is 10 to 20 μm.
[0017] The residual magnetic material 30 mainly contains residual magnetic powder obtained by mixing magnetic powder and soft magnetic powder. The mass percentage of the magnetic powder in the residual magnetic powder is 59-67%, and the magnetic powder contains, by mass percentage, 72.7-83.7% iron (Fe), 8-11% nickel (Ni), 3-5% cobalt (Co), 3-6% silicon (Si), 2-4% boron (B), 0.2-0.8% phosphorus (P), and 0.1-0.5% niobium (Nb). The mass percentage of the soft magnetic powder in the residual magnetic powder is 33-41%, and the soft magnetic powder contains iron-silicon-chromium alloy powder and carbonyl iron powder. Here, the mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 17-33%, and the iron-silicon-chromium alloy powder contains, by mass percentage, 90.5-93.5% iron (Fe), 4.5-6.5% silicon (Si), and 2-3% chromium (Cr). On the other hand, the mass percentage of the carbonyl iron powder in the soft magnetic powder is 67-83%. In this embodiment, the residual magnetic material 30 is manufactured by mixing the residual magnetic material powder with a thermosetting resin. In this embodiment, the thermosetting resin contains an unsaturated polyester resin, bisphenol A diglycidyl ether, and 4,4'-dihydroxydiphenylmethane, and the unsaturated polyester resin is thermally crosslinked by bisphenol A diglycidyl ether and 4,4'-dihydroxydiphenylmethane to form a thermosetting resin, but the composition of the thermosetting resin is not limited thereto.
[0018] In this embodiment, the residual magnetic material 30 further includes silicon dioxide. Specifically, the silicon dioxide is a mixture of gas-phase silicon dioxide and a thermosetting resin via a silane coupling agent.
[0019] The structure and materials of the low-loss inductor according to the present invention have been described. The manufacturing method of the low-loss inductor according to the present invention will be described below. As shown in Fig. 4 and Fig. 6, the manufacturing method of the low-loss inductor according to the present invention mainly includes steps S100 to S500, and may further include steps S600 and S700.
[0020] As shown in Fig. 4, in step S100, a main core is prepared and a remanent magnetic composite material powder is prepared. The main core includes a main core powder obtained by mixing an amorphous iron-based material powder and an amorphous nickel-based material powder. The mass percentage of the amorphous iron-based material powder in the main core powder is 70-90%, and the amorphous iron-based material powder includes, by mass percentage, 89.7-92.35% iron (Fe), 4-5% silicon (Si), 3.5-4% boron (B), 0.05-0.5% phosphorus (P), and 0.1-0.8% carbon (C). On the other hand, the mass percentage of the amorphous nickel-based material powder in the main core powder is 10 to 30%, and the amorphous nickel-based material powder contains, by mass percentage, 60.5 to 67.7% nickel (Ni), 25 to 28% iron (Fe), 3.5 to 5% boron (B), 3.5 to 5% silicon (Si), and 0.3 to 1.5% phosphorus (P). In this embodiment, the particle size of the amorphous iron-based material powder is 5 to 15 μm, and the particle size of the amorphous nickel-based material powder is 10 to 20 μm.
[0021] In step S100, the residual magnetic composite powder contains a residual magnetic powder obtained by mixing a magnetic powder and a soft magnetic powder. Here, the mass percentage of the magnetic powder in the residual magnetic powder is 59-67%, and the magnetic powder contains, by mass percentage, 72.7-83.7% iron (Fe), 8-11% nickel (Ni), 3-5% cobalt (Co), 3-6% silicon (Si), 2-4% boron (B), 0.2-0.8% phosphorus (P), and 0.1-0.5% niobium (Nb). On the other hand, the mass percentage of the soft magnetic powder in the residual magnetic powder is 33-41%, and the soft magnetic powder contains an iron-silicon-chromium alloy powder and a carbonyl iron powder. Here, the mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 17-33%, and the iron-silicon-chromium alloy powder contains, by mass percentage, 90.5-93.5% iron (Fe), 4.5-6.5% silicon (Si), and 2-3% chromium (Cr). On the other hand, the mass percentage of the carbonyl iron powder in the soft magnetic powder is 67-83%. In this embodiment, the particle size of the magnetic substance powder is 15-25 μm, and the particle size of the soft magnetic powder is 1-3 μm.
[0022] In this embodiment, step S100 includes the following steps S111 to S113 and steps S121 to S123. Here, steps S111 to S113 are steps for preparing a main core, while steps S121 to S123 are steps for preparing a remanent magnetic composite material powder.
[0023] As shown in FIG. 5, in step S111, the main core powder is mixed with an adhesive and a solvent to form a main core glue. In this embodiment, the adhesive may include an unsaturated polyester resin, bisphenol A diglycidyl ether, and 4,4'-dihydroxydiphenylmethane. However, the material of the adhesive is not limited to the above. The mass percentage of the unsaturated polyester resin in the adhesive in the main core glue is 0.1-0.3%, the mass percentage of the bisphenol A diglycidyl ether in the adhesive in the main core glue is 0.8-1.2%, and the mass percentage of the 4,4'-dihydroxydiphenylmethane in the main core glue is 0.2-0.4%. Bisphenol A diglycidyl ether and 4,4'-dihydroxydiphenylmethane are used as thermal crosslinking agents for crosslinking and curing the unsaturated polyester resin. In this embodiment, cyclohexanone and acetone are used as the solvent, but are not limited thereto. The mass percentages of cyclohexanone and acetone in the main core glue are 5 to 10%, respectively. Cyclohexanone and acetone are used to dissolve unsaturated polyester resin, bisphenol A diglycidyl ether, and 4,4'-dihydroxydiphenylmethane, disperse the main core powder in the cyclohexanone and acetone, and thereby adhere and coat the main core powder with the adhesive to form the main core glue.
[0024] In step S112, the main core glue is filled into the main core die to integrally mold the main core blank. In this embodiment, the main core is molded by applying high pressure. That is, the main core glue is pressurized in the main core die under a pressure of 500 to 900 MPa, and the unsaturated polyester resin is crosslinked by bisphenol A diglycidyl ether and 4,4'-dihydroxydiphenylmethane in the adhesive to form a thermosetting resin, which gradually hardens the main core glue to integrally form the main core blank. In one embodiment, a central pillar is further placed in the main core die so as to be located at the top of the main core die, and the central pillar is covered with the main core glue to form the main core blank.
[0025] In step S113, the main core blank is dried at 210° C. for 5 to 10 minutes to remove the solvent, and the main core blank is further hardened to form the main core.
[0026] Then, as shown in FIG. 6, in step S121, the residual magnetic material powder is mixed with an organic resin and a solvent to form a residual magnetic material suspension. In this embodiment, the organic resin may include an unsaturated polyester resin, bisphenol A diglycidyl ether, and 4,4'-dihydroxydiphenylmethane. However, the materials constituting the organic resin are not limited to these. The mass percentage of the unsaturated polyester resin in the organic resin in the residual magnetic material suspension is 0.05-015%, the mass percentage of the bisphenol A diglycidyl ether in the residual magnetic material suspension is 0.5-0.7%, and the mass percentage of the 4,4'-dihydroxydiphenylmethane in the residual magnetic material suspension is 0.1-0.2%. The bisphenol A diglycidyl ether and 4,4'-dihydroxydiphenylmethane in the organic resin are also used as thermal crosslinking agents to crosslink and harden the unsaturated polyester resin to form a thermosetting resin. In this embodiment, cyclohexanone and acetone are similarly used as the solvent, but are not limited thereto. The mass percentage of cyclohexanone in the solvent in the residual magnetic material suspension is 7 to 15%, and the mass percentage of acetone in the residual magnetic material suspension is 2 to 5%. Similarly, cyclohexanone and acetone are used to dissolve unsaturated polyester resin, bisphenol A diglycidyl ether, and 4,4'-dihydroxydiphenylmethane and disperse the residual magnetic material powder therein, thereby adhering and coating the residual magnetic material powder with the organic resin to form the residual magnetic material suspension.
[0027] In step S122, the residual magnetic material suspension is dried to remove the solvent. Compared with the mass percentage of the adhesive in the main core glue, the mass percentage of the organic resin including the unsaturated polyester resin, bisphenol A diglycidyl ether, and 4,4'-dihydroxydiphenylmethane in the residual magnetic material suspension is lower. That is, the viscosity of the residual magnetic material suspension is lower. Therefore, by drying the residual magnetic material suspension, a powdered residual magnetic material composite material in which the surface of the residual magnetic material powder is covered with a thermosetting organic resin, that is, a residual magnetic material composite material powder, is obtained.
[0028] In step S123, the gas-phase silicon dioxide and the silane coupling agent are mixed into the residual magnetic composite powder to form a silicon dioxide coating layer on the surface of the residual magnetic composite powder. Here, the mass percentage of the gas-phase silicon dioxide in the residual magnetic composite powder is 0.05-0.2%, and the particle size of the gas-phase silicon dioxide is 15-30 nm. The mass percentage of the silane coupling agent in the residual magnetic composite powder is 0.1-0.5%. In this embodiment, the thickness of the silicon dioxide coating layer is 10-20 nm. Since the residual magnetic composite powder has a structure in which the residual magnetic powder is covered with an organic resin, the silane coupling agent bonds the gas-phase silicon dioxide and the organic resin to improve the strength of the hetero-bonding between the silicon dioxide coating layer and the organic resin, and plays a role in preventing the collapse of the silicon dioxide coating layer, but does not separate the gas-phase silicon dioxide from the organic resin.
[0029] As shown in Fig. 4, in step S200, the coil is attached to the main magnetic core. In this embodiment, the winding portion of the coil is attached to the pillar portion of the main magnetic core, and the two end portions of the coil are folded and fixed to the base of the main magnetic core to form two electrodes. That is, as shown in Fig. 1, the two end portions of the coil 20 are each folded and fixed to both sides of the two protruding portions 112 of the base 111. Also, in this embodiment, the two end portions of the winding portion 21 are each folded four times to form four folded portions. 1, the end portion connected to the end of the uppermost turn of the winding portion 21 first extends rearward and is then bent downward to form a first bent portion 23, then bent forward below the base 111 of the main core 10 to form a second bent portion 24, then bent upward in front of the base 111 to form a third bent portion 25, and finally bent backward above the base 111 to form a fourth bent portion 26, thereby stably fixing the coil 20 on the main core 10. The electrode 22 is formed by the portion between the second bent portion 24 and the third bent portion 25.
[0030] In step S300, the main core with the coil wrapped around it and the residual magnetic composite powder are placed in a residual magnetic mold so that the main core is covered and the coil is partially covered by the residual magnetic composite powder (specifically, the winding portion of the coil is covered and the two electrodes of the coil are exposed).
[0031] In step S400, the residual magnetic composite material powder is hot-pressed in the residual magnetic material mold to integrally form the residual magnetic material. In this embodiment, the residual magnetic composite material powder is hot-pressed in the residual magnetic material mold under a pressure of 150 to 300 MPa and a temperature of 100 to 150°C. As a result, the unsaturated polyester resin is cross-linked by bisphenol A diglycidyl ether and 4,4'-dihydroxydiphenylmethane in the organic resin, and the residual magnetic material composite material powder and the silicon dioxide coating layer formed on its outer surface are bonded to each other by the high pressure, improving the insulation of the residual magnetic material.
[0032] In step S500, the residual magnetic body is removed from the residual magnetic body mold to obtain a low-loss inductor.
[0033] In step S600, an insulating paint is applied to the outer surface of the residual magnetic body of the inductor, and the insulating paint is dried to form an insulating rust-preventive layer 31 as shown in FIG. 3. In this embodiment, the insulating paint contains N-methyl-2-pyrrolidone, epoxy resin, and nanometer silicon powder. Here, the mass percentage of N-methyl-2-pyrrolidone in the insulating paint is 90-95%. The mass percentage of epoxy resin in the insulating paint is 4-8%. The mass percentage of nanometer silicon powder in the insulating paint is 1-2%, and the particle size of the nanometer silicon powder is 80-120 nm. The thickness of the insulating rust-preventive layer 31 is 10-20 μm. In this embodiment, N-methyl-2-pyrrolidone is used as a solvent for dissolving the epoxy resin as a resin and dispersing the nanometer silicon powder therein. However, the composition of the insulating paint is not limited to this.
[0034] In step S700, a solder layer 221 is formed on the bottom of each of the two electrodes as shown in Fig. 3. The thickness of the solder layer 221 is 15 to 25 µm. In one embodiment, the low-loss inductor is a surface mount device, in which case the solder layer is for joining the low-loss inductor to a corresponding contact on a circuit board.
[0035] The materials, structure and manufacturing method of the low-loss inductor according to the present invention are as described in the above embodiment. Three experimental groups of low-loss inductors based on the materials and manufacturing methods of the present invention are disclosed below, and one control group is disclosed. The main magnetic core and residual magnetic body in the inductor of the control group are manufactured by conventional materials and manufacturing methods. In all three experimental groups of the present invention, the same steps S122, S200, S300 and S500 were performed. The description thereof will be omitted below.
[0036] Hereinafter, experimental group 1 of the present invention will be described.
[0037] In the experimental group 1, the mass percentage of the amorphous iron-based material powder in the main core powder was 70%, and the amorphous iron-based material powder contained, by mass percentage, 92.35% iron (Fe), 4% silicon (Si), 3.5% boron (B), 0.05% phosphorus (P), and 0.1% carbon (C). On the other hand, the mass percentage of the amorphous nickel-based material powder in the main core powder was 30%, and the amorphous nickel-based material powder contained, by mass percentage, 60.5% nickel (Ni), 28% iron (Fe), 5% boron (B), 5% silicon (Si), and 1.5% phosphorus (P). The particle size of the amorphous iron-based material powder was 5 to 15 μm, and the particle size of the amorphous nickel-based material powder was 10 to 20 μm.
[0038] In addition, in the experimental group 1, the mass percentage of the magnetic powder in the residual magnetic powder was 59%, and the magnetic powder contained, by mass percentage, 83.7% iron (Fe), 8% nickel (Ni), 3% cobalt (Co), 3% silicon (Si), 2% boron (B), 0.2% phosphorus (P) and 0.1% niobium (Nb). On the other hand, the mass percentage of the soft magnetic powder in the residual magnetic powder was 41%, and the soft magnetic powder contained iron-silicon-chromium alloy and carbonyl iron powder. Here, the mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder was 17%, and the iron-silicon-chromium alloy powder contained, by mass percentage, 90.5% iron (Fe), 6.5% silicon (Si) and 3% chromium (Cr). On the other hand, the mass percentage of the carbonyl iron powder in the soft magnetic powder was 83%. The magnetic powder had a particle size of 15 to 25 μm, and the soft magnetic powder had a particle size of 1 to 3 μm.
[0039] Step S100: A main core was manufactured using the main core powder described above, and a remnant magnetic composite material powder was prepared using the remnant magnetic powder described above.
[0040] Step S111: The mass percentage of the unsaturated polyester resin in the main core glue was 0.1%. The mass percentage of bisphenol A diglycidyl ether in the main core glue was 1.2%. The mass percentage of 4,4'-dihydroxydiphenylmethane in the main core glue was 0.4%. The mass percentage of cyclohexanone in the main core glue was 10%. The mass percentage of acetone in the main core glue was 5%.
[0041] Step S112: The main core glue was pressed in a main core mold under a pressure of 900 MPa to harden the unsaturated polyester resin and form a main core blank.
[0042] Step S113: The main core blank was dried at a temperature of 210° C. for 5 minutes to remove the cyclohexanone and acetone and further harden the main core.
[0043] Step S121: The mass percentage of the unsaturated polyester resin in the residual magnetic material suspension was 0.15%. The mass percentage of bisphenol A diglycidyl ether in the residual magnetic material suspension was 0.7%. The mass percentage of 4,4'-dihydroxydiphenylmethane in the residual magnetic material suspension was 0.2%. The mass percentage of cyclohexanone in the residual magnetic material suspension was 15%. The mass percentage of acetone in the residual magnetic material suspension was 5%.
[0044] Step S123: The mass percentage of the gas phase silicon dioxide in the residual magnetic composite powder was 0.2%, and the particle size of the gas phase silicon dioxide was 30 nm. The mass percentage of the silane coupling agent in the residual magnetic composite powder was 0.5%. In this experimental group, the thickness of the silicon dioxide coating layer was 20 nm.
[0045] Step S400: In a residual magnetic body mold, the residual magnetic body composite powder was hot pressed under a pressure of 150 MPa and a temperature of 100° C. to form a residual magnetic body.
[0046] Step S600: The mass percentage of N-methyl-2-pyrrolidone in the insulating paint is 95%, the mass percentage of epoxy resin in the insulating paint is 4%, the mass percentage of nanometer silicon powder in the insulating paint is 1%, and the particle size of the nanometer silicon powder is 80 nm. In this experimental group, the thickness of the insulating rust prevention layer is 20 μm.
[0047] Step S700: The thickness of the solder layer formed on the bottom of each of the two electrodes was 25 μm.
[0048] Hereinafter, experimental group 2 of the present invention will be described.
[0049] In the experimental group 2, the mass percentage of the amorphous iron-based material powder in the main core powder was 90%, and the amorphous iron-based material powder contained, by mass percentage, 89.7% iron (Fe), 5% silicon (Si), 4% boron (B), 0.5% phosphorus (P), and 0.8% carbon (C). On the other hand, the mass percentage of the amorphous nickel-based material powder in the main core powder was 10%, and the amorphous nickel-based material powder contained, by mass percentage, 67.7% nickel (Ni), 25% iron (Fe), 3.5% boron (B), 3.5% silicon (Si), and 0.3% phosphorus (P). The particle sizes of the amorphous iron-based material powder and the amorphous nickel-based material powder were the same as those of the amorphous iron-based material powder and the amorphous nickel-based material powder described for the experimental group 1.
[0050] In addition, in the experimental group 2, the mass percentage of the magnetic powder in the residual magnetic powder was 67%, and the magnetic powder contained, by mass percentage, 72.7% iron (Fe), 11% nickel (Ni), 5% cobalt (Co), 6% silicon (Si), 4% boron (B), 0.8% phosphorus (P) and 0.5% niobium (Nb). The mass percentage of the soft magnetic powder in the residual magnetic powder was 33%, and the soft magnetic powder contained iron-silicon-chromium alloy and carbonyl iron powder. Here, the mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder was 33%, and the iron-silicon-chromium alloy powder contained, by mass percentage, 93.5% iron (Fe), 4.5% silicon (Si) and 2% chromium (Cr). Meanwhile, the mass percentage of the carbonyl iron powder in the soft magnetic powder was 67%. The particle sizes of the magnetic powder and the soft magnetic powder were the same as those of the magnetic powder and the soft magnetic powder described for Experimental Group 1.
[0051] Step S100: A main core was manufactured using the main core powder described above for this experimental group, and a remnant magnetic composite material powder was prepared using the remnant magnetic powder described above for this experimental group.
[0052] Step S111: The mass percentage of the unsaturated polyester resin in the main core glue was 0.3%. The mass percentage of bisphenol A diglycidyl ether in the main core glue was 0.8%. The mass percentage of 4,4'-dihydroxydiphenylmethane in the main core glue was 0.2%. The mass percentage of cyclohexanone in the main core glue was 5%. The mass percentage of acetone in the main core glue was 10%.
[0053] Step S112: In the main core die, the main core glue was pressed under a pressure of 500 MPa to harden the unsaturated polyester resin and form a main core blank.
[0054] Step S113: The main core blank was dried at a temperature of 210° C. for 10 minutes to remove the cyclohexanone and acetone and further harden the main core.
[0055] Step S121: The mass percentage of the unsaturated polyester resin in the residual magnetic material suspension was 0.15%. The mass percentage of bisphenol A diglycidyl ether in the residual magnetic material suspension was 0.5%. The mass percentage of 4,4'-dihydroxydiphenylmethane in the residual magnetic material suspension was 0.1%. The mass percentage of cyclohexanone in the residual magnetic material suspension was 7%. The mass percentage of acetone in the residual magnetic material suspension was 2%.
[0056] Step S123: The mass percentage of the gas phase silicon dioxide in the residual magnetic composite powder was 0.05%, and the particle size of the gas phase silicon dioxide was 15 nm. The mass percentage of the silane coupling agent in the residual magnetic composite powder was 0.1%. In this experimental group, the thickness of the silicon dioxide coating layer was 10 nm.
[0057] Step S400: In the residual magnetic body mold, the residual magnetic body composite powder was hot pressed under a pressure of 300 MPa and a temperature of 150° C. to integrally form a residual magnetic body.
[0058] Step S600: The mass percentage of N-methyl-2-pyrrolidone in the insulating paint is 90%, the mass percentage of epoxy resin in the insulating paint is 8%, the mass percentage of nanometer silicon powder in the insulating paint is 2%, and the particle size of the nanometer silicon powder is 120 nm. In this experimental group, the thickness of the insulating rust prevention layer is 10 μm.
[0059] Step S700: The thickness of the solder layer formed on the bottom of each of the two electrodes was 15 μm.
[0060] Hereinafter, experimental group 3 of the present invention will be described.
[0061] In the experimental group 3, the mass percentage of the amorphous iron-based material powder in the main core powder was 80%, and the amorphous iron-based material powder contained, by mass percentage, 91% iron (Fe), 4.5% silicon (Si), 3.75% boron (B), 0.35% phosphorus (P), and 0.4% carbon (C). On the other hand, the mass percentage of the amorphous nickel-based material powder in the main core powder was 20%, and the amorphous nickel-based material powder contained, by mass percentage, 60.5% nickel (Ni), 28% iron (Fe), 5% boron (B), 5% silicon (Si), and 1.5% phosphorus (P). The particle sizes of the amorphous iron-based material powder and the amorphous nickel-based material powder were the same as those of the amorphous iron-based material powder and the amorphous nickel-based material powder described above for the experimental groups 1 and 2.
[0062] In addition, in the experimental group 3, the mass percentage of the magnetic powder in the residual magnetic powder was 62.5%, and the magnetic powder contained, by mass percentage, 77.05% iron (Fe), 9.5% nickel (Ni), 4.5% cobalt (Co), 5% silicon (Si), 3% boron (B), 0.6% phosphorus (P) and 0.35% niobium (Nb). The mass percentage of the soft magnetic powder in the residual magnetic powder was 37.5%, and the soft magnetic powder contained iron-silicon-chromium alloy and carbonyl iron powder. Here, the mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder was 20%, and the iron-silicon-chromium alloy powder contained, by mass percentage, 92% iron (Fe), 5.5% silicon (Si) and 2.5% chromium (Cr). On the other hand, the mass percentage of the carbonyl iron powder in the soft magnetic powder was 80%. The particle sizes of the magnetic powder and the soft magnetic powder were the same as those of the magnetic powder and the soft magnetic powder described above for the experimental groups 1 and 2.
[0063] Step S100: A main core was manufactured using the main core powder described above for this experimental group, and a remnant magnetic composite material powder was prepared using the remnant magnetic powder described above for this experimental group.
[0064] Step S111: The mass percentage of the unsaturated polyester resin in the main core glue was 0.2%. The mass percentage of bisphenol A diglycidyl ether in the main core glue was 1%. The mass percentage of 4,4'-dihydroxydiphenylmethane in the main core glue was 0.3%. The mass percentage of cyclohexanone in the main core glue was 7%. The mass percentage of acetone in the main core glue was 7%.
[0065] Step S112: In the main core die, the main core glue was pressed under a pressure of 700 MPa to harden the unsaturated polyester resin and form a main core blank.
[0066] Step S113: The main core blank was dried at a temperature of 210° C. for 7 minutes to remove the cyclohexanone and acetone and further harden the main core.
[0067] Step S121: The mass percentage of the unsaturated polyester resin in the residual magnetic material suspension was 0.1%. The mass percentage of bisphenol A diglycidyl ether in the residual magnetic material suspension was 0.6%. The mass percentage of 4,4'-dihydroxydiphenylmethane in the residual magnetic material suspension was 0.15%. The mass percentage of cyclohexanone in the residual magnetic material suspension was 12%. The mass percentage of acetone in the residual magnetic material suspension was 3%.
[0068] Step S123: The mass percentage of the gas phase silicon dioxide in the residual magnetic composite powder was 0.15%, and the particle size of the gas phase silicon dioxide was 20 nm. The mass percentage of the silane coupling agent in the residual magnetic composite powder was 0.25%. In this experimental group, the thickness of the silicon dioxide coating layer was 15 nm.
[0069] Step S500: In the residual magnetic body mold, the residual magnetic body composite powder was hot pressed under a pressure of 250 MPa and a temperature of 120° C. to integrally form a residual magnetic body.
[0070] Step S600: The mass percentage of N-methyl-2-pyrrolidone in the insulating paint was 92.5%, the mass percentage of epoxy resin in the insulating paint was 6%, the mass percentage of nanometer silicon powder in the insulating paint was 1.5%, and the particle size of the nanometer silicon powder was 100 nm. In this experimental group, the thickness of the insulating rust-preventive layer was 15 μm. As can be seen from the composition of the insulating paint in experimental groups 1 to 3, the viscosity of the insulating paint changes depending on the content of nanometer silicon powder. The higher the viscosity of the insulating paint, the thinner the thickness of the formed insulating rust-preventive layer. Therefore, the thickness of the insulating rust-preventive layer can be adjusted by adjusting the mass percentage of nanometer silicon powder in the insulating paint. In addition, since the nanometer silicon powder has a high resistance, it has an insulating effect.
[0071] Step S700: The thickness of the solder layer formed on the bottom of each of the two electrodes was 15 μm.
[0072] The control group of the present invention will now be described.
[0073] In the control group, the main core was manufactured using a magnetic core powder containing a first magnetic material powder and a carbonyl iron powder. Here, the mass percentage of the first magnetic material powder in the magnetic core powder was 59%, the first magnetic material powder contained, by mass percentage, 91% iron (Fe), 3.5% silicon (Si), 5% boron (B) and 0.5% carbon (C), and the particle size of the first magnetic material powder was 25 μm. The mass percentage of the carbonyl iron powder in the magnetic core powder was 41%, and the particle size of the carbonyl iron powder was 4 μm.
[0074] The magnetic core powder was further mixed with an epoxy resin to form a magnetic core granulated powder, and the mass percentage of the magnetic core powder in the magnetic core granulated powder was 98.4%. The mass percentage of the epoxy resin in the magnetic core granulated powder was 1.6%. The magnetic core granulated powder was then placed in a main magnetic core mold and pressed in the main magnetic core mold under a pressure of 700 MPa to form a main magnetic core blank, which was then dried and hardened at a temperature of 180°C for 10 minutes to form a main magnetic core.
[0075] In the control group, the residual magnetic body was produced using the residual magnetic body powder containing the first magnetic material powder and carbonyl iron powder described above. The composition of the residual magnetic body powder was the same as that of the magnetic core powder, so the description is omitted.
[0076] The residual magnetic powder was further mixed with epoxy resin to form a residual magnetic granulated powder, in which the mass percentage of the residual magnetic powder in the residual magnetic granulated powder was 99%. The mass percentage of the epoxy resin in the residual magnetic granulated powder was 1%. Thereafter, the residual magnetic granulated powder and the main core with the coil mounted thereon were placed in a residual magnetic mold, and hot pressed in the residual magnetic mold under a pressure of 300 MPa and a temperature of 100 to 150°C to form a residual magnetic body and an inductor at the same time.
[0077] In the control group, the inductor was kept at a temperature of 180°C for 4 hours to further harden the inductor. After that, an insulating paint was applied to the outer surface of the residual magnetic body of the inductor and dried, and a solder layer was formed on the two electrodes of the inductor.
[0078] Table 1 shows the results of measuring the magnetic permeability and loss of the main cores and remanent magnetic bodies of the experimental groups 1 to 3 and the control group. The loss was measured under conditions of an operating frequency of 1 MHz and a magnetic flux density of 50 mT.
[0079] [Table 1]
[0080] Table 2 shows the results of measuring the inductance, saturation current, quality factor, and AC resistance of the low-loss inductors of the experimental groups 1 to 3 and the inductor of the control group.
[0081] [Table 2]
[0082] As can be seen from Table 1, the main core of each of the three low-loss inductors contains amorphous iron-based material powder and amorphous nickel-based material powder, so that the main core can be easily magnetized and demagnetized, and the loss of the main core can be significantly reduced, compared with the control group manufactured using conventional magnetic materials. In addition, the permeability of the main core manufactured using the main core powder according to the present invention is equivalent to the permeability of the residual magnetic material manufactured using the residual magnetic material powder according to the present invention. Compared with inductors manufactured using conventional materials, the loss of the inductor can be reduced, and the AC resistance can be significantly reduced, as shown in Table 2. Therefore, as can be seen from Table 2, the low-loss inductors manufactured using the main core powder and residual magnetic material powder according to the present invention have a higher quality factor Q than the conventional inductors, and the loss is indeed significantly reduced and the conversion efficiency is improved.
[0083] As can be seen from the above description, the main core powder used to manufacture the main core contains amorphous iron-based material powder and amorphous nickel-based material powder, and these amorphous material powders are easier to magnetize and demagnetize than conventional magnetic materials, and therefore have the characteristic of low loss. Therefore, by adjusting the composition of the main core powder, it is possible to reduce the loss of the main core while maintaining a high magnetic permeability of the main core. In addition, by using residual magnetic material powder with an adjusted composition of magnetic material powder and soft magnetic powder, it is possible to manufacture a residual magnetic material having the same magnetic permeability as the main core, which avoids magnetic leakage due to unequal magnetic permeability and further reduces the loss of the inductor, thereby further improving the conversion efficiency of the low-loss inductor.
[0084] Although the present invention has been described with reference to the above-mentioned embodiments, the present invention is not limited to these disclosed embodiments, and those skilled in the art can make various changes and modifications to obtain equivalents without departing from the technical spirit of the present invention. Therefore, the contents to which the above-mentioned embodiments have been changed, modified, and modified are also included in the technical spirit of the present invention.
Claims
1. A main core; A coil attached to the main magnetic core; a residual magnetic body integrally covering the main core and partially covering the coil, The main core includes a main core powder, the main core powder comprising: An amorphous iron-based material powder containing, by mass percentage, 89.7 to 92.35% iron (Fe), 4 to 5% silicon (Si), 3.5 to 4% boron (B), 0.05 to 0.5% phosphorus (P), and 0.1 to 0.8% carbon (C); an amorphous nickel-based material powder containing, by mass percentage, 60.5-67.7% nickel (Ni), 25-28% iron (Fe), 3.5-5% boron (B), 3.5-5% silicon (Si), and 0.3-1.5% phosphorus (P); The residual magnetic material includes a residual magnetic powder, and the residual magnetic powder includes A magnetic powder containing, by mass percentage, 72.7 to 83.7% iron (Fe), 8 to 11% nickel (Ni), 3 to 5% cobalt (Co), 3 to 6% silicon (Si), 2 to 4% boron (B), 0.2 to 0.8% phosphorus (P), and 0.1 to 0.5% niobium (Nb); a soft magnetic powder comprising an iron-silicon-chromium alloy powder and a carbonyl iron powder; The iron-silicon-chromium alloy powder contains, by mass percentage, 90.5 to 93.5% iron (Fe), 4.5 to 6.5% silicon (Si), and 2 to 3% chromium (Cr).
2. the mass percentage of the amorphous iron-based material powder in the main core powder is 70 to 90%; The mass percentage of the amorphous nickel-based material powder in the main core powder is 10 to 30%; The mass percentage of the magnetic powder in the residual magnetic powder is 59 to 67%, The mass percentage of the soft magnetic powder in the residual magnetic powder is 33 to 41%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 17 to 33%; 2. The low-loss inductor according to claim 1, wherein the mass percentage of the carbonyl iron powder in the soft magnetic powder is 67 to 83%.
3. The mass percentage of the amorphous iron-based material powder in the main core powder is 70%, and the amorphous iron-based material powder contains, by mass percentage, 92.35% iron (Fe), 4% silicon (Si), 3.5% boron (B), 0.05% phosphorus (P), and 0.1% carbon (C); The mass percentage of the amorphous nickel-based material powder in the main core powder is 30%, and the amorphous nickel-based material powder contains, by mass percentage, 60.5% nickel (Ni), 28% iron (Fe), 5% boron (B), 5% silicon (Si), and 1.5% phosphorus (P); The mass percentage of the magnetic powder in the residual magnetic powder is 59%, and the magnetic powder contains, by mass percentage, 83.7% iron (Fe), 8% nickel (Ni), 3% cobalt (Co), 3% silicon (Si), 2% boron (B), 0.2% phosphorus (P) and 0.1% niobium (Nb); The mass percentage of the soft magnetic powder in the residual magnetic powder is 41%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 17%, and the iron-silicon-chromium alloy powder contains, by mass percentage, 90.5% iron (Fe), 6.5% silicon (Si) and 3% chromium (Cr); The low-loss inductor of claim 2 , wherein the mass percentage of the carbonyl iron powder in the soft magnetic powder is 83%.
4. The mass percentage of the amorphous iron-based material powder in the main core powder is 90%, and the amorphous iron-based material powder contains, by mass percentage, 89.7% iron (Fe), 5% silicon (Si), 4% boron (B), 0.5% phosphorus (P) and 0.8% carbon (C); The mass percentage of the amorphous nickel-based material powder in the main core powder is 10%, and the amorphous nickel-based material powder contains, by mass percentage, 67.7% nickel (Ni), 25% iron (Fe), 3.5% boron (B), 3.5% silicon (Si), and 0.3% phosphorus (P); The mass percentage of the magnetic powder in the residual magnetic powder is 67%, and the magnetic powder contains, by mass percentage, 72.7% iron (Fe), 11% nickel (Ni), 5% cobalt (Co), 6% silicon (Si), 4% boron (B), 0.8% phosphorus (P) and 0.5% niobium (Nb); The mass percentage of the soft magnetic powder in the residual magnetic powder is 33%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 33%, and the iron-silicon-chromium alloy powder contains, by mass percentage, 93.5% iron (Fe), 4.5% silicon (Si) and 2% chromium (Cr); The low-loss inductor of claim 2 , wherein the mass percentage of the carbonyl iron powder in the soft magnetic powder is 67%.
5. The mass percentage of the amorphous iron-based material powder in the main core powder is 80%, and the amorphous iron-based material powder contains, by mass percentage, 91% iron (Fe), 4.5% silicon (Si), 3.75% boron (B), 0.35% phosphorus (P) and 0.4% carbon (C); The mass percentage of the amorphous nickel-based material powder in the main core powder is 20%, and the amorphous nickel-based material powder contains, by mass percentage, 60.5% nickel (Ni), 28% iron (Fe), 5% boron (B), 5% silicon (Si), and 1.5% phosphorus (P); The mass percentage of the magnetic powder in the residual magnetic powder is 62.5%, and the magnetic powder contains, by mass percentage, 77.05% iron (Fe), 9.5% nickel (Ni), 4.5% cobalt (Co), 5% silicon (Si), 3% boron (B), 0.6% phosphorus (P) and 0.35% niobium (Nb); The mass percentage of the soft magnetic powder in the residual magnetic powder is 37.5%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 20%, and the iron-silicon-chromium alloy powder contains, by mass percentage, 92% iron (Fe), 5.5% silicon (Si) and 2.5% chromium (Cr); The low-loss inductor according to claim 2 , wherein the mass percentage of the carbonyl iron powder in the soft magnetic powder is 80%.
6. A low loss inductor as claimed in any preceding claim, wherein the remanent magnetic material further comprises silicon dioxide.
7. The low-loss inductor of claim 6 , wherein the remnant magnetic body further comprises an insulating anti-corrosive layer formed on an outer surface of the remnant magnetic body.
8. The insulating anticorrosive layer comprises an epoxy resin and nanometer silicon powder; The mass percentage of the epoxy resin in the insulating rust-preventive layer is 80%, 8. The low-loss inductor as claimed in claim 7, wherein the mass percentage of the nanometer silicon powder in the insulating anti-corrosion layer is 20%.
9. The main core has a pillar portion and a central pillar, A base extends integrally from one end of the column, and protrusions are provided on two opposing edges of the base, The central pillar is integrally covered by the pillar portion so as to be located at an upper portion within the pillar portion, The coil has a winding portion and two end portions; The winding portion is attached to the column portion of the main core. The low-loss inductor of claim 8, wherein the two end portions are respectively bent and fixed to both sides of the two protrusions of the base so as to integrally form two electrodes, a solder layer is respectively formed on the bottom of the two electrodes, and the two electrodes and the solder layer are exposed from the residual magnetic material.
10. 10. The low-loss inductor according to claim 9, wherein the insulating anticorrosive layer has a thickness of 10-20 μm, and the solder layer has a thickness of 15-25 μm.
11. (a) providing a main core and preparing a remanent magnetic composite powder; (b) wrapping a coil around the main magnetic core; (c) placing the main core with the coil wrapped around it and the residual magnetic composite powder in a first mold such that the main core is covered and the coil is partially covered by the residual magnetic composite powder; (d) hot pressing the remnant magnetic composite powder in the first die to integrally form a remnant magnetic material; and (e) removing the residual magnetic body from the first die to obtain an inductor; In the step (a), The main core includes a main core powder, the main core powder comprising: An amorphous iron-based material powder containing, by mass percentage, 89.7 to 92.35% iron (Fe), 4 to 5% silicon (Si), 3.5 to 4% boron (B), 0.05 to 0.5% phosphorus (P), and 0.1 to 0.8% carbon (C); an amorphous nickel-based material powder containing, by mass percentage, 60.5-67.7% nickel (Ni), 25-28% iron (Fe), 3.5-5% boron (B), 3.5-5% silicon (Si), and 0.3-1.5% phosphorus (P); The remnant magnetic composite powder comprises a remnant magnetic powder, the remnant magnetic powder comprising: A magnetic powder containing, by mass percentage, 72.7 to 83.7% iron (Fe), 8 to 11% nickel (Ni), 3 to 5% cobalt (Co), 3 to 6% silicon (Si), 2 to 4% boron (B), 0.2 to 0.8% phosphorus (P), and 0.1 to 0.5% niobium (Nb); a soft magnetic powder comprising an iron-silicon-chromium alloy powder and a carbonyl iron powder; The iron-silicon-chromium alloy powder contains, by mass percentage, 90.5 to 93.5% iron (Fe), 4.5 to 6.5% silicon (Si), and 2 to 3% chromium (Cr).
12. the mass percentage of the amorphous iron-based material powder in the main core powder is 70 to 90%; The mass percentage of the amorphous nickel-based material powder in the main core powder is 10 to 30%; The mass percentage of the magnetic powder in the residual magnetic powder is 59 to 67%, The mass percentage of the soft magnetic powder in the residual magnetic powder is 33 to 41%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 17 to 33%; The method for producing a low-loss inductor according to claim 11, wherein the mass percentage of the carbonyl iron powder in the soft magnetic powder is 67 to 83%.
13. In the step (a), The mass percentage of the amorphous iron-based material powder in the main core powder is 70%, and the amorphous iron-based material powder contains, by mass percentage, 92.35% iron (Fe), 4% silicon (Si), 3.5% boron (B), 0.05% phosphorus (P), and 0.1% carbon (C); The mass percentage of the amorphous nickel-based material powder in the main core powder is 30%, and the amorphous nickel-based material powder contains, by mass percentage, 60.5% nickel (Ni), 28% iron (Fe), 5% boron (B), 5% silicon (Si), and 1.5% phosphorus (P); The mass percentage of the magnetic powder in the residual magnetic powder is 59%, and the magnetic powder contains, by mass percentage, 83.7% iron (Fe), 8% nickel (Ni), 3% cobalt (Co), 3% silicon (Si), 2% boron (B), 0.2% phosphorus (P) and 0.1% niobium (Nb); The mass percentage of the soft magnetic powder in the residual magnetic powder is 41%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 17%, and the iron-silicon-chromium alloy powder contains, by mass percentage, 90.5% iron (Fe), 6.5% silicon (Si) and 3% chromium (Cr); The method for producing a low-loss inductor according to claim 12, wherein a mass percentage of the carbonyl iron powder in the soft magnetic powder is 83%.
14. In the step (a), The mass percentage of the amorphous iron-based material powder in the main core powder is 90%, and the amorphous iron-based material powder contains, by mass percentage, 89.7% iron (Fe), 5% silicon (Si), 4% boron (B), 0.5% phosphorus (P) and 0.8% carbon (C); The mass percentage of the amorphous nickel-based material powder in the main core powder is 10%, and the amorphous nickel-based material powder contains, by mass percentage, 67.7% nickel (Ni), 25% iron (Fe), 3.5% boron (B), 3.5% silicon (Si), and 0.3% phosphorus (P); The mass percentage of the magnetic powder in the residual magnetic powder is 67%, and the magnetic powder contains, by mass percentage, 72.7% iron (Fe), 11% nickel (Ni), 5% cobalt (Co), 6% silicon (Si), 4% boron (B), 0.8% phosphorus (P) and 0.5% niobium (Nb); The mass percentage of the soft magnetic powder in the residual magnetic powder is 33%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 33%, and the iron-silicon-chromium alloy powder contains, by mass percentage, 93.5% iron (Fe), 4.5% silicon (Si) and 2% chromium (Cr); The method for producing a low-loss inductor according to claim 12, wherein a mass percentage of the carbonyl iron powder in the soft magnetic powder is 67%.
15. In the step (a), The mass percentage of the amorphous iron-based material powder in the main core powder is 80%, and the amorphous iron-based material powder has, by mass percentage, 91% iron (Fe), 4.5% silicon (Si), 3.75% boron (B), 0.35% phosphorus (P) and 0.4% carbon (C); The mass percentage of the amorphous nickel-based material powder in the main core powder is 20%, and the amorphous nickel-based material powder contains, by mass percentage, 60.5% nickel (Ni), 28% iron (Fe), 5% boron (B), 5% silicon (Si), and 1.5% phosphorus (P); The mass percentage of the magnetic powder in the residual magnetic powder is 62.5%, and the magnetic powder contains, by mass percentage, 77.05% iron (Fe), 9.5% nickel (Ni), 4.5% cobalt (Co), 5% silicon (Si), 3% boron (B), 0.6% phosphorus (P) and 0.35% niobium (Nb); The mass percentage of the soft magnetic powder in the residual magnetic powder is 37.5%, The mass percentage of the iron-silicon-chromium alloy powder in the soft magnetic powder is 20%, and the iron-silicon-chromium alloy powder is, by mass percentage, 92% iron (Fe), 5.5% silicon (Si) and 2.5% chromium (Cr); The method for producing a low-loss inductor according to claim 12, wherein a mass percentage of the carbonyl iron powder in the soft magnetic powder is 80%.
16. In the step (a), the main core is (a1) mixing the main core powder with an adhesive and a solvent to form a main core glue; (a2) filling the main core glue into a second mold to integrally form a main core blank; and (a3) drying the main core blank at a temperature of 210° C. for 5 to 10 minutes to remove the solvent, and further hardening the main core blank to form the main core.
17. In the step (a), the remanent magnetic composite powder is (a4) mixing the residual magnetic powder with an organic resin and a solvent to form a residual magnetic suspension; (a5) drying the residual magnetic material suspension to remove the solvent and obtain the residual magnetic material composite powder; (a6) mixing gas-phase silicon dioxide and a silane coupling agent into the residual magnetic composite powder to form a silicon dioxide coating layer on the surface of the residual magnetic composite powder; the mass percentage of the gas phase silicon dioxide in the remanent magnetic composite powder is 0.05-0.2%; The method for producing a low-loss inductor according to claim 16, wherein the mass percentage of the silane coupling agent in the remanent magnetic composite powder is 0.1-0.5%.
18. In the step (a1), the adhesive comprises an unsaturated polyester resin, bisphenol A diglycidyl ether and 4,4'-dihydroxydiphenylmethane, and the solvent comprises cyclohexanone and acetone; The mass percentage of the unsaturated polyester resin in the main core glue is 0.1 to 0.3%; The mass percentage of the bisphenol A diglycidyl ether in the main core glue is 0.8 to 1.2%; The mass percentage of the 4,4'-dihydroxydiphenylmethane in the main core glue is 0.2 to 0.4%; The mass percentages of the cyclohexanone and the acetone in the main core glue are each 5 to 10%; In the step (a2), the main core glue is pressed in the second mold under a pressure of 500 to 900 MPa to harden the adhesive and integrally mold the main core blank; In step (a4), the organic resin comprises an unsaturated polyester resin, bisphenol A diglycidyl ether, and 4,4'-dihydroxydiphenylmethane, and the solvent comprises cyclohexanone and acetone; The mass percentage of the unsaturated polyester resin in the residual magnetic material suspension is 0.05 to 0.15%; The mass percentage of the bisphenol A diglycidyl ether in the residual magnetic material suspension is 0.5 to 0.7%; The mass percentage of the 4,4'-dihydroxydiphenylmethane in the residual magnetic material suspension is 0.1 to 0.2%; the mass percentage of the cyclohexanone in the residual magnetic material suspension is 7 to 15%; The method for producing a low-loss inductor according to claim 17, wherein the mass percentage of the acetone in the residual magnetic material suspension is 2 to 5%.
19. 20. The method for manufacturing a low-loss inductor according to claim 18, wherein in the step (d), the remnant magnetic composite powder is hot-pressed in the first mold under a pressure of 150 to 300 MPa and a temperature of 100 to 150°C to integrally form the remnant magnetic material.
20. The method further includes a step (f) performed after the step (e), 20. The method for manufacturing a low-loss inductor according to claim 19, wherein in the step (f), an insulating paint is applied to an outer surface of the residual magnetic body of the inductor, and the insulating paint is dried to form an insulating rust-preventive layer.
21. The method for manufacturing a low-loss inductor according to claim 20, wherein the insulating paint contains, by mass percentage, 90-95% N-methyl-2-pyrrolidone, 4-8% epoxy resin, and 1-2% nanometer silicon powder.
22. The particle size of the amorphous iron-based material powder in the main core powder is 5 to 15 μm, The particle size of the amorphous nickel-based material powder in the main core powder is 10 to 20 μm; The particle size of the magnetic powder in the residual magnetic powder is 15 to 25 μm, The particle size of the soft magnetic powder in the residual magnetic powder is 1 to 3 μm, The particle size of the vapor-phase silicon dioxide is 15 to 30 nm; The method for manufacturing a low-loss inductor as claimed in claim 21, wherein the particle size of the nanometer silicon powder is 80-120 nm.
23. In the step (a2), a central pillar is disposed in the first die so as to be located at an upper portion in the first die, and the central pillar is integrally covered with the main core glue; 23. The method for manufacturing a low-loss inductor according to claim 22, wherein in the step (b), the winding portion of the coil is ring-mounted around a pillar portion of the main core, and two end portions of the coil are bent and fixed to a base of the main core to form two electrodes.
24. The method further includes a step (g) performed after the step (f), 24. The method for manufacturing a low-loss inductor according to claim 23, wherein in the step (g), a solder layer having a thickness of 15 to 25 μm is formed on the bottom of each of the two electrodes.
Citation Information
Patent Citations
Amorphous core and accelerator using the same
JP1999233327A
Dust core and its manufacturing method
JP2001267114A
Composite magnetic material, dust core using the same, and magnetic element
JP2007134381A
Electronic component
JP2016157751A
Coil component, electronic equipment, metal magnetic powder and support device
JP2019176053A