Shape-memory resin, skin beauty product, method for manufacturing skin care equipment, and method for manufacturing skin beauty product

A shape memory resin with specific compositions addresses the limitations of existing face masks by providing temperature-responsive properties and integration with cosmetic ingredients, ensuring flexible and stable deformation for skin applications.

JP7558937B2Active Publication Date: 2024-10-01SHISEIDO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021525981
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-14
Filing Date
2020-05-27
Publication Date
2024-10-01
Estimated Expiration
2040-05-27

AI Technical Summary

Technical Problem

Existing face masks using shape memory resin require a water-containing material for cosmetic retention, which limits application flexibility and integration with shape memory materials, and lack specific compositions for integral deformation.

Method used

A shape memory resin composed of 64 mol% to 85 mol% N-alkylacrylamide, 14 mol% to 35 mol% acrylic acid ester, and 0.01 mol% to 6 mol% crosslinking agent, combined with a polymerization process to create a skin beauty product or device that can be applied integrally with cosmetic ingredients.

Benefits of technology

The resin exhibits temperature-responsive shape memory properties, high strength, stability, biocompatibility, and transparency, allowing for flexible application and integration with cosmetic components, enhancing skin deformation and product usability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558937000001
    Figure 0007558937000001
  • Figure 0007558937000002
    Figure 0007558937000002
  • Figure 0007558937000003
    Figure 0007558937000003
Patent Text Reader

Abstract

A resin having shape-memory properties which includes a polymer comprising 64-85 mol% N-alkylacrylamide component, 14-35 mol% acrylic ester component, and 0.01-6 mol% crosslinking component.
Need to check novelty before this filing date? Find Prior Art

Description

Related Applications

[0001] The present invention is based on the priority claim of Japanese Patent Application No. 2019-111534 (filed June 14, 2019), the entire contents of which are incorporated herein by reference. [Technical field]

[0002] The present disclosure relates to a resin having shape memory.The present disclosure relates to an external skin device comprising the resin.The present disclosure relates to a method for producing the external skin device. [Background technology]

[0003] Face masks using shape-memory resins are known (for example, Patent Documents 1 and 2).

[0004] The face mask described in Patent Document 1 includes a film formed from a shape-memory resin. Patent Document 1 also discloses that a fabric impregnated with a lotion or the like is laminated on one side of the face mask.

[0005] The face mask sheet described in Patent Document 2 is a face mask sheet formed to cover the face in close contact with the skin, and has a shape-memory material that contracts in response to body temperature provided at least in the area corresponding to the relaxed part of the skin, so that the shape-memory material contracts in the direction of skin relaxation. Patent Document 2 also discloses that the shape-memory material is laminated on a water-absorbent sheet material, and the water-absorbent sheet material is impregnated with a cosmetic liquid. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-160833 A [Patent Document 2] JP 2007-143586 A Summary of the Invention [Problem to be solved by the invention]

[0007] The face masks described in Patent Documents 1 and 2 require a water-retaining material to retain cosmetic liquid, etc. However, it is desirable to be able to select the use of a water-retaining material depending on the purpose and application without necessarily requiring a water-retaining material.

[0008] In addition, in the face masks described in Patent Documents 1 and 2, a water-containing material is laminated on a shape-memory resin. However, in such a laminated structure, the shape-memory resin and the water-containing material cannot be deformed integrally. For example, when the shape-memory resin shrinks, it is difficult for the water-containing material to shrink in response to the shape-memory resin. In such a case, for example, the water-containing material will be twisted.

[0009] Neither Patent Document 1 nor Patent Document 2 discloses a specific composition of the shape-memory material that can be used for face masks.

[0010] Thus, there is a need for shape-memory resins that can be applied to the skin, particularly shape-memory resins that can be applied integrally with water-containing materials. There is also a need for external skin devices that use such shape-memory resins for cosmetic and / or beauty purposes, as well as methods of using and manufacturing the same. [Means for solving the problem]

[0011] According to a first aspect of the present disclosure, there is provided a polymer comprising 64 mol % to 85 mol % of an N-alkylacrylamide component, 14 mol % to 35 mol % of an acrylic acid ester component having a structure shown in Chemical Formula 1 below, and 0.01 mol % to 6 mol % of a crosslinking component. and polyethylene glycol A shape memory resin is provided, comprising: According to a second aspect of the present disclosure, there is provided a skin cosmetic product comprising a support and a shape-memory resin impregnated into the support. The shape-memory resin comprises a polymer containing 64 mol% to 85 mol% of an N-alkylacrylamide component, 14 mol% to 35 mol% of an acrylic acid ester component having the structure shown in Chemical Formula 1 below, and 01 mol% to 6 mol% of a crosslinking component, and the skin cosmetic product comprises a beauty ingredient and / or a cosmetic ingredient.

[0012] In the chemical formula shown in Chemical Formula 1, R 1 R is a hydrogen atom or an alkyl group, an alkenyl group, or an acyl group having 1 to 4 carbon atoms. 2is an alkyl group, an alkenyl group, or an acyl group having 10 to 20 carbon atoms.

[0013] [ka]

[0014] The present disclosure 3 According to the viewpoint, A method for producing a skin beauty product, comprising the steps of: preparing a mixture of 64 mol% to 85 mol% of N-alkylacrylamide, 14 mol% to 35 mol% of an acrylic acid ester having the structure shown in Chemical Formula 2 below, and 0.01 mol% to 6 mol% of a crosslinking agent, and a polymerization initiator; placing the mixture and a support in a mold; polymerizing the mixture while the support is impregnated with the mixture to produce a polymer; heating the polymer to a temperature equal to or higher than the glass transition temperature to expand it; cooling the polymer while it is expanded to produce a skin beauty product; and impregnating the skin beauty product with a beauty ingredient and / or a cosmetic ingredient. is provided.

[0015] The present disclosure 4 According to the aspect, the present invention relates to a monomer including 64 mol% to 85 mol% of N-alkylacrylamide, 14 mol% to 35 mol% of an acrylic acid ester having a structure shown in Chemical Formula 2 below, and 0.01 mol% to 6 mol% of a crosslinking agent, a polymerization initiator, Polyethylene glycol, The method for producing an external skin device includes the steps of: preparing a mixture by mixing the above-mentioned components; polymerizing the mixture to prepare a polymer; heating the polymer to a temperature equal to or higher than its glass transition temperature to expand it; and cooling the polymer in an expanded state.

[0016] In the chemical formula shown in Chemical Formula 2, R 3 R is a hydrogen atom or an alkyl group, an alkenyl group, or an acyl group having 1 to 4 carbon atoms. 4 is an alkyl group, an alkenyl group, or an acyl group having 10 to 20 carbon atoms.

[0017] [ka] Effect of the Invention

[0018] The shape-memory resin of the present disclosure has a temperature-responsive (temperature-dependent) shape memory property. For example, the shape-memory resin of the present disclosure can be induced to change to its original shape by human body temperature.

[0019] The shape-memory resin of the present disclosure has high strength. This allows the shape-memory resin of the present disclosure to be formed thinly. For example, the shape-memory resin can be molded into a film.

[0020] The shape-memory resin of the present disclosure has high stability over time in a shape-memory state.

[0021] The shape-memory resin of the present disclosure has biocompatibility, which allows the shape-memory resin of the present disclosure to be applied to the skin.

[0022] The shape-memory resin of the present disclosure can have high transparency. This allows the shape-memory resin of the present disclosure to be applied to many applications. For example, the shape-memory resin can be inconspicuous even when applied to the human body.

[0023] The topical device of the present disclosure can be applied to stretch the skin.

[0024] According to the method for producing an external skin device of the present disclosure, it is possible to produce the external skin device according to the second aspect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Preferred embodiments of each of the above aspects are described below.

[0026] According to a preferred embodiment of the first aspect, the N-alkylacrylamide component includes an N,N-dimethylacrylamide component.

[0027] According to a preferred embodiment of the first aspect, the acrylic ester component includes at least one of a stearyl acrylate component, a lauryl acrylate component, a 2-ethylhexyl acrylate component, and a butyl acrylate component.

[0028] According to a preferred embodiment of the first aspect, the acrylic ester component contains 40 mol % to 100 mol % of a stearyl acrylate component and 0 mol % to 60 mol % of a lauryl acrylate component, based on the total amount of the acrylic ester component.

[0029] According to a preferred embodiment of said first aspect, the cross-linking moiety comprises an N,N'-methylenebisacrylamide moiety.

[0030] According to a preferred embodiment of the first aspect, the polymer has a Young's modulus of 1 MPa or less.

[0031] According to a preferred embodiment of the first aspect, the average strain of the polymer is 500% or more.

[0032] According to a preferred embodiment of the first aspect, the shape-memory resin further contains polyethylene glycol.

[0033] According to a preferred embodiment of the first aspect, the content of polyethylene glycol is 0.1% by mass to 1% by mass with respect to the mass of the shape-memory resin.

[0034] According to a preferred embodiment of the first aspect, the water content of the shape-memory resin is 2% by mass to 40% by mass with respect to the mass of the shape-memory resin.

[0035] According to a preferred embodiment of the first aspect, the shape-memory resin has temperature-responsive shape memory.

[0036] According to a preferred embodiment of the first aspect, the shape-memory resin has flexibility.

[0037] According to a preferred embodiment of the second aspect, the external skin device further comprises a support, the support being impregnated with and / or coated with the shape-memory resin.

[0038] According to a preferred embodiment of the second aspect, the support has stretchability.

[0039] According to a preferred embodiment of the second aspect, the support is at least one of a nonwoven fabric, a woven fabric, a knitted fabric, a tuft, a felt, a fulled fabric, a paper, and a water-retaining material.

[0040] According to a preferred embodiment of the second aspect, the external skin device has a sheet shape.

[0041] According to a preferred embodiment of the second aspect, the external skin equipment has a shape that conforms to the surface shape of the skin.

[0042] According to a preferred embodiment of the second aspect, the external skin care device has a shape that fits along at least a part of the face.

[0043] According to a preferred embodiment of the second aspect, the external skin care device is at least one of a beauty product, a cosmetic product, and a medical product.

[0044] According to a preferred embodiment of the second aspect, the external skin device further comprises an external skin preparation.

[0045] According to a preferred embodiment of the third aspect, the method for producing an external dermatological device further comprises the step of placing the mixture in a mold before producing the polymer.

[0046] According to a preferred embodiment of the third aspect, the method for producing an external skin device further comprises the step of placing a support in a mold, in which the support is impregnated and / or coated with the mixture to produce a polymer.

[0047] According to a preferred embodiment of the third aspect, the support has stretchability.

[0048] According to a preferred embodiment of the third aspect, the support is at least one of a nonwoven fabric, a woven fabric, a knitted fabric, a tuft, a felt, a fulled fabric, a paper, and a water-retaining material.

[0049] According to a preferred embodiment of the third aspect, the mold has a shape of a part of a face.

[0050] According to a preferred embodiment of the third aspect, a release sheet is interposed between the mixture and the mold.

[0051] According to a preferred embodiment of the third aspect, the release sheet is a polytetrafluoroethylene sheet.

[0052] According to a preferred embodiment of the third aspect, the external skin device is formed in a sheet shape.

[0053] According to a preferred embodiment of the third aspect, the acrylic ester includes at least one of stearyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, and butyl acrylate.

[0054] According to a preferred embodiment of the third aspect, the acrylic ester contains 40 mol % to 100 mol % of stearyl acrylate and 0 mol % to 60 mol % of lauryl acrylate, based on the total amount of the acrylic ester.

[0055] According to a preferred embodiment of the third aspect, the N-alkylacrylamide includes N,N-dimethylacrylamide.

[0056] According to a preferred embodiment of the third aspect, the crosslinking agent includes N,N'-methylenebisacrylamide.

[0057] The shape-memory resin according to the first embodiment of the present disclosure will be described below. In the following description, the polymer will be described in terms of monomer unit.

[0058] The shape memory resin of the present disclosure comprises a polymer that includes an N-alkylacrylamide component, an acrylic ester component, and a crosslinking component.

[0059] [N-alkylacrylamide component] An example of the N-alkylacrylamide component is an N,N-dimethylacrylamide component. The N,N-dimethylacrylamide component may be 90 mol % or more, 95 mol % or more, or 100 mol % based on the total amount of the N-alkylacrylamide components.

[0060] The N-alkylacrylamide component is preferably 64 mol% or more, more preferably 70 mol% or more, based on the total amount of the components in the polymer. If the N-alkylacrylamide component is less than 64 mol%, the shape memory property is reduced. If the N-alkylacrylamide component is less than 85 mol%, more preferably 80 mol% or less, based on the total amount of the components in the polymer. If the N-alkylacrylamide component is more than 85 mol%, the shape memory property is reduced.

[0061] [Acrylic ester component] The acrylic ester component is the below described transformation 3 The compound may have the structure shown in 3 In the chemical formula shown in 1 R is a hydrogen atom or an alkyl group, an alkenyl group, or an acyl group having 1 to 4 carbon atoms. 2 is an alkyl group, an alkenyl group, or an acyl group having 10 to 20 carbon atoms.

[0062] [ka]

[0063] The acrylic acid ester component may be, for example, at least one of a stearyl acrylate component, a lauryl acrylate component, a 2-ethylhexyl acrylate component, and a butyl acrylate component. The total amount of the stearyl acrylate component, the lauryl acrylate component, the 2-ethylhexyl acrylate component, and the butyl acrylate component may be 90 mol% or more, 95 mol% or more, or 100 mol% based on the total amount of the acrylic acid ester components.

[0064] For example, the acrylic acid ester component may include a stearyl acrylate component and a lauryl acrylate component. In this case, the stearyl acrylate component may be, for example, 40 mol% or more, 50 mol% or more, 60 mol% or more, or 65 mol% or more based on the total amount of the acrylic acid ester components. The stearyl acrylate component may be, for example, 100 mol% or more based on the total amount of the acrylic acid ester components. % Below, 95mol % The amount of the lauryl acrylate component can be, for example, 5 mol % or more, 15 mol % or more, or 25 mol % or more, based on the total amount of the acrylic ester components. The amount of the lauryl acrylate component can be, for example, 60 mol % or more, based on the total amount of the acrylic ester components. % It can be 50 mol % or less, or 40 mol % or less. The stearyl acrylate component has the effect of increasing the glass transition temperature (Tg). The lauryl acrylate component has the effect of decreasing the glass transition temperature. By mixing the stearyl acrylate component and the lauryl acrylate component, the shrinkage temperature at which the shape is restored can be adjusted.

[0065] When the acrylic ester component contains a stearyl acrylate component and a lauryl acrylate component, the molar ratio of the stearyl acrylate component to the lauryl acrylate component may be 1 mol or more, 1.5 mol or more, or 2 mol or more of the stearyl acrylate component per 1 mol of the lauryl acrylate component, and 4 mol or less, 3.5 mol or less, or 3 mol or less of the stearyl acrylate component per 1 mol of the lauryl acrylate component.

[0066] The acrylic acid ester component is preferably 14 mol% or more, more preferably 20 mol% or more, based on the total amount of the components in the polymer. If the acrylic acid ester component is less than 14 mol%, the shape memory property is reduced. If the acrylic acid ester component is less than 35 mol% or less, more preferably 30 mol% or less, based on the total amount of the components in the polymer. If the acrylic acid ester component is more than 35 mol%, the shape memory property is reduced.

[0067] [Crosslinking component] The cross-linking moiety can include, for example, an N,N'-methylenebisacrylamide moiety.

[0068] The crosslinking component can be 0.01 mol% or more, 0.03 mol% or more, 0.05 mol% or more, 0.1 mol% or more, 0.3 mol% or more, 0.7 mol% or more, 1 mol% or more, 1.5 mol% or more, 2 mol% or more, 2.5 mol% or more, 3 mol% or more, 3.5 mol% or more, or 4 mol% or more, based on the total amount of the components in the polymer. The crosslinking component can be 6 mol% or less, 5 mol% or less, 4 mol% or less, 3 mol% or less, 2 mol% or less, 1 mol% or less, 0.8 mol% or less, 0.5 mol% or less, 0.2 mol% or less, 0.1 mol% or less, or 0.08 mol% or less, based on the total amount of the components in the polymer. The average strain, Young's modulus, and tensile strength can be adjusted by the content of the crosslinking component. In addition, by reducing the crosslinking component, the stability over time at room temperature in the shape memory state can be increased.

[0069] [Polymerization initiator] The shape-memory resin of the present disclosure may further include a polymerization initiator. Examples of the polymerization initiator include at least one of benzophenone, 2,2'-azobis(isobutyronitrate) component, 2,2'-azobis(2-methylpropionamydine) dihydrochloride component, 4,4'-azobis(4-cyanovaleric acid) component, and 2,2'-azobis(dimethylisobutyrate) component.

[0070] The polymerization initiator may be 0.02 mol % or more, or 0.05 mol % or more, based on the total amount of each component in the shape-memory resin. The polymerization initiator may be 0.2 mol % or less, or 0.15 mol % or less, based on the total amount of each component in the shape-memory resin.

[0071] [Water-containing] The shape-memory resin of the present disclosure may further contain water. The water content may be, for example, 2% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, 20% by mass or more, or 30% by mass or more, based on the mass of the shape-memory resin. The water content may be, for example, 40% by mass or less, 30% by mass or less, 20% by mass or less, 10% by mass or less, 8% by mass or less, or 7% by mass or less, based on the mass of the shape-memory resin.

[0072] [others] The shape-memory resin of the present disclosure may be conveniently blended with various additives such as skin external preparations, antioxidants, heat stabilizers, lubricants, antistatic agents, plasticizers, pigments, etc., depending on the application and molding purpose. In addition, these additive components may be blended in any of the polymerization reaction process and the processing and molding process. In the case of a shape-memory resin to be applied to the skin, the shape-memory resin may contain at least one of the following skin external preparations: moisturizers, film-forming agents, UV absorbers, amino acids, pH adjusters, skin nutrients, vitamins, fragrances, etc. The shape-memory resin of the present disclosure may contain the skin external preparation in the form of an aqueous solution.

[0073] The shape-memory resin of the present disclosure may contain alcohol. Examples of the alcohol include lower alcohols and polyhydric alcohols. Examples of the polyhydric alcohol include polyethylene glycol. The content of polyethylene glycol may be, for example, 0.001 mol% or more, or 0.002 mol% or more, based on the total amount of the monomers of the shape-memory resin. The content of polyethylene glycol may be, for example, 0.004 mol% or less, or 0.003 mol% or less, based on the total amount of the monomers of the shape-memory resin.

[0074] The shape-memory resin of the present disclosure may have, for example, a sheet shape. The shape-memory resin of the present disclosure may have a thickness according to the application and purpose. The shape-memory resin of the present disclosure may have, for example, a thickness of 0.8 mm or more, 1 mm or more, 1.5 mm or more, 2 mm or more, 2.5 mm or more, or 3 mm or more. The shape-memory resin of the present disclosure may have, for example, a thickness of 4 mm or less, 3.5 mm or less, 3 mm or less, 2.5 mm or less, 2 mm or less, or 1.5 mm or less. The shape-memory resin of the present disclosure may have a shape that follows the surface of the skin, for example, a shape that follows at least a part of the face.

[0075] [Physical properties / characteristics] The shape-memory resin of the present disclosure can have the following physical properties or characteristics.

[0076] The shape memory resin of the present disclosure can be transparent or translucent.

[0077] The shape-memory resin of the present disclosure has a shape-memory strength of 50% or more, 80% or more, 100% or more, 150% or more, 200% or more, 300% or more, 400% or more, 500% or more, or 600% or more. %The shape-memory resin of the present disclosure may have an average strain at break of 1000% or less, 900% or less, 800% or less, 700% or less, 600% or less, 500% or less, 400% or less, 300% or less, 200% or less, or 150% or less. The average strain at break may be measured in accordance with JISK6251. The average strain may be adjusted by the amount of crosslinking agent added. By increasing the average strain, the shrinkage effect due to shape recovery may be increased.

[0078] The shape-memory resin of the present disclosure may have a Young's modulus of 0.01 MPa or more, 0.1 MPa or more, 1 MPa or more, 2 MPa or more, 5 MPa or more, or 10 MPa or more. The shape-memory resin of the present disclosure may have a Young's modulus of 20 MPa or less, 10 MPa or less, 5 MPa or less, 1 MPa or less, 0.5 MPa or less, or 0.1 MPa or less. The Young's modulus can be measured in accordance with JIS K6251. The Young's modulus can be adjusted by the amount of crosslinking agent added. By increasing the Young's modulus, the contraction force during shape recovery can be increased.

[0079] The shape-memory resin of the present disclosure may have a tensile strength at break of 0.5 MPa or more, 1 MPa or more, 2 MPa or more, 3 MPa or more, 5 MPa or more, or 7 MPa or more. The shape-memory resin of the present disclosure may have a tensile strength at break of 15 MPa or less, 10 MPa or less, 8 MPa or less, 5 MPa or less, or 3 MPa or less. The tensile strength at break can be measured in accordance with JIS K6251.

[0080] The shape-memory resin of the present disclosure has an endothermic peak at 28°C to 48°C.

[0081] [Shape memory] The shape-memory properties of the shape-memory resin of the present disclosure and a method for using the shape-memory resin of the present disclosure (a method for expressing the shape-memory properties) will be described.

[0082] The shape-memory resin of the present disclosure has shape-memory properties. In particular, the resin composition of the present disclosure has temperature-responsive (temperature-dependent) shape-memory properties. For example, the shape-memory resin of the present disclosure can be induced to change to its original shape by human body temperature.

[0083] First, a shape-memory resin having a sheet shape is heated to a temperature at which it can be deformed. For example, the shape-memory resin is heated to a temperature equal to or higher than the glass transition temperature and equal to or lower than the melting point. The heating temperature is preferably, for example, 50° C. or higher. The heating temperature is preferably 70° C. or lower.

[0084] Next, the softened shape-memory resin is stretched to a degree that does not break. The shape-memory resin can be stretched, for example, 1.2 times or more, 1.5 times or more, 2 times or more, 3 times or more, or 5 times or more in one direction relative to its original length. In addition, the degree to which the shape-memory resin is stretched is preferably, for example, 10 times or less in one direction relative to its original length.

[0085] The extension direction is not limited to a uniaxial direction. For example, the shape-memory resin can be expanded in a planar direction (biaxial direction). When expanding the shape-memory resin in a planar direction, the resin can be expanded 1.5 times or more, 2 times or more, 3 times or more, or 5 times or more of its original area. In addition, the degree of expansion of the shape-memory resin is preferably, for example, 10 times or less of its original area.

[0086] Next, the shape-memory resin is cooled in the stretched or expanded state. For example, the shape-memory resin is cooled to 10°C or less, preferably 5°C or less or 0°C or less. As a result, the shape-memory resin is molded in the stretched or expanded state, and the original shape is memorized. Once the shape-memory resin is fixed in the stretched or expanded state, it is returned to room temperature (preferably 25°C or less).

[0087] In order to develop shape memory properties, the shape memory resin is heated. For example, it is preferable to heat the shape memory resin to 30°C or higher. The heating temperature is 45°C or lower, preferably 40°C or lower. For example, the shape memory resin can be heated by human body temperature. This causes the shape memory resin to shrink to its original shape. For example, the shape memory resin can shrink 20% to 30% in the elongated axial direction relative to the length before shrinkage. Also, the shape memory resin can shrink 20% to 60% relative to the area before shrinkage.

[0088] The shape-memory resin of the present disclosure can be a shape-memory resin that exhibits the following shape-memory properties. The shape-memory resin can have the above composition and / or be produced by the production method described below.

[0089] A sheet of shape-memory resin with a length of 20 mm, a width of 10 mm, and a thickness of 1 mm is prepared (first step). After the first step, the sheet is heated to 50°C to 70°C to soften the shape-memory resin (second step). In the softened state in the second step, the sheet is stretched in the length direction to 1.5 times its original length (third step). In the stretched state in the third step, the sheet is cooled to 0°C (fourth step). After the fourth step, the sheet is left to stand at room temperature of 25°C or less (fifth step). After standing, the sheet has a length of 26 mm or more. After the fifth step, the sheet is heated to 32°C to 45°C (sixth step). In the sixth step, the sheet shrinks. After shrinkage, the sheet can have a length of 24 mm or less.

[0090] The length of the shape-memory resin after restoration (shrinkage) is preferably 130% or less, more preferably 120% or less, and even more preferably 110% or less, of the original length before elongation.

[0091] According to the shape-memory resin of the present disclosure, the resin can memorize a shape. The shape can be restored by heating. In particular, the shape can be restored by human body temperature. As a result, the shape-memory resin of the present disclosure can be deformed by applying it to human skin.

[0092] The shape-memory resin of the present disclosure has a high shape-memory property that allows it to retain its shape-memorized state, and therefore it can be stored in the shape-memorized state (elongated state before deformation) for a long period of time.

[0093] The shape-memory resin of the present disclosure has water-absorbing properties, which allows the shape-memory resin of the present disclosure to retain external components for skin, such as cosmetic components.

[0094] The shape-memory resin of the present disclosure can be applied to, for example, beauty products, cosmetic products, medical products (treatment products), clothing products, shoe products, etc. The shape-memory resin of the present disclosure can be applied to, for example, masks.

[0095] A method for producing the shape-memory resin of the present disclosure will be described.

[0096] The shape-memory resin of the present disclosure can be produced by mixing monomers including N-alkylacrylamide, an acrylic acid ester, and a crosslinking agent with a polymerization initiator, and polymerizing the monomers.

[0097] The N-alkylacrylamide can be, for example, N,N-dimethylacrylamide.

[0098] The acrylic ester is, for example, 4 The compound may have the structure shown in 4 In the chemical formula shown in 3 is hydrogen or an alkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms; R 4 is an alkyl group, an alkenyl group, or an acyl group having 10 to 20 carbon atoms.

[0099] The acrylic ester may be at least one of stearyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, and butyl acrylate. In particular, the acrylic ester may be stearyl acrylate and / or lauryl acrylate.

[0100] [ka]

[0101] The crosslinking agent may be, for example, at least one of N,N'-methylenebisacrylamide, N,N'-methylenebisacrylamide, 2,2'-azobis(isobutyronitrate), 2,2'-azobis(2-methylpropionamydine) dihydrochloride, 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis(dimethylisobutyrate).

[0102] The polymerization initiator may be, for example, at least one of benzophenone, a 2,2'-azobis(isobutyronitrate) component, a 2,2'-azobis(2-methylpropionamydine) dihydrochloride component, a 4,4'-azobis(4-cyanovaleric acid) component, and a 2,2'-azobis(dimethylisobutyrate) component.

[0103] The proportions of the monomer and polymerization initiator added can be the same as the proportions of the respective components described in the first embodiment.

[0104] The shape-memory resin of the present disclosure can be produced by polymerizing the above-mentioned monomers by a known method.

[0105] The shape-memory resin can be formed into a sheet by a known method.

[0106] An external skin device according to a second embodiment of the present disclosure will now be described.

[0107] The external skin device of the present disclosure comprises the shape-memory resin according to the first embodiment.

[0108] The external skin device of the present disclosure may further include a support that supports the shape-memory resin. The support may also function as a carrier for supporting the shape-memory resin.

[0109] The support may have at least one of the following properties: porous, hydroscopic, stretchable, and flexible.

[0110] The support may be, for example, at least one of a nonwoven fabric, a woven fabric, a knitted fabric, a tufted fabric, a felt, a fulled fabric, a paper, and a water-containing material.

[0111] The support may have, for example, a sheet shape. The support may have, for example, a shape that conforms to the skin surface. The support may have, for example, a shape that conforms to at least a part of the face.

[0112] The support can have a thickness of, for example, 0.5 μm or more, 1 μm or more, 5 μm or more, 10 μm or more, 20 μm or more, 50 μm or more, 100 μm or more, 200 μm or more, 500 μm or more, 1 mm or more, or 2 mm or more. The support can have a thickness of, for example, 5 mm or less, 2 mm or less, 1 mm or less, 500 μm or less, 200 μm or less, 100 μm or less, 50 μm or less, or 10 μm or less.

[0113] The shape-memory resin can be impregnated into at least a part of the support. The shape-memory resin may be coated or laminated on at least a part of the support. The shape-memory resin may be coated or laminated on one side of the support, or on both sides of the support. It is preferable that the support is deformable in accordance with the deformation of the shape-memory resin.

[0114] The external skin device of the present disclosure may further include an external skin component. The external skin component may be contained in a shape-memory resin and / or a support. The external skin component may be an aqueous composition, an emulsion composition, or an oil-based composition containing the components listed below. The external skin component may be, for example, a cosmetic component and / or a beauty component. Examples of the external skin component include moisturizers, skin nutrients, vitamins, anti-inflammatory agents, whitening agents, various extracts, blood circulation promoters, antiseborrheic agents, anti-inflammatory agents, pH adjusters, fragrances, therapeutic agents, and the like.

[0115] The external skin device of the present disclosure makes it easier to apply the shape-memory resin according to the first embodiment to the skin, makes it easier to apply external skin ingredients to the skin, and makes it easier to transmit the deformation of the shape-memory resin to the skin.

[0116] A method for producing an external skin device according to the second embodiment will be described below. An example of a method for producing an external skin device in which a support is impregnated with a shape-memory resin will be described below.

[0117] First, a mold for molding the extracutaneous device is prepared. The mold can have, for example, a shape of a part of skin. For example, the mold can have a shape of at least a part of a face.

[0118] Next, the above-mentioned monomer, polymerization initiator, and support are placed in the mold. The monomer and polymerization initiator can be the same as those described above. The support can be the same as those described above.

[0119] A release sheet may be interposed between the mold and the monomer and / or support to facilitate removal of the external skin device from the mold. As the release sheet, for example, a polytetrafluoroethylene sheet can be used.

[0120] The monomer is then polymerized to produce an external skin device having the shape of the mold and in which the support is impregnated and / or laminated with the shape-memory resin.

[0121] In the above, a monomer is placed in a mold, but it is also possible to place an already prepared shape-memory resin and a support in a mold and heat the shape-memory resin above its glass transition temperature or melting point to impregnate, coat or laminate the shape-memory resin into the support.

[0122] Next, when an ingredient for external use on the skin, such as a cosmetic ingredient, is to be included, the external skin equipment can be impregnated with a liquid containing the ingredient for external use on the skin.

[0123] Next, a method for using the external skin device will be described.

[0124] The method of using the external skin device is the same as the method of using the shape-memory resin described above. After the shape-memory resin has been caused to memorize its original shape, the external skin device is attached to the desired skin. The shape-memory resin can then be deformed by body heat, exerting a deforming force on the skin.

[0125] The external skin device of the present disclosure can be applied to, for example, beauty products, cosmetic products, medical products (treatment products), clothing products, shoe products, etc. The external skin device of the present disclosure can be applied to, for example, masks.

[0126] The shape-memory resin and external skin device of the present disclosure may also include a shape-memory resin and external skin device obtained by the manufacturing method of the present disclosure. Some features of the shape-memory resin and external skin device of the present disclosure other than those described above are difficult to directly identify by the composition, structure, or properties of the shape-memory resin and external skin device of the present disclosure. In such cases, the shape-memory resin and external skin device of the present disclosure should be allowed to be identified by the manufacturing method. EXAMPLES

[0127] The shape-memory resin of the present disclosure will be described below with reference to examples. However, the shape-memory resin of the present disclosure is not limited to the following examples.

[0128] [Test Examples 1 to 7] Shape-memory resins with different compositions were prepared, and the physical properties of each shape-memory resin were measured. Table 1 shows the mixing ratio of the raw materials of the prepared shape-memory resins. The mixing ratio can be considered to be the same as the composition of the shape-memory resin. The mixing ratio of the monomer, crosslinking agent, and initiator shown in Table 1 is the ratio to the total amount of the monomer, crosslinking agent, and initiator.

[0129] For each composition, the average strain at break, Young's modulus, tensile strength at break, stability over time, and shape memory were measured. The average strain at break, Young's modulus, and tensile strength at break were measured in accordance with JIS K6251 by pulling both ends of a No. 7 dumbbell-shaped test piece at a speed of 100 mm / min with a tensile tester. The average strain at break and tensile strength are the values ​​at break.

[0130] The extensibility was evaluated by measuring the elongation percentage of a JIS K6251 No. 7 dumbbell-shaped test piece by applying a load in one direction at room temperature and using the following criteria. A: The degree of elongation was 200% or more of the original length; B: The degree of elongation was less than 200% of the original length.

[0131] The stability over time was measured by heating a test piece of 20 mm in length, 10 mm in width, and 1 mm in thickness to 50°C to soften it, and then stretching it in one axial direction (lengthwise direction) to twice its original length (200%). Next, the test piece in the stretched state was cooled to 0°C to fix the stretched state. The stretched test piece was left to stand in a thermostatic bath at 5°C for 24 hours, and the degree of shrinkage was evaluated according to the following criteria. The stability over time at 25°C was also tested in the same manner. The stability over time was tested for the resins of Test Examples 3 and 4. The stability over time of the resin of Test Example 3 was also confirmed for a test piece of 2 mm in thickness in the same manner. A: The length after 24 hours of standing was 190% or more of the original length; B: The length after 24 hours of standing was 160% or more but less than 190% of the original length; C: The length after standing for 24 hours was 130% or more and less than 160% of the original length.

[0132] Regarding shape memory, a test piece of 20 mm in length, 10 mm in width, and 1 mm in thickness was first heated to 50°C to soften it, and then stretched in one axial direction (lengthwise direction) to 1.5 times (150%) its original length. Next, the test piece in the stretched state was cooled to 0°C to fix the stretched state. Next, the test piece in the stretched state was heated to 40°C and contracted. The extent to which it had shrunk (whether it had recovered its shape) relative to its original length was evaluated according to the following criteria. A: The length after shape recovery was greater than 100% and less than 110% of the original length; B: The length after shape recovery was greater than 110% and less than 120% of the original length; C: The length after shape recovery was more than 120% of the original length.

[0133] The measurement results are shown in Table 2. The average strain, Young's modulus, and tensile strength are each the average value of five measurements.

[0134] The moisture content after synthesis shown in Table 1 is the moisture content when the shape-memory resin is left to stand at room temperature after synthesis. The saturated moisture content is the moisture content when the shape-memory resin is immersed in pure water at room temperature for 2 days or more and reaches a constant weight, in a saturated state (equilibrium swelling state). The moisture content was measured using an electronic moisture meter (Shimadzu MOC-120H). In Test Examples 4 to 6, the moisture content was not measured.

[0135] Shape-memory resins could be produced from N,N-dimethylacrylamide and stearyl acrylate. It was also found that shape-memory resins could be produced by further adding lauryl acrylate. It was confirmed that all of the resins in Test Examples 1 to 6 had sufficient shape-memory properties at temperatures close to human body temperature.

[0136] When the amount of the crosslinking agent added was increased, the average strain decreased, but the Young's modulus tended to increase. According to the physical properties shown in Table 2, it was found that the shape-memory resins of Test Examples 1 to 6 were all capable of exerting a significant force on the skin by deformation when they were applied to the skin and allowed to recover their shape.

[0137] Test Examples 3 and 4, which have a lauryl acrylate component as a constituent unit in addition to the N,N-dimethylacrylamide component and the stearyl acrylate component and in which the crosslinking agent is 0.01 mol % to 1 mol % or less, were able to improve the extensibility compared to the other test examples. Note that even in Test Examples 1, 2, 5, and 6, which were rated B in extensibility, the resin was able to be stretched at least 1.5 times, and as described above, the resin had sufficient extensibility to be used as a shape-memory resin.

[0138] It was confirmed that when the shape-memory resin in the shape-memory state (stretched state) was stored at a low temperature (5°C), the resin hardly contracted. When stored at a temperature closer to body temperature, some degree of shrinkage was confirmed, but the shape-memory resin was in a state that was sufficiently usable as a shape-memory resin. From this, it was confirmed that the shape-memory resin of the present disclosure has stability over time in the shape-memory state (stretched state). It was confirmed that the stability over time was equivalent for test pieces with thicknesses of 1 mm and 2 mm. In addition, in order to increase the stability over time, it is considered preferable to reduce the amount of crosslinking agent added, for example, to 0.2 mol% or less, preferably 0.1 mol% or less.

[0139] The water content was almost constant, independent of the composition. The water content of the shape-memory resin after synthesis was 4% by mass to 7% by mass. The water content in the saturated state was 30% by mass to 35% by mass. It is considered that the water content can be adjusted by the immersion time in water. Since the shape-memory resin has water absorption properties, the shape-memory resin itself can hold an aqueous solution of an ingredient for external use on the skin.

[0140] The shape-memory resins of Test Examples 1 to 6 were all semi-transparent.

[0141] [Table 1]

[0142] [Table 2]

[0143] The shape-memory resin, external skin device, and manufacturing method thereof of the present invention have been described based on the above-mentioned embodiments and examples, but are not limited to the above-mentioned embodiments and examples, and may include various modifications, changes, and improvements to each of the disclosed elements (including elements described in the claims, specification, and drawings) within the scope of the present invention and based on the basic technical idea of ​​the present invention. Furthermore, various combinations, substitutions, and selections of each of the disclosed elements are possible within the scope of the claims of the present invention.

[0144] Further objects, objectives and modes (including modifications) of the present invention will become apparent from the entire disclosure of the present invention including the claims.

[0145] With respect to numerical ranges set forth herein, unless otherwise stated, any numerical value or range falling within that range should be construed as being specifically set forth herein.

[0146] A part or all of the above-described embodiments may be described as, but are not limited to, the following supplementary notes. Each supplementary note may be combined with each claim in the claims.

[0147] [Appendix 1] It has a sheet shape, A shape-memory resin that shrinks to a length of 80% or less of its pre-heating length when heated from a temperature below 30°C to 32°C to 45°C.

[0148] [Appendix 2] The shape-memory resin, when a flat sheet of the shape-memory resin is heated to 32°C to 45°C, deforms to have the shape of a part of the skin.

[0149] [Appendix 3] A first step of preparing a sheet of said shape memory resin having a length of 20 mm, a width of 10 mm and a thickness of 1 mm; After the first step, a second step of heating the sheet to 50°C to 70°C; a third step of stretching the sheet in the longitudinal direction while in the softened state from the second step to 1.5 times its original length; a fourth step of cooling the sheet to 0° C. in the state stretched in the third step; A fifth step of leaving the sheet at room temperature of 25° C. or less after the fourth step; when the sheet has a length of 26 mm or more, The shape-memory resin, wherein the sheet shrinks when a sixth step of heating the sheet to 32°C to 45°C is carried out after the fifth step.

[0150] [Appendix 4] The shape-memory resin described in Appendix, wherein after the sixth step, the sheet has a length of 24 mm or less.

[0151] [Appendix 5] The shape-memory resin described in the appendix, wherein after the shape-memory resin is produced, the water content of the shape-memory resin when left standing in air at room temperature is 2% by mass to 8% by mass relative to the mass of the shape-memory resin.

[0152] [Appendix 6] The shape-memory resin according to the appendix, wherein the saturated water content of the shape-memory resin is 25% by mass to 40% by mass with respect to the mass of the shape-memory resin.

[0153] [Appendix 7] The shape-memory resin described in the appendix has an endothermic peak at 28°C to 48°C.

[0154] [Appendix 8] The shape-memory resin according to the appendix further contains an aqueous solution containing a skin topical agent.

[0155] [Appendix 9] The shape-memory resin according to the appendix, which has a sheet shape with a thickness of 0.01 mm to 3 mm.

[0156] [Appendix 10] A shape-memory resin as described in the appendix, which has a shape that conforms to the surface shape of the skin.

[0157] [Appendix 11] A shape-memory resin as described in the appendix, having a shape that conforms to a part of a face.

[0158] [Appendix 12] A makeup method and / or a beauty treatment method comprising a step of applying to the skin the shape-memory resin according to the first embodiment and / or the external skin equipment according to the second embodiment.

[0159] [Appendix 13] The cosmetic and / or beauty method described in the appendix, in which the shape-memory resin and / or external skin equipment is attached to the face.

[0160] [Appendix 14] The cosmetic and / or beauty method according to the appendix, wherein after being attached to the skin, the shape-memory resin and / or the external skin equipment shrinks on the skin due to body temperature. [Industrial Applicability]

[0161] The shape-memory resin, external skin device, and method of manufacturing an external skin device disclosed herein can be applied to cosmetics, beauty products, and medical products.

Claims

1. A support, A skin cosmetic product comprising: a shape-memory resin impregnated in the support; The shape-memory resin is 64 mol % to 85 mol % of an N-alkylacrylamide component; 14 mol % to 35 mol % of an acrylic acid ester component having a structure shown in Chemical Formula 1 below; 0.01 mol % to 6 mol % of a cross-linking component; The skin beauty product is a skin beauty product that contains a beauty ingredient and / or a cosmetic ingredient. 【Chemistry 1】 (In the chemical formula shown in Chemical Formula 1, R 1 is a hydrogen atom or an alkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms; R 2 is an alkyl group, an alkenyl group, or an acyl group having 10 to 20 carbon atoms.

2. 2. The cosmetic skin product of claim 1, wherein the N-alkylacrylamide component comprises an N,N-dimethylacrylamide component.

3. 3. The skin cosmetic product according to claim 1 or 2, wherein the acrylic ester component comprises at least one selected from the group consisting of a stearyl acrylate component, a lauryl acrylate component, a 2-ethylhexyl acrylate component, and a butyl acrylate component.

4. The skin cosmetic product according to any one of claims 1 to 3, wherein the acrylic acid ester component comprises, based on the total amount of the acrylic acid ester component, 40 mol% to 100 mol% of a stearyl acrylate component and 0 mol% to 60 mol% of a lauryl acrylate component.

5. A cosmetic skin product according to any one of claims 1 to 4, wherein the cross-linking component comprises an N,N'-methylenebisacrylamide component.

6. A cosmetic product for the skin according to any one of claims 1 to 5, wherein the polymer has a Young's modulus of 1 MPa or less.

7. A cosmetic skin product according to any one of claims 1 to 6, wherein the polymer has an average strain of 500% or more.

8. A skin cosmetic product described in any one of claims 1 to 7, wherein the shape memory resin further contains polyethylene glycol.

9. A skin cosmetic product as described in claim 8, wherein the content of the polyethylene glycol is 0.1 mass% to 1 mass% relative to the mass of the shape memory resin.

10. The cosmetic skin product according to any one of claims 1 to 9, wherein the water content of the shape-memory resin is 2% by mass to 40% by mass relative to the mass of the shape-memory resin.

11. A skin cosmetic product described in any one of claims 1 to 10, wherein the shape-memory resin has temperature-responsive shape-memory properties.

12. A skin cosmetic product described in any one of claims 1 to 11, wherein the shape-memory resin is flexible.

13. The cosmetic skin product according to claim 1, wherein in the chemical formula shown in Chemical Formula 1, R 1 is an alkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms.

14. The cosmetic product for skin according to any one of claims 1 to 13, wherein the support has elasticity.

15. The cosmetic product for skin according to any one of claims 1 to 14, wherein the support is at least one selected from the group consisting of nonwoven fabric, woven fabric, knitted fabric, tufted fabric, felt, fulled fabric, paper, and water-retaining material.

16. The cosmetic skin product according to any one of claims 1 to 15, which has a sheet shape.

17. The cosmetic product for skin according to any one of claims 1 to 16, which has a shape that conforms to the surface shape of the skin.

18. A cosmetic skin product according to any one of claims 1 to 17, having a shape that conforms to at least a part of the face.

19. 64 mol% to 85 mol% of an N-alkylacrylamide component; 14 mol % to 35 mol % of an acrylic acid ester component having a structure shown in Chemical Formula 2 below; A shape-memory resin comprising a polymer comprising 0.01 mol % to 6 mol % of a cross-linking component, and polyethylene glycol. 【Chemistry 2】 (In the chemical formula shown in Chemical Formula 2, R 1 is hydrogen or an alkyl group, alkenyl group, or acyl group having 1 to 4 carbon atoms, and R 2 is an alkyl group, alkenyl group, or acyl group having 10 to 20 carbon atoms.) 20. The shape-memory resin according to claim 19, wherein in the chemical formula shown in Chemical Formula 2, R 1 is an alkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms.

21. A method for producing a mixture comprising mixing a monomer containing 64 mol% to 85 mol% of N-alkylacrylamide, 14 mol% to 35 mol% of an acrylic acid ester having a structure shown in Chemical Formula 3 below, and 0.01 mol% to 6 mol% of a crosslinking agent, a polymerization initiator, and polyethylene glycol; polymerizing the mixture to form a polymer; heating the polymer above its glass transition temperature to expand it; and cooling the polymer in an expanded state. 【Chemistry 3】 (In the chemical formula shown in Chemical Formula 3, R 3 is hydrogen or an alkyl group, alkenyl group, or acyl group having 1 to 4 carbon atoms, and R 4 is an alkyl group, alkenyl group, or acyl group having 10 to 20 carbon atoms.) 22. The method for producing an external skin device according to claim 21, wherein in the chemical formula shown in Chemical Formula 3, R 3 is an alkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms.

23. A step of preparing a mixture by mixing monomers including 64 mol % to 85 mol % of N-alkylacrylamide, 14 mol % to 35 mol % of an acrylic acid ester having a structure shown in Chemical Formula 4 below, and 0.01 mol % to 6 mol % of a crosslinking agent, and a polymerization initiator; placing the mixture and a support in a mold; polymerizing the mixture while the mixture is impregnated into the support to produce a polymer; heating the polymer above its glass transition temperature to expand it; cooling the polymer in an expanded state to produce a cosmetic skin product; impregnating the skin beauty product with beauty ingredients and / or cosmetic ingredients; A method for producing a cosmetic product for the skin, comprising: 【Chemistry 4】 (In the chemical formula shown in Chemical Formula 4, R 3 is a hydrogen atom or an alkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms; R 4 is an alkyl group, an alkenyl group, or an acyl group having 10 to 20 carbon atoms.

24. The method for producing a cosmetic product for skin according to claim 23, wherein in the chemical formula shown in Chemical Formula 4, R 3 is an alkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms.

25. The method for producing a cosmetic product for skin according to claim 23 or 24, wherein the support has elasticity.

26. The method for producing a skin cosmetic product according to any one of claims 23 to 25, wherein the support is at least one selected from the group consisting of nonwoven fabric, woven fabric, knitted fabric, tufted fabric, felt, fulled fabric, paper, and water-retaining material.

27. A method for producing a cosmetic skin product according to any one of claims 23 to 26, wherein the mould has the shape of a part of a face.

28. The method for producing a cosmetic skin product according to any one of claims 23 to 27, further comprising interposing a release sheet between the mixture and the mold.

29. 29. The method of claim 28, wherein the release sheet is a polytetrafluoroethylene sheet.

30. A method for producing a skin cosmetic product described in any one of claims 23 to 29, wherein the skin cosmetic product is formed into a sheet.

31. The method for producing a cosmetic product for skin according to any one of claims 23 to 30, wherein the acrylic ester comprises at least one selected from the group consisting of stearyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, and butyl acrylate.

32. The method for producing a cosmetic product for skin according to any one of claims 23 to 31, wherein the acrylic ester comprises, based on the total amount of acrylic esters, 40 mol% to 100 mol% of stearyl acrylate and 0 mol% to 60 mol% of lauryl acrylate.

33. The method for producing a cosmetic skin product according to any one of claims 23 to 32, wherein the N-alkylacrylamide comprises N,N-dimethylacrylamide.

34. The method for producing a cosmetic skin product according to any one of claims 23 to 33, wherein the crosslinking agent comprises N,N'-methylenebisacrylamide.

Citation Information

Patent Citations

  • Face mask

    JP2005160833A

  • Face mask sheet and manufacturing method

    JP2007143586A

  • Transparent shape-memory gel, lens using the gel, and method of adjusting focal point of lens

    JP2013057062A

  • Intraocular lens

    JP2014104239A