Anode and method for producing same

A silicon oxide-based negative electrode with optimized binding energies and crystallite sizes, coated with carbon, enhances lithium-ion battery performance by preventing structural breakdown and improving capacity and stability.

JP7558904B2Active Publication Date: 2024-10-01SHIN ETSU CHEMICAL CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2021122791
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-27
Publication Date
2024-10-01
Estimated Expiration
2041-07-27

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries using silicon as a negative electrode material face challenges with initial charge/discharge characteristics and cycle stability due to structural breakdown and disproportionation during repeated charging and discharging, leading to poor battery performance.

Method used

A negative electrode comprising silicon oxide particles coated with a carbon layer and optimized through Li insertion, with specific binding energy ratios and crystallite sizes to enhance stability and prevent decomposition, is developed.

Benefits of technology

The solution improves battery capacity, initial efficiency, and cycle characteristics, achieving performance comparable to carbon-based active materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558904000002
    Figure 0007558904000002
  • Figure 0007558904000003
    Figure 0007558904000003
  • Figure 0007558904000004
    Figure 0007558904000004
Patent Text Reader

Abstract

To provide a negative electrode capable of increasing battery capacity with the improvement of initial efficiency and achieving sufficient battery cycle characteristics.SOLUTION: The negative electrode contains negative electrode active material particles and has been charged and discharged at least once. The negative electrode active material particles contain silicon oxide particles coated with a carbon layer. The silicon oxide particles have Li2SiO3. In O1s binding energy acquired by an XPS analysis for the inside of the particles, the intensity of a peak A acquired around 529.5 eV and the intensity of a peak B acquired around 532.5 eV satisfy the relationship (intensity of peak A)≤(intensity of peak B).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode and a method for producing the same. [Background technology]

[0002] In recent years, small electronic devices such as mobile terminals have become widespread, and there is a strong demand for further miniaturization, weight reduction, and longer life. In response to such market demands, development of secondary batteries that are small, lightweight, and capable of obtaining high energy density has been promoted. The application of these secondary batteries is being considered not only for small electronic devices, but also for large electronic devices such as automobiles and power storage systems such as homes.

[0003] Among these, lithium-ion secondary batteries are attracting great attention because they can be easily made small and have a high capacity, and because they offer a higher energy density than lead-acid batteries and nickel-cadmium batteries.

[0004] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.

[0005] While carbon-based active materials are widely used as negative electrode active materials, recent market demands have called for further improvements in battery capacity. To improve battery capacity, the use of silicon as a negative electrode active material is being considered. This is because the theoretical capacity of silicon (4199mAh / g) is more than 10 times greater than that of graphite (372mAh / g), and a significant improvement in battery capacity can be expected. In the development of silicon materials as negative electrode active materials, not only silicon itself but also alloys and compounds such as oxides are being considered. In addition, the active material shape is being considered, ranging from the standard coating type for carbon-based active materials to an integrated type that is directly deposited on the current collector.

[0006] However, when silicon is used as the main raw material for the negative electrode active material, the negative electrode active material expands and contracts during charging and discharging, making it prone to cracking, mainly near the surface layer of the negative electrode active material. In addition, ionic substances are generated inside the active material, making the negative electrode active material prone to cracking. When the surface layer of the negative electrode active material cracks, a new surface is created, increasing the reaction area of ​​the active material. At this time, a decomposition reaction of the electrolyte occurs on the new surface, and a coating, which is a decomposition product of the electrolyte, is formed on the new surface, consuming the electrolyte. This makes the cycle characteristics more likely to deteriorate.

[0007] To date, various studies have been conducted on negative electrode materials and electrode configurations for lithium-ion secondary batteries that use silicon materials as the main material in order to improve the initial battery efficiency and cycle characteristics.

[0008] Specifically, in order to obtain good cycle characteristics and high safety, silicon and amorphous silicon dioxide are simultaneously deposited using a gas phase method (see, for example, Patent Document 1). Also, in order to obtain high battery capacity and safety, a carbon material (electron conductive material) is provided on the surface layer of silicon oxide particles (see, for example, Patent Document 2). Furthermore, in order to improve cycle characteristics and obtain high input / output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer with a high oxygen ratio is formed near the current collector (see, for example, Patent Document 3). Also, in order to improve cycle characteristics, oxygen is contained in the silicon active material, and the active material is formed so that the average oxygen content is 40 at% or less and the oxygen content is high in the area close to the current collector (see, for example, Patent Document 4).

[0009] In addition, in order to improve the initial charge / discharge efficiency, the Si phase, SiO2, and M y Nanocomposites containing metal oxides are used (see, for example, Patent Document 5). In addition, in order to improve cycle characteristics, SiO x(0.8 ≤ x ≤ 1.5, particle size range = 1 μm to 50 μm) is mixed with a carbon material and fired at high temperature (see, for example, Patent Document 6). Further, in order to improve the cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1 to 1.2, and the active material is controlled within a range where the difference between the maximum value and the minimum value of the molar ratio near the interface between the active material and the current collector is 0.4 or less (see, for example, Patent Document 7). Further, in order to improve the battery load characteristics, a metal oxide containing lithium is used (see, for example, Patent Document 8). Further, in order to improve the cycle characteristics, a hydrophobic layer such as a silane compound is formed on the surface layer of the silicon material (see, for example, Patent Document 9). Further, in order to improve the cycle characteristics, silicon oxide is used, and conductivity is imparted by forming a graphite film on its surface layer (see, for example, Patent Document 10). In Patent Document 10, regarding the shift value obtained from the Raman spectrum of the graphite film, a broad peak appears at 1330 cm -1 and 1580 cm -1 , and the intensity ratio I 1330 / I 1580 is such that 1.5 < I 1330 / I 1580 < 3. Further, in order to improve the high battery capacity and cycle characteristics, particles having a silicon microcrystalline phase dispersed in silicon dioxide are used (see, for example, Patent Document 11). Further, in order to improve the overcharge and overdischarge characteristics, a silicon oxide in which the atomic ratio of silicon to oxygen is controlled to 1:y (0 < y < 2) is used (see, for example, Patent Document 12).

[0010] In addition, Hitachi Maxell started shipping a rectangular secondary battery for smartphones that adopted a nanosilicon composite in June 2010 for a lithium-ion secondary battery using silicon oxide (see, for example, Non-Patent Document 1). The silicon oxide proposed by Hohl is a composite material of Si 0+ ~Si 4+ and has various oxidation states (Non-Patent Document 2). Further, Kapaklis has proposed a disproportionation structure in which silicon oxide is divided into Si and SiO2 by applying a heat load (Non-Patent Document 3).

[0011] Miyachi et al. have focused on Si and SiO2, which contribute to charging and discharging, among silicon oxides having a disproportionated structure (Non-Patent Document 4), and Yamada et al. have proposed the following reaction formula between silicon oxide and Li (Non-Patent Document 5): 2SiO(Si+SiO2) + 6.85Li+ + 6.85e - → 1.4Li 3.75 Si + 0.4Li4SiO4 + 0.2SiO2 In the reaction formula, Si and SiO2 that make up silicon oxide react with Li, resulting in separation into Li silicide, Li silicate, and some unreacted SiO2.

[0012] The Li silicate formed here is irreversible, and once formed, it is a stable substance that does not release Li. The capacity per mass calculated from this reaction formula is close to the experimental value, and is recognized as the reaction mechanism of silicon oxide. Kim et al. have defined the irreversible component associated with the charge and discharge of silicon oxide, Li silicate, as Li4SiO4, and 7 Li-MAS-NMR and 29 The irreversible capacity was identified using Si-MAS-NMR (Non-Patent Document 6). This irreversible capacity is the weakest point of silicon oxide, and improvement is required. Therefore, Kim et al. have used the Li pre-doping method to form Li silicate in advance, significantly improving the initial efficiency as a battery and creating a negative electrode that can withstand practical use (Non-Patent Document 7).

[0013] Furthermore, instead of doping the electrode with Li, they proposed a method of treating the powder, which improved the irreversible capacity (Patent Document 13). [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2001-185127 A [Patent Document 2] JP 2002-042806 A [Patent Document 3] Japanese Patent Application Laid-Open No. 2006-164954 [Patent Document 4] Japanese Patent Application Laid-Open No. 2006-114454 [Patent Document 5] Japanese Patent Application Laid-Open No. 2009-070825 [Patent Document 6] Japanese Patent Application Laid-Open No. 2008-282819 [Patent Document 7] Japanese Patent Application Laid-Open No. 2008-251369 [Patent Document 8] Japanese Patent Application Laid-Open No. 2008-177346 [Patent Document 9] Japanese Patent Application Laid-Open No. 2007-234255 [Patent Document 10] Japanese Patent Application Laid-Open No. 2009-212074 [Patent Document 11] Japanese Patent Application Laid-Open No. 2009-205950 [Patent Document 12] Japanese Patent Application Laid-Open No. 06-325765 [Patent Document 13] Japanese Patent Application Laid-Open No. 2015-156355 [Non-Patent Document]

[0015] [Non-Patent Document 1] The official journal of the Battery Industry Association of Japan, "Denchi", May 1, 2010 issue, page 10 [Non-Patent Document 2] A. Hohl, T. Wieder, P. A. van Aken, T. E. Weirich, G. Denninger, M. Vidal, S. Oswald, C. Deneke, J. Mayer, and H. Fuess : J. Non-Cryst. Solids, 320, (2003 ), 255. [Non-Patent Document 3] V. Kapaklis, J. Non-Crystalline Solids, 354 (2008) 612 [Non-Patent Document 4] Mariko Miyachi, Hironori Yamamoto, and Hidemasa Kawai, J. Electrochem. Soc. 2007 volume 154, issue 4, A376-A380 [Non-Patent Document 5] M. Yamada, A. Inaba, A. Ueda, K. Matsumoto, T. Iwasaki, T. Ohzuku, J. Electrochem. Soc., 159, A1630 (2012) [Non-Patent Document 6] Taeahn Kim, Sangjin Park, and Seung M. Oh, J. Electrochem. Soc. volume 154,(2007), A1112-A1117. [Non-Patent Document 7] Hye Jin Kim, Sunghun Choi, Seung Jong Lee, Myung Won Seo, Jae Goo Lee, Erhan Deniz, Yong Ju Lee, Eun Kyung Kim, and Jang Wook Choi,. Nano Lett. 2016, 16, 282-288. Summary of the Invention [Problem to be solved by the invention]

[0016] As mentioned above, in recent years, small electronic devices such as mobile terminals have been improved in performance and functionality, and lithium-ion secondary batteries, which are the main power sources for these devices, are required to have increased battery capacity. As one method to solve this problem, the development of lithium-ion secondary batteries consisting of a negative electrode mainly made of silicon material is desired. In addition, lithium-ion secondary batteries using silicon materials are desired to have initial charge / discharge characteristics and cycle characteristics that are similar to those of lithium-ion secondary batteries using carbon-based active materials. Therefore, by using silicon oxide modified by insertion and partial desorption of Li as the negative electrode active material, cycle characteristics and initial charge / discharge characteristics have been improved. However, since lithium inserted inside the particles is likely to be stable in a state of low binding energy, the structure is broken and disproportionation progresses during repeated charging and discharging, resulting in insufficient battery characteristics.

[0017] The present invention has been made in consideration of the above problems, and aims to provide a negative electrode that can increase battery capacity by improving initial efficiency (also referred to as initial efficiency) and achieve sufficient battery cycle characteristics, and a method for manufacturing the same. [Means for solving the problem]

[0018] In order to achieve the above object, the present invention provides a negative electrode that includes negative electrode active material particles and has been charged and discharged at least once, wherein the negative electrode active material particles contain silicon oxide particles coated with a carbon layer, the silicon oxide particles have Li2SiO3, and in O1s binding energies obtained by XPS analysis of the inside of the particles, the intensity of peak A obtained in the vicinity of 529.5 eV and the intensity of peak B obtained in the vicinity of 532.5 eV have a relationship of (intensity of peak A)≦(intensity of peak B).

[0019] The negative electrode active material (hereinafter also referred to as silicon-based negative electrode active material) contained in the negative electrode of the present invention contains negative electrode active material particles (hereinafter also referred to as silicon-based negative electrode active material particles) containing silicon oxide particles, and therefore the battery capacity can be improved. In addition, the silicon oxide particles contain Li2SiO3, and thus the initial efficiency is improved. The negative electrode active material contained in the negative electrode of the present invention can be found to have an optimized phase structure by performing a single charge and discharge. In particular, it is important that the O1s binding energy inside the particle obtained by XPS analysis, peak A obtained near 529.5 eV and peak B obtained near 532.5 eV, have a relationship of (intensity of peak A) ≦ (intensity of peak B). In the case where a lower energy state is formed in the O1s binding energy of XPS analysis (i.e., the intensity of peak A becomes relatively stronger than that of peak B), further repeated charge and discharge causes decomposition, and as a result, silicification proceeds. The negative electrode of the present invention can prevent such problems, and this can be evaluated by the binding energy obtained as a result of XPS analysis.

[0020] Here, it is preferable that the silicon oxide particles have a phase structure estimated from the peak positions of the Si2p binding energy and O1s binding energy obtained by XPS analysis, which is a three-phase structure or less, and that the O1s binding energy peak near 531.5 eV is smaller than the peak near 532.5 eV.

[0021] A negative electrode containing negative electrode active material particles having such a structure is suppressed from being silicified during charging and discharging when incorporated into a secondary battery, and as a result, the battery characteristics are improved.

[0022] Furthermore, when the ratio of peak A obtained near 529.5 eV to peak B obtained near 532.5 eV in the O1s binding energy obtained by XPS analysis of the silicon oxide particles is taken as (intensity of peak A) / (intensity of peak B), it is preferable that (intensity of peak A) / (intensity of peak B) on the surface of the silicon oxide particles is greater than (intensity of peak A) / (intensity of peak B) inside the silicon oxide particles.

[0023] The surface layer of the silicon oxide particle material needs to smoothly transfer Li, so it is desirable that the O1s peak state near 529.5 eV is strong. However, the bulk interior of the silicon oxide particle needs to have a stable structure, so it is desirable that the peak near 532.5 eV is strong. Therefore, as described above, it is desirable that the (intensity of peak A) / (intensity of peak B) at the surface of the silicon oxide particle is greater than the (intensity of peak A) / (intensity of peak B) inside the silicon oxide particle.

[0024] Furthermore, the negative electrode active material particles have a peak attributable to a Si(111) crystal plane obtained by X-ray diffraction using Cu-Kα radiation before charging and discharging the negative electrode active material particles, the crystallite size corresponding to the crystal plane is 5.0 nm or less, and the ratio G / H of the intensity G of the peak attributable to the Si(111) crystal plane to the intensity H of the peak attributable to the Li2SiO3(111) crystal plane is expressed by the following formula (1): 0.4≦G / H≦1.0 (1) It is preferable that the following is satisfied.

[0025] In this way, by having a peak due to the Si (111) crystal plane and a crystallite size corresponding to the crystal plane of 5.0 nm or less, the silicon oxide particles can be made to contain as little crystalline Si as possible. This suppresses the reaction with the electrolyte and prevents the deterioration of the battery characteristics. As described above, the crystallite size is preferably 5.0 nm or less, and it is preferably substantially amorphous. At this time, Li2SiO3 also shows crystallinity, but the higher the crystallinity of Li2SiO3, the more stable the structure is, but the higher the resistance is. On the other hand, when the crystallinity is low, it is easy to dissolve in the slurry, so there is an optimal range. Therefore, it is preferable to satisfy the above formula (1).

[0026] The negative electrode active material particles preferably have a median diameter of 5.5 μm or more and 15 μm or less.

[0027] If the median diameter of the negative electrode active material particles is 5.5 μm or more, the reaction with the electrolyte is suppressed, and the deterioration of the battery characteristics can be suppressed. On the other hand, if the median diameter of the negative electrode active material particles is 15 μm or less, the expansion of the active material due to charging and discharging can be suppressed, and the electronic contact can be secured.

[0028] Moreover, the true density of the negative electrode active material particles before charging and discharging is preferably greater than 2.3 g / cc and less than 2.4 g / cc.

[0029] The true density of SiO is 2.2 g / cc, but by doping with lithium, the true density of the negative electrode active material particles can be increased to a higher true density of more than 2.3 g / cc, thereby increasing the density of the electrode. In addition, a true density of less than 2.4 g / cc can prevent cracks from easily occurring during expansion and contraction.

[0030] The present invention also provides a method for producing a negative electrode by using the produced negative electrode active material particles, comprising the steps of: preparing silicon oxide particles; coating the silicon oxide particles with a carbon layer; inserting lithium into the silicon oxide particles coated with the carbon layer by an oxidation-reduction method; and heat-treating the silicon oxide particles into which lithium has been inserted to form silicon oxide particles containing Li2SiO3. The method is characterized in that the temperature during the lithium insertion and the temperature during the heat treatment are adjusted so that, after the negative electrode is charged and discharged at least once, the silicon oxide particles contained in the negative electrode have an intensity of Peak A obtained near 529.5 eV and an intensity of Peak B obtained near 532.5 eV, as O1s binding energies obtained by XPS analysis of the inside of the particles, such that the intensity of Peak A is adjusted to be less than or equal to the intensity of Peak B.

[0031] According to such a method for producing a negative electrode, it is possible to produce a negative electrode having negative electrode active material particles having the above-mentioned O1s spectrum in XPS analysis. Effect of the Invention

[0032] The negative electrode of the present invention can provide high initial efficiency, high capacity, and high cycle characteristics when used in a secondary battery. In addition, the method for producing the negative electrode of the present invention can provide good cycle characteristics and can produce a negative electrode that has high capacity and good initial charge / discharge characteristics when used as a negative electrode for a secondary battery. [Brief description of the drawings]

[0033] [Figure 1] 1 is an O1s spectrum obtained by XPS analysis of negative electrode active material particles contained in the negative electrode of Example 1. [Diagram 2] 1 shows a Si2p spectrum obtained by XPS analysis of the negative electrode active material particles contained in the negative electrode of Example 1. [Diagram 3] 1 is an O1s spectrum obtained by XPS analysis of negative electrode active material particles contained in the negative electrode of Comparative Example 1. [Figure 4] 1 shows a Si2p spectrum obtained by XPS analysis of negative electrode active material particles contained in the negative electrode of Comparative Example 1. [Diagram 5] FIG. 2 is a cross-sectional view showing an example of the configuration of a negative electrode of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] Hereinafter, the present invention will be described in detail with reference to the preferred embodiments, but the present invention is not limited thereto.

[0035] As mentioned above, as one method for increasing the battery capacity of a lithium-ion secondary battery, the use of a negative electrode using silicon oxide as a main material as the negative electrode of the lithium-ion secondary battery has been considered. The lithium-ion secondary battery using this silicon oxide is desired to have initial charge / discharge characteristics similar to those of a lithium-ion secondary battery using a carbon-based active material. In addition, in Li-doped SiO, which can improve the initial charge / discharge characteristics, cycle characteristics similar to those of a carbon-based active material are desired. However, a silicon-based negative electrode active material that shows battery characteristics similar to those of a carbon-based active material when used as a negative electrode active material contained in a lithium-ion secondary battery, and a negative electrode containing the same, have not yet been proposed.

[0036] Therefore, the inventors conducted extensive research to obtain a negative electrode that, when used as a negative electrode for a secondary battery, can obtain high cycle characteristics while improving initial charge / discharge characteristics, thereby increasing battery capacity, and thus arrived at the present invention.

[0037] [Negative electrode of the present invention] The negative electrode of the present invention includes negative electrode active material particles and has been charged and discharged at least once, the negative electrode active material particles contain silicon oxide particles coated with a carbon layer, the silicon oxide particles have Li2SiO3, and in the O1s binding energy obtained by XPS analysis of the inside of the particles, the intensity of peak A obtained in the vicinity of 529.5 eV and the intensity of peak B obtained in the vicinity of 532.5 eV have a relationship of (intensity of peak A)≦(intensity of peak B).

[0038] XPS analysis can be performed, for example, by using a scanning X-ray photoelectron spectrometer PHI Quantera II manufactured by ULVAC-PHI, Inc. In this case, the X-ray beam diameter can be set to 100 μm, and a neutralization gun can be used.

[0039] The negative electrode active material (hereinafter also referred to as silicon-based negative electrode active material) contained in the negative electrode of the present invention contains negative electrode active material particles (hereinafter also referred to as silicon-based negative electrode active material particles) containing silicon oxide particles, so that the battery capacity can be improved. In addition, the silicon oxide particles contain Li2SiO3, so that the initial efficiency is improved. The phase structure of the negative electrode active material can be optimized by charging and discharging once. In particular, it is important that the O1s binding energy obtained by XPS analysis, peak A obtained near 529.5 eV and peak B obtained near 532.5 eV, have a relationship of (intensity of peak A)≦(intensity of peak B). In the O1s binding energy of XPS analysis, when a lower energy state is formed (i.e., the intensity of peak A is relatively stronger than that of peak B), further charging and discharging are repeated, and as a result, silicification proceeds. In the present invention, such problems can be solved by having the intensity of peak A obtained near 529.5 eV and the intensity of peak B obtained near 532.5 eV in the O1s binding energy obtained by XPS analysis of the inside of the particle satisfy the relationship (intensity of peak A)≦(intensity of peak B).

[0040] It is preferable that such a negative electrode active material forms low disproportionated SiO with energy on the high potential side from the stage of forming silicon oxide (SiO) particles, and in the carbon coating process, the heat load is preferably 900°C or less to maintain the structure. When bonding with lithium, it is necessary to make Li silicate into a silicate that is not easily destroyed by charging and discharging and that repeats decomposition and generation slowly. These can be evaluated by the bond energy.

[0041] In addition, in the negative electrode of the present invention, the phase structure estimated from the peak positions of the Si2p binding energy and the O1s binding energy obtained by XPS analysis of the silicon oxide particles has a three-phase structure or less, and it is preferable that the O1s binding energy peak near 531.5 eV is smaller than the peak near 532.5 eV.

[0042] The phase structure constituting the bulk of the negative electrode active material particles can be obtained from the XPS spectrum. From the Si2p spectrum, three phases of Si 0 valence, low valence Si, and tetravalent Si can be confirmed, but the O1s spectrum does not have the same structure corresponding to the structure shown by the Si2p spectrum. In particular, if there are many peaks indicating a low valence compound state (near 529.5 eV in the O1s spectrum), as described above, the compound will decompose during charging and discharging, resulting in siliconization, which will deteriorate the battery characteristics. Therefore, a peak near 532.5 eV is required in the O1s state, which is a higher valence state. Since the peak appearing near 531.5 eV indicates a low valence silicon compound, it is preferable that the peak present near 531.5 eV is smaller than the peak near 532.5 eV.

[0043] In the negative electrode of the present invention, when the ratio of peak A obtained near 529.5 eV to peak B obtained near 532.5 eV in the O1s binding energy obtained by XPS analysis of the silicon oxide particles is defined as (intensity of peak A) / (intensity of peak B), it is preferable that (intensity of peak A) / (intensity of peak B) on the surface of the silicon oxide particles is greater than (intensity of peak A) / (intensity of peak B) inside the silicon oxide particles.

[0044] The surface layer of the silicon oxide particle material needs to smoothly exchange Li, so a peak state of O1s near 529.5 eV is desirable. However, the inside of the bulk needs to have a stable structure, so a peak near 532.5 eV is desirable. Therefore, as described above, it is preferable that (intensity of peak A) / (intensity of peak B) at the surface of the silicon oxide particle is greater than (intensity of peak A) / (intensity of peak B) inside the silicon oxide particle.

[0045] In the negative electrode of the present invention, the negative electrode active material particles have a peak due to a Si(111) crystal plane obtained by X-ray diffraction using Cu-Kα radiation before charging and discharging the negative electrode active material particles, the crystallite size corresponding to the crystal plane is 5.0 nm or less, and the ratio G / H of the intensity G of the peak due to the Si(111) crystal plane to the intensity H of the peak due to the Li2SiO3(111) crystal plane is expressed by the following formula (1): 0.4≦G / H≦1.0 (1) It is preferable that the following is satisfied.

[0046] In this way, by having a peak due to the Si (111) crystal plane and setting the crystallite size corresponding to the crystal plane to 5.0 nm or less, it is possible to make the silicon oxide particles contain as little crystalline Si as possible. This makes it possible to suppress the reaction with the electrolyte and prevent the deterioration of the battery characteristics. As described above, the crystallite size is preferably 5.0 nm or less, and it is preferably substantially amorphous. At this time, Li2SiO3 also shows crystallinity, but the higher the crystallinity of Li2SiO3, the more stable the structure is, but the higher the resistance is. On the other hand, when the crystallinity is low, it is easy to dissolve in the slurry, so there is an optimal range. Therefore, it is preferable to satisfy the above formula (1).

[0047] In the negative electrode of the present invention, the negative electrode active material particles preferably have a median diameter of 5.5 μm or more and 15 μm or less. If the negative electrode active material particles have a median diameter of 5.5 μm or more, the reaction with the electrolyte is suppressed, and the deterioration of the battery characteristics can be suppressed. On the other hand, if the negative electrode active material particles have a median diameter of 15 μm or less, the expansion of the active material due to charging and discharging can be suppressed, and electronic contact can be ensured.

[0048] In the negative electrode of the present invention, the true density of the negative electrode active material particles is preferably greater than 2.3 g / cc and less than 2.4 g / cc before charge and discharge.

[0049] The true density of SiO is 2.2 g / cc, but by doping with lithium, the true density of the negative electrode active material particles can be increased to a higher true density of more than 2.3 g / cc, thereby increasing the density of the electrode. In addition, if the true density is less than 2.4 g / cc, it is possible to suppress the tendency for cracks to occur during expansion and contraction. For this reason, it is believed that there is an appropriate range for the true density of the negative electrode active material particles. <Non-aqueous electrolyte secondary battery negative electrode>

[0050] [Negative electrode composition] Next, a more specific configuration of the negative electrode of the present invention will be described.

[0051] Fig. 5 shows a cross-sectional view of a negative electrode containing the negative electrode active material of the present invention. As shown in Fig. 5, a negative electrode 10 has a negative electrode active material layer 12 on a negative electrode current collector 11. This negative electrode active material layer 12 may be provided on both sides or only one side of the negative electrode current collector 11. Furthermore, if the negative electrode active material of the present invention is used, the negative electrode current collector 11 may not be necessary.

[0052] [Negative electrode current collector] The negative electrode current collector 11 is made of a material having excellent electrical conductivity and excellent mechanical strength. Examples of the conductive material that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). It is preferable that this conductive material is a material that does not form an intermetallic compound with lithium (Li).

[0053] The negative electrode current collector 11 preferably contains carbon (C) and / or sulfur (S) in addition to the main elements. This is because the physical strength of the negative electrode current collector is improved. In particular, when the current collector has an active material layer that expands during charging, if the current collector contains the above elements, this has the effect of suppressing deformation of the electrode including the current collector. The contents of the above contained elements are not particularly limited, but are preferably 100 mass ppm or less for each. This is because a higher deformation suppression effect can be obtained. Such a deformation suppression effect can further improve cycle characteristics.

[0054] The surface of the negative electrode current collector 11 may be roughened or may not be roughened. The roughened negative electrode current collector is, for example, a metal foil that has been electrolytically treated, embossed, or chemically etched. The unroughened negative electrode current collector is, for example, a rolled metal foil.

[0055] [Negative electrode active material layer] The negative electrode active material layer 12 contains the negative electrode active material of the present invention capable of absorbing and releasing lithium ions, and may further contain other materials such as a negative electrode binder and a conductive assistant from the viewpoint of battery design. The negative electrode active material contains negative electrode active material particles, and the negative electrode active material particles contain silicon oxide particles containing a silicon compound containing oxygen.

[0056] The negative electrode active material layer 12 may also contain a mixed negative electrode active material containing the negative electrode active material of the present invention (silicon-based negative electrode active material) and a carbon-based active material. This reduces the electrical resistance of the negative electrode active material layer and can alleviate the expansion stress caused by charging. Examples of the carbon-based active material that can be used include pyrolytic carbons, cokes, glassy carbon fibers, organic polymer compound sintered bodies, and carbon blacks.

[0057] As described above, the negative electrode active material contained in the negative electrode of the present invention contains silicon oxide particles. The ratio of silicon to oxygen in the silicon oxide constituting the silicon oxide particles is SiO x It is preferable that the range of x is 0.8≦x≦1.2. If x is 0.8 or more, the oxygen ratio is higher than that of silicon alone, and therefore the cycle characteristics are good. If x is 1.2 or less, the resistance of the silicon oxide particles does not become too high, which is preferable. Among these, SiO x In the composition, it is preferable that x is close to 1, because high cycle characteristics can be obtained. Note that the composition of silicon oxide in the present invention does not necessarily mean 100% purity, and may contain trace amounts of impurity elements.

[0058] In addition, in the negative electrode of the present invention, as described above, the negative electrode active material particles contain silicon oxide particles coated with a carbon layer, and the silicon oxide particles contain Li2SiO3 as a Li compound. When charging and discharging is performed once in this state, various phase structures are obtained according to the state of Li silicate having various valences. When the crystallinity of Li2SiO3 is low, the valence is relatively low, and when the crystallinity is high, the valence is high, but since Si crystals tend to grow, there is an optimum value.

[0059] The degree of Li silicate enlargement and the degree of Si crystallization (for example, the crystallite size corresponding to the Si(111) crystal plane) can be confirmed by XRD (X-ray Diffraction). XRD measurement can be performed, for example, under the following conditions. The X-ray diffraction device used may be, for example, the D8 ADVANCE manufactured by Bruker. The X-ray source is Cu Kα radiation, and a Ni filter is used. Measurements are performed from 10 to 40° with an output of 40 kV / 40 mA, a slit width of 0.3°, a step width of 0.008°, and a counting time of 0.15 seconds per step.

[0060] The negative electrode binder contained in the negative electrode active material layer may be, for example, one or more of polymer materials, synthetic rubber, etc. Examples of the polymer materials include polyvinylidene fluoride, polyimide, polyamideimide, aramid, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, carboxymethyl cellulose, etc. Examples of the synthetic rubber include styrene butadiene rubber, fluorine-based rubber, ethylene propylene diene, etc.

[0061] As the negative electrode conductive assistant, for example, one or more of carbon materials such as carbon black, acetylene black, graphite, Ketjen black, carbon nanotubes, and carbon nanofibers can be used.

[0062] The negative electrode active material layer is formed, for example, by a coating method, in which the silicon-based negative electrode active material is mixed with the binder and, if necessary, a conductive additive and a carbon-based active material, and then the mixture is dispersed in an organic solvent, water, or the like and coated.

[0063] [Method of manufacturing the negative electrode] Next, an example of a method for producing the negative electrode of the present invention will be described.

[0064] In the method for producing an anode of the present invention, anode active material particles are produced by the steps of producing silicon oxide particles, coating the silicon oxide particles with a carbon layer, inserting lithium into the silicon oxide particles coated with the carbon layer by an oxidation-reduction method, and heat-treating the silicon oxide particles with lithium inserted to form silicon oxide particles containing Li2SiO3, and an anode is produced using the produced anode active material particles. At this time, by adjusting the temperature during lithium insertion and the temperature during heat treatment, the silicon oxide particles contained in the anode are adjusted so that the intensity of peak A obtained near 529.5 eV and the intensity of peak B obtained near 532.5 eV are in the relationship (intensity of peak A)≦(intensity of peak B) after charging and discharging the anode at least once, as the O1s binding energy obtained by XPS analysis of the inside of the particle.

[0065] More specifically, the negative electrode is produced, for example, by the following procedure.

[0066] First, silicon oxide particles are prepared. In the following, silicon oxide particles are prepared using SiO x The case where silicon oxide represented by (0.5≦x≦1.6) is used will be described. First, a raw material that generates silicon oxide gas is heated in the presence of an inert gas and under reduced pressure at a temperature range of 900°C to 1600°C to generate silicon oxide gas. In this case, a mixture of metal silicon powder and silicon dioxide powder can be used as the raw material. Considering the presence of oxygen on the surface of the metal silicon powder and trace amounts of oxygen in the reactor, it is desirable for the mixture molar ratio to be in the range of 0.9<metal silicon powder / silicon dioxide powder<1.2.

[0067] The generated silicon oxide gas is solidified and deposited on the adsorption plate. Next, the temperature inside the reactor is lowered to 50°C or less, and the silicon oxide deposit is taken out and pulverized using a ball mill, jet mill, or the like to obtain powder. In this manner, silicon oxide particles can be produced. The Si crystallites in the silicon oxide particles can be controlled by changing the vaporization temperature of the raw material that generates the silicon oxide gas, or by heat treatment after the generation of the silicon oxide particles.

[0068] Here, a carbonaceous layer is formed on the surface of the silicon oxide particles. A pyrolytic CVD method is preferable as a method for forming the carbonaceous layer. An example of a method for forming a carbonaceous layer by the pyrolytic CVD method will be described below.

[0069] First, silicon oxide particles are placed in a furnace. Next, a hydrocarbon gas is introduced into the furnace, and the temperature inside the furnace is increased. The decomposition temperature is preferably 900°C or less, and more preferably 850°C or less. By setting the decomposition temperature at 900°C or less, unintended disproportionation of the active material particles can be suppressed. After the temperature inside the furnace is increased to a predetermined temperature, a carbon layer is generated on the surface of the silicon oxide particles. The hydrocarbon gas that is the raw material for the carbon material is not particularly limited, but may be C n H m In the composition, it is desirable for n to be ≦ 2. If n ≦ 2, the production cost can be reduced and the physical properties of the decomposition products can be improved.

[0070] Next, Li is inserted into the silicon oxide particles prepared as described above. This produces negative electrode active material particles containing silicon oxide particles with lithium inserted. That is, this modifies the silicon oxide particles, and a Li compound (Li silicate) is produced inside the silicon oxide particles. In the method for producing a negative electrode of the present invention, Li is inserted by the oxidation-reduction method as described above.

[0071] In the modification by the oxidation-reduction method, for example, first, lithium can be inserted by immersing silicon active material particles in solution A in which lithium is dissolved in an ether-based solvent. This solution A may further contain a polycyclic aromatic compound or a linear polyphenylene compound. After lithium insertion, active lithium can be desorbed from the silicon active material particles by immersing the silicon active material particles in solution B containing a polycyclic aromatic compound or its derivative. The solvent for this solution B can be, for example, an ether-based solvent, a ketone-based solvent, an ester-based solvent, an alcohol-based solvent, an amine-based solvent, or a mixed solvent thereof. Alternatively, after immersion in solution A, the obtained silicon active material particles may be heat-treated under an inert gas. The Li compound can be stabilized by heat treatment. After that, washing may be performed using a method such as washing with alcohol, alkaline water in which lithium carbonate is dissolved, weak acid, or pure water.

[0072] As the ether solvent used in solution A, diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, or a mixture thereof can be used. Among these, it is particularly preferable to use tetrahydrofuran, dioxane, or 1,2-dimethoxyethane. These solvents are preferably dehydrated and deoxygenated.

[0073] Furthermore, the polycyclic aromatic compound contained in solution A may be one or more of naphthalene, anthracene, phenanthrene, naphthacene, pentacene, pyrene, picene, triphenylene, coronene, chrysene, and derivatives thereof, and the linear polyphenylene compound may be one or more of biphenyl, terphenyl, and derivatives thereof.

[0074] The polycyclic aromatic compound contained in solution B may be one or more of naphthalene, anthracene, phenanthrene, naphthacene, pentacene, pyrene, picene, triphenylene, coronene, chrysene, and derivatives thereof.

[0075] As the ether solvent for solution B, diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and the like can be used.

[0076] As the ketone solvent, acetone, acetophenone, etc. can be used.

[0077] As the ester solvent, methyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, and the like can be used.

[0078] As the alcohol-based solvent, methanol, ethanol, propanol, isopropyl alcohol, and the like can be used.

[0079] As the amine solvent, methylamine, ethylamine, ethylenediamine, and the like can be used.

[0080] The Li silicate produced in this way is mainly Li4SiO4, and it is difficult to make it into a battery in this state. Therefore, heat treatment is performed to convert it to Li2SiO3, but the degree of crystallization of the Li silicate and Si changes depending on the temperature at this time. In addition, the reaction temperature during Li insertion is also related. In particular, if Li is inserted at a temperature close to the boiling point of the solvent used, the crystallinity of Si will appear in the next heat treatment process, even though the crystallinity of the Li silicate will not be that large. Therefore, the balance between the heat treatment and the Li insertion process is important.

[0081] Also, if the temperature during Li insertion is too low, the reactivity is low. At least 50°C or higher is preferable. At such a temperature, the reactivity during Li insertion can be ensured. By increasing the reactivity during Li insertion to a predetermined level or higher, it is possible to prevent the Li concentration in the particle surface layer from becoming too high, and as a result, it is possible to suppress the progress of disproportionation in the surface layer during the heat treatment in the next step.

[0082] The material that has been subjected to Li doping by the oxidation-reduction method can be subjected to heat treatment at 500°C to 650°C after filtration to control the type and amount (abundance ratio) of Li silicate. When performing such control, it is important to perform heat treatment in a vacuum state or under inert gas. In addition, it is preferable to use a heat treatment device, not limited to the device here, for uniform heat treatment such as a rotary kiln. At this time, various Li silicate states can be created by using the vacuum state, inert gas flow rate (internal pressure), retort thickness, and rotation speed as factors. Those skilled in the art can easily determine experimentally what Li silicate state is created under what conditions. Similarly, silicon enlargement or amorphization of silicon can be controlled. Those skilled in the art can easily determine experimentally what conditions these controls are performed under.

[0083] In the method for producing the negative electrode of the present invention, the temperature during the lithium insertion and the temperature during the heat treatment are adjusted so that the intensity of the peak A obtained near 529.5 eV and the intensity of the peak B obtained near 532.5 eV have a relationship of (intensity of peak A) ≦ (intensity of peak B) as the O1s binding energy obtained by XPS analysis of the inside of the silicon oxide particles. Such conditions can be easily obtained experimentally by a person skilled in the art. In particular, the temperature during the lithium insertion and the temperature during the heat treatment are adjusted, but it is preferable to adjust the temperature during SiO deposition and the CVD temperature in addition to them.

[0084] The negative electrode active material prepared as described above is mixed with other materials such as a negative electrode binder and a conductive assistant to form a negative electrode mixture, and then an organic solvent or water is added to form a slurry. Next, the above-mentioned slurry is applied to the surface of the negative electrode current collector and dried to form a negative electrode active material layer. At this time, hot pressing or the like may be performed as necessary. In this manner, a negative electrode can be prepared.

[0085] [Separator] The separator separates the positive and negative electrodes, prevents current short circuit caused by contact between the electrodes, and allows lithium ions to pass through. The separator is formed of a porous film made of, for example, synthetic resin or ceramic, and may have a laminated structure in which two or more types of porous films are laminated. Examples of synthetic resins include polytetrafluoroethylene, polypropylene, and polyethylene.

[0086] [Electrolyte] At least a portion of the active material layer or the separator is impregnated with a liquid electrolyte (electrolytic solution). This electrolytic solution contains an electrolyte salt dissolved in a solvent, and may contain other materials such as additives.

[0087] The solvent may be, for example, a non-aqueous solvent. Examples of non-aqueous solvents include ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane, or tetrahydrofuran. Among these, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. This is because better characteristics can be obtained. In this case, more advantageous characteristics can be obtained by combining a high-viscosity solvent such as ethylene carbonate or propylene carbonate with a low-viscosity solvent such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate. This is because the dissociation property and ion mobility of the electrolyte salt are improved.

[0088] When an alloy-based negative electrode is used, it is particularly desirable that the solvent contains at least one of halogenated chain carbonates or halogenated cyclic carbonates. This allows a stable coating to be formed on the surface of the negative electrode active material during charging and discharging, particularly during charging. Here, the halogenated chain carbonate is a chain carbonate having a halogen as a constituent element (at least one hydrogen is substituted with a halogen). Also, the halogenated cyclic carbonate is a cyclic carbonate having a halogen as a constituent element (i.e., at least one hydrogen is substituted with a halogen).

[0089] The type of halogen is not particularly limited, but fluorine is preferred because it forms a better coating than other halogens. Also, the more halogens there are, the more desirable they are because the resulting coating is more stable and the decomposition reaction of the electrolyte is reduced.

[0090] Examples of halogenated chain carbonates include fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, etc. Examples of halogenated cyclic carbonates include 4-fluoro-1,3-dioxolan-2-one, 4,5-difluoro-1,3-dioxolan-2-one, etc.

[0091] It is preferable that the solvent additive contains an unsaturated carbon-bonded cyclic carbonate. This is because a stable coating is formed on the negative electrode surface during charging and discharging, and the decomposition reaction of the electrolyte can be suppressed. Examples of the unsaturated carbon-bonded cyclic carbonate include vinylene carbonate and vinylethylene carbonate.

[0092] It is also preferable that the solvent additive contains sultone (cyclic sulfonic acid ester), because this improves the chemical stability of the battery. Examples of sultones include propane sultone and propene sultone.

[0093] Furthermore, it is preferable that the solvent contains an acid anhydride, because this improves the chemical stability of the electrolyte. As the acid anhydride, for example, propane disulfonic acid anhydride can be mentioned.

[0094] The electrolyte salt may include at least one of light metal salts such as lithium salts, for example. Examples of the lithium salt include lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4).

[0095] The content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less relative to the solvent, because this provides high ionic conductivity. EXAMPLES

[0096] The present invention will be described in more detail below by showing examples and comparative examples of the present invention, but the present invention is not limited to these examples.

[0097] [Common conditions for the examples] First, the negative electrode active material contained in the negative electrode was prepared as follows. A mixture of silicon metal and silicon dioxide was introduced into a reactor, vaporized in a vacuum of 10 Pa, and deposited on an adsorption plate. After sufficient cooling, the deposit was removed. The deposit was pulverized in a ball mill. The SiO x The value of x was 1.0.

[0098] During deposition of silicon oxide (SiO), it was deposited with a nearly uniform temperature distribution. In reality, it is not possible to measure the temperature, but at low temperatures the density decreases and the color becomes yellowish when collected. On the other hand, at high temperatures the color becomes metallic. This is due in part to the crystallization of silicon. The SiO used in each example did not have such a concentration distribution during deposition.

[0099] After the silicon oxide particles were obtained as described above, the particle size of the silicon oxide particles was adjusted by classification, and then the surfaces of the silicon oxide particles were coated with a carbon material by performing pyrolysis CVD at a temperature range of 400°C to 900°C.

[0100] Next, a solvent with a water content reduced to 50 ppm was used to insert lithium into the silicon oxide particles by an oxidation-reduction method, followed by heating at a temperature in the range of 500°C to 650°C for further modification.

[0101] Next, the prepared negative electrode active material (silicon oxide particles), graphite, conductive additive 1 (carbon nanotubes, CNT), conductive additive 2 (carbon particles with a median diameter of approximately 50 nm), sodium polyacrylate, and carboxymethyl cellulose (hereinafter referred to as CMC) were mixed in a dry mass ratio of 9.3:83.7:1:1:4:1, and then diluted with pure water to prepare a negative electrode mixture slurry.

[0102] In addition, an electrolytic copper foil with a thickness of 15 μm was used as the negative electrode current collector. This electrolytic copper foil contained carbon and sulfur at a concentration of 70 mass ppm each. Finally, the negative electrode mixture slurry was applied to the negative electrode current collector and dried at 100° C. for 1 hour in a vacuum atmosphere. After drying, the deposition amount of the negative electrode active material layer per unit area on one side of the negative electrode (also called the area density) was 7.0 mg / cm 2 It was.

[0103] Next, the solvents ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed, and then the electrolyte salt (lithium hexafluorophosphate: LiPF6) was dissolved to prepare an electrolyte solution. In this case, the solvent composition was EC:DMC=30:70 in volume ratio, and the content of the electrolyte salt was 1 mol / kg relative to the solvent. As additives, vinylene carbonate (VC) and fluoroethylene carbonate (FEC) were added at 1.0 wt% and 2.0 wt%, respectively.

[0104] Next, a coin battery was assembled as follows. First, a 1 mm thick Li foil was punched out to a diameter of 16 mm and attached to an aluminum clad. The resulting negative electrode was punched out to a diameter of 15 mm, and the Li foil was placed face-to-face with a separator in between. After injecting the electrolyte, a 2032 coin battery was produced.

[0105] The initial efficiency was measured under the following conditions. First, the charge rate was set to 0.03C. At this time, charging was performed in CCCV mode. CV was set to 0V and the final current was set to 0.04mA. The discharge rate was 0.03C, the discharge voltage was 1.2V, and CC discharge was performed.

[0106] Then, the initial efficiency (sometimes called "initial efficiency") was calculated using the formula: initial efficiency (%) = (initial discharge capacity / initial charge capacity) x 100.

[0107] Based on the initial data obtained, a counter positive electrode was designed and a battery was evaluated.

[0108] The cycle characteristics were investigated as follows. First, to stabilize the battery, two cycles of charge and discharge were performed at 0.2C in an atmosphere of 25°C, and the discharge capacity of the second cycle was measured. The battery cycle characteristics were calculated from the discharge capacity of the third cycle, and the battery test was stopped after 100 cycles. Charge and discharge were performed at 0.7C and 0.5C. The charge voltage was 4.3V, the discharge cut-off voltage was 2.5V, and the charge cut-off rate was 0.07C.

[0109] The negative electrode thus obtained was charged and discharged once, and then the negative electrode active material was subjected to XPS analysis. For this XPS analysis, a scanning X-ray photoelectron spectrometer PHI Quantera II manufactured by ULVAC-PHI, Inc. was used. The X-ray beam diameter was set to 100 μm, and a neutralization gun was used.

[0110] The results of each of the examples and comparative examples are summarized in Table 1. Figures 1 and 2 respectively show the O1s spectrum and Si2p spectrum obtained by XPS analysis in Example 1. Figures 3 and 4 respectively show the O1s spectrum and Si2p spectrum obtained by XPS analysis in Comparative Example 1.

[0111] [Example 1] Pyrolytic CVD to coat the surface of silicon oxide particles with a carbon film was carried out using propane at 800°C. Li doping was carried out at a temperature 5°C lower than the boiling point of the solvent (diglyme), and the stabilization temperature after doping was 580°C.

[0112] In the negative electrode obtained in Example 1, there was no significant change in the physical properties before and after charging and discharging. However, referring to Fig. 1, it can be seen that after charging and discharging using such particles, the high-valence state inside the particles can be maintained in the O1s spectrum.

[0113] In this way, by finely adjusting the conditions for SiO formation, CVD, and Li doping, it is possible to precisely control the properties that react with Li, thereby improving the battery characteristics. [Comparative Example 1] Similar to Example 1, the pyrolytic CVD for coating the surfaces of silicon oxide particles with a carbon film was carried out at 950° C. In addition, the Li doping process was carried out at a temperature 10° C. lower than the boiling point of the solvent (diglyme), and the stabilization process temperature after doping was 570° C.

[0114] In the negative electrode obtained in Comparative Example 1, there was no significant change in the physical properties before and after charging and discharging. However, referring to Fig. 3, it can be seen that after charging and discharging using such particles, there are many low valence states in the O1s spectrum.

[0115] [Example 2] The change in valence was suppressed from the particle surface to the inside. Specifically, the Li doping reaction rate was set to be 10 times slower than in Example 1, and Li was doped slowly, so that a more uniform Li silicate phase could be formed from the particle surface to the inside. In this case, the Li acceptability was deteriorated, and the characteristics were shifted in a slightly worse direction than in Example 1.

[0116] [Examples 3 to 7] As in Example 1, the heat treatment temperature was changed within the range of 500° C. or more and 650° C. or less to control the crystallinity of Li silicate and Si.

[0117] As a result, it was found that the crystallinity of the Si is preferably substantially amorphous. This Li silicate and the crystallization of Si estimated from XRD are important control parameters, and change significantly depending on the conditions of Li insertion and heat treatment conditions.

[0118] [Examples 8 to 13] However, the particle size of the negative electrode active material particles was changed in the same manner as in Example 1. As a result, when the median diameter of the negative electrode active material particles was 5.5 μm or more and 15 μm or less, the reaction area was reduced and the cycle characteristics of the battery were significantly improved.

[0119] [Table 1]

[0120] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0121] 10...Negative electrode, 11...Negative electrode current collector, 12...Negative electrode active material layer.

Claims

1. A negative electrode comprising negative electrode active material particles and having been charged and discharged at least once, The negative electrode active material particles contain silicon oxide particles coated with a carbon layer, The silicon oxide particles are Li 2 SiO 3 and in O1s binding energies obtained by XPS analysis of the inside of a particle, the intensity of peak A obtained near 529.5 eV and the intensity of peak B obtained near 532.5 eV have a relationship of (intensity of peak A)≦(intensity of peak B).

2. The negative electrode according to claim 1, characterized in that the silicon oxide particles have a phase structure estimated from peak positions of Si2p binding energy and O1s binding energy obtained by XPS analysis of the silicon oxide particles, which has a three-phase structure or less, and the O1s binding energy peak near 531.5 eV is smaller than the peak near 532.5 eV.

3. 3. The negative electrode according to claim 1, wherein, when a ratio of a peak A obtained near 529.5 eV to a peak B obtained near 532.5 eV in O1s binding energy obtained by XPS analysis of the silicon oxide particles is defined as (intensity of peak A) / (intensity of peak B), (intensity of peak A) / (intensity of peak B) on the surface of the silicon oxide particles is larger than (intensity of peak A) / (intensity of peak B) inside the silicon oxide particles.

4. The negative electrode active material particles have a peak due to a Si (111) crystal plane obtained by X-ray diffraction using Cu-Kα radiation before charging and discharging the negative electrode active material particles, and the crystallite size corresponding to the crystal plane is 5.0 nm or less, and Li 2 SiO 3 The ratio G / H of the intensity G of the peak due to the Si (111) crystal plane to the intensity H of the peak due to the (111) crystal plane is expressed by the following formula (1): 0.4≦G / H≦1.0 (1) 4. The negative electrode according to claim 1, wherein the negative electrode satisfies the following:

5. 5. The negative electrode according to claim 1, wherein the negative electrode active material particles have a median diameter of 5.5 μm or more and 15 μm or less.

6. 6. The negative electrode according to claim 1, wherein the negative electrode active material particles have a true density of more than 2.3 g / cc and less than 2.4 g / cc before charging and discharging.

7. Producing silicon oxide particles; coating the silicon oxide particles with a carbon layer; inserting lithium into the silicon oxide particles coated with the carbon layer by a redox process; The lithium-intercalated silicon oxide particles are heat-treated to form Li 2 SiO 3 and forming silicon oxide particles containing the and producing a negative electrode by using the produced negative electrode active material particles, a temperature during the lithium insertion and a temperature during the heat treatment are adjusted so that, after the negative electrode is charged and discharged at least once, the silicon oxide particles contained in the negative electrode have an intensity of peak A obtained near 529.5 eV and an intensity of peak B obtained near 532.5 eV, as O1s binding energies obtained by XPS analysis of the inside of the particles, such that the intensity of peak A is equal to or less than the intensity of peak B.

Citation Information

Patent Citations

  • Nonaqueous electrolytic secondary battery and its manufacture

    JP1994325765A

  • Lithium secondary battery

    JP2001185127A

  • Non-aqueous electrolyte secondary battery

    JP2002042806A

  • Battery

    JP2006114454A

  • Negative electrode for lithium ion secondary battery, its manufacturing method, and lithium ion secondary battery using it

    JP2006164954A