CURABLE RESIN COMPOSITION, DRY FILM, CURED PRODUCT, AND ELECTRONIC COMPONENT
The curable resin composition, incorporating specific components, addresses storage stability and sensitivity issues by using an alkali-soluble resin, ethylenically unsaturated groups, and melamine cyanurate, resulting in improved heat resistance and insulation reliability for electronic components.
Patent Information
- Application Number
- JP2020041378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-10
AI Technical Summary
Existing photosensitive curable resin compositions face challenges in achieving both storage stability and physical properties such as heat resistance and insulation reliability, particularly when formulated as one-component dry films, with issues arising from the inclusion of thermosetting components like melamine catalysts that reduce storage stability.
A curable resin composition comprising an alkali-soluble resin, a compound with ethylenically unsaturated groups, an epoxy resin with an epoxy equivalent of 130 g/eq. or more, melamine cyanurate, and a photopolymerization initiator, specifically using acylphosphine-based initiators to enhance exposure sensitivity and suppress thermal curing during storage.
The composition achieves improved storage stability, exposure sensitivity, and excellent physical properties like heat resistance and insulation reliability, with reduced outgassing and enhanced drying control, suitable for forming durable films and electronic components.
Smart Images

Figure 0007558668000001 
Figure 0007558668000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition, a dry film, a cured product, and an electronic component. [Background technology]
[0002] 2. Description of the Related Art Conventionally, photosensitive curable resin compositions that can be developed with an alkaline aqueous solution have been used as materials for forming permanent coatings such as solder resists and coverlays on printed wiring boards by exposure and development (for example, Patent Document 1).
[0003] By blending a thermosetting component into such a curable resin composition, the physical properties such as heat resistance and insulation reliability of the cured product can be improved. If the curing is insufficient, the physical properties cannot be secured, so a thermosetting component with excellent thermosetting properties such as an epoxy resin is desirable, but if the thermosetting property of the curable resin composition is high, the curing reaction is likely to occur even in the temperature range during storage, so there is a problem with storage stability. In particular, when a thermosetting catalyst such as melamine is blended to improve the thermosetting property, the decrease in storage stability is remarkable.
[0004] Furthermore, for the purpose of improving photocurability and physical properties of the cured product, a compound having an ethylenically unsaturated group, such as an acrylate monomer, can be blended. However, it is desirable for a photosensitive curable resin composition containing such a compound having an ethylenically unsaturated group to have high exposure sensitivity in order to improve productivity. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 61-243869 Summary of the Invention [Problem to be solved by the invention]
[0006] For the reasons described above, it is difficult to achieve both storage stability and physical properties of the cured product, particularly when the photosensitive curable resin composition is a one-component type or made into a dry film, and excellent exposure sensitivity is also required.
[0007] Therefore, an object of the present invention is to provide a curable resin composition capable of forming a cured product having excellent storage stability and exposure sensitivity, and excellent physical properties such as heat resistance and insulation reliability, a dry film having a resin layer obtained from the composition, a cured product of the composition or the resin layer of the dry film, and an electronic component having the cured product. [Means for solving the problem]
[0008] As a result of intensive investigations aimed at achieving the above object, the present inventors have found that the above problems can be solved by blending an alkali-soluble resin, a compound having an ethylenically unsaturated group, an epoxy resin having an epoxy equivalent of 130 g / eq. or more, melamine cyanurate, and a photopolymerization initiator, and have thus completed the present invention.
[0009] That is, the curable resin composition of the present invention is characterized by containing (A) an alkali-soluble resin, (B) a compound having an ethylenically unsaturated group, (C) an epoxy resin having an epoxy equivalent of 130 g / eq. or more, (D) melamine cyanurate, and (E) a photopolymerization initiator.
[0010] In the curable resin composition of the present invention, the blending amount of the (D) melamine cyanurate is preferably 1 to 20 parts by mass based on 100 parts by mass of the (A) alkali-soluble resin.
[0011] In the curable resin composition of the present invention, the (E) photopolymerization initiator preferably contains an acylphosphine-based photopolymerization initiator.
[0012] The dry film of the present invention is characterized by having a resin layer obtained by applying the curable resin composition onto a film and drying it.
[0013] The cured product of the present invention is characterized by being obtained by curing the curable resin composition or the resin layer of the dry film.
[0014] The electronic part of the present invention is characterized by having the above-mentioned cured product. Effect of the Invention
[0015] According to the present invention, it is possible to provide a curable resin composition capable of forming a cured product having excellent storage stability and exposure sensitivity, and excellent physical properties such as heat resistance and insulation reliability, a dry film having a resin layer obtained from the composition, a cured product of the composition or the resin layer of the dry film, and an electronic component having the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The curable resin composition of the present invention is characterized by containing (A) an alkali-soluble resin, (B) a compound having an ethylenically unsaturated group, (C) an epoxy resin having an epoxy equivalent of 130 g / eq. or more (hereinafter also referred to simply as "(C) epoxy resin"), (D) melamine cyanurate, and (E) a photopolymerization initiator. Although the detailed mechanism is not clear, the combination of (B) a compound having an ethylenically unsaturated group, (C) an epoxy resin, and (D) melamine cyanurate unexpectedly improves the exposure sensitivity. By improving the exposure sensitivity, the coating film can be cured even with a low exposure dose, leading to an improvement in the production tact. In addition, although the detailed mechanism is not clear, it is thought that the improvement in storage stability is due to the suppression of the function of (D) melamine cyanurate as a thermosetting catalyst under storage conditions. Furthermore, the present invention has excellent workability because it improves stability during drying and has a wide drying control range. In addition, the present invention reduces the generation of outgassing compared to the case where melamine is blended as a thermosetting catalyst.
[0017] From the viewpoint of sensitivity, the curable resin composition of the present invention preferably does not contain titanium oxide, and in particular, it is more preferable that the curable resin composition does not contain titanium oxide produced by the chlorine process.
[0018] Each component of the curable resin composition of the present invention will be described below. In this specification, (meth)acrylate is a general term for acrylate, methacrylate, and a mixture thereof, and the same applies to other similar expressions.
[0019] [(A) Alkali-soluble resin] (A) Examples of the alkali-soluble resin include a compound having two or more phenolic hydroxyl groups, a carboxyl group-containing resin, a compound having a phenolic hydroxyl group and a carboxyl group, and a compound having two or more thiol groups. Among them, it is preferable that the alkali-soluble resin is a carboxyl group-containing resin or a phenolic resin, since the adhesion to the base is improved. In particular, it is more preferable that the alkali-soluble resin is a carboxyl group-containing resin, since it has excellent developability. The carboxyl group-containing resin may be a carboxyl group-containing photosensitive resin having an ethylenically unsaturated group, or a carboxyl group-containing resin not having an ethylenically unsaturated group.
[0020] Specific examples of the carboxyl group-containing resin include the compounds (which may be either oligomers or polymers) listed below.
[0021] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.
[0022] (2) Carboxyl group-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl group-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0023] (3) Terminal carboxyl group-containing urethane resins obtained by reacting acid anhydrides with the terminals of urethane resins obtained by polyaddition reaction of diisocyanate compounds such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0024] (4) Carboxyl group-containing urethane resins obtained by polyaddition reaction of diisocyanates with (meth)acrylates of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins, and biphenol type epoxy resins, or their partial acid anhydride modified products, carboxyl group-containing dialcohol compounds, and diol compounds.
[0025] (5) A carboxyl group-containing urethane resin obtained by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (4) above, to obtain a terminal (meth)acrylated carboxyl group-containing urethane resin.
[0026] (6) A carboxyl group-containing urethane resin having terminal (meth)acrylation obtained by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (4) above.
[0027] (7) Carboxyl group-containing resins obtained by reacting a multifunctional epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the hydroxyl groups present in the side chains.
[0028] (8) A carboxyl group-containing resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a difunctional epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0029] (9) A carboxyl group-containing polyester resin obtained by reacting a polyfunctional oxetane resin with a dicarboxylic acid and adding a dibasic acid anhydride to the resulting primary hydroxyl group.
[0030] (10) A carboxyl group-containing resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0031] (11) A carboxyl group-containing resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0032] (12) A carboxyl group-containing resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic anhydride, or the like.
[0033] (13) A carboxyl group-containing resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in the molecule, such as glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, to the carboxyl group-containing resin described in (1) to (12) above.
[0034] As the carboxyl group-containing resin, it is preferable to use the above carboxyl group-containing resins (7) and (10) to (13).
[0035] Examples of compounds having a phenolic hydroxyl group include compounds having a biphenyl skeleton or a phenylene skeleton, or both skeletons, and phenol compounds having various skeletons synthesized using phenol, orthocresol, paracresol, metacresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, 3,5-xylenol, catechol, resorcinol, hydroquinone, methylhydroquinone, 2,6-dimethylhydroquinone, trimethylhydroquinone, pyrogallol, phloroglucinol, etc.
[0036] Examples of resins having a phenolic hydroxyl group include well-known and commonly used phenolic resins such as phenol novolak resin, alkylphenol volak resin, bisphenol A novolak resin, dicyclopentadiene type phenolic resin, Xylok type phenolic resin, terpene modified phenolic resin, polyvinylphenols, bisphenol F, bisphenol S type phenolic resin, poly-p-hydroxystyrene, condensates of naphthol and aldehydes, and condensates of dihydroxynaphthalene and aldehydes.
[0037] Commercially available phenolic resins include, for example, HF1H60 (manufactured by Meiwa Chemical Industry Co., Ltd.), Phenolite TD-2090, Phenolite TD-2131, Besumoru CZ-256-A (manufactured by DIC Corporation), Shounol BRG-555, Shounol BRG-556 (manufactured by Aica Kogyo Co., Ltd.), and polyvinylphenols CST70, CST90, S-1P, and S-2P (manufactured by Maruzen Petrochemical Co., Ltd.).
[0038] The acid value of the alkali-soluble resin (A) is suitably in the range of 40 to 200 mgKOH / g, more preferably in the range of 45 to 120 mgKOH / g. When the acid value of the alkali-soluble resin is 40 mgKOH / g or more, alkaline development becomes easy, while an acid value of 200 mgKOH / g or less is preferable because drawing of a normal cured product pattern becomes easy.
[0039] The weight-average molecular weight of the alkali-soluble resin (A) varies depending on the resin skeleton, but is preferably in the range of 1,500 to 150,000, more preferably 1,500 to 100,000. When the weight-average molecular weight is 1,500 or more, the tack-free performance is good, the moisture resistance of the coating film after exposure is good, and the film loss during development is suppressed, and the decrease in resolution can be suppressed. On the other hand, when the weight-average molecular weight is 150,000 or less, the developability is good and the storage stability is also excellent.
[0040] The (A) alkali-soluble resin can be used alone or in combination of two or more kinds.
[0041] [(B) Compound having an ethylenically unsaturated group] (B) The compound having an ethylenically unsaturated group is preferably a photopolymerizable vinyl monomer. The photopolymerizable vinyl monomer may be any of the known and commonly used ones, for example, styrene derivatives such as styrene, chlorostyrene, and α-methylstyrene; vinyl esters such as vinyl acetate, vinyl butyrate, and vinyl benzoate; vinyl ethers such as vinyl isobutyl ether, vinyl-n-butyl ether, vinyl-t-butyl ether, vinyl-n-amyl ether, vinyl isoamyl ether, vinyl-n-octadecyl ether, vinyl cyclohexyl ether, ethylene glycol monobutyl vinyl ether, and triethylene glycol monomethyl vinyl ether; (meth)acrylamides such as acrylamide, methacrylamide, N-hydroxymethyl acrylamide, N-hydroxymethyl methacrylamide, N-methoxymethyl acrylamide, N-ethoxymethyl acrylamide, and N-butoxymethyl acrylamide; allyl compounds such as triallyl isocyanurate, diallyl phthalate, and diallyl isophthalate; 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, and the like. (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate and other (meth)acrylic acid esters; hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate and other hydroxyalkyl (meth)acrylates; methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate and other alkoxyalkylene glycol mono(meth)acrylates; ethylene glycol di(meth)acrylate, butanediol di(meth)acrylates, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate and other alkylene polyol poly(meth)acrylates;Examples of the polyoxyalkylene glycol poly(meth)acrylates include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, ethoxylated trimethylolpropane triacrylate, and propoxylated trimethylolpropane tri(meth)acrylate; poly(meth)acrylates such as hydroxypivalic acid neopentyl glycol ester di(meth)acrylate; and isocyanurate-type poly(meth)acrylates such as tris[(meth)acryloxyethyl]isocyanurate. These may be used alone or in combination of two or more types according to the required properties.
[0042] The blending amount of the (B) compound having an ethylenically unsaturated group is preferably 1 to 30 parts by mass per 100 parts by mass of the (A) alkali-soluble resin.
[0043] [(C) Epoxy resin with an epoxy equivalent of 130 g / eq. or more] The structure of the (C) epoxy resin is not particularly limited so long as it has an epoxy equivalent of 130 g / eq. or more, and examples thereof include epoxidized vegetable oil; bisphenol A type epoxy resins; hydroquinone type epoxy resins; bisphenol type epoxy resins; thioether type epoxy resins; brominated epoxy resins; novolac type epoxy resins; biphenol novolac type epoxy resins; bisphenol F type epoxy resins; hydrogenated bisphenol A type epoxy resins; glycidylamine type epoxy resins; hydantoin type epoxy resins; alicyclic epoxy resins; trihydroxyphenylmethane type epoxy resins; alkylphenol type epoxy resins (e.g., bixylenol type epoxy resins). ); biphenol type epoxy resin; bisphenol S type epoxy resin; bisphenol A novolac type epoxy resin; tetraphenylolethane type epoxy resin; heterocyclic epoxy resin; diglycidyl phthalate resin; tetraglycidyl xylenoylethane resin; naphthalene group-containing epoxy resin; epoxy resin having a dicyclopentadiene skeleton; triphenylmethane type epoxy resin; epoxy resin having a silsesquioxane skeleton; glycidyl (meth)acrylate copolymer epoxy resin; cyclohexylmaleimide and glycidyl (meth)acrylate copolymer epoxy resin; epoxy-modified polybutadiene rubber derivative; CTBN-modified epoxy resin, etc. (C) The epoxy resin may be used alone or in combination of two or more.
[0044] Commercially available epoxy resins (C) include YX-4000 manufactured by Mitsubishi Chemical Corporation and NC-3000 manufactured by Nippon Kayaku Co., Ltd.
[0045] The equivalent weight of the epoxy resin (C) is preferably 150 to 300 g / eq. If it is within this range, an excellent balance between developability and heat resistance is achieved.
[0046] The blending amount of the (C) epoxy resin is preferably 10 to 50 parts by mass, and particularly preferably 20 to 30 parts by mass, per 100 parts by mass of the (A) alkali-soluble resin. Within this range, the glass transition temperature of the cured product can be increased, and a cured product with excellent physical properties can be obtained.
[0047] [(D) Melamine cyanurate] (D) Melamine cyanurate is a compound represented by the following formula. TIFF0007558668000001.tif35158
[0048] (D) Melamine cyanurate may be a commercially available product, for example, MC-4000, MC-4500, MC-6000, etc. manufactured by Nissan Chemical Industries, Ltd. (D) Melamine cyanurate preferably has a small particle size, for example, the average particle size is preferably less than 2 μm, and the maximum particle size is preferably less than 20 μm.
[0049] The blending amount of (D) melamine cyanurate is preferably 1 to 20 parts by mass, more preferably 5 to 20 parts by mass, based on 100 parts by mass of the (A) alkali-soluble resin. When the blending amount is within the above range, a good balance between high sensitivity and physical properties such as heat resistance, electroless gold plating resistance, and insulation reliability is achieved.
[0050] [(E) Photopolymerization initiator] As the (E) photopolymerization initiator, any photopolymerization initiator known as a photopolymerization initiator or photoradical generator can be used. For example, bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dichlorobenzoyl)phenyl ... Sphing oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide and other bisacylphosphine oxides; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide monoacylphosphine oxides such as 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-hydroxy-2- Hydroxyacetophenones such as methyl-1-phenylpropan-1-one; benzoins such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ethers; benzophenones such as benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[ acetophenones such as 4-(4-morpholinyl)phenyl]-1-butanone and N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2 Anthraquinones such as tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyl ... oxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) and other oxime esters; bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyr-1-yl)ethyl)phenyl]titanium and other titanocenes;Examples of the photopolymerization initiator include phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, and tetramethylthiuram disulfide. Of the (E) photopolymerization initiators, it is preferable to contain an acylphosphine-based photopolymerization initiator such as bisacylphosphine oxides or monoacylphosphine oxides in order to increase the exposure sensitivity. The (E) photopolymerization initiator may be used alone or in combination of two or more.
[0051] The amount of the photopolymerization initiator (E) is preferably 0.5 to 20 parts by mass relative to 100 parts by mass of the alkali-soluble resin (A). When the amount is 0.5 part by mass or more, the surface curing property is good, and when the amount is 20 parts by mass or less, halation is unlikely to occur and good resolution can be obtained.
[0052] (Inorganic filler) The curable resin composition of the present invention may contain an inorganic filler. The inorganic filler is not particularly limited, and may be any known and commonly used inorganic filler, such as crystalline silica, fused silica, spherical silica, Neuburg silica, aluminum hydroxide, glass powder, talc, clay, magnesium carbonate, calcium carbonate, natural mica, synthetic mica, aluminum hydroxide, barium sulfate, barium titanate, iron oxide, non-fibrous glass, hydrotalcite, mineral wool, aluminum silicate, calcium silicate, zinc oxide, etc. Among them, silica is preferred because it has a small specific gravity, can be highly filled in the cured product, and can easily increase the strength.
[0053] The average particle size of the inorganic filler is preferably 5 μm or less, more preferably 1 μm or less, from the viewpoint of improving the resolution while maintaining the exposure sensitivity. On the other hand, from the viewpoint of suppressing halation and aggregation during exposure, it is preferably 0.02 μm or more. Here, in this specification, the average particle size of the inorganic filler is the average particle size (D50) including not only the particle size of the primary particles but also the particle size of the secondary particles (aggregates), and is the value of D50 measured by the laser diffraction method. An example of a measuring device using the laser diffraction method is Microtrac MT3300EXII manufactured by Microtrac-Bell.
[0054] The inorganic filler is preferably a surface-treated inorganic filler (also referred to as a "surface-treated inorganic filler"), and more preferably, the surface of the inorganic filler is subjected to a surface treatment capable of introducing a curable reactive group. Here, the curable reactive group is not particularly limited as long as it is a group that undergoes a curing reaction with a curable compound such as (A) an alkali-soluble resin or (C) an epoxy resin, and may be a photocurable reactive group or a thermosetting reactive group. Examples of the photocurable reactive group include a methacryl group, an acrylic group, a vinyl group, and a styryl group, and examples of the thermosetting reactive group include an epoxy group, an amino group, a hydroxyl group, a carboxyl group, an isocyanate group, an imino group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. The method of introducing a curable reactive group into the surface of the inorganic filler is not particularly limited, and may be introduced using a known, commonly used method, and the surface of the inorganic filler may be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group. As the coupling agent, a silane coupling agent, a titanium coupling agent, a zirconium coupling agent, an aluminum coupling agent, etc. may be used. In addition, examples of surface-treated inorganic fillers that do not have a curable reactive group include inorganic fillers that have been subjected to silica-alumina surface treatment, titanate-based coupling agent treatment, aluminate-based coupling agent treatment, and organic treatment.
[0055] The method for adjusting the average particle size of the inorganic filler is not particularly limited, but for example, it is preferable to pre-disperse the inorganic filler using a bead mill or a jet mill. In addition, as the inorganic filler, a commercially available product having an average particle size within the above range may be used as it is.
[0056] The inorganic filler is preferably blended in a slurry state, which facilitates high dispersion and prevents aggregation, making it easy to handle the inorganic filler having an average particle size in the above-mentioned specific range.
[0057] The inorganic filler may be used alone or in combination of two or more. The amount of the inorganic filler is preferably 20 to 50 mass %, more preferably 25 to 40 mass %, based on the solid content of the curable resin composition.
[0058] (Coloring agent) The curable resin composition of the present invention may contain a colorant. As the colorant, a known colorant such as red, blue, green, yellow, black, or white may be used, and any of a pigment, dye, and coloring matter may be used. However, from the viewpoint of reducing the environmental load and the effect on the human body, it is preferable that the colorant does not contain a halogen.
[0059] The colorant may be used alone or in combination of two or more. The amount of the colorant added is not particularly limited, but is preferably 10 parts by mass or less, and more preferably 0.01 to 7 parts by mass, per 100 parts by mass of the (A) alkali-soluble resin.
[0060] (Organic solvent) The curable resin composition of the present invention may contain an organic solvent for the purpose of adjusting the viscosity when preparing the composition or when applying it to a substrate or a carrier film. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. These organic solvents may be used alone or in combination of two or more kinds.
[0061] (Other optional ingredients) Furthermore, the curable resin composition of the present invention may contain other additives that are well known and commonly used in the field of electronic materials, such as thermal polymerization inhibitors, ultraviolet absorbers, silane coupling agents, plasticizers, flame retardants, antistatic agents, antiaging agents, antioxidants, antibacterial and antifungal agents, defoamers, leveling agents, thickeners, adhesion-imparting agents, thixotropy-imparting agents, photoinitiator assistants, sensitizers, photobase generators, curing agents, elastomers, thermoplastic resins, organic fillers, release agents, surface treatment agents, dispersants, dispersion assistants, surface modifiers, stabilizers, and phosphors.
[0062] The curable resin composition of the present invention may be used in the form of a dry film or in the form of a liquid depending on the application. When used in the form of a liquid, it may be a one-component type or a two-component or more type.
[0063] Next, the dry film of the present invention has a resin layer obtained by applying and drying the curable resin composition of the present invention on a carrier film. When forming a dry film, first, the curable resin composition of the present invention is diluted with the organic solvent to adjust the viscosity to an appropriate level, and then coated on a carrier film to a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like. Thereafter, the applied composition is usually dried at a temperature of 40 to 130°C for 1 to 30 minutes to form a resin layer. There is no particular restriction on the coating thickness, but it is generally appropriately selected within the range of 3 to 150 μm, preferably 5 to 60 μm, in terms of the film thickness after drying.
[0064] As the carrier film, a plastic film is used, and for example, a polyester film such as polyethylene terephthalate (PET), a polyimide film, a polyamideimide film, a polypropylene film, a polystyrene film, etc. can be used. There is no particular restriction on the thickness of the carrier film, but it is generally appropriately selected in the range of 10 to 150 μm. It is more preferably in the range of 15 to 130 μm.
[0065] After forming a resin layer made of the curable resin composition of the present invention on a carrier film, it is preferable to further laminate a peelable cover film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer. For example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. can be used as the peelable cover film. The cover film may be any film that has a smaller adhesive force than that between the resin layer and the carrier film when the cover film is peeled off.
[0066] In the present invention, the curable resin composition of the present invention may be applied to the cover film and dried to form a resin layer, and a carrier film may be laminated on the surface of the resin layer. That is, in the present invention, either a carrier film or a cover film may be used as the film to which the curable resin composition of the present invention is applied when producing a dry film.
[0067] The electronic component of the present invention has a cured product obtained from the curable resin composition of the present invention or the resin layer of the dry film, and is, for example, a printed wiring board or an inductor. As a method for producing a printed wiring board, for example, the curable resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100 ° C. to form a tack-free resin layer. In addition, in the case of a dry film, the resin layer is attached to the substrate by a laminator or the like so that the resin layer contacts the substrate, and then the carrier film is peeled off to form a resin layer on the substrate.
[0068] The substrates include printed wiring boards and flexible printed wiring boards on which circuits have been formed in advance using copper or the like, as well as materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven cloth epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, copper-clad laminates for high-frequency circuits using fluororesin, polyethylene, polyphenylene ether, polyphenylene oxide, cyanate, etc., and include copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, PET films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc. The circuits may be pretreated, for example, with GliCAP manufactured by Shikoku Kasei Co., Ltd., New Organic AP (Adhesion promoter) manufactured by MEC Co., Ltd., Nova Bond manufactured by Atotech Japan Co., Ltd., etc. to improve adhesion with hardened coatings such as solder resist, or with a rust inhibitor.
[0069] The volatilization drying carried out after application of the curable resin composition of the present invention can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which hot air in a dryer equipped with a heat source of an air heating method using steam is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).
[0070] After forming a resin layer on a printed wiring board, the resin layer is selectively exposed to active energy rays through a photomask with a predetermined pattern formed thereon, and the unexposed areas are developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3 mass% aqueous sodium carbonate solution) to form a pattern of a cured product. The cured product is then irradiated with active energy rays and then heat-cured (e.g., 100 to 220°C), or is irradiated with active energy rays after heat-curing, or is heat-cured only to form a final finish curing (main curing) to form a cured film with excellent properties such as adhesion and hardness.
[0071] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating active energy rays in the range of 350 to 450 nm. Furthermore, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:
[0072] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.
[0073] The curable resin composition of the present invention is preferably used to form a cured film on a printed wiring board, more preferably used to form a permanent coating, and even more preferably used to form a solder resist. For example, as a solder resist, it can also be preferably used to form a solder resist for IC packages. The curable resin composition of the present invention may also be used for applications such as an interlayer insulating layer formed on a multilayer printed wiring board or a coverlay formed on a flexible printed wiring board. EXAMPLES
[0074] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.
[0075] [Synthesis of alkali-soluble resin] (Synthesis of Carboxyl Group-Containing Resin A-1) To 600 g of diethylene glycol monoethyl ether acetate, 1,070 g (number of glycidyl groups (total number of aromatic rings): 5.0 mol) of orthocresol novolac epoxy resin (EPICLON N-695 manufactured by DIC Corporation, softening point 95°C, epoxy equivalent 214, average number of functional groups 7.6), 360 g (5.0 mol) of acrylic acid, and 1.5 g of hydroquinone were added, and the mixture was heated to 100°C with stirring to dissolve uniformly. Next, 4.3g of triphenylphosphine was added, heated to 110°C and reacted for 2 hours, then heated to 120°C and reacted for another 12 hours. 415g of aromatic hydrocarbon (Solvesso 150) and 456.0g (3.0 moles) of tetrahydrophthalic anhydride were added to the resulting reaction solution, reacted at 110°C for 4 hours, and cooled to obtain a solution of photosensitive carboxyl group-containing resin A-1. The solid content of the resin solution thus obtained was 65%, and the acid value of the solid content was 89mgKOH / g. Hereinafter, this solution of carboxyl group-containing resin is referred to as resin solution A-1.
[0076] (Synthesis of Carboxyl Group-Containing Resin A-2) Into an autoclave equipped with a thermometer, a nitrogen introduction device / alkylene oxide introduction device, and a stirrer, 119.4 parts of a novolac cresol resin (Showa Denko K.K.'s Shownol CRG951, OH equivalent: 119.4), 1.19 parts of potassium hydroxide, and 119.4 parts of toluene were introduced, and the system was replaced with nitrogen while stirring, and heated to increase the temperature. Next, 63.8 parts of propylene oxide were gradually added dropwise, and the temperature was increased to 125-132°C and 0-4.8 kg / cm. 2 The mixture was reacted at 40° C. for 16 hours. After that, it was cooled to room temperature, and 1.56 parts of 89% phosphoric acid was added to the reaction solution to neutralize the potassium hydroxide, to obtain a propylene oxide reaction solution of novolac cresol resin with a non-volatile content of 62.1% and a hydroxyl value of 182.2 mgKOH / g (307.9 g / eq.). This was an average of 1.08 moles of propylene oxide added per equivalent of phenolic hydroxyl group. 293.0 parts of the propylene oxide reaction solution of the obtained novolac cresol resin, 43.2 parts of acrylic acid, 11.53 parts of methanesulfonic acid, 0.18 parts of methylhydroquinone, and 252.9 parts of toluene were introduced into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and the mixture was reacted at 110°C for 12 hours while blowing air at a rate of 10 ml / min and stirring. The water produced by the reaction was distilled as an azeotrope with toluene, and 12.6 parts of water were distilled. After that, the mixture was cooled to room temperature, and the obtained reaction solution was neutralized with 35.35 parts of 15% aqueous sodium hydroxide solution, and then washed with water. After that, the toluene was distilled off while replacing it with 118.1 parts of diethylene glycol monoethyl ether acetate in an evaporator, and a novolac acrylate resin solution was obtained. Next, 332.5 parts of the obtained novolac-type acrylate resin solution and 1.22 parts of triphenylphosphine were introduced into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and 60.8 parts of tetrahydrophthalic anhydride were gradually added while blowing air at a rate of 10 ml / min and stirring, and the mixture was reacted at 95 to 101°C for 6 hours, cooled, and then removed. In this way, a solution of photosensitive carboxyl-containing resin A-2 with a solid content of 65% and an acid value of the solid content of 87.7 mgKOH / g was obtained. Hereinafter, this solution of carboxyl-containing photosensitive resin is referred to as resin solution A-2.
[0077] [Preparation of inorganic filler] (Preparation of inorganic filler slurry 1) A silica solvent dispersion was obtained by uniformly dispersing 50 g of spherical silica particles (SO-C2 manufactured by Admatechs, average particle size: 500 nm), 48 g of PMA as a solvent, and 2 g of a silane coupling agent having a methacryl group (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.).
[0078] (Preparation of inorganic filler slurry 2) A barium sulfate solvent dispersion was obtained by uniformly dispersing 50 g of barium sulfate (Sakai Chemical Industry Co., Ltd., Precipitation Barium 100), 48 g of PMA as a solvent, and 2 g of a dispersant (BYK-111).
[0079] [Examples 1 to 7, Comparative Examples 1 to 3] The various components in Table 1 below were mixed in the ratios (parts by mass) shown in the table, premixed with a stirrer, and then kneaded with a bead mill to prepare curable resin compositions. The amount of each component shown in the table is the part by mass of the solid content excluding the solvent. The stirring conditions for the stirrer were a rotation speed of 800 rpm, a stirring time of 10 min, and a stirrer blade of 12 cm. A conical type K-8 (manufactured by Buehler) was used as the bead mill, and the kneading was performed under the following conditions: zirconia beads, a rotation speed of 1000 rpm, a discharge volume of 20%, a bead particle size of 0.65 mm, and a filling rate of 88%.
[0080] <Preparation of dry film> The curable resin compositions prepared above were each applied onto a 38 μm polyester film using an applicator, and dried in a hot air circulation drying oven at 80° C. for 30 minutes to prepare a dry film having a resin layer with a thickness of 20 μm.
[0081] <Drying control width> The dry film was laminated onto a copper-clad laminate of 1.6 mm thick FR-4 and 18 μm thick copper foil that had been buffed (two rows of Scotch brite SF (equivalent to #600) and UEF (equivalent to #1000)), using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) in a first chamber at 100°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 30 seconds, and then pressed under conditions of a press pressure of 0.5 MPa and a press time of 30 seconds. The polyester film was then peeled off, and the substrate was dried in a hot air circulating drying oven at 90°C for 30 minutes, and then developed with a 1% by mass aqueous solution of sodium carbonate at 30°C for 90 seconds at a spray pressure of 0.2 MPa, followed by rinsing and drying for 30 seconds at a spray pressure of 0.1 MPa. The substrate was visually observed and evaluated as follows. ◯: No residue of the composition remains and the composition has been completely removed by development. △: The copper foil is exposed, but there is some residue. ×: Clear residual development was observed.
[0082] <Storage stability> The curable resin composition prepared above was stored in the dark at 50 °C, and the thickening rate over time was measured with a cone plate viscometer. When the thickening rate exceeded 200%, it was judged to be unusable, and the time until it became unusable was measured. The evaluation criteria are as follows. 〇 = The thickening rate is less than 200% even after 200 hours. × = The thickening rate is 200% or more after 200 hours.
[0083] <Tg by DMA measurement method> On the shiny surface side (copper foil) of GTS-MP foil (manufactured by Furukawa Circuit Foil Co., Ltd.), each dry film prepared above was laminated in a first chamber at 100 °C under a vacuum pressure of 3 hPa and a vacuum time of 30 seconds using a vacuum laminator (CVP-300: manufactured by Nichco Materials Co., Ltd.) so that the resin layer was in contact with the copper foil, and then pressed under conditions of a press pressure of 0.5 MPa and a press time of 30 seconds. Next, the polyester film was peeled off, and exposure was performed in a strip pattern of 50 mm × 3 mm using a DI exposure apparatus (light source: high-pressure mercury lamp) with an integrated light amount that becomes 8 or 9 steps on a step tablet (41 steps of Stouffer). Then, it was developed for 90 seconds with a 1 mass% aqueous sodium carbonate solution at 30 °C under a spray pressure of 0.2 MPa, washed with water for 30 seconds at a spray pressure of 0.1 MPa, and dried. Next, after ultraviolet irradiation under conditions of an integrated exposure amount of 2000 mJ / cm 2 it was cured by heating at 150 °C for 60 minutes in a hot air circulation drying furnace. Then, the sample was peeled off from the copper foil and subjected to DMS6100 (manufactured by Hitachi High-Technologies Corporation), and the Tg was measured with a frequency of 1 Hz. The evaluation criteria are as follows. ◎ = 180 °C or higher 〇 = Less than 180 °C and 170 °C or higher × = Less than 170 °C <Sensitivity> A copper-clad laminate of 1.6 mm thick FR-4 and 18 μm thick copper foil was electrolytically plated with 17 μm thick copper, and etched to the equivalent of 1.0 μm using MEC's CZ-8101B processing. The dry film was laminated on the laminate using a vacuum laminator (CVP-300: Nikko Materials Co., Ltd.) in the first chamber at 100°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 30 seconds, and then pressed under conditions of a pressure of 0.5 MPa and a press time of 30 seconds. Next, the polyester film was peeled off and the exposure was performed at 300 mJ / cm using a step tablet (Stofer 41 steps) in a DI exposure device (light source: high-pressure mercury lamp). 2 Thereafter, the substrate was developed with a 1% by mass aqueous solution of sodium carbonate at 30° C. for 90 seconds under conditions of a spray pressure of 0.2 MPa, washed with water at a spray pressure of 0.1 MPa for 30 seconds, and then dried to obtain an evaluation substrate. The evaluation criteria are as follows: ○: Sensitivity is 9 levels or higher. △: Sensitivity is 8 levels. ×: Sensitivity is 7 steps or less.
[0084] <Electroless gold plating resistance> A test substrate was prepared in the same manner as in the Tg evaluation substrate, except that the test substrate was the same as that used for the sensitivity evaluation, and a houndstooth check pattern of 5 mm square cutouts was used as the exposure pattern. The substrate was degreased by immersing in an acidic degreasing solution (20 Vol% aqueous solution of Metex L-5B, manufactured by Nippon MacDermid Co., Ltd.) at 30°C for 3 minutes, and then immersed in running water for 3 minutes and washed with water. Next, the test substrate was immersed in a 14.3 wt% aqueous solution of ammonium persulfate at room temperature for 3 minutes to perform soft etching, and then immersed in running water for 3 minutes and washed with water. The test substrate was immersed in a 10 Vol% aqueous solution of sulfuric acid at room temperature for 1 minute, and then immersed in running water for 30 seconds to 1 minute and washed with water. Next, the test substrate was immersed in a catalyst solution (10 Vol% aqueous solution of Metal Plate Activator 350, manufactured by Meltex Co., Ltd.) at 30°C for 7 minutes to apply a catalyst, and then immersed in running water for 3 minutes and washed with water. The test substrate to which the catalyst was applied was immersed in a nickel plating solution (20 Vol% aqueous solution of Melplate Ni-865M, manufactured by Meltex, pH 4.6) at 85°C for 20 minutes to perform electroless nickel plating. The test substrate was immersed in a 10 vol% aqueous sulfuric acid solution at room temperature for 1 minute, and then immersed in running water for 30 seconds to 1 minute to wash with water. Next, the test substrate was immersed in a gold plating solution (aqueous solution of Aurolectroless UP 15 Vol% and potassium gold cyanide 3 Vol%, manufactured by Meltex, pH 6) at 95°C for 10 minutes to perform electroless gold plating, then immersed in running water for 3 minutes to wash with water, and immersed in warm water at 60°C for 3 minutes to wash with hot water. After thorough rinsing, the water was drained well and dried to obtain an electroless gold-plated test substrate. The test substrate was peeled using a cellophane adhesive tape, and the peeling state was evaluated visually. The evaluation criteria were as follows: ○: No peeling △: Partial peeling is observed. × = Obvious peeling.
[0085] <Outgassing> The test substrate was the same as that used for the evaluation of sensitivity, and a test substrate was prepared in the same manner as in the preparation of the Tg evaluation substrate, except that the entire surface was exposed to light. Approximately 1 mg of the cured coating powder was sampled from the substrate and heated under the following thermal extraction conditions. The volatilized components were cold trapped, then rapidly heated and introduced into a GC / MS for evaluation. The following evaluation equipment was used, and the extraction conditions were as follows: (1) Evaluation device Thermal desorption equipment: Gestell TDU GC: Agilent Technologies 6890N MSD: Agilent Technologies 5973N (2) Extraction conditions Thermal extraction conditions: 220℃, 10 minutes The evaluation criteria are as follows: ○: Less than 0.04% ×: 0.04% or more
[0086] <Insulation reliability> The test substrate was prepared in the same manner as the Tg evaluation substrate, except that a comb-shaped pattern with L / S=20 / 20μm was formed and the entire surface was exposed to light. HAST was then performed under the conditions of 130℃, 85% RH, applied voltage of 5V, and measurement in a chamber. The evaluation criteria are as follows. 〇: Insulation resistance after 300 hours is 1×10 6 Ω or more ×: Insulation resistance after 300 hours is 1×10 6 Less than Ω
[0087] [Table 1]
[0088] *1: Solution of the carboxyl group-containing resin A-1 synthesized above *2: Solution of the carboxyl group-containing resin A-2 synthesized above *3: Mitsubishi Chemical YX-4000 (biphenol type epoxy resin, epoxy equivalent: 180-192g / eq.) *4: NC-3000 manufactured by Nippon Kayaku Co., Ltd. (biphenol novolac type epoxy resin, epoxy equivalent: 265-285g / eq.) *5: Nissan Chemical's TEPIC (tris(2,3-epoxypropyl)isocyanurate, epoxy equivalent: 100g / eq.) *6: IGM Resins Omnirad TPO H (2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide) *7: Inorganic filler slurry 1 prepared above *8: Inorganic filler slurry 2 prepared above *9: KAYARAD DPHA (dipentaerythritol hexaacrylate) manufactured by Nippon Kayaku Co., Ltd. *10: TMPTA (trimethylolpropane triacrylate) manufactured by Nippon Kayaku Co., Ltd. *11: Copper phthalocyanine blue Pigment blue 15 *12:CI Pigment Yellow 147 *13: Nissan Chemical Melamine Cyanurate, MC-6000
[0089] From the results shown in the above table, it can be seen that the curable resin compositions of Examples 1 to 7 of the present invention are excellent in storage stability and exposure sensitivity, and can form cured products having excellent physical properties such as heat resistance and insulation reliability.
Claims
1. A curable resin composition containing (A) an alkali-soluble resin, (B) a compound having an ethylenically unsaturated group, (C) an epoxy resin having an epoxy equivalent of 130 g / eq. or more, (D) melamine cyanurate, (E) a photopolymerization initiator, and a surface-treated inorganic filler, and not containing titanium oxide, The curable resin composition is characterized in that the blending amount of the surface-treated inorganic filler is 20 to 50 mass % based on the solid content of the curable resin composition.
2. The curable resin composition according to claim 1, characterized in that the blending amount of the melamine cyanurate (D) is 1 to 20 parts by mass based on 100 parts by mass of the alkali-soluble resin (A).
3. 3. The curable resin composition according to claim 1, wherein the photopolymerization initiator (E) contains an acylphosphine-based photopolymerization initiator.
4. A dry film comprising a resin layer obtained by applying the curable resin composition according to any one of claims 1 to 3 onto a film and drying the applied resin layer.
5. A cured product obtained by curing the curable resin composition according to any one of claims 1 to 3 or the resin layer of the dry film according to claim 4.
6. An electronic part comprising the cured product according to claim 5.
Citation Information
Patent Citations
Resist ink composition
JP1986243869A
Alkali-soluble resist ink composition having high emissivity, light reflectance, and heat resistance
JP2016024284A
Photosensitive resin composition and cured product of the same, and production method of photosensitive resin
JP2016139153A