Laser photothermal transfer film
The laser photothermal transfer film with a bismaleimide resin and diimonium series dyes addresses transmittance and heat resistance issues, enhancing transfer precision and efficiency by expanding upon laser irradiation.
Patent Information
- Application Number
- JP2021194904
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-11-30
AI Technical Summary
Existing photothermal transfer films using infrared-absorbing dyes and metal materials face issues with insufficient transmittance in the visible light region, leading to quality inspection problems and alignment issues with receiver elements, while films using acrylic resins have low heat resistance and thermal expansion coefficients, resulting in poor transfer ability.
A laser photothermal transfer film with a base film, a photothermal conversion layer containing a bismaleimide resin with a high expansion coefficient, and an adhesive layer, where the conversion layer includes specific infrared light absorbers, such as diimonium series dyes, to enhance transfer characteristics.
The film achieves improved transfer characteristics with high transmittance in the visible light range and precise adhesion to transfer substrates, allowing for efficient transfer of semiconductor elements by expanding the photothermal conversion layer upon laser irradiation.
Smart Images

Figure 0007558919000024 
Figure 0007558919000025 
Figure 0007558919000026
Abstract
Description
[Technical field]
[0001] The present invention relates to a laser photothermal transfer film in which a base film, a photothermal conversion layer which generates heat and expands upon laser irradiation, and an adhesive layer are laminated in this order. [Background technology]
[0002] The light absorbents for photothermal conversion used in photothermal transfer films include infrared absorbing dyes, pigments, metal materials, etc. Infrared absorbing dyes have the advantage that they have a maximum absorbance peak in the near infrared region, which is the typical infrared laser wavelength range used in laser photothermal transfer, but have a wide range of materials that show relatively low absorbance in the visible light region below 700 nm.
[0003] For example, Patent Document 1 discloses Prussian Blue (or Pigment Blue 27), copper phthalocyanine (Pigment Blue 15), polymethine dyes, cyanine dyes, and the like as materials for image-forming radiation absorbers suitable for use with 808 nm lasers.
[0004] Meanwhile, Patent Document 2 discloses dyes of the indolium salts or benzoindolium salts series as dyes that can be applied to a light-to-heat conversion layer whose maximum absorbance at 650-1200 nm wavelengths is three times larger than that at 400-650 nm wavelengths. Examples of benzoindolium salts are shown below. [ka]
[0005] Patent Document 3 discloses metal complex compounds of phthalocyanine-based compounds as light absorbents for laser photothermal transfer. Examples of phthalocyanine-metal complex compounds are shown below. However, when using the above dyes, the transmittance in the visible light region is insufficient, which causes problems in quality inspection of the produced transfer film and alignment with the receiver element. [ka] (M represents any of several hydrogen atoms, divalent metals, trivalent metal derivatives, or tetravalent metal derivatives, R1 to R8 each represent an alkyl group or an alkoxyalkyl group, X1 to X8 each represent sulfur or NR9, X1 = (either X3 or X4) = (either X5 or X6) = (either X7 or X8) = sulfur, and X2 = (the other of X3 and X4) = (the other of X5 and X6) = (the other X7 and X8) = NR9; R9 represents hydrogen or an alkyl group. However, the above R1, etc. apply only to the above formula.)
[0006] Patent Document 4 discloses a photothermal transfer film consisting of a base film, a photothermal conversion layer, and an adhesive layer. In this patent, after irradiation with an infrared laser, the photothermal conversion layer expands, making it possible to transfer a transfer object to a specific position. Examples of the binder mentioned above include acrylic resins (polyacrylate, polymethacrylate, polyacrylic acid, or copolymers of these with polyolefins, which may or may not have hydrophilic functional groups such as -OH and -COOH). These resins lack heat resistance and have a small thermal expansion coefficient, so they have low transfer capabilities. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Republic of Korea Publication No. 2009-0034364 [Patent Document 2] Republic of Korea Publication No. 2007-0067725 [Patent Document 3] U.S. Patent No. 6,066,729 [Patent Document 4] Republic of Korea Publication No. 2019-0106498 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above circumstances, and aims to provide a laser photothermal transfer film in which a bismaleimide resin with a high expansion coefficient is used as a binder for the photothermal conversion layer, thereby improving the transfer characteristics by causing the photothermal conversion layer to expand significantly after laser irradiation. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides The present invention provides a laser photothermal transfer film having three layers laminated in this order: a base film, a photothermal conversion layer, and an adhesive layer, wherein the photothermal conversion layer is a solid at room temperature that contains an infrared light absorber represented by general formula (1) and a bismaleimide resin represented by the following general formula (3) and / or general formula (4): [ka] (In the general formula (1), p is 1 or 2; R1 to R8 each independently represent a substituted or unsubstituted linear or branched alkyl group having 1 to 10 carbon atoms, which may be substituted with a cyano group, a nitro group, a carboxyl group, a sulfone group, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, an alkoxyalkoxy group, an acyloxy group, or an alkylamino group; X - is a fluoroalkyl phosphate anion represented by the following general formula (2). [ka] (In the general formula (2), x is 0 or 1, y is 1, 2 or 3, z is 6-y, and R9 to R 13are each independently hydrogen or fluorine. [ka] (In the general formula (3), A represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. Q represents a linear alkylene group having 6 or more carbon atoms. Each R independently represents a linear or branched alkyl group having 6 or more carbon atoms. n represents an integer of 1 to 10.) [ka] (In general formula (4), A' represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. B represents an alkylene chain having 6 to 18 carbon atoms and having a divalent aliphatic ring which may contain a heteroatom. Q' represents a linear alkylene group having 6 or more carbon atoms. Each R' independently represents a linear or branched alkyl group having 6 or more carbon atoms. n' represents an integer of 1 to 10. m represents an integer of 1 to 10.)
[0010] Such a laser photothermal transfer film can provide a laser photothermal transfer film with improved transfer properties.
[0011] In the present invention, the adhesive constituting the adhesive layer is preferably one or a combination of two or more selected from polyacrylate, polymethacrylate, epoxy, polystyrene, polyurethane, polysulfone, polyester, polyimide, and silicone resin.
[0012] Such a material is preferable as an adhesive for a laser photothermal transfer film.
[0013] In the present invention, it is preferable that the content of the infrared light absorbent in the light-to-heat conversion layer is 1 to 15% by mass, and the content of the bismaleimide resin is 85 to 99% by mass.
[0014] In such a laser photothermal transfer film, the infrared ray absorbent can be suitably dispersed in the binder resin, and sufficient heat can be generated by laser irradiation.
[0015] In the present invention, the adhesive layer preferably has a thickness of 1 to 10 μm.
[0016] Such a laser photothermal transfer film has sufficient adhesive strength, and the transfer medium adheres well, making it easy to control the transfer characteristics after laser irradiation.
[0017] In the present invention, the light-to-heat conversion layer preferably has a thickness of 0.1 to 20 μm.
[0018] In such a laser light-heat transfer film, the light-heat conversion layer expands by locally absorbing heat due to laser irradiation, facilitating transfer.
[0019] In the present invention, the infrared light absorbent preferably has a maximum absorption wavelength within a range of 780 to 1500 nm.
[0020] Such a laser photothermal transfer film exhibits high efficiency in photothermal conversion by near infrared rays.
[0021] In the present invention, the adhesive layer preferably has an adhesive strength of 0.1 to 10 N / 25 mm.
[0022] With such a laser photothermal transfer film, the transfer body can be well transferred to the transfer substrate by laser irradiation.
[0023] In the present invention, the base film is preferably made of a transparent thermoplastic resin.
[0024] With such a substrate film, the light-to-heat conversion layer can be expanded by irradiating it with laser light from the substrate film side.
[0025] In the present invention, it is preferable that the cured product of the bismaleimide resin has a thermal decomposition onset temperature of 300° C. or higher, a glass transition temperature of 150° C. or lower, and a thermal expansion coefficient at or above the glass transition temperature of 100 ppm / ° C. or higher.
[0026] Such a laser light thermal transfer film allows for accurate transfer from the laser light thermal transfer film to a transfer substrate. Effect of the Invention
[0027] As described above, according to the present invention, by using a bismaleimide resin with a large expansion coefficient as a binder for the photothermal conversion layer, the photothermal conversion layer expands significantly after laser irradiation, reducing the adhesive area between the transfer body and the adhesive layer, and by adjusting the adhesive strength within a specific range, it is possible to provide a laser photothermal transfer film with improved transfer characteristics. Therefore, it is extremely useful as a laser photothermal transfer film. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the laser photothermal transfer film of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a mounting flow for transferring an element using the laser photothermal transfer film of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing an example of 3D measurement of the expansion of the laser photothermal transfer film of the present invention after laser irradiation, the image being taken with a Keyence VHX digital microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] As a result of intensive research by the inventors to solve the above-mentioned problems, they found that the above-mentioned problems can be solved by a laser photothermal transfer film having three laminated layers: a base film, an infrared light absorber represented by the following general formula (1), a photothermal conversion layer containing a bismaleimide resin represented by the following general formula (3) and / or the following general formula (4), and an adhesive layer, and thus completed the present invention.
[0030] That is, the present invention provides: The laser photothermal transfer film is a laser photothermal transfer film having three layers laminated in this order: a base film, a photothermal conversion layer, and an adhesive layer, wherein the photothermal conversion layer is a solid at room temperature that contains an infrared light absorber represented by general formula (1) and a bismaleimide resin represented by the following general formula (3) and / or general formula (4). [ka] (In the general formula (1), p is 1 or 2; R1 to R8 each independently represent a substituted or unsubstituted linear or branched alkyl group having 1 to 10 carbon atoms, which may be substituted with a cyano group, a nitro group, a carboxyl group, a sulfone group, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, an alkoxyalkoxy group, an acyloxy group, or an alkylamino group; X - is a fluoroalkyl phosphate anion represented by the following general formula (2). [ka] (In the general formula (2), x is 0 or 1, y is 1, 2 or 3, z is 6-y, and R9 to R 13 are each independently hydrogen or fluorine. [ka] (In the general formula (3), A represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. Q represents a linear alkylene group having 6 or more carbon atoms. Each R independently represents a linear or branched alkyl group having 6 or more carbon atoms. n represents an integer of 1 to 10.) [ka] (In general formula (4), A' represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. B represents an alkylene chain having 6 to 18 carbon atoms and having a divalent aliphatic ring which may contain a heteroatom. Q' represents a linear alkylene group having 6 or more carbon atoms. Each R' independently represents a linear or branched alkyl group having 6 or more carbon atoms. n' represents an integer of 1 to 10. m represents an integer of 1 to 10.)
[0031] Thus, the present invention relates to a laser photothermal transfer film, which has a photothermal conversion layer and an adhesive layer laminated on a base film, the photothermal conversion layer containing a diimonium-series dye infrared light absorber and a bismaleimide resin with a large thermal expansion coefficient, and has high transmittance in the visible light range and improved transfer characteristics due to the adhesive layer having an appropriate range of adhesive strength.
[0032] The photothermal conversion layer is a heat-cured thin layer with a large thermal expansion coefficient that contains an infrared light absorbent of a diimonium dye series. By adjusting the thickness of the adhesive layer within a specific range and adjusting its adhesive strength, the photothermal conversion layer and the adhesive layer expand and deform after laser irradiation, reducing the contact area of the semiconductor element and decreasing the adhesive strength, making it possible to transfer the semiconductor element onto a specific substrate.
[0033] The present invention will be described in detail below, but the present invention is not limited thereto.
[0034] <Laser photothermal transfer film> The present invention is a laser photothermal transfer film that is solid at room temperature and includes three layers laminated in this order: a base film, a photothermal conversion layer, and an adhesive layer, and the photothermal conversion layer contains a specific infrared light absorbent and a specific bismaleimide resin. Note that, in the present invention, room temperature refers to 25°C.
[0035] As shown in Figure 1, the laser photothermal transfer film 1 of the present invention is formed by laminating three layers in this order: a base film 11, a photothermal conversion layer 12 containing a specific infrared light absorbent and a specific bismaleimide resin, and an adhesive layer 13. When the laser photothermal transfer film 1 is irradiated with laser light, the photothermal conversion layer 12 is heated and expands, causing the photothermal conversion layer 12 to push up the adhesive layer 13 located thereon and rise up. Each layer will be described below.
[0036] <Base film> The base film acts as a substrate for supporting the light-to-heat conversion layer, the adhesive layer, and the transfer material attached onto the adhesive layer.
[0037] As the substrate film, a polymer film can be used. Examples of suitable materials for use as the substrate film include polycarbonate, polyolefin, polyvinyl resin, and polyester. The substrate film is preferably a transparent thermoplastic resin. A polyester film that has both light transmittance and thermal stability, such as a polyethylene terephthalate or polyethylene naphthalate film, can be used, but is not limited thereto. A film having optical properties such as sufficient mechanical and thermal stability and high transmittance for light of a specific wavelength can be used.
[0038] The thickness of the above-mentioned base film is preferably 10 to 250 μm, and may be subjected to primer treatment, roughness treatment, etc. for the purpose of improving adhesion with the light-to-heat conversion layer, stretching or heat treatment for thermal stability, water repellency treatment, and may further contain a small amount of fine particles or filler to adjust light transmittance. Among them, the base film is preferably a biaxially stretched 50 to 200 μm polyethylene terephthalate (PET) film with a visible light transmittance of about 90% or more in order to transmit laser light.
[0039] <Light-to-heat conversion layer> The photothermal conversion layer is a solid at room temperature that contains an infrared light absorbent represented by general formula (1) and a bismaleimide resin represented by general formula (3) and / or general formula (4). One or more infrared light absorbents contained inside the photothermal conversion layer absorb light (laser) and convert it into heat, causing the photothermal conversion layer to expand, and the semiconductor element is transferred to the transfer substrate by the physical force caused by the thermal expansion.
[0040] The content of the infrared light absorbent in the light-heat conversion layer is preferably 1 to 15 mass %, and the content of the bismaleimide resin is preferably 85 to 99 mass %.
[0041] The light-to-heat conversion layer expands due to the localized absorption of heat by the laser irradiation, so it is preferable to make the light-to-heat conversion layer as thin as possible to facilitate transfer, with a thickness of 0.1 to 20 μm being preferred.
[0042] The infrared ray absorbing agent applied to the light-heat conversion layer of the light-heat transfer film of the present invention is a dye of the diimmonium salt series represented by the following general formula (1).
[0043] [ka] (In the general formula (1), p is 1 or 2; R1 to R8 each independently represent a substituted or unsubstituted linear or branched alkyl group having 1 to 10 carbon atoms, which may be substituted with a cyano group, a nitro group, a carboxyl group, a sulfone group, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, an alkoxyalkoxy group, an acyloxy group, or an alkylamino group; X - is a fluoroalkyl phosphate anion represented by the following general formula (2). [ka] (In the general formula (2), x is 0 or 1, y is 1, 2 or 3, z is 6-y, and R9 to R 13 are each independently hydrogen or fluorine.
[0044] In the present invention, for example, when a polyethylene terephthalate (PET) film having a thickness of 100 μm is used as the base film, the visible light transmittance of the biaxially stretched PET film can be about 90%. When the infrared light absorbent represented by the above general formula (1) is used in this base film, a photothermal transfer film that maintains the transfer performance and has a visible light transmittance of 60% or more can be produced.
[0045] The visible light transmittance is inversely proportional to the concentration of the infrared light absorbent used in the light-heat conversion layer. The diimonium salt-based organic dye used as the infrared light absorbent of the present invention has a higher absorbance in the near infrared light, specifically in the wavelength region of 780 to 1500 nm, than other organic dyes, and therefore has a high efficiency of light-heat conversion by near infrared light. On the other hand, the absorbance in the visible light region is not high, and the transparency in the visible light region is high. That is, it is preferable that the maximum absorption wavelength of the infrared light absorbent is within the range of 780 to 1500 nm.
[0046] The diimonium salt-based dye, which is an infrared light absorbent, is used together with a binder to adjust the adhesion to the base film and / or adhesive layer. The diimonium salt-based dye has excellent solubility in organic solvents, so it can be uniformly dispersed in the bismaleimide resin, which serves as the binder. As a result, it is possible to make the amount of heat generated by spot-irradiating laser uniform because it is uniformly dispersed in the resin. In addition, such good dispersibility has the advantage of reducing the thickness deviation of the light-to-heat conversion layer, which has a thickness of less than 10 μm.
[0047] The bismaleimide resin that serves as the binder of the light-to-heat conversion layer is a bismaleimide resin that is solid at 25°C, and is a maleimide compound having at least one dimer acid skeleton, at least one linear alkylene group having 6 or more carbon atoms, and at least two maleimide groups in the molecule. Since it has a linear alkylene group having 6 or more carbon atoms, it has excellent heat resistance, and since it has a large expansion coefficient, it expands greatly due to heat generated by absorption of laser light, and transfer can be easily performed. In the present invention, as such a bismaleimide resin, one represented by the following general formula (3) and / or general formula (4) is used.
[0048] [ka] (In the general formula (3), A represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. Q represents a linear alkylene group having 6 or more carbon atoms. Each R independently represents a linear or branched alkyl group having 6 or more carbon atoms. n represents an integer of 1 to 10.) [ka] (In general formula (4), A' represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. B represents an alkylene chain having 6 to 18 carbon atoms and having a divalent aliphatic ring which may contain a heteroatom. Q' represents a linear alkylene group having 6 or more carbon atoms. Each R' independently represents a linear or branched alkyl group having 6 or more carbon atoms. n' represents an integer of 1 to 10. m represents an integer of 1 to 10.)
[0049] Q in general formula (3) and Q' in general formula (4) are linear alkylene groups, each of which has 6 or more carbon atoms, preferably 6 or more and 20 or less, and more preferably 7 or more and 15 or less. Furthermore, the number of carbon atoms of R in general formula (3) and the number of carbon atoms of R' in general formula (4) are 6 or more, preferably 6 or more and 12 or less, and R and R' can be linear or branched alkyl groups.
[0050] A in general formula (3) and A' in general formula (4) represent a tetravalent organic group containing an aromatic ring or an aliphatic ring, and are particularly preferably represented by any of the tetravalent organic groups represented by the following structural formulas. [ka] (Note that the bond not bonded to a substituent in the above structural formula is bonded to the carbonyl carbon that forms a cyclic imide structure in general formula (3) and general formula (4).)
[0051] Furthermore, B in the general formula (4) is an alkylene chain having 6 to 18 carbon atoms and an aliphatic ring which may contain a divalent heteroatom, and the number of carbon atoms in the alkylene chain is preferably 8 to 15. B in the general formula (4) is preferably any of the alkylene chains having an aliphatic ring represented by the following structural formulas. [ka] (Note that the bond not bonded to a substituent in the above structural formula is bonded to the nitrogen atom that forms a cyclic imide structure in general formula (4).)
[0052] In general formula (3), n is an integer of 1 to 10, and preferably an integer of 2 to 7. In general formula (4), n' is an integer of 1 to 10, and preferably an integer of 2 to 7. In general formula (4), m is an integer of 1 to 10, and preferably an integer of 2 to 7.
[0053] The weight-average molecular weight (Mw) of the bismaleimide resin is not particularly limited as long as it is in a range in which it is solid at room temperature, but the weight-average molecular weight converted into a polystyrene standard by gel permeation chromatography (GPC) measurement is preferably 2,000 to 50,000, particularly preferably 2,500 to 40,000, and further preferably 3,000 to 20,000. If the molecular weight is 2,000 or more, the bismaleimide resin is solidified at room temperature, and if the molecular weight is 50,000 or less, the coating composition described below does not have too high a viscosity and is not likely to reduce flowability, and has good moldability. In this specification, Mw refers to the weight average molecular weight measured by GPC under the following conditions, using polystyrene as the standard.
[0054] <Measurement conditions> Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-L TSKgel SuperHZ4000(4.6mmI.D.×15cm×1) TSKgel SuperHZ3000(4.6mmI.D.×15cm×1) TSKgel SuperHZ2000 (4.6mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 5 μL (0.2% by mass in THF solution)
[0055] As the bismaleimide resin that can be used in the present invention, SLK3000, SLK689, SLK2600, etc., commercially available as the SLK series (manufactured by Shin-Etsu Chemical Co., Ltd.) are preferable.
[0056] It is possible to prepare a coating composition in the form of a varnish-like solution in which the above-mentioned infrared light absorbent, the bismaleimide resin as a binder, and the curing catalyst are dissolved and dispersed in an organic solvent such as anisole. This varnish-like solution is coated and laminated on a substrate film, and after coating, the solvent is removed by applying heat in a heating tank, and the bismaleimide resin is dried and solidified, thereby forming a light-to-heat conversion layer that contains the infrared light absorbent and the maleimide resin and is solid at room temperature on the substrate film.
[0057] The photothermal conversion layer may be solid at room temperature (25°C), and may contain a curing catalyst as necessary. The curing catalyst may be an imidazole catalyst, an organic peroxide, or the like, but is not particularly limited as long as it is a catalyst that reacts with the maleimide group.
[0058] The solid content of the coating composition is preferably 5 to 85% by mass, more preferably 5 to 60% by mass. If the solid content of the composition is 5% by mass or more, it is easy to process the coating layer to the desired thickness, and if it is 85% by mass or less, the viscosity of the coating resin does not increase, and the surface does not become rough after coating, which is preferable.
[0059] In addition, the content of the infrared light absorbent (diimonium salt-based dye) in the solid matter of the composition is preferably 1 to 15% by mass. If the content of the infrared light absorbent is 1% by mass or more, sufficient heat generation occurs, and if it is 15% by mass or less, the solubility of the infrared light absorbent is not reduced, making it suitable for dispersion in the binder resin.
[0060] Since the resin is heated by the heat generated by laser irradiation, the thermal decomposition onset temperature of the cured bismaleimide resin is preferably 300°C or higher, and more preferably 400°C or higher, and the glass transition temperature is preferably 150°C or lower, and more preferably 100°C or lower, and even more preferably 50°C or lower.
[0061] The thermal expansion coefficient of the cured bismaleimide resin is preferably 100 ppm / ° C. or less at temperatures below the glass transition temperature, and is preferably 100 ppm / ° C. or more, more preferably 150 ppm / ° C. or more, at temperatures above the glass transition temperature.
[0062] Generally, polyimide resins with heat resistance and a thermal decomposition starting temperature of 300°C or higher have a glass transition temperature of 200°C or higher, and a thermal expansion coefficient of 20 ppm / °C or lower below the glass transition temperature and 80 ppm / °C or lower above the glass transition temperature. Therefore, the expansion of the photothermal conversion layer after laser irradiation is smaller than that of the bismaleimide resin used in the present invention, and the transfer from the laser photothermal transfer film to the transfer substrate cannot be performed accurately. Therefore, it is necessary to keep the transfer substrate to which the semiconductor element or the like is transferred as close as possible to the laser photothermal transfer film. This makes it difficult to control the transfer force from the laser photothermal transfer film.
[0063] When the laser photothermal transfer film of the present invention is used, the expansion due to laser light irradiation is large, so the transfer substrate and the laser photothermal transfer film can be placed apart, and since the tip area of the photothermal conversion layer that expands convexly due to heat is reduced, the adhesive force is reduced and the semiconductor element can be easily transferred to the transfer substrate.
[0064] The coating composition may further contain a crosslinker, a moisturizer, a surfactant, a pH adjuster, a viscosity adjuster, a co-solvent, and the like.
[0065] Examples of laser light used for photothermal conversion include infrared laser, visible light laser, UV laser, and excimer laser, with infrared laser being preferred.
[0066] <Adhesive layer> The adhesive layer serves to attach the semiconductor element to the laser photothermal transfer film, and the adhesive strength of the adhesive layer is designed taking into consideration the adhesive strength of the transfer substrate. By appropriately adjusting the adhesive strength of the laser photothermal transfer film and the adhesive strength of the transfer substrate, problems such as the transfer body moving to the transfer substrate side or no transfer to the transfer substrate can be avoided when the two films are laminated. The adhesive strength of the laser transfer film is preferably 0.1 to 10 N / 25 mm in a 180° peel test (adherend SUS) in accordance with JIS Z 0237, and can be adjusted within the above range according to the adhesive strength of the transfer substrate side.
[0067] The thickness of the adhesive layer is preferably 1 to 10 μm. When the thickness of the adhesive layer is 1 μm or more, the adhesive strength is not reduced and the transfer body adheres well, and when the thickness is 10 μm or less, the transfer characteristics are easily controlled after laser irradiation.
[0068] The adhesive layer is preferably one or a combination of two or more selected from polyacrylate, polymethacrylate, epoxy, polystyrene, polyurethane, polysulfone, polyester, polyimide and silicone resin.
[0069] Among them, silicone adhesives are preferred because they have excellent heat resistance and contamination resistance. Silicone adhesives are particularly suitable materials because they have excellent thermal stability and are less likely to migrate from the adhesive layer to the semiconductor element. Examples of silicone adhesives include platinum addition curing types and condensation curing types that are mainly composed of MQ resin and high viscosity vinyl siloxane, but platinum addition curing types that cure quickly after being applied to the surface of the light-to-heat conversion layer are preferred.
[0070] The silicone adhesive can be diluted with a solvent such as toluene and applied to the light-to-heat conversion layer to a thickness of 1 to 10 μm using a film coater or applicator, followed by drying the solvent and curing the adhesive.
[0071] The transfer body transferred from the laser photothermal transfer film is not particularly limited as long as it has a solid shape, such as a semiconductor element, a light emitting element such as an LED, a ceramic substrate, a plastic or ceramic package containing a semiconductor element or an LED element, a ceramic substrate or resin sheet containing a phosphor, a laminated capacitor, etc. In particular, a display device using an LED can be created by transferring a micro LED or a mini LED to a transfer substrate that serves as a display substrate having a solder bump or an anisotropic conductive layer.
[0072] <Transcribing process> FIG. 2 shows an example of a mounting flow for transferring an element using the laser photothermal transfer film 1 of the present invention. The laser photothermal transfer film 1 has an adhesive release layer 14 laminated on a base film 11, and the adhesive release layer 14 is formed by laminating a photothermal conversion layer 12 and an adhesive layer 13 in this order from the side of the base film 11. On the other hand, on one surface of a transfer substrate 15, solder 16 is provided by printing or the like in the area where the element is to be transferred. After attaching an element 17 to the adhesive layer surface of the adhesive release layer 14 of the laser photothermal transfer film 1, the element 17 and the solder 16 are placed facing each other, the distance (gap 18) between the laser photothermal transfer film 1 and the transfer substrate 15 are set, and the film is set in a laser irradiation device. A laser is then irradiated from the base film 11 side to cause expansion 19 of the photothermal conversion layer. At this time, the photothermal conversion layer 12 pushes up the adhesive layer 13 above it and rises, and the element 17 is transferred to the solder 16 on the transfer substrate 15. EXAMPLES
[0073] The configuration and the effects of the present invention will be described in more detail below with reference to examples and comparative examples. Note that these examples are provided to more specifically explain the present invention, and the scope of the present invention is not limited to these examples.
[0074] The physical properties of the bismaleimide resins used in the examples and comparative examples are shown in Table 1.
[0075] [Table 1]
[0076] <Example 1> (1) Base film: An optical PET film manufactured by Toray Industries, Inc. was used as the base film (thickness: 100 μm). (2) Composition for photothermal conversion layer: A composition for photothermal conversion layer (coating composition) was prepared by dissolving a diimonium-series dye (manufactured by Nippon Kayaku, KAYASORB IRG-069), a bismaleimide resin (SLK3000), and a peroxide (dicumyl peroxide) as a curing catalyst in the amounts shown in Table 2 in anisole. (3) Adhesive: The adhesive layer for attaching the transfer body was prepared by mixing KR-3704 (manufactured by Shin-Etsu Chemical) and X-40-3237-1 (manufactured by Shin-Etsu Chemical) in a mass ratio of 75:25, to which was further added 0.5% of CAT PL-50T (manufactured by Shin-Etsu Chemical) to prepare an adhesive with a solid content of 35 mass%.
[0077] <Production of laser photothermal transfer film> The photothermal conversion layer composition was applied onto the substrate film using a Mayer bar, and dried and cured at 150°C for 2 hours to form a photothermal conversion layer with an average thickness of 2.5 μm. Next, an adhesive was applied using an applicator, and then dried at 100°C for 3 minutes to form an adhesive layer with an average thickness of 3 μm (adhesive strength of 0.3 N / 25 mm in a 180° peel test (adherend SUS) in accordance with JIS Z 0237), to produce a laser photothermal transfer film (Figure 1), and the transfer characteristics were evaluated by the method described below. The results are shown in Table 3.
[0078] <Example 2> A composition for a light-heat conversion layer was prepared by changing the amount of diimmonium salt and dissolving the amount of peroxide (dicumyl peroxide) as a curing catalyst in anisole as shown in Table 2. A laser light-heat transfer film was produced in the same manner as in Example 1 and the transfer characteristics were evaluated. The results are shown in Table 3.
[0079] <Example 3> A composition for a light-heat conversion layer was prepared by changing the amount of diimmonium salt and dissolving the amount of peroxide (dicumyl peroxide) as a curing catalyst in anisole as shown in Table 2. A laser light-heat transfer film was produced in the same manner as in Example 1 and the transfer characteristics were evaluated. The results are shown in Table 3.
[0080] <Example 4> The bismaleimide resin was changed to SLK689 and SLK2600, and peroxide (dicumyl peroxide) was dissolved in anisole in the amount shown in Table 2 as a curing catalyst to prepare a composition for a light-heat conversion layer. A laser light-heat transfer film was produced in the same manner as in Example 1, and the transfer characteristics were evaluated. The results are shown in Table 3.
[0081] <Example 5> The amount of diimonium salt was changed, and peroxide (dicumyl peroxide) was not added, but the amount shown in Table 2 was dissolved in anisole to prepare a composition for a light-heat conversion layer. A laser light-heat transfer film was produced in the same manner as in Example 1, and the transfer characteristics were evaluated. The results are shown in Table 3.
[0082] <Example 6> A composition for a light-heat conversion layer was prepared by changing the amount of diimmonium salt and dissolving the amount of peroxide (dicumyl peroxide) as a curing catalyst in anisole as shown in Table 2. A laser light-heat transfer film was produced in the same manner as in Example 1 and the transfer characteristics were evaluated. The results are shown in Table 3.
[0083] <Example 7> A composition for a light-heat conversion layer was prepared by changing the amount of diimmonium salt and dissolving the amount of peroxide (dicumyl peroxide) as a curing catalyst in anisole as shown in Table 2. A laser light-heat transfer film was produced in the same manner as in Example 1 and the transfer characteristics were evaluated. The results are shown in Table 3.
[0084] <Comparative Example 1> The bismaleimide resin was replaced with a polyimide resin, and the amount shown in Table 2 was dissolved in NMP to prepare a composition for a light-heat conversion layer. A laser light-heat transfer film was produced in the same manner as in Example 1, and the transfer characteristics were evaluated. The results are shown in Table 3.
[0085] <Evaluation of transfer characteristics> A transfer substrate was prepared by applying 20 μm of solder paste by screen printing to a predetermined electrode on a PCB substrate. On the other hand, 100 optical semiconductor elements (500 μm square) for evaluation were attached to the laser photothermal transfer film consisting of three layers of a substrate, a photothermal conversion layer, and an adhesive layer prepared in the above examples and comparative examples, and then the distance between the laser photothermal transfer film and the transfer substrate was set to 150 μm and set in a laser irradiation device. A laser beam was irradiated from the substrate side of the laser photothermal transfer film with an energy of 100 W using a Nd:YAG 1064 nm laser device, and the optical semiconductor elements were transferred onto the solder paste of the transfer substrate due to the expansion of the photothermal conversion layer. The number of optical semiconductor elements transferred onto the transfer substrate was measured to evaluate the transfer characteristics.
[0086] <Example 8> The expansion of the laser photothermal transfer film of Example 1 after being irradiated with a laser was photographed using a Keyence VHX digital microscope. The photograph is shown in FIG. In the present invention, the light-to-heat conversion layer contains a specific bismaleimide resin, which allows for such a high protuberance to be obtained. When the expansion after laser irradiation was measured in 3D, the height was 200 μm.
[0087] [Table 2]
[0088] [Table 3]
[0089] The laser photothermal transfer films of Examples 1 to 7, which used a bismaleimide resin as the resin contained in the composition for the photothermal conversion layer, had better transfer properties than the laser photothermal transfer film of Comparative Example 1, which used a polyimide resin. Therefore, using a bismaleimide resin with a large expansion coefficient as the binder for the photothermal conversion layer is useful for providing a laser photothermal transfer film with improved transfer properties. [Explanation of symbols]
[0090] 1...Laser photothermal transfer film, 11...Base film, 12...Photothermal conversion layer, 13...Adhesive layer, 14...Adhesive release layer, 15...Transfer substrate, 16...Solder, 17...Element, 18...Gap, 19...Expansion of photothermal conversion layer
Claims
1. A laser photothermal transfer film having three layers laminated in this order: a base film, a photothermal conversion layer, and an adhesive layer, wherein the photothermal conversion layer is a solid at room temperature that contains an infrared light absorber represented by general formula (1) and a bismaleimide resin represented by the following general formula (3) and / or general formula (4): 【Chemistry 1】 (In the general formula (1), p is 1 or 2, and R 1 From R 8 are each independently a substituted or unsubstituted linear or branched alkyl group having 1 to 10 carbon atoms, which may be substituted with a cyano group, a nitro group, a carboxyl group, a sulfone group, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, an alkoxyalkoxy group, an acyloxy group or an alkylamino group; X - is a fluoroalkyl phosphate anion represented by the following general formula (2): 【Chemistry 2】 (In the general formula (2), x is 0 or 1, y is 1, 2 or 3, z is 6-y, and R 9 From R 13 are each independently hydrogen or fluorine. 【Chemistry 3】 (In general formula (3), A represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. Q represents a linear alkylene group having 6 or more carbon atoms. R each independently represents a linear or branched alkyl group having 6 or more carbon atoms. n represents an integer of 1 to 10.) 【Chemistry 4】 (In general formula (4), A' represents a tetravalent organic group containing an aromatic ring or an aliphatic ring. B represents an alkylene chain having 6 to 18 carbon atoms and having an aliphatic ring which may contain a divalent heteroatom. Q' represents a linear alkylene group having 6 or more carbon atoms. Each R' independently represents a linear or branched alkyl group having 6 or more carbon atoms. n' represents an integer from 1 to 10. m represents an integer from 1 to 10.)
2. 2. The laser photothermal transfer film according to claim 1, wherein the adhesive constituting the adhesive layer is one or a combination of two or more selected from polyacrylate, polymethacrylate, epoxy, polystyrene, polyurethane, polysulfone, polyester, polyimide, and silicone resin.
3. 3. The laser photothermal transfer film according to claim 1, wherein the content of the infrared light absorber in the photothermal conversion layer is 1 to 15% by mass, and the content of the bismaleimide resin is 85 to 99% by mass.
4. 4. The laser photothermal transfer film according to claim 1, wherein the adhesive layer has a thickness of 1 to 10 μm.
5. 5. The laser photothermal transfer film according to claim 1, wherein the light-to-heat conversion layer has a thickness of 0.1 to 20 μm.
6. 6. The laser light thermal transfer film according to claim 1, wherein the infrared ray absorbent has a maximum absorption wavelength within a range of 780 to 1500 nm.
7. 7. The laser photothermal transfer film according to claim 1, wherein the adhesive layer has an adhesive strength of 0.1 to 10 N / 25 mm.
8. 8. The laser light thermal transfer film according to claim 1, wherein the base film is made of a transparent thermoplastic resin.
9. 9. The laser photothermal transfer film according to claim 1, wherein the cured product of the bismaleimide resin has a thermal decomposition onset temperature of 300° C. or higher, a glass transition temperature of 150° C. or lower, and a thermal expansion coefficient at or above the glass transition temperature of 100 ppm / ° C. or higher.
Citation Information
Patent Citations
Thermal transfer sheet
JP2001301345A
Resin composition for laser engraving, relief printing plate precursor for laser engraving and method for manufacturing the same, and method for making the relief printing plate
JP2012121300A
Selective transfer of separated parts facilitated by laser.
JP2014515883A
Method of parallelly assembling discrete components on substrate
JP2020188261A
KR2007-0067725