AI Technical Summary
【0012】 本発明に係る電極は、電極活物質シートと、前記電極活物質シートに少なくとも一部が挿入されるメッシュ構造体を含む集電体と、を含んでおり、釘などの金属物体が電極を貫通するとしても、メッシュ構造体と金属物体が互いに接触しないか、または金属物体がメッシュ構造体と接触するとしてもメッシュ構造体の一部のみが切れるだけである。このため、金属物体と集電体が接する面積を減少させることができるため、電気的短絡を防止し、釘刺し安全性を向上させることができる。
Smart Images

Figure 0007558608000003 
Figure 0007558608000004 
Figure 0007558608000001
Abstract
Description
[Technical Field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0024422, filed February 27, 2020, the entire contents of which are incorporated herein by reference. The present invention relates to an electrode, a method for producing the same, and a secondary battery including the same. [Background technology]
[0002] The rapid increase in fossil fuel use has led to an increasing demand for alternative and clean energy, and as part of this, the most actively researched field is the field of power generation and storage using electrochemical reactions.
[0003] Currently, a representative example of an electrochemical device that uses electrochemical energy is a secondary battery. Secondary batteries generate electrical energy through electrochemical oxidation and reduction reactions and are used in a wide variety of applications. For example, secondary batteries are increasingly being used in a variety of applications, including portable devices such as mobile phones, laptop computers, digital cameras, video cameras, tablet PCs, and power tools; various electrically driven power devices such as electric bicycles, electric motorcycles, electric cars, hybrid cars, electric boats, and electric airplanes; power storage devices used to store electricity generated through renewable energy sources or surplus electricity; and uninterruptible power supplies (UPSs) that provide a stable supply of power to various information and communication devices, including server computers and communication base stations.
[0004] Generally, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The positive and negative electrodes are generally fabricated by applying an electrode slurry containing an electrode active material onto a current collector, followed by rolling and drying. The secondary battery is inserted into an exterior material and used in the form of a battery pack.
[0005] Meanwhile, when a secondary battery is subjected to a strong impact from a sharp metallic object, the object may penetrate an electrode. In this case, the metallic object may be electrically connected to a current collector, or electrodes of opposite polarity may be electrically connected by the metallic object, forming a short circuit. This may cause a large short-circuit current to flow through the short circuit, generating a large amount of heat. The resulting heat may induce rapid decomposition of the electrolyte, resulting in the rapid generation of a large amount of gas and heat, which may cause the secondary battery to explode.
[0006] Therefore, in the field of secondary batteries, various methods have been attempted to improve safety for nail penetration, such as increasing the resistance of the electrode to reduce the amount of current, forming a coating layer on the electrode, etc. However, these methods have the problem of causing an increase in resistance or a decrease in the amount of current, which goes against the development direction of secondary batteries that require high output. Therefore, in the field of secondary batteries, which require high output, there is a demand for the development of secondary batteries with improved nail penetration safety.
[0007] Korean Patent Publication No. 10-2014-0015841 discloses a lithium secondary battery including electrodes with a double coating layer formed thereon to improve safety against nail penetration, but there are limitations to solving the above-mentioned problems. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 10-2014-0015841 Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide an electrode that is excellent in nail penetration safety, has reduced resistance, and has excellent output characteristics. Another object of the present invention is to provide a method for manufacturing the above-mentioned electrode. Another object of the present invention is to provide a secondary battery including the electrode. [Means for solving the problem]
[0010] The present invention provides an electrode comprising: an electrode active material sheet containing an electrode active material and a binder polymer; and a current collector containing a mesh structure, wherein at least a portion of the mesh structure is inserted into the electrode active material sheet; and the binder polymer has a thermal decomposition temperature of 270°C to 315°C.
[0011] The present invention also provides a method for manufacturing the aforementioned electrode, comprising the steps of: preparing a current collector including a mesh structure and an electrode active material sheet including an electrode active material and a binder polymer; and positioning the electrode active material sheet on the current collector and applying pressure to insert at least a portion of the mesh structure into the electrode active material sheet. The present invention also provides a secondary battery including the above-described electrode. [Effects of the Invention]
[0012] The electrode according to the present invention includes an electrode active material sheet and a current collector including a mesh structure at least a portion of which is inserted into the electrode active material sheet, and even if a metal object such as a nail penetrates the electrode, the mesh structure and the metal object do not come into contact with each other, or even if the metal object comes into contact with the mesh structure, only a portion of the mesh structure is broken. This reduces the contact area between the metal object and the current collector, thereby preventing electrical shorts and improving safety against nail penetration.
[0013] Furthermore, according to the electrode of the present invention, a binder polymer having a thermal decomposition temperature within a specific range is contained in the electrode active material sheet, which improves the heat resistance of the electrode active material sheet to a preferred level, thereby improving nail penetration safety and reducing the resistance within the electrode active material sheet, making it possible to realize an electrode and secondary battery with simultaneously improved nail penetration safety and output characteristics.
[0014] Furthermore, the electrode manufacturing method of the present invention can be performed by placing an electrode active material sheet on a current collector including a mesh structure and then applying pressure, thereby enabling the manufacture of an electrode with improved nail penetration safety and output characteristics. Furthermore, an electrode active material sheet manufactured using a binder polymer having a specific range of thermal decomposition temperature can have excellent adhesive strength with the current collector. [Brief explanation of the drawings]
[0015] [Figure 1] 1A to 1C are diagrams for schematically illustrating a method for manufacturing an electrode according to the present invention. [Figure 2] 1 is a schematic plan view of an electrode manufactured by the electrode manufacturing method of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0016] The terms and words used in this specification and claims should not be interpreted in a limited way to their ordinary or dictionary meanings, but should be interpreted in a way that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best explain their inventions.
[0017] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. The singular expressions include the plural expressions unless otherwise clearly indicated in the context.
[0018] It should be understood that in this specification, the terms "comprises," "comprises," or "having" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but do not preclude the presence or possible addition of one or more other features, numbers, steps, components, or combinations thereof.
[0019] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method is generally capable of measuring particle sizes from the submicron range to several mm, and can provide results with high reproducibility and high resolution. The present invention will be specifically described below.
[0020] <Electrode> The present invention relates to an electrode, specifically an electrode for a lithium secondary battery. Specifically, the electrode according to the present invention comprises an electrode active material sheet containing an electrode active material and a binder polymer, and a current collector containing a mesh structure, at least a portion of the mesh structure being inserted into the electrode active material sheet, and the thermal decomposition temperature of the binder polymer is 270°C to 315°C.
[0021] The electrode according to the present invention includes an electrode active material sheet and a current collector including a mesh structure at least a portion of which is inserted into the electrode active material sheet, and even if a metal object such as a nail penetrates the electrode, the mesh structure and the metal object do not come into contact with each other, or even if the metal object comes into contact with the mesh structure, only a portion of the mesh structure is broken. This reduces the contact area between the metal object and the current collector, thereby preventing electrical shorts and improving safety against nail penetration.
[0022] Furthermore, according to the electrode of the present invention, a binder polymer having a thermal decomposition temperature within a specific range is contained in the electrode active material sheet, which improves the heat resistance of the electrode active material sheet to a preferred level, thereby improving nail penetration safety and reducing the resistance within the electrode active material sheet, making it possible to realize an electrode and secondary battery with simultaneously improved nail penetration safety and output characteristics.
[0023] The electrode active material sheet includes an electrode active material and a binder polymer. The electrode active material may be selected from a positive electrode active material and a negative electrode active material, specifically, a negative electrode active material. The positive electrode active material and the negative electrode active material may be general positive electrode active materials and negative electrode active materials used in the relevant field without any limitation.
[0024] The negative electrode active material may be at least one selected from a carbon-based active material and a silicon-based active material, and specifically may be a carbon-based active material. The carbon-based active material may include at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon, and preferably includes at least one selected from the group consisting of artificial graphite and natural graphite.
[0025] The average particle size (D 50 ) may be 3 μm to 25 μm, preferably 8 μm to 15 μm, in order to achieve structural stability of the active material during charge and discharge and to further facilitate the accessibility of the binder polymer for binding the active material and the current collector.
[0026] The silicon-based active material is SiO x It may contain a compound represented by (0≦x<2). In the case of SiO2, x is preferably within the above range because SiO2 does not react with lithium ions and cannot store lithium.
[0027] The average particle size (D 50) may be 1 μm to 15 μm, preferably 2 μm to 10 μm, in terms of achieving structural stability of the active material during charge and discharge and further facilitating the accessibility of the binder polymer that binds the active material and the current collector.
[0028] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium composite metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium. More specifically, the lithium composite metal oxide may be a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), a lithium-nickel-cobalt-based oxide (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), a lithium-manganese-cobalt-based oxide (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < Z1 < 2), etc.), a lithium-nickel-manganese-cobalt-based oxide (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc.), or a lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1), etc.) etc. may be mentioned, and one or more of these compounds may be included. Among them, in terms of being able to enhance the capacity characteristics and safety of the battery, the lithium composite metal oxide is LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (for example, Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.). Considering the significance of the improvement effect according to the control of the type and content ratio of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc., and one or more mixtures of these may be used. The electrode active material may be contained in the electrode active material sheet at 80% to 99% by weight, preferably 90% to 97% by weight.
[0029] The binder polymer may be used for binding between the electrode active material sheet and the current collector and between the electrode active materials in the electrode active material sheet. The thermal decomposition temperature of the binder polymer is 270° C. to 315° C. When the thermal decomposition temperature of the binder polymer is within this range, the heat resistance and strength of the binder polymer can be improved to a desirable level, thereby significantly reducing the risk of the electrode exploding even if the electrode is penetrated by an external object, and the resistance of the electrode active material sheet can be reduced, thereby improving the output characteristics of the electrode.
[0030] If the thermal decomposition temperature of the binder polymer is less than 270°C, the heat resistance and strength of the binder polymer may not be improved to an appropriate level, resulting in reduced nail penetration safety. If the thermal decomposition temperature of the binder polymer is more than 315°C, the heat resistance of the binder polymer may increase, but the adhesive strength of the binder polymer may be significantly reduced. As a result, the active material may detach from the current collector, reducing stability and increasing the resistance of the electrode active material sheet, potentially impairing output characteristics.
[0031] Preferably, the thermal decomposition temperature of the binder polymer may be 290°C to 305°C. When the temperature is in this range, the heat resistance, strength, and adhesive force of the binder polymer can all be improved to excellent levels, thereby improving nail penetration safety and battery characteristics.
[0032] The binder polymer may include a first binder polymer and a second binder polymer that are different from each other. By using both the first binder polymer and the second binder polymer, it is possible to realize a binder polymer having a desired thermal decomposition temperature, thereby enabling the manufacture of an electrode with improved nail penetration safety and output characteristics.
[0033] The first binder polymer may be at least one selected from the group consisting of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), and fluororubber, preferably at least one selected from styrene-butadiene rubber and polyvinylidene fluoride, more preferably styrene-butadiene rubber. Using such a material as the first binder polymer is preferred because it can further improve adhesion to a current collector including a mesh structure.
[0034] The second binder polymer may be polytetrafluoroethylene (PTFE). When polytetrafluoroethylene is used as the second binder polymer, the second binder polymer can be smoothly dispersed in the electrode active material layer during dry formation of the electrode active material layer, improving the heat resistance and strength of the electrode active material sheet to a desirable level, thereby improving nail penetration safety even if an external metallic object penetrates the electrode. Furthermore, when the second binder polymer is used together with the first binder polymer, a sheet-shaped electrode active material sheet can be produced by dry mixing the electrode active material and the binder polymer, allowing the electrode active material sheet to be smoothly inserted into a current collector including a mesh structure, as described below.
[0035] The weight-average molecular weight of the polytetrafluoroethylene may be 8,000 to 56,000, preferably 24,000 to 50,000. When the weight-average molecular weight is within the above range, the heat resistance and strength of the electrode active material sheet can be improved, and the adhesive strength can be further improved, which is preferable.
[0036] The binder polymer may contain the first binder polymer and the second binder polymer in a weight ratio of 60:40 to 99.9:0.1, preferably a weight ratio of 75:25 to 99:1, and more preferably a weight ratio of 85:15 to 92.5:7.5. In this case, the thermal decomposition temperature of the binder polymer according to the present invention can be easily achieved, and the effects of simultaneously improving the nail penetration safety and output characteristics described above are preferably achieved, which is preferable.
[0037] When the binder polymer includes the first binder polymer and the second binder polymer, both the first binder polymer and the second binder polymer may satisfy the thermal decomposition temperature range according to the present invention, and the thermal decomposition temperature of the entire binder polymer may satisfy the thermal decomposition temperature range according to the present invention depending on the types and weight ratio of the first binder polymer and the second binder polymer.
[0038] The thermal decomposition temperature of the binder polymer may be measured by thermogravimetric analysis (TGA). The thermal decomposition temperature of the binder polymer may be defined as the temperature (onset temperature) at which the mass of the binder polymer decreases due to thermal decomposition when analyzed by TGA.
[0039] The binder polymer may be contained in the electrode active material sheet in an amount of 0.5 wt % to 20 wt %, preferably 1 wt % to 10 wt %, and this range is preferable because it can sufficiently improve the adhesive strength with the current collector while preventing an increase in resistance due to the addition of an excessive amount of the binder polymer.
[0040] The electrode active material sheet may further include a conductive material in addition to the electrode active material and the binder polymer. The conductive material is not particularly limited as long as it does not induce chemical changes in the battery and is conductive. For example, graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives may be used.
[0041] The conductive material may be contained in the electrode active material sheet in an amount of 0.1% by weight to 10% by weight, preferably 0.5% by weight to 5% by weight. The electrode active material sheet may have a thickness of 50 μm to 500 μm, preferably 100 μm to 300 μm.
[0042] The current collector includes a mesh structure. Because the electrode according to the present invention uses a current collector including a mesh structure, even if an external object penetrates the electrode, the contact area between the external object and the current collector can be reduced compared to commonly used sheet-shaped current collectors, thereby reducing the possibility of fire or explosion due to an electrical short circuit.
[0043] The mesh structure may be a three-dimensional net-like structure, and may have meshes or holes formed by the intersection of a plurality of straight lines or curves. At least a portion of the mesh structure may be inserted into the electrode active material sheet. According to the electrode of the present invention, at least a portion of the mesh structure may be inserted into the electrode active material sheet, and the mesh within the mesh structure may be present inside the electrode active material sheet.
[0044] The mesh structure may contain at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and aluminum-cadmium alloy, and more preferably contains copper.
[0045] Since at least a portion of the current collector including the mesh structure is inserted into the electrode active material sheet, the size and thickness of the mesh structure may be adjusted in consideration of the size and thickness of the electrode active material sheet.
[0046] The mesh structure includes a plurality of meshes. The width of the holes formed by the meshes in the mesh structure is 0.010 mm. 2 ~225mm 2 , preferably 0.25 mm 2 ~9.0mm 2 When the thickness is within this range, the possibility of electrical connection between the mesh structure and an external object, such as a nail, being pierced can be reduced while improving the adhesive strength with the electrode active material sheet, thereby improving safety against nail penetration and reducing the possibility of the electrode active material sheet detaching from the mesh structure. In this specification, a "mesh hole" can be defined as a planar figure formed by the intersection of adjacent straight lines or curves within the mesh, and the planar figure may be a polygon such as a triangle or a rectangle, or a circle.
[0047] The electrode may be a positive electrode and / or a negative electrode, specifically a negative electrode. Specifically, copper may be used as the current collector of the negative electrode. However, because copper is highly flexible, there is a high possibility that an external object such as a nail may penetrate the sheet-shaped current collector and come into contact with the positive electrode current collector, thereby inducing an electrical short circuit. However, when the electrode of the present invention is used as a negative electrode, it is preferable because it has excellent nail penetration safety and can prevent the risk of an electrical short circuit.
[0048] <Electrode manufacturing method> The present invention also provides a method for producing an electrode, specifically, a method for producing the electrode described above.
[0049] Specifically, the method for manufacturing an electrode of the present invention provides a method for manufacturing the aforementioned electrode, which includes the steps of preparing a current collector including a mesh structure and an electrode active material sheet including an electrode active material and a binder polymer, and positioning the electrode active material sheet on the current collector and applying pressure to the electrode active material sheet so that at least a portion of the mesh structure is inserted into the electrode active material sheet.
[0050] According to the method for manufacturing an electrode of the present invention, the electrode can be manufactured by placing an electrode active material sheet on a current collector including a mesh structure and applying pressure, thereby enabling the manufacture of an electrode with improved nail penetration safety and output characteristics. Furthermore, an electrode active material sheet manufactured using a binder polymer having a specific range of thermal decomposition temperature can have excellent adhesive strength with the current collector.
[0051] Hereinafter, the method for manufacturing an electrode according to the present invention will be described in detail with reference to the drawings. When assigning reference numerals to components in each drawing, identical components may be assigned the same reference numerals when displayed in other drawings as much as possible. Furthermore, when describing the present invention, if it is determined that a detailed description of related known structures or functions may obscure the gist of the present invention, such a detailed description will be omitted.
[0052] Fig. 1 is a diagram for schematically explaining the method for producing an electrode of the present invention, and Fig. 2 is a plan view of an electrode produced by the method for producing an electrode of the present invention. Referring to FIG. 1, the method for manufacturing an electrode of the present invention includes the steps of preparing a current collector 10 including a mesh structure 11, and electrode active material sheets 20a and 20b including an electrode active material and a binder polymer.
[0053] The mesh structure 11 includes a plurality of meshes. As shown in FIGS. 1 and 2, the width of the mesh holes 12 in the mesh structure 11 is 0.010 mm. 2 ~225mm 2 , preferably 0.25 mm 2 ~9.0mm 2When the thickness is within this range, the possibility of electrical connection between the mesh structure and an external object, such as a nail, being pierced can be reduced while improving the adhesive strength with the electrode active material sheet, thereby improving safety against nail penetration and reducing the possibility of the electrode active material sheet detaching from the mesh structure. In this specification, the "mesh hole 12" can be defined as a planar figure formed by the intersection of adjacent straight lines or curves within the mesh, and the planar figure may be a polygon such as a triangle or a rectangle, or a circle. The current collector 10 including the mesh structure 11 is as explained in the electrode described above.
[0054] The electrode active material sheets 20a, 20b may be manufactured by a method including the following steps: (a) mixing an electrode active material and a binder polymer to prepare a granular composite; (b) sieving the granular composite; and (c) pressing the granular composite to produce an electrode active material sheet;
[0055] According to the method for manufacturing an electrode active material sheet, a granular composite is prepared by mixing an electrode active material and a binder polymer (step (a)). When the electrode active material and the binder are mixed, the adhesive force of the binder allows the electrode active material and the binder to be combined to form a granular composite. The electrode active material and the binder polymer are as described above in the electrode.
[0056] A conductive material may be further mixed with the electrode active material and the binder polymer, as described above in connection with the electrode.
[0057] The electrode active material and the binder polymer may be mixed by dry mixing, which is preferable because the dry mixing does not require a drying step of the mixture.
[0058] The method for manufacturing an electrode active material sheet includes a step of sieving the granular composite (step (b)). The sieving step can improve the uniformity of the granular composite, thereby enabling the components in the electrode active material sheet to be distributed uniformly.
[0059] According to the method for manufacturing an electrode active material sheet, the granular composite is pressed to manufacture an electrode active material sheet (step (c)). By applying pressure to the granular composite, the granular composite aggregates, and a sheet-shaped electrode active material sheet can be manufactured. The rest of the electrode active material sheets 20a and 20b are the same as those described above in connection with the electrodes.
[0060] The electrode manufacturing method of the present invention also includes a step of placing the electrode active material sheets 20a, 20b on the current collector 10 and pressing them to insert at least a portion of the mesh structure 11 into the electrode active material sheets 20a, 20b.
[0061] As shown in FIGS. 1 and 2, the electrode active material sheets 20a and 20b are placed on the current collector 10 and then pressed, so that the mesh structure 11 is inserted into at least a portion of the electrode active material sheets 20a and 20b.
[0062] The electrode active material sheets 20a and 20b may be disposed on one or both sides of the current collector 10. For example, as shown in FIG. 1, the electrode active material sheets 20a and 20b may be disposed on both sides of the current collector 10.
[0063] The pressure may be applied by linear pressure, for example, by applying roll presses 30a and 30b to the electrode active material sheet placed on the current collector, so that at least a portion of the mesh structure is inserted into the electrode active material sheet.
[0064] <Secondary battery> The present invention also provides a secondary battery, more specifically a lithium secondary battery, including the above-described electrode.
[0065] Specifically, the secondary battery may include a negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. The negative electrode and / or the positive electrode, preferably the negative electrode, may be the above-described electrode.
[0066] The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator typically used in secondary batteries can be used without particular limitations. It is particularly preferable that the separator exhibits low resistance to electrolyte ion migration and excellent electrolyte humidification. Specifically, porous polymer films, such as those made from polyolefin-based polymers such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers, or laminates of two or more layers thereof, may be used. Conventional porous nonwoven fabrics, such as nonwoven fabrics made from high-melting-point glass fibers or polyethylene terephthalate fibers, may also be used. To ensure heat resistance or mechanical strength, a separator coated with a ceramic component or a polymeric material may be used, and may be selectively used as a single-layer or multi-layer structure.
[0067] Examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in manufacturing lithium secondary batteries.
[0068] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt. Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0069] In particular, among the carbonate organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are preferably used because they are high-viscosity organic solvents with high dielectric constants and dissociate lithium salts well. When such cyclic carbonates are mixed with linear carbonates having low viscosity and low dielectric constants, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte having high electrical conductivity can be prepared, and therefore these cyclic carbonates are more preferably used.
[0070] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte solution. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3- , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - One or more selected from the group consisting of:
[0071] In addition to the constituent components of the electrolyte, the electrolyte may further include one or more additives, such as a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.
[0072] According to another embodiment of the present invention, there is provided a battery module including the secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the secondary battery having high capacity, high rate characteristics, and high cycle characteristics, and can be used as a power source for medium to large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.
[0073] Below, preferred examples are presented to help understand the present invention. However, the following examples are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope and technical spirit of the present description, and it goes without saying that such changes and modifications fall within the scope of the appended claims.
[0074] Example Example 1 <Production of electrode active material sheets> The binder polymers used were a mixture of styrene-butadiene rubber as the first binder polymer and polytetrafluoroethylene (weight average molecular weight: 40,000 g / mol) as the second binder polymer in a weight ratio of 90:10. The thermal decomposition temperature of the binder polymer measured by thermogravimetric analysis (TGA) was 297°C.
[0075] As the negative electrode active material, artificial graphite (average particle size (D 50 A granular composite was prepared by dry-mixing a granular composite with a sieve of 18 μm (product name: Super-C, manufactured by Timcal) as a conductive material in a weight ratio of 95:4:1. The granular composite was added to distilled water to a solid content of 85%, stirred for 2 hours using a planetary mixer, and then sieved through a 5 mm mesh diameter sieve. The granular composite was arranged in a sheet form and pressed by linear pressure using a roll press to produce an electrode active material sheet.
[0076] <Electrode manufacturing> The dimensions of the mesh are 36mm x 56mm x 0.05mm, the mesh diameter is 1mm, and the mesh hole size is 1mm. 2 A current collector including a copper mesh structure (1 mm wide x 1 mm long) was prepared.
[0077] The electrode active material sheets produced above were placed on both sides of a current collector, and linear pressure was applied using a roll press to insert the mesh structure into the electrode active material sheets, resulting in the negative electrode of Example 1. In the negative electrode produced above, the thickness of the electrode active material sheets was 200 μm.
[0078] Example 2 A negative electrode was manufactured in the same manner as in Example 1, except that a mixture of the first binder polymer and the second binder polymer in a weight ratio of 95:5 was used as the binder polymer (thermal decomposition temperature: 308°C).
[0079] Example 3 A negative electrode was manufactured in the same manner as in Example 1, except that a mixture of the first binder polymer and the second binder polymer in a weight ratio of 80:20 was used as the binder polymer (thermal decomposition temperature: 284°C).
[0080] Comparative Example 1 A negative electrode was manufactured in the same manner as in Example 1, except that only the second binder polymer (thermal decomposition temperature: 326° C.) used in Example 1 was used as the binder polymer.
[0081] Comparative Example 2 The same method as in Example 1 was carried out, except that only the first binder polymer (thermal decomposition temperature: 263°C) used in Example 1 was used as the binder polymer. However, in the case of Comparative Example 2, the dispersibility of the binder polymer used was low, so it was impossible to manufacture a negative electrode itself.
[0082] Comparative Example 3 The negative electrode active material used in Example 1, a binder polymer mixture of styrene-butadiene rubber and carboxymethyl cellulose in a weight ratio of 2:1, and carbon black (product name: Super-C, manufacturer: Timcal) as a conductive material were added to distilled water in a weight ratio of 95:4:1 to prepare a negative electrode slurry.
[0083] The negative electrode slurry was applied to a sheet-shaped copper current collector (thickness: 20 μm), rolled, and dried in a vacuum oven at 130° C. for 10 hours to form a negative electrode active material layer (thickness: 210 μm), thereby manufacturing a negative electrode.
[0084] [Table 1]
[0085] Experimental Example <Secondary battery manufacturing> LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, carbon black as a conductive material, and PVdF as a binder were mixed in a weight ratio of 94:3.5:2.5 and added to N-methyl-2-pyrrolidone (NMP) to prepare a cathode slurry. The prepared cathode slurry was coated on an aluminum current collector, dried, rolled, and then cut to a certain size to prepare a cathode.
[0086] An electrode assembly was prepared by interposing a porous polyethylene separator between the positive electrode prepared as described above and the negative electrode of Example 1. The electrode assembly was then placed inside a case, and an electrolyte was injected into the case to prepare a secondary battery of Example 1.
[0087] The electrolyte used was an organic solvent in which ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a volume ratio of 30:70, to which LiPF6 was added as a lithium salt at a concentration of 1M.
[0088] Secondary batteries of Examples 2 to 3 and Comparative Examples 1 to 3 were manufactured in the same manner as in Example 1, except that the negative electrodes of Examples 2 to 3 and Comparative Examples 1 to 3 were used, respectively.
[0089] Experimental Example Experimental example 1: Nail penetration safety test The secondary batteries manufactured in Examples 1 to 3 and Comparative Examples 1 to 3 were fully charged at 0.1 C and 4.2 V, and then a nail with a diameter of 10 mm was lowered at a speed of 25 mm / s to pass through the center of the battery, and the penetration experiment was completed when the length of the nail protruding from the battery was 10 mm. Five secondary batteries manufactured in Examples 1 to 3 and Comparative Examples 1 to 3 were prepared, and the above penetration experiment was repeated five times.
[0090] Table 2 shows 1) the number of times secondary batteries ignited during the five experiments, and 2) the maximum temperature of unignited secondary batteries, if any.
[0091] [Table 2]
[0092] Referring to Table 2, it can be seen that the secondary batteries of the examples have a lower number of ignitions and a lower maximum temperature of the unignited secondary batteries than the comparative examples, and therefore have superior nail penetration safety. [Explanation of symbols]
[0093] 10: Current collector 11: Mesh structure 12: Mesh hole 20a, 20b: Electrode active material sheets 30a, 30b: Roll press
Claims
1. an electrode active material sheet including an electrode active material and a binder polymer; A current collector including a mesh structure having a three-dimensional network; Including, At least a portion of the mesh structure is present in a state of being inserted inside the electrode active material sheet, the binder polymer is composed only of a first binder polymer and a second binder polymer, the first binder polymer being at least one selected from the group consisting of styrene-butadiene rubber, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer, and fluororubber; the second binder polymer is polytetrafluoroethylene; The binder polymer has a thermal decomposition temperature of 270°C to 315°C.
2. 2. The electrode for a lithium secondary battery according to claim 1, wherein the binder polymer comprises the first binder polymer and the second binder polymer in a weight ratio of 60:40 to 99.9:0.
1.
3. 3. The electrode for a lithium secondary battery according to claim 1, wherein the binder polymer is contained in the electrode active material sheet in an amount of 0.5% by weight to 20% by weight.
4. 4. The electrode for a lithium secondary battery according to claim 1, wherein the mesh structure includes at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy.
5. The electrode for a lithium secondary battery according to claim 1 , wherein the electrode for a lithium secondary battery is a negative electrode.
6. 6. The electrode for a lithium secondary battery according to claim 5, wherein the electrode active material is at least one selected from the group consisting of a carbon-based active material and a silicon-based active material.
7. The mesh hole width in the mesh structure is 0.010 mm 2 ~225mm 2 The electrode for a lithium secondary battery according to claim 1 ,
8. A step of preparing a current collector including a mesh structure having a net shape and an electrode active material sheet including an electrode active material and a binder polymer; placing the electrode active material sheet on the current collector and applying pressure to insert at least a portion of the mesh structure into the electrode active material sheet; The method for producing the electrode for a lithium secondary battery according to claim 1 , comprising:
9. The method for producing an electrode for a lithium secondary battery according to claim 8 , wherein the electrode active material sheet is produced by a method including the steps of: (a) mixing an electrode active material and a binder polymer to prepare a granular composite; (b) sieving the granular composite; and (c) pressing the granular composite to produce an electrode active material sheet.
10. The method for producing an electrode for a lithium secondary battery according to claim 8 or 9, wherein the pressing is performed by linear pressure.
11. A secondary battery comprising the electrode for a lithium secondary battery according to claim 1 .
Citation Information
Patent Citations
Electrode for alkaline secondary battery
JP2002025547A
Electrode for nonaqueous electrolyte secondary battery, method for manufacturing the same, and non-aqueous secondary battery
JP2011134691A
Method of manufacturing lithium ion secondary battery
JP2014078318A
Method of rectifying warpage of electrode and device of rectifying warpage of electrode
JP2014238971A
Method for manufacturing electrode body
JP2019129075A