Negative electrode active material, its manufacturing method, and lithium secondary battery having a negative electrode including the same
A silicon-containing amorphous coating layer on a carbon-based material with small silicon particles addresses the volume expansion issue in lithium secondary batteries, improving the life characteristics and cycle performance by buffering stress and preventing cracks.
Patent Information
- Application Number
- JP2023096372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-08-14
- Filing Date
- 2023-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-08-13
AI Technical Summary
Lithium secondary batteries using carbon-based negative electrode materials face limitations in energy density and discharge capacity due to the volume expansion of silicon during charging and discharging, leading to deteriorated life characteristics in Si/carbon composites.
A negative electrode active material is developed with a silicon-containing amorphous coating layer on a carbon-based material, where silicon particles are 5 nm or less, and a carbon matrix is used to buffer the volume expansion, suppressing cracks and improving life characteristics.
The silicon-containing amorphous coating layer effectively alleviates volume change and crack formation in the negative electrode, enhancing the life characteristics and cycle performance of lithium secondary batteries.
Smart Images

Figure 0007559142000006 
Figure 0007559142000007 
Figure 0007559142000008
Abstract
Description
[Technical field]
[0001] The present invention was made with funding from the Ministry of Trade, Industry and Energy under the project number 1415156147 entitled "Development of materials and cell process technology for ultra-long-life lithium secondary batteries (>450Wh / L) for EES," and relates to a negative electrode active material, a manufacturing method thereof, and a lithium battery having a negative electrode including the same. [Background technology]
[0002] Lithium secondary batteries have excellent charge / discharge efficiency and capacity, no memory effect, and low self-discharge even when not in use, and have been used as a core component of portable electronic devices since their commercialization. Recently, the applications of lithium secondary batteries have expanded from fields where small and medium-sized batteries are used, such as cleaning machines and power tools, to fields where medium and large-sized batteries are used, such as electric vehicles, energy storage devices, and various robots.
[0003] Lithium secondary batteries using carbon-based negative electrode materials are widely used due to their high cost competitiveness and excellent energy life characteristics. However, they still have limitations in terms of low density and discharge capacity. Therefore, attempts have been made to develop negative electrodes for lithium secondary batteries that provide improved energy density and capacity.
[0004] From the viewpoint of improving the energy density and capacity, research has been attempted to use silicon, which has a theoretical energy density of 3,600 mAh / g, as a negative electrode active material. x , Si-metal alloys, and Si-carbon composites are being investigated as candidates.
[0005] Among such candidates, silicon-carbon composites have attracted attention from the standpoints of efficiency and life characteristics, but there is a limit at which the life characteristics of the negative electrode active material deteriorate due to the volume expansion of silicon during charging and discharging.
[0006] Accordingly, there is a need to develop a negative electrode active material of a Si-carbon composite substrate with improved life characteristics in a stable form compared to the negative electrode active material of an existing Si-carbon composite substrate.
SUMMARY OF THE INVENTION
PROBLEMS TO BE SOLVED BY THE INVENTION
[0007] One aspect is to provide a novel negative electrode active material. Another aspect is to provide a method for manufacturing the negative electrode active material. Still another aspect is to provide a lithium secondary battery including a negative electrode employing the negative electrode active material.
MEANS FOR SOLVING THE PROBLEMS
[0008] According to one aspect, a carbon-based material, a silicon-containing amorphous coating layer located on the carbon-based material and represented by SiC x are included, in the SiC x x is 0 < x < 0.5, and a negative electrode active material for a lithium secondary battery is provided, wherein the silicon-containing amorphous coating layer includes silicon particles having a particle size of 5 nm or less.
[0009] According to another aspect, a step of preparing a carbon-based material, and a step of providing a silicon-containing amorphous coating layer represented by SiC (0 < x < 0.5) on the surface of the carbon-based material are included, and a method for manufacturing a negative electrode active material for a lithium secondary battery is provided. x (0 < x < 0.5)
[0010] According to still another aspect, a lithium secondary battery including a negative electrode including the negative electrode active material, a positive electrode, and an electrolyte is provided.
EFFECTS OF THE INVENTION
[0011] The negative electrode active material according to one aspect is SiC on a carbon-based material.x By including the silicon-containing amorphous coating layer represented by the formula (I), a volume change of Si particles during charging and discharging is suppressed, and cracks in the negative electrode active material are alleviated, so that the life characteristics of a lithium secondary battery using a negative electrode including the negative electrode active material can be improved. [Brief description of the drawings]
[0012] [Figure 1] 1 is an XRD graph of a negative active material according to an embodiment. [Diagram 2] 5A and 5B are SEM and TEM photographs of a surface and a cross section of a negative active material according to an embodiment. [Diagram 3] 1 shows an EELS line scanning result of a negative active material according to an embodiment. [Figure 4] 1 shows an elemental content analysis result of a negative active material according to an embodiment. [Diagram 5] 1 is a graph showing electrochemical evaluation data of half cells according to Example 1 and Comparative Example 1. [Figure 6] 1 is a graph showing electrochemical evaluation data of half cells according to Example 2 and Example 1. [Figure 7] 1 is a graph showing differential capacity of half cells prepared in Examples 3 to 6 and Comparative Examples 2 and 3. [Figure 8] 1 is a graph showing XRD analysis results of silicon-containing amorphous coating layers in negative active materials obtained in Preparation Examples 4, 8, and 10. [Figure 9] 1 is a graph showing electrochemical evaluation data of full cells according to Example 7 and Comparative Example 4. [Figure 10] 1 is a photograph showing a cross section of a negative electrode active material of full cells according to Example 7 and Comparative Example 4 after 50 cycles of charging and discharging. [Figure 11] 1 is a graph showing electrochemical evaluation data of the full cells prepared in Examples 8 to 10. [Figure 12] 1 is a schematic diagram of a lithium secondary battery according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present inventive concept described below can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, they do not limit the present inventive concept to specific embodiments, and should be understood to include all modifications, equivalents, or alternatives included in the technical scope of the present inventive concept.
[0014] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In the following, terms such as "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the context.
[0015] In the drawings, the diameters, lengths, and thicknesses of the various components, layers, and regions are shown enlarged or reduced to clearly depict them. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, or plate, is described as being "on" or "above" another part, this does not only mean that it is directly on top of the other part, but also includes cases where there is another part between them. Throughout the specification, terms such as first and second may be used to describe various components, but the components are not limited by the terms. The terms are used only to distinguish one component from another. In the drawings, some components may be omitted, but this is for the purpose of aiding in the understanding of the features of the invention, and is not intended to exclude the omitted components.
[0016] Hereinafter, a negative electrode active material, a method for manufacturing the negative electrode active material, and a lithium secondary battery employing the negative electrode including the same according to an exemplary embodiment will be described in more detail.
[0017] A negative electrode active material according to an embodiment includes a carbon-based material and a silicon-containing amorphous coating layer located on the carbon-based material and represented by SiC x wherein, in SiC x x satisfies 0.07 < x < 0.7, and the silicon-containing amorphous coating layer includes silicon particles having a particle size of 5 nm or less.
[0018] According to an embodiment, the SiC x is a composite of silicon and carbon, and may include silicon particles, carbon particles, silicon carbide (SiC), or a combination thereof, but is not limited thereto.
[0019] According to an embodiment, in the SiC x x also satisfies 0.2 < x < 0.5. For example, x also satisfies 0.2 < x < 0.3. For example, x is also 0.25.
[0020] As will be described later, the silicon-containing amorphous coating layer is formed by vapor phase co-deposition of a silicon raw material and a carbon raw material. Therefore, an increase in the x value means an increase in the volume occupied by carbon in the obtained silicon-containing amorphous coating layer. As a result, the volume occupied by silicon and the size of the silicon particles are relatively smaller than when the x value is small.
[0021] Such a phenomenon is a specific result of vapor phase co-deposition of a silicon raw material and a carbon raw material. In the case of other thin film forming processes, for example, a method such as a sputtering method, it is difficult to control the size of silicon particles during the thinning process. According to an embodiment, the silicon particles may include crystalline silicon particles.
[0022] According to an embodiment, the silicon-containing amorphous coating layer does not show a peak at 0.43 V in differential capacitance analysis (dQ / dV). It is generally known that when micro silicon particles are included, a peak is shown at 0.43 V in differential capacitance analysis. However, the silicon-containing amorphous coating layer does not show such a peak, and therefore does not contain silicon particles having a micro-sized particle size.
[0023] According to an embodiment, the silicon nanoparticles may have a diameter of 3 to 5 nm, for example, a diameter of 4 to 5 nm.
[0024] The smaller the particle size of the silicon nanoparticles, the smaller the magnitude of stress due to volume expansion, and therefore the life characteristics of the active material can be improved.
[0025] On the other hand, if the size of silicon particles exceeds 5 nm, the stress of silicon particles becomes large, resulting in vacant spaces in the silicon-containing amorphous coating layer, and if the size of silicon particles is less than 3 nm, the amount of amorphous carbon contained in the silicon-containing amorphous coating layer becomes too large, making it difficult for Li ions to pass through, resulting in high resistance during charging and discharging, and thus deteriorating the battery characteristics.
[0026] The silicon-containing amorphous coating layer may have a structure in which silicon nanoparticles are contained in a carbon matrix. The carbon matrix may be amorphous carbon. The amorphous carbon matrix may act to buffer the expansion of silicon particles during charging, and may expand isotropically in volume, which may reduce stress applied to the coating layer compared to a case where the coating layer expands in one direction, thereby suppressing cracks in the coating layer.
[0027] The silicon-containing coating layer may further include a carbon coating layer at the outermost portion, and can maintain an amorphous state even at high temperatures exceeding 900° C. for deposition of the outermost carbon coating layer. Without being bound by theory, it is believed that carbon does not crystallize in the silicon-containing amorphous coating layer because the silicon-containing amorphous coating layer exists as a mixture of silicon and amorphous carbon.
[0028] The amorphous carbon matrix accommodates the expansion of silicon nanoparticles during charging and buffers the stress applied to the silicon-containing amorphous coating layer, thereby suppressing the volumetric change of the silicon nanoparticles, thereby preventing cracks in the negative electrode active material and significantly improving cycle characteristics.
[0029] According to an embodiment, the silicon-containing amorphous coating layer includes silicon nanoparticles and a carbon matrix, and the carbon matrix is included in an amount of 10 to 60 parts by weight based on 100 parts by weight of the total silicon-containing amorphous coating layer.
[0030] For example, the carbon matrix may be included in an amount of, but is not limited to, 10 to 55 parts by weight, 10 to 50 parts by weight, 10 to 45 parts by weight, 10 to 40 parts by weight, 15 to 60 parts by weight, 20 to 60 parts by weight, 25 to 60 parts by weight, or 30 to 60 parts by weight, based on 100 parts by weight of the total silicon-containing amorphous coating layer.
[0031] When the content of the carbon matrix satisfies the above range, the expansion of the silicon nanoparticles can be effectively controlled, and an improvement in the life characteristics can be expected.
[0032] The carbon matrix is inactive to lithium ions and does not participate in the absorption and release of lithium ions.
[0033] According to an embodiment, the thickness of the silicon-containing amorphous coating layer is 5 nm to 4,000 nm. For example, the thickness of the silicon-containing amorphous coating layer is 5 nm to 3,000 nm, 5 nm to 2,000 nm, 5 nm to 1,000 nm, 5 nm to 500 nm, 5 nm to 400 nm, 5 nm to 300 nm, 5 nm to 200 nm, 5 nm to 100 nm, 5 nm to 90 nm, 5 nm to 80 nm, 5 nm to 70 nm, 5 nm to 60 nm, or 5 nm to 50 nm, but is not limited thereto, and is formed to a sufficient thickness to include the carbon matrix.
[0034] According to an embodiment, the silicon-containing coating layer may be disposed on a portion or the entire surface of the carbon-based material, for example, the silicon-containing coating layer may be disposed on the surface of the carbon-based material in a continuous layer.
[0035] According to an embodiment, the carbon-based material is also porous. Porous carbon-based materials are stable due to small volume change during charging and discharging. In addition, the space formed by the porosity can accommodate volume change, which is advantageous in terms of life characteristics. According to an embodiment, the carbon-based material may include, but is not limited to, natural graphite, artificial graphite, hard carbon, soft carbon, or a combination thereof, and may be any material that is capable of reversibly absorbing and releasing lithium ions and is made of carbon that is commonly used in lithium secondary batteries.
[0036] According to an embodiment, the carbon coating layer disposed on the surface of the silicon-containing coating layer may contain amorphous carbon. For example, the carbon contained in the carbon coating layer is also a fired product of a carbon precursor. The carbon precursor can be any one that can be used in the art as long as a carbon-based material can be obtained by firing. For example, the carbon precursor is also one or more selected from the group consisting of polymers, coal tar pitch, petroleum pitch, mesophase pitch, coke, low-molecular middle oil, coal-based pitch, and their derivatives. By forming a carbon coating layer on the outermost surface of the composite negative electrode active material, an SEI will be formed, and Li + ions can be prevented from contacting with the electrolyte and the like through selective passage. Moreover, the carbon coating layer suppresses volume expansion during charge and discharge, serves as an electron transfer path in the composite negative electrode active material, and contributes to the improvement of electrical conductivity.
[0037] The thickness of the carbon coating layer is also 2 nm to 5 μm, and is also any range represented by any two arbitrary values selected within the range. When the thickness of the carbon coating layer is within the above range, the electrical conductivity is improved, and at the same time, the volume expansion can be sufficiently suppressed. When the thickness of the carbon coating layer is less than 2 nm, it is impossible to expect the role of a buffer layer that can improve sufficient electrical conductivity and accommodate the volume expansion of silicon. When the thickness of the carbon coating layer exceeds 5 μm, during charge and discharge, during lithium insertion and release, the carbon coating layer acts as a resistance, causing rate-limiting reduction.
[0038] Hereinafter, a method for manufacturing a negative electrode active material according to an embodiment will be described. According to an embodiment, a step of preparing a carbon-based material, and providing a silicon-containing amorphous coating layer represented by SiC x (0.07 < x < 0.7) on the surface of the carbon-based material are provided, and a method for manufacturing a negative electrode active material is provided.
[0039] According to an embodiment, providing the silicon-containing coating layer may include providing a silane-based gas and a hydrocarbon-based gas.
[0040] According to an embodiment, providing the silicon-containing amorphous coating layer may include depositing a silane-based gas and a hydrocarbon-based gas on a surface of a carbon-based material by chemical vapor deposition (CVD).
[0041] According to an embodiment, the silane-based gas and the hydrocarbon-based gas may be provided sequentially or simultaneously, for example, the silane-based gas and the hydrocarbon-based gas may be provided simultaneously.
[0042] According to an embodiment, the silane-based gas may be a silicon-based precursor such as silane (SiH4), dichlorosilane (SiH2Cl2), silicon tetrafluoride (SiF4), silicon tetrachloride (SiCl4), methylsilane (CH3SiH3), disilane (Si2H6), or a combination thereof.
[0043] According to an embodiment, the hydrocarbon gas may be any straight or branched organic compound composed of carbon and hydrogen. Non-limiting examples of the hydrocarbon gas include methane, ethane, propane, butane, ethylene, and acetylene.
[0044] When the silane-based gas and the hydrocarbon-based gas are supplied simultaneously, the volume ratio of the silane-based gas to the hydrocarbon-based gas may be 1:0.01 volume % to 1:1 volume %, for example, the volume ratio of the silane-based gas to the hydrocarbon-based gas may be 1:0.01 volume % to 1:0.5 volume %.
[0045] The silicon-containing amorphous coating layer is formed by co-deposition of a silane-based gas and a hydrocarbon-based gas, so that the particle size of silicon particles in the coating layer tends to increase as the amount of the silane-based gas increases, and the particle size of silicon particles in the coating layer tends to decrease as the amount of the silane-based gas decreases. Conversely, if the amount of the hydrocarbon-based gas is increased, the space in which the silicon particles can exist becomes relatively smaller, so the particle size of the silicon particles becomes smaller, and if the amount of the hydrocarbon-based gas is decreased, the particle size of the silicon particles may become larger. In this way, the particle size of silicon particles contained in the silicon-containing amorphous coating layer can be controlled by the above method.
[0046] When the volume ratio of the silane-based gas and the hydrocarbon-based gas satisfies the above range, a carbon matrix capable of minimizing the volume expansion of silicon nanoparticles contained in the silicon-containing coating layer is contained in the silicon-containing coating layer, thereby minimizing the volume change of the negative active material during charging and discharging, and improving cycle characteristics.
[0047] According to an embodiment, the step of providing the silicon-containing coating layer may be performed at a temperature of 400° C. to 900° C. For example, the step of providing the silicon-containing coating layer may be performed at a temperature of 500° C. to 900° C., 600° C. to 900° C., or 700° C. to 900° C., but is not limited thereto, and may be selected depending on the composition and thickness of the desired coating layer.
[0048] According to an embodiment, the carbon matrix may include amorphous carbon. According to an embodiment, the carbon matrix may be included in an amount of 10 to 60 parts by weight based on 100 parts by weight of the total silicon-containing coating layer.
[0049] According to an embodiment, after providing the silicon-containing amorphous coating layer, the method may further include providing a carbon coating layer including amorphous carbon.
[0050] For example, the step of providing the carbon coating layer may further include the step of providing a carbon precursor and then heat treating the carbon precursor. For example, the heat treatment may be carried out at a temperature between 800°C and 1,100°C.
[0051] If the heat treatment temperature is less than 800°C, the thermal decomposition does not occur sufficiently, and if it exceeds 1,100°C, a side reaction between the nanoparticles, for example silicon nanoparticles, and the carbon precursor causes the formation of crystalline SiC, resulting in a decrease in capacity.
[0052] The heat treatment may be performed for 1 hour or more. If the heat treatment is performed for less than 1 hour, the carbon precursor is not sufficiently pyrolyzed, making it difficult to form a uniform carbon coating layer.
[0053] The step of forming the carbon coating layer may be performed under an inert atmosphere, for example, under an argon atmosphere or a nitrogen atmosphere, thereby allowing the introduction of a uniform carbon coating layer.
[0054] According to another aspect, a negative electrode for a lithium secondary battery includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector and including the above-described negative electrode active material.
[0055] The negative electrode may include a binder between the negative electrode current collector and the negative electrode active material layer, or within the negative electrode active material layer. For details of the binder, see below. The negative electrode and the lithium secondary battery including the same can also be manufactured by the following method.
[0056] The negative electrode may include the negative electrode active material described above. For example, the negative electrode active material, a binder, and optionally a conductive agent may be mixed in a solvent to prepare a negative electrode active material composition, which may then be molded into a predetermined shape or applied to a current collector such as a copper foil.
[0057] The binder used in the negative electrode active material composition is a component that helps bind the negative electrode active material to the conductive agent or the negative electrode active material to the current collector, and may be included between the negative electrode current collector and the negative electrode active material layer or within the negative electrode active material layer, and is added in an amount of 1 to 50 parts by weight based on 100 parts by weight of the negative electrode active material. For example, the binder may be added in a range of 1 to 30 parts by weight, 1 to 20 parts by weight, or 1 to 15 parts by weight based on 100 parts by weight of the negative electrode active material.
[0058] Examples of such binders include polyvinylidene fluoride, polyvinylidene chloride, polybenzimidazole, polyimide, polyvinyl acetate, polyacrylonitrile, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polystyrene, polymethyl methacrylate, polyaniline, acrylonitrile butadiene styrene, phenolic resins, epoxy resins, polyethylene terephthalate, polytetrafluoroethylene, polyphenylene sulfide, polyamide-imide, polyetherimide, polyethersulfone, polyamide, polyacetal, polyphenylene oxide, polybutylene terephthalate, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubbers, and various copolymers.
[0059] The negative electrode may further include a conductive agent to provide a conductive path to the negative electrode active material and further improve electrical conductivity. The conductive agent may be any material generally used in lithium batteries, and examples of the conductive agent include carbon-based materials such as carbon black, acetylene black, ketjenbreck, and carbon fiber (e.g., vapor-grown carbon fiber); metal-based materials such as metal powder or metal fiber of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and conductive materials including mixtures thereof.
[0060] The solvent may be N-methylpyrrolidone (NMP), acetone, water, etc. The content of the solvent is 1 to 10 parts by weight based on 100 parts by weight of the composite negative electrode active material. When the content of the solvent is within the above range, the operation for forming the active material layer is easy.
[0061] The current collector is generally made to a thickness of 3 to 500 μm. The current collector is not particularly limited as long as it is conductive and does not induce chemical changes in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The surface may be made finely uneven to strengthen the binding force of the negative electrode active material, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.
[0062] The negative electrode active material composition thus prepared may be directly coated on a current collector to prepare a negative electrode plate, or may be cast on a separate support, and the negative electrode active material film peeled off from the support may be laminated on a copper foil current collector to obtain a negative electrode plate. The negative electrode is not limited to the forms listed above, and may be in forms other than those listed above.
[0063] The negative electrode active material composition can be used not only to manufacture electrodes for lithium batteries, but also to manufacture printable batteries by printing the composition on a flexible electrode substrate.
[0064] Next, the positive electrode is prepared. For example, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The positive electrode active material composition is directly coated on a metal current collector to manufacture a positive electrode plate. Alternatively, the positive electrode active material composition may be cast on a separate support, and the film peeled from the support may be laminated on a metal current collector to manufacture a positive electrode plate. The positive electrode is not limited to the forms listed above, and may be in a form other than the forms listed above.
[0065] The positive electrode active material is a lithium-containing metal oxide, and any commonly used material in the art may be used without limitation. For example, LiCoO2, LiMn x O 2x (x=1,2), LiNi 1-x Mn x O 2x (0 <x<1)、LiNi 1-x-y Co x Mn y Examples include O2 (0≦x≦0.5, 0≦y≦0.5) and LiFePO4.
[0066] Here, it goes without saying that the compound may have a coating layer on its surface, or may be used in combination with a compound having a coating layer. The coating layer may include a coating element compound such as an oxide of the coating element, a hydroxide of the coating element, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compounds forming the coating layer may be amorphous or crystalline. The coating element contained in the coating layer may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating layer forming step may use any coating method as long as the compound uses such an element and can be coated by a method (e.g., spray coating method, immersion method, etc.) that does not adversely affect the physical properties of the positive electrode active material, and a detailed description thereof will be omitted since it is fully understood by those skilled in the art.
[0067] In the positive electrode active material composition, the conductive agent, binder, and solvent may be the same as those in the negative electrode active material composition.
[0068] The contents of the positive electrode active material, the conductive agent, the binder, and the solvent are at levels generally used in lithium secondary batteries. Depending on the use and configuration of the lithium battery, one or more of the conductive agent, the binder, and the solvent may be omitted.
[0069] Next, a separator to be inserted between the positive electrode and the negative electrode is prepared. The separator may be any separator that is generally used in lithium batteries. A separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte wettability may be used. For example, the separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or a combination thereof, and may be in the form of a nonwoven fabric or a woven fabric. For example, a separator that can be wound, such as polyethylene or polypropylene, may be used for a lithium ion battery, and a separator that has excellent organic electrolyte wettability may be used for a lithium ion polymer battery. For example, the separator may be manufactured by the following method.
[0070] A separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition may be directly coated on an electrode and dried to form a separator. Alternatively, the separator composition may be cast on a support and dried, and the separator film may be peeled off from the support and laminated on an electrode to form a separator.
[0071] The polymer resin used to manufacture the separator is not particularly limited, and any material that is used as a binder for electrode plates can be used, such as vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or a mixture thereof.
[0072] Next, the electrolyte is prepared. For example, the electrolyte may be an organic electrolyte solution. The electrolyte may also be a solid. For example, the electrolyte may be boron oxide, lithium oxynitride, etc., but is not limited thereto. Any electrolyte that is used as a solid electrolyte in the art may be used. The solid electrolyte may also be formed on the negative electrode by a method such as sputtering.
[0073] For example, the organic electrolyte may be prepared by dissolving a lithium salt in an organic solvent. The organic solvent may be any that can be used as an organic solvent in the art, such as propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or a mixture thereof.
[0074] The lithium salt may be any lithium salt that can be used in the art. For example, LiPF, LiBF, LiSbF, LiAsF, LiClO, LiCF, SO, Li(CFSO)N, LiC, F, SO, LiAlO, LiAlCl, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (where x and y are natural numbers), LiCl, LiI, or a mixture thereof.
[0075] As can be seen from FIG. 12, the lithium battery 1 includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded and housed in a battery case 5. An organic electrolyte is then injected into the battery case 5, and the battery case 5 is sealed by a cap assembly 6 to complete the lithium battery 1. The battery case 5 may be cylindrical, rectangular, thin-film, etc. For example, the lithium battery 1 may be a thin-film battery. The lithium battery 1 may be a lithium-ion battery.
[0076] A separator may be disposed between the positive electrode and the negative electrode to form a battery structure, and the battery structure may be stacked in a bi-cell structure, and then immersed in an organic electrolyte. The resulting structure may then be housed in a pouch and sealed to complete a lithium ion polymer battery.
[0077] In addition, a plurality of the battery structures may be stacked to form a battery pack, which may be used in any device requiring high capacity and high output, such as a notebook computer, a smartphone, or an electric vehicle (EV).
[0078] Here, the lithium secondary battery has excellent life characteristics and high rate characteristics, and can be used in electric vehicles, for example, hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs), and in fields requiring large amounts of power storage, for example, electric bicycles and power tools.
[0079] The present invention will be described in more detail with reference to the following Production Examples, Examples and Comparative Examples. However, the Examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention. EXAMPLES
[0080] (Production of negative electrode active material) Manufacturing Example 1 Spherical graphite was prepared as a carbon-based material, and SiH4(g) and ethylene were subjected to vapor phase chemical vapor deposition at a volume ratio of 10:1.6 at a rate of 50 sccm for 40 minutes under conditions of 475°C, to obtain a negative electrode active material in which a 20 nm-thick silicon-containing amorphous coating layer was formed on the surface of the carbon-based material.
[0081] At this time, the volume ratio of the carbon matrix dispersed in the silicon-containing amorphous coating layer in the negative active material was about 30%.
[0082] Manufacturing Example 2 Spherical graphite was prepared as a carbon-based material, and SiH4(g) was vapor-phase chemically deposited on the carbon-based material at a rate of 50 sccm for 20 minutes at 475°C to obtain a negative electrode active material in which a 15 nm-thick silicon coating layer was formed on the surface of the carbon-based material.
[0083] Production Example 3 Spherical graphite was prepared as a carbon-based material, and a 20-nm-thick silicon-containing amorphous coating layer was formed on the surface of the carbon-based material by chemical vapor deposition of SiH4(g) and ethylene in a volume ratio of 10:1.6 at a rate of 50 sccm for 20 minutes at 475°C.
[0084] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0085] At this time, the volume ratio of the carbon matrix dispersed in the silicon-containing amorphous coating layer in the negative active material was about 30%.
[0086] Production Example 4 Spherical graphite was prepared as a carbon-based material, and SiH4(g) was vapor-phase chemically deposited at a rate of 50 sccm for 20 minutes at 475°C to form a 15 nm thick silicon coating layer on the surface of the carbon-based material.
[0087] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed for 120 minutes at 25°C, and then heat-treated for 120 minutes at 900°C to obtain a negative electrode active material including a silicon coating layer and a carbon coating layer on the carbon-based material.
[0088] Production Example 5 Spherical graphite was prepared as a carbon-based material, and a 20-nm-thick silicon-containing amorphous coating layer was formed on the surface of the carbon-based material by chemical vapor deposition of SiH4(g) and ethylene in a volume ratio of 10:0.4 at a rate of 50 sccm for 20 minutes at 475°C.
[0089] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0090] At this time, the volume ratio of the inactive matrix dispersed in the silicon-containing amorphous coating layer to the negative active material was about 7%.
[0091] Production Example 6 Spherical graphite was prepared as a carbon-based material, and a 20-nm-thick silicon-containing amorphous coating layer was formed on the surface of the carbon-based material by chemical vapor deposition of SiH4(g) and ethylene in a volume ratio of 10:0.8 at a rate of 50 sccm for 20 minutes at 475°C.
[0092] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0093] At this time, the volume ratio of the inactive matrix dispersed in the silicon-containing amorphous coating layer to the negative active material was about 13%.
[0094] Production Example 7 Spherical graphite was prepared as a carbon-based material, and a 20-nm-thick silicon-containing amorphous coating layer was formed on the surface of the carbon-based material by chemical vapor deposition of SiH4(g) and ethylene in a volume ratio of 10:1.2 at a rate of 50 sccm for 20 minutes at 475°C.
[0095] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0096] At this time, the volume ratio of the inactive matrix dispersed in the silicon-containing amorphous coating layer to the negative active material was about 20%.
[0097] Production Example 8 Spherical graphite was prepared as a carbon-based material, and a 20-nm-thick silicon-containing amorphous coating layer was formed on the surface of the carbon-based material by chemical vapor deposition of SiH4(g) and ethylene in a volume ratio of 10:1.6 at a rate of 50 sccm for 20 minutes at 475°C.
[0098] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0099] At this time, the volume ratio of the inactive matrix dispersed in the silicon-containing amorphous coating layer to the negative active material was about 25%.
[0100] Production Example 9 Spherical graphite was prepared as a carbon-based material, and chemical vapor deposition was performed for 20 minutes at 475°C using a mixture of SiH4(g) and ethylene in a volume ratio of 10:2 at a rate of 50 sccm to form a 20 nm-thick silicon-containing amorphous coating layer on the surface of the carbon-based material.
[0101] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0102] At this time, the volume ratio of the inactive matrix dispersed in the silicon-containing amorphous coating layer to the negative active material was about 30%.
[0103] Manufacturing Example 10 Spherical graphite was prepared as a carbon-based material, and a 20-nm-thick silicon-containing amorphous coating layer was formed on the surface of the carbon-based material by chemical vapor deposition of SiH4(g) and ethylene in a volume ratio of 10:4 at a rate of 50 sccm for 20 minutes at 475°C.
[0104] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0105] At this time, the volume ratio of the inactive matrix dispersed in the silicon-containing amorphous coating layer to the negative active material was about 50%.
[0106] Manufacturing Example 11 Spherical graphite was prepared as a carbon-based material, and chemical vapor deposition was performed for 20 minutes at 475°C using a volume ratio of SiH4(g) and ethylene of 10:5 at a rate of 50 sccm to form a 20 nm-thick silicon-containing amorphous coating layer on the surface of the carbon-based material.
[0107] Next, 10 g of the carbon-based material coated with the silicon coating layer and 1.5 g of pitch carbon source were placed in a mixer and mixed at 25°C for 120 minutes, and then heat-treated at 900°C for 120 minutes to obtain a negative electrode active material including a silicon-containing amorphous coating layer and a carbon coating layer on the carbon-based material.
[0108] At this time, the volume ratio of the inactive matrix dispersed in the silicon-containing amorphous coating layer in the negative active material was about 70%.
[0109] (Crystallization of the first coating layer) The negative active material prepared in Preparation Example 2 and the negative active material prepared in Preparation Example 3 were analyzed by an X-ray diffraction analyzer, and the results are shown in Figure 1. In addition, the surface and cross section of the negative active material were photographed by SEM and TEM, and the photographs are shown in Figure 2.
[0110] 1, a silicon crystal peak is clearly seen in the negative active material according to Preparation Example 2, which includes a silicon coating layer formed from silane gas, while the silicon crystal peak is not noticeable in the negative active material according to Preparation Example 3, which includes a silicon-containing amorphous coating layer formed from a composite gas (cogas) of silane gas and ethylene. This means that silicon crystals are not present in the negative active material according to Preparation Example 3, or the crystal size is so small that it is difficult to analyze with an analyzer.
[0111] 2, it can be seen that a silicon-containing amorphous coating layer is present on the surface of the carbon-based material of the negative active material prepared according to Preparation Example 3, and that the silicon-containing amorphous coating layer is present in the form of crystalline silicon particles distributed within the amorphous matrix material. Specifically, the upper left and upper right photos are SEM and TEM photos of the surface of the negative active material prepared according to Preparation Example 3. The middle left and middle right photos are SEM and TEM photos of the cross section of the negative active material, and the presence of the first coating layer is clearly seen. The lower left and lower right photos are SEM and TEM photos of the boundary surface of the first coating layer in the negative active material, and it can be seen that silicon nanoparticles are present therein while the first coating layer is amorphous.
[0112] (Bonding analysis of silicon-containing coating layers) In the negative electrode active material produced by Production Example 3, electron energy loss spectroscopy (EELS) line scanning was performed on the region from the carbon-based material through the silicon-containing amorphous coating layer to the outermost carbon coating layer, and the results are shown in FIG. 3.
[0113] 3, it can be seen that amorphous carbon and silicon are present in the silicon-containing amorphous coating layer on the surface of the carbon-based material in the negative active material prepared in Preparation Example 3. In addition, since a SiC peak is confirmed through XPS analysis, it can be seen that the silicon-containing amorphous coating layer contains Si particles, amorphous carbon, and SiC.
[0114] (Elemental content analysis of silicon-containing amorphous coating layer) In the negative active material prepared in Preparation Example 3, the content of constituent elements in the corresponding regions was analyzed using TEM and EDS equipment from the carbon-based material through the silicon-containing amorphous coating layer to the outermost coating layer, and the results are shown in FIG. 4 and Table 1 below.
[0115] [Table 1]
[0116] As can be seen from FIG. 4 and Table 1, the silicon-containing amorphous coating layer contains both silicon atoms and carbon atoms. In addition, it was confirmed that the weight ratio of carbon atoms is much higher than that of silicon atoms at the interface of the silicon-containing amorphous coating layer, but the weight ratio of silicon atoms is even higher than that of carbon atoms inside the silicon-containing amorphous coating layer. This suggests that most of the silicon atoms are distributed inside the silicon-containing amorphous coating layer.
[0117] (Preparation of half-cell) Example 1 A slurry was prepared from the negative active material obtained in Preparation Example 1 so that the ratio of the negative active material, conductive agent, and binder was 95.8:1:3.2. The conductive agent was Super P, and the binder was carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR).
[0118] The slurry was uniformly coated on a copper foil, dried in an oven at 80° C. for about 2 hours, roll-pressed, and further dried in a vacuum oven at 110° C. for about 12 hours to prepare a negative electrode.
[0119] The negative electrode thus prepared was used as a working electrode, lithium foil was used as a counter electrode, a polyethylene film was inserted between the negative electrode and the counter electrode as a separator, 10.0% by weight of FEC was added to a mixed solvent in which EC / EMC / DEC were mixed in a volume ratio of 3 / 5 / 2, and LiPF6 was added as a lithium salt to a concentration of 1.3M to prepare a liquid electrolyte. A CR2016 half cell was prepared according to a commonly known process.
[0120] Examples 2 to 6 Half cells were prepared in the same manner as in Example 1, except that the negative active materials obtained in Preparation Examples 3, 6, 8, 10, and 11 were used instead of the negative active material obtained in Preparation Example 1, respectively.
[0121] Comparative Examples 1 to 3 Half cells were prepared in the same manner as in Example 1, except that the negative active materials obtained in Preparation Examples 2, 4, and 5 were used instead of the negative active material obtained in Preparation Example 1, respectively.
[0122] Evaluation example 1: Electrochemical property evaluation 1 The half cells prepared in Example 1 and Comparative Example 1 were charged at 25° C. at a charging rate of 0.1 C-rate until the voltage reached 0.01 V. At this time, the cells were charged to a constant voltage at a constant current, and then charged at a constant voltage until the current reached 0.01 C or less. The cells were then discharged at a constant current of 0.1 C-rate until the voltage reached 1.5 V. After two charge-discharge cycles, the cells were repeatedly charged 30 times at a charge-discharge rate of 0.5 C-rate in the voltage range of 0.01 V to 1.5 V. Some of the results of the charge-discharge experiment are shown in Table 2 below, and the graph of the charge-discharge experiment result is shown in FIG. 5.
[0123] The initial efficiency was calculated from the following formula 1. [Formula 1] Initial efficiency [%] = [discharge capacity at first cycle / charge capacity at third cycle] x 100
[0124] [Table 2]
[0125] As can be seen from Table 2, the half cells according to Example 1 and Comparative Example 1 have substantially the same capacity, but referring to Figure 5, it can be seen that as multiple charge / discharge cycles are performed, the coulombic efficiency increases significantly, and the capacity after 30 charge / discharge cycles is also superior to that of Comparative Example 1. This result is believed to be due to the fact that in the case of Example 1, detachment of silicon particles from the negative electrode due to volumetric changes in the silicon particles is suppressed, improving cycle characteristics.
[0126] Evaluation example 2: Electrochemical property evaluation 2 A charge-discharge experiment was carried out on the half cells prepared in Example 1 and Example 2 in the same manner as in Evaluation Example 1. Some of the results are shown in Table 3 below, and the charge-discharge experiment result graph is shown in FIG.
[0127] [Table 3]
[0128] As can be seen from Table 3, the capacity and initial efficiency of the half cell according to Example 2 are slightly lower than those of Example 1, but as the charge-discharge cycle progresses, it can be seen from Figure 6 that the Coulombic efficiency is significantly improved. This result is believed to be due to the fact that the addition of the carbon coating layer in Example 2 improves electrical conductivity and prevents direct contact between the electrolyte and the active material, and the outermost carbon coating layer helps to suppress volume expansion of silicon particles due to the silicon-based inactive matrix.
[0129] Evaluation example 3: Differential capacity analysis The half cells prepared in Examples 3 to 6 and Comparative Examples 2 and 3 were charged at 25° C. at a charging rate of 0.1 C-rate until the voltage reached 0.005 V, at which point they were charged to a constant voltage at a constant current, and then charged at a constant voltage until the current was below 0.01 C. They were then discharged at a constant current of 0.1 C-rate until the voltage reached 1.5 V.
[0130] The voltage profile obtained from the above was differentiated to obtain a differential capacity graph, which is shown in FIG. 7. Referring to FIG. 7, the presence or absence of a 0.43 V peak can be confirmed. The 0.43 V peak indicates that lithium reacts with silicon to form Li 3.75 This means that the Si phase is formed. 3.75 The Si phase is the maximum amount of lithium that can react with silicon at 25°C. In such a case, the expansion rate of silicon theoretically expands to 300% and causes fatal performance degradation. 3.75 If the Si phase is not formed, the expansion coefficient will decrease, which will contribute to improving performance.
[0131] Evaluation Example 4: Particle size measurement of silicon nanoparticles in a silicon-containing amorphous coating layer XRD analysis was performed on the silicon-containing amorphous coating layers in the negative active materials obtained in Preparation Examples 4, 8, and 10, and the XRD data is shown in Figure 8. Based on the XRD data, silicon crystals in the silicon-containing amorphous coating layers were analyzed, and the Si crystal size was calculated using the Scherrer equation.
[0132] [Table 4]
[0133] (Preparation of full cell) Example 7 Anode production A slurry was prepared by using the negative electrode active material obtained in Preparation Example 3, super.P as a conductive agent, CMC as a thickener, and SBR as a binder in a weight ratio of 96:1:1.5:1.5 for the negative electrode active material / conductive agent / thickener / binder. The slurry was applied to a copper current collector having a thickness of 18 μm using a conventional method. The current collector to which the slurry was applied was dried at room temperature, secondary dried at 120° C., rolled, and punched to prepare a negative electrode to be applied to a cell.
[0134] Cathode manufacturing A mixture of lithium cobalt oxide (LCO) positive active material, carbon conductive agent (super.P), and polyvinylidene fluoride (PVdF) in a weight ratio of 94:3:3 was mixed with N-methylpyrrolidone (NMP) through a homogenizer to prepare a positive active material slurry. The positive active material slurry was applied to a thickness of about 120 μm on a 15 μm thick aluminum current collector using a doctor blade, dried at room temperature, and then dried again under vacuum at 120°C and roll pressed to prepare a positive electrode having a positive active material layer disposed on the current collector.
[0135] Manufacture of lithium secondary batteries The negative electrode was wound into a 16 mm circle, and the positive electrode was wound into a 15 mm circle. A separator was then placed between the positive and negative electrodes to produce a 2032-type coin full cell.
[0136] A 14 μm thick polyethylene-polypropylene copolymer separator was used as the separator.
[0137] The electrolyte used was a mixed solvent of EC (ethylene carbonate):DEC (diethylene carbonate):FEC (fluoroethylene carbonate) (volume ratio of 2:6:2) in which 1.3 M LiPF6 was dissolved.
[0138] Examples 8 to 10 A 2032-type coin full cell was fabricated in the same manner as in Example 7, except that the negative active material obtained in Preparation Example 3 was replaced with the negative active materials obtained in Preparation Examples 7 to 9, respectively.
[0139] Comparative Example 4 A 2032-type coin full cell was fabricated in the same manner as in Example 7, except that the negative active material obtained in Preparation Example 3 was replaced with the negative active material obtained in Preparation Example 4.
[0140] Evaluation example 5: Life characteristic evaluation For the full cells prepared in Example 7 and Comparative Example 4, charging was started at 25° C. at a charging rate of 0.2 C-rate, and the voltage was charged to 4.2 V. At this time, charging was performed at a constant current to have a constant voltage, and then charging was performed at a constant voltage until the current was 0.05 C or less. Then, discharging was performed at a constant current rate of 0.2 C-rate until the voltage reached 2.5 V. In the cycle, charging was performed at 0.5 C-rate, charging was performed at a constant current to have a constant voltage, and then charging was performed at a constant voltage until the current was 0.1 C or less. During discharging, discharging was performed at 1 C-rate until the voltage reached 2.7 V. Such charge-discharge cycles were performed 100 times. In addition, the discharge capacity at each cycle was calculated relative to the initial capacity, and the results are shown in FIG. 9. In addition, after 50 charge-discharge cycles, the negative electrode was cut and the cross section was observed. The cross-sectional shape of the negative electrode is shown in FIG. 10.
[0141] As shown in FIG. 9, the negative active material including the silicon coating layer exhibits a capacity retention rate of 64% of the initial capacity after 100 charge / discharge cycles, while the negative active material including the silicon-containing amorphous coating layer exhibits a capacity retention rate of 84%, showing excellent improvement in life characteristics.
[0142] In addition, as shown in FIG. 10, after 50 charge-discharge cycles, cracks were found in the negative electrode active material including the silicon coating layer, whereas almost no cracks were found in the negative electrode active material including the silicon-containing amorphous coating layer, confirming that stress due to volume expansion during the charge-discharge process was sufficiently alleviated.
[0143] Evaluation example 6: Life characteristic evaluation (II) The full cells prepared in Examples 8 to 10 were charged at 25° C. at a charging rate of 0.2 C-rate, and charged to a voltage of 4.2 V. At this time, the cells were charged to a constant voltage at a constant current, and then charged to a constant voltage at a constant current of 0.05 C or less. The cells were then discharged at a constant current of 0.2 C-rate until the cells reached 2.5 V. In the cycle, the cells were charged at a 0.5 C-rate, charged to a constant voltage at a constant current, and then charged to a constant voltage at a constant current of 0.1 C or less. During discharge, the cells were discharged at a 1 C-rate until the cells reached 2.7 V. The charge-discharge cycle was repeated 100 times. The initial capacity and efficiency are shown in Table 5 below, and the capacity retention rate due to the charge-discharge cycle was measured and shown in FIG. 11.
[0144] [Table 5]
[0145] As can be seen from Table 5, all of Examples 8 to 10 showed good initialization efficiency. Example 9 showed the highest capacity. Also, referring to FIG. 11, as the charge-discharge cycle progressed, Example 9 showed a superior capacity retention rate compared to Examples 8 and 10.
[0146] Although the preferred embodiment of the present invention has been described above with reference to the drawings and examples, it is understood that the present invention is merely illustrative and that various modifications and equivalent embodiments are possible if one has ordinary skill in the art. Therefore, the scope of the present invention is defined by the claims.
Claims
1. A carbon-based material; SiC x and a silicon-containing amorphous coating layer represented by The SiC x In the formula, x is 0.07<x<0.7; The silicon-containing amorphous coating layer includes silicon particles having a particle size of 5 nm or less, the silicon-containing amorphous coating layer comprises silicon nanoparticles and a carbon matrix; The carbon matrix occupies 10 to 60 parts by weight based on 100 parts by weight of the silicon-containing amorphous coating layer.
2. The SiC x 2. The negative electrode active material for a lithium secondary battery according to claim 1, wherein x satisfies the relationship 0.2<x<0.
5.
3. The negative electrode active material for a lithium secondary battery according to claim 1 , wherein the silicon particles include crystalline silicon particles.
4. The negative electrode active material for a lithium secondary battery according to claim 1 , wherein the silicon-containing amorphous coating layer does not show a peak at 0.43 V in differential capacitance analysis (dQ / dV).
5. 2. The negative electrode active material for a lithium secondary battery according to claim 1, wherein the silicon nanoparticles have a particle size of 3 to 5 nm.
6. 2. The negative electrode active material for a lithium secondary battery according to claim 1, wherein the silicon-containing amorphous coating layer has a thickness of 5 nm to 4,000 nm.
7. The negative electrode active material for a lithium secondary battery according to claim 1 , wherein the silicon-containing amorphous coating layer is disposed on a part or the whole of a surface of the carbon-based material.
8. 2. The negative electrode active material for a lithium secondary battery according to claim 1, wherein the carbon-based material comprises natural graphite, artificial graphite, hard carbon, soft carbon, or a combination thereof.
9. The negative electrode active material for a lithium secondary battery according to claim 1 , wherein a carbon coating layer containing amorphous carbon is disposed on the silicon-containing amorphous coating layer.
10. Providing a carbon-based material; On the surface of the carbon-based material, SiC x providing a silicon-containing amorphous coating layer, where x is an integer of 0.07<x<0.7; providing the silicon-containing amorphous coating layer includes simultaneously providing a silane-based gas and a hydrocarbon-based gas; the silicon-containing amorphous coating layer comprises silicon nanoparticles and a carbon matrix; The carbon matrix is present in an amount of 10 to 60 parts by weight based on 100 parts by weight of the silicon-containing amorphous coating layer.
11. 11. The method of claim 10, wherein a volume ratio of the silane-based gas to the hydrocarbon-based gas is in the range of 1:0.01 volume % to 1:1 volume %.
12. 11. The method of claim 10, wherein a volume ratio of the silane-based gas to the hydrocarbon-based gas is in the range of 1:0.01 volume % to 1:0.5 volume %.
13. 11. The method of claim 10, wherein the forming of the silicon-containing amorphous coating layer is performed at a temperature of 400 to 900[deg.] C.
14. The method of claim 10, further comprising providing a carbon coating layer including amorphous carbon after providing the silicon-containing amorphous coating layer.
15. The method of claim 14, wherein the providing the carbon coating layer comprises providing a carbon precursor and then heat treating the carbon precursor.
16. The method of claim 15, wherein the heat treatment is performed at a temperature of 800°C to 1,100°C.
17. A negative electrode comprising the negative electrode active material according to any one of claims 1 to 9; A positive electrode and and an electrolyte.
Citation Information
Patent Citations
Method for preparing lithium iron phosphate positive material
CN103390750A
Negative electrode active material for lithium secondary battery and lithium secondary battery including the same
JP2012064565A
Silicon-containing particle, negative electrode material of nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2014192064A
Negative electrode for all-solid battery
JP2017054720A
Negative electrode active material and lithium secondary battery including the same
US20180219216A1